Glass fiber for reinforcement, chopped strand, fiber sheet, and rod

JP2023095934A5Inactive Publication Date: 2024-11-12NIPPON SHEET GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023074907
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-15
Filing Date
2023-04-28
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There is a need for new reinforcing glass fibers suitable for reinforcing various products, particularly concrete and rubber products, with improved mechanical properties and chemical durability.

Method used

The composition of the glass fibers is optimized by adjusting the content of SiO2, Al2O3, and Fe2O3 to 12 to 25% by mass, along with optional CaO, to enhance elastic modulus, alkali resistance, and acid resistance, while maintaining spinnability and reducing production costs.

Benefits of technology

The new glass fibers exhibit high elastic modulus, excellent chemical durability, and improved alkali and acid resistance, making them suitable for reinforcing a wide range of products including concrete, rubber, and plastic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a novel glass fiber for reinforcement suitable for reinforcing various products.SOLUTION: A glass fiber for reinforcement according to the invention includes SiO2, Al2O3, and Fe2O3. A content percentage of Fe2O3 is 12-25 mass% in the glass fiber for reinforcement. The glass fiber for reinforcement is used for reinforcing concrete products, rubber products, and plastic products.SELECTED DRAWING: Figure 3A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to reinforcing glass fibers, chopped strands, fiber sheets and rods. [Background technology]

[0002] Glass fibers are used as reinforcing materials for products that are subject to stress. Glass fibers are processed into an appropriate form depending on the intended use. As an example, rubber reinforcing cords having strands formed by bundling glass fibers are used to reinforce rubber products. Rubber reinforcing cords are embedded in rubber products such as rubber belts and tires to suppress the elongation and strength reduction of the rubber products, thereby contributing to improving the dimensional stability and extending the fatigue life of the rubber products. Patent Document 1 discloses glass fibers used in rubber reinforcing cords. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2006 / 057405 Summary of the Invention [Problem to be solved by the invention]

[0004] There is a need for new reinforcing glass fibers suitable for reinforcing various products, such as concrete products.

[0005] Therefore, an object of the present invention is to provide a new reinforcing glass fiber suitable for reinforcing various products. [Means for solving the problem]

[0006] As a result of extensive research, the present inventors have newly discovered that the properties of reinforcing glass fibers can be improved by appropriately adjusting the content of Fe2O3 among the various components contained in the reinforcing glass fibers, and have thus completed the present invention.

[0007] The present invention provides containing SiO2, Al2O3 and Fe2O3, A reinforcing glass fiber having an Fe2O3 content of 12 to 25 mass % is provided.

[0008] Furthermore, the present invention provides Chopped strands are provided which contain the reinforcing glass fibers described above.

[0009] Furthermore, the present invention provides A fiber sheet is provided which contains the reinforcing glass fibers described above.

[0010] Furthermore, the present invention provides A rod is provided that includes the reinforcing glass fibers described above. [Effects of the Invention]

[0011] According to the present invention, a new reinforcing glass fiber suitable for reinforcing various products can be provided. [Brief explanation of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing an example of a spinning apparatus for producing reinforcing glass fibers. [Figure 2] FIG. 1 is a diagram showing an example of an apparatus for producing chopped strands. [Figure 3A] FIG. 1 is a perspective view showing an example of a concrete product. [Figure 3B] FIG. 3B is an enlarged cross-sectional view of the concrete product shown in FIG. 3A. [Figure 4] FIG. 10 is a diagram showing another example of a concrete product. [Figure 5] 1 is a diagram showing an example of the structure of a rubber belt including a rubber reinforcing cord. DETAILED DESCRIPTION OF THE INVENTION

[0013] The present invention will be described in detail below, but the following description is not intended to limit the present invention to a specific embodiment.

[0014] [Reinforcing glass fiber] The reinforcing glass fiber of this embodiment contains SiO2, Al2O3, and Fe2O3, and may further contain CaO. In the reinforcing glass fiber of this embodiment, the content of Fe2O3 is 12 to 25 mass%.

[0015] In this specification, SiO2 is sometimes referred to as the S component, and the SiO2 content is sometimes expressed as [S]. Al2O3 is sometimes referred to as the A component, and the Al2O3 content is sometimes expressed as [A]. Fe2O3 is sometimes referred to as the F component, and the Fe2O3 content is sometimes expressed as [F]. CaO is sometimes referred to as the C component, and the CaO content is sometimes expressed as [C].

[0016] SiO2 is an essential main component that forms the skeleton of glass. It also adjusts the devitrification temperature and viscosity of glass, and is a component that improves chemical durability, particularly acid resistance. If the SiO2 content is too low, acid resistance may decrease. On the other hand, if the SiO2 content is too high, the elastic modulus (e.g., Young's modulus) may decrease. The SiO2 content is, for example, 40 mass% or more, and may be 43 mass% or more, 45 mass% or more, 48 mass% or more, 50 mass% or more, or even 53 mass% or more. The SiO2 content is, for example, 68 mass% or less, 65 mass% or less, 63 mass% or less, or even 60 mass% or less. The SiO2 content is preferably 50 to 63 mass%, and may be 40 to 50 mass% in some cases.

[0017] Al2O3 is a component that forms the skeleton of glass and also adjusts the devitrification temperature and viscosity of glass. It is also a component that improves chemical durability, particularly water resistance. On the other hand, Al2O3 is a component that deteriorates acid resistance, among other chemical durability. If the Al2O3 content is too low, water resistance may decrease. On the other hand, if the Al2O3 content is too high, acid resistance and alkali resistance may decrease. The Al2O3 content is, for example, 2 mass% or more, and may be 5 mass% or more, 7 mass% or more, or even 10 mass% or more. The Al2O3 content is, for example, 20 mass% or less, or may be 15 mass% or less. The Al2O3 content is preferably 5 to 15 mass%.

[0018] In the reinforcing glass fiber, the total content of SiO2 and Al2O3 is, for example, 40 to 70 mass%. If the total of [S] and [A] is less than 40 mass% or if the total of [S] and [A] is more than 70 mass%, the melting temperature of the raw material for the reinforcing glass fiber may be too high, the viscosity of the molten raw material may be too high, or the viscosity of the molten raw material may be too low, which may result in a decrease in the melt spinnability of the raw material. The total content of SiO2 and Al2O3 is preferably 50 mass% or more, more preferably 55 mass% or more. The total content of SiO2 and Al2O3 may be 65 mass% or less.

[0019] In the reinforcing glass fiber, the ratio of the Al2O3 content to the total content of SiO2 and Al2O3 ([A] / ([A]+[S])) is, for example, 0.10 to 0.40, and preferably 0.15 to 0.40. If [A] / ([A]+[S]) is less than 0.10 or if [A] / ([A]+[S]) is more than 0.40, the melt spinnability of the raw material for the reinforcing glass fiber may decrease. [A] / ([A]+[S]) is preferably 0.35 or less, more preferably 0.30 or less, even more preferably 0.25 or less, and particularly preferably 0.20 or less.

[0020] In the reinforcing glass fiber of this embodiment, Fe2O3 plays an important role. That is, when Fe2O3 is contained in the reinforcing glass fiber within an appropriate range, the acid resistance and alkali resistance of the reinforcing glass fiber are improved. Furthermore, since Fe2O3 is present in large amounts as a raw material, the cost of using the raw material can be reduced. Furthermore, Fe2O3 can also improve the elastic modulus of the reinforcing glass fiber. On the other hand, if the reinforcing glass fiber contains excessive Fe2O3, the acid resistance decreases and devitrification may occur. In the reinforcing glass fiber, the Fe2O3 content is 12 to 25 mass%. If the Fe2O3 content exceeds 25 mass%, the viscosity of the molten raw material of the reinforcing glass fiber may be too low, making it difficult to produce the reinforcing glass fiber. Furthermore, the acid resistance may also decrease. The Fe2O3 content is preferably 15 mass% or more, and may be 17 mass% or more. The Fe2O3 content is preferably 23 mass% or less, and more preferably 20 mass% or less. The content of Fe2O3 is preferably 15 to 25 mass %, more preferably 15 to 23 mass %, and in some cases may be 20 to 25 mass %.

[0021] In conventional glass fibers, the Fe2O3 content is often set to 1% by mass or less. In the reinforcing glass fiber of this embodiment, by adjusting the Fe2O3 content to 12 to 25% by mass, it is possible to reduce batch costs during production of the reinforcing glass fiber, improve acid resistance and alkali resistance, and obtain a high elastic modulus. Furthermore, if the Fe2O3 content is high, the reinforcing glass fiber may become discolored. The reinforcing glass fiber of this embodiment is suitable for applications where discoloration is not an issue, particularly for reinforcing concrete products and rubber products.

[0022] CaO is a component that improves alkali resistance, particularly cement resistance. CaO also tends to improve the elastic modulus of reinforcing glass fibers. The CaO content in reinforcing glass fibers is, for example, 5 to 30% by mass. If the CaO content is less than 5% by mass, the melting start temperature of the raw material for the reinforcing glass fiber is high, which is undesirable from the viewpoint of energy saving, and alkali resistance also tends to be poor. If the CaO content exceeds 30% by mass, the viscosity of the molten raw material for the reinforcing glass fiber is too low, which may make it difficult to produce the reinforcing glass fiber. The CaO content is preferably 10% by mass or more, and may be 13% by mass or more, 15% by mass or more, 17% by mass or more, or 20% by mass or more. The CaO content may be 25% by mass or less. The CaO content may be 18 to 30% by mass, and in some cases, may be 15 to 25% by mass, or 20 to 30% by mass.

[0023] From the viewpoint of improving the elastic modulus and alkali resistance of the reinforcing glass fiber, it is preferable that the CaO content in the reinforcing glass fiber is 18 to 30 mass% and the Fe2O3 content is 15 to 25 mass%. From the same viewpoint, the CaO content in the reinforcing glass fiber may be 15 to 25 mass% and the Fe2O3 content may be 15 to 23 mass%. In the reinforcing glass fiber, the total content of CaO and Fe2O3 may be, for example, 30 mass% or more, 31 mass% or more, 33 mass% or more, or even 35 mass% or more. The total content of CaO and Fe2O3 may be, for example, 60 mass% or less, or 50 mass% or less.

[0024] In the reinforcing glass fiber of this embodiment, the Fe2O3 content is appropriately adjusted, and, if necessary, the total content of SiO2 and Al2O3, the mass ratio calculated by Al2O3 / (SiO2+Al2O3), the CaO content, etc. are also appropriately adjusted. As a result, the reinforcing glass fiber tends to have better mechanical properties such as elastic modulus and chemical durability such as alkali resistance and acid resistance than conventional reinforcing glass fibers.

[0025] The reinforcing glass fiber of this embodiment may further contain components other than the above-mentioned components. For example, the reinforcing glass fiber may contain trace components derived from impurities in the raw materials, manufacturing equipment, etc. Examples of trace components include MgO, Na2O, KO, TiO2, and CrO2. The content of the trace components in the reinforcing glass fiber is, for example, less than 10% by mass, and may be less than 5% by mass.

[0026] The method for producing the reinforcing glass fiber is not particularly limited and includes, for example, the steps of forming a melt from raw materials and spinning the melt into reinforcing glass fibers. The raw material for the reinforcing glass fiber may be a mixture of each of the individual compounds of SiO, AlO, FeO, and CaO, or, from the viewpoint of cost, may be a mixture containing at least one selected from the group consisting of a silica source rich in SiO, an alumina source rich in AlO, a silica-alumina source rich in both SiO and AlO, an iron oxide source rich in FeO, and a calcium oxide source rich in CaO. The composition of this mixture may be adjusted by mixing a high-purity raw material with the raw material such as the silica source.

[0027] The silica source is not particularly limited, and examples thereof include amorphous silica, silica sand, fumed silica, and volcanic ash.

[0028] The alumina source is not particularly limited, and examples thereof include alumina and other ores such as mullite.

[0029] The silica-alumina source is not particularly limited, and examples thereof include kaolinite, montmorillonite, feldspar, and zeolite.

[0030] The iron oxide source is not particularly limited, and examples thereof include iron oxide, iron hydroxide, and iron ore.

[0031] The calcium oxide source is not particularly limited, and examples thereof include calcium carbonate as well as other minerals such as calcite and dolomite.

[0032] In addition to the above examples, waste from thermal power plants and waste from metal refining can also be used as one of the silica source, alumina source, silica-alumina source, iron oxide source, and calcium oxide source.

[0033] Examples of thermal power plant waste include fly ash and clinker ash. Fly ash and clinker ash are rich in SiO2 and Al2O3 and are therefore suitable as silica-alumina sources. However, fly ash and clinker ash tend to have low Fe2O3 contents, making it difficult to produce the reinforcing glass fiber of this embodiment using only these materials. When using fly ash or clinker ash, blending it with an appropriate amount of iron oxide source allows the reinforcing glass fiber of this embodiment to be produced at low cost. Coal gasification slag (CGS), which is produced as a waste product from integrated coal gasification combined cycle (IGCC), has almost the same chemical composition as fly ash. Therefore, coal gasification slag can also be used as a silica-alumina source. Coal gasification slag has the advantage of being granular and therefore easy to handle.

[0034] Metal refining waste includes steel slag and copper slag. Steel slag has a high CaO content and can be used as a calcium oxide source. Steel slag includes blast furnace slag, converter slag, and reduced slag. Copper slag has a high Fe2O3 content and can be used as an iron oxide source.

[0035] As described above, fly ash, clinker ash, or coal gasification slag can be used as the silica-alumina source. Copper slag can be used as the iron oxide source. Steel slag can be used as the calcium oxide source. In other words, industrial waste can be used as the silica-alumina source, iron oxide source, and calcium oxide source.

[0036] In addition to the above examples, volcanic rocks such as basalt and andesite can also be used as silica-alumina sources.

[0037] Tables 1 to 3 below show specific examples of the compositions of the silica-alumina source, iron oxide source, and calcium oxide source described above. FA(1) to FA(9) and FA(12) in Tables 1 and 2 are examples of fly ash compositions emitted from thermal power plants in Japan. FA(10) in Table 2 is an example of copper slag composition produced at a copper refinery in Japan. FA(11) is an example of coal gasification slag composition emitted from a coal gasification combined cycle power plant in Japan. FA(13) is an example of blast furnace slag composition produced at a steelworks in Japan. FA(14) is an example of reduced slag composition produced at a steelworks in Japan. BA(1) and BA(2) in Table 3 are examples of compositions of basalt-based rocks (volcanic rocks) with a uniquely high iron oxide content collected in Akita and Fukui prefectures. The compositions in Tables 1 to 3 are values ​​measured by X-ray fluorescence analysis.

[0038] [Table 1]

[0039] [Table 2]

[0040] [Table 3]

[0041] In the production method of this embodiment, after the raw materials are melted to form a melt, the melt may be subjected to spinning without solidifying. This method is called a direct melt method. In addition, in the production method of this embodiment, the step of forming a melt from the raw materials may include a step of solidifying the molten raw materials to obtain a solidified body, and a step of melting the solidified body to form a melt. Since the solidified body that serves as the intermediate raw material is called a marble, this method is known as a marble melt method.

[0042] The raw material and the solidified body are melted in, for example, a melting furnace. In the manufacturing method of this embodiment, in the step of spinning the reinforcing glass fibers from the molten material, the reinforcing glass fibers may be continuously manufactured using a bushing attached to the bottom of the melting furnace.

[0043] FIG. 1 shows an example of a spinning apparatus for producing reinforcing glass fibers. As shown in FIG. 1, a molten material melted in a melting furnace is drawn out from a bushing 10 having a number of (e.g., 2,400) nozzles at the bottom to form a number of reinforcing glass fibers 11. Cooling water may be sprayed onto the reinforcing glass fibers 11, and then a binder (sizing agent) 14 may be applied by an application roller 13 of a binder applicator 12. The number of reinforcing glass fibers 11 to which the binder 14 has been applied may be bundled by a reinforcing pad 15 into strands 16, each consisting of, for example, approximately 800 reinforcing glass fibers 11. Each strand 16 may be traversed by a traverse finger 17 and wound around a cylindrical tube 19 fitted to a collet 18. When the cylindrical tube 19 around which the strand 16 has been wound is removed from the collet 18, a cake (strand wound body) 20 is obtained. Details of the strands will be described later.

[0044] The reinforcing glass fibers are, for example, long fibers. In some cases, the reinforcing glass fibers may be short fibers.

[0045] The diameter of the reinforcing glass fiber can be 15 μm or less, or even 10 μm or less. In a reinforcing cord having strands formed by bundling a large number of reinforcing glass fibers, the use of reinforcing glass fibers with a smaller diameter makes the strands relatively flexible and easier to bend. Therefore, reinforcing glass fibers with a smaller diameter can improve the flexural strength of the cord. Furthermore, the cross-sectional area of ​​the cord can be reduced when compared with cords with the same strength. The lower limit of the diameter of the reinforcing glass fiber is not particularly limited, but may be, for example, 2 μm or 3 μm. However, the reinforcing glass fiber may be thicker, with a diameter exceeding 15 μm, or even reaching 20 μm or more.

[0046] The variation in diameter of the reinforcing glass fiber can be ±3 μm or less, and even ±2 μm or less. Reinforcing glass fibers with large variations and inconsistent diameters have a wavy outer shape, which is prone to stress and reduces flexural strength. Therefore, it is preferable for the diameter of the reinforcing glass fiber to be small. Here, the variation in diameter of the reinforcing glass fiber is determined by measuring the diameter of the reinforcing glass fiber at 50 random locations and calculating the difference between the simple average and the maximum value (indicated by +) and the difference between the simple average and the minimum value (indicated by -). The diameter of the reinforcing glass fiber can be determined by the above simple average.

[0047] The cross section of the reinforcing glass fiber may be, for example, approximately circular, and the circularity may be 0.7 or more. Here, the circularity is calculated by the following formula: (4πS / L) where S is the cross-sectional area of ​​the reinforcing glass fiber and L is the circumferential length of the cross section. 2 ) where a cross section with this value of 1 is a perfect circle. Circularity can be measured using a scanning electron microscope. In this case, it is convenient to use image processing software such as Image J by Wayne Rasband.

[0048] The density of the reinforcing glass fiber is not particularly limited, and is, for example, 2.4 to 2.8 g / cm 3 is.

[0049] The reinforcing glass fiber of this embodiment has high amorphousness, and therefore hardly experiences a decrease in strength due to peeling at the interface between the crystalline phase and the amorphous phase, resulting in high strength. The amorphization degree, which is a measure of amorphism in the reinforcing glass fiber, is usually 90% or more, and may be 95% or more, depending on the composition. The amorphization degree can be calculated from an X-ray diffraction (XRD) spectrum using the following formula (1): Amorphousity (%)=[Ia / (Ic+Ia)]×100 (1) (In formula (1), Ic is the sum of the integral values ​​of the scattering intensity of the crystalline peak when X-ray diffraction analysis is performed on the reinforcing glass fiber, and Ia is the sum of the integral values ​​of the scattering intensity of the amorphous halo.)

[0050] The reinforcing glass fiber is, for example, substantially composed of only an amorphous phase. The reinforcing glass fiber being substantially composed of only an amorphous phase means that only an amorphous halo is observed in the X-ray diffraction spectrum, and no peaks of a crystalline phase are observed.

[0051] The reinforcing glass fiber of this embodiment has, for example, excellent mechanical properties. As an example, the elastic modulus (Young's modulus) E of the reinforcing glass fiber is, for example, 80 MPa or more, preferably 85 MPa or more, and more preferably 90 MPa or more. Reinforcing glass fibers having an elastic modulus of 85 MPa or more, particularly 90 MPa or more, are particularly suitable for reinforcing rubber products and plastic products. The upper limit of the elastic modulus E of the reinforcing glass fiber is not particularly limited, and may be, for example, 100 MPa. The elastic modulus E (MPa) of the reinforcing glass fiber can be determined by measuring the longitudinal wave velocity v of elastic waves propagating through a sample using a conventional ultrasonic method. l (m / s) and shear wave velocity v t (m / s) and the density ρ (kg / m 3 ) can be calculated by the following formula: A specific example of a sample used in the ultrasonic method or Archimedes method is a plate-shaped sample glass having the same composition as the reinforcing glass fiber. E=10 -6 ρ v t 2 ·(v l 2 -4 / 3·v t 2 ) / (v l 2 -v t 2 )

[0052] The tensile strength of the reinforcing glass fiber is, for example, 2500 N / mm 2 or more, preferably 3000N / mm 2 More preferably, it is 3500N / mm 2 More preferably, it is 4000N / mm 2 More preferably, it is 4500N / mm 2and more preferably 4900N / mm 2 The upper limit of the tensile strength of the reinforcing glass fiber is not particularly limited, and may be, for example, 10,000 N / mm 2 and 5000N / mm 2 The tensile strength of the reinforcing glass fiber can be measured by a method conforming to the provisions of JIS R1657:2003.

[0053] The tensile modulus of the reinforcing glass fiber is, for example, 0.8 × 10 5 kN / mm 2 and preferably 1.0 × 10 which exceeds the tensile modulus of high strength / high elasticity glass (for example, MAGNAVI (registered trademark) of Nippon Sheet Glass Co., Ltd.). 5 kN / mm 2 The tensile modulus of elasticity of the reinforcing glass fiber can be measured by a method conforming to Method A defined in JIS R1657:2003.

[0054] The reinforcing glass fiber of this embodiment also tends to have excellent thermal stability. The glass transition temperature Tg of the reinforcing glass fiber is, for example, 700°C or higher, preferably 850°C or higher, which exceeds the glass transition temperature of high-strength / high-modulus glass (e.g., S2 glass from AGY Corporation, T glass from Nitto Boseki Co., Ltd., and U glass from Nippon Sheet Glass Co., Ltd.), more preferably 900°C or higher, and even more preferably 1000°C or higher. The upper limit of the glass transition temperature Tg of the reinforcing glass fiber is not particularly limited, and is, for example, 1500°C. The glass transition temperature Tg can be measured using a commercially available differential thermal dilatometer.

[0055] The reinforcing glass fiber of this embodiment also tends to have excellent chemical durability (alkali resistance and acid resistance). The alkali resistance can be measured, for example, by the mass loss rate ΔW measured by the method described below. BASE The mass reduction rate of the reinforcing glass fiber, ΔW BASE is, for example, 0.30% by mass or less, preferably 0.25% by mass or less, and more preferably 0.20% by mass or less.BASE Reinforcing glass fibers, which have low alkali resistance and excellent alkali resistance, are suitable for reinforcing concrete products and plastic products. In particular, when reinforcing glass fibers are used to reinforce concrete products, there is a tendency for the reinforcing glass fibers to be required to have high alkali resistance.

[0056] Mass reduction rate ΔW BASE The chemical durability of optical glass can be measured using the following method, which conforms to the Japan Optical Glass Industry Association standard "Method for Measuring Chemical Durability of Optical Glass (Powder Method)" (JOGIS 06). First, the reinforcing glass fiber (or a plate-shaped sample glass having the same composition as the reinforcing glass fiber) is crushed. The crushed sample is separated into pieces that pass through a 600 μm test sieve and remain on a 425 μm test sieve, and these pieces are used as the measurement sample. The test sieve is specified in JIS Z8801. Next, the measurement sample is weighed and immersed in a 10% by weight sodium hydroxide aqueous solution at 99°C for one hour. A sufficient amount of sodium hydroxide aqueous solution is used for the measurement sample, for example, 80 mL for a 5 g sample. After immersion, the supernatant is removed by decantation, and the remaining sample is dried and its mass is measured. The ratio of the difference between the mass of the measurement sample and the mass of the residual sample to the mass of the measurement sample before immersion in the sodium hydroxide aqueous solution was calculated, and the calculated value was taken as the mass loss rate ΔW BASE It can be considered as follows.

[0057] Acid resistance can be measured by, for example, the mass loss rate ΔW ACID The mass reduction rate of the reinforcing glass fiber, ΔW ACID is, for example, 1.50% by mass or less, preferably 1.00% by mass or less, more preferably 0.50% by mass or less, and even more preferably 0.20% by mass or less. ACID Reinforcing glass fiber has low mass and excellent acid resistance, making it suitable for reinforcing plastic products. ACID is the mass loss rate ΔW except that a sulfuric acid aqueous solution with a temperature of 99°C and a concentration of 21.2 mass% is used instead of the sodium hydroxide aqueous solution. BASE can be measured by the same method as

[0058] The reinforcing glass fiber of this embodiment can be used to reinforce various products. For example, the reinforcing glass fiber may be used to reinforce concrete products, rubber products, or plastic products.

[0059] (Reinforcement of concrete products) As described above, reinforcing glass fibers may be used to reinforce concrete products. In another aspect, the present invention provides a concrete product comprising the reinforcing glass fibers of this embodiment. In a preferred embodiment, the concrete product has a cement composition and reinforcing glass fibers embedded in the cement composition. In another preferred embodiment, the concrete product has a main body and a covering member that covers the surface of the main body, and the covering member contains the reinforcing glass fibers. The covering member may further contain a material such as resin or cement.

[0060] The reinforcing glass fibers may be processed appropriately depending on the type of concrete product, etc. In particular, chopped strands, fiber sheets, rods, etc. can be used to reinforce concrete products. In another aspect, the present invention provides chopped strands containing the reinforcing glass fibers of this embodiment, a fiber sheet containing the reinforcing glass fibers of this embodiment, a rod containing the reinforcing glass fibers of this embodiment, etc.

[0061] [Chopped strands] Chopped strands containing reinforcing glass fibers can be produced, for example, by cutting a strand formed by bundling reinforcing glass fibers. The number of reinforcing glass fibers contained in a strand is not particularly limited and is, for example, 100 to 10,000, typically 400 to 4,000. The strands can be formed by bundling a predetermined number of spun reinforcing glass fibers using a sizing agent commonly used for strand formation, such as an elastomeric sizing agent, when spinning the reinforcing glass fibers. The formed strands may be wound on a collet or the like and subjected to a predetermined treatment, such as drying. The strands can be produced by the method described with reference to FIG. 1.

[0062] FIG. 2 is a diagram showing an example of an apparatus for producing chopped strands. As shown in FIG. 2, for example, a cake 20 produced by the spinning apparatus of FIG. 1 is placed in a crill 21, and strands 16 are pulled out from the cake 20 and bundled into a strand bundle (roving) 23 by a bundling guide 22. Water or a treatment liquid is sprayed onto the strand bundle 23 by a spraying device 24. The strand bundle 23 is then cut by a rotary blade 26 of a cutting device 25 to obtain chopped strands 27. Note that chopped strands may also be produced by directly cutting the strands 16 with the rotary blade (chopper) 26 of the cutting device 25 (direct chopper) without winding them up like the cake 20 in FIG. 1. Alternatively, chopped strands may also be produced by cutting a single strand 16. In this specification, chopped strands formed from a strand bundle may be referred to as "bundled chopped strands." Chopped strands formed from a single strand are sometimes called "non-converged chopped strands."

[0063] The chopped strands can be used, for example, by mixing them with a cement composition. As an example, a mixture of unbundled chopped strands and a cement composition can be sprayed onto the surface of the main body of a concrete product to form a covering member that covers the surface of the main body. This covering member can prevent concrete material from peeling off from the surface of the main body. On the other hand, a mixture of bundled chopped strands and a cement composition is suitable for reinforcing the entire concrete product. The bundled chopped strands in this mixture play a role similar to that of straw used in earthen walls and mortar.

[0064] Chopped strands have a large specific surface area and a large area in contact with cement. Therefore, in chopped strands used to reinforce concrete products, it is particularly preferable that the reinforcing glass fibers have excellent alkali resistance. The reinforcing glass fibers also need to have a practically sufficient elastic modulus.

[0065] [Fiber sheet] The fiber sheet containing reinforcing glass fibers may be a woven fabric or a nonwoven fabric. Examples of woven fabrics include cloths using rovings or yarns as warp and / or weft threads. Examples of nonwoven fabrics include chopped strand mats made from chopped strands. Nonwoven fabrics may also be made from short fibers.

[0066] The fiber sheet can be used by impregnating it with, for example, cement mortar or a resin such as an epoxy resin. The fiber sheet may be used with its surface covered with a layer made of resin (a resin layer). In this specification, a fiber sheet impregnated with cement mortar or a resin, or a fiber sheet whose surface is covered with a resin layer, may be referred to as a protective sheet. The protective sheet can be manufactured by known methods such as a hand lay-up molding method, an SMC (Sheet Molding Compound) molding method, or a BMC (Bulk Molding Compound) molding method.

[0067] <Concrete products> 3A and 3B show an example of a concrete product including the protective sheet. Specifically, FIGS. 3A and 3B show segments 31 used as a concrete product for lining a tunnel using the shield tunneling method. The segments 31 have an arc-shaped plate shape, and can be joined together to form a cylindrical lining in a hole excavated by a shield machine. Specifically, a ring can be formed by joining multiple segments 31 together in the circumferential direction. A lining can be formed by joining multiple segments 31 together in the axial direction of the ring.

[0068] A joint plate 33 is provided on the circumferential joining end surface 31A of each segment 31. By fastening and fixing the joint plates 33 of multiple segments 31 together, the multiple segments 31 can be joined in the circumferential direction. A joining rod (not shown) protruding from the joining end surface 31B is provided on one joining end surface 31B of each segment 31 in the axial direction of the ring. A connector 32 that engages with the joining rod is provided on the other joining end surface 31B. An insertion hole H is formed in the connector 32, into which the joining rod is inserted.

[0069] 3B is an enlarged cross-sectional view of segment 31 near joining end surface 31B. As shown in FIG. 3B, segment 31 further includes a protective sheet 41 disposed on joining end surface 31B. In other words, in segment 31, the surface of protective sheet 41 forms joining end surface 31B. Protective sheet 41 functions as a covering member that covers the surface of the main body of segment 31. When multiple segments 31 are joined together, their joining end surfaces 31B, i.e., protective sheets 41, come into contact with each other.

[0070] As shown in FIGS. 3A and 3B, the segments 31 may further include a sealing member 44 that seals the segments 31 when the segments 31 are joined together.

[0071] In the shield tunneling method, the shield machine excavates the ground using the cutter at its tip, while extending the jack rod with the jack spreader in contact with a lining body composed of segments 31. This allows the shield machine to receive a reaction force from the lining body through the jack, and this reaction force allows the shield machine to propel itself forward. Because the shield machine is equipped with multiple jacks, multiple spreaders are in contact with the lining body. Therefore, when pressing forces from the multiple spreaders act on the lining body toward the outside of the lining body, stress may be generated between two adjacent segments 31 in the lining body. The protective sheet 41 buffers this stress, thereby preventing cracks from occurring near the joint end surface 31B.

[0072] [rod] A rod containing reinforcing glass fibers is, for example, formed by bundling reinforcing glass fibers. For example, the rod is produced by braiding the reinforcing glass fibers. In the rod, the bundled reinforcing glass fibers may be solidified with cement or a resin such as an epoxy resin. The rod can be used, for example, as a substitute for reinforcing bars.

[0073] <Concrete products> FIG. 4 shows an example of a concrete product including the rods. More specifically, FIG. 4 shows a utility pole 50 as the concrete product. The utility pole 50 is partially buried underground 60 and extends upward. The utility pole 50 includes a cement composition 52 containing mortar and the like, filled therein, and a plurality of rods 55 embedded in the cement composition 52. The rods 55 are arranged parallel to one another along the direction in which the utility pole 50 extends from the bottom of the utility pole 50. It is particularly preferable that the reinforcing glass fibers in the rods 55 used to reinforce the utility pole 50 have an excellent elastic modulus. The reinforcing glass fibers must also have sufficient alkali resistance for practical use.

[0074] The utility pole 50 shown in FIG. 4 can be produced, for example, by inserting a rod 55 into a hollow utility pole through an opening or the like, and then filling the interior of the utility pole with a cement composition 52. Details of this production method are described, for example, in Japanese Patent Application Laid-Open No. 2006-2543. Japanese Patent Application Laid-Open No. 2006-2543 uses an aramid rod made of aramid fiber. The rod 55 containing reinforcing glass fiber of this embodiment tends to have better alkali resistance than an aramid rod.

[0075] [others] Examples of concrete products reinforced with reinforcing glass fibers are not limited to those mentioned above. Reinforcing glass fibers can be used as aggregates, reinforcing materials, etc. for various concrete products. Reinforcing glass fibers also tend to have good mechanical properties and thermal stability, so they can be used in concrete products that require heat resistance (e.g., concrete products used in power plants, melting furnaces, coke ovens, etc.) or building materials that require fire resistance (e.g., fire-resistant structures for buildings, fire-resistant coating materials, etc.).

[0076] Furthermore, the reinforcing glass fiber can be used after being processed into forms other than the above-mentioned chopped strands, fiber sheet, and rod, such as a strand, roving, yarn, cord, etc. The yarn can be obtained by twisting one or more strands.

[0077] (reinforcement of rubber products) As described above, the reinforcing glass fiber may be used to reinforce a rubber product. In another aspect, the present invention provides a rubber product including the reinforcing glass fiber of the present embodiment. As an example, the rubber product has a rubber composition (matrix rubber) and the reinforcing glass fiber embedded in the rubber composition.

[0078] The reinforcing glass fiber may be processed appropriately depending on the type of rubber product. Specifically, a cord or the like can be used to reinforce the rubber product. In another aspect, the present invention provides a cord containing the reinforcing glass fiber of this embodiment.

[0079] [code] The cord (rubber reinforcing cord) includes a strand formed by bundling the above-mentioned reinforcing glass fibers (rubber reinforcing fibers). The number of reinforcing glass fibers contained in the strand is not particularly limited, and is, for example, 100 to 2000, typically 200 to 600. The strand can be formed by bundling a predetermined number of spun reinforcing glass fibers using a sizing agent commonly used for forming strands, such as an elastomeric sizing agent, when spinning the reinforcing glass fibers. The formed strand may be wound on a collet or the like and subjected to a predetermined treatment, such as drying.

[0080] Preferably, the cord is formed by bundling a plurality of strands to form a strand assembly. However, the cord may consist of a single strand. The strand or strand assembly preferably contains 200 to 36,000 reinforcing glass fibers, and more preferably 200 to 7,800 reinforcing glass fibers. The diameter of the strand or strand assembly is preferably 10 tex to 8,350 tex, and more preferably 68 tex to 1,430 tex.

[0081] In the cord, the strands may be coated with a first coating layer formed from treatment liquid A containing latex and at least one selected from a resorcinol-formaldehyde condensate and a vulcanizing agent. By coating the strands with the first coating layer, the adhesion between the cord and the matrix rubber in which the cord is embedded can be improved. The first coating layer may coat a single strand, or may coat a strand assembly formed by bundling two or more strands.

[0082] The type of latex is not particularly limited, but may be at least one selected from vinylpyridine-styrene-butadiene terpolymer (VP) latex, chlorosulfonated polystyrene (CSM) latex, acrylonitrile-butadiene copolymer (NBR) latex, and nitrile group-containing highly saturated polymer latex. The use of these materials can improve the heat resistance and water resistance of the reinforcing cord. Examples of nitrile group-containing highly saturated polymers include hydrogenated copolymers and terpolymers containing acrylonitrile as a structural unit, such as hydrogenated NBR (H-NBR), and materials containing acrylonitrile and saturated hydrocarbons as structural units, such as butadiene-ethylene-acrylonitrile terpolymers.

[0083] The resorcinol-formaldehyde condensate (RF) is not particularly limited, and may be a novolak type, a resol type, or a mixture thereof. The molar ratio of resorcinol (R) to formaldehyde (F) in the RF is preferably R:F=1:1 to 3. RF is generally commercially available as a liquid containing solids, and those with a solid content of approximately 5% to 10% by weight can be suitably used.

[0084] The vulcanizing agent is not particularly limited, and examples thereof include at least one selected from maleimide compounds and organic diisocyanate compounds. When treatment liquid A contains a vulcanizing agent, the content of the vulcanizing agent in treatment liquid A may be in the range of 5 to 100 parts by weight, and preferably in the range of 20 to 75 parts by weight, per 100 parts by weight of the solid content of the latex. In this case, a better balance can be achieved between the flexibility of the cord and its adhesion to the matrix rubber.

[0085] The organic diisocyanate compound is not particularly limited, but for example, hexamethylene diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), toluene diisocyanate, xylene diisocyanate, naphthalene diisocyanate, methylene bis(phenyl isocyanate), etc. may be used.

[0086] Treatment liquid A may contain one or more of these organic diisocyanate compounds, and may be a mixture of isomers of the compounds that have substituent isomers, such as toluene diisocyanate and methylene bis(phenyl isocyanate). The organic diisocyanate compounds may be used with their isocyanate groups protected by phenols or lactams.

[0087] The maleimide compound is not particularly limited, but for example, bismaleimide, phenylmaleimide, diphenylmethane-4,4'-bismaleimide, etc. may be used.

[0088] The solid content of treatment liquid A is preferably in the range of 10% by weight to 40% by weight, more preferably in the range of 25% by weight to 35% by weight. If the content is too low, the formation of the first coating layer will be insufficient, while if the content is too high, it will be difficult to control the amount of treatment liquid A applied to the strands, and the thickness of the first coating layer will likely be uneven.

[0089] Treatment solution A may contain, as needed, a base such as ammonia to adjust the pH, and may also contain stabilizers, antioxidants, etc. Treatment solution A may also contain a filler such as carbon black, which can result in a cord with even better adhesion to the matrix rubber.

[0090] The first coating can be formed on the strand by applying a method commonly used in cord production. For example, the strand (including the aggregate) can be continuously immersed in a coating bath containing treatment solution A, and after the strand is pulled out of the coating bath, excess treatment solution can be removed and the strand can be dried as needed. The strand on which the first coating has been formed can be used as a cord as is, or, if necessary, can be subjected to various processes such as twisting and formation of a second coating layer, as described below.

[0091] The first coating layer may be formed in an amount equivalent to about 10% by weight to 30% by weight of the weight of the strand.

[0092] The cord may have a structure in which two or more yarns formed by first twisting strands covered with the first covering layer are bundled together and then further final twisted. In this case, the strength is further improved, and the cord can have better resistance to bending fatigue. The number of times of primary twisting may be about 0.5 to 4 times, preferably about 1.2 to 3 times, per 2.54 cm (1 inch) in the longitudinal direction. The yarns formed by primary twisting may be bundled together in an amount of about 2 to 20 strands, preferably about 6 to 15 strands, and then final twisted in an amount of 0.5 to 4 times, preferably about 1 to 2.8 times, per 2.54 cm in the longitudinal direction.

[0093] The cord may be covered with a second covering layer containing rubber, in which case the cord can have improved adhesion to the matrix rubber.

[0094] The type of rubber is not particularly limited and may be selected appropriately depending on the type of matrix rubber, etc. For example, when the matrix rubber is a nitrile group-containing highly saturated polymer, it is preferable that the second coating layer contains CSM as the rubber, since this provides better adhesion. Also, when the matrix rubber is a mixed rubber in which zinc polymethacrylate (ZDMA) is dispersed in a nitrile group-containing highly saturated polymer, it is preferable that the second coating layer contains a nitrile group-containing highly saturated copolymer or a mixed rubber with the same composition as the matrix rubber, since this provides better adhesion.

[0095] The second coating layer may be formed, for example, by impregnating a strand (including an aggregate), a strand (including an aggregate) coated with the first coating layer, or a yarn obtained by further twisting a strand, in treatment liquid B containing dissolved rubber or a rubber precursor, followed by drying. Since CSM and nitrile group-containing highly saturated polymers are soluble in aromatic hydrocarbons such as benzene, toluene, and xylene, halogenated hydrocarbons such as trichloroethylene, ketones such as methyl ethyl ketone, and esters such as ethyl acetate, treatment liquid B may contain these organic substances as solvents.

[0096] Treatment liquid B may contain a vulcanizing agent, and examples of the vulcanizing agent include the above-mentioned maleimide compounds and organic diisocyanate compounds, as well as sulfur; organic peroxides such as dicumyl peroxide and 1,3-bis(t-butylperoxy-m-isopropyl)benzene; and aromatic nitroso compounds such as p-dinitronaphthalene and p-dinitrosobenzene. Treatment liquid B may also contain inorganic fillers, antioxidants, vulcanization aids, plasticizers, etc., as necessary.

[0097] The content of substances other than the solvent in treatment solution B (rubber, vulcanizing agent, etc.) can be set appropriately depending on the type of substance, but if it is in the range of about 3 to 25% by weight, preferably about 5 to 15% by weight, the second coating layer can be easily formed. The content of rubber or rubber precursor in the substances other than the solvent is preferably about 20 to 60% by weight, and if treatment solution B contains a vulcanizing agent, the content of the vulcanizing agent in the substances other than the solvent is preferably about 0.5 to 30% by weight.

[0098] When forming the second coating layer, for example, treatment liquid B may be applied to the surface of a strand (including an aggregate) or a twisted yarn in an amount of about 1% by weight to 15% by weight, preferably about 2% by weight to 6% by weight, calculated as the amount of substances other than the solvent, relative to the weight of the strand.

[0099] <Rubber products> Examples of rubber products reinforced with the cords include rubber belts, rubber tires, and rubber hoses. An example of a rubber belt is a power transmission belt. Examples of power transmission belts include meshing power transmission belts and friction power transmission belts. An example of a meshing power transmission belt is a toothed belt, such as a timing belt for automobiles. Examples of friction power transmission belts include flat belts, round belts, V-belts, and V-ribbed belts. Rubber tires are typically automobile tires or bicycle tires. In cords used to reinforce rubber products, it is particularly preferable that the reinforcing glass fiber has an excellent elastic modulus.

[0100] Figure 5 shows an example of the structure of a rubber belt including cords. The rubber belt 1 has the shape of a so-called toothed belt and includes a matrix rubber 3 and a plurality of cords 2 embedded in the matrix rubber 3. The cords 2 are arranged parallel to each other along the longitudinal direction of the rubber belt 1, in other words, along a direction perpendicular to the belt width direction, across which the protruding portions 4, which form the "teeth," cross. A tooth cloth 5 is attached to the surface of the rubber belt 1 on which the protruding portions 4 are formed, for the purpose of suppressing wear, etc.

[0101] [others] The reinforcing glass fibers can also be processed into forms other than the cords described above, such as those described above for concrete products.

[0102] (Reinforcement of plastic products) As described above, the reinforcing glass fiber may be used to reinforce a plastic product (resin product). Another aspect of the present invention provides a plastic product comprising the reinforcing glass fiber of this embodiment. In a preferred embodiment, the plastic product has a resin composition (matrix resin) and reinforcing glass fibers embedded in the resin composition. In another preferred embodiment, the plastic product has a main body and a covering member that covers the surface of the main body, and the covering member contains the reinforcing glass fiber. The covering member may further contain a material such as resin. A plastic product reinforced with reinforcing glass fibers is sometimes called FRP (Fiber Reinforced Plastic).

[0103] The matrix resin may contain a thermosetting resin or a thermoplastic resin. Thermosetting resins are not particularly limited, and examples thereof include epoxy resins, modified epoxy resins such as vinyl ester resins, phenolic resins, unsaturated polyester resins, polyimide resins, and bismaleimide resins. Thermoplastic resins are not particularly limited, and examples thereof include polyolefin resins, polyamide resins, polycarbonate resins, polyphenylene sulfide resins, and polyether ether ketone resins. Resin products containing thermoplastic resins can be easily produced by injection molding, stampable molding, or the like.

[0104] The reinforcing glass fibers may be processed appropriately depending on the type of plastic product. Specifically, chopped strands, fiber sheets, etc. can be used to reinforce plastic products. The reinforcing glass fibers can also be processed into forms other than chopped strands and fiber sheets. Examples of other forms include those described above for concrete products.

[0105] <Plastic products> Plastic products reinforced with the reinforcing glass fiber of this embodiment can be used for applications such as sporting goods, vehicles such as automobiles, ships, building materials, aircraft, septic tanks, bathtubs, blades for wind power generation, timber, poles, tanks, pipes, sewer pipes (drainage pipes), fuel tanks, and home appliances.

[0106] Plastic products used in sporting goods applications include fishing line, fishing rods, golf club shafts, skis, canoes, tennis and badminton rackets, and strings. Plastic products used in vehicle applications include vehicle bodies, lamp housings, front-end panels, bumpers, seat housings, and drive shafts. Plastic products used in marine applications include ship bodies, masts, and decks. Plastic products used in aircraft applications include primary structural materials, secondary structural materials, interior materials, seats, and accessory parts. Plastic products used in home appliances include circuit boards, panels, switchgear, insulators, and appliance bodies.

[0107] In plastic products used in natural environments, such as drainage pipes, reinforcing glass fibers may come into contact with acidic liquids such as acid rain. Therefore, it is particularly preferable for these reinforcing glass fibers to have excellent acid resistance. These reinforcing glass fibers also need to have a modulus of elasticity sufficient for practical use.

[0108] The reinforcing glass fiber of this embodiment can also be used as a high-temperature insulating material used in vehicle mufflers, engine parts, blast furnaces, etc. The reinforcing glass fiber of this embodiment can also be used as a separator used in batteries such as lead-acid batteries.

[0109] In addition, from another aspect, the present invention is The total content of SiO2 and Al2O3 is 40 to 70 mass%; The mass ratio calculated by Al2O3 / (SiO2+Al2O3) is 0.15 to 0.40, The content of Fe2O3 is 16 to 25 mass%, The present invention provides a rubber reinforcing fiber having a CaO content of 5 to 30 mass %.

[0110] In one embodiment of the present invention, the rubber reinforcing fiber is a long fiber.

[0111] In one embodiment of the present invention, the tensile strength of the rubber reinforcing fiber is 4500 N / mm 2 That's all.

[0112] In one embodiment of the present invention, the tensile modulus of the rubber reinforcing fiber is 1.0 × 10 5 kN / mm 2 That's all.

[0113] In one embodiment of the present invention, the glass transition temperature Tg of the rubber reinforcing fiber is 850° C. or higher.

[0114] From another aspect, the present invention provides: The present invention provides a rubber reinforcing cord having strands formed by bundling the above rubber reinforcing fibers.

[0115] From another aspect, the present invention provides: A rubber product is provided that is reinforced with the rubber reinforcing cord. [Example]

[0116] The present invention will be described in more detail below with reference to examples and comparative examples.

[0117] Raw material mixture batches were prepared by weighing and homogeneously mixing glass raw materials so as to obtain the compositions shown in Tables 4 and 5. The glass raw materials used included silicon dioxide, aluminum oxide, calcium carbonate, and diiron trioxide.

[0118] Next, the prepared raw material mixed batch was melted at 1500 to 1600°C in an electric furnace and maintained in a molten state for about 4 hours to achieve a uniform composition. After that, a portion of the obtained molten glass composition (glass melt) was poured onto an iron plate and slowly cooled to room temperature in the electric furnace to obtain a plate-shaped sample glass to be used for evaluation.

[0119] (elastic modulus) The sample glass was cut and each surface was mirror-polished to prepare a 25 × 25 × 5 mm plate-shaped sample, and the density ρ of each sample was measured by the Archimedes method. The elastic modulus was measured in accordance with the ultrasonic pulse method of JIS R1602-1995. Specifically, using the sample used in the density measurement described above, the sound speed of the ultrasonic pulse was measured for longitudinal and shear waves, and this was substituted into the above formula along with the density to calculate the elastic modulus E. The propagation speed was calculated using an ultrasonic thickness gauge MODEL 25DL PLUS manufactured by Olympus Corporation by dividing the time it took for an ultrasonic pulse with a frequency of 20 kHz to propagate through the thickness of the sample, reflect, and return by the propagation distance (twice the thickness of the sample).

[0120] (alkali and acid resistance) The sample glass was crushed and the mass loss rate ΔW was measured by the method described above. BASE and mass reduction rate ΔW ACID was measured.

[0121] The above-mentioned properties were measured for each sample obtained, and the results are shown in Tables 4 and 5.

[0122] [Table 4]

[0123] [Table 5]

[0124] As can be seen from Tables 4 and 5, glass compositions having high elastic modulus and excellent alkali resistance and acid resistance were obtained from each Example. The reinforcing glass fibers formed from these glass compositions are suitable for reinforcing various products, such as concrete products.

[0125] As can be seen from the results of Examples 1 to 3, when the SiO2 content is decreased and the CaO content is increased, the elastic modulus increases and the mass reduction rate ΔW BASEOn the other hand, in this case, the mass reduction rate ΔW ACID The acid resistance tended to decrease.

[0126] As can be seen from the results of Examples 2 and 4, and the results of Examples 3 and 5, when the Al2O3 content was decreased and the CaO content was increased, both the alkali resistance and the acid resistance tended to improve, while there was almost no change in the elastic modulus.

[0127] As can be seen from the results of Examples 1, 6, and 7, when the SiO2 content was decreased and the Fe2O3 content was increased, the elastic modulus tended to increase. In this case, there was no clear correlation between the alkali resistance and the composition.

[0128] As can be seen from Comparative Examples 1 and 2, when the Fe2O3 content was below 12 mass%, the elastic modulus was low when the value of Al2O3 / (Al2O3+SiO2) was small, and devitrification occurred when the value of Al2O3 / (Al2O3+SiO2) was large. As can be seen from Comparative Examples 3 and 4, when the Fe2O3 content exceeded 25 mass%, devitrification occurred. It is difficult to produce reinforcing glass fibers from the glass compositions of Comparative Examples 2 to 4, in which devitrification occurred.

[0129] Comparative Examples 5 and 6 correspond to glass compositions of C-glass and E-glass, respectively, which are general-purpose chemical-resistant glasses. These glass compositions had a low modulus of elasticity and did not achieve both acid resistance and alkali resistance. [Industrial Applicability]

[0130] The reinforcing glass fiber of this embodiment is suitable for reinforcing various products, for example, concrete products.

Claims

1. SiO 2 , Al 2 O 3 and Fe 2 O 3 Including, Fe 2 O 3 The reinforcing glass fiber has a content of 12 to 25 mass %.

2. Further comprising CaO, 2. The reinforcing glass fiber according to claim 1, wherein the CaO content is 5 to 30 mass %.

3. SiO 2 and Al 2 O 3 and the total content is 40 to 70 mass %, A 2 O 3 / (SiO 2 +Al 2 O 3 3. The reinforcing glass fiber according to claim 1, wherein the mass ratio calculated by the above formula (1) is 0.10 to 0.

40.

4. Tensile strength is 2500N / mm 2 The reinforcing glass fiber according to any one of claims 1 to 3.

5. The reinforcing glass fiber according to any one of claims 1 to 4, having an elastic modulus of 80 MPa or more.

6. The reinforcing glass fiber according to any one of claims 1 to 5, having a glass transition point Tg of 700°C or higher.

7. Mass loss rate ΔW when immersed in a 10% sodium hydroxide aqueous solution at 99° C. for 1 hour BASE The reinforcing glass fiber according to any one of claims 1 to 6, wherein the content of the sintered glass fiber is 0.30 mass% or less.

8. A reinforcing glass fiber according to any one of claims 1 to 7, used to reinforce concrete products.

9. Mass loss rate ΔW when immersed in a 10% sodium hydroxide aqueous solution at 99° C. for 1 hour BASE The reinforcing glass fiber according to claim 8, wherein the content of the SiO 2 is 0.25 mass % or less.

10. A reinforcing glass fiber according to any one of claims 1 to 7, used to reinforce rubber products.

11. A reinforcing glass fiber according to any one of claims 1 to 7, used to reinforce plastic products.

12. 12. The reinforcing glass fiber according to claim 10, having an elastic modulus of 85 MPa or more.

13. 13. The reinforcing glass fiber according to claim 12, having an elastic modulus of 90 MPa or more.

14. Further comprising CaO, The CaO content is 18 to 30 mass%; Fe 2 O 3 The reinforcing glass fiber according to any one of claims 8 and 10 to 13, wherein the content of is 15 to 25 mass%.

15. Further comprising CaO, The CaO content is 15 to 25 mass%; Fe 2 O 3 The reinforcing glass fiber according to any one of claims 8 and 10 to 13, wherein the content of is 15 to 23 mass%.

16. The reinforcing glass fiber according to any one of claims 1 to 15, which is a long fiber.

17. A chopped strand comprising the reinforcing glass fiber according to any one of claims 1 to 15.

18. A fiber sheet comprising the reinforcing glass fiber according to any one of claims 1 to 15.

19. A rod comprising a reinforcing glass fiber according to any one of claims 1 to 15.