Optical element, optical device, and method for manufacturing an optical element, particularly for reflecting EUV radiation
Patent Information
- Application Number
- JP2023526422
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-29
- Filing Date
- 2021-10-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-05
AI Technical Summary
Existing reflective optical elements in EUV lithography systems face challenges in protecting against reactive hydrogen species, particularly when they have complex three-dimensional structures, leading to volatile hydride formation and degradation of optical components.
Doping the substrate and structural layers of reflective optical elements with noble metals throughout their volume, rather than just near the surface, to enhance hydrogen recombination and reduce volatile hydride formation.
This approach effectively prevents or reduces the formation of volatile hydrides, enhancing the hydrogen-induced outgassing resistance and radiation resistance of optical elements without increasing absorption and maintaining structural integrity.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] [Reference to related applications] This application claims priority to German Patent Application No. 10 2020 213 639.4, dated 29 October 2020, which incorporates its entire disclosure by reference.
[0002] The present invention relates to a reflective optical element that reflects EUV radiation in particular, comprising a substrate and a reflective coating deposited on the substrate. The method also relates to an optical device, preferably for microlithography, particularly for EUV lithography, which includes at least one of the above-mentioned reflective optical elements, for example, in the form of a projection exposure apparatus. The present invention also relates to a method for manufacturing a reflective optical element, comprising the steps of preparing a substrate and depositing a reflective coating on the substrate, preferably a step of depositing a structurable layer on the substrate before depositing the reflective coating and structuring it after deposition. [Background technology]
[0003] The optical device may be, for example, an optical device for EUV lithography, i.e., an optical system that can be used in the field of EUV lithography. In addition to projection exposure equipment for EUV lithography that is useful for the manufacture of semiconductor components, the optical device may be, for example, an inspection system for inspecting photomasks (hereinafter also referred to as reticles) used in such projection exposure equipment, an inspection system for inspecting structured semiconductor substrates (hereinafter also referred to as wafers), or a measurement system used for measuring projection exposure equipment or a part thereof for EUV lithography, for example, for measuring the projection optical unit.
[0004] EUV lithography systems or EUV measurement systems and the components installed therein operate in a vacuum with low partial pressure hydrogen added. The hydrogen acts as a continuous cleaning agent for the optical surface. During operation, molecular hydrogen is excited by the generated EUV light, forming hydrogen radicals (H*) and hydrogen ions (H+). The interaction of these hydrogen species with the exposed surface of a reflective optical element (EUV mirror) made of, for example, Si-containing materials (single crystal / polycrystalline or amorphous silicon, quartz glass, silicon nitride, silicon carbide, especially silicon-impregnated silicon carbide composites (SiSiC), aluminum magnesium silicate ceramics such as cordierite ceramics, glass, or glass ceramics with very low thermal expansion, such as ULE®, Zerodur®, Clearceram®, etc.) generates volatile hydrides, particularly silanes, which are also called HIO ("hydrogen-induced gas release"). Further deposition of volatile hydrides on the optical surface can lead to degradation of the optical components.
[0005] The literature discloses various methods that can prevent or reduce the formation of volatile hydrides.
[0006] Patent Document 1 proposes covering components of an EUV lithography apparatus exposed to a hydrogen-containing atmosphere with at least partially a protective layer of a noble metal (e.g., from the group of rhodium, ruthenium, iridium, palladium, and platinum). The minimum thickness of the protective layer should be selected so that the protective layer is not permeable to hydrogen ions and / or hydrogen radicals.
[0007] Patent Document 2 discloses an optical element in which a shield providing protection from the etching effect of the surrounding hydrogen plasma is attached to at least one surface region of a body separated by a gap. The distance between the shield and the surface region is less than twice the Debye length of the surrounding plasma. The shield may also be applied indirectly or directly to the body. The shield may consist of a hydrogen recombining material (e.g., Ir, Ru, Pt, Pd) or may have a coating of a hydrogen recombining material. The gap may be partially or completely filled with a filler (e.g., aluminum oxide, zirconium nitride, yttrium oxide, cerium oxide, zirconium oxide, niobium oxide, titanium oxide, tantalum oxide, tungsten oxide, metals, preferably noble metals, especially Ru, Rh, Pd, Ir, Pt, Au, and compositions thereof). In yet another embodiment, the shield may take the form of a coating.
[0008] Patent Document 3 discloses an optical element that reflects EUV radiation, having an uppermost layer of a hydrogen desorption material (e.g., Pd, Ag, Au, and their alloys) with a hydrogen desorption temperature of less than 340K. To achieve the desired effect of releasing hydrogen, the uppermost layer does not necessarily need to form a continuous layer. Material accumulation of hydrogen desorption material in the form of clusters or islands can also achieve this purpose if the distance between them is sufficiently small.
[0009] Patent Document 4 discloses an EUV mirror exposed to a hydrogen plasma during operation, wherein the body comprises at least one material that forms at least one volatile hydride upon contact between the surface region and activated hydrogen (H+, H*). To prevent the formation of volatile hydrides, noble metal ions (e.g., Rh, Ru, Ir, Au, Pd, Pt) are implanted into the surface region of the body. By implanting noble metal ions into a volume region near the surface below the surface, the formation of volatile hydrides can be significantly reduced. This utilizes the fact that noble metal ions generally have a strong catalytic effect on the recombination of activated hydrogen, i.e., hydrogen radicals and / or hydrogen ions, for the formation of atomic hydrogen. In contrast to the aforementioned solution, the implantation of noble metal ions merely dops the body and does not form a layer.
[0010] However, if the reflective optical element is a structured optical unit, for example, implanting noble metal ions into a volume region near the surface of the main body provides only limited protection. In such optical units, a structureable layer of amorphous silicon, for example, is deposited on the substrate to form a structure, for example, in the form of a lattice structure. The lattice structure can be formed, for example, on an EUV collector mirror and act as a spectroscopic filter. Since deposition that completely and uniformly covers the structured surface is extremely difficult (the layer often has pores, channels, or other defects or irregularities at its steep edges), such structured layers, and silicon layers of reflective multilayer Mo-Si layers or coatings, are subject to etching attacks by reactive hydrogen species.
[0011] Patent Document 5 discloses a mirror for an illumination optical unit of a projection exposure apparatus equipped with a spectroscopic filter in the form of a lattice structure. The lattice structure can be completely covered by a continuous protective layer in the form of a reflective coating having multiple Si-Mo bilayers. A low edge steepness of the lattice structure can improve the coverage of the lattice structure by the protective layer, thus increasing the hydrogen stability of the reflective optical element.
[0012] When attempting to achieve complete coverage of a lattice structure even with relatively high edge sharpness, reflective multilayer coatings can be deposited as conformal coatings, as described in Patent Document 6. Here, conformal or isotropic coating processes in the form of atomic layer deposition are proposed to achieve essentially constant layer thickness along the three-dimensional profile. However, depositing reflective multilayer coatings that may have more than 50 layers of Mo and Si bilayers by atomic layer deposition is extremely complex.
[0013] Patent Document 7 describes an optical element provided with a protective layer system having a first layer, a second layer, and a third layer. Metal particles and / or ions can be implanted into at least one layer of the protective layer system. The ions can be noble metal ions, for example noble metal ions, particularly platinum group metal ions. At least one layer of the protective layer system can be doped with metal (nano) particles, for example atoms in the form of noble metal particles (for example, Pd, Pt, Rh, Ir). The noble metal ions or foreign atoms can act as hydrogen and / or oxygen blockers.
[0014] All of the above-described methods assume the large-area processing of three-dimensional objects in complex forms, which involves a considerable degree of complexity.
Prior Art Documents
Patent Documents
[0015]
Patent Document 1
Patent Document 2
Patent Document 3
Patent Document 4
Patent Document 5
Patent Document 6
Patent Document 7
Summary of the Invention
Problems to be Solved by the Invention
[0016] An object of the present invention is to specify a reflective optical element, an optical device, and a method for manufacturing an optical element that enable protection from reactive species, particularly reactive hydrogen species, and can be implemented with a low degree of complexity.
Means for Solving the Problem
[0017] This object is achieved, in its first aspect, by an optical element of the aforementioned type doped with at least one noble metal within the volume of the substrate.
[0018] In the recognition of the present inventors, doping the substrate material with a hydrogen recombination material in the form of a noble metal during the manufacturing process of the substrate is much more efficient than injecting noble metal ions into the volume region near the surface as described in the aforementioned Patent Document 4.
[0019] In contrast to the main body described in Patent Document 4, the doping with a noble metal in the case of the reflective optical element of the present invention is not limited to the volume region near the surface having an implantation depth of less than 1000 nm. Instead, the substrate is also doped with a noble metal in the volume, that is, in a volume region at a distance greater than 1000 nm from the surface of the substrate, for example, greater than 1 mm, greater than 2 mm, greater than 5 mm, etc. In particular, the substrate may be doped with a noble metal throughout its volume.
[0020] In one embodiment, the substrate is formed from glass or glass ceramics with very low thermal expansion, such as titanium-doped fused silica (ULE (registered trademark)), Zerodur (registered trademark), Clearceram (registered trademark), etc., ceramics such as silicon nitride ceramics, silicon carbide ceramics, silicon carbonitride ceramics, magnesium aluminum silicate ceramics, particularly cordierite ceramics, or composite materials, particularly silicon-impregnated silicon carbide composites (SiSiC). In principle, it is possible to dope any substrate material used in EUV lithography with a noble metal.
[0021] The substrate is preferably formed from silicon, particularly from single crystal, pseudo-single crystal, or polycrystalline silicon, or possibly from amorphous silicon. Silicon doped with precious metals in the form of gold (see paper "Properties of Gold-Doped Silicon", CB Collins et al., Phys. Rev. 105(1957) 1168-1173) or platinum is commercially available and can therefore be used in the manufacture of substrates for reflective optical elements. Gold or platinum-saturated single-crystal silicon is used, for example, as a window in high-power generators in microwave technology (see "Radiation effects on dielectric losses of Au-doped silicon", J. Molla et al., Journal of Nuclear Materials, 258-263 (1998) 1884-1888) or in radiation detectors (see "Gold and Platinum Doped Radiation Resistant Silicon Diode Detectors", RL Dixon et al., Radiation Protection Dosimetry 17 (1986) 527-530).
[0022] Single-crystal silicon is also a common material for the manufacture of substrates for X-ray, EUV, and synchrotron optics, and polishing techniques for this purpose are well-established. Useful methods for the manufacture of single-crystal silicon include all conventional methods such as the Czochralski method ("A new method for measuring the crystallization rate of metals," see J. Czochralski, Zeitschrift fur physikalische Chemie, 92 (1918) 219-221) or the Bridgman-Stockberger method ("Certain Physical Properties of Single Crystals of Tungsten, Antimony, Bismuth, Tellurium, Cadmium, Zinc, and Tin," see P.W. Bridgeman, Proceedings of the American Academy of Arts and Sciences 60 (1925) 305-383). These methods are also suitable for producing single-crystal silicon saturated with gold or platinum.
[0023] For particularly large crystals, Schott Solar AG has developed a method for producing pseudo-single-crystal silicon based on the vertical temperature gradient solidification (VGF) method (German Patent Application Publication No. 102012110147, German Patent Application Publication No. 102012102597). This method or the VGF method is suitable for producing pseudo-single-crystal silicon saturated with gold or platinum.
[0024] A further aspect of the present invention relates to the aforementioned type of reflective optical element which can be particularly combined with the reflective optical element of the first aspect of the present invention. This reflective optical element comprises a structural layer formed between a substrate and a reflective coating and which preferably forms or has a lattice structure, the structural layer being doped with (at least) one noble metal.
[0025] As described above, reflective coatings can form a protective layer on the structural layer, which prevents or at least limits etching attacks by reactive hydrogen species and, consequently, gas release of volatile hydrides. However, if the flanks of the lattice structure have excessively steep flank angles, for example, exceeding 60°, the structural layer will generally not be completely covered by the reflective coating unless it is deposited by a complex isotropic coating method, such as atomic layer deposition.
[0026] However, structural layers that can be formed from amorphous silicon (see Patent Document 5 above) can be protected from hydrogen attack by doping them with a noble metal that acts as a hydrogen recombination material. As will be explained in detail below, in order to achieve doping with a noble metal, it is possible to use a sputtering target doped with a noble metal when depositing a structural layer or a structureable layer by sputtering deposition.
[0027] Yet another aspect of the present invention relates to a reflective optical element of the same type as described above, which can be particularly combined with the reflective optical elements of the first and / or second aspects, and in which a noble metal is doped into at least one silicon layer of the reflective coating, particularly the reflective Mo-Si coating.
[0028] In particular, when the reflective coating is deposited on a structural layer, or when the reflective coating itself is structured to form a lattice structure, under-etching of individual layers of the reflective coating is possible, as shown in the paper "Multilayer EUV optics with integrated IR suppression gratings", T. Feigl et al., Proceedings of 2016 EUVL Workshop (P69), Berkeley, June 13-16, 2016). Under-etching in this case usually occurs on the sides of the (structured) reflective coating, typically on individual layers of the reflective coating that are particularly susceptible to etching attacks.
[0029] In one developmental form, the structural layer and / or reflective coating contains silicon doped with a noble metal. As described above, the material of the structural layer may be, for example, amorphous silicon that can be structured relatively simply. If the reflective coating is a multilayer coating used for reflecting EUV radiation at a perpendicular incidence angle (less than 45°), it may have alternating layers (double layers) of Mo and Si, depending on the operating wavelength for which the reflective coating is designed. As described above, silicon can form volatile silanes when in contact with hydrogen. Silane formation can be prevented or at least reduced by doping the Si layer of the reflective Mo-Si coating with a noble metal. When a noble metal-doped sputtering target is used in sputtering deposition, the reflective coating, more specifically the individual layers of the reflective coating, may already be doped with the noble metal during deposition (see below).
[0030] When silicon is doped with precious metals, a significant increase in absorption of the doped silicon is not expected at the preferred dopant concentrations (see below), so doping can achieve improvements in HIO resistance and radiation resistance with little effort.
[0031] In yet another embodiment, the reflective coating forms a multilayer coating that reflects EUV radiation. Such a multilayer coating typically has multiple alternating layers of materials with a large real part of the refractive index at the operating wavelength and materials with a small real part of the refractive index at the operating wavelength. The materials are, for example, silicon and molybdenum, but other combinations of materials are possible depending on the operating wavelength.
[0032] In yet another embodiment, the noble metal is selected from the group including Ru, Rh, Pd, Ag, Os, Ir, Pt, Au, and combinations or alloys thereof. As mentioned above, noble metals generally have a strong catalytic effect on activated hydrogen for forming atomic hydrogen, i.e., on the recombination of hydrogen radicals and / or hydrogen ions. As also mentioned above, Pt or Au-doped silicon is commercially available and can therefore be used in particular. However, it will also become apparent that it is possible to dope noble metals into other materials that form or are present in the volume of a substrate, structural layer, and / or reflective coating.
[0033] In yet another embodiment, the volume of the substrate, the structural layer, and / or the dopant concentration of the noble metal in the reflective coating is 10 10 cm -3 ~10 20 cm -3 Preferably 10 12 cm -3 ~10 16 cm -3 The dopant concentrations described allow for doping of the structural layer of the reflective coating with noble metals, such as Au or Pt, without significantly increasing the absorption of EUV radiation. It has also been found that the above range of dopant concentrations is advantageous for substrate doping.
[0034] In yet another embodiment, the reflective optical element takes the form of a collector mirror for the illumination optical unit of a projection exposure apparatus. Such a collector mirror may have, for example, one or more elliptical and / or hyperbolic reflective surfaces corresponding to a surface having a reflective coating. Illumination radiation may be incident on the reflective surface of the collector mirror at an oblique angle (GI), i.e., at an angle of incidence greater than 45°, or at a normal angle (NI), i.e., at an angle of incidence less than 45°.
[0035] Collector mirrors typically have a structural layer in the form of a lattice structure that acts as a spectral filter to suppress external light, i.e., radiation outside the EUV wavelength range, such as in the infrared wavelength range. It will become clear that the reflective optical element does not necessarily have to take the form of a collector mirror, and may be any other reflective optical element.
[0036] A further aspect of the present invention relates to an optical apparatus comprising at least one reflective optical element as described above, preferably a projection exposure apparatus for microlithography, and more particularly for EUV lithography. Such a projection exposure apparatus comprises an illumination optical system for transmitting illumination radiation from a radiation source to a reticle containing an imaging structure, and a projection optical unit for imaging the structure of the reticle onto a wafer. The reflective optical element may be arranged in the illumination optical system, or it may be arranged in the projection optical system.
[0037] As described above, the reflective optical element is placed in a vacuum environment with low partial pressure hydrogen in such a projection exposure apparatus. During the operation of the projection exposure apparatus, reactive hydrogen species are generated by interaction with EUV radiation. By doping the substrate, structural layer, and / or reflective coating with a noble metal, it is possible to improve both the HIO resistance and radiation resistance of the substrate, structural layer, and / or reflective coating at low cost and without inconvenience.
[0038] A further aspect of the present invention relates to a method of the aforementioned type for depositing a reflective coating and / or a structureable layer by sputtering deposition, wherein a noble metal-doped sputtering target, preferably containing silicon, is used in the sputtering deposition.
[0039] In sputtering deposition, high-energy ions collide with a solid material (sputtering target). This separates particles or atoms from the sputtering target, converts them to a gas phase, and deposits them on the substrate. To ensure the atoms separated from the sputtering target reach the substrate, sputtering deposition is usually performed in a high-vacuum processing chamber. High-energy ions can be, for example, noble gas ions, particularly argon ions. There are several types of sputtering deposition.
[0040] In DC voltage sputtering deposition, a DC voltage is applied between the sputtering target and the substrate to generate a plasma, accelerating positively charged noble gas ions to the sputtering target (cathode) and negatively charged particles ejected from the sputtering target to the substrate (anode). In magnetron sputtering rings, a magnetic field is superimposed on the electric field to increase the ionization rate. Further types of sputtering deposition that are similarly possible include, for example, HF sputtering, reactive sputtering, ion beam sputtering, or atomic beam sputtering.
[0041] As described above, sputtering targets for sputtering the layer to be structured or the layer of the reflective coating can be doped with a precious metal. For this purpose, for example, it is possible to manufacture sputtering targets of silicon doped with gold or platinum and use them for sputtering the structured layer or reflective coating. Here, it is possible to take advantage of the fact that gold or platinum-doped silicon is commercially available. However, it will be clear that sputtering targets may also be doped with other precious metals.
[0042] A further aspect of the present invention relates to the aforementioned type of method, which can be combined with the above method in particular. In this method, a substrate prepared for subsequent coating is doped with at least one precious metal within its volume. In this case, the substrate is already doped with at least one precious metal during its manufacture, and the doped substrate is ready for coating.
[0043] In this embodiment, the reflective coating and, optionally, the coating of the structured layer may be carried out using a sputtering target doped with a precious metal, but is not required. In particular, if the reflective optical element does not have a structured layer or a structured layer, it is possible to deposit a conventional reflective coating that is not doped with a precious metal onto the substrate.
[0044] It is clear that reflective optical elements do not necessarily need to be designed to reflect radiation in the EUV wavelength range; they may also be designed to reflect radiation in other wavelength ranges, such as VUV wavelength ranges.
[0045] Further features and advantages of the present invention will become apparent from the following description of exemplary embodiments of the invention with reference to the drawings illustrating essential details of the invention, and from the claims. Each of the individual features can be implemented individually or in any combination of several in one variant of the invention.
[0046] An example is shown in the schematic diagram and will be explained in the following description. [Brief explanation of the drawing]
[0047] [Figure 1] This is a schematic meridional cross-sectional view of a projection exposure system for EUV lithography. [Figure 2] This is a schematic diagram of the reflective optical element of the projection exposure apparatus shown in Figure 1, which has a substrate doped with a precious metal. [Figure 3] This is a schematic diagram similar to Figure 2, in which the reflective optical element has a structural layer doped with a precious metal. [Figure 4] This is a schematic diagram of a sputtering deposition system having a sputtering target doped with precious metals. [Modes for carrying out the invention]
[0048] In the following description of the drawings, the same reference numerals are used for components that are identical or have the same function.
[0049] The essential components of the microlithography projection exposure apparatus 1 will be described below as an example, with reference to Figure 1. The description of the basic configuration of the projection exposure apparatus 1 and its components should not be considered limiting here.
[0050] The illumination system 2 of the projection exposure apparatus 1 includes not only a radiation source 3 but also an illumination optical unit 4 for illuminating the object field of view 5 on the object surface 6. The object being exposed here is a reticle 7 positioned in the object field of view 5. The reticle 7 is held by a reticle holder 8. The reticle holder 8 is displaceable, particularly in the scanning direction, by a reticle displacement drive 9.
[0051] For explanatory purposes, a Cartesian xyz coordinate system is shown in Figure 1. The x-direction extends perpendicular to the plane of the figure. The y-direction extends horizontally, and the z-direction extends vertically. The scanning direction extends in the y-direction in Figure 1. The z-direction extends perpendicular to the object plane 6.
[0052] The projection exposure apparatus 1 includes a projection optical unit 10. The projection optical unit 10 functions to image the object field of view 5 onto the image field of view 11 of the image plane 12. The structure on the reticle 7 is imaged onto the photosensitive layer of the wafer 13, which is positioned in the region of the image field of view 11 of the image plane 12. The wafer 13 is held by a wafer holder 14. The wafer holder 14 is displaceable, particularly in the y-direction, by a wafer displacement drive 15. On the one hand, the displacement of the reticle 7 by the reticle displacement drive 9 and on the other hand, the displacement of the wafer 13 by the wafer displacement drive 15 can be synchronized with each other.
[0053] Radiation source 3 is an EUV radiation source. Radiation source 3 emits EUV radiation 16, which is also referred to below as the radiation used or illumination radiation. In particular, the radiation used has wavelengths in the range of 5 nm to 30 nm. Radiation source 3 may be a plasma source, such as an LPP ("laser-generated plasma") source or a GDPP ("gas discharge plasma") source. It may also be a synchrotron-based radiation source. Radiation source 3 may be a free electron laser (FEL).
[0054] Illumination radiation 16 generated from radiation source 3 is focused by a collector mirror 17. The collector mirror 17 may be a collector mirror having one or more elliptical and / or hyperbolic reflecting surfaces. Illumination radiation 16 may be incident at an oblique angle (GI), i.e., at an angle of incidence greater than 45°, or at a normal angle (NI), i.e., at an angle of incidence less than 45°, on at least one reflecting surface of the collector mirror 17. The collector mirror 17 may be structured and / or coated to first optimize its reflectivity for the radiation used, and second to suppress external light.
[0055] The illumination radiation 16 propagates through the intermediate focal point of the intermediate focal plane 18 downstream of the collector mirror 17. The intermediate focal plane 18 can separate the radiation source module, which has the radiation source 3 and the collector mirror 17, from the illumination optical unit 4.
[0056] The illumination optical unit 4 comprises a deflection mirror 19 and a first facet mirror 20 located downstream of it in the beam path. The first facet mirror 20 includes a plurality of individual first facets 21, also referred to below as field facets. Figure 1 shows only some of the above facets 21 as an example. A second facet mirror 22 is located downstream of the first facet mirror 20 in the beam path of the illumination optical unit 4. The second facet mirror 22 includes a plurality of second facets 23.
[0057] The illumination optical unit 4 consequently forms a dual-facet system. This basic principle is also referred to as a fly-eye integrator. Using the second facet mirror 22, the individual first facet 21 is imaged into the object field of view 5. The second facet mirror 22 is also the last beam shaping mirror or, in fact, the final mirror for the illumination radiation 16 in the upstream beam path of the object field of view 5.
[0058] The projection optical unit 10 includes a plurality of mirrors Mi, which are numbered sequentially according to their arrangement in the beam path of the projection exposure apparatus 1.
[0059] In the example shown in Figure 1, the projection optical unit 10 includes six mirrors M1 to M6. Substitution with four, eight, ten, twelve, or any other number of mirrors Mi is equally possible. The second-to-last mirror M5 and the last mirror M6 each have a through aperture for illumination radiation 16. The projection optical unit 10 is a double-shielded optical unit. The projection optical unit 10 has an image-side numerical aperture greater than 0.5 and may be greater than 0.6, for example, 0.7 or 0.75.
[0060] Similar to the mirrors of the illumination optical unit 4, mirror Mi may have a highly reflective coating for illumination radiation 16.
[0061] Figure 2 shows a deflection mirror 19 of an illumination optical system 4, having a single-crystal silicon substrate 25 on which a reflective coating 26 that reflects illumination radiation 16 is deposited. The deflection mirror 19 is exposed to reactive hydrogen species in the form of hydrogen ions (H+) and hydrogen radicals (H*). The reactive hydrogen species H+ and H* may react with the silicon material of the substrate 25 on exposed surfaces of the substrate 25, such as the lateral surface 25a, to form volatile hydrides, such as silanes. These volatile hydrides can further deposit on the optical surface, leading to its degradation.
[0062] To suppress the formation of volatile hydrides, the substrate 25 of the deflection mirror 19 in the example shown in Figure 2 is doped with a noble metal 27, more specifically gold, throughout its entire volume V. The noble metal 27, in the form of gold atoms, implanted into the silicon substrate 25 acts as a hydrogen recombination material, reacting reactive hydrogen species H+ and H* to form molecular hydrogen, thus suppressing the formation of volatile hydrides.
[0063] The gold doping of the substrate 25 is carried out during the manufacturing of the single-crystal silicon substrate 25. The single-crystal silicon substrate 25 was lifted from the melt during its manufacture (Czochralski process). The material of the melt from which the substrate 25 was lifted was doped with precious metal 27. It is also possible to manufacture single-crystal silicon substrate 25 doped with precious metal 27 by other methods, for example, using the Bridgman-Stockbacker process. It is also possible to manufacture pseudo-single-crystal silicon substrate 25 or polycrystalline silicon substrate doped with a precious metal, for example, gold.
[0064] It is also possible to dope the silicon substrate 25 with other precious metals, such as Ru, Rh, Pd, Ag, Os, Ir, Pt, and combinations or alloys thereof. Doping the silicon substrate 25 with Au or Pt has been found to be advantageous because these types of materials are already commercially available. However, it is also possible to dope the silicon substrate 25 with at least one precious metal other than Au or Pt.
[0065] The doping of the substrate 25 with precious metals as described above can also be performed for other substrate materials suitable for the manufacture of reflective optical elements for EUV lithography. These substrate materials include, for example, quartz glass, glass or glass ceramics with very low thermal expansion, such as ULE®, Zerodur®, Clearceram®, etc., ceramics, such as silicon nitride, silicon carbide, especially silicon-impregnated silicon carbide composites (SiSiC), and magnesium aluminum silicate ceramics such as cordierite ceramics. It will also become clear that the doping of the substrate 25 can be performed with two or more different precious metals 27.
[0066] Figure 3 shows, as an example, the collector mirror 17 of the illumination optical unit 2 of the projection exposure apparatus 1 shown in Figure 1. The collector mirror 17 differs from the deflection mirror 19 shown in Figure 2 in that a structural layer 28 is formed between the substrate 25 and the reflective coating 26. The structural layer 28 has a structural surface in the form of a lattice structure 29 and is formed from amorphous silicon. The lattice structure 29 acts as a spectral filter to suppress external light, i.e., radiation with wavelengths outside the EUV wavelength range, such as in the infrared wavelength range. The reflective coating 26 is deposited on the structural layer 28 or the lattice structure 29.
[0067] In principle, the structural layer 28 is protected from reactive hydrogen species H+ and H* by the deposited reflective coating 26. However, in the example shown in Figure 3, the (maximum) edge steepness of the lattice structure 29 is large, approximately 90°. Deposition of the reflective coating 26 in the form of a continuous layer completely covering the structural layer 28 is possible even with such a large edge steepness if the deposition is carried out by an isotropic coating method, for example, by atomic layer deposition. However, in the illustrated example, the deposition of the reflective coating 26 to form a multilayer coating with approximately 50 Si / Mo bilayers using an isotropic coating method is extremely complex. Furthermore, as shown in Figure 3, the collector mirror 17 is not flat, but usually has an elliptical or hyperbolic curvature, which further makes coating by atomic layer deposition difficult.
[0068] In the illustrated example, the reflective coating 26 is deposited on the structural layer 28 by anisotropic coating, more specifically by sputtering deposition. The structural layer 28 is doped with a noble metal 27 for protection from reactive hydrogen species H+, H*. The same applies to the reflective coating 26 deposited on the structural layer 28, because this reflective coating 26, or more specifically its silicon-containing layer, is exposed to reactive hydrogen species H+, H*, particularly along the steep flanks of the lattice structure 29. It is possible to deposit a protective layer system (not shown) on the reflective coating 26, in which the noble metal can similarly be injected into one or more layers.
[0069] For efficient doping of one or more layers of the structural layer 28, reflective coating 26, and optionally protective layer system, sputtering deposition is performed using a sputtering target 37 doped with a precious metal 27, as described below with reference to Figure 4.
[0070] Figure 4 shows a very simple configuration of a sputtering deposition system 30 having a high-vacuum processing chamber 31. A noble gas 32 in the form of argon is supplied to the processing chamber 31 through a gas inlet. The noble gas 32 enters the space between the plate-shaped cathode 33 and the plate-shaped anode 34 of the processing chamber 31, where a constant electric field is generated over time. A constant voltage is applied over time between the cathode 33 and the anode 34 to generate the electric field. A magnet 35, positioned away from the space of the cathode 33, generates a magnetic field 36 in the space in addition to the electric field.
[0071] The noble gas 32 is ionized in the space between the cathode 33 and the anode 34 to form noble gas ions 32a. The noble gas ions 32a are accelerated toward the cathode 33, knocking out negatively charged particles 38 from the sputtering target 37 attached thereto. The particles 38 are then accelerated toward the anode 34 and deposited on the substrate 25 of the reflective optical element 17 attached thereto.
[0072] In the illustrated example, the sputtering target 37 is formed from single-crystal or pseudo-single-crystal silicon doped with a noble metal 27. As a doping effect, the structureable layer 28' deposited on the substrate 25 by sputtering is also doped with the noble metal 27. Correspondingly, it is also possible to deposit a reflective coating 26, or more specifically, a silicon layer of the reflective coating 26, using a silicon sputtering target 37 doped with the noble metal 27.
[0073] Before forming the reflective coating 26, the structurable layer 28' is structured to form a structural layer 28 having a lattice structure 29. The structuring can be performed, for example, by a dry or wet chemical etching process of the structurable layer using the structural layer. The structural layer acting as a sacrificial layer can be structured, for example, using lithographic exposure or by some other method.
[0074] The dopant concentration of the noble metal 27 in the volume V of the substrate 25, the structural layer 28, and the reflective coating 26 is usually on the order of 10 10 cm -3 ~10 20 cm -3 and preferably on the order of 10 12 cm -3 ~10 16 cm -3 In the case of such dopant concentrations, a significant increase in the absorption of the doped silicon in the reflective coating 26 or the structural layer 28 or the substrate 25 is not expected, so the doping described herein can achieve an improvement in the HIO resistance and radiation resistance of the reflective optical element 17 at low cost and without inconvenience.
[0075] It will be apparent that doping with the noble metal 27 does not necessarily have to be performed on both the substrate 25 and the structural layer 28 and the reflective coating 26. For example, if the substrate 25 is protected from reactive hydrogen species in some other way, it is possible to omit doping of the substrate 25. Such protection can be achieved, for example, by the shield described in the aforementioned Patent Document 2 incorporated herein by reference in its entirety. If the structural layer 28 is completely covered by the reflective coating 26, doping of the structural layer 28 may not be necessary.
Claims
1. A substrate (25); A reflective coating (26) deposited on the substrate (25); A reflective optical element (17, 19) for reflecting, in particular, EUV radiation (16), comprising: A reflective optical element, characterized in that the substrate (25) is doped in its volume (V) with at least one noble metal (27), A reflective optical element, wherein the substrate (25) is doped with the at least one noble metal (27) in a volumetric region extending from a surface of the substrate (25) to a distance greater than 1 mm from the surface of the substrate (25).
2. 2. A reflective optical element according to claim 1, wherein the substrate (25) is made of glass, in particular titanium-doped quartz glass, of glass ceramics, of ceramics, preferably silicon nitride ceramics, silicon carbide ceramics, silicon carbonitride ceramics, magnesium aluminium silicate ceramics, in particular cordierite ceramics, or of a composite material, in particular silicon-impregnated silicon carbide composite SiSiC.
3. 2. A reflecting optical element according to claim 1, wherein the substrate (25) is made of silicon, in particular of monocrystalline, pseudo monocrystalline or polycrystalline silicon.
4. 3. A reflective optical element according to claim 1 or 2, wherein the substrate (25) is doped with the at least one precious metal (27) in a volumetric region extending from the surface of the substrate (25) to a distance of more than 2 mm, in particular more than 5 mm, from the surface of the substrate (25).
5. A reflective optical element according to any one of the preceding claims, wherein said substrate (25) is doped throughout its volume with said at least one noble metal (27).
6. A reflective optical element according to the preamble of claim 1, in particular according to any one of claims 1 to 5, A structural layer (28) formed between said substrate (25) and said reflective coating (26), preferably forming a grating structure (29), said structural layer (28) being doped with a noble metal (27). The reflective optical element further comprises:
7. A reflecting optical element according to the preamble of claim 1, in particular according to any one of claims 1 to 6, wherein said reflective coating (26) is doped with a noble metal (27).
8. A reflective optical element according to any one of the preceding claims, wherein the structure layer (28) and / or the reflective coating (26) comprises silicon doped with the noble metal (27).
9. A reflective optical element according to any one of the preceding claims, wherein said reflective coating forms a multi-layer coating (26) for reflecting EUV radiation (16).
10. 10. The reflective optical element according to claim 1, wherein the noble metal (27) is selected from the group consisting of Ru, Rh, Pd, Ag, Os, Ir, Pt, and Au.
11. 11. The reflective optical element according to claim 1, wherein the dopant concentration of the noble metal (27) is 10 10 cm -3 ~10 20 cm -3 , preferably 10 12 cm -3 ~10 16 cm -3 A reflective optical element.
12. The reflective optical element according to any one of claims 1 to 11, which is in the form of a collector mirror (17) of an illumination optical system (2) of a projection exposure apparatus (1).
13. An optical apparatus, preferably a projection exposure apparatus (1) for microlithography, in particular for EUV lithography, comprising: Optical device comprising at least one reflective optical element (17, 19) according to any one of the preceding claims.
14. A method for manufacturing a reflective optical element (17, 19) according to any one of claims 1 to 12, comprising the steps of: Providing a substrate (25); depositing a reflective coating (26) on said substrate (25), preferably before depositing said reflective coating (26) a structurable layer (28') on said substrate (25) and structuring it after deposition; In a method comprising:
10. A method according to claim 9, wherein the reflective coating (26) and / or the structurable layer (28') are deposited by sputtering deposition, the sputtering deposition being achieved using a sputtering target (37) doped with a noble metal (27), preferably comprising silicon.
15. A method according to the preamble of claim 14, in particular according to claim 14, in which the provided substrate (25) is doped in its volume (V) with at least one noble metal (27).