Method for producing lyocell staple fiber

JP2022542961A5Active Publication Date: 2024-12-05LENZING AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022506112
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-08-02
Filing Date
2020-07-29
Publication Date
2024-12-05
Estimated Expiration
2040-07-29

AI Technical Summary

Technical Problem

Existing methods for producing crosslinked lyocell staple fibers are inefficient and result in fiber damage, reduced strength, and high chemical consumption, while conventional processing techniques fail to achieve optimal fiber properties such as residual crimps and low fibrillation resistance.

Method used

A novel method combining tow post-treatment and fleece post-treatment by washing and cross-linking continuous cellulose filaments before cutting, followed by forming a nonwoven fleece and pressing, which allows for milder treatment conditions and improved fiber properties.

Benefits of technology

The method produces lyocell staple fibers with enhanced residual crimps, increased fiber strength, and reduced fibrillation resistance, achieving Hoeller coefficients F1 ≥ 2.1 and F2 ≥ 3.0, with a coefficient of variation in wet abrasion resistance (CV NSF) of less than 50%, outperforming conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2021023594000001
    Figure 2021023594000001
  • Figure 2021023594000002
    Figure 2021023594000002
Patent Text Reader

Abstract

The present invention comprises the following steps in the following order: a) extruding filaments from a solution of cellulose in an organic solvent; b) precipitating cellulose to form continuous cellulose filaments; c) washing the cellulose filaments; d) contacting the cellulose filaments with a cross-linking agent; e) reacting the cellulose filaments with a cross-linking agent in a reaction chamber; f) washing the treated cellulose filaments; g) cutting the cleaned cellulose filaments to form staple fibers; h) forming a nonwoven fabric from the staple fibers and pressing the nonwoven fabric; i) applying a finishing touch to the nonwoven fabric and pressing the nonwoven fabric; The present invention relates to a method for producing lyocell staple fiber, comprising:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing lyocell staple fibers, and to lyocell staple fibers that can be obtained by the method according to the present invention. [Background technology]

[0002] In response to the environmental problems associated with the known viscose process for producing cellulose fibers, strenuous efforts have been made over the past few decades to provide more environmentally friendly alternatives. One such possibility, which has attracted particular attention in recent years, involves dissolving cellulose in an organic solvent without forming derivatives and extruding a molded body from the solution. Fibers spun from such a solution have received the common name lyocell from BISFA (The International Bureau for the Standardization of Man-made Fibers), where the organic solvent is understood to be a mixture of organic chemicals and water.

[0003] Furthermore, such fibers are also known by the term "solvent-spun fibers."

[0004] In particular, mixtures of tertiary amine oxides and water have been found to be perfectly suitable as organic solvents for producing lyocell fibers and other lyocell molded bodies, respectively. Thus, N-methylmorpholine-N-oxide (NMMO) is primarily used as the amine oxide. Other suitable amine oxides are disclosed in EP0553070A. Ionic liquids are also suitable as organic solvents. A method for producing cellulose molded bodies from a solution of cellulose in a mixture of NMMO and water is disclosed, for example, in USA4,246,221 or WO93 / 19230A. According to this method, the cellulose solution is extruded from a spinneret, stretched in an air gap, and precipitated from the solution in an aqueous precipitation tank. This process will hereafter be referred to as the "amine oxide process" or "lyocell process," and the abbreviation "NMMO" will hereafter represent all tertiary amine oxides capable of dissolving cellulose. Fibers produced by the amine oxide process are characterized by high fiber strength, high wet modulus, and high snag strength, not only in the conditioned state but also in the wet state.

[0005] Commercially manufactured lyocell fibers are primarily in the form of staple fibers.

[0006] When the spinning solution is extruded through the spinneret, continuous filaments are initially formed from the solution. Even after settling in the spinning vat, the continuous cellulose filaments remain. When these cellulose filaments are cut into individual lengths, they become staple fibers.

[0007] Extensive prior art is known regarding the processing of lyocell fibers after spinning.

[0008] The following steps are necessary for processing lyocell fibers in any case (note that this list should not be interpreted as a chronological order of the process): - Wash it multiple times; - To apply finishing touches; - Taking measures to induce crimp in the fibers; - Drying the fibers once or, if necessary, several times; - And cutting the fibers into staple fibers.

[0009] Furthermore, lyocell fibers are known to have a particular tendency to fibrillate. Numerous measures have already been proposed for this property, and treating lyocell fibers with a crosslinking agent is a commercially important procedure.

[0010] Suitable crosslinking agents are described, for example, in EP0538977A, WO97 / 49856A, and WO99 / 19555A. Other crosslinking agents are known from, for example, WO94 / 09191A and WO95 / 28516A.

[0011] Particularly preferred crosslinking agents are substances of formula (I) <00000- 繊維に捲縮を誘導するための対策を講じること; - 一回または必要であれば数回繊維を乾燥すること; - および繊維をステープルファイバに切断すること。

[0009] さらに、リヨセル繊維はフィブリルしやすいという特定の傾向を有することが知られている。この特性に対して数多くの対策が既に提示されており、リヨセル繊維を架橋剤で処理することは商業的に重要な手順である。

[0010] 適切な架橋剤は、例えば、EP0538977A、WO97 / 49856A、およびWO99 / 19555Aに記載されている。他の架橋剤は、例えば、WO94 / 09191AおよびWO95 / 28516Aから公知である。

[0011] 特に好ましい架橋剤は、式(I)

[0012]

化

[0013] さらに、セルロースフィラメントをいつステープルファイバに切断するか、およびそれからの結果として、どのような形態で(連続フィラメントまたは既に切断されたステープルファイバ)リヨセル繊維を上で示した様々な処理ステップに供するかという問題に関して、先行技術は様々な概念を提供している。

[0014] For example, methods are known from WO94 / 27903A and WO95 / 24520A for performing washing and crimping steps on cellulose filaments that have not yet been cut. This is also called "tow post-treatment." In this method, crimping is induced in the fibers using a so-called "stuffer box." WO98 / 28516A describes that lyocell fibers can be treated with a crosslinking agent within the scope of tow post-treatment.

[0015] On the other hand, WO97 / 14829A provides a method in which cellulose filaments are cut into staple fibers immediately after spinning and the first washing bath.

[0016] In the method of WO97 / 14829A, a nonwoven fleece is formed from staple fibers, and so-called "permanent crimp" is obtained in the fibers by compressing or pressing the nonwoven fabric. Further processing steps until the first drying of the fibers are carried out in the form of staple fibers or in the form of this nonwoven fabric. Hereafter, this concept will be referred to as "fleece post-processing."

[0017] Alternative methods for producing crosslinked fibers are known from US5,562,739A, GB2373784A, and WO2004 / 007818A1.

[0018] Further details regarding the processing of newly spun fibers are known from CN204265902(U), CN203960407(U), CN203904520(U), CN203403200(U), CN203402582(U), CN204000264(U), CN203999953(U), CN106757906(A), and CN108360182(A).

[0019] In particular, in relation to the production of lyocell staple fibers treated with crosslinking agents (hereinafter referred to as "crosslinked fibers"), known processing methods for newly spun fibers present problems in terms of both chemical consumption and method efficiency. [Overview of the project] [Problems that the invention aims to solve]

[0020] The object of the present invention is to provide an improved method for producing cross-linked lyocell staple fibers. [Means for solving the problem]

[0021] The objective is to follow these steps in the following order: a) Step of extruding a filament from a cellulose solution in an organic solvent, b) A step of precipitating cellulose to form continuous cellulose filaments, c) Step of washing the cellulose filament, d) A step of bringing cellulose filaments into contact with a crosslinking agent, e) A step of reacting cellulose filaments with a crosslinking agent in a reaction chamber, f) A step of washing the treated cellulose filament, g) Step of cutting the washed cellulose filaments into staple fibers, h) A step of forming a nonwoven fleece from staple fibers and pressing the nonwoven fleece, i) A step to finish the nonwoven fleece and press the nonwoven fleece, This is achieved by a method for producing lyocell staple fibers, including [the specified element].

[0022] Preferred embodiments are shown in the dependent claims. [Brief explanation of the drawing]

[0023] [Figure 1] This figure shows a block diagram illustrating the sequence of a preferred embodiment of the method according to the present invention. [Figure 2] This figure shows an image of the lyocell staple fiber according to the present invention under a polarized optical microscope. [Figure 3]This figure shows a comparison of the Hoeller coefficients of prior art lyocell fibers and lyocell staple fibers according to the present invention. [Modes for carrying out the invention]

[0024] Surprisingly, it was found that elements of the two concepts—towing post-treatment and fleece post-treatment—can be combined in a novel way, resulting in a significant improvement in the properties of the fibers.

[0025] According to the present invention, the initial washing of the fibers (to remove solvents), contact with the crosslinking agent, and reaction with the crosslinking agent are carried out while the fibers remain in the form of (continuous) cellulose filaments, i.e., in tow form. The cellulose filaments are then cut into staple fibers only after being newly washed (hereinafter also referred to as "crosslinking agent washing"), formed into nonwoven fleece, pressed, and finished.

[0026] Compared to so-called "fleece post-treatment," applying the crosslinking agent treatment in steps c) to f), particularly step e), to toe-form fibers was found to result in significant savings in terms of applied energy and chemicals used. This also means that milder conditions can be used for fiber treatment compared to "fleece post-treatment."

[0027] However, through the final process steps h) and i) in the nonwoven form, the fibers further exhibit the valuable property of "residual crimp".

[0028] According to WO97 / 14829, “residual crimp” is understood as the presence of at least two compression points on average per millimeter of filament length, where these compression points are maintained on the dry fiber and are visible as a change in color when viewed under linearly polarized light. Preferably, this “residual crimp” is still detectable even after the mechanical stress that occurs during carding and spinning.

[0029] Surprisingly, the crosslinked fibers obtained by the method according to the present invention have better fiber data (i.e., as fleece or toe) than fibers treated with the same crosslinking agent by prior art.

[0030] A preferred embodiment of the method according to the present invention is characterized by drying the filament or staple fiber for the first time after step i).

[0031] The reaction of cellulose filaments with crosslinking agents is usually carried out at high temperatures.

[0032] In particular, the reaction in step e) can be carried out with energy input.

[0033] Furthermore, the reaction in step e) is preferably carried out in the presence of vapor. Naturally, other options, such as processing with electromagnetic waves, particularly microwaves, also occur.

[0034] In a preferred embodiment, step e) of the method according to the present invention is carried out in a steam chamber. For example, a J-box can be used for this step.

[0035] The duration of Step e) may be 3 to 30 minutes, preferably 10 to 25 minutes, and particularly preferably 15 to 20 minutes.

[0036] The crosslinking agent can be used in an amount such that the crosslinking agent content G (unit moles) per 1 kg of cellulose (atro) is given by the following formula: G × R = 0.10 to 0.45, preferably 0.10 to 0.35, and especially preferably 0.20 to 0.35 (In the formula, R represents the number of reactive groups in the crosslinking agent.) The following applies: R is at least 2, and for the crosslinking agent NHDT having formula (I), R=2. For other crosslinking agents, R may be >2. For example, for the sodium salt of p-[(4,6-dichloro-1,3,5-triazine-2yl)amino]benzenesulfonic acid ("SDTB") which can be used as a crosslinking agent, the following applies: R=3.

[0037] For the purposes of this invention, it will be understood by those skilled in the art that the term "reactive group" refers to a group that can covalently bond with the OH group of cellulose.

[0038] The amount required to achieve the desired content of crosslinking agent in cellulose can be determined by those skilled in the art within the scope of preliminary tests. Typically, it can be assumed that it can be found in the fiber in the range of 30% to 70% by weight, particularly 40% to 60% by weight, of the crosslinking agent originally used.

[0039] The amount of crosslinking agent obtained in the fiber can be determined by analyzing the characteristic properties of the crosslinking agent. For example, in the case of nitrogenous crosslinking agents, this can be determined by using quantitative nitrogen analysis of the fiber.

[0040] In a preferred embodiment, the compound of formula (I)

[0041] [ka] (In the formula, X represents a halogen, R = H or the ionic part, and n = 0 or 1) Alternatively, a salt of each of these compounds, preferably the sodium salt of 2,4-dichloro-6-hydroxy-1,3,5-triazine, is used as a crosslinking agent in the method according to the present invention. Hereafter, this compound will be abbreviated as "NHDT".

[0042] This compound has two reactive groups (two halogen moieties).

[0043] The crosslinking agent of the compound of formula (I) is preferably used in an amount of 30 to 80 g, preferably 45 to 60 g, per 1 kg of cellulose (atro).

[0044] The object of the present invention is to have residual crimp and a coefficient of variation (CV) of wet abrasion resistance (NSF). NSF This is solved by lyocell staple fibers that can be obtained by the method according to the present invention described above, using the crosslinking agent NHDT, wherein the content is 50% or less.

[0045] In a variation of a preferred embodiment, the lyocell staple fiber according to the present invention has a CV of 45% or less, particularly preferably 40% or less. NSF It has.

[0046] NSF is a key numerical value representing the fiber's resistance to fibrillation that occurs during fabric washing, and is determined by the test method shown in the examples. Based on the good wet abrasion resistance of the fiber according to the present invention, this requirement, which is essential for crosslinked fibers, is also met.

[0047] Coefficient of variation (CV) of fibers NSF This is determined by the measurement method described in the subsequent section on embodiments.

[0048] As clearly stated above, the low CV of the fibers according to the present invention NSF The values ​​represent a striking characteristic that is extremely important when compared to fibers produced by fleece crosslinking in NHDT. As mentioned above, conventional fleece post-treatment causes fiber damage during the crosslinking reaction, thereby not only reducing strength but also leading to greater variation in (reduced) strength because not all cellulose chains are damaged to the same degree. This ultimately affects the coefficient of variation CV of wet abrasion resistance. NSF The price will increase.

[0049] As shown in Tables 4 and 5 below, according to Examples 1 to 8, all fibers according to the present invention have a CV of less than 45%. NSF It has a value, and for the most part, the CV is even below 40% NSF It has a value. Such a low CV NSFThis is not expected for fibers crosslinked with NHDT by post-treatment of fleece. From the evaluation of numerous examples of fleece crosslinked fibers (e.g., LENZING (trademark) Lyocell LF type with a fineness of 1.7 dtex, manufactured by Lenzing Aktiengesellschaft (Werkstrasse 2, A-4860 Lenzing), a commercially available lyocell staple fiber), they all have a CV value in the range between 60% and 80%. NSF It has been shown to have a value.

[0050] The object of the present invention can also be obtained by the method according to the invention using the crosslinking agent NHDT, and further having the following properties: - The fibers have a fineness in the range of 1.2 dtex to 1.5 dtex, preferably 1.25 dtex to 1.45 dtex. - The fibers have residual crimp. - The fibers have a fiber strength of at least 36 cN / tex in the positive quantity state, preferably in the range of 38 cN / tex to 42 cN / tex. - The fibers have a Hoeller coefficient in the range of F1≥2.1, preferably ≥2.4, particularly preferably 2.5 to 3.2, and - The fibers have a Hoeller coefficient in the range of F2≥3.0, preferably ≥3.5, particularly preferably 4.0 to 5.5. It is realized by lyocell staple fibers characterized by a combination of the above.

[0051] ​​​​​​​​- The fibers have a Hoeller coefficient F1 ≥ 2.8, preferably ≥ 3.0, and particularly preferably in the range of 3.2 to 3.5, and - The fibers have a Hoeller coefficient F2 ≥ 3.0, preferably ≥ 3.6, and particularly preferably in the range of 3.9 to 5.5. It is realized by lyocell staple fibers, characterized by a combination of these elements.

[0052] In a variation of the preferred embodiment, these fibers having finenesses of 0.6 dtex to 1.2 dtex and 1.2 dtex to 1.5 dtex, as described above, each have a coefficient of variation CV of wet abrasion resistance of 50% or less, particularly 45% or less. NSF It has.

[0053] Commercially produced fibers typically consist of multiple fibers. Those skilled in the art will understand that, in this specification, the term “fiber fineness” refers to the average of several measurements, preferably 20 measurements, of several fibers.

[0054] First, the fibers according to the present invention differ from commercially available cross-linked lyocell fibers produced by conventional post-towing treatments in terms of the residual crimp characteristics described above.

[0055] Compared to NHDT-crosslinked lyocell fibers produced by fleece post-processing, the fibers according to the present invention are distinguished, particularly by their increased fiber strength in the positive weight state.

[0056] Furthermore, the fibers according to the present invention have a significantly lower CV, as described above. NSF In this respect, it differs from lyocell fibers crosslinked with NHDT by the fleece post-treatment process.

[0057] In 1984, Holler and Puchegger (Melliand Textilberichte 1984, 65, 573-574) introduced a "new method to characterize regenerated cellulose fibers."

[0058] The authors provided a graph that reflects the properties of fibers based on two calculated coefficients. These coefficients are plotted on two axes, generating a so-called "Hoeller graph." In this graph, different fiber types occupy different regions.

[0059] The mechanical textile fiber properties that produce these two coefficients are well known to experts and can be found in Chapter 7 of the BISFA "Testing methods viscose, modal, lyocell und acetate staple fibers and tows" ["Prufverfahren Viskose,Modal,lyocell und Acetat Stapelfasern und Seile"] 2004 edition, and can be tested accordingly.

[0060] The two Hoeller coefficients F1 and F2 are calculated as follows: F1 = -1.109 + 0.03992 * FFk - 0.06502 * FDk + 0.04634 * FFn - 0.04048 * FDn + 0.08936 * BISFA modulus of elasticity + 0.02748 * SFk + 0.02559 * KFk and F2=-7.070+0.02771*FFk+0.04335*FDk+0.02541*FFn+0.03885*FDn-0.01542*BISFA modulus+0.2891*SFk+0.1640*KFk, During the ceremony, FFk is the fiber strength in the correct weight state. FDk is the elongation of the fiber in the correct weight state. FFn is the fiber strength in a wet state. FDn is the elongation of fibers in a wet state. The BISFA modulus is the wet modulus at 5% elongation. SFk is the hooking strength in the correct state. SDK is a hook extension in the correct state. KFk is the knot strength in the correct weight state. That is the case.

[0061] According to Lenzinger Berichte 2013, 91, 07-12, in the Hoeller graph, fibers from different production processes (e.g., direct dissolution or derivatization) can be clearly distinguished from one another. Even within the direct dissolution fiber type, fibers produced from different direct solvents (e.g., fibers spun from a solution in an ionic liquid versus those from a solution in NMMO) occupy different regions.

[0062] Commercially available lyocell fibers (non-crosslinked) exhibit Hoeller F1 values ​​between 2 and 3 and Hoeller F2 values ​​between 2 and 8 (WO2015 / 101543 and Lenzinger Berichte 2013, 91, 07-12). Fibers produced from direct solutions in ionic liquids range from Hoeller F1 values ​​between 3 and 5.5 and Hoeller F2 values ​​between 7 and 10.5 (Lenzinger Berichte 2013, 91, 07-12). WO2015 / 101543 discloses a novel lyocell fiber type with a lower range of Hoeller F2 values ​​between 1 and 6 and Hoeller F1 values ​​between -0.6 and the upper right boundary, defined by F2-4.5*F1≧3, particularly ≧1.

[0063] Therefore, WO2015 / 101543 describes a (non-crosslinked) lyocell fiber having a specific position in the Hoeller graph. The claimed lyocell fiber was produced using a high-quality wood pulp mixture with a high α content and a low non-cellulose content, such as hemicellulose, to achieve a specific molecular weight distribution and optimized spinning parameters. This is achieved by reducing the effects of air gaps, performing spinning at high temperatures, and using a lower draw ratio. The fiber is characterized by increased wet abrasion resistance despite not being crosslinked.

[0064] Further forms of non-crosslinked lyocell fibers in other areas of the Hoeller graph are disclosed in WO2019 / 170670A1.

[0065] The fibers according to the present invention have Hoeller coefficients of F1≧2.1 and F2≧3.0 for fineness in the range of 1.2dtex to 1.5dtex, and Hoeller coefficients of F1≧2.8 and F2≧3.0 for fineness in the range of 0.6dtex to 1.2dtex. Crosslinked lyocell fibers having such high Hoeller coefficients F1 and F2 for each fineness have not yet been described.

[0066] The following table summarizes the values ​​of fabric parameters related to the determination of the Hoeller coefficient for several example lyocell fibers A to H.

[0067] [Table 1]

[0068] Fiber A is a commercially available crosslinked fiber with mechanical crimp, produced according to conventional post-towing treatment, and is treated with a crosslinking agent different from the crosslinking agent used in the production of the fiber according to the present invention.

[0069] Fiber B is a commercially available crosslinked lyocell fiber treated with the same crosslinking agent as the fiber according to the present invention. However, fiber B is also produced by post-towing treatment.

[0070] Fiber C is a commercially available fiber produced by fleece post-treatment and treated with the same crosslinking agent as the fiber according to the present invention.

[0071] Fiber D, like fiber C, is produced by fleece post-treatment and is an ultrafine fiber treated with the same crosslinking agent as the fiber according to the present invention, but its low fineness is significantly different from fiber C.

[0072] For another comparison, we also included fiber E, a standard non-crosslinked lyocell fiber. This comparison allows us to estimate how the crosslinking process affects the fabric parameters.

[0073] Similarly, we also showed fiber F, which is a non-crosslinked lyocell ultrafine fiber. This fiber is suitable for comparison with crosslinked ultrafine fibers, or for determining the effect of the crosslinking process on the fabric parameters of ultrafine fibers.

[0074] Table 1, shown above, shows the Hoeller coefficients for fibers G and H according to the present invention. According to this, fiber G is a fiber having a fineness within the range of fibers A, B, C, and E, which are not part of the present invention. Fiber H is an ultrafine fiber having a fineness within the range of fibers D and F, which are not part of the present invention. According to Table 1, the Hoeller coefficients of the fibers according to the present invention differ significantly from those of other crosslinked lyocell fibers A to D, and similarly differ significantly from those of non-crosslinked lyocell fibers E and F. In particular, they differ significantly when compared to fibers within the same fineness range.

[0075] In Figure 3, which shows the results of numerous measurements for fibers of types A to H, the differences in Hoeller coefficients F1 and F2 are more clearly visible graphically.

[0076] Therefore, the fibers according to the present invention exhibit extremely high strength.

[0077] In particular, conventional fleece post-treatments result in a significant decrease in fiber strength as a result of damage during the cross-linking reaction, as shown based on fibers C and D. This damage is caused by hydrolysis of the cellulose chains. Shorter chains result in reduced fiber strength.

[0078] Conversely, fibers produced by post-towing treatment exhibit the disadvantage of being extremely brittle, regardless of the chemistry of the crosslinking agent, in addition to a lack of residual crimp. This is evident from the low snagging and knot strength of fibers A and B. In this case, fibers G and H according to the present invention produce excellent values, meaning that the problem of embrittlement did not occur, and as a result the Hoeller coefficient F2 is significantly higher.

[0079] Most notably, the Hoeller coefficient F1 also increases compared to standard fibers (fibers E and F). This is because the weighting of the fiber's elongation in dry and wet conditions (FDk, FDn) is negative in this case. In particular, the wet elongation (FDn) decreases significantly due to the crosslinking of the fiber.

[0080] In addition, the slippage (SDk) is also important. Similarly, a low slippage is equivalent to a brittle fiber. Brittle fibers are difficult to process, which is due in part to the formation of dust during the spinning process.

[0081] The fibers according to the present invention are superior to commercially available lyocell fibers crosslinked with NHDT in terms of fiber elongation (FDk) in their positive weight state. The fiber elongation (FDk) of the fibers according to the present invention in their positive weight state is preferably 10% or more, and particularly preferably 10% to 11%.

[0082] As a result of these characteristics, the fibers according to the present invention preferably have a working capacity of 380%*cN / tex or more. The working capacity shown in Table 2 is obtained from the product of the fiber strength FFn[cN / tex] and the elongation FDk[%].

[0083] [Table 2]

[0084] Compared to commercially produced fibers crosslinked with NHDT, the fibers according to the present invention also have an increased nitrogen content with the same amount of crosslinking agent, i.e., a higher efficiency of the crosslinking reaction.

[0085] Furthermore, the fibers according to the present invention are preferably characterized by a wet abrasion resistance (NSF) of 300 r / dtex or more, more preferably 400 r / dtex or more, and particularly preferably 450 r / dtex or more. Non-crosslinked lyocell fibers have an NSF of approximately 40 to 80 r / dtex.

[0086] The crosslinking agent content G (unit mole) per 1 kg of cellulose (atro) in the fiber according to the present invention is preferably given by the following formula: G × R = 0.10 to 0.45, preferably 0.10 to 0.35, and especially preferably 0.20 to 0.35 (In the formula, R represents the number of reactive groups in the crosslinking agent, as defined above.) Follow the rules.

[0087] Particularly preferably, the crosslinking agent content of the compound of formula (I) is 2.0 to 3.0% by weight based on cellulose (atro).

[0088] The present invention also relates to a fiber bundle containing at least 20 kg of lyocell staple fibers according to the present invention. Thus, the present invention provides the fibers according to the present invention in commercial quantities.

[0089] Such quantities of lyocell staple fibers are unlikely to be produced in laboratory systems with only one or a few spinnerets, especially those with only a few spinning holes, as are used for scientific research.

[0090] Conversely, it is obvious that there is a significant difference between such laboratory systems and commercial production in terms of the manufacturability of fibers with certain textile parameters.

[0091] The present invention also relates to a woven article containing lyocell staple fibers according to the present invention.

[0092] Textile articles are preferably provided in the form of yarn. In either case, the production of yarn requires a certain amount of fiber; in other words, at least several kilograms of fiber are required, which is unlikely to be produced in the laboratory system described above.

[0093] Table 3 below illustrates the yarn data of two commercially produced fiber bales (comparative bales 1 and 2) of fiber C, compared with a single bale of each fiber G according to the present invention produced by Examples 2 and 5, as described below.

[0094] [Table 3]

[0095] In addition to high yarn strength and elongation, bales made from the fibers according to the present invention achieve improved product quality based on reduced variations in thickness and fineness, as well as a reduced number of nits. As described, the reduced brittleness of the fibers also reduces the dust value. This improves the processability of the fibers in spinning machines.

[0096] Detailed description of the drawing Figure 1 is a block diagram of the process steps when carried out to produce a preferred embodiment of the fiber according to the present invention. The initial washing of the fiber (to remove solvent), contact of the fiber with the crosslinking agent, and reaction with the crosslinking agent are carried out while the fiber remains in the form of (continuous) cellulose filaments, i.e., tow. The cellulose filaments are cut into staple fibers only after washing off the crosslinking agent. The individual steps are listed below in chronological order: 1) Production of spinning solution; 2) Spinning of fibers, including extrusion of filaments from a cellulose solution in an organic solvent and precipitation of cellulose to form continuous cellulose filaments; 3) Cleaning cellulose filaments using tow cleaning; 4) Impregnation by contacting cellulose filaments with a crosslinking agent; 5) Reaction of cellulose filaments with crosslinking agents in the reaction chamber; 6) Washing of the crosslinking agent by washing the treated cellulose filaments; 7) Cutting the washed cellulose filaments into staple fibers; 8) Formation of nonwoven fleece from staple fibers; 9) Dehydration by pressing nonwoven fleece; 10) Finishing the nonwoven fleece and pressing the nonwoven fleece again; 11) Drying; 12) Production of textile bales.

[0097] Figure 2 shows a polarized light microscope image of a preferred embodiment of the lyocell staple fiber according to the present invention (Example 1 from Table 4 below). Using linear polarization, irregular crimping points maintained on the dry fiber during spinning are visualized. According to WO97 / 14829, "residual crimp" is understood to mean that there are at least two crimping points on average per millimeter of filament length. The fiber in Figure 2 has the valuable property of "residual crimp" obtained as a result of the final process steps h) and i) (process steps 9-11 in Figure 1, respectively) of the method according to the present invention. The microcrimp of the lyocell staple fiber in Figure 2 is 10⁷ / 2 cm.

[0098] Figure 3 shows Hoeller Figure 50, which compares Hoeller coefficients F1 and F2 of preferred embodiments of prior art lyocell fibers and lyocell staple fibers according to the present invention.

[0099] Figure 50 shows the measurement results for fibers of types A to H. See Table 1 and the descriptions related to fibers A to H. Axes 51 and 52 correspond to Hoeller coefficients F1 and F2, respectively. Figure 50 can then be divided into several regions 53 to 58, where region 53 contains points for fibers A and B, region 54 contains points for fibers C and D, region 55 contains points for fiber E, and region 56 contains points for fiber F. Fibers G (region 57) and H (region 58) according to the present invention are clearly separated from the other regions 53 to 56. [Examples]

[0100] Examples 1-5 Continuous cellulose filaments were spun in a semi-commercial pilot plant using a known method to form fiber tows, which were continuously washed to make them NMMO-free. After washing, the fiber tows were pressed to minimize the carryover of wash water to the subsequent impregnation bath. The impregnation bath contained a crosslinking agent (NHDT) and was continuously reinforced with the crosslinking agent from a strong bath. Immediately after contact with the crosslinking agent, a sodium hydroxide solution was applied in a further bath. The sodium hydroxide bath was also continuously reinforced with sodium hydroxide solution to maintain a consistent and appropriate concentration over a long period.

[0101] To reduce side reactions, the tank was cooled to 10°C. The modified fiber tow was then introduced into a steam chamber designed in the shape of a J-box.

[0102] The dwell time could be measured using the corresponding mark on the toe and a stopwatch.

[0103] The fiber tow was drawn from the J-box and subjected to crosslinking agent washing to remove excess chemicals. Immediately thereafter, the tow was fed to a cutting tower to form staple fibers. The fiber staples were rinsed with water and subjected to nonwoven fleece formation. After the nonwoven fleece was formed, it was pressed and subjected to finishing. The finished nonwoven fleece was pressed again, opened by a nonwoven fleece separator, dried in a suitable dryer to produce finished fibers, and then subjected to a packaging machine.

[0104] Table 4 below summarizes the test parameters of several tests (Examples 1-5) relating to the production of fibers having a fineness in the range of approximately 1.35 dtex according to the present invention. This experiment demonstrates the effects of various important production parameters, namely NHDT dosage, alkaline solution concentration, and residence time.

[0105] [Table 4]

[0106] In Example 2, the residence time was reduced due to an increase in production speed. It was shown that cross-linked fibers could be produced similarly, but with a lower nitrogen filling rate.

[0107] Table 5 below further shows the test parameters for several tests (Examples 6-8) relating to the production of ultrafine fibers according to the present invention having a fineness in the range of approximately 0.9 dtex. The production parameters, namely NHDT dosage, alkaline solution concentration, and residence time, were kept essentially constant throughout the tests. Thus, the test data show the natural, production-related fluctuations in the fabric parameters of the fibers produced by the method according to the present invention.

[0108] [Table 5]

[0109] In all Examples 1-8, the coefficient of variation CV of wet abrasion resistance was independent of the fineness of the produced fibers. NSF This indicates that in each case it was below 45%, or even below 40% in most of the examples.

[0110] In principle, the technology according to the present invention is also suitable for various other modifications to fiber strands, such as applying reactive dyes and then crosslinking them.

[0111] However, the technology according to the present invention is also generally suitable for the application of other modifiers other than crosslinking agents, such as chitosan (WO2010 / 031091A1).

[0112] In addition to the crosslinking agent NHDT mentioned above, other crosslinking agents such as those described in the literature mentioned above, or other reactive resins that cure by the action of atmospheric humidity, oxygen, or temperature, such as single or multi-component systems, particularly epoxy, acrylate, polyurethane, and similar compounds, can also be used. In particular, the conditions required when applying chemicals can be adjusted very easily. For example, the impregnation tank can be heated. The reaction chambers can also be adapted to the required temperature or residence time.

[0113] Test method Determination of wet abrasion resistance (NSF) Wet abrasion resistance (NSF) is a key value indicating the fiber's resistance to fibrillation. This key value was determined using the wet abrasion method described in "Zur Fasernassscheuerung von Viskosefasern," Faserforschung und Textiltechnik 19 (1968), No. 10, pp. 447-452. In this process, the fiber is rotated on a wet roller and rubbed. The number of rotations until the fiber breaks in half is determined.

[0114] The abrasion resistance of single fibers, preloaded with weights in a wet state, is determined using a steel rotating shaft covered with a filament hose (viscose filament stocking). The number of rotations until the fiber wears down and breaks is counted and correlated with the fineness of each fiber.

[0115] To calibrate the measurements, or to ensure that filament stocking wear does not affect the measurements, the wet abrasion resistance of the calibration fiber is determined at regular intervals, particularly at least daily. The calibration measurements should preferably not deviate by more than 20% from the long-term average of all calibration measurements using a new filament stocking; otherwise, the filament stocking must be replaced. Within the scope of this invention, 1.3 dtex fineness LENZING® Lyocell A100 type TAHT-crosslinked lyocell staple fiber (e.g., produced by the process described in WO95 / 28516) from Lenzing AG (Werkstrasse 2, A-4860 Lenzing) was used for calibration. The long-term average wet abrasion resistance NSF of all calibration measurements of this fiber was 471 r / dtex.

[0116] Wet abrasion resistance was determined using Lenzing Instruments' "Delta 100" device. The steel shaft was continuously moved longitudinally during measurement to prevent groove formation in the filament hose.

[0117] The source of the filament hoses (viscose filament stockings) was VOM BAUR GmbH&KG. (Markstrasse 34, D-42369 Wuppertal).

[0118] From 20 bundles of fibers, one fiber with a length of 38 mm is placed on a steel shaft with a thickness of 1 cm in each case, and a preloading weight is applied. The steel shaft, covered with a filament hose, is continuously moistened during rotation. During the measurement, the steel shaft is rotated at a speed of 500 revolutions per minute and simultaneously moved back and forth diagonally relative to the fiber axis, resulting in a pendulum motion of approximately 1 cm.

[0119] The number of rotations until the fiber abrasion and the preload weight touched the contactor was determined. After 5000 rotations, the measurement should be stopped under any circumstances to avoid erroneous measurements. The measured wet abrasion resistance NSF was obtained by dividing the average of all 20 measurements by the fineness of each fiber [r / dtex].

[0120] Test parameters: Water flow rate: 8.2 mL / min Rotation speed: 500 rpm Wear angle: 40° Preload weight: 50 mg

[0121] Fibers with a density of 200 r / dtex or higher, and especially 400 r / dtex or higher, constitute low-fibrillation (LF) fibers, or fibers resistant to fibrillation in conventional wet processes.

[0122] Coefficient of variation (CV) of wet abrasion resistance NSF decision CV of lyocell staple fibers according to the present invention NSF This is the standard deviation σ of wet abrasion resistance (NSF). NSF and expected value μ NSF This is the ratio: CV NSF =σ NSF / μ NSF . Because we can only determine wet abrasion resistance using measurements from samples with limited sample sizes, the average NSF across measurements of random samples is not used. * The expected value μ NSF It is used as an approximation. Therefore, the approximated CV * NSF is the standard deviation s NSF The average value NSF * By standardizing, the following can be obtained: CV * NSF =s NSF / NSF * . When the sample size goes from n to infinity, CV is determined from random samples. * NSFThis is the CV determined from the expected value. NSF It converges to [a certain point].

[0123] If the sample size is insufficiently small or the sample is inappropriate, for example, if the fibers are taken from only a portion of the sample, the determined CV * NSF Therefore, CV NSF There is a possibility of significant deviation from the range.

[0124] Therefore, the coefficient of variation CV of lyocell staple fibers NSF To determine a meaningful value, each NSF should be determined using a sufficiently large fiber sample from a sufficiently large sample (e.g., a fiber bale). For this purpose, it is preferable to take fiber stalks from different locations in the sample and determine the NSF of each individual fiber from the fiber stalk as described above. Thus, using at least 20 fiber stalks from different locations in the bale, the average value NSF * and coefficient of variation CV * NSF This is determined from these 20 measurements.

[0125] As a check, additional fiber samples are taken again from at least 20 different fiber bundles, independently of the previously selected fiber bundles, and examined. Then, the mean NSF value is calculated from all predetermined NSF values ​​of all samples. * and coefficient of variation CV * NSF The average NSF obtained in this way is calculated. * or coefficient of variation CV * NSF However, if the value for the first sample differs by more than 10% from the previously determined value, especially if it differs by more than 5%, the above procedure must be repeated until sufficient convergence to the determined value is obtained.

[0126] Depending on the homogeneity of the sample to be examined, a total random sample of more than 100 fibers, and in some cases more than 1000 fibers, may be required in this manner to determine the coefficient of variation.

[0127] A nitrogen analyzer for determining the nitrogen filling rate by burning a sample. The nitrogen content of the fibers is determined by measuring the N content by burning the sample (for example, using a LECO FP 328 nitrogen analyzer). From this, the amount of crosslinking agent can be determined.

[0128] Counting of minute crimps To obtain a composite sample, fibers were taken from fiber samples removed from a fiber sack at various positions. A drop of glycerin was placed on a slide, and several individual fibers from the composite sample were placed in it as straight as possible. A coverslip was placed on top of the drop of glycerin containing several individual fibers. The slide was placed under a polarizing microscope. The number of minute crimps within the area of ​​the coverslip (2 × 2 cm) was counted.

[0129] Dust test (thread) Dust formation in the spinning process is induced, for example, by brittle fibers and their poor processability. Dust formation was measured in a pilot plant. Fibers to be tested were wound. Approximately 500g of yarn was wound at a bobbin speed of 1000m / min. The amount of yarn wound was determined to the nearest 1mg. Fiber dust generated in this process was collected and weighed to the nearest 0.1mg using a chemical balance. The amount of fiber dust indicates the degree of mechanical damage inflicted on the fibers during processing at the spinning mill. A higher amount of dust [ppm] indicates that the fibers are more susceptible to damage during processing.

[0130] The following formula was used for the calculation: Dust (in ppm) = (Weighed fiber dust [g] * 1,000,000) / Amount of yarn wound [g] For example: 97.83 ppm = (0.0520 g * 1,000,000) / 531.512 g

[0131] Fineness / thickness variations and knit The yarn has various surface irregularities, such as variations in fineness, thickness, and knit. Tests for variations in fineness, thickness, and knit were carried out using the following steps. The yarn to be tested was checked using a USTER® tester. The tester uses a capacitance method to determine the variation in the weight of the fiber strands, thereby inferring surface irregularities. The average weight of the yarn was determined based on the first 100m of yarn. The subsequent 1000m of yarn was measured in 1cm increments. The deviation from the initial average was recorded. The number of deviations (-50% for variations in fineness / +50% for variations in thickness / +>100% for knit) was counted. Knit is a variation in thickness shorter than 1cm and exhibits a deviation of yarn weight from the average weight of the yarn >100%. The USTER® Tester usually indicates how many knits occurred at deviations of >140% or >200% (see Table 3).

Claims

1. Steps in the following order: a) extruding filaments from a solution of cellulose in an organic solvent; b) precipitating cellulose to form continuous cellulose filaments; c) washing the cellulose filaments; d) contacting the cellulose filaments with a cross-linking agent; e) reacting the cellulose filaments with a cross-linking agent in a reaction chamber; f) washing the treated cellulose filaments; g) cutting the washed cellulose filaments into staple fibers; h) forming a nonwoven fleece from the staple fibers and pressing the nonwoven fleece; i) applying a finishing touch to the nonwoven fleece and pressing the nonwoven fleece; 1. A method for producing lyocell staple fiber, comprising:

2. 2. The method according to claim 1, characterized in that the filaments or staple fibers are dried only after step i).

3. 3. The method according to claim 1 or 2, characterized in that the reaction in step e) is carried out with an energy input.

4. 4. The process according to claim 3, characterized in that the reaction in step e) is carried out in the presence of steam.

5. 5. The method of claim 4, wherein step e) is carried out in a steam chamber.

6. 6. The method according to claim 1, wherein the duration of step e) is from 3 to 30 minutes, preferably from 10 to 25 minutes, particularly preferably from 15 to 20 minutes.

7. The crosslinking agent is used in an amount such that there is a content G (in moles) of crosslinking agent per kg of cellulose (atro), said content G being in accordance with the following formula: G×R=0.10 to 0.45, preferably 0.10 to 0.35, particularly preferably 0.20 to 0.35 where R represents the number of reactive groups in the crosslinker.

7. The method according to claim 1, wherein the first and second electrodes are connected to a first electrode.

8. Compounds of formula (I) 【Chemistry 1】 where X represents a halogen, R=H or an ionic moiety, and n=0 or 1.

8. The method according to claim 1, wherein the crosslinking agent is a salt of this compound, preferably the sodium salt of 2,4-dichloro-6-hydroxy-1,3.5-triazine.

9. 9. The process according to claim 8, characterized in that the crosslinking agent of the compound of formula (I) is used in an amount of 30 to 80 g, preferably 45 to 60 g, per kg of cellulose (atro).

10. The fiber has residual crimp and the coefficient of variation of wet abrasion resistance (CV NSF 10. Lyocell staple fibre obtainable by the process according to claim 8 or 9, characterized in that the % of saturation is 50% or less, in particular 45% or less.

11. The following characteristics: the fibers have a fineness ranging from 1.2 dtex to 1.5 dtex, preferably from 1.25 dtex to 1.45 dtex; - the fibers have residual crimp; the fibers have a fiber strength in the normal weight state of at least 36 cN / tex, preferably in the range of 38 cN / tex to 42 cN / tex; the fibers have a Hoeller coefficient F1 ≥ 2.1, preferably ≥ 2.4, particularly preferably in the range from 2.5 to 3.2; the fibers have a Hoeller coefficient F2 ≥ 3.0, preferably ≥ 3.5, particularly preferably in the range from 4.0 to 5.5; 10. Lyocell staple fiber obtainable by the method according to claim 8 or 9, characterized by the combination of:

12. The following characteristics: the fibers have a fineness in the range from 0.6 dtex to 1.2 dtex, preferably from 0.7 dtex to 1.15 dtex, particularly preferably from 0.8 dtex to 1.1 dtex; - the fibers have residual crimp; the fibers have a fiber strength in the nominal weight state of at least 40 cN / tex, preferably in the range from 42 cN / tex to 49 cN / tex, particularly preferably from 43.5 cN / tex to 46 cN / tex; the fibers have a Hoeller coefficient F1 ≥ 2.8, preferably ≥ 3.0, particularly preferably in the range from 3.2 to 3.5; the fibers have a Hoeller coefficient F2 ≥ 3.0, preferably ≥ 3.6, particularly preferably in the range from 3.9 to 5.5; 10. Lyocell staple fiber obtainable by the method according to claim 8 or 9, characterized by the combination of:

13. 13. Lyocell staple fiber according to claim 11 or 12, characterized in that the fiber has a coefficient of variation of wet abrasion resistance (NSF CV) of not more than 50%, in particular not more than 45%.

14. Lyocell staple fiber according to any of claims 10 to 13, characterized by a fiber elongation in the positive weight state of 10% or more, preferably between 10% and 11%.

15. 15. Lyocell staple fiber according to any one of claims 10 to 14, characterized by a wet abrasion resistance (NSF) of 300 r / dtex (revolutions / dtex) or more, preferably 400 r / dtex or more, particularly preferably 450 r / dtex or more.

16. The following formula: G×R=0.10 to 0.45, preferably 0.10 to 0.35, particularly preferably 0.20 to 0.35 where R represents the number of reactive groups in the crosslinker.

16. Lyocell staple fiber according to any one of claims 10 to 15, characterized in that it has a content G (in moles) of crosslinking agent per kg of cellulose (atro) according to:

17. 17. Lyocell staple fiber according to claim 16, characterized in that the content of crosslinking agent of compound of formula (I) is 1.8 to 4.5% by weight, preferably 1.9 to 3.7% by weight, particularly preferably 2.0 to 3.0% by weight, based on cellulose (atro).

18. A fiber bundle containing at least 20 kg of lyocell staple fiber according to any one of claims 10 to 17.

19. A textile article comprising the lyocell staple fiber according to any one of claims 10 to 17.

20. 20. The textile article of claim 19 in the form of a yarn.