Bone implant with porous membrane and method for manufacturing same

JP2023544553A5Pending Publication Date: 2024-10-01BEIJING HUAYU CHUANGXIN SCI & TRADE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023519352
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-09-25
Filing Date
2021-09-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing orthopedic implant materials, particularly those made from tantalum, face issues with aesthetic appearance due to dark color and inadequate biomechanical compatibility, leading to stress shielding and poor integration with human bone, especially in dental and cranial implants.

Method used

The development of bone implants using tantalum, niobium, or titanium-based materials coated with porous membranes such as lithium tantalate, lithium niobate, or titanium oxide, which provide controlled elastic modulus, improved biocompatibility, and aesthetic appearance by mimicking bone color.

Benefits of technology

The proposed implants offer enhanced biomechanical compatibility, improved stress distribution, and aesthetic appeal by matching the color of human bone, while maintaining excellent corrosion resistance and antibacterial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a bone implant having a porous lithium tantalate membrane and a method for manufacturing the bone implant. The bone implant includes (1) a substrate and (2) a porous membrane located on the substrate, where the substrate is selected from a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, and a titanium substrate, and the porous membrane is selected from a porous lithium tantalate membrane, a porous lithium niobate membrane, a porous lithium tantalate-lithium niobate composite membrane, and a porous titanium oxide membrane. The bone implant of the present invention has one or more of the following advantageous effects: (1) the bone implant has excellent corrosion resistance; (2) the elastic modulus of the bone implant can be controlled by process conditions, thereby achieving higher biocompatibility with the elastic modulus of human or animal bones (e.g., alveolar bone and skull); (3) the white color of the bone implant is close to the color of bone itself, providing an aesthetic appearance; and (4) the bone implant has excellent antibacterial properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a bone implant (implant) having a porous membrane and a method for producing said bone implant. [Background technology]

[0002] Metallic materials have excellent overall mechanical properties and fatigue resistance, making them particularly suitable as orthopedic implant materials. With the ever-changing development of materials science, orthopedic implant materials have undergone a process of development, with relatively good results achieved, including stainless steel, cobalt-chromium alloys, and titanium alloys. However, the complex environment within the human body can cause corrosion of materials, leading to the release of toxic elements and a decrease in the biocompatibility of certain metallic materials. Furthermore, prior art materials, such as stainless steel, cobalt-chromium alloys, and titanium alloys, are dark in color, even black, which affects the aesthetic performance of the materials and limits their range of application. These drawbacks have a certain negative impact on the application of metallic materials as biomedical materials. Summary of the Invention [Problem to be solved by the invention]

[0003] Porous tantalum has emerged in recent years as a relatively ideal orthopedic implant material. It is a refractory metal with a melting point of nearly 3000°C, a dark gray appearance, and a smooth surface. Compared to existing medical metal materials, tantalum has two main advantages: (1) it has better corrosion resistance; (2) tantalum has better biocompatibility, and porous tantalum has a relatively low elastic modulus. However, tantalum's dark gray color can affect the aesthetic appearance, especially when used in dental implants.

[0004] Porous tantalum is a relatively ideal orthopedic implant material, but the elastic modulus of orthopedic materials made of tantalum described in the literature is between that of cortical bone and cancellous bone. However, the elastic modulus of porous tantalum is closer to that of cancellous bone in the human body, but significantly lower than that of cortical bone. Meanwhile, the bone tissue that bears the load in the human body is mainly cortical bone, and based on the effects of animal experiments and clinical applications, the elastic modulus of bone implants should be closer to that of human cortical bone; if it is too high, stress shielding will occur, and if it is too low, it will not be suitable for force transmission. The present invention can provide elastic moduli ranging from low to high depending on the selection of different film coating conditions.

[0005] However, from a biomechanical perspective, the elastic modulus of dental implants affects the stress distribution at the bone interface. Generally, the higher the elastic modulus of a dental implant, the smaller the internal stress in the bone near the neck, but the greater the internal stress in the bone near the root end. The lower the elastic modulus of a dental implant, the greater the relative displacement movement between the dental implant and the bone interface. When the elastic modulus of a dental implant is close to that of cortical bone and cancellous bone, biomechanical compatibility is relatively good. A higher elastic modulus is better, and some scholars suggest that an appropriate elastic modulus for a dental implant is 70 to 200 GPa, with some sources reporting that the elastic modulus of cortical bone is approximately 18 GPa.

[0006] However, for cranial (skull) implants, the elastic modulus requirements may be different.

[0007] Dental implants are made by creating a rod or cone out of titanium alloy or other materials, and then forming a thread on the outer surface, the purpose of which is to allow the human bone to grow into the thread and to unite the implant with the human bone, thereby enhancing the compatibility and strength of the implant with the human body. However, there is a limit to the depth of the thread, and if it is too deep, it may affect the strength of the implant.

[0008] Therefore, there is still a need to find bone implants, especially dental implants and cranial (skull) implants, that have a certain aesthetic appearance and / or higher biocompatibility. [Means for solving the problem]

[0009] (Contents of the invention) Therefore, the present invention provides (1) a substrate, and (2) a porous membrane located on the substrate; Including, the substrate is selected from a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, and a titanium substrate; and The porous film is selected from a porous lithium tantalate film, a porous lithium niobate film, a porous lithium tantalate-lithium niobate mixture film, and a porous titanium oxide film. A bone implant or composite is provided.

[0010] Furthermore, the present invention provides (1) a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, or a titanium substrate; and (2) A porous lithium tantalate film located on the tantalum substrate and containing tantalum oxide, a porous lithium niobate film located on the niobium substrate and containing niobium oxide, a porous lithium tantalate-lithium niobate mixture film located on the tantalum-niobium alloy substrate and containing tantalum oxide and niobium oxide, or a porous titanium oxide film located on the titanium substrate. The present invention provides a bone implant or composite comprising:

[0011] The present invention also provides (1) providing a substrate; and (2) forming a porous membrane on the substrate; Including, the substrate is selected from a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, and a titanium substrate; and The porous film is selected from a porous lithium tantalate film, a porous lithium niobate film, a porous lithium tantalate-lithium niobate mixture film, and a porous titanium oxide film. A method for producing the bone implant or composite is provided.

[0012] Furthermore, the present invention provides (1) providing a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, or a titanium substrate; and (2) forming a porous lithium tantalate film, a porous lithium niobate film, or a porous lithium tantalate-lithium niobate mixture film on a tantalum substrate, a niobium substrate, or a tantalum-niobium alloy substrate, or forming a porous titanium oxide film on a titanium substrate; Including, the lithium tantalate film contains tantalum oxide; The lithium niobate film contains niobium oxide, and The composite film contains tantalum oxide and niobium oxide. A method for producing the bone implant or composite is provided.

[0013] The present invention also relates to the use of said composite in medical materials, such as dental implants.

[0014] The bone implant of the present invention has one or more of the following advantageous effects: (1) The provided metal compound film is porous, which is advantageous for guiding the infiltration of human bone and enhancing the compatibility and strength of the implant. At the same time, the compound film layer resembles a ceramic body, has insulating and heat-insulating effects, and reduces the irritation caused by sudden heat to the human body. (2) The film layer is not produced by ion deposition in a solution, but is produced when the implant metal participates in an electrochemical reaction. It has a performance transition layer, and the film layer and the substrate are firmly bonded, resulting in excellent corrosion resistance. (3) The elastic modulus of the bone implant can be controlled by process conditions, thereby achieving high biocompatibility with the elastic modulus of human or animal bone (e.g., alveolar bone). (4) The white color of the bone implant is close to the color of bone itself, resulting in an aesthetic appearance. (5) Because the film layer is obtained by a coating process at high temperatures (over 400°C), the bone implant has excellent antibacterial properties. [Brief explanation of the drawings]

[0015] [Figure 1a] Shown is an SEM image of a pure tantalum sheet that is not coated with a porous lithium tantalate film. [Figure 1b] Shown is an SEM image of a pure tantalum sheet that is not coated with a porous lithium tantalate film. [Figure 1c] Shown is an SEM image of a pure tantalum sheet that is not coated with a porous lithium tantalate film. [Figure 2a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 2b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 2c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 2d]1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 3a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 3b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 3c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 4a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 4b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 4c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 5a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 5b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 5c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 6a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 6b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 6c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 7a]1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 7b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 7c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 7d] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 8a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 8b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 8c] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 9] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 10] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 11] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 12] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 13] 1 shows photographs of the appearance of a tantalum thin plate and a tantalum dental implant coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 14]1 shows photographs of the appearance of a tantalum thin plate and a tantalum dental implant coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 14a] 1 shows a photograph of the appearance of a porous tantalum dental implant coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15a] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15b] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15c] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15d] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15e] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15f] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 15g] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 16a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 16b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 17a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 17b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 18a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 18b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 19a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 19b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 20a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 20b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 21a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 21b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 22a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 22b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23a] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23b] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23c] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23d] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23e] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23f] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23g] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23h] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 23i] 1 shows a photograph of the appearance of a tantalum thin plate coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 24a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 24b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 25a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 25b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 26a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 26b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 27a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 27b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 28a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 28b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 29a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 29b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 30a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 30b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 31a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 31b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 32a] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 32b] 1 shows an SEM image of a tantalum sheet coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 33a] 1 shows a photograph of the appearance of a tantalum skull coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 33b] FIG. 1 shows a cross-sectional view of a tantalum skull coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 33c] FIG. 1 shows a top view of a tantalum skull coated with a porous lithium tantalate film according to one embodiment of the present invention. [Figure 34] 1 shows a photograph of the appearance of a tantalum-niobium alloy thin plate coated with a porous lithium tantalate-lithium niobate mixture film according to one embodiment of the present invention. [Figure 35a] 1 shows an SEM image of a tantalum-niobium alloy thin plate coated with a porous lithium tantalate-lithium niobate mixture film according to one embodiment of the present invention. [Figure 35b] 1 shows an SEM image of a tantalum-niobium alloy thin plate coated with a porous lithium tantalate-lithium niobate mixture film according to one embodiment of the present invention. [Figure 36] 1 shows a photograph of the appearance of a tantalum-niobium alloy thin plate coated with a porous lithium tantalate-lithium niobate mixture film according to one embodiment of the present invention. [Figure 37a] 1 shows an SEM image of a tantalum-niobium alloy thin plate coated with a porous lithium tantalate-lithium niobate mixture film according to one embodiment of the present invention. [Figure 37b] 1 shows an SEM image of a tantalum-niobium alloy thin plate coated with a porous lithium tantalate-lithium niobate mixture film according to one embodiment of the present invention. [Figure 38] 1 shows a photograph of the appearance of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 39a] 1 shows an SEM image of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 39b] 1 shows an SEM image of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 40] 1 shows a photograph of the appearance of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 41]1 shows a photograph of the appearance of a niobium skull coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 42a] 1 shows an SEM image of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 42b] 1 shows an SEM image of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 43] 1 shows a photograph of the appearance of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 44a] 1 shows an SEM image of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. [Figure 44b] 1 shows an SEM image of a niobium thin plate coated with a porous lithium niobate film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0016] In one embodiment, the present invention provides a method for producing a pharmaceutical composition comprising: (1) a tantalum substrate, and (2) a porous lithium tantalate film containing tantalum oxide located on the tantalum substrate; The present invention provides a bone implant or tantalum composite comprising:

[0017] In one embodiment, the present invention provides a method for producing a pharmaceutical composition comprising: (1) a niobium substrate, and (2) a porous lithium niobate film containing niobium oxide located on the niobium substrate; The present invention provides a bone implant or a niobium composite comprising:

[0018] In one embodiment, the present invention provides a method for producing a pharmaceutical composition comprising: (1) a tantalum-niobium alloy substrate; and (2) a porous lithium tantalate-lithium niobate mixture film containing tantalum oxide and niobium oxide located on the tantalum-niobium alloy substrate; The present invention provides a bone implant or a tantalum-niobium alloy composite comprising:

[0019] In one embodiment, the present invention provides a method for producing a pharmaceutical composition comprising: (1) a titanium substrate; and (2) a porous titanium oxide film located on the titanium substrate; The present invention provides a bone implant or titanium composite comprising:

[0020] In one embodiment, the bone implant or tantalum composite includes: (1) a tantalum substrate; and (2) a porous lithium tantalate membrane located on at least a portion of the surface of the tantalum substrate, the porous lithium tantalate membrane having a pore size of 0.1-1 μm, and the fissure-like pores can reach a length of about 40 μm.

[0021] In one embodiment, the bone implant or niobium composite includes: (1) a niobium substrate; and (2) a porous lithium niobate film located on at least a portion of the surface of the niobium substrate, the porous lithium niobate film having a pore size of 0.1-1 μm, and the fissure-like pores can reach a length of about 40 μm.

[0022] In one embodiment, the bone implant or tantalum-niobium alloy composite includes: (1) a tantalum-niobium alloy substrate; and (2) a porous lithium tantalate-lithium niobate composite membrane located on at least a portion of the surface of the tantalum-niobium alloy substrate, the composite membrane having pores with a diameter of 0.1-1 μm, and the length of the fissure-like pores can reach about 40 μm.

[0023] In one embodiment, the bone implant or titanium composite includes: (1) a titanium substrate; and (2) a porous titanium oxide membrane located on at least a portion of the surface of the titanium substrate, the porous titanium oxide membrane having pores of 0.1-1 μm in diameter, and fissure-like pores that can reach lengths of about 40 μm.

[0024] In the context of the present invention, the holes are not limited to circular holes, but may also be holes with irregular shapes, for example crack-like holes.

[0025] In one embodiment of the invention, the bone implant or composite has a porosity of 30% or more, such as a porosity of 50-80%, or a porosity of 60-90%.

[0026] In the context of the present invention, bone implant, composite and composite material can be used interchangeably.

[0027] The tantalum substrate applicable to the present invention includes a pure tantalum substrate and a tantalum alloy substrate, of which the tantalum alloy substrate is preferably a tantalum-niobium alloy substrate.

[0028] In one embodiment of the invention, the bone implant, such as a dental implant, has an elastic modulus of 150 GPa or greater.

[0029] In a further embodiment of the invention, the bone implant, such as a dental implant, has an elastic modulus of 170 GPa or greater.

[0030] In a further embodiment of the invention, the bone implant, such as a dental implant, has an elastic modulus of 150-200 GPa.

[0031] In a further embodiment of the invention, the bone implant, such as a dental implant, has an elastic modulus of 170-190 GPa.

[0032] In one embodiment of the invention, the bone implant, for example a cranial (skull) implant, has an elastic modulus of 10-160 GPa as measured by nanoindentation.

[0033] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 20-150 GPa as measured by nanoindentation.

[0034] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 30-140 GPa as measured by nanoindentation.

[0035] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 40-130 GPa measured by nanoindentation.

[0036] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 50-120 GPa as measured by nanoindentation.

[0037] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 60-110 GPa measured by nanoindentation.

[0038] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 70-100 GPa measured by nanoindentation.

[0039] In a further embodiment of the invention, the bone implant, such as a cranial (skull) implant, has an elastic modulus of 80-90 GPa measured by nanoindentation.

[0040] In one embodiment of the present invention, the entire surface of the tantalum substrate is covered with a porous lithium tantalate film.

[0041] In one embodiment of the present invention, the entire surface of the niobium substrate is covered with a porous lithium niobate film.

[0042] In one embodiment of the present invention, the entire surface of the tantalum-niobium alloy substrate is covered with a porous lithium tantalate-lithium niobate mixture film.

[0043] In one embodiment of the present invention, the entire surface of the titanium substrate is covered with a porous titanium oxide film.

[0044] From a biomechanical perspective, the elastic modulus of a dental implant affects the stress distribution at the bone interface. Generally, the higher the elastic modulus of a dental implant, the smaller the internal stress in the bone near the neck, but the greater the internal stress in the bone near the root end. The lower the elastic modulus of a dental implant, the greater the relative displacement movement between the dental implant and the bone interface. When the elastic modulus of a dental implant is close to that of cortical bone or cancellous bone, the biomechanical compatibility is relatively poor. An appropriate elastic modulus for a dental implant is 70 GPa or higher. The bone implant, including the dental implant of the present invention, has an elastic modulus of 150 GPa or higher. Therefore, the highly appropriate elastic modulus of the dental implant of the present invention provides excellent biomechanical compatibility.

[0045] In one embodiment of the invention, the bone implants include bone prostheses, for example cranial and dental implants.

[0046] In one embodiment of the present invention, the skull is porous, such as the tantalum skull shown in FIG. 33a and the niobium skull shown in FIG.

[0047] In one embodiment of the present invention, the dental implant comprises a denture base, a body, and a neck connecting the denture base and the body. Methods for manufacturing dental implants are known to those skilled in the art, and reference can be made to Chinese Patent Application Publication No. 109758245, Chinese Patent Application Publication No. 109965996, and Chinese Patent Application Publication No. 110610046.

[0048] In one preferred embodiment of the present invention, the dental implant includes a denture base portion, a main body portion, and a neck portion connecting the denture base portion and the main body portion, and the main body portion has an external thread on its outer surface that contacts the alveolar bone.

[0049] In one embodiment of the invention, the bone implant has a color similar to that of bone.In one preferred embodiment of the invention, the bone implant, in particular for a denture base, is white.

[0050] In one embodiment of the present invention, the substrate is porous. Porous substrates have excellent mechanical properties and tissue compatibility. Reconstruction of human tissue, bone grafting, and replacement can all be implanted into bone defects using porous materials, allowing bone to grow in along the porous pores and host interface, firmly bonding and integrating the porous material with bone tissue. Once implanted as a scaffolding material, the porous material does not need to decompose within the body due to its excellent tissue compatibility, eliminating the need for surgery for removal. The porous metal has a robust texture, and its wear resistance and fatigue resistance are superior to those of cancellous bone, ceramic products, and freeze-dried bone chips, allowing it to withstand sufficient physiological loads.

[0051] Tantalum, niobium, tantalum-niobium alloy, and titanium are refractory metals, and the porous metals are generally produced by methods known in the art. For example, porous tantalum can be produced by powder sintering or by vapor deposition. Other methods for producing porous tantalum in the art are also available.

[0052] In one embodiment of the present invention, the tantalum used is dense. All prior art documents the use of porous tantalum as a medical orthopedic material, but there is no mention of the use of dense tantalum metal as a medical orthopedic material. Regarding dental implants, from a biomechanical perspective, the elastic modulus of a dental implant affects the stress distribution at the bone interface. Generally, a higher elastic modulus of a dental implant reduces the internal stress of the bone near the neck, but increases the internal stress of the bone near the root end. The lower the elastic modulus of a dental implant, the greater the relative displacement movement between the dental implant and the bone interface. When the elastic modulus of a dental implant is close to that of cortical bone and cancellous bone, the biomechanical compatibility is relatively poor. The elastic modulus of a suitable dental implant is 70 GPa or higher. Because dental implants frequently perform the function of chewing, they are subjected to very high loads, and the tensile strength and elastic modulus of porous tantalum cannot meet these load requirements. The tensile strength and elastic modulus of dense metal tantalum are both relatively high, making it more suitable for use in dental implants.

[0053] One embodiment of the present invention is to coat a porous tantalum dental implant with a layer of porous lithium tantalate film, thereby increasing the mechanical properties of the dental implant, such as tensile strength and modulus of elasticity.

[0054] One embodiment of the present invention is to coat a porous lithium niobate film onto a porous niobium dental implant, thereby increasing the mechanical properties of the dental implant, such as tensile strength and modulus of elasticity.

[0055] One embodiment of the present invention is to coat a porous lithium tantalate-lithium niobate composite film onto a porous tantalum niobium dental implant, thereby increasing the mechanical properties of the dental implant, such as tensile strength and modulus of elasticity.

[0056] A further embodiment of the present invention is to coat a porous lithium tantalate film on dense tantalum metal, which not only increases its tensile strength and elastic modulus and better meets the tensile strength and elastic modulus requirements of dental implants, but also, by having a porous lithium tantalate film on the surface of the tantalum substrate, the dental implant can be more compatible with human biological tissues, allowing the human biological tissues to bond with the tantalum substrate through the porous lithium tantalate film, thereby allowing the tantalum material to be fully and firmly bonded and integrated with human tissues, such as alveolar bone.

[0057] In one embodiment of the present invention, the unexposed portion of the bone implant, e.g., dental implant, may not be coated with a lithium tantalate film layer and only employs pure tantalum material, while the denture base and neck are preferably coated with a lithium tantalate film, thereby enhancing the aesthetic appearance.

[0058] Methods for producing dense tantalum materials are known to those skilled in the art and can be obtained by methods such as casting, rolling, and the like.

[0059] In one embodiment of the present invention, the method for manufacturing the bone implant includes: (1) providing a tantalum substrate; and (2) forming a layer of porous lithium tantalate film on the tantalum substrate.

[0060] In one embodiment of the present invention, the method for producing the bone implant includes: (1) providing a niobium substrate; and (2) forming a layer of porous lithium niobate film on the niobium substrate.

[0061] In one embodiment of the present invention, the method for manufacturing the bone implant includes: (1) providing a tantalum-niobium alloy substrate; and (2) forming a layer of a porous lithium tantalate-lithium niobate composite film on the tantalum-niobium alloy substrate.

[0062] In one embodiment of the present invention, the method for producing the bone implant includes: (1) providing a titanium substrate; and (2) forming a layer of porous titanium oxide film on the titanium substrate.

[0063] In one embodiment of the invention, the substrate has the shape required for a bone implant, such as a dental implant and the shape of a skull.

[0064] In one preferred embodiment of the present invention, a porous lithium tantalate film is coated onto a tantalum substrate having the required shape for a bone implant.

[0065] In another embodiment of the present invention, a porous lithium tantalate film is coated on a tantalum substrate having a required shape for the bone implant, and unnecessary porous lithium tantalate film is removed from the bone implant by cutting or grinding, so that the porous lithium tantalate film is retained only on a portion of the surface of the bone implant. Specifically, first, a large number of manufactured combinations with acceptable outer dimensions but no internal holes are processed, and then the lithium tantalate film coating process is carried out, and then the internal holes are processed. In this way, the internal holes can be kept free from the film coating process.

[0066] In one preferred embodiment of the present invention, a porous lithium tantalate film is coated onto the surface of a portion of a tantalum substrate having the required shape for a bone implant.

[0067] In one embodiment of the present invention, the porous membrane has a thickness of 1-20 μm, preferably 2-10 μm, more preferably 3-5 μm.

[0068] In step (2), the porous lithium tantalate film is formed by a molten salt electrochemical method.

[0069] In one embodiment of the present invention, in step (2), the tantalum substrate is placed in a molten mixture of an oxygen-containing inorganic lithium salt (e.g., LiNO3) or an oxygen-containing inorganic lithium salt and lithium hydroxide, or a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt, at 250°C to 650°C, and a current of 1 to 1000 mA / cm 2 A porous lithium tantalate film is formed by applying a constant anode voltage of 1 to 66 V at a boost current density of 100 V for 0.01 to 200 hours.

[0070] In a further embodiment of the present invention, in step (2), the tantalum substrate is placed in a molten mixture of an oxygen-containing inorganic lithium salt (e.g., LiNO3) or an oxygen-containing inorganic lithium salt and lithium hydroxide, or a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt, at 440°C to 600°C, and a current of 1 to 1000 mA / cm 2 A porous lithium tantalate film is formed by applying a constant anode voltage of 10 to 30 V for 5 minutes to 10 hours at a boost current density of 10 V to 30 V.

[0071] In a further embodiment of the present invention, in step (2), the tantalum substrate is placed in a molten mixture of an oxygen-containing inorganic lithium salt (e.g., LiNO) or an oxygen-containing inorganic lithium salt and lithium hydroxide, or a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt, at 570°C to 598°C, and a current of 5 to 20 mA / cm 2 At a boost current density of 10 to 20 V, a constant anode voltage of 10 to 20 V is applied for 8 to 30 minutes to form a porous lithium tantalate film.

[0072] In one preferred embodiment, in step (2), an ultrasonic generator may be placed in the mixed melt or the mixed molten liquid.

[0073] Preferably, in step (2), the molten salt electrochemical method is a molten lithium salt electrochemical method.

[0074] Before step (2), the tantalum substrate may be subjected to an anodizing step.

[0075] The anodization process forms a Ta2O5 film, such as an amorphous Ta2O5 film, on the tantalum substrate, which is pore-free and suitable for use on tantalum capacitors.

[0076] The Ta2O5 film may be porous, which is advantageous for producing a porous lithium tantalate film. Specifically, the implant is placed in concentrated sulfuric acid at 190°C to 245°C (i.e., forming a porous Ta2O5 film in 98% concentrated sulfuric acid).

[0077] In one embodiment of the present invention, the anodization step forms a layer of amorphous Ta2O5 film on the tantalum substrate by anodization. In particular, in the anodization step, the tantalum substrate is placed in an oxygen-containing electrolyte solution at a temperature of from room temperature to 380°C, preferably from room temperature to 300°C, and a current of 1 to 200 mA / cm 2 A single layer of amorphous Ta2O5 film is formed by applying a constant anode voltage of 3 to 800 V for 0.01 to 2 hours at a boosted current density of 1000 V.

[0078] In the anodization process, if the temperature of the solution is high, the applied voltage should be low, and vice versa. For example, for a 0.01% H3PO4 solution at room temperature, a voltage of up to 600 V can be applied. Regardless of the solution, the applied voltage should be below the flashover voltage of the solution.

[0079] In the anodization process, the oxygen-containing electrolyte solution may be an aqueous solution, a non-aqueous solution, or a mixture of an aqueous electrolyte and an organic compound.

[0080] The aqueous oxygen-containing electrolyte may be, for example, an aqueous solution of an acid, base, or salt. The solution temperature is between room temperature (about 25°C) and 95°C, the anode voltage is between 5 and 600V, and the voltage is applied for 60 to 90 minutes. If the temperature is too high, the water volatilizes too quickly. If the solution temperature is relatively high, the anode voltage should be relatively low.

[0081] The non-aqueous oxygen-containing electrolyte may be concentrated anhydrous sulfuric acid or a molten salt or a mixture of a molten salt and a base, such as potassium nitrate, sodium nitrate, lithium nitrate, or a mixture of these with a base such as lithium, sodium, or potassium.

[0082] Another type of oxygen-containing electrolyte solution can be a mixture of aqueous electrolyte and organic compounds, such as ethanol, ethylene glycol, n-butanol, etc. The temperature of the aqueous solution should be below 95°C, otherwise the water will evaporate quickly and it is difficult to control.

[0083] In one embodiment of the present invention, the manufacturing method of the present invention includes a prior nitriding or carburizing treatment of the tantalum substrate. However, the nitriding or carburizing treatment is not required. To obtain a relatively high hardness, the nitriding or carburizing treatment can be adopted.

[0084] In one preferred embodiment, an ion nitriding furnace is used, the tantalum substrate is used as the cathode, the furnace temperature is 500-1000°C, the furnace pressure is 20-2000 Pa, the fill gas is nitrogen and hydrogen, the nitrogen:hydrogen ratio is 2:1 to 1:10, and nitriding is carried out for 0.5-6 hours to form a nitride layer on the surface of the tantalum substrate, and the hardness of the tantalum substrate after nitriding is controlled to be between HV180 and 480.

[0085] According to one embodiment of the present invention, 1) Select a tantalum rod, niobium rod, tantalum-niobium alloy rod, or titanium rod with an appropriate diameter; 2) Providing a processed cylindrical or conical implant (including processing external threads and internal threads, etc., and providing a connecting body and base to mate with the implant); 3) carrying out an electrochemical film coating process in a lithium-containing salt melt; Including, It can produce white lithium tantalate, lithium niobate, or lithium tantalate-lithium niobate mixed films on the surface of tantalum, niobium, and tantalum-niobium alloy implants, and can produce a single layer of porous titanium oxide film on the surface of titanium implants. A method for manufacturing a dental implant is provided.

[0086] This invention proposes to replace the screw thread with a suitable hole, which can penetrate the inner wall of the implant, i.e., drilling, without affecting the strength of the implant. The advantage of this solution is that it increases the contact area between the implant and the human bone, thereby improving the compatibility and strength of the implant.

[0087] Of course, the outer hole does not need to be drilled, and the thickness can be kept constant, so that the implant inner hole thread can be processed, which is advantageous for fixing the link or base.

[0088] According to one embodiment of the present invention, 1) Providing a dental implant blank and designing punching parameters; That is, determining the dimensions of the cylindrical or conical implant, including the outer diameter of the cylinder and the diameter of the inner hole, then developing the cylindrical body with holes into a plan view, designing and determining the size of the holes, the spacing or distribution of the holes, and the punching depth of the holes, and the shape of the holes, i.e., straight holes or tapered holes; 2) punching holes; That is, punching the spinneret according to the design requirements using a punching method or laser punching; 3) Polishing, That is, after punching, the excess material on the surface should be removed by polishing. For example, when using laser punching, there is generally no excess material around the hole, so polishing is relatively easy. 4) Welding punched and polished tantalum sheets using argon arc or laser to the original cylindrical or conical implant design, and then making any necessary repairs and threading. 5) carrying out the surface treatment on the porous implant and the base using an electrochemical method, thereby forming a composite porous film corresponding to the implant metal, to obtain a film-coated dental implant with holes; The present invention provides a method for manufacturing a dental implant, comprising:

[0089] According to one embodiment of the present invention, 1) Drilling an inlet, i.e., a hole on one side that will come into contact with the bone of the human body. Control the diameter size of the hole to 0.08-0.30 mm, preferably 0.16-0.22 mm; 2) The exit hole, i.e., the hole at one end interconnecting the hole and the implant inner hole, is controlled to have a diameter of 0.28-0.06 mm, preferably 0.22-0.13 mm. The hole shape can be tapered or straight. Tapered holes can be more advantageous in guiding the human bone to grow into the implant. The present invention provides a method for drilling an implant, comprising:

[0090] According to one embodiment of the present invention, a no-drilling implant design is provided, which ensures that the inner wall of the central hole of the dental implant can be threaded if necessary to install the base connector. The hole on the implant is kept 0.6-0.8 mm, otherwise no drilling is required, which makes it easier to thread the inner hole.

[0091] In the context of the present invention, niobium and tantalum-niobium alloy substrates are equally applicable to embodiments relating to tantalum substrates.

[0092] Unless otherwise specified, the tensile strength and modulus are measured according to GB / T22315-2008 standard.

[0093] The specific embodiments described below are intended to aid those skilled in the art in understanding the present invention, but are not intended to limit the scope of the present invention.

[0094] 1. (1) a substrate, and (2) a porous membrane located on the substrate; Including, The substrate is selected from a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, and a titanium substrate, preferably the substrate is selected from a tantalum substrate, a niobium substrate, and a tantalum-niobium alloy substrate; and The porous film is selected from a porous lithium tantalate film, a porous lithium niobate film, a porous lithium tantalate-lithium niobate composite film, and a porous titanium oxide film, preferably the porous film is selected from a porous lithium tantalate film, a porous lithium niobate film, and a porous lithium tantalate-lithium niobate composite film. Bone implants.

[0095] 2. (1) a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, or a titanium substrate; and (2) A porous lithium tantalate film located on the tantalum substrate and containing tantalum oxide, a porous lithium niobate film located on the niobium substrate and containing niobium oxide, a porous lithium tantalate-lithium niobate mixture film located on the tantalum-niobium alloy substrate and containing tantalum oxide and niobium oxide, or a porous titanium oxide film located on the titanium substrate. 2. The bone implant of embodiment 1, comprising:

[0096] 3. The bone implant of embodiment 1 or 2, wherein the porous lithium tantalate film, the porous lithium niobate film, the porous lithium tantalate-lithium niobate mixture film, or the porous titanium oxide film has a pore size of 0.1-1 μm.

[0097] 4. The bone implant according to embodiment 1 or 2, wherein the porous lithium tantalate film, the porous lithium niobate film, the porous lithium tantalate-lithium niobate mixture film or the porous titanium oxide film has a thickness of 1-20 μm, preferably 2-10 μm, more preferably 3-5 μm.

[0098] 5. A bone implant according to embodiment 1 or 2, having an elastic modulus of 150 GPa or greater.

[0099] 6. A bone implant according to embodiment 1 or 2, having an elastic modulus of 170 GPa or greater.

[0100] 7. A bone implant according to embodiment 1 or 2, having an elastic modulus of 150-200 GPa.

[0101] 8. A bone implant according to embodiment 7, having an elastic modulus of 170-190 GPa.

[0102] 9. A bone implant according to embodiment 1 or 2, which has a color similar to bone.

[0103] 10. The bone implant according to embodiment 1 or 2, including bone prostheses, dental implants and skulls.

[0104] 11. The bone implant of embodiment 10, wherein the dental implant comprises a denture base portion, a body portion, and a neck portion connecting the denture base portion and the body portion.

[0105] 12. A bone implant according to embodiment 1 or 2, having an elastic modulus of 10-160 GPa, preferably an elastic modulus of 20-150 GPa, more preferably an elastic modulus of 30-140 GPa.

[0106] 13. The bone implant according to embodiment 1 or 2, wherein the tantalum, niobium or tantalum-niobium alloy substrate is porous.

[0107] 14. The bone implant according to embodiment 1 or 2, wherein the tantalum, niobium or tantalum-niobium alloy substrate is dense.

[0108] 15. (1) providing a substrate; and (2) forming a porous membrane on the substrate; Including, The substrate is selected from a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, and a titanium substrate, preferably the substrate is selected from a tantalum substrate, a niobium substrate, and a tantalum-niobium alloy substrate; and The porous film is selected from a porous lithium tantalate film, a porous lithium niobate film, a porous lithium tantalate-lithium niobate composite film, and a porous titanium oxide film, preferably the porous film is selected from a porous lithium tantalate film, a porous lithium niobate film, and a porous lithium tantalate-lithium niobate composite film. A method for producing a bone implant according to any one of embodiments 1-14.

[0109] 16. (1) providing a tantalum substrate, a niobium substrate, a tantalum-niobium alloy substrate, or a titanium substrate; and (2) forming a porous lithium tantalate film, a porous lithium niobate film, or a porous lithium tantalate-lithium niobate mixture film on the tantalum substrate, the niobium substrate, or the tantalum-niobium alloy substrate, or forming a porous titanium oxide film on the titanium substrate; Including, The lithium tantalate film contains tantalum oxide, The lithium niobate film contains niobium oxide, and The composite film contains tantalum oxide and niobium oxide. 16. The method of embodiment 15.

[0110] 17. The method according to embodiment 15 or 16, wherein in step (2), the porous membrane is formed by a molten salt electrochemical method.

[0111] 18. The method of embodiment 15 or 16, wherein prior to step (2), a Ta2O5 film is formed on the tantalum substrate.

[0112] 19. The method of embodiment 18, wherein an amorphous Ta2O5 film is formed on the tantalum substrate by anodization.

[0113] 20. In the step of forming a Ta2O5 film on a tantalum substrate, the tantalum substrate is placed in an oxygen-containing electrolyte solution at a temperature of from room temperature to 380°C, preferably from room temperature to 300°C, and a current of 1 to 200 mA / cm 2 20. The method of embodiment 19, wherein an anode voltage of 3 to 800 V is applied at a boosted current density of 0.01 to 2 hours to form an amorphous Ta2O5 film.

[0114] 21. The method of embodiment 15 or 16, wherein prior to step (2), a Nb2O5 film is formed on the niobium substrate.

[0115] 22. The method of embodiment 21, wherein an amorphous Nb2O5 film is formed on the niobium substrate by anodization.

[0116] 23. In the step of forming an Nb2O5 film on a niobium substrate, the niobium substrate is placed in an oxygen-containing electrolyte solution at a temperature of from room temperature to 380°C, preferably from room temperature to 300°C, and a current of 1 to 200 mA / cm 2 23. The method of embodiment 22, wherein an anode voltage of 3 to 800 V is applied at a boosted current density of 0.01 to 2 hours to form an amorphous Nb2O5 film.

[0117] 24. The method of embodiment 15 or 16, wherein prior to step (2), a Ta2O5-Nb2O5 mixture film is formed on a tantalum-niobium alloy substrate.

[0118] 25. The method of embodiment 24, wherein an amorphous Ta2O5-Nb2O5 mixture film is formed on the tantalum-niobium alloy substrate by anodization.

[0119] 26. In the step of forming a Ta2O5-Nb2O5 mixture film on a tantalum-niobium alloy substrate, the tantalum-niobium alloy substrate is placed in an oxygen-containing electrolyte solution at a temperature of from room temperature to 380°C, preferably from room temperature to 300°C, and a current of 1 to 200 mA / cm 2 26. The method of embodiment 25, wherein an anode voltage of 3 to 800 V is applied at a boosted current density of 0.01 to 2 hours to form an amorphous Ta2O5-Nb2O5 composite film.

[0120] 27. The method of any one of embodiments 20, 23, and 26, wherein the oxygen-containing electrolyte solution is an aqueous solution, a non-aqueous solution, or a mixture of an aqueous electrolyte and an organic compound.

[0121] 28. The method of embodiment 27, wherein the molten salt electrochemistry is a molten lithium salt electrochemistry.

[0122] 29. A tantalum substrate, a niobium substrate, or a tantalum-niobium alloy substrate is placed in a molten mixture of an oxygen-containing inorganic lithium salt or an oxygen-containing inorganic lithium salt and lithium hydroxide, or a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt, at 250°C to 650°C, and a current of 1 to 1000 mA / cm 2 17. The method according to embodiment 15 or 16, wherein an anode voltage of 1 to 66 V is applied at a boosted current density of 1 to 66 V for 0.01 to 200 hours to form a film layer comprising a lithium-containing compound.

[0123] 30. In step (2), the tantalum substrate, the niobium substrate, or the tantalum-niobium alloy substrate is placed in a molten mixture of an oxygen-containing inorganic lithium salt or an oxygen-containing inorganic lithium salt and lithium hydroxide, or a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt, at 440°C to 600°C, and a current of 5 to 20 mA / cm 2 30. The method of embodiment 29, wherein an anode voltage of 10 to 30 V is applied at a boosted current density of 10 V for 5 minutes to 10 hours to form a film layer comprising a lithium-containing compound.

[0124] 31. In step (2), the tantalum substrate, the niobium substrate, or the tantalum-niobium alloy substrate is placed in a molten mixture of an oxygen-containing inorganic lithium salt or an oxygen-containing inorganic lithium salt and lithium hydroxide, or a molten mixture of a salt and lithium hydroxide, or a molten mixture of a lithium salt and an oxygen-containing salt, at 570°C to 598°C, and a current of 5 to 20 mA / cm 2 30. The method of embodiment 29, wherein an anode voltage of 10 to 20 V is applied at a boosted current density of 10 V to 20 V for 8 minutes to 30 minutes to form a film layer comprising a lithium-containing compound.

[0125] 32. The method of embodiment 29, wherein the oxygen-containing inorganic lithium salt is LiNO3.

[0126] 33. The method of embodiment 29, wherein in step (c), an ultrasonic generator is placed in the mixed melt or the mixed molten liquid.

[0127] 34. The method of embodiment 15 or 16, wherein the tantalum, niobium, or tantalum-niobium alloy substrate is nitrided or carburized.

[0128] 35. Use of a bone implant in medical materials, wherein the bone implant is as described in any one of embodiments 1-14 or is produced by the method according to any one of embodiments 15-34.

[0129] 36. The use according to embodiment 35, wherein the medical material is a dental implant or a skull. [Example]

[0130] The nature and objects of the present invention will be further understood hereinafter by means of embodiments and in conjunction with the accompanying drawings, however, it is understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.

[0131] Example 1 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0132] Step 2: An anode voltage of 10 V was applied to the tantalum thin plate in a molten lithium nitrate solution at 570°C, and the voltage was kept constant for 30 minutes to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0133] 2a-2d show SEM images of the sample of Example 1.

[0134] FIG. 9 shows a photograph of the appearance of the sample of Example 1.

[0135] Example 2 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0136] Step 2: An anode voltage of 10 V was applied to the tantalum thin plate in a molten lithium nitrate solution at 580°C, and the voltage was kept constant for 25 minutes to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0137] 3a-3c show SEM images of the sample of Example 2.

[0138] FIG. 10 shows a photograph of the appearance of the sample of Example 2.

[0139] Example 3 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0140] Step 2: An anode voltage of 10 V was applied to the tantalum thin plate in a molten lithium nitrate solution at 598°C, and the voltage was kept constant for 10 minutes to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0141] 4a-4c show SEM images of the sample of Example 3.

[0142] FIG. 11 shows a photograph of the appearance of the sample of Example 3.

[0143] Example 4 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0144] Step 2: A solution with a volume ratio of ethylene glycol:0.01%H3PO4=2:1 was used for the tantalum thin plate, the solution temperature was 90°C, and an anode voltage of 60V was applied, and the voltage was kept constant for 3 hours, after which the plate was washed.

[0145] Step 3: An anode voltage of 10 V was applied to the tantalum thin plate obtained in step (2) in a molten lithium nitrate solution at 598°C, and the voltage was kept constant for 8 minutes to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0146] 5a-5c show SEM images of the sample of Example 4.

[0147] FIG. 12 shows a photograph of the appearance of the sample of Example 4.

[0148] Example 5 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0149] Step 2: A solution with a volume ratio of ethylene glycol:0.01%H3PO4=2:1 was used for the tantalum thin plate, the solution temperature was 90°C, and an anode voltage of 143V was applied, and the voltage was kept constant for 3 hours, after which the plate was washed.

[0150] Step 3: An anode voltage of 28 V was applied to the tantalum thin plate obtained in step (2) in a molten lithium nitrate solution at 482°C, and the voltage was kept constant for 6.5 hours to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0151] 6a-6c show SEM images of the sample of Example 5.

[0152] Example 6 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0153] Step 2: An anode voltage of 33 V was applied to the tantalum thin plate in a molten lithium nitrate solution at 440°C, and the voltage was kept constant for 12 hours to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0154] 7a-7d show SEM images of the sample of Example 6.

[0155] Example 7 Step 1: Metallic tantalum was processed into a dense tantalum thin plate.

[0156] Step 2: A solution with a volume ratio of ethylene glycol:0.01%H3PO4=2:1 was used for the tantalum thin plate, the solution temperature was 90°C, and an anode voltage of 60V was applied, and the voltage was kept constant for 3 hours, after which the plate was washed.

[0157] Step 3: An anode voltage of 10 V was applied to the tantalum thin plate obtained in step (2) in a molten lithium nitrate solution at 598°C, and the voltage was kept constant for 10 minutes to cause a reaction, forming a porous lithium tantalate film layer on the tantalum thin plate.

[0158] 8a-8c show SEM images of the sample of Example 7.

[0159] Example 8 Step 1: Metallic tantalum was processed into dense tantalum sheet and tantalum dental implant, respectively.

[0160] Step 2: An anodic voltage of 10 V was applied to each of the tantalum thin plate and tantalum dental implant (a threaded tantalum rod with a diameter of 6 mm and a hole with a diameter of 2 mm) in a molten lithium nitrate:potassium nitrate (weight ratio of 1:1) solution at 580°C, and the voltage was kept constant for 30 minutes to allow the reaction to occur, thereby forming a porous lithium tantalate film layer on the tantalum thin plate and the tantalum dental implant.

[0161] FIG. 13 shows a photograph of the appearance of the sample of Example 8.

[0162] Example 9 Step 1: Metallic tantalum was processed into dense tantalum sheet and tantalum dental implant (a threaded tantalum rod with a diameter of 6 mm and a hole with a diameter of 2 mm), respectively.

[0163] Step 2: First, an anodic voltage of 60 V was applied to each of the tantalum thin plate and the tantalum dental implant in a 0.05 wt % H3PO4 aqueous solution at 90°C, and the voltage was kept constant for 1.5 hours, after which the tantalum thin plate and the tantalum dental implant were washed.

[0164] Step 3: An anodic voltage of 10 V was applied to the tantalum thin plate and tantalum dental implant obtained in step (2) in molten lithium nitrate:potassium nitrate (weight ratio 1:1) at 598°C, and the voltage was kept constant for 8 minutes to allow the reaction to occur, forming a porous lithium tantalate film layer on the tantalum thin plate and tantalum dental implant.

[0165] FIG. 14 shows a photograph of the appearance of the sample of Example 9.

[0166] Example 9a A 10V anodic voltage was applied to a porous tantalum dental implant in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution at 580°C, and the reaction was carried out at a constant voltage for 25 minutes.

[0167] FIG. 14a shows a photograph of the appearance of the sample of Example 9a.

[0168] Comparative Example 1 Metallic tantalum was processed into a dense tantalum thin plate, but the step of forming a porous lithium tantalate film layer on the tantalum thin plate was not carried out.

[0169] 1a-1c show SEM images of the sample of Comparative Example 1.

[0170] [Table 1] [Table 2] Note: In Table 2, the thickness of the film after film coating for each sample is approximately 10 μm, and the transition layer below the film is also approximately 30 μm, which indicates that its proportion in the coarse tantalum test piece is very small. Therefore, the measured data is very close to that of pure tantalum, and the measurement data in Table 2 is basically close to the elastic modulus of pure tantalum and cannot represent the elastic modulus of the surface layer of the film coating of the sample of the present invention. On the other hand, values ​​measured using a nanoindentation method, such as an instrument model TI-950, can show the change in elastic modulus due to the different film coating processes of the present invention.

[0171] The data in Tables 1 and 2 reveal the following: Compared to tantalum thin plates that are not coated with a porous lithium tantalate film, the tensile strength and modulus of elasticity of tantalum thin plates coated with a porous lithium tantalate film are both significantly improved, and the modulus of elasticity in particular is far greater than the 70 GPa modulus required for the production of dental implants, which is highly advantageous.

[0172] By comparing SEM images of a tantalum thin plate coated with a porous lithium tantalate film and a tantalum thin plate not coated with a porous lithium tantalate film, it can be seen that the tantalum thin plate coated with the porous lithium tantalate film of the present invention has many open pores with pore sizes ranging from about 1 to 30 micrometers and a rough surface, and these pores and uneven, rough surface are advantageous for cell attachment and tissue interdigitation, and can strengthen the connection strength between a bone implant, such as a dental implant, and bone tissue, thereby allowing the bone implant to better bond with human biological tissue via the porous lithium tantalate film and the tantalum substrate, and allowing the tantalum substrate to be more firmly bonded and integrated with human tissue, such as alveolar bone. On the other hand, the tantalum thin plate not coated with a porous lithium tantalate film has relatively few pores and a smooth, flat surface, which is unfavorable for the tantalum substrate and human tissue, such as alveolar bone, to be firmly bonded together.

[0173] In addition, SEM images show that the smallest dimension of the pores in the tantalum thin plate coated with the porous lithium tantalate film is in the range of about 10 nanometers to 1 micrometer, which is much smaller than the size of bacteria (usually larger than 5 micrometers). Therefore, the bone implant coated with the porous lithium tantalate film of the present invention can effectively inhibit bacterial invasion and has a certain antibacterial effect.

[0174] From Figures 9-12, it can be seen that the tantalum sheet coated with the porous lithium tantalate film is white in color and has an aesthetic appearance, making it particularly suitable for fabricating dental implants.

[0175] Example 10 A lithium tantalate film layer was formed on the tantalum thin plate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0176] FIG. 15a shows a photograph of the appearance of the sample of Example 10.

[0177] 16a-16b show SEM images of the sample of Example 10.

[0178] Example 11 A lithium tantalate film layer was formed on each of the tantalum thin plate and the tantalum skull substrate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0179] FIG. 15b (tantalum thin plate) and FIG. 33a (skull) show photographs of the appearance of the sample of Example 11.

[0180] 17a-17b show SEM images of the sample of Example 11.

[0181] Example 12 A lithium tantalate film layer was formed on a tantalum thin plate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0182] FIG. 15c shows a photograph of the appearance of the sample of Example 12.

[0183] 18a-18b show SEM images of the sample of Example 12.

[0184] Example 13 First, a solution with a volume ratio of ethylene glycol: 0.01 wt% H3PO4 = 2:1 was used on a thin tantalum plate. The solution temperature was 90°C, and an anode voltage of 60 V was applied. The voltage was kept constant for 1.5 hours, and then the plate was washed. Then, a lithium tantalate film layer was formed in a molten lithium nitrate: potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0185] FIG. 15d shows a photograph of the appearance of the sample of Example 13.

[0186] 19a-19b show SEM images of the sample of Example 13.

[0187] Example 14 First, a solution with a volume ratio of ethylene glycol: 0.01 wt% H3PO4 = 2:1 was used on a thin tantalum plate. The solution temperature was 90°C, and an anode voltage of 60 V was applied. The voltage was kept constant for 1.5 hours, and then the plate was washed. Then, a lithium tantalate film layer was formed in a molten lithium nitrate: potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0188] FIG. 15e shows a photograph of the appearance of the sample of Example 14.

[0189] 20a-20b show SEM images of the sample of Example 14.

[0190] Example 15 First, a solution with a volume ratio of ethylene glycol: 0.01 wt% H3PO4 = 2:1 was used on a thin tantalum plate. The solution temperature was 90°C, and an anode voltage of 143 V was applied. The voltage was kept constant for 1.5 hours, and then the plate was washed. Then, a lithium tantalate film layer was formed in a molten lithium nitrate: potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0191] FIG. 15f shows a photograph of the appearance of the sample of Example 15.

[0192] 21a-22b show SEM images of the sample of Example 15.

[0193] Example 16 A lithium tantalate film layer was formed on a tantalum thin plate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution under the process conditions shown in Table 3.

[0194] FIG. 15g shows a photograph of the appearance of the sample of Example 16.

[0195] 22a-22b show SEM images of the sample of Example 16.

[0196] Example 17 First, a tantalum thin plate was immersed in a 98% concentrated H2SO4 solution at a temperature of 220°C, and an anode voltage of 150 V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0197] FIG. 23a shows a photograph of the appearance of the sample of Example 17.

[0198] 24a-24b show SEM images of the sample of Example 17.

[0199] Example 18 First, a tantalum thin plate was immersed in a 98% concentrated H2SO4 solution at a temperature of 220°C, and an anode voltage of 150 V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0200] FIG. 23b shows a photograph of the appearance of the sample of Example 18.

[0201] 25a-25b show SEM images of the sample of Example 18.

[0202] Example 19 First, a tantalum thin plate was immersed in a 98% concentrated H2SO4 solution at a temperature of 220°C, and an anode voltage of 150 V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0203] FIG. 23c shows a photograph of the appearance of the sample of Example 19.

[0204] 26a-26b show SEM images of the sample of Example 19.

[0205] Example 20 First, a tantalum thin plate was immersed in a 98% concentrated H2SO4 solution at a temperature of 220°C, and an anode voltage of 82V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0206] FIG. 23d shows a photograph of the appearance of the sample of Example 20.

[0207] 27a-27b show SEM images of the sample of Example 20.

[0208] Example 21 First, a tantalum thin plate was immersed in a 98% concentrated H2SO4 solution at a temperature of 210°C, and an anode voltage of 82V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0209] FIG. 23e shows a photograph of the appearance of the sample of Example 21.

[0210] 28a-28b show SEM images of the sample of Example 21.

[0211] Example 22 First, a tantalum thin plate was placed in a 98% concentrated H2SO4 solution at a temperature of 210°C, and an anode voltage of 82V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0212] FIG. 23f shows a photograph of the appearance of the sample of Example 22.

[0213] 29a-29b show SEM images of the sample of Example 22.

[0214] Example 23 First, a tantalum thin plate was immersed in a 98% concentrated H2SO4 solution at a temperature of 210°C, and an anode voltage of 82V was applied. The voltage was kept constant for 30 minutes, after which the plate was washed and dried. A lithium tantalate film layer was then formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate film layer are shown in Table 3.

[0215] FIG. 23g shows a photograph of the appearance of the sample of Example 23.

[0216] 30a-30b show SEM images of the sample of Example 23.

[0217] Example 24 Anodization was carried out on a tantalum sheet in a solution of 98% concentrated H2SO4, the temperature was 220°C, and an anodic voltage of 150V was applied and kept constant for 30 minutes, as shown in Table 3.

[0218] FIG. 23h shows a photograph of the appearance of the sample of Example 24.

[0219] 31a-31b show SEM images of the sample of Example 24.

[0220] Example 25 A titanium oxide film layer was formed on the titanium thin plate by anodizing in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the titanium oxide film layer are shown in Table 3.

[0221] FIG. 23i shows a photograph of the appearance of the sample of Example 25.

[0222] 32a-32b show SEM images of the sample of Example 25.

[0223] The data in Table 3 show that the tantalum composite coated with porous lithium tantalate film has an appropriate modulus of elasticity, making it suitable for fabricating, for example, engineered cranial (skull) implants.

[0224] By comparing SEM images of a tantalum thin plate coated with a porous lithium tantalate film and a tantalum thin plate not coated with a porous lithium tantalate film, it can be seen that the tantalum thin plate coated with the porous lithium tantalate film of the present invention has many open pores with a pore size ranging from about 0.1 to 30 micrometers, even honeycomb-like open pores, and a rough surface, and these pores and uneven, rough surface are advantageous for cell attachment and tissue interdigitation, and can strengthen the connection strength between a bone implant, such as a dental implant, and bone tissue, such as the skull (skull), so that the bone implant can be better bonded to human biological tissue via the porous lithium tantalate film and the tantalum substrate, and the tantalum substrate can be more firmly bonded and integrated with human tissue. On the other hand, the tantalum thin plate not coated with a porous lithium tantalate film has relatively few pores and a smooth surface, which is unfavorable for the tantalum substrate to be firmly bonded to human tissue, such as the alveolar bone and the skull (skull).

[0225] The titanium thin plate with a titanium oxide film layer prepared in Example 25 exhibits an appropriate elastic modulus, and its SEM image shows that the film layer has a fibrous porous interactive network (see Figure 32b), which is advantageous for cell attachment and tissue interdigitation and can strengthen the connection strength of bone implants, such as bone tissue (e.g., skull), so that the bone implant can better bond with human biological tissues through the porous titanium oxide film layer and the titanium substrate, and the titanium substrate can be more firmly bonded and integrated with human tissues.

[0226] In addition, SEM images show that the smallest dimension of the pores in the tantalum thin plate coated with the porous lithium tantalate film is in the range of about 10 nanometers to 1 micrometer, which is much smaller than the size of bacteria (which is usually larger than 5 micrometers). Therefore, the bone implant coated with the porous lithium tantalate film of the present invention can effectively inhibit bacterial invasion and has a certain antibacterial effect.

[0227] Example 26 A lithium tantalate-lithium niobate composite film layer was formed on a tantalum-niobium alloy thin plate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate-lithium niobate composite film layer are shown in Table 3.

[0228] FIG. 34 shows a photograph of the appearance of the sample of Example 26.

[0229] 35a-35b show SEM images of the sample of Example 26.

[0230] Example 27 First, a solution with a volume ratio of ethylene glycol:0.01 wt% H3PO4 = 2:1 was used on a tantalum-niobium alloy thin plate. The solution temperature was 90°C, and an anode voltage of 143 V was applied. The voltage was kept constant for 1.5 hours, and then the plate was washed. Then, a lithium tantalate-lithium niobate composite film layer was formed in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium tantalate-lithium niobate composite film layer are shown in Table 3.

[0231] FIG. 36 shows a photograph of the appearance of the sample of Example 27.

[0232] 37a-37b show SEM images of the sample of Example 27.

[0233] Example 28 A lithium niobate film layer was formed on the niobium thin plate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium niobate film layer are shown in Table 3.

[0234] FIG. 38 shows a photograph of the appearance of the sample of Example 28.

[0235] 39a-39b show SEM images of the sample of Example 28.

[0236] Example 29 A lithium niobate film layer was formed on the niobium thin plate and the niobium skull substrate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium niobate film layer are shown in Table 3.

[0237] FIG. 40 (niobium thin plate) and FIG. 41 (niobium skull) show photographs of the appearance of the sample of Example 29.

[0238] 42a-42b show SEM images of the sample of Example 29.

[0239] Example 30 A lithium niobate film layer was formed on the niobium thin plate in a molten lithium nitrate:potassium nitrate (weight ratio 1:1) solution. The process conditions for forming the lithium niobate film layer are shown in Table 3.

[0240] FIG. 43 shows a photograph of the appearance of the sample of Example 30.

[0241] 44a-44b show SEM images of the sample of Example 31.

[0242] Table 3. Sample preparation and elastic modulus (measured by nanoindenter TI-950, NHT, Hysitron, US) [Table 3] The elastic moduli in Table 3 were measured using a nanoindenter TI-950 (US, Hysitron, NHT).

[0243] The data in Table 3 show that the composites coated with the porous lithium tantalate-lithium niobate mixture film and the composites having the porous lithium niobate film have suitable elastic moduli, which are suitable for fabricating, for example, cranial bone (skull) implants.

[0244] While particular embodiments of the present invention have been shown and described, it should be understood that other modifications, alternatives, and options are known to those skilled in the art. Such modifications, alternatives, and optional embodiments may be made without departing from the spirit and scope of the present invention, which is determined by the appended claims. Various features of the present invention are set forth in the appended claims.

Claims

1. (1) a substrate, and (2) a porous membrane located on the substrate; Including, the substrate is a tantalum substrate and the porous film is a porous lithium tantalate film; the substrate is a niobium substrate and the porous film is a porous lithium niobate film; or The substrate is a tantalum-niobium alloy substrate, and the porous film is a porous lithium tantalate-lithium niobate mixture film. Bone implants.

2. (1) a tantalum substrate, a niobium substrate, or a tantalum-niobium alloy substrate; and (2) a porous lithium tantalate film containing tantalum oxide located on the tantalum substrate; a porous lithium niobate film located on the niobium substrate and containing niobium oxide; or a porous lithium tantalate-lithium niobate mixture film containing tantalum oxide and niobium oxide and disposed on the tantalum-niobium alloy substrate; The bone implant of claim 1 , comprising:

3. 2. The bone implant of claim 1, wherein the porous lithium tantalate film, the porous lithium niobate film, or the porous lithium tantalate-lithium niobate mixture film has a pore size of 0.1-1 μm.

4. 2. The bone implant of claim 1, wherein the porous lithium tantalate film, the porous lithium niobate film, or the porous lithium tantalate-lithium niobate mixture film has a thickness of 1-20 μm.

5. 2. The bone implant of claim 1 having an elastic modulus of 150 GPa or more, or an elastic modulus of 30-140 GPa.

6. The bone implant of claim 1 , including bone prostheses, dental implants and skull implants.

7. 2. The bone implant of claim 1, wherein the tantalum substrate, the niobium substrate, or the tantalum-niobium alloy substrate is porous or dense.

8. (1) providing a tantalum substrate, a niobium substrate, or a tantalum-niobium alloy substrate; and (2) forming a porous lithium tantalate film on the tantalum substrate; forming a porous lithium niobate film on the niobium substrate; or forming a porous lithium tantalate-lithium niobate mixture film on the tantalum-niobium alloy substrate; Including, the lithium tantalate film contains tantalum oxide; The lithium niobate film contains niobium oxide, and The mixture film contains tantalum oxide and niobium oxide. A method for producing the bone implant of claim 1.

9. The method according to claim 8, wherein in step (2), the porous film is formed by a molten lithium salt electrochemical method.

10. Before step (2), amorphous Ta is formed on the tantalum substrate by anodization. 2 O 5 9. The method of claim 8, further comprising forming an amorphous Nb 2 O 5 film on the niobium substrate by anodization prior to step (2), or forming an amorphous Ta 2 O 5 -Nb 2 O 5 mixture film on the tantalum-niobium alloy substrate by anodization prior to step (2).

11. Ta on tantalum substrate 2 O 5 In the process of forming the film, the tantalum substrate is placed in an oxygen-containing electrolyte solution at room temperature to 380° C., and a current of 1 to 200 mA / cm is applied. 2A constant anode voltage of 3 to 800 V was applied for 0.01 to 2 hours at a boost current density of 1000 V to form amorphous Ta. 2 O 5 The method of claim 10, further comprising forming a membrane.

12. Nb on niobium substrate 2 O 5 In the process of forming the film, the niobium substrate is placed in an oxygen-containing electrolyte solution at room temperature to 380° C., and a current of 1 to 200 mA / cm is applied. 2 A constant anode voltage of 3 to 800 V was applied for 0.01 to 2 hours at a boost current density of 1000 V to form amorphous Nb 2 O 5 The method of claim 10, further comprising forming a membrane.

13. Ta on a tantalum-niobium alloy substrate 2 O 5 -Nb 2 O 5 In the step of forming the mixture film, the tantalum-niobium alloy substrate is placed in an oxygen-containing electrolyte solution at room temperature to 380° C., and a current of 1 to 200 mA / cm is applied. 2 A constant anode voltage of 3 to 800 V was applied for 0.01 to 2 hours at a boost current density of 1000 V to form amorphous Ta. 2 O 5 -Nb 2 O 5 The method of claim 10, further comprising forming a mixture film.

14. A tantalum substrate, a niobium substrate, or a tantalum-niobium alloy substrate is placed in an oxygen-containing inorganic lithium salt or a mixed melt of an oxygen-containing inorganic lithium salt and lithium hydroxide, or a mixed melt of a salt and lithium hydroxide, or a mixed melt of a lithium salt and an oxygen-containing salt, at 250° C. to 650° C., and a current of 1 to 1000 mA / cm 2 10. The method of claim 9, wherein an anode voltage of 1 to 66 V is applied at a boosted current density of 0.01 to 200 hours to form a membrane layer containing a lithium-containing compound.

15. The oxygen-containing inorganic lithium salt is LiNO 3 The method of claim 14, wherein

16. 13. Use of a bone implant in a medical material, said bone implant being as defined in claim 1.

17. The use according to claim 16, wherein said medical material is a dental implant or a skull.

18. (1) Providing a dental implant tantalum blank and designing punching parameters; (2) punching holes; (3) Polishing; (4) Welding the punched and polished tantalum sheets into the originally designed cylindrical or conical implants using argon arc welding or laser welding, and making any necessary repairs and machining of female threads; (5) carrying out a surface treatment on the porous implant and the base using an electrochemical method to generate a composite porous membrane corresponding to the implant metal, to obtain a coated dental implant having pores, the porous membrane being a porous lithium tantalate membrane; 1. A method for producing a dental implant having a hole, comprising:

19. (1) Perforation entrance; (2) Exit; Including, The implant is a bone implant according to claim 1. How to drill an implant.

20. A non-drilling implant, wherein the holes on the implant are 0.6 to 0.8 mm, and the implant is a bone implant as described in claim 1.