Multilayer sound-damping interlayers containing ethylene vinyl acetal.

JP2023544296A5Active Publication Date: 2024-10-01KURARAY EURO GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023519266
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-09-28
Filing Date
2021-09-21
Publication Date
2024-10-01
Estimated Expiration
2041-09-21

AI Technical Summary

Technical Problem

Existing laminated safety glass interlayers, primarily using polyvinyl butyral (PVB), face challenges with insufficient mechanical stability, sound attenuation, and adhesion to glass, necessitating improved sound insulation and structural integrity.

Method used

A multilayer interlayer film comprising ethylene vinyl acetal membranes, with varying ethylene unit content and acetalization degrees, is used to enhance sound attenuation, mechanical stability, and thermal properties, incorporating thermoplastic elastomers and plasticizers for improved adhesion and processability.

Benefits of technology

The multilayer film achieves enhanced sound insulation, mechanical stability, and thermal stability, with improved adhesion to glass, while maintaining environmental sustainability and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a multilayer sound-damping interlayer comprising ethylene vinyl acetal.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a multilayer sound-damping interlayer comprising ethylene vinyl acetal. [Background technology]

[0002] Laminated safety glass (LSG) generally consists of two glass panels and an interlayer that bonds the glass panels. Partially acetalized polyvinyl alcohol containing plasticizers, especially polyvinyl butyral (PVB), is the primary interlayer material. LSG is used, for example, in the automotive industry as windshields and side windows, and in the architectural industry as safety glass.

[0003] An increasingly important feature of laminated glass is its sound-damping properties. This can be achieved, for example, by using particularly soft, sound-absorbing monolayer films. However, these films often have insufficient mechanical stability and do not exhibit sufficient adhesion to the glass.

[0004] Alternatively, a multi-layer system can be used in which the individual layers differ in terms of their mechanical strength, so that sound absorption is achieved by mechanical decoupling. Such a multi-layer system, including PVB, is described, for example, in US Patent Application Publication No. 2010 / 028642.

[0005] However, there remains a need in the industry for improved sound attenuating interlayers. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] US Patent Application Publication No. 2010 / 028642 Summary of the Invention [Problem to be solved by the invention]

[0007] Accordingly, it is an object of the present invention to provide an interlayer film having improved sound attenuation properties, improved mechanical stability, improved environmental footprint, improved thermal stability, improved water uptake profile, improved processability during film formation, or improved manufacturing or raw material costs.

[0008] These and other objects are surprisingly achieved by the present invention. [Means for solving the problem]

[0009] In a first aspect, the present invention relates to a sound-damping interlayer for laminated glazing comprising at least two individual films, at least one of the individual films comprising ethylene vinyl acetal. DETAILED DESCRIPTION OF THE INVENTION

[0010] Preferably, the sound-damping intermediate film contains ethylene vinyl acetal having an ethylene unit content in the range of 25 to 60 mol %, more preferably 30 to 55 mol %, and even more preferably 35 to 50 mol %.

[0011] The proportion of ethylene units in ethylene vinyl alcohol is preferably 25 to 60 mol %, more preferably 30 to 55 mol %, and even more preferably 35 to 50 mol %.

[0012] Preferably, the sound-damping intermediate film includes at least three individual films, with a first individual film (A) and a third individual film (C) constituting outer layers and a second individual film (B) constituting an inner layer.

[0013] Also preferably, the first individual membrane (A) and the third individual membrane (C) contain ethylene vinyl acetal, and more preferably, the first individual membrane (A), the second individual membrane (B) and the third individual membrane (C) contain ethylene vinyl acetal.

[0014] Thus, this embodiment of the invention relates to a multilayer film that, when used as an interlayer for laminated safety glass, includes two outer layers facing the glass and at least one inner layer comprising ethylene vinyl acetal. The inner layer is typically selected to be softer than the two outer layers and is often referred to as a sound-damping layer. When the individual films all comprise ethylene vinyl acetal, the ethylene vinyl acetal is typically of different grades, e.g., differing in the amount of ethylene units in the polymer chain, the degree of acetalization, and / or the degree of saponification.

[0015] Preferably, ethylene vinyl alcohol is obtained by copolymerizing ethylene with vinyl acetate and hydrolyzing the resulting copolymer. The hydrolysis reaction can be carried out using a conventionally known alkaline or acid catalyst, and among these, the hydrolysis reaction using methanol as a solvent and caustic soda (NaOH) as a catalyst is convenient.

[0016] The method for producing the ethylene vinyl acetal used in this embodiment of the present invention is not particularly limited, but it can be produced by a method in which an aldehyde is added to an ethylene vinyl alcohol solution under acidic conditions and subjected to an acetalization reaction.

[0017] The reaction product obtained after the acetalization reaction is neutralized with an alkali and then washed with water to obtain ethylene vinyl acetal.

[0018] The catalyst for the acetalization reaction is not particularly limited, and any organic or inorganic acid may be used, examples of which include acetic acid, paratoluenesulfonic acid, nitric acid, sulfuric acid, hydrochloric acid, and carbonic acid.

[0019] The degree of saponification of the acetate groups is not particularly limited, but is preferably 95 mol % or more, more preferably 98 mol % or more, even more preferably 99 mol % or more, and most preferably 99.9 mol % or more.

[0020] Preferably, the proportion of vinyl alcohol units in the ethylene vinyl acetal resin of the present invention is 20 to 71 mol % based on all monomer units constituting the resin.

[0021] The acetalization degree of the ethylene vinyl acetal used in the present invention is preferably 1 mol% to 80 mol%, and more preferably 5 mol% or more but less than 70 mol%, with the lower limit of the acetalization degree being more preferably more than 6 mol%, more than 7 mol%, more than 8 mol%, or more than 9 mol%, and most preferably more than 10 mol%. Furthermore, the upper limit of the acetalization degree is more preferably 38 mol% or less, then 36 mol% or less, then 34 mol% or less, and then 32 mol% or less, in that order, and most preferably less than 30 mol%. Another preferred acetalization degree is 30 to 50 mol%.

[0022] Preferably, the acetal groups each have from 1 to 7 carbon atoms, ie, they are derived from a condensation reaction with an aldehyde having from 1 to 7 carbon atoms. More preferably, they are methanal (formaldehyde), acetaldehyde, n-propanal (propionaldehyde), n-butanal (butyraldehyde), iso-butanal (2-methyl-1-propanal, iso-butyraldehyde), n-pentanal (valeraldehyde), iso-pentanal (3-methyl-1-butanal), sec-pentanal (2-methyl-1-butanal), tert-pentanal (2,2-dimethyl-1-propanal), n-hexanal (capronaldehyde), isohexanal (2-methyl-1-pentanal, 3-methyl-1-pentanal, 4-methyl-1-pentanal), 2,2-dimethyl-1-butanal, 2,3-dimethyl-1-butanal The list of methylbutanal, 3,3-dimethyl-1-butanal, 2-ethyl-1-butanal, n-heptanal, 2-methyl-1-hexanal, 3-methyl-1-hexanal, 4-methyl-1-hexanal, 5-methyl-1-hexanal, 2,2-dimethyl-1-pentanal, 3,3-dimethyl-1-pentanal, 4,4-dimethyl-1-pentanal, 2,3-dimethyl-1-pentanal, 2,4-dimethyl-1-pentanal, 3,4-dimethyl-1-pentanal, 2-ethyl-1-pentanal, 2-ethyl-2-methyl-1-butanal, 2-ethyl-3-methyl-1-butanal, 3-ethyl-2-methyl-1-butanal, cyclohexylaldehyde, and benzaldehyde. Most preferably, they are derived from a condensation reaction with iso-butyraldehyde or n-butyraldehyde.

[0023] Also preferably, the ethylene vinyl acetal is a mixed acetal, i.e., it contains at least two different acetal groups. In other words, the ethylene vinyl acetal used in the present invention contains a first acetal group resulting from the reaction of two hydroxyl groups of each ethylene vinyl alcohol with an aldehyde, and at least a second acetal group resulting from the reaction of the other two hydroxyl groups of each ethylene vinyl alcohol with a second aldehyde, the first aldehyde being different from the second aldehyde. Preferred aldehydes are the same as those used for the acetal having one acetal group described above.

[0024] Preferably, the ethylene vinyl acetal used in the process of the present invention has a glass transition temperature (Tg) of 30, 35, 40, 45, or 50° C. or higher. Also preferably, the Tg is 90, 75, 70, 65, 60, or 55° C. More preferably, the ethylene vinyl acetal used in the process of the present invention has a Tg of 30 to 90° C., most preferably 35 to 75° C., specifically 40 to 55° C.

[0025] The glass transition temperature was determined by differential scanning calorimetry (DSC) using a heating rate of 10 K / min in the temperature interval from -50 °C to 200 °C according to DIN 53765. A first heating ramp, followed by a cooling ramp, followed by a second heating ramp was used. The position of the glass transition temperature was determined on the measurement curve associated with the second heating ramp according to DIN 51007. The DIN midpoint (Tg DIN) was defined as the intersection of a horizontal line at half the step height with the measurement curve. The step height was defined by the vertical distance between the two intersections of the central tangent and the baseline of the measurement curve before and after the glass transition.

[0026] The melting point (melting temperature, Tm) is determined by differential scanning calorimetry (DSC) in accordance with DIN EN ISO 11357-3:2018.

[0027] The vinyl alcohol content and vinyl acetate content of ethylene vinyl acetal were determined according to DIN ISO 3681 (acetate content) and DIN ISO 53240 (PVA content). The vinyl acetal content can be calculated as the remainder from the sum of the vinyl alcohol content and vinyl acetate content determined according to DIN ISO 53401 / 53240 and the amount of ethylene required to make up 100. The degree of acetalization can be calculated by dividing the vinyl acetal content by the sum of the vinyl alcohol content, vinyl acetal content, and vinyl acetate content. Conversion from wt% to mol% can be performed using formulas known to those skilled in the art.

[0028] The ethylene content of ethylene vinyl acetal resin is measured by NMR spectroscopy. First, ethylene vinyl acetal resin is dissolved in ethanol, and 2N hydroxylamine hydrochloride solution and hydrochloric acid are added. The mixture is stirred under reflux in a water bath with a condenser for 4 hours. After cooling, aqueous ammonia is added. Methanol is then added to precipitate the polymer, which is then washed with water and dried to obtain ethylene vinyl alcohol copolymer. Next, this ethylene vinyl alcohol copolymer is dissolved in DMSO (dimethyl sulfoxide) at 120°C, cooled to room temperature, and then N,N-dimethyl-4-aminopyridine and acetic anhydride are added. The mixture is stirred for 1 hour, and then precipitated with ion-exchanged water and acetone and dried to obtain ethylene vinyl acetate copolymer. This polymer is then dissolved in DMSO-d6 and measured using a 400 MHz proton NMR spectrometer. The resulting spectrum is integrated 256 times. The molar ratio of ethylene units in ethylene-vinyl alcohol copolymer is calculated from the intensity ratio of methine protons (peaks at 1.1 to 1.9 ppm) derived from ethylene units and vinyl acetate units to the terminal methyl protons (peak at 2.0 ppm) derived from vinyl acetate units. Note that, because ethylene units are not affected by the acetalization reaction, the molar ratio (n) of ethylene units in ethylene-vinyl alcohol copolymer before the acetalization reaction is equal to the molar ratio (n) of ethylene units in the ethylene-vinyl acetal resin obtained after the acetalization reaction.

[0029] The interlayer film of the present invention may also contain other polymers different from the above-mentioned ethylene vinyl acetal. It may contain one or more other ethylene vinyl acetal grades differing in hydroxyl content, ethylene content, acetate content, and / or degree of polymerization and / or degree of acetalization and / or type of acetal. Alternatively, it may contain any polymer selected from the group consisting of polylactic acid (PLA), acrylonitrile-butadiene-styrene copolymer (ABS), polyamide (PA), polycarbonate (PC), polyethylene terephthalate (PET), polyethylene terephthalate copolymer (PETG), polyhydroxyalkanoate (PHA), wood-filled composites, metal-filled composites, carbon fiber-filled composites, thermoplastic elastomers (TPE), thermoplastic polyurethanes (TPU), polyolefins, polypropylene (PP), acrylonitrile styrene acrylate (ASA), polyacrylates, polymethacrylates, ionomers, polyvinyl acetals such as polybutyral, and mixtures thereof.

[0030] Preferably, the first individual film (A) and the third individual film (C) comprise ethylene vinyl acetal, and the second individual film (B) comprises a thermoplastic elastomer.

[0031] Thermoplastic elastomers generally include materials having soft and hard segments, such as polystyrene-based elastomers (soft segment: polybutadiene, polyisoprene / hard segment: polystyrene), polyolefin-based elastomers (soft segment: ethylene propylene rubber / hard segment: polypropylene), polyvinyl chloride-based elastomers (soft segment: polyvinyl chloride / hard segment: polyvinyl chloride), polyurethane-based elastomers (soft segment: polyether, polyester, or polycarbonate / hard segment: polyurethane), and polyester-based elastomers (soft segment: aliphatic polyester / hard segment: aromatic polyester). ), polyether ester elastomers (soft segment: polyether / hard segment: polyester), polyamide elastomers (soft segment: polypropylene glycol, polytetramethylene ether glycol, polyester, or polyether / hard segment: polyamide (e.g., nylon resin), polybutadiene elastomers (soft segment: amorphous butyl rubber / hard segment: syndiotactic 1,2-polybutadiene resin), acrylic elastomers (soft segment: polyacrylate ester / hard segment: polymethyl methacrylate), etc. The above thermoplastic elastomers may be used alone or in combination of two or more thereof.

[0032] The hard segment content in the thermoplastic elastomer is preferably about 5% by mass or more, or about 7% by mass or more, or about 8% by mass or more, or about 10% by mass or more, or about 14% by mass or more, or about 16% by mass or more, or about 18% by mass or more, based on the total amount of the thermoplastic elastomer. The hard segment content is preferably about 40% by mass or less, or about 30% by mass or less, or about 20% by mass or less, based on the total amount of the thermoplastic elastomer. If the hard segment content is less than about 5% by mass, molding of Layer B becomes difficult, the tan d peak height decreases, the bending rigidity of the laminate decreases, or sound insulation properties in the high frequency range tend to decrease. If the hard segment content exceeds about 40% by mass, the properties of the thermoplastic elastomer tend to be difficult to exhibit, the stability of sound insulation performance decreases, or sound insulation properties around room temperature tend to decrease.

[0033] The soft segment content in the thermoplastic elastomer is preferably about 60% by mass or more, about 70% by mass or more, or about 80% by mass or more, based on the total amount of thermoplastic elastomer. The soft segment content is preferably about 95% by mass or less, about 92% by mass or less, about 90% by mass or less, about 88% by mass or less, about 86% by mass or less, about 84% by mass or less, or about 82% by mass or less, based on the total amount of thermoplastic elastomer. If the soft segment content is less than about 60% by mass, the properties of the thermoplastic elastomer tend to be less fully exhibited. If the soft segment content is more than about 95% by mass, molding of Layer B becomes difficult, the tan d peak height decreases, the bending rigidity of the laminate decreases, or sound insulation in the high-frequency range decreases. Here, when multiple thermoplastic elastomers are blended, the hard segment and soft segment contents in the thermoplastic elastomer are considered to be the average values ​​of the blend.

[0034] From the viewpoint of achieving both moldability and sound insulation, it is more preferable to use a block copolymer having a hard segment and a soft segment as the thermoplastic elastomer. Furthermore, from the viewpoint of further improving sound insulation, it is preferable to use a polystyrene-based elastomer.

[0035] Furthermore, as the thermoplastic elastomer, crosslinked rubbers such as natural rubber, isoprene rubber, butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, ethylene propylene rubber, urethane rubber, silicone rubber, chlorosulfonated polyethylene rubber, acrylic rubber, and fluororubber may be used.

[0036] The thermoplastic elastomer is preferably a copolymer of an aromatic vinyl monomer and a vinyl monomer or a conjugated diene monomer, or a hydrogenated product of such a copolymer. From the viewpoint of achieving both the function of a rubber exhibiting sound insulation properties and the function of a plastic, the copolymer is preferably a block copolymer having an aromatic vinyl polymer block and an aliphatic unsaturated hydrocarbon polymer block, for example, a polystyrene-based elastomer.

[0037] When a block copolymer having an aromatic vinyl polymer block and a vinyl polymer block or a conjugated diene polymer block, for example, an aromatic vinyl polymer block and an aliphatic unsaturated hydrocarbon polymer block, is used as the thermoplastic elastomer, the bonding type of these polymer blocks is not particularly limited and may be any of a linear bonding type, a branched bonding type, a radial bonding type, or a bonding type in which two or more of these are combined. Among these, a linear bonding type is preferred.

[0038] When the aromatic vinyl polymer block is represented by "a" and the aliphatic unsaturated hydrocarbon polymer block is represented by "b", examples of the linear bond type include a diblock copolymer represented by ab, a triblock copolymer represented by aba or bab, a tetrablock copolymer represented by abab, a pentablock copolymer represented by ababa or babab, an (ab)nX type copolymer (X represents a coupling residue, and n represents an integer of 2 or more), and mixtures thereof. Among them, a diblock copolymer or a triblock copolymer is preferred, and a triblock copolymer represented by aba is more preferred.

[0039] Examples of the aliphatic unsaturated hydrocarbon monomer constituting the aliphatic unsaturated hydrocarbon polymer block include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 4-phenyl-1-butene, 6-phenyl-1-hexene, 3-methyl-1-butene, 4-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3-methyl-1-hexene, 4-methyl-1-hexene, 5-methyl-1-hexene, 5-methyl-1-butene, 5-methyl-1-pentene, 5-methyl-1-hex ... Examples of the aliphatic unsaturated hydrocarbon monomer include methyl-1-hexene, 3,3-dimethyl-1-pentene, 3,4-dimethyl-1-pentene, 4,4-dimethyl-1-pentene, vinylcyclohexane, hexafluoropropene, tetrafluoroethylene, 2-fluoropropene, fluoroethylene, 1,1-difluoroethylene, 3-fluoropropene, trifluoroethylene, 3,4-dichloro-1-butene, butadiene, isoprene, dicyclopentadiene, norbornane, and acetylene. These aliphatic unsaturated hydrocarbon monomers may be used alone or in combination of two or more thereof.

[0040] The method for producing the block copolymer is not particularly limited, but it can be produced by, for example, anionic polymerization, cationic polymerization, radical polymerization, etc. For example, in the case of anionic polymerization, specific examples include the following. (i) A method of sequentially polymerizing an aromatic vinyl monomer, a conjugated diene monomer, and then an aromatic vinyl monomer using an alkyllithium compound as an initiator. (ii) A method in which an aromatic vinyl monomer and a conjugated diene monomer are polymerized successively using an alkyllithium compound as an initiator, and then a coupling agent is added to carry out coupling. (iii) A method of sequentially polymerizing a conjugated diene monomer and then an aromatic vinyl monomer using a dilithium compound as an initiator.

[0041] Specific examples of suitable thermoplastic elastomers can be found, for example, by reference to US Patent Application Publication No. 2010 / 239802.

[0042] In one preferred embodiment, the thermoplastic elastomer comprises at least (A) a polymer block mainly composed of aromatic vinyl compound units, and (B) a polymer block composed primarily of 1,3-butadiene units, or composed primarily of isoprene and 1,3-butadiene units; wherein the content of polymer block (A) is about 5% to about 40% by mass based on the total amount of the hydrogenated block copolymer, the hydrogenation rate of polymer block (B) is about 70% or more, and the glass transition temperature of the hydrogenated block copolymer is about -45°C to about 30°C.

[0043] In another preferred embodiment, the thermoplastic elastomer is a hydrogenated block copolymer formed by hydrogenating a block copolymer including at least a polymer block (C) mainly composed of aromatic vinyl compound units and a polymer block (D) mainly composed of 1,3-butadiene units or mainly composed of isoprene units and 1,3-butadiene units, wherein the content of the polymer block (C) is about 10% by mass to about 40% by mass based on the total amount of the hydrogenated block copolymer, the hydrogenation rate of the polymer block (D) is about 80% or more, and the glass transition temperature of the hydrogenated block copolymer is less than about −45° C.

[0044] In the above two preferred embodiments, it is desirable that the aromatic vinyl compound is styrene, and / or that the polymer blocks (B) and (D) are mainly composed of isoprene units and 1,3-butadiene units, and / or that the hydrogenated block copolymer is a triblock copolymer having an A1-B-A2 or C1-D-C2 type structure.

[0045] In another embodiment of the present invention, the first individual membrane (A) and the third individual membrane (C) comprise ethylene vinyl acetal, and the second individual membrane (B) comprises polyvinyl acetal.

[0046] Preferably, the individual membranes (B) are based on polyvinyl butyral (PVB), obtained by acetalizing polyvinyl alcohol with butyraldehyde, although other aldehydes such as those mentioned above can also be used to advantage.

[0047] Preferably, the individual membrane (B) contains polyvinyl acetal having a polyvinyl acetate group content of 5 to 8 mol %.

[0048] Preferably, the individual membranes (B) comprise polyvinyl acetal with a proportion of polyvinyl alcohol groups of less than 18 wt%, more preferably less than 14 wt%, most preferably 11 to 13.5 wt%, specifically 11.5 to 13 wt%.

[0049] Specific examples of suitable polyvinyl acetals can be found, for example, by reference to US Patent Application Publication No. 2010 / 028642.

[0050] In another preferred embodiment, the second individual membrane (B) comprises ethylene vinyl acetal, which is thus the softer core material complemented by two harder outer membranes.

[0051] Preferably, the first individual membrane (A) and the third individual membrane (C) comprise polyvinyl acetal.

[0052] Suitably, the polyvinyl acetal has a polyacetate group content of 0.1 to 11 mol %, preferably 0.1 to 4 mol %, and more preferably 0.1 to 2 mol %.

[0053] Preferably, the polyvinyl acetal has a polyvinyl alcohol group content of 17 to 22% by weight, preferably 18 to 21% by weight, more preferably 19.0 to 20.5% by weight.

[0054] Specific examples of suitable polyvinyl acetals can be found, for example, by reference to US Patent Application Publication No. 2010 / 028642.

[0055] In another preferred embodiment of the present invention, the first individual membrane (A) and the third individual membrane (C) comprise an ionomer.

[0056] Ionomer resins are partially neutralized ethylene a,b-unsaturated carboxylic acid copolymers, including resins having structural units derived from ethylene, structural units derived from an a,b-unsaturated carboxylic acid, and optionally other structural units as described below, in which at least a portion of the structural units derived from an a,b-unsaturated carboxylic acid are neutralized with ions.

[0057] In the ethylene-a,b-unsaturated carboxylic acid copolymer serving as the base polymer, the content of structural units derived from a,b-unsaturated carboxylic acid (based on the mass of the entire copolymer) is typically 2% by mass or more, or 5% by mass or more, and the content of structural units derived from a,b-unsaturated carboxylic acid (based on the mass of the entire copolymer) is typically 30% by mass or less.

[0058] Examples of the a,b-unsaturated carboxylic acid that constitutes the ionomer include, but are not limited to, acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and mixtures of two or more thereof. In one embodiment, the a-ethylenically unsaturated carboxylic acid is selected from acrylic acid, methacrylic acid, and mixtures thereof. In another embodiment, the a,B-ethylenically unsaturated carboxylic acid is methacrylic acid.

[0059] The ethylene-acid copolymer may further contain copolymerized units of one or more additional comonomers, such as a,b-ethylenically unsaturated carboxylic acid esters. When present, alkyl esters having 3 to 10 or 3 to 8 carbon atoms are typically used. Specific examples of suitable esters of unsaturated carboxylic acids include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, octyl acrylate, octyl methacrylate, undecyl acrylate, undecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, and dodecyl acrylate. Examples of the additional comonomer include, but are not limited to, methyl acrylate, dodecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, isobornyl acrylate, isobornyl methacrylate, lauryl acrylate, lauryl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethyl maleate, diethyl maleate, dibutyl maleate, dimethyl fumarate, diethyl fumarate, dibutyl fumarate, dimethyl fumarate, vinyl acetate, vinyl propionate, and mixtures of two or more thereof. In one embodiment, the additional comonomer is selected from methyl acrylate, methyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, glycidyl methacrylate, vinyl acetate, and mixtures of two or more thereof. In another embodiment, the additional comonomer is one or more of n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, and isobutyl methacrylate. In another embodiment, the additional comonomer is one or both of n-butyl acrylate and isobutyl acrylate.

[0060] Suitable ethylene acid copolymers have a melt flow rate (MFR) determined according to ASTM method D1238-89 at 190°C and 2.16 kg of from about 1, or from about 2, to about 4000 g / 10 min, or to 1000 g / 10 min, or to about 400 g / 10 min.

[0061] Finally, suitable ethylene acid copolymers can be synthesized as described, for example, in U.S. Pat. Nos. 3,404,134, 5,028,674, 6,500,888, 6,518,365, 8,334,033, and 8,399,096.

[0062] To obtain an ionomer, the ethylene acid copolymer is partially neutralized by reaction with one or more bases. Examples of suitable procedures for neutralizing ethylene acid copolymers are described in U.S. Pat. Nos. 3,404,134 and 6,518,365. After neutralization, from about 1%, or from about 10%, or from about 15%, or from about 20% to about 90%, or from about 60%, or from about 55%, or from about 30% of the hydrogen atoms of the carboxylic acid groups present in the ethylene acid copolymer are replaced with other cations. In other words, from about 1%, or from about 10%, or from about 15%, or from about 20% to about 90%, or from about 60%, or from about 55%, or from about 30% of the total content of carboxylic acid groups present in the ethylene acid copolymer are neutralized. Alternatively expressed, the neutralization level is from about 1%, or from about 10%, or from about 15%, or from about 20% to about 90%, or to about 60%, or to about 55%, or to about 30%, based on the total content of carboxylic acid groups present in the ethylene acid copolymer as calculated or measured on the unneutralized ethylene acid copolymer. The neutralization level can be adjusted for the particular end use.

[0063] Ionomers contain cations as counterions to the carboxylate anions. Suitable cations include any positively charged species that are stable under the conditions under which the ionomer composition is synthesized, processed, and used. Suitable cations can be used in combination of two or more. In some preferred ionomers, the cations are metal cations, which can be monovalent, divalent, bivalent, or polyvalent. Useful monovalent metal cations include, but are not limited to, cations of sodium, potassium, lithium, silver, mercury, copper, etc. Useful divalent metal cations include, but are not limited to, cations of beryllium, magnesium, calcium, strontium, barium, copper, cadmium, mercury, tin, lead, iron, cobalt, nickel, zinc, etc. Useful trivalent metal cations include, but are not limited to, cations of aluminum, scandium, iron, yttrium, etc. Useful polyvalent metal cations include, but are not limited to, cations of titanium, zirconium, hafnium, vanadium, tantalum, tungsten, chromium, cerium, iron, etc. When the metal cation is polyvalent, a complexing agent such as stearate, oleate, salicylate, or phenolate radical can be included, as described in U.S. Pat. No. 3,404,134. In another preferred composition, the metal cation used is a monovalent or divalent metal cation. Preferred metal cations are sodium, lithium, magnesium, zinc, potassium, and combinations of one or more of these metal cations. In a more preferred composition, the cation is sodium cation, magnesium cation, zinc cation, or combinations thereof.

[0064] In one embodiment, the counterions to the carboxylate anions in the ionomer are sodium cations, and counterions other than sodium cations may optionally be present in small amounts of less than 5 equivalent percent, less than 3 equivalent percent, less than 2 equivalent percent, or less than 1 equivalent percent, based on the total equivalents of carboxylate groups in the ionomer. In one embodiment, the counterions are substantially sodium ions.

[0065] Preferably, at least one of the individual membranes (A), (B) or (C) is wedge-shaped, and more preferably, the individual membranes (A), (B) and (C) are all wedge-shaped.

[0066] The present invention therefore relates to a combination of wedge-shaped and non-wedge-shaped individual membranes or to a partially or completely wedge-shaped interlayer that is entirely based on wedge-shaped individual membranes. Wedge-shaped interlayers are commonly used in automobiles equipped with head-up displays to prevent double images.

[0067] Preferably, at least one of the individual films (A), (B) and (C) contains a plasticizer in an amount of 10 to 50% by weight. Thus, the individual film contains, in addition to the polymeric material, up to 50% by weight (based on the total weight of the composition) of one or more plasticizers. Any compound known to plasticize the corresponding polymer can be used. Preferred plasticizers are diesters of aliphatic diols, in particular aliphatic polyether diols and / or polyether polyols, with aliphatic carboxylic acids, preferably diesters of polyalkylene oxides, in particular diethylene glycol, triethylene glycol and tetraethylene glycol with aliphatic (C6-C10) carboxylic acids, preferably 2-ethylbutyric acid and n-heptanoic acid, and also diesters of aliphatic or aromatic (C2-C18) dicarboxylic acids, preferably adipic acid, sebacic acid, phthalic acid with aliphatic (C4-C12) alcohols, preferably dihexyl adipate, phthalate, trimellitate, phosphate, fatty acid esters, in particular triethylene glycol-bis-(2-ethylbutyrate), triethylene glycol ethylhexanoate (3G8), aromatic carboxylic acid esters, in particular dibenzoates and / or hydroxycarboxylic acid esters. Particularly preferred plasticizers are ISOFOL 12+5 EO, a 2-butyloctanol with an average ethoxylation degree of 5, dihexyl adipate (DHA), 1,2-cyclohexanedicarboxylic acid diisononyl ester (DINCH), dipropylene glycol dibenzoate (DPGDB), diethylene glycol dibenzoate (MONOCIZER PB-3A), MONOCIZER PB-10, and mixtures thereof. Mixtures of plasticizers with different and identical compositions as well as single plasticizers may be used. The term "different compositions" refers to both the type and proportion of plasticizers in the mixture. In the starting state before lamination, the plasticizer may be present in an amount of at least 22% by weight, e.g., 22.0 to 45.0% by weight, preferably 25.0 to 32.0% by weight, and particularly 26.0 to 30.0% by weight.

[0068] Optionally, the interlayer film of the present invention may also contain other ingredients in addition to the ethylene vinyl acetal described above, such as antioxidants, optical brighteners, stabilizers, processing aids, organic or inorganic nanoparticles, pyrogenic silicic acid, silica, surfactants, and / or rheology modifiers.

[0069] The damping properties were determined according to ISO 16940 for test specimens consisting of a 0.8 mm thick interlayer laminated between 2 mm thick glass panels. In each case, the first mode was determined and the corresponding loss factor of the first mode was determined.

[0070] The sound absorption effect of the inventive film should be highest at the application temperature of the future glazing laminate. For automotive glazing, the application temperature is around 20°C, as the window is heated in winter and cooled in summer by the air conditioning unit. In the test setup described above, the inventive film preferably exhibits maximum attenuation in the temperature range of 15-25°C. Preferably, the loss factor value is greater than 0.1, more preferably greater than 0.15, and most preferably greater than 0.2.

[0071] The method for producing the interlayer film is not particularly limited. Specifically, the starting resin composition can be molded into a film by extrusion molding, blow molding, injection molding, solution casting, or the like, preferably by extrusion molding. The resin temperature during extrusion is preferably 170 to 250°C, more preferably 180 to 240°C, and even more preferably 190 to 230°C. If the resin temperature is too high, the ethylene vinyl acetal resin will undergo partial decomposition.

[0072] The individual membranes used in accordance with the present invention can each be of almost any thickness, so long as the sound-insulating properties are not adversely affected. The individual membranes can all have, for example, the same thickness, although combinations of individual membranes of different thicknesses are also possible. In one preferred arrangement of the intermediate membranes of the present invention as a three-layer membrane A / B / C, the outer membranes A and C have approximately the same thickness, while the sound-absorbing membrane B can be as thin as possible. If the total thickness of the multilayer membrane is 0.8 mm, the sound-absorbing membrane may be 0.05 to 0.35 mm thick. The multilayer membranes of the present invention preferably have a total thickness customary in the industry, such as 0.38, 0.76, or 1.14 mm (i.e., multiples of 0.38 mm).

[0073] The interlayer film of the present invention has a certain roughness on at least one surface to prevent adhesion between interlayer films, for example, when the film is wound around a roll, and to improve degassing properties during the lamination process. This roughness can be achieved using conventional methods. Examples include methods for providing a melt fracture structure by adjusting extrusion conditions or by embossing the surface. Conventional embossing depths and shapes can be used.

[0074] A further aspect of the present invention relates to the use of the interlayer film of the present invention as an adhesive film for laminated glass.

[0075] The laminated glass can be produced by inserting and laminating the interlayer film of the present invention, as well as at least one film containing polyvinyl acetal, between two or more glass plates made of inorganic or organic glass. There are no particular restrictions on the glass to be laminated onto the interlayer film for laminated glass of the present invention, but in addition to inorganic glass such as float glass, tempered glass, wired glass, or heat-absorbing glass plates, conventionally known organic glass such as polymethyl methacrylate or polycarbonate can be used. There are no particular restrictions on the thickness of the glass, but it is preferably 1 to 10 mm, more preferably 2 to 6 mm.

[0076] Lamination methods for obtaining the above-mentioned laminated glass are known in the art, and examples thereof include a method using a vacuum laminator, a method using a vacuum bag, a method using a vacuum ring, and a method using a nip roll. Furthermore, a method of subjecting the glass to an autoclave process after temporary bonding can also be additionally performed. [Example]

[0077] For the purposes of the present invention, various glass / glass laminates are produced which contain the inventive film as an interlayer in the form of three combined individual films, with films A and C in direct contact with the glass surface and film B disposed between films A and C. Tables 1 and 2 show the compositions of each film.

[0078] [Table 1]

[0079] [Table 2]

[0080] [Preparation of the interlayer film of the present invention] The interlayers of the present invention are produced by film extrusion techniques known to those skilled in the art. To achieve a multilayer structure, individual layers A and C are extruded using twin-screw extruder 1, and individual layer B is extruded using twin-screw extruder 2. Depending on the example (see table above), the following amounts of di-(2-butoxyethyl)-adipic acid (DBEA) are fed to the extruders:

[0081] A feedblock, positioned before the melts from Extruder 1 and Extruder 2 enter a 34 cm wide extrusion die, combines the layers to form a three-layer membrane in which Layers A and C are of the same composition and Layer B is in contact with both Layers A and C. The melt comprising the three-layer structure is extruded onto a chilled chill roll and relaxed to form the final interlayer, which is wound onto an additional unchilled roll. Results for individual examples are shown in Table 2.

[0082] The formulation of Example 1.1 includes 15 wt. % of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 2 based on resin weight and 10 wt. % of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 1 based on resin weight.

[0083] The formulation of Example 1.2 includes 20 wt. % of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 2 based on the amount of resin, and 10 wt. % of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 1 based on the amount of resin.

[0084] The formulation for Example 2.1 includes 27.5 wt % based on resin of 3G8 added to Extruder 1 and 15 wt % based on resin of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 2.

[0085] The formulation for Example 2.2 includes 27.5 wt % based on resin of 3G8 added to Extruder 1 and 20 wt % based on resin of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 2.

[0086] The formulation for Example 3.1 includes 37.5 wt % 3G8 added to Extruder 2 based on the amount of resin.

[0087] The formulation for Example 3.2 includes 37.5 wt % based on resin of 3G8 added to Extruder 2 and 10 wt % based on resin of di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 1.

[0088] The formulation of Example 5.1 includes 10 wt % di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 2 based on the amount of resin.

[0089] The formulation of Example 5.2 includes 15 wt % di-(2-butoxyethyl)-adipate (DBEA) added to Extruder 2 based on the amount of resin.

[0090] [Materials used according to the present invention] <Ethylene vinyl acetal (ACEV1) of layer A and layer C> 100 parts by weight of an ethylene vinyl alcohol copolymer (saponification degree: 99) containing 44 mol% of ethylene units synthesized according to the production method described in Japanese Patent Application Laid-Open No. 2016-28139 is dispersed in 315 parts by weight of 1-propanol, and the solution temperature is raised to 60 °C while stirring. Then, 40 parts by weight of 1M hydrochloric acid is added, and then 16.7 parts by weight of n-butyl aldehyde is added while maintaining the temperature at 60 °C. As the reaction proceeds, the ethylene vinyl alcohol copolymer dissolves and the reaction mixture becomes a homogeneous solution. After 36 hours, 6.4 parts by weight of sodium hydrogen carbonate is added to stop the reaction. After adding 500 parts by weight of 1-propanol to the reaction solution to make it uniform, it is added dropwise to 2000 parts by weight of water to precipitate the resin. Then, the operations of filtration and washing with water are repeated 3 times, and the obtained solid is vacuum dried at 60 °C for 8 hours. The ethylene vinyl acetal thus obtained has an ethylene unit content of 44 mol% and an acetalization degree of 31 mol%.

[0091] <Ethylene vinyl acetal (ACEV2) of layer B> 100 parts by weight of an ethylene vinyl alcohol copolymer (saponification degree: 99) containing 48 mol% of ethylene units synthesized according to the production method described in Japanese Patent Application Laid-Open No. 2016-28139 is dispersed in 315 parts by weight of 1-propanol, and the solution temperature is raised to 60 °C while stirring. Then, 40 parts by weight of 1M hydrochloric acid is added, and further 34.2 parts by weight of n-butyl aldehyde is added while maintaining the temperature at 60 °C. As the reaction proceeds, the ethylene vinyl alcohol copolymer dissolves and the reaction mixture becomes a homogeneous solution. After 36 hours, 6.4 parts by weight of sodium hydrogen carbonate is added to stop the reaction. After adding 500 parts by weight of 1-propanol to the reaction solution to make it uniform, it is added dropwise to 2000 parts by weight of water to precipitate the resin. Then, the operations of filtration and washing with water are repeated 3 times, and the obtained solid is vacuum dried at 60 °C for 8 hours.

[0092] <Polyvinyl butyral layer A (PVB1)> 100 parts by weight of polyvinyl alcohol, Kuraray Poval® 28-99 (commercially available from Kuraray Europe GmbH), was dissolved in 1075 parts by weight of water while heating to 90°C. At 40°C, 57.9 parts by weight of n-butyl aldehyde was added, and 100 parts by weight of 20% hydrochloric acid was added while stirring at 12°C. After polyvinyl butyral (PVB) precipitated, the mixture was heated to 71°C and stirred at this temperature for 2 hours. After cooling to room temperature, the PVB was separated, washed with water until neutral, and dried. PVB with a polyvinyl alcohol content of 19.0% by weight (27.5 mol%) and a polyvinyl acetate content of 1.3% by weight (1 mol%) was obtained.

[0093] <Polyvinyl butyral layer B (PVB2)> Using 100 parts by weight of polyvinyl alcohol with a degree of hydrolysis of 92.5 mol%, Kuraray Poval® 50-92 (a product available from Kuraray Europe GmbH), and 68 parts by weight of n-butyl aldehyde, a PVB with a polyvinyl alcohol content of 12.0 wt% (18.3 mol%) and a polyvinyl acetate content of 9.6 wt% (7.5 mol%) was obtained.

[0094] <tpe1> This hydrogenated polystyrene-polyisoprene-polystyrene triblock copolymer thermoplastic elastomer contains 75% 1,2-bonds and 3,4-bonds. It has a hard block / soft block ratio [Mw(Al) / Mw(A2)] of 1.00, a glass transition temperature of -15°C, a styrene content of 21% by mass, a hydrogenation rate of 84%, and a weight-average molecular weight of 120,000. It is commercially available from Kuraray Co., Ltd. (Tokyo, Japan) as "Hybler™ H7125."

[0095] <Ionomer> The ionomer used in the midlayer is available from Kuraray America, Inc. (Wilmington, DE, USA) under the trademark "SENTRY GLAS® XTRA™." This material is made from CI2, as described in U.S. Patent Application Publication No. 20190030863.

[0096] [Laminate fabrication] Clear glass (Planilux® 2.1 mm, washed with deionized water <5 μS in a flat glass washer) is combined with an interlayer having layers A and B always facing the glass to give a test stack measuring 30×30 cm.

[0097] The various sandwiches are passed through a commercial glass lamination nipper line to produce pre-laminates. Lamination is carried out in an autoclave under standard conditions (140°C, 12 bar for 90 minutes with a 30 minute hold time).

[0098] [measurement] To quantify the coupling and damping properties of our novel interlayers, impedance tests according to ISO 16940 (as of December 2008) are used on 25 x 300 mm laminated beams cut from the laminate. Here, the loss factor (LF) is directly related to damping, while the resonant frequency (f) relates to coupling via bending stiffness, which can be calculated from the resonant frequency. Because plasticizers redistribute between the different layers of the multilayer film after a "thermal shock," such as a typical autoclave process for safety glass laminates, evaluation of the impedance properties is performed at exactly 20°C after six weeks of equilibration of the laminate.

Claims

1. 1. An interlayer film for laminated glass comprising at least two individual films, the first individual film (A) comprising ethylene vinyl acetal.

2. 2. The interlayer film of claim 1, wherein the ethylene vinyl acetal contains ethylene units in the range of 25 to 60 mol %.

3. 3. The intermediate membrane according to claim 1 or 2, comprising at least three individual membranes, a first individual membrane (A) and a third individual membrane (C) constituting outer layers and a second individual membrane (B) constituting an inner layer.

4. 4. The interlayer of claim 3, wherein the first individual membrane (A) and the third individual membrane (C) comprise ethylene vinyl acetal.

5. 5. The interlayer of claim 4, wherein the first individual film (A), the second individual film (B) and the third individual film (C) comprise ethylene vinyl acetal.

6. 4. The interlayer of claim 3, wherein the first individual membrane (A) and the third individual membrane (C) comprise ethylene vinyl acetal and the second individual membrane (B) comprises a thermoplastic elastomer.

7. 4. The interlayer of claim 3, wherein the first individual film (A) and the third individual film (C) comprise ethylene vinyl acetal and the second individual film (B) comprises polyvinyl acetal.

8. 4. The interlayer of claim 3, wherein the second individual membrane (B) comprises ethylene vinyl acetal.

9. 9. The interlayer of claim 8, wherein the first discrete membrane (A) and the third discrete membrane (C) comprise polyvinyl acetal.

10. 4. The interlayer of claim 3, wherein the first individual membrane (A) and the third individual membrane (C) comprise an ionomer.

11. 11. The interlayer according to any one of claims 1 to 10, wherein at least one of the individual membranes (A), (B) or (C) is wedge-shaped.

12. 12. The interlayer of claim 11, wherein the individual membranes (A), (B) and (C) are wedge-shaped.

13. 13. The interlayer according to any one of claims 1 to 12, wherein at least one of the individual membranes (A), (B) and (C) comprises a plasticizer in an amount of 10 to 50 wt.%.

14. The interlayer film according to any one of claims 1 to 13, having a loss factor value, measured according to ISO 16940 (as of December 2008), of greater than 0.

1.

15. A laminated glass comprising two glass sheets combined with the interlayer film according to any one of claims 1 to 14.