AI Technical Summary
Existing methods for decomposing carbon dioxide, such as those using oxygen-deficient iron oxides, suffer from low decomposition capacity and inefficiency under conventional reaction conditions.
A method involving the use of a reducing agent with high reducing ability, such as oxygen-deficient iron oxide (Fe3O4-δ or completely oxygen-deficient iron) to react with carbon dioxide, maintaining the magnetite crystal structure and producing nano-sized carbon particles efficiently.
This approach achieves high reaction efficiency in decomposing carbon dioxide while producing carbon materials at a low cost, contributing to carbon dioxide reduction and emission reduction.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to a method for producing carbon materials by reducing carbon dioxide, a carbon material, a method for decomposing carbon dioxide, and a reducing agent. [Background technology]
[0002] For example, steel plants, thermal power plants, cement manufacturing plants, and waste incineration facilities emit large amounts of carbon dioxide (CO2). Therefore, from the perspective of preventing global warming, it is important to capture carbon dioxide instead of releasing it into the atmosphere.
[0003] Conventionally, technologies for separating and recovering carbon dioxide include chemical absorption, physical absorption, and membrane separation. Furthermore, technologies for decomposing the recovered carbon dioxide include semiconductor photocatalysis, photochemical reduction using metal colloid catalysts, metal complexes, and other catalysts, electrochemical reduction, and decomposition methods using chemical fixation and transformation reactions, such as reactions with bases, transfer reactions, dehydration reactions, and addition reactions. However, all of these carbon dioxide decomposition methods have been impractical in terms of reaction efficiency, cost, and energy consumption.
[0004] For this reason, for example, Patent Document 1 discloses a method for producing carbon by reducing carbon dioxide using magnetite, i.e., oxygen-depleted iron oxide, which has vacancies that are oxygen-depleted sites in its lattice, and then obtaining methane and methanol from the carbon. In the invention of Patent Document 1, it is stated that a closed system capable of continuously and efficiently decomposing carbon dioxide can be realized by decomposing carbon dioxide with oxygen-depleted iron oxide, and then reducing the resulting iron oxide with hydrogen back to oxygen-depleted iron oxide. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-184912
Summary of the Invention
Problems to be Solved by the Invention
[0006] However, under the reaction conditions disclosed in Patent Document 1, the oxygen deficiency degree of the oxygen-deficient iron oxide is small (when the oxygen-deficient iron oxide is represented by Fe3O , , 4-δ ,
[0010] , , , , ,
[0009] , δ is at most about 0.16), and there is a problem that the decomposition ability of carbon dioxide is low and carbon dioxide cannot be efficiently decomposed.
[0007] This invention has been made in view of the above circumstances, and aims to provide a method for producing a carbon material capable of efficiently producing a carbon material by decomposing carbon dioxide with a reducing agent having a high reducing ability at a high reaction efficiency, a carbon material obtained thereby, a method for decomposing carbon dioxide, and a reducing agent. [[ID=1
[0011] Furthermore, in the present invention, the reducing agent generation step may be performed at a reaction temperature in the range of 300°C or higher and 450°C or lower.
[0012] Furthermore, in the present invention, the concentration of hydrogen used in the reducing agent generation step may be in the range of 5% by volume or more and 100% by volume or less.
[0013] Furthermore, the present invention may further include a carbon recovery step, which is a post-carbon generation step, in which the oxidized reducing agent is dissolved and the carbon is separated.
[0014] Furthermore, in this invention, the carbon may be nano-sized carbon with a particle diameter of 1 μm or less.
[0015] Furthermore, in the present invention, the carbon generation step may be performed at a reaction temperature in the range of 300°C to 450°C.
[0016] Furthermore, in the present invention, the carbon generation step may be performed with a reaction pressure in the range of 0.01 MPa or more and 5 MPa or less.
[0017] Furthermore, in this invention, the magnetite has a specific surface area of 0.1 m² as determined by the BET method. 2 / g or more, 10m 2 It may also be in a range of less than / g.
[0018] Furthermore, in the present invention, the magnetite may have an average particle diameter (volume cumulative mean diameter (50% diameter); the same applies hereinafter) in the range of 1 μm or more and 1000 μm or less.
[0019] Furthermore, in this invention, the magnetite has a bulk density of 0.3 g / cm³. 3 More than 3g / cm 3 The following range is also acceptable.
[0020] The carbon material of the present invention is characterized by being manufactured by the carbon material manufacturing method described in each of the above sections.
[0021] The carbon dioxide decomposition method of the present invention has a carbon dioxide decomposition step of reacting carbon dioxide with a reducing agent to decompose carbon dioxide, and the reducing agent is obtained by reducing magnetite while maintaining its crystal structure, Fe3O 4-δ (where δ is 1 or more and less than 4), or oxygen completely deficient iron (δ = 4) obtained by completely reducing magnetite, and is characterized by using the oxygen-deficient iron oxide represented by
[0022] The reducing agent of the present invention is obtained by reducing magnetite while maintaining its crystal structure, Fe3O 4-δ (where δ is 1 or more and less than 4), and is characterized by containing at least one of oxygen-deficient iron oxide represented by and oxygen completely deficient iron (δ = 4) obtained by completely reducing magnetite.
[0023] In addition, in the present invention, it may be obtained by reacting the magnetite with hydrogen and subjecting the magnetite to a deoxidation reaction.
[0024] In addition, in the present invention, the deoxidation reaction may be carried out at a reaction temperature in the range of 300 °C or higher and 450 °C or lower.
[0025] In addition, in the present invention, the magnetite has a specific surface area by the BET method of 0.1 m 2 / g or more and 10 m 2 / g or less.
[0026] In addition, in the present invention, the magnetite may have an average particle size in the range of 1 μm or more and 1000 μm or less.
[0027] In addition, in the present invention, the magnetite may have a bulk density in the range of 0.3 g / cm 3 or more and 3 g / cm 3 or less.
Advantages of the Invention
[0028] According to the present invention, it is possible to provide a method for producing carbon materials that can efficiently produce carbon materials by decomposing carbon dioxide with high reaction efficiency using a reducing agent with high reducing ability, a carbon material obtained thereby, a method for decomposing carbon dioxide that can decompose carbon dioxide with high reaction efficiency using a reducing agent with high reducing ability, and a reducing agent. [Brief explanation of the drawing]
[0029] [Figure 1] This is a flowchart showing a method for producing a carbon material according to the first embodiment of the present invention. [Figure 2] This is a schematic diagram showing the crystal structure of a quarter unit cell of magnetite. [Figure 3] This graph shows the results of Example 1. [Figure 4] This graph shows the results of Example 2. [Figure 5] This graph shows the results of Example 3. [Figure 6] This graph shows the results of Example 4. [Figure 7] This graph shows the results of Example 5. [Figure 8] This graph shows the results of Example 6. [Figure 9] This is an SEM image of the product after the reducing agent reacts with carbon dioxide. [Figure 10] This graph shows the measurement results of the oxygen defect degree δ in Example 7. [Figure 11] This graph shows the measurement results of the oxygen vacancy consumption rate in Example 7. [Figure 12] This graph shows the measurement results of the oxygen defect degree δ in Example 8. [Figure 13] This graph shows the measurement results of the oxygen vacancy consumption rate in Example 8. [Figure 14] This graph shows the results using nanoparticle magnetite in Example 9. [Figure 15] This graph shows the results using the fine-particle magnetite in Example 9. [Figure 16]This graph shows the results using powdered magnetite in Example 9. [Figure 17] This shows the XRD analysis results of the sample after hydrogen reduction in Example 10. [Figure 18] This shows the XRD analysis results of the sample after carbon dioxide decomposition in Example 10. [Figure 19] This shows the XRD analysis results of the sample after hydrogen reduction in Example 11. [Figure 20] This shows the XRD analysis results of the sample after carbon dioxide decomposition in Example 11. [Modes for carrying out the invention]
[0030] The following describes, with reference to the drawings, a method for producing a carbon material according to one embodiment of the present invention, the carbon material itself, a method for decomposing carbon dioxide, and a reducing agent. The embodiments described below are provided specifically to better illustrate the spirit of the invention and do not limit the present invention unless otherwise specified. Furthermore, the drawings used in the following description may be enlarged for convenience to make the features of the present invention easier to understand, and the dimensional ratios of each component may not be the same as in reality.
[0031] Figure 1 is a flowchart illustrating, step by step, a method for manufacturing a carbon material and a method for decomposing carbon dioxide according to one embodiment of the present invention. First, the reducing agent used in this embodiment will be described. The reducing agent is a material that reacts with carbon dioxide in the carbon generation process (carbon dioxide decomposition process) S1 described later to reduce carbon dioxide and decompose it into carbon and oxygen. The reducing agent used in this embodiment is Fe3O 4-δ We use an oxygen-depleted iron oxide of magnetite (triiron tetroxide) represented by (where δ is between 1 and 4), or oxygen-depleted iron (δ=4) obtained by completely reducing magnetite.
[0032] Figure 2 is a schematic diagram showing the crystal structure of a quarter unit cell of magnetite. Magnetite has a spinel-type crystal lattice structure crystallographically, and contains oxygen ions (O 2- ) are arranged in a cubic close-packed configuration, and in the gaps (Asite, Bsite), +3 valent iron (Fe +3 ), +2 valent iron (Fe 2+ The elements are arranged in a 2:1 ratio. Magnetite is represented by the general formula Fe3O4.
[0033] The reducing agent in this embodiment is an oxygen-depleted iron oxide (1 ≤ δ < 4) obtained by removing oxygen ions at arbitrary positions shown in Figure 2 while maintaining the crystal structure of magnetite, i.e., the spinel-type crystal lattice structure, or oxygen-completely depleted iron (δ = 4) obtained by completely reducing magnetite. Such reducing agents are produced in the reducing agent generation process described later.
[0034] Oxygen-depleted iron oxides are Fe3O 4-δ It is represented by δ, and the range of δ is set to between 1 and less than 4 depending on the proportion of oxygen ions removed from magnetite. Furthermore, when all oxygen ions are removed from magnetite (i.e., δ=4), it becomes the oxygen-depleted iron described above.
[0035] δ is defined as the oxygen defect degree, and it is the ratio of oxygen defects to magnetite in an oxygen-defective iron oxide that maintains the crystal structure of magnetite, i.e., the spinel-type crystal lattice structure. This oxygen defect degree δ can be calculated by measuring the difference between the mass of magnetite before and after the reaction with hydrogen in the reducing agent generation process S3. Since the amount of mass decrease (difference) is equal to the amount of oxygen released from the magnetite (the position of this released oxygen in the lattice becomes an atomic vacancy, i.e., a defect), the oxygen defect degree δ (δ=1~4) can be calculated from this amount of mass decrease.
[0036] Then, the areas where oxygen ions have detached from magnetite become atomic vacancies while maintaining the spinel-type crystal lattice structure. As a result, more cations are trapped within the crystal lattice, and the spacing between lattices widens. These atomic vacancies resulting from oxygen detachment cause a deoxygenation reaction, i.e., a reduction reaction, with carbon dioxide acting as a reducing agent.
[0037] Here, in order to maintain the activity of the obtained reducing agent, it is preferable to prevent oxidation of the reducing agent due to air mixing, etc., between the reducing agent generation step S3 and the carbon generation step S1. For example, if the reducing furnace and the carbon dioxide decomposition furnace are sealed to prevent air mixing while the reducing agent can be transferred, the reducing agent obtained in the reducing agent generation step S3 can be used in the carbon generation step S1 without oxidation.
[0038] The reducing agent (oxygen-depleted iron oxide, oxygen-completely depleted iron) in this embodiment only needs to have an average particle size greater than 1 μm, preferably between 1 μm and 20 μm, and also preferably between 50 μm and 200 μm.
[0039] Experimental results show that when the average particle size of the reducing agent is smaller than 1 μm, the proportion of carbon monoxide produced during the decomposition of carbon dioxide increases, resulting in a lower carbon recovery rate. By using a reducing agent with an average particle size of 1 μm or larger, a high carbon recovery rate can be maintained, and at the same time, the aggregation of reducing agent particles is reduced, thus avoiding problems such as adhesion to the reactor walls, making it possible to apply the technology to industrial reactors such as rotary kilns.
[0040] Furthermore, by keeping the average particle size of the reducing agent below 20 μm, a high reaction rate can be maintained. Also, when the average particle size of the reducing agent exceeds 50 μm but is 200 μm or less, the scattering of particles decreases and the fluidization performance improves, making it possible to apply it to industrial reactors such as fluidized beds. In this case, compared to rotary kiln type reactors, solid-gas contact and heat transfer are better, equipment costs are lower, and the size of the reactor can be made more compact.
[0041] The carbon material manufacturing method of this embodiment comprises a carbon generation step (carbon dioxide decomposition step) S1, a carbon separation step (carbon recovery step) S2, and a reducing agent generation step S3, and is a recycling system that repeatedly utilizes the reducing agent. Furthermore, the carbon dioxide decomposition method of this embodiment comprises a carbon generation step (carbon dioxide decomposition step) S1. The carbon generation process (carbon dioxide decomposition process) S1 involves reacting carbon dioxide (CO2) introduced from an external source with the aforementioned reducing agent to decompose the carbon dioxide into carbon and oxygen, while also oxidizing the reducing agent to magnetite.
[0042] The carbon generation process S1 involves decomposing (reducing) carbon dioxide by contacting a powdered reducing agent, for example, with gaseous carbon dioxide while stirring, using a reactor (carbon dioxide decomposition furnace) such as a fluidized bed or rotary kiln. While a circulating fluidized bed can also be used as the reactor, it has several disadvantages compared to a fluidized bed, including a higher overall reactor height, higher equipment costs, a more complex design and operation of the particle recirculation loop, shorter particle residence time (residence time in the reactor is on the order of seconds), limited particle size range for the reducing agent, accelerated particle wear, and high energy costs required to maintain high gas flow rates and circulate the powder.
[0043] The reaction temperature in carbon production step S1 may be in the range of 300°C or higher and 450°C or lower, preferably 350°C or higher and 450°C or lower. The reaction pressure may be in the range of 0.01 MPa or higher and 5 MPa or lower, preferably 0.1 MPa or higher and 1 MPa or lower. Thus, by setting the reaction temperature within a range of 300°C to 450°C, the reducing agent can maintain its spinel-type crystal lattice structure. If the reaction temperature is high, for example, above 500°C, there is a concern that repeated use of magnetite may cause the reducing agent to lose its spinel-type crystal lattice structure. In addition, the energy consumed during the reaction increases. If the reaction pressure is 0.01 MPa or higher, the reaction rate required for a practical process can be obtained. Furthermore, if it is 0.1 MPa or higher, it becomes possible to directly handle actual exhaust gas with low carbon dioxide concentrations. Also, if the reaction pressure is 5 MPa or lower, the manufacturing cost of the equipment can be reduced.
[0044] In the carbon generation process S1, it is also preferable to effectively utilize heat sources such as heat (waste heat) generated from the operation of carbon dioxide supply sources such as steel mills, thermal power plants, cement factories, and waste incineration facilities, electricity and heat storage derived from renewable energy, and thermal energy from high-temperature gas reactors, which are nuclear reactors capable of extracting high-temperature heat, in order to raise the temperature to this reaction temperature range.
[0045] In carbon production step S1, increasing the reaction temperature and pressure can increase the rate of carbon dioxide decomposition (reduction), thereby improving the efficiency of carbon dioxide treatment. On the other hand, if the reaction temperature is too high, the spinel structure of the reducing agent may be destroyed.
[0046] The decomposition of carbon dioxide in carbon production step S1 involves the following two-step reaction: (1) and (2). CO2→CO(intermediate product)+O 2- ...(1) CO → C+O 2- ...(2) Then, the oxygen produced in equations (1) and (2) above is inserted into the atomic vacancies of oxygen-depleted iron oxide (equation (3)) and oxygen-completely-depleted iron (equation (4)) in the following equations (3) and (4). Fe3O 4-δ +δO 2- →Fe3O4 (where δ = 1 or greater and less than 4) ... (3) 3Fe + 4O 2- →Fe3O4···(4)
[0047] In addition, in the carbon dioxide decomposition method of this embodiment, only the above formula (1) can be performed in the carbon generation step (carbon dioxide decomposition step) S1. The obtained carbon monoxide (CO) can be used as a raw material for obtaining useful chemical products such as hydrocarbons such as methane and methanol, and various resins, by hydrogenation.
[0048] In the carbon production step S1, if all carbon dioxide is reacted up to equation (2), no gas is produced as the final product. That is, it is thought that all the oxygen in the carbon dioxide is incorporated into either oxygen-depleted iron oxide or oxygen-completely depleted iron. Taking this into consideration, the reaction between carbon dioxide and oxygen-depleted iron oxide is represented by equation (5), and the reaction between carbon dioxide and oxygen-completely depleted iron is represented by equation (6). 2Fe3O 4-δ +δCO2→2Fe3O4+δC (where δ = 1 or greater and less than 4) ··(5) 3Fe + 2CO2 → Fe3O4 + 2C··(6)
[0049] The reason why oxygen-depleted iron oxides and oxygen-completely-depleted iron used as reducing agents in carbon production step S1 can decompose carbon dioxide into carbon is that these reducing agents have a spinel-type crystal lattice structure, which is a metastable crystal structure formed in a non-equilibrium state. Even at room temperature, they gradually react with oxygen, taking in oxygen ions and attempting to change into the more stable Fe3O4. In other words, it is thought that this occurs because the unstable spinel-type crystal lattice structure, which has atomic vacancies in the lattice, attempts to change into a more stable spinel-type crystal lattice structure without atomic vacancies.
[0050] During the stabilization (magnetization) process of these oxygen-depleted iron oxides and fully oxygen-depleted iron, when oxygen ions are incorporated into the crystal, the crystal attempts to maintain electrical neutrality by releasing electrons from its surface. In oxygen-depleted iron oxides and fully oxygen-depleted iron, +2 valent Fe(Fe 2+ Although it exists as an atom capable of releasing electrons, it is thought that the instability of oxygen-depleted iron oxide and oxygen-completely-depleted iron crystals generates an unusual reduction potential.
[0051] In carbon generation step S1, it is preferable to maintain the oxygen concentration in the reaction environment at 4% by volume or less in order to maximize the carbon dioxide decomposition capacity of the oxygen-depleted iron oxide or oxygen-depleted iron used as a reducing agent. If the oxygen concentration in the reaction environment in carbon generation step S1 is higher than 4% by volume, there is a concern that oxygen from the reaction atmosphere will be incorporated into the oxygen-depleted sites of the reducing agent (oxygen-depleted iron oxide or oxygen-depleted iron) before the oxygen constituting carbon dioxide can be incorporated into the reducing agent, thereby reducing the carbon dioxide decomposition capacity of the reducing agent.
[0052] In carbon production step S1, the carbon produced by the decomposition of carbon dioxide is generated as nano-sized particulate carbon material with a particle diameter of 1 μm or less. In carbon production step S1, under the same temperature conditions, the reaction rate of equation (1) is slower than the reaction rate of equation (2). However, by increasing the reaction rate of equation (1), the reaction of equation (2) proceeds rapidly, and fine nano-sized carbon particles can be produced. The reaction rates of equations (1) and (2) can be increased by increasing the oxygen defect degree δ and by increasing the reaction temperature and reaction pressure. These nano-sized particulate carbon particles either adhere to or form a coating on the surface of magnetite, which is produced when oxygen-depleted iron oxide or fully oxygen-depleted iron is oxidized.
[0053] On the other hand, in this embodiment, the reducing agent becomes magnetite (Fe3O4) through the decomposition of carbon dioxide in the carbon generation step S1, and hematite (Fe2O3) is not produced.
[0054] The carbon separation process (carbon recovery process) S2 separates the magnetite, which has carbon generated and attached to its surface, produced in the carbon generation process S1, i.e., the oxidized reducing agent, into carbon and magnetite. In this embodiment, carbon is formed in a state where it is relatively firmly attached to the surface of magnetite. Therefore, methods for separating carbon include, for example, physically scraping the carbon off the magnetite using impact force, shear force, or friction, followed by separation based on specific gravity or particle size; magnetic separation utilizing the ferromagnetism of magnetite, such as physical separation; and chemical separation, which involves selectively dissolving only the magnetite or only the carbon using strong acids or solvents.
[0055] In the case of physical separation, the separated magnetite can be used as a reducing agent raw material in the reducing agent generation process S3 described later. On the other hand, in chemical separation, for example, carbon can be easily obtained by dissolving magnetite with hydrochloric acid and recovering the carbon that does not dissolve in hydrochloric acid by solid-liquid separation such as filtration. In this case, magnetite cannot be directly used as a reducing agent raw material in the reducing agent generation step S3, and a step is required to return it to magnetite through the hydrolysis reaction of the generated iron chloride.
[0056] The carbon (carbon material) obtained through the above process is a nano-sized particulate carbon material with a particle size of 1 μm or less, and hardly any particles larger than 1 μm are produced. This nano-sized carbon powder is high-purity carbon with a purity of, for example, 99% or more, and can be directly used as carbon black, activated carbon, or graphite in functional carbon materials such as various catalysts, electrode materials, toners, and colorants.
[0057] The reducing agent generation step S3 removes oxygen ions contained in the magnetite separated in the carbon separation step S2 or in the magnetite introduced from the outside (deoxygenation reaction), thereby producing oxygen-depleted iron oxide or oxygen-completely-depleted iron, in which any position of the oxygen atom in the magnetite becomes a vacancy while maintaining the crystal structure of the magnetite, i.e., the spinel-type crystal lattice structure.
[0058] In the reducing agent generation process S3, when magnetite is introduced from an external source, the raw material for the magnetite (magnetite material) is not limited to pure magnetite; it may also contain other substances. For example, inexpensive and readily available iron sand can be used. Additionally, hematite (Fe2O3) and used hand warmers made using the iron oxidation method (whose main component is iron hydroxide) can also be used as magnetite materials.
[0059] The magnetite in this embodiment has a specific surface area of 0.1 m² as determined by the BET method. 2 / g or more, 10m 2 A range of less than or equal to / g, preferably 0.3m 2 / g or more, 8m 2 A range of less than or equal to / g, more preferably 1m 2 / g or more, 6m 2 The range is less than or equal to / g. The specific surface area of magnetite is 0.1m². 2 If the specific surface area of magnetite is 10 m² or more, the contact area between the solid and gas necessary for a solid-gas reaction can be secured, and the reaction rate required for a practical process can be obtained. 2 If the value is less than / g, a fast reaction rate can be ensured, and the proportion of carbon monoxide produced during the decomposition of carbon dioxide will be reduced, improving the carbon recovery rate.
[0060] Furthermore, the reducing agent obtained by reducing magnetite in the reducing agent generation step S3 of this embodiment has a larger specific surface area than the magnetite before reduction. The specific surface area of the reducing agent is 0.1 m². 2 / g or more, 30m 2 Less than or equal to / g, preferably 0.3m 2 / g or more, 25m 2 / g or less, more comfortably 1m 2 / g or more, 18m 2 The amount is less than or equal to / g. Furthermore, the specific surface area of the reducing agent is 1 or more and 3 or less than the specific surface area of magnetite, preferably 1 or more and 2.5 or less, and more preferably 1 or more and 2.0 or less.
[0061] Furthermore, the magnetite in this embodiment has an average particle diameter in the range of 1 μm or more and 1000 μm or less, preferably in the range of 1 μm or more and less than 20 μm, or in the range of more than 50 μm and 200 μm or less. If the average particle diameter of the magnetite is 1 μm or more, the proportion of carbon monoxide produced when decomposing carbon dioxide will be reduced, and the carbon recovery rate can be improved. Furthermore, by making the average particle diameter larger than 1 μm, the aggregation and scattering of particles will be reduced, and the fluidity and handling will be improved, so problems such as adhesion to the reactor wall and clinker formation can be avoided, making it possible to apply it to industrial reactors such as rotary kilns and fluidized beds. In addition, if the average particle diameter of the magnetite is 1000 μm or less, the contact area between the solid and gas necessary for solid-gas reactions can be secured, and the reaction rate required for a practical process can be obtained.
[0062] Furthermore, the magnetite in this embodiment has a bulk density of 0.3 g / cm³. 3 More than 3g / cm 3 The following range, preferably 0.4 g / cm³ 3 More than 2g / cm 3 The following range, more preferably 0.5 g / cm³ 3 More than 1g / cm 3 The range is as follows: Magnetite bulk density is 0.3 g / cm³ 3 If the above conditions are met, the particle cohesiveness and scattering will be reduced, and the fluidity will be improved, making it possible to apply it to industrial reactors such as rotary kilns and fluidized beds. 3 Under the following conditions, sufficient porosity can be ensured between and within particles, allowing the reactant gas to diffuse easily into the particles, and enabling the reaction rate required for a practical process to be obtained.
[0063] In the reducing agent generation step S3, a reaction apparatus (reduction furnace) such as a fluidized bed or rotary kiln is used to bring powdered magnetite material into contact with hydrogen gas while stirring. This causes oxygen atoms in the magnetite material to detach and react with hydrogen to produce water (water vapor). At the same time, the magnetite from which the oxygen atoms have detached retains its crystalline structure, i.e., the spinel-type crystal lattice structure, but the positions of the detached oxygen atoms become vacancies, forming oxygen-depleted iron oxide or oxygen-completely-depleted iron.
[0064] In the reducing agent generation process S3, if the magnetite material contains hematite, the hematite is reduced to magnetite, and then further reduced to oxygen-depleted iron oxide or oxygen-completely depleted iron.
[0065] The reaction temperature in the reducing agent generation step S3 can be in the range of 300°C or higher and 450°C or lower, preferably 350°C or higher and 400°C or lower. If the reaction temperature is 300°C or higher, the reaction rate required for a practical process can be obtained. Furthermore, if the reaction temperature is 450°C or lower, the crystal structure of the reducing agent will not be destroyed during the reaction, high reactivity can be maintained, and the reducing agent can be reused repeatedly. In addition, the energy consumption during the reaction can be reduced.
[0066] Furthermore, the reaction pressure in the reducing agent generation step S3 may be in the range of 0.1 MPa or more and 5 MPa or less, preferably 0.1 MPa or more and 1 MPa or less. If the reaction pressure is 0.1 MPa or more, the reaction rate required for a practical process can be obtained, and the size of the reaction apparatus can be made compact. Also, if the reaction pressure is 5 MPa or less, the manufacturing cost of the apparatus can be reduced.
[0067] The concentration of hydrogen gas used in the reducing agent generation step S3 should be in the range of 5% by volume or more and 100% by volume or less, preferably in the range of 10% by volume or more and 90% by volume or less. Even if the concentration of hydrogen gas is, for example, around 90% by volume, there is virtually no significant difference in reducing ability compared to hydrogen gas with a concentration of 100% by volume. Therefore, by using hydrogen gas with a concentration of around 90% by volume, which is less expensive than hydrogen gas with a concentration of 100% by volume, a reducing agent can be produced from magnetite at a low cost.
[0068] In the reduction of magnetite by hydrogen in the reducing agent generation step S3, the reducing agent is generated as follows. Fe3O4 + δH2 → Fe3O 4-δ +δH2O (where δ = 1 or greater and less than 4) ... (7) Fe3O4 + 4H2 → 3Fe + 4H2O ... (8)
[0069] The oxygen-depleted iron oxide obtained in the reducing agent generation step S3 is Fe3O 4-δ It is expressed as such, and δ is set to a range of 1 to less than 4 depending on the proportion of oxygen ions removed from magnetite. Furthermore, when all oxygen ions are removed from magnetite (i.e., δ=4), it becomes oxygen-depleted iron.
[0070] Then, the areas where oxygen ions have detached from magnetite become atomic vacancies while maintaining the magnetite's crystal structure, i.e., its spinel-type crystal lattice structure. As a result, more cations are trapped within the crystal lattice due to the detachment, and the spacing between lattices widens. These atomic vacancies resulting from oxygen detachment then act as a reducing agent in the carbon production process S1, causing a deoxygenation reaction of carbon dioxide.
[0071] According to the carbon material manufacturing method of this embodiment described above, the crystal structure of magnetite is maintained, and an oxygen-defective iron oxide (Fe3O) with many atomic vacancies due to the departure of oxygen atoms is produced. 4-δ By using oxygen-defective iron (δ=4), obtained by completely reducing magnetite (where δ=1 or greater and less than 4), as a reducing agent to reduce carbon dioxide, nano-sized carbon particles can be produced efficiently and at low cost.
[0072] Furthermore, by supplying the magnetite material (oxidized reducing agent) remaining after carbon separation in carbon separation step S2 to reducing agent generation step S3, and converting it back into a reducing agent using hydrogen, a closed system can be constructed to decompose carbon dioxide and produce carbon materials, thereby contributing to the reduction of carbon dioxide emissions, a greenhouse gas.
[0073] Furthermore, in the carbon generation process (carbon dioxide decomposition process) S1, the carbon separation process S2, and the reducing agent generation process S3, for example, by effectively utilizing the heat (waste heat) generated as a result of the operation of steel mills, thermal power plants, cement factories, and waste incineration facilities as a heat source during the reaction, the amount of waste heat released into the atmosphere can be suppressed, contributing to the prevention of global warming. In addition, by effectively utilizing electricity and heat storage derived from renewable energy, as well as the thermal energy of high-temperature gas reactors, which are reactors that can extract high-temperature heat, CO2 emissions can be suppressed, contributing to the realization of carbon neutrality and a decarbonized society.
[0074] While embodiments of the present invention have been described above, these embodiments are presented as examples only and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their variations are included in the scope and spirit of the invention, as well as in the claims and their equivalents.
[0075] For example, in the embodiment described above, the general composition of magnetite is given as Fe3O4, but the magnetite material used in this embodiment may contain other substances, such as titanium (Ti). Such other substances, such as titanium, may contribute to the reduction of carbon dioxide as a catalyst. [Examples]
[0076] The effects of the present invention were verified below. The properties of each magnetite material used in the examples are summarized in Table 1.
[0077] [Table 1]
[0078] (Example 1) We conducted an experiment to investigate the relationship between the reaction temperature and the degree of oxygen deficiency δ in the reducing agent production process. A fixed-bed reactor was used as the reaction apparatus, and 1 g of magnetite (average particle size approximately 800 nm, specific surface area 10.2 m² by BET method) was added. 2 / g, bulk density 0.7g / cm³ 3 A reducing agent was produced by reacting it with hydrogen to reduce magnetite while maintaining its crystal structure. Furthermore, the particle size distribution and average particle size of magnetite can be confirmed using a particle size distribution analyzer (MT3300EXII: manufactured by Microtrac-Bell Co., Ltd.), and the crystal structure can be confirmed using an X-ray diffractometer (D2 PHASER: manufactured by Bruker Co., Ltd.).
[0079] With a reaction time of 1 hour, a hydrogen flow rate of 1.0 L / min, and a hydrogen concentration of 100% by volume, the reaction temperatures were set to 280°C, 300°C, 320°C, 350°C, 360°C, and 370°C, respectively. By reducing magnetite with hydrogen (deoxygenation reaction), samples (reducing agents) were obtained at each reaction temperature. For the reducing agents obtained at each reaction temperature (oxygen-depleted iron oxide, oxygen-completely depleted iron), the degree of oxygen deficiency δ of the reducing agent was calculated by considering the amount of mass reduction before and after the reaction as the amount of oxygen removed from the magnetite. The results of Example 1 are shown graphically in Figure 3. Note that points in Figure 3 where the oxygen defect degree δ exceeds 4 are due to measurement errors, and the actual value of δ is effectively 4. This point is also true for the following examples.
[0080] As shown in Figure 3, by setting the reaction temperature to a range of 320°C to 360°C under the reaction conditions described above, the oxygen defect degree δ can be maximized, and it was confirmed that oxygen-completely defective iron (δ=4), which is obtained by completely reducing magnetite, can be acquired with δ=4.
[0081] (Example 2) We conducted an experiment to investigate the relationship between reaction time and oxygen deficiency degree δ in the reducing agent generation process.
[0082] Reaction temperatures were set to 280°C, 310°C, 330°C, and 350°C, and reaction times to 30 minutes, 60 minutes, and 180 minutes. By reducing magnetite with hydrogen, reducing agents were obtained at each reaction temperature and time. The oxygen deficiency degree δ of the reducing agent was then calculated. All conditions other than reaction temperature and reaction time were the same as in Example 1. The results of Example 2 are shown in a graph in Figure 4.
[0083] As shown in Figure 4, under the reaction conditions described above, if the reaction temperature is 330°C or higher, the oxygen vacancy degree δ can be maximized by extending the reaction time (reduction time) to over 60 minutes, resulting in δ=4, i.e., oxygen-deficient iron obtained by completely reducing magnetite. Furthermore, it was confirmed that if the reaction temperature is in the range of 330°C to 350°C, oxygen-deficient iron oxides maintaining the magnetite crystal structure with δ=2 to 2.8 can be obtained even with a reaction time of about 30 minutes.
[0084] (Example 3) We conducted an experiment to investigate the relationship between hydrogen flow rate and oxygen deficiency degree δ in the reducing agent generation process.
[0085] With a reaction temperature of 330°C, hydrogen flow rates were set to 0.1 L / min, 0.25 L / min, 0.5 L / min, 0.75 L / min, and 1.0 L / min, respectively. Samples were obtained for each hydrogen flow rate by reducing magnetite with hydrogen. The oxygen defect degree δ of the reducing agent was then calculated. All conditions other than the reaction temperature and hydrogen flow rate were the same as in Example 1. The results of Example 3 are shown graphically in Figure 5. The oxygen deficiency degree δ, as described in Reference 1, is also included for reference.
[0086] As shown in Figure 5, it was confirmed that under the reaction conditions described above, if the hydrogen flow rate is 0.75 L / min or higher, the oxygen defect degree δ can be maximized, resulting in δ=4, i.e., oxygen-deficient iron. Furthermore, it was confirmed that even with a hydrogen flow rate of around 0.5 L / min, oxygen-deficient iron oxides with a δ of 3.5 or higher can be obtained.
[0087] (Example 4) We conducted an experiment to investigate the relationship between hydrogen concentration and oxygen deficiency degree δ in the reducing agent generation process.
[0088] With a reaction temperature of 330°C, samples were obtained at hydrogen concentrations of 50%, 75%, 90%, and 100% by volume by reducing magnetite with hydrogen. The oxygen defect degree δ of the reducing agent was then calculated from each obtained reducing agent. All conditions other than the reaction temperature and hydrogen concentration were the same as in Example 1. The results of Example 4 are shown in a graph in Figure 6.
[0089] As shown in Figure 6, it was confirmed that under the reaction conditions described above, if the hydrogen concentration is 90 vol% or higher, the oxygen deficiency degree δ can be maximized, resulting in δ=4, i.e., oxygen-completely deficient iron. Even at a hydrogen gas concentration of around 90 vol%, there is virtually no difference in reducing ability compared to hydrogen gas at a concentration of 100 vol%. By using hydrogen gas at a concentration of around 90 vol% which is less expensive than hydrogen gas at 100 vol%, a reducing agent with the oxygen deficiency degree δ maximized can be produced at low cost. Furthermore, it was confirmed that even at a hydrogen gas concentration of around 75 vol%, oxygen-deficient iron oxide with δ=3.5 or higher can be obtained.
[0090] (Example 5) We conducted an experiment to investigate the relationship between reaction temperature and oxygen vacancy consumption rate in the carbon production process. The oxygen vacancy consumption rate is the percentage of oxygen ions from carbon dioxide that are incorporated into atomic vacancies in the spinel-type crystal lattice structure of a reducing agent when a certain amount of reducing agent is reacted with carbon dioxide. This rate ranges from 0 to 100%, and the closer this value is to 100%, the higher the carbon dioxide decomposition (reduction) capacity of the reducing agent.
[0091] A fixed-bed reactor was used as the reaction apparatus, and carbon was produced by reacting carbon dioxide with a reducing agent (oxygen-completely deficient iron) with an oxygen deficiency degree δ of approximately 4 at a reaction temperature of 315°C to 390°C. The oxygen deficiency consumption rate was then calculated based on the difference between the mass of the reducing agent and oxygen deficiency degree δ before the reaction and the mass of the oxidized reducing agent (magnetite) and oxygen deficiency degree δ after the reaction. The results of Example 5 are shown in a graph in Figure 7.
[0092] As shown in Figure 7, under the reaction conditions described above, the oxygen vacancy consumption rate is 40% or higher when the reaction temperature is 360°C or higher. In particular, when the reaction temperature is 370°C or higher, the oxygen vacancy consumption rate is 50% or higher, and oxygen ions from carbon dioxide can be incorporated into more than 50% of the total number of atomic vacancies in the lattice of the spinel-type crystal lattice structure of the reducing agent. Therefore, it was confirmed that by setting the reaction temperature in the carbon production process to 360°C or higher, carbon can be efficiently produced by decomposing carbon dioxide using the reducing agent.
[0093] (Example 6) We conducted experiments to investigate the relationship between the type of magnetite material and the oxygen vacancy consumption rate in the carbon generation process and the oxygen vacancy degree δ in the reducing agent generation process.
[0094] As magnetite materials, we prepared 1g and 0.5g of nanoparticle magnetite with an average particle size of approximately 800nm, 0.5g of fine particle magnetite with an average particle size of approximately 1.1μm, 1g of iron sand from Japan, and 1g of iron sand from New Zealand. Using each of these magnetite materials, we used a fixed-bed reactor as the reaction apparatus, and reduced each magnetite material to produce reducing agents under the conditions of a reaction temperature of 350°C, a reaction time of 1 hour, a hydrogen flow rate of 1.0 L / min, and a hydrogen concentration of 100% by volume. The oxygen deficiency degree δ of these reducing agents was then calculated.
[0095] Furthermore, when the specific surface area of the reducing agent obtained by reducing fine magnetite particles was measured, it was found to be 9.36 m². 2 It was / g. 5.28m before reduction. 2 From the values per gram, it can be seen that the specific surface area has increased by approximately 1.77 times.
[0096] Next, using each reducing agent, a fixed-bed reactor was used as the reaction apparatus, and carbon dioxide was reacted at a reaction temperature of 360°C. The oxygen deficiency consumption rate was calculated based on the difference between the mass of the reducing agent and the oxygen deficiency degree δ before the reaction and the mass of the oxidized reducing agent and the oxygen deficiency degree δ after the reaction. The results of Example 6 are shown graphically in Figure 8. Figure 9 shows an SEM image of the product after reacting the reducing agent (δ=4), produced by hydrogen reduction of fine magnetite particles, with carbon dioxide.
[0097] As shown in Figure 8, it was confirmed that most of the reducing agents produced by hydrogen reduction using nanoparticle magnetite and fine particle magnetite had an oxygen deficiency degree δ of 4, resulting in oxygen-completely deficient iron where almost all the oxygen in the magnetite had been removed, leaving atomic vacancies. On the other hand, iron sand from New Zealand had an oxygen deficiency degree δ of less than 1 after hydrogen reduction, indicating that it has low carbon dioxide decomposition (reduction) capacity as a reducing agent.
[0098] Furthermore, the oxygen vacancy consumption rate of these reducing agents was approximately 60% to 80% for those prepared using fine-particle magnetite, confirming their particularly superior carbon dioxide decomposition ability. From these results, it was found that using fine-particle magnetite with an average particle size of approximately 1.1 μm is particularly preferable as the magnetite material.
[0099] Furthermore, the SEM image shown in Figure 9 reveals that the white areas of the amorphous product are oxidized reducing agent, and the black areas are nano-sized carbon particles. This confirms that when the reducing agent reacts with carbon dioxide, carbon is produced so that it adheres to the surface of the reducing agent.
[0100] (Example 7) We conducted experiments to investigate the particle size of magnetite material, the degree of oxygen deficiency δ in the reducing agent generation process, and the oxygen deficiency consumption rate in the carbon generation process. As magnetite materials, we prepared nanoparticle magnetite with an average particle size of approximately 800 nm, fine particle magnetite with an average particle size of approximately 1.1 μm, powdered magnetite with an average particle size of approximately 40 μm, and large-particle powdered magnetite with an average particle size of approximately 70 μm. Each of these magnetite materials was reduced at a reaction temperature of 330°C to produce reducing agents, and the oxygen defect degree δ of these reducing agents was calculated. The conditions other than the reaction temperature were the same as in Example 6.
[0101] Next, carbon dioxide was reacted with each reducing agent at a reaction temperature of 380°C, and the oxygen vacancy consumption rate was calculated. All conditions other than the reaction temperature were the same as in Example 6. Figure 10 shows the measurement results for the oxygen deficiency degree δ in Example 7, and Figure 11 shows the measurement results for the oxygen deficiency consumption rate.
[0102] As shown in Figure 10, the reducing agent obtained by hydrogen reduction shows almost no difference depending on the particle size of the raw material magnetite. On the other hand, as shown in Figure 11, the oxygen vacancy consumption rate after reacting these reducing agents with carbon dioxide is particularly superior for the reducing agent made from fine-particle magnetite. Therefore, it was found that it is preferable to produce the reducing agent using fine-particle magnetite as the raw material.
[0103] (Example 8) We conducted experiments to investigate the relationship between the raw materials for the reducing agent, the degree of oxygen deficiency δ in the reducing agent production process, and the oxygen deficiency consumption rate in the carbon production process. As magnetite materials, we prepared nanoparticle magnetite with an average particle size of approximately 800 nm, fine particle magnetite with an average particle size of approximately 1 μm, powdered magnetite with an average particle size of approximately 40 μm, iron sand from Japan, iron sand from New Zealand, copper slag, and iron powder. Then, under the same conditions as in Example 6, we calculated the oxygen defect degree δ of these reducing agents. Note that since the iron powder was in a completely reduced state, we arbitrarily set δ = 4.
[0104] Next, carbon dioxide was reacted with each reducing agent under the same conditions as in Example 6, and the oxygen vacancy consumption rate was calculated. The measurement results for the oxygen deficiency degree δ in Example 8 are shown in Figure 12, and the measurement results for the oxygen deficiency consumption rate are shown in Figure 13.
[0105] As shown in Figure 12, the reducing agents obtained by hydrogen reduction, those made from magnetite, all have a value of 3.5 or higher, indicating excellent performance. On the other hand, the oxygen defect degree δ of copper slag is almost 0.
[0106] On the other hand, as shown in Figure 13, the oxygen vacancy consumption rate after reacting these reducing agents with carbon dioxide was particularly superior for the reducing agent made from fine magnetite particles. Furthermore, copper slag and iron powder showed an oxygen vacancy consumption rate of almost 0%, indicating that they have no ability to decompose (reduce) carbon dioxide. The difference in oxygen vacancy consumption rates between domestically produced iron sand and New Zealand iron sand is thought to be due to the catalytic effect of trace amounts of titanium contained in domestically produced iron sand.
[0107] (Example 9) Experiments were conducted to investigate whether the reducing agent deteriorated and the amount of carbon produced when the reducing agent generation process and the carbon generation process were repeatedly performed for different particle sizes of magnetite material. A reducing agent was produced using the same magnetite material and reaction conditions as in Example 7, and its mass was measured (reducing agent production step).
[0108] Next, carbon dioxide was decomposed using each reducing agent at a reaction temperature of 380°C, and the mass of the reducing agent + product (carbon) after the reaction was measured. Note that no carbon separation step was performed after the carbon generation step; the generated carbon was left as is. This reducing agent generation step and carbon generation step were repeated three times with each reducing agent, and the mass of the sample was measured at each step. In Example 9, the results using nanoparticle magnetite are shown in Figure 14, the results using fine particle magnetite are shown in Figure 15, and the results using powdered magnetite are shown in Figure 16.
[0109] As shown in Figures 14 to 16, regardless of the particle size of magnetite used as the raw material for the reducing agent, the mass of carbon measured by combustion-infrared absorption increased almost linearly with each repeated reduction agent generation process and carbon generation process. This confirmed that there was no degradation of the reducing agent, and that the reducing agent could be reused to perform multiple reduction agent generation and carbon generation processes. Furthermore, when fine particle magnetite or powdered magnetite was used as the raw material for the reducing agent, the increase in carbon mass was larger compared to when nanoparticle magnetite was used. Considering that this increase is due to carbon accumulation, it was confirmed that it is preferable to use fine particle magnetite or powdered magnetite as the raw material for the reducing agent.
[0110] On the other hand, when nanoparticle magnetite was used as a raw material for the reducing agent, the mass of carbon was almost halved when the reducing agent production process was performed after the carbon generation process, suggesting that the generated carbon was gasified and removed from the system. However, no such loss due to the reaction of generated carbon was observed with fine particle magnetite or powdered magnetite. From this, it was found that because nanoparticle magnetite has high reaction activity and a large surface area, the generated and attached carbon easily reacts with oxygen in the reducing agent or hydrogen in the reducing agent production process, and carbon loss is likely to occur with repeated use. From the perspective of such carbon gasification loss, it was confirmed that it is preferable to use fine particle magnetite or powdered magnetite as a raw material for the reducing agent.
[0111] (Example 10) We conducted an experiment to investigate the carbon dioxide decomposition performance when hematite (Fe2O3) is used as the magnetite material. As a sample, powdered α-Fe2O3 (average particle size 1 μm, purity 99.9% by mass (manufactured by Kojun Chemical Laboratory)) was used. As a pretreatment, the temperature was raised to 110°C under argon gas flow conditions, held for 10 minutes, then suctioned to create a vacuum, and held for another 10 minutes.
[0112] Using the pre-treated sample obtained in this way, a fixed-bed reactor was used as the reaction apparatus, and the sample was reduced to produce a reducing agent under the conditions of a reaction temperature of 330°C, a reaction time of 1 hour, a hydrogen flow rate of 1.0 L / min, and a hydrogen concentration of 100% by volume, and the mass of the reduced agent was measured. Table 2 shows the mass changes of the sample before pretreatment, after pretreatment, and after hydrogen reduction. For reference, the mass changes when magnetite is used as the raw material are also included. Furthermore, Figure 17 shows the XRD analysis results of the sample after hydrogen reduction, and Figure 18 shows the XRD analysis results of the sample after carbon dioxide decomposition.
[0113] [Table 2]
[0114] According to the results shown in Table 2, the weight change due to hydrogen reduction suggests that hematite is completely reduced to an oxygen-depleted iron state.
[0115] Furthermore, XRD analysis results indicate that the product is almost entirely Fe, suggesting that the hematite is completely reduced to an oxygen-depleted iron state.
[0116] Next, using the hematite-derived reducing agent obtained, carbon dioxide was decomposed at a reaction temperature of 370°C until there was no pressure change. The change in the amount of substance in the gas phase was calculated using the ideal gas law based on the pressure and temperature inside the reactor, and the mass of the product (carbon) was measured by combustion-infrared absorption method (carbon production process). Table 3 shows the changes in the amount of gaseous substance after the decomposition of carbon dioxide, the mass of the product (carbon), and the change in the amount of gaseous substance per mole of iron in the reducing agent. For reference, the case when magnetite is used as the raw material is also included.
[0117] [Table 3]
[0118] As shown in Table 3, it was confirmed that carbon dioxide can be decomposed using a reducing agent obtained by hydrogen reduction of hematite. Furthermore, the fact that the hematite-derived reducing agent was black after the decomposition of carbon dioxide, and the results of XRD analysis, suggest that even if the reducing agent is hematite-derived, it is only oxidized to magnetite after the decomposition of carbon dioxide (it does not revert back to hematite).
[0119] (Example 11) An experiment was conducted to investigate the carbon dioxide decomposition performance using a powder containing iron hydroxide extracted from used hand warmers as a raw material for generating a reducing agent. As used hand warmers, we used "Pokapoka Kazoku Regular 10-pack (PKN-10R)" manufactured by Iris Ohyama Co., Ltd. As a pretreatment, the temperature was raised to 110°C under argon gas flow conditions, held for 10 minutes, then suctioned to create a vacuum, and held for another 10 minutes.
[0120] The pre-treated used hand warmers (in powder form) obtained in this manner were reduced using a fixed-bed reactor under the following conditions: reaction temperature 330°C, reaction time 1 hour, hydrogen flow rate 1.0 L / min, and hydrogen concentration 100% by volume to produce a reducing agent, and its mass was measured. Table 4 shows the mass changes of the sample before and after pretreatment, and before and after hydrogen reduction. For reference, the mass changes when hematite is used as the raw material are also listed. Furthermore, Figure 19 shows the XRD analysis results of the sample after hydrogen reduction, and Figure 20 shows the XRD analysis results of the sample after carbon dioxide decomposition.
[0121] [Table 4]
[0122] Since the reducing agent derived from used hand warmers after hydrogen reduction was black, similar to the reducing agents derived from magnetite and hematite, it is thought that the used hand warmers were reduced to a state of completely oxygen-deficient iron. Furthermore, XRD analysis results indicate that the product is almost entirely Fe, suggesting that the iron hydroxide in used hand warmers is reduced to a state of oxygen-depleted iron.
[0123] Next, the reducing agent obtained from used hand warmers was used to decompose carbon dioxide at a reaction temperature of 370°C until there was no pressure change, and the mass was measured. The mass changes of the sample before and after carbon dioxide decomposition are shown in Table 4 above.
[0124] As shown in Table 4, it was confirmed that carbon dioxide can be decomposed using a reducing agent obtained by hydrogen reduction of used hand warmers. Furthermore, the fact that the reducing agent was black after the decomposition of carbon dioxide, and the results of XRD analysis, suggest that even if the reducing agent is derived from used hand warmers, it is only oxidized to magnetite (not returned to iron hydroxide) after the decomposition of carbon dioxide. [Industrial applicability]
[0125] This invention can be applied to various plants that emit large amounts of carbon dioxide, such as steel plants, thermal power plants, cement manufacturing plants, and waste incineration facilities, to reduce carbon dioxide emissions and, incidentally, to produce high value-added carbon materials such as nano-sized particulate carbon. Therefore, it has industrial applicability.
Claims
1. An oxide having at least one of oxygen deficiency represented by Fe3O4-δ (where δ is 1 or more and less than 4) and oxygen deficiency (δ=4), A reducing agent having an oxygen defect consumption rate of 40% or more after a reduction reaction with carbon dioxide at 360°C.
2. The reducing agent described in claim 1, characterized in that the average particle diameter is in the range of 1 μm or more and 500 μm or less.