Resin composition and syringe filled with resin composition

JP2024069215A5Active Publication Date: 2024-11-29AJINOMOTO CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024020521
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-02-14
Publication Date
2024-11-29
Estimated Expiration
2041-01-19

AI Technical Summary

Technical Problem

Existing resin compositions used in semiconductor chip packages face challenges with dispensability, discharge workability, and resin flowability, leading to issues such as resin leakage and poor mold filling during compression molding.

Method used

A resin composition and syringe system are developed, where the syringe is filled with a resin that satisfies specific conditions regarding shape change over time, viscosity, and composition, ensuring good dispensability, discharge workability, and resin flowability, as defined by formulas (1) and (2).

Benefits of technology

The solution provides a resin composition with improved dispensability, discharge workability, and resin flowability, reducing resin leakage and ensuring accurate resin supply, thereby enhancing the compression moldability of semiconductor chip packages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a syringe filled with a resin composition which has good dispensing property, discharge workability and resin flowability.SOLUTION: A syringe filled with a resin composition includes a syringe and a resin composition made to fill the syringe, wherein the resin composition forms a resin dome of the resin composition by being dispensed onto a horizontally installed silicon wafer surface, when a height between a contact surface with a silicon wafer of the resin dome and a resin dome apex after 60 seconds from a dispensing completion time point is represented by H1, and a height between the contact surface with the silicon wafer of the resin dome and the resin dome apex after 180 seconds from the dispensing completion time point is represented by H2 in evaluation test of the resin composition for measuring a shape change of the resin dome, the condition of the following expression (1): 0.15<H2 / H1<0.90 is satisfied.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a syringe filled with the resin composition, and the like. [Background technology]

[0002] In recent years, the demand for small, highly functional electronic devices such as smartphones and tablet devices has been increasing. These small electronic devices usually use encapsulation materials for semiconductor chip packages. As such encapsulation materials, those formed by curing resin compositions are known (Patent Documents 1 to 3).

[0003] Known methods for molding the sealing material include melt casting, transfer molding, injection molding, and compression molding. In the compression molding method, for example, a resin composition is dispensed onto a substrate using a syringe, the mold is clamped, and pressure and, if necessary, heat are applied to the resin composition to perform compression molding. When dispensing a resin composition using a syringe, good dispensability and discharge workability are required from the viewpoint of improving workability. In addition, good resin flowability is required to prevent resin leakage from the mold during compression molding. However, at present, these problems have not yet been sufficiently solved by simply adjusting the thixotropy and viscosity of the resin composition.

[0004] Incidentally, a syringe filled with a resin composition that contains voids that can suppress air contamination that causes intermittent discharge has been known (Patent Document 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-137370 A [Patent Document 2] JP 2012-188555 A [Patent Document 3] JP 2016-74920 A [Patent Document 4] JP 2020-127919 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a resin composition and a syringe filled with the resin composition, which have good dispensability, ejection operability, and resin flowability. [Means for solving the problem]

[0007] In order to achieve the objects of the present invention, the inventors conducted extensive research and unexpectedly discovered that when a resin composition is dispensed onto a silicon wafer surface to form a resin dome of the resin composition, and the change in shape of the resin dome over time satisfies certain conditions, the dispenseability, ejection operability and resin flowability are excellent, which led to the completion of the present invention.

[0008] That is, the present invention includes the following. [1] A resin composition-filled syringe comprising a syringe and a resin composition filled in the syringe, The resin composition comprises: In a resin composition evaluation test, a resin composition is dispensed onto a horizontally placed silicon wafer surface to form a resin dome of the resin composition, and a change in the shape of the resin dome is measured. The height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 60 seconds after dispensing is completed is H1. If the height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 180 seconds after dispensing is H2, A syringe filled with a resin composition, which satisfies the condition of the following formula (1): 0.15 <H2 / H1<0.90 ···(1) [2] The evaluation test is The syringe filled with the resin composition according to the above-mentioned [1] includes dispensing 40 g±1.5 g of the resin composition at 23°C onto the surface of the silicon wafer at a rate of 2 g / sec under a condition of 23°C from a discharge port installed at a position 5 cm high from the surface of the silicon wafer, and stopping the dispensing to form a resin dome of the resin composition. [3] In the evaluation test, If the discharge port and the resin dome are not in contact when the dispensing of the resin composition is stopped, the time when 40 g±1.5 g of the resin composition has been dispensed is regarded as the dispensing completion time. The syringe filled with the resin composition described in [2] above, in which if the outlet and the resin dome are in contact when the dispensing of the resin composition is stopped, the outlet is pulled up after the dispensing is stopped to separate the outlet from the resin dome, and the point at which the outlet separates from the resin dome is regarded as the point at which the dispensing is completed. [4] The diameter of the contact surface of the resin dome with the silicon wafer 60 seconds after dispensing is completed is L1. The syringe filled with the resin composition according to any one of the above [1] to [3], further satisfying the condition of the following formula (2), where L2 is the diameter of the contact surface of the resin dome with the silicon wafer 180 seconds after the completion of dispensing. 0.40 <L1 / L2<0.96 ···(2) [5] The syringe filled with a resin composition according to any one of the above [1] to [4], wherein the viscosity of the resin composition at 25°C is 100 Pa·s or more and 500 Pa·s or less. [6] The syringe filled with the resin composition according to any one of the above [1] to [5], wherein the resin composition contains (A) a thermosetting resin. [7] The syringe filled with the resin composition according to any one of the above [1] to [6], wherein the resin composition contains (B) an inorganic filler. [8] The syringe filled with the resin composition according to any one of the above [1] to [7], wherein the resin composition contains (C) a silane coupling agent. [9] In an evaluation test of a resin composition, a resin dome of the resin composition is formed by dispensing the resin composition on the surface of a horizontally placed silicon wafer, and the change in the shape of the resin dome is measured. The height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 60 seconds after dispensing is completed is H1. If the height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 180 seconds after dispensing is H2, A resin composition that satisfies the condition of the following formula (1). 0.15 <H2 / H1<0.90 ···(1)

[10] The evaluation test The resin composition according to the above-mentioned [9], comprising dispensing 40 g±1.5 g of the resin composition at 23°C onto the surface of the silicon wafer at a rate of 2 g / sec under a condition of 23°C from a discharge port installed at a position 5 cm high from the surface of the silicon wafer, and stopping the dispensing to form a resin dome of the resin composition.

[11] In the evaluation test, If the discharge port and the resin dome are not in contact when the dispensing of the resin composition is stopped, the time when 40 g±1.5 g of the resin composition has been dispensed is regarded as the dispensing completion time. The resin composition according to

[10] above, wherein if the discharge port and the resin dome are in contact when dispensing of the resin composition is stopped, the discharge port is pulled up after dispensing is stopped to separate the discharge port from the resin dome, and the point at which the discharge port separates from the resin dome is regarded as the point at which the dispensing is completed.

[12] The diameter of the contact surface of the resin dome with the silicon wafer 60 seconds after dispensing is completed is L1. If the diameter of the contact surface of the resin dome with the silicon wafer 180 seconds after dispensing is L2, The resin composition according to any one of the above [9] to

[11] , further satisfying the condition of the following formula (2): 0.40 <L1 / L2<0.96 ···(2)

[13] The resin composition according to any one of the above [9] to

[12] , wherein the viscosity of the resin composition at 25°C is 100 Pa·s or more and 500 Pa·s or less.

[14] The resin composition according to any one of the above [9] to

[13] , comprising (A) a thermosetting resin.

[15] The resin composition according to any one of the above [9] to

[14] , further comprising (B) an inorganic filler.

[16] The resin composition according to any one of the above [9] to

[15] , further comprising a silane coupling agent (C).

[17] The resin composition according to any one of the above [9] to

[16] for forming an insulating layer of a semiconductor chip package.

[18] The resin composition according to any one of the above [9] to

[16] for forming an insulating layer of a circuit board.

[19] The resin composition according to any one of the above [9] to

[16] for encapsulating a semiconductor chip in a semiconductor chip package.

[20] A cured product of the resin composition according to any one of [9] to

[19] above.

[21] A circuit board comprising an insulating layer formed from a cured product of the resin composition according to any one of the above [9] to

[19] .

[22] A semiconductor chip package comprising the circuit board according to

[21] above and a semiconductor chip mounted on the circuit board.

[23] A semiconductor chip package comprising: a semiconductor chip; and a cured product of the resin composition according to any one of [9] to

[19] above that encapsulates the semiconductor chip.

[24] A semiconductor device comprising the semiconductor chip package according to

[22] or

[23] above.

[25] A method for evaluating a resin composition, comprising dispensing a resin composition on a surface of a horizontally placed silicon wafer to form a resin dome of the resin composition, and measuring a change in shape of the resin dome, comprising: The height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 60 seconds after dispensing is completed is H1. If the height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 180 seconds after dispensing is H2, A method for evaluating a resin composition, comprising determining whether or not the condition of the following formula (1) is satisfied: 0.15 <H2 / H1<0.90 ···(1) Effect of the Invention

[0009] According to the resin composition of the present invention, it is possible to provide a resin composition and a syringe filled with the resin composition, which have good dispensability, ejection operability, and resin flowability. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a syringe filled with a resin composition according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a side view that illustrates an example of a nozzle that is attached to a syringe filled with a resin composition according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a horizontal cross-sectional view showing a resin dome formed on a silicon wafer at the completion of dispensing in an evaluation test of one embodiment, together with a part of a syringe filled with the resin composition. [Figure 4] FIG. 4 is a plan view seen from the vertical direction, which illustrates a resin dome formed on a silicon wafer at the time of completion of dispensing in an evaluation test of one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0012] <Syringe filled with resin composition> The syringe filled with a resin composition of the present invention comprises a syringe and a resin composition filled in the syringe.

[0013] The configuration of the syringe filled with the resin composition of the present invention and the nozzle attached thereto will be described using an example. Fig. 1 is a cross-sectional view that shows an example of a syringe filled with the resin composition according to one embodiment of the present invention. Fig. 2 is a side view that shows an example of a nozzle attached to the syringe filled with the resin composition according to one embodiment of the present invention.

[0014] As shown in Fig. 1, a syringe 10 filled with a resin composition includes a syringe 11 and a resin composition 12 filled in the syringe 11, and a plunger 13 for pushing out the resin composition 12 is provided in the syringe 11. The syringe 10 filled with the resin composition also includes a female thread portion 14 formed of a thread for mounting a nozzle 20 on the inner surface of one end of the syringe 11 on the reduced diameter side, a discharge port 15 for discharging the resin composition at the tip of the one end, and an opening 16 into which a plunger rod is inserted at the other end opposite to the discharge port 15. The discharge port 15 has a tip cap 17 that closes the discharge port 15 and is removed when used, and the opening 16 has an end cap 18 that closes the opening 16 and is removed when used.

[0015] In one embodiment, the syringe 11 may be any syringe that can be used as a dispensing syringe for a sealing material that can be filled with the resin composition of the present invention, and it is particularly preferable to use a product standard "12 Oz syringe". An example of a commercially available "12 Oz syringe" is "5194C" manufactured by Sanei Tech Co., Ltd. The "12 Oz syringe" may have an inner diameter of the discharge port 15 of 14.22 mm, an outer diameter of 19.30 mm, an inner diameter of the opening 16 of 40.26 mm, and a length from the discharge port 15 to the opening 16 of the syringe 11 of 311.40 mm.

[0016] The syringe 10 filled with the resin composition may be used with a nozzle 20 attached. When the nozzle 20 is attached to the syringe 10 filled with the resin composition, the tip cap 17 is removed. As shown in FIG. 2, the nozzle 20 is composed of a tube portion 21 and a syringe connecting portion 22, and a part of the tube portion 21 is inserted and fixed into the syringe connecting portion 22. The tip of the nozzle 20 on the tube portion 21 side has a nozzle discharge portion 23 for discharging the resin composition, and the other end on the syringe connecting portion 22 side has a nozzle opening 24 for feeding the resin composition 12 from the inside of the syringe 11 when the nozzle 20 is fixed to the syringe 10 filled with the resin composition, and the nozzle 20 is generally tubular. The outer surface of the other end on the syringe connecting portion 22 side has a male thread portion 25 consisting of a thread that meshes with the female thread portion 14 for attaching and fixing the nozzle 20 to the syringe 10 filled with the resin composition. The tube portion 21 is formed of a soft material and has a structure in which dispensing can be stopped by pushing it with an external pressure to block the resin composition.

[0017] <Resin composition and its evaluation test (evaluation method)> The resin composition used in the present invention satisfies the condition of formula (1) (preferably also satisfies the condition of formula (2)) described below in the results of evaluation tests of the resin composition described below.

[0018] The evaluation tests (evaluation methods) for the resin compositions will be described below.

[0019] In the evaluation test for evaluating the resin composition, the resin composition is dispensed onto the surface of a horizontally placed silicon wafer to form a resin dome of the resin composition, and the change in shape of the resin dome is measured to determine whether or not the condition of formula (1) described below (preferably also the condition of formula (2)) is satisfied.

[0020] In the evaluation test, a syringe may be used, and the resin composition may be dispensed from the outlet of the syringe. The syringe used in the evaluation test may be, for example, a syringe 10 filled with the resin composition as shown in FIG. 1. When dispensing, the tip cap 17 and the end cap 18 of the syringe are removed. In addition, when dispensing to measure the specific conditions described below regarding the shape of the resin dome, the nozzle 20 may or may not be attached. In the evaluation test, a normal dispenser is used when dispensing. An example of a commercially available dispenser used in the evaluation test is the "Liquid Manual Dispenser" manufactured by Apic Yamada Co., Ltd.

[0021] The silicon wafer used in the evaluation test may have an arithmetic mean roughness (Ra) of 10 Å or less, and the size is not particularly limited as long as the evaluation test can be performed.

[0022] The formation of a resin dome by dispensing in an evaluation test of one embodiment will be described with reference to schematic diagrams. Fig. 3 is a horizontal cross-sectional view showing a resin dome formed on a silicon wafer at the time of completion of dispensing in an evaluation test of one embodiment together with a part of a syringe filled with a resin composition. Fig. 4 is a vertical plan view showing a resin dome formed on a silicon wafer at the time of completion of dispensing in an evaluation test of one embodiment.

[0023] In this embodiment, a syringe without a nozzle attached is used in the evaluation test. In this embodiment, a case where the nozzle 20 is not attached will be described as in the following Test Example 3. First, as shown in FIG. 3, the height H from the surface of a horizontally placed silicon wafer 40 to the discharge port 15 was measured. s The syringe 10 filled with the resin composition is placed with the tip cap 17 and the end cap 18 removed so that the length is 5 cm.

[0024] Next, in this embodiment, 40 g±1.5 g of the resin composition at 23° C., the same as the outside air, is dispensed onto the silicon wafer surface from the outlet 15 of the resin composition-filled syringe 10 at a rate of 2 g / sec under 23° C. conditions, and dispensing is stopped when 40 g±1.5 g has been dispensed, forming a resin dome 20 of the resin composition. Stopping dispensing means stopping the supply of the resin composition onto the silicon wafer surface by stopping the plunger, blocking the outlet (nozzle outlet), or blocking the tube part of the nozzle when a nozzle is used. In this embodiment, dispensing is stopped when 40 g±1.5 g of the resin composition has been dispensed, so that the amount of resin composition in the resin dome 20 is 40 g±1.5 g.

[0025] In addition, in this embodiment, if the discharge port and the resin dome are in contact at the time when dispensing of the resin composition is stopped, the discharge port is pulled up after dispensing is stopped to separate the discharge port from the resin dome.

[0026] In addition, in this embodiment, if the discharge port and the resin dome are not in contact when the dispensing of the resin composition is stopped, the dispensing completion time is the time when 40 g±1.5 g of the resin composition has been dispensed, and if the discharge port and the resin dome are in contact when the dispensing of the resin composition is stopped, the discharge port is pulled up after dispensing is stopped, and the dispensing completion time is the time when the discharge port separates from the resin dome.

[0027] The resin dome 30 of the resin composition is a dome-shaped mass of liquid resin composition as shown in FIG. 3. Since the resin composition usually spreads in a circular shape from the point where the resin composition falls, the contact surface with the silicon wafer 40 can be circular as shown in FIG. 4.

[0028] The resin dome 30 of the resin composition usually spreads circularly around the dropping point of the resin composition over time after dispensing. Therefore, the height H0 from the contact surface of the resin dome 30 with the silicon wafer 40 to the resin dome apex decreases over time. Accordingly, the resin composition in the present invention satisfies the following formula (1) as a predetermined first condition indicating the change over time in the shape of the resin dome 30, where the height (the distance in the direction perpendicular to the surface of the silicon wafer 40) from the contact surface of the resin dome 30 with the silicon wafer 40 to the resin dome apex 60 seconds after the completion of dispensing is H1, and the height (the distance in the direction perpendicular to the surface of the silicon wafer 40) from the contact surface of the resin dome 20 with the silicon wafer 30 to the resin dome apex 180 seconds after the completion of dispensing is H2. 0.15 < H2 / H1 < 0.90 ···(1)

[0029] Under the condition of the above formula (1), H2 / H1 satisfies 0.15 < H2 / H1, preferably 0.20 < H2 / H1, more preferably 0.25 < H2 / H1, still more preferably 0.30 < H2 / H1, and particularly preferably 0.33 < H2 / H1. On the other hand, H2 / H1 satisfies H2 / H1 < 0.90, preferably H2 / H1 < 0.85, and particularly preferably H2 / H1 < 0.82.

[0030] By satisfying the condition of the above formula (1), the resin composition in the present invention may have the characteristic of good dispensability in one embodiment. Since the dispensability is good, it can be smoothly discharged from the discharge port 15 (nozzle discharge portion 23) in the syringe 10 filled with the resin composition, and the backflow phenomenon is less likely to occur, so the workability can be good.

[0031] Further, by satisfying the conditions of the above formula (1), the resin composition in the present invention can have a characteristic that the ejection workability is good in one embodiment. Since the ejection workability is good, the dripping property is good, it is difficult for liquid separation and resin sagging to occur, and the resin composition can be dispensed with an accurate resin supply amount. The dripping property refers to the property that the ejection of the resin composition from the nozzle ejection part 23 stops promptly when the dispensing is stopped. Further, the liquid separation refers to the property that the resin composition discharged from the nozzle ejection part 23 easily separates without adhering to the discharge port 15.

[0032] Further, by satisfying the conditions of the above formula (1), the resin composition in the present invention can have a characteristic that the resin flowability is good in one embodiment. Since the resin flowability is good, it is difficult for unfilled portions to occur in the mold, and since it is difficult for resin leakage from the mold during compression molding to occur, the compression moldability can be excellent.

[0033] Further, the diameter L0 of the contact surface of the resin dome 30 with the silicon wafer 40 increases with time after dispensing. Thereby, as a predetermined second condition indicating the change over time of the shape of the resin dome 30, the resin composition in the present invention, when the diameter of the contact surface of the resin dome 30 with the silicon wafer 40 60 seconds after the completion of dispensing is L1 and the diameter of the contact surface of the resin dome 30 with the silicon wafer 40 180 seconds after the completion of dispensing is L2, preferably further satisfies the conditions of the following formula (2). 0.40 < L1 / L2 < 0.96 ···(2)

[0034] In the conditions of the above formula (2), L1 / L2 satisfies 0.40 < L1 / L2, preferably 0.45 < L1 / L2, particularly preferably 0.48 < L1 / L2. On the other hand, L1 / L2 satisfies L1 / L2 < 0.96, preferably L1 / L2 < 0.94, more preferably L1 / L2 < 0.92, particularly preferably L1 / L2 < 0.90.

[0035] In one embodiment, the resin composition of the present invention satisfies the condition of the above formula (2), and thereby the dispensability, discharge workability, and resin flowability of the resin composition can be further improved.

[0036] From the time dispensing was completed until 180 seconds later, the temperature was kept at 23°C, the same as during dispensing.

[0037] From the viewpoints of further improving the resin flowability and further preventing resin leakage from the mold during compression molding, the viscosity of the resin composition of the present invention at 25°C is usually 1 Pa·s or more, preferably 2.5 Pa·s or more, 10 Pa·s or more, more preferably 30 Pa·s or more, 50 Pa·s or more, even more preferably 80 Pa·s or more, 90 Pa·s or more, still more preferably 100 Pa·s or more, 110 Pa·s or more, and particularly preferably 120 Pa·s or more, 130 Pa·s or more. From the viewpoint of further improving the dispensability and further preventing the backflow phenomenon, the upper limit of the viscosity of the resin composition at 25°C is usually 2000 Pa·s or less, preferably 1000 Pa·s or less, 900 Pa·s or less, preferably 800 Pa·s or less, 700 Pa·s or less, preferably 650 Pa·s or less, 600 Pa·s or less, preferably 500 Pa·s or less, 450 Pa·s or less, particularly preferably 400 Pa·s or less, 380 Pa·s or less. The above viscosity can be measured using an E-type viscometer.

[0038] In the present invention, the resin composition may contain components selected from (A) a thermosetting resin, (B) an inorganic filler, (C) a radical polymerizable compound, (D) a radical polymerization initiator, (E) a thermoplastic resin, (F) a curing accelerator, (G) a polyether skeleton-containing compound, (H) other additives, and (I) an organic solvent. Those skilled in the art can adjust the resin composition to satisfy the conditions of the above formulas (1) and (2) by changing the selection and content of these components. Each component contained in the resin composition will be described in detail below.

[0039] <(A) Thermosetting resin> In the present invention, the resin composition may contain (A) a thermosetting resin. As the thermosetting resin, a thermosetting resin that can be used as a sealing material for electronic devices can be used. As the (A) thermosetting resin, for example, an epoxy resin, an epoxy acrylate resin, a urethane acrylate resin, a urethane resin, a cyanate resin, a benzoxazine resin, an unsaturated polyester resin, a phenolic resin, a melamine resin, a silicone resin, etc. can be mentioned.

[0040] <(A-1) Epoxy resin> In the present invention, the resin composition may contain (A-1) an epoxy resin as (A) a thermosetting resin. (A-1) An epoxy resin refers to a resin having an epoxy group.

[0041] (A-1) Epoxy resins include, for example, bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, etc. Epoxy resins may be used alone or in combination of two or more types.

[0042] In the present invention, the resin composition preferably contains, as the epoxy resin (A-1), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on 100% by mass of the non-volatile components of the epoxy resin (A-1).

[0043] The (A-1) epoxy resin includes an epoxy resin that is liquid at a temperature of 25° C. (hereinafter sometimes referred to as a "liquid epoxy resin") and an epoxy resin that is solid at a temperature of 25° C. (hereinafter sometimes referred to as a "solid epoxy resin"). In the present invention, the resin composition may contain, as the (A-1) epoxy resin, only a solid epoxy resin, only a liquid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin, but it is more preferable that the resin composition contains a liquid epoxy resin, and it is particularly preferable that the (A-1) epoxy resin contains only a liquid epoxy resin.

[0044] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0045] As the liquid epoxy resin, glycirol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane dimethanol type epoxy resin, cyclic aliphatic glycidyl ether, and epoxy resin having a butadiene structure are preferred, and glycirol type epoxy resin, cyclic aliphatic glycidyl ether, bisphenol A type epoxy resin, and bisphenol F type epoxy resin are more preferred.

[0046] Specific examples of liquid epoxy resins include "EX-992L" manufactured by Nagase ChemteX Corporation, "YX7400" manufactured by Mitsubishi Chemical Corporation, "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" manufactured by Mitsubishi Chemical Corporation. " (bisphenol F type epoxy resin); "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", "604" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L", "EP-3980S" (glycidylamine type epoxy resin) manufactured by ADEKA Corporation; "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA Corporation; "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation; "EX-991L" (alkyleneoxy skeleton-containing epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin with ester skeleton) manufactured by Daicel Corporation; Examples of such epoxy resins include "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (epoxy resins having a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resins) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EG-280" (fluorene structure-containing epoxy resin) manufactured by Osaka Gas Chemicals Co., Ltd.; and "EX-201" (cyclic aliphatic glycidyl ether) manufactured by Nagase ChemteX Corporation.

[0047] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0048] Preferred solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, and phenolphthalein type epoxy resins.

[0049] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; and "EXA-73" manufactured by DIC Corporation. 11", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN475V" manufactured by Nippon Steel Chemical & Material Co., Ltd. (Naphthalene type epoxy resin); "ESN485" (Naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (Dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (Bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (Biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (Anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX77" manufactured by Mitsubishi Chemical Co., Ltd. Examples of epoxy resins include "PG-100" (phenol aralkyl type epoxy resin), "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals, "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical, "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical, "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical, "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical, and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. These may be used alone or in combination of two or more types.

[0050] The epoxy equivalent of the (A-1) epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0051] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin (A-1) is preferably 100 to 5000, more preferably 250 to 3000, and further preferably 400 to 1500. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0052] The content of the (A-1) epoxy resin in the resin composition is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.01 mass% or more, preferably 0.1 mass% or more, more preferably 1 mass% or more, and particularly preferably 3 mass% or more, and preferably 30 mass% or less, more preferably 20 mass% or less, and particularly preferably 15 mass% or less; and when the total nonvolatile components other than the (B) inorganic filler in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 1 mass% or more, preferably 10 mass% or more, more preferably 20 mass% or more, and particularly preferably 30 mass% or more, and preferably 90 mass% or less, more preferably 85 mass% or less, and particularly preferably 80 mass% or less.

[0053] <(A-2) Epoxy hardener> In the present invention, when the resin composition contains an epoxy resin (A-1) as the thermosetting resin (A), it may further contain an epoxy curing agent (A-2) as an optional component. The epoxy curing agent (A-2) functions as an epoxy resin curing agent that reacts with the epoxy resin (A-1) to cure the resin composition.

[0054] The (A-2) epoxy curing agent is not particularly limited, but examples thereof include active ester curing agents, phenolic curing agents, carbodiimide curing agents, acid anhydride curing agents, amine curing agents, benzoxazine curing agents, cyanate ester curing agents, and thiol curing agents. The (A-2) epoxy curing agent may be used alone or in combination of two or more. The (A-2) epoxy curing agent preferably contains an epoxy curing agent selected from active ester curing agents and phenolic curing agents.

[0055] As the active ester curing agent, generally, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferably used.

[0056] The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. From the viewpoint of improving heat resistance in particular, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred.

[0057] Examples of active ester-based curing agents include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, and phenol novolak. Here, the term "dicyclopentadiene type diphenol compound" refers to a diphenol compound obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0058] Specifically, the active ester curing agent is preferably a dicyclopentadiene type active ester curing agent, a naphthalene type active ester curing agent containing a naphthalene structure, an active ester curing agent containing an acetylated product of phenol novolac, or an active ester curing agent containing a benzoylated product of phenol novolac, and among these, at least one selected from a dicyclopentadiene type active ester curing agent and a naphthalene type active ester curing agent is more preferable. As the dicyclopentadiene type active ester curing agent, an active ester curing agent containing a dicyclopentadiene type diphenol structure is preferable.

[0059] Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation) as active ester curing agents containing a dicyclopentadiene-type diphenol structure; and "EXB-8151-62T", "EXB-8100L-65T", "EXB-815060T", and "EXB-81 Examples of such curing agents include "EXB-9416-70BK", "HPC-8150-60T", and "HPC-8150-62T" (manufactured by DIC Corporation); "EXB9401" (manufactured by DIC Corporation) as a phosphorus-containing active ester curing agent; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester curing agent which is an acetylated product of phenol novolac; "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester curing agents which are benzoylated products of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Corporation) as an active ester curing agent containing a styryl group and a naphthalene structure.

[0060] Examples of phenol-based curing agents include curing agents having one or more, preferably two or more, hydroxyl groups bonded to an aromatic ring such as a benzene ring or a naphthalene ring in one molecule. Among them, compounds having a hydroxyl group bonded to a benzene ring are preferred.

[0061] Specific examples of phenol-based curing agents include "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Kasei Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", and "KA-1165" manufactured by DIC Corporation; "GDP-6115L", "GDP-6115H", and "ELPC75" manufactured by Gun-ei Chemical Co., Ltd.; and "2,2-diallyl bisphenol A" manufactured by Sigma-Aldrich Corporation.

[0062] Examples of the carbodiimide-based curing agent include curing agents having one or more, preferably two or more, carbodiimide structures in one molecule, such as aliphatic biscarbodiimides, such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides, such as phenylene-bis(xylylcarbodiimide); and aliphatic polycarbodiimides, such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide). ; polycarbodiimides such as aromatic polycarbodiimides such as poly(phenylenecarbodiimide), poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide].

[0063] Commercially available carbodiimide curing agents include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0064] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule, and a curing agent having two or more acid anhydride groups in one molecule is preferable. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and the like. Examples of acid anhydrides include polymeric acid anhydrides such as biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and styrene-maleic acid resins, which are copolymers of styrene and maleic acid. Commercially available acid anhydride hardeners include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" from New Japan Chemical Co., Ltd., "YH-306" and "YH-307" from Mitsubishi Chemical Co., Ltd., and "HN-2200" and "HN-5500" from Hitachi Chemical Co., Ltd.

[0065] The amine-based curing agent may be a curing agent having one or more, preferably two or more, amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc., and among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or secondary amine, and more preferably a primary amine. Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxyphenyl)propane. propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. As the amine-based curing agent, commercially available products may be used, and examples thereof include "SEIKACURE-S" manufactured by Seika Corporation, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.

[0066] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0067] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0068] Examples of thiol-based curing agents include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.

[0069] The reactive group equivalent of the epoxy curing agent (A-2) is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent is the mass of the curing agent per equivalent of reactive group.

[0070] The content of the (A-2) epoxy curing agent in the resin composition is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.01 mass% or more, preferably 0.1 mass% or more, more preferably 1 mass% or more, particularly preferably 2 mass% or more, and preferably 20 mass% or less, more preferably 10 mass% or less, and particularly preferably 7 mass% or less; and when the total nonvolatile components other than the (B) inorganic filler in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.1 mass% or more, preferably 1 mass% or more, more preferably 5 mass% or more, particularly preferably 10 mass% or more, and preferably 80 mass% or less, more preferably 70 mass% or less, and particularly preferably 60 mass% or less.

[0071] <(B) Inorganic filler> In the present invention, the resin composition may contain (B) an inorganic filler as an optional component.

[0072] (B) An inorganic compound is used as the material of the inorganic filler. Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Moreover, as the silica, spherical silica is preferable. (B) The inorganic filler may be used alone or in combination of two or more types.

[0073] The 50% cumulative diameter D50 of the (B) inorganic filler is preferably 0.2 μm or more, more preferably 0.3 μm or more, particularly preferably 0.4 μm or more, and is preferably 15 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. If the 50% cumulative diameter D50 of the (B) inorganic filler is too small, the dispensability decreases and the backflow phenomenon may easily occur.

[0074] The 90% cumulative diameter D90 of the (B) inorganic filler is preferably 2 μm or more, more preferably 3 μm or more, particularly preferably 3.5 μm or more, and is preferably 30 μm or less, more preferably 27 μm or less, and even more preferably 25 μm or less. Such a small 90% cumulative diameter D90 indicates that the (C) inorganic filler does not contain large particles. If the (B) inorganic filler has a too small 90% cumulative diameter D90, the dispensability decreases and the backflow phenomenon may easily occur.

[0075] (B) The ratio D50 / D90 of the 50% cumulative diameter D50 to the 90% cumulative diameter D90 of the inorganic filler is preferably 0.2 or more, more preferably 0.3 or more, particularly preferably 0.35 or more, and is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.65 or less.

[0076] (B) The difference between the 50% cumulative diameter D50 and the 90% cumulative diameter D90 of the inorganic filler (D90-D50) is preferably 2 μm or more, more preferably 2.5 μm or more, particularly preferably 3 μm or more, and is preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 16 μm or less.

[0077] The 50% cumulative diameter D50 and 90% cumulative diameter D90 of the (B) inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of the (B) inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device. The particle size (i.e., median diameter) at which the cumulative frequency from the small diameter side is 50% can be taken as the 50% cumulative diameter D50. The particle size at which the cumulative frequency from the small diameter side is 90% can be taken as the 90% cumulative diameter D90. The measurement sample can be prepared by weighing 100 mg of the (B) inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample can be measured using a laser diffraction particle size distribution measuring device with blue and red light source wavelengths used, and the volume-based particle size distribution of the (B) inorganic filler can be measured using a flow cell method, and the 50% cumulative diameter D50 and 90% cumulative diameter D90 can be calculated from the obtained particle size distribution. An example of a laser diffraction particle size distribution measuring device is "LA-960" manufactured by Horiba, Ltd.

[0078] The specific surface area of ​​the (B) inorganic filler is preferably 1 m or less from the viewpoint of significantly obtaining the desired effects of the present invention. 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area is determined by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0079] (B) Commercially available inorganic fillers include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company, Ltd.; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; and "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.

[0080] (B) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. The surface treatment agent may be used alone or in any combination of two or more.

[0081] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0082] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the (B) inorganic filler. Specifically, 100 parts by mass of the (B) inorganic filler is preferably surface-treated with 0.2 to 5 parts by mass of the surface treatment agent, more preferably with 0.2 to 3 parts by mass, and even more preferably with 0.3 to 2 parts by mass.

[0083] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the (B) inorganic filler. From the viewpoint of improving the dispersibility of the (B) inorganic filler, the amount of carbon per unit surface area of ​​the (B) inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the resin sheet layer, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0084] The carbon amount per unit surface area of ​​the (B) inorganic filler can be measured after the surface-treated (B) inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the (B) inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the carbon amount per unit surface area of ​​the (B) inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0085] The content of the (B) inorganic filler in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, from the viewpoint of obtaining the desired effect of the present invention more significantly, for example, 0 mass% or more, 1 mass% or more, preferably 10 mass% or more, 20 mass% or more, more preferably 30 mass% or more, 40 mass% or more, even more preferably 50 mass% or more, 60 mass% or more, even more preferably 65 mass% or more, 70 mass% or more, particularly preferably 75 mass% or more, 78 mass% or more, and the upper limit is preferably 95 mass% or less, more preferably 92 mass% or less, even more preferably 90 mass% or less, particularly preferably 89 mass% or less. If the content of the (B) inorganic filler is too high, the dispensability may decrease and the backflow phenomenon may easily occur.

[0086] <(C) Silane coupling agent> In the present invention, the resin composition may contain a silane coupling agent (C) as an optional component other than the components (A) and (B).

[0087] (C) Examples of the silane coupling agent include aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, alkoxysilane compounds, organosilazane compounds, and titanate coupling agents. Among them, epoxysilane coupling agents containing epoxy groups and mercaptosilane coupling agents containing mercapto groups are preferred. The silane coupling agents may be used alone or in combination of two or more.

[0088] As the (C) silane coupling agent, for example, a commercially available product may be used. Examples of commercially available silane coupling agents include "KBM403" (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM803" (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBE903" (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., and "SZ-31 " (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy type silane coupling agent), Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM503" (3-methacryloxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM5783", and the like.

[0089] The amount of (C) silane coupling agent is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.0001 mass% or more, preferably 0.001 mass% or more, more preferably 0.01 mass% or more, particularly preferably 0.05 mass% or more, and preferably 1 mass% or less, more preferably 0.5 mass% or less, and particularly preferably 0.3 mass% or less; when the total nonvolatile components in the resin composition other than (B) inorganic filler is taken as 100 mass%, it is, for example, 0 mass% or more, 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, particularly preferably 0.5 mass% or more, and preferably 10 mass% or less, more preferably 5 mass% or less, and particularly preferably 2 mass% or less.

[0090] <(D) Curing accelerator> The resin composition of the present invention may contain a curing accelerator (D) as an optional component other than the components (A) to (C). The curing accelerator (D) functions as a curing catalyst that accelerates the curing of the resin composition.

[0091] (D) Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. Among these, imidazole-based curing accelerators are preferred. The curing accelerators may be used alone or in combination of two or more.

[0092] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.

[0093] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, 1,8-diazabicyclo[5,4,0]undecene-7,4-dimethylaminopyridine, and 2,4,6-tris(dimethylaminomethyl)phenol, of which 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene are preferred.

[0094] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.

[0095] As the imidazole-based curing accelerator, commercially available products may be used, such as "P200-H50" manufactured by Mitsubishi Chemical Corporation, and "Curezol 2MZ", "2E4MZ", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", "Cl1Z-A", "2MZ-OK", "2MA-OK", "2MA-OK-PW", and "2PHZ" manufactured by Shikoku Chemical Industry Co., Ltd.

[0096] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.

[0097] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0098] The content of the (D) curing accelerator in the resin composition is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.05 mass% or more, particularly preferably 0.1 mass% or more, and preferably 5 mass% or less, more preferably 1 mass% or less, and particularly preferably 0.5 mass% or less; and when the total nonvolatile components other than the (B) inorganic filler in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.01 mass% or more, preferably 0.1 mass% or more, more preferably 0.5 mass% or more, particularly preferably 1 mass% or more, preferably 20 mass% or less, more preferably 10 mass% or less, and particularly preferably 5 mass% or less.

[0099] <(E) Radical Polymerizable Compound> The resin composition of the present invention may contain a radically polymerizable compound (E) as an optional component other than the components (A) to (D).

[0100] As the (E) radical polymerizable compound, a compound having an ethylenically unsaturated bond can be used. As such (E) radical polymerizable compound, for example, a compound having a radical polymerizable group such as a vinyl group, an allyl group, a 1-butenyl group, a 2-butenyl group, an acryloyl group, a methacryloyl group, a fumaroyl group, a maleoyl group, a vinylphenyl group, a styryl group, a cinnamoyl group, and a maleimide group (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl group) can be mentioned. As the (E) radical polymerizable compound, one type may be used alone, or two or more types may be used in combination.

[0101] Specific examples of the (E) radical polymerizable compound include (meth)acrylic radical polymerizable compounds having one or more acryloyl groups and / or methacryloyl groups, styrene radical polymerizable compounds having one or more vinyl groups directly bonded to an aromatic carbon atom, allyl radical polymerizable compounds having one or more allyl groups, maleimide radical polymerizable compounds having one or more maleimide groups, etc. Among these, (meth)acrylic radical polymerizable compounds are preferred.

[0102] The radical polymerizable compound (E) preferably contains a polyalkylene oxide structure. By using the radical polymerizable compound (E) containing a polyalkylene oxide structure, it is possible to increase the flexibility of the cured product of the resin composition of the present invention, reduce warping of the cured product, or improve adhesion between the cured product and the conductor layer.

[0103] The polyalkylene oxide structure has the formula -(R f O) n In this formula, n is usually an integer of 2 or more. This integer n is preferably 4 or more, more preferably 9 or more, and even more preferably 11 or more, and is usually 101 or less, preferably 90 or less, more preferably 68 or less, and even more preferably 65 or less. In formula (4), R f each independently represents an alkylene group which may have a substituent. The number of carbon atoms in the alkylene group is preferably 1 or more, more preferably 2 or more, and is preferably 6 or less, more preferably 5 or less, even more preferably 4 or less, even more preferably 3 or less, and particularly preferably 2. Specific examples of the polyalkylene oxide structure include a polyethylene oxide structure, a polypropylene oxide structure, a poly-n-butylene oxide structure, a poly(ethylene oxide-co-propylene oxide) structure, a poly(ethylene oxide-ran-propylene oxide) structure, a poly(ethylene oxide-alt-propylene oxide) structure, and a poly(ethylene oxide-block-propylene oxide) structure.

[0104] The number of polyalkylene oxide structures contained in one molecule of the (E) radical polymerizable compound may be 1 or 2 or more. The number of polyalkylene oxide structures contained in one molecule of the (E) radical polymerizable compound is preferably 2 or more, more preferably 4 or more, even more preferably 9 or more, particularly preferably 11 or more, and is preferably 101 or less, more preferably 90 or less, even more preferably 68 or less, particularly preferably 65 or less. When the (E) radical polymerizable compound contains two or more polyalkylene oxide structures in one molecule, those polyalkylene oxide structures may be the same as or different from each other.

[0105] Examples of commercially available products of the radical polymerizable compound (E) containing a polyalkylene oxide structure include monofunctional acrylates "AM-90G", "AM-130G", and "AMP-20GY" manufactured by Shin-Nakamura Chemical Co., Ltd.; bifunctional acrylates "A-1000", "A-B1206PE", "A-BPE-20", and "A-BPE-30"; monofunctional methacrylates "M-20G", "M-40G", "M-90G", "M-130G", and "M-230G"; and bifunctional methacrylates "23G", "BPE-900", "BPE-1300N", and "1206PE". Other examples include "Light Ester BC", "Light Ester 041MA", "Light Acrylate EC-A", and "Light Acrylate EHDG-AT" manufactured by Kyoeisha Chemical Co., Ltd.; "FA-023M" manufactured by Hitachi Chemical Co., Ltd.; "Blenmer (registered trademark) PME-4000", "Blenmer (registered trademark) 50POEO-800B", "Blenmer (registered trademark) PLE-200", "Blenmer (registered trademark) PLE-1300", "Blenmer (registered trademark) PSE-1300", "Blenmer (registered trademark) 43PAPE-600B", and "Blenmer (registered trademark) ANP-300" manufactured by NOF Corporation. Among these, "M-130G" (n is 13 on average) having a polyalkylene oxide structure (specifically, a polyethylene oxide structure) and "M-230G" (n is 23 on average) having a polyalkylene oxide structure (specifically, a polyethylene oxide structure) are preferred.

[0106] The ethylenically unsaturated bond equivalent of the (E) radically polymerizable compound is preferably 20 g / eq. to 3000 g / eq., more preferably 50 g / eq. to 2500 g / eq., further preferably 70 g / eq. to 2000 g / eq., and particularly preferably 90 g / eq. to 1500 g / eq. The ethylenically unsaturated bond equivalent represents the mass of the radically polymerizable compound per equivalent of the ethylenically unsaturated bond.

[0107] The weight average molecular weight (Mw) of the radically polymerizable compound (E) is preferably 150 or more, more preferably 250 or more, even more preferably 400 or more, and is preferably 40,000 or less, more preferably 10,000 or less, even more preferably 5,000 or less, and particularly preferably 3,000 or less.

[0108] The content of the (E) radical polymerizable compound in the resin composition is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.1 mass% or more, preferably 0.5 mass% or more, more preferably 1 mass% or more, particularly preferably 3 mass% or more, and preferably 15 mass% or less, more preferably 10 mass% or less, and particularly preferably 5 mass% or less; and when the total nonvolatile components other than the (B) inorganic filler in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 1 mass% or more, preferably 5 mass% or more, more preferably 10 mass% or more, particularly preferably 20 mass% or more, and preferably 40 mass% or less, more preferably 30 mass% or less, and particularly preferably 25 mass% or less.

[0109] <(F) Radical polymerization initiator> The resin composition of the present invention may further contain (F) a radical polymerization initiator as an optional component. As the (F) radical polymerization initiator, a thermal polymerization initiator that generates free radicals when heated is preferable. As the (F) radical polymerization initiator, one type may be used alone, or two or more types may be used in combination.

[0110] (F) Examples of the radical polymerization initiator include peroxide-based radical polymerization initiators, azo-based radical polymerization initiators, etc. Among these, peroxide-based radical polymerization initiators are preferred.

[0111] Examples of the peroxide radical polymerization initiator include hydroperoxide compounds such as 1,1,3,3-tetramethylbutyl hydroperoxide; dialkyl peroxide compounds such as tert-butylcumyl peroxide, di-tert-butyl peroxide, di-tert-hexyl peroxide, dicumyl peroxide, 1,4-bis(1-tert-butylperoxy-1-methylethyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexyne; dilauroyl peroxide, didecanoyl peroxide, dicyclohexyl peroxydicarbonate, and bis(4-tert-butylcyclohexyl)peroxydica. diacyl peroxide compounds such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyneodecanoate, tert-hexylperoxyisopropyl monocarbonate, tert-butyl peroxylaurate, (1,1-dimethylpropyl)2-ethylperhexanoate, tert-butyl 2-ethylperhexanoate, tert-butyl 3,5,5-trimethylperhexanoate, tert-butylperoxy-2-ethylhexyl monocarbonate, tert-butylperoxymaleic acid, and other peroxy ester compounds.

[0112] Examples of the azo radical polymerization initiator include azonitrile compounds such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, and 2-phenylazo-4-methoxy-2,4-dimethyl-valeronitrile; 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide], 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide], and the like. azo amide compounds such as 2,2'-azobis[2-methyl-N-[2-(1-hydroxybutyl)]-propionamide], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], 2,2'-azobis(2-methylpropionamide) dihydrate, 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), and 2,2'-azobis(N-cyclohexyl-2-methylpropionamide); alkyl azo compounds such as 2,2'-azobis(2,4,4-trimethylpentane) and 2,2'-azobis(2-methylpropane); and the like.

[0113] The radical polymerization initiator (F) is preferably one having a medium temperature activity. Specifically, the radical polymerization initiator (F) preferably has a 10-hour half-life temperature T10 (°C) in a specific low temperature range. The 10-hour half-life temperature T10 is preferably 50°C to 110°C, more preferably 50°C to 100°C, and even more preferably 50°C to 80°C. Examples of commercially available products of such radical polymerization initiator (F) include "Luperox 531M80" manufactured by Arkema Fuji Co., Ltd., "Perhexyl (registered trademark) O" manufactured by NOF Corporation, and "MAIB" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0114] The content of the radical polymerization initiator (F) in the resin composition is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.0001 mass% or more, preferably 0.001 mass% or more, more preferably 0.01 mass% or more, particularly preferably 0.05 mass% or more, and preferably 1 mass% or less, more preferably 0.5 mass% or less, and particularly preferably 0.1 mass% or less; and when the total nonvolatile components other than the inorganic filler (B) in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, particularly preferably 0.3 mass% or more, and preferably 3 mass% or less, more preferably 1 mass% or less, and particularly preferably 0.5 mass% or less.

[0115] <(G) Polyether skeleton-containing compound> The resin composition of the present invention may contain (G) a polyether skeleton-containing compound as an optional component other than the components (A) to (F). The (G) polyether skeleton-containing compound may be used alone or in combination of two or more.

[0116] The (G) polyether skeleton-containing compound is a polymer compound having a polyether skeleton. The polyether skeleton contained in the (G) polyether skeleton-containing compound is preferably a polyoxyalkylene skeleton composed of one or more monomer units selected from ethylene oxide units and propylene oxide units. Therefore, the (G) polyether skeleton-containing compound preferably does not contain a polyether skeleton containing a monomer unit having 4 or more carbon atoms, such as a butylene oxide unit or a phenylene oxide unit.

[0117] The (G) polyether skeleton-containing compound may contain a silicone skeleton. Examples of silicone skeletons include polydialkylsiloxane skeletons such as polydimethylsiloxane skeletons; polydiarylsiloxane skeletons such as polydiphenylsiloxane skeletons; polyalkylarylsiloxane skeletons such as polymethylphenylsiloxane skeletons; polydialkyl-diarylsiloxane skeletons such as polydimethyl-diphenylsiloxane skeletons; polydialkyl-alkylarylsiloxane skeletons such as polydimethyl-methylphenylsiloxane skeletons; polydiaryl-alkylarylsiloxane skeletons such as polydiphenyl-methylphenylsiloxane skeletons, and the like. The polydialkylsiloxane skeleton is preferred, and the polydimethylsiloxane skeleton is particularly preferred. The (G) polyether skeleton-containing compound containing a silicone skeleton may be, for example, polyoxyalkylene-modified silicone, alkyl-etherified polyoxyalkylene-modified silicone (polyoxyalkylene-modified silicone in which at least a part of the polyether skeleton terminal is an alkoxy group), and the like. The polyether skeleton-containing compound (G) may contain a hydroxy group.

[0118] (G) Examples of polyether skeleton-containing compounds include linear polyoxyalkylene glycols (linear polyalkylene glycols) such as polyethylene glycol, polypropylene glycol, and polyoxyethylene polyoxypropylene glycol; polyoxyethylene glyceryl ether, polyoxypropylene glyceryl ether, polyoxyethylene polyoxypropylene glyceryl ether, polyoxyethylene trimethylolpropane ether, polyoxypropylene trimethylolpropane ether, polyoxyethylene polyoxypropylene trimethylolpropane ether, polyoxyethylene diglyceryl ether, polyoxypropylene diglyceryl ether, polyoxyethylene polyoxypropylene diglyceryl ether, polyoxyethylene pentaerythritol ether, polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene sorbitol ... Polyoxyalkylene glycols (polyalkylene glycols) such as multi-chain polyoxyalkylene glycols (multi-chain polyalkylene glycols) such as propylene sorbitol and polyoxyethylene polyoxypropylene sorbitol; polyoxyalkylene alkyl ethers such as polyoxyethylene monoalkyl ethers, polyoxyethylene dialkyl ethers, polyoxypropylene monoalkyl ethers, polyoxyethylene polyoxypropylene monoalkyl ethers, and polyoxyethylene polyoxypropylene dialkyl ethers; polyoxyalkylene esters such as polyoxyethylene monoesters, polyoxyethylene diesters, polypropylene glycol monoesters, polypropylene glycol diesters, polyoxyethylene polyoxypropylene monoesters, and polyoxyethylene polyoxypropylene diesters (including acetates, propionates, butyrates, (meth)acrylates, etc.);Polyoxyalkylene alkyl ether esters (including acetates, propionates, butyrates, (meth)acrylates, etc.) such as polyoxyethylene monoesters, polyoxyethylene diesters, polyoxypropylene monoesters, polyoxypropylene diesters, polyoxyethylene polyoxypropylene monoesters, polyoxyethylene polyoxypropylene diesters, polyoxyethylene alkyl ether esters, polyoxypropylene alkyl ether esters, and polyoxyethylene polyoxypropylene alkyl ether esters; polyoxyalkylene alkylamines such as polyoxyethylene alkylamines, polyoxypropylene alkylamines, and polyoxyethylene polyoxypropylene alkylamines; polyoxyalkylene alkylamides such as polyoxyethylene alkylamides, polyoxypropylene alkylamides, and polyoxyethylene polyoxypropylene alkylamides; polyoxyethylene dimethicone, poly Polyoxyalkylene-modified silicones such as polyoxypropylene dimethicone, polyoxyethylene polyoxypropylene dimethicone, polyoxyethylene polydimethylsiloxy alkyl dimethicone, polyoxypropylene polydimethylsiloxy alkyl dimethicone, and polyoxyethylene polyoxypropylene polydimethylsiloxy alkyl dimethicone; alkyl etherified polyoxyalkylene-modified silicones (polyoxyalkylene-modified silicones in which at least a portion of the polyether skeleton terminal is an alkoxy group) such as polyoxyethylene alkyl ether dimethicone, polyoxypropylene alkyl ether dimethicone, polyoxyethylene polyoxypropylene alkyl ether dimethicone, polyoxyethylene alkyl ether polydimethylsiloxy alkyl dimethicone, and polyoxyethylene polyoxypropylene alkyl ether polydimethylsiloxy alkyl dimethicone;

[0119] The number average molecular weight of the (G) polyether skeleton-containing compound is preferably 500 to 40000, more preferably 500 to 20000, and even more preferably 500 to 10000. The weight average molecular weight of the (G) polyether skeleton-containing compound is preferably 500 to 40000, more preferably 500 to 20000, and even more preferably 500 to 10000. The number average molecular weight and weight average molecular weight can be measured as polystyrene-equivalent values ​​by gel permeation chromatography (GPC).

[0120] The polyether skeleton-containing compound (G) is preferably liquid at 25°C. The viscosity of the polyether skeleton-containing compound (G) at 25°C is preferably 100000 mPa·s or less, more preferably 50000 mPa·s or less, even more preferably 30000 mPa·s or less, even more preferably 10000 mPa·s or less, even more preferably 5000 mPa·s or less, even more preferably 4000 mPa·s or less, even more preferably 3000 mPa·s or less, even more preferably 2000 mPa·s or less, and particularly preferably 1500 mPa·s or less. The lower limit of the viscosity of the polyether skeleton-containing compound (G) at 25°C is preferably 10 mPa·s or more, more preferably 20 mPa·s or more, even more preferably 30 mPa·s or more, even more preferably 40 mPa·s or more, and particularly preferably 50 mPa·s or more. The viscosity may be a viscosity (mPa·s) obtained by measurement using a B-type viscometer.

[0121] (G) Commercially available polyether skeleton-containing compounds include, for example, NOF Corp.'s "Pronon #102", "Pronon #104", "Pronon #201", "Pronon #202B", "Pronon #204", "Pronon #208", "Unilube 70DP-600B", and "Unilube 70DP-950B" (polyoxyethylene polyoxypropylene glycol); ADEKA Corp.'s "Pluronic L-23", "Pluronic L-31", "Pluronic L-44", "Pluronic L-61", "ADEKA Pluronic L-62", "Pluronic L-64", "Pluronic L-71", "Pluronic L-72", "Pluronic L-101", "Pluronic L-121", "Pluronic P-84", "Pluronic P-85", "Pluronic P-103", "Pluronic F-68", "Pluronic F-88", "Pluronic F-108", and "Pluronic 25R-1"; "Pluronic 25R-2", "Pluronic 17R-2", "Pluronic 17R-3", "Pluronic 17R-4" (Polyoxyethylene polyoxypropylene glycol); "KF-6011", "KF-6011P", "KF-6012", "KF-6013", "KF-6015", "KF-6016", "KF-6017", "KF-6017P", "KF-6043", "KF-6004", "KF35" manufactured by Shin-Etsu Silicone Co., Ltd. 1A", "KF352A", "KF353", "KF354L", "KF355A", "KF615A", "KF945", "KF-640", "KF-642", "KF-643", "KF-644", "KF-6020", "KF-6204", "X22-4515", "KF-6028", "KF-6028P", "KF-6038", "KF-6048", and "KF-6025" (polyoxyalkylene-modified silicone).

[0122] The content of the (G) polyether skeleton-containing compound in the resin composition is not particularly limited, but when the total nonvolatile components in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, particularly preferably 0.5 mass% or more, preferably 5 mass% or less, more preferably 2 mass% or less, and particularly preferably 1 mass% or less; when the total nonvolatile components other than the (B) inorganic filler in the resin composition is taken as 100 mass%, it is, for example, 0 mass% or more, 0.1 mass% or more, preferably 0.5 mass% or more, more preferably 1 mass% or more, particularly preferably 5 mass% or more, preferably 15 mass% or less, more preferably 10 mass% or less, and particularly preferably 7 mass% or less.

[0123] <(H) Other Additives> The resin composition of the present invention may contain any additive as a non-volatile component other than the above-mentioned components (A) to (G). Examples of such additives include organic fillers such as rubber particles, polyamide fine particles, and silicone particles; thermoplastic resins such as polycarbonate resins, phenoxy resins, polyvinyl acetal resins, polyolefin resins, polysulfone resins, and polyester resins; organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; urea silanes. antioxidants such as hindered phenol antioxidants and hindered amine antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; and stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic acid anhydride-based stabilizers. The additives may be used alone or in combination of two or more kinds in any ratio.

[0124] <(I) Organic solvent> The resin composition of the present invention may further contain (I) any organic solvent as a volatile component. The (I) organic solvent may be used alone or in combination of two or more at any ratio. The smaller the amount of the solvent, the more preferable. The amount of the solvent is preferably 3% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, even more preferably 0.01% by mass or less, and particularly preferably no solvent (0% by mass) relative to 100% by mass of the total non-volatile components in the resin composition of the present invention.

[0125] <Method of producing resin composition> The resin composition of the present invention can be produced, for example, by mixing the above-mentioned components. The above-mentioned components may be mixed partially or entirely at the same time, or may be mixed in sequence. In the process of mixing each component, the temperature may be appropriately set, and thus heating and / or cooling may be performed temporarily or throughout. In addition, stirring or shaking may be performed in the process of mixing each component.

[0126] <Applications of resin composition> The resin composition of the present invention can be suitably used as a resin composition (resin composition for encapsulation) for encapsulating electronic devices such as organic EL devices and semiconductors, and in particular, can be suitably used as a resin composition for encapsulating semiconductors (resin composition for semiconductor encapsulation), preferably as a resin composition for encapsulating semiconductor chips (resin composition for semiconductor chip encapsulation). In addition, the resin composition can be used as a resin composition for insulating applications for insulating layers other than encapsulation. For example, the resin composition can be suitably used as a resin composition for forming an insulating layer of a semiconductor chip package (resin composition for insulating layer of semiconductor chip package) and a resin composition for forming an insulating layer of a circuit board (including a printed wiring board) (resin composition for insulating layer of circuit board).

[0127] From the viewpoint of utilizing the advantage of being able to improve the resolution of the layer of the photosensitive resin composition formed on the cured layer of the resin composition of the present invention, the resin composition of the present invention is preferably used as a material for forming a sealing layer or an insulating layer of a semiconductor chip package. Examples of the semiconductor chip package include FC-CSP, MIS-BGA package, ETS-BGA package, Fan-out type WLP (Wafer Level Package), Fan-in type WLP, Fan-out type PLP (Panel Level Package), and Fan-in type PLP.

[0128] The resin composition may also be used as an underfill material, for example, as a material for MUF (Molding Under Filling) that is used after a semiconductor chip is connected to a substrate.

[0129] Furthermore, the resin composition can be used in a wide range of applications in which resin compositions are used, such as resin sheets, sheet-like laminate materials such as prepregs, solder resists, die bonding materials, hole filling resins, and component embedding resins.

[0130] <Resin sheet> The resin sheet has a support and a resin composition layer provided on the support. The resin composition layer is a layer formed from the resin composition of the present invention.

[0131] From the viewpoint of thinning, the thickness of the resin composition layer is preferably 600 μm or less, more preferably 500 μm or less. The lower limit of the thickness of the resin composition layer is preferably 1 μm or more, 5 μm or more, more preferably 10 μm or more, even more preferably 50 μm or more, and particularly preferably 100 μm or more.

[0132] The thickness of the cured layer obtained by curing the resin composition layer is preferably 600 μm or less, more preferably 500 μm or less. The lower limit of the thickness of the cured layer is preferably 1 μm or more, 5 μm or more, more preferably 10 μm or more, even more preferably 50 μm or more, and particularly preferably 100 μm or more.

[0133] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0134] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"); polycarbonate (hereinafter sometimes abbreviated as "PC"); acrylic polymers such as polymethyl methacrylate (hereinafter sometimes abbreviated as "PMMA"); cyclic polyolefins; triacetyl cellulose (hereinafter sometimes abbreviated as "TAC"); polyether sulfide (hereinafter sometimes abbreviated as "PES"); polyether ketone; polyimide; and the like. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0135] When a metal foil is used as the support, examples of the metal foil include copper foil and aluminum foil. Among them, copper foil is preferable. As the copper foil, a foil made of a single metal of copper may be used, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0136] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, an antistatic treatment or the like.

[0137] In addition, the support may be a support with a release layer having a release layer on the surface to be bonded to the resin composition layer. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Examples of commercially available release agents include alkyd resin-based release agents such as "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation. Examples of the support with a release layer include "Lumirror T60" manufactured by Toray Industries, Inc.; "Purex" manufactured by Teijin Limited; and "Unipeel" manufactured by Unitika Limited.

[0138] The thickness of the support is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the total thickness of the support with a release layer is preferably in the above range.

[0139] The resin sheet can be produced, for example, by applying the resin composition of the present invention onto a support using a coating device such as a die coater. If necessary, the resin composition of the present invention may be dissolved in an organic solvent to prepare a resin varnish, and the resin sheet may be produced by applying the resin varnish. By using an organic solvent, the viscosity can be adjusted to improve the coatability. When the resin composition or resin varnish of the present invention containing an organic solvent is used, the resin composition or resin varnish of the present invention is usually dried after application to form the resin composition layer of the present invention.

[0140] Examples of the organic solvent include ketone solvents such as acetone, methyl ethyl ketone, and cyclohexanone; acetate ester solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitol solvents such as cellosolve and butyl carbitol; aromatic hydrocarbon solvents such as toluene and xylene; amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone; etc. The organic solvent may be used alone or in combination of two or more kinds at any ratio.

[0141] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are such that the content of the organic solvent in the resin composition layer is usually 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish of the present invention, for example, when the resin composition or resin varnish of the present invention containing 30% by mass to 60% by mass of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0142] The resin sheet may include any layer other than the support and the resin composition layer as necessary. For example, in the resin sheet, a protective film similar to that of the support may be provided on the surface of the resin composition layer not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is, for example, 1 μm to 40 μm. The protective film can prevent the adhesion of dirt and the like to the surface of the resin composition layer and scratches. When the resin sheet has a protective film, the resin sheet can be used by peeling off the protective film. In addition, the resin sheet can be stored by being wound into a roll.

[0143] The resin sheet can be suitably used to form an insulating layer in the manufacture of a semiconductor chip package (resin sheet for insulating a semiconductor chip package). For example, the resin sheet can be used to form an insulating layer of a circuit board (resin sheet for insulating a circuit board). Examples of packages using such boards include FC-CSP, MIS-BGA packages, and ETS-BGA packages.

[0144] The resin sheet can also be suitably used to seal a semiconductor chip (semiconductor chip sealing resin sheet). Applicable semiconductor chip packages include, for example, fan-out type WLP, fan-in type WLP, fan-out type PLP, fan-in type PLP, etc.

[0145] The resin sheet may also be used as a material for the MUF that is used after the semiconductor chip is connected to the substrate.

[0146] Furthermore, the resin sheet can be used in a wide range of other applications requiring high insulation reliability, for example, the resin sheet can be suitably used to form an insulating layer of a circuit board such as a printed wiring board.

[0147] <Circuit board> The circuit board includes a cured product of a resin composition. Usually, the circuit board includes a cured product layer formed of the cured product of the resin composition, and the cured product layer can function as an insulating layer or a sealing layer. The circuit board can be manufactured, for example, by a manufacturing method including the following steps (1) and (2). (1) A step of forming a resin composition layer on a substrate. (2) A step of thermally curing the resin composition layer to form a cured product layer.

[0148] In step (1), a substrate is prepared. Examples of the substrate include glass epoxy substrates, metal substrates (stainless steel, cold rolled steel plate (SPCC), silicon wafer, etc.), polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The substrate may have a metal layer such as copper foil on the surface as a part of the substrate. For example, a substrate having a peelable first metal layer and a second metal layer on both surfaces may be used. When such a substrate is used, a conductor layer as a wiring layer that can function as a circuit wiring is usually formed on the surface of the second metal layer opposite to the first metal layer. Examples of materials for the metal layer include copper foil, copper foil with a carrier, and materials for the conductor layer described later, and copper foil is preferred. Examples of substrates having a metal layer include an ultra-thin copper foil with a carrier "Micro Thin" manufactured by Mitsui Mining & Smelting Co., Ltd.

[0149] A conductor layer may be formed on one or both surfaces of the substrate. In the following description, a member including a substrate and a conductor layer formed on the substrate surface may be referred to as a "substrate with wiring layer" as appropriate. Examples of the conductor material included in the conductor layer include materials including one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. The conductor material may be a single metal or an alloy. Examples of the alloy include alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, and ease of patterning in the formation of the conductor layer, chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper as single metals; and alloys of nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy as alloys; are preferred. Among these, the single metals chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver and copper; and nickel-chromium alloys; are more preferable, and the single metal copper is particularly preferable.

[0150] The conductor layer may be patterned, for example, to function as a wiring layer. In this case, the line (circuit width) / space (width between circuits) ratio of the conductor layer is not particularly limited, but is preferably 20 / 20 μm or less (i.e., pitch is 40 μm or less), more preferably 10 / 10 μm or less, even more preferably 5 / 5 μm or less, even more preferably 1 / 1 μm or less, and particularly preferably 0.5 / 0.5 μm or more. The pitch does not need to be the same throughout the conductor layer. The minimum pitch of the conductor layer may be, for example, 40 μm or less, 36 μm or less, or 30 μm or less.

[0151] The thickness of the conductor layer depends on the design of the substrate, but is preferably 3 μm to 35 μm, more preferably 5 μm to 30 μm, further preferably 10 μm to 20 μm, and particularly preferably 15 μm to 20 μm.

[0152] After preparing the substrate, a resin composition layer is formed on the substrate. When a conductor layer is formed on the surface of the substrate, the resin composition layer is preferably formed so that the conductor layer is embedded in the resin composition layer.

[0153] The resin composition layer can be formed, for example, by a compression molding method. In the compression molding method, for example, a substrate on which the resin composition is dispensed using a syringe is placed in a mold, and pressure and, if necessary, heat are applied to the resin composition in the mold to form a resin composition layer on the substrate.

[0154] A specific operation of the compression molding method can be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. A resin composition is dispensed onto a substrate using a syringe. The substrate onto which the resin composition has been dispensed is attached to the lower mold. The upper and lower molds are then clamped together, and heat and pressure are applied to the resin composition to perform compression molding.

[0155] The molding conditions vary depending on the composition of the resin composition, and appropriate conditions can be adopted so that good sealing is achieved. For example, the temperature of the mold during molding is preferably 70°C or higher, more preferably 80°C or higher, particularly preferably 90°C or higher, and preferably 200°C or lower, more preferably 170°C or lower, particularly preferably 150°C or lower. The pressure applied during molding is preferably 1 MPa or higher, more preferably 3 MPa or higher, particularly preferably 5 MPa or higher, preferably 50 MPa or lower, more preferably 30 MPa or lower, particularly preferably 20 MPa or lower. The cure time is preferably 1 minute or higher, more preferably 2 minutes or higher, particularly preferably 3 minutes or higher, preferably 60 minutes or lower, more preferably 30 minutes or lower, particularly preferably 20 minutes or lower. Usually, the mold is removed after the formation of the resin composition layer. The mold may be removed before or after the resin composition layer is thermally cured.

[0156] The resin composition layer may be formed, for example, by laminating a resin sheet and a substrate. This lamination can be performed, for example, by bonding the resin sheet to the substrate from the support side under heat and pressure, thereby laminating the resin composition layer to the substrate. Examples of the member for heat-pressing the resin sheet to the substrate (hereinafter, sometimes referred to as a "heat-pressing member") include a heated metal plate (such as a SUS plate) or a metal roll (such as a SUS roll). It is preferable to press the heat-pressing member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate.

[0157] The lamination of the substrate and the resin sheet may be carried out, for example, by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C. The thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably 0.29MPa to 1.47MPa. The thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. The lamination is preferably carried out under reduced pressure conditions of 13hPa or less.

[0158] After lamination, the laminated resin sheets may be smoothed under normal pressure (atmospheric pressure), for example, by pressing the support side with a thermocompression member. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The lamination and smoothing treatment may be performed successively using a vacuum laminator.

[0159] After forming the resin composition layer on the substrate, the resin composition layer is thermally cured to form a cured layer. The thermal curing conditions for the resin composition layer may vary depending on the type of resin composition, but the curing temperature is usually in the range of 120°C to 240°C (preferably in the range of 150°C to 220°C, more preferably in the range of 170°C to 200°C), and the curing time is in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).

[0160] Before the resin composition layer is thermally cured, the resin composition layer may be subjected to a preheating treatment at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of usually 50° C. or more and less than 120° C. (preferably 60° C. or more and 110° C. or less, more preferably 70° C. or more and 100° C. or less) for usually 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).

[0161] In the manner described above, a circuit board having a cured layer formed of a cured product of the resin composition can be produced. The method for producing a circuit board may further include any optional step. For example, when a circuit board is manufactured using a resin sheet, the manufacturing method of the circuit board may include a step of peeling off the support of the resin sheet. The support may be peeled off before or after the resin composition layer is thermally cured.

[0162] The method for producing a circuit board may include, for example, a step of polishing the surface of the cured layer after forming the cured layer. The polishing method is not particularly limited. Examples of the polishing method include a chemical mechanical polishing method using a chemical mechanical polishing device, a mechanical polishing method using a buff, and a surface grinding method using a rotating grindstone.

[0163] The method for producing a circuit board may include, for example, a step (3) of connecting the conductor layers between layers, for example, a step of drilling holes in the cured material layer. This allows holes such as via holes and through holes to be formed in the cured material layer. Examples of methods for forming via holes include laser irradiation, etching, and mechanical drilling. The dimensions and shape of the via holes may be appropriately determined depending on the design of the circuit board. In addition, in the step (3), the interlayer connection may be performed by polishing or grinding the cured material layer.

[0164] After the via holes are formed, it is preferable to carry out a step of removing smears in the via holes. This step is sometimes called a desmear step. For example, when the conductive layer is formed on the cured material layer by a plating step, the via holes may be subjected to a wet desmear treatment. When the conductive layer is formed on the cured material layer by a sputtering step, a dry desmear step such as a plasma treatment step may be carried out. Furthermore, the cured material layer may be subjected to a roughening treatment by the desmear step.

[0165] In addition, before forming a conductor layer on the cured layer, the cured layer may be subjected to a roughening treatment. According to this roughening treatment, the surface of the cured layer including the inside of the via hole is usually roughened. The roughening treatment may be either a dry type or a wet type. An example of the dry type roughening treatment is a plasma treatment. An example of the wet type roughening treatment is a method in which a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid are performed in this order.

[0166] After the via holes are formed, a conductor layer may be formed on the cured layer. By forming a conductor layer at the position where the via holes are formed, the newly formed conductor layer and the conductor layer on the surface of the substrate are electrically connected to each other, and interlayer connection is performed. Examples of the method for forming the conductor layer include plating, sputtering, and vapor deposition. For example, a conductor layer having a desired wiring pattern may be formed by plating the surface of the cured layer by an appropriate method such as a semi-additive method or a full-additive method. In addition, for example, when the support in the resin sheet is a metal foil, a conductor layer having a desired wiring pattern may be formed by a subtractive method. The material of the conductor layer formed may be a single metal or an alloy. In addition, this conductor layer may have a single layer structure, or may have a multi-layer structure including two or more layers of different types of materials.

[0167] Here, an example of an embodiment in which a conductor layer is formed on a cured material layer will be described in detail. A mask layer is formed on the surface of the cured material layer, and openings are formed in a part of the mask layer as a mask pattern. Thereafter, a metal layer is formed by sputtering, and then the mask layer is removed. This allows the formation of a conductor layer having a desired wiring pattern. The mask layer is usually formed by a layer of a photosensitive resin composition. The openings of the mask layer can be formed by exposing and developing the layer of the photosensitive resin composition.

[0168] The method for producing a circuit board may include a step (4) of removing the substrate. By removing the substrate, a circuit board having a cured layer and a conductor layer embedded in the cured layer is obtained. This step (4) can be performed, for example, when a substrate having a peelable metal layer is used.

[0169] <Semiconductor chip package> The semiconductor chip package includes a cured product of the resin composition. Examples of the semiconductor chip package include the following.

[0170] The semiconductor chip package according to the first example includes the above-mentioned circuit board and a semiconductor chip mounted on the circuit board. This semiconductor chip package can be manufactured by bonding the semiconductor chip to the circuit board.

[0171] The bonding conditions between the circuit board and the semiconductor chip may be any conditions that allow conductive connection between the terminal electrodes of the semiconductor chip and the circuit wiring of the circuit board. For example, the conditions used in flip-chip mounting of the semiconductor chip may be used. Also, for example, the semiconductor chip and the circuit board may be bonded via an insulating adhesive.

[0172] An example of a bonding method is a method of bonding a semiconductor chip to a circuit board. The bonding conditions are that the bonding temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and the bonding time is usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).

[0173] Another example of the bonding method is a method of bonding a semiconductor chip to a circuit board by reflow. The reflow conditions may be in the range of 120°C to 300°C.

[0174] After the semiconductor chip is bonded to the circuit board, the semiconductor chip may be filled with a molded underfill material, which may be the resin composition described above.

[0175] The semiconductor chip package according to the second example includes a semiconductor chip and a cured resin composition that encapsulates the semiconductor chip. In such a semiconductor chip package, the cured resin composition usually functions as an encapsulation layer. An example of the semiconductor chip package according to the second example is a fan-out type WLP.

[0176] The method for manufacturing such a semiconductor chip package includes: (A) a step of laminating a temporary fixing film on a substrate; (B) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (C) forming an encapsulation layer on the semiconductor chip; (D) peeling the substrate and the temporary fixing film from the semiconductor chip; (E) a step of forming a rewiring formation layer on the surface from which the substrate and the temporary fixing film of the semiconductor chip have been peeled off; (F) forming a rewiring layer as a conductor layer on the rewiring formation layer; and (G) forming a solder resist layer on the rewiring layer; The method for manufacturing the semiconductor chip package further comprises: (H) A process of dicing and separating multiple semiconductor chip packages into individual semiconductor chip packages. may also include

[0177] (Process (A)) Step (A) is a step of laminating a temporary fixing film on a substrate. The lamination conditions for the substrate and the temporary fixing film can be the same as the lamination conditions for the substrate and the resin sheet in the method for producing a circuit board.

[0178] Examples of substrates include silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel sheet (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; and substrates made of bismaleimide triazine resin such as BT resin.

[0179] The temporary fixing film may be made of any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. Commercially available products include "Riva Alpha" manufactured by Nitto Denko Corporation.

[0180] (Process (B)) Step (B) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor chip packages to be produced, etc. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.

[0181] (Process (C)) Step (C) is a step of forming an encapsulating layer on the semiconductor chip. The encapsulating layer can be formed by a cured product of a resin composition. The encapsulating layer is usually formed by a method including a step of forming a resin composition layer on a semiconductor chip and a step of thermally curing the resin composition layer to form a cured product layer as the encapsulating layer. The formation of the resin composition layer on the semiconductor chip can be performed by the same method as the method of forming a resin composition layer on a substrate explained in the <circuit substrate> above, except that a semiconductor chip is used instead of a substrate.

[0182] After forming a resin composition layer on the semiconductor chip, the resin composition layer is thermally cured to obtain an encapsulation layer that covers the semiconductor chip. This encapsulates the semiconductor chip with a cured product of the resin composition. The thermal curing conditions of the resin composition layer may be the same as the thermal curing conditions of the resin composition layer in the manufacturing method of the circuit board. Furthermore, before thermally curing the resin composition layer, a preheating treatment may be performed on the resin composition layer at a temperature lower than the curing temperature. The treatment conditions of this preheating treatment may be the same as the preheating treatment in the manufacturing method of the circuit board.

[0183] (Process (D)) Step (D) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable to adopt an appropriate peeling method according to the material of the temporary fixing film. For example, the peeling method may be a method of heating, foaming or expanding the temporary fixing film to peel it off. In addition, for example, the peeling method may be a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off.

[0184] In the method of peeling off the temporary fixing film by heating, foaming or expanding it, the heating conditions are usually 100° C. to 250° C. for 1 second to 90 seconds or 5 minutes to 15 minutes. In the method of peeling off the temporary fixing film by reducing the adhesive strength of the temporary fixing film by irradiating it with ultraviolet light, the irradiation amount of ultraviolet light is usually 10 mJ / cm 2 ~1000mJ / cm 2 It is.

[0185] When the substrate and the temporary fixing film are peeled off from the semiconductor chip as described above, the surface of the encapsulation layer is exposed. The manufacturing method of the semiconductor chip package may include polishing the exposed surface of the encapsulation layer. The polishing can improve the smoothness of the surface of the encapsulation layer. The polishing method can be the same as that described in the manufacturing method of the circuit board.

[0186] (Process (E)) Step (E) is a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled off. Usually, this rewiring formation layer is formed on the semiconductor chip and the sealing layer.

[0187] The material of the rewiring formation layer may be any material having insulating properties. When the sealing layer is formed of a cured product of a resin composition, the rewiring formation layer formed on the sealing layer is preferably formed of a photosensitive resin composition.

[0188] After forming the rewiring formation layer, a via hole is usually formed in the rewiring formation layer in order to connect the semiconductor chip and the rewiring layer to each other. When the rewiring formation layer is formed of a photosensitive resin, the method of forming the via hole usually includes exposing the surface of the rewiring formation layer through a mask. Examples of the active energy ray include ultraviolet light, visible light, electron beams, and X-rays, and ultraviolet light is particularly preferred. Examples of the exposure method include a contact exposure method in which a mask is brought into close contact with the rewiring formation layer and exposed to light, and a non-contact exposure method in which a mask is not brought into close contact with the rewiring formation layer and exposed to light using parallel light.

[0189] The exposure can form a latent image in the redistribution layer, and then development can be performed to remove a part of the redistribution layer to form a via hole as an opening portion penetrating the redistribution layer. The development can be performed by either wet development or dry development. Examples of the development method include a dip method, a paddle method, a spray method, a brushing method, and a scraping method, and the paddle method is preferable from the viewpoint of resolution.

[0190] The shape of the via hole is not particularly limited, but is generally circular (approximately circular). The top diameter of the via hole is preferably 50 μm or less, more preferably 30 μm or less, further preferably 20 μm or less, and particularly preferably 10 μm or less. Here, the top diameter of the via hole refers to the diameter of the opening of the via hole on the surface of the rewiring formation layer.

[0191] (Process (F)) Step (F) is a step of forming a rewiring layer as a conductor layer on the rewiring formation layer. The method of forming the rewiring layer on the rewiring formation layer may be the same as the method of forming a conductor layer on the cured layer in the method of manufacturing a circuit board. Steps (E) and (F) may be repeated to alternately stack the rewiring layers and the rewiring formation layers (build up).

[0192] (Process (G)) Step (G) is a step of forming a solder resist layer on the rewiring layer. The material of the solder resist layer can be any material having insulating properties. Among them, photosensitive resins and thermosetting resins are preferred from the viewpoint of ease of manufacturing the semiconductor chip package. Also, a resin composition may be used as the thermosetting resin.

[0193] In step (G), bumping processing may be performed to form bumps, if necessary. The bumping processing can be performed by a method such as solder balls or solder plating. In addition, the formation of via holes in the bumping processing can be performed in the same manner as in step (E).

[0194] (Process (H)) The method for manufacturing a semiconductor chip package may include a step (H) in addition to the steps (A) to (G). The step (H) is a step of dicing a plurality of semiconductor chip packages into individual semiconductor chip packages to separate them. The method for dicing the semiconductor chip packages into individual semiconductor chip packages is not particularly limited.

[0195] <Semiconductor device> The semiconductor device includes a semiconductor chip package. Examples of the semiconductor device include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.). EXAMPLES

[0196] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (25°C) and atmospheric pressure (1 atm), respectively.

[0197] <Examples 1 to 9 and Comparative Examples 1 to 4> A resin composition was prepared by mixing the respective components in the prescribed amounts shown in Table 1 below. Details of each component shown in Table 1 are as follows.

[0198] (A-1) Epoxy resin: Celloxide 2021P: Alicyclic epoxy resin with an ester structure (Daicel's "Celloxide 2021P", liquid epoxy resin, epoxy equivalent 126g / eq.) HP4032D: Naphthalene type epoxy resin (DIC's "HP4032D", liquid epoxy resin, epoxy equivalent 151g / eq.) EX-991L: Alkyleneoxy skeleton-containing epoxy resin (Nagase ChemteX Corporation "EX-991L", liquid epoxy resin, epoxy equivalent 450g / eq.) EG-280: Fluorene structure-containing epoxy resin ("EG-280" manufactured by Osaka Gas Chemicals, liquid epoxy resin, epoxy equivalent 460g / eq.) YX7400: Polyalkyleneoxy structure-containing resin (Mitsubishi Chemical's "YX7400", liquid epoxy resin, epoxy equivalent 440g / eq) EP-3950L: Glycidylamine type epoxy resin (ADEKA "EP-3950L", liquid epoxy resin, epoxy equivalent 95g / eq.) EP-3980S: Glycidylamine type epoxy resin (ADEKA "EP-3980S", liquid epoxy resin, epoxy equivalent 115g / eq.) EP-4088S: Dicyclopentadiene type epoxy resin (ADEKA "EP-4088S", liquid epoxy resin, epoxy equivalent 170g / eq.) ZX1059: A 1:1 (mass ratio) mixture of bisphenol A epoxy resin and bisphenol F epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical & Materials Co., Ltd., liquid epoxy resin, epoxy equivalent 169g / eq.) JP-100: Epoxy resin with a butadiene structure ("JP-100" manufactured by Nippon Soda Co., Ltd., liquid epoxy resin, epoxy equivalent 210g / eq.)

[0199] (A-2) Epoxy hardener: 2,2-Diallylbisphenol A: Phenol-based hardener (Sigma-Aldrich, active group (phenolic hydroxyl group) equivalent: 154 g / eq.) Kayahard AA: Amine-based hardener (4,4'-diamino-3,3'-diethyldiphenylmethane, "Kayahard AA" manufactured by Nippon Kayaku, active group (amino group) equivalent: 64g / eq.) MH-700: Acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd., active group (acid anhydride group) equivalent: 164g / eq. (1 equivalent of acid anhydride group (-COOCO-) is calculated as 2 equivalents of active group))

[0200] (B) Inorganic filler: Silica A: Silica particles (50% cumulative diameter D50 = 1.5 μm, D90 = 3.5 μm, specific surface area 2.78 m 2 / g, surface-treated with KBM573 (manufactured by Shin-Etsu Chemical Co., Ltd.) Silica B: Silica particles (50% cumulative diameter D50 = 4 μm, D90 = 12 μm, specific surface area 3.01 m 2 / g, surface-treated with KBM573 (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0201] (C) Silane coupling agent: KBM-803: ("KBM803" manufactured by Shin-Etsu Chemical Co., Ltd., 3-mercaptopropyltrimethoxysilane) KBM-403: (Shin-Etsu Chemical Co., Ltd. "KBM403", 3-glycidoxypropyltrimethoxysilane)

[0202] (D) Curing accelerator: 2E4MZ: Imidazole-based curing accelerator ("2E4MZ" manufactured by Shikoku Chemical Industry Co., Ltd.) 2MA-OK-PW: Imidazole-based curing accelerator ("2MA-OK-PW" manufactured by Shikoku Kasei Co., Ltd.)

[0203] (E) Radical polymerizable compound: M-130G: A compound having a methacryloyl group and a polyethylene oxide structure ("M-130G" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 628 g / eq.) M-230G: A compound having a methacryloyl group and a polyethylene oxide structure ("M-230G" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 1068 g / eq.)

[0204] (F) Radical polymerization initiator: Perhexyl O: Radical polymerization initiator (NOF Corporation, "Perhexyl (registered trademark) O")

[0205] (G) Polyether skeleton-containing compound: Polyether polyol A: Resin synthesized as follows. 22.6g of ε-caprolactone monomer (Daicel Corporation's "Placcel M"), 10g of polypropylene glycol, diol type, 3,000 (Fujifilm Wako Pure Chemical Industries, Ltd.), and 1.62g of tin(II) 2-ethylhexanoate (Fujifilm Wako Pure Chemical Industries, Ltd.) were charged into a reaction vessel, heated to 130°C under a nitrogen atmosphere, and stirred for about 16 hours to react. The product after the reaction was dissolved in chloroform, and the product was reprecipitated with methanol and then dried to obtain polyester polyol resin A with a hydroxyl group terminal and an aliphatic skeleton. GPC analysis showed Mn=9000. L-64: Polyoxyethylene polyoxypropylene glycol (ADEKA "L-64") KF-6012: Polyoxyalkylene modified silicone resin ("KF-6012" manufactured by Shin-Etsu Chemical Co., Ltd., viscosity (25°C): 1500 mm 2 / s)

[0206] <Test Example 1: Viscosity Measurement> The viscosity of the resin compositions obtained in the examples and comparative examples was measured at a temperature of 25°C and a rotation speed of 1 rpm using an E-type viscometer RE-80U (manufactured by Toki Sangyo Co., Ltd.) with a cone rotor of 3° x R9.7 calibrated with the viscosity calibration standard liquid JS52000.

[0207] <Test Example 2: Evaluation of dispensability, ejection workability, and resin flowability> A 12 oz syringe (Saneitec Co., Ltd. 5194C, end cap A605, tip cap 5192RT, plunger 5196PRS, syringe outlet inner diameter 14.22 mm, outer diameter 19.30 mm, opening inner diameter 40.26 mm, length from outlet to opening 311.40 mm) was prepared, and a nozzle (tube material made of silicone, syringe connection material made of polypropylene, tube total length 52 mm, tube part exposed from syringe connection part length 25 mm, syringe connection part total length 52 mm, nozzle outlet part (tube part side) outer diameter 12 mm, inner diameter 9 mm, nozzle opening (syringe connection part side) outer diameter 14.22 mm) was attached to the syringe outlet, and the syringe was attached to a dispenser (Apic Yamada Co., Ltd. "Liquid Manual Dispenser"). The height from the surface of a horizontally placed 12-inch silicon wafer (Ra 10 Å or less) to the nozzle outlet (the distance perpendicular to the surface of the silicon wafer) was set to 3 cm, and 40 g±1.5 g of the resin composition was dispensed from the nozzle outlet onto the 12-inch silicon wafer at room temperature (23°C) at a rate of 2 g / sec. Dispensing was stopped when 40 g±1.5 g had been dispensed, forming a resin dome of the resin composition.

[0208] Evaluation of dispensability: When a backflow phenomenon occurred in which the resin composition leaked from the side of the plunger during dispensing, the case was marked "x", and when no backflow occurred, the case was marked "good".

[0209] Evaluation of dispensing workability: If the resin composition did not separate from the nozzle outlet well enough that the nozzle outlet and the dispensed resin composition remained connected when dispensing was stopped and could not be separated, or if resin dripped from the nozzle outlet after dispensing was completed, the evaluation was marked "X." If neither of these occurred, the evaluation was marked "O."

[0210] Evaluation of resin flow: After dispensing, the resin was molded in a compression molding device at 120°C and 6 MPa. If the resin was able to be molded without any unfilled areas in the mold, it was marked as "Good". If the resin leaked from the mold and soiled the device, it was marked as "Poor".

[0211] <Test Example 3: Calculation of H2 / H1 and L1 / L2 Values> A 12 oz syringe (5194C manufactured by San-ei Tech Co., Ltd., end cap A605, tip cap 5192RT, plunger 5196PRS, inner diameter of syringe outlet 14.22 mm, outer diameter 19.30 mm, inner diameter of opening 40.26 mm, length from outlet to opening 311.40 mm) filled with 200 g of the resin composition (room temperature (23°C)) obtained in the examples or comparative examples was prepared, and the syringe was attached to a dispenser ("Liquid Manual Dispenser" manufactured by Apic Yamada Co., Ltd.) without attaching a nozzle to the syringe. The height from the surface of a horizontally placed 12-inch silicon wafer (Ra 10 Å or less) to the outlet of the syringe (the distance in the direction perpendicular to the surface of the silicon wafer) was set to 5 cm, and 40 g ± 1.5 g of the resin composition was dispensed from the outlet of the syringe onto the 12-inch silicon wafer at a rate of 2 g / sec at room temperature (23°C). When 40 g ± 1.5 g had been dispensed, dispensing was stopped to form a resin dome of the resin composition. In Comparative Example 3, the outlet and the resin dome were in contact when dispensing was stopped, so an operation was performed to pull up the outlet after dispensing was stopped and separate the outlet from the resin dome.

[0212] After the resin dome was formed, the change in shape of the resin dome was observed at room temperature (23°C). The height H1 from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 60 seconds after dispensing was completed, the diameter L1 of the contact surface of the resin dome with the silicon wafer, the height H2 from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 180 seconds after dispensing was completed, and the diameter L2 of the contact surface of the resin dome with the silicon wafer were measured. The H2 / H1 and L1 / L2 values ​​were calculated, and the cases where the following formulas (1) and (2) were satisfied were evaluated as "Good", and the cases where they were not satisfied were evaluated as "Poor".

[0213] In addition, in the examples and comparative examples other than Comparative Example 3, the dispensing completion time was determined as the point at which 40 g±1.5 g of the resin composition had been dispensed, and in Comparative Example 3, the dispensing completion time was determined as the point at which the discharge port separated from the resin dome after the operation of pulling the discharge port away from the resin dome. 0.15 <H2 / H1<0.90 ···(1) 0.40 <L1 / L2<0.96 ···(2)

[0214] The non-volatile component contents of the resin compositions of the Examples and Comparative Examples, and the measurement results and evaluation results of the Test Examples are shown in Table 1 below.

[0215] [Table 1]

[0216] As shown in Table 1, when condition (1) is satisfied, the dispensability, ejection workability, and resin flowability are good. [Explanation of symbols]

[0217] 10. Syringe filled with resin composition 11 Syringe 12 Resin composition 13 Plunger 14 Female thread 15 Outlet 16 Opening 17 Tip cap 18 End Cap 20 Nozzles 21 Tube section 22 Syringe connection part 23 Nozzle discharge section 24 Nozzle opening 25 Male thread 30 Resin Dome 40 Silicon Wafer

Claims

1. A syringe filled with a resin composition, the syringe comprising: a syringe; and a resin composition filled in the syringe, the resin composition comprises (A-1) an epoxy resin and (B) an inorganic filler, the 90% cumulative diameter D90 of the (B) component is 30 μm or less, and the difference (D90-D50) between the 90% cumulative diameter D90 and the 50% cumulative diameter D50 is 20 μm or less, When the nonvolatile components in the resin composition are taken as 100 mass%, the content of the (B) component is 65 mass% or more and 95 mass% or less, When the total amount of non-volatile components other than the component (B) in the resin composition is taken as 100 mass%, the content of the component (A-1) is 10 mass% or more and 90 mass% or less, The content of the organic solvent (J) in the resin composition is 1% by mass or less based on 100% by mass of all non-volatile components in the resin composition; The resin composition comprises: In a resin composition evaluation test, a resin composition is dispensed onto a horizontally placed silicon wafer surface to form a resin dome of the resin composition, and a change in the shape of the resin dome is measured. The height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 60 seconds after the completion of dispensing is H 1 , The height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 180 seconds after the completion of dispensing is H 2 In this case, A syringe filled with a resin composition, which satisfies the condition of the following formula (1): 0.15<H 2 / H 1 <0.90 ・・・(1)

2. The evaluation test 2. The syringe filled with the resin composition according to claim 1, comprising dispensing 40 g±1.5 g of the resin composition at 23° C. onto the surface of the silicon wafer at a rate of 2 g / sec under a condition of 23° C. from a discharge port installed at a position 5 cm high from the surface of the silicon wafer, and stopping the dispensing to form a resin dome of the resin composition.

3. In the evaluation test, If the discharge port and the resin dome are not in contact with each other when the dispensing of the resin composition is stopped, the time when 40 g±1.5 g of the resin composition has been dispensed is regarded as the dispensing completion time.

3. The syringe filled with a resin composition as described in claim 2, wherein if the outlet and the resin dome are in contact when the dispensing of the resin composition is stopped, the outlet is pulled up after the dispensing is stopped to separate the outlet from the resin dome, and the point at which the outlet separates from the resin dome is regarded as the point at which the dispensing is completed.

4. The diameter of the contact surface of the resin dome with the silicon wafer 60 seconds after the completion of dispensing is L 1 , If the diameter of the contact surface of the resin dome with the silicon wafer 180 seconds after the completion of dispensing is L 2 , The syringe filled with the resin composition according to any one of claims 1 to 3, further satisfying the condition of the following formula (2): 0.40<L 1 / L 2 <0.96 (2)

5. A syringe filled with a resin composition according to any one of claims 1 to 4, wherein the viscosity of the resin composition measured using an E-type viscometer at a temperature of 25°C and a rotation speed of 1 rpm is 1000 Pa·s or less.

6. A syringe filled with a resin composition described in any one of claims 1 to 5, wherein the viscosity of the resin composition measured using an E-type viscometer at a temperature of 25°C and a rotation speed of 1 rpm is 100 Pa·s or more and 500 Pa·s or less.

7. In an evaluation test of a resin composition, a resin dome of the resin composition is formed by dispensing the resin composition on a surface of a horizontally placed silicon wafer, and a change in the shape of the resin dome is measured, The height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 60 seconds after the completion of dispensing is defined as H 1 , If the height from the contact surface of the resin dome with the silicon wafer to the apex of the resin dome 180 seconds after the completion of dispensing is H 2 , A resin composition that satisfies the condition of the following formula (1): the resin composition comprises (A-1) an epoxy resin and (B) an inorganic filler, the 90% cumulative diameter D90 of the (B) component is 30 μm or less, and the difference (D90-D50) between the 90% cumulative diameter D90 and the 50% cumulative diameter D50 is 20 μm or less, When the nonvolatile components in the resin composition are taken as 100 mass%, the content of the (B) component is 65 mass% or more and 95 mass% or less, When the total amount of non-volatile components other than the component (B) in the resin composition is taken as 100 mass%, the content of the component (A-1) is 10 mass% or more and 90 mass% or less, A resin composition, wherein the content of (J) an organic solvent in the resin composition is 1 mass% or less, based on 100 mass% of all nonvolatile components in the resin composition. 0.15<H2 / H1<0.90...(1)

8. The evaluation test 8. The resin composition according to claim 7, comprising dispensing 40 g±1.5 g of the resin composition at 23° C. onto the silicon wafer surface at a rate of 2 g / sec under a condition of 23° C. from a discharge port installed at a position 5 cm high from the silicon wafer surface, and stopping the dispensing to form a resin dome of the resin composition.

9. In the evaluation test, If the discharge port and the resin dome are not in contact with each other when the dispensing of the resin composition is stopped, the time when 40 g±1.5 g of the resin composition has been dispensed is regarded as the dispensing completion time. The resin composition according to claim 8, wherein if the outlet and the resin dome are in contact when dispensing of the resin composition is stopped, the outlet is pulled up after dispensing is stopped to separate the outlet from the resin dome, and the point at which the outlet separates from the resin dome is regarded as the point at which the dispensing is completed.

10. The diameter of the contact surface of the resin dome with the silicon wafer 60 seconds after the completion of dispensing is L 1 , If the diameter of the contact surface of the resin dome with the silicon wafer 180 seconds after the completion of dispensing is L 2 , The resin composition according to any one of claims 7 to 9, further satisfying the condition of the following formula (2): 0.40<L 1 / L 2 <0.96 (2)

11. A resin composition described in any one of claims 7 to 10, wherein the viscosity of the resin composition measured using an E-type viscometer at a temperature of 25°C and a rotation speed of 1 rpm is 1000 Pa·s or less.

12. A resin composition described in any one of claims 7 to 11, wherein the viscosity of the resin composition measured using an E-type viscometer at a temperature of 25°C and a rotation speed of 1 rpm is 100 Pa·s or more and 500 Pa·s or less.

13. A resin composition described in any one of claims 7 to 12 for forming an insulating layer of a semiconductor chip package.

14. A resin composition described in any one of claims 7 to 12 for forming an insulating layer of a circuit board.

15. A resin composition described in any one of claims 7 to 12 for encapsulating a semiconductor chip in a semiconductor chip package.

16. A cured product of the resin composition described in any one of claims 7 to 15.

17. A circuit board comprising an insulating layer formed from a cured product of the resin composition described in any one of claims 7 to 15.

18. A semiconductor chip package comprising the circuit board described in claim 17 and a semiconductor chip mounted on the circuit board.

19. A semiconductor chip package comprising a semiconductor chip and a cured product of the resin composition according to any one of claims 7 to 15 that encapsulates the semiconductor chip.

20. A semiconductor device comprising a semiconductor chip package according to claim 18 or 19.