Optical element and manufacturing method therefor
Patent Information
- Application Number
- JP2021201921
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-13
AI Technical Summary
Existing optical elements, particularly cemented lenses, suffer from distortion during bonding due to the use of ultraviolet curable resins, which shrink and cause stress, leading to precision issues and deformation, especially in lenses with thin central thicknesses.
The solution involves applying coating layers on the transparent substrates that will be bonded, ensuring the main components of these coating layers are substantially the same, with a specific ratio of mass percentages, to equalize the forces exerted by the adhesive and minimize distortion.
This approach significantly reduces distortion during the bonding process, ensuring high precision and maintaining optical integrity by equalizing the forces across the bonded lenses.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to optical elements, methods for manufacturing the same, optical instruments, and imaging devices, and more particularly to cemented lenses used in optical instruments such as cameras, binoculars, and microscopes, optical instruments having the same, and imaging devices. [Background technology]
[0002] In the optical systems of optical instruments such as cameras and binoculars, cemented lenses, which are made by bonding multiple lenses or prisms together with an optically transparent resin, are widely used. One of the purposes of using cemented lenses is aberration correction. Even with a single material, the refractive index differs depending on the wavelength of light. Therefore, in a convex lens, the focal position of light differs depending on the wavelength. For example, the focal positions differ for the typical wavelengths of C-line (656 nm: red) and F-line (486 nm: blue). This phenomenon is called chromatic aberration. To improve chromatic aberration, it is known that a convex lens and a concave lens with a different wavelength dispersion are used as a chromatic aberration lens (also called an achromatic lens). In other words, by combining a chromatic aberration lens with a convex lens, the focal positions of light of different wavelengths can be matched. This is called chromatic aberration correction.
[0003] When combining a chromatic aberration lens and a convex lens, if a gap is left between the two lenses, interfacial reflection occurs, resulting in a loss of incident light. Therefore, to reduce interfacial reflection, the two lenses are bonded together using a bonding resin. Traditionally, a natural resin called balsam was used as the bonding resin, but in recent years, organic resins with higher adhesive strength, especially UV-curing resins, have been used.
[0004] UV-curable resins are resins that harden when exposed to light such as ultraviolet light, generating radicals that cause monomers to polymerize. When bonding lenses, alignment work is performed to match the optical axis, and when bonding lenses with bonding resin, it is necessary to hold the parts in place after alignment until the resin hardens. Generally, UV-curable resins harden faster than other curing resins or balsam resins that utilize heat softening, thus shortening the holding time and making them suitable for bonding optical components.
[0005] However, UV-curable resins are known to shrink in volume during the curing reaction process. Therefore, when bonding lenses with UV-curable resins, problems arise regarding dimensional accuracy and stress generation due to shrinkage (Patent Document 1). On the other hand, with the miniaturization and increased precision of lenses, there is a need to bond lenses together with high precision and to suppress deformation during the bonding process. In particular, there is a need to bond lenses that are prone to deformation, such as lenses with thin central wall thickness, with high precision (Patent Document 1). [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-160963 [Overview of the project] [Problems that the invention aims to solve]
[0007] In view of the above, the present invention aims to provide an optical element that exhibits excellent optical properties and minimizes distortion generated during the bonding (joining) of lenses. [Means for solving the problem]
[0008] An optical element comprising a first transparent substrate, a second transparent substrate, and an adhesive layer provided between the first transparent substrate and the second transparent substrate, moreover, A first coating layer located on the first transparent substrate and in contact with the adhesive layer, The second transparent substrate has a second coating layer that is in contact with the adhesive layer, The main component of the material of the first coating layer and the main component of the material of the second coating layer are the same. The proportion of the main component of the material of the first coating layer is X A X is the mass percentage of the main component of the material of the second coating layer. B If we consider mass as a percentage, then 8 / 10 ≤ X A / X B The present invention provides an optical element characterized by the fact that ≤ 10 / 8 holds true. [Effects of the Invention]
[0009] According to the present invention, it is possible to provide optical elements with less distortion during bonding, particularly bonded lenses. [Brief explanation of the drawing]
[0010] [Figure 1] A diagram illustrating lens distortion during the joining process. [Figure 2] A diagram illustrating how lens distortion caused during bonding is eliminated. [Figure 3] Examples of cemented lenses [Figure 4] Examples of manufacturing cemented lenses [Figure 5] Examples of imaging devices [Modes for carrying out the invention]
[0011] The inventors used an ultraviolet-curing resin as an adhesive and measured the surface shape of the lenses at each step of the lens bonding process. Contrary to expectations, they found that lens distortion began to occur when the adhesive was filled in, even before it had fully cured. Furthermore, it was considered that one of the causes of distortion lies in the difference in force generated between the adhesive and each lens as the adhesive spreads between the lenses being joined, and that this difference is due to the different materials of the lenses being joined. Since a joined lens consists of multiple different glass materials, the materials of the multiple lenses are inherently different. Therefore, the inventors attempted to eliminate the difference in force between the adhesive and each lens by providing a coating layer on the side of each lens to be joined that faces the adhesive, and by making the material of these coating layers roughly the same. As a result of diligent research, they found that the distortion of the joined lenses could be improved, and thus completed the present invention.
[0012] As a first embodiment of the present invention, An optical element comprising a first transparent substrate, a second transparent substrate, and an adhesive layer provided between the first transparent substrate and the second transparent substrate, moreover, A first coating layer located on the first transparent substrate and in contact with the adhesive layer, The second transparent substrate has a second coating layer that is in contact with the adhesive layer, The main component of the material of the first coating layer and the main component of the material of the second coating layer are the same. The proportion of the main component of the material of the first coating layer is X A X is the mass percentage of the main component of the material of the second coating layer. B If we consider mass as a percentage, then 8 / 10 ≤ X A / X B The present invention provides an optical element characterized by the fact that ≤ 10 / 8 holds true.
[0013] Furthermore, as a second embodiment of the present invention, A method for manufacturing an optical element comprising a first transparent substrate, a second transparent substrate, and an adhesive layer, A step of providing a first coating layer on any surface of the first transparent substrate, A step of providing a second coating layer on any surface of the second transparent substrate, A filling step of filling the space between the first coating layer and the second coating layer with adhesive, including a curing step of curing the adhesive, the main component of the material of the first coating layer is the same as the main component of the material of the second coating layer, let the proportion of the main component of the material of the first coating layer be X A mass%, and the proportion of the main component of the material of the second coating layer be X B mass%, then 8 / 10 ≦ X A / X B ≦ 10 / 8 is satisfied, and a manufacturing method is provided.
[0014] The material of the first coating layer and the material of the second coating layer are preferably substantially the same. "Above" does not refer to up and down, but indicates a relative positional relationship, meaning that when the objects are viewed from a certain direction, they are in an up-and-down relationship, and it does not mean that the objects are in contact with each other. That is, in the above description, "the first coating layer on the first transparent substrate and in contact with the adhesive layer" means that the first coating layer is in contact with the adhesive layer on the side of the first transparent substrate, and the first coating layer may or may not be in contact with the first transparent substrate. The same applies to "the second coating layer on the second transparent substrate and in contact with the adhesive layer".
[0015] Regarding the reason why the distortion of the bonding lens is improved according to the present invention, it will be described with reference to FIGS. 1 and 2. In FIG. 1, it is an example in which an adhesive 130 is directly filled between the first transparent substrate 11 and the second transparent substrate 12 without providing a coating layer.
[0016] The uncured liquid adhesive 130 has elastic properties, and a corresponding stress is generated when the adhesive is spread. Since the first transparent substrate 11 and the second transparent substrate 12 are made of different materials, the force generated between the adhesive 130 and the first transparent substrate 11 is different from the force generated between the adhesive 130 and the second transparent substrate 12.
[0018] As a result, if we define one end of the contact point between the adhesive 130 and the substrate as it spreads, point P on the first transparent substrate 11 (or second transparent substrate 12) side and point Q on the second transparent substrate 12 (or first transparent substrate 11) side, and one end of the adhesive 130 in the space between the first transparent substrate 11 and the second transparent substrate 12 as point C, then while C moves to C', P and Q move to P' and Q' respectively, but the distances between P-P' and Q-Q' are different. Consequently, the force applied to the adhesive layer changes from horizontal f to diagonal f', and we believe that the change in the amount of elongation between each transparent substrate and the adhesive is the cause of lens distortion.
[0019] On the other hand, in Figure 2, the optical element 10 has a first coating layer 101 on the side in contact with the adhesive layer 13 of the first transparent substrate 11, and a second coating layer 102 on the side in contact with the adhesive layer 13 of the second transparent substrate 12, and these coating layers are made of roughly the same material. Therefore, the distances of P-P' and Q-Q' are equal, the force applied to the adhesive layer is kept horizontal, and no lens distortion occurs.
[0020] (Explanation of terms) In this specification, "components" are not limited in any way and include all substances, compositions, compounds, elements, etc. that constitute a material. The components are bonded to each other by chemical bonds such as covalent bonds, metallic bonds, ionic bonds, hydrogen bonds, and van der Waals forces, thereby constituting the material.
[0021] In this specification, the main component refers to a component that accounts for 22% or more by mass of a given material. In this specification, materials that are substantially the same are defined as follows: The main components of material A and material B are the same, and the proportion of the main component in material A is X. A X represents the mass percentage of the main component in material B.B If we consider mass as a percentage, then 8 / 10 ≤ X A / X B The relationship ≤ 10 / 8 holds true. When this relationship holds, material A and material B are said to be approximately identical. Here, the term "main component" does not refer to just one component; for example, material A may have 1 to 4 main components, and material B may have 1 to 4 main components. Matching principal components means that at least one principal component is the same. Having the same main component as two materials means that at least one of their main components is identical. It is sufficient for at least one of the main components of material A and the main components of material B to be the same, but it is preferable that the number of main components of material A and the number of main components of material B are the same, and that all of the main components of material A and material B are the same. Furthermore, it is preferable that the total proportion of the main components in material A is 72% by mass or more, and the total proportion of the main components in material B is 72% by mass or more.
[0022] For example, in the following case, material A and material B are essentially the same. Material A and Material B each have one main component, and their main components are the same (let's call this component 1). Material A has component 1 X 1A Mass %, Material B is component 1 X 1B It has a mass of %, and 8 / 10 ≤ X 1A / X 1B The condition ≤ 10 / 8 is satisfied. 72 ≤ X 1A , 72≦X 1B It is preferable that the following conditions are met. For example, if material A contains 72% by mass of component 1 and a total of 28% by mass of other components other than the main component, and material B contains 80% by mass of component 1 and a total of 20% by mass of other components other than the main component, then material A and material B are generally the same. Also, for example, if material A contains 100% by mass of component 1 and material B contains 80% by mass of component 1 and a total of 20% by mass of other components other than the main component, then material A and material B are generally the same.
[0023] If either material A or material B has two main components, then at least one of the main components of material A and material B is the same (let's call it component 1), and material A has component 1 as X 1A Mass %, Material B has component 1 as X1B It has a mass of %, and 8 / 10 ≤ X 1A / X 1B The condition ≤ 10 / 8 is satisfied. Alternatively, more preferably, material A and material B each have two main components, and these main components are the same (let's call them component 1 and component 2), and material A has component 1 as X 1A Mass %, component 2 is X 2A Mass %, Material B has component 1 as X 1B Mass %, component 2 is X 2B It has a mass of %, and 8 / 10 ≤ X 1A / X 1B ≤ 10 / 8, and 8 / 10 ≤ X 2A / X 2B The material satisfies one of the following conditions ≤ 10 / 8, and more preferably all of them. For example, a preferred example where material A contains 36% by mass of component 1, 40% by mass of component 2, and a total of 24% by mass of other components other than the main component, and material B contains 40% of component 1, 36% of component 2, and a total of 24% by mass of other components other than the main component, is a preferred example where material A and material B are roughly the same.
[0024] If either material A or material B has three main components, then at least one of the main components of material A and material B is the same (let's call it component 1), and material A has component 1 as X 1A Mass %, Material B has component 1 as X 1B It has a mass of %, and 8 / 10 ≤ X 1A / X 1B The condition ≤ 10 / 8 is satisfied. Alternatively, more preferably, material A and material B each have three main components, and these main components are the same (let's call them component 1, component 2, and component 3), and material A has component 1 as X 1A Mass %, component 2 is X 2A Mass%, component 3 is X 3A Mass %, Material B has component 1 as X 1B Mass %, component 2 is X 2B Mass%, component 3 is X 3B Mass%, present, 8 / 10≦X 1A / X 1B ≤10 / 8, 8 / 10 ≤X 2A / X 2B ≤10 / 8, 8 / 10 ≤X 3A / X 3BThe material satisfies one of the following conditions ≤ 10 / 8, and more preferably all of them. For example, if material A has 23% by mass of component 1, 25% by mass of component 2, 30% by mass of component 3, and a total of 22% by mass of other components other than the main components, and material B has 25% by mass of component 1, 23% by mass of component 2, 31% by mass of component 3, and a total of 21% by mass of other components other than the main components, then material A and material B are a preferred example of materials being roughly the same.
[0025] If either material A or material B has four main components, then at least one of the main components of material A and material B is the same (let's call it component 1), and material A has component 1 as X 1A Mass %, Material B has component 1 as X 1B It has a mass of %, and 8 / 10 ≤ X 1A / X 1B The condition ≤ 10 / 8 is satisfied. Alternatively, more preferably, material A and material B each have four main components, and these main components are the same (let's call them component 1, component 2, component 3, and component 4), and material A has component 1 as X 1A Mass %, component 2 is X 2A Mass%, component 3 is X 3A Mass%, component 4 is X 4A Mass %, Material B has component 1 as X 1B Mass %, component 2 is X 2B Mass%, component 3 is X 3B With mass%, component 4 has X4B mass%, and 8 / 10≦X 1A / X 1B ≤10 / 8, 8 / 10 ≤X 2A / X 2B ≤10 / 8, 8 / 10 ≤X 3A / X 3B ≤10 / 8, 8 / 10 ≤X 4A / X 4B The material satisfies one of the following conditions ≤ 10 / 8, and more preferably all of them. For example, if material A has 24% by mass of component 1, 25% by mass of component 2, 23% by mass of component 3, 24% by mass of component 4, and a total of 4% by mass of other components other than the main components, and material B has 25% by mass of component 1, 23% by mass of component 2, 24% by mass of component 3, 25% by mass of component 4, and a total of 3% by mass of other components other than the main components, then material A and material B are a preferred example of materials being roughly the same.
[0026] Furthermore, preferably, all the main components are the same, and the total proportion of the main components in material A is 80% by mass or more, and the total proportion of the main components in material B is 80% by mass or more. Material A and material B are said to be the same when all the components and their respective proportions are substantially the same. When material A and material B are the same, A and B are also generally the same insofar as material A and material B have main components.
[0027] Preferred embodiments of the present invention will be described below. (Optical element) Figure 3 is a schematic cross-sectional view showing one embodiment of a bonded lens, which is an optical element of the present invention. The optical element 10 is a type of optical element called a bonded lens, in which two transparent substrates are bonded together via an adhesive layer 13. L refers to incident light, and L C This is the refracted light of line C, L F This is the refracted light of the F line, f C The focal point of the C line is f F This indicates the focus of the F line. By joining two transparent substrates, f F and f C These match. In Figure 3, the optical element 10 comprises a first transparent substrate 11, a second transparent substrate 12, and an adhesive layer 13. Note that either the transparent substrate 11 or the transparent substrate 12 may be referred to as the first transparent substrate or the second transparent substrate. For convenience, in this figure, the first transparent substrate 11 is represented by a convex lens and the second transparent substrate 12 is represented by a concave lens.
[0028] The outer shapes of the first transparent substrate 11 and the second transparent substrate 12 are preferably substantially circular when viewed from a planar direction parallel to the incident light.
[0029] Distortion during bonding of transparent substrates is particularly likely to occur when the optical element is a concave bonded lens with a thin central wall thickness. Distortion is also more likely to occur when the diameter of the optical element is large. In this specification, the thickness of the central wall thickness of the optical element may be expressed as t, and the outer diameter of the lens of the optical element may be expressed as D, or outer diameter D. The outer diameter of the optical element refers to the diameter of the optical element when the shape of the optical element, viewed from a plane parallel to the light incident on the optical element, is approximated as a circle. Because distortion during bonding is eliminated in the optical element of the present invention, it is possible for the ratio of t to D, i.e., t / D, to satisfy t / D < 0.02.
[0030] (Transparent base material) The first transparent substrate 11 and the second transparent substrate 12 may be made of transparent resins such as acrylic resin, polycarbonate resin, polystyrene resin, allyl diglycol carbonate resin, polyurethane resin, or polythiourethane resin, or transparent glass-like materials such as common optical glass represented by silicate glass, borosilicate glass, or phosphate glass, or quartz glass, or glass ceramic glass. In this specification, "transparent" means that the transmittance of light in the wavelength range of 400 nm to 780 nm is 10% or more.
[0031] A bonded lens, by its very nature, is made by bonding a low-dispersion glass material to a high-dispersion glass material, and the materials of the first transparent substrate 11 and the second transparent substrate 12 are often different. However, in the optical element of the present invention, the materials of the first transparent substrate 11 and the second transparent substrate 12 may be different, or they may be approximately the same or completely the same.
[0032] (Coating layer) The optical element of the present invention has a first coating layer 101 and a second coating layer 102. The first coating layer 101 is on a first transparent substrate 11 and is in contact with an adhesive layer 13. However, the first coating layer 101 and the first transparent substrate 11 may be in contact, or they may not be in contact, with another layer in between. The second coating layer 102 is on a second transparent substrate 12 and is in contact with an adhesive layer 13. However, the second coating layer 102 and the second transparent substrate 12 may be in contact, or they may not be in contact, with another layer in between. The material of the first coating layer 101 and the material of the second coating layer 102 are preferably about the same.
[0033] The components of the first coating layer 101 and the second coating layer 102 are not particularly limited and include all substances, compositions, compounds, elements, etc. that constitute the material. The components are bonded to each other in the material by metallic bonds, covalent bonds, ionic bonds, hydrogen bonds, van der Waals forces, etc. Examples of preferred components of the first coating layer 101 and the second coating layer 102 include SiO2, Al2O3, Ta2O5, ZrO2, Y2O3, Na2O, CaO, MgO, Nb2O 5、 Examples include metal or metalloid oxides or fluorides such as MgF2, resins such as acrylic resin, polycarbonate resin, polystyrene resin, allyl diglycol carbonate resin, polyurethane resin, and polythiourethane resin, and additives added for purposes such as controlling surface reflectivity or providing optical modification. The main components of the first coating layer 101 and the second coating layer 102 are similar to those of the main components, but additives often do not become the main components because their content is low.
[0034] If the first coating layer and the second coating layer each have only one main component, then their main components are the same. Let this main component be component 1', and if the first coating layer has component 1', then X 1’A In mass%, the second coating layer contains component 1' of X 1’B If it has a mass of %, then 8 / 10 ≤ X 1’A / X 1’B It satisfies ≤ 10 / 8. When there is one main component, the proportion of the main component in the first coating layer and the second coating layer is both 72% by mass or more, that is, 72 ≤ X 1’A and 72 ≤ X 1’B is preferable.
[0035] When the first coating layer and the second coating layer each have two main components, at least one of their main components coincides. Preferably, both have two main components, and the two coincide. Let the main components be component 1' and component 2'. When the first coating layer has component 1' at X 1’A % by mass and component 2' at X 2’A % by mass, and the second coating layer has component 1' at X 1’B % by mass and component 2' at X 2’B % by mass, 8 / 10 ≤ X 1’A / X 1’B ≤ 10 / 8, 8 / 10 ≤ X 2’A / X 2’B ≤ 10 / 8 satisfies any one of them. Preferably, the sum of the proportions of the main component in the first coating layer and the second coating layer is both 72% by mass or more, that is, 72 ≤ X 1’A +X 2’ ≤ 100 A and 72 ≤ X 1’B +X 2’B ≤ 100 is preferable.
[0036] When the first coating layer and the second coating layer each have three main components, at least one of their main components coincides. Preferably, both have three main components, and the three coincide. Let the main components be component 1', component 2', and component 3'. When the first coating layer has component 1' at X 1’A % by mass, component 2' at X 2’A % by mass, and component 3' at X 3’A % by mass, and the second coating layer has component 1' at X 1’B % by mass, component 2' at X 2’B % by mass, and component 3' at X 3’B % by mass, 8 / 10 ≤ X 1’A / X1’B ≤10 / 8, 8 / 10 ≤X 2’A / X 2’B ≤10 / 8, 8 / 10 ≤X 3’A / X 3’B Satisfying one of the following conditions: ≤ 10 / 8. Preferably, the sum of the proportions of the main component in the first coating layer and the second coating layer is 72% by mass or more, i.e., 72 ≤ X 1’A +X 2’A +X 3’A ≤ 100 and 72 ≤ X 1’B +X 2’B +X 3’B It is preferable that the value is ≤100.
[0037] When the first coating layer and the second coating layer each have four main components, at least one of these main components is the same. Preferably, both have four main components, and these four components are the same, and these main components are designated as component 1', component 2', component 3', and component 4', and the first coating layer has component 1' as X 1’A Mass %, component 2' is X 2’A Mass%, component 3' is X 3’A Mass%, component 4' is X 4’A It has a mass of %, and the second coating layer has component 1' X 1’B Mass %, component 2' is X 2’B Mass%, component 3' is X 3’B Mass%, component 4' is X 4’B If it has a mass of %, then 8 / 10 ≤ X 1’A / X 1’B ≤10 / 8, 8 / 10 ≤X 2’A / X 2’B ≤10 / 8, 8 / 10 ≤X 3’A / X 3’B ≤10 / 8, 8 / 10 ≤X 4’A / X 4’B Satisfying one of the following conditions: ≤ 10 / 8.
[0038] The main components of the first coating layer 101 and the second coating layer 102 are not particularly limited, but preferred examples include SiO2, Al2O3, and Ta2O5.
[0039] The first coating layer 101 and the second coating layer 102 are preferably each 5 nm or thicker. If the coating layer is as thin as a monolayer, it will not be sufficiently effective in reducing the distortion of the optical element. A separate coating layer may be provided between the first coating layer 101 and the first transparent substrate 11. That is, the first transparent substrate 11 may include multiple coating layers. A separate coating layer may be provided between the second coating layer 102 and the second transparent substrate 12. That is, the second transparent substrate 12 may include multiple coating layers.
[0040] (adhesive layer) The adhesive layer 13 contains the cured product of the adhesive 130 and is a layer that adheres the first transparent substrate 11 and the second transparent substrate 12. Since the optical element is suitably used as a lens, its internal transmittance is preferably 99% or higher.
[0041] The adhesive 130 forming the adhesive layer 13 preferably contains a curable resin, and more preferably contains a photocurable resin and a photopolymerization initiator. The type of photocurable resin is not particularly limited, but resins with high transmittance when cured, such as acrylic resins, urethane acrylic resins, silicone acrylic resins, and epoxy resins, are preferred. The photopolymerization initiator absorbs light and generates radicals, and these radicals polymerize the monomers or oligomers of the photocurable resin.
[0042] The thickness of the adhesive layer 13 is preferably 0.1 μm or more and 100 μm or less, from the viewpoint of achieving both adhesive strength and optical performance. The thickness of the adhesive layer 13 is the average thickness between the first transparent substrate 11 containing the first coating layer 101 and the second transparent substrate 12 containing the second coating layer 102. If the thickness of the adhesive layer 13 is less than 0.1 μm, the adhesive layer 13 will not be able to absorb the strain caused by the difference in the coefficient of linear expansion between the first transparent substrate 11 and the second transparent substrate 12 when the temperature changes significantly, which may lead to a deterioration in optical performance. On the other hand, if the thickness of the adhesive layer 13 exceeds 100 μm, the adhesive strength may be insufficient. Furthermore, the difference between the maximum and minimum thickness of the adhesive layer 13 is preferably 10 μm or less. If the difference between the maximum and minimum thickness of the adhesive layer 13 exceeds 10 μm, the distribution of the elastic modulus in the adhesive layer 13 becomes large, which affects the optical properties. More preferably, the difference between the maximum and minimum thickness of the adhesive layer 13 is 5 μm or less.
[0043] The elastic modulus of the adhesive layer 13 is preferably 0.1 GPa or more and 1.0 GPa or less. If the elastic modulus of the adhesive layer 13 is less than 0.1 GPa, the centers of the first transparent substrate 11 and the second transparent substrate 12 may be misaligned, and the desired optical performance may not be obtained. On the other hand, if the elastic modulus of the adhesive layer 13 exceeds 1.0 GPa, the adhesive layer 13 becomes brittle, and the mechanical strength of the optical element may decrease.
[0044] (Manufacturing method) The method for manufacturing the optical element of the present invention will now be described. The terms, optical element, transparent substrate, coating layer, and adhesive layer are defined as described above.
[0045] A first coating layer 101 is formed on one surface of the first transparent substrate 11, and a second coating layer 102 is formed on one surface of the second transparent substrate 12. The coating layer can be formed using physical deposition methods such as vacuum deposition or sputtering, or chemical deposition methods using resins or organic-inorganic composite materials. When forming the coating layer, it is preferable not to cause distortion of the transparent substrate. Particularly preferable, the coating layer is formed by vacuum deposition or sputtering.
[0046] The first transparent substrate 11 and the second transparent substrate 12 may be further pre-treated to improve adhesion with the adhesive layer 13. Preferred pre-treatments include ozone treatment and silane coupling treatment. Ozone treatment makes the adhesive 130 easier to wet and spread. Silane coupling treatment is performed by treating with a silane coupling agent. Examples of silane coupling agents include hexamethyldisilazane, methyltrimethoxysilane, trimethylchlorosilane, and triethylchlorosilane. Furthermore, a further inorganic oxide film may be formed to improve adhesion between the first transparent substrate 11 and the first coating layer 101. Furthermore, a further inorganic oxide film may be formed to improve adhesion between the second transparent substrate 12 and the second coating layer 102.
[0047] Next, an adhesive 130 is filled between the first coating layer 101 and the second coating layer 102 to form an adhesive layer 13, and then cured. The method of filling and curing the adhesive 130 is not particularly limited, but a specific example will be explained using Figure 4.
[0048] First, the filling process of filling the space between the first coating layer 101 and the second coating layer 102 with adhesive 130 will be described. An example of the filling process is shown in Figures 4(A) to 4(D). Specifically, the second transparent substrate 12, which is a concave lens, is placed on a base 21 positioned with respect to a virtual central axis 22, with the second coating layer 102 facing upwards (Figure 4(A)). Uncured adhesive 130 is then placed (Figure 4(B)). It is preferable to place the adhesive 130 near the center of the concave lens side, rather than on the convex lens side. This is because if the adhesive 130 is placed on the convex lens, the curvature of the lens may cause the adhesive 130 to move while it is still uncured, making it difficult to bond evenly. After the adhesive 130 is placed, the first transparent substrate 11, which is a convex lens, is brought closer using a jig (not shown) to spread the adhesive 130 (Figure 4(C)). The thickness of the adhesive 130 can be controlled by the jig to a predetermined value. When spreading the adhesive 130, the weight of the transparent substrate, which is a convex lens, may be used to spread the adhesive 130, or force may be applied to spread it evenly within the plane between the transparent substrates. The substrate may also be rotated when spreading the adhesive 130. Furthermore, the positions of the lenses to be bonded are aligned and the adhesive 130 is spread to a specified film thickness (Figure 4(D)). In conjunction with or after the above filling process, a centering process is performed to align the lens position and optical axis as needed (not shown). In the centering process, for example, first, the centering reference is observed through the lens to be bonded using a detection means such as a camera. Subsequently, the first transparent substrate 11 is aligned with the virtual central axis 22 using a centering means such as a stage, with the second transparent substrate 12 positioned relative to the virtual central axis 22 as a reference.
[0049] After the filling process, a curing process is performed to cure the adhesive 130 (Figure 4(E)). The curing process is appropriately selected depending on the type of adhesive 130. If the adhesive 130 is a photocurable resin, it can be cured by irradiating it with light. In Figure 4(E), ultraviolet light is irradiated from the side of the first transparent substrate 11 by the light source 25 to cure the adhesive 130 and form the adhesive layer 13.
[0050] (Imaging device) Figure 5 shows the configuration of a single-lens reflex digital camera, which is an example of a preferred embodiment of the imaging device of the present invention. In Figure 5, the camera body 602 and the lens barrel 601, which is an optical device, are coupled together, and the lens barrel 601 is a so-called interchangeable lens that can be attached to and detached from the camera body 602.
[0051] Light from the subject passes through an optical system consisting of multiple lenses 603, 605, etc., arranged on the optical axis of the imaging optical system within the housing 620 of the lens barrel 601, and is received by the image sensor 610. The optical element of the present invention can be used, for example, as a lens 605.
[0052] Here, the lens 605 is supported by the inner barrel 604 inside the housing and is movably supported relative to the outer barrel of the lens barrel 601 for focusing and zooming.
[0053] During the observation period before shooting, light from the subject is reflected by the main mirror 607 inside the camera body housing 621, passes through the prism 611, and the image is projected onto the photographer through the viewfinder lens 612. The main mirror 607 is, for example, a half-mirror, and the light that passes through the main mirror is reflected by the sub-mirror 608 towards the AF (autofocus) unit 613, and this reflected light is used, for example, for distance measurement. The main mirror 607 is also attached and supported by the main mirror holder 640 by adhesive or other means. During shooting, the main mirror 607 and sub-mirror 608 are moved out of the optical path via a drive mechanism (not shown), the shutter 609 is opened, and the image of the photographic light incident from the lens barrel 601 is projected onto the image sensor 610. The aperture 606 is configured to change the brightness and depth of field during shooting by changing the aperture area. [Examples]
[0054] The present invention will be described in more detail below with reference to examples and comparative examples.
[0055] <Evaluation Method> (Surface shape measurement) The surface shape of the fabricated cemented lenses was evaluated using an interferometer before and after bonding. Specifically, the number of ass fibers in the lens before bonding and the fabricated cemented lens were measured. Lenses with an increase or decrease of one or more ass fibers compared to the lens before bonding were evaluated as defective, while lenses with no increase or decrease of less than one ass fiber compared to the lens before bonding were evaluated as good.
[0056] [Example 1] A concave lens with a diameter of 67 mm and a central wall thickness of 1.3 mm (Ohara S-LAH55) was prepared as the first transparent substrate, and a convex lens with a diameter of 65 mm and a central wall thickness of 5 mm (Ohara S-FPL51) was prepared as the second transparent substrate. A 100 nm thick silica coating layer was deposited on the surfaces of both the first and second transparent substrates that come into contact with the adhesive. Next, an adhesive (World Lock 5517, Kyoritsu Chemical Industry Co., Ltd.) was applied to bond the first transparent substrate and the second transparent substrate in an amount that resulted in an adhesive layer thickness of 20 μm. The bonded lens was then cured using a 365 nm wavelength LED light source to fabricate a bonded lens. The fabricated bonded lens was then evaluated.
[0057] [Example 2] A bonded lens was fabricated and evaluated in the same manner as in Example 1, except that alumina was deposited as a coating layer on the surfaces of the first and second transparent substrates that come into contact with the adhesive.
[0058] [Example 3] A bonded lens was fabricated and evaluated in the same manner as in Example 2, except that a mixture consisting of Al2O3 / Ta2O5=90 / 10 was deposited as a coating layer on the surface of the first transparent substrate that contacts the adhesive, instead of alumina.
[0059] [Example 4] A bonded lens was fabricated and evaluated in the same manner as in Example 2, except that a mixture consisting of Al2O3 / Ta2O5=80 / 20 was deposited as a coating layer on the surface of the first transparent substrate that contacts the adhesive, instead of alumina.
[0060] [Comparative Example 1] A bonded lens was fabricated and evaluated in the same manner as in Example 1, except that no coating layer was applied to the first and second transparent substrates.
[0061] [Comparative Example 2] A bonded lens was fabricated and evaluated in the same manner as in Comparative Example 1, except that alumina was deposited as a coating layer on the surface of the first transparent substrate that was in contact with the adhesive.
[0062] [Comparative Example 3] A bonded lens was fabricated and evaluated in the same manner as in Comparative Example 1, except that alumina was deposited as a coating layer on the surface of the second transparent substrate that was in contact with the adhesive. The results are shown in Table 1. From these results, it was found that when the first transparent substrate and the second transparent substrate have coating layers made of roughly the same material, a good bonded lens with minimal surface shape change could be obtained.
[0063] [Comparative Example 4] A bonded lens was fabricated and evaluated in the same manner as in Comparative Example 3, except that silica was deposited as a coating layer on the surface of the first transparent substrate that was in contact with the adhesive.
[0064] [Table 1] [Industrial applicability]
[0065] Distortion that occurs when bonding lenses is a common problem in the manufacturing of optical elements, and the present invention has high potential for industrial application. [Explanation of Symbols]
[0066] 10 optical elements 11 1st transparent base material 12 Second transparent base material 101 First coating layer 102 Second coating layer 13 adhesive layer 130 adhesive L incident light L CRefracted light (C-line) L F Refracted light (F-line) f C Focus (C line) f F Focus (F line) 21 bases 25 light sources
Claims
1. An optical element including a first transparent substrate, a second transparent substrate, and an adhesive layer provided between the first transparent substrate and the second transparent substrate, wherein an outer diameter D and a thickness t satisfy t / D<0.02, moreover, a first coating layer on the first transparent substrate and in contact with the adhesive layer; a second coating layer on the second transparent substrate and in contact with the adhesive layer; the main component of the material of the first coating layer is the same as the main component of the material of the second coating layer; The ratio of the main component of the material of the first coating layer is X A The proportion of the main component of the material of the second coating layer is X% by mass. B In terms of mass%, 8 / 10≦X A / X B An optical element characterized in that ≦10 / 8 holds.
2. The first coating layer and the second coating layer are mainly composed of SiO 2 and Al 2 O 3 2. The optical element according to claim 1, comprising at least one of the following:
3. 3. The optical element according to claim 1, wherein the first coating layer is in contact with the first transparent substrate, and the second coating layer is in contact with the second transparent substrate.
4. 4. The optical element according to claim 3, wherein the first coating layer and the second coating layer each have a thickness of 5 nm or more.
5. 5. The optical element according to claim 1, wherein the adhesive layer has a thickness of 0.1 μm or more and 100 μm or less.
6. 6. The optical element according to claim 5, wherein the difference between the maximum thickness of the adhesive layer and the minimum thickness of the adhesive layer is 5 [mu]m or less.
7. 7. The optical element according to claim 1, wherein the adhesive layer has a modulus of elasticity of 0.1 GPa or more and 1.0 GPa or less.
8. A method for manufacturing an optical element including a first transparent substrate, a second transparent substrate, and an adhesive layer, wherein an outer diameter D and a thickness t satisfy t / D<0.02, providing a first coating layer on either side of the first transparent substrate; providing a second coating layer on either side of the second transparent substrate; a filling step of filling an adhesive between the first coating layer and the second coating layer; and a curing step of curing the adhesive; the main component of the material of the first coating layer is the same as the main component of the material of the second coating layer; The ratio of the main component of the material of the first coating layer is X A The proportion of the main component of the material of the second coating layer is X% by mass. B In terms of mass%, 8 / 10≦X A / X B ≦10 / 8.
9. 9. The method for manufacturing an optical element according to claim 8, wherein the adhesive is a photocurable resin.
10. 10. The method for manufacturing an optical element according to claim 8, wherein the first coating layer is provided so as to be in contact with the first transparent substrate, and the second coating layer is provided so as to be in contact with the second transparent substrate.
11. the second transparent substrate is a concave lens; The method for manufacturing an optical element according to claim 10 , wherein the adhesive is placed on the second coating layer.
12. 1. An optical instrument comprising: a housing; and an optical system having at least one lens disposed within the housing, An optical instrument, wherein at least one of the lenses is the optical element according to any one of claims 1 to 7.
13. An imaging device including a housing, an optical system having at least one lens disposed in the housing, and an imaging element that receives light that has passed through the optical system, An imaging device, wherein at least one of the lenses is the optical element according to claim 1 .