Hardcoat compositions, articles and methods containing methyl or ethyl trialkoxysilanes

JP2023546017A5Active Publication Date: 2024-10-033M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023521447
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-08
Filing Date
2021-09-23
Publication Date
2024-10-03
Estimated Expiration
2041-09-23

AI Technical Summary

Technical Problem

Existing rewritable surfaces, such as dry erase articles, lack durability and effective erasability, particularly with permanent markers, and hardcoat compositions suffer from stability issues.

Method used

A hardcoat composition comprising R1Si(OR)3 silane monomers, optionally with R2Si(OR)mSi(OR)4 monomers, and silica nanoparticles, optionally with a hydrophilic silane surface layer, forming a polysiloxane network for improved durability and erasability.

Benefits of technology

The composition provides durable, easily erasable surfaces that effectively remove permanent marker writing with water, while maintaining stability and mechanical integrity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An article is described that includes a substrate and a hard coat layer disposed on the substrate. The hard coat layer comprises: i) a compound represented by formula R 1 Si(OR)3 (wherein R and R 1 is methyl or ethyl), ii) a first hydrophobic silane monomer having the formula (R 2 ) 4-m Si(OR) m or Si(OR) (wherein R, R 1 and R 2 is an organic group, where R 1 and an optional second silane monomer having a silane group (wherein m is not methyl or ethyl, and m is in the range of 1 to 3). The hardcoat layer may further comprise 10% to 30% by weight of silica nanoparticles. A surface layer comprising a hydrophilic silane may be disposed on the hardcoat layer. Methods of using articles having rewritable surfaces, hardcoat coating compositions, and methods of making the hardcoat compositions and articles are also described.
Need to check novelty before this filing date? Find Prior Art

Description

Summary of the Invention

[0001] Articles with rewritable surfaces, such as dry erase articles, have been described (see, for example, International Publication No. 2011163175). However, there remains a need for rewritable writing surfaces that exhibit durable performance and good erasability, particularly the erasability of permanent markers with water. There also remains a need for hard coat coating compositions with good stability.

[0002] In some embodiments, articles (e.g., dry erase boards and anti-fog face shields) are described that include a substrate and a hard coat layer disposed on the substrate. The hard coat layer comprises: i) a compound represented by the formula R 1 Si(OR)3 (wherein R and R 1 is methyl or ethyl), ii) a first hydrophobic silane monomer having the formula (R 2 ) 4-m Si(OR) m or Si(OR) (wherein R, R 1 and R 2 is an organic group, where R 1 and an optional second silane monomer having a silane group having a silane group moiety (wherein m is not methyl or ethyl, and m is in the range of 1 to 3). When present, the second silane monomer is present in an amount less than 20 wt. % based on the total of the first and second silane monomers. The hardcoat layer preferably further comprises 10 wt. % to 30 wt. % silica nanoparticles. In some preferred embodiments, a surface layer comprising a hydrophilic silane, such as a zwitterionic silane, is disposed on the hardcoat layer.

[0003] Methods of using articles having rewritable surfaces, hardcoat coating compositions, and methods of making the hardcoat compositions and articles are also described. [Brief explanation of the drawings]

[0004] [Figure 1]FIG. 1 is a schematic cross-sectional view of an exemplary article including a hydrolysis and condensation hard coat layer disposed on a substrate, a surface layer including a hydrophilic silane disposed on the hard coat layer, and other optional layers. [Figure 2] 1 is a schematic cross-sectional view of an exemplary article including a hydrolysis and condensation hard coat layer disposed on a substrate. DETAILED DESCRIPTION OF THE INVENTION

[0005] In one embodiment, a hard coat coating composition is described. The hard coat coating composition has the formula R 1 Si(OR)3 (wherein R and R 1 is methyl or ethyl). Thus, the first hydrophobic silane monomer is methyltrimethoxysilane, ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, and combinations thereof. In some embodiments, the first hydrophobic silane is methyltrimethoxysilane, methyltriethoxysilane, or combinations thereof. The classification of alkoxysilane monomers as hydrophobic or hydrophilic is typically determined by the presence of R 1 It is based on the R 1 Alkoxysilane monomers where is alkyl are considered hydrophobic.

[0006] In some embodiments, the hardcoat composition comprises a first silane monomer as described immediately above and a silane monomer of formula (R 2 ) 4-m Si(OR) m or Si(OR) (wherein R and R 2 is an organic group, where R 2 is not methyl or ethyl, and m is 1, 2, or 3, more typically 2 or 3.

[0007] Thus, the second silane monomer is a different silane monomer than the first silane monomer. 2The second silane monomer is also hydrophobic, such as when R is a hydrocarbon group having at least 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 carbon atoms. 2 R has up to 30, 28, 26, 24, 22, or 20 carbon atoms. 2 may be linear, branched, or cyclic. Typically, R 2 is aliphatic, such as when it is alkyl, alkenyl, or alkynyl. Aliphatic groups may optionally contain heteroatoms (e.g., oxygen, nitrogen, or sulfur). Alternatively, R 2 may contain aromatic groups.

[0008] Representative second monomers include, for example, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane.

[0009] In some embodiments, the second monomer is (R 2 ) 4-m Si(OR) m (In the formula, R and m are as defined above, and R 2 contains a group reactive with hydroxyl, such as an epoxy silane. Suitable epoxy silanes for use herein include, but are not limited to, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane; (3-glycidoxypropyl)trimethoxysilane; (3-glycidoxypropyl)triethoxysilane; and mixtures thereof.

[0010] In some embodiments, the second monomer is Si(OR) 4 , a tetraalkoxysilane, such as tetraethyl orthosilicate (“TEOS”), and oligomeric forms of tetraalkoxysilane.

[0011] When a second monomer is present, the weight ratio of the first silane monomer to the second silane monomer is at least 4:1. In typical embodiments, the weight ratio of the first silane monomer to the second silane monomer is at least 5:1, 6:1, 7:1, 8:1, or 9:1. In other words, the first silane monomer is at least 80, 81, 82, 83, 84, 85, 86, 87, 88, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by weight of the total of the first and second silane monomers. Thus, the second silane monomer is no more than 20% by weight of the total of the first and second silane monomers. In some embodiments, the total amount of the second silane monomer is no greater than 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 weight percent of the total of the first and second silane monomers.

[0012] The hard coat composition optionally, but preferably, further comprises silica nanoparticles. The inclusion of silica nanoparticles can improve durability and increase pencil hardness compared to the same hard coat without silica nanoparticles. The nanoparticles have an average primary particle size of less than 1 micron. In typical embodiments, the silica nanoparticles have an average primary particle size of 750, 500, 250, 200, 150, or 100 nm or less. In preferred embodiments, the silica nanoparticles have an average primary particle size of 75, 50, 25, 20, 15, or 10 nm or less. The term "primary particle size" refers to the average size of a single, unagglomerated particle of silica. The average particle size may be measured using a transmission electron microscope. The silica particles may be spherical or non-spherical and are typically discrete particles rather than aggregates.

[0013] The silica particles typically have a narrow particle size distribution, i.e., a polydispersity (i.e., particle size distribution) of 2.0 or less, preferably 1.5 or less. If desired, larger silica particles may be added, provided that the presence of the larger particles does not reduce the coatability of the hard coat composition or reduce the stability of the hard coat coating composition.

[0014] In some embodiments, the silica nanoparticles are not surface-modified.Smaller nanoparticles having an average particle size of less than 20, 15, or 10 nanometers can be used to prepare hard coat compositions with good stability and durability without surface modification.Larger silica nanoparticles, i.e., 20 nm or larger, preferably have a surface treatment.

[0015] In some embodiments, the silica nanoparticles are surface-modified with a first or second silane monomer as described above. In some embodiments, the surface treatment includes a second monomer in which R is an epoxy group. In other embodiments, the surface treatment includes a second monomer in which R is an amine group, as described in WO 2015 / 088808, which is incorporated herein by reference.

[0016] The method for producing a hardcoat coating composition generally comprises: The method includes: i) combining the first hydrophobic silane monomer and an optional second silane monomer in an aqueous solution; ii) adding 10% to 30% by weight of silica nanoparticles to the aqueous solution; and iii) adding, preferably, 10% to 30% by weight of silica nanoparticles to the aqueous solution, and hydrolyzing and condensing the first hydrophobic silane monomer and the optional second silane monomer, thereby forming a polysiloxane continuous network. In some embodiments, steps iii) and iv) are performed before step ii).

[0017] The aqueous solution comprises water and preferably a high-boiling organic solvent, such as 1-methoxy-2-propanol. The boiling point of the solvent is typically at least 80, 90, 100, 110, or 120° C. In the absence of such a solvent, the cured coating surface is uneven, typically uneven in thickness, and exhibits other coating defects.

[0018] In some embodiments, non-aqueous silica sols (also called silica organosols) in which the liquid phase is primarily an organic solvent may be used in the method for producing a hard coat composition. However, in typical embodiments, the silica nanoparticles utilized in the method are dispersions of submicron-sized silica nanoparticles in an aqueous liquid phase, optionally containing an organic solvent mixture. Inorganic silica sols in aqueous media are known in the art and are commercially available. Silica sols in water or water-alcohol solutions are commercially available under the trade name NALCO from Nalco Water, Naperville, IL. One useful silica sol is NALCO™ 1130, a silica sol with an average particle size of 8 nanometers, a pH of 10.5, and a solids content of 30% by weight. Other commercially available silica nanoparticles suitable for use in the present invention include NALCO™ 1115, NALCO™ 2326, NALCO™ 2327, and NALCO™ 2329.

[0019] Hardcoat coating compositions generally contain sufficient acid to provide a pH of 6 or less than 5. In some embodiments, it has been found that the pH of the coating composition can be adjusted to a pH of 5-6 after lowering the pH to less than 5. This allows for coating pH-sensitive substrates. Sodium-stabilized silica nanoparticles are typically first acidified before diluting with an organic solvent such as ethanol. Dilution before acidification can result in insufficient or uneven coating. Ammonium-stabilized silica nanoparticles can generally be diluted and acidified in any order.

[0020] Hardcoat coating compositions typically contain a (e.g., weaker) acid with a pKa >4, such as acetic acid. In some embodiments, hardcoat coating compositions typically contain a (e.g., weaker) acid with a pKa >4 in combination with a stronger acid with a pKa (H2O) of ≦3.5, <2.5, or less than 1. Useful acids include both organic and inorganic acids, and can be exemplified by oxalic acid, citric acid, H2SO3, H3PO4, CF3CO2H, HCl, HBr, HI, HBrO3, HNO3, HClO4, H2SO4, CH3SO3H, CF3SO3H, CF3CO2H, and CH3SO2OH. Mixtures of organic and inorganic acids can be utilized. In some embodiments, the weight ratio of the stronger acid (e.g., nitric acid) to the weaker acid (e.g., acetic acid) is 5:1, 4:1, 3:1, 2:1, or less than 1:1.

[0021] Acidified silica nanoparticle hard coat coating compositions can be coated directly onto hydrophobic organic and inorganic substrates without the use of either organic solvents or surfactants. The wetting properties of these inorganic nanoparticle aqueous dispersions on hydrophobic surfaces, such as polyethylene terephthalate ("PET") or polycarbonate ("PC"), are a function of the pH of the dispersion and the pKa of the acid. Hard coat coating compositions typically bead (i.e., pop) on organic substrates at neutral or basic pH.

[0022] The hydrolysis and condensation hard coat composition typically comprises silica nanoparticles dispersed in a continuous gelled polysiloxane network. As used herein, the term "continuous" refers to covering the surface of the substrate substantially without discontinuities or gaps in the areas where the hydrolysis and condensation hard coat composition is applied.

[0023] To uniformly coat a hard coat composition onto a hydrophobic substrate from an aqueous system, it may be desirable to increase the surface energy of the substrate and / or decrease the surface tension of the coating composition. Surface energy can be increased by oxidizing the substrate surface using corona discharge, actinic radiation, or flame treatment methods prior to coating. These methods can also improve adhesion of the coating to the substrate. Other methods that can increase the surface energy of an article include the use of an organic polymer primer, such as a thin coating of polyvinylidene chloride (PVDC). Alternatively, the surface tension of the coating composition can be decreased by the addition of a lower alcohol (C1-C8). In some embodiments, it may be beneficial to add a wetting agent, such as a surfactant, to the hard coat composition.

[0024] As used herein, the term "surfactant" describes a molecule that contains hydrophilic (polar) and hydrophobic (non-polar) regions on the same molecule, and can reduce the surface tension of the coating solution. Useful surfactants include anionic surfactants, cationic surfactants, and nonionic surfactants, such as those described in U.S. Patent No. 6,040,053 (Scholz et al.) and U.S. Patent No. 10,316,212 (Jing et al.), which are incorporated herein by reference, as well as silicone surfactants, such as those commercially available from BYK under the trade name BYK-333, and DOWSIL (trademark) Q2-5211, a silicone polyether copolymer available from Dow.

[0025] In some embodiments, the surfactant is included in the hardcoat coating composition at a concentration of at least 0.5, 1, 1.5, or 2% by weight of the aqueous hardcoat coating composition. In typical embodiments, the amount of surfactant is 5% or less by weight of the aqueous hardcoat coating composition.

[0026] Other useful wetting agents include polyethoxylated alkyl alcohols (e.g., BRIJ™ 30 and BRIJ™ 35 from ICI Americas, Inc., and TERGITOL™ TMN-6™ Specialty Surfactant from Union Carbide Chemical and Plastics Co.), polyethoxylated alkyl phenols (e.g., TRITON™ X-100 from Union Carbide Chemical and Plastics Co., ICONOL™ NP-70 from BASF Corp.), and polyethylene glycol / polypropylene glycol block copolymers (e.g., BASF Chemical and Plastics Co., ICONOL™ NP-70, all from BASF Corp.). Examples of suitable wetting agents include TETRONIC™ 1502 block copolymer surfactant, TETRONIC™ 908 block copolymer surfactant, and PLURONIC™ F38 block copolymer surfactant manufactured by PLURONIC Corp. When present, such wetting agents are used in amounts of less than 0.1 wt. % of the coating composition, preferably 0.003 wt. % to 0.05 wt. % of the coating composition, depending on the amount of silica nanoparticles. It may be desirable to rinse or soak the coated article in water to remove excess surfactant or wetting agent.

[0027] The hard coat layer alone or in combination with the surface layer containing the hydrophilic silane may have a glossy or matte surface. A matte surface typically has a lower transmittance and a higher haze value than a glossy surface. For example, the haze is generally at least 5%, 6%, 7%, 8%, 9%, or 10% as measured according to ASTM D1003. A glossy surface typically has a gloss value of at least 90 or 95 as measured at 60° according to ASTM D 2457-03, while a matte surface has a gloss value of less than 85, 80, 70, 65, 60, 55, 50, 45, or 40. In some embodiments, the gloss value of the matte surface is at least 20 or 30.

[0028] Matte surfaces can hide imperfections such as scratches and contaminants such as dirt, smudges, fingerprints, etc. Another benefit of having a matte surface is that it makes them more visually appealing. Furthermore, the delicate feel and friction of a matte surface creates the sensation of writing on traditional paper.

[0029] The hard coat layer alone or in combination with a surface layer can be made matte using a variety of known techniques. In some embodiments, the surface can be roughened or textured to provide a matte surface by embossing the surface with a suitable bead-blasted or otherwise roughened tool and curing the composition against a suitable roughened master or removable liner.

[0030] In other embodiments, the hard coat composition may comprise matte particles of a suitable size, such as silica, glass beads, or organic polymer beads, such as polyethylene (PE), polystyrene (PS), or polymethyl methacrylate (PMMA). In some embodiments, the organic polymer beads have a density of about 1 g / cm. 3 (e.g., = ±0.1 g / cm 3 Such matte particles typically have an average particle size ranging from about 1 to 10 microns. In some embodiments, the size of the matte particles is at least 2 or 3 microns and no more than 4 or 5 microns. Furthermore, the concentration of such matte particles may range from at least 2% by weight to about 5% by weight or more.

[0031] See Table 22 in the Examples section below. Organic polymer beads may be a preferred particle for matte surfaces in terms of removability. Matte samples containing polymer beads larger than the thickness of the dried and cured hard coat exhibited varying levels of ghosting that was impossible to remove with water. In contrast, samples with 3 μm beads resulted in complete and easy removal. The amount of ghosting decreased with decreasing average particle size, and ghosting was reduced when the matting agent particle size was similar to the thickness of the dried and cured hard coat. Scanning electron microscopy showed that particles larger than the hard coat thickness were exposed to air and not completely covered by the polysiloxane hard coat. This resulted in weak or no bond between the exposed portions and the upper silane layer, allowing ink to come into direct contact with the polymer beads, making removal extremely difficult. If the matte particles have an average particle size of 6 microns and the dried and cured hard coat has an average thickness of 3 microns, the average particle size is twice (i.e., 2X) the average thickness of the dried and cured hard coat. In preferred embodiments, the average particle size of the matte particles is less than (in other words, about equal to) 2X, 1.9X, 1.8X, 1.7X, 1.6X, 1.5X, 1.4X, 1.3X, 1.2X, 1.1X, or 1X the average particle size of the matte particles.

[0032] The aqueous hard-coat coating compositions described herein and illustrated by the examples are storage stable for 3 months at room temperature (25° C.) or 1 month at 50° C. The aqueous hard-coat coating compositions do not gel, opacify, or otherwise significantly deteriorate.

[0033] The hard coat coating composition is preferably coated onto the article using conventional techniques such as bar, roll, curtain, rotogravure, spray, or dip coating techniques. To ensure uniform coating and film wetting, it may be desirable to increase the surface energy by oxidizing the substrate surface or applying a primer before coating, as described above. The aqueous hard coat coating composition is applied at a uniform average thickness that varies less than 20 nm, more preferably less than 10 nm, to avoid visible interference color variations in the coating.

[0034] The hydrolysis and condensation hard coat composition typically has an average thickness ranging from at least 1, 2, or 3 microns to a maximum of 10 microns. More typically, the thickness of the hydrolysis and condensation hard coat composition is 9, 8, 7, 6, or 5 micrometers or less. The mechanical properties of the hard coat can improve with increasing thickness. However, the flexibility of the hard coat can also decrease with increasing thickness. The thickness of the hard coat can be measured using an ellipsometer, such as a Gaertner Scientific Corp. Model No. L115C ellipsometer.

[0035] If desired, the hardcoat coating can be coated on both sides of the substrate, or (not shown), the hardcoat coating can be coated on one side of the substrate, as shown in FIG.

[0036] Once coated, the substrate is typically dried and heat cured in a recirculating oven at temperatures between 90°C and 150°C. An inert gas may be circulated. Depending on the substrate, the temperature may be further increased to accelerate the drying process.

[0037] The hard coat coating composition itself provides a tough, abrasion-resistant layer that protects the substrate from damage caused by scratches, abrasion, solvents, etc. Although the hydrolysis and condensation hard coat composition alone can provide a rewritable or anti-fog surface, in a preferred embodiment, a surface layer containing a hydrophilic silane is disposed on the hydrolysis and condensation hard coat composition. Advantageously, ghosting from permanent marker writing and dry-erase markers can be more easily removed with water from the surface layer containing the hydrophilic silane.

[0038] The hydrophilic silane surface layer can be applied in a monolayer thickness and can be as thick as 10 microns. The hydrophilic silane surface layer typically has a thickness of 9, 8, 7, 6, 5, 4, 3, 2, or 1 micron or less.

[0039] Most of the -OH groups formed during hydrolysis are crosslinked by the acid of the hardcoat coating composition, but the cured hardcoat layer may contain some -OH groups on the surface that can covalently bond with hydrophilic silanes in the surface layer to form siloxane (Si-O-Si) bonds.

[0040] In some embodiments, the hydrophilic silane of the surface layer comprises a non-zwitterionic sulfonate-organosilanol compound, such as those disclosed in U.S. Pat. Nos. 4,152,165 (Langager et al.) and 4,338,377 (Beck et al.).

[0041] In some embodiments, the non-zwitterionic sulfonate-organosilanol compounds used in the solutions and compositions of the present invention have the following formula (I): [ka] [In the formula, each Q is independently selected from hydroxyl, an alkyl group containing 1 to 4 carbon atoms, and an alkoxy group containing 1 to 4 carbon atoms; M is selected from hydrogen, alkali metals, and organic cations of strong organic bases having an average molecular weight of less than 150 and a pKa greater than 11; X is an organic linking group; Y is selected from the group consisting of hydrogen, alkaline earth metals (e.g., magnesium, calcium, etc.), organic cations of protonated weak bases having an average molecular weight of less than 200 and a pKa of less than 11 (e.g., 4-aminopyridine, 2-methoxyethylamine, benzylamine, 2,4-dimethylimidazole, 3-[2-ethoxy(2-ethoxyethoxy)]propylamine), alkali metals, and organic cations of strong organic bases having an average molecular weight of less than 150 and a pKa of greater than 11 (e.g., + N(CH3)4, + N(CH2CH3)4), with the proviso that when Y is selected from hydrogen, alkaline earth metals, and organic cations of the protonated weak bases, M is hydrogen; r is equal to the valence of Y, n is 1 or 2. It has.

[0042] Preferably, the non-zwitterionic compound of formula (I) is an alkoxysilane compound (eg, where Q is an alkoxy group containing 1 to 4 carbon atoms).

[0043] The weight percentage of oxygen in these compounds of formula (I) is at least 30%, preferably at least 40%. Most preferably, it is in the range of 45% to 55%. The weight percentage of silicon in these compounds is 15% or less. Each of these percentages is based on the weight of the compound in its acid form, free of water.

[0044] The organic linking group X in formula (I) is preferably selected from an alkylene group, a cycloalkylene group, an alkyl-substituted cycloalkylene group, a hydroxy-substituted alkylene group, a hydroxy-substituted monooxaalkylene group, a divalent hydrocarbon group having a monooxa skeletal substitution, a divalent hydrocarbon group having a mono-thia skeletal substitution, a divalent hydrocarbon group having a monooxa-thia skeletal substitution, a divalent hydrocarbon group having a dioxo-thia skeletal substitution, an arylene group, an arylalkylene group, an alkylarylene group, and a substituted alkylarylene group. Most preferably, X is selected from an alkylene group, a hydroxy-substituted alkylene group, and a hydroxy-substituted monooxaalkylene group.

[0045] Suitable examples of non-zwitterionic compounds of formula (I) are described in U.S. Pat. Nos. 4,152,165 (Langager et al.) and 4,338,377 (Beck et al.), and include, for example, the following: (HO)3Si-CH2CH2CH2-O-CH2-CH(OH)-CH2SO3 - H + , (HO)3Si-CH2CH(OH)-CH2SO3 - H + , (HO)3Si-CH2CH2CH2SO3 - H + , (HO)3Si-C6H4-CH2CH2SO3 - H + , (HO)2Si-[CH2CH2SO3 - H + ]2, (HO)-Si(CH3)2-CH2CH2SO3 - H + , [ka] , and (HO)3Si-CH2CH2SO3 - K + .

[0046] In some embodiments, the surface layer comprises a zwitterionic silane. Examples of zwitterionic sulfonate-functional compounds include those disclosed in U.S. Pat. No. 5,936,703 (Miyazaki et al.) and WO 2007 / 146680 and WO 2009 / 119690.

[0047] In some embodiments, the zwitterionic sulfonate-organosilanol compound has the following formula (II): [ka] [In the formula, Each R 1 are independently hydrogen, a methyl group, or an ethyl group; Each R 2 are independently a methyl group or an ethyl group, Each R 3 and R 4 are independently saturated or unsaturated, linear, branched, or cyclic organic groups, which may optionally be joined together with atoms of the W group to form a ring; W is an organic linking group; p and m are integers of 1 to 3, q is 0 or 1; p+q=3] It has.

[0048] The organic linking group W in formula (II) is preferably selected from saturated or unsaturated, linear, branched, or cyclic organic groups. The linking group W is preferably an alkylene group that may contain a carbonyl group, a urethane group, a urea group, a heteroatom such as oxygen, nitrogen, and sulfur, or a combination thereof. Examples of suitable linking groups W include alkylene groups, cycloalkylene groups, alkyl-substituted cycloalkylene groups, hydroxy-substituted alkylene groups, hydroxy-substituted monooxaalkylene groups, divalent hydrocarbon groups with mono-oxa skeletal substitutions, divalent hydrocarbon groups with mono-thia skeletal substitutions, divalent hydrocarbon groups with monooxo-thia skeletal substitutions, divalent hydrocarbon groups with dioxo-thia skeletal substitutions, arylene groups, arylalkylene groups, alkylarylene groups, and substituted alkylarylene groups.

[0049] Suitable examples of zwitterionic compounds of formula (II) are described in U.S. Pat. No. 5,936,703 (Miyazaki et al.) and WO 2007 / 146680 and WO 2009 / 119690, and include the following zwitterionic functional groups (-WN + (R 3 )(R 4 )-(CH2) m -SO3 - ) are listed. [ka]

[0050] In some embodiments, the zwitterionic silane has the following formula (III): [ka] [In the formula, Each R 1 are independently hydrogen, a methyl group, or an ethyl group; Each R 2 are independently a methyl group or an ethyl group, p and m are integers of 1 to 3, q is 0 or 1; p+q=3] It is a sulfonate-organosilanol having the formula:

[0051] Suitable examples of zwitterionic compounds of formula (III) are described in U.S. Pat. No. 5,936,703 (Miyazaki et al.), e.g., (CH3O)3Si-CH2CH2CH2-N + (CH3)2-CH2CH2CH2-SO3 - , and [ka] Examples include:

[0052] Other examples of suitable zwitterionic compounds include: [ka] Examples include:

[0053] Other hydrophilic functional groups suitable for silanes include, but are not limited to, phosphonate, carboxylate, gluconamide, sugar, polyvinyl alcohol, and quaternary ammonium.

[0054] Aqueous hydrophilic silane coating compositions typically contain one or more hydrophilic silane compounds in an amount of at least 0.1, 0.5, or 1 wt %, based on the total weight of the coating solution. Hydrophilic silane coating compositions typically contain hydrophilic silane compounds in an amount of no more than 10, 9, 8, 7, 6, or 5 wt %, based on the total weight of the coating composition. Generally, for a monolayer coating thickness, a relatively dilute coating composition is used. In some embodiments, a more concentrated coating composition can be used. In some embodiments, the surface can be subsequently rinsed to remove excess hydrophilic silane.

[0055] The hydrophilic silane coating composition preferably comprises an alcohol, water, or a hydroalcoholic solution (i.e., an alcohol and / or water). Typically, such alcohols are lower alcohols (e.g., C1-C8 alcohols, more typically C1-C4 alcohols), such as methanol, ethanol, propanol, and 2-propanol. Preferably, the hydrophilic functional coating composition is an aqueous solution. As used herein, the term "aqueous solution" refers to a solution containing 50% or more by weight of water. Such solutions may use water as the only solvent or may use a combination of water with an organic solvent, such as an alcohol or acetone. Organic solvents may also be included in the hydrophilic treatment composition to improve the freeze-thaw stability of the hydrophilic treatment composition. Typically, the hydrophilic silane coating composition is a dilution containing at least 90% by weight of an aqueous solution.

[0056] The hydrophilic silane coating composition may be acidic, basic, or neutral. The hydrophilic silane coating composition may optionally include surfactants and wetting agents as described above.

[0057] In some embodiments, the hydrophilic silane coating composition optionally further comprises a tetraalkoxysilane (e.g., tetraethyl orthosilicate (“TEOS”)), oligomers thereof; and / or a silicate, such as an alkyl polysilicate (e.g., poly(diethoxysiloxane)), lithium silicate, sodium silicate, potassium silicate, or a combination thereof, which can provide improved durability.

[0058] When present, such components are typically present in amounts less than the aforementioned hydrophilic zwitterionic silane or non-zwitterionic silane. In some embodiments, the weight ratio of hydrophilic (e.g., zwitterionic silane or non-zwitterionic silane) to silicate is at least 1:1, 2:1, or 3:1.

[0059] The hydrophilic silane coating may optionally contain a water-soluble polymer having hydroxyl groups. In the presence of acid, the hydroxyl groups on these polymers can condense to form a water-insoluble coating. The hydroxyl groups can also react with the silanol groups on the silica nanoparticle hard coat. Suitable hydrophilic polymers having hydroxyl groups include, but are not limited to, polyvinyl alcohol, hydroxymethyl cellulose, hydroxyethyl cellulose, dextran, guar gum, and mixtures thereof. When present, such water-soluble polymers having hydroxyl groups are typically present in amounts less than the hydrophilic zwitterionic silane or non-zwitterionic silane, as described above.

[0060] The hydrophilic silane coating composition typically contains at least 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100 weight percent solids of a hydrophilic zwitterionic silane or non-zwitterionic silane, as described above.

[0061] The hydrophilic silane coating composition can be coated onto the cured hardcoat layer using conventional techniques such as bar, roll, curtain, rotogravure, spray, wipe or dip coating techniques. Preferred methods include spray, bar and roll coating.

[0062] After coating, the hydrophilic functional article is typically dried in a recirculating oven at temperatures between 30°C and 200°C. An inert gas may be circulated. Depending on the heat resistance of the substrate, the temperature may be further increased to accelerate the drying process. Drying drives a condensation reaction between the hydrophilic coating and the -OH groups on the surface of the hard coat layer.

[0063] Referring to Figure 2, the article described herein includes a hardcoat layer 13, as described above, disposed on a surface of a substrate 15. Substrates for dry erase surfaces can include, for example, glass, porcelain steel, painted steel, painted metal, painted hardboard, melamine, coated films, coated paper, and coated fiberboard sheets. In an exemplary embodiment, the substrate comprises an organic polymer material. The organic polymer substrate may comprise a polymer sheet, film, or molding compound.

[0064] In some preferred embodiments, and referring to FIG. 1 , the articles described herein include a hardcoat layer 13, as described above, disposed on a surface of a substrate 15, and a surface layer 14 disposed on a major surface 16 of the hydrolyzed and cured hardcoat layer.

[0065] A hard coat in combination with a hydrophilic surface layer increases the hydrophilicity of the substrate. As used herein, the term "hydrophilic" refers to a surface that is wetted by an aqueous solution, and does not describe whether the layer absorbs the aqueous solution. A surface is called "hydrophilic" if a drop of water or an aqueous solution exhibits a static water contact angle of less than 50°. A hydrophobic substrate has a water contact angle of 50° or greater.

[0066] In some embodiments, the substrate of the rewritable or anti-fog article may be transparent or translucent to visible light, where transparent means transmitting at least about 85% of incident light within the visible spectrum (wavelengths from about 400 to about 700 nm).

[0067] The substrate used herein can be flexible or inflexible as desired. Illustrative examples of suitable substrates include polyesters (e.g., polyethylene terephthalate, polybutylene terephthalate), polyacrylates such as polycarbonate, allyl diglycol carbonate, polymethyl methacrylate, polystyrene, polysulfone, polyethersulfone, homoepoxy polymers, epoxy addition polymers with polydiamines, polydithiols, polyethylene copolymers, fluorinated surfaces, cellulose esters such as acetate and butyrate, glass, ceramic, porcelain, coated paper, metals, organic and inorganic composite surfaces, and the like, including blends and laminates thereof.

[0068] In other embodiments, the substrate may be colored or opaque. The composition has been found to provide an easily cleanable surface for substrates such as flexible films used in label applications. Flexible films can be made from polyesters such as PET, or polyolefins such as PP (polypropylene), PE (polyethylene), and PVC (polyvinyl chloride). The substrate can be formed into a film using conventional film-making techniques, such as extrusion of the substrate resin into a film and optional uniaxial or biaxial orientation of the extruded film. The substrate can be treated to improve adhesion between the substrate and the hard-coat coating, for example, using chemical treatment, corona treatment such as air or nitrogen corona, plasma, flame, or actinic radiation. If desired, an optional tie layer (not shown) can also be applied between the substrate and the hard-coat coating composition to enhance interlayer adhesion. The other major surface of substrate 22 can also be treated using the treatments described above to improve adhesion between the substrate and (e.g., pressure-sensitive) adhesive layer 18 temporarily covered by release liner 20. Major surface 22 of substrate 15 in FIG. 2 may also include such an adhesive layer and release liner layer. The substrate may be provided with graphics such as words or symbols known in the art.

[0069] In yet other embodiments, the substrate may be metallic or may have a metallic surface (eg, vapor-deposited metal), such as aluminum or stainless steel.

[0070] In some embodiments, articles having an anti-fog surface are described. Exemplary articles include medical and non-medical protective eyewear, including eyeglasses, goggles, face masks, face shields, and respirators, as well as mirrors, motor vehicle windows, and windshields.

[0071] In some embodiments, articles having rewritable surfaces are described. Exemplary articles include dry erase boards and films, file folders, labels, name tags, notebook covers and dividers, tabs for attaching files, and the like.

[0072] The dry erase article may further include other optional elements such as a frame, a means for storing materials and tools such as a writing implement, an eraser, a cloth, scratch paper, a handle for carrying, a protective cover, a means for hanging on a vertical surface, an easel, etc.

[0073] In some embodiments, the article (eg, label dry erase film) may further include a (eg, pressure-sensitive) adhesive coating on the backside of the substrate and a release liner.

[0074] In another embodiment, a method of using an article having a rewritable surface is described, the method comprising providing an article comprising a substrate, a hydrolysis and condensation hard coat described herein, and a surface layer preferably comprising a hydrophilic silane; writing on the rewritable surface layer with a (e.g., oil-based or dry-erase) marker; and removing the writing. In some embodiments, removing the writing comprises wiping the rewritable surface with an eraser, cloth, or paper towel. As used herein, "wiping" refers to gently wiping, typically by hand, with, for example, a tissue, paper towel, or cloth, without much pressure (e.g., generally 800 grams or less), with one or more strokes or rubbing (typically only a few strokes are required). In some embodiments, removing further comprises applying an aqueous cleaning solution, optionally containing an organic solvent, to the rewritable surface layer. The aqueous cleaning solution may comprise a cationic, anionic, or / and nonionic surfactant known in the art.

[0075] The rewritable surface of the dry erase article exhibits excellent writability with conventional dry erase markers and permanent markers. Importantly, permanent marker writing and ghosting can be easily removed from the hydrophilic silane surface layer by wiping with water.

[0076] The hard coat layers described herein are also suitable for other articles such as coatings for (e.g., flexible) electronics, including insulating layers (e.g., dielectric coatings) and protective coatings and films for various electronic components such as (e.g., LCD, LED, and OLED) display surfaces and camera and sensor lenses. [Example]

[0077] Unless otherwise stated or readily apparent from the context, all parts, percentages, ratios, etc. in the examples and elsewhere in this specification are by weight.

[0078] [Table 1]

[0079] Test Method Water resistance, mechanical durability, and oil-based marker removal test methods The water resistance test was performed by immersing the sample in water for 3 to 48 hours, during which the water was continuously removed and replenished to evaluate the water resistance.

[0080] After water immersion, coating durability was evaluated by 5,000 cycles of wet reciprocating abrasion testing at 15.0 Newtons using a Taber Industries 5900 Reciprocating Abrader (North Tonawanda, New York, USA). The abrasion cycle speed was 75 cycles / min. The test stroke was 5.1 centimeters long. A 2.5 centimeter button was covered with a Kimberly-Clark L30 or L40 Wypal (Irving, Texas, USA) towel and an abrasion cloth square manufactured by Test Fabrics Inc. (AATCC Crockmeter Standard Rubbing Cloth, West Pittson, Pennsylvania, USA). The square (contacting the coating surface) was wetted with deionized water during the abrasion test. Durability scores are reported as follows: 0 is the best, no scratches at all; 5 is the worst, severe scratches and coating removal.

[0081] After the wet abrasion test (without scratches), the abraded area was marked with a permanent marker (Sharpie black, Oak Brook, Illinois, USA), and the permanent black Sharpie was aged on the surface for 60 hours. The permanent mark removal test was evaluated by gently wiping with a wet Kimwipe tissue. The test sample was considered good if the test area of ​​the sample showed complete removal of scratches and permanent marks and no ghosting.

[0082] Anti-fogging test method Anti-fog tests were performed by immersing film samples in water for one hour. The water was circulated by continuously replenishing with fresh water. After immersion, the film samples were dried overnight at ambient conditions. Each film sample was then exposed to water vapor generated by heating a 500 mL beaker of water to 60°C for one minute and placing the film sample hydrophilic side down against a one-inch round hole in a glass cover placed over the beaker. A good anti-fog sample remained transparent after one minute.

[0083] Preparation example General Procedure for Preparing Polysiloxane Hard Coat Solution Containing Nanosilica-1130 A 25 g dispersion of 1130 (30 wt.% solids) was placed in a screw-cap jar. Acetic acid was added to the dispersion while stirring. MTES was added to the stirred solution, and vigorous stirring was continued at room temperature for 24 to 72 hours. 1-Methoxy-2-propanol was then added to the solution. Various ratios of 1130 to MTES were utilized, as shown in Table 1. The solutions contained 2 wt.% BYK-UV 3500 surfactant to improve the coatability of the silicone hardcoat solution on specific substrates (0.02 grams of BYK-UV 3500 was added to each 10 gram solution).

[0084] [Table 2]

[0085] General Preparation Procedure for Polysiloxane Hard Coat, 2 Steps 1) Pre-hydrolysis of methyltriethoxysilane [MTES / H2O(1 / 6)] A jar with a screw-on cap was charged with the desired amounts of MTES, 5 wt. % acetic acid solution, and 1 wt. % nitric acid, as shown in Table 2. The molar ratio of MTES to water was 1:6 (30.288 g of dilute acid per 50 g of MTES), and the solution was designated MTES / HO (1 / 6). The resulting MTES solution was stirred, and the silanes were hydrolyzed at ambient conditions for the times shown in Table 2 to form silanols and oligomers.

[0086] [Table 3]

[0087] 2) Preparation of 20 nm size (3-glycidoxypropyl)trimethoxysilane modified 2327 Five grams of (3-glycidoxypropyl)trimethoxysilane (GPTMS) was added to 250 grams of aqueous 2327 solution dispersion (40%), and the solution was stirred overnight at 60°C in a screw-cap jar. After reaction, the GPTMS-modified 2327 solution was cooled to room temperature, and 150 grams of 1-methoxy-2-propanol (1M2P) was added to the modified particle solution while stirring. The final weight ratio of GPTMS:2327:1M2P was equal to 5:250:150. The final GPTMS-modified 2327 (designated 2327-epoxy) was 25% by weight in the water / 1-methoxy-2-propanol mixture.

[0088] General procedure for preparing polysiloxane hard coat solutions containing 20 nm nanosilica-2327 (2327-A, 2327-B, 2327-C) To prepare a polysiloxane hardcoat solution containing 2327 dispersion (40 wt% solids, 24 grams), a screw-cap jar was charged with the prehydrolyzed methyltriethoxysilane solution and the (3-glycidoxypropyl)trimethoxysilane-modified 2327 solution in the weight ratios shown in Table 3 below. The solution contained 2 wt% BYK-UV 3500 surfactant to improve the coatability of the silicone hardcoat solution on certain substrates. (0.02 grams of BYK-UV 3500 was added to each 10 gram solution.)

[0089] [Table 4]

[0090] Preparation of Zwitterionic Silane / LSS-35 Hydrophilic Topcoat Aqueous Solution A screw-cap jar was charged with 18.46 grams of zwitterionic silane (45.5 wt%), 16.36 grams of LSS-75 (22 wt%), and 365.18 grams of deionized water. The weight ratio of zwitterionic silane to LSS-75 was 70:30, with a total weight percentage of 3 wt%. The hydrophilic top coating solution was 3% ZS / LSS (70 / 30).

[0091] Preparation of aqueous zwitterionic silane topcoat solutions To an aqueous solution of 26.37 grams of zwitterionic silane (45.5 wt %), 373.63 grams of deionized water was added to dilute the silane solution to a 3 wt % aqueous solution, designated 3% ZS.

[0092] Preparation of Hydrophilic Silicone Hard Coat Films, Method I Each polysiloxane hard coat solution was coated onto Mitsubishi film using a No. 12 Mayer Rod, and the resulting coating was thermally cured at 140°C for 5 minutes. The dried hard coat had a thickness of 3-4 microns. The cured silicone hard coat was corona treated using an ETP BD-20AC Laboratory Corona Treater (Electro-Technic Products, Chicago, IL, USA). The 3% ZS / LSS (70 / 30) solution prepared above was then coated onto the corona-treated polysiloxane hard coat using a No. 3 Mayer Rod and dried at 140°C for 5 minutes. The dried surface layer had a thickness of 0.5-1 micron.

[0093] Preparation of Hydrophilic Silicone Hardcoat Films, Method II Each polysiloxane hard coat solution was coated onto Mitsubishi film using a #12 Mayer Rod, and the resulting coating was thermally cured at 140°C for 5 minutes. The dried hard coat had a thickness of 3-4 microns. The cured silicone hard coat was corona treated using an ETP BD-20AC Laboratory Corona Treater. The 3% ZS prepared above was then coated onto the corona-treated polysiloxane hard coat using a #3 Mayer Rod and dried at 140°C for 5 minutes. The dried surface layer had a thickness of 0.5-1 micron.

[0094] Preparation of Hydrophilic Silicone Hardcoat Films, Method III Film-coated rolls were prepared using a Yasui Seiki conventional roller coater (YS Coater) (Bloomington, IN, USA) with a 6-inch wide die. The corona treater was obtained from Pillar Technologies, Hartland, Wisconsin, USA, had a 7-inch width, and was nitrogen purged. The coating parameters are shown in Table 4.

[0095] The polysiloxane hard coat was coated and cured through a YS coater, and the hydrophilic top layer was coated and cured through a YS coater onto the nitrogen corona treated polysiloxane hard coat.

[0096] [Table 5]

[0097] Examples / Comparative Examples EX-1~3 Polysiloxane solutions 1130-A, 1130-B, and 1130-C were separately coated onto Mitsubishi PET film with a #12 Meyer bar and heat cured for 5 minutes, as listed in Table 1. The samples were corona treated and then topcoated with the zwitterionic silane / LSS-35 hydrophilic solution shown in Table 5 and dried at 140°C for 5 minutes. The example films were evaluated separately based on their mechanical durability and Sharpie removal performance, all on the same test spot.

[0098] [Table 6]

[0099] Examples EX-4 to EX-6 The examples were the same as those described in Examples EX-1 to EX-3, except that the hydrophilic topcoat was a 3 wt % ZS solution in water.

[0100] [Table 7]

[0101] The films of Examples EX-1-3 showed easier removal of Sharpie marks by gently wiping with a wet Kimwipe tissue when compared to Examples EX-4-6.

[0102] Examples EX-7 to EX-9 Polysiloxane solutions 2327-A, 2327-B, and 2327-C were separately coated onto Mitsubishi PET film with a #12 Meyer bar and heat cured for 5 minutes, as described in Table 3. The samples were corona treated and then topcoated (Method I) with the zwitterionic silane / LSS-35 hydrophilic solution shown in Table 7 and dried at 140°C for 5 minutes. The example films were separately evaluated for mechanical durability and Sharpie removal performance according to the test methods described above.

[0103] [Table 8]

[0104] Examples EX-10 to EX-12 The examples were the same as those described in Examples EX-7 to EX-9, except that the hydrophilic topcoat was a 3 wt % ZS solution in water.

[0105] [Table 9]

[0106] Anti-fogging experiments for Examples EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D) Polysiloxane hardcoats EX-1 to EX-3 and EX-7 to EX-9 were prepared by adding DISPERBYK-185 surfactant (0.01 grams of surfactant per 10 grams of solution) instead of BYK-UV 3500 and were designated EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D). The films of Examples EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D) were evaluated by the method described in the Anti-Fog Test Method.

[0107] The control film was a Mitsubishi PET film (without any coating). The control film fogged up immediately when exposed to hot water vapor at 60° C., while the films of Examples EX-1(D) to EX-3(D) and EX-7(D) to EX-9(D) remained optically clear and no haze formed.

[0108] [Table 10]

[0109] Examples EX-13 to EX-16 Polysiloxane hardcoat solutions 1130-B and 2327-B were coated onto 4 mil Mitsubishi PET by a YS coater at a line speed of 3 ft / min and cured at 140°C by Method III described above. The coated hardcoats were then heated to 1.0 kilowatts (25.83 J / cm). 2 ) or 1.5 kilowatts (38.75 J / cm 2 ), and then the treated side was coated with a 3 wt % ZW / LSS hydrophilic solution at a speed of 5 ft / min and dried at 120°C.

[0110] [Table 11]

[0111] Examples EX-17 to EX-24 Coating solutions containing 1130 were prepared using a one-step procedure. 1130 and MTES were stirred in an acidic environment (acetic acid) for 24 to 72 hours. Particle to silane weight ratios of 1:3, 1:5, and 1:7 were used, optionally including 5% GPTMS or 10% C16 silane. The polysiloxane hardcoat solutions were coated onto 4 mil Mitsubishi PET using a YS coater at a line speed of 3 ft / min and cured at 140°C using Method III described above. The coated hardcoats were then heated at 1.0 kilowatts (25.83 J / cm). 2 ) or 1.5 kilowatts (38.75 J / cm 2 ), and then the treated side was coated with a 3 wt % ZW / LSS hydrophilic solution at a speed of 5 ft / min and dried at 120° C. The example films were evaluated separately based on their mechanical durability (2000 cycles instead of 5000 cycles) and Sharpie removal performance.

[0112] 1130:MTES (1:7) with 5% GPTMS was more viscous and began to gel after 2 months; 1130:MTES (1:7) and 1130:MTES (1:7) with 10% C16 silane also became significantly more viscous after 2 months.

[0113] [Table 12]

[0114] Examples EX-25 to 28 Coating solutions containing 2327 were prepared using a two-step procedure. MTES was hydrolyzed for 5 hours (with the addition of nitric acid "NA") or 3 days (without NA) and then mixed with GPTMS-modified 2327 in 1-methoxy-2-propanol. The particle to silane weight ratios were 1:3, 1:5, and 1:7. The polysiloxane hardcoat solutions were coated onto 4 mil Mitsubishi PET using a YS coater at a line speed of 3 ft / min and cured at 140°C using Method III described above. The coated hardcoats were then heated at 1.0 kilowatts (25.83 J / cm). 2 ) or 1.5 kilowatts (38.75 J / cm 2 ), and then the treated side was coated with a 3 wt % ZW / LSS hydrophilic solution at a speed of 5 ft / min and dried at 120° C. The example films were evaluated separately based on their mechanical durability (2000 cycles instead of 5000 cycles) and Sharpie removal performance.

[0115] [Table 13]

[0116] Smaller particles will work without surface modification, but modification is more favorable for stability, especially at higher concentrations.

[0117] Examples EX-29 to EX-38 This set of examples was prepared using the same method as above and exhibited similar durability and ink removal as the previous examples. However, when a hydrophilic silane was present, the permanent marker was more easily removed with water. Some of Examples 29-38 exhibited dewetting. Surface treating the particles corrected the dewetting problem.

[0118] [Table 14]

[0119] Examples EX-39 to EX-42 A NALCO 1130 dispersion (30 wt%, 100 g) was weighed into a glass jar. While vigorously stirring the solution using a magnetic stirrer, acetic acid was added to the dispersion to adjust the pH to 5-6. Methyltrimethoxysilane was then added to the stirred solution, and the mixture was hydrolyzed for 24-72 hours. After the reaction was complete, 1-methoxy-2-propanol was added to the reacted solution, and the solution was divided into three parts. One part of the solution was left as is, while the other two parts were supplemented with 1 wt% and 2 wt% surfactant (BYK-UV-3500). The resulting siloxane hard coat solution was coated onto a PET substrate and dried at 140°C for 10-15 minutes. Circles were drawn on the cured hard coat surface with various dry-erase and permanent markers. The pen marks were then aged at 50°C for 24 hours, after which a mark removal test was performed.

[0120] [Table 15]

[0121] [Table 16]

[0122] [Table 17]

[0123] [Table 18]

[0124] [Table 19]

[0125] [Table 20]

[0126] Comparative Example Sample Preparation CE-1: Methyltrimethoxysilane (4 g) and ethanol (16 g) were placed in a small glass bottle equipped with a magnetic stir bar and stirred. DI water (0.4 g) and acetic acid were added to the solution to adjust the pH to 5-6. The solution was stirred for 24 hours to complete the hydrolysis. The resulting hydrolyzed solution was coated onto a PET substrate and dried at 140°C for 10 minutes. The cured coating surface was unevenly coated and had many defects.

[0127] The cured coating surface was marked with different dry erase pens and oil-based marker pens. After the inks were dried at room temperature, the marks were removed with a paper towel.

[0128] CE-2: Methyltrimethoxysilane (2.8 g), tetraethoxysilane (TEOS) (1.2%), and ethanol (16 g) were placed in a small glass bottle equipped with a magnetic stir bar and stirred. DI water (0.4 g) and acetic acid were added to the solution to adjust the pH to 5-6. The solution was stirred for 24 hours to complete the hydrolysis. The resulting hydrolysis solution was coated onto a PET substrate and dried at 140°C for 10 minutes. The cured coating surface was unevenly coated and had many defects. The cured coating surface was marked with different dry-erase pens and oil-based marker pens. After the ink dried at room temperature, the marks were removed with a paper towel.

[0129] [Table 21]

[0130] EX-51~EX-56 Solution preparation: Micron-sized polymeric matte particles were added to the 1130-B solution (containing 1 wt. % BYK-UV 3500) at a concentration of 2 wt. % to 5 wt. % total hardcoat solids. The solution was then vigorously agitated using a shear mixer to aid in the dispersion of the matte agent in the hardcoat solution.

[0131] The samples listed in Table 22 were coated onto 4 mil Mitsubishi PET film using a reverse gravure coater to obtain a dried and cured hardcoat thickness of 3.5-4 μm, corona treated, and subsequently topcoated with a zwitterionic silane / LSS-75 (4 / 6, wt% / wt%) hydrophilic solution. All polymeric matting agents were added at 5 wt% hardcoat solids. The sample films were evaluated for Shapie marker erasability with water.

[0132] [Table 22]

[0133] EX-57~EX-58: Varying concentrations of 3 μm PMMA beads were added to the 1130-B solution (containing 1 wt% BYK-UV 3500) at a total solids content of 3% to 5% by weight of the hard coat solution. The solution was then vigorously stirred using a shear mixer to aid in the dispersion of the matting agent in the hard coat solution. The resulting solution was coated using a reverse gravure coater, corona treated, and finally coated with a zwitterionic silane / LSS-75 hydrophilic solution. The matte samples were analyzed for dry erase performance, where 12 of the most commonly used dry erase markers of different brands and colors were selected and evaluated. The samples were cut into 30 cm x 50 cm sheets, and approximately 20 cm lines were drawn using each marker, resulting in 12 different marker lines aligned vertically on each sample. The samples were then placed in a 120°F oven for 48 hours to simulate marker aging at ambient temperature for at least 6 months. Finally, the dry erasability of the different markers was tested using an Expo marker eraser. Each line was erased with 10 passes of the Expo marker eraser under a 2.4 kg weight. The number of passes required for each marker to be completely removed was recorded. A higher total score (maximum is 120) correlates with poorer performance.

[0134] Table 23 shows that the dry erase performance of the samples decreased with decreasing gloss value. Higher concentrations of matting agent increased the roughness of the sample, thereby trapping more ink in the surface valleys and impairing the dry erase removability of the marker. Samples containing 3 wt% MB30X-3 matting agent demonstrated dry erase performance comparable to glossy products (with a score of 43 / 120) while maintaining low glare functionality with a gloss of 53. Reducing the gloss by 10 significantly reduced dry erase removability, increasing the total score to 90 / 120. Typically, dry erase performance is at least 40 and less than 90, 80, or 70.

[0135] [Table 23]

[0136] EX-59~EX-61 Three weight percent of 3 μm polystyrene beads (SSX-3) was added to 1130-B hard coat solution containing 1 weight percent BYK-UV3500. The resulting solution was vigorously stirred using a shear mixer and coated to a thickness of 3.5-4 μm using a reverse gravure coater line. It was then coated at 4-12 J / cm. 2 The hard coat was activated using different levels of corona treatment using a Universal Treater line with an energy dose of 1000 kJ / cm². Finally, a silane topcoat was immediately coated onto the corona-treated hard coat using the same reverse gravure coater. The oil-based erasability of the samples was analyzed using a Taber Abraser instrument equipped with a microfiber cloth attachment. The samples were immersed in deionized water overnight and then aged at 120°F for 1 hour before analysis. Each sample was tested for removal of six different oil-based marker inks using a wet microfiber cloth with a 1.5 kg weight for up to six rounds (10 cycles per round, each cycle corresponding to one back-and-forth movement of the Taber Abraser head). Additionally, the durability of the samples was evaluated by abrading samples covered with black Expo dry-erase marker ink for up to six rounds (400 cycles per round, each cycle corresponding to one back-and-forth movement of the Taber Abraser head) using a Taber Abraser equipped with a 2 kg weight. Kleenex tissue paper was applied to the abrasion head to serve as the dry abrasion medium. After each round, the functionality of the coating was evaluated using a permanent marker and water, with higher scores indicating better performance in both the erasability and durability tests.

[0137] As shown in Table 24, all matte samples demonstrated high erasability scores with nearly 100% permanent marker removal after up to 6 x 10 cycles of testing. Furthermore, all matte samples maintained their excellent functionality even after 2400 cycles of abrasion, demonstrating that the matte hardcoat provided strong support for the silane topcoat and effectively prevented it from peeling.

[0138] [Table 24]

Claims

1. An article, A) a substrate; B) a hard coat layer disposed on the substrate, i) Formula R 1 Si(OR) 3 (Wherein, R and R 1 is methyl or ethyl; ii) Formula (R 2 ) 4-m Si(OR) m Or Si(OR) 4 (In the formula, R, R 1 and R 2 is an organic group, where R 2 is not methyl or ethyl, and m ranges from 1 to 3; a second silane monomer, if present, present in an amount of less than 20 weight percent based on the combined weight of the first and second silane monomers; iii) optionally, 10% to 30% by weight of silica nanoparticles; a hard coat layer comprising a hydrolysis and condensation reaction product of a composition comprising C) a surface layer comprising a hydrophilic silane disposed on the hard coat layer; Including, articles.

2. The article of claim 1 , wherein the hydrophilic silane comprises a zwitterionic silane.

3. The article of claim 2 , wherein the surface layer further comprises lithium silicate, sodium silicate, potassium silicate, or a combination thereof.

4. The article of any one of claims 1 to 3, wherein the hardcoat layer comprises silica nanoparticles having an average primary particle size of less than 25, 15, or 10 nm.

5. The article of any one of claims 1 to 4, wherein the first silane monomer is present in an amount of at least 85%, 90%, or 95% by weight based on the total of the first and second silane monomers.

6. The article of any one of claims 1 to 5, wherein the hardcoat layer comprises silica nanoparticles having a hydrophilic silane surface treatment.

7. The article of claim 6 , wherein the hydrophilic silane surface treatment is an epoxyalkoxysilane.

8. The article of any one of claims 1 to 7, wherein the substrate comprises an organic polymeric material.

9. The article according to any one of claims 1 to 8, wherein the surface layer is a rewritable surface.

10. 10. The article of claim 9, wherein the article is a dry erase board or film, a label, a file folder, a file tab, or a notebook cover or divider.

11. The article of claim 1 , wherein the surface layer is an anti-fog surface layer.

12. 12. The article of claim 11, wherein the article is a face mask.

13. An article, A) a substrate; B) a hard coat layer disposed on the substrate, i) Formula R 1 Si(OR) 3 (Wherein, R and R 1 is methyl or ethyl; ii) Formula (R 2 ) 4-m Si(OR) m Or Si(OR) 4 (In the formula, R, R 1 and R 2 is an organic group, where R 1 is not methyl or ethyl, and m ranges from 1 to 3; a second silane monomer, if present, present in an amount of less than 20 weight percent based on the combined weight of the first and second silane monomers; iii) 10% to 30% by weight of silica particles having an average primary particle size of less than 100 nm; a hard coat layer comprising a hydrolysis and condensation reaction product of a composition comprising Including, articles.

14. The article of claim 13, wherein the article is further characterized by any one of claims 4 to 12.

15. 1. A method of using an article having a rewritable surface, comprising: Providing an article according to any one of claims 1 to 11, 13 and 14; writing on said rewritable surface layer with a marker; removing the writing; and A method comprising: