Method for transferring thin layer to support substrate having different thermal expansion coefficient

JP2023118728A5Active Publication Date: 2024-10-17SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023094292
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-06-30
Filing Date
2023-06-07
Publication Date
2024-10-17
Estimated Expiration
2038-06-21

AI Technical Summary

Technical Problem

Existing methods for transferring thin layers to a support substrate face challenges when the thermal expansion coefficients of the materials are significantly different, leading to uncontrolled cracking or delamination during heat treatment.

Method used

A method involving a donor substrate with a handling substrate, where the thermal expansion coefficients are balanced, allowing for the introduction of light species to create an embrittlement surface, followed by assembly and separation at controlled high temperatures to transfer a thin layer with different thermal expansion to a support substrate.

Benefits of technology

Enables the transfer of thin layers with different thermal expansion coefficients without unintentional cracking or delamination, facilitating high-temperature processing and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a novel method for transferring a thin layer made of a first material onto a support substrate made of a second material.SOLUTION: Provided is a method for transferring a thin layer (3) made of a first material to a support substrate (7) made of a second material, the first material and the second material having different thermal expansion coefficients. The method includes the steps of: preparing a donor substrate (1) composed of an assembly of a thick layer (1a) formed of the first material and a handling substrate (1b), the thermal expansion coefficient of the handling substrate (1b) being similar to that of the support substrate (7), and the donor substrate (1) having a main face (4) on the side of the thick layer (1a); introducing light species into the thick layer (1a) to define the thin layer (3) between an embrittlement plane (2) and the main face (4); assembling the main face (4) of the donor substrate with one face (6) of the support substrate (7); and detaching the thin layer (3) from the embrittlement plane (2), the step including the application of heat treatment.SELECTED DRAWING: Figure 1C
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to the field of heterogeneous structures, which combine two substrates having different coefficients of thermal expansion. More specifically, this invention relates to a method for transferring a thin layer to a support substrate. This manufacturing method is used, for example, in fields such as microelectronics, micromechanics, and photonics. [Background technology]

[0002] Various methods for forming thin layers on a support substrate are known from the prior art. Such methods may include, for example, molecular beam epitaxy, plasma sputtering, plasma deposition (laser pulsed deposition), or the application of the Smart Cut® technique, which obtains thin layers from a bulk substrate by cracking at a fragile zone (or brittle surface) formed within the bulk substrate by the injection of lightweight species.

[0003] More specifically, the present invention relates to the formation of thin layers made of ferroelectric material obtained by applying a method such as that taught in French Patent Application Publication No. 2914492.

[0004] The SmartCut method is particularly suitable when the thermal expansion coefficient of the thin layer material to be transferred is similar to that of the support substrate on which the transfer is to be performed.

[0005] Conversely, the temperature that the assembly formed from the support substrate and the donor substrate can withstand is limited. Therefore, French Patent Application Publication No. 2856192 reminds us that heat treatment exceeding a temperature determined by the thermal expansion coefficient of the material may cause uncontrolled cracking of one of the substrates and / or delamination of the donor substrate or thin layer. This is problematic in the smartcut method, as it may be necessary to perform at least one heat treatment at a sufficient temperature, for example, to strengthen the adhesion of the donor substrate to the support substrate or to promote cracking of the donor substrate at the brittle surface. [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] One objective of the present invention is to propose a method for transferring a thin layer made of a first material to a support substrate made of a second material, wherein the first and second materials have different coefficients of thermal expansion, thereby at least partially solving the above-mentioned problems. In particular, the invention aims to find applications of this method in transferring a thin layer made of a ferroelectric material to a support substrate made of silicon, for example, a support substrate made of silicon, which has a different coefficient of thermal expansion than the coefficient of thermal expansion of the material from which the thin layer is composed. [Means for solving the problem]

[0007] To achieve one of these objectives, the subject of the present invention proposes a method for transferring a thin layer made of a first material to a support substrate made of a second material, wherein the first and second materials have different coefficients of thermal expansion. According to the present invention, the method for transferring a thin layer includes the steps of: preparing a donor substrate comprising an assembly of a thick layer formed from the first material and a handling substrate, wherein the coefficient of thermal expansion of the handling substrate is similar to that of the support substrate, and the donor substrate has a main surface on the thick layer side; introducing a lightweight material into the thick layer to create an embrittlement surface within the thick layer and defining a thin layer between the embrittlement surface and the main surface of the donor substrate; assembling the main surface of the donor substrate and one surface of the support substrate; and separating the thin layer from the embrittlement surface, which includes a separation step of applying heat treatment.

[0008] The assembly formed from the donor substrate and support can be exposed to temperatures considerably higher than those applied in the context of the "direct" approach of the prior art, thereby eliminating the risk of uncontrolled cracking of one of the substrates or delamination of the donor substrate or thin layer, and eliminating the need for any handling substrates. The equilibrium structure of this assembly in terms of its coefficient of thermal expansion facilitates the step of separating the thin layer, in particular, by exposing the assembly to relatively high temperatures.

[0009] According to other advantages and non-limiting features of the present invention, which can be obtained individually or in any technically implementable combination, The thermal expansion coefficient of the first material constituting the thick layer and the thermal expansion coefficient of the second material constituting the support substrate differ by at least 10% at room temperature. The difference between the thermal expansion coefficients of the handling substrate components and the thermal expansion coefficients of the support components is smaller in absolute value than the difference between the thermal expansion of the thick layer and the thermal expansion of the support substrate. The lightweight species being injected are hydrogen ions and / or helium ions. The first material is a ferroelectric material such as LiTaO3, LiNbO3, LiAlO3, BaTiO3, PbZrTiO3, KNbO3, BaZrO3, CaTiO3, PbTiO3, or KTaO3. The material of the support substrate is silicon. The handling substrate has the same properties as the support substrate. The handling substrate has a thickness equal to the thickness of the support substrate. The thick layer has a thickness between 10 and 400 micrometers so as to allow sampling of one or more thin layers. The donor board is obtained by joining the source board and the handling board. The bonding is achieved by molecular adhesion. The step includes thinning the source substrate to form a thick layer. The thinning step is carried out by milling, and / or mechanical and chemical polishing and / or etching.

[0010] Other features and advantages of the present invention will become apparent from the detailed description of the invention below, which is given with reference to the accompanying drawings. [Brief explanation of the drawing]

[0011] [Figure 1A] This is a diagram of one embodiment of the method according to the present invention. [Figure 1B] This is a diagram of one embodiment of the method according to the present invention. [Figure 1C] It is a diagram of an embodiment of the method according to the present invention. [Figure 1D] It is a diagram of an embodiment of the method according to the present invention. [Figure 2] It is a schematic diagram of a method for forming a donor substrate according to the present invention.

Embodiments for Carrying out the Invention

[0012] For the sake of simplicity of the following description, the same reference numerals are used for the same elements or elements performing the same functions in the prior art or in various embodiments of the presented method.

[0013] The drawings are shown schematically rather than to scale for ease of viewing. In particular, the thicknesses of the layers are not to scale with respect to the lateral dimensions of those layers. <(

[0014] In other parts of this description, the term "coefficient of thermal expansion" used with respect to a layer or a substrate refers to the coefficient of expansion in a defined direction on the major surface defining this layer or this substrate. When the material is anisotropic, the coefficient value to be retained is the value of the maximum amplitude. The coefficient value is the value measured at room temperature.

[0015] The present invention relates to a method of transferring a thin layer 3 made of a first material to a support substrate 7 made of a second material. The first and second materials have different coefficients of thermal expansion. The term "different" means that these coefficients differ by at least 10%.

[0016] In the context of this description, by way of example, the thin layer 3 is made of a ferroelectric material and the support 7 is considered to be made of silicon (the coefficient of thermal expansion is expected to be 2.6×10 -6 K -1 ).

[0017] A ferroelectric material is a material that has an electric polarization in its natural state, and it is recalled that this polarization can be reversed when an external electric field is applied. A ferroelectric domain refers to each continuous region of a material where the polarization is uniform (all dipole moments are aligned parallel to each other in a given direction). Thus, a ferroelectric material can be characterized as "single-domain" if the material consists of a single region where the polarization is uniform, or "multi-domain" if the ferroelectric material contains multiple regions with possibly different polarities

[0018] Generally, overall, it is desirable to have a ferroelectric thin layer with single-domain properties.

[0019] Referring to FIG. 1A, the donor substrate 1 is composed of a thick layer 1a of a ferroelectric material such as LiTaO3 (2×10 -6 K -1 (z), 16×10 -6 K -1 (x, y)), LiNbO3, LiAlO3, BaTiO3, PbZrTiO3, KNbO3, BaZrO3, CaTiO3, PbTiO3 or KTaO3, and a handling substrate 1b. The donor substrate 1 can take the form of a standard-sized circular wafer, for example, with a diameter of 150 mm or 200 mm. However, the present invention is not limited to these dimensions or this shape in any way. The thick layer 1a of the material can be sampled from an ingot of the ferroelectric material, and this sampling is carried out so that the thick layer 1a has a predetermined crystal orientation. This orientation is selected according to the intended application. Thus, when it is desired to form a SAW filter using the characteristics of the thin layer, it is a common method to select the orientation 42°RY. However, the present invention is not limited to any specific crystal orientation.

[0020] It is advantageous for the handling substrate 1b to be made of one (or more) materials that give a thermal expansion coefficient close to that of the material constituting the support substrate 7. The term "close" means that, as an absolute value, the difference between the thermal expansion coefficient of the handling substrate 1b and the thermal expansion coefficient of the support 7 is smaller than the difference between the thermal expansion of the thick layer 1a and the thermal expansion of the support substrate 7.

[0021] It is preferable that the handling substrate 1b and the support substrate have the same coefficient of thermal expansion. During the assembly of the donor substrate and support, a structure is formed that can withstand heat treatment at relatively high temperatures. For ease of implementation, this can be achieved by selecting the handling substrate 1b to be made of the same material as the support substrate 7.

[0022] To form the donor substrate 1, a bulk block of ferroelectric material is pre-assembled with a handling substrate 1b, for example, by molecular adhesive bonding technique. Next, a layer 1a of ferroelectric material is formed by thinning, for example, by milling and / or mechanochemical polishing and / or etching. This method is schematically shown in Figure 2. It can be assumed that an adhesive layer is formed on one and / or the other of the contacting surfaces (for example, by deposition of silicon oxide and / or silicon nitride) before assembly. Assembly may include the application of low-temperature heat treatment (e.g., 50-300°C, typically 100°C), which can increase the bonding energy to a level sufficient to enable the subsequent thinning step.

[0023] The handling substrate 1b can be selected to have a thickness substantially equal to the thickness of the support substrate 7. The thinning step is performed such that the thick layer 1a has a thickness small enough that the strength of the thick layer 1a is reduced by stress generated during the heat treatment applied elsewhere in the method. At the same time, this thickness is large enough that a thin layer 3 or more such layers can be sampled from its thickness. This thickness can be, for example, 5 to 400 microns.

[0024] The method includes introducing at least one lightweight species into the donor substrate 1. This introduction can correspond to the implantation of lightweight species, such as hydrogen ions and / or helium ions, into the main surface 4 of the donor substrate 1, i.e., ion bombardment.

[0025] In a method known per se as shown in Fig. 1B, the implanted ions play the role of forming a brittle surface 2 that defines the boundary between a thin layer 3 of a ferroelectric material to be transferred, located on the side of the main surface 4, and another part 5 that constitutes the other part of the substrate.

[0026] In fact, the dose and implantation energy of the implanted species are selected according to the thickness of the layer to be transferred and the physicochemical properties of the donor substrate. Thus, in the case of a donor substrate 1 made of LiTaO3, in order to define the boundary of a thin layer 3 of about 200 - 2000 nm, 1 E 16 - 5 E 17 at / cm 2 dose of hydrogen may be selected to be implanted at an energy of 30 - 300 keV.

[0027] In the next step shown in Fig. 1C, the main surface 4 of the donor substrate 1 is assembled together with one surface 6 of a support substrate 7. The support substrate 7 can have the same dimensions and the same shape as the donor substrate. For reasons of utility and cost, the support substrate 7 is a single - crystal or poly - crystal silicon wafer. However, more generally, the support substrate 7 can be made of any material such as silicon, sapphire or glass, and can have any shape.

[0028] Before this step, it can be assumed that the surfaces of the substrates to be assembled are prepared by steps of cleaning, brushing, drying, polishing or plasma activation.

[0029] The assembly step can correspond to positioning the donor substrate 1 in close contact with the support substrate 7 by molecular adhesion and / or electrostatic bonding. Optionally, especially when two substrates 1 and 7 are assembled by direct bonding, at least one intermediate layer may be formed before assembly on the main surface 4 of the donor substrate 1, or on the flat surface 6 of the support substrate 7 to be assembled, or both, to facilitate the assembly of the two substrates 1 and 7. This intermediate layer may consist of, for example, silicon oxide, silicon nitride, or polycrystalline silicon, and have a thickness ranging from several nanometers to several microns. The intermediate layer can be produced according to various techniques known in the prior art, such as thermal oxidation, thermal nitriding, or chemical deposition (PECVD, LPCVD, etc.).

[0030] At the end of this assembly step, an assembly shown in Figure 1C is obtained, which includes two bonded substrates, the flat surface 6 of the support substrate 7 being bonded to the main surface 4 of the donor substrate 1.

[0031] Next, the assembly is processed to separate the thin layer 3 of ferroelectric material from the donor substrate 1, for example, by cleavage at the brittle surface 2.

[0032] Therefore, this separation step may include applying a heat treatment to the assembly in a temperature range of approximately 80°C to 500°C to enable the transfer of the thin layer 3 to the support substrate 7. In addition to the heat treatment, this step may include applying a blade or a spray of gas or liquid fluid to the embrittlement surface 2. In the case of ferroelectric materials, care is taken not to exceed the Curie temperature of the ferroelectric material so as not to degrade the properties of the thin layer.

[0033] After this separation step, the structure 9 shown in Figure 1D is obtained. This structure 9 includes a thin layer 3 of ferroelectric material, which includes a first free surface 8 and a main surface 4 positioned relative to the support substrate 7.

[0034] The assembly formed from the donor substrate 1 and the support 7 can be exposed to temperatures considerably higher than those applied in the context of the "direct" approach of the prior art, thereby eliminating the risk of uncontrolled cracking of one of the substrates or delamination of the donor substrate 1 or the thin layer 3, and thus the donor substrate does not contain any handling substrate. Therefore, the equilibrium structure of this assembly in terms of its coefficient of thermal expansion facilitates the step of separating the thin layer 3 by exposing the assembly to relatively high temperatures, for example, 80°C to 500°C.

[0035] Next, finishing steps can be performed on the thin layer 3 and, in particular, the free surface 8 of the thin film, in order to restore and / or improve the desired properties of the thin layer. As is well known, this finishing may include polishing, etching, sacrificial oxidation, or annealing in a neutral, reducing, or oxidizing atmosphere.

[0036] In the context of the example described so far in which the thin layer 3 is made from a ferroelectric material, this finishing step can correspond to polishing following the heat treatment of the thin layer 3, and this sequence can restore the initial single-domain properties that the thick layer 1a had, for example, by having the thin layer 3 after transfer inherit the 42°RY orientation. However, the present invention is not limited in any way to a specific finishing sequence.

[0037] The heat treatment allows for the correction of crystal defects present in the thin layer 3. In addition, the heat treatment contributes to the solidification of the bond between the thin layer 3 and the support 7. The heat treatment brings the structure to a temperature between 300°C and the Curie temperature of the ferroelectric material over a period of time ranging from 10 seconds to 10 hours. This heat treatment is preferably carried out by exposing the free surface of the thin layer 3 to an oxidizing or neutral gas atmosphere.

[0038] The preparation method further includes thinning the thin layer 3 after heat treatment. This thinning can correspond to polishing the first free surface 8 of the thin layer 3 by, for example, mechanical, mechochemical and / or chemical etching thinning techniques. This prepares the free surface 8 such that its roughness is minimal, for example, less than 0.5 nm RMS relative to 5 × 5 μm as measured by atomic force measurement (AFM), and allows for the removal of surface portions of the first free surface 8 of the thin layer 3 that tend to contain residual defects.

[0039] Naturally, the present invention is not limited to the examples described, and variations of the embodiments may be introduced into the present invention without departing from the scope of the present invention as defined by the claims.

[0040] Furthermore, the present invention is applicable to any "heterogeneous" structure in which there is a difference in the coefficient of thermal expansion between the thin layer 3 and the support substrate 7, such as in the case of a silicon-on-quartz or silicon-on-sapphire structure.

[0041] 1... Donor substrate, 1a... Thick layer, 1b... Handling substrate, 3... Thin layer, 4... Main surface of donor substrate, 6... One surface of support substrate, 7... Support substrate.

Claims

1. A method for transferring a thin layer (3) of a first material onto a supporting substrate (7) of a second material, said first material and said second material having different thermal expansion coefficients, comprising: a step of preparing a donor substrate (1) consisting of an assembly of a thick layer (1a) formed from the first material and a handling substrate (1b), wherein the difference between the thermal expansion coefficient of a component of the handling substrate (1b) and the thermal expansion coefficient of a component of the support substrate (7) is smaller in absolute value than the difference between the thermal expansion coefficient of the thick layer (1a) and the thermal expansion coefficient of the support substrate (7), and the donor substrate (1) has a main surface (4) on the side of the thick layer (1a); b) introducing light species into said thick layer (1a) to generate an embrittled surface (2) in said thick layer (1a) and to define said thin layer (3) between said embrittled surface (2) and said main surface (4) of said donor substrate (1), said implanted light species being hydrogen ions and / or helium ions; c. assembling the main surface (4) of the donor substrate and one surface (6) of the support substrate (7); d) a step of separating said thin layer (3) from said embrittled surface (2), comprising applying a heat treatment; Including, the thermal expansion coefficient of the first material constituting the thick layer (1a) and the thermal expansion coefficient of the second material constituting the support substrate (7) differ by at least 10% at room temperature; the first material is a ferroelectric material; The step a Bonding a bulk block of ferroelectric material to said handling substrate (1b); thinning said bulk block of ferroelectric material to form said thick layer (1a); The method of claim 1, further comprising:

2. 2. The method of claim 1, wherein the first material is a ferroelectric material such as LiTaO3, LiNbO3, LiAlO3, BaTiO3, PbZrTiO3, KNbO3, BaZrO3, CaTiO3, PbTiO3, or KTaO3.

3. The method according to claim 1 or 2, wherein the material of the support substrate (7) is silicon.

4. The method according to any one of the preceding claims, wherein the handle substrate (1b) has a thickness equal to a thickness of the support substrate (7).

5. The method according to any one of claims 1 to 4, wherein said thick layer (1a) has a thickness between 10 and 400 micrometers to allow sampling of one or more thin layers.

6. The method of claim 1 , wherein the bonding is accomplished by molecular adhesion.

7. The method of claim 1 , wherein the thinning is performed by milling and / or chemical-mechanical polishing and / or etching.