Gas barrier coating material and gas barrier laminate
Patent Information
- Application Number
- JP2022090376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-06-02
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2042-06-02
AI Technical Summary
Conventional gas barrier materials require high-temperature, long-time crosslinking processes, which reduce productivity and can lead to a decrease in barrier properties, and there is a lack of technologies that balance productivity and barrier performance effectively.
A gas barrier coating material containing polycarboxylic acid, polyamine compound, and Zn compound, with specific mole ratios and optional crosslinking agents, is used for low-temperature, short-time heat treatment to form a gas barrier laminate with improved barrier properties.
The solution provides a gas barrier material with enhanced balance between productivity and barrier properties, maintaining excellent gas barrier performance even after retort treatment.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a coating material for gas barrier and a gas barrier laminate.
Background Art
[0002] As a gas barrier material, a laminate in which an inorganic layer, which is a gas barrier layer, is provided on a base material layer is used. However, this inorganic layer is weak against friction and the like, and in such a gas barrier laminate, cracks may occur in the inorganic layer due to rubbing or stretching during post-processing such as printing, lamination, or filling of contents, resulting in a decrease in gas barrier properties. Therefore, as a gas barrier material, a laminate using an organic layer as a gas barrier layer is also used.
[0003] As a gas barrier material using an organic layer as a gas barrier layer, a laminate having a gas barrier layer formed of a mixture containing a polycarboxylic acid and a polyamine compound is known. Examples of technologies related to such a gas barrier laminate include those described in Patent Documents 1 and 2.
[0004] Patent Document 1 (Japanese Patent Application Laid-Open No. 2005-225940) discloses a gas barrier film having a gas barrier layer formed from a polycarboxylic acid and a polyamine and / or a polyol, and having a crosslinking degree of the polycarboxylic acid of 40% or more. The document describes that such a gas barrier film has excellent gas barrier properties similar to those under low humidity conditions even under high humidity conditions.
[0005] Patent Document 2 (Japanese Patent Publication No. 2013-10857) discloses a film in which a mixture of polyamine and polycarboxylic acid, obtained by mixing polyamine / polycarboxylic acid in a weight ratio of 12.5 / 87.5 to 27.5 / 72.5, is coated on at least one side of a substrate made of plastic film. The same document states that such a gas barrier film has excellent gas barrier properties, particularly oxygen barrier properties, even after boiling, and also has excellent flexibility, transparency, moisture resistance, chemical resistance, etc. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2005-225940 [Patent Document 2] Japanese Patent Publication No. 2013-10857 [Overview of the Initiative] [Problems that the invention aims to solve]
[0007] The required level of technology for various properties of gas barrier materials is constantly increasing. The present inventors have investigated conventional gas barrier materials, such as those described in Patent Documents 1 and 2. As a result, it became clear that gas barrier materials such as those described in Patent Documents 1 and 2 may have reduced productivity because they require high-temperature, long-duration heating to crosslink the polycarboxylic acid and polyamine. Furthermore, it has become clear that if the heating temperature for crosslinking polycarboxylic acid and polyamine is lowered or the heat treatment time is shortened to improve productivity, the proportion of amide bonds formed by the crosslinking of polycarboxylic acid and polyamine may decrease, resulting in a reduction in barrier properties. From these findings, the inventors discovered that conventional gas barrier materials have room for improvement in terms of balancing productivity and barrier properties. While many technologies have focused on improving barrier performance, no technology has been reported to date that balances barrier properties and productivity.
[0008] This invention has been made in view of the above circumstances, and provides a gas barrier coating material in which productivity and barrier properties are improved by low-temperature, short-time heat treatment. [Means for solving the problem]
[0009] According to the present invention, the following gas barrier coating material and gas barrier laminate are provided.
[0010] [1] A gas barrier coating material comprising a polycarboxylic acid, a polyamine compound, and a Zn compound, A gas barrier coating in which the ratio of (number of moles of Zn compound in the gas barrier coating) to (number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating) is 0.40 or more and 0.70 or less. [2] The gas barrier coating material described in [1] above, Furthermore, it is a gas barrier coating material that also contains a crosslinking agent. [3] The gas barrier coating material described in [2] above, A gas barrier coating material comprising one or more compounds selected from the group consisting of epoxysilane compounds, carbodiimide compounds, and isocyanate compounds as the crosslinking agent. [4] A gas barrier coating material as described in any of the above [1] to [3], A gas barrier coating material comprising one or more compounds selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid, as the polycarboxylic acid. [5] A gas barrier coating material according to any one of [1] to [4] above, The gas barrier coating material, wherein the polyamine compound contains one or more compounds selected from the group consisting of polyallylamine, polyvinylamine, polyethyleneimine, and poly(trimethyleneimine). [6] A gas barrier coating material according to any one of [1] to [5] above, The gas barrier coating material further containing a polyphosphoric acid compound or a salt thereof. [7] The gas barrier coating material according to [6] above, The gas barrier coating material, wherein (the number of moles of P contained in the polyphosphoric acid compound or a salt thereof in the gas barrier coating material) / (the number of moles of COO- groups contained in the polycarboxylic acid in the gas barrier coating material) in the gas barrier coating material is 0.005 or more and 0.20 or less. [[ID=十六]][8] A gas barrier coating material according to any one of [1] to [7] above, The gas barrier coating material, wherein (the number of moles of amino groups contained in the polyamine compound in the gas barrier coating material) / (the number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating material) in the gas barrier coating material is 0.40 or more and 0.70 or less. [9] Comprising a base material layer and a gas barrier layer provided on at least one surface of the base material layer, The gas barrier laminate, wherein the gas barrier layer contains a cured product of the gas barrier coating material according to any one of [1] to [8] above. The gas barrier laminate according to
[11] above, wherein when the inorganic layer has an interlayer on the base material layer or between the base material layer and the inorganic layer, the inorganic layer is a vapor deposition film provided on the interlayer and is composed of one or more inorganic substances selected from the group consisting of silicon oxide, aluminum oxide, and aluminum, the gas barrier laminate.
Advantages of the Invention
[0011] According to the present invention, it is possible to provide a gas barrier material in which the balance between productivity and barrier properties is improved by heat treatment at a low temperature for a short time. <00ooo101>
Brief Description of the Drawings
[0012] [Figure 1] It is a cross-sectional view schematically showing an example of the structure of the gas barrier laminate in the embodiment
Embodiments for Carrying Out the Invention
[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The drawings are schematic views and do not match the actual dimensional ratios. In this specification, "~" between numbers in the text represents from above to below and includes both end values unless otherwise specified. In this specification, (meth)acrylic means at least one of acrylic and methacrylic. In the present embodiment, the composition can include each component alone or in combination of two or more. <00001ll6>
[0014] The gas barrier coating material of the present embodiment is a gas barrier coating material containing a polycarboxylic acid, a polyamine compound, and a Zn compound, and (the number of moles of the Zn compound in the gas barrier coating material) / (the number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating material) in the gas barrier coating material is 0.40 or more and 0.70 or less.
[0015] The gas barrier coating material of this embodiment contains a polycarboxylic acid, a polyamine compound, and a Zn compound, thereby providing a gas barrier material with improved barrier properties, such as oxygen barrier properties and water vapor barrier properties, before and after retort treatment. Furthermore, by including a larger amount of Zn compound in the gas barrier coating material of this embodiment, such that (number of moles of Zn compound in the gas barrier coating material) / (number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating material) is 0.40 or more and 0.70 or less, compared to conventional methods, it is possible to provide a gas barrier material with improved barrier properties even with low-temperature, short-time heat treatment compared to conventional manufacturing methods.
[0016] In the gas barrier coating material of this embodiment, the ratio of (number of moles of Zn compound in the gas barrier coating material) to (number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating material) is 0.40 or higher, preferably 0.41 or higher, and more preferably 0.42 or higher, from the viewpoint of further improving the gas barrier performance after retort treatment. From a similar viewpoint, the ratio of (moles of Zn compound in the gas barrier coating) to (moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating) is 0.70 or less, preferably 0.60 or less, and more preferably 0.50 or less.
[0017] The components contained in the gas barrier coating material of this embodiment will be described in detail.
[0018] (Polycarboxylic acid) The polycarboxylic acid contained in the gas barrier coating material of this embodiment has two or more carboxyl groups in its molecule. Specifically, examples include homopolymers of α,β-unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, fumaric acid, crotonic acid, cinnamic acid, 3-hexenoic acid, and 3-hexenodioic acid, or copolymers thereof. Alternatively, the α,β-unsaturated carboxylic acid may be a copolymer of the above α,β-unsaturated carboxylic acid with esters such as ethyl esters, olefins such as ethylene, etc.
[0019] Among these, homopolymers or copolymers thereof of acrylic acid, methacrylic acid, itaconic acid, fumaric acid, crotonic acid, and cinnamic acid are preferred, more preferably one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid, even more preferably at least one polymer selected from polyacrylic acid and polymethacrylic acid, and still more preferably at least one polymer selected from acrylic acid homopolymers and methacrylic acid homopolymers.
[0020] In this embodiment, polyacrylic acid includes both homopolymers of acrylic acid and copolymers of acrylic acid and other monomers. In the case of copolymers of acrylic acid and other monomers, polyacrylic acid contains, for example, 90% or more by mass, preferably 95% or more by mass, and more preferably 99% or more by mass of constituent units derived from acrylic acid in 100% by mass of the polymer. Furthermore, in this embodiment, polymethacrylic acid includes both homopolymers of methacrylic acid and copolymers of methacrylic acid and other monomers. In the case of copolymers of methacrylic acid and other monomers, polymethacrylic acid contains, for example, 90% or more by mass, preferably 95% or more by mass, and more preferably 99% or more by mass of constituent units derived from methacrylic acid in 100% by mass of the polymer.
[0021] Polycarboxylic acids are polymers formed by the polymerization of carboxylic acid monomers. From the viewpoint of achieving an excellent balance between gas barrier properties and handling ease, the molecular weight of polycarboxylic acids is preferably 500 to 2,500,000, more preferably 5,000 to 2,000,000, more preferably 10,000 to 1,500,000, even more preferably 100,000 to 1,200,000, even more preferably 300,000 to 1,100,000, even more preferably 500,000 to 1,000,000, and even more preferably 600,000 to 900,000. In this embodiment, the molecular weight of the polycarboxylic acid is the weight-average molecular weight on a polyethylene oxide basis, and can be measured using gel permeation chromatography (GPC).
[0022] The polycarboxylic acid may be at least partially neutralized with a volatile base. Neutralizing the polycarboxylic acid with a volatile base can suppress gelation when the polycarboxylic acid is mixed with a Zn compound or a polyamine compound. Therefore, from the viewpoint of preventing gelation, it is preferable to partially or completely neutralize the carboxyl group of the polycarboxylic acid with a volatile base. The neutralized product can be obtained by partially or completely neutralizing the carboxyl group of the polycarboxylic acid with a volatile base, that is, by partially or completely converting the carboxyl group of the polycarboxylic acid into a carboxylate salt. This prevents gelation when adding polyamine compounds or Zn compounds. Partially neutralized products can be prepared by adding a volatile base to an aqueous solution of a polycarboxylic acid polymer, and the desired degree of neutralization can be achieved by adjusting the ratio of polycarboxylic acid to volatile base. In this embodiment, the degree of neutralization of the polycarboxylic acid by the volatile base is preferably 70 to 300 equivalents, more preferably 90 to 250 equivalents, and even more preferably 100 to 200 equivalents, from the viewpoint of sufficiently suppressing gelation caused by the neutralization reaction with the amino group of the polyamine compound.
[0023] Any water-soluble base can be used as the volatile base. Examples of volatile bases include ammonia, morpholine, alkylamines, tertiary amines such as 2-dimethylaminoethanol, N-methylmonophorine, ethylenediamine, and triethylamine, or aqueous solutions thereof, or mixtures thereof. From the viewpoint of obtaining good gas barrier properties, aqueous ammonia is preferred.
[0024] (Polyamine compounds) The gas barrier coating material of this embodiment contains a polyamine compound. By including a polyamine compound, the barrier properties of the resulting gas barrier material can be improved. Polyamine compounds are compounds having two or more amino groups in their main chain, side chain, or terminal, and are preferably polymers. Specifically, examples include aliphatic polyamines such as polyallylamine, polyvinylamine, polyethyleneimine, and poly(trimethyleneimine); polyamides having amino groups in their side chains, such as polylysine and polyarginine; and polyamines in which some of the amino groups have been modified. From the viewpoint of obtaining good gas barrier properties, the polyamine compound preferably comprises one or more compounds selected from the group consisting of polyallylamine, polyvinylamine, polyethyleneimine, and poly(trimethyleneimine), more preferably polyethyleneimine, and even more preferably polyethyleneimine.
[0025] The number-average molecular weight of the polyamine compound is preferably 50 to 2,000,000, more preferably 100 to 1,000,000, even more preferably 1,500 to 500,000, even more preferably 1,500 to 100,000, even more preferably 1,500 to 50,000, even more preferably 3,500 to 20,000, even more preferably 5,000 to 15,000, and even more preferably 7,000 to 12,000, from the viewpoint of an excellent balance between gas barrier properties and handling ease. In this embodiment, the molecular weight of the polyamine compound can be measured using the boiling point elevation method or the viscosity method.
[0026] In the gas barrier coating material of this embodiment, the ratio of (number of moles of amino groups contained in the polyamine compound in the gas barrier coating material) to (number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating material) is preferably 0.40 or higher, more preferably 0.43 or higher, even more preferably 0.45 or higher, even more preferably 0.50 or higher, and even more preferably 0.53 or higher, from the viewpoint of further improving the gas barrier performance after retort treatment. From a similar viewpoint, the ratio (number of moles of amino groups contained in the polyamine compound in the gas barrier coating) / (number of moles of -COO- groups contained in the polycarboxylic acid in the gas barrier coating) is preferably 0.70 or less, more preferably 0.65 or less, even more preferably 0.60 or less, and even more preferably 0.58 or less. Although the details of the reason are not clear, it is thought that the amide crosslinks formed by the amino groups constituting the polyamine compound and the metal crosslinks formed by the Zn constituting the salt of the polycarboxylic acid and Zn form a well-balanced and dense structure, thereby enabling the production of a gas barrier layer 103 with excellent gas barrier performance after retort treatment and a gas barrier laminate having the same.
[0027] (Zn compound) The Zn compound contained in the gas barrier coating material of this embodiment specifically includes zinc (Zn) oxides, hydroxides, halides, carbonates, phosphates, phosphites, hypophosphites, sulfates, or sulfites. From the viewpoint of water resistance and impurities, it is at least one of zinc oxide and zinc hydroxide, and more preferably zinc oxide.
[0028] In the gas barrier coating material of this embodiment, the ratio of (moles of Zn compound in the gas barrier coating material) to (moles of amino groups contained in the polyamine compound in the gas barrier coating material) is preferably 0.50 or higher, more preferably 0.60 or higher, even more preferably 0.70 or higher, and even more preferably 0.75 or higher, from the viewpoint of further improving the gas barrier performance after retort treatment. From a similar viewpoint, the ratio (number of moles of Zn compound in the gas barrier coating) / (number of moles of amino groups contained in the polyamine compound in the gas barrier coating) is preferably 1.00 or less, more preferably 0.95 or less, and even more preferably 0.90 or less.
[0029] The gas barrier coating material of this embodiment may contain components other than those described above. For example, the gas barrier coating material of this embodiment preferably further contains a carbonate-based ammonium salt. The carbonate-based ammonium salt is added to improve the solubility of the Zn compound by converting it into a zinc ammonium complex, thereby preparing a homogeneous solution containing the Zn compound. By including a carbonate-based ammonium salt in the gas barrier coating material, the amount of soluble Zn compound can be increased, and as a result, the gas barrier coating material containing the Zn compound can be made even more homogeneous. Examples of carbonate-based ammonium salts include ammonium carbonate and ammonium bicarbonate. Ammonium carbonate is preferred because it is highly volatile and does not easily remain in the resulting gas barrier layer. The ratio of (moles of ammonium carbonate salt in the gas barrier coating) to (moles of Zn compound in the gas barrier coating) is preferably 0.05 or higher, more preferably 0.10 or higher, even more preferably 0.25 or higher, even more preferably 0.50 or higher, and even more preferably 0.75 or higher, from the viewpoint of further improving the solubility of the Zn compound. Furthermore, from the viewpoint of further improving the coating properties as a gas barrier coating material, the ratio (number of moles of carbonate-based ammonium salt in the gas barrier coating material) / (number of moles of Zn compound in the gas barrier coating material) is preferably 10.0 or less, more preferably 5.0 or less, even more preferably 2.0 or less, and even more preferably 1.5 or less.
[0030] (Phosphorus compounds or their salts) When the gas barrier layer of the gas barrier laminate described later is subjected to mass spectrometry, PO 2- and / or PO 3- A phosphorus is detected. In order to provide such a gas barrier layer, the gas barrier coating material of this embodiment preferably contains a phosphorus introduction source. It is more preferable that such a phosphorus introduction source contains a phosphorus compound or a salt thereof. The phosphorus compound in the phosphorus compound or its salt contains one or more -P-OH groups in its molecular structure. The phosphorus compound may be incorporated into the mixture as a salt. From the viewpoint of further improving the water vapor barrier properties after retort processing, the phosphorus compound preferably contains two or more -P-OH groups, and more preferably three or more -P-OH groups. Also, from the viewpoint of productivity, the number of -P-OH groups in the phosphorus compound may be, for example, 10 or less.
[0031] Specific examples of phosphorus compounds include phosphoric acid compounds, phosphite compounds, phosphonic acid compounds, hypophosphite compounds, polyphosphate compounds, and their derivatives. Specifically, polyphosphate compounds have a condensed structure of two or more phosphate groups in their molecular structure, and examples include diphosphate (pyrophosphate), triphosphate, and polyphosphate compounds in which four or more phosphate groups are condensed. Specific examples of derivatives include esters of the above-mentioned phosphorus compounds such as phosphorylated starch and phosphate-crosslinked starch; halides such as chlorides; anhydrides such as tetraphosphorus decoxide; and compounds having a structure in which a hydrogen atom bonded to a phosphorus atom is substituted with an alkyl group, such as nitrilotris (methylenephosphonic acid) and N,N,N',N'-ethylenediaminetetrakis (methylenephosphonic acid).
[0032] From the viewpoint of further improving the balance between barrier properties and productivity, the phosphorus compound is one or more selected from the group consisting of phosphate compounds, phosphite compounds, hypophosphite compounds, polyphosphate compounds, phosphonic acid compounds and salts thereof, and more preferably at least one selected from the group consisting of phosphate compounds and phosphite compounds, phosphonic acid compounds and salts thereof.
[0033] Furthermore, specific examples of salts in phosphorus compound salts include salts of monovalent metals such as sodium and potassium; and ammonium salts. From the viewpoint of barrier properties, ammonium salts are preferred for phosphorus compound salts. A specific example of such a compound is diammonium hydrogen phosphate.
[0034] (Polyphosphate compounds or their salts) Among the phosphorus compounds or salts thereof mentioned above, polyphosphate compounds or salts thereof are preferred as phosphorus sources from the viewpoint of providing water resistance in addition to improving productivity and barrier properties as described above.
[0035] Specific examples of salts in polyphosphate compounds include salts of monovalent metals such as sodium and potassium; and ammonium salts. From the viewpoint of barrier properties, ammonium salts are preferred for polyphosphate compounds. Specific examples of polyphosphate compounds or their salts include, preferably, low polymer polyphosphates or their salts, such as low polymer polyphosphate, low polymer ammonium polyphosphate, low polymer sodium polyphosphate, and low polymer potassium polyphosphate; pyrophosphates or their salts, such as pyrophosphate, ammonium pyrophosphate, sodium pyrophosphate, and potassium pyrophosphate; tripolyphosphates or their salts, such as tripolyphosphate, ammonium tripolyphosphate, sodium tripolyphosphate, and potassium tripolyphosphate; and at least one selected from the group consisting of tetrapolyphosphate, ammonium tetrapolyphosphate, sodium tetrapolyphosphate, potassium tetrapolyphosphate, and their salts. Among these, from the viewpoint of further improving the balance between the barrier properties and pot life of the gas barrier coating material, low polymer polyphosphate or its salts are preferred, and low polymer ammonium polyphosphate is more preferred. Herein, in this specification, "low polymer polyphosphate" refers to, for example, polyphosphate with a degree of polymerization of 5 to 100.
[0036] In this embodiment, the ratio of (moles of P contained in the phosphorus compound or its salt in the gas barrier coating) / (moles of COO- groups contained in the polycarboxylic acid in the gas barrier coating) or (moles of P contained in the polyphosphate compound or its salt in the gas barrier coating) / (moles of COO- groups contained in the polycarboxylic acid in the gas barrier coating) is preferably 0.005 or higher, more preferably 0.007 or higher, and even more preferably 0.010 or higher, from the viewpoint of improving barrier properties. In the case of phosphorus compounds that contain one P atom in their chemical formula, such as phosphoric acid, the number of moles of P atoms and the number of moles of the phosphorus compound have the same meaning. Furthermore, in the case of phosphorus compounds and polyphosphate compounds that contain multiple P atoms in their chemical formula, the number of moles of P atoms is obtained by multiplying the number of moles of the phosphorus compound and polyphosphate compound by the number of P atoms contained in their chemical formula. Furthermore, from the viewpoint of barrier properties and productivity, the ratio of (moles of P contained in the phosphorus compound or its salt in the gas barrier coating) / (moles of COO- groups contained in the polycarboxylic acid in the gas barrier coating) or (moles of P contained in the polyphosphate compound or its salt in the gas barrier coating) / (moles of COO- groups contained in the polycarboxylic acid in the gas barrier coating) is preferably 0.20 or less, more preferably 0.15 or less, even more preferably 0.12 or less, and even more preferably 0.10 or less.
[0037] (Surfactants) Furthermore, the gas barrier coating material of this embodiment preferably further contains a surfactant, in addition to improving productivity and barrier properties as described above, from the viewpoint of suppressing the occurrence of repelling when applying it as a gas barrier coating material. The surfactant content is preferably 0.01 to 3% by mass, and more preferably 0.01 to 1% by mass, when the total solid content of the gas barrier coating material (the total amount of components remaining as solids when cured) is taken as 100% by mass. In this specification, the solid content of the gas barrier coating material refers to the components that remain as solids when the gas barrier coating material is cured.
[0038] Examples of surfactants include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. From the viewpoint of obtaining good coating properties, nonionic surfactants are preferred, polyoxyalkylene alkyl ethers are more preferred, and polyoxyethylene alkyl ethers are even more preferred.
[0039] Examples of nonionic surfactants include polyoxyalkylene alkylaryl ethers, polyoxyalkylene alkyl ethers, polyoxyalkylene fatty acid esters, sorbitan fatty acid esters, silicone-based surfactants, acetylene alcohol-based surfactants, and fluorine-containing surfactants.
[0040] Examples of polyoxyalkylene alkylaryl ethers include polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, and polyoxyethylene dodecylphenyl ether. Examples of polyoxyalkylene alkyl ethers include polyoxyethylene alkyl ethers such as polyoxyethylene oleyl ether and polyoxyethylene lauryl ether. Examples of polyoxyalkylene fatty acid esters include polyoxyethylene oleate ester, polyoxyethylene laurate ester, and polyoxyethylene distearate ester. Examples of sorbitan fatty acid esters include sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, polyoxyethylene monooleate, and polyoxyethylene stearate. Examples of silicone-based surfactants include dimethylpolysiloxane. Examples of acetylene alcohol-based surfactants include 2,4,7,9-tetramethyl-5-decine-4,7-diol, 3,6-dimethyl-4-octin-3,6-diol, and 3,5-dimethyl-1-hexyn-3-ol. Examples of fluorine-containing surfactants include fluorine alkyl esters.
[0041] (Crosslinking agent) In addition to improving productivity and barrier properties as described above, the gas barrier coating material of this embodiment preferably further contains a crosslinking agent to improve alkali resistance to alkaline liquids (e.g., alkaline detergents).
[0042] As such a crosslinking agent, known crosslinking agents can be used, but preferably it comprises one or more compounds selected from the group consisting of epoxysilane compounds, carbodiimide compounds, and isocyanate compounds, and more preferably it comprises one or more compounds selected from the group consisting of epoxysilane compounds and carbodiimide compounds.
[0043] In the gas barrier coating material of this embodiment, the crosslinking agent content is preferably 0.010% by mass or more, and more preferably 0.015% by mass or more, when the total solid content of the gas barrier coating material is considered to be 100% by mass. By having a crosslinking agent content above the above lower limit, the alkali resistance of the gas barrier layer formed with the gas barrier coating material of this embodiment becomes more favorable. Furthermore, the crosslinking agent content is preferably 2% by mass or less, more preferably 1% by mass or less, and even more preferably 0.05% by mass or less. By keeping the crosslinking agent content below the above upper limit, the productivity and barrier properties of the gas barrier coating material of this embodiment become more favorable.
[0044] The gas barrier coating material of this embodiment may contain additives other than those described above. For example, various additives such as lubricants, slip agents, anti-blocking agents, antistatic agents, anti-fogging agents, pigments, dyes, and inorganic or organic fillers may be added.
[0045] Furthermore, the solid content concentration of the gas barrier coating material of this embodiment is preferably 0.5 to 15% by mass, more preferably 1 to 10% by mass, even more preferably 1 to 5% by mass, and even more preferably 1 to 3% by mass, from the viewpoint of improving the coatability when applying it as a gas barrier coating material.
[0046] (Gas barrier laminate) Figure 1 is a schematic cross-sectional view showing an example of the configuration of a gas barrier laminate in an embodiment. The gas barrier laminate of this embodiment comprises a base layer 101 and a gas barrier layer 103 provided on at least one surface of the base layer 101, wherein the gas barrier layer 103 includes a cured product of the gas barrier coating material. In this case, it is preferable that the gas barrier laminate of this embodiment further comprises an inorganic layer 102 provided between the base layer 101 and the gas barrier layer 103. The specific configuration of each layer in the gas barrier laminate of this embodiment will be described in detail below.
[0047] (Gas barrier layer) Specifically, the gas barrier layer 103 can be manufactured by applying and curing a gas barrier coating material. In this way, the gas barrier layer 103 in this embodiment can include a cured product of the gas barrier coating material. The gas barrier coating material of this embodiment can be obtained as follows. First, the carboxyl groups of the polycarboxylic acid are completely or partially neutralized by adding a volatile base as appropriate. Then, a Zn compound and an ammonium carbonate salt as appropriate are mixed to form metal salts on all or some of the carboxyl groups of the polycarboxylic acid that were neutralized with the volatile base, and on the carboxyl groups of the polycarboxylic acid that were not neutralized with the volatile base. Subsequently, by adding a polyamine compound, the gas barrier coating material of this embodiment is obtained. By mixing polycarboxylic acid, Zn compound, and optionally carbonate-based ammonium salt and polyamine compound in this procedure, the formation of aggregates can be suppressed, and a more uniform gas barrier coating material can be obtained. This makes it possible to more effectively promote the dehydration condensation reaction between the -COO- group contained in the polycarboxylic acid and the amino group contained in the polyamine compound.
[0048] More details are as follows. Below, we will explain using the case where volatile bases and carbonate-based ammonium salts are incorporated into gas barrier coatings as an example. First, a solution is prepared in which the carboxyl groups constituting the polycarboxylic acid are completely or partially neutralized. By adding a volatile base to the polycarboxylic acid, the carboxyl groups of the polycarboxylic acid are completely or partially neutralized. By neutralizing the carboxyl groups of the polycarboxylic acid, gelation that occurs when the carboxyl groups constituting the polycarboxylic acid react with the amino groups constituting the Zn compounds or polyamine compounds during the addition of these compounds can be effectively prevented, resulting in a more uniform gas barrier coating material. Next, a Zn compound and a carbonate-based ammonium salt are added and dissolved, and the resulting Zn ions form a Zn salt with the -COO- group constituting the polycarboxylic acid. At this time, the -COO- group that forms a salt with the Zn ions refers to both the carboxyl group that was not neutralized by the base and the -COO- group that was neutralized by the base. In the case of a -COO- group that was neutralized by the base, the Zn ions contained in the Zn compound are replaced and coordinate to form a Zn salt of the -COO- group. After forming the Zn salt, a gas barrier coating material can be obtained by further adding a polyamine compound and, if a phosphorus compound or its salt is included, a phosphorus compound or its salt.
[0049] The gas barrier coating material manufactured in this manner is applied to the substrate layer 101, the inorganic layer 102, or the intervening layer between the substrate layer 101 and the gas barrier layer 103 formed on the inorganic layer 102, and then dried and cured to form the gas barrier layer 103. At this time, the -COO- groups constituting the polycarboxylic acid and the Zn of the Zn salt form metal crosslinks, and the amino groups constituting the polyamine form amide crosslinks, resulting in a gas barrier layer 103 with excellent gas barrier properties. A more detailed manufacturing method for the gas barrier layer 103 will be described later.
[0050] From the viewpoint of improving barrier properties, the thickness of the gas barrier layer 103 after drying and curing is preferably 0.05 μm or more, more preferably 0.07 μm or more, and even more preferably 0.1 μm or more. Furthermore, from the viewpoint of thinning the entire gas barrier laminate, the thickness of the gas barrier layer 103 after drying and curing is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 1 μm or less, and even more preferably 0.5 μm or less.
[0051] (base material layer) The base layer 101 may be a single layer or two or more layers. The shape of the base layer 101 is not limited, but examples include a sheet or film shape, a tray, a cup, a hollow body, etc.
[0052] The material for the base layer 101 is not limited to any material that can stably form the inorganic layer 102 described later on the base layer 101 and that can be coated with a gas barrier coating solution on top of the inorganic layer 102. Examples of materials for the base layer 101 include resins such as thermosetting resins and thermoplastic resins, organic materials such as paper; inorganic materials such as glass, ceramics, porcelain, silicon oxide, silicon oxide-nitride, silicon nitride, cement, aluminum, aluminum oxide, iron, copper, stainless steel, and other metals; and multilayer base layers made of organic materials together or combinations of organic and inorganic materials. Among these, for example, in the case of various film applications such as packaging materials and panels, a plastic film using at least one selected from the group consisting of thermosetting resins and thermoplastic resins, or an organic material such as paper, is preferred.
[0053] As the thermosetting resin, known thermosetting resins can be used. Examples include epoxy resins, unsaturated polyester resins, phenolic resins, urea-melamine resins, polyurethane resins, silicone resins, and polyimides.
[0054] As the thermoplastic resin, known thermoplastic resins can be used. Examples include polyolefins (polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.), polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, polymetaxylene adipamide, etc.), polyvinyl chloride, polyimide, ethylene-vinyl acetate copolymer or its saponified product, polyvinyl alcohol, polyacrylonitrile, polycarbonate, polystyrene, ionomer, fluororesin, or mixtures thereof.
[0055] Among these, from the viewpoint of achieving good transparency, one or more resins selected from the group consisting of polypropylene, polyethylene terephthalate (PET), polyethylene naphthalate, polyamide, polyimide, and polybutylene terephthalate are preferred. Furthermore, from the viewpoint of excellent pinhole resistance, tear resistance, and heat resistance, one or more resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate are preferred. From a similar viewpoint, the base layer 101 is preferably a layer containing one or more resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate, and more preferably a layer of these one or more resins.
[0056] Furthermore, when a hygroscopic material such as polyamide is used for the base layer 101, the base layer 101 in the gas barrier laminate tends to absorb moisture and swell, leading to a decrease in gas barrier performance under high humidity, gas barrier performance after retort processing, and gas barrier performance when filled with acidic contents. However, in this embodiment, even when a hygroscopic material is used as the base layer 101, the decrease in gas barrier performance under high humidity and gas barrier performance after retort processing of the gas barrier laminate can be effectively suppressed.
[0057] Alternatively, a film formed from a thermosetting resin or thermoplastic resin may be stretched in at least one direction, preferably two axial directions, to form the base layer 101. From the viewpoint of excellent transparency, rigidity, and heat resistance, the base layer 101 is preferably a biaxially oriented film formed from one or more thermoplastic resins selected from the group consisting of polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide, and polybutylene terephthalate, and more preferably a biaxially oriented film formed from one or more thermoplastic resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate.
[0058] Furthermore, the surface of the base layer 101 may be coated with polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyalool copolymer, acrylic resin, urethane resin, or the like. Furthermore, the base layer 101 may be surface-treated to improve its adhesion to the gas barrier layer 103. Specifically, the surface of the base layer 101 facing the gas barrier layer 103 may be subjected to surface activation treatments such as corona treatment, flame treatment, plasma treatment, or primer coating.
[0059] From the viewpoint of obtaining good film properties, the thickness of the substrate layer 101 is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and also preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 300 μm or less.
[0060] (Inorganic layer) The gas barrier laminate of this embodiment preferably further comprises an inorganic layer 102 provided between the base layer 101 and the gas barrier layer 103. The inorganic materials constituting the inorganic layer 102 include, for example, metals, metal oxides, metal nitrides, metal fluorides, and metal oxynitrides that can form a thin film with barrier properties. Examples of inorganic materials constituting the inorganic layer 102 include one or more selected from elements, oxides, nitrides, fluorides, or oxynitrides, such as: Group 2A elements of the periodic table such as beryllium, magnesium, calcium, strontium, and barium; transition elements of the periodic table such as titanium, zirconium, ruthenium, hafnium, and tantalum; Group 2B elements of the periodic table such as zinc; Group 3A elements of the periodic table such as aluminum, gallium, indium, and thallium; Group 4A elements of the periodic table such as silicon, germanium, and tin; and Group 6A elements of the periodic table such as selenium and tellurium. In this embodiment, the group names of the inorganic layer 102 in the periodic table are shown using the old CAS formula.
[0061] Furthermore, among the inorganic materials mentioned above, one or more inorganic materials selected from the group consisting of silicon dioxide, aluminum oxide, and aluminum are preferred, and aluminum oxide is more preferred, due to their excellent balance of barrier properties, cost, etc. Furthermore, silicon dioxide may also contain silicon monoxide and silicon dioxide.
[0062] The inorganic layer 102 is formed from the above-mentioned inorganic material. The inorganic layer 102 preferably includes an aluminum oxide layer composed of aluminum oxide because it offers an excellent balance of barrier properties, cost, etc. The inorganic layer 102 may consist of a single inorganic layer or multiple inorganic layers. Furthermore, if the inorganic layer 102 consists of multiple inorganic layers, they may be composed of inorganic layers of the same type or different types.
[0063] The thickness of the inorganic layer 102 is, from the viewpoint of balancing improved barrier properties and improved handling, for example, 1 nm or more, preferably 4 nm or more, and also, for example, 1000 nm or less, preferably 500 nm or less, more preferably 100 nm or less, even more preferably 50 nm or less, even more preferably 30 nm or less, even more preferably 15 nm or less, and even more preferably 10 nm or less. Here, the thickness of the inorganic layer 102 can be determined, for example, by observation images obtained using a transmission electron microscope or a scanning electron microscope.
[0064] The method for forming the inorganic layer 102 is not limited; for example, the inorganic layer 102 can be formed on one or both sides of the substrate layer 101 by vacuum deposition, ion plating, sputtering, chemical vapor deposition, physical vapor deposition (CVD), plasma CVD, sol-gel method, etc. Among these, film formation under reduced pressure, such as by sputtering, ion plating, chemical vapor deposition (CVD), physical vapor deposition (PVD), and plasma CVD, is desirable. This is expected to improve the surface smoothness of the inorganic layer 102 and reduce pores by rapidly reacting with chemically active molecular species containing silicon, such as silicon nitride and silicon oxidized nitride. To carry out these bonding reactions rapidly, it is desirable that the inorganic atoms or compounds are chemically active molecular or atomic species. Furthermore, from the viewpoint of improving the balance between the barrier properties and productivity of the gas barrier laminate, the inorganic layer 102 is preferably a deposited film.
[0065] The inorganic layer 102 is a vapor-deposited film provided on the base layer 101, or on an intervening layer if an intervening layer is present between the base layer 101 and the inorganic layer 102, from the viewpoint of improving the balance between the barrier properties and productivity of the gas barrier laminate. It is composed of one or more inorganic materials selected from the group consisting of silicon dioxide, aluminum oxide, and aluminum, and is preferably composed of aluminum oxide.
[0066] (Undercoat layer) An undercoat layer may be provided between the base layer 101 and the inorganic layer 102. However, in this embodiment, the gas barrier coating material has sufficient barrier properties even without an undercoat layer, and from the viewpoint of improving productivity by omitting the process of providing an undercoat layer, it is preferable not to provide an undercoat layer.
[0067] When an undercoat layer is provided, from the viewpoint of improving the adhesion between the base material layer 101 and the inorganic material layer 102, the material of the undercoat layer can be one or more selected from the group consisting of polyurethane resin, polyester resin, oxazoline resin, and (meth)acrylic resin.
[0068] Examples of polyurethane resins include various polyurethane resins, polyurethane polyurea resins, and their prepolymers. Specific examples of such urethane resins include reaction products of diisocyanate components such as tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, and dicyclohexyl diisocyanate with diol components such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexanedimethanol, bisphenol, polyester diol, polyetherdiol, polycarbonate diol, and polyethylene glycol; and reaction products of urethane prepolymers having isocyanate groups at the ends with amino compounds, aminosulfonates, polyhydroxycarboxylic acids, bisulfites, etc.
[0069] Examples of polyester resins used in the undercoat layer include various polyester resins and their modified products. Specific examples of such polyester resins include reaction products of polycarboxylic acid components such as terephthalic acid, phthalic acid, isophthalic acid, trimellitic acid, pyromellitic acid, 2-sulfoisophthalic acid, 5-sulfoisophthalic acid, adipic acid, sebacic acid, succinic acid, and dodecanedioic acid with diol components such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexanedimethanol, and bisphenol. Modified products using acrylic resins, epoxy resins, etc., are also included.
[0070] When using an oxazoline resin for the undercoat layer, it is preferable that the undercoat layer be composed of an oxazoline-based resin composition containing an oxazoline group-containing aqueous polymer, an aqueous (meth)acrylic resin, and an aqueous polyester resin.
[0071] From the viewpoint of obtaining good adhesion, the thickness of the undercoat layer is preferably 0.001 μm or more, more preferably 0.005 μm or more, even more preferably 0.01 μm or more, even more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and still more preferably 0.2 μm or more. Furthermore, from an economic standpoint, the thickness of the undercoat layer is preferably 1.0 μm or less, more preferably 0.6 μm or less, even more preferably 0.5 μm or less, and may also be, for example, 0.4 μm or less, or for example, 0.3 μm or less.
[0072] (adhesive layer) The gas barrier laminate may further be provided with an adhesive layer. The adhesive layer is provided, for example, between the gas barrier layer 103 and the upper layer of the gas barrier layer 103. Furthermore, when the upper layer is formed from multiple layers, the adhesive layer may be provided between the multiple layers. Here, the upper layer of the gas barrier layer 103 refers to the layer laminated on the side of the gas barrier layer 103 opposite to the inorganic layer 102. The adhesive layer may contain any known adhesive. Examples of adhesives include laminate adhesives composed of organic titanium resin, polyethyleneimine resin, urethane resin, epoxy resin, acrylic resin, polyester resin, oxazoline group-containing resin, modified silicone resin, alkyl titanate, polyester polybutadiene, etc., or one-component or two-component polyols and polyvalent isocyanates, water-based urethanes, ionomers, etc. Alternatively, an aqueous adhesive mainly composed of acrylic resin, vinyl acetate resin, urethane resin, polyester resin, etc. may be used. Furthermore, depending on the application of the gas barrier laminate 100, other additives such as curing agents and silane coupling agents may be added to the adhesive. When the gas barrier laminate is used in hot water treatment such as retorts, dry laminating adhesives such as polyurethane adhesives are preferred from the viewpoint of heat resistance and water resistance, and solvent-based two-component curing type polyurethane adhesives are more preferred.
[0073] (Method for manufacturing gas barrier laminates) In this embodiment, the method for manufacturing the gas barrier laminate 100 includes, for example, the steps of preparing a base layer 101, forming an inorganic layer 102 on the base layer 101, and forming a gas barrier layer 103 on the upper part of the base layer 101 on which the inorganic layer 102 is formed.
[0074] For the step of forming the inorganic layer 102 on the base layer 101, for example, the method for forming the inorganic layer 102 described above can be used.
[0075] The process of forming the gas barrier layer 103 includes, for example, the steps of applying a gas barrier coating material to an inorganic layer 102 and then drying it to obtain a coated layer, and the steps of heating the coated layer and causing a dehydration condensation reaction between the carboxyl group contained in the polycarboxylic acid and the amino group contained in the polyamine compound to form a gas barrier layer 103 having amide bonds.
[0076] The method for applying the gas barrier coating to the inorganic layer 102 is not limited, and conventional methods can be used. For example, methods using known coating machines such as Meyer bar coaters, air knife coaters, direct gravure coaters, gravure offset coaters, arc gravure coaters, gravure reverse coaters, and jet nozzle type gravure coaters, reverse roll coaters such as top-feed reverse coaters, bottom-feed reverse coaters, and nozzle-feed reverse coaters, five-roll coaters, lip coaters, bar coaters, bar reverse coaters, and die coaters can be used.
[0077] Drying and heat treatment may be performed either after drying, or simultaneously. The drying and heat treatment method is not limited as long as it can achieve the effects of the present invention, and any method that can harden the gas barrier coating material and heat the hardened gas barrier coating material is acceptable. Examples include convection heat transfer using ovens and dryers, conduction heat transfer using heating rolls, radiation heat transfer using electromagnetic waves such as infrared, far-infrared, and near-infrared heaters, and internal heat generation using microwaves. As for the apparatus used for drying and heat treatment, an apparatus that can perform both drying and heat treatment is preferred from the viewpoint of manufacturing efficiency. Specifically, a hot air oven is preferred from the viewpoint that it can be used for various applications such as drying, heating, and annealing, and a heating roll is preferred from the viewpoint that it has excellent heat conduction efficiency to the film. In addition, the methods used for drying and heat treatment may be combined as appropriate. Specifically, a hot air oven and a heating roll may be used in combination, for example, if the gas barrier coating material is dried in a hot air oven and then heat-treated with a heating roll, the heat treatment process is shortened, which is preferable from the viewpoint of manufacturing efficiency. Alternatively, it is preferable to perform drying and heat treatment using only a hot air oven.
[0078] Regarding the heat treatment conditions, for example, the heat treatment temperature is 80 to 180°C and the heat treatment time is 1 second to 5 minutes, preferably the heat treatment temperature is 90 to 160°C and the heat treatment time is 10 seconds to 3 minutes, more preferably the heat treatment temperature is 100 to 150°C and the heat treatment time is 15 seconds to 2 minutes, and even more preferably the heat treatment temperature is 110 to 140°C and the heat treatment time is 30 seconds to 90 seconds. Furthermore, as described above, heat treatment can be performed in a shorter time by using a heating roll in combination. Furthermore, from the viewpoint of effectively promoting the dehydration condensation reaction between the -COO- group contained in the polycarboxylic acid and the amino group contained in the polyamine compound, it is important to adjust the heat treatment temperature and heat treatment time according to the amount of gas barrier coating material applied.
[0079] When the gas barrier coating is dried and heat-treated, the carboxyl groups of the polycarboxylic acid react with polyamines and Zn compounds, forming covalent bonds and ionic crosslinks, thereby creating a gas barrier layer 103 that maintains good gas barrier properties even after retort treatment.
[0080] In this embodiment, the gas barrier laminate exhibits excellent gas barrier performance and can be suitably used as a packaging material for various purposes, such as packaging materials, particularly food packaging materials for contents requiring high gas barrier properties, as well as for medical, industrial, and everyday goods applications.
[0081] Furthermore, the gas barrier laminate in this embodiment can be suitably used, for example, as a vacuum insulation film where high barrier performance is required; as a sealing film for sealing electroluminescent elements, solar cells, etc.
[0082] In this embodiment, a specific example of a laminated structure comprising a gas barrier laminate is shown below. (Laminated structure example 1) Substrate layer 101 (PET substrate) / Gas barrier layer 103 / Adhesive layer / Polyolefin layer (Laminated structure example 2) Substrate layer 101 (PET substrate) / Inorganic layer 102 (Alumina vapor-deposited layer) / Gas barrier layer 103 / Adhesive layer / Polyolefin layer (Laminated structure example 3) Substrate layer 101 (PET substrate) / Inorganic layer 102 (Alumina vapor-deposited layer) / Gas barrier layer 103 / Adhesive layer / Polyamide layer / Adhesive layer / Polyolefin layer Here, by including a polyolefin layer composed of polyolefins such as polyethylene, polypropylene, poly(4-methyl-1-pentene), and poly(1-butene) in the laminated structure, it is possible to further suppress the deterioration of gas barrier performance under high humidity and after retort treatment, while improving pinhole resistance, tear resistance, and heat resistance in the gas barrier laminate.
[0083] The embodiments of the present invention have been described above with reference to the drawings, but these are merely examples of the present invention, and various other configurations can also be adopted. [Examples]
[0084] This embodiment will be described in detail below with reference to examples and comparative examples. However, this embodiment is not limited in any way to the descriptions of these examples.
[0085] (Example 1) (1) Preparation of gas barrier coatings A 7.29% by mass aqueous solution of ammonium polyacrylate was obtained by mixing polyacrylic acid (manufactured by Toagosei Co., Ltd., product name: AC-10H, weight-average molecular weight: 800,000), 10% by mass aqueous ammonia (manufactured by Wako Pure Chemical Industries, Ltd.), and purified water so that the amount of ammonia relative to the carboxyl groups of polyacrylic acid was 250 equivalents. Next, zinc oxide (manufactured by Kanto Chemical Co., Ltd.) and ammonium carbonate were added to the obtained ammonium polyacrylate aqueous solution, mixed, and stirred to prepare a mixture (A). Here, the amount of zinc oxide added was such that (moles of zinc oxide in the gas barrier coating) / (moles of -COO- groups contained in polyacrylic acid in the gas barrier coating) (hereinafter also referred to as "ZnO / PAA") was the value shown in Table 1. In addition, the amount of ammonium carbonate was such that (moles of carbonate-based ammonium salt in the gas barrier coating) / (moles of zinc oxide in the gas barrier coating) was 1.5. Next, purified water was added to polyethyleneimine (manufactured by Nippon Shokubai Co., Ltd., product name: SP-200, number average molecular weight: 10,000) to obtain a 10% aqueous polyethyleneimine solution. Next, the above mixed solution (A) and the above polyethyleneimine aqueous solution were mixed in a ratio such that (the number of moles of amino groups contained in polyethyleneimine in the gas barrier coating) / (the number of moles of -COO- groups contained in polyacrylic acid in the gas barrier coating) (hereinafter also referred to as "PEI / PAA") was the value shown in Table 1 to prepare mixed solution (B). Furthermore, purified water was added to the above mixture (B) so that the solid content concentration was 1.5% by mass, and the mixture was stirred until it became a homogeneous solution. Then, a surfactant (polyoxyethylene lauryl ether, manufactured by Kao Corporation, product name: Emulgen 120) was mixed in such an amount as 0.3% by mass relative to the solid content of the mixture (B) to prepare a gas barrier coating material.
[0086] (Example 2) A gas barrier coating was prepared in accordance with Example 1, except that the amount of zinc oxide added was changed so that the ZnO / PAA ratio was as shown in Table 1.
[0087] (Comparative Examples 1 and 2) A gas barrier coating was prepared in accordance with Example 1, except that the amount of zinc oxide added was changed so that the ZnO / PAA ratio was as shown in Table 1. In this case, a ZnO / PAA ratio of 0 means that no zinc oxide was added.
[0088] (Example 3) A 7.29% by mass aqueous solution of ammonium polyacrylate was obtained by mixing polyacrylic acid (manufactured by Toagosei Co., Ltd., product name: AC-10H, weight-average molecular weight: 800,000), 10% by mass aqueous ammonia (manufactured by Wako Pure Chemical Industries, Ltd.), and purified water so that the amount of ammonia relative to the carboxyl groups of polyacrylic acid was 250 equivalents. Next, zinc oxide (manufactured by Kanto Chemical Co., Ltd.) and ammonium carbonate were added to the obtained ammonium polyacrylate aqueous solution, mixed, and stirred to prepare a mixture (A). Here, the amount of zinc oxide added was such that the ZnO / PAA ratio was as shown in Table 1. The amount of ammonium carbonate added was such that (moles of carbonate-based ammonium salt in the gas barrier coating material) / (moles of zinc oxide in the gas barrier coating material) was 1.5. Next, purified water was added to polyethyleneimine (manufactured by Nippon Shokubai Co., Ltd., product name: SP-200, number average molecular weight: 10,000) to obtain a 10% aqueous polyethyleneimine solution. Furthermore, a 10% by mass solution of diammonium hydrogen phosphate was prepared by adding purified water to diammonium hydrogen phosphate (NH4)2HPO4, manufactured by Kanto Chemical Co., Ltd. Next, the above mixture (A), the polyethyleneimine aqueous solution, and the diammonium hydrogen phosphate solution as a phosphorus source were mixed in a ratio such that the PEI / PAA ratio was the value shown in Table 1, and the ratio (number of moles of P contained in the phosphorus compound or its salt in the gas barrier coating) / (number of moles of -COO- groups contained in the polyacrylic acid in the gas barrier coating) (hereinafter also referred to as "P / PAA") was the value shown in Table 1 to prepare mixture (B). Furthermore, purified water was added to the above mixture (B) so that the solid content concentration was 1.5% by mass, and the mixture was stirred until it became a homogeneous solution. Then, a surfactant (polyoxyethylene lauryl ether, manufactured by Kao Corporation, product name: Emulgen 120) was mixed in such an amount as 0.3% by mass relative to the solid content of the mixture (B) to prepare a gas barrier coating material.
[0089] (Example 4) A gas barrier coating was prepared in accordance with Example 3, except that the amount of diammonium hydrogen phosphate solution added was changed so that the P / PAA ratio was as shown in Table 1.
[0090] (Example 5) A 25% by mass solution of low-polymer ammonium polyphosphate (manufactured by Amada Co., Ltd., product number: water-soluble ammonium polyphosphate flame retardant NNA20, P2O5 content 59%) was prepared by adding it to purified water. The gas barrier coating was prepared in accordance with Example 3, except that the above-mentioned low-polymerization ammonium polyphosphate solution was used as the phosphorus source instead of the above-mentioned diammonium hydrogen phosphate solution, and the mixture was prepared in a ratio such that (the number of moles of P contained in the polyphosphate compound or its salt in the gas barrier coating) / (the number of moles of -COO- groups contained in the polyacrylic acid in the gas barrier coating) (hereinafter also referred to as "P / PAA") was the value shown in Table 1.
[0091] (Examples 6 and 7) A gas barrier coating was prepared in accordance with Example 5, except that the amount of low-polymerization ammonium polyphosphate solution added was changed so that the P / PAA ratio was as shown in Table 1.
[0092] (Example 8) A gas barrier coating was prepared in accordance with Example 6, except that the amount of zinc oxide added was changed so that the ZnO / PAA ratio was as shown in Table 1, and an epoxysilane compound (manufactured by Shin-Etsu Silicone Co., Ltd., product number: KBM-403) was added to the above mixture (B) as a crosslinking agent in an amount of 0.020% by mass relative to the solid content of the mixture (B).
[0093] (Example 9) A gas barrier coating was prepared in accordance with Example 8, except that a carbodiimide compound (manufactured by Nisshinbo Chemical Co., Ltd., product number: Carbodilite SV-02) was used as the crosslinking agent instead of epoxysilane.
[0094] (Example 10) A gas barrier coating was prepared in accordance with Example 8, except that an isocyanate compound (manufactured by Mitsui Chemicals, product number: Takenate® WD726) was used as the crosslinking agent instead of epoxysilane.
[0095] (Example 11) A gas barrier coating was prepared in accordance with Example 8, except that the amount of low-polymerization ammonium polyphosphate solution added was changed so that the P / PAA ratio was as shown in Table 1, and the amount of crosslinking agent added was changed to 0.015% by mass.
[0096] [Fabrication of gas barrier laminates] (Fabrication of gas barrier laminate 1) A biaxially oriented polyethylene terephthalate film (PET12, manufactured by Unitika Corporation) with a thickness of 12 μm was used as the substrate. The gas barrier coatings obtained in each example and comparative example were applied to the corona-treated surface of the film using a meyer bar so that the coating thickness after drying was 0.3 μm. Subsequently, a heat treatment was performed using a hot air dryer at 130°C for 60 seconds. This yielded a gas barrier laminate 1.
[0097] (Fabrication of gas barrier laminate 2) A 12 μm thick biaxially oriented polyethylene terephthalate film (PET12, manufactured by Unitika Corporation) was used as the base material. Aluminum was heated and evaporated onto the corona-treated surface using high-frequency induction heating, and then deposited while introducing oxygen, forming a 7 nm thick aluminum oxide film. This resulted in an aluminum oxide vapor-deposited PET film. The water vapor transmission rate of this aluminum oxide vapor-deposited PET film was 1.5 g / m². 2 It was 24 hours. Next, a gas barrier coating was applied to the vapor-deposited layer using a meyer bar so that the coating thickness after drying was 0.3 μm. A heat treatment was then performed using a hot air dryer at 130°C for 60 seconds to obtain a gas barrier laminate 2.
[0098] [Preparation of test film] (Preparation of test film 1) An ester-based adhesive (polyurethane adhesive (Mitsui Chemicals, Tohcello Co., Ltd., product name: RXC-22): 9 parts by mass, isocyanate-based curing agent (Mitsui Chemicals, product name: Takelac A525S): 1 part by mass, and ethyl acetate: 7.5 parts by mass) was applied to one surface of a 70 μm thick unoriented polypropylene film (Mitsui Chemicals, Tohcello Co., Ltd., product name: Takelac A525S), 1 part by mass, and ethyl acetate: 7.5 parts by mass) was applied. Next, the barrier surface (the surface coated with the gas barrier coating material) of the gas barrier laminate 1 obtained in each example and comparative example was laminated to the adhesive-coated surface of the unoriented polypropylene film to obtain a test film 1 before retort treatment.
[0099] (Preparation of test film 2) An ester-based adhesive (polyurethane adhesive (Mitsui Chemicals, Tohcello Co., Ltd., product name: RXC-22): 9 parts by mass, isocyanate-based curing agent (Mitsui Chemicals, product name: Takelac A525S): 1 part by mass, and ethyl acetate: 7.5 parts by mass) was applied to one surface of a 70 μm thick unoriented polypropylene film (Mitsui Chemicals, Tohcello Co., Ltd., product name: Takelac A525S), 1 part by mass, and ethyl acetate: 7.5 parts by mass) was applied. Next, the barrier surface (the surface coated with the gas barrier coating material) of the gas barrier laminate 2 obtained in each example and comparative example was laminated to the adhesive-coated surface of the unoriented polypropylene film to obtain a test film 2 before retort treatment.
[0100] (Preparation of test film 3) An ester-based adhesive (polyurethane adhesive (Mitsui Chemicals, product name: Takelac A525S): 9 parts by mass, isocyanate-based curing agent (Mitsui Chemicals, product name: Takenate A50): 1 part by mass, and ethyl acetate: 7.5 parts by mass) was applied to both sides of a 15 μm thick nylon film (Unitika Corporation, product name: Emblem ONBC). Then, the barrier surface (the side coated with the gas barrier coating material) of the gas barrier laminate 2 obtained in each example and comparative example was laminated to a 60 μm thick unoriented polypropylene film (Mitsui Chemicals Tohcello Co., Ltd., product name: RXC-22) to obtain a test film 3 before retort treatment.
[0101] [Evaluation Method] (Retort processing (water filling)) The test films 1-3 obtained in the above [Preparation of Test Films] before retort processing were folded so that the unstretched polypropylene film was on the inside, and two sides were heat-sealed to form a bag. Then, 70 mL of water was added as the contents, and the other side was heat-sealed to form a bag. This was then retorted in a high-temperature, high-pressure retort sterilization apparatus at 130°C for 30 minutes. After retort processing, the water was removed from the contents, and test films 1-3 after retort processing (water-filled) were obtained.
[0102] (Oxygen permeability [mL / (m 2 (·day·MPa)]) The oxygen permeability of test films 1-2 before retort treatment and test films 1-3 after retort treatment (water filling), obtained by the method described above, was measured using a Mokon OX-TRAN2 / 21 under conditions of JIS K 7126, at a temperature of 20°C and a humidity of 90% RH. The results are shown in Table 1. In the table, oxygen permeability [mL / (m³) is expressed. 2 (·day·MPa) is called OTR.
[0103] (Water vapor transmission [g / (m³) 2 ·day)]) The test films 1-2 before retort treatment and test films 1-3 after retort treatment (water filling), obtained by the method described above, are stacked with the unstretched polypropylene film facing inwards to form a gas barrier laminated film. The gas barrier laminate is folded over, three sides are heat-sealed to form a bag, calcium chloride is added as the contents, and the other side is heat-sealed to create a bag with a surface area of 0.01 m². 2 Bags were prepared to achieve the following conditions, and left for 300 hours at 40°C and 90%RH. The water vapor transmission rate was measured by the difference in weight. The results are shown in Table 1. In the table, the water vapor transmission rate is expressed as [g / (m³]. 2 ·day)] is called WVTR.
[0104] (Laminate film immersion test) Test films 1-3 obtained in the above [Preparation of Test Films] were folded so that the unstretched polypropylene film was on the inside, and heat-sealed to form a bag. The bagged test films were immersed in alkaline detergent JOY® (manufactured by P&G) diluted 10 times with tap water. After one week, the test films were visually inspected to evaluate whether or not delamination (delami) had occurred. The results are shown in Table 1. A: No Delami occurred. B: Delami is present.
[0105] [Table 1]
[0106] As shown in Table 1, in each example, a gas barrier material with an improved balance of productivity and barrier properties was obtained by performing low-temperature, short-duration heat treatment compared to each comparative example. Furthermore, the water vapor permeability could be further improved by adding polyphosphate compounds. Furthermore, by adding a crosslinking agent, we were able to improve the alkali resistance of the laminate film. [Explanation of Symbols]
[0107] 100 Gas barrier laminate 101 Base material layer 102 Inorganic layer 103 Gas barrier layer
Claims
1. A gas barrier coating material comprising a polycarboxylic acid, a polyamine compound, and a Zn compound, The gas barrier coating material has a ratio of (the number of moles of Zn compound in the gas barrier coating material) / (the number of moles of -COO- groups contained in polycarboxylic acid in the gas barrier coating material) of 0.40 or more and 0.70 or less.
2. The gas barrier coating material according to claim 1, A gas barrier coating material which further contains a crosslinking agent.
3. The gas barrier coating material according to claim 2, The gas barrier coating material, wherein the crosslinking agent comprises one or more compounds selected from the group consisting of epoxysilane compounds, carbodiimide compounds and isocyanate compounds.
4. The gas barrier coating material according to any one of claims 1 to 3, The gas barrier coating material, wherein the polycarboxylic acid comprises one or more compounds selected from the group consisting of polyacrylic acid, polymethacrylic acid, and a copolymer of acrylic acid and methacrylic acid.
5. The gas barrier coating material according to any one of claims 1 to 3, The gas barrier coating material, wherein the polyamine compound comprises one or more compounds selected from the group consisting of polyallylamine, polyvinylamine, polyethyleneimine, and poly(trimethyleneimine).
6. The gas barrier coating material according to any one of claims 1 to 3, The gas barrier coating material further comprises a polyphosphate compound or a salt thereof.
7. The gas barrier coating material according to claim 6, The gas barrier coating material has a ratio of (the number of moles of P contained in the polyphosphate compound or a salt thereof in the gas barrier coating material) / (the number of moles of COO- groups contained in the polycarboxylic acid in the gas barrier coating material) of 0.005 or more and 0.20 or less.
8. The gas barrier coating material according to any one of claims 1 to 3, The gas barrier coating material has a ratio of (the number of moles of amino groups contained in a polyamine compound in the gas barrier coating material) / (the number of moles of -COO- groups contained in a polycarboxylic acid in the gas barrier coating material) of 0.40 or more and 0.70 or less.
9. A gas barrier layer is provided on at least one surface of the base layer, A gas barrier laminate, wherein the gas barrier layer comprises a cured product of the gas barrier coating material according to any one of claims 1 to 3.
10. The gas barrier laminate according to claim 9, The gas barrier layer has a thickness of 0.05 μm or more and 10 μm or less.
11. The gas barrier laminate according to claim 9, The gas barrier laminate further comprises an inorganic layer provided between the base layer and the gas barrier layer.
12. The gas barrier laminate according to claim 11, The gas barrier laminate, wherein the inorganic layer is a vapor-deposited film provided on the base layer, or on an intervening layer when an intervening layer is present between the base layer and the inorganic layer, and is composed of one or more inorganic materials selected from the group consisting of silicon oxide, aluminum oxide, and aluminum.