Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery
Patent Information
- Application Number
- JP2023220488
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium ion secondary battery positive electrode active materials exhibit suboptimal output characteristics, particularly in applications requiring high power density and reduced internal resistance.
A lithium transition metal-containing composite oxide with a layered rock salt type structure, composed of secondary particles formed by agglomerated primary particles, featuring specific particle size, pore structure, and uniform distribution of additive elements, enhancing the contact area with electrolytes.
The solution significantly improves the output characteristics of lithium ion secondary batteries by promoting lithium ion insertion and desorption, leading to higher power output and better cycle stability.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material for lithium ion secondary batteries, which is made of a lithium transition metal-containing composite oxide, and to a lithium ion secondary battery using the positive electrode active material for lithium ion secondary batteries as a positive electrode material. [Background technology]
[0002] In recent years, with the widespread use of portable electronic devices such as smartphones, tablet terminals, digital cameras, and notebook computers, there is a strong demand for the development of small, lightweight secondary batteries with high energy density. There is also a strong demand for the development of high-capacity, high-output secondary batteries as power sources for electric vehicles such as hybrid electric vehicles, plug-in hybrid electric vehicles, and battery-powered electric vehicles.
[0003] A lithium ion secondary battery is a secondary battery that satisfies such requirements. This lithium ion secondary battery is composed of a negative electrode, a positive electrode, a non-aqueous electrolyte or a solid electrolyte, and the active materials used as the materials for the negative electrode and the positive electrode are materials that can extract and insert lithium. The non-aqueous electrolyte includes a non-aqueous electrolyte solution obtained by dissolving a lithium salt, which is a supporting salt, in an organic solvent, and the solid electrolyte includes an inorganic or organic solid electrolyte that is non-flammable and has lithium ion conductivity.
[0004] Among lithium-ion secondary batteries, those that use lithium transition metal-containing composite oxides with layered rock-salt or spinel crystal structures as the positive electrode material can obtain a voltage of about 4 V, and therefore research, development, and commercialization of these batteries as batteries with high energy density are underway.
[0005] Positive electrode materials for lithium-ion secondary batteries include lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel, which is cheaper than cobalt, and lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3Co 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 A positive electrode active material made of a lithium-transition metal-containing composite oxide such as lithium-sulfur oxide (LiO2) has been proposed.
[0006] In recent years, among these lithium transition metal-containing composite oxides, lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 A ternary positive electrode active material made of lithium nickel manganese cobalt-containing composite oxide (NMC), which contains at least nickel, manganese, and cobalt as transition metals, including CrO2), has attracted attention as a material that has excellent thermal stability, high capacity, good battery capacity cycle characteristics, and can provide high output with low resistance. Lithium nickel manganese cobalt composite oxide is a compound that has a layered rock salt type crystal structure, like lithium cobalt composite oxide and lithium nickel composite oxide.
[0007] Regarding lithium-transition metal-containing composite oxides, the focus of their development is on increasing their output by reducing their internal resistance. In particular, there is a high demand for further reduction in internal resistance to increase output in applications as power sources for electric vehicles.
[0008] In order to improve the output characteristics and cycle characteristics of a positive electrode active material made of a lithium transition metal-containing composite oxide such as a lithium nickel-containing composite oxide or a lithium nickel manganese cobalt-containing composite oxide, it is important to use particles with a small particle size and a narrow particle size distribution. Particles with a small particle size have a large specific surface area, and when used as a positive electrode active material, they can sufficiently secure the reaction area with the electrolyte, and furthermore, the positive electrode can be made thin, and the movement distance of lithium ions between the positive electrode and the negative electrode can be shortened. Therefore, by using particles with a small particle size, it is possible to reduce the positive electrode resistance. In addition, by using particles with a narrow particle size distribution, the voltage applied to the particles in the electrode can be made uniform, making it possible to suppress the decrease in battery capacity due to selective deterioration of the fine particles.
[0009] In order to further improve the output characteristics, research and development is also being conducted on improving the particle structure of lithium transition metal-containing composite oxides. For example, it is considered that forming a space portion into which the electrolyte can enter inside the positive electrode active material is effective for improving the output characteristics. By adopting such a structure, the reaction area with the electrolyte can be increased compared to a positive electrode active material with a solid structure having a similar particle size, so that the positive electrode resistance can be significantly reduced. It is known that the positive electrode active material inherits the particle properties of its precursor, the transition metal-containing composite hydroxide. In other words, in order to obtain a positive electrode active material with a space portion, it is necessary to appropriately control the particle size, particle size distribution, particle structure, etc. of the secondary particles of the transition metal-containing composite hydroxide, which is the precursor.
[0010] For example, JP2012-246199A and WO2012 / 131881A disclose a method for producing transition metal-containing composite hydroxide particles, which serve as a precursor of a positive electrode active material, by a crystallization reaction clearly separated into two stages: a nucleation step in which nucleation is mainly performed, and a particle growth step in which particle growth is mainly performed. In these methods, by appropriately adjusting the pH value and reaction atmosphere in the nucleation step and the particle growth step, transition metal-containing composite hydroxide particles are obtained that have a small particle size and a narrow particle size distribution, and are composed of a low-density center part made of fine primary particles and a high-density outer shell part made of plate-like or needle-like primary particles. The positive electrode active material obtained from such composite hydroxide particles has a hollow structure, which increases the contact area with the electrolyte, making it possible to improve the output characteristics.
[0011] WO2014 / 181891 and JP2018-104276A disclose a method for producing transition metal-containing composite hydroxide particles, which includes a nucleation step in which the pH value of an aqueous nucleation solution containing at least a metal compound containing a transition metal and an ammonium ion donor is controlled to be 12.0 or more and 14.0 or less to generate nuclei, and a particle growth step in which the pH value of an aqueous particle growth solution containing the generated nuclei is controlled to be lower than the pH value of the nucleation step and to be 10.5 or more and 12.0 or less to grow the nuclei, and the initial stage of the nucleation step and the particle growth step are a non-oxidizing atmosphere, and at a predetermined timing in the particle growth step, the atmosphere is switched to an oxidizing atmosphere, and then the atmosphere is switched back to a non-oxidizing atmosphere at least once. This method makes it possible to obtain transition metal-containing composite hydroxide particles which have a small particle size and a narrow particle size distribution, have a core formed by the aggregation of plate-like or needle-like primary particles, and have two layered structures in which a low-density layer formed by the aggregation of fine primary particles and a high-density layer formed by the aggregation of plate-like primary particles are alternately stacked outside the core.
[0012] The positive electrode active material using these transition metal-containing composite hydroxide particles as a precursor has a small particle size, a narrow particle size distribution, and a multi-layer structure having a hollow structure or spaces. Therefore, it is said that the secondary battery using these positive electrode active materials can simultaneously improve the battery capacity, output characteristics, and cycle characteristics. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2012-246199 A [Patent Document 2] WO2012 / 131881 publication [Patent Document 3] WO2014 / 181891 publication [Patent Document 4] JP 2018-104276 A Summary of the Invention [Problem to be solved by the invention]
[0014] However, there is room for improvement in the output characteristics of the positive electrode active materials described in these documents, and further improvement in the output characteristics is therefore required.
[0015] In view of the above problems, an object of the present invention is to provide a positive electrode active material for a lithium ion secondary battery that is capable of exhibiting excellent output characteristics when used in a lithium ion secondary battery. [Means for solving the problem]
[0016] The positive electrode active material for a lithium ion secondary battery according to an embodiment of the present invention is The composite oxide particles are represented by the general formula (A): Li 1+u Ni x Mn y Co z M tand a lithium transition metal-containing composite oxide particle having a composition represented by the formula: O2 (wherein, -0.05≦u≦0.5, x+y+z+t=1, 0.3≦x≦0.9, 0≦y≦0.5, 0≦z≦0.5, 0≦t≦0.1, and M is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W), and a crystal structure having a layered rock salt structure, The lithium transition metal-containing composite oxide particles are composed of secondary particles formed by agglomeration of primary particles, The secondary particles are 50% cumulative diameter d50 calculated from particle size distribution measurements of particles 3.0 μm to 7.0 μm 1.8m 2 / g or more 5.5m 2 / g or less BET specific surface area, A pore peak diameter of 0.01 μm or more and 0.30 μm or less in the pore portion obtained by mercury intrusion porosimetry, and A log differential pore volume [dV / d(logD)] of 0.2 ml / g or more and 0.6 ml / g or less in the range of the pore peak diameter of 0.01 μm or more and 0.30 μm or less, and For each of a plurality of primary particles among the primary particles, each of which has a primary particle diameter in the range of 0.1 μm or more and 1.0 μm or less, the concentration of the added element M is measured at a plurality of locations by cross-sectional STEM or TEM-EDX analysis, and a coefficient of variation of the concentration of the added element M, which is the standard deviation of the concentration of the added element M divided by the average concentration of the added element M, is calculated. The coefficient of variation is 1.5 or less.
[0017] The 50% cumulative diameter d50 of the secondary particles is preferably 4.0 μm or more and 6.0 μm or less.
[0018] It is preferable that the index showing the spread of the particle size distribution of the secondary particles, [(d90-d10) / d50] (where d10 is the 10% cumulative diameter obtained from the particle size distribution measurement values, and d90 is the 90% cumulative diameter obtained from the particle size distribution measurement values), is 1.0 or less.
[0019] The secondary particles preferably have a d90 / d10 value of 1.0 or more and 2.0 or less.
[0020] The secondary particles preferably have an aggregate portion, one or more through holes that connect the outer periphery of the aggregate portion, and two or more spaces that are present inside the aggregate portion and communicate with the through holes. The number of through holes is preferably two or more. The two or more spaces preferably communicate with the through holes or other spaces.
[0021] The additional element M is preferably one or more selected from the group consisting of Mg, Al, Si, Ti, Zr, Nb, Mo, and W. The additional element M is preferably W.
[0022] The lithium ion secondary battery according to the embodiment of the present invention comprises a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte (non-aqueous electrolyte secondary battery), or comprises a positive electrode, a negative electrode, and a solid electrolyte (solid electrolyte secondary battery), and is characterized in that the positive electrode active material for the lithium ion secondary battery according to the present invention is used as the positive electrode active material used in the positive electrode. Effect of the Invention
[0023] In the positive electrode active material for lithium ion secondary batteries according to the embodiment of the present invention, the contact area with the non-aqueous electrolyte or solid electrolyte is sufficiently large, so that the insertion and desorption of lithium ions at the particle interface is promoted, and the output characteristics can be improved. Therefore, the lithium ion secondary battery to which the positive electrode active material for lithium ion secondary batteries according to the embodiment of the present invention is applied can provide high output characteristics, and therefore, its industrial significance is very great. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is an SEM photograph of a cross section of a secondary particle constituting the positive electrode active material for a lithium ion secondary battery of Example 1 of the present invention. [Diagram 2]Figure 2 is a SEM photograph of the cross section of the secondary particles constituting the positive electrode active material for the lithium ion secondary battery of Comparative Example 1. [Diagram 3] Figure 3 is a schematic cross-sectional view of the 2032 type coin-shaped battery used for battery evaluation. [Figure 4] Figure 4 is a graph showing a measurement example of impedance evaluation. [Diagram 5] Figure 5 is a schematic explanatory diagram of the equivalent circuit used for analysis.
Mode for Carrying Out the Invention
[0025] 1. Positive Electrode Active Material for Lithium Ion Secondary Battery The positive electrode active material for a lithium ion secondary battery (hereinafter referred to as "positive electrode active material") according to an example of an embodiment of the present invention is composed of lithium transition metal-containing composite oxide particles (hereinafter referred to as "composite oxide particles"), and is characterized by having the following requirements (1) to (7).
[0026] (1) Composition The composite oxide particles have a composition represented by the general formula (A): Li 1+u Ni x Mn y Co z M t O2 (where -0.05 ≦ u ≦ 0.5, x + y + z + t = 1, 0.3 ≦ x ≦ 0.9, 0 ≦ y ≦ 0.5, 0 ≦ z ≦ 0.5, 0 < t ≦ 0.1, and M is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W).
[0027] In the positive electrode active material of the present invention, the value of u, which indicates the excess amount of lithium (Li), is in the range of -0.05 to 0.5. It is preferably in the range of 0 to 0.50, more preferably in the range of 0 to 0.35. By restricting the value of u to the above range, it is possible to improve the output characteristics and battery capacity of a lithium ion secondary battery using this positive electrode active material as a positive electrode material. On the other hand, if the value of u is less than -0.05, the positive electrode resistance of the secondary battery increases, so that the output characteristics may not be improved. If it exceeds 0.5, not only the initial discharge capacity decreases, but also the positive electrode resistance may increase.
[0028] Nickel (Ni) is an element that contributes to the high potential and high capacity of a secondary battery, and the value of x, which indicates its content, is in the range of 0.3 to 0.9. It is preferably in the range of 0.4 to 0.7, more preferably in the range of 0.4 to 0.6. If the value of x is less than 0.3, the energy density of a secondary battery using this positive electrode active material may not be sufficiently improved. If the value of x exceeds 0.9, the content of other elements that improve output characteristics and durability characteristics decreases, and the characteristics as a positive electrode active material may not be sufficiently obtained.
[0029] Manganese (Mn) is an element that contributes to improving thermal stability, and the value of y, which indicates the content of manganese, is in the range of 0 to 0.5, and preferably in the range of 0.1 to 0.4. If the value of y exceeds 0.5, Mn may be eluted from the positive electrode active material during high-temperature operation, which may deteriorate the charge-discharge cycle characteristics.
[0030] Cobalt (Co) is an element that contributes to improving charge / discharge cycle characteristics and output characteristics, and the value z indicating the content of Co is in the range of 0 to 0.5, preferably 0.1 to 0.4. If the value z exceeds 0.5, the initial discharge capacity of a secondary battery using this positive electrode active material may decrease.
[0031] In the positive electrode active material of the present invention, the following additive element M can be contained. As the additive element M, one or more selected from magnesium (Mg), aluminum (Al), silicon (Si), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo), hafnium (Hf), tantalum (Ta), and tungsten (W) can be used.
[0032] The additive element M is preferably at least one selected from the group consisting of Mg, Al, Si, Ti, Zr, Nb, Mo, and W, and more preferably W.
[0033] The value of t indicating the content of the additive element M is in the range of more than 0 and 0.05 or less. Preferably, it is in the range of 0.001 or more and 0.03 or less. When the value of t exceeds 0.05, the metal elements contributing to the Redox reaction decrease, so the battery capacity of the secondary battery decreases.
[0034] The additive element M may be dispersed inside the composite oxide particles or may coat the surface of the composite oxide particles. In any case, it is preferable to control the content of the additive element M so as to be within the above range.
[0035] The composite oxide particles of the present invention are preferably composed of a lithium nickel manganese cobalt-containing composite oxide (NMC) containing Ni, Mn, and Co as main transition metals. In this case, the composite oxide particles have the general formula (B): Li 1+u Ni x Mn y Co z M t O2 (-0.05 ≦ u ≦ 0.5, x + y + z + t = 1, 0.3 ≦ x ≦ 0.7, 0.15 ≦ y ≦ 0.4, 0.15 ≦ z ≦ 0.4, 0 < t ≦ 0.05, M is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W).
[0036] The composition of the positive electrode active material can be confirmed by, for example, inductively coupled plasma emission spectrometry or Rietveld analysis of parameters obtained by powder X-ray diffraction.
[0037] When the positive electrode active material of the present invention has a composition represented by the above general formula (A) or (B), it is of the layered rock salt type and has a hexagonal crystal structure.
[0038] (2) Particle structure In the positive electrode active material of the present invention, the composite oxide particles are composed of secondary particles formed by aggregation of a plurality of primary particles.
[0039] The secondary particles preferably have an agglomeration portion, one or more communicating holes that communicate with the outer periphery of the agglomeration portion, and two or more spaces that are present inside the agglomeration portion and communicate with the communicating holes.
[0040] The two or more spaces preferably communicate with the communication hole or with another space. The number of the communication holes is also preferably two or more.
[0041] When the composite oxide particles have such a secondary particle structure, it becomes possible to easily realize the particle properties of the positive electrode active material of the present invention, which will be described later.
[0042] If the pores in the outer periphery are not connected to the internal space, the space inside the particle is isolated, the electrolyte cannot penetrate sufficiently into the composite oxide particle (secondary particle), and a sufficient reaction field cannot be secured, so that the desired battery performance may not be fully achieved in a secondary battery using this positive electrode active material. Each of the two or more internal spaces can directly communicate with the pores in the outer periphery. Alternatively, they can communicate with the pores in the outer periphery via other pores.
[0043] This structure allows the electrolyte to penetrate sufficiently into the space inside the particle through the communicating holes on the outer periphery, making it possible to desorb and insert lithium not only on the surface of the particle but also inside the particle, ensuring a sufficient reaction field and making it possible to significantly reduce the internal resistance of the battery.
[0044] Therefore, when a lithium ion secondary battery is constructed by using a positive electrode active material having such a structure as a positive electrode material, it becomes possible to further improve the output characteristics.
[0045] (3) Particle size In the positive electrode active material of the present invention, the secondary particles have a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement value. The 50% cumulative diameter d50 of the secondary particles is preferably 4.0 μm or more and 6.5 μm or less, and more preferably 4.0 μm or more and 6.0 μm or less.
[0046] More specifically, the 50% cumulative diameter d50 is the particle size at which the cumulative volume calculated from the volume integrated value measured by a laser light diffraction scattering particle size analyzer is 50% of the total volume of all particles (the particle size at the point where the cumulative curve of the particle size distribution is 50% when the total volume is set to 100%).
[0047] If the d50 of the particles constituting the positive electrode active material is within the above range, not only can the battery capacity per unit volume of a secondary battery using this positive electrode active material be increased, but also the safety and output characteristics can be improved.
[0048] On the other hand, if the 50% cumulative diameter d50 is less than 3.0 μm, the packing property of the positive electrode active material decreases, and it may be difficult to increase the battery capacity per unit volume. If the 50% cumulative diameter d50 exceeds 7.0 μm, the reaction area of the positive electrode active material decreases, and the interface with the electrolyte decreases, so that it may be difficult to improve the output characteristics.
[0049] (4) BET specific surface area In the positive electrode active material of the present invention, the secondary particles have a diameter of 1.8 m2 / g or more 5.5m 2 The BET specific surface area is 2.0 m 2 / g or more 5.0m 2 / g or less, and 2.5m 2 / g or more 4.5m 2 It is more preferable that the molecular weight is not more than 1 / g.
[0050] The BET specific surface area of the secondary particles is an index of particle properties (contact area with electrolyte) of the positive electrode active material. When the secondary particles have an aggregate portion, one or more through holes that connect the outer periphery of the aggregate portion, and two or more spaces that are present inside the aggregate portion and connect to the through holes, the BET specific surface area represents the surface area including the through holes (openings) present in the outer periphery of the secondary particles and the microcavities (spaces) inside the secondary particles.
[0051] The BET specific surface area is measured by the BET method using nitrogen gas adsorption.
[0052] The BET specific surface area of the secondary particles is 1.8 m 2 When the BET specific surface area of the secondary particles is less than 5.5 m / g, when a secondary battery is constructed using this positive electrode active material, the reaction area with the electrolyte cannot be sufficiently secured, and there is a possibility that the output characteristics are not sufficiently improved. 2 If it exceeds 1 / g, the reaction area between the positive electrode active material and the electrolyte becomes too large, which may decrease the durability of the secondary battery.
[0053] (5) Pore peak diameter In the positive electrode active material of the present invention, the secondary particles have a pore peak diameter of 0.01 μm or more and 0.30 μm or less in a pore portion obtained by mercury intrusion porosimetry, preferably 0.02 μm or more and 0.28 μm or less, more preferably 0.05 μm or more and 0.25 μm or less.
[0054] Specifically, the pore peak diameter is defined as the diameter at which the pore peak exists in a pore distribution plot of the secondary particles obtained by mercury intrusion porosimetry.
[0055] The pore peak diameter of the secondary particles is an index representing the particle properties (average pore diameter) of the positive electrode active material. More specifically, when the pore peak diameter of the secondary particles constituting the positive electrode active material is within the above-mentioned range, it means that the particles are a positive electrode active material having pores.
[0056] If the secondary particle pore peak diameter is less than 0.01 μm, the particle strength cannot be maintained due to the small pore diameter, and the particles may be crushed, which may impair the battery performance.If the secondary particle pore peak diameter exceeds 0.30 μm, when a secondary battery is constructed using this positive electrode active material, the reaction area with the electrolyte may not be sufficiently secured, and the output characteristics may not be fully exhibited.
[0057] (6) Log differential pore volume In the positive electrode active material of the present invention, the secondary particles have a log differential pore volume [dV / d(logD)] of 0.2 ml / g to 0.6 ml / g in the pore peak diameter range of 0.01 μm to 0.30 μm, preferably 0.2 ml / g to 0.6 ml / g, more preferably 0.25 ml / g to 0.5 ml / g.
[0058] The log differential pore volume [dV / d(logD)] at the pore peak diameter is an index representing the particle properties (volume of all cavities) of the positive electrode active material. More specifically, the log differential pore volume [dV / d(logD)] at the pore peak diameter is a value at the pore peak diameter in the log differential pore volume distribution obtained by dividing the differential pore volume dV calculated for each pore diameter based on the pore distribution plot of the secondary particles obtained by mercury intrusion by the logarithmic differential value d(logD) of the pore diameter. In the secondary particles constituting the positive electrode active material, when the log differential pore volume [dV / d(logD)] is in the above range, it means that the particle has an appropriate amount of space formed therein, and a sufficient reaction area is obtained.
[0059] If the log differential pore volume [dV / d(logD)] at the pore peak diameter is less than 0.2 ml / g, sufficient voids may not be formed inside the secondary particles, and sufficient reaction area may not be obtained. If the log differential pore volume [dV / d(logD)] at the pore peak diameter is more than 0.6 ml / g, many voids will be structurally present inside the secondary particles, resulting in a low bulk density and poor packing, and therefore, when a secondary battery is constructed using the positive electrode active material, sufficient battery capacity per unit volume may not be obtained.
[0060] (7) Coefficient of variation of the concentration of added element M In the positive electrode active material of the present invention, the coefficient of variation (CV) indicating the variation in concentration of the additive element M within the primary particles constituting the secondary particles is 1.5 or less, preferably 1.3 or less, and more preferably 1.2 or less.
[0061] The coefficient of variation of the concentration of the additional element M is an index showing the variation of the concentration of the additional element M throughout the primary particle including the grain interior and grain boundaries of the primary particle.
[0062] The coefficient of variation of the concentration of the additive element M is obtained as follows. First, the positive electrode active material is processed into a thin slice using a focused ion beam device (FIB) or an ion milling device to expose the cross section of the secondary particle. Using a scanning transmission electron microscope (STEM) or a transmission electron microscope (TEM), two connected primary particles having a primary particle diameter in the range of 0.1 μm to 1.0 μm are targeted in the cross section of the secondary particle, and multiple locations of each of the two primary particles are irradiated with an electron beam, and the energy of the characteristic X-ray of the generated additive element M is analyzed with an energy dispersive X-ray analyzer (EDX) to determine the concentration of the additive element M at each location.
[0063] From the obtained data on the concentration of the additional element M, the average concentration (μ) of the additional element M and the standard deviation (σ) of the concentration of the additional element M are obtained.
[0064] The coefficient of variation (CV) of the concentration of the added element M is calculated by the formula: CV=σ / μ.
[0065] If the coefficient of variation (CV) of the concentration of the additive element M exceeds 1.5, the distribution of the additive element M in the primary particles and / or secondary particles will become biased, and in a secondary battery using this positive electrode active material, the battery performance such as the battery capacity and output characteristics may be impaired.
[0066] (8) Particle size distribution Although optional, in the positive electrode active material of the present invention, the index showing the spread of the particle size distribution of the secondary particles, [(d90-d10) / d50], is preferably 1.0 or less, more preferably 0.7 or less, and even more preferably 0.6 or less. A positive electrode active material made of secondary particles having such a narrow particle size distribution has a small proportion of fine particles and coarse particles, and therefore a secondary battery using this has excellent safety, cycle characteristics, and output characteristics.
[0067] When [(d90-d10) / d50] exceeds 1.0, the ratio of fine particles and coarse particles in the positive electrode active material increases. For example, when the ratio of fine particles is high, the secondary battery is likely to generate heat due to local reactions of the fine particles, and not only does this lower safety, but the cycle characteristics may also be poor due to selective deterioration of the fine particles. In addition, when the ratio of coarse particles is high, the reaction area between the electrolyte and the positive electrode active material cannot be sufficiently secured, and the output characteristics may be poor.
[0068] In the case of industrial-scale production, it is not realistic to use a positive electrode active material with an excessively small [(d90-d10) / d50]. Therefore, in consideration of cost and productivity, it is preferable that the lower limit of [(d90-d10) / d50] is about 0.3.
[0069] The meaning and calculation method of d10 and d90 in the index showing the spread of particle size distribution [(d90-d10) / d50] are the same as those of d50 described above, where d90 is the particle size at which the cumulative volume of each particle, calculated from the smaller particle size side, is 90% of the total volume of all particles, and d10 is the particle size at which the cumulative volume of each particle, calculated from the smaller particle size side, is 10% of the total volume of all particles.
[0070] (9)d90 / d10 Although optional, in the positive electrode active material of the present invention, the ratio of the d90 value to the d10 value obtained from the particle size distribution measurement value of the secondary particles (d90 / d10) is preferably 1.0 or more and 2.0 or less, and more preferably 1.2 or more and 1.8 or less.
[0071] If the d90 / d10 value of the secondary particles constituting the positive electrode active material is within this range, not only can the battery capacity per unit volume of the secondary battery using this positive electrode active material be increased, but also the safety and output characteristics can be improved. If the d90 / d10 value of the secondary particles exceeds 2.0, the reaction area of the positive electrode active material decreases, and the interface with the electrolyte decreases, which may make it difficult to improve the output characteristics.
[0072] (10)Crystallite size determined from the X-ray diffraction pattern of the (003) plane Although optional, when the crystallite diameter of the primary particles of the composite oxide particles constituting the positive electrode active material of the present invention is determined by the Scherrer equation from the half-width of the peak of the (003) plane by X-ray diffraction, the crystallite diameter is preferably in the range of 300 Å to 1500 Å, more preferably in the range of 400 Å to 1300 Å, and even more preferably in the range of 700 Å to 1250 Å. A positive electrode active material having a crystallite diameter in such a range has extremely high crystallinity, and can reduce the positive electrode resistance of a secondary battery and improve its output characteristics.
[0073] If the crystallite diameter of the (003) plane is less than 300 Å, the primary particles are too fine and the pores between the primary particles in the positive electrode active material are too fine, making it difficult for the electrolyte to penetrate into the positive electrode active material, reducing the reaction area with the electrolyte and degrading the output characteristics of the secondary battery.If the crystallite diameter of the (003) plane exceeds 1500 Å, the primary particles become too coarse, drastically reducing the proportion of pores in the secondary particles and reducing the penetration paths for the electrolyte, reducing the reaction area with the electrolyte and degrading the output characteristics of the secondary battery.
[0074] 2. Manufacturing method of positive electrode active material for lithium-ion secondary batteries The positive electrode active material of the present invention is not limited by its production method so long as it has the above-mentioned composition, crystal structure, particle structure, and particle properties.
[0075] However, by producing the positive electrode active material of the present invention by the production method described below, it becomes possible to easily produce a positive electrode active material having the above-mentioned composition, crystal structure, particle structure, and particle properties.
[0076] Specifically, the positive electrode active material of the present invention can be obtained by switching between an oxidizing atmosphere and a non-oxidizing atmosphere during a crystallization process to prepare a transition metal-containing composite hydroxide such as a nickel-manganese-cobalt-containing composite hydroxide, mixing the composite hydroxide or heat-treated particles obtained by heat-treating the composite hydroxide with a lithium compound, and calcining the resulting lithium mixture.
[0077] Hereinafter, each step will be described in detail using as an example a case in which the composite oxide particles are lithium nickel manganese cobalt-containing composite oxide particles.
[0078] (1) Crystallization process Appropriate amounts of water, aqueous sodium hydroxide solution, and aqueous ammonia are supplied into a reaction tank to prepare a pre-reaction aqueous solution adjusted to a pH value of 11 to 13 at a liquid temperature of 25°C and an ammonium ion concentration of 9 g / L to 15 g / L. Meanwhile, it is desirable to dissolve nickel sulfate, manganese sulfate, cobalt sulfate, and a compound of added element M (sulfate, sodium salt, etc.) in water so that the molar ratio of each metal element (Ni, Co, Mn, M) satisfies the above formula (A), and prepare a raw material aqueous solution of 1.0 mol / L to 3.0 mol / L. In order to suppress the coefficient of variation of the additive element M dissolved inside the particles and to prevent the additive element M from co-precipitating locally around the transition metal element, it is more preferable to dissolve nickel sulfate, manganese sulfate, and cobalt sulfate in water so that the molar ratio of each metal element (Ni, Co, Mn) satisfies the above formula (A), prepare a raw material aqueous solution of 1.0 mol / L or more and 3.0 mol / L or less, prepare a separate aqueous solution containing a compound of the additive element M, and add the amount of the additive element M to the raw material aqueous solution so that the amount satisfies the above formula (A).
[0079] Next, the raw material aqueous solution is supplied to the pre-reaction aqueous solution while blowing in a non-oxidizing atmosphere gas with an oxygen concentration of 2% by volume or less, such as argon gas or nitrogen, to perform nucleation. At this time, it is desirable to supply an aqueous sodium hydroxide solution and an aqueous ammonia solution appropriately to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above-mentioned ranges.
[0080] After the nucleation is completed, an acid such as sulfuric acid is added to adjust the pH value to 10 to 12 at a liquid temperature of 25°C and lower than the pH value in the nucleation step, thereby forming an aqueous solution for particle growth. After it is confirmed that the pH value has reached a predetermined value, the raw material aqueous solution is supplied to grow the nuclei (particles) generated in the nucleation step. When an aqueous solution containing a compound of the additive element M is separately prepared, the aqueous solution containing the compound of the additive element M can be added only in the particle growth step or only at a specific stage of the particle growth step.
[0081] As the first stage of particle growth, crystallization is continued in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less for a certain period of time from the start of the particle growth step while stirring with a stirrer.
[0082] In the second stage, while continuing to supply the raw material aqueous solution, a micro-nano bubble generator is used to circulate extremely fine bubbles of oxidizing atmosphere gas consisting of air or oxygen in the reaction tank, and switching operation 1 is performed to adjust the reaction atmosphere to an oxidizing atmosphere with an oxygen concentration of 21% by volume or more. After the start of switching operation 1, crystallization is performed while maintaining the oxidizing atmosphere and stirring with a stirrer for a certain period of time.
[0083] In the third step, while continuing to supply the raw material aqueous solution, a micro-nano bubble generator is used to circulate extremely fine bubbles of a non-oxidizing gas in the reaction tank, and the reaction atmosphere is adjusted to a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less, in a switching operation 2. After the start of the switching operation 2, crystallization is carried out while maintaining the non-oxidizing atmosphere and stirring with a stirrer for a certain period of time.
[0084] In the fourth step, while continuing to supply the raw material aqueous solution, a micro-nano bubble generator is used to circulate extremely fine bubbles of an oxidizing gas in the reaction tank, and the reaction atmosphere is adjusted to an oxidizing atmosphere with an oxygen concentration of 21% by volume or more, in a switching operation 3. After the start of the switching operation 3, crystallization is carried out while maintaining the oxidizing atmosphere and stirring with a stirrer for a certain period of time.
[0085] In the fifth step, while continuing to supply the raw material aqueous solution, a micro-nano bubble generator is used to circulate extremely fine bubbles of a non-oxidizing gas in the reaction tank, and the reaction atmosphere is adjusted to a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less, in a switching operation 4. After the start of the switching operation 4, crystallization is carried out while maintaining the non-oxidizing atmosphere and stirring with a stirrer for a certain period of time.
[0086] In the present invention, a micro-nano bubble generator is used as a device for switching and maintaining the reaction atmosphere of the aqueous solution for particle growth. The diameter of the bubbles (micro-nano bubbles) generated by the micro-nano bubble generator is 0.01 mm or less, and since the buoyancy is small, the bubbles remain in the water for a long time, so that the reaction atmosphere can be quickly switched between a non-oxidizing atmosphere gas and an oxidizing atmosphere gas, and the oxygen concentration can be made lower or higher. Similarly, it is preferable to use a micro-nano bubble generator in the nucleation step from the viewpoint of quickly maintaining a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less and forming dense nuclei.
[0087] The time for each stage in the particle growth process is as follows: stage 2≦stage 4<stage 1≦stage 3≦stage 5. The crystallization time for the entire particle growth process is preferably within 8 hours.
[0088] Similarly, the particle growth step may be performed by switching operations 5 and 6 to provide a sixth stage in an oxidizing atmosphere and a seventh stage in a non-oxidizing atmosphere. Furthermore, the particle growth step may be performed by switching operations 7 and 8 to provide an eighth stage in an oxidizing atmosphere and a ninth stage in a non-oxidizing atmosphere. Furthermore, the particle growth step may be performed by additionally performing switching operations 9 and 10 to provide a tenth stage in an oxidizing atmosphere and an eleventh stage in a non-oxidizing atmosphere.
[0089] In these cases, the time for each stage in the particle growth process is: stage 2 ≦ stage 4 ≦ stage 6 ≦ stage 8 ≦ stage 10 < stage 1 ≦ stage 3 ≦ stage 5 ≦ stage 7 ≦ stage 9 ≦ stage 11. In each stage, a micro / nano bubble generator is used as a device for switching and maintaining the reaction atmosphere of the aqueous solution for particle growth.
[0090] After the crystallization is completed, the resulting product is washed with water, filtered and dried to obtain the desired nickel-cobalt-manganese-containing composite hydroxide particles.
[0091] In the particle growth step, it is desirable to appropriately supply an aqueous sodium hydroxide solution and an aqueous ammonia solution throughout this step, and to maintain the pH value and the ammonium ion concentration of the aqueous solution for particle growth within the above-mentioned ranges.
[0092] The composite hydroxide particles obtained by such a crystallization process have a particle structure in which low-density layers and high-density layers are mutually laminated around a high-density center. By using composite hydroxide particles having such a particle structure as a precursor, composite oxide particles having a particle structure including aggregated portions, one or more communicating holes connecting the outer peripheries of the aggregated portions, and two or more spaces present inside the aggregated portions and connecting with the communicating holes can be easily obtained.
[0093] (2)Mixing process The mixing step is a step of mixing the above-mentioned composite hydroxide particles or heat-treated particles obtained by subjecting the composite hydroxide particles to a heat treatment with a lithium compound to obtain a lithium mixture.
[0094] In the mixing step, the composite hydroxide particles and the lithium compound are mixed so that the ratio (Li / Me) of the sum of the atomic numbers of metal atoms other than Li in the lithium mixture, specifically Ni, Mn, Co, and the additive element M, to the atomic number of Li (Li), is 0.95 to 1.5, preferably 1.0 to 1.5, more preferably 1.0 to 1.35, and even more preferably 1.0 to 1.2. That is, since Li / Me does not change before and after the firing step, it is necessary to mix the composite hydroxide and the lithium compound so that the Li / Me in the mixing step becomes the Li / Me of the target positive electrode active material.
[0095] The lithium compound used in the mixing step is not particularly limited, but it is preferable to use lithium hydroxide, lithium nitrate, lithium carbonate, or a mixture thereof in terms of availability. In particular, it is preferable to use lithium hydroxide or lithium carbonate in terms of ease of handling and stability of quality.
[0096] For mixing, a general mixer such as a shaker mixer, a Loedige mixer, a Julia mixer, or a V blender can be used.
[0097] (3) Calcination process When lithium hydroxide or lithium carbonate is used as the lithium compound, a calcination step can be performed after the mixing step and before the calcination step, in which the lithium mixture is calcined at a temperature lower than the calcination temperature described below and between 350° C. and 800° C., preferably between 450° C. and 750° C. This allows Li to be sufficiently diffused in the composite hydroxide particles, and more uniform composite oxide particles can be obtained.
[0098] The holding time at the above temperature is preferably 1 hour to 10 hours, more preferably 3 hours to 6 hours. The atmosphere in the calcination step is preferably an oxidizing atmosphere, similar to the firing step described below, and more preferably an atmosphere with an oxygen concentration of 18 volume % to 100 volume %.
[0099] (4) Firing process The calcination step is a step in which the lithium mixture obtained in the mixing step is calcined under predetermined conditions to diffuse Li into the composite hydroxide and cause a reaction, thereby obtaining composite oxide particles.
[0100] The furnace used in the firing step is not particularly limited, and may be any furnace capable of heating the lithium mixture in air or oxygen flow. However, from the viewpoint of maintaining a uniform atmosphere in the furnace, an electric furnace that does not generate gas is preferred, and either a batch-type or continuous-type electric furnace can be suitably used. This point is the same for the furnaces used in the heat treatment step and the calcination step.
[0101] a) Firing temperature The calcination temperature of the lithium mixture is set to 720°C or more and 980°C or less. If the calcination temperature is less than 720°C, the composite hydroxide particles and Li do not react sufficiently, and excess Li or unreacted composite hydroxide remains, or the crystallinity of the obtained positive electrode active material becomes insufficient. On the other hand, if the calcination temperature exceeds 980°C, the interconnected holes and spaces in the composite oxide particles are crushed, which may lead to a decrease in the BET specific surface area of the finally obtained positive electrode active material (secondary particles), as well as a decrease in the pore peak diameter and the log differential pore volume at the pore peak diameter. In addition, the particles of the positive electrode active material are sintered intensely, causing abnormal grain growth, and the proportion of amorphous coarse particles increases.
[0102] By controlling the firing temperature, it is possible to control the BET specific surface area, pore peak diameter, log differential pore volume at the pore peak diameter, and 50% cumulative diameter d50 obtained from particle size distribution measurement values of the positive electrode active material (secondary particles). From the viewpoint of controlling the BET specific surface area, pore peak diameter, log differential pore volume at the pore peak diameter, and 50% cumulative diameter d50 obtained from particle size distribution measurement values of the positive electrode active material (secondary particles), it is preferable to set the firing temperature of the lithium mixture to 730°C or higher and 970°C or lower, and more preferably to set it to 750°C or higher and 970°C or lower.
[0103] The heating rate in the calcination step is preferably set to 1° C. / min to 10° C. / min, more preferably 3° C. / min to 8° C. / min. Furthermore, during the calcination step, at a temperature near the melting point of the lithium compound, the heating rate is lowered to 0.3° C. / min to 6° C. / min, more preferably. This allows the composite hydroxide particles and the lithium compound to react more uniformly.
[0104] b) Baking time During the firing time, the holding time at the above firing temperature is preferably at least 2 hours, and more preferably 3 hours to 20 hours. If the holding time at the firing temperature is less than 2 hours, Li may not be sufficiently diffused into the composite oxide particles, and excess Li or unreacted composite oxide particles may remain, or the crystallinity of the resulting positive electrode active material may be insufficient.
[0105] c) Firing atmosphere The atmosphere during firing is preferably an oxidizing atmosphere, more preferably an atmosphere with an oxygen concentration of 18% by volume or more and 100% by volume or less, and even more preferably an atmosphere with an oxygen concentration of 50% by volume or more and 100% by volume or less. A mixed atmosphere of oxygen and an inert gas with the above oxygen concentration is particularly preferable. That is, firing is preferably performed in air or in an oxygen stream. If the oxygen concentration is less than 18% by volume, the crystallinity of the positive electrode active material may be insufficient.
[0106] (5) Crushing process The secondary particles constituting the positive electrode active material obtained by the firing process may be aggregated or lightly sintered. In such a case, it is preferable to crush the aggregates or sintered bodies. This allows the average particle size and particle size distribution of the obtained positive electrode active material to be adjusted to a suitable range. The crushing refers to an operation of applying mechanical energy to an aggregate consisting of a plurality of secondary particles generated by sintering necking between particles during firing, separating the secondary particles themselves almost without destroying them, and loosening the aggregates.
[0107] As a crushing method, known means can be used, for example, a pin mill, a hammer mill, etc. In this case, it is preferable to control the crushing force within an appropriate range so as not to destroy the secondary particles themselves.
[0108] As described above, by adjusting the firing conditions, it is possible to control the BET specific surface area, pore peak diameter, and log differential pore volume at the pore peak diameter, as well as the 50% cumulative diameter d50 obtained from particle size distribution measurement values of the positive electrode active material (secondary particles), and ultimately, it is possible to easily obtain the positive electrode active material of the present invention having predetermined particle properties.
[0109] 3. Lithium-ion secondary battery The lithium ion secondary battery of the present invention can have the same configuration as a general non-aqueous electrolyte secondary battery, including components such as a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. Alternatively, the lithium ion secondary battery of the present invention can have the same configuration as a general solid electrolyte secondary battery, including components such as a positive electrode, a negative electrode, and a solid electrolyte. That is, the present invention can be widely applied to a non-aqueous electrolyte secondary battery to an all-solid-state lithium ion secondary battery, as long as the secondary battery is charged and discharged by desorption and insertion of lithium ions. Note that the embodiments described below are merely examples, and the present invention can be applied to lithium ion secondary batteries in various forms that have been modified and improved based on the embodiments described in this specification.
[0110] (1) Components a) Positive electrode Using the positive electrode active material of the present invention, a positive electrode of a lithium ion secondary battery is produced, for example, as follows.
[0111] First, the conductive material and the binder are mixed with the positive electrode active material of the present invention, and if necessary, activated carbon, a solvent for viscosity adjustment, etc. are added, and these are kneaded to prepare a positive electrode composite paste. At that time, the mixing ratio of each in the positive electrode composite paste is also an important factor that determines the performance of the lithium ion secondary battery. For example, when the solid content of the positive electrode composite excluding the solvent is 100 parts by mass, the content of the positive electrode active material can be 60 parts by mass or more and 95 parts by mass or less, the content of the conductive material can be 1 part by mass or more and 20 parts by mass or less, and the content of the binder can be 1 part by mass or more and 20 parts by mass or less, as in the case of the positive electrode of a general lithium ion secondary battery.
[0112] The obtained positive electrode composite paste is applied to the surface of a current collector made of, for example, aluminum foil, and dried to evaporate the solvent. If necessary, pressure may be applied by a roll press or the like to increase the electrode density. In this way, a sheet-shaped positive electrode can be produced. The sheet-shaped positive electrode can be cut to an appropriate size according to the intended battery and used to produce the battery. The method for producing the positive electrode is not limited to the above-mentioned example, and other methods may be used.
[0113] As the conductive material, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.) and carbon black-based materials such as acetylene black and ketjen black can be used.
[0114] The binder serves to bind the active material particles together, and may be, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, or polyacrylic acid.
[0115] In addition, if necessary, a solvent for dispersing the positive electrode active material, conductive material, and activated carbon and dissolving the binder can be added to the positive electrode mixture. Specifically, an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent. Activated carbon can also be added to the positive electrode mixture to increase the electric double layer capacity.
[0116] b) Negative electrode The negative electrode can be made of metallic lithium, a lithium alloy, etc. Also, a negative electrode active material capable of absorbing and desorbing lithium ions can be mixed with a binder, and an appropriate solvent can be added to make a paste-like negative electrode mixture, which can be applied to the surface of a metal foil current collector such as copper, dried, and compressed to increase the electrode density as necessary.
[0117] As the negative electrode active material, for example, a material containing lithium such as metallic lithium or a lithium alloy, natural graphite or artificial graphite capable of absorbing and desorbing lithium ions, a fired organic compound such as phenolic resin, or a powder of a carbon material such as coke can be used. In this case, as with the positive electrode, a fluorine-containing resin such as PVDF can be used as the negative electrode binder, and an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent for dispersing these negative electrode active materials and binders.
[0118] c) Separator The separator is sandwiched between the positive electrode and the negative electrode in the lithium ion secondary battery, and has the function of separating the positive electrode and the negative electrode and retaining the electrolyte. As such a separator, for example, a thin membrane such as polyethylene or polypropylene having a large number of fine pores can be used, but there is no particular limitation as long as it has the above function. In addition, a solid electrolyte can also be used.
[0119] d) electrolytes The nonaqueous electrolyte used in the nonaqueous electrolyte secondary battery is, for example, a nonaqueous electrolytic solution obtained by dissolving a lithium salt, which serves as a supporting salt, in an organic solvent.
[0120] The organic solvent used in the nonaqueous electrolyte may be one selected from the following: cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as ethyl methyl sulfone and butane sultone; and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. These may be used alone or in combination of two or more.
[0121] As the supporting salt, LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, and composite salts of these can be used.
[0122] The non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.
[0123] The solid electrolyte used in solid electrolyte secondary batteries such as all-solid-state lithium ion secondary batteries has the property of being able to withstand high voltages. Solid electrolytes include inorganic solid electrolytes and organic solid electrolytes.
[0124] The oxide solid electrolyte may be an oxide that contains oxygen (O) and has lithium ion conductivity and electronic insulation properties, such as Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li3PO4, Li3PO4N X , LiBON X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≦X≦1), Li 1+X Al X Ge 2-X (PO4)3(0≦X≦1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≦X≦2 / 3), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 S 0.6 P 0.4 O4 etc. can be used.
[0125] As the sulfide solid electrolyte, sulfides containing sulfur (S) and having lithium ion conductivity and electronic insulation, such as Li2S-SiS2, Li2S-P2S5, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, etc. can be used.
[0126] As the inorganic solid electrolyte other than the oxide solid electrolyte and the sulfide solid electrolyte, for example, Li3N, LiI, Li3N-LiI-LiOH, etc. can be used.
[0127] As the organic solid electrolyte, a polymeric compound exhibiting ion conductivity can be used. For example, polyethylene oxide, polypropylene oxide, copolymers thereof, etc. can be used. The organic solid electrolyte can also contain a supporting salt (lithium salt).
[0128] When a solid electrolyte is used, the solid electrolyte can be mixed into the positive electrode material in order to ensure contact between the electrolyte and the positive electrode active material.
[0129] (2) Structure of lithium-ion secondary battery The configuration of the lithium ion secondary battery is not particularly limited, and may be a non-aqueous electrolyte secondary battery having a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc., or a solid electrolyte secondary battery having a positive electrode, a negative electrode, a solid electrolyte, etc. The shape of the secondary battery is not particularly limited, and may be a cylindrical shape, a laminated shape, or various other shapes.
[0130] In the case of a non-aqueous electrolyte secondary battery, for example, a positive electrode and a negative electrode are laminated with a separator therebetween to form an electrode body, the obtained electrode body is impregnated with a non-aqueous electrolyte, the positive electrode current collector and a positive electrode terminal connected to the outside, and the negative electrode current collector and a negative electrode terminal connected to the outside are connected using a current collecting lead or the like, and the battery is sealed in a battery case to complete a lithium ion secondary battery.
[0131] (3) Characteristics of lithium-ion secondary batteries As described above, the lithium ion secondary battery of the present invention uses the positive electrode active material of the present invention as a positive electrode material, and therefore has excellent output characteristics and durability characteristics.
[0132] (4) Uses of lithium-ion secondary batteries As described above, the lithium ion secondary battery of the present invention has excellent output characteristics and durability characteristics, and can be suitably used as a power source for power tools and eco-friendly automobiles, which require a high level of these characteristics. EXAMPLES
[0133] The present invention will be described in detail below with reference to examples and comparative examples. Throughout the nucleation step and the particle growth step, the pH value of the reaction solution was measured by a pH controller, and the supply amount of the sodium hydroxide solution was adjusted based on the measured value, thereby controlling the fluctuation width of the pH value of the reaction solution in each step within the range of ±0.2.
[0134] Example 1 a) Preparation of composite hydroxides [Nucleation process] First, 17 L of water was put into the reaction tank and the temperature in the tank was set to 40° C. while stirring. At this time, a micro-nano bubble generator made of ceramic porous body (manufactured by Noritake Co., Ltd., micro-nano bubble high-efficiency gas-liquid reaction device) was used to circulate extremely fine nitrogen gas bubbles in the reaction tank for 1 hour, and the reaction atmosphere was made into a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less. Next, an appropriate amount of 25% by mass sodium hydroxide aqueous solution and 25% by mass ammonia water were supplied into the reaction tank, and the pH value was adjusted to 12.6 based on a liquid temperature of 25° C., and the ammonium ion concentration was adjusted to 10 g / L, thereby forming a pre-reaction aqueous solution.
[0135] At the same time, nickel sulfate, manganese sulfate, and cobalt sulfate were dissolved in water so that the molar ratio of the respective metal elements was Ni:Co:Mn=5:2:3, to prepare a 2 mol / L raw material aqueous solution.
[0136] W was used as the additive element M. Sodium tungstate dihydrate was dissolved in water to prepare an aqueous sodium tungstate solution so that the molar ratio of the metal elements including the additive element M in the resulting composite hydroxide particles was Ni:Mn:Co:W=5.0:2.0:3.0:0.1.
[0137] Next, the raw material aqueous solution was fed to the pre-reaction aqueous solution at 115 ml / min to form an aqueous solution for nucleation, and nucleation was carried out for 1 minute. At this time, 25% by mass of sodium hydroxide aqueous solution and 25% by mass of ammonia water were fed at appropriate times to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above-mentioned ranges.
[0138] [Particle growth process] After the nucleation was completed, the supply of all aqueous solutions was stopped temporarily, and sulfuric acid was added to adjust the pH value to 11.0 at a liquid temperature of 25°C, forming an aqueous solution for particle growth. After it was confirmed that the pH value had reached the specified value, the raw aqueous solution was supplied at a constant rate of 100 ml / min, the same as in the nucleation process, to grow the nuclei (particles) generated in the nucleation process. The sodium tungstate aqueous solution was supplied at a constant rate of 10 ml / min simultaneously with the raw aqueous solution in the third and fourth stages.
[0139] In the first stage, while stirring with a stirrer, extremely fine nitrogen gas bubbles were circulated using a micro-nano bubble generator, and crystallization was continued for 35 minutes in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less from the start of the particle growth process.
[0140] In the second stage, while continuing to supply the raw material aqueous solution, a micro-nano bubble generator was used to circulate extremely fine air bubbles in the reaction tank, and the reaction atmosphere was adjusted to an oxidizing atmosphere with an oxygen concentration of 21% by volume (switching operation 1). After the start of switching operation 1, crystallization was carried out for 20 minutes while maintaining the oxidizing atmosphere and stirring with a stirrer.
[0141] In the third stage, while continuing to supply the raw material aqueous solution and supplying the sodium tungstate aqueous solution, a micro-nano bubble generator was used to circulate extremely fine nitrogen bubbles in the reaction tank, and the reaction atmosphere was adjusted to a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less (switching operation 2). After the start of switching operation 2, crystallization was carried out for 65 minutes while maintaining the non-oxidizing atmosphere and stirring with a stirrer.
[0142] In the fourth step, while continuing to supply the raw material aqueous solution and the sodium tungstate aqueous solution, a micro-nano bubble generator was used to circulate extremely fine air bubbles in the reaction tank, and the oxygen concentration was adjusted to an oxidizing atmosphere of 21% by volume (switching operation 3). After the start of switching operation 3, crystallization was carried out for 40 minutes while maintaining the oxidizing atmosphere and stirring with a stirrer.
[0143] In the fifth step, the supply of the aqueous sodium tungstate solution was stopped, while the supply of the raw aqueous solution was continued, and ultrafine nitrogen bubbles were circulated in the reaction tank using a micro-nano bubble generator, and the reaction atmosphere was adjusted to a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less (switching operation 4). After the start of switching operation 4, crystallization was carried out for 110 minutes while maintaining the non-oxidizing atmosphere and stirring with a stirrer.
[0144] Thereafter, the supply of all aqueous solutions including the raw material aqueous solution was stopped to terminate the particle growth process. The resulting product was washed with water, filtered and dried to obtain composite hydroxide particles.
[0145] In the particle growth step, a 25% by mass aqueous sodium hydroxide solution and a 25% by mass aqueous ammonia solution were appropriately supplied throughout the step to maintain the pH value and ammonium ion concentration of the aqueous solution for particle growth within the above-mentioned ranges.
[0146] b) Preparation of positive electrode active material The obtained composite hydroxide was thoroughly mixed with lithium hydroxide using a shaker mixer so that the Li / Me ratio was 1.10, to obtain a lithium mixture (mixing step).
[0147] This lithium mixture was heated to 965° C. at a heating rate of 1.3° C. / min in an oxygen atmosphere (oxygen concentration: 100% by volume), sintered by maintaining at this temperature for 3 hours, and then cooled to room temperature (sintering step).
[0148] In order to eliminate aggregation or slight sintering of the obtained lithium transition metal-containing composite oxide particles, this positive electrode active material was crushed (crushing step).
[0149] c) Evaluation of positive electrode active material [composition] The composition of this positive electrode active material was analyzed by an ICP emission spectrometer (Shimadzu Corporation, ICPE-9000).
[0150] [Particle size distribution] A laser light diffraction / scattering particle size analyzer (Microtrack MT3300EXII, manufactured by Microtrack-Bell Corporation) was used to measure the 50% cumulative diameter d50, 10% cumulative diameter d10, and 90% cumulative diameter d90 obtained from the particle size distribution measurements of the positive electrode active material (secondary particles).
[0151] [BET specific surface area] The BET specific surface area of the positive electrode active material (secondary particles) was determined using an independent 4-station specific surface area / pore distribution measuring device (QUADRASORB SI, manufactured by Quantachrome Instruments).
[0152] [Pore peak diameter and log differential pore volume at the pore peak diameter] The pore peak diameter of the positive electrode active material (secondary particles) and the log differential pore volume at the pore peak diameter were determined by mercury intrusion method using an automatic mercury polysimeter pore distribution measuring device (AutoPore IV9520, manufactured by Micromeritics).
[0153] [Particle structure] A part of the positive electrode active material was embedded in a resin, processed with a cross-section polisher (IB-19530CP, manufactured by JEOL Ltd.) to make it possible to observe the cross section, and then observed with a SEM (FE-SEM: JSM-6360LA, manufactured by JEOL Ltd.). As shown in Fig. 1, it was confirmed that the positive electrode active material of the present invention is formed of secondary particles formed by agglomeration of a plurality of primary particles, has about six communicating holes on the outer periphery of the secondary particle, has about eight spaces inside the secondary particle, and the communicating holes on the outer periphery are connected to the voids inside.
[0154] [Coefficient of variation] An ion milling device (Cryo-ion slicer, IB-09060CIS, manufactured by JEOL Ltd.) was used to process the cross section of the positive electrode active material (secondary particle) into a thin slice. Using a TEM (JEM-ARM200F, manufactured by JEOL Ltd.), a primary particle of about 0.5 μm (two connected particles sandwiching a grain boundary) was targeted in the cross section of the secondary particle, and a total of 10 points arbitrarily selected from the entire primary particle including the grain interior and grain boundary of each primary particle were irradiated with an electron beam. The energy of the generated W characteristic X-rays was analyzed using EDX (NSS, manufactured by Thermo Fisher Scientific Co., Ltd.), and the average W concentration (μ), standard deviation (σ) of the W concentration, and coefficient of variation (CV) of the W concentration in each entire primary particle were analyzed. Table 1 shows a graph of the measurement results of the W concentration by TEM-EDX analysis of the obtained primary particles.
[0155] As a result, the average concentration (μ) of W was 1.0, the standard deviation (σ) of the W concentration was 1.1, and the coefficient of variation (CV) of the W concentration was 1.1.
[0156] [Table 1] d) Preparation of secondary batteries A 2032-type coin battery 10 was produced as shown in Fig. 3. Specifically, 52.5 mg of the positive electrode active material obtained as described above, 15 mg of acetylene black, and 7.5 mg of PTFE were mixed and pressed at a pressure of 100 MPa to produce a positive electrode 1 with a diameter of 11 mm and a thickness of 100 µm.
[0157] Next, a 2032-type coin battery was produced using this positive electrode 1 in a glove box in an Ar atmosphere with a dew point controlled at -60°C. A lithium metal with a diameter of 14 mm and a thickness of 1 mm was used for the negative electrode 2 of the 2032-type coin battery, and an equal mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1M LiClO4 as a supporting electrolyte (manufactured by Ube Industries, Ltd.) was used for the non-aqueous electrolyte. In addition, a polyethylene porous film with a thickness of 25 μm was used for the separator 3. In this way, a 2032-type coin battery 10 was assembled, which has a gasket 4 and a wave washer 5, and is provided with a positive electrode can 6 and a negative electrode can 7.
[0158] e) Battery evaluation [Positive electrode resistance] The positive electrode resistance was measured using the impedance measurement method. A 2032 coin cell was charged at 3.8 V and measured by the AC impedance method using a frequency response analyzer and a potentiogalvanostat (Solartron, 1255B), obtaining the impedance spectrum shown in Figure 4. The impedance spectrum obtained showed two semicircles in the high frequency and intermediate frequency regions, and a straight line in the low frequency region, so the positive electrode interface resistance was analyzed using the equivalent circuit shown in Figure 5. Here, Rs is the bulk resistance, R1 is the positive electrode film resistance, and R ct indicates the electrolyte / positive electrode interface resistance, W indicates the Warburg component, and CPE1 and CPE2 indicate constant phase elements. The positive electrode interface resistance is based on the positive electrode active material of Comparative Example 1 described later, and the resistance reduction rate relative to this is shown.
[0159] The overall composition and characteristics of the obtained positive electrode active material, as well as the characteristics of the obtained lithium ion secondary battery, are shown in Table 2. Note that, regarding these, Table 1 also shows the same for Examples 2 to 5, Comparative Example 1, and Comparative Example 2.
[0160] Example 2 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the lithium mixture was heated to 915° C. and calcined by maintaining it at this temperature for 3 hours.
[0161] Example 3 A positive electrode active material was obtained and evaluated in the same manner as in Example 2, except that the sodium tungstate aqueous solution was prepared so that the molar ratio of each metal element was Ni:Mn:Co:W=5.0:2.0:3.0:0.07.
[0162] Example 4 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the lithium mixture was fired at 985°C.
[0163] Example 5 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the lithium mixture was fired at 885°C.
[0164] Comparative Example 1 In the crystallization step, the oxygen concentration was adjusted to 21% by volume in an oxidizing atmosphere up to the switching operation 1 of the nucleation step and the particle growth step, and the oxygen concentration was adjusted to 2% by volume or less in a non-oxidizing atmosphere thereafter to obtain a composite hydroxide. A positive electrode active material was obtained and evaluated in the same manner as in Example 1. Figure 2 shows the particle structure of the obtained positive electrode active material. It was confirmed that the positive electrode active material was formed of secondary particles formed by agglomeration of multiple primary particles, had one continuous hole on the outer periphery of the secondary particle, had one space inside the secondary particle, and had a hollow structure in which the continuous hole on the outer periphery was connected to the internal void.
[0165] Comparative Example 2 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the lithium mixture was baked at 815°C.
[0166] [Table 2] It was confirmed that, when any of the positive electrode active materials of Examples 1 to 5 within the scope of the present invention were used in a lithium ion secondary battery, the positive electrode resistance was reduced and the output characteristics were improved in comparison with Comparative Example 1 and Comparative Example 2. [Explanation of symbols]
[0167] 1 Positive electrode (electrode for evaluation) 2 negative electrode 3. Separator 4 Gasket 5 Wave Washer 6 Positive electrode can 7 Anode can 10 Coin cell battery
Claims
1. A method for producing a positive electrode active material for a lithium ion secondary battery, comprising: a crystallization step of preparing a transition metal-containing composite hydroxide; a mixing step of mixing the composite hydroxide or heat-treated particles of the composite hydroxide with a lithium compound to obtain a lithium mixture; and a firing step of firing the lithium mixture to obtain a positive electrode active material for a lithium ion secondary battery, The crystallization step comprises: a nucleation step in which water, sodium hydroxide and an aqueous ammonia solution are supplied into a reaction tank, and the pH value of the pre-reaction aqueous solution is adjusted to be 11 to 13 at a liquid temperature of 25° C. and the ammonium ion concentration is 9 g / L to 15 g / L, and a raw material aqueous solution containing at least a transition metal is supplied to the pre-reaction aqueous solution while blowing in a non-oxidizing atmosphere gas having an oxygen concentration of 2 vol % or less, thereby generating nuclei; a particle growth step in which, after completion of nucleation, a pH value is adjusted to 10 or more and 12 or less at a liquid temperature of 25° C. and to a value lower than the pH value in the nucleation step, thereby forming an aqueous solution for particle growth, and the raw material aqueous solution is supplied to the aqueous solution for particle growth, thereby growing the nuclei generated in the nucleation step into particles; Equipped with The particle growth step includes: A first stage in which crystallization is continued for a certain period of time in a non-oxidizing atmosphere having an oxygen concentration of 2% by volume or less from the start of the particle growth step while stirring with a stirrer; A switching operation 1 is performed in which, while continuing the supply of the raw material aqueous solution, extremely fine bubbles of an oxidizing atmosphere gas consisting of air or oxygen are circulated in the reaction tank using a micro / nano bubble generator to adjust the reaction atmosphere to an oxidizing atmosphere having an oxygen concentration of 21% by volume or more, and after the start of the switching operation 1, crystallization is performed while maintaining the oxidizing atmosphere and stirring with a stirrer for a certain period of time; and A switching operation 2 is performed in which, while continuing the supply of the raw material aqueous solution, extremely fine bubbles of a gas of a non-oxidizing atmosphere are circulated in the reaction tank using a micro-nano bubble generator to adjust the reaction atmosphere to a non-oxidizing atmosphere having an oxygen concentration of 2% by volume or less, and after the start of the switching operation 2, crystallization is performed while maintaining the non-oxidizing atmosphere and stirring with a stirrer for a certain period of time; and A fourth step is to carry out a switching operation 3 in which, while continuing the supply of the raw material aqueous solution, a micro-nano bubble generator is used to circulate extremely fine bubbles of an oxidizing atmosphere gas in the reaction tank to adjust the reaction atmosphere to an oxidizing atmosphere having an oxygen concentration of 21% by volume or more, and after the start of the switching operation 3, crystallization is carried out while maintaining the oxidizing atmosphere and stirring with a stirrer for a certain period of time; A fifth step is to carry out a switching operation 4 in which, while continuing the supply of the raw material aqueous solution, a micro-nano bubble generator is used to circulate extremely fine bubbles of a gas of a non-oxidizing atmosphere in the reaction tank, thereby adjusting the reaction atmosphere to a non-oxidizing atmosphere having an oxygen concentration of 2% by volume or less, and after the start of the switching operation 4, crystallization is carried out while stirring with a stirrer for a certain period of time while maintaining the non-oxidizing atmosphere; and In the calcination step, the lithium mixture is calcined at a calcination temperature of 720° C. or more and 980° C. or less for at least 2 hours. A method for producing a positive electrode active material for a lithium ion secondary battery, comprising:
2. A method for producing a positive electrode active material for a lithium ion secondary battery as described in claim 1, wherein the time for each stage in the particle growth process is set so that stage 2 ≦ stage 4 < stage 1 ≦ stage 3 ≦ stage 5, and the crystallization time for the entire particle growth process is within 8 hours.
3. A method for producing a positive electrode active material for a lithium ion secondary battery as described in claim 1, further comprising a pre-firing step of pre-firing the lithium mixture at a temperature lower than the firing temperature and not lower than 350°C and not higher than 800°C prior to the firing step.
4. A lithium transition metal-containing composite oxide particle having a composition represented by general formula (A): Li1+uNixMnyCozMtO2 (wherein, -0.05≦u≦0.5, x+y+z+t=1, 0.3≦x≦0.9, 0≦y≦0.5, 0≦z≦0.5, 0<t≦0.1, and M is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W), and a crystal structure of a layered rock salt type structure, The lithium transition metal-containing composite oxide particles are composed of secondary particles formed by agglomeration of primary particles, The secondary particles are 50% cumulative diameter d50 obtained from particle size distribution measurements of 3.0 μm or more and 7.0 μm or less; a BET specific surface area of 1.8 m 2 / g or more and 5.5 m 2 / g or less; A pore peak diameter of 0.01 μm or more and 0.30 μm or less in a pore portion obtained by mercury intrusion porosimetry, and A log differential pore volume [dV / d (log D)] of 0.2 ml / g or more and 0.6 ml / g or less in the pore peak diameter range of 0.01 μm or more and 0.30 μm or less, and among the primary particles, a plurality of primary particles having a primary particle diameter in the range of 0.1 μm or more and 1.0 μm or less are subjected to cross-sectional STEM or TEM-EDX analysis to measure the concentration of the additive element M at a plurality of locations, and a coefficient of variation of the concentration of the additive element M, which is a value obtained by dividing the standard deviation of the concentration of the additive element M by the average concentration of the additive element M, is calculated, and the coefficient of variation is 1.5 or less. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 , which produces a positive electrode active material for a lithium ion secondary battery.
5. A method for producing a positive electrode active material for a lithium ion secondary battery as described in claim 4, wherein the secondary particles have an agglomeration portion, one or more communicating holes connecting the outer periphery of the agglomeration portion, and two or more spatial portions present inside the agglomeration portion and connecting with the communicating holes.