Hydraulic composition for centrifugal molding
Patent Information
- Application Number
- JP2021188287
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-19
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-11-19
AI Technical Summary
Existing hydraulic compositions for centrifugal molding face challenges in maintaining moldability over a wide range of compounding conditions, leading to the discharge of cement sludge, which is environmentally harmful and labor-intensive to treat, particularly when using polycarboxylic acid-based dispersants.
A hydraulic composition containing specific monomers and copolymers, including fumaric acid, maleic acid, and polyamidepolyamines, which adsorb to cement sludge components, preventing their discharge by maintaining them within the molded product.
The composition effectively suppresses sludge formation, reducing environmental burden and labor requirements, while ensuring excellent moldability and strength of the centrifugally molded products.
Smart Images

Figure 2023075404000001 
Figure 2023075404000002 
Figure 2023075404000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a hydraulic composition for centrifugal molding and a method for producing a hardened body of the hydraulic composition. [Background technology]
[0002] Centrifugal molding is a known method for manufacturing hollow cylindrical concrete molded products such as pipes, piles, and poles. In this centrifugal molding method, mixed concrete material is poured into a mold, and the mold is rotated at high speed. The resulting centrifugal force presses the concrete against the inner surface of the mold, thereby compacting it.
[0003] In hydraulic compositions for centrifugal molding, naphthalene-based dispersants are often used as dispersants from the viewpoint of moldability of centrifugal molded products. However, both domestically and internationally, there is a growing need for higher strength and earthquake resistance. As disclosed in Non-Patent Document 1, in areas where high-strength hardened bodies are required, that is, in areas where the unit water content of concrete is small, mixing with naphthalene-based dispersants becomes difficult, making practical use challenging. For this reason, the use of polycarboxylic acid-based dispersants with high water-reducing properties is progressing. However, a problem that arises when using polycarboxylic acid-based dispersants is the sludge, which is cement sludge discharged as a result of centrifugal molding.
[0004] Sludge, being highly alkaline and containing heavy metal ions, has a significant environmental impact and requires considerable expense and effort to treat. In particular, when using polycarboxylic acid-based dispersants, maintaining the moldability of centrifugal molded products without discharging sludge requires keeping the unit water content of the hydraulic composition within a specific range. This narrow control range, coupled with fluctuations in the required amount of dispersant due to variations in surface water content, temperature, and humidity, makes control difficult, hindering the production of centrifugal molded products with good moldability. Therefore, there is a need for a hydraulic composition for centrifugal molding that exhibits excellent moldability over a wide range of formulation conditions, including water content and dispersant addition amount.
[0005] Patent Document 1 describes a hydraulic composition for centrifugal molding, comprising (A) a dispersant for hydraulic powders consisting of a polymer compound containing an aromatic ring, and (B) one or more compounds selected from specific compounds represented by general formulas (B1) to (B4), hydraulic powder, aggregate, and water, wherein the water / hydraulic powder ratio is greater than 25% by mass and 35% by mass or less.
[0006] Patent Document 2 describes a strength-improving additive for centrifugal-formed concrete, characterized in that it comprises (a) a copolymer consisting of 50 to 98% by mass of monomer (a) represented by formula (1), 1 to 49% by mass of monomer (b) represented by a specific formula, and 0.1 to 5% by mass of monomer (c) represented by a specific formula, and (b) a copolymer of a polyoxyalkylene derivative and an unsaturated carboxylic acid compound, wherein the ratio of (a):(b) = 50 to 80:20 to 50 by mass {with the total mass of (a) and (b) being 100}.
[0007] Patent Document 3 describes a concrete composition for centrifugal molding containing cement, a high-strength material, and a water-soluble copolymer as an admixture, wherein the water-soluble copolymer is a water-soluble copolymer obtained by polymerizing a monomer mixture containing one or more vinyl monomers (a) having a polyoxyalkylene chain with an average of 2 to 100 moles of alkylene oxide having 2 to 3 carbon atoms, and one or more vinyl monomers (b) having a carboxyl group, a sulfonic acid group, or an amide group, or a water-soluble salt thereof. [Prior art documents] [Patent Documents]
[0008] [Patent Document 1] Japanese Patent Publication No. 2018-48068 [Patent Document 2] Japanese Patent Publication No. 2010-235384 [Patent Document 3] Japanese Patent Publication No. 2001-253750 [Non-patent literature]
[0009] [Non-Patent Document 1] Transactions of the Architectural Institute of Japan, Structural Division, No. 606, pp. 29-34, Architectural Institute of Japan, a general incorporated foundation, issued in August 2006
Summary of the Invention
Problems to be Solved by the Invention
[0010] The present invention provides a hydraulic composition for centrifugal molding having excellent sludge suppressing ability and a method for producing a hardened body of the hydraulic composition.
Means for Solving the Problems
[0011] The present invention relates to a hydraulic composition for centrifugal molding, which contains the following component (A), cement, aggregate, and water, and in which the water / cement ratio is 20% by mass or more and 35% by mass or less. Component (A): A copolymer containing at least one monomer (A1) selected from fumaric acid, (anhydrous) maleic acid, and salts thereof, a monomer (A2) represented by the following general formula (A2), and a monomer (A3) represented by the following general formula (A3) as constituent monomers, wherein in the constituent monomers of the copolymer, the proportion of monomer (A1) is 1% by mass or more and 30% by mass or less, the proportion of monomer (A2) is 1% by mass or more and 20% by mass or less, and the proportion of monomer (A3) is 50% by mass or more and 90% by mass or less.
[0012] [Chemical Formula]
[0013] [In General Formula (A2), R 21a , R 22a , R 23a[These may be the same or different groups, and are a hydrogen atom, a methyl group, or COOM; M is a hydrogen atom, an alkali metal, an alkaline earth metal (1 / 2 atom), an ammonium group, an alkylammonium group, or a substituted alkylammonium group; and Z is a group that bonds to the carbon atoms of the main chain via an amide bond in a polyamide polyamine obtained by condensing a dibasic acid with a polyalkylene polyamine, and / or a modified polyamide polyamine obtained by adding 0.1 moles to 10 moles of an alkylene oxide having 2 to 4 carbon atoms per equivalent of the active imino group, amino group, or amide residue of the polyamide polyamine.]
[0014] [ka]
[0015] [In general formula (A3), R 31a , R 32a R may be the same or different, and is a hydrogen atom or a methyl group. 33a is a hydrogen atom or -COO(AO) n X is an alkyl group or hydrogen atom having 1 to 4 carbon atoms, AO is a group selected from ethyleneoxy and propyleneoxy groups, n is the average number of moles of AO added, a number between 5 and 150, p is a number between 0 and 2, and q is a number of 0 or 1.
[0016] The present invention also relates to a method for producing a hardened hydraulic composition, comprising the following steps. Step 1: A step of mixing the above-mentioned component (A), cement, aggregate, and water in a water / cement ratio of 20% by mass or more and 35% by mass or less to obtain a hydraulic composition, and filling a mold with the obtained hydraulic composition. Step 2: A step in which the hydraulic composition filled into the mold obtained in Step 1 is clamped by applying centrifugal force. Step 3: A step to solidify the molded hydraulic composition obtained in Step 2 within the mold. [Effects of the Invention]
[0017] The present invention provides a hydraulic composition for centrifugal molding having excellent sludge suppression ability, and a method for producing a hardened body of the hydraulic composition.
[0018] In recent years, the Sustainable Development Goals (SDGs) have been proposed to realize a sustainable society. This invention can reduce environmental impact by suppressing sludge emissions and streamline manufacturing processes, and is considered to be a technology that can contribute to SDGs No. 7, 8, 9, 11, 12, and 14, for example. [Modes for carrying out the invention]
[0019] The inventors of the present invention have found that the centrifugal moldable hydraulic composition of the present invention does not easily discharge sludge. The reason for this effect is not entirely clear, but it is presumed to be as follows. In the manufacture of molded bodies of centrifugal moldable hydraulic compositions, the cement sludge in the hydraulic composition, being of low density, accumulates in the center of the molded body due to centrifugal force, causing sludge. It is presumed that the cement sludge mainly consists of relatively low-density components among the hydration products generated by the hydration reaction of cement, particularly calcium silicate. In the centrifugal moldable hydraulic composition of the present invention, since the monomer (A2) in the constituent monomer of component (A) has an amino group, it is thought that component (A) is adsorbed onto the calcium silicate in the cement sludge, starting from the amino group of monomer (A2). On the other hand, component (A) of the present invention exhibits excellent cement particle dispersion ability due to monomer (A3) in the constituent monomers of component (A), as monomer (A1) has strong adsorption properties to calcium catiosite on the surface of cement. Therefore, component (A) can also be adsorbed on the cement surface, and it is thought that component (A) keeps the calcium silicate in the cement sludge near the cement particles, suppressing its outflow as sludge.
[0020] [Hydraulic composition for centrifugal molding] The present invention relates to a hydraulic composition for centrifugal molding, which contains a component (A), cement, aggregate, and water, and has a water / cement ratio of 20% by mass or more and 35% by mass or less.
[0021] <Component (A)> Component (A) is a copolymer containing at least one monomer (A1) selected from fumaric acid, (anhydrous) maleic acid, and salts thereof, a monomer (A2) represented by the following general formula (A2), and a monomer (A3) represented by the following general formula (A3) as constituent monomers. In the constituent monomers of the copolymer, the proportion of monomer (A1) is 1% by mass or more and 30% by mass or less, the proportion of monomer (A2) is 1% by mass or more and 20% by mass or less, and the proportion of monomer (A3) is 50% by mass or more and 90% by mass or less.
[0022] [Chemical formula]
[0023] [In general formula (A2), R 21a , R 22a , R 23a may be the same or different, and each is a hydrogen atom, a methyl group, or COOM, where M is a hydrogen atom, an alkali metal, an alkaline earth metal (1 / 2 atom), an ammonium group, an alkylammonium group, or a substituted alkylammonium group. Z is a group in which a polyamide polyamine obtained by condensing a dibasic acid and a polyalkylene polyamine and / or a modified polyamide polyamine obtained by adding 0.1 mol or more and 10 mol or less of an alkylene oxide having 2 to 4 carbon atoms per equivalent of an active imino group, an amino group, or an amide residue of the polyamide polyamine is bonded to a carbon atom of the main chain through an amide bond.]
[0024] [Chemical formula]
[0025] [In general formula (A3), R 31a , R 32a may be the same or different, and each is a hydrogen atom or a methyl group, and R33a is a hydrogen atom or -COO(AO) n X is an alkyl group or hydrogen atom having 1 to 4 carbon atoms, AO is a group selected from ethyleneoxy and propyleneoxy groups, n is the average number of moles of AO added, a number between 5 and 150, p is a number between 0 and 2, and q is a number of 0 or 1.
[0026] Monomer (A1) is one or more monomers selected from fumaric acid, (anhydride) maleic acid, and salts thereof, and from the viewpoint of copolymerizability, fumaric acid or a salt thereof is preferred. Examples of salts include alkali metal salts, alkaline earth metal salts, ammonium salts, alkylammonium salts, and substituted alkylammonium salts. (Anhydride) maleic acid means that it is maleic acid and / or maleic anhydride.
[0027] In monomer (A2), in general formula (A2), R 21a From the viewpoint of reactivity, it is preferably a hydrogen atom or a COOM, more preferably a COOM. In general formula (A2), R 22a From the viewpoint of copolymerizability, it is preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom. In general formula (A2), R 23a From the viewpoint of copolymerizability, it is preferably a hydrogen atom or COOM, more preferably COOM.
[0028] In general formula (A2), the dibasic acid constituting Z is an aliphatic saturated dibasic acid having 2 or more carbon atoms, preferably 4 or more, and 10 or less, preferably 8 or less, from the viewpoint of copolymerizability. Examples of dibasic acids include one or more selected from oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid, and from the viewpoint of copolymerizability, one or more selected from adipic acid, glutaric acid, and succinic acid are preferred. Furthermore, as the polyalkylene polyamine constituting Z, one or more can be selected from ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, hexaethyleneheptamine, and a mixture of high-molecular-weight polyethylene polyamines which are mixtures containing a large amount of ethylene units and nitrogen atoms. From the viewpoint of copolymerizability, it is preferable to select one or more from diethylenetriamine, triethylenetetramine, and a mixture of high-molecular-weight polyethylene polyamines which are mixtures containing a large amount of ethylene units and nitrogen atoms.
[0029] Monomer (A2) is a monomer formed by a polyamide polyamine, which is a condensate of these dibasic acids and polyalkylene polyamines, and / or a modified polyamide polyamine obtained by adding 0.1 moles or more, preferably 1 mole or more, and 10 moles or less, preferably 5 moles or less, of alkylene oxide having 2 to 4 carbon atoms, preferably ethylene oxide, to 1 equivalent of the active imino group, amino group, or amide residue of the polyamide polyamine, from the viewpoint of copolymerizability, and then bonding to one or more selected from maleic anhydride, maleic acid, fumaric acid, acrylic acid, methacrylic acid, and salts thereof via an amide bond.
[0030] In monomer (A3), in general formula (A3), R 31a From the viewpoint of copolymerization, hydrogen atoms are preferred. In general formula (A3), R 32a From the viewpoint of copolymerizability, a methyl group is preferred. In general formula (A3), R 33a From the viewpoint of copolymerization, hydrogen atoms are preferred. In general formula (A3), X is preferably a methyl group or a hydrogen atom from the viewpoint of copolymerizability. In general formula (A3), AO is preferably an alkylene oxy group having 2 to 3 carbon atoms from the viewpoint of cement dispersibility. AO preferably contains an ethylene oxy group.
[0031] In general formula (A3), n is the average number of moles of AO added, and is a number between 5 and 150. From the viewpoint of cement dispersibility, n is preferably 10 or more, more preferably 20 or more, even more preferably 30 or more, and even more preferably 40 or more. From the viewpoint of workability, n is preferably 120 or less, more preferably 90 or less, and even more preferably 60 or less.
[0032] In general formula (A3), p is preferably 1 or 2 from the viewpoint of copolymerization. In general formula (A3), q is preferably 0 from the viewpoint of copolymerizability.
[0033] The copolymer of component (A) may contain monomers other than monomer (A1), monomer (A2), and monomer (A3) (hereinafter also referred to as monomer (A4)) as constituent monomers. Examples of monomer (A4) include (meth)acrylic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-(methacryloyloxy)ethyl phosphate (HEMA-P), allyl sulfonic acid, methallyl sulfonic acid, and salts thereof, such as alkali metal salts, alkaline earth metal salts, ammonium salts, or amine salts. Furthermore, constituent units using monomers such as (meth)acrylamide, N-methyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-(meth)acrylamide-2-methasulfonic acid, 2-(meth)acrylamide-2-ethanesulfonic acid, 2-(meth)acrylamide-2-propanesulfonic acid, styrene, and styrenesulfonic acid can be used. (Meth)acrylic means acrylic or methacrylic.
[0034] (A) In the constituent monomers of the copolymer, the proportion of monomer (A1) is 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and 30% by mass or less, preferably 25% by mass or less, and more preferably 20% by mass or less, from the viewpoint of cement dispersibility. In the copolymer of component (A), the proportion of monomer (A2) is 1% by mass or more, preferably 1.5% by mass or more, more preferably 2.0% by mass or more, from the viewpoint of sludge suppression, and 20% by mass or less, preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, from the viewpoint of cement dispersibility. (A) In the constituent monomers of the copolymer, the proportion of monomer (A3) is 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 75% by mass or more, and 90% by mass or less, preferably 87% by mass or less, and more preferably 84% by mass or less, from the viewpoint of cement dispersibility.
[0035] The copolymer of component (A) has a total proportion of monomer (A1), monomer (A2), and monomer (A3) of the total constituent monomers that is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and preferably 100% by mass or less, and may be 100% by mass, from the viewpoint of sludge suppression.
[0036] The weight-average molecular weight of copolymer (A) is preferably 10,000 or more, more preferably 15,000 or more, even more preferably 20,000 or more, and preferably 70,000 or less, more preferably 60,000 or less, even more preferably 50,000 or less, even more preferably 40,000 or less, and even more preferably 30,000 or less, from the viewpoint of cement dispersibility. This weight-average molecular weight was measured by gel permeation chromatography (GPC) under the following conditions. *GPC conditions Equipment: GPC (HLC-8320GPC), manufactured by Tosoh Corporation. Columns: G4000PWXL + G2500PWXL (manufactured by Tosoh Corporation) Eluent: 0.2M phosphate buffer / CH3CN=9 / 1 Flow rate: 1.0mL / min Column temperature: 40℃ Detection: RI Sample size: 0.2 mg / mL Standard substances: Polyethylene glycol equivalent (monodisperse polyethylene glycol: molecular weights 87,500, 250,000, 145,000, 46,000, 24,000)
[0037] <Cement> The hydraulic composition for centrifugal molding of the present invention contains cement. Examples of cement include ordinary Portland cement, beelite cement, moderate-heat cement, rapid-hardening cement, ultra-rapid-hardening cement, sulfate-resistant cement, alumina cement, and CSA cement, with ordinary Portland cement, moderate-heat cement, rapid-hardening cement, and ultra-rapid-hardening cement being preferred. In addition, these cements may be blast furnace slag cement, fly ash cement, silica fume cement, etc., to which powders having possolane action and / or latent hydraulic properties, such as blast furnace slag, fly ash, and silica fume, or stone powder (calcium carbonate powder), etc., which will be described later, have been added.
[0038] <High strength admixture> The hydraulic composition for centrifugal molding of the present invention may contain a high-strength admixture. Examples of high-strength admixtures include powders having pozzolanic action and / or latent hydraulic properties, such as blast furnace slag, fly ash, anhydrous gypsum, and silica fume, as well as stone powder (calcium carbonate powder). Here, if the cement or high-strength admixture contains powders selected from powders having pozzolanic action, powders having latent hydraulic properties, and stone powder (calcium carbonate powder), in the present invention, the amounts of these powders are also such that they harden through a hydration reaction, such as with cement. High-strength admixtures can be used that, from the viewpoint of strength development, have a median diameter (D50; μm) of 1 μm or more, more preferably 5 μm or more, and more preferably 50 μm or less, and more preferably 40 μm or less, measured using a laser diffraction / scattering particle size distribution analyzer (e.g., LA-920 (manufactured by Horiba, Ltd.)) with ethanol as the dispersion medium.
[0039] <Aggregates> The hydraulic composition for centrifugal molding of the present invention contains aggregate. The aggregate can be selected from fine aggregate and coarse aggregate. Examples of fine aggregate include those specified in JIS A0203-2014, number 2311. Examples of fine aggregate include river sand, land sand, mountain sand, sea sand, lime sand, silica sand and their crushed forms, blast furnace slag fine aggregate, ferronickel slag fine aggregate, lightweight fine aggregate (artificial and natural), and recycled fine aggregate. Examples of coarse aggregate include those specified in JIS A0203-2014, number 2312. For example, examples of coarse aggregate include river gravel, land gravel, mountain gravel, sea gravel, lime gravel, their crushed forms, blast furnace slag coarse aggregate, ferronickel slag coarse aggregate, lightweight coarse aggregate (artificial and natural), and recycled coarse aggregate. Different types of fine aggregate and coarse aggregate may be mixed, or a single type may be used.
[0040] <Composition of hydraulic composition, etc.> In the hydraulic composition for centrifugal molding of the present invention, the content of component (A) is such that, from the viewpoint of the fluidity of the hydraulic composition and sludge suppression, 1 m of the hydraulic composition for centrifugal molding 3 Preferably, it is 0.4 kg or more, more preferably 0.8 kg or more, even more preferably 1.2 kg or more, and preferably 1.5 kg or less, more preferably 1.4 kg or less, and even more preferably 1.3 kg or less.
[0041] In the hydraulic composition for centrifugal molding of the present invention, the water / cement ratio (hereinafter sometimes referred to as W / B) is 20% by mass or more, preferably 21% by mass or more, from the viewpoint of fluidity of the hydraulic composition, and 35% by mass or less, preferably 30% by mass or less, more preferably 27% by mass or less, and even more preferably 25% by mass or less, from the viewpoint of strength development of the hydraulic composition. In the hydraulic composition for centrifugal molding of the present invention, the water / hydraulic powder ratio (hereinafter sometimes referred to as W / C) is 20% by mass or more, preferably 21% by mass or more, from the viewpoint of fluidity of the hydraulic composition, and 35% by mass or less, preferably 30% by mass or less, more preferably 27% by mass or less, and even more preferably 25% by mass or less, from the viewpoint of strength development of the hydraulic composition. Here, the water / cement ratio is the mass percentage (mass%) of water and cement in the hydraulic composition, and is calculated as water / cement × 100. The water / hydraulic powder ratio is the mass percentage (mass%) of water and hydraulic powder in the hydraulic composition, and is calculated as water / hydraulic powder × 100. The water / hydraulic powder ratio is calculated based on the amount of powder that has properties that harden through a hydration reaction. If the powder that hardens through a hydration reaction contains high-strength admixtures in addition to cement, these amounts are also included in the amount of hydraulic powder. The same applies to other quantitative relationships of the hydraulic composition with respect to hydraulic powder.
[0042] In the centrifugal molding hydraulic composition of the present invention, the cement content is such that, from the viewpoint of strength development of the hydraulic composition, 1 m of centrifugal molding hydraulic composition 3 Preferably, it is 400 kg or more, more preferably 450 kg or more, even more preferably 500 kg or more, and preferably 700 kg or less, more preferably 650 kg or less, and even more preferably 600 kg or less.
[0043] In the hydraulic composition for centrifugal molding of the present invention, the content of the high-strength admixture is such that, from the viewpoint of strength development of the hydraulic composition, 1 m of the hydraulic composition for centrifugal molding 3 Preferably, the weight is 50 kg or less, more preferably 30 kg or less, and even more preferably 10 kg or less. The hydraulic composition for centrifugal molding of the present invention does not need to contain a high-strength admixture.
[0044] When the hydraulic composition for centrifugal molding is concrete, the amount of coarse aggregate used is preferably 50% or more, more preferably 55% or more, even more preferably 60% or more, and preferably 100% or less, more preferably 90% or less, and even more preferably 80% or less, from the viewpoint of developing the strength of the hydraulic composition, reducing the amount of hydraulic powder such as cement used, and improving the ability to fill into formwork, etc. The bulk volume is 1 m³ of concrete. 3 This is the ratio of the volume of coarse aggregate (including voids) inside. Furthermore, when the hydraulic composition for centrifugal molding is concrete, the amount of fine aggregate used is preferably 500 kg / m³ from the viewpoint of improving the ability to fill into formwork, etc.3 Above, a comfortable 600 kg / m 3 More preferably 650 kg / m 3 The above is true, and preferably 1000 kg / m 3 More preferably 900 kg / m 3 The following applies: When the hydraulic composition for centrifugal molding is mortar, the amount of fine aggregate used is preferably 800 kg / m³. 3 In summary, a comfortable 900 kg / m 3 More preferably 1000 kg / m 3 The above is true, and preferably 2000 kg / m 3 More preferably, 1800 kg / m 3 More preferably, 1700 kg / m 3 The following applies:
[0045] Examples of hydraulic compositions for centrifugal molding include concrete, with cement-based concrete being particularly preferred. The hydraulic composition of the present invention is useful in any of the following fields: self-leveling, refractories, plaster, lightweight or heavy concrete, AE, repair, pre-packed, tremie, ground improvement, grouting, and cold-weather applications.
[0046] The hydraulic composition for centrifugal molding of the present invention may contain conventional cement dispersants, water-soluble polymer compounds, air entrainers, cement wetting agents, expansive agents, waterproofing agents, retarders, quick-setting agents, foaming agents, foaming agents, waterproofing agents, fluidizing agents, thickeners, flocculants, drying shrinkage reducing agents, strength enhancers, hardening accelerators, preservatives, defoaming agents, rust inhibitors, etc. (except those corresponding to component (A)).
[0047] [Method for producing hydraulic compositions] The present invention provides a method for producing a hydraulic composition for centrifugal molding, comprising mixing component (A), cement, aggregate, and water in a water / cement ratio of 20% by mass or more and 35% by mass or less. This method produces the hydraulic composition for centrifugal molding of the present invention, which contains component (A), cement, aggregate, and water. Furthermore, the method for producing the hydraulic composition for centrifugal molding of the present invention may include the addition of a high-strength admixture.
[0048] Specific examples and preferred embodiments of component (A), cement, high-strength admixture, and aggregate used in the method for producing the hydraulic composition for centrifugal molding of the present invention are the same as those described in the hydraulic composition for centrifugal molding of the present invention. The cement and high-strength admixtures are used such that the W / B and W / C ratios are within the ranges specified in the hydraulic composition for centrifugal molding of the present invention. The amount of aggregate used is also the same as that specified in the hydraulic composition for centrifugal molding of the present invention. In the method for producing the hydraulic composition for centrifugal molding of the present invention, the content of each component described in the hydraulic composition for centrifugal molding of the present invention can be appropriately applied by replacing the content of each component with the amount of mixture. The matters described in the present invention concerning the hydraulic composition for centrifugal molding can be appropriately applied to the method for producing the hydraulic composition for centrifugal molding of the present invention.
[0049] In the method for producing the hydraulic composition of the present invention, from the viewpoint of productivity, it is preferable to pre-mix component (A) with water and then mix it with cement.
[0050] (A) The mixing of component (A), cement, optionally high-strength admixture, aggregate, water, and any other components used as needed can be carried out using a mixer such as a mortar mixer or a forced twin-shaft mixer. Furthermore, the mixture is preferably mixed for 1 minute or more, more preferably for 2 minutes or more, and preferably for 5 minutes or less, more preferably for 3 minutes or less. When preparing the hydraulic composition, the materials and agents and their amounts described in the section on hydraulic compositions can be used.
[0051] The obtained hydraulic composition is further filled into a mold, centrifuged, and then cured to harden. Examples of molds include those for buildings and concrete products. Methods for filling the mold include directly pouring the composition from a mixer and introducing the hydraulic composition into the mold by pumping it.
[0052] During the curing of a hydraulic composition, heat curing may be performed to accelerate hardening. Here, heat curing can accelerate hardening by holding the hydraulic composition at a temperature of 40°C to 90°C.
[0053] [Method for manufacturing a hardened body of a hydraulic composition] The present invention provides a method for producing a hardened body of a hydraulic composition, comprising the following steps. Step 1: A step in which component (A), cement, aggregate, and water are mixed in a water / cement ratio of 20% by mass or more and 35% by mass or less to obtain a hydraulic composition, and the obtained hydraulic composition is filled into a mold. Step 2: A step in which the hydraulic composition filled into the mold obtained in Step 1 is clamped by applying centrifugal force. Step 3: A step to solidify the molded hydraulic composition obtained in Step 2 within the mold.
[0054] In the preparation of the hydraulic composition in step 1, a high-strength admixture may be added. Specific examples and preferred embodiments of component (A), cement, high-strength admixture, and aggregate used in the method for producing a hardened body of the hydraulic composition of the present invention are the same as those described for the hydraulic composition for centrifugal molding of the present invention. The cement and high-strength admixtures are used such that the W / B and W / C ratios are within the ranges specified in the hydraulic composition for centrifugal molding of the present invention. The amount of aggregate used is also the same as that specified in the hydraulic composition for centrifugal molding of the present invention. Furthermore, in step 1 of the method for producing a hardened body of the hydraulic composition of the present invention, the content of each component described in the hydraulic composition for centrifugal molding of the present invention can be appropriately applied by replacing the content of each component with the amount of mixture. The matters described in the present invention regarding the hydraulic composition for centrifugal molding and the method for producing the hydraulic composition for centrifugal molding can be appropriately applied to the method for producing a cured body of the hydraulic composition of the present invention.
[0055] The method for producing the cured product of the present invention preferably includes the following step 4 in addition to steps 1 to 3. Step 4: A step in which the hydraulic composition that has solidified in Step 3 is steam-cured in a mold.
[0056] The method for producing a cured product of the present invention may include the following step 5 in addition to steps 1 to 4. Step 5: After Step 4, the hydraulic composition is cooled and removed from the mold.
[0057] The method for producing a cured product of the present invention may include the following step 6 in addition to steps 1 to 5. Step 6: A step of curing the hardened body of the hydraulic composition obtained in Step 5 at room temperature and pressure.
[0058] In step 1, a method of adding a mixture containing water and component (A) to a mixture containing aggregate and cement and mixing them is preferred because it allows for easy and uniform mixing even when producing a hydraulic composition.
[0059] A specific method for step 1 is to mix cement with an optional high-strength admixture and aggregate, add a mixture containing water and component (A) in the aforementioned mixing amounts, and knead to prepare a hydraulic composition.
[0060] One method for filling the mold with the hydraulic composition obtained in step 1 is to discharge the mixed hydraulic composition from the mixing means and manually pour it into the mold and level it.
[0061] In step 2, the hydraulic composition filled into the mold is clamped by centrifugal force, and it is preferable to change the centrifugal force at least once. In step 2, the hydraulic composition can be clamped by applying a centrifugal force that changes in stages. That is, in step 2, the hydraulic composition can be clamped by changing the centrifugal force at least once, and furthermore, by applying a centrifugal force that changes in stages and increases in stages.
[0062] In step 2, it is preferable to clamp the hydraulic composition filled into the mold with a centrifugal force of 0.5G or more. The centrifugal force for centrifugal molding is preferably 0.5G or more, preferably 30G or less, and more preferably 25G or less. From the viewpoint of reducing energy costs and moldability, it is preferable to maintain the centrifugal force in the range of 15G or more, 30G or less, and even more preferably 25G or less (also called high centrifugal force) for 1 minute or more.
[0063] Centrifugal compaction is performed with a centrifugal force of, for example, 0.5G to 30G, preferably for 5 minutes or more, more preferably 7 minutes or more, even more preferably 9 minutes or more, and preferably 40 minutes or less. From the viewpoint of compacting the molded body smoothly, compaction by maintaining a high centrifugal force, for example, 20G or more, is preferably performed for 1 minute or more, more preferably 3 minutes or more, even more preferably 5 minutes or more, and preferably 15 minutes or less. That is, in step 3, the hydraulic composition can be molded with a centrifugal force of 0.5G to 30G, preferably for 5 minutes or more, more preferably 7 minutes or more, even more preferably 9 minutes or more, and preferably 40 minutes or less. Also in step 3, compaction by maintaining a centrifugal force of 20G or more can be performed preferably for 1 minute or more, more preferably 3 minutes or more, even more preferably 5 minutes or more, and preferably 15 minutes or less.
[0064] Centrifugal compaction can be carried out in stages, and from the viewpoint of moldability, it is preferable to gradually increase the centrifugal force G. The process can be carried out under the stage conditions shown below until the desired centrifugal force is reached. For example, in the case of five stages, in step 3, it is preferable to compact the hydraulic composition under the following conditions: (1) the initial velocity, which is the first stage, is a centrifugal force of 0.5G or more and less than 2G for more than 0 minutes and 15 minutes or less; (2) the second velocity, which is the second stage, is a centrifugal force of 2G or more and less than 5G for more than 0 minutes and 15 minutes or less; (3) the third velocity, which is the third stage, is a centrifugal force of 5G or more and less than 10G for more than 0 minutes and 15 minutes or less; (4) the fourth velocity, which is the fourth stage, is a centrifugal force of 10G or more and less than 20G for more than 0 minutes and 15 minutes or less; (5) the fifth velocity, which is the fifth stage, is a centrifugal force of 20G or more and 30G or less for more than 0 minutes and 15 minutes or less.
[0065] In step 3, the hydraulic composition obtained in step 2 is allowed to set. Specifically, it is cured in the air for 3 to 4 hours after mixing.
[0066] In step 4, the hardened hydraulic composition in the mold obtained in step 3 is steam-cured. In step 4, steam curing is preferably carried out at a temperature of 40°C to 90°C, and more preferably at a temperature of 60°C to 90°C. Furthermore, in step 4, it is preferable to perform steam curing after pre-curing. For example, after performing pre-curing by setting the ambient temperature of the mold filled with the hydraulic composition (hereinafter sometimes referred to as ambient temperature) to room temperature, preferably 10°C to 40°C, and leaving it for 1 to 4 hours, steam curing can be performed by setting the ambient temperature to 40°C to 90°C, and then to 60°C to 90°C. Pre-curing was performed as a "preliminary step" in the examples and comparative examples described later. Pre-curing should preferably be at least one hour to minimize strength reduction due to cracking of the hardened material. Furthermore, if the method for manufacturing the cured body of the present invention includes step 5, steps 4 and 5 can be carried out continuously under a series of temperature controls. Steam curing is performed by applying steam around a mold filled with a hydraulic composition and maintaining it at a predetermined temperature for a certain period of time. After applying steam, the steam curing period may include (1) the period of temperature rise until the predetermined temperature is reached, (2) the period of maintaining it at the predetermined temperature for a certain period of time, and (3) the period of temperature decrease after maintaining it at the predetermined temperature for a certain period of time.
[0067] As specific steam curing conditions in the method for manufacturing a cured body of the present invention, in step 4, the ambient temperature around the mold is raised to 60°C to 85°C at a heating rate of 10°C to 30°C per hour, and the raised temperature is maintained for 2 hours to 8 hours. Then, in step 5, the ambient temperature is cooled to room temperature, for example, 20°C, at a cooling rate of 5°C to 20°C per hour, and the molded body is demolded. From the viewpoint of suppressing the reduction in strength due to cracking of the hardened material, the heating rate is preferably 20°C or less per hour. One example of preferred conditions is a method in which a mold filled with a hydraulic composition is left for 3 hours at an ambient temperature of room temperature, for example, 10°C to 30°C (pre-curing), the ambient temperature is raised to 70°C to 90°C at a rate of 20°C per hour, the temperature is maintained at 70°C to 90°C for 2 to 6 hours, the ambient temperature is then cooled to room temperature, for example, 20°C at a rate of 10°C per hour (step 4), and the molded body is demolded after being left at that temperature for 20 to 30 hours (step 5). Furthermore, it is also possible to perform autoclave curing at approximately 180°C.
[0068] In step 6, the hardened hydraulic composition obtained in step 5 is cured at room temperature and atmospheric pressure. Specifically, it is stored at 20°C and atmospheric pressure.
[0069] The present invention provides a method for producing a hardened hydraulic composition, comprising steps 1 to 5, wherein the time from the start of preparation of the hydraulic composition to demolding in step 5 is 8 hours or more and 30 hours or less. Here, the start of preparation of the hydraulic composition refers to the point in time when cement and water first come into contact.
[0070] The hardened hydraulic composition obtained by the manufacturing method of the present invention can be used as a centrifugal-formed concrete product, specifically, piles, poles, Hume pipes, etc. The hardened hydraulic composition obtained by the manufacturing method of the present invention exhibits excellent formability after a certain period of time (15 minutes to 60 minutes) from mixing, resulting in less unevenness on the inner surface and end faces of the product, excellent surface aesthetics, and a smooth inner surface finish, thereby improving the performance of cutting machines during pile driving and excavation methods. [Examples]
[0071] The components (A) and (A') (comparison components for (A)) shown in Table 1 were as follows.
[0072] (A) component (a-1): A copolymer synthesized according to Production Example A1 in paragraph 0048 and Production Example C1 in paragraph 0058 of Japanese Patent Publication No. 2009-161379, monomer (A1) / monomer (A2) / monomer (A3) = fumaric acid, maleic anhydride / polyamide polyamine, which is a condensate of adipic acid and polyalkylene polyamine, to which ethylene oxide is added, resulting in a monomer / metharyl polyethylene glycol (50) polypropylene glycol (2) ether (block adduct, average number of added moles in parentheses) = 13.8 mass% / 2.7 mass% / 83.5 mass%, weight-average molecular weight = 26,000, and the obtained polymer is a sodium salt.
[0073] (A') component (a'-1): Copolymer 1 described in paragraph 0082 of Japanese Patent Publication No. 2020-66553, sodium acrylate / sodium methacrylate / methoxypolyethylene glycol (45) monomethacrylate (the number in parentheses for the monomer is the average number of moles added) = 29 mol% / 45 mol% / 26 mol%, weight-average molecular weight = 30,000, and the obtained polymer is a sodium salt.
[0074] (1) Concrete mix Table 1 shows the concrete mix design. The following concrete materials were used. W / B is the water / cement ratio (mass%). In Table 1, the amounts of cement (C), tap water (W), sand (S), and gravel (G) added per cubic meter of concrete are shown. 3 This is the amount added (kg) relative to [the specified value]. Cement (C): Manufactured by Taiheiyo Cement Corporation, specific gravity 3.14 • Tap water (W): The amount listed in Table 1 was used as the weight containing component (A) or component (A'). • Sand (S): From Koka, Shiga Prefecture, specific gravity 2.58 • Gravel (G): From Ieshima Island, Hyogo Prefecture, specific gravity 2.63
[0075] (2) Concrete preparation A composition containing component (A) or component (A') and water was prepared in the amounts shown in Table 1. This composition was added to the water (W) of the concrete mix material and stirred to prepare the mixing water. The concrete was prepared by adding gravel, about half the amount of sand, cement, and the remaining sand in that order to a forced twin-shaft mixer (manufactured by KYC Corporation). Dry mixing was performed for 30 seconds, then the prepared mixing water was quickly added and mixed for 240 seconds to obtain the concrete.
[0076] (3) Evaluation of concrete fluidity The slump (cm) of the concrete immediately after mixing was measured according to JIS A 1101. The results are shown in Table 1.
[0077] (4) Evaluation of centrifugal moldability Ten minutes after mixing, the concrete was placed in a centrifugal molding mold (inner diameter 20 cm, outer diameter 25 cm, height 40 cm), sealed with a rubber stopper, and then centrifugal compaction was performed at the following conditions: initial velocity of 1 G for 2 minutes, second velocity of 3 G for 2 minutes, third velocity of 7 G for 2 minutes, fourth velocity of 15 G for 3 minutes, and fifth velocity of 25 G for 3 minutes. After centrifugal compaction, the rubber stopper of the centrifugal molding mold was opened, and the cylindrical molded body inside the mold was tilted vertically at a 45° angle. The generated sludge was collected using a 500 mL disposable cup, and the sludge weight (g) was measured. The sludge weight is the average of the sludge weights generated from n=2 molded bodies, and if sludge collection was difficult, it was recorded as 0 g. The results are shown in Table 1.
[0078] [Table 1]
[0079] In Table 1, the amount of component (A) or component (A') added per cubic meter of concrete. 3 This is the amount added (kg) relative to the total amount, and represents the amount of solid content (effective content) added.
[0080] In Table 1, Examples 1-5 using component (A) of the present invention were less prone to sludge formation even when subjected to fluctuations in water content (fluctuations in W / B ratio) compared to Comparative Examples 1-3 using component (A'). This is thought to be because component (A), which exhibits excellent adsorption properties for cement particles and low-density hydration products, suppressed separation due to centrifugal force and, consequently, sludge formation.
Claims
1. A hydraulic composition for centrifugal molding comprising the following component (A), cement, aggregate, and water, wherein the water / cement ratio is 20% by mass or more and 35% by mass or less. Component (A): A copolymer containing, as constituent monomers, one or more monomers (A1) selected from fumaric acid, maleic acid (anhydride), and salts thereof, a monomer (A2) represented by the following general formula (A2), and a monomer (A3) represented by the following general formula (A3), wherein, among the constituent monomers of the copolymer, the proportion of monomer (A1) is 1% by mass or more and 30% by mass or less, the proportion of monomer (A2) is 1% by mass or more and 20% by mass or less, and the proportion of monomer (A3) is 50% by mass or more and 90% by mass or less. 【Chemistry 1】 [In general formula (A2), R 21a , R 22a , R 23a may be the same or different and are a hydrogen atom, a methyl group, or COOM, M is a hydrogen atom, an alkali metal, an alkaline earth metal (1 / 2 atom), an ammonium group, an alkylammonium group, or a substituted alkylammonium group, and Z is a group that bonds to a carbon atom of the main chain via an amide bond in a polyamidepolyamine obtained by condensing a dibasic acid with a polyalkylenepolyamine and / or a modified polyamidepolyamine obtained by adding 0.1 mol to 10 mol of an alkylene oxide having 2 to 4 carbon atoms per equivalent of an active imino group, amino group, or amide residue of the polyamidepolyamine.] 【Chemistry 2】 [In general formula (A3), R 31a , R 32a may be the same or different and are a hydrogen atom or a methyl group; R 33a is a hydrogen atom or -COO(AO) n X, X is an alkyl group having 1 to 4 carbon atoms or a hydrogen atom, AO is a group selected from an ethyleneoxy group and a propyleneoxy group, n is the average number of moles of AO added and is a number of 5 to 150, p is a number of 0 to 2, and q is a number of 0 or 1.
2. 2. The hydraulic composition for centrifugal molding according to claim 1, wherein the proportion of the monomer (A1) in the constituent monomers of the copolymer of component (A) is 8% by mass or more and 30% by mass or less.
3. 3. The hydraulic composition for centrifugal molding according to claim 1 or 2, wherein the total proportion of the monomers (A1), (A2) and (A3) in the constituent monomers of the copolymer of component (A) is 95 mass% or more.
4. The content of the component (A) per 1 m of the hydraulic composition for centrifugal molding is 3 The hydraulic composition for centrifugal molding according to any one of claims 1 to 3, wherein the weight of the hydraulic composition is 0.4 kg or more and 1.5 kg or less.
5. The content of high-strength admixture in centrifugal molding hydraulic composition is 3 The hydraulic composition for centrifugal molding according to any one of claims 1 to 4, wherein the hydraulic composition has a maximum load of 50 kg or less.
6. A method for producing a hardened hydraulic composition, comprising the following steps: Step 1: A step of mixing the following (A) component, cement, aggregate, and water in a water / cement ratio of 20 mass% or more and 35 mass% or less to obtain a hydraulic composition, and filling the obtained hydraulic composition into a formwork. Step 2: A step of clamping the hydraulic composition filled in the form obtained in step 1 by applying centrifugal force. Step 3: A step of allowing the clamped hydraulic composition obtained in step 2 to set in the form. Component (A): A copolymer containing, as constituent monomers, one or more monomers (A1) selected from fumaric acid, maleic acid (anhydride), and salts thereof, a monomer (A2) represented by the following general formula (A2), and a monomer (A3) represented by the following general formula (A3), wherein, among the constituent monomers of the copolymer, the proportion of monomer (A1) is 1% by mass or more and 30% by mass or less, the proportion of monomer (A2) is 1% by mass or more and 20% by mass or less, and the proportion of monomer (A3) is 50% by mass or more and 90% by mass or less. 【Chemistry 3】 [In general formula (A2), R 21a , R 22a , R 23a may be the same or different and are a hydrogen atom, a methyl group, or COOM, M is a hydrogen atom, an alkali metal, an alkaline earth metal (1 / 2 atom), an ammonium group, an alkylammonium group, or a substituted alkylammonium group, and Z is a group that bonds to a carbon atom of the main chain via an amide bond in a polyamidepolyamine obtained by condensing a dibasic acid with a polyalkylenepolyamine and / or a modified polyamidepolyamine obtained by adding 0.1 mol to 10 mol of an alkylene oxide having 2 to 4 carbon atoms per equivalent of an active imino group, amino group, or amide residue of the polyamidepolyamine.] 【Chemistry 4】 [In general formula (A3), R 31a , R 32a may be the same or different and are a hydrogen atom or a methyl group; R 33a is a hydrogen atom or -COO(AO) n X, X is an alkyl group having 1 to 4 carbon atoms or a hydrogen atom, AO is a group selected from an ethyleneoxy group and a propyleneoxy group, n is the average number of moles of AO added and is a number of 5 to 150, p is a number of 0 to 2, and q is a number of 0 or 1.
7. 7. The method for producing a hardened hydraulic composition according to claim 6, wherein the proportion of the monomer (A1) in the constituent monomers of the copolymer of component (A) is from 8% by mass to 30% by mass.
8. The method for producing a hydraulic composition hardened body according to claim 6 or 7, wherein the total proportion of the monomer (A1), the monomer (A2) and the monomer (A3) in the constituent monomers of the copolymer of component (A) is 95 mass% or more.
9. In step 1, the mixing amount of component (A) is 1 m 3 The method for producing a hardened hydraulic composition according to any one of claims 6 to 8, wherein the weight of the hardened hydraulic composition is 0.4 kg or more and 1.5 kg or less.
10. The method for producing a hardened hydraulic composition according to any one of claims 6 to 9, further comprising the following step 4 after step 3: Step 4: A step of steam curing the set hydraulic composition obtained in step 3 in a formwork.
11. The method for producing a hardened hydraulic composition according to claim 10, wherein in step 4, the steam curing temperature is 40°C or higher and 90°C or lower.