Alkaline battery separator with controlled pore size

JP2023086729A5Pending Publication Date: 2024-11-27SWM LUXEMBOURG SARL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023044957
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-09-26
Filing Date
2023-03-22
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Existing alkaline battery separators face challenges with mechanical integrity, processability, and cost due to coarse fibers, leading to issues like stiffness, poor drop resistance, and increased risk of short circuits from dendrite formation, while the need for controlled pore sizes is unmet.

Method used

Development of alkaline battery separators comprising blends of polyvinyl alcohol (PVA) and cellulose derivatives with controlled pore sizes, achieved through fibrillation of cellulose fibers like Tencel, resulting in a blend with specific proportions and controlled pore sizes ranging from 1.6-12 μm.

Benefits of technology

The solution enhances mechanical properties, reduces fiber entanglement, and minimizes short circuits, providing improved ion transport and discharge performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an alkaline battery separator including a blend of polyvinyl alcohol and cellulose or cellulose derivatives with controlled pore size and a method of manufacturing such a separator.SOLUTION: An alkaline battery separator including a blend of polyvinyl alcohol and cellulose derivative with controlled pore size highly fibrillates cellulose derivative and optionally cellulose, and combines it with PVA. A method of manufacturing an alkaline battery separator including a blend of polyvinyl alcohol and a cellulose derivative with controlled pore size.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to an alkaline battery separator comprising a blend of polyvinyl alcohol and cellulose or a cellulose derivative having a controlled pore size, and a method of manufacturing such a separator.

Background Art

[0002] Separator paper for alkaline batteries serves as a mechanical barrier between electrodes to prevent short circuits while allowing the transport of ions by the electrolyte in the pores. The separator must have good mechanical integrity, chemical inertness, and a consistent porosity and flexibility with well-defined contours to uniformly transport ions between the electrodes. Separator paper used in alkaline batteries often contains a blend of polyvinyl alcohol (PVA) fibers and cellulose, or cellulose derivatives such as rayon or tencel. Generally, PVA fibers promote dimensional stability in potassium hydroxide electrolyte, while cellulose and its derivatives assist in absorption properties. In addition to the fiber composition, separators are designed at various levels of basis weight. The availability of thick PVA as well as rayon fibers has enabled a trend towards material lightweighting, aiming to save space within the cell to allow for a greater amount of active material and enhance discharge performance. However, considering technical and economic concerns, low levels of basis weight are no longer considered the ultimate goal. Technical concerns include the processability that causes the rigidity and mechanical properties of the battery, which lead to insufficient drop resistance. The inclusion of thick fibers contributes significantly to the cost. New types of anodes with higher performance have been developed. However, these anodes also have a stronger tendency to generate dendrites that cause short circuits, and therefore battery manufacturers are seeking to enhance the barrier properties. There is a need for separators having a controlled and predetermined pore size, i.e., the average diameter, maximum diameter, and volume can be preselected.

Summary of the Invention

[0003] This disclosure generally relates to alkaline battery separators comprising a blend of PVA and cellulose derivatives having a controlled pore size of less than approximately 4.0 μm. In one embodiment, the separator comprises about 30% to about 60% PVA and about 40% to about 60% lyocell fibers such as Tencel. In another embodiment, the separator comprises at least 55% PVA and at least 45% Tencel. In one embodiment, the alkaline battery is a Zn / MnO2 battery. In another embodiment, the present disclosure relates to a method for producing an alkaline battery separator having a controlled pore size, comprising the steps of: highly fibrillating a cellulose derivative and optionally cellulose; and combining it with PVA. The descriptions herein of desirable features fulfilled by various embodiments of this disclosure do not imply or suggest that any or all of these features, individually or collectively, are present as essential features in any of the most common embodiments of this disclosure or any of its more limited embodiments. [Modes for carrying out the invention]

[0004] Unless otherwise indicated, any quantitative values ​​are approximate, regardless of whether words such as "about" or "approximately" are used. The materials, methods, and examples described herein are illustrative and not intended to limit the scope of the text. Any molecular weight values ​​are approximate and provided for illustrative purposes only. This specification discloses an alkaline battery separator comprising a blend of polyvinyl alcohol and a cellulose derivative. The separator has a controlled pore size, i.e., the pore size can be predetermined or selected. In some embodiments, the alkaline battery separator comprises a blend of polyvinyl alcohol, a cellulose derivative, and cellulose. The separator can be used in various alkaline batteries, such as Zn / MnO2 batteries. Cellulose and cellulose derivatives may include, but are not limited to, natural cellulose (such as wood fibers and pulp, cotton, and hemp) and regenerated cellulose (e.g., rayon and Tencel).

[0005] The separator may contain PVA in proportions of at least about 20% by mass, at least about 30% by mass, and at least about 55% by mass. The separator may contain lyocell fibers such as Tencel in proportions of at least about 25% by mass, at least about 35% by mass, and at least about 45% by mass. In one embodiment, the separator contains at least 55% PVA and at least 45% lyocell fibers such as Tencel. The separator may contain about 0% to about 30% cellulose. Generally, a method for producing a separator includes a step of highly fibrillating a cellulose derivative, such as lyocell fibers like Tencel, and optionally the cellulose, before combining it with PVA. Fibrillation of cellulose can be achieved using a mechanical refiner, such as a single-disc refiner, double-disc refiner, conical refiner, rotary cylinder refiner, or other type of refiner, which is used to mechanically grind or process the cellulose or cellulose derivative to produce individual fibers and smaller fibril units. The feed material for this step may be a pre-treated cellulosic material (e.g., wood chips, annual plants) formed into pulp. The pretreatment of the cellulosic material used to produce the pulp may be the result of chemical digestion such as kraft pulping, sulfite pulping, soda pulping, mechanical refining, a combination of chemical digestion and refining, or other known processes.

[0006] Fibrillation can occur at various durations and energy levels, such as 125 to 200 minutes, with total energies of 185 to 200 kW corresponding to a specific edge load (SEL) of 0.65 to 0.75 J / m. The fibrillation process is carried out with a 30 g / l fiber suspension. Generally, fibrillation occurs over a long period at low energy, with the goal of introducing a predetermined amount of energy into the cellulose, such as a total energy of 1200 to 1500 kWh / T (specific energy of 700 to 1150 kWh / T), to reach a fibrillation level between 37 and 25 CSF, within the range of Canadian standard filtration efficiency (CSF) of 140 to 100. The resulting fibrillated fibers typically have a width of 16 to 20 μm and a length of 1000 to 1150 μm. In the fibrillation process, longer durations are preferable to higher energy levels to avoid fiber breakage. Once the fibrillation process is carried out and controlled, the cellulose and / or cellulose derivatives are diluted with cold water to cool to a temperature below 40°C in anticipation of the addition of both water-soluble PVA fibers and primary PVA fibers in the pulper. Generally, both types of PVA fibers have a cut length of 2–4 mm. If finer fibers (e.g., low denier (d) or dTex) are used, shorter fibers are required to avoid unexpected fiber entanglement. The fiber blend is thoroughly mixed in the pulper before being transferred to the paper machine box.

[0007] When testing with a PMI dimensional measuring instrument, the mass is 20-40 g / m². 2 Typical separators between these fibers have an average pore diameter in the range of 1.6–12 μm and a maximum pore diameter in the range of 6–40 μm. The highly fibrillated fibers described herein have a smaller average pore diameter, a smaller maximum pore diameter, and a smaller difference between the average and maximum pore diameters. The average pore size of the separators described herein may be less than about 5 μm, less than about 4 μm, less than about 3 μm, or less than about 2.0 μm. The maximum pore size may be less than about 16 μm, for example, about 4 μm to about 25 μm, about 5 μm to about 20 μm, and about 9 μm to about 16 μm. In one embodiment, the average pore size is about 1.5 μm to about 3 μm. [Examples]

[0008] (Example 1) PVA (0.5d) (VPB 0.53) and soluble PVA (VPB 105-2) were purchased from Kuraray Co. Tencel (Lenzing Co.), cut to a length of 3 mm, was fibrillated for 115 minutes under a SEL of 0.65 J / m using a 24” double disc refiner to achieve a CSF of 117 and a final fiber length of 1.1 mm. After the fibrillation process was carried out and controlled, the fibrillated Tencel fibers were diluted with cold water and cooled to a temperature below 40°C before proceeding to the addition of both water-soluble PVA fibers and main PVA fibers in the pulper. The fiber blend was thoroughly mixed in the pulper for 10 minutes before being transferred to the paper machine box. The slurry was processed at a speed of 90 m / min on an inclined wire paper machine to produce porous sheets with the parameters described in Table 1. Thickness, as well as MD and CD tensile strengths, were measured according to ISO 534 and ISO 1924-2, respectively. Thickness was measured by applying pressures of 100 kPa and 20 kPa. KOH absorption capacity and rate were measured from a 34% KOH solution according to industry standard methods. ASTM The average and maximum pore diameters were measured according to 316. (Example 2) Example 2 was prepared as described for Example 1, except that the main PVA fiber was selected at 0.3d (VPB 033; Kurary Co.) and Tencel was fibrillated to 120 CSF after fibrillation under 0.69 J / m SEL for 155 minutes. Before processing on the paper machine, the PVA and Tencel were combined in a ratio of 55% by mass:45% by mass. (Example 3) As described for Example 2, Example 3 was prepared using 0.3d PVA VPB 033. The first batch of 1.7dTex Tencel was fibrillated at 250 CSF under a SEL of 0.52 J / m for 20 minutes. The second batch of Tencel was fibrillated at 30 CSF and prepared by refining under a SEL of 0.08 J / m for 34 hours. The resulting fiber blend, consisting of 55% PVA, 33% Tencel from the first batch, and 12% Tencel from the second batch, was then processed in a paper machine.

[0009] (Example 4) Example 4 was prepared using 0.3d PVA VPB 033, as described for Example 3. A batch of 1.4dTex Tencel was fibrillated at 95 CSF by refining for 135 minutes under 0.52 J / m SEL. 30 g / m 2 Before processing, PVA and Tencel were combined in a ratio of 40% by mass:60% by mass. (Example 5) Example 5 was prepared using 0.3d PVA VPB 033 as described for Example 4. A batch of 1.4dTex Tencel was fibrilized at 95 CSF by refining for 135 minutes under 0.52 J / m SEL. 20 g / m 2 Before processing, PVA and Tencel were combined in a ratio of 55% by mass:45% by mass.

[0010] [Table 1]

[0011] While the present invention has been described in detail herein according to certain preferred embodiments, many modifications and changes can be made therein by those skilled in the art. Therefore, the foregoing disclosure should not be construed as being limited thereto, but rather as being limited only by the spirit and scope of the following claims, including such obvious modifications.

Claims

1. An alkaline battery separator comprising a blend of polyvinyl alcohol and a cellulose derivative having a controlled average pore size of less than about 4.0 μm.

2. 10. The alkaline battery separator of claim 1, wherein said average pore size is from about 1.5 μm to about 3 μm.

3. 10. The alkaline battery separator of claim 1, wherein said cellulosic comprises lyocell fiber.

4. 3. The alkaline battery separator of claim 2 comprising at least 55% polyvinyl alcohol and at least 45% lyocell fibers.

5. 4. The alkaline battery separator of claim 3 further comprising regenerated cellulose.

6. 10. The alkaline battery separator of claim 1 having a controlled maximum pore size of less than about 5 μm.

7. A battery comprising the battery separator of claim 1.

8. A battery comprising the battery separator of claim 2.

9. A battery comprising the battery separator of claim 3.

10. A battery comprising the battery separator of claim 4.

11. A battery comprising the battery separator of claim 5.

12. A battery comprising the battery separator of claim 6.