Spray drying of solid epoxy or phenoxy resins

JP2023551379A5Active Publication Date: 2024-11-08HUNTSMAN ADVANCED MATERIALS AMERICAS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023527677
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-09
Filing Date
2021-11-05
Publication Date
2024-11-08
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

High molecular weight epoxy or phenoxy resins are difficult to spray dry effectively, resulting in large particle sizes and high energy consumption, and traditional solvent removal methods produce low-quality pellets with thermal degradation issues.

Method used

Dissolve high molecular weight epoxy or phenoxy resins in a blend of protic and aprotic solvents and use a closed cycle spray dryer to produce a dry powder with an average particle size of 150 μm or less.

Benefits of technology

The method produces high-quality powdered resins with reduced thermal exposure, faster dissolution, and lower residual solvent content, improving production efficiency and reducing regulatory risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A high molecular weight solid epoxy or phenoxy resin is dissolved in a blend of alcoholic and aprotic solvents, and the resulting solution is spray dried in a closed-cycle spray dryer to form a powdered epoxy or phenoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 63 / 111,325, filed November 9, 2020, the contents of which are incorporated herein by reference.

[0002] This application relates to a method for spray drying solid epoxy or phenoxy resins. More specifically, a high molecular weight solid epoxy or phenoxy resin is dissolved in a blend of an alcohol solvent and an aprotic solvent, and the resulting solution is spray dried in a closed cycle spray dryer to form a powdered epoxy or phenoxy resin. [Background technology]

[0003] High molecular weight epoxy or phenoxy resins are often considered thermoplastics and are typically used in applications such as injection molding, extrusion, coatings, and adhesives. A common organic solvent that dissolves epoxy or phenoxy resins is methyl ethyl ketone (MEK). However, epoxy or phenoxy resins dissolved in MEK do not spray dry well. Similarly, spray drying has not been successful in the past with other solid epoxy or phenoxy resin solutions.

[0004] Powdered resins have been made by cryogenically grinding polymers as an alternative to spray drying, but the resulting average particle size is about 200 μm, which is significantly larger than desired for powdered epoxy or phenoxy resins, and the process is energy intensive and expensive.

[0005] In past practice, high molecular weight epoxy or phenoxy resins have typically been synthesized in the presence of a solvent, the solution washed with water to remove salts formed during the reaction, and the solvent removed to yield solid pellets. Solvent removal has been achieved by utilizing thin film equipment under high temperature and vacuum, such as a Filmtruder® device. However, there is a limit to the amount of solvent that can be removed in this manner, and the start-up of the process has typically resulted in an initial period of dark product and carbonized material that must be disposed of as waste. Furthermore, pellets are not as useful as powdered epoxy or phenoxy resins. Summary of the Invention

[0006] The present disclosure generally provides a method for forming a dry powder thermoplastic resin composition by dissolving a solid thermoplastic resin selected from the group consisting of a solid epoxy resin and a solid phenoxy resin in a blend of a protic solvent and an aprotic solvent to form a slurry, and spray-drying the slurry to form a dry powder thermoplastic resin composition. The present disclosure also provides a dry powder thermoplastic resin composition obtained by the above method, which contains a plurality of particles selected from epoxy resin particles and phenoxy resin particles, the particles having an average particle size of about 150 μm or less. The dry powder thermoplastic resin composition of the present disclosure can be used, for example, in coatings, adhesives, plastics, composite materials, and electronic components. [Brief explanation of the drawings]

[0007] [Figure 1] 1 is a flow chart illustrating a method for forming a powdered epoxy or phenoxy resin in accordance with an embodiment of the present disclosure; and [Figure 2] 1 illustrates a spray drying apparatus for use in embodiments of the present disclosure. DETAILED DESCRIPTION OF THE INVENTION

[0008] The following terms shall have the following meanings:

[0009] The term "comprising" and its derivatives are not intended to exclude the presence of any additional elements, steps, or procedures, whether or not they are disclosed herein. For the avoidance of doubt, all compositions claimed herein through the use of the term "comprising" may include any additional additives or compounds unless stated to the contrary. In contrast, the term "consisting essentially of," when used herein, excludes any other elements, steps, or procedures from any subsequent recitation unless they are essential to operability, and the term "consisting of," when used, excludes any element, step, or procedure not specifically delineated or listed. The term "or," unless otherwise stated, refers to the listed members individually as well as in any combination.

[0010] The articles "a" and "an" are used herein to refer to one or more than one (i.e., at least one) of the grammatical object of the article. By way of example, "a protic solvent" means one protic solvent or more than one protic solvent. Phrases such as "in one embodiment," "according to one embodiment," and the like generally mean that the particular feature, structure, or characteristic that follows the phrase is included in at least one embodiment of the present disclosure and may also be included in more than one embodiment of the present disclosure. Importantly, such phrases do not necessarily refer to the same embodiment. When "may," "can," "could," or "might" are used herein to describe that an element or feature is included or has a certain characteristic, it does not require that the particular element or feature be included or have a certain characteristic.

[0011] The term "about," as used herein, allows for a degree of variability in values ​​or ranges, for example, the degree can be within 10%, within 5%, or within 1% of the stated value or stated range limit.

[0012] The terms "preferred" and "preferably" refer to embodiments that may offer certain benefits, under certain circumstances. However, other embodiments may also be preferred, under the same or different circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the present disclosure.

[0013] The term "optional" or "optionally" means that the subsequently described event, circumstance, or material may or may not occur or be present, and that the description includes both the occurrence or presence and non-occurrence or absence of the event, circumstance, or material.

[0014] Values ​​expressed in range format should be interpreted in an open manner, not only to include the numbers specified as the limits of the range, but also to include all individual numbers or subranges subsumed within that range, as if each number and subrange were specifically written down. For example, a range such as 1 to 6 should be considered to specifically disclose subranges such as 1 to 3, 2 to 4, 3 to 6, etc., as well as the individual numbers subsumed within that range, e.g., 1, 2, 3, 4, 5, and 6. This is true regardless of the breadth of the range.

[0015] The term "substantially free" refers to a composition in which a particular compound or moiety is present in an amount that has no practical effect on the composition. In some embodiments, "substantially free" can refer to a composition in which a particular compound or moiety is present in an amount of less than 2% by weight, or less than 1% by weight, or less than 0.5% by weight, or less than 0.1% by weight, or less than 0.05% by weight, or even less than 0.01% by weight, based on the total weight of the composition, or an amount of the particular compound or moiety that is not present in the composition.

[0016] The term "dry powder thermoplastic composition" typically refers to a composition characterized, among other features, by its residual moisture content, which is preferably sufficiently low to prevent the formation of agglomerates that may reduce or inhibit powder flowability. As used herein, the term "residual moisture content (or "residual moisture")" refers to the total amount of solvent present in a dry powder thermoplastic composition. The total residual moisture content can be determined using any suitable method known in the art, such as Karl Fischer titration or thermogravimetric analysis (TGA). In one embodiment, the dry powdered thermoplastic resin composition according to the present invention has a residual moisture content of 10% (w / w) or less, or 9% (w / w) or less, or 8% (w / w) or less, or 7% (w / w) or less, or 6% (w / w) or less, or 5% (w / w) or less, or 4% (w / w) or less, or 3% (w / w) or less, or 2% (w / w) or less, or 1% (w / w) or less, or 0.5% (w / w) or less, or even 0.25% (w / w) or less. In further embodiments, the residual moisture content of the dry powdered thermoplastic resin composition is in the range of about 0.01% (w / w) to about 5% (w / w), about 0.01% (w / w) to about 3% (w / w), about 0.01% (w / w) to about 2% (w / w), about 0.01% (w / w) to about 1.5% (w / w), about 0.01% (w / w) to about 1.25% (w / w), about 0.01% (w / w) to about 1% (w / w), or about 0.01% (w / w) to about 0.75% (w / w).

[0017] The term "average particle size," as used herein, refers to the particle size corresponding to 50% of the particles in a distribution curve in which particles are accumulated in order of particle size from the smallest particle to the largest particle. In this specification, the total number of accumulated particles is 100%. The average particle size can be measured by methods known to those skilled in the art. For example, the average particle size can be measured using a particle size analyzer, or can be measured using transmission electron microscope (TEM) or scanning electron microscope (SEM) images. As an example of another measurement method, the average particle size can be measured using a measurement device that uses dynamic light scattering. According to this method, the number of particles within a predetermined size range can be counted, and the average particle size can be calculated therefrom.

[0018] 1, an exemplary method for forming a powdered epoxy or phenoxy resin includes providing a solid epoxy or phenoxy resin (10), dissolving the solid epoxy or phenoxy resin in a blend of an alcohol solvent and an aprotic solvent (20), and spray drying the resulting solution in a closed-cycle spray dryer to form a powdered epoxy or phenoxy resin (30). A closed-cycle spray dryer is used in step 30 because an inert atmosphere is desirable for atomizing the solvent in the drying chamber.

[0019] An exemplary method relates to high molecular weight solid resins having an average molecular weight of at least 1000 daltons, preferably at least 10,000 daltons, more preferably at least 30,000 daltons, more preferably at least 50,000 daltons, and most preferably from about 50,000 to about 55,000 daltons.

[0020] The alcohol solvent molecules in step 20 of the exemplary method have 2 to 6 carbon atoms. Examples of alcohol solvents include ethanol, propanol, isopropanol, butanol, pentaol, and the like. The preferred alcohol solvent is butanol.

[0021] Examples of aprotic solvents for step 20 of the exemplary method include methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dichloromethane, and tetrahydrofuran. A preferred aprotic solvent is toluene.

[0022] The weight ratio of alcohol solvent to aprotic solvent in the blend in step 20 of the exemplary method can be, for example, about 30:70 (w / w) to about 70:30 (w / w), preferably about 40:60 (w / w) to about 60:40 (w / w), and more preferably about 50:50 (w / w).

[0023] The solution obtained in step 20 of the exemplary method contains, for example, about 1 wt % to about 10 wt % epoxy or phenoxy resin, preferably about 5 wt % to about 10 wt % epoxy or phenoxy resin, based on the total weight of the obtained solution.

[0024] The powdered epoxy or phenoxy resin resulting from the exemplary method contains, for example, about 5 wt. % or less residual solvent, preferably about 1.5 wt. % or less residual solvent, more preferably about 0.5 wt. % or less residual solvent, and most preferably about 0.3 wt. % or less residual solvent, based on the total weight of the powdered epoxy or phenoxy resin.

[0025] The average particle size of the powdered epoxy or phenoxy resin resulting from the exemplary method is, for example, about 20 μm or less, and preferably about 12 μm or less.

[0026] Compared to particles typically obtained by removing solvent under high heat and vacuum using thin-film equipment, spray drying allows for solvent removal at lower temperatures because atomization of the solvent significantly increases surface area and improves evaporation efficiency. The choice of solvent appears to make a significant difference in the ability to spray dry solid epoxy or phenoxy resin solutions, which has not been successful in the past. Spray drying epoxy or phenoxy resins dissolved in a blend of alcoholic and aprotic solvents produces powders with relatively small particle size that can be processed through the spray dryer without "stringing."

[0027] The powdered epoxy or phenoxy resin obtained from the spray-drying step 30 of the exemplary method offers significant advantages over pellets obtained from typical prior practice. Solvent removal by spray drying reduces heat exposure compared to using thin-film equipment. This significantly improves quality because black specks and yellowing resulting from heat exposure no longer form. Furthermore, powdered epoxy or phenoxy resin dissolves faster in, for example, solvents, liquid epoxy resins, amines, acrylates, and polyols than pellets obtained from typical prior practice. This is advantageous for manufacturing and reduces cycle times for water-based and solvent-based derivatization. As a specific example, powdered epoxy or phenoxy resin dissolves nearly twice as fast as pellets, resulting in a 40% reduction in derivatization. Additionally, the lower percentage of residual solvent in powdered epoxy or phenoxy resin reduces concerns about future regulatory risks associated with residual solvents, a factor in markets such as electronics, composites, and thermoplastic adhesives.

[0028] In accordance with another embodiment, provided is a method for forming a dry powder thermoplastic resin composition, the method comprising dissolving a solid thermoplastic resin selected from the group consisting of a solid epoxy resin and a solid phenoxy resin in a blend of a protic solvent and an aprotic solvent to form a slurry. and spray drying the slurry to form a dry powder thermoplastic resin composition. The method according to the present invention can be carried out in bulk or as a continuous process. In one embodiment, the method is carried out as a continuous process.

[0029] In some embodiments, the solid thermoplastic resin is a solid epoxy resin. A solid epoxy resin can be solid or semi-solid at room temperature (25° C.) and can soften but not exhibit a rapid drop in viscosity when the temperature is increased. In one embodiment, the molecular weight of the solid epoxy resin can be about 1000 g / mol or more, or about 2000 g / mol or more, or about 5000 g / mol or more, or about 10,000 g / mol or more. In other embodiments, the solid epoxy resin can have a molecular weight of about 60,000 g / mol or less, or about 50,000 g / mol or less, or about 40,000 g / mol or less, or about 30,000 g / mol or less. In yet other embodiments, the solid epoxy resin can have a molecular weight of from about 1000 g / mol to about 55,000 g / mol, or from about 2500 g / mol to about 45,000 g / mol, or from about 5000 g / mol to about 35,000 g / mol, or from about 10,000 g / mol to about 25,000 g / mol.

[0030] In yet another embodiment, the solid epoxy resin can have an epoxy equivalent weight (EEW) of about 250 g / eq to about 3000 g / eq, or about 300 g / eq to about 2000 g / eq, or about 325 g / eq to about 1500 g / eq, or about 350 g / eq to about 1200 g / eq, or about 360 g / eq to about 1100 g / eq, or about 500 g / eq to about 1000 g / eq. In other embodiments, the softening point of the solid epoxy resin at room temperature can be about 40°C to 120°C, or about 50°C to 110°C, or about 60°C to 100°C.

[0031] Various solid epoxy resins can be used without particular limitations as long as they are solid or semi-solid at room temperature. Examples include, but are not limited to, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AF-based epoxy resin, o-cresol novolak epoxy resin, phenol novolak epoxy resin, modified phenol epoxy resin, naphthalene epoxy resin, triphenolmethane epoxy resin, alkyl-modified triphenolmethane epoxy resin, triazine nucleus-containing epoxy resin, dicyclopentadiene epoxy resin, glycidylamine epoxy resin, biphenyl epoxy resin, biphenyl aralkyl epoxy resin, hydrogenated bisphenol A epoxy resin, aliphatic epoxy resin, stilbene epoxy resin, trisphenol-methane triglycidyl ether, isocyanate-modified bisphenol A-based epoxy resin, isocyanate-modified bisphenol F-based epoxy resin, isocyanate-modified bisphenol AF-based epoxy resin, and bisphenol A novolak epoxy resin, bisphenol F novolak epoxy resin, or bisphenol AF novolak epoxy resin.

[0032] In another embodiment, the solid thermoplastic resin is a solid phenoxy resin, which can be obtained by the condensation reaction of a dihydric phenol compound with epichlorohydrin or the polyaddition reaction of a dihydric phenol compound with a difunctional epoxy resin.

[0033] Examples of dihydric phenolic compounds used in the production of solid phenoxy resins include hydroquinone, resorcinol, 4,4-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ketone, 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)prop ... Examples of suitable hydroxyl groups include 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(3-phenyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-tert-butylphenyl)propane, 1,3-bis(2-(4-hydroxyphenyl)propyl)benzene, 1,4-bis(2-(4-hydroxyphenyl)propyl)benzene, 2,2-bis(4-hydroxyphenyl)-1,1,1-3,3,3-hexafluoropropane, and 9,9'-bis(4-hydroxyphenyl)fluorene. Among these, 4,4-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ketone, 2,2-bis(4-hydroxyphenyl)propane, and 9,9'-bis(4-hydroxyphenyl)fluorene are particularly preferred.

[0034] Examples of difunctional epoxy resins used to produce solid phenoxy resins include epoxy oligomers obtained by the condensation reaction of the above-mentioned dihydric phenol compounds with epichlorohydrin. Examples of such epoxy oligomers include hydroquinone diglycidyl ether, resorcinol diglycidyl ether, bisphenol S-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, methylhydroquinone diglycidyl ether, chlorohydroquinone diglycidyl ether, 4,4'-dihydroxydiphenyloxide diglycidyl ether, 2,6-dihydroxynaphthalene diglycidyl ether, dichlorobisphenol A diglycidyl ether, tetrabromobisphenol A-type epoxy resins, and 9,9'-bis(4)-hydroxyphenyl)fluorene diglycidyl ether. Among these, bisphenol A type epoxy resin, bisphenol S type epoxy resin, hydroquinone diglycidyl ether, bisphenol F type epoxy resin, tetrabromobisphenol A type epoxy resin, or 9,9'-bis(4)-hydroxyphenyl)fluorene diglycidyl ether is preferred.

[0035] The production of solid phenoxy resin can be carried out either without a solvent or in the presence of a reaction solvent. Examples of the reaction solvent include organic solvents such as methyl ethyl ketone, dioxane, tetrahydrofuran, acetophenone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, sulfolane, and toluene. Phenoxy resins obtained using a reaction solvent can be converted into solid resins free of the reaction solvent by subjecting the resulting phenoxy resin to a solvent removal treatment using an evaporator or the like. In other embodiments, the reaction solvent is not removed but is used as part of the blend that is subsequently spray-dried.

[0036] The average molecular weight (g / mol) of the solid phenoxy resin can be about 1000 or more, or about 5000 or more, or about 10,000 or more. In other embodiments, the average molecular weight of the solid phenoxy resin can be about 500,000 or less, or about 200,000 or less, or about 150,000 or less, or about 100,000 or less. In still other embodiments, the average molecular weight (g / mol) of the solid epoxy resin can be from about 10,000 to about 250,000, or from about 20,000 to about 150,000, or from about 25,000 to about 80,000.

[0037] In another embodiment, the hydroxyl equivalent weight (g / eq) of the solid phenoxy can be from about 50 to about 1,000, or from about 100 to about 750, or from about 200 to about 500.

[0038] According to another embodiment, the solid phenoxy resin may have the following structural formula: [ka] wherein n is an integer from about 8 to about 400, and X is selected from the following: [ka]

[0039] In one particular embodiment, n is an integer from about 20 to 400, or from about 25 to 150, or from about 35 to 100, or from about 38 to 60. In another embodiment, X is [ka] is.

[0040] In the first step of the process, a solid epoxy resin or a solid phenoxy resin is dissolved in a blend comprising a protic solvent and an aprotic solvent to form a slurry. As used herein, a "protic solvent" refers to a solvent that is primarily proton (H + It generally refers to a solvent having a hydrogen atom attached to an oxygen atom (as in a hydroxyl group) or a hydrogen atom attached to a nitrogen atom (as in an amine group) so as to be able to donate a protic bond. In one embodiment, the protic solvent can be a C1-C6-alkanol, a C2-C4-alkanediol, an ether alkanol, water, acetic acid, formic acid, and mixtures thereof.

[0041] C1-C6-alkanols generally include methanol, ethanol, propanol, isopropanol, n-butanol, sec-butanol, and tert-butanol. Preferred C1-C4-alkanols include ethanol, n-propanol, isopropanol, and n-butanol. Particularly preferred is n-butanol.

[0042] C2-C4-alkanediols include ethylene glycol or propylene glycol. Ether alkanols include diethylene glycol.

[0043] In one embodiment, the protic solvent is a C1-C4-alkanol. Surprisingly, it has been found that the use of a C1-C4 alkanol as the solvent for the blend is particularly advantageous with respect to the ability to spray dry the solid thermoplastic resin and to produce a powder with a relatively small average particle size.

[0044] In one embodiment, the blend comprises about 1 wt% or more of a protic solvent, based on the total weight of the blend. In other embodiments, the blend comprises about 5 wt% or more, or about 10 wt% or more, or about 20 wt% or more, or about 30 wt% or more of a protic solvent, based on the total weight of the blend. In yet other embodiments, the blend comprises about 99 wt% or less, or about 90 wt% or less, or about 80 wt% or less, or about 70 wt% or less of a protic solvent, based on the total weight of the blend.

[0045] The blend also includes an aprotic solvent. As used herein, "aprotic solvent" refers to a solvent that cannot donate a proton. In one embodiment, the aprotic solvent is selected from aromatic solvents, alkane solvents, ether solvents, ester solvents, acetone, acetonitrile, dimethylformamide, and mixtures thereof.

[0046] In one embodiment, the aromatic solvent is benzene, toluene, xylene (ortho-xylene, meta-xylene, or para-xylene), mesitylene, chlorobenzene (MCB), 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, or a mixture thereof. Suitable aromatic solvents are selected from toluene, xylene (ortho-xylene, meta-xylene, or para-xylene), chlorobenzene, and mixtures thereof.

[0047] Alkane solvents include aliphatic hydrocarbons such as pentane, hexane, heptane, cyclohexane, petroleum ether, or mixtures thereof, and halogenated hydrocarbons such as methylene chloride, chloroform, or mixtures thereof.

[0048] Ether solvents include open-chain and cyclic ethers, in particular diethyl ether, methyl tert-butyl ether (MTBE), 2-methoxy-2-methylbutane, cyclopentyl methyl ether, 1,4-dioxane, tetrahydrofuran (THF), 2-methyltetrahydrofuran (CH3-THF), or mixtures thereof.

[0049] Ester solvents include carboxylic acid esters, for example, ethyl acetate or butyl acetate.

[0050] In one embodiment, the aprotic solvent is selected from toluene, xylene (ortho-xylene, meta-xylene, or para-xylene), chlorobenzene, heptane, tetrahydrofuran, 2-methyltetrahydrofuran, methyl tert-butyl ether, 1,4-dioxane, ethyl acetate, butyl acetate, acetone, acetonitrile, and mixtures thereof.

[0051] In one particular embodiment, the aprotic solvent is an aromatic solvent. Surprisingly, it has been found that the use of an aromatic solvent as the aprotic solvent in the blend is particularly advantageous with respect to the ability to spray dry the solid thermoplastic resin and to produce a dry powder with a relatively small average particle size.

[0052] In another embodiment, the blend comprises about 1 wt% or more aprotic solvent, based on the total weight of the blend. In other embodiments, the blend comprises about 5 wt% or more, or about 10 wt% or more, or about 20 wt% or more, or about 30 wt% or more aprotic solvent, based on the total weight of the blend. In yet other embodiments, the blend comprises about 99 wt% or less, or about 90 wt% or less, or about 80 wt% or less, or about 70 wt% or less aprotic solvent, based on the total weight of the blend.

[0053] In yet other embodiments, the blend comprises a protic solvent and an aprotic solvent (protic:aprotic solvent) in a weight ratio of about 10:90 (w / w) to about 90:10 (w / w). In yet other embodiments, the blend comprises a protic solvent to an aprotic solvent in a weight ratio of about 25:75 (w / w) to about 75:25 (w / w), or about 30:70 (w / w) to about 70:30 (w / w), or about 40:60 (w / w) to about 60:40 (w / w), or about 45:55 (w / w) to about 55:45 (w / w).

[0054] In one embodiment, a solid epoxy resin or a solid phenoxy resin is dissolved in the blend to form a slurry containing about 1 wt.% or more of the epoxy or phenoxy resin, based on the total weight of the blend. In other embodiments, a solid epoxy resin or a solid phenoxy resin is dissolved in the blend to form a slurry containing about 3 wt.% or more, or about 5 wt.% or more, or about 7 wt.% or more, or about 10 wt.% or more, or about 15 wt.% or more of the epoxy or phenoxy resin, based on the total weight of the blend.

[0055] In another embodiment, a solid epoxy resin or a solid phenoxy resin is dissolved in the blend to form a slurry containing about 20% or less by weight of the epoxy or phenoxy resin, based on the total weight of the blend. In other embodiments, a solid epoxy resin or a solid phenoxy resin is dissolved in the blend to form a slurry containing about 17% or less by weight, or about 15% or less by weight, or about 12% or less by weight, or about 10% or less by weight of the epoxy or phenoxy resin, based on the total weight of the blend.

[0056] In yet another embodiment, a solid epoxy resin or a solid phenoxy resin is dissolved in the blend to form a slurry containing about 1 wt % to about 15 wt % of the epoxy or phenoxy resin, based on the total weight of the blend. In other embodiments, a solid epoxy resin or a solid phenoxy resin is dissolved in the blend to form a slurry containing about 2 wt % to about 13 wt %, or about 3 wt % to about 12 wt %, or about 5 wt % to about 10 wt % of the epoxy or phenoxy resin, based on the total weight of the blend.

[0057] The slurry is then spray-dried to form a dry powder thermoplastic resin composition comprising a plurality of thermoplastic resin (i.e., epoxy resin or phenoxy resin) particles. The term "particle" refers to individual solid particles of the dry powder thermoplastic resin composition. The individual particles of the dry powder thermoplastic resin composition are preferably physically separated from one another, i.e., the individual particles comprising the dry powder are unbound and capable of reversible contact with one another (as opposed to irreversible bonding between individual particles).

[0058] As used herein, the term "spray drying" refers to a process that generally involves breaking a liquid into small droplets (atomization) and rapidly removing the solvent from the droplets in a spray drying apparatus, where a strong driving force exists to evaporate the solvent from the droplets. The strong driving force for solvent evaporation is generally provided by the high surface-to-mass ratio of the droplets and by maintaining the solvent partial pressure in the spray drying apparatus sufficiently lower than the vapor pressure of the solvent at the temperature of the droplets being dried. This can be achieved, for example, by maintaining a partial vacuum in the spray drying apparatus, or by mixing the droplets with a warm drying gas, or a combination thereof. The spray drying process results in particles, preferably dry particles, more preferably in the form of a dry particle composition.

[0059] Typically, a slurry containing a solid thermoplastic resin and a solvent blend is first broken down into small droplets. These droplets can be suspended in a gas or gas mixture, such as air. The resulting mixture of droplets and gas is typically referred to as a "spray" or "mist." The process of breaking down a slurry into droplets is known as "atomization" and can be carried out using any suitable device (atomizer) known in the art. Various types of atomizers suitable for use in the methods of the present disclosure are known in the art, including, for example, rotary atomizers, pressure nozzles, two-fluid nozzles, fountain nozzles, ultrasonic nebulizers, and vibrating orifice aerosol generators.

[0060] In one embodiment, atomization of the slurry results in spherical droplets. As used herein, the term "spherical" includes not only geometrically perfect spheres, but also less regular shapes, such as spheroids, ellipsoids, ovals, or rounded droplets.

[0061] Once the slurry is atomized, the resulting spray droplets are mixed with a drying gas, allowing the solvent blend to rapidly evaporate in the drying chamber. Rapid evaporation typically results in a cooling effect, so that the dried particles do not reach the drying air temperature. This is particularly advantageous when drying heat-sensitive materials. The drying chamber can be of any shape and can have one or more chambers. The drying gas can be capable of at least partially absorbing the solvent that evaporates from the droplets and can be introduced into the drying chamber through an inlet, such as a disperser. The disperser can be located in the upper half of the drying chamber, for example, near the atomizer, allowing for rapid mixing of the drying gas and the droplets. The drying gas flow exits the drying chamber through an outlet, which can be located at the bottom of the drying chamber. .

[0062] The characteristics of the drying chamber can be matched, inter alia, to the atomizer used. To ensure uniform product quality, droplets can be allowed to contact the surface of the drying chamber only if they are sufficiently dry. The dry powder can be collected at the bottom of the drying chamber. In one embodiment, the drying chamber is designed as a cone, and the drying gas flow outlet is located at the center of the cone, where cold, moist air can be removed from the drying chamber. The cone and outlet thus designed act as a cyclone separator, depositing the dry powder at the bottom of the drying chamber. Cyclone separation is preferably used to separate dry particles or microdroplets from the drying gas through vortex separation, in some embodiments without the use of a filter. For this purpose, a high-speed rotational flow is preferably established in the cylindrical or conical vessel of the cyclone. Typically, the drying gas flows spirally from the top (large end) of the cyclone to the bottom (small end) and then exits the cyclone in a straight flow through the center of the cyclone. Larger or denser particles do not follow sharp turns in the rotating flow and instead hit the outer wall and fall to the bottom of the cyclone where they can be collected. Alternatively, a filter, such as a bag filter or a combination of a cyclone separator and filter, can be used to separate the dry powder and dry gas.

[0063] Depending on the type of flow, i.e., the relative arrangement of the atomizer and the drying gas inlet, or the relative movement of the spray and drying gas, respectively, several types of spray drying apparatus can be distinguished, all of which can be used in the method according to the present disclosure. In one embodiment, the spray drying apparatus is configured as a co-current apparatus (the spray and drying gas move in the same direction), as a counter-current apparatus (the spray and drying gas move in opposite directions), or as a mixed-flow apparatus (a combination of co-current and counter-current). In one embodiment, the spray drying apparatus is a co-current apparatus.

[0064] Moreover, spray dryers can be classified according to the type of drying gas cycle they use. For example, a spray dryer can be an open-cycle device (drying gas entering the spray dryer through an inlet is vented to the atmosphere through an outlet) or a closed-cycle spray dryer (drying gas entering the spray dryer through an inlet is vented through an outlet and regenerated and reused). In one embodiment, the spray dryer is a closed-cycle spray dryer.

[0065] The drying gas can be any suitable gas or gas mixture. In one embodiment, an inert gas is used as the drying gas. The inert gas can be, for example, nitrogen, nitrogen-enriched air, helium, CO2, or argon.

[0066] In one embodiment, the spray drying apparatus, as defined herein, reduces the residual moisture content of the dry powdered thermoplastic resin composition to a desired level in one pass through the system. If the residual moisture content of the dry powdered thermoplastic resin composition after one cycle is higher than desired, the residual moisture content can be further reduced by a second (or multiple) drying stage until the desired residual moisture content is achieved.

[0067] An example of a spray drying apparatus is shown in Figure 2, which further illustrates the principles of spray drying. A slurry input stream (1) is sprayed through a nozzle (2) into a drying gas stream (3) where it is evaporated. As the solvent evaporates from the slurry upon being introduced into the drying gas stream (3), the droplets are cooled. Solid spherical particles are formed while water rapidly leaves the droplets. A nozzle is used to achieve a sufficiently small droplet size (atomizer) and to maximize heat transfer and solvent evaporation rate. The solid spherical particles are then dispersed in a cyclone device (4). The dried spherical particles are cooled and collected in a collection vessel (5) connected to a cyclone device (4) and are ready to be packaged in various ways.

[0068] The final product is collected as described above. The final product is preferably in the form of a dry powder comprising thermoplastic resin spherical particles as defined herein. In one embodiment, the thermoplastic resin spherical particles have an average particle size of about 150 μm or less, or about 125 μm or less, or about 100 μm or less, or about 75 μm or less, or about 50 μm or less, or about 25 μm or less, or about 20 μm or less, or about 10 μm or less, or about 5 μm or less. In other embodiments, the thermoplastic resin spherical particles have an average particle size of about 1 μm or more, or about 5 μm or more, or about 10 μm or more, or about 15 μm or more, or about 25 μm or more. In still other embodiments, the thermoplastic resin spherical particles have an average particle size of about 0.5 μm to about 150 μm, or about 1 μm to about 100 μm, or about 2 μm to about 50 μm, or about 3 μm to about 25 μm, or about 4 μm to about 15 μm.

[0069] The dry powder thermoplastic resin composition can be used in a variety of applications / formulations including, but not limited to, automotive, industrial, construction, aerospace, marine, civil engineering, personal protective equipment, coatings, consumer or do-it-yourself products, composite films, plastics, magnetic tape coatings, rigid and flexible packaging coatings, epoxy baking primers, repair primers, zinc-rich primers, shop and heavy equipment primers, appliance and coil coating primers, chemical resistant finishes, wood coatings, pipe coatings, phenolic or flexibility modifiers for poly(ethylene terephthalate), cellophane, polystyrene, aluminum foil, polycarbonate, cardboard, poly(methyl methacrylate), kraft paper, canvas, "B" stage phenolic impregnated paper, fiberglass cloth, and felt.

[0070] Prophetic Example A sample with a phenoxy resin concentration of approximately 10% (w / w) is prepared as a starting solution. 10 g of solid phenoxy resin is mixed with 90 g of a 50:50 (w / w) n-butanol / toluene solvent blend. The slurry is stirred for approximately 10 minutes until a clear solution is obtained. 50 g of the slurry is transferred to a 50 ml glass beaker containing a magnetic stir bar. The slurry is continuously stirred during spray drying. The beaker is sealed with parafilm foil to prevent any solvent from evaporating during the drying process.

[0071] The slurry is spray-dried in a closed-cycle spray dryer. Nitrogen is used as the drying gas. The drying gas flow rate is approximately 140 L / min, resulting in an internal pressure of approximately 60 mbar. The laminar drying gas flow and piezoelectric atomization result in gentle evaporation. The inlet temperature is varied between 20°C, 25°C, 30°C, 35°C, and 40°C. The outlet and spray head temperatures also vary depending on the spray cap size selected. A spray rate of 60% is used. After reaching the inlet temperature, a 50:50 (w / w) n-butanol / toluene blend is sprayed to stabilize the outlet temperature. The slurry is then sprayed, and the dry powder is collected in an electrostatic particle collector. The morphology and particle size of the solid phenoxy resin particles in the dry powder can be characterized using scanning electron microscopy (SEM), which may reveal spherical particles with an average particle size of approximately 10 μm. The moisture content may be determined by Moisture Analyzer B-302 and found to be about 1% (w / w).

[0072] From the foregoing, it will be appreciated that numerous modifications and variations may be effected without departing from the true spirit and scope of the novel concepts of the present invention. It will be appreciated, of course, that no limitations with respect to the specific embodiments illustrated and described are intended or should be inferred.

Claims

1. 1. A method for forming a dry powder thermoplastic resin composition, comprising: dissolving a solid thermoplastic resin selected from the group consisting of solid epoxy resins and solid phenoxy resins in a blend of protic and aprotic solvents to form a slurry; and spray drying the slurry to form the dry powdered thermoplastic resin composition; The method comprising:

2. 2. The method of claim 1, wherein the solid epoxy resin comprises bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AF based epoxy resin, o-cresol novolak epoxy resin, phenol novolak epoxy resin, modified phenolic epoxy resin, naphthalene epoxy resin, triphenol methane epoxy resin, alkyl modified triphenol methane epoxy resin, triazine nucleus containing epoxy resin, dicyclopentadiene epoxy resin, glycidylamine epoxy resin, biphenyl epoxy resin, biphenyl aralkyl epoxy resin, hydrogenated bisphenol A epoxy resin, aliphatic epoxy resin, stilbene epoxy resin, trisphenol-methane triglycidyl ether, isocyanate modified bisphenol A based epoxy resin, isocyanate modified bisphenol F based epoxy resin, isocyanate modified bisphenol AF based epoxy resin, isocyanate modified bisphenol A novolak epoxy resin, bisphenol F novolak epoxy resin, bisphenol AF novolak epoxy resin, or combinations thereof.

3. The solid phenoxy resin has the following structural formula: [Formula 1] wherein n is an integer from about 8 to about 400, and X is [chemical 2] Selected from: The method of claim 1.

4. The protic solvent is 1 -C 6 -Alkanol, C 2 -C 4 alkanediols, ether alkanols, water, acetic acid, formic acid, and mixtures thereof, and the aprotic solvent is selected from aromatic solvents, alkane solvents, ether solvents, ester solvents, acetone, acetonitrile, dimethylformamide, and mixtures thereof.

5. 2. The method of claim 1, wherein the blend comprises the protic and aprotic solvents in a weight ratio (protic solvent:aprotic solvent) of about 30:70 (w / w) to about 70:30 (w / w).

6. 6. The method of claim 5, wherein the slurry contains about 5% to about 10% by weight of the epoxy or phenoxy resin, based on the total weight of the slurry.

7. 2. The method according to claim 1, wherein the solid phenoxy resin is obtained by a condensation reaction of a dihydric phenol compound and epichlorohydrin, or by a polyaddition reaction of a dihydric phenol compound and a difunctional epoxy resin.

8. 10. The method of claim 1, wherein the slurry is spray dried in a closed cycle spray drying apparatus.

9. 2. A dry powdered thermoplastic resin composition obtainable by the method of claim 1, comprising a plurality of particles selected from epoxy resin particles and phenoxy resin particles.

10. 10. The dry powder thermoplastic resin composition of claim 9, wherein the plurality of particles has an average particle size of about 150 μm or less.

11. 10. The method of claim 9, wherein the dry powdered thermoplastic resin composition has a residual moisture content of about 2% (w / w) or less.

12. 1. A method for forming a dry powdered thermoplastic resin, comprising: dissolving a solid thermoplastic resin selected from a solid phenoxy resin in a blend of a protic solvent and an aprotic solvent to form a slurry; and and spray drying the slurry to form the dry powdered thermoplastic resin composition. the dry powdered thermoplastic resin composition comprises a plurality of phenoxy resin particles having an average particle size of about 3 μm to about 25 μm and a residual moisture content of about 0.01% (w / w) to about 1.5% (w / w), and the spray drying is performed in a closed cycle spray drying apparatus. The method.

13. 1. A method for forming a powdered epoxy or phenoxy resin comprising: providing a solid epoxy or phenoxy resin having an average molecular weight of at least about 1000 Daltons; dissolving the solid epoxy or phenoxy resin in a blend of an alcohol solvent and an aprotic solvent to form a resulting solution; and spray drying the resulting solution in a closed cycle spray dryer to form the powdered epoxy or phenoxy resin; Including, the alcohol solvent has 2 to 6 carbon atoms, the blend has a weight ratio of the alcohol solvent to the polar aprotic solvent of about 30:70 to about 70:30, and the resulting solution has about 1% to about 10% by weight of an epoxy or phenoxy resin based on the total weight of the resulting solution. The method.

14. 14. The method of claim 13, wherein the solid epoxy or phenoxy resin has an average molecular weight of at least about 10,000 Daltons.

15. 14. The method of claim 13, wherein the ratio of the alcohol solvent to the aprotic solvent is from about 40:60 to about 60:

40.

16. 14. The method of claim 13, wherein the alcohol solvent is selected from the group consisting of ethanol, propanol, isopropanol, butanol, pentanol, and hexanol, and the aprotic solvent is selected from the group consisting of methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dichloromethane, and tetrahydrofuran.

17. The method of claim 13, wherein the resulting solution contains from about 5% to about 10% by weight of an epoxy or phenoxy resin.

18. 14. The method of claim 13, wherein the powdered epoxy or phenoxy resin has an average particle size of about 20 μm or less.

19. 1. A powdered epoxy or phenoxy resin comprising: about 5% by weight or less of residual solvent; and at least about 95% by weight of a solid epoxy or phenoxy resin, the solid epoxy or phenoxy resin having an average molecular weight of at least about 1000 Daltons; and an average particle size of about 20 μm or less, and said weight percentages are based on the total weight of said powdered epoxy or phenoxy resin; said powdered epoxy or phenoxy resin;