Method of producing glass article
Patent Information
- Application Number
- JP2022051634
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-10-30
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Devitrification derived from yttrium-containing oxides occurs during the down-draw method for glass ribbon formation, leading to defects in glass articles due to the diffusion of yttrium oxide and TiO2 in molten glass, which affects production efficiency and quality.
A method involving a down-draw process with a Mg-rich layer, preferably spinel (MgAl2O4), formed on an alumina-based molded body to suppress the diffusion of yttrium-containing oxides, using a diffusion suppression layer to prevent reactions with TiO2 in the molten glass.
Effectively reduces devitrification from yttrium-containing oxides, ensuring high-quality glass articles with suppressed ultraviolet transmittance and preventing coloring, suitable for applications like cover glass for solar cells in outer space.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for manufacturing a glass article. [Background technology]
[0002] In the manufacturing process of glass articles such as glass sheets and glass rolls, for example, a down-draw method is used to continuously form a glass ribbon by causing molten glass to flow down along the surface of a forming body. The formed glass ribbon is cooled to approximately room temperature while being transported downstream, and then cut into predetermined lengths to obtain glass sheets, or wound into a roll to obtain a glass roll (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 2018-062433 Summary of the Invention [Problem to be solved by the invention]
[0004] In the above-mentioned compact, in order to improve the mechanical strength, an yttrium-containing oxide (e.g., a composite oxide of yttrium and aluminum, YAlO) is used as a constituent of the compact. 12 ) may be added.
[0005] As a result of extensive research, the present inventors have discovered for the first time the problem that when a glass ribbon containing TiO2 is formed using a formed body containing such an yttrium-containing oxide, yttrium oxide (YO3) dissolves from the yttrium-containing oxide, which is an additive of the formed body, into the molten glass and diffuses, causing devitrification. Since such devitrification products derived from the yttrium-containing oxide can cause defects in the glass ribbon and / or glass article, it is important to reduce their generation in terms of production efficiency and quality improvement. It is believed that the devitrification products derived from the yttrium-containing oxide are generated by a reaction between yttrium oxide diffused into the molten glass and TiO2 in the molten glass. In other words, the devitrification products derived from the yttrium-containing oxide are believed to be devitrification products containing yttrium oxide and TiO2 (YO3-TiO2 crystals).
[0006] An object of the present invention is to reliably reduce the generation of devitrified matter originating from yttrium-containing oxides contained in a formed body when a glass ribbon is formed using a down-draw method. [Means for solving the problem]
[0007] (1) The present invention, which has been invented to solve the above-mentioned problems, is a method for manufacturing a glass article, which includes a forming step of forming a glass ribbon by a down-draw method, in which a first molten glass containing TiO2 is caused to flow along the surface of a formed body containing an yttrium-containing oxide, and the formed body is characterized in that it has an Mg-rich layer containing magnesium on the surface of the formed body.
[0008] In this way, an Mg-rich layer is formed on the surface of the formed body. The Mg-rich layer functions as a diffusion-suppressing layer that suppresses the diffusion of the yttrium-containing oxide. Therefore, the yttrium-containing oxide contained in the formed body can be reliably suppressed from diffusing into the first molten glass. Therefore, the reaction between the yttrium-containing oxide contained in the formed body and TiO2 contained in the first molten glass is less likely to occur, and the generation of devitrified products derived from the yttrium-containing oxide can be reliably reduced.
[0009] (2) In the above configuration (1), it is preferable that the compact is an alumina-based compact, and the Mg-rich layer contains spinel as a main component.
[0010] In this way, since the alumina-based compact contains alumina, it becomes easier to form an Mg-rich layer containing spinel (MgAl2O4) as a main component on the surface of the compact.
[0011] (3) In the above configuration (1) or (2), the first molten glass preferably contains MgO.
[0012] This makes it easier to form and maintain a Mg-rich layer on the surface of the compact.
[0013] (4) In the above configurations (1) to (3), a forming step may be further provided as a pre-forming step of forming a Mg-rich layer on the surface of the formed body by causing a second molten glass containing MgO to flow down along the surface of the formed body.
[0014] In this way, a sufficient Mg-rich layer can be formed on the surface of the compact before the compacting step.
[0015] (5) In the above configurations (1) to (4), it is preferable that the first molten glass contains, as a glass composition, in mass%, 50 to 80% SiO2, 3 to 25% Al2O3, 0 to 20% B2O3, 0 to 25% Li2O3 + Na2O + K2O, 0 to 20% MgO, 0 to 20% CaO, 0 to 20% SrO, 0 to 20% BaO, 0 to 1% As2O3, 0.0001 to 2% SnO2, and 0.001 to 10% TiO2, and that the mass ratio SnO2 / (As2O3 + SnO2) is 0.001 to 1.
[0016] In this way, there is a possibility that devitrification may occur due to the inclusion of TiO2, but application of the present invention can reliably suppress this and provide a high-quality glass article. Furthermore, a glass article made of the above glass composition can suppress ultraviolet transmittance while preventing coloration due to ultraviolet light, and can be suitably used, for example, as a cover glass for solar cells used in outer space (glass substrate for space solar power generation), etc. [Effects of the Invention]
[0017] According to the present invention, when a glass ribbon is formed using a down-draw method, it is possible to reliably reduce the generation of devitrified substances originating from yttrium-containing oxides contained in a formed body. [Brief explanation of the drawings]
[0018] [Figure 1] 1 is a longitudinal sectional view of a glass article manufacturing apparatus according to an embodiment of the present invention. [Figure 2] FIG. 2 is an enlarged longitudinal cross-sectional view showing the periphery of a molded body of the glass article manufacturing apparatus according to the embodiment of the present invention. [Figure 3] 3 is a vertical cross-sectional view showing a step of forming an Mg-rich layer on the surface of the compact of FIG. 2. FIG. DETAILED DESCRIPTION OF THE INVENTION
[0019] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings, in which the X direction is the horizontal direction and the Z direction is the vertical direction.
[0020] 1, the glass article manufacturing apparatus according to this embodiment is an apparatus for manufacturing a glass sheet Gp as a glass article. The manufacturing apparatus includes a processing apparatus 1 for a glass ribbon G, a cutting apparatus 2, and an inspection apparatus 3.
[0021] The processing device 1 includes a forming zone 11 for continuously forming a glass ribbon G, a heat treatment zone 12 for heat treating (slowly cooling) the glass ribbon G, a cooling zone 13 for cooling the glass ribbon G to near room temperature, and roller pairs 14 arranged in multiple vertical stages in each of the forming zone 11, the heat treatment zone 12, and the cooling zone 13.
[0022] The forming zone 11 and the heat treatment zone 12 are constituted by furnaces in which the transport path of the glass ribbon G is surrounded by walls, and heating devices such as heaters for adjusting the temperature of the glass ribbon G are arranged at appropriate locations within the furnaces. On the other hand, the cooling zone 13 is open to the external atmosphere at room temperature without the transport path of the glass ribbon G being surrounded by walls, and no heating device such as a heater is arranged therein. By passing through the heat treatment zone 12 and the cooling zone 13, the glass ribbon G is given a desired thermal history.
[0023] In the internal space of the forming zone 11, a forming body 15 is disposed, which forms a glass ribbon G from a first molten glass Gm1 by an overflow downdraw method. Here, the first molten glass Gm1 refers to molten glass for forming the glass ribbon G that will become a product. The first molten glass Gm1 supplied to the forming body 15 overflows from a groove (not shown) formed in a top portion 15a of the forming body 15, and the overflowing first molten glass Gm1 flows along both side surfaces 15b, which have a wedge-shaped cross section, of the forming body 15 and joins (is fused and integrated) at a lower end 15c, thereby continuously forming a plate-shaped glass ribbon G. The formed glass ribbon G is in a longitudinal position (preferably a vertical position). Note that the glass ribbon G and the glass sheet Gp have substantially the same glass composition as the first molten glass Gm1. As a result of the joining (is fused and integrated), a mating surface is formed inside the glass ribbon G and the glass sheet Gp (for example, at the center in the thickness direction).
[0024] The compact 15 is made of an yttrium-containing oxide (e.g., YAlO, which is a composite oxide of yttrium and aluminum) in order to ensure mechanical strength. 12). In the present embodiment, the formed body 15 is an alumina-based formed body containing an yttrium-containing oxide. The alumina-based formed body containing an yttrium-containing oxide preferably has an alumina content of 90 to 98 mass % and an yttrium-containing oxide content of 2 to 10 mass %. The formed body 15 may also be a zircon-based formed body. However, in the case of a zircon-based formed body, when a first molten glass Gm1 having a specific tempered glass composition is allowed to flow down, zirconia derived from the formed body 15 may be mixed into the first molten glass Gm1, which may cause defects in the glass ribbon G and / or the glass sheet Gp. Therefore, from the viewpoint of preventing the occurrence of defects due to such zirconia, the formed body 15 is more preferably an alumina-based formed body.
[0025] The internal space of the heat treatment zone 12 has a predetermined temperature gradient downward. The glass ribbon G in the vertical position is heat-treated (slowly cooled) so that its temperature decreases as it moves downward through the internal space of the heat treatment zone 12. This heat treatment reduces internal strain in the glass ribbon G. The temperature gradient in the internal space of the heat treatment zone 12 can be adjusted, for example, by a heating device provided on the inner wall surface of the heat treatment zone 12.
[0026] The multiple roller pairs 14 are configured to clamp both widthwise ends of the glass ribbon G in a vertical position from both the front and back sides. Of the multiple roller pairs 14, the roller pair arranged at the top is a cooling roller 14a equipped with an internal cooling mechanism. Note that, in the internal space of the heat treatment zone 12, the multiple roller pairs 14 may include rollers that do not clamp both widthwise ends of the glass ribbon G. In other words, the distance between the opposing roller pairs 14 may be made larger than the sheet thickness of both widthwise ends of the glass ribbon G, and the glass ribbon G may pass between the roller pairs 14.
[0027] In this embodiment, both widthwise ends of the glass ribbon G obtained by the processing device 1 include portions (hereinafter also referred to as "ear portions") that are thicker than the widthwise central portion due to the influence of shrinkage during the molding process, etc.
[0028] The cutting device 2 includes a scribe line forming device 21 and a breaking device 22, and is configured to cut the glass ribbon G in a vertical position that has descended from the processing device 1 in the width direction at predetermined lengths. In this way, glass plates Gp are sequentially cut out from the glass ribbon G.
[0029] The glass plate Gp is a glass substrate (mother glass plate) from which one or more product glass plates are obtained. The thickness of the glass plate Gp is, for example, 0.2 mm to 10 mm, and the size of the glass plate Gp is, for example, 700 mm × 700 mm to 3000 mm × 3000 mm. The glass plate Gp is used as a substrate or cover glass in, for example, a display or a solar cell. The substrate and cover glass are not limited to a flat shape and may also be curved.
[0030] The scribe line forming device 21 is a device that forms a scribe line S on one of the front and back surfaces of the glass ribbon G at a scribe line forming position P1 provided below the processing device 1. In this embodiment, the scribe line forming device 21 includes a wheel cutter 23 that forms a scribe line S on one of the front and back surfaces of the glass ribbon G along its width direction, and a support member 24 (e.g., a support bar or a support roller) that supports the other of the front and back surfaces of the glass ribbon G at a position corresponding to the wheel cutter 23.
[0031] The wheel cutter 23 and the support member 24 are configured to descend following the descending glass ribbon G, while forming a scribe line S across the entire width or a portion of the width of the glass ribbon G. In this embodiment, the scribe line S is also formed at both widthwise ends including the ear portions where the plate thickness is relatively large. The scribe line S may also be formed by irradiating a laser or the like.
[0032] The slicing device 22 is a device that slicing the glass ribbon G along the scribe line S at a slicing position P2 provided below the scribe line formation position P1 to obtain a glass sheet Gp. In this embodiment, the slicing device 22 includes a slicing member 25 that abuts against the formation region of the scribe line S from the side where the scribe line S is not formed, and a chuck 26 that grips a lower region of the glass ribbon G below the slicing position P2.
[0033] The breaking member 25 descends following the descending glass ribbon G, and is composed of a plate-like body (surface plate) having a flat surface that comes into contact with the entire width or part of the width direction of the glass ribbon G. The contact surface of the breaking member 25 may be a curved surface that is curved in the width direction.
[0034] A plurality of chucks 26 are provided at both widthwise ends of the glass ribbon G, spaced apart in the longitudinal direction of the glass ribbon G. All of the plurality of chucks 26 provided at each widthwise end are held by the same arm (not shown). As each arm operates, the plurality of chucks 26 follow the descending glass ribbon G and perform an operation to bend the glass ribbon G using the breaking member 25 as a fulcrum. This applies bending stress to the scribe line S and its vicinity, breaking the glass ribbon G in the width direction along the scribe line S. As a result, a glass sheet Gp is cut out from the glass ribbon G. The cut glass sheet Gp is transferred from the chuck 26 to a chuck 28 of another conveying device 27, and then conveyed in a vertical position along the width direction (the left-right direction along the surface of the glass sheet Gp). Note that the conveying direction of the glass sheet Gp by the conveying device 27 is not limited to the width direction and can be set to any direction. The chucks 26, 28 may be changed to another holding method, such as negative pressure suction. The method for cutting the glass ribbon G is not limited to scribing, and other methods such as laser cutting or laser melting may be used.
[0035] The inspection device 3 is a device that inspects for the presence or absence of defects. Defects include, for example, devitrification caused by yttrium-containing oxides. Note that the inspection device 3 may be configured to measure, for example, thickness deviation (sheet thickness), streaks (striae), and the type, position (coordinates), and size of defects (e.g., bubbles, foreign matter, etc.) of the glass sheet Gp, in addition to the devitrification caused by yttrium-containing oxides.
[0036] The inspection device 3 inspects glass plates Gp cut out from the glass ribbon G. In this embodiment, the inspection device 3 includes a light source 31 arranged at a fixed position on one of the front and back surfaces of the glass plate Gp, and a sensor 32 arranged at a fixed position on the other of the front and back surfaces of the glass plate Gp. The light source 31 irradiates light toward the glass plate Gp, and the sensor 32 receives the light irradiated from the light source 31 and transmitted through the glass plate Gp. The inspection device 3 detects the presence or absence of defects based on a change in the amount of light received by the sensor 32.
[0037] The area that can be inspected by the light source 31 and the sensor 32 of the inspection device 3 is a line extending in the Z direction. The inspection area by the light source 31 and the sensor 32 is scanned over the entire surface of each of the front and back surfaces of the glass plate Gp by moving the glass plate Gp with the conveying device 27. This allows the glass plate Gp to be inspected for defects.
[0038] In the present embodiment, the first molten glass Gm1 (glass ribbon G) is, for example, an aluminosilicate glass or alkali-free glass containing TiO2. The content of TiO2 in the first molten glass Gm1 is, for example, 0.001% or more by mass.
[0039] Specifically, the first molten glass Gm1 preferably contains, as a glass composition, in mass %, 50 to 80% SiO2, 3 to 25% Al2O3, 0 to 20% B2O3, 0 to 25% Li2O + Na2O + KO, 0 to 20% MgO, 0 to 20% CaO, 0 to 20% SrO, 0 to 20% BaO, 0 to 1% As2O3, 0.0001 to 2% SnO2, and 0.001 to 10% TiO2, with a mass ratio of SnO2 / (As2O3 + SnO2) of 0.001 to 1. A glass plate Gp produced from the first molten glass Gm1 having such a glass composition can suppress ultraviolet transmittance while preventing coloration due to ultraviolet rays, and can be suitably used, for example, as a cover glass for solar cells used in outer space (glass substrate for space solar power generation), etc.
[0040] The reasons for limiting the content range of each component as described above are explained below. Note that the % indication below refers to % by mass unless otherwise specified.
[0041] SiO2 is a component that forms a network, and its content is preferably 50 to 80%, more preferably 55 to 75%, even more preferably 55 to 70%, and particularly preferably 55 to 65%. A high SiO2 content increases high-temperature viscosity, reduces melting properties, and tends to facilitate the precipitation of devitrified cristobalite particles. On the other hand, a low SiO2 content reduces weather resistance and makes vitrification more difficult.
[0042] Al2O3 is a component that increases the strain point and Young's modulus and suppresses the precipitation of devitrified cristobalite particles, and its content is preferably 3 to 25%, more preferably 5 to 23%, even more preferably 7 to 21%, even more preferably 9 to 18%, particularly preferably 11 to 17%, and most preferably 13 to 17%. A high Al2O3 content tends to increase the liquidus temperature, making it difficult to form into a thin plate. On the other hand, a low Al2O3 content tends to decrease the strain point and Young's modulus, increase high-temperature viscosity, and reduce meltability.
[0043] B2O3 acts as a flux, lowering viscosity and improving meltability. Its content is preferably 5 to 20%, more preferably 7 to 15%, even more preferably 8 to 13%, particularly preferably 8 to 12%, and most preferably 8 to 11%. A high B2O3 content tends to lower the strain point and Young's modulus, and to reduce weather resistance. On the other hand, a low B2O3 content increases the liquidus temperature, making it difficult to mold into a thin plate. Furthermore, high-temperature viscosity increases, tending to reduce meltability.
[0044] Li2O, Na2O, and K2O are components that adjust the thermal expansion coefficient and reduce high-temperature viscosity. The total amount of these components (Li2O + Na2O + K2O) is preferably 0 to 25%, more preferably 1 to 20%, even more preferably 10 to 18%, and most preferably 12 to 18%. If the total amount of these components is too large, the strain point decreases, making heat resistance more likely to decrease. Furthermore, the thermal expansion coefficient may become too large, potentially impairing compatibility with surrounding components. The Li2O content is preferably 0 to 10%, more preferably 0 to 5%, even more preferably 0 to 3%, and most preferably 0 to 0.5%. The Na2O content is preferably 0 to 25%, more preferably 5 to 20%, even more preferably 10 to 18%, and most preferably 12 to 16%. The K2O content is preferably 0 to 10%, more preferably 0 to 5%, even more preferably 0 to 3%, and most preferably 0 to 0.5%.
[0045] MgO is a component that improves meltability without lowering the strain point, and its content is preferably 0 to 20%, more preferably 0 to 7%, even more preferably 0 to 5%, particularly preferably 0 to 3%, and most preferably 0 to 2%. If the MgO content is high, the liquidus temperature will be high, making it difficult to form into a thin plate, the thermal expansion coefficient will be high, impairing compatibility with surrounding components, and the density will be high. On the other hand, if the MgO content is low, the strain point and Young's modulus will be low, and high-temperature viscosity will be high, making it difficult to melt. From the viewpoint of forming and maintaining a Mg-rich layer MR (described in detail below) on the surface of the compact 15, the MgO content is preferably 0.3% or more.
[0046] CaO is a component that improves meltability without lowering the strain point, and its content is preferably 0 to 20%, more preferably 0 to 12%, even more preferably 3 to 10%, and particularly preferably 3 to 9%. If the CaO content is too high, the liquidus temperature will be high, making molding difficult, the thermal expansion coefficient will be high, impairing compatibility with surrounding components, and the density will be high. On the other hand, if the CaO content is too low, the strain point and Young's modulus will be low, and high-temperature viscosity will be high, making melting difficult.
[0047] SrO is a component that improves meltability without lowering the strain point, and its content is preferably 0 to 20%, more preferably 0 to 9%, even more preferably 0.5 to 8%, and particularly preferably 0.5 to 7%. If the SrO content is too high, the liquidus temperature will be high, making molding difficult, the thermal expansion coefficient will be high, impairing compatibility with surrounding components, and the density will be high. On the other hand, if the SrO content is too low, the strain point and Young's modulus will be low, and the high-temperature viscosity will be high, making melting difficult.
[0048] BaO is a component that improves meltability without lowering the strain point, and its content is preferably 0 to 20%, more preferably 0 to 8%, even more preferably 0 to 5%, and particularly preferably 0 to 3%. If the BaO content is too high, the liquidus temperature will be high, making molding difficult, the thermal expansion coefficient will be high, impairing compatibility with surrounding members, and the density will be high. If the BaO content is too low, the strain point and Young's modulus will be low, and the high-temperature viscosity will be high, making melting difficult.
[0049] Although the inclusion of a mixture of alkaline earth metal oxides, MgO, CaO, SrO, and BaO, can improve melting properties and devitrification resistance, increasing the content of these components tends to increase density, making it difficult to reduce the weight of the glass substrate. Therefore, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is preferably 0 to 30%, more preferably 0 to 20%, even more preferably 0 to 15%, and particularly preferably 0 to 10%.
[0050] The Fe2O3 content is 0 to 0.05%, preferably 0.0001 to 0.05%, more preferably 0.0001 to 0.03%, even more preferably 0.005 to 0.02%, and most preferably 0.005 to 0.015%. If the Fe2O3 content is too high, the visible light transmittance may be too low. If the Fe2O3 content is too low, the ultraviolet light transmittance may be too high.
[0051] As2O3 is a clarifier, but also a component that promotes solarization (changes in properties due to the influence of light irradiation, such as discoloration due to ultraviolet rays). The content of As2O3 is preferably 0 to 1%, more preferably 0 to 0.8%, even more preferably 0 to 0.5%, particularly preferably 0 to 0.3%, and most preferably 0 to 0.005%.
[0052] SnO2 is a component that suppresses solarization. Its content is preferably 0.0001 to 2%, more preferably 0.001 to 1.5%, even more preferably 0.01 to 1%, particularly preferably 0.05 to 0.5%, and most preferably 0.05 to 0.3%. If the SnO2 content is too high, devitrification resistance tends to decrease. On the other hand, if the SnO2 content is too low, it becomes difficult to obtain the above effects. Note that, although an SnO2 raw material may be used as the SnO2 source, it is also acceptable to incorporate SnO2 from trace components contained in other raw materials.
[0053] To ensure the effect of suppressing solarization, it is important to strictly control the mass ratio SnO2 / (As2O3+SnO2), and the value is preferably 0.001 to 1, 0.01 to 1, 0.1 to 1, 0.3 to 1, 0.5 to 1, 0.7 to 1, 0.9 to 1, and particularly 1.
[0054] TiO2 is a component that reduces ultraviolet transmittance and has the effect of suppressing solarization. Furthermore, as the TiO2 content increases, devitrification products derived from yttrium-containing oxides are more likely to occur, and the effect of suppressing devitrification according to the present invention becomes more pronounced. The TiO2 content is preferably 0.001 to 10%, more preferably 0.02 to 8%, even more preferably 0.5 to 6%, particularly preferably 1 to 5%, and most preferably 2 to 4.5%. Note that as the TiO2 content increases, devitrification resistance tends to decrease.
[0055] CeO2 is a component that reduces ultraviolet transmittance and has the effect of suppressing solarization. Its content is preferably 0.001 to 10%, more preferably 0.02 to 8%, even more preferably 0.5 to 6%, particularly preferably 1 to 5%, and most preferably 2 to 4.5%. Note that, if the CeO2 content is high, devitrification resistance is likely to decrease.
[0056] In addition to the above components, other components may be incorporated in a total amount as needed.
[0057] ZnO is a component that increases Young's modulus and improves meltability. Its content is preferably 0 to 10%, more preferably 0 to 5%, even more preferably 0 to 3%, particularly preferably 0 to 1%, and most preferably 0 to 0.5%. When the ZnO content is high, the density and thermal expansion coefficient tend to increase. Also, the devitrification resistance and strain point tend to decrease.
[0058] ZrO2 is a component that improves weather resistance. Its content is preferably 0 to 2%, more preferably 0 to 1%, even more preferably 0 to 0.5%, particularly preferably 0 to 0.2%, and most preferably 0 to 0.1%. If the ZrO2 content is high, devitrified particles of zircon tend to precipitate.
[0059] Sb2O3 is a component that acts as a fining agent. Its content is preferably 0 to 2%, more preferably 0 to 1.5%, even more preferably 0 to 1%, and particularly preferably 0 to 0.5%. As the Sb2O3 content increases, the density tends to increase.
[0060] Cl is a component that acts as a fining agent. Its content is preferably 0 to 1%, more preferably 0 to 0.5%. If the Cl content is high, more Cl is evaporated from the glass melt, making striae more likely to occur.
[0061] Rare earth oxides such as Nb2O5 and La2O3 are components that increase Young's modulus. However, the raw materials themselves are expensive and they also reduce devitrification resistance. Therefore, the content of rare earth oxides is preferably 3% or less, 2% or less, 1% or less, and particularly 0.5% or less.
[0062] 2, the compact 15 has an Mg-rich layer MR containing magnesium on its surface (for example, the top 15a and the side surface 15b). The Mg-rich layer MR functions as a diffusion suppression layer that suppresses the diffusion of the yttrium-containing oxide contained in the compact 15.
[0063] The Mg-rich layer MR means a layer having a high concentration of magnesium. The magnesium content in the Mg-rich layer MR is preferably, for example, 1 mass % or more.
[0064] The Mg-rich layer MR preferably contains spinel (MgAl2O4) as a main component. If the compact 15 is an alumina-based compact as in this embodiment, the compact 15 contains alumina, which makes it easier to form the Mg-rich layer MR containing spinel on the surface of the compact 15. When the Mg-rich layer MR contains spinel as a main component in this way, the upper limit of the Mg content in the Mg-rich layer MR is 17 mass%. Therefore, regardless of whether the Mg-rich layer MR contains spinel as a main component, the Mg content in the Mg-rich layer MR is preferably 17 mass% or less.
[0065] The thickness of the Mg-rich layer MR is preferably 100 μm or less, more preferably 20 μm to 100 μm, and most preferably 50 μm to 100 μm.
[0066] Next, a method for manufacturing a glass article according to this embodiment will be described. This manufacturing method is a method for manufacturing a glass plate Gp as a glass article using the above-mentioned manufacturing apparatus.
[0067] As shown in FIG. 1, the manufacturing method includes a molding step, a heat treatment step, a cooling step, a cutting step, and an inspection step.
[0068] The forming step is a step of forming a glass ribbon G in the forming zone 11 .
[0069] The heat treatment step is a step in which the glass ribbon G that has been subjected to the forming step is subjected to heat treatment in the heat treatment zone 12.
[0070] The cooling step is a step of cooling the glass ribbon G that has been subjected to the heat treatment step in the cooling zone 13.
[0071] The cutting step is a step in which the glass ribbon G that has been subjected to the cooling step is conveyed and cut in the width direction by a cutting device 2 to obtain glass sheets Gp.
[0072] The inspection step is a step of inspecting the glass plate Gp for defects (including devitrified matter derived from yttrium-containing oxides) using an inspection device 3 or the like. Note that, before the inspection step, a cutting step of cutting off the edge portions of the glass plate Gp may be performed.
[0073] As shown in FIG. 2, in the forming step, a first molten glass Gm1 is caused to flow down along the surface of a formed body 15 containing an yttrium-containing oxide, thereby continuously forming a glass ribbon G.
[0074] A Mg-rich layer MR is formed on the surface of formed body 15 as a diffusion-suppressing layer that suppresses diffusion of the yttrium-containing oxide contained in formed body 15. That is, the Mg-rich layer MR can reliably suppress diffusion of the yttrium-containing oxide contained in formed body 15 into first molten glass Gm1 during the forming step. As a result, reaction between yttrium oxide diffused from the yttrium-containing oxide contained in formed body 15 into the first molten glass Gm1 and TiO2 contained in the first molten glass Gm1 is less likely to occur, and the generation of devitrified products derived from the yttrium-containing oxide (for example, Y2O3-TiO2 crystals) can be reliably reduced.
[0075] When the first molten glass Gm1 contains 0.3 mass % or more of MgO, it is possible to suppress the diffusion of magnesium ions from the Mg-rich layer MR into the first molten glass Gm1. In other words, it is possible to suppress the Mg-rich layer MR from being reduced, disappearing, or altered due to the diffusion of magnesium ions. Therefore, it is possible to stably maintain the Mg-rich layer MR on the surface of the formed body 15. Note that when the first molten glass Gm1 does not substantially contain MgO, the Mg-rich layer MR is likely to be reduced, but the Mg-rich layer MR can suppress the diffusion of yttrium-containing oxides contained in the formed body 15 into the first molten glass Gm1 during the period until the Mg-rich layer MR disappears. In other words, the Mg-rich layer MR can be used as a diffusion-suppressing layer even when the first molten glass Gm1 does not substantially contain MgO.
[0076] As shown in FIG. 3, the present manufacturing method further includes a forming step of forming an Mg-rich layer MR as a pre-step of the molding step.
[0077] In the forming step, the second molten glass Gm2 containing MgO is caused to flow down along the surface of the formed body 15, thereby forming the Mg-rich layer MR.
[0078] Specifically, when the second molten glass Gm2 containing MgO is caused to flow down along the surface of the formed body 15, magnesium ions diffuse from the second molten glass Gm2 into the formed body 15, and an Mg-rich layer MR is formed on the surface of the formed body 15. Thereafter, as the diffusion of magnesium ions from the second molten glass Gm2 into the formed body 15 continues, the thickness of the Mg-rich layer MR increases to a predetermined thickness. As a result, the Mg-rich layer MR is sufficiently formed on the surface of the formed body 15. During this process, the yttrium-containing oxide contained in the surface of the formed body 15 diffuses into the second molten glass Gm2, and the content of the yttrium-containing oxide in the Mg-rich layer MR decreases, for example, to between 0% and 0.1% by mass.
[0079] In this embodiment, since the formed body 15 is an alumina-based formed body, in the above-described forming step, the alumina of the formed body 15 reacts with the MgO of the second molten glass Gm2 to form an Mg-rich layer MR containing spinel as a main component.
[0080] The second molten glass Gm2 is, for example, an aluminosilicate glass or alkali-free glass containing MgO. The second molten glass Gm2 preferably has a glass composition containing MgO that is the same as or similar to that of the first molten glass Gm1 used in forming the glass ribbon G that will become the product. Alternatively, the second molten glass Gm2 is preferably a glass containing MgO that is substantially free of TiO (for example, a TiO content of less than 0.001%).
[0081] When the second molten glass Gm2 is substantially free of TiO2, even if a glass ribbon is formed in the forming step while the second molten glass Gm2 is caused to flow down along the surface of the forming body 15, no devitrified matter derived from yttrium-containing oxides is generated in the obtained glass ribbon. Therefore, it becomes possible to stably obtain glass substrates from the obtained glass ribbon.
[0082] From the viewpoint of promoting the formation of the Mg-rich layer MR, the MgO content of the second molten glass Gm2 is preferably 1 mass % or more, and more preferably 2 mass % or more. When the first molten glass Gm1 and the second molten glass Gm2 have different glass compositions, the MgO content of the second molten glass Gm2 is preferably higher than the MgO content of the first molten glass Gm1.
[0083] When the first molten glass Gm1 and the second molten glass Gm2 have different glass compositions, it is preferable to perform a base material changing step after forming the Mg-rich layer MR, in which the molten glass supplied to the forming body 15 is gradually changed from the second molten glass Gm2 to the first molten glass Gm1. The forming step starts after the base material changing step is completed.
[0084] The method for forming the Mg-rich layer MR is not limited to this, and the Mg-rich layer MR may be formed by, for example, sputtering.
[0085] Although the glass article manufacturing apparatus and manufacturing method according to an embodiment of the present invention have been described, the embodiment of the present invention is not limited to this, and various modifications can be made without departing from the spirit of the present invention.
[0086] In the above embodiment, if the Mg-rich layer MR disappears during the molding process, the forming process may be performed again to form a new Mg-rich layer MR. In other words, the forming process and the molding process may be repeated alternately.
[0087] In the above-described embodiment, the glass plate Gp may be a chemically strengthened glass made of aluminosilicate glass. In this case, a strengthening step of chemically strengthening the glass plate Gp is carried out, for example, at the customer's site.
[0088] In the above embodiment, the glass article is a glass plate Gp. However, the glass article may be, for example, a glass roll obtained by winding a glass ribbon G into a roll. [Explanation of symbols]
[0089] 1 Processing equipment 2 Cutting device 3 Inspection equipment 11 Forming Zone 12 Heat Treatment Zone 13 Cooling Zone 14a Roller pair (cooling roller) 15 Molded body 21 Scribe line forming device 22 Folding device 23 Wheel cutter 24 Support member 25 Breaking parts 27 Transport equipment G Glass ribbon Gm1 First molten glass Gp glass plate MR Mg-rich layer
Claims
1. By the down-draw method, TiO 2 A method for producing a glass article, comprising a forming step of forming a glass ribbon by flowing a first molten glass comprising the The method for producing a glass article, wherein the molded body has a Mg-rich layer containing magnesium on a surface of the molded body.
2. The molded body is an alumina-based molded body, The method for producing a glass article according to claim 1 , wherein the Mg-rich layer contains spinel as a main component.
3. The method for producing a glass article according to claim 1 or 2, wherein the first molten glass contains MgO.
4. The method for producing a glass article according to any one of claims 1 to 3, further comprising a forming step, as a preceding step of the forming step, of forming the Mg-rich layer on a surface of the formed body by flowing a second molten glass containing MgO down along the surface of the formed body.
5. The first molten glass has a glass composition, in mass%, of SiO 2 50-80%, Al 2 O 3 3-25%, B 2 O 3 0-20%, Li 2 O+Na 2 O+K 2 O 0-25%, MgO 0-20%, CaO 0-20%, SrO 0-20%, BaO 0-20%, As 2 O 3 0-1%, SnO 2 0.0001-2%, TiO 2 Contains 0.001 to 10% by mass of SnO 2 / (As 2 O 3 + SnO 2 5. The method for producing a glass article according to claim 1, wherein the value of n is 0.001 to 1.