Fixed-bed reactor system for the oxidative dehydrogenation of ethane.
Patent Information
- Application Number
- JP2023526540
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-06
- Filing Date
- 2021-11-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-11-05
AI Technical Summary
Existing oxidative dehydrogenation (ODH) processes face challenges in controlling thermal runaway in catalyst beds, leading to increased conversion rates and risks, which are mitigated by reducing maximum catalyst bed temperature without sacrificing conversion and yield.
A fixed bed reactor system with a catalyst bed capacity profile that increases gradually or stepwise from the upstream to the downstream end, utilizing varying catalyst capacity, dilution ratios, and porosity to manage temperature gradients.
Minimizes the risk of thermal runaway while maintaining high ethane conversion and ethylene yield by controlling temperature spikes and improving cooling efficiency.
Abstract
Description
[Technical Field]
[0001] (Claiming priority) This application claims priority to U.S. Provisional Application No. 63 / 110,385, filed on November 6, 2020, the entirety of which is incorporated herein by reference. (Technical field) This specification relates to a reactor system for the oxidative dehydrogenation (ODH) of ethane to ethylene. [Background technology]
[0002] The concept of ODH has been known since at least the late 1960s. Since then, considerable effort has been made to improve the process, including improving catalyst efficiency and selectivity. For ODH to become a mainstream commercial option, the economic benefits must outweigh the risks associated with the potential thermal runaway of the ODH reaction. Thermal runaway occurs when the exothermic conversion of ethane causes a rapid increase in the catalyst bed temperature, and the cooling mechanism is insufficient to keep the temperature down. A rapid increase in catalyst bed temperature increases the ethane conversion rate, which in turn causes the catalyst bed temperature to rise further, leading to further increases in the ethane conversion rate and other factors. To minimize this risk, operators may choose to limit the catalyst capacity in the reactor or increase the size of the reactor. These options are not cost-effective. The first option reduces the ethylene yield, and the second option increases capital investment to build a larger reactor. Provided herein is a reactor system that reduces the maximum catalyst bed temperature without sacrificing conversion rate and yield. [Overview of the project]
[0003] It was discovered that a reduction in the maximum catalyst bed temperature in a fixed-bed reactor during the oxidative dehydrogenation process of ethane can be achieved by loading the catalyst bed in such a way that it provides an increase in catalyst capacity from the upstream end to the downstream end along the length of the catalyst bed.
[0004] In a first aspect, a fixed bed reactor system for the oxidative dehydrogenation (ODH) of ethane to ethylene is provided, the system including a catalyst bed having a catalyst volume profile that increases gradually or stepwise from an upstream end to a downstream end of the catalyst bed.
[0005] In an additional aspect, the catalyst bed includes at least two non-overlapping catalyst bed sections arranged in series along the length of the catalyst bed. The catalyst bed sections are identified by a change in catalyst volume, and each catalyst bed section, except for the first catalyst bed section, has a higher catalyst volume than the immediately preceding catalyst bed section.
[0006] The catalyst volume, or the ability to convert ethane to ethylene, can be evaluated by determining the 35% conversion temperature. This 35% conversion temperature depends on how much catalyst is present, how diluted the catalyst is with a catalyst additive and / or heat-dispersing particles within the catalyst bed, and the porosity within the catalyst bed.
[0007] In a second aspect, a process for the oxidative dehydrogenation of ethane is provided, the process including introducing a feed stream containing ethane and oxygen into a fixed bed reactor including a catalyst bed, the catalyst bed having a catalyst volume that increases gradually or stepwise from an upstream end to a downstream end to form a product stream containing ethylene.
[0008] A third aspect provides a method for loading a catalyst bed into a fixed-bed reactor for use in an oxidative dehydrogenation process, the method comprising the steps of: preparing two or more catalyst bed compositions comprising an ODH catalyst; determining the catalyst capacity for each catalyst bed composition; pouring the catalyst bed compositions into a fixed-bed reactor sequentially and separately at a rate slow enough to allow for high-density, random packing, with the catalyst bed composition having the lowest catalyst capacity poured into the upstream end and the catalyst bed composition having the highest catalyst capacity poured into the downstream end; and fixing the poured catalyst bed compositions within the fixed-bed reactor to form a loaded catalyst bed, wherein the catalyst bed compositions form separate catalyst bed sections, the catalyst bed sections being identified by a change in catalyst capacity, the catalyst capacity increasing from the upstream end to the downstream end.
[0009] (Brief explanation of the drawing) To facilitate the identification of descriptions of specific elements or actions, the highest digit of the reference numeral refers to the figure number in which that element is first introduced. Schematic diagrams of catalyst beds according to embodiments of this disclosure are intended to facilitate the understanding of different catalyst bed loading scenarios. Those skilled in the art will understand that the size and shape of catalyst particles and heat dissipation particles in the figures are illustrative for illustrative purposes only, and that the particles are not at a constant scale but actually vary in size and shape. For simplification, labeling is limited to a single example of catalyst particles and heat dissipation particles in each figure. [Brief explanation of the drawing]
[0010] [Figure 1] A schematic diagram of a typical catalyst bed with uniform catalyst capacity is shown. [Figure 2] A schematic diagram of a catalyst bed in which the catalyst capacity gradually increases, according to one embodiment, is shown. [Figure 3] A schematic diagram of a catalyst bed comprising two sections with different dilution ratios using the same catalyst, according to one embodiment, is shown. [Figure 4] A schematic diagram of a catalyst bed comprising two sections having different catalyst compositions, according to one embodiment, is shown. [Figure 5]A schematic diagram of a catalyst bed comprising two sections having different catalyst compositions, according to one embodiment, is shown. [Figure 6] A schematic diagram of a catalyst bed comprising two sections having different porosities and different lengths, according to one embodiment, is shown. [Figure 7] A schematic diagram of a catalyst bed according to one embodiment is shown, comprising two sections having different catalyst compositions and separated by a catalyst-free region. [Figure 8] A schematic diagram of a catalyst bed according to one embodiment is shown, comprising two consecutive sections separated from a third section by a catalyst-free region, where these sections differ in porosity or catalyst composition. [Figure 9] A schematic diagram of a catalyst bed according to one embodiment is shown, comprising two consecutive sections housed in a first reactor, separated from a third section housed in a second reactor, wherein these sections differ in porosity or catalyst composition. [Figure 10] The temperature profiles for Examples 1 to 4 are shown. [Modes for carrying out the invention]
[0011] Provided herein is a reactor system for the oxidative dehydrogenation (ODH) of ethane to ethylene. Embodiments of this reactor system address a catalyst capacity profile that increases along the length of the catalyst bed in the reactor system. Specifically disclosed herein is a reactor system including a catalyst bed characterized by increasing catalyst capacity from the upstream end to the downstream end of the catalyst bed. The arrangement of a catalyst bed with increasing catalyst capacity along its length provides a mechanism to minimize the highest process temperature of the catalyst bed at the upstream end, where ethane and oxygen first come into contact with the ODH catalyst and where the risk of an uncontrollable temperature spike is highest.
[0012] Unless otherwise indicated in the examples of operation or elsewhere, all numbers or expressions used herein and in the claims relating to quantities of ingredients, reaction conditions, etc., should be understood in all cases to be modified by the term “approximately.” Therefore, unless otherwise indicated, the numerical parameters described herein and in the appended claims are approximations that may vary depending on the characteristics that this disclosure wishes to achieve. Each numerical parameter should be interpreted by applying ordinary rounding techniques, at least in light of the reported number of significant figures, not as an attempt to limit the application of the doctrine of equivalents to the claims.
[0013] <Definition> As used herein, the term "catalyst capacity" refers to the ability of a catalyst bed to convert ethane to ethylene and can be used to describe the entire catalyst bed, individual catalyst bed sections, or points along the length of the catalyst bed. Catalyst capacity depends on the catalyst composition, dilution ratio, and porosity.
[0014] As used herein, the term “catalyst bed” refers to one or more regions occupied by catalyst particles and, if present, heat dissipation particles, including the spaces between those particles. The region is intended to have a start and end point along the length of the reactor system.
[0015] As used herein, the term “catalyst bed length” refers to the length of the catalyst bed, starting from the upstream end where ethane and oxygen first come into contact with the ODH catalyst and ending at the downstream end where a final product flow is formed and ethane and oxygen can come into contact with the active ODH catalyst, excluding areas without catalyst. For example, in a multi-reactor system, the catalyst bed length is intended to include the entire length from the upstream end of the first catalyst bed section of the first reactor to the downstream end of the last catalyst bed section of the last reactor in the series, excluding intervening sections without catalyst. Similarly, in a single-reactor system with multiple catalyst bed sections separated by areas without ODH catalyst, the catalyst bed length is intended to cover the length from the upstream end of the first catalyst bed section to the downstream end of the last catalyst bed section, excluding intervening sections without ODH catalyst.
[0016] As used herein, the term “catalyst bed section” refers to a section or region within a catalyst bed that can be identified by changes in catalyst capacity in relation to adjacent catalyst bed sections. Adjacent catalyst bed sections may be continuous in that they share a common boundary, or they may be separated by areas without catalyst. Adjacent catalyst bed sections sharing a common boundary generally do not overlap, however, during the loading and settling of the catalyst bed, some catalyst particles may permeate from each section and fall across the boundary into adjacent sections. A catalyst bed section has a uniform distribution of the catalyst bed composition, including catalyst particles and, if present, heat dissipation particles of similar size and composition, and therefore has a uniform dilution ratio and uniform porosity.
[0017] As used herein, the term “catalyst particles” refers to particles loaded into a catalyst bed and containing an active ODH catalyst, and includes, but is not limited to, any catalytic additives, including binders, supports, and carriers, if present. The preparation of catalyst particles for use in the ODH process is within the scope of the expertise of those skilled in the art.
[0018] As used herein, the term "conversion rate" refers to the proportion of ethane carbon atoms in the feed that are converted into carbonaceous products, and can be calculated according to the following formula: TIFF2023547659000002.tif65155 In the formula, the net mass flow rate of converted C2H6 is equal to the mass flow rate of C2H6 in the supply flow rate minus the mass flow rate of C2H6 in the product flow rate.
[0019] As used herein, the term “dilution ratio” refers to the degree to which the catalyst is diluted by heat dissipation particles and catalyst additives (such as binders, carriers, and supports) in the entire catalyst bed or in individual catalyst bed sections. The dilution ratio is calculated according to the following formula: TIFF2023547659000003.tif20108
[0020] As used herein, the term “flammability envelope” refers to the envelope that defines the flammable zone in a mixture of fuel (e.g., ethane), oxygen, and a heat removal diluent gas.
[0021] As used herein, the term “gas space velocity per hour” refers to the ratio of the volumetric flow rate of the gas to the volume of the active phase in the catalyst bed, where the gas includes the reaction gas species and any heat-removed diluent gas under standard conditions (i.e., 0°C, 1 bar).
[0022] As used herein, the term “heat dissipation particles” refers to inert, non-catalytic particles. These particles can be used within a catalyst bed or one or more catalyst bed sections to improve cooling uniformity and reduce hot spots by increasing the radial heat transfer coefficient directly from the catalyst bed or catalyst bed sections to the reactor walls. The heat dissipation particles have the same or higher thermal conductivity than catalyst particles.
[0023] As used herein, the term “heat removal dilution gas” refers to a gas that can dilute a flow and remove heat from the flow.
[0024] As used herein, the term “inert metal rod” refers to a metal rod that is catalytically inactive, having a substantially cylindrical shape and having at least one dimension smaller than the inner diameter of the reactor. An inert metal rod may include a heat pipe. An inert metal rod may have fins.
[0025] As used herein, “ODH catalyst” refers to a catalyst that catalyzes the conversion of ethane to ethylene in the presence of oxygen. This term is intended to cover the final product of catalyst synthesis before the removal of catalyst additives, which include, but are not limited to, binders, carriers, and supports. Catalysts include all ODH catalysts known in the art, particularly the mixed metal oxide catalysts described herein. References to “catalysts” are intended to mean ODH catalysts unless otherwise indicated. References to ODH catalysts may include mixtures of different ODH catalysts (or catalyst species), all of which are capable of converting ethane to ethylene in the presence of oxygen. The term “catalyst species” may be used to refer to a catalyst having a specific empirical formula.
[0026] As used herein, the term “catalyst capacity profile” refers to the change in catalyst capacity along the length of the catalyst bed.
[0027] As used herein, the term "porosity" refers to the value obtained by dividing the volume of voids or inert spaces within the catalyst bed that are not occupied by catalyst particles or heat-dissipating particles by the total volume of the catalyst bed. It may be stated that the catalyst bed as a whole, or individual sections of the entire catalyst bed, have porosity.
[0028] As used herein, the term “residence time” refers to a measure of the amount of time a substance flowing through a volume spends within that volume.
[0029] As used herein, the term “space velocity per second” refers to the ratio of the mass flow rate of the gas to the mass of the active phase in the catalyst bed, when the gas contains the reactant gas species and any heat-removing diluent gases.
[0030] <Fixed-bed reactor system> ODH of ethane involves contacting a mixture of ethane and oxygen with one or more mixed metal oxide catalysts in one or more ODH reactors under conditions that promote oxidative conversion from ethane to ethylene, and can be carried out in various types of reactors, including conventional fixed-bed reactors, multi-tube (shell-and-tube) reactors, and tubular reactors. Figure 1 shows a catalyst bed 1 in an ODH reactor where catalyst particles 2 (dark gray circles) and heat dissipation particles 3 (light gray circles) of similar size are uniformly distributed in approximately equal numbers, with areas 4 (indicated by hatching) without catalyst particles on each side of the catalyst bed. The catalyst particles 2 and heat dissipation particles 3 are immobilized and contained by the sides of the reactor or tube and the areas 4. In the ODH of the ethane process, ethane and oxygen (indicated by hollow arrows) are introduced at the upstream end 5 of the reactor or tube, pass through the catalyst bed 1 where conversion occurs, and the product flow or outlet flow is taken out at the downstream end 6 of the reactor or tube. In a tubular reactor, the catalyst bed is contained within a single tube (reactor), whereas in a shell-and-tube reactor, the catalyst bed is contained across multiple tubes enclosed in a shell, with coolant flowing between the tubes.
[0031] Designing a fixed-bed reactor suitable for use with the reactor systems disclosed herein can follow known techniques for this type of reactor. Those skilled in the art will know what features are required with respect to shape and dimensions, reactant input, product output, temperature and pressure control, and means for immobilizing the catalyst. Fluidized bed reactors are not relevant to this disclosure, although they are known to be used for ethane ODH.
[0032] <Maximum process temperature> The ODH of ethane generates heat, and the upstream end, where ethane and oxygen first come into contact with the catalyst, typically shows the greatest temperature surge within the catalyst bed. As it moves downstream along the length of the catalyst bed, the temperature of the catalyst bed decreases and settles at a constant temperature (isotherm). The highest process temperature occurs, depending on the flow rate and / or flow velocity, typically within the first 10–40% of the length of the catalyst bed. A temperature gradient or temperature difference may exist from the center of the catalyst bed to the reactor wall. The temperature of the reactor wall is similar to the temperature of the coolant surrounding the reactor, and the ability of the coolant to remove heat from the reactor is tested when there is a larger temperature gradient. The larger the temperature gradient, the higher the risk of thermal runaway. The object of this disclosure is to minimize the risk of thermal runaway by minimizing the temperature difference.
[0033] ODH reactor systems are designed with cooling mechanisms to extract heat during operation and maintain the catalyst bed temperature at a steady or near-steady state. However, there remains a risk that a rapid rise in temperature may exceed the cooling capacity, leading to thermal runaway. To avoid this risk, operators can choose to reduce the amount of ethane and / or oxygen in the feed, taking into account the amount of catalyst loaded into the reactor. The effect is that less ethane is converted, thus reducing the catalyst capacity and, consequently, less heat is generated. Unfortunately, this reduces the ethylene yield, making it less cost-effective. If the reactor is made larger with a similar initial amount of ethane to achieve the same yield, theoretically, the larger volume will dilute the feed more, reducing the risk, but this may result in excessive capital investment and downtime. Alternatively, the reactor can be reloaded with less of the same catalyst, or with a less active catalyst, but the effect remains the same. Lower activity results in a lower yield.
[0034] In the setup described above in relation to Figure 1, the ethane conversion rate decreases from the upstream end to the downstream end, but the catalyst capacity along the length of the reactor, or the ability to convert ethane to ethylene, remains relatively constant. This is because catalyst particles of similar size and heat dissipation particles of similar size are uniformly distributed, and therefore all catalyst particles contain similar amounts of the same catalyst. The catalyst capacity profile, where catalyst particles and heat dissipation particles are uniformly distributed, will be constant or relatively constant along the length of the catalyst bed.
[0035] Embodiments of this disclosure relate to a fixed-bed reactor system for the oxidative dehydrogenation of ethane to ethylene, comprising a catalyst bed containing an ODH catalyst, wherein the catalyst capacity increases along the length of the catalyst bed. In some embodiments, the catalyst capacity increases gradually from the upstream end to the downstream end of the catalyst bed. In other embodiments, the catalyst capacity increases in one or more steps. The change in catalyst capacity along the length of the catalyst bed, or the catalyst capacity profile, is a function of the loading design, or how the catalyst particles are loaded and packed into the catalyst bed. The reactor system may include a single reactor or a plurality of reactors.
[0036] <Catalyst> To change the catalytic capacity of a catalyst bed, the user can either change the amount of catalyst present or change the composition of the catalyst. Changing the amount of catalyst is straightforward. Changing the composition requires changing the catalyst species that make up the catalyst. For a catalyst containing a single species, simple substitution with different catalyst species having different activities is possible, or one or more catalyst species can be added to form a catalyst containing multiple species. For a catalyst containing a mixture of two or more catalyst species, the contribution of each species present in the mixture can be adjusted, specific species can be removed from the mixture, or catalyst species that were not previously present can be added.
[0037] Catalyst species with different empirical formulas may exhibit different conversion rates under the same conditions. Comparing different catalysts for their ability to convert ethane to ethylene can be achieved by determining the temperature at which 35% conversion of ethane occurs. Determining the 35% conversion temperature can be done by loading the catalyst to be tested into a reactor, passing a feed containing ethane and oxygen over the catalyst under typical ODH operating conditions to form a product flow, and identifying the temperature at which 35% of the ethane is converted to the product. Loading large, commercial-sized reactors, especially shell-and-tube reactors with thousands of tubes, is time-consuming and not economically feasible for the purpose of determining the 35% conversion temperature of catalysts. Small-scale reactors or microreactor units (MRUs) are ideal for determining and comparing the 35% conversion temperatures of various catalyst species. For comparisons between catalyst species, it is necessary to load catalyst species of similar quantity, size, and shape into similar volumes and test them under identical ODH operating conditions (e.g., feed composition, pressure, flow rate). Detailed MRU settings are described below. Using these settings, the 35% conversion temperature can be evaluated for representative samples of individual catalyst species, mixtures of one or more catalyst species, catalyst particles, or catalyst beds or catalyst bed sections (catalyst bed compositions).
[0038] Catalysts with a lower 35% conversion temperature have a higher ability to convert ethane to ethylene compared to catalysts with a higher 35% conversion temperature. When comparing two different catalyst beds, where different catalysts are uniformly distributed, but the dilution ratio and porosity are the same or nearly the same, the catalyst bed with the lowest 35% conversion temperature will have a higher catalyst capacity.
[0039] <Dilution Ratio> The catalyst can be diluted in a catalyst bed by combining the catalyst with catalyst additives such as a support and / or binder to form catalyst particles. The catalyst bed can also be filled with heat dissipation particles, not just the catalyst or catalyst particles. The dilution ratio, i.e., the degree to which the catalyst is diluted by either or both the catalyst additives and / or heat dissipation particles, affects the catalyst capacity. The dilution ratio is calculated by dividing the total mass of the heat dissipation particles and catalyst additives (support, binder, etc.) by the total mass of the catalyst bed (the total mass of the catalyst plus the total mass of the heat dissipation particles and catalyst additives). Changing the dilution ratio of the catalyst bed can include changing the amount of catalyst relative to the heat dissipation particles present in the catalyst bed, and / or changing the amount of catalyst additive relative to the catalyst in the formation of the catalyst particles, or both.
[0040] The dilution ratios applicable to use in the fixed-bed reactor systems disclosed herein may theoretically range from 0.0 to about 0.95. However, with a few exceptions, most catalyst species require a binder to maintain their structural properties. The minimum amount of binder is generally about 5% by weight of the complete catalyst including the binder, and the dilution ratio is 0.05 when no heat dissipation particles are present on the catalyst bed.
[0041] Examples of heat dissipation particles include, for example, DENSTONE® 99 (Saint-Gobain Ceramics & Plastics, Inc.) alumina particles, or SS316 particles, or inert metal rods that can be inserted to create inert spaces within the catalyst bed. Inert, non-catalytic heat dissipation particles can be used in one or more ODH reactors. The heat dissipation particles may be present within the catalyst bed and comprise one or more non-catalytic inert particles having a melting point at least about 50°C higher than the upper temperature control limit of the reaction, at least about 250°C higher than the upper temperature control limit of the reaction in some embodiments, and at least about 500°C higher than the upper temperature control limit of the reaction in further embodiments. The heat dissipation particles may have particle sizes in the range of about 0.5 to about 15 mm, in some embodiments about 0.5 to about 7.5 mm, and in some embodiments about 1.0 to about 5.0 mm. The heat dissipation particles may have a thermal conductivity greater than about 30 W / mK (watts / meter Kelvin) within the reaction temperature control limit. In some embodiments, the heat dissipation particles are metal alloys and compounds having a thermal conductivity greater than about 50 W / mK (watts / meter-kelvin) within the reaction temperature control limit. Non-limiting examples of suitable metals that can be used in these embodiments include, but are not limited to, silver, copper, gold, aluminum, steel, stainless steel, molybdenum, and tungsten. The heat dissipation particles can be added to the catalyst bed in an amount of about 5 to about 95% by weight, about 30 to about 70% by weight in some embodiments, and about 45 to about 60% by weight in other embodiments, based on the total weight of the catalyst bed. The particles are used to improve cooling uniformity and reduce hot spots within the catalyst bed by directly transferring heat to the reactor walls. The heat dissipation particles can optionally be pressed or extruded together with the catalyst in the formation of the catalyst particles.
[0042] Lowering the dilution ratio of the catalyst bed has the effect of increasing the catalyst capacity. In a comparison of two different catalyst beds, if the same catalyst is uniformly distributed in each and they have the same or nearly the same porosity, the catalyst bed with a lower dilution ratio will have a higher catalyst capacity.
[0043] <Void Fraction> When catalyst particles, and possibly heat dissipation particles, are packed into a catalyst bed, spaces are created between the particles, resulting in porosity. Porosity can be altered by changing the size and shape of the catalyst particles and / or heat dissipation particles. For example, larger particles result in more void space. Also, ring-shaped catalyst particles will have a higher porosity than discs of similar diameter and thickness. Determining porosity is the prerogative of those skilled in the art. The chosen method for measuring porosity is irrelevant if the same method is used when comparing catalyst bed compositions.
[0044] Porosity can be calculated using the size, shape, and quantity of each component in the catalyst bed. If the particle size and shape are known, software programs are available to calculate porosity assuming random packing. Porosity can also be measured by dispensing a sample of the catalyst bed into a container at room temperature and atmospheric pressure to its full capacity, and then filling the container with a low-viscosity fluid. The porosity can then be determined by dividing the amount of low-viscosity fluid required to fill the container by the volume of the container. Selecting a low-viscosity fluid that does not penetrate much into the catalyst bed components (is absorbed into the pores) or dissolves the catalyst bed components is within the scope of the expertise of those skilled in the art. Suitable examples include, but are not limited to, oil (for water-absorbing catalyst bed components) and water (for hydrophobic catalyst bed components). For low-viscosity liquids, time is required for diffusion throughout the material and for bubbles to detach from the catalyst bed (typically about 15 minutes). It is important that the catalyst bed fills the container to a volume that simulates loading and packing in a reactor. The size of the container can be any size, as long as it allows for the same level of filling as the reactor. For example, when filling a reactor tube with an inner diameter of 0.5 inches with a catalyst bed, a cylindrical container with an inner diameter of 0.5 inches might be ideal. The length of the cylinder should ideally be 6 inches or more.
[0045] In some embodiments of this disclosure, the porosity is 0.30 to 0.70. In some embodiments of this disclosure, the porosity is 0.30 to 0.60. In some embodiments of this disclosure, the porosity is 0.40 to 0.50.
[0046] By changing the porosity, the operator reduces the surface area of the catalyst per unit fixed volume of the catalyst bed. This effect is due to a reduction in the number of active sites on the catalyst surface where the majority of the ethane-to-ethylene conversion occurs, thereby reducing the catalyst capacity. When comparing two different catalyst beds, each having a similar uniform distribution of catalyst particles and similar dilution ratios, but with different porosities, the catalyst bed with lower porosity will have a higher catalyst capacity.
[0047] <Gradual Increase> Figure 2 shows catalyst bed 1 in which the dilution ratio gradually decreases along the length of the catalyst bed. As shown in Figure 2, along the catalyst bed from the upstream end 5 to the downstream end 6, the frequency of thermally diluted particles 3 gradually decreases and the frequency of catalyst particles 2 increases. The effect is to increase the catalyst capacity from the upstream end to the downstream end.
[0048] In some embodiments of the present disclosure, the dilution ratio gradually decreases along the length of the catalyst bed, so that the catalyst capacity gradually increases along the length of the catalyst bed.
[0049] It is also conceivable to provide a catalyst bed in which the 35% conversion temperature gradually increases from the upstream end to the downstream end. The 35% conversion temperature can be gradually increased by using a mixture of catalyst particles, each having a different 35% conversion temperature. From the upstream end to the downstream end, the frequency of catalyst particles with higher 35% conversion temperatures may decrease, and the frequency of catalyst particles with lower 35% conversion temperatures may increase. The 35% conversion temperature of a catalyst bed section is the average value of the 35% conversion temperatures of different catalyst particle types, taking weight fraction into account, at each point along the length of the catalyst bed section.
[0050] In some embodiments of this disclosure, the catalyst capacity gradually increases along the length of the catalyst bed because the 35% conversion temperature of the catalyst particles gradually decreases along the length of the catalyst bed.
[0051] It is also conceivable to provide a catalyst bed in which the porosity gradually decreases from the upstream end to the downstream end. The porosity can be gradually reduced by using a mixture of catalyst particles having different sizes and / or shapes. From the upstream end to the downstream end, the frequency of less densely packed catalyst particles (creating more void space) may decrease, while the frequency of more densely packed catalyst particles may increase.
[0052] In some embodiments of this disclosure, the porosity gradually decreases along the length of the catalyst bed, so the catalyst capacity gradually increases along the length of the catalyst bed.
[0053] <Catalyst Capacity Steps> Shell-and-tube reactors can have thousands of tubes, and loading the catalyst bed while gradually increasing the catalyst capacity along the length of each tube seems feasible and beneficial, but logistically difficult and costly. Developing a cost-effective method for loading thousands of tubes while increasing the catalyst capacity profile would be beneficial. However, in practice, it may be simpler and more cost-effective to divide the catalyst bed into sections with different uniform catalyst capacities. This is a catalyst bed with sections of different uniform catalyst capacities, where a first upstream section is followed by one or more subsequent sections, each section having an upstream end and a downstream end, ending with a final downstream section. Except for the first upstream section and the final downstream section, each section can be an upstream or downstream section in relation to its adjacent sections. For example, in a 4-section catalyst bed, the second section is a downstream section relative to the first upstream section and an upstream section relative to the third section, and the third section is a downstream section relative to the second section and an upstream section relative to the final downstream section. The sections may be continuous or separated by regions without a catalyst.
[0054] In some embodiments, the catalyst bed includes at least two non-overlapping catalyst bed sections arranged in series along the length of the catalyst bed, each catalyst bed section having an upstream end and a downstream end, with one or more downstream sections following a first upstream catalyst bed section, the last catalyst bed section ending at the downstream end of the catalyst bed, and the catalyst bed sections are identified by a change in catalyst capacity, with each catalyst bed section having a higher catalyst capacity than the preceding upstream catalyst bed section.
[0055] Figure 3 is a schematic diagram of catalyst bed 1 housed in a single reactor and including an upstream section 7 and a downstream section 8 (shown in parentheses). The sections are continuous, but the catalyst capacity changes as shown by the dashed lines. Each section extends approximately half the length of the catalyst bed and is filled with a similar total number of catalyst particles and heat dissipation particles of similar size. The dilution ratio of upstream section 7 is higher than that of downstream section 8 because it contains more heat dissipation particles 3 compared to the catalyst particles 2 in that section. The catalyst capacity of upstream section 7 is lower than that of downstream section 8.
[0056] In some embodiments of the present disclosure, one or more catalyst bed sections have a lower dilution ratio than the previous catalyst bed section.
[0057] In some embodiments of the present disclosure, one or more catalyst bed sections have a lower dilution ratio than the previous catalyst bed section, and those catalyst bed sections contain a similar amount of the same catalyst.
[0058] The dilution ratio of the catalyst bed section can range from 0 (when there are no heat dissipation particles or catalyst additives) to 0.95 (when heat dissipation particles or catalyst additives constitute 95% of the mass of the catalyst bed section). While it is possible to fill the catalyst bed with catalyst only, this may be technically limited, and preferably the dilution ratio of the catalyst bed section is in the range of 0.30 to 0.9, more preferably in the range of 0.50 to 0.80.
[0059] In some embodiments of the present disclosure, the reactor system includes one or more catalyst bed sections having a dilution ratio of 0.00 to 0.95. In some embodiments of the present disclosure, the reactor system includes one or more catalyst bed sections having a dilution ratio of 0.30 to 0.90. In some embodiments of the present disclosure, the reactor system includes one or more catalyst bed sections having a dilution ratio of 0.50 to 0.80.
[0060] The greater the difference in dilution ratio between catalyst bed sections, the greater the expected impact on the corresponding maximum process temperature and, consequently, the temperature difference. The greatest impact occurs when an upstream catalyst bed section with a dilution ratio of 0.75 is followed by a downstream catalyst bed section with a dilution ratio of 0 (no heat-dissipating particles), which is 100% lower. Even small differences, including a difference of around 2%, may prove beneficial.
[0061] In some embodiments, one or more catalyst bed sections have a dilution ratio 2 to 100% lower than that of the previous section. In some embodiments, one or more catalyst bed sections have a dilution ratio 5 to 70 percent lower than that of the previous section. In some embodiments, one or more catalyst bed sections have a dilution ratio 10–50% lower than that of the previous section.
[0062] <35% conversion temperature> Figure 4 is a schematic diagram of catalyst bed 1 housed in a single reactor and including an upstream section 7 and a downstream section 8. The sections are continuous, but the catalyst capacity changes as shown by the dashed lines. The sections are of similar size, each filled with a similar total number of catalyst particles and heat dissipation particles, and cover approximately half the length of the catalyst bed. The 35% conversion temperature of the upstream section 7 is higher than that of the downstream section 8. This is because the downstream section 8 contains potent catalyst particles 9 (black circles) which have a lower 35% conversion temperature than catalyst particles 2. The 35% conversion temperature in the downstream section 8, which contains a mixture of catalyst particles 2 and the more potent catalyst particles 9, is, on average, lower than the 35% conversion temperature in the upstream section 7, where all catalyst particles are catalyst particles 2. This loading design gives the downstream section 8 a higher catalyst capacity.
[0063] In some embodiments of the present disclosure, one or more catalyst bed sections have a 35% conversion temperature lower than that of the previous catalyst bed section.
[0064] In some embodiments of the present disclosure, one or more catalyst bed sections have a catalyst having a 35% conversion temperature lower than the catalyst in the preceding catalyst bed section, and these catalyst bed sections have similar dilution ratios and porosity.
[0065] In some embodiments, the reactor system comprises an upstream bed section and a downstream bed section, the upstream and downstream bed sections having similar dilution ratios and porosity, and the catalyst in the downstream bed section having a 35% conversion temperature higher than the catalyst in the upstream bed section.
[0066] In some embodiments, the reactor system comprises an upstream bed section and a downstream bed section, the upstream and downstream bed sections having similar dilution ratios and porosity, the catalyst in the downstream bed section having a 35% conversion temperature higher than the catalyst in the upstream bed section, and the catalyst in one or both of the upstream and downstream bed sections containing two or more catalyst species.
[0067] Figure 5 is a schematic diagram of catalyst bed 1 housed in a single reactor and including an upstream section 7 and a downstream section 8. The sections are continuous, but the catalyst capacity changes as shown by the dashed lines. The sections are similar in size, and each is packed with catalyst particles and heat dissipation particles in similar numbers per unit volume, covering approximately half the length of the catalyst bed. The 35% conversion temperature of the upstream section 7 is higher than that of the downstream section 8. This is because the downstream section 8 contains powerful catalyst particles 9 (black circles) with a lower 35% conversion temperature than catalyst particles 2. This loading design gives the downstream section 8 a higher catalyst capacity. The upstream section 7 and the downstream section 8 may be different in size so that the proportion of the catalyst bed length is unevenly divided between the two sections.
[0068] In some embodiments, the reactor system consists of an upstream bed section and a downstream bed section, the upstream bed section and the downstream bed section having similar dilution ratios and porosity. The catalyst in the downstream bed section has a 35% higher conversion temperature than the catalyst in the upstream bed section. The catalyst in either or both of the upstream and downstream bed sections comprises two or more catalyst species. The upstream and downstream sections constitute 0.2 to 0.8 of the catalyst bed length.
[0069] Figure 6 is a schematic diagram of catalyst bed 1, housed in a single reactor and containing an upstream section 7 and a downstream section 8. The sections are continuous, but the catalyst capacity changes as indicated by the dashed lines. The sections are unequal in size, with the upstream section 7 extending approximately one-third of the catalyst bed length, and the downstream section 8 extending the last two-thirds of the catalyst bed length. The upstream section 7 contains catalyst particles and heat dissipation particles that are larger in size than those in the downstream section 8. Furthermore, the catalyst particles and heat dissipation particles in the downstream section 8 include not only smaller particles but also particles of varying sizes. As a result, the downstream section 8 is more densely packed and has a much lower porosity. Since the amount of catalyst per unit volume and the dilution ratio of the sections are similar, the catalyst capacity of the downstream section 8 is higher than that of the upstream section 7.
[0070] In some embodiments of the present disclosure, one or more catalyst bed sections have a lower porosity than the previous catalyst bed section.
[0071] In some embodiments, the reactor system comprises an upstream bed section and a downstream bed section, the upstream and downstream bed sections having similar types and amounts of catalyst, as well as similar dilution ratios and porosities, wherein the porosity of the upstream section is higher than that of the downstream section.
[0072] Similar to dilution ratios, a larger difference in porosity between catalyst bed sections is expected to have a greater impact on the maximum process temperature and temperature difference. The greatest effect occurs when an upstream catalyst bed section with a maximum porosity of 0.7 is followed by a downstream catalyst bed section with the lowest possible porosity of 0.3, which is 57.1% lower. It is thought that even small differences, including a difference of about 2.0%, may prove beneficial. In some embodiments, one or more catalyst bed sections have a porosity 2.0–57% lower than the preceding section.
[0073] In some embodiments of the present disclosure, one or more catalyst bed sections have a porosity 5.0 to 45% lower than that of the previous catalyst bed section. In some embodiments of the present disclosure, one or more catalyst bed sections have a porosity 10 to 25% lower than that of the previous catalyst bed section.
[0074] The catalyst bed sections may be separated by catalyst-free regions. Figures 7 and 8 are schematic diagrams of catalyst beds housed in a single reactor. Figure 7 shows an upstream section 7 and a downstream section 8, and Figure 8 shows an additional intermediate section 10 adjacent to the upstream section 7 and the downstream section 8. In Figure 7, a catalyst-free intervening region 11 separates the two sections, and in Figure 8, the intervening region 11 separates the upstream section 7 and the intermediate section 10. The intervening region 11 is similar to region 4 in that it can support the catalyst bed sections by fixing its components and prevent displacement during operation. The intervening region can be any material that allows the feed gas and product gas to pass through the reactor and from one catalyst bed section to the next. Examples of intervening regions include, but are not limited to, sections of heat dissipation particles, partitions, static mixers, or any material or structure that prevents catalyst particles and heat dissipation particles from passing between sections. For example, in a vertically oriented reactor, a partition plate with holes too small in diameter for catalyst particles to pass through prevents the catalyst particles from falling into the lower section while allowing the process gas to pass through. Selecting the appropriate material or design for the intervening area is within the scope of the expertise of those skilled in the art.
[0075] A catalyst bed can include catalyst bed sections that extend across one or more reactors, with each reactor containing one or more catalyst bed sections. Figure 9 is a schematic diagram of a catalyst bed extending across two reactors (indicated by dotted boxes), where the first reactor 12 includes two catalyst bed sections (upstream section 7 and intermediate section 10), and the second reactor 13 includes a downstream section 8. In this scenario, the intermediate section 10 is separated from the downstream section 8 by a connection between the first and second reactors. The sections in Figure 9 are in series, and the upstream section 7 has the lowest catalyst capacity because it has a larger porosity than the intermediate section 10, which has an intermediate catalyst capacity. The downstream section 8 has the highest catalyst capacity because it has a similar porosity to the intermediate section 10 and contains more potent catalyst particles 9.
[0076] In some embodiments, the reactor system includes two or more catalyst bed sections that extend across two or more reactors.
[0077] In some embodiments, the reactor system includes two or more catalyst bed sections, each containing a different catalyst.
[0078] <Method for preparing a fixed-bed reactor> Loading a fixed bed into a reactor is within the scope of knowledge of those skilled in the art. The operator typically selects a specific type, size, and shape of catalyst particles (including whether the catalyst particles contain catalyst additives) and a type, size, and quantity of heat dissipation particles. The catalyst bed composition is prepared by mixing all components before loading to promote uniform distribution. Typically, fixed bed reactors for ODH are vertically positioned, and the catalyst bed composition is simply poured into tubes, or into multiple tubes of a shell-and-tube reactor, by hand or using robotic means, at a rate slow enough to allow for high-density filling. The catalyst particles and heat dissipation particles, which are components of the catalyst bed, settle naturally. The result is a fixed bed reactor with a catalyst bed in which catalyst particles and heat dissipation particles are uniformly distributed, and the catalyst bed has a uniform catalyst capacity. Expertise in loading reactors in this manner is common.
[0079] Provided herein is a method for loading a catalyst bed into a fixed-bed reactor, wherein the catalyst bed comprises one or more non-overlapping sections arranged sequentially from the upstream end to the downstream end of the catalyst bed, with the catalyst capacity increasing from the upstream end to the downstream end.
[0080] Provided herein is a method for loading a catalyst bed into a fixed-bed reactor for the oxidative dehydrogenation of ethane, wherein the fixed-bed reactor has an upstream end and a downstream end, and the method is A step of preparing two or more catalyst bed compositions containing an ODH catalyst, A step of determining the catalyst capacity for each catalyst bed composition, The process involves pouring the catalyst bed composition into a fixed-bed reactor sequentially and separately at a rate slow enough to allow for high-density and random packing, pouring the catalyst bed composition with the lowest catalyst capacity into the upstream end and the catalyst bed composition with the highest catalyst capacity into the downstream end. The process includes fixing the poured catalyst bed composition in a fixed-bed reactor to form a loaded catalyst bed, Here, the catalyst bed composition forms separate catalyst bed sections, which are identified by a change in catalyst capacity, and the catalyst capacity increases from the upstream end to the downstream end.
[0081] Provided herein is a method for loading a catalyst bed into a fixed-bed reactor comprising one or more tubes, wherein each tube has an upstream end and a downstream end, and the method is: A step of preparing two or more catalyst bed compositions containing an ODH catalyst, A step of evaluating the catalyst capacity for each catalyst bed composition and ordering the catalyst bed compositions from the lowest relative catalyst capacity to the highest relative catalyst capacity. The process involves sequentially pouring catalyst bed compositions into one or more tubes of a fixed-bed reactor, at a rate slow enough to allow for high-density, random packing, with the catalyst bed composition having the lowest catalyst capacity being poured into the upstream end and the catalyst bed composition having the highest catalyst capacity being poured into the downstream end. A step of fixing the poured catalyst bed composition inside one or more tubes. Includes, Here, the catalyst bed composition forms separate catalyst bed sections, which are identified by a change in catalyst capacity, and the catalyst capacity increases from the upstream end to the downstream end.
[0082] The preparation of catalyst bed compositions is within the scope of the knowledge of those skilled in the art. To design a fixed-bed reactor having one or more sections with different catalyst capacities, operators can vary the relevant factors of catalyst composition, dilution ratio, and / or porosity. To evaluate the differences in catalyst capacity of catalyst bed compositions, operators can consider comparing their properties and predicting which composition will have a higher catalyst capacity. This may be straightforward if two of the factors are identical. For example, catalyst bed compositions having the same catalyst composition and dilution ratio but significantly different porosity will clearly have different catalyst capacities, and it will be obvious that the catalyst bed composition with the smallest porosity will have a larger catalyst capacity. In particular, if the difference is large in one relevant factor, the prediction may be straightforward. However, if two or more factors are different, the prediction may or may not be reliable. It is preferable to compare the relative 35% conversion temperatures of the catalyst bed compositions as a whole.
[0083] In some embodiments of this disclosure, catalyst capacity is evaluated by ordering catalyst bed compositions by relative 35% conversion temperature, where the catalyst bed composition having the highest relative 35% conversion temperature corresponds to the catalyst bed composition having the lowest relative catalyst capacity.
[0084] Evaluating the 35% conversion temperature of a catalyst bed composition involves loading a sample of the catalyst bed composition into a miniature reactor unit and passing the feed through the reactor while monitoring the temperature and ethane conversion rate within the reactor. Different process conditions, such as feed composition, pressure, and flow rate, can result in different 35% conversion temperatures for a particular catalyst bed composition. "Relative" catalyst capacity means that while the actual 35% conversion temperature is relevant, it is not essential for comparing two or more catalyst bed compositions. Rather, it is important to compare the 35% conversion temperatures of each composition relative to others, thereby establishing a ranking.
[0085] The MRU may include reactor tubes made from stainless steel tubing (e.g., SWAGELOK® Tubing) and have a size that allows for the loading of catalyst bed compositions, reflecting the loading into a fixed-bed reactor intended for use in an ODH process. Ideally, the MRU reactor tubes share the same inner and outer diameters as the tubes or multiple tubes of the fixed-bed reactor in question. While not required, the length of the MRU tubes must be sufficient to allow for steady-state operation. A length in the range of 6 inches to 3 feet would be ideal. A movable thermocouple or multipoint thermocouple (e.g., WIKA Instruments Ltd.'s 6-point K-type thermocouple) can be inserted into the MRU reactor tubes to measure and control the temperature within the catalyst bed. A room-temperature stainless steel condenser can be placed behind the MRU reactor tubes to collect water and acetic acid condensates. The gas product flow may be fed into a gas chromatograph (e.g., GC; Agilent 6890N Gas Chromatograph, Using Chrom Perfect-Analysis, Version 6.1.10 for data evaluation) and the levels of various chemical species present in the product flow may be measured to monitor conversion and selectivity.
[0086] Samples of catalyst bed compositions are tested separately. The test is carried out by slowly loading the composition into the MRU reactor tube to ensure dense loading. A pre-mixed feed gas containing ethane and oxygen, and optionally an inert diluent, can be supplied to the reactor under standardized flow and pressure conditions. The feed composition and standardized conditions can be selected by the operator to approximate the conditions of a typical ODH process, and these conditions must be identical for all catalyst bed composition tests in order to properly evaluate the "relative" 35% conversion temperature. A typical feed composition may include 20 mol% ethane, 10 mol% oxygen, and 70 mol% inert diluent (e.g., nitrogen). The pressure may be atmospheric pressure, and the flow rate 2.0–3.5 h -1The WHSV can be kept constant. The temperature can also be gradually increased while monitoring the ethane conversion rate. The 35% conversion temperature is the temperature at which 35% conversion occurs during steady-state operation.
[0087] By loading the fixed-bed reactor described herein, a method for controlling or limiting the maximum process temperature under steady-state operating conditions becomes possible. Cooling systems for ODH processes are typically designed relative to the process isotherm, and temperatures close to the isotherm are easily controlled. In multi-tube (shell-and-tube) reactors, larger tube diameters compared to smaller ones can potentially increase ethylene yield. However, larger tubes result in a greater temperature difference between the internal core of the catalyst bed (where the temperature is highest) and the tube walls. The coolant temperature approaches the isotherm temperature and becomes nearly the same as the tube wall temperature. In regions where the temperature rises sharply or the catalyst bed temperature exceeds the isotherm temperature, there is a risk of thermal runaway if the temperature difference exceeds the cooling system's ability to remove heat. Typically, the maximum process temperature is observed in the first 20% of the catalyst bed length, where exothermic conversion is highest and heat is released. The temperature difference between the highest reaction temperature in the first section of the oxidative dehydrogenation reactor catalyst bed and the temperature in the subsequent catalyst bed section can be approximately 1 to 50°C, or approximately 2 to 30°C, and in some cases, approximately 5 to 20°C. Typically, the larger the diameter of the reactor tube, the greater the temperature difference. Larger diameter tubes offer the opportunity to improve yields, but they also carry the risk of thermal runaway due to the large temperature difference. Loading larger diameter reactor tubes with increased catalyst capacity offers the opportunity to improve yields without the risk of thermal runaway.
[0088] Reducing the catalyst capacity in the upstream section decreases heat release due to conversion and the associated exothermic reaction, minimizing the risk of uncontrollable temperature spikes. Furthermore, compared to a scenario where the upstream section has a similar catalyst capacity and the supply ethane is depleted to low levels before reaching the downstream section, more ethane is available, potentially allowing the downstream section to contribute more to conversion. Finally, another potential benefit is that having a higher catalyst capacity at the downstream end provides an opportunity to consume residual oxygen, potentially lowering oxygen levels in the product stream and avoiding risks associated with processing in the presence of oxygen. The product stream typically passes through a separation train that includes a carbon dioxide removal step with an oxygen-sensitive amine column, and oxygen accumulation within the separation train can form an explosive mixture.
[0089] Varying the catalyst capacity profile between different tubes in a shell-and-tube reactor is conceivable but impractical because variations in isotherms between tubes would impose difficulties on the operator in controlling the cooling.
[0090] <ODHプロセス> The fixed-bed reactor systems described herein can be used for ODH processes, and typical conditions are described below. Conditions within the reactor are controlled by the operator and include, but are not limited to, parameters such as temperature, pressure, and flow rate. Conditions vary and can be optimized with respect to specific ethane / oxygen feed composition, specific mixed metal oxide catalysts, or whether a thermal removal diluent gas is used in mixing the reactants. An ODH reactor for dehydrogenating ethane to ethylene includes at least one feed stream containing oxygen and 20% by volume or more of ethane, and at least one outlet stream containing ethylene, unreacted ethane, one or more carboxylic acids, water, and oxygen.
[0091] The use of an ODH reactor to carry out an ODH process consistent with this disclosure is within the knowledge of those skilled in the art. ODH of ethane can be carried out as follows: the maximum process temperature can be about 300°C to about 450°C, in some cases about 300°C to about 425°C, in other cases about 300°C to about 400°C, in some cases about 310°C to about 350°C; the pressure can be about 0.5 to about 100 psig (3.447 to 689.47 kPag), in some cases about 15 to about 50 psig (103.4 to 344.73 kPag); and the residence time in the ODH reactor, with the volume of the activated mixed metal oxide catalyst as the numerator and the flow rate of the feed gas as the denominator, can be about 0.002 to about 30 seconds, in some cases about 1 second to about 10 seconds.
[0092] In embodiments, the ODH process has a selectivity for ethylene of over approximately 85%, and in some cases, over approximately 90%. The flow of reactants and heat-removed diluent gases can be described in any number of ways known in the art. Typically, flow is described and measured in relation to the volume of all feed gas (reactants and diluents) passing through the volume of the activated catalyst bed per hour, or gas space velocity per hour (GHSV). GHSV is approximately 50 to approximately 10,000 h -1 It can be set to a range of approximately 500 hours. -1 ~approximately 1000h -1 The flow rate can also be measured as weight per hour space velocity (WHSV), which represents the flow of gas exceeding the weight of the activated catalyst per hour, excluding the heat removal diluent, expressed in weight rather than volume. WHSV is approximately 0.5h -1 ~about 18.75h -1 Depending on the situation, it can take approximately 1.0 to 10.0 hours. -1 It may also be within that range.
[0093] The gas flow through the ODH reactor can also be described as the linear velocity (m / s) of the gas flow, which in this art is defined as the gas flow rate divided by the reactor cross-sectional area, divided by the porosity of the mixed metal oxide catalyst bed. The flow rate generally refers to the sum of the volumetric flows of all gases entering the reactor at standard temperature and pressure (i.e., 0°C and 1 bar), measured at the temperature and pressure at the point where oxygen and ethane first come into contact with the mixed metal oxide catalyst. The cross-section of the ODH reactor is also measured at the inlet to the mixed metal oxide catalyst bed. The linear velocity can range from approximately 5 cm / sec to approximately 1500 cm / sec, and in some cases from approximately 10 cm / sec to approximately 500 cm / sec.
[0094] The space-time yield (productivity) of ethylene per 1 kg g / hour of mixed metal oxide catalyst is, at approximately 350 to 400°C, often over 200, sometimes over 500, sometimes over 900, sometimes exceeding 1500, sometimes exceeding 3000, and under certain conditions exceeding 3500. It should be noted that the productivity of mixed metal oxide catalysts increases with increasing temperature until the selectivity decreases.
[0095] Mixtures of ethane and oxygen are often composed in ratios that fall outside the flammable envelope. For example, the ratio of ethane to oxygen may be outside the upper limit of the flammable envelope. In this case, the percentage of oxygen in the mixture is about 30% by volume or less, sometimes about 25% by volume or less, and otherwise about 20% by volume or less. This percentage of oxygen in the mixture depends on the temperature up to the reactor inlet, and is therefore often conditional on remaining outside the flammability limit before entering the reactor tubes. Within the reactor tubes, oxygen may be within the flammable envelope, but the catalyst bed itself may act as a flame arrestor. If preheating is carried out completely to the reaction temperature, the oxygen can be reduced to about 10%.
[0096] When the oxygen ratio is high, the ratio of ethane may be selected to keep the mixture outside the flammable envelope, if possible. Those skilled in the art can determine the appropriate level, but it is recommended that the ratio of ethane does not exceed 40% by volume. If the mixed gas before ODH contains 20% by volume of oxygen and 40% by volume of ethane, the remainder needs to be supplemented with a heat removal diluent gas (such as one or more of nitrogen, carbon dioxide, and steam). The heat removal diluent gas needs to be in a gaseous state under the conditions at the reactor inlet and inside the reactor and should not increase the flammability of the hydrocarbons added to the reactor, which are characteristics that those skilled in the art will understand when determining which heat removal diluent gas to employ. The heat removal diluent gas can be added to either the ethane-containing gas or the oxygen-containing gas before entering the ODH reactor, or can be added directly to the ODH reactor.
[0097] Mixtures that fall within the flammable envelope are not ideal but may be employed when the mixture is present under conditions that prevent the propagation of an explosion event. That is, the flammable mixture is produced within a medium in which ignition is immediately extinguished. For example, a user can design a reactor in which oxygen and ethane are mixed in that they are surrounded by a flame suppressant. Any ignition is extinguished by the surrounding flame suppressant. Flame suppressants include, but are not limited to, metal or ceramic parts such as stainless steel walls and ceramic supports. Another possibility is to mix oxygen and ethane at a low temperature such that ignition does not lead to an explosion and introduce them into the reactor before raising the temperature. Flammable conditions do not exist until the mixture is surrounded by a flame retardant within the reactor.
[0098] <ODH catalyst> Any of the mixed metal oxide catalysts used as ODH catalysts known in the art are suitable for use in the methods disclosed herein. Non-limiting examples of suitable oxidative dehydrogenation catalysts include those comprising one or more mixed metal oxide catalysts selected from the following: i) A catalyst of the following formula: <out Mo a V b Te c Nbd Pd e O f (In the formula, a, b, c, d, e, and f are the relative atomic weights of the elements Mo, V, Te, Nb, Pd, and O, respectively; a=1, b=0.01~1.0, c=0.01~1.0, d=0.01~1.0, 0.00≦e≦0.10, and f is the number that satisfies at least the valence states of the metal present in the catalyst); ii) The catalyst of the following formula: Ni g A h B i D j O f (In the formula, g is a number between 0.1 and 0.9, often between 0.3 and 0.9, otherwise between 0.5 and 0.85, and possibly between 0.6 and 0.8; h is a number between 0.04 and 0.9; i is a number between 0 and 0.5; j is a number between 0 and 0.5; f is a number that satisfies at least the valence state of the metal in the catalyst; A is Ti, Ta, V, Nb, Hf, W, Y, Zn, Zr, Si, and Al or similar) These are selected from mixtures; B is selected from La, Ce, Pr, Nd, Sm, Sb, Sn, Bi, Pb, Tl, In, Te, Cr, Mn, Mo, Fe, Co, Cu, Ru, Rh, Pd, Pt, Ag, Cd, Os, Ir, Au, Hg, and mixtures thereof; D is selected from Ca, K, Mg, Li, Na, Sr, Ba, Cs, Rb, and mixtures thereof; O is oxygen. iii) Catalyst of the following formula: Mo a E k G l O f (wherein E is selected from Ba, Be, Ca, Cr, Mn, Nb, Ta, Ti, Te, V, W and mixtures thereof; G is selected from Al, Bi, Ce, Co, Cu, Fe, K, Mg, V, Ni, P, Pb, Sb, Si, Sn, Ti, U and mixtures thereof; a=1; k is 0-2; l=0-2, where the sum of l for Co, Ni, Fe and mixtures thereof is less than 0.5; f is the number that satisfies at least the valence states of the metals in the catalyst); iv) The catalyst of the following formula: V mMo n Nb o Te p Me q O f (wherein Me is selected from Ta, Ti, W, Hf, Zr, Sb and mixtures thereof; m is 0.1 to 3; n is 0.5 to 1.5; o is 0 to 3; p is 0.001 to 5; q is 0 to 2; f is a number that satisfies at least the valence state of the metal in the catalyst); and v) The catalyst of the following equation: Mo a V r X s Y t Z u M v O f (In the formula, X is at least one of Nb and Ta; Y is at least one of Sb and Ni; Z is at least one of Te, Ga, Pd, W, Bi and Al; M is at least one of Be, Fe, Co, Cu, Cr, Ti, Ce, Zr, Mn, Pb, Mg, Sn, Pt, Si, La, K, Ag and In; a=1.0 (normalized); r=0.05~1.0; s=0.001~1.0; t=0.001~1.0; u=0.001~0.5; v=0.001~0.3; f is the number that satisfies at least the valence states of the metal in the catalyst).
[0099] If the catalyst is prepared using a conventional hydrothermal process, it may have the following equation: Mo 1.0 V 0.25-0.45 Te 0.10-0.16 Nb 0.15-0.19 O d (In the formula, d is the number that satisfies at least the valence states of the metal in the catalyst).
[0100] Embodiments of the ODH catalyst material are mixed metal oxides having the following formula: Mo1V 0.1-1 Nb 0.1-1 Te 0.01-0.2 X 0-0.2 O f (In the formula, X is selected from Pd, Sb, Ba, Al, W, Ga, Bi, Sn, Cu, Ti, Fe, Co, Ni, Cr, Zr, Ca, and their oxides and mixtures, and f is the number that satisfies the valence state of the metal present in the catalyst.)
[0101] Embodiments of the ODH catalyst material are mixed metal oxides containing Mo, V, O, and iron (Fe). The molar ratio of Mo to V can be 1:0.25 to 1:0.50, or 1:0.30 to 1:0.45, or 1:0.30 to 1:0.35, or 1:0.35 to 1:0.45. The molar ratio of Mo to Fe can be 1:0.25 to 1:5.5, or 1:3 to 1:5.5, or 1:4.25 to 1:4.75, or 1:4.45 to 1:4.55, or 1:0.1 to 1:1, or 1:0.25 to 1:0.75, or 1:0.4 to about 1:0.6, or about 1:0.4, or about 1:0.6, or 1:1.3 to 1:2.2, or 1:1.6 to 1:2.0, or 1:1.80 to 1:1.90. Furthermore, oxygen is present in an amount that satisfies the valence of at least the present metal oxide. The catalyst may have at least a portion of Fe in the catalyst material that exists as Fe(III). The catalyst may have at least a portion of Fe in the catalyst material that exists as amorphous iron. The catalyst may have at least a portion of Fe in the catalyst material that exists as iron oxide, iron oxide hydroxide, or a combination thereof. The iron oxide may include iron oxide selected from hematite (α-Fe2O3), maghemite (γ-Fe2O3), magnetite (Fe3O4), or a combination thereof. The iron hydroxide may include iron hydroxide selected from goethite, akagenite, lepidocrocite, or a combination thereof. The catalyst may contain at least a portion of iron as goethite and at least a portion of iron as hematite.
[0102] Embodiments of the ODH catalyst material are mixed metal oxides having the following formula: Mo1V 0.1-1 Nb 0.1-1 Te 0.01-0.2 X 0-0.2 O f (In the formula, X is selected from Pd, Sb, Ba, Al, W, Ga, Bi, Sn, Cu, Ti, Fe, Co, Ni, Cr, Zr, Ca, and their oxides and mixtures, and f is the number that satisfies the valence state of the metal present in the catalyst.)
[0103] Embodiments of the ODH catalyst material are mixed metal oxides containing Mo, V, O, and iron (Fe). The molar ratio of Mo to V can be 1:0.25 to 1:0.50, or 1:0.30 to 1:0.45, or 1:0.30 to 1:0.35, or 1:0.35 to 1:0.45. The molar ratio of Mo to Fe can be 1:0.25 to 1:5.5, or 1:3 to 1:5.5, or 1:4.25 to 1:4.75, or 1:4.45 to 1:4.55, or 1:0.1 to 1:1, or 1:0.25 to 1:0.75, or 1:0.4 to about 1:0.6, or about 1:0.4, or about 1:0.6, or 1:1.3 to 1:2.2, or 1:1.6 to 1:2.0, or 1:1.80 to 1:1.90. Furthermore, oxygen is present in an amount that satisfies the valence states of the metals present in the catalyst. The catalyst may contain at least a portion of the Fe in the catalyst material that exists as Fe(III). The catalyst may contain at least a portion of the Fe in the catalyst material that exists as amorphous iron. The catalyst may contain at least a portion of the Fe in the catalyst material, which exists as iron oxide, iron hydroxide, or a combination thereof. The iron oxide may include iron oxide selected from hematite (α-Fe2O3), maghemite (γ-Fe2O3), magnetite (Fe3O4), or a combination thereof. The iron hydroxide may include iron hydroxide selected from goethite, akagenite, lepidocrocite, or a combination thereof. The catalyst may contain at least a portion of the iron as goethite and at least a portion of the iron as hematite.
[0104] Embodiments of the ODH catalyst material are given by the empirical formula Mo1V 0.25-0.5 O dThe mixed metal oxide has the following properties, where d is the number that satisfies the valence states of the metals present in the catalyst. The molar ratio of Mo to V can be 1:0.25 to 1:0.5, or 1:0.3 to 1:0.49.
[0105] Embodiments of the ODH catalyst material are mixed metal oxides containing Mo, V, O, and aluminum (Al). The molar ratio of Mo to V can be 1:0.1 to 1:0.50, or 1:0.25 to 1:0.50, or 1:0.3 to 1:0.49, or 1:0.30 to 1:0.45, or 1:0.30 to 1:0.35, or 1:0.35 to about 1:0.45. The molar ratio of Mo to Al is 1:1.5 to 1:6.5, or 1:3.0 to 1:6.5, or 1:3.25 to 1:5.5.5, or 1:3.5 to 1:4.1, or 1:4.95 to 1:5.05, or 1:4.55 to 1:4.65, or 1:1.5 to 1:3.5, or 1:2.0 to 1:2.2, or 1:2.9 to 1:3.1. Oxygen is present in an amount that satisfies the valence states of at least the metals present in the catalyst. At least a portion of the Al in the catalyst material can exist as aluminum oxide, and the aluminum oxide can be aluminum hydroxide oxide. The aluminum hydroxide oxide can include aluminum hydroxide oxide selected from gibbsite, bayerite, boehmite, or a combination thereof. At least a portion of the Al in the catalyst material can exist as gamma alumina.
[0106] Embodiments of the ODH catalyst material are mixed metal oxides containing Mo, V, O, Al, and Fe. The molar ratio of Mo to V can be 1:0.1 to 1:0.5, or 1:0.30 to 1:0.45, or 1:0.30 to 1:0.35, or 1:0.35 to 1:0.45. The molar ratio of Mo to Al can be 1:1.5 to 1:6.0. The molar ratio of Mo to Fe can be 1:0.25 to 5:5. Oxygen is present in an amount that satisfies the valence states of at least the metals present in the catalyst. The molar ratio of Mo to Fe can be 1:0.1 to 1:1, and the molar ratio of Mo to Al can be 1:3.5 to 1:5.5. The molar ratio of Mo to Fe can be 1:0.25 to 1:0.75, and the molar ratio of Mo to Al can be 1:3.75 to 1:5.25. The molar ratio of Mo to Fe can be between 1:0.35 and 1:0.65, and the molar ratio of Mo to Al can be between 1:3.75 and 1:5.25. The molar ratio of Mo to Fe can be between 1:0.35 and 1:0.45, and the molar ratio of Mo to Al can be between 1:3.9 and 1:4.0. The molar ratio of Mo to Fe can be between 1:0.55 and 0:65, and the molar ratio of Mo to Al can be between 1:4.95 and 1:5.05. The molar ratio of Mo to Fe can be between 1:1.3 and 1:2.2, and the molar ratio of Mo to Al can be between 1:2.0 and 1:4.0. The molar ratio of Mo to Fe can be between 1:1.6 and 1:2.0, and the molar ratio of Mo to Al can be between 1:2.5 and 1:3.5. The molar ratio of Mo to Fe can be 1:1.80 to 1:1.90, and the molar ratio of Mo to Al can be 1:2.9 to 1:3.1. At least a portion of the Fe in the catalyst material can exist as Fe(III). At least a portion of the Fe in the catalyst material can exist as amorphous Fe. At least a portion of the Fe in the catalyst material can exist as iron oxide, iron hydroxide, or a combination thereof. In some embodiments, the iron oxide includes iron oxide selected from hematite (α-Fe2O3), maghemite (γ-Fe2O3), magnetite (Fe3O4), or a combination thereof.Iron hydroxide oxide can include iron hydroxide oxide selected from goethite, akagenite, lepidocrocite, or a combination thereof. At least a portion of the Fe in the catalyst material can exist as goethite, and at least a portion of the Fe in the catalyst material can exist as hematite. At least a portion of the Al in the catalyst material can exist as aluminum oxide. Aluminum oxide can include aluminum hydroxide oxide. Aluminum hydroxide oxide can include aluminum hydroxide oxide selected from gibbsite, bayerite, boehmite, or a combination thereof. At least a portion of the aluminum in the catalyst material can exist as gamma alumina.
[0107] Embodiments of the ODH catalyst material are mixed metal oxides containing Mo, V, Be, and O. The molar ratio of Mo to V can be 1:0.25 to 1:0.65, or 1:0.35 to 1:0.55, or 1:0.38 to 1:0.48. The molar ratio of Mo to Be can be 1:0.25 to 1:0.85, or 1:0.35 to 1:0.75, or 1:0.45 to 1:0.65. Oxygen is present in an amount that satisfies the valence states of the metals present in the catalyst.
[0108] Embodiments of the ODH catalyst material are mixed metal oxides containing Mo, V, Be, Al, and O. The molar ratio of Mo to V can be 1:0.25 to 1:0.65, or 1:0.35 to 1:0.55, or 1:0.38 to 1:0.48. The molar ratio of Mo to Be can be 1:0.25 to 1:1.7, or 1:0.35 to 1:0.75, or 1:0.45 to 1:0.65. The molar ratio of Mo to Al can be 1:1 to 1:9, or 1:2 to 1:8, or 1:4 to 1:6. Oxygen is present in an amount that satisfies the valence states of at least the metals present in the catalyst. At least a portion of the aluminum in the catalyst material can exist as aluminum oxide. The aluminum oxide can include aluminum hydroxide oxide. The aluminum hydroxide oxide can include aluminum hydroxide oxide selected from gibbsite, bayerite, boehmite, or a combination thereof. At least a portion of the aluminum in the catalyst material can exist as gamma alumina.
[0109] Embodiments of the ODH catalyst material have an amorphous phase comprising about 20% to about 50% by weight, or about 25% to about 45% by weight, or about 45% to about 75% by weight, or about 55% to about 65% by weight, or about 50% to about 85% by weight, or about 55% to about 75% by weight, or about 60% to about 70% by weight.
[0110] Embodiments of the ODH catalyst material have an average microcrystal size of approximately 50 nm or more, or more than approximately 75 nm or more than approximately 100 nm or more than approximately 125 nm or approximately 75 nm to approximately 150 nm or approximately 75 nm to approximately 250 nm or approximately 125 nm to approximately 175 nm.
[0111] Embodiments of the ODH catalyst material have an average particle size of approximately 0.5 μm to approximately 10 μm, or approximately 2 μm to approximately 8 μm, or approximately 3 μm to approximately 5 μm, or approximately 0.5 μm to approximately 20 μm, or approximately 5 μm to approximately 15 μm, or approximately 7 μm to approximately 11 μm.
[0112] Embodiments of the ODH catalyst material are characterized by having at least one XRD diffraction peak (2θ degrees) selected from 6.5±0.2, 7.8±0.2, 8.9±0.2, 10.8±0.2, 13.2±0.2, 14.0±0.2, 22.1±0.2, 23.8±0.2, 25.2±0.2, 26.3±0.2, 26.6±0.2, 27.2±0.2, 27.6±0.2, 28.2±0.2, 29.2±0.2, 30.5±0.2, and 31.4±0.2, where the XRD is obtained using CuKα radiation. Embodiments of the ODH catalyst material are characterized by having at least one XRD diffraction peak (2θ degrees) selected from 6.6±0.2, 6.8±0.2, 8.9±0.2, 10.8±0.2, 13.0±0.2, 22.1±0.2, 26.7±0.2, 27.2±0.2, and 28.2±0.2, where the XRD is obtained using CuKα radiation.
[0113] Embodiments of the ODH catalyst material may contain approximately 0.8% to approximately 30% by weight of calcium. The catalyst material may contain approximately 0.15% to approximately 2.8% by weight of calcium. The catalyst material may contain approximately 0.5% to approximately 75% by weight of calcium carbonate. The catalyst material may contain approximately 5% to approximately 15% by weight of calcium carbonate.
[0114] Catalysts can be supported or agglomerated using binders, carriers, diluents, or accelerators. Some binders include acidic, basic, or neutral binder slurries of TiO2, ZrO2, Al2O3, AlO(OH), and mixtures thereof. Another useful binder is Nb2O5. Agglomerated catalysts can be extruded into suitable shapes (such as rings, spheres, or saddles) of sizes typically used in fixed-bed reactors. When extruding catalysts, various extrusion aids known in the art can be used. In some cases, the resulting support may be 300 m² as measured by BET. 2 It can have a high cumulative surface area of / g, and in some cases approximately 35m² 2 Less than / g, sometimes about 20m 2 Less than / g, otherwise about 3m2 The value is less than / g, and the cumulative pore volume is approximately 0.05 to 0.50 cm³. 3 It may be expressed as / g.
[0115] The catalyst may be used alone or in combination. In some embodiments, the catalyst may also be used with an accelerator such as Pd, Pt, or Ru to enhance catalytic activity. Relatively speaking, the catalyst initially used up to the first 40% of the catalyst bed length in the direction of reactant flow has a reactivity of about 90% or less, and in some cases about 80% or less, of the average catalytic capacity reactivity in the remaining length of the catalyst bed.
[0116] The mixed metal oxide catalyst can be a supported catalyst. The support can be selected from oxides of titanium, zirconium, aluminum, magnesium, yttrium, lanthanum, silicon, zeolite, and clay, as well as mixed compositions thereof, or a carbon matrix. The mixed metal oxide catalyst may also be supplemented with a binder to enhance the cohesive force between catalyst particles and, if present, optionally improve the adhesion of the catalyst to the support. The mixed metal oxide catalyst can be diluted with an inert material such as DENSTONE® 99 alumina particles or SS316 particles.
[0117] With or without a support, mixed metal oxide catalysts can have a length-to-diameter ratio of 1:1 to 10:1, and in some cases, a length-to-diameter ratio of 1:1 to 5:1. With or without a support, mixed metal oxide catalysts can be spherical, cylindrical, slab-shaped, or any other shape. With or without a support, mixed metal oxide catalysts can contain particles having notches at each end of each cylinder, and in some embodiments, particles having up to three notches at the ends of each cylinder. With or without a support, mixed metal oxide catalysts can also contain one or more continuous external "bumps" or ridges that can extend the length of the particles. Mixed metal oxide catalysts can be in the shape of hollow cylinders or rings. With or without a support, mixed metal oxide catalysts can contain at least one passage through each particle. Those skilled in the art will know which features are required with respect to the shape and dimensions of mixed metal oxide catalysts. [Examples]
[0118] Experiments on the oxidative dehydrogenation of ethane were conducted using a fixed-bed reactor unit (FBRU) apparatus. The FBRU apparatus consisted of two vertical fixed-bed tubular reactors arranged in series. Each reactor was an SS316L tube with an outer diameter of 1 inch and a length of 34 inches, encased in an electrically heated jacket and sealed with ceramic insulating material. Each reactor contained an identical catalyst bed consisting of 143 g of catalyst. The chemical formula of the catalyst was determined by PIXE analysis, as shown in MoV 0.30-0.40 Te 0.10-0.20 Nb 0.10-0.20 O X Here, X is calculated based on the highest oxidation state of the metal oxide present in this catalyst, and the relative atomic weight of each component relative to a relative amount of Mo (1) is shown in subscript. The 35% conversion temperature of the catalyst was approximately 380°C when measured in an MRU setup with 2g of catalyst and feed compositions of 36 / 18 / 46 volume% ethane, oxygen, and nitrogen, respectively, at a feed gas flow rate of 154 sccm and atmospheric pressure outlet pressure.
[0119] To minimize the risk of catalyst bed movement during the experiment, quartz powder was packed above and below the catalyst bed in both reactors and secured in place with glass wool.
[0120] The experiment included an experimental run using a supply chain containing ethane, carbon dioxide, and water, which was pre-mixed and heated to a temperature of approximately 220°C or lower before being introduced into the first reactor. The product from the first reactor was transferred to the second reactor without adding any further components, and the same temperature was maintained in each reactor. The temperature of each catalyst bed in each reactor was monitored using four thermocouples placed at equal intervals along the length of each catalyst bed. The reactor temperature was controlled using the highest temperature between the thermocouple points of each catalyst bed, with corresponding back pressure regulators used to control the water pressure and boiling point in the reactor water jacket surrounding each reactor. The reaction temperature of each reactor was calculated as the average of all eight points.
[0121] A simulation of the ODH reactor was developed using gPROMS ProcessBuilder® 1.2.0. The component properties of Multiflash were defined using the SRK equation of state. The dynamics model of the ODH reaction was developed using gPROMS ProcessBuilder 1.2.0, and the dynamics parameters were estimated using fixed-bed reactor data from the FBRU experiment described above. The mixed metal oxide catalyst used was Mo a V b Te c Nb d O e (In the formula, a, b, c, d, and e are the relative atomic weights of the elements Mo, V, Te, Nb, and O, respectively; a=1, b=0.01~1.0, c=0.01~1.0, d=0.01~1.0, and 0.e is the number that satisfies the valence state of the catalyst). Table 1 shows a comparison of FBRU experimental data at 360°C with model predictions. The model predictions are in good agreement with the reactor data.
[0122] [Table 1]
[0123] The following examples illustrate the effect on the maximum process temperature when the catalyst capacity profile is changed by varying the dilution ratio or porosity. In each simulation example, the mass flow rate of each component supplied to the simulated ODH reactor was constant, as shown in Table 2. The simulated feed temperature and pressure were also constant, at 350°C and 196.5 kPa, respectively. Table 3 shows the simulated thermophysical properties of the ODH catalyst. The results for each simulation example are shown in Table 4. The reactor dimensions were changed to maintain the same amount of catalyst (g) across the entire catalyst bed. The total amount of catalyst in each example was set to 197.9 g.
[0124] [Table 2]
[0125] [Table 3]
[0126] [Example 1] (Comparative Example 1) The simulation conditions for Example 1 were as follows: 197.9 g of activated catalyst, a dilution ratio of 0.55, and the catalyst particles were cylindrical with average lengths of 5 mm and diameters of 3.175 mm, respectively. The porosity was set to 0.421. The simulated reactor had a length of 2.7 m, an outer diameter of 25.4 mm, and a wall thickness of 2.1 mm. The coolant inlet temperature was set to the same as the feed temperature, i.e., 350°C, and the outlet temperature was 352°C. The heat transfer coefficient of the wall coolant was 1000 W / m 2 It was set to K. The results are shown in Table 4.
[0127] [Example 2] (Comparative Example 2) Example 2 followed the same simulation conditions, porosity, and shape and size of the ODH catalyst as Example 1. The simulation also included 197.9 g of active catalyst, but it occupied only 40 volume percent of the catalyst bed. To reduce the volume percent of the active catalyst while maintaining the same amount of catalytic active phase, the reactor length was increased to 3.0 m (actually by increasing the dilution ratio) while maintaining the outer diameter at 25.4 mm and the wall thickness at 2.1 mm. The coolant inlet temperature was set to the same as the feed temperature, i.e., 350°C, and the outlet temperature was 352°C. In this case, the heat transfer coefficient of the wall coolant was 470 W / m 2 It was set to K. The results are shown in Table 4.
[0128] The results of these comparative examples demonstrate that the maximum process temperature and temperature gradient can be reduced by loading a similar amount of catalyst into a larger reactor. Both comparative examples contain the same amount of catalyst, but in Example 2 (Comparative Example 2), the catalyst is distributed within a larger volume. Increasing the reactor volume may increase construction costs.
[0129] [Example 3] Example 3 also used the same simulation conditions, porosity, and ODH catalyst shape and size as Example 1. The simulation involved dividing the catalyst bed into two sections. The upstream section covered the first 70% of the catalyst bed length and had 133.5 g of catalyst with a dilution ratio of 0.40, while the downstream section covered the last 30% of the catalyst bed length and had 64.4 g of catalyst with a dilution ratio of 0.55. To maintain the same total amount of catalyst in the reactor as in Example 1, the reactor length was increased from 2.7 m to 2.9 m. The outer diameter and wall thickness remained the same. The coolant inlet temperature was assumed to be the same as the feed temperature, i.e., 350°C, and the outlet temperature was 352°C. In this case, the heat transfer coefficient of the wall coolant was 1000 W / m 2 The temperature was set to K. As can be seen from the results shown in Table 4, the maximum process temperature observed in the upstream section was approximately 10.8°C and 2.6°C lower compared to both Example 1 and Example 2, respectively.
[0130] [Example 4] In Example 4, the dilution ratio was set to 0.55 over the length of the catalyst bed. Similar to Example 3, the catalyst bed was divided into two sections, with the upstream section covering the first 70% of the catalyst bed length and the downstream section covering the remaining 30%. By adjusting the catalyst shape to particles with a length of 7.5 mm and a diameter of 4.8 mm, the porosity of the upstream section was increased to 0.436 compared to 0.421 in the downstream section. The downstream section was set to catalyst particles with a length of 5.0 mm and a diameter of 3.2 mm. The upstream section was set to contain 137.5 g of catalyst, and the downstream section to contain 60.4 g of catalyst, for a total of 197.9 g. The catalyst bed length was set to 2.7 m, the outer diameter to 25.4 mm, and the wall thickness to 2.1 mm. The coolant inlet temperature was assumed to be the same as the feed temperature, i.e., 350°C, and the outlet temperature was 352°C. In this case, the heat transfer coefficient of the wall coolant is 1000 W / m 2 It was set to K. The results are shown in Table 4.
[0131] [Table 4]
[0132] Figure 10 shows the effect of a different catalyst capacity profile than in the previous example on the temperature profile in the simulated ODH reactor. In particular, Figure 10 shows the temperature profile for the described example. The lines for all four examples, Examples 1 to 4, all indicate the maximum process temperature (y-axis) occurring within the first 10% of the catalyst bed, as shown as dimension / reactor length (x-axis).
[0133] It was found that manipulating either the dilution ratio or the porosity actually changes the volume fraction of the active phase in the catalyst and alters the catalyst dimensions, thereby altering the temperature profile. Even small changes in the dilution ratio (8.3% decrease from upstream to downstream) or porosity (3.5% decrease from upstream to downstream) resulted in changes in the maximum process temperature, decreasing by 10.8°C and 12.9°C, respectively. The temperature difference also decreased by 10.2°C and 13.7°C, respectively, with changes in the dilution ratio and porosity. Larger changes in catalyst capacity between sections may lead to further decreases in the maximum process temperature and temperature difference.
[0134] Considering the axial temperature profile of a tubular reactor, the peak process temperature occurs near the reactor inlet, between 0 and 20% of the reactor length. The temperature profile gradually decreases towards the isotherm towards the end of the tubular reactor. Approximately 70% of the ethane conversion achieved in a tubular reactor occurs within 20% of the simulated reactor inlet. This peak process temperature also affects the selectivity of ethylene. A large difference between the peak process temperature and the isotherm temperature can reduce the selectivity of ethylene. In the example above, the selectivity does not change significantly, but it is expected that as the change in catalyst capacity increases, the difference between the peak temperature and the isotherm will decrease further, and the selectivity will likely improve. Also, if the peak process temperature is not properly controlled, hot spots may occur within the reactor. To control this peak process temperature, the coolant flow on the shell side of the reactor can be manipulated.
[0135] These examples illustrate how to control or reduce the peak process temperature in the first section (up to 50% by volume) of the catalyst bed of an oxidative dehydrogenation reactor, illustrating how the oxidative dehydrogenation reactor can convert a portion of the ethane supply flow to ethylene and shift the position of the peak process temperature in the opposite direction to the supply flow of reactants and heat removal diluent gases. This can be done by using a catalyst bed with a lower catalyst capacity (having lower reactivity per unit volume than the remaining section(s) of the catalyst bed) in the first section of the reactor.
[0136] The detailed descriptions, embodiments, and examples provided herein are for illustrative purposes only and are not intended to limit the scope of this disclosure. They should be understood to include various additional aspects, modifications, or changes that would be obvious to those skilled in the art. [Industrial applicability]
[0137] This disclosure relates to a fixed-bed reactor system for use in an ethane oxidation dehydrogenation process.
Claims
1. A fixed bed reactor system for the oxidative dehydrogenation (ODH) of ethane to ethylene, comprising a catalyst bed, the catalyst volume profile increasing gradually or stepwise from an upstream end to a downstream end of the catalyst bed.
2. 2. The fixed bed reactor system of claim 1, wherein the catalyst bed comprises at least two non-overlapping catalyst bed sections arranged in series along the length of the catalyst bed, the catalyst bed sections being identified by a change in catalyst volume, each catalyst bed section having a higher catalyst volume than the previous upstream catalyst bed section.
3. 3. The fixed bed reactor system of claim 2, wherein one or more catalyst bed sections have a lower 35% conversion temperature than a preceding catalyst bed section.
4. 10. The fixed bed reactor system of claim 1, wherein one or more catalyst bed sections have a 35% conversion temperature that is 2 to 10° C. lower than a previous catalyst bed section.
5. 3. The fixed bed reactor system of claim 2, wherein one or more catalyst bed sections have a lower dilution ratio than a previous catalyst bed section.
6. 6. The fixed bed reactor system of claim 5, wherein one or more catalyst bed sections have a dilution ratio that is 2 to 15% lower than the previous catalyst bed section.
7. 3. The fixed bed reactor system of claim 2, wherein one or more catalyst bed sections have a voidage that is 10 to 25% lower than the previous catalyst bed section.
8. 1. A process for the oxidative dehydrogenation (ODH) of ethane to ethylene, comprising: introducing a feed stream comprising ethane and oxygen into a fixed bed reactor system, the fixed bed reactor system comprising a catalyst bed, the catalyst volume profile of the ODH catalyst increasing along the length of the catalyst bed from the upstream end to the downstream end; contacting ethane with an ODH catalyst along the length of the catalyst bed in the presence of oxygen to convert at least a portion of the ethane to ethylene; removing a product stream comprising ethylene from the ODH reactor proximate to the downstream end of the catalyst bed; The process includes:
9. 1. A method for reducing a maximum reaction temperature in a first section of an oxidative dehydrogenation reactor catalyst bed comprised of at least one mixed metal oxide catalyst, comprising: the oxidative dehydrogenation reactor comprises at least one feed stream and at least one outlet stream; the catalyst bed is comprised of at least two catalyst bed sections, a first catalyst bed section being upstream of a subsequent catalyst bed section, wherein the first catalyst bed section is no more than 50% by volume of the catalyst bed; The method comprises: i) having a higher dilution ratio in the first catalyst bed section than in each subsequent catalyst bed section, such that the dilution ratio in each subsequent catalyst bed section divided by the dilution ratio in the first catalyst bed section is in the range of 0.3 to 0.98; and ii) having a higher voidage in the first catalyst bed section than in each subsequent catalyst bed section, such that the ratio of the voidage in each subsequent catalyst bed section divided by the voidage in the first catalyst bed section is in the range of 0.3 to 0.98; The method includes one or more of the following:
10. The method of claim 9 , wherein the catalyst bed comprises heat-dissipating particles.
11. The method of claim 10 , wherein the heat-dissipating particles are comprised of inert metal rods.
12. The method of claim 10, wherein the heat-dissipating particles are comprised of DENSTONE® 99 particles.
13. The method of claim 10 , wherein the heat-dissipating particles are comprised of SS316.
14. The method of claim 10, wherein the heat-dissipating particles are comprised of particles having a particle size in the range of 0.5 to 5 mm.
15. The process of claim 9, wherein the catalyst bed is composed of particles having a particle size in the range of 0.5 to 5 mm.
16. The method of claim 9, wherein the mixed metal oxide catalyst is comprised of particles having a particle size in the range of 0.5 μm to 20 μm.
17. 10. The method of claim 9, wherein the dilution ratio in each subsequent catalyst bed section divided by the dilution ratio in the first catalyst bed section is in the range of 0.85 to 0.
98.
18. 10. The process of claim 9, wherein the ratio of the void fraction in each of the subsequent catalyst bed sections divided by the void fraction in the first catalyst bed section is in the range of 0.35 to 0.
55.
19. 10. The method of claim 9, wherein the mixed metal oxide catalyst is comprised of particles having a length to diameter ratio of from 1:1 to 5:
1.
20. 10. The method of claim 9, wherein the mixed metal oxide catalyst is comprised of particles containing at least one passageway through each particle.
21. 10. The method of claim 9, wherein the mixed metal oxide catalyst is comprised of cylindrical particles.
22. 10. The method of claim 9, wherein the oxidative dehydrogenation reactor comprises at least two sections of a catalyst bed comprised of at least one mixed metal oxide catalyst, at least one feed stream to the oxidative dehydrogenation reactor comprises oxygen and at least 20 volume percent ethane, and at least one outlet stream comprises one or more of ethylene, ethane, one or more carboxylic acids, water, and oxygen.
23. 10. The process of claim 9, wherein the temperature difference between the maximum reaction temperature in the first section of the oxidative dehydrogenation reactor catalyst bed and the temperature in the subsequent catalyst bed section is from 5 to 20°C.
24. 10. The process of claim 9, wherein the maximum reaction temperature is from 310°C to 350°C.
25. The process of claim 9, wherein the oxidative dehydrogenation reactor is at a pressure of from 15 to 50 psig.
26. The process of claim 9, wherein the oxidative dehydrogenation reactor has a residence time of 0.1 to 10 seconds.
27. The oxidative dehydrogenation reactor is operated for 500 to 3,000 hours. -1 10. The process of claim 9, wherein the gas hourly space velocity is
28. 10. The method of claim 9, wherein at least one oxidative dehydrogenation reactor comprises a fixed bed reactor.
29. 1. A method for loading a catalyst bed into a fixed bed reactor for the oxidative dehydrogenation of ethane, the fixed bed reactor having an upstream end and a downstream end, the method comprising: preparing two or more catalyst bed compositions comprising an ODH catalyst; determining the catalyst volume for each of the catalyst bed compositions; pouring the catalyst bed compositions separately, in sequence, into a fixed bed reactor at a rate slow enough to allow for dense random packing, with the catalyst bed composition having the lowest catalyst volume poured at the upstream end and the catalyst bed composition having the highest catalyst volume poured at the downstream end; fixing the poured catalyst bed composition within a fixed bed reactor to form a loaded catalyst bed; Including, wherein the catalyst bed composition forms distinct catalyst bed sections, the catalyst bed sections being distinguished by a change in catalyst volume, the catalyst volume increasing from the upstream end to the downstream end; method.
30. 30. The method of claim 29, wherein the catalyst capacity is evaluated by determining the 35% conversion temperature for each of the catalyst bed compositions and ordering the catalyst bed composition having the highest relative 35% conversion temperature corresponding to the catalyst bed composition having the lowest relative catalyst capacity.