Fouling release coating composition

JP2023543462A5Inactive Publication Date: 2024-10-04JOTUN AS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023519437
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-09-29
Filing Date
2021-09-28
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing foul release coatings for marine applications require high temperatures for curing, which is inefficient and impractical for shipyards operating in cold climates, and they often use toxic organotin catalysts that are environmentally hazardous.

Method used

A low molecular weight polysiloxane-based binder system combined with low molecular weight amidine or amine catalysts, optionally with metal catalysts like bismuth, zinc, or lithium, allows for curing at low temperatures (0-10°C) without using organotin compounds.

Benefits of technology

The system achieves effective curing at low temperatures, reducing environmental toxicity and improving operational efficiency in shipyards by avoiding the use of hazardous organotin catalysts while maintaining coating performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2022069482000001
    Figure 2022069482000001
  • Figure 2022069482000002
    Figure 2022069482000002
Patent Text Reader

Abstract

(a) a polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a weight average Mw of 50,000 g / mol or less, e.g., 8,000 to 50,000 g / mol, wherein binder A constitutes at least 27 wt. % of the total polysiloxane-based binder system; (b) at least one low molecular weight amidine or low molecular weight amine compound; 1. A tin compound-free fouling release coating composition comprising:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a stain-removing coating composition that does not contain a tin catalyst compound and can be cured at low temperatures. In particular, the present invention provides a stain-removing composition that can be cured at low temperatures and comprises a low weight-average molecular weight polysiloxane or a combination of a low and high weight-average molecular weight polysiloxane and an amidine or amine catalyst. [Background technology]

[0002] Anti-fouling coatings are used on ships to prevent fouling by marine organisms. These coatings are based on the principle that the anti-fouling surface has a very low coefficient of friction, making it difficult for marine organisms to adhere to the surface, especially when the ship is underway, and thus allowing the action of the sea to wash away marine organisms from the hull.

[0003] Therefore, the anti-fouling coating is characterized by low surface tension and low modulus of elasticity, resulting in biological adhesion not adhering to the surface, or the biological adhesion being easily washed away by friction of water against the surface.

[0004] Such coatings often contain a polysiloxane-based binder having reactive (curable) groups such as hydroxyl or silyl units. The polysiloxane-based binder can be hydrolyzed and condensed in the presence of moisture and a catalyst.

[0005] Organotin (dioctyltin and dibutyltin) compounds are robust and therefore widely used to accelerate reactions such as room-temperature vulcanization (RTV) formulations. However, organotin compounds used as catalysts are considered toxicologically harmful. Therefore, avoiding the use of organotin compounds in detarnish coatings would be beneficial from both health and environmental perspectives. Environmental regulatory bodies, aiming to protect human health and the environment, are also expected to increase restrictions on the use of organotin compounds in formulated products.

[0006] Therefore, there are several disclosures relating to the curing of polysiloxanes using tin-free curing techniques, recommending other organometallic compounds as alternatives to organotin catalysts. Preferably, any substituted catalyst compound should ensure similar properties to organometallic tin compounds with respect to curing time, pot life, storage, and coating properties.

[0007] Many systems known from prior art cure at room temperature or high temperatures to ensure sufficient crosslinking rate. A specific problem encountered in fouling-removing coatings is the issue of low-temperature curing. Since shipyards operate year-round, low-temperature curing of marine coatings is important. In some locations, the application temperature can reach very low temperatures during winter. Most shipyards are currently located in China and South Korea, where winters are cold. Conventional room-temperature curing coatings require excessive curing time, affecting productivity and performance.

[0008] There are applications in various fields where tin catalysts can be avoided.

[0009] Patent document 1 (European Patent No. 2776162) is in the field of sealants and rubbers and therefore does not describe stain removal applications. This reference describes a composition comprising a polymer having at least a reactive silyl group, a crosslinking agent, a catalyst selected from Fe(III) or Bi(III) complexes, an adhesion promoter, and at least one acidic compound.

[0010] The focus is on replacing tin catalysts while maintaining good curing properties and good adhesion. In the examples, two different silanol-terminated polysiloxanes with viscosities of 25 Pas and 3.6 Pas are used. The inventors demonstrate that a combination of silanol-terminated polysiloxanes with viscosities of 20 Pas and 3.5 Pas in a ratio of '078 does not result in curing at low temperatures.

[0011] Patent Document 2 provides a coating composition comprising a curable organosiloxane polymer, an organic bismuth compound, and a silane coupling agent, and applies a layer of the coating composition to an aged coating layer on a substrate. In the example, a hydroxy-terminated polydimethylsiloxane having a viscosity of 4000 mPas is used.

[0012] Patent document 3 describes a composition for the production of artificial stone comprising at least one organosilicon component and at least one nitrogen compound selected from guanidine and amidine. A siloxane binder having a very high viscosity (3,000 to 13,000 mPas) is produced from a low molecular weight compound.

[0013] Patent Document 4 describes a curable composition for release coatings used with an adhesive comprising at least one polyorganosiloxane, a fluorinated polyorganosiloxane, or a combination thereof, and an amidine or guanidine catalyst.

[0014] Paragraph 54 states that different combinations of hydroxyl-containing polyorganosiloxanes can be used, with the preferred option being the use of high molecular weight (300,000-1,000,000, most preferably 500,000-700,000) polysiloxanes and low molecular weight (150-150,000) polysiloxanes. Curing was not obtained at room temperature, but only at high temperatures.

[0015] Patent document 5 describes a polysiloxane composition cured with bismuth and amidine for inkjet printing. The organopolysiloxane resin has a weight-average molecular weight in the range of 800 to 7500.

[0016] Patent document 6 falls under the field of self-adhesive curing agent compositions. The curing agent composition of Example 3 contains a low molecular weight polydimethylsiloxane. [Prior art documents] [Patent Documents]

[0017] [Patent Document 1] International Publication No. 2013 / 071078 [Patent Document 2] International Publication No. 2015 / 082408 [Patent Document 3] U.S. Patent Application Publication No. 2017 / 0210856 [Patent Document 4] U.S. Patent Application Publication No. 2014 / 0342166 [Patent Document 5] U.S. Patent Application Publication No. 2015 / 0174904 [Patent Document 6] U.S. Patent Application Publication No. 2012 / 0101237 [Overview of the project] [Problems that the invention aims to solve]

[0018] The object of the present invention is to provide a low-temperature curable coating composition comprising a tin-free polysiloxane-based binder. This object is achieved by using a low weight-average molecular weight (or low viscosity) polysiloxane, or by using a combination of polysiloxane binders in which one binder has a low molecular weight and the other has a high molecular weight, in combination with an amine or amidine-based catalyst system. [Means for solving the problem]

[0019] Surprisingly, the inventors have found that tin-free curing can be achieved at low temperatures, such as 5°C, by using a low molecular weight (or low viscosity) polysiloxane or a mixture of two different polysiloxane binders with different molecular weights in combination with a low molecular weight amidine or amine catalyst. When only one high molecular weight polysiloxane-based binder was used, curing did not occur at 5°C using the catalyst system of the present invention.

[0020] To enhance the robustness of the system and ensure a suitable pot life, it is preferable to also add a metal catalyst such as a bismuth, zinc, or lithium-based catalyst. The stain-removing coating composition of the present invention is low in toxicity. The stain-removing composition of the present invention may also be cured at a lower temperature.

[0021] In one aspect, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a weight-average Mw of 50,000 g / mol or less, for example, 8,000 to 50,000 g / mol, wherein binder A constitutes at least 27% by weight (dry weight) of the total polysiloxane-based binder system, (b) at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing [a specific component].

[0022] In another aspect, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a viscosity of 2,800 mPas or less, for example, 300 to 2,800 mPa, wherein binder A constitutes at least 27% by weight (dry weight) of the total polysiloxane-based binder system, (b) at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing [a specific component].

[0023] In another aspect, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and B, wherein the weight-average Mw of binder A is 50,000 g / mol or less, the weight-average Mw of binder B is 55,000 g / mol or more, and binder A constitutes at least 27% by weight (dry weight) of the total polysiloxane-based binder system; (b) at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing [a specific component].

[0024] In another aspect, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and B, wherein the viscosity of binder A is 2,800 mPas or less, the viscosity of binder B is 3,500 mPas or more, and binder A constitutes at least 27% by weight (dry weight) of the total polysiloxane-based binder system, (b) at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing [a specific component].

[0025] In another aspect, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least one curable polysiloxane-based binder having a PDI greater than 2.5 and an Mw of 20,000 to 120,000 g / mol, (b) at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing [a specific component].

[0026] In another aspect, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least one curable polysiloxane-based binder having a PDI greater than 2.5 and a viscosity of 400 to 30,000 mPas, (b) at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing [a specific component].

[0027] In one embodiment, the defacement-removing coating composition of the present invention further comprises a metal catalyst selected from compounds of iron, zirconium, lithium, potassium, bismuth, cerium, and / or zinc.

[0028] The stain-removing coating composition of the present invention preferably further comprises a metal catalyst selected from compounds of iron, zirconium, lithium, potassium, bismuth, and / or zinc.

[0029] The stain-removing coating composition of the present invention preferably further contains a crosslinking agent.

[0030] In another aspect, the present invention provides a method for applying a defouling and peeling coating composition to a substrate, comprising applying the defouling and peeling coating composition as defined herein to the substrate, for example by spraying, and curing the coating composition. Ideally, the curing process may be carried out at a temperature of 10°C or less, for example, 0 to 10°C.

[0031] In another aspect, the present invention relates to a method for applying and curing a stain-removing coating composition onto a substrate, wherein the composition does not contain a tin compound. (a) A polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a weight-average Mw of 50,000 g / mol or less, (b) at least one low molecular weight amidine or low molecular weight amine compound, A stain-removing coating composition containing, The present invention provides a method comprising applying a stain-removing coating composition to a substrate and curing it at a temperature of 10°C or lower, for example, 0 to 10°C.

[0032] In another aspect, the present invention relates to a method for applying and curing a stain-removing coating composition onto a substrate, comprising applying a stain-removing coating composition, which does not contain a tin compound. (a) A polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a viscosity of 2,800 mPas or less, (b) at least one low molecular weight amidine or low molecular weight amine compound, A stain-removing coating composition containing, The present invention provides a method comprising applying a fouling-removing coating composition to a substrate and curing it at a temperature of 10°C or lower, for example, 0 to 10°C. A preferred substrate is a marine substrate.

[0033] In another aspect, the present invention provides a substrate comprising the previously defined cured de-fouling and de-fouling coating composition.

[0034] In another aspect, the present invention provides a method for low-temperature curing on a substrate, comprising exposing a detangling coating composition as defined herein to a temperature of 10°C or less, for example, 0 to 10°C.

[0035] definition As used herein, the terms “defacement-removing composition” or “defacement-removing coating composition” refer to a composition that, when applied to a surface, provides a defacement-removing surface that makes it difficult for marine organisms to permanently adhere to it.

[0036] As used herein, the term “binder system” refers to the film-forming components of the composition. The polysiloxane-based binder of the composition is the main binder of the binder system, i.e., it forms at least 50% by weight, for example, at least 75% by weight of the binder system. As used herein, the term “binder system” does not include additive oils. Additive oils are not considered film-forming components as used herein.

[0037] In one embodiment, the binder system consists of a polysiloxane-based binder. Therefore, the binder system may consist of polysiloxane-based binder A or polysiloxane-based binder A and binder B.

[0038] As used herein, the term “paint” means a composition comprising a defouling and peeling coating composition as described herein, and optionally, a solvent ready for spraying, for example. Thus, the defouling and peeling coating composition may be a paint itself, or it may be a concentrate to which a solvent is added in order to produce a paint.

[0039] As used herein, the term "polysiloxane" refers to a polymer containing a siloxane, i.e., a -Si-O-repeating unit.

[0040] As used herein, the term “polysiloxane-based binder” refers to a binder containing at least 50% by weight, preferably at least 60% by weight, and more preferably at least 70% by weight, of repeating units containing the motif-Si-O-, based on the total weight of the polymer. A polysiloxane-based binder may contain up to 99.99% by weight of repeating units containing the motif-Si-O-, based on the total weight of the polymer. The repeating units-Si-O- may be linked in a single sequence or may be interrupted by non-siloxane moieties, such as organic-based moieties.

[0041] As used herein, the term “non-degradable polysiloxane-based binder” refers to a polysiloxane-based binder that is not hydrolyzed or eroded in seawater.

[0042] The term "tin compound-free" means that the stain-removing composition of the present invention contains less than 0.1% by weight of tin-containing compounds, and ideally does not contain any tin-containing compounds.

[0043] As used herein, the term "alkyl" refers to a saturated, linear, branched, or cyclic group.

[0044] As used herein, the term "cycloalkyl" refers to a cyclic alkyl group.

[0045] As used herein, the term "alkylene" refers to a divalent alkyl group.

[0046] As used herein, the term "alkenyl" refers to an unsaturated, linear, branched, or cyclic group.

[0047] As used herein, the term "aryl" refers to a group comprising at least one aromatic ring. The term aryl encompasses fused ring systems in which one or more aromatic rings are fused to a cycloalkyl ring. An example of an aryl group is phenyl, i.e., C6H5.

[0048] As used herein, the term “substitution” refers to a group in which one or more hydrogen atoms in the group, for example up to six, more specifically one, two, three, four, five, or six, are independently replaced by the corresponding number of substituents described.

[0049] As used herein, the term "arylalkyl" group refers to a group whose bond to Si is via an alkyl moiety.

[0050] As used herein, the term "polyether" refers to a compound containing two or more -O- bonds interrupted by alkylene units.

[0051] As used herein, the terms "poly(alkylene oxide)", "poly(oxyalkylene)", and "poly(alkylene glycol)" refer to compounds containing an alkylene-O-repeating unit. Typically, the alkylene is ethylene or propylene.

[0052] Where used herein, the term wt% refers to the dry weight of the coating composition unless otherwise specified.

[0053] As used herein, the term "PDI" or polydispersity index refers to the ratio of Mw / Mn, where Mw is the weight-average molecular weight and Mn is the number-average molecular weight. PDI is sometimes also called D (degree of dispersion).

[0054] As used herein, the term "volatile organic compound (VOC)" refers to a compound having a boiling point of 250°C or less.

[0055] As used herein, “antifouling agent” refers to a biologically active compound or mixture of biologically active compounds that prevents the attachment of marine organisms to a surface and / or prevents the growth of marine organisms on a surface and / or promotes the detachment of marine organisms from a surface. [Modes for carrying out the invention]

[0056] The present invention relates to a desiccation-removing coating composition comprising a polysiloxane-based binder containing at least two different curable polysiloxane-based binders of different molecular weights, or at least one polysiloxane having a specific PDI and Mw together with a low molecular weight amidine or low molecular weight amine compound. By using the binder system of the present invention in combination with specific low molecular weight amines or amidine compounds, it was possible to cure the coating composition at low temperatures such as 0-10°C, for example, 2-8°C, without using a tin catalyst.

[0057] Polysiloxane-based binder The binder system in the defacement-removing coating composition comprises at least one curable polysiloxane-based binder component A. In one embodiment, the required polysiloxane-based binder system comprises two distinct polysiloxane polymers A and B having different molecular weights or viscosities as defined herein.

[0058] The polysiloxane-based binder is preferably a non-degradable, curable polysiloxane-based binder.

[0059] Any polysiloxane-based binder present in the coating composition of the present invention includes at least 50% by weight of polysiloxane portion, preferably more than 60% by weight of polysiloxane portion, and more preferably more than 70% by weight of polysiloxane portion, for example, 99.99% by weight or more of polysiloxane portion. Typical ranges include 50 to 100% by weight of polysiloxane portion, 60 to 99.999% by weight of polysiloxane portion, or 70 to 99.99% by weight of polysiloxane portion in the polysiloxane-based binder.

[0060] The polysiloxane moiety is defined as a repeating unit containing the motif -Si-O-, based on the total weight of the polysiloxane-based binder. The weight percentage of the polysiloxane moiety can be determined based on the stoichiometric weight ratio of the starting materials in the polysiloxane synthesis. Alternatively, the polysiloxane content can be determined using analytical techniques such as IR or NMR.

[0061] Typically, the weight percentage of the polysiloxane moiety is calculated based on the molar ratio of the reactive starting materials in the polysiloxane synthesis. If a molar excess of monomers is present in the reaction mixture, such excess is not counted. Only monomers capable of reacting are counted based on the stoichiometry of the reaction.

[0062] Information regarding the weight percentage of polysiloxane in commercially available polysiloxane-based binders is readily available from suppliers.

[0063] It should be understood that polysiloxane-based binders consist of a single repeating sequence of siloxane units or may be interrupted by non-siloxane moieties, such as organic moieties. It is preferable that polysiloxane-based binders contain only Si-O repeating units.

[0064] The organic portion may include, for example, alkylene, arylene, poly(alkylene oxide), amide, thioether, or a combination thereof, preferably the organic portion may include, for example, alkylene, arylene, poly(alkylene oxide), amide, or a combination thereof.

[0065] Curability means that a polysiloxane-based binder contains functional groups that enable crosslinking reactions to occur between polysiloxane-based binder molecules or via crosslinking agents.

[0066] Any polysiloxane-based binder is preferably an organopolysiloxane having terminal and / or pendant curing-reactive functional groups. At least two curing-reactive functional groups per molecule are preferred. Examples of curing-reactive functional groups are silanol, alkoxy, acetoxy, enoxy and / or ketoxime. Preferred polysiloxane-based binders contain curing-reactive functional groups selected from silanol, alkoxy or acetoxy groups. The curing reaction is typically a condensation curing reaction. The polysiloxane-based binder may optionally contain two or more types of curing-reactive groups and may be cured, for example, by both condensation curing and amine / epoxy curing.

[0067] The polysiloxane-based binder may consist of only one type of polysiloxane or may be a mixture of different polysiloxanes as long as it meets the requirements of the present invention. Preferred polysiloxane-based binders such as binder A and / or B present in the fouling-release coating composition of the present invention are represented by the following formula (D1).

[0068] [Chemical formula]

[0069] In the formula, each R 1 is independently selected from a hydroxyl group, a C 1-6 -alkoxy group, or O—Si(R [[ID=2S]] 5 )3— z (R 6 ) z and each R 2 is independently selected from C 1-10 alkyl, C 6-10 aryl, C 7-10 alkylaryl or C 1-6 alkyl substituted with poly(alkylene oxide) and / or the groups described for R 1 , each R 3 and R 4 are independently C1-10 Alkyl, C 6-10 Ariel, C 7-10 C substituted with alkylaryl or poly(alkylene oxide) 1-6 Selected from alkyl groups, Each R 5 Independently, C 1-6 These are hydrolyzable groups such as alkoxy groups, acetoxy groups, enoxy groups, or ketoxy groups. Each R 6 Independently, C 1-6 Selected from alkyl groups, z is an integer between 0 and 2, x is an integer of at least 2, y is at least an integer of 2.

[0070] Preferably, R 1 The hydroxyl group and O-Si(R 5 )3- z (R 6 ) z Selected from, R 5 It is a C1-C6 alkoxy group, R 6 is C 1-6 It is alkyl, and z is 0 or an integer between 1 and 2. More preferably, R 1 The hydroxyl group and O-Si(R 5 ) 3-z (R 6 ) z Selected from, R 5 It is a C1-C3 alkoxy group, R 6 is C 1-3 It is alkyl, and z is an integer of 0 or 1 to 2. More preferably, R 1 This is a hydroxyl group.

[0071] Preferably, R 2 C 1-10 It is an alkyl group. More preferably, R 2 C 1-4 Alkyl alkyl groups, more preferably C 1-2 Alkyl groups, more preferably methyl groups. Preferably, each R 2 They are the same.

[0072] Preferably, R 3 C 1-10 It is an alkyl group. More preferably, R 3 C 1-4 Alkyl alkyl groups, more preferably C 1-2 Alkyl groups, more preferably methyl groups. Preferably, each R 3 They are the same.

[0073] Preferably, R 4 C 1-10 It is an alkyl group. More preferably, R 4 C 1-4 Alkyl alkyl groups, more preferably C 1-2 Alkyl groups, more preferably methyl groups. Preferably, each R 4 They are the same.

[0074] More preferably, R 1 R is a hydroxyl group, 2 , R 3 and R 4 These are methyl groups, respectively.

[0075] Another preferred polysiloxane-based binder present in the stain-removing coating composition of the present invention, such as binder A and / or B, is represented by the following formula (D2).

[0076] [ka]

[0077] During the ceremony, Each R 1 These are independently a hydroxyl group, C 1-6 -alkoxy group, or O-Si(R 5 )3- z (R 6 ) z Selected from, Each R 2 ~R 4 It is methyl, Each R 5Independently, C 1-6 These are hydrolyzable groups such as alkoxy groups, acetoxy groups, enoxy groups, or ketoxy groups. Each R 6 Independently, C 1-6 Selected from alkyl groups, z is an integer between 0 and 2, x is an integer of at least 2, y is at least an integer of 2.

[0078] Another preferred polysiloxane-based binder present in the stain-removing coating composition of the present invention, such as binder A and / or B, is represented by the following formula (D3).

[0079] [ka]

[0080] In the formula, R 1 , R 2 , R 3 , R 4 Furthermore, x and y are as defined for (D1), and R x is C 2-3 The molecules are alkyl, with each L1 being 0-50 and each L2 being 0-50, where L1+L2 is 2-50, preferably 4-40, more preferably 4-20, and most preferably 4-10, and L3 is 1-200, preferably 2-100, and most preferably 5-50. The polysiloxane moiety must form a minimum of 50% by weight of the molecule.

[0081] The polysiloxane-based binder A or B of the present invention is preferably represented by formula D1.

[0082] The polysiloxane-based binder A or B of the present invention is preferably polydimethylsiloxane.

[0083] Those skilled in the art recognize that polysiloxane-based binders may contain small amounts of impurities, such as cyclic siloxanes, including D4, D5, and D6 cyclic siloxanes, which are residues from polysiloxane synthesis, where the designation (D4, D5, or D6) refers to the number of repeating Si-O units in the cyclic polysiloxane (i.e., 4, 5, or 6 repeating Si-O units in the cyclic polysiloxane). For health, safety, and environmental reasons, it is preferable to limit the amount of cyclic polysiloxane present in the coating. In one preferred embodiment, the polysiloxane-based binder contains less than 5%, preferably less than 2%, and more preferably less than 1% of cyclic polysiloxane. In one particularly preferred embodiment, the polysiloxane-based binder does not contain cyclic polysiloxane.

[0084] The weight-average molecular weight of the polysiloxane-based binder A is preferably 50,000 g / mol or less, for example, 3,500 to 50,000, and more preferably 8,000 to 50,000 g / mol. In a more preferred embodiment, the weight-average molecular weight of the polysiloxane-based binder A is 10,000 to 48,000, more preferably 15,000 to 45,000, and particularly 20,000 to 40,000 g / mol.

[0085] In one embodiment, the number-average molecular weight (Mn) of the polysiloxane-based binder A is less than 25,000 g / mol, for example, 1,000 to 24,000 g / mol, preferably 2,000 to 24,000 g / mol. In a more preferred embodiment, the number-average molecular weight of the polysiloxane-based binder A is 3,000 to 19,500 g / mol, more preferably 4,000 to 19,500 g / mol, and particularly 5,000 to 19,500 g / mol. The number-average molecular weight (Mn) values ​​referred to herein correspond to values ​​experimentally obtained by GPC measured against a polystyrene standard, for example. This method is shown in the experimental section below.

[0086] In one embodiment, the polysiloxane-based binder system comprises at least two polysiloxane-based binders, Binder A and B. The weight-average Mw of Binder B is 55,000 or more, for example, 60,000 to 120,000 g / mol, more preferably 65,000 to 110,000 g / mol.

[0087] The viscosity of the polysiloxane-based binder A is preferably 2,800 mPas or less, for example, 400 to 2,800, more preferably 400 to 2,000, and particularly preferably 500 to 1,500 mPas.

[0088] In one embodiment, the polysiloxane-based binder system comprises at least two polysiloxane-based binders, Binder A and B. The viscosity of Binder B is 3,500 mPas or more, for example, 4,000 to 30,000 mPas, and more preferably 5,000 to 25,000 mPas.

[0089] The binder system forms at least 35% by weight of the defacement-removing coating composition (dry weight), for example, at least 40% by weight, particularly at least 45% by weight, for example, 35-75% by weight of the defacement-removing coating composition (dry weight).

[0090] Binder A forms at least 27% by weight, for example, at least 40% by weight of the binder system. In some embodiments, binder A is the only polysiloxane polymer in the binder system. Thus, it may form at least 80% by weight of the binder system, for example, at least 90% by weight. In some embodiments, the binder system may contain 100% by weight of binder A.

[0091] When two binders are present, each binder forms at least 27% by weight of the binder system, preferably at least 40% by weight of the binder system. The ratio of binder A to binder B is preferably in the range of 30:70 to 70:30, preferably 40:60 to 60:40, and more preferably 45:55 to 55:45.

[0092] Alternatively, each binder may form a detangling coating composition of at least 20% by weight.

[0093] When a mixture of binder A and binder B is used, the PDI of the binder mixture is preferably at least 2.5, for example 2.5 to 10, and particularly 3.0 to 8.0.

[0094] When a mixture of binder A and binder B is used in the binder system, the PDI of the binder system is preferably at least 2.5, for example 2.5 to 10, and particularly preferably 3.0 to 8.0.

[0095] When a mixture of binder A and binder B is used in the binder system, the viscosity of the binder system is preferably 400 to 30,000 mPas, more preferably 1,000 to 25,000 mPas, and even more preferably 2,000 to 15,000 mPas, for example, 2,500 to 11,000 mPas.

[0096] When a mixture of binder A and binder B is used in the binder system, the weight-average molecular weight of the binder system is preferably 25,000 to 100,000 g / mol, more preferably 30,000 to 80,000, and even more preferably 40,000 to 80,000 g / mol. When a mixture of binder A and binder B is used in the binder system and the weight-average molecular weight of the binder system exceeds 50,000, it is also preferable that the PDI of the binder system is at least 2.5.

[0097] In one embodiment, the binder system of the present invention may include at least one polysiloxane binder A having a PDI of 2.5 or higher, for example, 2.5 to 10, and particularly 3.0 to 8.0. Preferably, the polysiloxane binder includes two different polysiloxanes.

[0098] If there is only one binder, it is preferable that the binder forms at least 60% by weight, preferably at least 80% by weight, of the binder system. Alternatively, binder A forms at least 40% by weight of the defacement-removing coating composition.

[0099] Hydrophilic modified polysiloxane The coating composition of the present invention may further contain a hydrophilic modified polysiloxane. It should be understood that this component is different from the polysiloxane binder components A and B described above.

[0100] Hydrophilic modified polysiloxanes do not contain silicone-reactive groups such as Si-OH groups or Si-OR (alkoxy) groups that can react with binders or crosslinking agents (if present) at the relevant curing temperature (0-40°C). Therefore, it should be understood that hydrophilic modified polysiloxanes are intended to be non-reactive in the curing reaction, particularly with respect to the binder component. This component is not considered part of the binder system.

[0101] Hydrophilic modified polysiloxanes are widely used as surfactants and emulsifiers because they contain both hydrophilic and lipophilic groups within the same molecule. The hydrophilic modified polysiloxane according to the present invention is a polysiloxane modified with hydrophilic groups to be more hydrophilic than the corresponding unsubstituted polysiloxane having the same number of polysiloxane units. Hydrophilicity can be obtained by modification with hydrophilic groups such as ethers (e.g., polyoxyalkylene groups such as polyethylene glycol and polypropylene glycol), alcohols (e.g., poly(glycerol)), amides (e.g., pyrrolidone, polyvinylpyrrolidone, (meth)acrylamide), acids (e.g., carboxylic acids, poly(meth)acrylic acid), and amines (e.g., polyvinylamine, (meth)acrylic polymers containing amine groups). Typically, hydrophilic modified polysiloxanes are oily.

[0102] In one preferred embodiment, the hydrophilic group is nonionic.

[0103] In this specification, "nonionic" means that the hydrophilic modified polysiloxane does not contain a salt moiety. In particular, it typically does not contain a metal cation.

[0104] The hydrophilicity of a nonionic hydrophilic modified polysiloxane can be determined according to the HLB (hydrophilic-lipophilic balance) parameter. When the hydrophilic modified polysiloxane of the present invention is nonionic, the HLB (hydrophilic-lipophilic balance) is in the range of 1 to 12, preferably 1.0 to 10, more preferably 1.0 to 8.0, and most preferably 2.0 to 7.0. In certain embodiments, the nonionic hydrophilic modified polysiloxane has an HLB in the range of 3.0 to 6.0.

[0105] HLB is typically determined herein according to Griffin's model (Reference: Griffin, WCCalculation of HLB values ​​of non-ionic surfactants, J.Soc.Cosmet.Chem.1954, 5, 249-256) using the formula “weight% hydrophilic groups” / 5. The HLB parameter is an established parameter for nonionic surfactants and is readily available from commercially available hydrophilic modified polysiloxane suppliers. A higher HLB value for a surfactant indicates higher hydrophilicity. Weight% hydrophilic groups refers to the weight percentage of hydrophilic groups in the hydrophilic modified polysiloxane.

[0106] One function of hydrophilic modified polysiloxanes is to facilitate the dissolution and transport of any biocides to the surface of the coating film. It is also well known that the formation of a hydration layer at the coating-water interface is important for fouling protection performance.

[0107] If the hydrophilicity of the hydrophilic modified polysiloxane is too high, for example, due to a large amount of hydrophilic groups in the molecule, this can lead to premature depletion of the biocide and the hydrophilic modified polysiloxane due to an excessively high leaching rate. High hydrophilicity will also result in insufficient compatibility with the polysiloxane-based binder matrix, especially when high oil content (more than 10% by weight) is used, leading to insufficient film uniformity and poor adhesion.

[0108] Methods for controlling the leaching rate of biocides and hydrophilic modified polysiloxanes include the molecular weight, hydrophilicity, and miscibility with the binder of the hydrophilic modified polysiloxane. Very low molecular weight hydrophilic modified polysiloxanes tend to enable high leaching rates, while excessively high molecular weights may prevent the leaching of biocides and hydrophilic modified polysiloxanes from reaching the desired rate.

[0109] Therefore, in preferred embodiments, the hydrophilic modified polysiloxane has a number-average molecular weight (Mn) in the range of 500 to 18,000 g / mol, for example, 1,000 to 16,000 g / mol, and particularly in the range of 2,000 to 15,050 g / mol or 4,000 to 15,050 g / mol. More preferred Mn ranges for the hydrophilic modified polysiloxane include 500 to 15,000 g / mol, 1,000 to 13,000 g / mol, or 3,000 to 10,000 g / mol. The number-average molecular weight (Mn) values ​​referred to herein correspond to values ​​experimentally obtained by GPC measured against a polystyrene standard, for example. This method is given in the experimental section below.

[0110] In preferred embodiments, the hydrophilic modified polysiloxane has a weight-average molecular weight (Mw) in the range of 1,000 to 50,000 g / mol, preferably 2,000 to 45,000 g / mol, 3,000 to 42,000 g / mol, 4,000 to 40,000 g / mol, or 5,000 to 40,000 g / mol. More preferred ranges include 5,000 to 30,000 g / mol, for example, 5,000 to 25,000 g / mol or 10,000 to 20,000 g / mol. The weight-average molecular weight (Mw) values ​​referred to herein correspond to values ​​experimentally obtained by GPC measured against a polystyrene standard, for example. This method is given in the experimental section below.

[0111] It is also preferable that the hydrophilic modified polysiloxane has a viscosity in the range of 20 to 4,000 mPa-s, for example, in the range of 30 to 3,000 mPa-s, and particularly in the range of 50 to 2,500 mPa-s, when measured according to the method shown in the experimental section.

[0112] Hydrophilic modified polysiloxane may be included in the coating composition in an amount of 1.0 to 30% by weight, preferably 2.0 to 20% by weight, and more preferably 4 to 15% by weight, based on dry weight. If two or more types of hydrophilic modified polysiloxane are present, these amounts refer to the total sum of the hydrophilic modified polysiloxane components.

[0113] Of particular interest are hydrophilic modified polysiloxanes in which the relative weight of the hydrophilic portion is 5% or more (e.g., 5-60%), 6% or more (e.g., 6-50%), and especially 10% or more (e.g., 10-40%) of the total weight of the hydrophilic modified polysiloxane.

[0114] The weight percentage of the hydrophilic portion can be calculated based on the stoichiometric ratio of the starting materials in the synthesis of hydrophilic modified polysiloxane, or it can be determined using analytical techniques such as IR or NMR.

[0115] If there is a molar excess of reactants, such molar excess is not counted when determining the weight percentage of the hydrophilic portion. Only monomers that can react based on the stoichiometry of the reaction are counted.

[0116] Hydrophilic modified polysiloxanes may contain small amounts of impurities such as cyclic siloxanes, including D4, D5, and D6 cyclic siloxanes, which are residues from polysiloxane synthesis. The names (D4, D5, or D6) refer to the number of repeating Si-O units in the cyclic polysiloxane (i.e., 4, 5, or 6 repeating Si-O units in the cyclic polysiloxane). From a health, safety, and environmental standpoint, it is preferable to limit the amount of cyclic polysiloxane present in the coating composition. In one preferred embodiment, the hydrophilic modified polysiloxane contains less than 5%, preferably less than 2%, and more preferably less than 1% of cyclic polysiloxane. In one particularly preferred embodiment, the hydrophilic modified polysiloxane does not contain cyclic polysiloxane.

[0117] In one preferred embodiment, the hydrophilic modified polysiloxane is a polyether-modified polysiloxane.

[0118] Preferably, the polyether group comprises at least three repeating units, for example, at least five repeating units. In many interesting embodiments, the oligomer or polymer comprises 5 to 100 repeating units, for example, 5 to 50, or 8 to 50, or 8 to 20 repeating units.

[0119] In some preferred embodiments, the polyether group (i.e., oligomer or polymer group) has a number-average molecular weight (n) in the range of 100 to 2500 g / mol, for example, in the range of 200 to 2000 g / mol, particularly in the range of 300 to 2000 g / mol, or in the range of 400 to 1000 g / mol.

[0120] Of particular interest are polyether-modified polysiloxanes in which the relative weight of the polyether portion is 5% or more of the total weight (e.g., 5-60%), for example, 6% or more of the total weight of the polyether-modified polysiloxane (e.g., 6-50%), and especially 10% or more (e.g., 10-40%).

[0121] In one modified embodiment of the present invention, the polyether-modified polysiloxane is a polysiloxane grafted with poly(oxyalkylene) chains. An exemplary structure of such a polyether-modified polysiloxane is given by formula (A).

[0122] [ka]

[0123] In the formula, each R 7 Independently, C 1-5 -Selected from alkyl (including linear or branched hydrocarbon groups) and aryl (e.g., phenyl(-C6H5)), particularly methyl, Each R 8 These are independently -H, C 1-4 -Alkyl (e.g., -CH3, -CH2CH3, -CH2CH2CH3, -CH(CH3)2, -CH2CH2CH2CH3), phenyl (-C6H5), and C 1-4 -Alkylcarbonyl (e.g., -C(=O)CH3, -C(=O)CH2CH3 and -C(=O)CH2CH2CH3), particularly selected from -H, methyl, and -C(=O)CH3, Each R 9 Independently, C 2-5-alkylene (e.g., -CH2CH2-, -CH2CH(CH3), -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH(CH2CH3)-), arylene (e.g., 1,4-phenylene) and C substituted with aryl 2-5 -alkylene (e.g., 1-phenylethylene), especially C such as -CH2CH2- and -CH2CH(CH3)- 2-5 selected from -alkylene k is 0 to 240, l is 1 to 60, k + l is 1 to 240, and n is 0 to 50, m is 0 to 50, and m + n is 1 to 50.

[0124] In particular, R 7 is methyl, each R 8 is independently selected from -H or C 1-4 -alkyl or -C(=O)CH3, each R 9 is -CH2CH2-, or -CH2CH2CH2-, or -CH2CH(CH3)-), k is 0 to 240, l is 1 to 60, k + l is 1 to 240, and n is 0 to 50, m is 0 to 50, and m + n is 1 to 50. All R 7 groups are preferably the same.

[0125] Examples of commercially available polyether-modified polysiloxanes of this type are KF352A, KF353, KF945, KF6012, KF6017 from ShinEtsu and XIAMETER OFX-5220, DOWSIL OFX-5247, XIAMETER OFX-5329, XIAMETER OFX-5330 from DOW.

[0126] Another modification of the present invention is that the polyether-modified polysiloxane is a polysiloxane in which a poly(oxyalkylene) chain is incorporated into its backbone. An exemplary example of the structure of such a hydrophilic modified polysiloxane is formula (B).

[0127] [Chemical formula]

[0128] In the formula, each R 7 is independently selected from C 1-5 -alkyl (including linear or branched hydrocarbon groups) and aryl (e.g., phenyl (-C6H5)), particularly methyl. Each R 8 is independently -H, C 1-4 -alkyl (e.g., -CH3, -CH2CH3, -CH2CH2CH-CH(CH3)2, -CH2CH2CH2CH3), phenyl (-C6H5), and C 1-4 -alkylcarbonyl (e.g., -C(=O)CH3, C(=O)CH2CH3, and -C(=O)CH2CH2CH3), particularly selected from -H, methyl, and -C(=O)CH3. Each R 9 is independently C 2-5 -alkylene (e.g., -CH2CH2-, -CH2CH(CH3)-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH(CH2CH3)-), arylene (e.g., 1,4-phenylene), and C 2-5 -alkylene substituted with aryl (e.g., 1-phenylethylene), particularly C 2-5 -alkylene such as -CH2CH2- and -CH2CH(CH3)-. k is from 0 to 240, and n is from 0 to 50, m is from 0 to 50, and m + n is from 1 to 50. Particularly, R 7 is methyl, each R 8 is independently selected from -H or C 1-4 -alkyl or -C(=O)CH3, each R 9 is -CH2CH2-, -CH2CH(CH3)-, or -CH2CH2CH2-, k is from 0 to 240, Furthermore, n is between 0 and 50, m is between 0 and 50, and m+n is between 1 and 50.

[0129] All R 7 The base is preferably the same.

[0130] Commercial hydrophilic modified polysiloxanes of this type include DOWSIL 2-8692 and XIAMETER OFX-3667 from DOW.

[0131] In yet another variation, polyether-modified polysiloxanes are polysiloxanes in which polyoxyalkylene chains are incorporated into their backbone and grafted onto them. An exemplary example of such a hydrophilic-modified polysiloxane structure is shown in formula (C):

[0132] [ka]

[0133] In the formula, each R 7 Independently, C 1-5 -Selected from alkyl (including linear or branched hydrocarbon groups) and aryl (e.g., phenyl(-C6H5)), particularly methyl, Each R 8 These are independently -H, C 1-4 -Alkyl (e.g., -CH3, -CH2CH3, -CH2CH2CH3, -CH(CH3)2, -CH2CH2CH2CH3), phenyl (-C6H5), and C 1-4 -Alkylcarbonyl (e.g., -C(=O)CH3, -C(=O)CH2CH3 and -C(=O)CH2CH2CH3), particularly selected from -H, methyl, and -C(=O)CH3, Each R 9 Independently, C 2-5 -Alkylenes (e.g., -CH2CH2-, -CH2CH(CH3)-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH(CH2CH3)-), arylenes (e.g., 1,4-phenylene), and aryl-substituted C 2-5- From alkylenes (e.g., 1-phenylethylene), especially C such as -CH2CH2- and -CH2CH(CH3)- 2-5 - Selected from alkylene, k is between 0 and 240, l is between 1 and 60, and k+l is between 1 and 240. n is between 0 and 50, m is between 0 and 50, and m+n is between 1 and 50.

[0134] In particular, R 7 It is methyl, Each R 8 is -H, or C 1-4 -alkyl, or -C(=O)CH3, Each R 9 These are -CH2CH2-, -CH2CH2CH2-, - or -CH2CH(CH3)-, k is between 0 and 240, y is between 1 and 60, and x+y is between 1 and 240. n is between 0 and 50, m is between 0 and 50, and m+n is between 1 and 50.

[0135] In the structures (A), (B), and (C) above, the groups -CH2CH(CH3)-, -CH2CH(CH2CH3)-, etc., can exist in either of two possible orientations. Similarly, it should be understood that the k and l times present segments are typically randomly distributed within the polysiloxane structure.

[0136] In these embodiments and variations, the polyether or poly(oxyalkylene) is preferably selected from polyoxyethylene, polyoxypropylene, and poly(oxyethylene-co-oxypropylene) (sometimes called polyethylene glycol, polypropylene glycol, and poly(ethylene glycol-co-propylene glycol)). Thus, in the above structures (A), (B), and (C), each R linking the two oxygen atoms 9 It is preferable that the R is selected from -CH2CH2- and -CH2CH(CH3)-, and each R connects the silicon atom and the oxygen atom. 9 C 2-5 - Preferably selected from alkyl groups.

[0137] In some embodiments of the above structures (A), (B), and (C), R 8 It is preferably not hydrogen.

[0138] It should be understood that one or more polyether-modified polysiloxanes may be of different types, for example, two or more of the types described above.

[0139] In another preferred embodiment, the hydrophilic modified polysiloxane comprises a polyglycerol group or a pyrrolidone group.

[0140] Crosslinking agent and / or curing agent The polysiloxane-based binder of the present invention is curable and contains curing-reactive functional groups such as silanols, alkoxysilanes, ketoximes, and / or alkoxy groups. Preferably, the polysiloxane-based binder contains at least two curing-reactive functional groups. Optionally, the polysiloxane-based binder contains two or more types of curing-reactive functional groups. Preferably, the polysiloxane-based binder contains a single type of curing-reactive functional group. A suitable crosslinking agent and / or curing agent is selected depending on the curing-reactive functional groups present in the polysiloxane-based binder.

[0141] In preferred polysiloxane-based binders, the curing-reactive functional group is silanol and / or alkoxysilane. In even more preferred polysiloxane-based binders, the curing-reactive functional group is silanol, In some cases, it may be necessary to add a crosslinking agent to obtain the desired crosslinking density. When the curing reactive functional group is a silanol, preferred crosslinking agents are organosilicon compounds represented by the following general formula, their partially hydrolyzed condensates, or mixtures thereof.

[0142] [ka]

[0143] During the ceremony, Each R is independently a monovalent hydrocarbon group having 1 to 6 carbon atoms, or a C(alkylene oxide) substituted with a poly(alkylene oxide). 1-6 Alkyl, or structure (O-(O-(CR D 2) r’ ) r1’ -(O-(CR D 2) s’ ) s1’ -(Si(R PP )2-O) t’ -Si(R PP ) Selected from 3 polysiloxanes, where r', r1', s', and s1' are integers from 0 to 10, and each R D is H or C 1-4 Selected independently of alkyl, each R PP C 1-10 Alkyl, C 6-10 Ariel, C 7-10 Selected independently from alkylaryls, t' is an integer between 1 and 50. Each K is independently selected from hydrolyzable groups such as alkoxy groups, and d is 0, 1, or 2, more preferably 0 or 1.

[0144] Preferred crosslinking agents of this type include tetraethoxysilane, vinyltris(methylethyloxymo)silane, methyltris(methylethyloxymo)silane, vinyltrimethoxysilane, methyltrimethoxysilane, and vinyltriisopropenoxysilane, as well as their hydrolysis condensation products.

[0145] When the curing-reactive functional group is di- or tri-alkoxy, a separate crosslinking agent is generally not required.

[0146] The crosslinking agent is preferably present in an amount of 0 to 10% by weight, preferably 2.0 to 8.0% by weight, of the total dry weight of the coating composition. Suitable crosslinking agents, such as Wacker's Silicate TES-40 WN and Evonik's Dynasylan A, are commercially available.

[0147] This component is not considered part of the binder system.

[0148] Catalyst component (B) To assist the curing process, the coating composition of the present invention includes an organic catalyst component (B), which is a low molecular weight amidine or a low molecular weight amine compound such as aminosilane. The term "low molecular weight" means that its molecular weight is less than 1000 g / mol, for example, 50 to 500 g / mol, preferably 100 to 400 g / mol. In preferred embodiments, the low molecular weight amidine or low molecular weight amine compound is not guanidine or a guanidine derivative. In more preferred embodiments, the defouling and peeling coating composition disclosed herein does not contain a guanidine-based catalyst.

[0149] Guanidine derivatives are compounds that contain the following motifs:

[0150] [ka]

[0151] A suitable amidine is a compound containing the following motifs:

[0152] [ka]

[0153] Preferably, amidine is represented by the following general formula:

[0154] [ka]

[0155] In the formula, R1, R2, and R4 are each independently selected from hydrogen, a monovalent organic group, a monovalent heteroorganic group, and combinations thereof. R3 is a monovalent organic group, a monovalent heteroorganic group, or a combination thereof. And / or any two or more of R1, R2, R3, and R4 may, depending on the circumstances, bond together to form a ring structure.

[0156] R1, R2, and R4 are preferably hydrogen or a C1-6 alkyl or phenyl group.

[0157] R3 is C 1-6 It is an alkyl group or a phenyl group.

[0158] More preferably, R2 + R4 combine to form a ring, and / or R1 + R3 combine to form a ring. Such rings are preferably aliphatic 5-7 membered rings.

[0159] A preferred option is a cyclic amidine, preferably a bicyclic amidine, such as 1,8-diazabicyclo-5,4,0-7-undecene (DBU). The chemical structure of DBU is shown below.

[0160] [ka]

[0161] The catalyst may also be a low molecular weight organic amine compound such as triethylamine, cyclic amine, tetramethylethylenediamine, 1,4-ethylenepiperazine, and pentamethyldiethylenetriamine.

[0162] However, preferred amines are aminosilanes, such as aminoalkyltrialkoxysilanes, such as 3-aminopropyltriethoxysilane or 3-aminopropyltrimethoxysilane, or bis(alkyltrialkoxysilyl)amines, preferably including bis(3-propyltrimethoxysilyl)amine or bis(3-propyltriethoxysilyl)amine. Another option is N,N-dibutylaminomethyltriethoxysilane.

[0163] Suitable aminosilanes are those of general formula (I) or (II)

[0164] [ka]

[0165] In the formula, z is an integer between 1 and 3.

[0166] [ka]

[0167] In the formula, y is an integer between 1 and 2. Each R is a hydrocarbyl group having 1 to 12 C atoms, which may contain an ether or aminolinker. R 1 This is a hydrocarbyl group having 1 to 12 C atoms, Each X independently represents an alkoxy group.

[0168] Y is an amino acid bonded to R.

[0169] The Y group can be attached to any part of the R chain.

[0170] The amino group is preferably N-di-C1-6-alkyl or NH2.

[0171] It is particularly preferable that X is a C1-6 alkoxy group, especially a methoxy or ethoxy group. It is also particularly preferable that there are two or three alkoxy groups. Therefore, z is ideally 2 or 3, especially 3.

[0172] The subscript y is preferably 2.

[0173] R 1 Preferably, it is a C1-4 alkyl group such as methyl.

[0174] R is a hydrocarbyl group having up to 12 carbon atoms. Hydrocarbyl means a group containing only C and H atoms. It may include an alkylene chain or a combination of an alkylene chain with a ring such as a phenyl or cyclohexyl ring. The phrase "may contain an ether or aminolinker" means that the carbon chain may be interrupted by -O- or -NH- groups in the chain.

[0175] R is preferably an unbranched alkyl chain having 2 to 8 unsubstituted (clearly other than Y) carbon atoms.

[0176] Therefore, the preferred silane general formula is that of structure (III).

[0177] [ka]

[0178] In the formula, z' is an integer between 2 and 3. R' is an unsubstituted, unbranched alkyl chain having 2 to 8 carbon atoms, which may contain an ether or aminolinker. Y' is an amino functional group bonded to the R' group, and X' represents an alkoxy group.

[0179] Examples of such silanes include the product manufactured by Degussa of Rheinfelden and sold under the trademark name Dynasylan(R)D, Silquest(R) silane manufactured by Momentive, and many representative GENOSIL(R) silane manufactured by Wacker.

[0180] Preferred aminosilanes include aminopropyltrimethoxysilane (Dynasylan AMMO; Silquest Al 110), aminopropyltriethoxysilane (Dynasylan AMEO) or N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (Dynasylan DAMO, Silquest Al 120), N-(2-aminoethyl)-3-aminopropyltriethoxysilane, triamino-functional trimethoxysilane (Silquest A-1130), bis(gamma-trimethoxysilylpropyl)amine (Silquest Al 170), N-ethyl-gamma-aminoisobityltrimethoxysilane (Silquest A-Link 15), N-phenyl-gamma-aminopropyltrimethoxysilane (Silquest Y-9669), and 4-amino-3,3-dimethylbutyltrimethoxysilane (Silquest Y-9669). This includes (1637), (N-cyclohexylaminomethyl)triethoxysilane (Genosil XL 926), (N-phenylaminomethyl)trimethoxysilane (Genosil XL 973), and mixtures thereof.

[0181] Other specific silanes of interest include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(aminoethyl)-aminopropyltrimethoxysilane H2NCH2CH2NHCH2CH2CH2Si(OCH3)3, 3-aminopropylmethyldiethoxysilane, and 3-(2-aminoethylamino)propylmethyldimethoxysilane (H2NCH2CH2NHCH2CH2CH2SiCH3(OCH3)2).

[0182] The amount of component (B) present in the coating composition may be 0.05 to 5.0% by weight, preferably 0.1 to 4.0% by weight, for example 0.25 to 4.0% by weight, and more preferably 0.5 to 3.0% by weight (dry weight).

[0183] This component is not considered part of the binder system.

[0184] metal catalyst To assist the curing process, enhance robustness, and ensure adequate pot life, the coating compositions of the present invention preferably contain a metal catalyst. Typical examples of catalysts that can be used include catalysts containing Zn, Li, K, Bi, Fe, Ce, or Zr, such as their salts and organometallic complexes. The salts are preferably salts and / or chelates of long-chain carboxylic acids or organometallic salts.

[0185] The metal catalyst is preferably bismuth(III), iron(II), iron(III), zinc(II), zirconium(IV), cerium(III), potassium, or a lithium compound, with bismuth(III) and lithium being particularly preferred. Zinc-containing catalysts are also particularly preferred.

[0186] Examples of anionic organic groups include methoxide, ethoxide, n-propoxide, isopropoxide, n-butoxide, isobutoxide, sec-butoxide, tert-butoxide, triethanolamine, and 2-ethylhexyloxide group; acetate, formate, n-octoate, 2-ethylhexanoate, 2,4,4-trimethylpentanoate, 2,2,4-trimethylpentanoate, 6-methylheptaneate, Carboxylic acid groups such as oleate, ricinolate, palmitate, hexoate, hexadecanate, 2-ethylhexanoate, benzoate, 1,4-dibenzoate, stearate, acrylate, laurate, methacrylate, 2-carboxyethyl acrylate, oxalate, 10-undecylenate, dodecanoate, citrate, 3-oxopentanoate, 3-oxobutanoate, and neodecanoate groups; di Examples include amide groups such as methylamide, diethylamide, ethylmethylamide, and dipropylamide; lactic acid groups; trialkylsiloxy groups, more specifically trimethylsiloxy and triethylsiloxy groups; and carbonate groups (O-CO-OR') and carbamate groups (O-CO-NR'2) (wherein R' may be the same or different, monovalent or divalent, and may be a substituted hydrocarbon group, and further may be hydrogen, trimethoxysilylpropyl, triethoxysilylpropyl, dimethoxymethylsilylpropyl, diethoxymethylsilylpropyl, N-[3-(trimethoxysilyl)propyl]-2-aminoethyl, N-[3-(triethoxysilyl)propyl]-2-aminoethyl, N-[3-(dimethoxymethylsilyl)propyl]-2-aminoethyl, or N-[3-(diethoxymethylsilyl)propyl]-2-aminoethyl groups).

[0187] Examples of metal salt compounds include bismuth(III) 2-ethylhexanoate, bismuth(III) neodecanoate, bismuth(III) acetate, bismuth(III) octanoate, iron(II) acetate, tert-iron butoxide, iron(III) citrate, iron(II) lactate, iron(II) oxalate, iron(III) oxalate, iron(III) 2-ethylhexanoate, zinc(II) acetate, zinc(II) formate, zinc(II) benzoate, zinc(II) 2-ethylhexanoate, n-zinc octoate, zinc(II) stearate, zinc(II) ethoxide, zinc(II) acrylate, zinc(II) methacrylate, zinc(II) naphthenate, zinc(II) oxalate, and 10- These include zinc(II) undecylenate, zinc(II) 3-oxopentanoate, zinc(II) 3-oxobutanoate, zirconium(IV) acetate, zirconium(IV) 2-ethylhexanoate, zirconium(IV) lactate, zirconium(IV) n-butoxide, zirconium(IV) tert-butoxide, zirconium(IV) isopropoxide, zirconium(IV) n-propoxide, zirconium(IV) 2-carboxyethyl acrylate, zirconium(IV) tetrakis(diethylamide), zirconium(IV) tetrakis(ethylmethylamide), and zirconium(IV) bis(diethyl citrate)-di-n-propoxide. The use of cerium neodecanoate is also anticipated.

[0188] The metal chelate compounds include bismuth(III) 2,2,6,6-tetramethyl-3,5-heptane dionate, bismuth(III) acetylacetonate, iron(II) acetylacetonate, iron(III) acetylacetonate, iron(III) 2,2,6,6-tetramethyl-3,5-heptane dionate, iron(II) 2,2,6,6-tetramethyl-3,5-heptane dionate, zinc(II) hexafluoroacetylacetonate, zinc(II) 1,3-diphenyl-1,3-propane dionate, zinc(II) 1-phenyl-5-methyl-1,3-hexane dionate, zinc(II) 1,3-cyclohexane dionate, and zinc(II) 2-acetylcyclohexane Xanonate, zinc(II) 2-acetyl-1,3-cyclohexanedione, zinc(II) ethyl salicylate, zinc(II) dimalonate, zinc(II) dimalonate, zinc(II) ethyl acetoacetate, benzyl salicylate zinc(II), zinc(II) acetylacetonate, zinc(II) 2,2,6,6-tetramethyl-3,5-heptanedione, tin(II) acetylacetonate, zirconium(IV) acetylacetonate, zirconium(IV) 2,2,6,6-tetramethyl-3,5-heptanedione, zirconium(IV) trifluoroacetylacetonate, zirconium(IV) hexafluoroacetylacetonate.

[0189] Suitable lithium catalysts include lithium 2-ethylhexanoate and lithium neodecanoate. Commercially available lithium catalysts include, for example, Borchers Deca Lithium 2 from Borchers SAS.

[0190] Suitable potassium catalysts include potassium 2-ethylhexanoate and potassium neodecanoate. Examples of commercially available potassium catalysts include 15% potassium Hex-Cem® EU from Borchers SAS and TIB KAT K30 from TIB Chemicals.

[0191] Examples of suitable zinc catalysts are zinc 2-ethylhexanoate, zinc naphthenate, and zinc stearate. Examples of commercially available zinc catalysts include K-KAT XK-672, K-KAT XK-661, and K-KAT 670 from King Industries and Borchi Kat 22 from Borchers.

[0192] Examples of suitable bismuth catalysts are organic bismuth compounds such as bismuth 2-ethylhexanoate, bismuth octanoate, and bismuth neodecanoate. Examples of commercially available organic bismuth catalysts are Borchi Kat 24 and Borchi Kat 315 from Borchers, K-KAT XK-651 from King Industries, Reaxis C739E50 from Reaxis, and TIB KAT 716 from TIB Chemicals.

[0193] Other suitable catalysts are iron catalysts such as iron stearate and iron 2-ethylhexanoate, and zirconium catalysts such as zirconium naphthenate, tetrabutyl zirconate, tetrakis(2-ethylhexyl) zirconate, triethanolamine zirconate, tetra(isopropenyloxy)-zirconate, zirconium tetrabutanolate, zirconium tetrapropanolate, and zirconium tetraisopropanolate. A more preferred catalyst is a zirconium ester.

[0194] In a preferred embodiment, the metal additive is a bismuth and / or lithium catalyst.

[0195] Preferably, the metal catalyst is present in the coating composition of the present invention in an amount of 0.1 to 5.0% by weight, more preferably 0.5 to 4.0% by weight, based on the total dry weight of the coating composition.

[0196] This component is not considered part of the binder system.

[0197] Antifouling agent The fouling release coating composition of the present invention may contain an antifouling agent.

[0198] The terms antifouling agent, biologically active compound, antifouling agent, biocide, and toxicant are used in the industry to describe known compounds that act to prevent marine fouling on surfaces. When present, the antifouling agent can be inorganic, organometallic or organic. Preferably, when present, the antifouling agent is an organometallic antifouling agent. Suitable antifouling agents are commercially available.

[0199] Examples of inorganic antifouling agents include copper and copper compounds such as copper oxide, for example cuprous oxide and cupric oxide; copper alloys such as copper-nickel alloys; and copper salts such as copper thiocyanate and copper sulfide.

[0200] Examples of organometallic antifouling agents include zinc pyrithione; organic copper compounds such as copper pyrithione, copper acetate, copper di(ethyl 4,4,4-trifluoroacetoacetate), copper naphthenate, copper oxine, copper nonylphenol sulfonate, copper bis(ethylenediamine) bis(dodecylbenzenesulfonate), and copper bis(pentachlorophenolate); and dithiocarbamate compounds such as zinc bis(dimethyldithiocarbamate) [ziram], zinc ethylene bis(dithiocarbamate) [zineb], manganese ethylene bis(dithiocarbamate) [maneb], and manganese ethylene bisdithiocarbamate) [mancozeb] which forms a complex with a zinc salt.

[0201] Examples of organic antifouling agents include heterocyclic compounds such as 2-(tert-butylamino)-4-(cyclopropylamino)-6-(methylthio)-1,3,5-triazine [sibutrin], 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one [DCOIT], encapsulated 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one [DCOIT], 1,2-benzoisothiazolin-3-one, 2-(thiocyanatomethylthio)-1,3-benzothiazole [benthiazole], and 2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine; urea derivatives such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea [diuron]; and N-(dichlorofluoromethylthio)phthalimide, N-dichlorofluoromethylthio Other examples include carboxylic acid, sulfonic acid, and sulfenic acid amides and imides such as N',N'-dimethyl-N-phenylsulfamide [dichlorofluanide], N-dichlorofluoromethylthio-N',N'-dimethyl-Np-tolylsulfamide [tolylsulfanide], and N-(2,4,6-trichlorophenyl)maleimide; pyridinetriphenylborane [TPBP], aminetriphenylborane, 3-iodo-2-propynyl N-butylcarbamate [iodocarb], 2,4,5,6-tetrachloroisophthalonitrile, p-((diiodomethyl)sulfonyl)toluene, and 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile [tralopyryl] and quaternary ammonium salts.

[0202] Other examples of antifouling agents include tetraalkylphosphonium halogenides, guanidine derivatives, imidazole-containing compounds such as 4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole [medetomidine] and its derivatives, macrocyclic lactones such as avermectin and its derivatives such as ivermectin, spinosin and its derivatives such as spinosad, capsaicin and its derivatives such as phenylcapsaicin, and enzymes such as oxidases, which are proteolytic, hemicelluloselytic, celluloselytic, lipolytic, and aminolytic enzymes.

[0203] Preferred antifouling agents are zinc pyrithione, copper pyrithione, zinc ethylenebis(dithiocarbamate) [zineb], 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one [DCOIT], and encapsulated 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one [DCOIT]. Particularly preferred antifouling agents are zinc pyrithione and copper pyrithione, especially copper pyrithione.

[0204] If present, biocides may constitute 1-20% of the dry weight of the total coating composition, preferably 1-15%, 2-15%, or 3-12% of the dry weight of the total coating composition.

[0205] This component is not considered part of the binder system.

[0206] Added oil The coating composition of the present invention may contain additive oils. Preferably, the coating composition of the present invention contains 0 to 30% by weight, more preferably 0.1 to 20% by weight, of additive oils based on the dry weight of the coating composition. The hydrophilic modified polysiloxanes described herein are not considered "additive oils." Therefore, additive oils are oils different from the hydrophilic modified polysiloxanes described herein.

[0207] Suitable non-reactive additive oils include silicone oils, such as methylphenyl silicone oil, petroleum, polyolefin oils, polyaromatic oils, fluororesins, such as polytetrafluoroethylene or fluid fluorinated alkyl or alkoxy-containing polymers, or lanolin and lanolin derivatives and other sterols and / or sterol derivatives as disclosed in International Publication No. 2013024106A1, or combinations thereof. A preferred non-reactive additive oil is methylphenyl silicone oil.

[0208] Further additive oils that may be present in the coating composition of the present invention are fluorinated amphiphilic polymers / oligomers, as described in International Publication No. 2014131695. Suitable additive oils may also be based on polysiloxane side chains and methacrylate copolymers having polyethers or nitrogen-containing hydrophilic groups, as described in International Publication Nos. 2019101912 A1 and International Publication Nos. 2019101920 A1.

[0209] This component is not considered part of the binder system.

[0210] pigment The coating composition of the present invention preferably comprises one or more pigments. The pigments may be inorganic pigments, organic pigments, or mixtures thereof. Inorganic pigments are preferred. The pigments may be surface-treated.

[0211] Representative examples of pigments include black iron oxide, red iron oxide, yellow iron oxide, titanium dioxide, zinc oxide, carbon black, graphite, red molybdate, yellow molybdate, zinc sulfide, antimony oxide, sodium aluminum sulfosilicate, quinacridone, phthalocyanine blue, phthalocyanine green, indanthron blue, cobalt aluminum oxide, carbazole dioxazine, isoindoline orange, bis-acetoaceto-tridiol, benzimidazolon, quinafthron yellow, isoindoline yellow, tetrachloroisoindolinone, quinophthalone yellow, and metal flake materials (e.g., aluminum flakes). Preferred pigments are black iron oxide, red iron oxide, yellow iron oxide, phthalocyanine blue, and titanium dioxide. In one preferred embodiment, titanium dioxide is surface-treated with a silicone compound, a zirconium compound, or a zinc compound.

[0212] The amount of pigment present in the coating composition of the present invention is preferably 0 to 25% by weight, more preferably 0.5 to 15% by weight, based on the total dry weight of the coating composition.

[0213] This component is not considered part of the binder system.

[0214] solvent The fouling release coating composition of the present invention preferably contains a solvent. Solvents suitable for use in the composition of the present invention are commercially available.

[0215] Examples of suitable organic solvents and thinners include aromatic hydrocarbons such as xylene, toluene, mesitylene; ketones such as methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, methyl isoamyl ketone, cyclopentanone, cyclohexanone; esters such as butyl acetate, tert-butyl acetate, amyl acetate, isoamyl acetate, ethylene glycol methyl ether acetate, propylene glycol methyl ether acetate; ethers such as ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dibutyl ether, dioxane, tetrahydrofuran; alcohols such as n-butanol, isobutanol, benzyl alcohol; ether alcohols such as butoxyethanol, 1-methoxy-2-propanol; aliphatic hydrocarbons such as white spirit; and optionally, mixtures of two or more solvents and thinners.

[0216] The amount of solvent present in the fouling release coating composition of the present invention is preferably as small as possible in order to minimize the VOC content. Preferably, the solvent is present in the composition of the present invention in an amount of 0 to 35% by weight, more preferably 1 to 30% by weight, based on the total weight of the composition. Those skilled in the art will understand that the solvent content may vary depending on the other components present.

[0217] This component is not regarded as part of the binder system.

[0218] Filler The coating composition of the present invention may optionally contain a filler.

[0219] Examples of fillers that can be used in the coating composition according to the present invention include zinc oxide, barium sulfate, calcium sulfate, calcium carbonate, fumed silica, bentonite, and silica or silicates containing other clays (such as talc, feldspar, kaolin, white clay, nepheline sienite, etc.), and solid silicone resins, which are generally condensed branched polysiloxanes. Some fillers, such as fumed silica, may have a thickening effect on the coating composition.

[0220] A preferred filler is a fumed silica filler. The fumed silica filler may have an untreated surface or a hydrophobic modified surface. Preferably, the fumed silica filler has a hydrophobic modified surface. Examples of commercially available fumed silica fillers are TS-610, TS-530, EH-5, H-5, and M-5 from Cabot, and Aerosil® R972, Aerosil® R974, Aerosil® R976, Aerosil® R104, Aerosil® R202, Aerosil® R208, Aerosil® R805, Aerosil® R812, Aerosil® R816, Aerosil® R7200, Aerosil® R8200, Aerosil® R9200, and Aerosil® R711 from Evonik.

[0221] The amount of filler present in the coating composition of the present invention is preferably 0 to 25% by weight, more preferably 0.1 to 10% by weight, and even more preferably 0.15 to 5.0% by weight, based on the total dry weight of the coating composition.

[0222] This component is not considered part of the binder system.

[0223] additives The coating composition of the present invention may contain one or more additives. Examples of additives that may be present in the coating composition of the present invention include reinforcing agents, thixotropes, thickeners, anti-settling agents, dehydrating agents, dispersants, wetting agents, surfactants, binders, plasticizers, and dyes.

[0224] Examples of thixotropes, thickeners, and anti-settling agents include silica such as fumed silica, organically modified clay, amide wax, polyamide wax, amide derivatives, polyethylene wax, oxidized polyethylene wax, hydrogenated castor oil wax, and mixtures thereof. Preferably, each of the thixotrope, thickener, and anti-settling agent is present in the composition of the present invention in an amount of 0 to 10% by weight, more preferably 0.1 to 6% by weight, and even more preferably 0.1 to 2.0% by weight, based on the total dry weight of the composition.

[0225] Dehydrating agents and drying agents that can be used in de-fouling and peel-off coating compositions include organic and inorganic compounds. Dehydrating agents may be hygroscopic materials that absorb water or bind water as crystal water, often called a desiccant. Examples of drying agents include calcium sulfate hemihydrate, anhydrous calcium sulfate, anhydrous magnesium sulfate, anhydrous sodium sulfate, anhydrous zinc sulfate, molecular sieves, and zeolites. Dehydrating agents may be compounds that chemically react with water. Examples of dehydrating agents that react with water include orthoesters such as trimethyl orthoformate, triethyl orthoformate, tripropyl orthoformate, triisopropyl orthoformate, tributyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, tributyl orthoacetate, and triethyl orthopropionate; ketals; acetals; enol ethers; orthoborates such as trimethyl borate, triethyl borate, tripropyl borate, triisopropyl borate, tributyl borate, and tri-tert-butyl borate; and organosilanes such as trimethoxymethylsilane, vinyltrimethoxysilane, phenyltrimethoxysilane, tetraethoxysilane, and ethyl polysilicate.

[0226] Preferably, the dehydrating agent is present in the composition of the present invention in an amount of 0 to 5% by weight, more preferably 0.5 to 2.5% by weight, and even more preferably 1.0 to 2.0% by weight, based on the total dry weight of the composition.

[0227] Therefore, in a preferred embodiment, the present invention does not contain tin compounds. (a) A binder A based on curable polysiloxane, having a weight-average Mw of 50,000 g / mol or less or a viscosity of 2,800 mPas or less, and 30% by weight or more (b) 0.1 to 5.0% by weight of at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing (dry weight) [the specified ingredient].

[0228] Therefore, in a preferred embodiment, the present invention does not contain tin compounds. (a) A binder A based on curable polysiloxane, having a weight-average Mw of 50,000 g / mol or less or a viscosity of 2,800 mPas or less, and 20% by weight or more. (b) A binder B with a weight-average Mw of 55,000 g / mol or more and a viscosity of weight-average Mw or 3,500 mPas or more, comprising 20% ​​by weight or more of a curable polysiloxane-based binder B (c) 0.1 to 5.0% by weight of at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing (dry weight) [the specified ingredient].

[0229] Therefore, in a preferred embodiment, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and B, wherein the weight-average Mw of binder A is 50,000 g / mol or less, the weight-average Mw of binder B is 55,000 g / mol or more, and binder A constitutes at least 27% by weight of the total polysiloxane-based binder system, and at least 40% by weight of the polysiloxane-based binder system. A polysiloxane-based binder system comprising at least 40% by weight of at least two different curable polysiloxane-based binders A and B, wherein the viscosity of binder A is 2,800 mPas or less, the viscosity of binder B is 3,500 mPas or more, and binder A constitutes at least 27% by weight (dry weight) of the total polysiloxane-based binder system, or A polysiloxane-based binder system comprising at least 40% by weight of a polysiloxane-based binder A having a weight-average Mw of 50,000 g / mol or less, wherein binder A constitutes at least 60% by weight of the total polysiloxane-based binder system, or A polysiloxane-based binder system comprising at least 40% by weight of a polysiloxane-based binder A having a viscosity of less than 2,800 mPas, wherein binder A constitutes at least 60% by weight of the total polysiloxane-based binder system, (b) 0.1 to 5.0% by weight of at least one low molecular weight amidine or low molecular weight amine compound, The present invention provides a stain-removing coating composition containing (dry weight) [the specified ingredient].

[0230] Therefore, in a preferred embodiment, the present invention does not contain tin compounds. (a) A polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and B, wherein the weight-average Mw of binder A is 50,000 g / mol or less, the weight-average Mw of binder B is 55,000 g / mol or more, and binder A constitutes at least 27% by weight of the total polysiloxane-based binder system, and at least 40% by weight of the polysiloxane-based binder system. A polysiloxane-based binder system comprising at least 40% by weight of at least two different curable polysiloxane-based binders A and B, wherein the viscosity of binder A is 2,800 mPas or less, the viscosity of binder B is 3,500 mPas or more, and binder A constitutes at least 27% by weight (dry weight) of the total polysiloxane-based binder system, or A polysiloxane-based binder system comprising at least 40% by weight of a polysiloxane-based binder A having an Mw of 5,000 g / mol or less, wherein binder A constitutes at least 60% by weight of the total polysiloxane-based binder system, or A polysiloxane-based binder system comprising at least 40% by weight of a curable polysiloxane-based binder A having a viscosity of 2,800 mPas or less, wherein binder A constitutes at least 60% by weight of the total polysiloxane-based binder system, (b) 0.1 to 5.0% by weight of at least one low molecular weight amidine or low molecular weight amine compound, (c) At least one metal catalyst, preferably 0.1 to 5.0% by weight, which is a salt of Zn, Li, K, Fe, Bi, or Zr, or an organometallic compound, (d) 0 to 30% by weight, preferably 1.0 to 30% by weight of hydrophilic modified polysiloxane, (e) 0 to 8.0% by weight, preferably 2.0 to 8.0% by weight of a crosslinking agent, The present invention provides a stain-removing coating composition containing (dry weight) [the specified ingredient].

[0231] Compositions and paints The present invention also relates to a method for preparing such a defouling and peeling coating composition by mixing the components present in the composition. Any conventional manufacturing method may be used.

[0232] The compositions described herein may be prepared, for example, at concentrations suitable for use in spray coating. In this case, the composition is a paint itself. Alternatively, the composition may be a concentrate for preparing a paint. In this case, further solvents and optionally other components are added to the compositions described herein to form a paint. Preferred solvents are as described above with respect to the compositions.

[0233] After mixing, and optionally after the addition of a solvent, the de-fouling and de-fouling coating composition or paint is preferably filled into a container. Suitable containers include cans, drums, and tanks.

[0234] The defacement-removing coating composition may be supplied in 1 pack, 2 packs, or 3 packs. Preferably, the composition is supplied in 2 packs or 3 packs.

[0235] When supplied as a two-pack, the first container preferably contains a polysiloxane-based binder, and the second container preferably contains an optional curing agent and catalyst component (B). Instructions for mixing the contents of the containers may be provided as needed. An optional hydrophilic modified polysiloxane is preferably part of the first container. An optional catalyst is preferably part of the second container.

[0236] In certain embodiments, the present invention provides a kit for preparing a fouling removal composition as defined herein.

[0237] The stain-removing coating composition and paint of the present invention preferably have a solid content of 50 to 99% by weight, more preferably 60 to 99% by weight, and even more preferably 65 to 99% by weight.

[0238] Preferably, the stain-removing coating composition and paint of the present invention have a volatile organic compound (VOC) content of 50 to 400 g / L, preferably 50 to 350 g / L, for example, 50 to 300 g / L. The VOC content can be calculated (ASTM D5201-05A) or measured (US EPA Method 24 or ISO 11890-1).

[0239] The coating compositions of the present invention can be applied to any pre-treated coating layer designed for polysiloxane-based defouling coatings. Examples of such coating layers include epoxy anticorrosion layers and silicone-containing tie layers designed to ensure adhesion between the substrate and the final polysiloxane-based defouling coating. An example of such a tie layer is described in International Publication No. 2013 / 107827. The tie layer may optionally contain an antifouling agent.

[0240] Preferably, the tie layer has a different color from the top layer. This makes damage easier to see and ensures that the correct film thickness has been applied. Preferably, the tie layer is pink, yellow, or gray, and most preferably, the tie layer is pink.

[0241] Furthermore, the coating composition according to the present invention can also be applied to a substrate containing an aged anti-fouling layer or a fouling-removing layer. Before applying the coating composition according to the present invention to such an aged layer, the old layer is washed with high-pressure water to remove the dirt.

[0242] The coating composition according to the present invention can be applied in one or more layers. Preferably, the coating composition according to the present invention is applied in one layer.

[0243] The dry film thickness of each coating layer in the coating composition of the present invention is preferably 50 to 500 μm, more preferably 100 to 400 μm, and most preferably 150 to 300 μm. The stain-removing coating composition of the present invention will typically cure at a humidity of 20-90%, preferably 30-85%, and more preferably 40-85%.

[0244] The fouling-removing coating compositions and paints of the present invention can be applied to all or part of the surface of any article subject to marine fouling. The surface may be permanently or intermittently submerged in water (e.g., by tidal movements, loading of various cargoes, or swells). The article surface would typically be the hull of a ship, or the surface of a fixed offshore object such as an oil platform or buoy. Application of the coating compositions and paints can be achieved by any convenient means, for example, by painting (e.g., using a brush or roller), or more preferably by spraying the coating onto the article. Typically, the surface needs to be separated from seawater to allow coating. Application of the coating can be achieved as is conventionally known in the art. After the coating is applied, the coating is preferably dried and / or cured.

[0245] Purpose The anti-fouling coating of the present invention is typically applied to the surface of marine substrates, preferably to parts of marine structures that are immersed during use. Typical marine substrates include ships (but not limited to, all kinds of boats, ships, yachts, motorboats, motorcraft, ocean liners, tugboats, tankers, container ships and other cargo ships, submarines, and warships), pipes, coastal and offshore machinery, structures and all kinds of objects, such as piers, piles, bridge substructures, hydraulic equipment and structures, underwater oil well structures, nets and other aquatic cultivation equipment, and buoys. The surface of the substrate may be a "native" surface (e.g., a steel surface).

[0246] Examples Judgment method Binder viscosity measurement The viscosity of the binder was determined according to ASTM D2196 Test Method A using a Brookfield DV-I Prime digital viscometer with an LV-2 or LV-4 spindle at 12 rpm. The binder was adjusted to 23.0°C ± 0.5°C before measurement.

[0247] Determination of the average molecular weight distribution of polymers The polymer properties were revealed by gel permeation chromatography (GPC) measurements. The molecular weight distribution (MWD) was determined using a Malvern Omnisec Resolve and Reveal system with two series-connected Agilent PLgel 5 μm Mixed-D columns. The columns were calibrated by conventional calibration using narrow polystyrene standards. The analytical conditions are shown in Table 1 below.

[0248] [Table 1]

[0249] Samples were prepared by dissolving a polymer solution equivalent to 25 mg of dry polymer in 5 ml of THF. After holding the samples at room temperature for a minimum of 3 hours, they were sampled for GPC analysis. Prior to analysis, the samples were filtered through a 0.45 μm nylon filter. The number-average molecular weight (Mn), weight-average molecular weight (Mw), and polydispersity index are reported.

[0250] Preparation of coating composition First, a coating composition was prepared by mixing the components in part (A) shown in Tables 3, 4, and 5 below using a high-speed dissolving machine equipped with an impeller disc. Immediately before application of the coating, the components of part (B) were mixed with the components of part (A).

[0251] curing test The curing time was determined using a mechanical recording device. The coating was applied to a 305 mm × 25 mm × 3 mm glass strip. The strip was positioned so that a stylus could be lowered into the wet film. The stylus moved along the glass strip at a constant speed. A Beck Koller drying time recorder (TQC drying time recorder, AB3600) was set to a 24-hour test time. The coating was applied at 5°C to a glass strip with a wet film thickness of 300 μm. Measurements were performed in a curing chamber at 5°C / 85% RH. The non-stick time (TFT) of the detangling coating composition was the time from application of the coating composition to the glass plate until no needle marks were visible. An acceptable TFT is a maximum of 4 hours. The coating film is considered cured (hard-dried), and once a certain degree of hardness is achieved, no visible marks are left even when the coating is touched firmly with a finger. The drying state (wet, sticky, contact-dried, or hard-dried) was determined after 24 hours. The coating must be hard-dried after 24 hours to satisfy the requirements of the present invention. Both the requirement of a maximum of 4 hours of TFT and a hard-dry coating after 24 hours must be achieved for the curing to be considered sufficient.

[0252] [Table 2]

[0253] [Table 3]

[0254] [Table 4]

[0255] [Table 5]

[0256] [Table 6]

[0257] Regarding the above example, the following observations can be made.

[0258] Comparative Examples C1-C3, C11, and Examples 1-17 demonstrate the effect of using different catalysts in compositions based on a mixture of binders having Mw 24238 and 98279 (viscosities 440 and 22050 mPas).

[0259] Examples 1 and 2 show that when either DBU or aminosilane is used, a 50:50 mixture of B0.5 (440 mPas) and B20 (22,050 mPas) cures at 5°C. Adding a metal catalyst may be desirable to improve the robustness of the system and ensure sufficient pot life.

[0260] Examples 3 to 10 show curing with DBU or aminosilane in combination with bismuth, lithium, cerium, and zinc catalysts.

[0261] Comparative Example C1 shows that the TFT and hardness obtained using a conventional tin catalyst are equivalent to those obtained using the catalyst system of the present invention.

[0262] When the tin catalyst shown in Comparative Example C1 is replaced with only a bismuth or lithium catalyst (Comparative Examples C2 and C3), the TFT increases significantly, and the required hardness cannot be obtained.

[0263] Comparative Example C11 demonstrates that the required TFT or hardness cannot be obtained even when using a guanidine-based catalyst.

[0264] Examples 11 to 17 of the present invention contain copper pyrithione in the formulation, and curing is achieved at 5°C using DBU or AMEO alone or in combination with bismuth, zinc, and lithium catalysts.

[0265] Comparative Examples C4 to C10 and Examples 18, 19, and 20 of the present invention demonstrate the effects of combining low molecular weight and high molecular weight binders.

[0266] In Examples 1-17, a binder mixture of B20 (22,050 mPas) and B0.5 (440 mPas) was used in a 50:50 ratio. In Example 18, the ratio was B20:B0.5 (73:28). It was observed that TFT increased significantly by reducing the amount of low molecular weight binder.

[0267] Example 19 demonstrates that the required TFT and hardness can be achieved after 24 hours using a binder mixture of B20 (22,050 mPas) and B1 (1,000 mPas) in a 50:50 mixing ratio.

[0268] On the other hand, Comparative Example C10 shows that using a binder mixture of B20 (22,050 mPas) and B3.5 (3,800 mPas) in a mixing ratio of 73:28 does not work. This is due to the molecular weight of the B3.5 binder being too high to achieve the desired effect of the present invention. Comparative Example C9 shows that the combination of B20 and B5 also does not work.

[0269] Example 20 demonstrates that one binder B1 with a viscosity of 1000 mPas (Mw35,629 g / mol) cured within the required TFT with appropriate hardness.

[0270] Comparative Examples C5 to C8 demonstrate that when only one binder that does not meet the requirements of the present invention is used, sufficient curing does not occur at 5°C using the catalyst system of the present invention.

[0271] Comparative Examples C1 and C4 demonstrate that the TFT and hardness after 24 hours are equivalent for both binder and single binder combinations when using a tin-based catalyst.

[0272] The comparative examples C5 to C11 did not form a non-adhesive film during the 24-hour test.

Claims

1. (a) a polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a weight average molecular weight of 50,000 g / mol or less, wherein binder A constitutes at least 27% by weight of the total polysiloxane-based binder system; (b) at least one low molecular weight amidine or low molecular weight amine compound; 1. A tin compound-free fouling release coating composition comprising:

2. (a) a polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a viscosity of 2,800 mPas or less, wherein binder A constitutes at least 27% by weight of the total polysiloxane-based binder system; (b) at least one low molecular weight amidine or low molecular weight amine compound; 1. A tin compound-free fouling release coating composition comprising:

3. Does not contain tin compounds (a) a polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and Binder B, where Binder A has a weight average molecular weight of 50,000 g / mol or less and Binder B has a weight average molecular weight of 55,000 g / mol or more, and Binder A constitutes at least 27% by weight of the total polysiloxane-based binder system; (b) at least one low molecular weight amidine or low molecular weight amine compound; 2. The fouling release coating composition of claim 1, comprising:

4. Does not contain tin compounds (a) a polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and Binder B, where Binder A has a viscosity of 2,800 mPas or less and Binder B has a viscosity of 3,500 mPas or more, and Binder A constitutes at least 27% by weight of the total polysiloxane-based binder system; (b) at least one low molecular weight amidine or low molecular weight amine compound; 3. The fouling release coating composition of claim 2, comprising:

5. 5. The fouling release coating composition of claim 3 or 4, wherein said mixture of said at least two polysiloxane-based binders A and B has a PDI greater than 2.

5.

6. A fouling release coating composition according to claim 1, wherein the polysiloxane-based binder A has a weight-average molecular weight of 8,000 to 50,000 g / mol and / or a viscosity of 300 to 2,800 mPas.

7. The polysiloxane-based binder A or binder B has the formula (D1): 【Chemistry 1】 (In the formula, Each R 1 are independently a hydroxyl group, C 1-6 -alkoxy group, or O-Si(R 5 ) 3 - z (R 6 ) z is selected from Each R 2 is independently 1-10 Alkyl, C 6-10 Aryl, C 7-10 Alkylaryl or poly(alkylene oxide) substituted C 1-6 Alkyl and / or R 1 is selected from the groups described for Each R 3 and R 4 is independently 1-10 Alkyl, C 6-10 Aryl, C 7-10 Alkylaryl or poly(alkylene oxide) substituted C 1-6 alkyl, Each R 5 is independently 1-6 a hydrolyzable group such as an alkoxy group, an acetoxy group, an enoxy group, or a ketoxy group, Each R 6 is independently 1-6 alkyl groups, z is 0 or an integer from 1 to 2; x is an integer of at least 2; The fouling release coating composition of any one of claims 1 to 6, wherein y is an integer of at least 2.

8. The fouling release coating composition of any one of claims 1 to 7, wherein component (b) is an aminosilane.

9. 9. The fouling release coating composition of any one of claims 1 to 8, wherein component (b) is an aminoalkyltrialkoxysilane or a bis(alkyltrialkoxysilyl)amine such as bis(3-propyltriethoxysilyl)amine or 3-aminopropyltriethoxysilane.

10. Component (b) has the formula: 【Chemistry 2】 (In the formula, R 1 , R 2 , R 3 , R 4 are each independently selected from hydrogen, a monovalent organic group, a monovalent heteroorganic group, and combinations thereof; And R 1 , R 2 , R 3 , R 4 The fouling release coating composition of any one of claims 1 to 9, wherein any two or more of the following are amidines:

11. 11. The fouling release coating composition of any one of claims 1 to 10, wherein component (b) is 1,8-diazabicyclo5.4.0-7-undecene (DBU).

12. 12. The fouling release coating composition of any one of claims 1 to 11, further comprising at least one metal catalyst which is a salt or organometallic compound of Zn, Li, K, Fe, Bi, Ce, or Zr.

13. Does not contain tin compounds (a) at least 40% by weight of a polysiloxane-based binder system comprising at least two different curable polysiloxane-based binders A and Binder B, where Binder A has a weight average molecular weight of 50,000 g / mol or less and Binder B has a weight average molecular weight of 55,000 g / mol or more, and Binder A constitutes at least 27% by weight of the total polysiloxane-based binder system; or A polysiloxane-based binder system comprising at least 40% by weight of at least two different curable polysiloxane-based binders A and Binder B, where Binder A has a viscosity of 2,800 mPas or less and Binder B has a viscosity of 3,500 mPas or more, and Binder A constitutes at least 27% by weight of the total polysiloxane-based binder system; or a polysiloxane-based binder system comprising at least 40% by weight of at least one curable polysiloxane-based binder having a weight average molecular weight of 50,000 g / mol or less, said binder constituting at least 60% by weight of the total polysiloxane-based binder system; or at least 40% by weight of a polysiloxane-based binder system, the polysiloxane-based binder system comprising at least one curable polysiloxane-based binder having a viscosity of 2,800 mPas or less, said binder constituting at least 60% by weight of the total polysiloxane-based binder system; (b) 0.1 to 5.0% by weight of at least one low molecular weight amidine or low molecular weight amine compound; (c) 0.0 to 5.0 wt. % of at least one metal catalyst which is a salt or organometallic compound of Zn, Li, K, Fe, Bi, or Zr; (d) 0 to 30% by weight of a hydrophilically modified polysiloxane; (e) 0 to 8.0 wt. % of a crosslinker; (dry weight) of a fouling release coating composition.

14. The method of claim 1, wherein: (i) at least one metal catalyst is present in an amount of 0.1 to 5.0 weight percent. (ii) the hydrophilically modified polysiloxane is present in an amount of 1.0 to 30 wt. %; (iii) the crosslinker is present in an amount of 2.0 to 8.0 wt. %; or a combination thereof.

15. 1. A method for applying and curing a fouling release coating composition to a substrate, such as a marine substrate, comprising the steps of: (a) a polysiloxane-based binder system comprising at least one curable polysiloxane-based binder A having a weight average molecular weight of 50,000 g / mol or less; (b) at least one low molecular weight amidine or low molecular weight amine compound; applying a fouling release coating composition comprising: a) a coating composition for coating a substrate; and curing said fouling release coating composition at a temperature of 10° C. or less.

16. The method of claim 15, wherein the curing is carried out at a temperature of 0 to 10°C.

17. A substrate comprising the cured fouling release coating composition of any one of claims 1 to 14.