Method for manufacturing a semiconductor device
Patent Information
- Application Number
- JP2024074371
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-07-27
- Filing Date
- 2024-05-01
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2039-06-26
AI Technical Summary
Existing semiconductor devices face issues with shape defects and poor electrical characteristics, particularly in large display devices with high screen sizes and resolutions, leading to increased wiring resistance and instability.
A transistor configuration is designed with a specific layer structure where the first insulating layer, metal oxide layer, functional layer, and conductive layer overlap, and their etching rates are matched to prevent undercuts, ensuring the layers have similar top surface shapes, thereby reducing shape defects and enhancing electrical stability.
The configuration results in a transistor with reduced shape defects and improved electrical characteristics, providing a highly reliable semiconductor device suitable for large, high-resolution displays.
Abstract
Description
[Technical field]
[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device. 2. Description of the Related Art One embodiment of the present invention relates to a method for manufacturing a semiconductor device or a display device.
[0002] Note that one embodiment of the present invention is not limited to the above technical field. Examples of the technical field of one embodiment of the present invention disclosed in this specification and the like include a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, an electronic device, a lighting device, an input device, an input / output device, a driving method thereof, or a manufacturing method thereof. A semiconductor device refers to any device that can function by utilizing semiconductor characteristics. [Background technology]
[0003] As a semiconductor material applicable to transistors, oxide semiconductors using metal oxides have been attracting attention. For example, Patent Document 1 discloses a semiconductor device in which a plurality of oxide semiconductor layers are stacked, and an oxide semiconductor layer serving as a channel among the plurality of oxide semiconductor layers contains indium and gallium, and the proportion of indium is made higher than the proportion of gallium, thereby increasing the field effect mobility (sometimes simply referred to as mobility, or μFE).
[0004] Metal oxides that can be used for the semiconductor layer can be formed by sputtering or the like, and therefore can be used for the semiconductor layer of transistors that constitute large display devices. In addition, since it is possible to use a part of the production equipment for transistors using polycrystalline silicon or amorphous silicon by improving it, capital investment can be reduced. In addition, transistors using metal oxides have higher field-effect mobility than those using amorphous silicon, and therefore a high-performance display device provided with a driver circuit can be realized.
[0005] Furthermore, in display devices, the screen size is tending to become larger, with development being carried out with screen sizes of 60 inches or more diagonally, and even 120 inches or more diagonally, in mind. Additionally, screen resolution is also trending higher, from full high vision (1920 x 1080 pixels, also known as "2K"), to ultra high vision (3840 x 2160 pixels, also known as "4K"), to super high vision (7680 x 4320 pixels, also known as "8K").
[0006] Larger screen sizes and higher definitions tend to increase the wiring resistance in the display section. Patent Document 2 discloses a technology for forming a low-resistance wiring layer using copper (Cu) in order to suppress the increase in wiring resistance in a liquid crystal display device using amorphous silicon transistors. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2014-7399 A [Patent Document 2] JP 2004-163901 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of one embodiment of the present invention is to provide a transistor which is less likely to have a defective shape.An object of one embodiment of the present invention is to provide a transistor with good electrical characteristics.An object of one embodiment of the present invention is to provide a semiconductor device with good electrical characteristics.An object of one embodiment of the present invention is to provide a semiconductor device with stable electrical characteristics.An object of one embodiment of the present invention is to provide a semiconductor device with high reliability.An object of one embodiment of the present invention is to provide a display device with high reliability.
[0009] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description of the specification, drawings, claims, etc. [Means for solving the problem]
[0010] One embodiment of the present invention is a semiconductor device having a transistor, the transistor having a semiconductor layer, a first insulating layer, a metal oxide layer, a functional layer, and a conductive layer, the first insulating layer is located over the semiconductor layer, the metal oxide layer is located over the first insulating layer, the functional layer is located over the metal oxide layer, and the conductive layer is located over the functional layer, the semiconductor layer, the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer have overlapping regions, end portions of the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer are located inside end portions of the semiconductor layer in a channel length direction of the transistor, and the functional layer has an etching rate in one etchant slower than an etching rate of the conductive layer.
[0011] Another embodiment of the present invention is a semiconductor device that has a transistor, the transistor has a semiconductor layer, a first insulating layer, a metal oxide layer, a functional layer, and a conductive layer, the first insulating layer is located over the semiconductor layer, the metal oxide layer is located over the first insulating layer, the functional layer is located over the metal oxide layer, and the conductive layer is located over the functional layer, the semiconductor layer, the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer have overlapping regions, end portions of the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer are located inside end portions of the semiconductor layer in a channel length direction of the transistor, and the functional layer is etched at a slower rate in an etchant containing hydrogen peroxide than the conductive layer.
[0012] Another embodiment of the present invention is a semiconductor device including a transistor, the transistor including a semiconductor layer, a first insulating layer, a metal oxide layer, a functional layer, and a conductive layer, the first insulating layer being located over the semiconductor layer, the metal oxide layer being located over the first insulating layer, the functional layer being located over the metal oxide layer, and the conductive layer being located over the functional layer, the semiconductor layer, the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer have overlapping regions, end portions of the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer are located inside end portions of the semiconductor layer in a channel length direction of the transistor, and the functional layer has an etching rate slower than an etching rate of the conductive layer in an etchant including one or more of phosphoric acid, acetic acid, nitric acid, hydrochloric acid, and sulfuric acid.
[0013] In the above-described semiconductor device, it is preferable that the first insulating layer, the metal oxide layer, the functional layer, and the conductive layer have generally the same top surface shape.
[0014] In the above-described semiconductor device, it is preferable that the first insulating layer, the metal oxide layer and the functional layer have generally the same top surface shape, and that an end of the conductive layer is located inside an end of the first insulating layer.
[0015] In addition, in the above-mentioned semiconductor device, it is preferable that the first insulating layer and the metal oxide layer have roughly the same top surface shape, that the functional layer and the conductive layer have roughly the same top surface shape, and that an end of the conductive layer is located more inward than an end of the first insulating layer.
[0016] In the above-described semiconductor device, it is preferable that the metal oxide layer, the functional layer and the conductive layer have substantially the same top surface shape, and that an end of the conductive layer is located inside an end of the first insulating layer.
[0017] In addition, in the above-mentioned semiconductor device, it is preferable that the metal oxide layer and the functional layer have roughly the same top surface shape, the end of the conductive layer is located more inward than the end of the metal oxide layer, and the end of the metal oxide layer is located more inward than the end of the first insulating layer.
[0018] In addition, in the above-mentioned semiconductor device, it is preferable that the semiconductor layer further has a second insulating layer, the semiconductor layer has a first region that does not overlap with the first insulating layer, the second insulating layer contacts the first region, and the second insulating layer contains silicon, nitrogen, and hydrogen. Effect of the Invention
[0019] According to one embodiment of the present invention, a transistor which is less likely to have a defective shape can be provided. Alternatively, a transistor with good electrical characteristics can be provided. Alternatively, a semiconductor device with good electrical characteristics can be provided. Alternatively, a semiconductor device with stable electrical characteristics can be provided. Alternatively, a highly reliable semiconductor device can be provided. Alternatively, a highly reliable display device can be provided.
[0020] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these can be extracted from the description in the specification, drawings, claims, etc. [Brief description of the drawings]
[0021] [Figure 1] Fig. 1(A) is a top view showing a configuration example of a semiconductor device, and Figs. 1(B) and 1(C) are cross-sectional views showing the configuration example of a semiconductor device. [Diagram 2] 2A is a top view showing a configuration example of a semiconductor device, and FIGS. 2B and 2C are cross-sectional views showing the configuration example of a semiconductor device. [Diagram 3] Fig. 3(A) is a top view showing a configuration example of a semiconductor device, and Figs. 3(B) and 3(C) are cross-sectional views showing the configuration example of a semiconductor device. [Figure 4] Fig. 4(A) is a top view showing a configuration example of a semiconductor device, and Figs. 4(B) and 4(C) are cross-sectional views showing the configuration example of a semiconductor device. [Diagram 5] Fig. 5(A) is a top view showing a configuration example of a semiconductor device, and Figs. 5(B) and 5(C) are cross-sectional views showing the configuration example of a semiconductor device. [Figure 6]6A, 6B, 6C, 6D, 6E, and 6F are cross-sectional views showing examples of the configuration of a semiconductor device. [Figure 7] Fig. 7(A) is a top view showing a configuration example of a semiconductor device, and Figs. 7(B) and 7(C) are cross-sectional views showing the configuration example of a semiconductor device. [Figure 8] 8A, 8B, and 8C are cross-sectional views showing configuration examples of a semiconductor device. [Figure 9] 9A, 9B, and 9C are diagrams illustrating a method for manufacturing a semiconductor device. [Figure 10] 10A and 10B are diagrams illustrating a method for manufacturing a semiconductor device. [Figure 11] 11A and 11B are diagrams illustrating a method for manufacturing a semiconductor device. [Figure 12] 12A and 12B are diagrams illustrating a method for manufacturing a semiconductor device. [Figure 13] 13A and 13B are diagrams illustrating a method for manufacturing a semiconductor device. [Figure 14] 14A and 14B are diagrams illustrating a method for manufacturing a semiconductor device. [Figure 15] 15(A), (B), and (C) are top views of the display device. [Figure 16] FIG. 16 is a cross-sectional view of the display device. [Figure 17] FIG. 17 is a cross-sectional view of the display device. [Figure 18] FIG. 18 is a cross-sectional view of the display device. [Figure 19] FIG. 19 is a cross-sectional view of the display device. [Figure 20] Fig. 20(A) is a block diagram of a display device, and Fig. 20(B) and (C) are circuit diagrams of the display device. [Figure 21] 21A, 21C, and 21D are circuit diagrams of the display device, and FIG 21B is a timing chart of the display device. [Figure 22] 22(A) and (B) show examples of the configuration of a display module. [Diagram 23] 23(A) and (B) show configuration examples of electronic devices. [Figure 24] 24(A), (B), (C), (D), and (E) are configuration examples of electronic devices. [Diagram 25] 25(A), (B), (C), (D), (E), (F), and (G) are configuration examples of electronic devices. [Figure 26] 26(A), (B), (C), and (D) show examples of the configuration of electronic devices. [Figure 27] Figures 27(A) and (B) are cross-sectional STEM images. [Figure 28] FIG. 28 is a diagram showing the Id-Vg characteristics of a transistor. [Figure 29] Figures 29(A) and (B) are cross-sectional STEM images. [Diagram 30] FIG. 30 is a diagram showing the Id-Vg characteristics of a transistor. [Diagram 31] 31(A) and (B) are diagrams showing the cross-sectional structure of the sample. [Diagram 32] 32(A) and (B) show the results of TDS analysis. [Diagram 33] 33(A) and (B) are diagrams showing hydrogen concentrations. [Diagram 34] Fig. 34(A) is a graph showing hydrogen concentration, and Fig. 34(B) is a graph showing hydrogen concentration and carrier density. [Diagram 35] FIG. 35 is a diagram showing the Id-Vg characteristics of a transistor. [Diagram 36] FIG. 36 is a diagram showing the Id-Vg characteristics of a transistor. [Figure 37] 37(A) and (B) are diagrams showing the amount of variation in threshold voltage in a reliability test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the embodiments will be described with reference to the drawings. However, it will be easily understood by those skilled in the art that the embodiments can be implemented in many different ways, and that the modes and details can be changed in various ways without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the following embodiments.
[0023] In addition, in each figure described in this specification, the size, layer thickness, or area of each component may be exaggerated for clarity.
[0024] In addition, the ordinal numbers "first," "second," and "third" used in this specification are used to avoid confusion of components and do not limit the numbers.
[0025] In addition, in this specification, the terms indicating the position, such as "above" and "below", are used for convenience in order to explain the positional relationship between components with reference to the drawings. In addition, the positional relationship between components changes as appropriate depending on the direction in which each component is depicted. Therefore, the terms are not limited to those described in the specification, and can be rephrased appropriately depending on the situation.
[0026] In this specification and the like, the functions of a source and a drain of a transistor may be interchanged when transistors of different polarities are used, when the direction of current flow is changed during circuit operation, etc. For this reason, the terms source and drain can be used interchangeably.
[0027] In this specification, the channel length direction of a transistor refers to one of the directions parallel to the line connecting the source region and the drain region at the shortest distance. In other words, the channel length direction corresponds to one of the directions of a current flowing through a semiconductor layer when the transistor is in an on-state. The channel width direction refers to a direction perpendicular to the channel length direction. Depending on the structure and shape of the transistor, the channel length direction and the channel width direction may not be determined to be one.
[0028] In addition, in this specification, "electrical connection" includes a case where a connection is made via "something having some electrical action." Here, "something having some electrical action" is not particularly limited as long as it enables transmission and reception of an electrical signal between the connection objects. For example, "something having some electrical action" includes electrodes and wiring, as well as switching elements such as transistors, resistive elements, inductors, capacitors, and other elements having various functions.
[0029] In addition, in this specification and the like, the terms "film" and "layer" can be interchangeable. For example, the terms "conductive layer" and "insulating layer" can sometimes be interchangeable with the terms "conductive film" and "insulating film".
[0030] In this specification and the like, unless otherwise specified, the off-state current refers to the drain current when the transistor is in an off state (also called a non-conducting state or a cut-off state). Unless otherwise specified, the off-state refers to the voltage V between the gate and the source of an n-channel transistor. gs is the threshold voltage V th (For p-channel transistors, V th The term "higher" refers to a state of being.
[0031] In this specification and the like, a display panel, which is one aspect of a display device, has a function of displaying (outputting) an image or the like on a display surface. Therefore, the display panel is one aspect of an output device.
[0032] In addition, in this specification, a display panel having a connector such as an FPC (Flexible Printed Circuit) or TCP (Tape Carrier Package) attached to the substrate, or a substrate having an IC mounted thereon using a COG (Chip On Glass) method or the like, may be referred to as a display panel module, display module, or simply a display panel.
[0033] In this specification and the like, a touch panel, which is one aspect of a display device, has a function of displaying an image or the like on a display surface and a function as a touch sensor that detects that a detectable object such as a finger or a stylus touches, presses, or approaches the display surface. Thus, the touch panel is one aspect of an input / output device.
[0034] The touch panel can also be called, for example, a display panel (or display device) with a touch sensor or a display panel (or display device) with a touch sensor function. The touch panel can have a display panel and a touch sensor panel. Alternatively, the touch panel can have a function as a touch sensor inside or on the surface of the display panel.
[0035] In addition, in this specification and the like, a touch panel substrate on which a connector and / or an IC are mounted may be referred to as a touch panel module, a display module, or simply a touch panel.
[0036] (Embodiment 1) In this embodiment, a semiconductor device and a display device according to one embodiment of the present invention, and a manufacturing method thereof will be described.
[0037] One embodiment of the present invention is a transistor including a semiconductor layer in which a channel is formed on a formation surface, a gate insulating layer (also referred to as a first insulating layer) on the semiconductor layer, a functional layer on the gate insulating layer, and a conductive layer (also referred to as a first conductive layer) functioning as a gate electrode on the functional layer. The semiconductor layer preferably contains a metal oxide (hereinafter also referred to as an oxide semiconductor) that exhibits semiconductor characteristics.
[0038] It is preferable to use a low-resistance material for the conductive layer. By using a low-resistance material for the conductive layer, parasitic resistance can be reduced, and a transistor having a high on-current can be obtained, and a semiconductor device having a high on-current can be obtained. Furthermore, in a large display device or a high-definition display device, signal delay can be suppressed by reducing the wiring resistance, and high-speed driving can be achieved. Copper, silver, gold, aluminum, or the like can be used for the conductive layer. Copper is particularly preferable because of its excellent mass productivity.
[0039] When the edge of the layer on which the conductive layer is formed is located inside the edge of the conductive layer, that is, when an undercut occurs, the coverage of the layer formed later is reduced, and defects such as step discontinuities and voids occur in the layer. Shape defects such as undercuts may cause defects such as variations in the electrical characteristics of transistors.
[0040] In one embodiment of the present invention, a functional layer is provided as a layer on which a conductive layer is formed, and an etching rate of an etchant used for processing the conductive layer is approximately the same as or slower than that of the conductive layer. With such a structure, occurrence of undercut can be suppressed, and a transistor with less tendency to have a defective shape can be obtained. In addition, a transistor with good electrical characteristics can be obtained.
[0041] In addition, it is preferable to use a material for the functional layer that has high adhesion to the conductive layer, which can prevent an etchant from penetrating between the functional layer and the conductive layer during formation of the functional layer and the conductive layer, thereby preventing the generation of voids.
[0042] A more specific example will be described below with reference to the drawings.
[0043] <Configuration example 1> FIG. 1A is a top view of a transistor 100, FIG. 1B corresponds to a cross-sectional view of a cut surface taken along dashed line A1-A2 in FIG. 1A, and FIG. 1C corresponds to a cross-sectional view of a cut surface taken along dashed line B1-B2 in FIG. 1A. Note that FIG. 1A omits some of the components of the transistor 100 (such as a protective layer). The dashed line A1-A2 direction corresponds to the channel length direction, and the dashed line B1-B2 direction corresponds to the channel width direction. Note that, as with FIG. 1A, the top views of the transistors in the following drawings are also illustrated with some of the components omitted.
[0044] The transistor 100 is provided over a substrate 102 and includes an insulating layer 103, a semiconductor layer 108, an insulating layer 110, a metal oxide layer 114, a functional layer 113, a conductive layer 112, an insulating layer 116, an insulating layer 118, and the like. The island-shaped semiconductor layer 108 is provided over the insulating layer 103. The insulating layer 110 is provided to cover part of an upper surface of the insulating layer 103 and part of an upper surface of the semiconductor layer 108. The metal oxide layer 114, the functional layer 113, and the conductive layer 112 are stacked in this order over the insulating layer 110 and have portions that overlap with the semiconductor layer 108.
[0045] The insulating layer 110, the metal oxide layer 114, the functional layer 113 and the conductive layer 112 are processed so that their top surface shapes roughly match each other.
[0046] In this specification, the phrase "top surface shapes roughly match" refers to at least a portion of the contours of stacked layers overlapping. For example, this includes cases where the upper and lower layers are processed using the same mask pattern, or where a portion of the mask pattern is the same. However, strictly speaking, the contours may not overlap, and the edge of the upper layer may be located inside the edge of the lower layer, or the edge of the upper layer may be located outside the edge of the lower layer. In this case, the phrase "top surface shapes roughly match" is also used.
[0047] The insulating layer 116 is provided to cover the top surface and side surfaces of the conductive layer 112, the side surfaces of the functional layer 113, the side surfaces of the metal oxide layer 114, the side surfaces of the insulating layer 110, the top surface and side surfaces of the semiconductor layer 108, and the top surface of the insulating layer 103. The insulating layer 118 is provided to cover the insulating layer 116. The insulating layer 116 and the insulating layer 118 function as protective layers and can suppress diffusion of impurity elements from the outside.
[0048] Part of the functional layer 113 and the conductive layer 112 function as a gate electrode. Part of the insulating layer 110 functions as a gate insulating layer. The transistor 100 is a so-called top-gate transistor in which a gate electrode is provided over the semiconductor layer .
[0049] 1A and 1B, the transistor 100 may have a conductive layer 120a and a conductive layer 120b over the insulating layer 118. The conductive layer 120a and the conductive layer 120b function as a source electrode and a drain electrode. The conductive layer 120a and the conductive layer 120b are electrically connected to a region 108N described later through an opening 141a and an opening 141b provided in the insulating layer 118 and the insulating layer 116, respectively.
[0050] The semiconductor layer 108 preferably comprises a metal oxide.
[0051] For example, the semiconductor layer 108 preferably contains indium, an element M (wherein the element M is one or more elements selected from gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium), and zinc. In particular, the element M is preferably one or more elements selected from aluminum, gallium, yttrium, and tin.
[0052] In particular, it is preferable to use an oxide containing indium, gallium, and zinc for the semiconductor layer 108.
[0053] The semiconductor layer 108 may have a stacked structure in which layers with different compositions, layers with different crystallinity, or layers with different impurity concentrations are stacked.
[0054] One or more materials selected from copper, silver, gold, and aluminum can be used for the conductive layer 112. Copper is particularly preferable because it has low resistance and is suitable for mass production.
[0055] The metal oxide layer 114 located between the insulating layer 110 and the functional layer 113 functions as a barrier film that prevents oxygen contained in the insulating layer 110 from diffusing toward the conductive layer 112. Furthermore, the metal oxide layer 114 also functions as a barrier film that prevents hydrogen and water contained in the conductive layer 112 from diffusing toward the insulating layer 110. The metal oxide layer 114 can be made of a material that is less permeable to oxygen and hydrogen than the insulating layer 110, for example.
[0056] The metal oxide layer 114 can prevent oxygen from diffusing from the insulating layer 110 to the conductive layer 112, even when the conductive layer 112 is made of a metal material that easily absorbs oxygen, such as aluminum or copper. Even when the conductive layer 112 contains hydrogen, the metal oxide layer 114 can prevent hydrogen from diffusing from the conductive layer 112 to the semiconductor layer 108 through the insulating layer 110. As a result, the carrier density in the channel formation region of the semiconductor layer 108 can be made extremely low.
[0057] An insulating material or a conductive material can be used for the metal oxide layer 114. When the metal oxide layer 114 has insulating properties, it functions as a part of the gate insulating layer. On the other hand, when the metal oxide layer 114 has conductive properties, it functions as a part of the gate electrode.
[0058] It is preferable to use an insulating material having a higher dielectric constant than silicon oxide as the metal oxide layer 114. In particular, it is preferable to use an aluminum oxide film, a hafnium oxide film, a hafnium aluminate film, or the like, because the driving voltage can be reduced.
[0059] A conductive oxide such as indium oxide, indium tin oxide (ITO), or silicon-containing indium tin oxide (ITSO) can also be used as the metal oxide layer 114. In particular, a conductive oxide containing indium is preferable because of its high conductivity.
[0060] In addition, it is preferable to use an oxide material containing one or more elements that are the same as those of the semiconductor layer 108 for the metal oxide layer 114. In particular, it is preferable to use an oxide semiconductor material that can be used for the semiconductor layer 108. In this case, it is preferable to use a metal oxide film formed using the same sputtering target as that for the semiconductor layer 108 for the metal oxide layer 114, because this allows the use of a common device.
[0061] Alternatively, when a metal oxide material containing indium and gallium is used for both the semiconductor layer 108 and the metal oxide layer 114, it is preferable to use a material with a higher gallium composition (content) than the semiconductor layer 108 because the blocking property against oxygen can be further improved. In this case, by using a material with a higher indium composition than the metal oxide layer 114 for the semiconductor layer 108, the field-effect mobility of the transistor 100 can be increased.
[0062] The metal oxide layer 114 is preferably formed using a sputtering apparatus. For example, when an oxide film is formed using a sputtering apparatus, oxygen can be suitably added to the insulating layer 110 and the semiconductor layer 108 by forming the oxide film in an atmosphere containing oxygen gas.
[0063] It is preferable that a conductive material having oxidation resistance is used for the functional layer 113 located between the metal oxide layer 114 and the conductive layer 112. By using a material having oxidation resistance, it is possible to prevent the resistance of the functional layer 113 from increasing.
[0064] In addition, the etching rate of the metal oxide layer 114 and the functional layer 113 in an etchant used to process the conductive layer 112 is preferably the same as or slower than that of the conductive layer 112 .
[0065] When the etching rate of the metal oxide layer 114 and the functional layer 113 is faster than that of the conductive layer 112, undercuts are likely to occur in which the ends of the metal oxide layer 114 and the functional layer 113 are located inside the ends of the conductive layer 112. When undercuts occur, the coverage of the insulating layers 116 and 118 formed later decreases, causing defects such as discontinuities and low-density regions (also called voids) in the insulating layers 116 and 118.
[0066] In one embodiment of the present invention, the etching rates of the metal oxide layer 114 and the functional layer 113 are set to be approximately the same as or slower than the conductive layer 112, whereby occurrence of undercut can be suppressed and a transistor that is less likely to have a defective shape can be obtained. In addition, a transistor with favorable electrical characteristics can be obtained.
[0067] Moreover, the functional layer 113, the metal oxide layer 114, and the conductive layer 112 can be formed in the same process by using the etchant used in processing the conductive layer 112. Furthermore, the top surface shapes of the metal oxide layer 114, the functional layer 113, and the conductive layer 112 can be made to roughly match each other.
[0068] The etching rate of the insulating layer 110 is preferably slower than that of the metal oxide layer 114, the functional layer 113, and the conductive layer 112. By configuring the insulating layer 110 so that the etching rate is slower than that of the metal oxide layer 114, the functional layer 113, and the conductive layer 112, the amount of the insulating layer 110 that is etched during the formation of the metal oxide layer 114, the functional layer 113, and the conductive layer 112 can be reduced.
[0069] In addition, the functional layer 113 preferably has high adhesion to the metal oxide layer 114 and the conductive layer 112. For example, when the conductive layer 112 is formed on the metal oxide layer 114 and the adhesion between these layers is low, an etchant may enter between the metal oxide layer 114 and the conductive layer 112 when the metal oxide layer 114 and the conductive layer 112 are formed, and a gap may be generated between the metal oxide layer 114 and the conductive layer 112. In one embodiment of the present invention, by providing the functional layer 113 between the metal oxide layer 114 and the conductive layer 112, the adhesion between the metal oxide layer 114, the functional layer 113, and the conductive layer 112 is improved, and the generation of a gap between these layers can be suppressed, so that a transistor with a shape defect that is unlikely to occur can be obtained. In addition, a transistor with good electrical characteristics can be obtained.
[0070] In addition, it is preferable that the functional layer 113 releases a small amount of impurities having hydrogen. Examples of impurities having hydrogen include hydrogen and water. When an impurity having hydrogen is released from the functional layer 113 and the hydrogen reaches the channel formation region of the semiconductor layer 108, the hydrogen is bonded to oxygen in the channel formation region and is released as water, causing oxygen vacancies (hereinafter, V O In addition, oxygen vacancies (V O ) and hydrogen, oxygen vacancies (V O ) with hydrogen (hereafter referred to as V O H) may be formed. O H may be a carrier generation source and may adversely affect the electrical characteristics and reliability of a transistor. By using the functional layer 113 that releases a small amount of impurities containing hydrogen, good electrical characteristics and reliability can be obtained.
[0071] Moreover, it is preferable that the functional layer 113 releases a small amount of oxygen-containing impurities. Examples of oxygen-containing impurities include oxygen and water. When oxygen-containing impurities are released from the functional layer 113, the resistance of the conductive layer 112 may increase if the oxygen reaches the conductive layer 112. By using a functional layer 113 that releases a small amount of oxygen-containing impurities, it is possible to prevent the resistance of the conductive layer 112 from increasing.
[0072] Metal oxides can be used as the functional layer 113. For example, oxides containing indium, such as indium oxide, indium tin oxide (ITO), and indium tin oxide containing silicon (ITSO), can be used. ITSO is particularly preferable because it is difficult to crystallize due to the inclusion of silicon, and has high flatness, which increases the adhesion to a film formed on ITSO. Metal oxides such as indium zinc oxide, zinc oxide, and zinc oxide containing gallium can also be used.
[0073] Also, as the functional layer 113, an oxide having indium, element M (element M is one or more selected from gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, or magnesium), and zinc can be used. In particular, element M is preferably one or more selected from aluminum, gallium, yttrium, or tin. For example, in In-Ga-Zn oxide, the atomic ratio of In is greater than the atomic ratio of Ga, which is preferable because it increases the conductivity. In particular, the atomic ratio of In, element M, and Zn in the functional layer 113 is preferably In:M:Zn=4:2:3 or nearby. Alternatively, the atomic ratio of In, M, and Zn is preferably In:M:Zn=5:1:6 or nearby. Furthermore, the composition of the semiconductor layer 108 may be such that the atomic ratio of In, the element M, and Zn in the semiconductor layer 108 is approximately equal. That is, the semiconductor layer 108 may include a material in which the atomic ratio of In, the element M, and Zn is In:M:Zn=1:1:1 or a material in the vicinity thereof.
[0074] Furthermore, the functional layer 113 can be made of a metal such as aluminum, titanium, chromium, nickel, copper, yttrium, zirconium, molybdenum, silver, tantalum, or tungsten, or an alloy containing these as a main component.
[0075] The functional layer 113 is preferably made of a material different from the metal oxide layer 114 and the conductive layer 112. In this specification and the like, a different material refers to a material having different constituent elements, or a material having the same constituent elements but different composition. Even if the metal oxide layer 114 has low adhesion to the conductive layer 112, by providing the functional layer 113 having a material different from that of the metal oxide layer 114 between the metal oxide layer 114 and the conductive layer 112, the adhesion to the metal oxide layer 114 and the conductive layer 112 can be increased.
[0076] The functional layer 113 may have a structure in which two or more layers of the above-mentioned materials are laminated.
[0077] The semiconductor layer 108 has a channel formation region overlapping with the conductive layer 112 with the insulating layer 110 interposed therebetween. The semiconductor layer 108 also has a pair of regions 108N that sandwich the channel formation region. The region 108N is a region of the semiconductor layer 108 that does not overlap with either the conductive layer 112 or the insulating layer 110 and is in contact with the insulating layer 116.
[0078] The region 108N can also be referred to as a region having a lower resistance than the channel formation region, a region with a high carrier density, a region with a high oxygen defect density, a region with a high impurity concentration, or an n-type region.
[0079] The region 108N is a region that contains an impurity element (hereinafter, referred to as a first element). Examples of the first element include hydrogen, boron, carbon, nitrogen, fluorine, phosphorus, sulfur, arsenic, aluminum, magnesium, and rare gases. Representative examples of rare gases include helium, neon, argon, krypton, and xenon. In particular, it is preferable that the region 108N contains boron, phosphorus, magnesium, or aluminum. The region 108N may contain two or more of these elements.
[0080] It is preferable to use an oxide film for the insulating layer 103 and the insulating layer 110 in contact with the channel formation region of the semiconductor layer 108. For example, an oxide film such as a silicon oxide film, a silicon oxynitride film, or an aluminum oxide film can be used. As a result, oxygen desorbed from the insulating layer 103 or the insulating layer 110 during heat treatment or the like in the manufacturing process of the transistor 100 can be supplied to the channel formation region of the semiconductor layer 108, thereby reducing oxygen vacancies in the semiconductor layer 108. Although the insulating layer 110 and the insulating layer 103 are shown as having a single-layer structure in FIGS. 1B and 1C, each of them may have a stacked structure of two or more layers.
[0081] In addition, the insulating layer 103 preferably has a stacked structure of a nitride film and an oxide film on the nitride film. For example, silicon nitride, silicon nitride oxide, aluminum nitride, aluminum nitride oxide, or the like can be used as the nitride film. By providing a nitride film on the lower side of the insulating layer 103, it is possible to suppress the diffusion of impurities from a layer below the insulating layer 103 to a layer above the insulating layer 103. In addition, by providing an oxide film on the upper side of the insulating layer 103 in contact with the channel formation region, oxygen desorbed from the insulating layer 103 can be supplied to the channel formation region. For example, the insulating layer 103 can have a stacked structure of a silicon nitride film and a silicon oxynitride film on the silicon nitride film.
[0082] In this specification and the like, an oxynitride refers to a substance whose composition contains more oxygen than nitrogen, and an oxynitride is included in the category of oxides. A nitride oxide refers to a substance whose composition contains more nitrogen than oxygen, and a nitride oxide is included in the category of nitrides.
[0083] An end portion of the insulating layer 110 is located over the semiconductor layer 108. The insulating layer 110 overlaps with the conductive layer 112 and has a region which functions as a gate insulating layer.
[0084] Here, it is preferable that the impurity concentration in the region 108N has a concentration gradient such that the concentration becomes higher closer to the insulating layer 116. This allows the total amount of the first element in the region 108N to be lower than when the concentration is uniform throughout the region 108N, and therefore the amount of impurities that may diffuse into the channel formation region due to the influence of heat during the manufacturing process can be kept low. In addition, since the resistance becomes lower toward the upper part of the region 108N, the contact resistance with the conductive layer 120a (or the conductive layer 120b) can be more effectively reduced.
[0085] As described later, the process of doping the region 108N with the first impurity element can be performed using the insulating layer 110 as a mask, thereby allowing the region 108N to be formed in a self-aligned manner.
[0086] The region 108N has an impurity concentration of 1×10 19 atoms / cm 3 That's it, 1×10 23 atoms / cm 3 Less than or equal to 5×10 19 atoms / cm 3 That's it, 5 x 10 22 atoms / cm 3 Less than or equal to 1×10 20 atoms / cm 3 That's it, 1×10 22 atoms / cm 3 It is preferred to include a region in which:
[0087] The concentration of impurities contained in the region 108N can be analyzed by, for example, secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), etc. When XPS analysis is used, the concentration distribution in the depth direction can be known by combining ion sputtering from the front side or rear side with XPS analysis.
[0088] In addition, in the region 108N, the first element is preferably present in an oxidized state. For example, it is preferable to use an element that is easily oxidized, such as boron, phosphorus, magnesium, aluminum, or silicon, as the first element. Since such an element that is easily oxidized can be stably present in an oxidized state by bonding with oxygen in the semiconductor layer 108, even if a high temperature (for example, 400° C. or higher, 600° C. or higher, or 800° C. or higher) is applied in a later process, desorption is suppressed. Furthermore, the first element removes oxygen from the semiconductor layer 108, and many oxygen vacancies are generated in the region 108N. These oxygen vacancies bond with hydrogen in the film to become a carrier supply source, and the region 108N becomes in an extremely low resistance state.
[0089] In addition, when a high-temperature process is performed in a later step, if a large amount of oxygen is supplied to region 108N from the outside or a film in the vicinity of region 108N, the resistance may increase. Therefore, when performing a high-temperature process, it is preferable to perform the process in a state where semiconductor layer 108 is covered with insulating layer 116 that has a high barrier property against oxygen.
[0090] The insulating layer 116 is provided in contact with a region 108N of the semiconductor layer 108.
[0091] The insulating layer 116 functions as a hydrogen supply source for the region 108N. For example, the insulating layer 116 is preferably a film that releases hydrogen when heated. By providing such an insulating layer 116 in contact with the region 108N and performing a heat treatment after the formation of the insulating layer 116, hydrogen can be supplied to the region 108N to reduce the resistance.
[0092] The insulating layer 116 is preferably formed by using a deposition gas containing hydrogen elements, so that hydrogen can be effectively supplied to the region 108N during the deposition of the insulating layer 116.
[0093] The insulating layer 116 can be, for example, an insulating film made of silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum nitride, aluminum nitride oxide, or the like.
[0094] As described above, the region 108N is in a state where it contains many oxygen vacancies due to the addition of the first element. Therefore, by supplying hydrogen from the insulating layer 116 in addition to the hydrogen contained in the semiconductor layer 108, the carrier density can be further increased.
[0095] The insulating layer 118 functions as a protective layer that protects the transistor 100. For example, an inorganic insulating material such as an oxide or a nitride can be used as the insulating layer 118. More specific examples of the insulating layer 118 that can be used include inorganic insulating materials such as silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum oxide, aluminum oxynitride, aluminum nitride, hafnium oxide, and hafnium aluminate. The insulating layer 118 can also be used as a planarization layer. In that case, an organic resin material can be used as the insulating layer 118.
[0096] Although the protective layer has a stacked structure of the insulating layer 116 and the insulating layer 118 in this embodiment, the insulating layer 118 does not have to be provided if it is not necessary. The insulating layer 118 may have a stacked structure of two or more layers.
[0097] Here, the semiconductor layer 108 and oxygen vacancies that may be formed in the semiconductor layer 108 will be described.
[0098] Oxygen vacancies formed in the channel formation region of the semiconductor layer 108 affect transistor characteristics and are therefore problematic. For example, when oxygen vacancies are formed in the semiconductor layer 108, hydrogen bonds to the oxygen vacancies and they can become carrier sources. When a carrier source is generated in the channel formation region, the electrical characteristics of the transistor 100 fluctuate, typically causing a shift in the threshold voltage. Therefore, it is preferable to have fewer oxygen vacancies in the channel formation region.
[0099] Thus, in one embodiment of the present invention, an insulating film in the vicinity of a channel formation region of the semiconductor layer 108, specifically, the insulating layer 110 located above the channel formation region and the insulating layer 103 located below the channel formation region, includes an oxide film. By transferring oxygen from the insulating layer 103 and the insulating layer 110 to the channel formation region by heat or the like during a manufacturing process, oxygen vacancies in the channel formation region can be reduced.
[0100] The semiconductor layer 108 preferably has a region in which the atomic ratio of In to the element M is greater than 1. The higher the In content, the more the field-effect mobility of the transistor can be improved.
[0101] Here, in the case of metal oxides containing In, Ga, and Zn, the bonding strength between In and oxygen is weaker than that between Ga and oxygen, so oxygen vacancies are likely to be formed in the metal oxide film when the In content is high. The same tendency is observed when a metal element represented by M is used instead of Ga. If many oxygen vacancies exist in the metal oxide film, the electrical characteristics and reliability of the transistor are degraded.
[0102] However, in one embodiment of the present invention, a metal oxide material with a high In content can be used because an extremely large amount of oxygen can be supplied to the channel formation region of the semiconductor layer 108 containing a metal oxide. As a result, a transistor having extremely high field-effect mobility, stable electrical characteristics, and high reliability can be realized.
[0103] For example, metal oxides in which the atomic ratio of In to element M is 1.5 or more, or 2 or more, or 3 or more, or 3.5 or more, or 4 or more can be suitably used.
[0104] In particular, the atomic ratio of In, M, and Zn in the semiconductor layer 108 is preferably In:M:Zn=4:2:3 or nearby. Alternatively, the atomic ratio of In, M, and Zn is preferably In:M:Zn=5:1:6 or nearby. Furthermore, the composition of the semiconductor layer 108 may be such that the atomic ratio of In, M, and Zn in the semiconductor layer 108 is approximately equal. That is, the semiconductor layer 108 may contain a material in which the atomic ratio of In, M, and Zn is In:M:Zn=1:1:1 or nearby.
[0105] For example, by using the transistor with high field-effect mobility in a gate driver that generates a gate signal, a display device with a narrow frame width (also called a narrow frame) can be provided. In addition, by using the transistor with high field-effect mobility in a source driver (particularly, a demultiplexer connected to an output terminal of a shift register of the source driver), a display device with a small number of wirings connected to the display device can be provided.
[0106] Even if the semiconductor layer 108 has a region in which the atomic ratio of In to the element M is greater than 1, the field-effect mobility may be reduced if the semiconductor layer 108 has high crystallinity. The crystallinity of the semiconductor layer 108 can be analyzed, for example, by X-ray diffraction (XRD) or a transmission electron microscope (TEM).
[0107] Here, the carrier density in the channel formation region of the semiconductor layer 108 can be reduced by lowering the impurity concentration and the defect state density (reducing oxygen vacancies). A transistor using such a metal oxide film for a channel formation region of the semiconductor layer rarely has electrical characteristics in which the threshold voltage is negative (also referred to as normally-on). In addition, a transistor using such a metal oxide film can have a significantly small off-current.
[0108] When a metal oxide film with high crystallinity is used for the semiconductor layer 108, damage during processing of the semiconductor layer 108 or during deposition of the insulating layer 110 can be suppressed, and a highly reliable transistor can be realized. On the other hand, when a metal oxide film with relatively low crystallinity is used for the semiconductor layer 108, electrical conductivity is improved, and a transistor with high field-effect mobility can be realized.
[0109] As the semiconductor layer 108, it is preferable to use a metal oxide film having a c-axis aligned crystal (CAAC) structure, a metal oxide film having a nano crystal (nc) structure, or a metal oxide film having a mixture of the CAAC structure and the nc structure, which will be described later.
[0110] The semiconductor layer 108 may have a stacked structure of two or more layers.
[0111] For example, a semiconductor layer 108 in which two or more metal oxide films having different compositions are stacked can be used. For example, when an In-M-Zn oxide is used, it is preferable to stack two or more films formed from a sputtering target in which the atomic ratio of In, M, and Zn is In:M:Zn=5:1:6, In:M:Zn=4:2:3, In:M:Zn=1:1:1, In:M:Zn=2:2:1, In:M:Zn=1:3:4, In:M:Zn=1:3:2, or a ratio close to these values.
[0112] Alternatively, a semiconductor layer 108 in which two or more metal oxide films with different crystallinity are stacked can be used. In that case, it is preferable to use the same oxide target and to form the films successively under different film formation conditions without exposure to air.
[0113] In this case, the semiconductor layer 108 may have a stacked structure of a metal oxide film having an nc structure and a metal oxide film having a CAAC structure. Alternatively, the semiconductor layer 108 may have a stacked structure of a metal oxide film having an nc structure and a metal oxide film having an nc structure. Note that the function or material configuration of metal oxides that can be suitably used for each metal oxide film can be referenced in the description of CAC (Cloud-Aligned Composite) described later.
[0114] For example, the oxygen flow ratio during the formation of the first metal oxide film is set to be smaller than the oxygen flow ratio during the formation of the second metal oxide film. Alternatively, oxygen is not allowed to flow during the formation of the first metal oxide film. This allows oxygen to be effectively supplied during the formation of the second metal oxide film. In addition, the first metal oxide film can be a film with lower crystallinity and higher electrical conductivity than the second metal oxide film. On the other hand, by making the second metal oxide film provided on the upper portion a film with higher crystallinity than the first metal oxide film, damage during processing of the semiconductor layer 108 and during the formation of the insulating layer 110 can be suppressed.
[0115] More specifically, the oxygen flow ratio during deposition of the first metal oxide film is 0% or more and less than 50%, preferably 0% or more and 30% or less, more preferably 0% or more and 20% or less, and typically 10%. The oxygen flow ratio during deposition of the second metal oxide film is 50% or more and 100% or less, preferably 60% or more and 100% or less, more preferably 80% or more and 100% or less, further preferably 90% or more and 100% or less, and typically 100%. Although the conditions during deposition of the first metal oxide film and the second metal oxide film, such as pressure, temperature, and power, may be different, it is preferable to make the conditions other than the oxygen flow ratio the same, since this shortens the time required for the deposition process.
[0116] With this structure, a transistor 100 with excellent electrical characteristics and high reliability can be realized.
[0117] The following describes a configuration example of a transistor that is partially different from the above-mentioned configuration example 1. Note that, in the following, a description of parts that overlap with the above-mentioned configuration example 1 may be omitted. Also, in the drawings shown below, parts that have the same functions as the above-mentioned configuration example 1 may be indicated with the same hatching pattern and may not be assigned reference numerals.
[0118] <Configuration example 2> 2A is a top view of the transistor 100A, FIG. 2B is a cross-sectional view of the transistor 100A in the channel length direction, and FIG. 2C is a cross-sectional view of the transistor 100A in the channel width direction.
[0119] The transistor 100A differs from the first structural example mainly in that a conductive layer 106 is provided between the substrate 102 and the insulating layer 103. The conductive layer 106 has a channel formation region of the semiconductor layer 108 and a region overlapping with the functional layer 113 and the conductive layer 112.
[0120] In the transistor 100A, the conductive layer 106 functions as a first gate electrode (also referred to as a bottom gate electrode), and the functional layer 113 and the conductive layer 112 function as a second gate electrode (also referred to as a top gate electrode). Part of the insulating layer 103 functions as a first gate insulating layer, and part of the insulating layer 110 functions as a second gate insulating layer.
[0121] A portion of the semiconductor layer 108 overlapping with at least one of the functional layer 113, the conductive layer 112, and the conductive layer 106 functions as a channel formation region. Note that for ease of explanation, the portion of the semiconductor layer 108 overlapping with the functional layer 113 and the conductive layer 112 may be referred to as a channel formation region hereinafter; however, in reality, a channel may also be formed in a portion that does not overlap with the functional layer 113 and the conductive layer 112 but overlaps with the conductive layer 106 (a portion including the region 108N).
[0122] 2A and 2C, the conductive layer 106 may be electrically connected to the functional layer 113 and the conductive layer 112 through the metal oxide layer 114, the insulating layer 110, and the opening 142 provided in the insulating layer 103. This allows the conductive layer 106, the functional layer 113, and the conductive layer 112 to be supplied with the same potential.
[0123] The conductive layer 106 can be formed using a material similar to that of the conductive layer 112, the conductive layer 120a, or the conductive layer 120b. In particular, it is preferable to use a material containing copper for the conductive layer 106 because the wiring resistance can be reduced. Furthermore, if a material containing a high melting point metal such as tungsten or molybdenum is used for the conductive layer 106, processing can be performed at a high temperature in a later step.
[0124] 2(A) and 2(C), in the channel width direction, the functional layer 113, the conductive layer 112, and the conductive layer 106 preferably protrude outward beyond the end portion of the semiconductor layer 108. In this case, as shown in FIG. 2(C), the entire semiconductor layer 108 in the channel width direction is covered with the functional layer 113, the conductive layer 112, and the conductive layer 106 via the insulating layer 110 and the insulating layer 103.
[0125] With such a structure, the semiconductor layer 108 can be electrically surrounded by an electric field generated by the pair of gate electrodes. In particular, it is preferable to apply the same potential to the conductive layer 106, the functional layer 113, and the conductive layer 112. This makes it possible to effectively apply an electric field for inducing a channel in the semiconductor layer 108, thereby increasing the on-state current of the transistor 100A. This also enables miniaturization of the transistor 100A.
[0126] Note that the functional layer 113 and the conductive layer 112 may not be connected to the conductive layer 106. In this case, a constant potential may be applied to one of a pair of gate electrodes, and a signal for driving the transistor 100A may be applied to the other. In this case, the threshold voltage when the transistor 100A is driven by the other electrode can also be controlled by the potential applied to one electrode.
[0127] This concludes the description of configuration example 2.
[0128] <Configuration example 3> 3A is a top view of the transistor 100B, FIG. 3B is a cross-sectional view of the transistor 100B in the channel length direction, and FIG. 3C is a cross-sectional view of the transistor 100B in the channel width direction.
[0129] The transistor 100B differs from Configuration Example 1 mainly in that an end of the conductive layer 112 is located inside an end of the insulating layer 110. In other words, the insulating layer 110 has a portion that protrudes outward from the end of the conductive layer 112 at least on the semiconductor layer 108. Moreover, the insulating layer 110, the metal oxide layer 114, and the functional layer 113 have top surface shapes that roughly match each other.
[0130] As shown in Figures 3(B) and 3(C), the thickness of the functional layer 113 in the area that does not overlap with the conductive layer 112 may be thinner than the thickness of the functional layer 113 in the area that overlaps with the conductive layer 112.
[0131] The insulating layer 116 is provided to cover the upper and side surfaces of the conductive layer 112, the side surfaces of the functional layer 113, the side surfaces of the metal oxide layer 114, the side surfaces of the insulating layer 110, the upper and side surfaces of the semiconductor layer 108, and the upper surface of the insulating layer 103.
[0132] This concludes the description of configuration example 3.
[0133] <Configuration Example 4> 4A is a top view of a transistor 100C, FIG. 4B is a cross-sectional view of the transistor 100C in a channel length direction, and FIG. 4C is a cross-sectional view of the transistor 100C in a channel width direction.
[0134] The transistor 100C differs from Configuration Example 1 mainly in that the ends of the conductive layer 112 and the functional layer 113 are located inside the ends of the insulating layer 110. In other words, the insulating layer 110 has a portion that protrudes outward from the ends of the conductive layer 112 and the functional layer 113 at least on the semiconductor layer 108. The conductive layer 112 and the functional layer 113 have top surface shapes that roughly match each other. The insulating layer 110 and the metal oxide layer 114 have top surface shapes that roughly match each other.
[0135] As shown in Figures 4(B) and 4(C), the thickness of the metal oxide layer 114 in the region that does not overlap with the conductive layer 112 may be thinner than the thickness of the metal oxide layer 114 in the region that overlaps with the conductive layer 112 and the functional layer 113.
[0136] The semiconductor layer 108 has a pair of regions 108L sandwiching a channel formation region therebetween, and a pair of regions 108N outside the pair of regions 108L. The region 108L is a region of the semiconductor layer 108 that overlaps with the insulating layer 110 but does not overlap with the conductive layer 112. The region 108L can be called an offset region.
[0137] The region 108L can also be referred to as a region having the same or lower resistance, the same or higher carrier density, the same or higher oxygen defect density, or the same or higher impurity concentration compared to the channel formation region.
[0138] Region 108L can also be said to be a region having the same or higher resistance, the same or lower carrier density, the same or lower oxygen defect density, or the same or lower impurity concentration compared to region 108N.
[0139] The carrier density in the region 108L may not be uniform, and may have a gradient such that the carrier density decreases from the region 108N side to the channel formation region. For example, either one or both of the hydrogen concentration and the oxygen vacancy concentration in the region 108L may have a gradient such that the concentration decreases from the region 108N side to the channel formation region side.
[0140] A portion of an end of the insulating layer 110 is located on the semiconductor layer 108. The insulating layer 110 has a region that overlaps with the conductive layer 112 and functions as a gate insulating layer, and a portion that does not overlap with the conductive layer 112 (i.e., a portion that overlaps with the region 108L).
[0141] The insulating layer 116 is provided to cover the upper surface and side surfaces of the conductive layer 112, the side surfaces of the functional layer 113, the side surfaces of the metal oxide layer 114, the side surfaces of the insulating layer 110, the upper surface and side surfaces of the semiconductor layer 108, and the upper surface of the insulating layer 103. Since the insulating layer 110 is present between the region 108L and the insulating layer 110, the region 108L is not in contact with the insulating layer 116, and therefore less hydrogen is supplied to the region 108L than to the region 108N. Furthermore, the impurity concentration is also lower than that of the region 108N, and therefore the region 108L can be made to have a higher resistance than the region 108N.
[0142] As described later, the region 108L can be formed in a self-aligned manner, so that a photomask for forming the region 108L is not required, and the manufacturing cost can be reduced. Furthermore, by forming the region 108L in a self-aligned manner, the relative positional deviation between the region 108L and the functional layer 113 and the conductive layer 112 does not occur, so that the width of the region 108L in the semiconductor layer 108 can be approximately the same.
[0143] The region 108L where the electric field of the gate is not applied (or is applied less than the channel formation region) can be formed stably without variation in the region other than the low-resistance region 108N in the semiconductor layer 108. As a result, the source-drain breakdown voltage of the transistor can be improved, and a highly reliable transistor can be realized. The width of the region 108L is set to 10 nm or more and 10 μm or less, preferably 30 nm or more and 5 μm or less, and more preferably 50 nm or more and 1 μm or less. If the width of the region 108L in the channel length direction is long, the effective channel length becomes long, and the driving speed of the transistor may become slow. By setting the width as described above, a transistor with a high driving speed can be obtained.
[0144] When a conductive material is used for the metal oxide layer 114, an electric field of the gate is applied to the semiconductor layer 108 in the region overlapping with the metal oxide layer 114, and therefore the region 108L is not formed.
[0145] This concludes the description of configuration example 4.
[0146] <Configuration Example 5> 5A is a top view of a transistor 100D, FIG. 5B is a cross-sectional view of the transistor 100D in a channel length direction, and FIG. 5C is a cross-sectional view of the transistor 100D in a channel width direction.
[0147] The transistor 100D differs from Configuration Example 1 mainly in that the ends of the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are located inside the end of the insulating layer 110. In other words, the insulating layer 110 has a portion that protrudes outward from the ends of the conductive layer 112, the functional layer 113, and the metal oxide layer 114 at least on the semiconductor layer 108. In addition, the conductive layer 112, the functional layer 113, and the metal oxide layer 114 have top surface shapes that roughly match each other.
[0148] The insulating layer 116 is provided to cover the top surface and side surfaces of the conductive layer 112, the side surfaces of the functional layer 113, the side surfaces of the metal oxide layer 114, the top surface and side surfaces of the insulating layer 110, the top surface and side surfaces of the semiconductor layer 108, and the top surface of the insulating layer 103. The insulating layer 118 is provided to cover the insulating layer 116. An enlarged view of the region surrounded by a dashed line in FIG. 5B is shown in FIG. 6A.
[0149] The semiconductor layer 108 has a pair of regions 108L sandwiching a channel formation region, and a pair of regions 108N outside the pair of regions 108L. The region 108L, to which the electric field of the gate is not applied (or is less applied than the channel formation region), can be formed stably without variation in the region other than the low-resistance region 108N in the semiconductor layer 108. As a result, the source-drain breakdown voltage of the transistor can be improved, and a highly reliable transistor can be realized. In addition, by providing the region 108L between the channel formation region and the low-resistance region 108N, the current density at the boundary between the channel formation region and the region 108N can be reduced, and heat generation at the boundary between the channel and the source or drain can be suppressed, resulting in a highly reliable semiconductor device.
[0150] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, a part of the insulating layer 110 that does not overlap with the conductive layer 112 may be etched, and the thickness of the insulating layer 110 may become thinner. Specifically, as shown in FIG 6B, the thickness of the insulating layer 110 in a region that does not overlap with the conductive layer 112 may become thinner than the thickness of the insulating layer 110 in a region that overlaps with the conductive layer 112. In other words, the thickness of the insulating layer 110 in a region that does not overlap with the channel formation region may become thinner than the thickness of the insulating layer 110 in a region that overlaps with the channel formation region.
[0151] Although the insulating layer 110 is shown as a single-layer structure in Fig. 5(B), Fig. 5(C), Fig. 6(A) and Fig. 6(B), it may be a laminated structure of two or more layers. Fig. 6(C) shows an example in which the insulating layer 110 has a two-layer structure of an insulating layer 110a and an insulating layer 110b on the insulating layer 110a. Note that since the insulating layers 110a and 110b can be made of insulating films of the same material, the interface between the insulating layers 110a and 110b may not be clearly visible. Therefore, in this embodiment, the interface between the insulating layers 110a and 110b is shown by a dashed line.
[0152] The insulating layer 110a in contact with the channel formation region of the semiconductor layer 108 preferably has a low defect density near the interface with the channel formation region and in the film. The insulating layer 110a preferably has a low concentration of impurities containing hydrogen in the film. The insulating layer 110a preferably causes little damage to the semiconductor layer 108 when the insulating layer 110a is formed. By using a film with a low defect density and impurity concentration for the insulating layer 110a and using film formation conditions that cause little damage to the semiconductor layer 108, a transistor with good electrical characteristics can be obtained.
[0153] For example, when a film containing silicon is used as the insulating layer 110, the insulating layer 110a can be formed under deposition conditions in which the ratio of silicon-containing gas to deposition gas used during deposition is low. By using deposition conditions in which the ratio of silicon-containing gas to deposition gas is low, the insulating layer 110a can be formed with a low defect density and impurity concentration. In addition, by reducing the deposition power during the formation of the insulating layer 110a, damage to the semiconductor layer 108 can be reduced.
[0154] The insulating layer 110 b in contact with the metal oxide layer 114 preferably has an etching rate in an etchant used to process the conductive layer 112 that is approximately the same as or slower than that of the conductive layer 112 .
[0155] It is preferable that the insulating layer 110b is a film denser than the insulating layer 110a. The dense insulating layer 110b can be formed under film formation conditions that result in a slower film formation rate than the insulating layer 110a. Furthermore, the dense insulating layer 110b is suppressed from adsorbing water to its surface. In other words, by providing the insulating layer 110b on the upper surface of the insulating layer 110, it is possible to suppress adsorption of water to the surface of the insulating layer 110.
[0156] When water is adsorbed on the surface of the insulating layer 110, and hydrogen contained in the adsorbed water reaches the channel formation region, carriers are formed in the channel formation region, which may adversely affect the electrical characteristics and reliability of the transistor. By providing the insulating layer 110b, which is less likely to adsorb water, on the upper surface of the insulating layer 110, carrier formation in the channel formation region can be suppressed, and good electrical characteristics and reliability can be obtained.
[0157] The insulating layer 110b can be formed under film formation conditions that provide a slower film formation rate than the insulating layer 110a. For example, when a film containing silicon is used as the insulating layer 110, the insulating layer 110b can be formed under conditions that provide a lower ratio of silicon-containing gas to the film formation gas used during film formation. Furthermore, compared to the insulating layer 110a, the insulating layer 110b can be formed as an insulating layer that is less likely to adsorb water by increasing the film formation power during film formation.
[0158] It is preferable that the insulating layer 110b has a slower etching rate in one etchant than the insulating layer 110a. The insulating layer 110b may have a higher film density than the insulating layer 110a. The difference in film density between the insulating layer 110a and the insulating layer 110b can be evaluated, for example, by the density (brightness) of a TEM image.
[0159] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, the thickness of the insulating layer 110b in a region that does not overlap with the conductive layer 112 may be thin. As shown in FIG 6D, it is preferable that the insulating layer 110b remain in a region that does not overlap with the conductive layer 112. By having the insulating layer 110b remain in a region that does not overlap with the conductive layer 112, water can be prevented from being adsorbed to the insulating layer 110.
[0160] The insulating layer 110b in the region overlapping with the conductive layer 112 is preferably formed to a thickness such that the insulating layer 110b remains in a region not overlapping with the conductive layer 112. The thickness of the insulating layer 110b in the region overlapping with the conductive layer 112 is set to 1 nm to 50 nm, preferably 2 nm to 40 nm, and more preferably 3 nm to 30 nm.
[0161] 6(E) shows an example in which the insulating layer 110 has a three-layer structure including an insulating layer 110a, an insulating layer 110b on the insulating layer 110a, and an insulating layer 110c between the insulating layers 110a and 110b. Since the insulating layers 110a, 110b, and 110c can be made of insulating films made of the same material, the interfaces between the insulating layers 110a, 110b, and 110c may not be clearly visible. Therefore, in this embodiment, the interfaces between the insulating layers 110a, 110b, and 110c are shown by dashed lines.
[0162] The insulating layer 110c can be formed under conditions that provide a faster deposition rate than the insulating layers 110a and 110b. By using the insulating layer 110c with a faster deposition rate, the insulating layer 110 having a stacked structure can be formed with high productivity.
[0163] For example, when a film containing silicon is used as the insulating layer 110, the insulating layer 110c can be formed under conditions in which the ratio of a silicon-containing gas to a deposition gas is higher than those of the insulating layers 110a and 110b. The insulating layer 110c can be formed as an insulating layer with fewer impurities by increasing the power during deposition. Furthermore, the insulating layer 110c can be formed as an insulating layer with fewer impurities by increasing the pressure during deposition.
[0164] The insulating layer 110c preferably has an etching rate in one etchant faster than the insulating layers 110a and 110b. The insulating layer 110c may have a lower film density than the insulating layers 110a and 110b. The difference in film density between the insulating layers 110a, 110b, and 110c may be evaluated by, for example, the density (brightness) of a TEM image. The insulating layer 110c may have a higher hydrogen concentration in the film than the insulating layers 110a and 110b. The difference in hydrogen concentration between the insulating layers 110a, 110b, and 110c may be evaluated by, for example, secondary ion mass spectrometry.
[0165] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, the thickness of the insulating layer 110b in a region that does not overlap with the conductive layer 112 may be thin. As shown in FIG 6F, it is preferable that the insulating layer 110b remain in the region that does not overlap with the conductive layer 112. By having the insulating layer 110b remain in the region that does not overlap with the conductive layer 112, adsorption of water to the insulating layer 110 can be suppressed.
[0166] 7(A), 7(B), and 7(C), the end of the conductive layer 112 may be located inside the end of the functional layer 113 and the metal oxide layer 114. Fig. 7(A) is a top view of the transistor 100E, Fig. 7(B) is a cross-sectional view of the transistor 100E in the channel length direction, and Fig. 7(C) is a cross-sectional view of the transistor 100E in the channel width direction.
[0167] The transistor 100E is mainly different from the configuration example 1 in that the ends of the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are located inside the ends of the insulating layer 110, and the ends of the conductive layer 112 are located inside the ends of the functional layer 113 and the metal oxide layer 114. In other words, the insulating layer 110 has a portion that protrudes outward from the ends of the conductive layer 112, the functional layer 113, and the metal oxide layer 114 at least on the semiconductor layer 108. Furthermore, the functional layer 113 and the metal oxide layer 114 have a portion that protrudes outward from the ends of the conductive layer 112 at least on the insulating layer 110. Furthermore, the functional layer 113 and the metal oxide layer 114 have upper surface shapes that are approximately the same as each other.
[0168] By using a material for the conductive layer 112 that has an etching rate in an etchant used to process the conductive layer 112 faster than those of the metal oxide layer 114 and the functional layer 113, the end of the conductive layer 112 can be configured to be located inside the ends of the functional layer 113 and the metal oxide layer 114.
[0169] The insulating layer 116 is provided so as to cover the upper surface and side surfaces of the conductive layer 112, the upper surface and side surfaces of the functional layer 113, the side surfaces of the metal oxide layer 114, the upper surface and side surfaces of the insulating layer 110, the upper surface and side surfaces of the semiconductor layer 108, and the upper surface of the insulating layer 103. The insulating layer 118 is provided so as to cover the insulating layer 116.
[0170] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, a part of the insulating layer 110 that does not overlap with the conductive layer 112 may be etched, and the thickness of the insulating layer 110 may become thinner. FIG. 8A shows an enlarged view of a region surrounded by a dashed line in FIG. 7B. As shown in FIG. 8A, the thickness of the insulating layer 110 in a region that does not overlap with the conductive layer 112 may be thinner than the thickness of the insulating layer 110 in a region that overlaps with the conductive layer 112. In other words, the thickness of the insulating layer 110 in a region that does not overlap with the channel formation region may be thinner than the thickness of the insulating layer 110 in a region that overlaps with the channel formation region.
[0171] In Fig. 7(B), Fig. 7(C) and Fig. 8(A), the insulating layer 110 is shown as a single layer structure, but it may be a laminated structure of two or more layers. Fig. 8(B) shows an example in which the insulating layer 110 has a two-layer structure of an insulating layer 110a and an insulating layer 110b on the insulating layer 110a. Fig. 8(C) shows an example in which the insulating layer 110 has a three-layer structure of an insulating layer 110a, an insulating layer 110b on the insulating layer 110a, and an insulating layer 110c between the insulating layer 110a and the insulating layer 110b.
[0172] When the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, the thickness of the insulating layer 110b in a region that does not overlap with the conductive layer 112 may be thin. Furthermore, as shown in Figures 8B and 8C, it is preferable that the insulating layer 110b remain in the region that does not overlap with the conductive layer 112. By using a structure in which the insulating layer 110b remains in the region that does not overlap with the conductive layer 112, adsorption of water to the insulating layer 110 can be suppressed.
[0173] Also, in the above-described transistors 100, 100A, 100B, and 100C, the insulating layer 110 is preferably formed to have a stacked structure. By forming the insulating layer 110 to have a two-layer structure of the insulating layer 110a and the insulating layer 110b on the insulating layer 110a, water can be prevented from being adsorbed on the surface of the insulating layer 110, and good electrical characteristics and reliability can be obtained. Furthermore, by forming the insulating layer 110 to have a three-layer structure of the insulating layer 110a, the insulating layer 110b on the insulating layer 110a, and the insulating layer 110c between the insulating layer 110a and the insulating layer 110b, the insulating layer 110 having a stacked structure can be formed with high productivity.
[0174] This concludes the description of configuration example 5.
[0175] <Production method example 1> A method for manufacturing a semiconductor device according to one embodiment of the present invention will be described below with reference to the drawings. Here, the transistor 100A given in the above structure example will be used as an example.
[0176] The thin films (insulating film, semiconductor film, conductive film, etc.) constituting the semiconductor device can be formed by sputtering, chemical vapor deposition (CVD), vacuum deposition, pulsed laser deposition (PLD), atomic layer deposition (ALD), etc. CVD methods include plasma enhanced chemical vapor deposition (PECVD) and thermal CVD. One type of thermal CVD method is metal organic chemical vapor deposition (MOCVD).
[0177] Furthermore, thin films (insulating films, semiconductor films, conductive films, etc.) constituting a semiconductor device can be formed using methods such as spin coating, dipping, spray coating, inkjet, dispensing, screen printing, offset printing, etc., and tools (equipment) such as doctor knife, slit coating, roll coating, curtain coating, knife coating, etc.
[0178] Furthermore, when processing the thin film constituting the semiconductor device, the thin film can be processed using a photolithography method or the like. Alternatively, the thin film may be processed using a nanoimprint method, a sandblasting method, a lift-off method or the like. Furthermore, an island-shaped thin film may be directly formed by a film formation method using a shielding mask such as a metal mask.
[0179] There are two typical photolithography methods. One is a method in which a resist mask is formed on the thin film to be processed, the thin film is processed by etching or the like, and the resist mask is then removed. The other is a method in which a photosensitive thin film is formed, and then exposed and developed to process the thin film into the desired shape.
[0180] In the photolithography method, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. In addition, ultraviolet light, KrF laser light, ArF laser light, or the like may be used. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure. Extreme ultraviolet light, X-rays, or an electron beam are preferable because they enable extremely fine processing. When exposure is performed by scanning a beam such as an electron beam, a photomask is not required.
[0181] For etching the thin film, a dry etching method, a wet etching method, a sandblasting method, or the like can be used.
[0182] 9 to 11 show cross sections of the transistor 100A at various stages in a manufacturing process thereof. In each of the drawings, a cross section in the channel length direction is shown on the left side of a central dashed line, and a cross section in the channel width direction is shown on the right side.
[0183] [Formation of Conductive Layer 106] A conductive film is formed over the substrate 102 and processed by etching to form a conductive layer 106 that functions as a first gate electrode.
[0184] [Formation of insulating layer 103] Subsequently, the insulating layer 103 is formed to cover the substrate 102 and the conductive layer 106 (FIG. 9(A)). The insulating layer 103 can be formed by using a PECVD method, an ALD method, a sputtering method, or the like.
[0185] When the insulating layer 103 has a stacked structure, insulating films that become the insulating layer 103 are formed in order. When the insulating layer 103 has a stacked structure of, for example, a nitride film and an oxide film over the nitride film, the nitride film and the oxide film are formed in this order.
[0186] The nitride film included in the insulating layer 103 may have a stacked structure of two or more layers. In the case where the insulating layer 103 has a stacked structure of, for example, a first silicon nitride film, a second silicon nitride film on the first silicon nitride film, a third silicon nitride film on the second silicon nitride film, and a silicon oxynitride film on the third silicon nitride film, the first silicon nitride film, the second silicon nitride film, the third silicon nitride film, and the silicon oxynitride film are formed in this order.
[0187] When the insulating layer 103 has a stacked structure of a first silicon nitride film, a second silicon nitride film, a third silicon nitride film, and a silicon oxynitride film, the first silicon nitride film preferably has a function of blocking impurities. By providing the first silicon nitride film, it is possible to suppress the diffusion of impurities from a layer below the insulating layer 103 to a layer above the insulating layer 103. It is preferable that the second silicon nitride film has low stress and high dielectric strength. By providing the second silicon nitride film, it is possible to obtain the insulating layer 103 with low stress and high dielectric strength. It is preferable that the third silicon nitride film has a function of blocking impurities containing hydrogen that are little released. By providing the third silicon nitride film, it is possible to suppress the diffusion of hydrogen into the channel formation region. It is preferable that the silicon oxynitride film has low defect density and little release of impurities containing hydrogen.
[0188] For example, the insulating layer 103 is formed by a plasma CVD method using a mixed gas of silane, nitrogen, and ammonia, forming a first silicon nitride film having a function of blocking impurities. Next, a mixed gas having a higher ammonia flow rate than the first silicon nitride film is used to form a second silicon nitride film having a low stress and a high dielectric strength. Next, a mixed gas having a lower ammonia flow rate than the second silicon nitride film is used to form a third silicon nitride film having a function of blocking impurities having hydrogen and releasing less impurities having hydrogen. Next, a mixed gas of silane and dinitrogen monoxide is used to form a silicon oxynitride film having a low defect density and releasing less impurities having hydrogen, thereby forming the insulating layer 103. In addition, by switching the film forming conditions in the same chamber, the first silicon nitride film, the second silicon nitride film, the third silicon nitride film, and the silicon oxynitride film can be continuously formed in a vacuum, and the insulating layer 103 can be formed with high productivity.
[0189] Alternatively, after forming the third silicon nitride film, a plasma treatment can be performed in an atmosphere containing oxygen to oxidize the surface of the third silicon nitride film, thereby forming a silicon oxynitride film on the third silicon nitride film.
[0190] The second silicon nitride film may have a lower film density than the first silicon nitride film and the third silicon nitride film. The difference in film density among the first silicon nitride film, the second silicon nitride film, and the third silicon nitride film may be evaluated, for example, by the concentration (brightness) of a TEM image. Furthermore, the second silicon nitride film may have a higher hydrogen concentration than the first silicon nitride film and the third silicon nitride film. The difference in hydrogen concentration among the first silicon nitride film, the second silicon nitride film, and the third silicon nitride film may be evaluated, for example, by secondary ion mass spectrometry.
[0191] After the insulating layer 103 is formed, a treatment for supplying oxygen to the insulating layer 103 may be performed. For example, a plasma treatment or a heat treatment in an oxygen atmosphere can be performed. Alternatively, oxygen may be supplied to the insulating layer 103 by a plasma ion doping method, an ion implantation method, or the like. Note that the heat treatment is not necessarily performed after the insulating layer 103 is formed.
[0192] [Formation of Semiconductor Layer 108] Subsequently, a metal oxide film is formed on the insulating layer 103, and then processed to form island-shaped semiconductor layers 108 (FIG. 9(B)).
[0193] The metal oxide film is preferably formed by a sputtering method using a metal oxide target.
[0194] In addition, oxygen gas and an inert gas (e.g., helium gas, argon gas, xenon gas, etc.) may be mixed when forming the metal oxide film. Note that the higher the ratio of oxygen gas to the total deposition gas when forming the metal oxide film (hereinafter, also referred to as the oxygen flow ratio), the higher the crystallinity of the metal oxide film can be, and a highly reliable transistor can be realized. On the other hand, the lower the oxygen flow ratio, the lower the crystallinity of the metal oxide film can be, and a transistor with increased on-current can be obtained.
[0195] When the semiconductor layer 108 has a stacked structure, it is preferable to deposit the films successively in the same deposition chamber using the same sputtering target, since this can improve the interface. In particular, the deposition conditions for each metal oxide film may be different in terms of pressure, temperature, power, and the like during deposition, but it is preferable to keep the conditions other than the oxygen flow rate the same, since this can shorten the time required for the deposition process. In addition, when metal oxide films with different compositions are stacked, it is preferable to deposit the films successively without exposing them to the air.
[0196] It is preferable to set the deposition conditions so that the metal oxide film is a metal oxide film having a CAAC structure, a metal oxide film having an nc structure, or a metal oxide film having a mixture of the CAAC structure and the nc structure. Since the deposition conditions under which the metal oxide film to be deposited has a CAAC structure and the deposition conditions under which the metal oxide film has an nc structure vary depending on the composition of the sputtering target used, the substrate temperature, oxygen flow rate ratio, pressure, power, and the like may be appropriately set according to the composition.
[0197] The deposition conditions for the metal oxide film are a substrate temperature of room temperature or higher and 450° C. or lower, preferably room temperature or higher and 300° C. or lower, more preferably room temperature or higher and 200° C. or lower, and further preferably room temperature or higher and 140° C. or lower. For example, when a large glass substrate or a resin substrate is used as the substrate 102, it is preferable to set the substrate temperature to room temperature or higher and lower than 140° C., as this increases productivity. The crystallinity can be reduced by depositing the metal oxide film at room temperature or without heating the substrate.
[0198] Furthermore, before forming the metal oxide film, it is preferable to perform a treatment for removing water, hydrogen, organic components, and the like adsorbed on the surface of the insulating layer 103, and a treatment for supplying oxygen into the insulating layer 103. For example, heat treatment can be performed at a temperature of 70° C. or higher and 200° C. or lower in a reduced pressure atmosphere. Alternatively, plasma treatment may be performed in an atmosphere containing oxygen. Furthermore, when plasma treatment is performed in an atmosphere containing nitric oxide gas, organic substances on the surface of the insulating layer 103 can be suitably removed. After such a treatment, it is preferable to continuously form a metal oxide film without exposing the surface of the insulating layer 103 to the air.
[0199] The metal oxide film may be processed by wet etching or dry etching, or both of them may be used. At this time, a part of the insulating layer 103 that does not overlap with the semiconductor layer 108 may be etched and become thinner.
[0200] After the metal oxide film is formed or after it is processed into the semiconductor layer 108, heat treatment may be performed to remove hydrogen or water in the metal oxide film or the semiconductor layer 108. The temperature of the heat treatment can be typically set to 150° C. or higher and lower than the distortion point of the substrate, or 250° C. or higher and 450° C. or lower, or 300° C. or higher and 450° C. or lower. Note that the heat treatment does not have to be performed after the metal oxide film is formed or after it is processed into the semiconductor layer 108. The heat treatment may be performed at any stage after the metal oxide film is formed. Alternatively, the heat treatment may be performed together with a later heat treatment or a step in which heat is applied.
[0201] The heat treatment can be performed in an atmosphere containing a rare gas or nitrogen. Alternatively, the heat treatment can be performed in the atmosphere containing a rare gas or nitrogen, and then in an atmosphere containing oxygen. As the atmosphere containing nitrogen or the atmosphere containing oxygen, ultra dry air (CDA: Clean Dry Air) can be used. Note that it is preferable that the atmosphere for the heat treatment does not contain hydrogen, water, or the like. By using a gas that has been highly purified to a dew point of −60° C. or less, preferably −100° C. or less, it is possible to prevent hydrogen, water, or the like from being taken into the semiconductor layer 108 as much as possible. The heat treatment can be performed using an electric furnace, a rapid thermal annealing (RTA: Rapid Thermal Annealing) device, or the like. By using an RTA device, the heat treatment time can be shortened.
[0202] It is preferable to form the insulating film 110f promptly after forming the semiconductor layer 108. When the surface of the semiconductor layer 108 is exposed, water may be adsorbed onto the surface of the semiconductor layer 108. When water is adsorbed onto the surface of the semiconductor layer 108, hydrogen is diffused into the semiconductor layer 108 by a subsequent heat treatment or the like, and V O H may be formed. V O Since H can be a carrier generation source, it is preferable that the amount of adsorbed water in the semiconductor layer 108 is small.
[0203] [Formation of insulating film 110f and metal oxide film 114f] Subsequently, an insulating film 110f and a metal oxide film 114f are formed to cover the insulating layer 103 and the semiconductor layer .
[0204] The insulating film 110f is a film that will later become the insulating layer 110. As the insulating film 110f, it is preferable to form an oxide film such as a silicon oxide film or a silicon oxynitride film using a plasma enhanced chemical vapor deposition apparatus (PECVD apparatus, or simply called a plasma CVD apparatus). Alternatively, it may be formed using a PECVD method using microwaves.
[0205] When the insulating layer 110 has a laminated structure, the insulating films that become the insulating layer 110 are formed in order. For example, as shown in Fig. 6(C), Fig. 6(D) and Fig. 8(B), when the insulating layer 110 has a two-layer structure of insulating layer 110a and insulating layer 110b, the insulating film that becomes insulating layer 110a and the insulating film that becomes insulating layer 110b are formed in this order.
[0206] For example, the insulating layer 110 is formed by forming an insulating film that will become the insulating layer 110a by a plasma CVD method using a mixed gas of silane and dinitrogen monoxide. Next, an insulating film that will become the insulating layer 110b is formed under conditions of lower pressure and higher power than those for the insulating film that will become the insulating layer 110a, thereby forming the insulating layer 110. Also, by switching the film formation conditions in the same chamber, the insulating film that will become the insulating layer 110a and the insulating film that will become the insulating layer 110b can be formed successively in a vacuum, and the insulating layer 110 can be formed with high productivity.
[0207] Furthermore, as shown in Figures 6(E), 6(F) and 8(C), when insulating layer 110 has a three-layer structure of insulating layer 110a, insulating layer 110c and insulating layer 110b, an insulating film that will become insulating layer 110a, an insulating film that will become insulating layer 110c, and an insulating film that will become insulating layer 110b are formed in this order.
[0208] For example, the insulating layer 110 is formed by a plasma CVD method using a mixed gas of silane and dinitrogen monoxide to form an insulating film that will become the insulating layer 110a. Next, an insulating film that will become the insulating layer 110c is formed under high power conditions using a mixed gas having a higher silane flow rate ratio to dinitrogen monoxide flow rate than the insulating film that will become the insulating layer 110a. Next, an insulating film that will become the insulating layer 110b is formed under low pressure conditions using a mixed gas having a lower silane flow rate ratio to dinitrogen monoxide flow rate than the insulating film that will become the insulating layer 110c, thereby forming the insulating layer 110. Also, by switching the film formation conditions in the same chamber, the insulating film that will become the insulating layer 110a, the insulating film that will become the insulating layer 110c, and the insulating film that will become the insulating layer 110b can be formed continuously in a vacuum, and the insulating layer 110 can be formed with high productivity.
[0209] After the insulating film 110f is formed, impurities in the insulating film 110f and adsorbed water on the surface of the insulating film 110f may be removed by performing a heat treatment. The heat treatment may be performed at a temperature of 200° C. or more and 400° C. or less in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas. Note that the heat treatment does not have to be performed after the insulating film 110f is formed. The heat treatment may be performed at any stage after the insulating film 110f is formed. The heat treatment may also be performed together with a later heat treatment or a process in which heat is applied.
[0210] The metal oxide film 114f is a film that will later become the metal oxide layer 114. The metal oxide film 114f is preferably formed by, for example, a sputtering method in an atmosphere containing oxygen, which allows oxygen to be supplied to the insulating film 110f during the formation of the metal oxide film 114f.
[0211] When the metal oxide film 114f is formed by a sputtering method using an oxide target containing a metal oxide similar to that for the semiconductor layer 108, the above method can be used.
[0212] The metal oxide film 114f may be formed by reactive sputtering using oxygen as a deposition gas and a metal target. When aluminum is used as the metal target, an aluminum oxide film can be formed.
[0213] During the formation of the metal oxide film 114f, the higher the ratio of the oxygen flow rate to the total flow rate of the film formation gas introduced into the film formation chamber of the film formation apparatus (oxygen flow rate ratio) or the higher the oxygen partial pressure in the film formation chamber, the more oxygen can be supplied to the insulating film 110f. The oxygen flow rate ratio or oxygen partial pressure is, for example, 50% to 100%, preferably 65% to 100%, more preferably 80% to 100%, and even more preferably 90% to 100%. In particular, it is preferable to set the oxygen flow rate ratio to 100% and the oxygen partial pressure as close to 100% as possible.
[0214] In this manner, by forming the metal oxide film 114f by a sputtering method in an atmosphere containing oxygen, oxygen can be supplied to the insulating film 110f during the formation of the metal oxide film 114f, and oxygen can be prevented from being released from the insulating film 110f. As a result, an extremely large amount of oxygen can be trapped in the insulating film 110f. Then, a large amount of oxygen is supplied to the channel formation region of the semiconductor layer 108 by a subsequent heat treatment, and oxygen vacancies in the channel formation region can be reduced, thereby realizing a highly reliable transistor.
[0215] The deposition conditions for the metal oxide film 114f may be such that the substrate temperature is from room temperature to 450° C., preferably from room temperature to 300° C., more preferably from room temperature to 200° C., and even more preferably from room temperature to 140° C. When a large glass substrate or a resin substrate is used as the substrate 102, for example, the deposition temperature is preferably from room temperature to less than 140° C., since this increases productivity. If the deposition temperature for the metal oxide film 114f is high, the crystallinity of the metal oxide film 114f may increase, and the etching rate may become slow. If the deposition temperature for the metal oxide film 114f is low, the crystallinity of the metal oxide film 114f may decrease, and the etching rate may become fast. The deposition temperature for the metal oxide film 114f may be appropriately selected so that the etching rate is desirable for the etchant used to process the metal oxide film 114f.
[0216] After the metal oxide film 114f is formed, heat treatment may be performed so that oxygen is supplied from the insulating film 110f to the semiconductor layer 108. The heat treatment may be performed in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas at a temperature of 200° C. to 400° C. Note that the heat treatment does not necessarily have to be performed after the metal oxide film 114f is formed. The heat treatment may be performed at any stage after the formation of the metal oxide film 114f. Alternatively, the heat treatment may be performed together with a later heat treatment or a step in which heat is applied.
[0217] Next, the metal oxide film 114f, the insulating film 110f, and a part of the insulating layer 103 are etched to form an opening reaching the conductive layer 106 (FIG. 9C). This allows the functional layer 113 and the conductive layer 112, which will be formed later, to be electrically connected to the conductive layer 106 through the opening.
[0218] [Formation of functional film 113f and conductive film 112f] Next, a functional film 113f to be the functional layer 113 and a conductive film 112f to be the conductive layer 112 are formed on the metal oxide film 114f (FIG. 10(A)). The functional film 113f is preferably formed by a sputtering method using a sputtering target of a metal or alloy. The conductive film 112f is preferably formed by a sputtering method using a sputtering target of a metal or alloy.
[0219] [Formation of insulating layer 110, metal oxide layer 114, and conductive layer 112] Next, a resist mask 115 is formed over the conductive film 112f. After that, in the region not covered with the resist mask 115, the conductive film 112f, the functional film 113f, and the metal oxide film 114f are removed to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114 (FIG. 10B).
[0220] A wet etching method can be suitably used to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114. For example, an etchant containing hydrogen peroxide can be used for the wet etching method. For example, an etchant containing one or more of phosphoric acid, acetic acid, nitric acid, hydrochloric acid, and sulfuric acid can be used. In particular, when a material containing copper is used for the conductive layer 112, an etchant containing phosphoric acid, acetic acid, and nitric acid can be suitably used.
[0221] In one embodiment of the present invention, the etching rates of the metal oxide layer 114 and the functional layer 113 are approximately the same as or slower than that of the conductive layer 112, so that the functional layer 113, the metal oxide layer 114, and the conductive layer 112 can be formed in the same process. Furthermore, the top surfaces of the metal oxide layer 114, the functional layer 113, and the conductive layer 112 can be made to roughly match each other. Moreover, since they can be formed in the same process, the process can be simplified and productivity can be increased.
[0222] During the formation of the conductive layer 112, the functional layer 113, and the metal oxide layer 114, the conductive layer 112 may be recessed from the functional layer 113 and the metal oxide layer 114. That is, an end of the conductive layer 112 is located inside an end of the metal oxide layer 114. Furthermore, as the conductive layer 112 is recessed from the functional layer 113 and the metal oxide layer 114, the thickness of the functional layer 113 in a region that does not overlap with the conductive layer 112 may be thinner than the thickness of the functional layer 113 in a region that overlaps with the conductive layer 112 (see FIGS. 3(A), 3(B), and 3(C)).
[0223] Furthermore, when the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are formed, the conductive layer 112 and the functional layer 113 may be recessed from the metal oxide layer 114. That is, the ends of the conductive layer 112 and the functional layer 113 are located inside the ends of the metal oxide layer 114. Furthermore, as the conductive layer 112 and the functional layer 113 are recessed from the metal oxide layer 114, the thickness of the metal oxide layer 114 in a region that does not overlap with the conductive layer 112 may be thinner than the thickness of the metal oxide layer 114 in a region that overlaps with the conductive layer 112 and the functional layer 113 (see FIG. 4(A), FIG. 4(B), and FIG. 4(C)).
[0224] The conductive layer 112, the functional layer 113, and the metal oxide layer 114 may be formed by etching at least twice using different etching conditions or techniques. For example, the conductive film 112f may be etched first, and then the functional film 113f and the metal oxide film 114f may be etched under different etching conditions.
[0225] Next, the insulating film 110f is removed from the region not covered with the resist mask 115 to form the insulating layer 110 (FIG. 11(A)). The insulating layer 110 can be formed by using either or both of a wet etching method and a dry etching method. Note that the insulating layer 110 may be formed in a state where the resist mask 115 is removed, but by leaving the resist mask 115, the thickness of the conductive layer 112 can be prevented from becoming thin.
[0226] After the insulating layer 110 is formed, the resist mask 115 is removed.
[0227] [Formation of insulating layer 116 and region 108N (hydrogen supply process)] Next, a process of supplying hydrogen to the exposed region of the semiconductor layer 108 is performed. Here, hydrogen is supplied by forming an insulating layer 116 containing hydrogen in contact with the exposed region of the semiconductor layer 108 (FIG. 11B).
[0228] The insulating layer 116 is preferably formed by a plasma CVD method using a deposition gas containing hydrogen. For example, a silicon nitride film is formed using a deposition gas containing silane gas and ammonia gas. By using ammonia gas in addition to silane gas, a large amount of hydrogen can be contained in the film. Also, hydrogen can be supplied to the exposed portion of the semiconductor layer 108 during the film formation.
[0229] After the insulating layer 116 is formed, heat treatment is preferably performed so that part of hydrogen released from the insulating layer 116 is supplied to part of the semiconductor layer 108. The heat treatment is preferably performed in an atmosphere containing one or more of nitrogen, oxygen, and a rare gas at a temperature of 150° C. to 450° C., preferably 200° C. to 400° C.
[0230] By supplying hydrogen in this manner, an extremely low resistance region 108N can be formed in the semiconductor layer 108.
[0231] Furthermore, oxygen can be supplied from the insulating layer 110 to the channel formation region of the semiconductor layer 108 by the heat treatment.
[0232] [Formation of insulating layer 118] Subsequently, an insulating layer 118 is formed on the insulating layer 116 (FIG. 12(A)).
[0233] When the insulating layer 118 is formed by the plasma CVD method, if the deposition temperature is too high, depending on the impurities contained in the region 108N, the impurities may diffuse to the peripheral portion including the channel formation region of the semiconductor layer 108. As a result, the resistance of the channel formation region may decrease, or the resistance of the region 108N may increase. The deposition temperature of the insulating layer 116 or the insulating layer 118 is preferably, for example, 150° C. or more and 400° C. or less, preferably 180° C. or more and 360° C. or less, and more preferably 200° C. or more and 250° C. or less. By depositing the insulating layer 118 at a low temperature, good electrical characteristics can be imparted even to a transistor with a short channel length.
[0234] After the insulating layer 118 is formed, heat treatment may be performed.
[0235] [Formation of Openings 141a and 141b] Next, a mask is formed by lithography at desired positions on the insulating layer 118, and then parts of the insulating layer 118 and the insulating layer 116 are etched to form the openings 141a and 141b that reach the region 108N.
[0236] [Formation of Conductive Layer 120a and Conductive Layer 120b] Subsequently, a conductive film is formed over the insulating layer 118 so as to cover the openings 141a and 141b, and the conductive film is processed into a desired shape to form the conductive layers 120a and 120b (FIG. 12B).
[0237] Through the above steps, the transistor 100A can be manufactured.
[0238] <Production method example 2> A method for manufacturing a semiconductor device according to one embodiment of the present invention will be described below with reference to the drawings. Here, the transistor 100D illustrated in the above structure example will be described as an example. Note that descriptions of parts that overlap with the above will be omitted, and differences will be described.
[0239] 13A and 13B show cross sections of the transistor 100D at each stage of a manufacturing process. In each figure, a cross section in the channel length direction is shown on the left side of the central dashed line, and a cross section in the channel width direction is shown on the right side.
[0240] The steps up to the formation of the conductive film 112f are the same as those in <Manufacturing Method Example 1>. Therefore, the manufacturing method of the transistor in FIGS.
[0241] [Formation of insulating layer 110, metal oxide layer 114, and conductive layer 112] Subsequently, the conductive film 112f, the functional film 113f, and the metal oxide film 114f are etched to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114 (FIG. 13(A)).
[0242] At this time, the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are processed so that their ends are located inside the contour of the resist mask 115. A wet etching method is preferably used to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114. The width of the region 108L can be controlled by adjusting the etching time.
[0243] In addition, in forming the conductive layer 112, the functional layer 113, and the metal oxide layer 114, the conductive film 112f, the functional film 113f, and the metal oxide film 114f may be etched by anisotropic etching, and then the side surfaces of the conductive film 112f, the functional film 113f, and the metal oxide film 114f may be etched by isotropic etching to set back the end faces (also referred to as side etching). This makes it possible to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114 whose end portions are located inside the end portions of the insulating layer 110 in a plan view.
[0244] Next, the insulating film 110f is removed from the region not covered by the resist mask 115 to form the insulating layer 110 (FIG. 13(B)). The insulating layer 110 can be formed by either or both of a wet etching method and a dry etching method.
[0245] After the insulating layer 110 is formed, the resist mask 115 is removed.
[0246] The above description can be applied to the subsequent steps.
[0247] Through the above steps, the transistor 100D can be manufactured.
[0248] <Production method example 3> A method for manufacturing a semiconductor device according to one embodiment of the present invention will be described below with reference to the drawings. Here, the transistor 100E illustrated in the above configuration example will be described as an example. Note that descriptions of parts that overlap with the above will be omitted, and differences will be described.
[0249] 14A and 14B show cross sections of the transistor 100E at various stages in a manufacturing process. In each figure, a cross section in the channel length direction is shown on the left side of the central dashed line, and a cross section in the channel width direction is shown on the right side.
[0250] The steps up to the formation of the conductive film 112f are the same as those in <Manufacturing Method Example 1>. Therefore, the manufacturing method of the transistor in FIGS.
[0251] [Formation of insulating layer 110, metal oxide layer 114, and conductive layer 112] Subsequently, the conductive film 112f, the functional film 113f, and the metal oxide film 114f are etched to form the conductive layer 112, the functional layer 113, and the metal oxide layer 114 (FIG. 14(A)).
[0252] At this time, the conductive layer 112, the functional layer 113, and the metal oxide layer 114 are processed so that their ends are located inside the contour of the resist mask 115. In addition, by using a material for the conductive layer 112 that has a slower etching rate than the functional layer 113 and the metal oxide layer 114, the end of the conductive layer 112 is located inside the end of the functional layer 113 and the metal oxide layer 114. It is preferable to use a wet etching method for forming the conductive layer 112, the functional layer 113, and the metal oxide layer 114. The width of the region 108L can be controlled by adjusting the etching time.
[0253] Next, the insulating film 110f is removed from the region not covered by the resist mask 115 to form the insulating layer 110 (FIG. 14(B)). The insulating layer 110 can be formed by either or both of a wet etching method and a dry etching method.
[0254] After the insulating layer 110 is formed, the resist mask 115 is removed.
[0255] The above description can be applied to the subsequent steps.
[0256] Through the above steps, the transistor 100E can be manufactured.
[0257] <Components of Semiconductor Device> Next, components included in the semiconductor device of this embodiment will be described in detail.
[0258] 〔substrate〕 There are no significant limitations on the material of the substrate 102, but the substrate must have at least sufficient heat resistance to withstand subsequent heat treatment. For example, a single crystal semiconductor substrate made of silicon or silicon carbide, a polycrystalline semiconductor substrate, a compound semiconductor substrate such as silicon germanium, an SOI substrate, a glass substrate, a ceramic substrate, a quartz substrate, a sapphire substrate, or the like may be used as the substrate 102. Furthermore, any of these substrates on which semiconductor elements are provided may be used as the substrate 102.
[0259] Alternatively, a flexible substrate may be used as the substrate 102, and the transistor 100 and the like may be formed directly on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 102 and the transistor 100 and the like. The peeling layer can be used to separate a semiconductor device that is partially or entirely completed thereon from the substrate 102 and transfer the semiconductor device to another substrate. In this case, the transistor 100 and the like can also be transferred to a substrate with poor heat resistance or a flexible substrate.
[0260] [Insulating layer 103] The insulating layer 103 can be formed by a sputtering method, a CVD method, an evaporation method, a pulsed laser deposition (PLD) method, or the like as appropriate. For example, the insulating layer 103 can be formed of a single layer or a stack of an oxide insulating film or a nitride insulating film. Note that in order to improve the interface characteristics with the semiconductor layer 108, at least a region of the insulating layer 103 that is in contact with the semiconductor layer 108 is preferably formed of an oxide insulating film. For the insulating layer 103, a film that releases oxygen when heated is preferably used.
[0261] The insulating layer 103 may be formed using, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, hafnium oxide, gallium oxide, Ga-Zn oxide, or the like, and may be formed as a single layer or a stacked layer.
[0262] When a film other than an oxide film, such as a silicon nitride film, is used on the side of the insulating layer 103 in contact with the semiconductor layer 108, it is preferable to perform a pretreatment such as an oxygen plasma treatment on the surface in contact with the semiconductor layer 108 to oxidize the surface or the vicinity of the surface.
[0263] [Conductive Film] The conductive layer 106 and the conductive layer 112 functioning as a gate electrode, the conductive layer 120a functioning as one of the source electrode and the drain electrode, and the conductive layer 120b functioning as the other of the source electrode and the drain electrode can each be formed using a metal element selected from chromium, copper, aluminum, gold, silver, zinc, molybdenum, tantalum, titanium, tungsten, manganese, nickel, iron, and cobalt, or an alloy containing the above-mentioned metal elements or an alloy combining the above-mentioned metal elements.
[0264] In addition, the conductive layers 106, 112, 120a, and 120b may be formed using oxide conductors or metal oxide films such as In-Sn oxide, In-W oxide, In-W-Zn oxide, In-Ti oxide, In-Ti-Sn oxide, In-Zn oxide, In-Sn-Si oxide, and In-Ga-Zn oxide.
[0265] Here, an oxide conductor (OC) will be described. For example, when oxygen vacancies are formed in a metal oxide having semiconductor properties and hydrogen is added to the oxygen vacancies, a donor level is formed near the conduction band. As a result, the metal oxide becomes highly conductive and becomes a conductor. A metal oxide that has become a conductor can be called an oxide conductor.
[0266] Alternatively, the conductive layer 106 or the like may have a stacked structure of a conductive film containing the above oxide conductor (metal oxide) and a conductive film containing a metal or an alloy. By using a conductive film containing a metal or an alloy, wiring resistance can be reduced. In this case, it is preferable to use a conductive film containing an oxide conductor on the side in contact with an insulating layer that functions as a gate insulating film.
[0267] The conductive layer 106, the conductive layer 112, the conductive layer 120a, and the conductive layer 120b preferably contain one or more of the above-mentioned metal elements selected from titanium, tungsten, tantalum, and molybdenum. In particular, a tantalum nitride film is preferably used. The tantalum nitride film is conductive, has high barrier properties against copper, oxygen, or hydrogen, and releases little hydrogen from itself, and therefore can be preferably used as a conductive film in contact with the semiconductor layer 108 or in the vicinity of the semiconductor layer 108.
[0268] [Insulating layer 110] The insulating layer 110, which functions as a gate insulating film of the transistor 100 or the like, can be formed by a PECVD method, a sputtering method, or the like. The insulating layer 110 can be an insulating layer containing one or more of a silicon oxide film, a silicon oxynitride film, a silicon nitride oxide film, a silicon nitride film, an aluminum oxide film, a hafnium oxide film, a yttrium oxide film, a zirconium oxide film, a gallium oxide film, a tantalum oxide film, a magnesium oxide film, a lanthanum oxide film, a cerium oxide film, and a neodymium oxide film. Note that the insulating layer 110 may have a stacked structure of two layers or a stacked structure of three or more layers.
[0269] The insulating layer 110 in contact with the semiconductor layer 108 is preferably an oxide insulating film and more preferably has a region containing oxygen in excess of the stoichiometric composition. In other words, the insulating layer 110 is an insulating film that can release oxygen. For example, oxygen can be supplied to the insulating layer 110 by forming the insulating layer 110 in an oxygen atmosphere, performing heat treatment, plasma treatment, or the like on the insulating layer 110 after the film formation in an oxygen atmosphere, or forming an oxide film on the insulating layer 110 in an oxygen atmosphere.
[0270] Also, a material such as hafnium oxide, which has a higher dielectric constant than silicon oxide or silicon oxynitride, can be used as the insulating layer 110. This allows the insulating layer 110 to be thicker and suppresses leakage current due to tunnel current. In particular, crystalline hafnium oxide is preferable because it has a higher dielectric constant than amorphous hafnium oxide.
[0271] [Semiconductor Layer] When the semiconductor layer 108 is an In-M-Zn oxide, the sputtering target used for depositing the In-M-Zn oxide preferably has an atomic ratio of In to element M of 1 or more. Examples of atomic ratios of metal elements in such a sputtering target include In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=2:1:3, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and the like.
[0272] In addition, it is preferable to use a target containing a polycrystalline oxide as the sputtering target because it is easy to form the semiconductor layer 108 having crystallinity. The atomic ratio of the semiconductor layer 108 to be formed includes a variation of ±40% of the atomic ratio of the metal elements contained in the sputtering target. For example, when the composition of the sputtering target used for the semiconductor layer 108 is In:Ga:Zn=4:2:4.1 [atomic ratio], the composition of the semiconductor layer 108 to be formed may be close to In:Ga:Zn=4:2:3 [atomic ratio].
[0273] When the atomic ratio is described as In:Ga:Zn=4:2:3 or thereabout, this includes the case where, when In is 4, Ga is 1 or more and 3 or less, and Zn is 2 or more and 4 or less. When the atomic ratio is described as In:Ga:Zn=5:1:6 or thereabout, this includes the case where, when In is 5, Ga is greater than 0.1 and 2 or less, and Zn is greater than 5 and 7 or less. When the atomic ratio is described as In:Ga:Zn=1:1:1 or thereabout, this includes the case where, when In is 1, Ga is greater than 0.1 and 2 or less, and Zn is greater than 0.1 and 2 or less.
[0274] The energy gap of the semiconductor layer 108 is 2 eV or more, preferably 2.5 eV or more. By using a metal oxide having a wider energy gap than silicon, the off-state current of the transistor can be reduced.
[0275] In addition, the semiconductor layer 108 preferably has a non-single crystal structure. The non-single crystal structure includes, for example, a CAAC structure, a polycrystalline structure, a microcrystalline structure, or an amorphous structure, which will be described later. Among the non-single crystal structures, the amorphous structure has the highest density of defect states, and the CAAC structure has the lowest density of defect states.
[0276] In the following, we explain about CAAC (c-axis aligned crystal). CAAC is an example of a crystal structure.
[0277] The CAAC structure is one of the crystal structures of thin films having multiple nanocrystals (crystal regions with a maximum diameter of less than 10 nm), and each nanocrystal has a c-axis oriented in a specific direction, and the a-axis and b-axis have no orientation, and the nanocrystals are continuously connected to each other without forming grain boundaries. In particular, thin films having a CAAC structure have the characteristic that the c-axis of each nanocrystal is likely to be oriented in the thickness direction of the thin film, the normal direction of the surface on which it is formed, or the normal direction of the thin film surface.
[0278] CAAC-OS (Oxide Semiconductor) is an oxide semiconductor with high crystallinity. On the other hand, since no clear crystal grain boundaries can be identified in CAAC-OS, it can be said that the decrease in electron mobility caused by the crystal grain boundaries is unlikely to occur. In addition, since the crystallinity of an oxide semiconductor can be decreased by the inclusion of impurities or the generation of defects, CAAC-OS can be said to be an oxide semiconductor with few impurities and defects (such as oxygen vacancies). Therefore, oxide semiconductors with CAAC-OS have stable physical properties. Therefore, oxide semiconductors with CAAC-OS are resistant to heat and have high reliability.
[0279] In crystallography, it is common to take a unit cell with a specific axis as the c-axis out of the three axes (crystal axes) that make up the unit cell: the a-axis, the b-axis, and the c-axis. In particular, in crystals with a layered structure, it is common to take the two axes parallel to the plane direction of the layers as the a-axis and the b-axis, and the axis that intersects the layers as the c-axis. A typical example of a crystal with such a layered structure is graphite, which is classified as a hexagonal crystal system, and the a-axis and b-axis of its unit cell are parallel to the cleavage plane, and the c-axis is perpendicular to the cleavage plane. For example, YbFe 2 O 4 InGaZnO with a type crystal structure 4 The crystals can be classified as hexagonal, with the a-axis and b-axis of the unit cell being parallel to the plane of the layers and the c-axis being perpendicular to the layers (i.e., the a-axis and b-axis).
[0280] In an oxide semiconductor film having a microcrystalline structure (microcrystalline oxide semiconductor film), crystal parts may not be clearly identified in an image observed by TEM. The crystal parts included in a microcrystalline oxide semiconductor film often have a size of 1 nm to 100 nm, or 1 nm to 10 nm. In particular, an oxide semiconductor film having nanocrystals (nc), which are microcrystals having a size of 1 nm to 10 nm, or 1 nm to 3 nm, is called an nc-OS (nanocrystalline oxide semiconductor) film. In addition, in an image observed by TEM, for example, in an nc-OS film, crystal grain boundaries may not be clearly identified.
[0281] The nc-OS film has periodic atomic arrangement in a microscopic region (for example, a region of 1 nm to 10 nm, particularly a region of 1 nm to 3 nm). In addition, the nc-OS film does not show regularity in crystal orientation between different crystal parts. Therefore, no orientation is seen in the entire film. Therefore, the nc-OS film may be indistinguishable from an amorphous oxide semiconductor film depending on the analysis method. For example, when the nc-OS film is subjected to structural analysis using an XRD apparatus using X-rays with a diameter larger than that of the crystal parts, no peak indicating a crystal plane is detected in the out-of-plane analysis. When the nc-OS film is subjected to electron beam diffraction (also called selected area electron beam diffraction) using an electron beam with a probe diameter (for example, 50 nm or more) larger than that of the crystal parts, a diffraction pattern such as a halo pattern is observed. On the other hand, when electron diffraction (also known as nanobeam electron diffraction) is performed on an nc-OS film using an electron beam with a probe diameter (for example, 1 nm to 30 nm) that is close to or smaller than the size of the crystal part, a circular (ring-shaped) area of high brightness is observed, and multiple spots may be observed within that area.
[0282] The nc-OS film has a lower density of defect states than an amorphous oxide semiconductor film. However, the nc-OS film does not have regularity in the crystal orientation between different crystal parts. Therefore, the nc-OS film has a higher density of defect states than the CAAC-OS film. Therefore, the nc-OS film may have a higher carrier density and higher electron mobility than the CAAC-OS film. Therefore, a transistor using the nc-OS film may exhibit high field-effect mobility.
[0283] The nc-OS film can be formed by lowering the oxygen flow rate ratio during film formation compared to the CAAC-OS film. Also, the nc-OS film can be formed by lowering the substrate temperature during film formation compared to the CAAC-OS film. For example, the nc-OS film can be formed at a relatively low substrate temperature (for example, 130°C or lower) or without heating the substrate, making it suitable for use on large glass substrates or resin substrates, and improving productivity.
[0284] An example of the crystal structure of a metal oxide will be described. In the following, a metal oxide film formed by a sputtering method using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) will be described as an example. A metal oxide formed by a sputtering method using the above target and with a substrate temperature of 100°C to 130°C tends to have either a crystalline structure of nc (nano crystal) structure or a CAAC structure, or a mixed structure of these. On the other hand, a metal oxide formed by a sputtering method with a substrate temperature of room temperature (RT) tends to have an nc crystalline structure. Note that room temperature (RT) here includes the temperature when the substrate is not heated.
[0285] <Metal oxide composition> A structure of a cloud-aligned composite (CAC)-OS that can be used for the transistor disclosed in one embodiment of the present invention will be described below.
[0286] In this specification, etc., the term CAAC (c-axis aligned crystal) and CAC (Cloud-Aligned Composite) may be used. CAAC represents an example of a crystal structure, and CAC represents an example of a function or material configuration.
[0287] CAC-OS or CAC-metal oxide has a conductive function in a part of the material and an insulating function in a part of the material, and the material as a whole has a function as a semiconductor. When CAC-OS or CAC-metal oxide is used in the active layer of a transistor, the conductive function is a function of flowing electrons (or holes) that become carriers, and the insulating function is a function of not flowing electrons that become carriers. By making the conductive function and the insulating function act complementarily, a switching function (on / off function) can be imparted to CAC-OS or CAC-metal oxide. By separating the respective functions in CAC-OS or CAC-metal oxide, both functions can be maximized.
[0288] Moreover, the CAC-OS or CAC-metal oxide has a conductive region and an insulating region. The conductive region has the above-mentioned conductive function, and the insulating region has the above-mentioned insulating function. In addition, in the material, the conductive region and the insulating region may be separated at the nanoparticle level. In addition, the conductive region and the insulating region may be unevenly distributed in the material. In addition, the conductive region may be observed to be connected in a cloud shape with a blurred periphery.
[0289] In addition, in the CAC-OS or CAC-metal oxide, the conductive regions and the insulating regions may each be dispersed in the material with a size of 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm.
[0290] In addition, the CAC-OS or CAC-metal oxide is composed of components having different band gaps. For example, the CAC-OS or CAC-metal oxide is composed of a component having a wide gap due to an insulating region and a component having a narrow gap due to a conductive region. In this configuration, when carriers are caused to flow, the carriers mainly flow in the component having the narrow gap. In addition, the component having the narrow gap acts complementarily on the component having the wide gap, and carriers also flow in the component having the wide gap in conjunction with the component having the narrow gap. Therefore, when the above CAC-OS or CAC-metal oxide is used in the channel formation region of a transistor, a high current driving force in the on state of the transistor, that is, a large on-current and a high field effect mobility can be obtained.
[0291] That is, CAC-OS or CAC-metal oxide can also be called a matrix composite or a metal matrix composite.
[0292] The above is a description of the components.
[0293] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0294] (Embodiment 2) In this embodiment, an example of a display device including the transistor described in the above embodiment will be described.
[0295] <Configuration example> 15A shows a top view of a display device 700. The display device 700 has a first substrate 701 and a second substrate 705 bonded together with a sealant 712. A pixel portion 702, a source driver circuit portion 704, and a gate driver circuit portion 706 are provided over the first substrate 701 in a region sealed by the first substrate 701, the second substrate 705, and the sealant 712. The pixel portion 702 is provided with a plurality of display elements.
[0296] Further, an FPC terminal portion 708 to which an FPC 716 (Flexible printed circuit) is connected is provided in a portion of the first substrate 701 that does not overlap with the second substrate 705. Various signals and the like are supplied to each of the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706 by the FPC 716 via the FPC terminal portion 708 and signal lines 710.
[0297] There may be a plurality of gate driver circuits 706. The gate driver circuits 706 and the source driver circuits 704 may each be formed separately on a semiconductor substrate or the like and may be in the form of a packaged IC chip. The IC chip can be mounted on the first substrate 701 or the FPC 716.
[0298] The transistors included in the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706 can be the transistors that are the semiconductor device of one embodiment of the present invention.
[0299] Examples of the display element provided in the pixel unit 702 include a liquid crystal element and a light-emitting element. Examples of the liquid crystal element include a transmissive liquid crystal element, a reflective liquid crystal element, and a semi-transmissive liquid crystal element. Examples of the light-emitting element include a self-luminous light-emitting element such as an LED (Light Emitting Diode), an OLED (Organic LED), a QLED (Quantum-dot LED), and a semiconductor laser. Examples of the light-emitting element include a shutter-type or optical interference-type MEMS (Micro Electro Mechanical Systems) element, and a display element using a microcapsule type, an electrophoresis type, an electrowetting type, or an electronic liquid powder (registered trademark) type can also be used.
[0300] A display device 700A shown in FIG. 15B is an example of a display device that uses a flexible resin layer 743 instead of the first substrate 701 and can be used as a flexible display.
[0301] In the display device 700A, the pixel portion 702 is not rectangular, but has arc-shaped corners. As shown in region P1 in FIG. 15B, the pixel portion 702 and the resin layer 743 have cutouts formed by cutting out parts of the pixel portion 702 and the resin layer 743. A pair of gate driver circuit units 706 are provided on both sides of the pixel portion 702. The gate driver circuit units 706 are provided at the corners of the pixel portion 702 along the arc-shaped contour.
[0302] The resin layer 743 has a protruding shape at a portion where the FPC terminal portion 708 is provided. A part of the resin layer 743 including the FPC terminal portion 708 can be folded back to the rear side in a region P2 in Fig. 15(B) by folding back a part of the resin layer 743. With the FPC 716 overlapping the rear side of the pixel portion 702, the display device 700A can be mounted on an electronic device, thereby saving space in the electronic device.
[0303] An IC 717 is mounted on an FPC 716 connected to the display device 700A. The IC 717 has a function as, for example, a source driver circuit. In this case, the source driver circuit unit 704 in the display device 700A can be configured to include at least one of a protection circuit, a buffer circuit, a demultiplexer circuit, and the like.
[0304] 15C is a display device that can be suitably used in electronic devices having a large screen. The display device 700B can be suitably used in, for example, a television device, a monitor device, a personal computer (including a notebook type or a desktop type), a tablet terminal, a digital signage, and the like.
[0305] The display device 700B includes a plurality of source driver ICs 721 and a pair of gate driver circuit units 722.
[0306] The multiple source driver ICs 721 are each attached to an FPC 723. One terminal of each of the multiple FPCs 723 is connected to the first substrate 701, and the other terminal is connected to a printed circuit board 724. By bending the FPC 723, the printed circuit board 724 can be disposed on the back side of the pixel portion 702 and mounted on the electronic device, thereby enabling space saving of the electronic device.
[0307] On the other hand, the gate driver circuit portion 722 is formed on the first substrate 701. This makes it possible to realize an electronic device with a narrow frame.
[0308] With this configuration, a large-sized, high-resolution display device can be realized. For example, a display device with a diagonal screen size of 30 inches or more, 40 inches or more, 50 inches or more, or 60 inches or more can be realized. Also, a display device with an extremely high resolution such as 4K2K or 8K4K resolution can be realized.
[0309] <Cross-section example> A configuration using liquid crystal elements as display elements and a configuration using EL elements will be described below with reference to Figs. 16 to 19. Figs. 16 to 18 are cross-sectional views taken along dashed line QR in Fig. 15(A). Fig. 19 is a cross-sectional view taken along dashed line ST in display device 700A shown in Fig. 15(B). Figs. 16 and 17 show configurations using liquid crystal elements as display elements, and Figs. 18 and 19 show configurations using EL elements.
[0310] [Description of common parts of the display device] 16 to 19 includes a lead wiring portion 711, a pixel portion 702, a source driver circuit portion 704, and an FPC terminal portion 708. The lead wiring portion 711 includes a signal line 710. The pixel portion 702 includes a transistor 750 and a capacitor 790. The source driver circuit portion 704 includes a transistor 752. FIG. 17 illustrates a case where the capacitor 790 is not included.
[0311] The transistors described in Embodiment 1 can be used as the transistors 750 and 752.
[0312] The transistor used in this embodiment has an oxide semiconductor film that is highly purified and in which formation of oxygen vacancies is suppressed. The off-state current of the transistor can be reduced. Thus, the retention time of an electric signal such as an image signal can be increased, and the writing interval of the image signal can be set to be long. Thus, the frequency of a refresh operation can be reduced, which leads to an effect of reducing power consumption.
[0313] In addition, the transistor used in this embodiment mode can achieve a relatively high field effect mobility and thus can be driven at high speed. For example, by using such a transistor capable of high speed driving in a display device, a switching transistor in a pixel portion and a driver transistor used in a driver circuit portion can be formed on the same substrate. In other words, a configuration without using a driver circuit formed from a silicon wafer or the like is possible, and the number of components in the display device can be reduced. In addition, by using a transistor capable of high speed driving in the pixel portion, a high-quality image can be provided.
[0314] The capacitor 790 shown in FIG. 16, FIG. 18, and FIG. 19 has a lower electrode formed by processing the same film as the first gate electrode of the transistor 750, and an upper electrode formed by processing the same metal oxide as the semiconductor layer. The upper electrode has a low resistance like the source and drain regions of the transistor 750. In addition, a part of an insulating film functioning as the first gate insulating layer of the transistor 750 is provided between the lower electrode and the upper electrode. That is, the capacitor 790 has a stacked structure in which an insulating film functioning as a dielectric film is sandwiched between a pair of electrodes. In addition, a wiring obtained by processing the same film as the source and drain electrodes of the transistor is connected to the upper electrode.
[0315] In addition, a planarization insulating film 770 is provided over the transistor 750 , the transistor 752 , and the capacitor 790 .
[0316] The transistor 750 in the pixel portion 702 and the transistor 752 in the source driver circuit portion 704 may have different structures. For example, a top-gate transistor may be used for one of them, and a bottom-gate transistor may be used for the other. Note that the gate driver circuit portion 706 is similar to the source driver circuit portion 704.
[0317] The signal line 710 is formed of the same conductive film as the source and drain electrodes of the transistors 750 and 752. In this case, it is preferable to use a low-resistance material such as a material containing copper, because signal delays caused by wiring resistance are small and display on a large screen is possible.
[0318] The FPC terminal portion 708 has a wiring 760, a part of which functions as a connection electrode, an anisotropic conductive film 780, and an FPC 716. The wiring 760 is electrically connected to a terminal of the FPC 716 via the anisotropic conductive film 780. Here, the wiring 760 is formed of the same conductive film as the source electrodes and drain electrodes of the transistors 750 and 752.
[0319] A flexible substrate such as a glass substrate or a plastic substrate can be used as the first substrate 701 and the second substrate 705. When a flexible substrate is used as the first substrate 701, an insulating layer having a barrier property against water and hydrogen is preferably provided between the first substrate 701 and the transistor 750 or the like.
[0320] In addition, on the second substrate 705 side, a light-shielding film 738, a colored film 736, and an insulating film 734 in contact with these are provided.
[0321] [Example of the configuration of a display device using a liquid crystal element] A display device 700 shown in FIG. 16 includes a liquid crystal element 775 and a spacer 778. The liquid crystal element 775 includes a conductive layer 772, a conductive layer 774, and a liquid crystal layer 776 between them. The conductive layer 774 is provided on the second substrate 705 side and functions as a common electrode. The conductive layer 772 is electrically connected to a source electrode or a drain electrode of the transistor 750. The conductive layer 772 is formed over a planarization insulating film 770 and functions as a pixel electrode.
[0322] A material that transmits or reflects visible light can be used for the conductive layer 772. As a light-transmitting material, for example, an oxide material containing indium, zinc, tin, or the like can be used. As a reflective material, for example, a material containing aluminum, silver, or the like can be used.
[0323] When a reflective material is used for the conductive layer 772, the display device 700 becomes a reflective liquid crystal display device. On the other hand, when a light-transmitting material is used for the conductive layer 772, the display device becomes a transmissive liquid crystal display device. In the case of a reflective liquid crystal display device, a polarizing plate is provided on the viewing side. On the other hand, in the case of a transmissive liquid crystal display device, a pair of polarizing plates is provided to sandwich a liquid crystal element.
[0324] 17 shows an example of a display device 700 using a horizontal electric field (for example, FFS mode) liquid crystal element 775. A conductive layer 774 functioning as a common electrode is provided over a conductive layer 772 with an insulating layer 773 interposed therebetween. The alignment state of a liquid crystal layer 776 can be controlled by an electric field generated between the conductive layer 772 and the conductive layer 774.
[0325] 17, a storage capacitor can be formed using a stacked structure of a conductive layer 774, an insulating layer 773, and a conductive layer 772. Therefore, there is no need to provide a separate capacitor, and the aperture ratio can be increased.
[0326] 16 and 17, an alignment film may be provided in contact with the liquid crystal layer 776. Optical members (optical substrates) such as a polarizing member, a phase difference member, and an anti-reflection member, and light sources such as a backlight and a sidelight may be provided as appropriate.
[0327] Thermotropic liquid crystal, low molecular liquid crystal, polymer liquid crystal, polymer dispersed liquid crystal (PDLC), polymer network liquid crystal (PNLC), ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. can be used for the liquid crystal layer 776. In addition, when the in-plane switching mode is adopted, liquid crystal exhibiting a blue phase without using an alignment film may be used.
[0328] In addition, the liquid crystal element modes that can be used include TN (Twisted Nematic) mode, VA (Vertical Alignment) mode, IPS (In-Plane-Switching) mode, FFS (Fringe Field Switching) mode, ASM (Axially Symmetric aligned Micro-cell) mode, OCB (Optically Compensated Birefringence) mode, ECB (Electrically Controlled Birefringence) mode, and guest-host mode.
[0329] Also, a scattering type liquid crystal element using a polymer dispersed liquid crystal or a polymer network type liquid crystal for the liquid crystal layer 776 can be used. In this case, a configuration for performing black and white display without providing the colored film 736, or a configuration for performing color display using the colored film 736 can be used.
[0330] Furthermore, as a method for driving the liquid crystal element, a time-division display method (also called a field sequential driving method) that performs color display based on a time-sequential additive color mixing method may be applied. In this case, the color film 736 may not be provided. When the time-division display method is used, there is an advantage that the aperture ratio of the pixel can be improved and the resolution can be increased because there is no need to provide sub-pixels that exhibit the respective colors of R (red), G (green), and B (blue).
[0331] [Display device using light-emitting element] 18 includes a light-emitting element 782. The light-emitting element 782 includes a conductive layer 772, an EL layer 786, and a conductive film 788. The EL layer 786 includes an organic compound or an inorganic compound such as quantum dots.
[0332] Examples of materials that can be used for the organic compounds include fluorescent materials and phosphorescent materials, while examples of materials that can be used for the quantum dots include colloidal quantum dot materials, alloy quantum dot materials, core-shell quantum dot materials, and core quantum dot materials.
[0333] 18, an insulating film 730 that covers part of a conductive layer 772 is provided over a planarization insulating film 770. Here, the light-emitting element 782 is a top-emission light-emitting element that has a light-transmitting conductive film 788. Note that the light-emitting element 782 may have a bottom-emission structure in which light is emitted to the conductive layer 772 side or a dual-emission structure in which light is emitted to both the conductive layer 772 side and the conductive film 788 side.
[0334] The colored film 736 is provided at a position overlapping the light-emitting element 782, and the light-shielding film 738 is provided at a position overlapping the insulating film 730, in the lead-out wiring portion 711, and in the source driver circuit portion 704. The colored film 736 and the light-shielding film 738 are covered with an insulating film 734. The space between the light-emitting element 782 and the insulating film 734 is filled with a sealing film 732. Note that when the EL layer 786 is formed in an island shape for each pixel or in a striped shape for each pixel column, that is, when the EL layer 786 is formed by coloring, the colored film 736 may not be provided.
[0335] A configuration of a display device that can be suitably applied to a flexible display is shown in Fig. 19. Fig. 19 is a cross-sectional view taken along dashed line ST in the display device 700A shown in Fig. 15(B).
[0336] 19 has a stacked structure of a supporting substrate 745, an adhesive layer 742, a resin layer 743, and an insulating layer 744 instead of the first substrate 701 shown in FIG. 18. A transistor 750, a capacitor 790, and the like are provided over the insulating layer 744 provided over the resin layer 743.
[0337] The support substrate 745 is a substrate that contains an organic resin, glass, or the like, and is thin enough to be flexible. The resin layer 743 is a layer that contains an organic resin such as polyimide or acrylic. The insulating layer 744 contains an inorganic insulating film such as silicon oxide, silicon oxynitride, or silicon nitride. The resin layer 743 and the support substrate 745 are attached to each other by an adhesive layer 742. The resin layer 743 is preferably thinner than the support substrate 745.
[0338] 19 has a protective layer 740 instead of the substrate 705 shown in FIG. 18. The protective layer 740 is attached to the sealing film 732. A glass substrate, a resin film, or the like can be used as the protective layer 740. In addition, an optical member such as a polarizing plate or a scattering plate, an input device such as a touch sensor panel, or a configuration in which two or more of these are laminated may be used as the protective layer 740.
[0339] An EL layer 786 included in the light-emitting element 782 is provided in an island shape over the insulating film 730 and the conductive layer 772. By creating the EL layer 786 so that each subpixel emits a different light color, color display can be achieved without using the colored film 736. A protective layer 741 is provided to cover the light-emitting element 782. The protective layer 741 has a function of preventing impurities such as water from diffusing into the light-emitting element 782. The protective layer 741 is preferably an inorganic insulating film. A stacked structure including at least one inorganic insulating film and at least one organic insulating film is more preferably used.
[0340] FIG. 19 also shows a bendable region P2. In the region P2, in addition to the support substrate 745 and the adhesive layer 742, there is a portion where no inorganic insulating film such as the insulating layer 744 is provided. In the region P2, a resin layer 746 is provided to cover the wiring 760. By providing as little inorganic insulating film as possible in the bendable region P2 and by using a configuration in which only a conductive layer containing a metal or alloy and a layer containing an organic material are laminated, it is possible to prevent cracks from occurring when the display device 700A is bent. Furthermore, by not providing the support substrate 745 in the region P2, a part of the display device 700A can be bent with an extremely small radius of curvature.
[0341] [Example of configuration in which an input device is provided on a display device] An input device may be provided in the display device shown in Figures 16 to 19. As the input device, for example, a touch sensor or the like can be given.
[0342] For example, various types of sensors can be used, such as a capacitance type, a resistive film type, a surface acoustic wave type, an infrared type, an optical type, a pressure sensitive type, etc. Alternatively, two or more of these types may be used in combination.
[0343] The touch panel may have a configuration such as an in-cell type touch panel in which an input device is formed between a pair of substrates, a so-called on-cell type touch panel in which an input device is formed on a display device, or an out-cell type touch panel in which the input device is attached to a display device.
[0344] At least a part of the configuration examples exemplified in this embodiment and the corresponding drawings can be appropriately combined with other configuration examples or drawings.
[0345] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0346] (Embodiment 3) In this embodiment, a display device including a semiconductor device of one embodiment of the present invention will be described with reference to FIGS.
[0347] 20A includes a pixel portion 502, a driver circuit portion 504, a protective circuit 506, and a terminal portion 507. Note that the protective circuit 506 does not necessarily have to be provided.
[0348] The transistor of one embodiment of the present invention can be applied to the transistors in the pixel portion 502 and the driver circuit portion 504. The transistor of one embodiment of the present invention can also be applied to the protection circuit 506.
[0349] The pixel section 502 has a plurality of pixel circuits 501 that drive a plurality of display elements arranged in X rows and Y columns (X and Y are each independently a natural number of 2 or more).
[0350] The driver circuit unit 504 includes driver circuits such as a gate driver 504a that outputs scan signals to the scan lines GL_1 to GL_X and a source driver 504b that supplies data signals to the data lines DL_1 to DL_Y. The gate driver 504a may include at least a shift register. The source driver 504b may include, for example, a plurality of analog switches. The source driver 504b may also include a shift register.
[0351] The terminal portion 507 refers to a portion provided with terminals for inputting power, control signals, image signals, and the like from an external circuit to the display device.
[0352] 20A is connected to various wirings such as a scanning line GL between the gate driver 504a and the pixel circuit 501, or a data line DL between the source driver 504b and the pixel circuit 501.
[0353] In addition, the gate driver 504a and the source driver 504b may be provided on the same substrate as the pixel portion 502, or a substrate on which a gate driver circuit or a source driver circuit is separately formed (e.g., a drive circuit substrate formed of a single crystal semiconductor film or a polycrystalline semiconductor film) may be mounted on the substrate by COG or TAB (Tape Automated Bonding).
[0354] Further, the pixel circuits 501 shown in FIG. 20A can have the structures shown in FIG. 20B and FIG. 20C, for example.
[0355] 20B includes a liquid crystal element 570, a transistor 550, and a capacitor 560. The pixel circuit 501 is connected to a data line DL_n, a scanning line GL_m, a potential supply line VL, and the like.
[0356] The potential of one of a pair of electrodes of the liquid crystal element 570 is set as appropriate according to the specifications of the pixel circuit 501. The orientation state of the liquid crystal element 570 is set by written data. Note that a common potential (common potential) may be applied to one of the pair of electrodes of the liquid crystal element 570 included in each of the multiple pixel circuits 501. Also, different potentials may be applied to one of the pair of electrodes of the liquid crystal element 570 in the pixel circuits 501 in each row.
[0357] 20C includes transistors 552 and 554, a capacitor 562, and a light-emitting element 572. The pixel circuit 501 is connected to a data line DL_n, a scanning line GL_m, a potential supply line VL_a, a potential supply line VL_b, and the like.
[0358] A high power supply potential VDD is applied to one of the potential supply lines VL_a and VL_b, and a low power supply potential VSS is applied to the other. A current flowing through the light emitting element 572 is controlled in accordance with a potential applied to the gate of the transistor 554, thereby controlling the light emission luminance of the light emitting element 572.
[0359] At least a part of the configuration examples exemplified in this embodiment and the corresponding drawings can be appropriately combined with other configuration examples or drawings.
[0360] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0361] (Embodiment 4) In the following, a pixel circuit including a memory for correcting a gray scale displayed in a pixel and a display device including the pixel circuit will be described. The transistors exemplified in the first embodiment can be applied to the transistors used in the pixel circuits exemplified below.
[0362] <Circuit configuration> 21A shows a circuit diagram of a pixel circuit 400. The pixel circuit 400 includes a transistor M1, a transistor M2, a capacitor C1, and a circuit 401. The pixel circuit 400 is connected to a wiring S1, a wiring S2, a wiring G1, and a wiring G2.
[0363] The transistor M1 has a gate connected to the wiring G1, one of its source and drain connected to the wiring S1, and the other of its source and drain connected to one electrode of the capacitor C1. The transistor M2 has a gate connected to the wiring G2, one of its source and drain connected to the wiring S2, and the other of its source and drain connected to the other electrode of the capacitor C1 and the circuit 401.
[0364] The circuit 401 is a circuit including at least one display element. Various elements can be used as the display element, but typically, a light-emitting element such as an organic EL element or an LED element, a liquid crystal element, or a MEMS (Micro Electro Mechanical Systems) element can be used.
[0365] The node connecting the transistor M1 and the capacitor C1 is referred to as a node N1, and the node connecting the transistor M2 and the circuit 401 is referred to as a node N2.
[0366] In the pixel circuit 400, the potential of the node N1 can be maintained by turning off the transistor M1. Also, the potential of the node N2 can be maintained by turning off the transistor M2. Also, by writing a predetermined potential to the node N1 via the transistor M1 while the transistor M2 is in the off state, the potential of the node N2 can be changed according to the change in the potential of the node N1 due to capacitive coupling via the capacitor C1.
[0367] Here, the transistor including an oxide semiconductor, as exemplified in Embodiment 1, can be used as one or both of the transistor M1 and the transistor M2. Therefore, the potentials of the nodes N1 and N2 can be held for a long period of time due to an extremely low off-state current. Note that when the period during which the potentials of the nodes are held is short (specifically, when the frame frequency is 30 Hz or more), a transistor including a semiconductor such as silicon may be used.
[0368] <Driving method example> Next, an example of an operation method of the pixel circuit 400 will be described with reference to Fig. 21(B). Fig. 21(B) is a timing chart relating to the operation of the pixel circuit 400. Note that, for ease of explanation, the influence of various resistances such as wiring resistance, parasitic capacitances of transistors and wiring, threshold voltages of transistors, and the like will not be taken into consideration here.
[0369] 21B, one frame period is divided into a period T1 and a period T2. The period T1 is a period in which a potential is written to the node N2, and the period T2 is a period in which a potential is written to the node N1.
[0370] [Period T1] In the period T1, a potential that turns on the transistor is applied to both the wiring G1 and the wiring G2. In addition, a fixed potential V ref is supplied to the line S2, and the first data potential V w supplies.
[0371] The node N1 is connected to a potential V ref A first data potential V w Therefore, the capacitance C1 has a potential difference V w -V ref is held.
[0372] [Period T2] In the next period T2, a potential that turns on the transistor M1 is applied to the wiring G1, and a potential that turns off the transistor M2 is applied to the wiring G2. data A predetermined constant potential is applied to the wiring S2, or the wiring S2 may be in a floating state.
[0373] A second data potential V data At this time, the second data potential V data In response to the change in potential, the potential of the node N2 changes by a potential dV. That is, a potential obtained by adding the first data potential Vw and the potential dV is input to the circuit 401. Note that although the potential dV is shown to be a positive value in FIG. 21B, it may be a negative value. That is, the potential of the second data potential V data is the potential V ref It may be lower.
[0374] Here, the potential dV is roughly determined by the capacitance value of the capacitor C1 and the capacitance value of the circuit 401. When the capacitance value of the capacitor C1 is sufficiently larger than the capacitance value of the circuit 401, the potential dV is equal to the second data potential V data The potential becomes close to
[0375] In this manner, the pixel circuit 400 can generate a potential to be supplied to the circuit 401 including a display element by combining two types of data signals. Therefore, it is possible to perform gray scale correction within the pixel circuit 400.
[0376] In addition, the pixel circuit 400 can generate a potential that exceeds the maximum potential that can be supplied to the wirings S1 and S2. For example, when a light-emitting element is used, high dynamic range (HDR) display or the like can be performed. When a liquid crystal element is used, overdrive driving or the like can be realized.
[0377] <Application Examples> [Example using liquid crystal element] A pixel circuit 400LC shown in Fig. 21C includes a circuit 401LC. The circuit 401LC includes a liquid crystal element LC and a capacitor C2.
[0378] The liquid crystal element LC has one electrode connected to the other electrode of the capacitance C1, the other of the source and drain of the transistor M2, and one electrode of the capacitance C2, and the other electrode connected to a potential V com2 The other electrode of the capacitor C2 is connected to the wiring to which the potential V com1 Connect with the wiring given.
[0379] The capacitor C2 functions as a storage capacitor. Note that the capacitor C2 can be omitted if not required.
[0380] Since the pixel circuit 400LC can supply a high voltage to the liquid crystal element LC, it can, for example, realize high-speed display by overdrive driving, apply a liquid crystal material with a high driving voltage, etc. In addition, by supplying a correction signal to the wiring S1 or wiring S2, it is possible to correct the gradation according to the operating temperature, the deterioration state of the liquid crystal element LC, etc.
[0381] [Example using light-emitting element] The pixel circuit 400EL shown in Fig. 21D includes a circuit 401EL. The circuit 401EL includes a light-emitting element EL, a transistor M3, and a capacitor C2.
[0382] The transistor M3 has a gate connected to one electrode of the capacitance C2, and one of its source and drain connected to the potential V H The other electrode of the capacitor C2 is connected to a wiring to which a potential V com The light-emitting element EL has the other electrode connected to a wiring that is supplied with a potential V L Connect with the wiring given.
[0383] The transistor M3 has a function of controlling the current supplied to the light-emitting element EL. The capacitor C2 functions as a storage capacitor. The capacitor C2 can be omitted if not required.
[0384] In this embodiment, the anode side of the light-emitting element EL is connected to the transistor M3, but the cathode side of the light-emitting element EL may be connected to the transistor M3. H and potential V L You can change the value as appropriate.
[0385] In the pixel circuit 400EL, a large current can be passed through the light-emitting element EL by applying a high potential to the gate of the transistor M3, thereby realizing, for example, HDR display, etc. In addition, by supplying a correction signal to the wiring S1 or wiring S2, it is also possible to correct variations in the electrical characteristics of the transistor M3 and the light-emitting element EL.
[0386] Note that the present invention is not limited to the circuits illustrated in FIGS. 21C and 21D, and a configuration in which a transistor, a capacitor, or the like is added may be used.
[0387] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0388] (Embodiment 5) In this embodiment, a display module that can be manufactured using one embodiment of the present invention will be described.
[0389] A display module 6000 shown in FIG. 22A includes a display device 6006 connected to an FPC 6005, a frame 6009, a printed circuit board 6010, and a battery 6011 between an upper cover 6001 and a lower cover 6002.
[0390] For example, a display device manufactured using one embodiment of the present invention can be used as the display device 6006. The display device 6006 can provide a display module with extremely low power consumption.
[0391] The shape and dimensions of the upper cover 6001 and the lower cover 6002 can be changed appropriately according to the size of the display device 6006.
[0392] The display device 6006 may have a function as a touch panel.
[0393] The frame 6009 may have a function of protecting the display device 6006, a function of blocking electromagnetic waves generated by the operation of the printed circuit board 6010, a function as a heat sink, and the like.
[0394] The printed circuit board 6010 includes a power supply circuit, a signal processing circuit for outputting a video signal and a clock signal, a battery control circuit, and the like.
[0395] FIG. 22B is a schematic cross-sectional view of a display module 6000 equipped with an optical touch sensor.
[0396] The display module 6000 has a light emitting section 6015 and a light receiving section 6016 provided on a printed circuit board 6010. Also, in an area surrounded by an upper cover 6001 and a lower cover 6002, a pair of light guiding sections (light guiding section 6017a, light guiding section 6017b) are provided.
[0397] The display device 6006 is provided so as to overlap a printed circuit board 6010 and a battery 6011 with a frame 6009 interposed therebetween. The display device 6006 and the frame 6009 are fixed to a light guiding portion 6017a and a light guiding portion 6017b.
[0398] Light 6018 emitted from a light-emitting unit 6015 passes through a light-guiding unit 6017a, an upper portion of the display device 6006, and a light-guiding unit 6017b to reach a light-receiving unit 6016. When the light 6018 is blocked by a detection object such as a finger or a stylus, a touch operation can be detected.
[0399] A plurality of light emitting units 6015 are provided, for example, along two adjacent sides of the display device 6006. A plurality of light receiving units 6016 are provided at positions facing the light emitting units 6015. This makes it possible to obtain information on the position where a touch operation has been performed.
[0400] The light emitting unit 6015 may be a light source such as an LED element, and it is particularly preferable to use a light source that emits infrared light. The light receiving unit 6016 may be a photoelectric element that receives the light emitted by the light emitting unit 6015 and converts it into an electric signal. Preferably, a photodiode that can receive infrared light may be used.
[0401] The light guiding portion 6017a and the light guiding portion 6017b that transmit light 6018 allow the light emitting portion 6015 and the light receiving portion 6016 to be disposed below the display device 6006, and it is possible to prevent external light from reaching the light receiving portion 6016 and causing the touch sensor to malfunction. In particular, if a resin that absorbs visible light and transmits infrared light is used, it is possible to more effectively prevent the touch sensor from malfunctioning.
[0402] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0403] (Embodiment 6) In this embodiment, examples of electronic devices to which the display device of one embodiment of the present invention can be applied will be described.
[0404] An electronic device 6500 shown in FIG. 23A is a portable information terminal that can be used as a smartphone.
[0405] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, and a light source 6508. The display portion 6502 has a touch panel function.
[0406] The display device of one embodiment of the present invention can be applied to the display portion 6502.
[0407] FIG. 23B is a schematic cross-sectional view including the end portion of the housing 6501 on the microphone 6506 side.
[0408] A light-transmitting protective member 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, optical members 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, etc. are arranged in the space surrounded by the housing 6501 and the protective member 6510.
[0409] A display panel 6511, an optical member 6512, and a touch sensor panel 6513 are fixed to the protective member 6510 by adhesive layers (not shown).
[0410] A part of the display panel 6511 is folded back in an area outside the display unit 6502. An FPC 6515 is connected to the folded back part. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on a printed circuit board 6517.
[0411] The flexible display panel of one embodiment of the present invention can be applied to the display panel 6511. Therefore, an extremely lightweight electronic device can be realized. In addition, since the display panel 6511 is extremely thin, a large-capacity battery 6518 can be mounted thereon while keeping the thickness of the electronic device small. In addition, by folding back a part of the display panel 6511 and arranging a connection portion with the FPC 6515 on the back side of the pixel portion, an electronic device with a narrow frame can be realized.
[0412] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0413] (Embodiment 7) In this embodiment, electronic devices including a display device manufactured according to one embodiment of the present invention will be described.
[0414] The electronic devices exemplified below each have a display device according to one embodiment of the present invention in a display portion. Therefore, the electronic devices have high resolution. In addition, the electronic devices can have both high resolution and a large screen.
[0415] The display portion of the electronic device according to one embodiment of the present invention can display images with a resolution of, for example, full high definition, 4K2K, 8K4K, 16K8K, or higher.
[0416] Examples of electronic devices include electronic devices with relatively large screens such as television devices, notebook personal computers, monitor devices, digital signage, pachinko machines, and game machines, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, personal digital assistants, and audio playback devices.
[0417] An electronic device to which one embodiment of the present invention is applied can be incorporated along a flat or curved surface of an inner or outer wall of a house or building, or the interior or exterior of an automobile or the like.
[0418] FIG. 24A is a diagram showing the appearance of the camera 8000 with the viewfinder 8100 attached.
[0419] The camera 8000 includes a housing 8001, a display unit 8002, an operation button 8003, a shutter button 8004, etc. In addition, a detachable lens 8006 is attached to the camera 8000.
[0420] In addition, the camera 8000 may have the lens 8006 and the housing integrated together.
[0421] The camera 8000 can capture an image by pressing a shutter button 8004 or touching a display unit 8002 that functions as a touch panel.
[0422] The housing 8001 has a mount having electrodes, and can be connected to a strobe device and the like in addition to the finder 8100 .
[0423] The finder 8100 includes a housing 8101, a display portion 8102, a button 8103, and the like.
[0424] The housing 8101 is attached to the camera 8000 by a mount that engages with the mount of the camera 8000. The viewfinder 8100 can display an image received from the camera 8000 on a display unit 8102.
[0425] The button 8103 has a function such as a power button.
[0426] The display device of one embodiment of the present invention can be applied to a display portion 8002 of a camera 8000 and a display portion 8102 of a viewfinder 8100. Note that the camera 8000 may have a built-in viewfinder.
[0427] FIG. 24B is a diagram showing the external appearance of the head mounted display 8200.
[0428] The head mounted display 8200 includes a mounting portion 8201, a lens 8202, a main body 8203, a display portion 8204, and a cable 8205. The mounting portion 8201 includes a built-in battery 8206.
[0429] A cable 8205 supplies power from a battery 8206 to a main body 8203. The main body 8203 includes a wireless receiver or the like and can display received video information on a display portion 8204. The main body 8203 also includes a camera and can use information on the movements of the user's eyeballs and eyelids as an input means.
[0430] The mounting unit 8201 may have a function of recognizing the line of sight by providing a plurality of electrodes at positions that contact the user, capable of detecting a current that flows with the movement of the user's eyeballs. The mounting unit 8201 may also have a function of monitoring the user's pulse rate based on the current that flows through the electrodes. The mounting unit 8201 may also have various sensors, such as a temperature sensor, a pressure sensor, and an acceleration sensor, and may have a function of displaying the user's biological information on the display unit 8204 and a function of changing the image displayed on the display unit 8204 according to the movement of the user's head.
[0431] The display device of one embodiment of the present invention can be applied to the display portion 8204.
[0432] 24C, 24D, and 24E are diagrams showing the external appearance of a head mounted display 8300. The head mounted display 8300 includes a housing 8301, a display portion 8302, a band-shaped fixture 8304, and a pair of lenses 8305.
[0433] A user can view the display on the display unit 8302 through the lens 8305. Note that it is preferable to arrange the display unit 8302 in a curved manner because the user can feel a high sense of presence. In addition, by viewing another image displayed in a different area of the display unit 8302 through the lens 8305, it is possible to perform 3D display using parallax. Note that the present invention is not limited to a configuration in which one display unit 8302 is provided, and two display units 8302 may be provided, with one display unit being provided for each eye of the user.
[0434] Note that the display device of one embodiment of the present invention can be applied to the display portion 8302. A display device including the semiconductor device of one embodiment of the present invention has extremely high definition, so that a user cannot see pixels even when the image is enlarged using a lens 8305 as in FIG.
[0435] The electronic devices shown in Figures 25(A) to 25(G) have a housing 9000, a display unit 9001, a speaker 9003, operation keys 9005 (including a power switch or an operation switch), a connection terminal 9006, a sensor 9007 (including a function of measuring force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor or infrared rays), a microphone 9008, etc.
[0436] 25(A) to 25(G) have various functions. For example, the electronic devices may have a function of displaying various information (still images, videos, text images, etc.) on a display unit, a touch panel function, a function of displaying a calendar, date, or time, a function of controlling processing by various software (programs), a wireless communication function, a function of reading and processing a program or data recorded on a recording medium, and the like. Note that the functions of the electronic devices are not limited to these, and the electronic devices may have various functions. The electronic devices may have multiple display units. In addition, the electronic devices may have a function of providing a camera or the like in order to capture still images or videos and store them in a recording medium (external or built-in to the camera), a function of displaying the captured images on the display unit, and the like.
[0437] The electronic devices shown in FIGS. 25A to 25G will be described in detail below.
[0438] 25A is a perspective view of a television set 9100. The television set 9100 can incorporate a display portion 9001 having a large screen, for example, a screen size of 50 inches or more, or 100 inches or more.
[0439] FIG. 25B is a perspective view showing a mobile information terminal 9101. The mobile information terminal 9101 can be used as, for example, a smartphone. Note that the mobile information terminal 9101 may be provided with a speaker 9003, a connection terminal 9006, a sensor 9007, and the like. The mobile information terminal 9101 can display text and image information on a plurality of surfaces. FIG. 25B shows an example in which three icons 9050 are displayed. Information 9051 shown in a dashed rectangle can also be displayed on another surface of the display unit 9001. Examples of the information 9051 include notifications of incoming e-mail, SNS, and phone calls, titles of e-mail and SNS, sender names, date and time, time, remaining battery level, and antenna reception strength. Alternatively, the icon 9050 or the like may be displayed at the position where the information 9051 is displayed.
[0440] 25(C) is a perspective view showing a mobile information terminal 9102. The mobile information terminal 9102 has a function of displaying information on three or more surfaces of a display unit 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different surfaces. For example, a user can check information 9053 displayed in a position that can be observed from above the mobile information terminal 9102 while the mobile information terminal 9102 is stored in a breast pocket of clothes. The user can check the display without taking the mobile information terminal 9102 out of the pocket and determine, for example, whether to answer a call.
[0441] 25D is a perspective view showing a wristwatch-type mobile information terminal 9200. The mobile information terminal 9200 can be used as, for example, a smart watch. The display surface of the display unit 9001 is curved, and display can be performed along the curved display surface. The mobile information terminal 9200 can also perform hands-free conversation by communicating with, for example, a headset capable of wireless communication. The mobile information terminal 9200 can also perform data transmission and charging with another information terminal through a connection terminal 9006. Note that charging may be performed by wireless power supply.
[0442] 25(E), 25(F), and 25(G) are perspective views showing a foldable mobile information terminal 9201. FIG. 25(E) shows the mobile information terminal 9201 in an unfolded state, FIG. 25(G) shows the mobile information terminal 9201 in a folded state, and FIG. 25(F) shows the mobile information terminal 9201 in a state in the middle of changing from one of FIG. 25(E) and FIG. 25(G) to the other. The mobile information terminal 9201 has excellent portability in a folded state, and has excellent viewability of the display due to a seamless wide display area in an unfolded state. A display portion 9001 of the mobile information terminal 9201 is supported by three housings 9000 connected by a hinge 9055. For example, the display portion 9001 can be bent with a curvature radius of 1 mm or more and 150 mm or less.
[0443] 26A shows an example of a television set. A television set 7100 includes a display unit 7500 built in a housing 7101. Here, the housing 7101 is supported by a stand 7103.
[0444] 26A can be operated using an operation switch provided on a housing 7101 or a separate remote control 7111. Alternatively, a touch panel may be applied to the display portion 7500, and the television set 7100 may be operated by touching the touch panel. The remote control 7111 may have a display portion in addition to operation buttons.
[0445] The television device 7100 may also include a television broadcast receiver and a communication device for network connection.
[0446] 26B shows a laptop personal computer 7200. The laptop personal computer 7200 includes a housing 7211, a keyboard 7212, a pointing device 7213, an external connection port 7214, and the like. A display portion 7500 is incorporated in the housing 7211.
[0447] 26(C) and 26(D) show an example of digital signage.
[0448] 26C includes a housing 7301, a display portion 7500, a speaker 7303, and the like. The digital signage 7300 may further include an LED lamp, an operation key (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, and the like.
[0449] 26D shows a digital signage 7400 attached to a cylindrical pillar 7401. The digital signage 7400 has a display unit 7500 provided along the curved surface of the pillar 7401.
[0450] The larger the display unit 7500, the more information can be provided at one time, and the larger the display area, the more easily it catches people's attention, which has the effect of increasing the effectiveness of advertising, for example.
[0451] It is preferable to apply a touch panel to the display unit 7500 so that the user can operate it. This allows the display unit 7500 to be used not only for advertising purposes, but also for providing information desired by the user, such as route information, traffic information, and commercial facility guide information.
[0452] 26C and 26D, the digital signage 7300 or the digital signage 7400 is preferably capable of wirelessly linking with an information terminal 7311 such as a smartphone carried by a user. For example, advertising information displayed on the display unit 7500 can be displayed on the screen of the information terminal 7311, or the display on the display unit 7500 can be switched by operating the information terminal 7311.
[0453] Furthermore, a game using the information terminal 7311 as an operation means (controller) can be executed on the digital signage 7300 or the digital signage 7400. This allows an unspecified number of users to simultaneously participate in and enjoy the game.
[0454] The display device of one embodiment of the present invention can be applied to the display portion 7500 in FIGS.
[0455] Although the electronic device in this embodiment has a display portion, one embodiment of the present invention can also be applied to an electronic device that does not have a display portion.
[0456] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification. EXAMPLES
[0457] In this example, the etching rates of copper, titanium, molybdenum, ITSO, metal oxide, and silicon oxynitride were evaluated as examples of materials that can be used for the conductive layer 112, the functional layer 113, the metal oxide layer 114, or the insulating layer 110. For silicon oxynitride, three types of films (silicon oxynitride 1, silicon oxynitride 2, and silicon oxynitride 3) formed under different film formation conditions were evaluated.
[0458] For the evaluation, samples having various films formed on glass substrates were used.
[0459] The copper film used in this example was formed by sputtering using a Cu target under conditions of a pressure of 1.0 Pa and a power supply of 15 kW (DC). The substrate temperature during film formation was 100° C. Argon gas was used as the film formation gas.
[0460] The titanium film used in this example was formed by sputtering using a Ti target under conditions of a pressure of 0.3 Pa and a power supply of 8 kW (DC). The substrate temperature during film formation was room temperature. Argon gas was used as the film formation gas.
[0461] The molybdenum film used in this example was formed by sputtering using a Mo target under conditions of a pressure of 0.85 Pa and a power supply of 35 kW (DC). The substrate temperature during film formation was 80° C. Argon gas was used as the film formation gas.
[0462] The ITSO film used in this example was formed using an ITSO target (In 2 O 3 :SnO 2 :SiO 2 The deposition was performed by sputtering using a mixture of 1000 and 10000 sapphire gas (weight ratio: 85:10:5) at a pressure of 0.15 Pa and a power source of 1 kW (DC). The substrate temperature during deposition was 80° C. Argon gas was used as the deposition gas.
[0463] The metal oxide film used in this example was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW (AC). The substrate temperature during film formation was room temperature. A mixed gas of oxygen gas and argon gas was used as the film formation gas, and the oxygen flow rate ratio was 10%. The film composition of the sample formed using a target with a composition of In:Ga:Zn=4:2:4.1 [atomic ratio] was approximately In:Ga:Zn=4:2:3 [atomic ratio].
[0464] The silicon oxynitride film 1 used in this example was formed by PECVD using a mixed gas of silane gas at a flow rate of 24 sccm and nitrous oxide gas at a flow rate of 18000 sccm under conditions of a pressure of 200 Pa and a film-forming power of 130 W. The substrate temperature during film formation was 350° C. The silicon oxynitride film 1 corresponds to the insulating layer 110a described in the first embodiment.
[0465] The silicon oxynitride film 2 used in this example was formed by PECVD using a mixed gas of silane gas with a flow rate of 200 sccm and nitrous oxide gas with a flow rate of 10,000 sccm under conditions of a pressure of 300 Pa and a film-forming power of 750 W. The substrate temperature during film formation was 350° C. The silicon oxynitride film 2 corresponds to the insulating layer 110c shown in the first embodiment.
[0466] The silicon oxynitride film 3 used in this example was formed by PECVD using a mixed gas of silane gas at a flow rate of 20 sccm and dinitrogen monoxide gas at a flow rate of 3000 sccm under conditions of a pressure of 40 Pa and a film formation power of 500 W. The substrate temperature during film formation was 350° C. The silicon oxynitride film 3 corresponds to the insulating layer 110b shown in the first embodiment.
[0467] The etchant used was a mixture of two chemicals, chemical A and chemical B, in a 5:1 volume ratio immediately before use. Chemical A was an aqueous solution of phosphoric acid (less than 5 weight%), hydrofluoric acid (less than 1 weight%), nitric acid (less than 10 weight%), and additives (less than 22 weight%). Chemical B was an aqueous solution of hydrogen peroxide (31 weight%). The etchant temperature during etching was 30°C.
[0468] The etching rates of various films are shown in Table 1. In Table 1, IGZO(4:2:3) refers to the metal oxide film described above, SiON1 refers to the silicon oxynitride film 1 described above, SiON2 refers to the silicon oxynitride film 2 described above, and SiON3 refers to the silicon oxynitride film 3 described above.
[0469] [Table 1]
[0470] As shown in Table 1, it was confirmed that the etching rates of titanium, molybdenum, ITSO, metal oxide, silicon oxynitride 1, silicon oxynitride 2, and silicon oxynitride 3 are slower than that of copper. It was also confirmed that the etching rate of the silicon oxynitride film 3 that can be used for the insulating layer 110b is slower than that of the silicon oxynitride film 1 that can be used for the insulating layer 110a and that of the silicon oxynitride film 2 that can be used for the insulating layer 110c. It was also confirmed that the etching rate of the silicon oxynitride film 2 that can be used for the insulating layer 110c is faster than that of the silicon oxynitride film 1 that can be used for the insulating layer 110a and that of the silicon oxynitride film 3 that can be used for the insulating layer 110b. EXAMPLES
[0471] In this example, a sample (sample A) corresponding to the transistor 100B shown in FIG. 3 was fabricated, and the cross-sectional shape was evaluated.
[0472] <Sample preparation> First, a tungsten film having a thickness of 100 nm was formed on a glass substrate by sputtering, and then processed to obtain a first gate electrode.
[0473] Next, a first silicon nitride film having a thickness of 50 nm, a second silicon nitride film having a thickness of 200 nm, a third silicon nitride film having a thickness of 50 nm, and a first silicon oxynitride film having a thickness of 3 nm were formed in this order as a first gate insulating layer.
[0474] The first silicon nitride film and the third silicon nitride film were formed by PECVD using a mixed gas of silane gas with a flow rate of 200 sccm, nitrogen gas with a flow rate of 2000 sccm, and ammonia gas with a flow rate of 100 sccm, under conditions of a pressure of 100 Pa and a film formation power of 2000 W. The substrate temperature during film formation was 350°C.
[0475] The second silicon nitride film was formed by PECVD using a mixed gas of silane gas at a flow rate of 290 sccm, nitrogen gas at a flow rate of 2000 sccm, and ammonia gas at a flow rate of 2000 sccm, under conditions of a pressure of 200 Pa and a film formation power of 3000 W. The substrate temperature during film formation was 350°C.
[0476] The first silicon oxynitride film was formed by PECVD using a mixed gas of silane gas with a flow rate of 20 sccm and dinitrogen monoxide gas with a flow rate of 3000 sccm under conditions of a pressure of 40 Pa and a film formation power of 3000 W. The substrate temperature during film formation was 350°C.
[0477] Next, a first metal oxide film having a thickness of 30 nm was formed on the first gate insulating layer. The first metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was room temperature. A mixed gas of oxygen gas and argon gas was used as the film formation gas, and the oxygen flow rate ratio was set to 10%.
[0478] Next, heat treatment was performed at 370°C for 1 hour in a nitrogen atmosphere, and then heat treatment was performed at 370°C for 1 hour in a mixed gas atmosphere of nitrogen and oxygen (nitrogen gas flow rate: oxygen gas flow rate = 1:1). An oven was used for the heat treatment.
[0479] Next, the first metal oxide film was processed into islands to form a first metal oxide layer.
[0480] Subsequently, a second silicon oxynitride film having a thickness of 5 nm, a third silicon oxynitride film having a thickness of 130 nm, and a fourth silicon oxynitride film having a thickness of 5 nm were formed in this order as a second gate insulating layer.
[0481] The second silicon oxynitride film was formed (film formation condition 1) by PECVD using a mixed gas of silane gas with a flow rate of 24 sccm and nitrous oxide gas with a flow rate of 18000 sccm under conditions of a pressure of 200 Pa and a film formation power of 130 W. The substrate temperature during film formation was 350° C. The second silicon oxynitride film corresponds to the insulating layer 110a described in the first embodiment.
[0482] The third silicon oxynitride film was formed (film formation condition 2) by PECVD using a mixed gas of silane gas with a flow rate of 200 sccm and nitrous oxide gas with a flow rate of 10,000 sccm under conditions of a pressure of 300 Pa and a film formation power of 750 W. The substrate temperature during film formation was 350° C. The third silicon oxynitride film corresponds to the insulating layer 110c described in the first embodiment.
[0483] The fourth silicon oxynitride film was formed (film formation condition 3) by PECVD using a mixed gas of silane gas at a flow rate of 20 sccm and nitrous oxide gas at a flow rate of 3000 sccm under conditions of a pressure of 40 Pa and a film formation power of 500 W. The substrate temperature during film formation was 350° C. The fourth silicon oxynitride film corresponds to the insulating layer 110b shown in the first embodiment.
[0484] The deposition rates and etching rates of the second silicon oxynitride film (deposition condition 1), the third silicon oxynitride film (deposition condition 2), and the fourth silicon oxynitride film (deposition condition 3) are shown in Table 2. In Table 2, etching rate 1 indicates the etching rate in the etchant shown in Example 1, and etching rate 2 indicates the etching rate in 0.5 weight % hydrofluoric acid.
[0485] [Table 2]
[0486] Subsequently, a heat treatment was carried out for 1 hour at 370° C. in a nitrogen atmosphere using an oven.
[0487] Next, a second metal oxide film having a thickness of 20 nm was formed on the fourth silicon oxynitride film. The second metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was 200°C. Oxygen gas (oxygen flow rate ratio 100%) was used as the film formation gas.
[0488] Next, an ITSO film having a thickness of 10 nm and a copper film having a thickness of 100 nm were formed in this order on the second metal oxide film. The ITSO film and the copper film were formed by a sputtering method. The ITSO film was formed using an ITSO target (In 2 O 3 :SnO 2 :SiO 2 = 85:10:5 [weight ratio]) was used. A Cu target was used for depositing the copper film.
[0489] Next, a resist mask was formed on the copper film, and the second metal oxide film, the ITSO film, and the copper film were processed to form a second metal oxide layer, an ITSO layer, and a copper layer. A wet etching method was used for the processing. The etchant can be referred to in the description of Example 1 above, so a detailed description is omitted.
[0490] Next, the second silicon oxynitride film was etched using the resist mask to form a second gate insulating layer. The etching was performed by dry etching. After that, the resist mask was removed.
[0491] Next, a fourth silicon nitride film having a thickness of 100 nm and a fifth silicon oxynitride film having a thickness of 300 nm were formed in this order as a protective layer covering the transistor. The fourth silicon nitride film and the fifth silicon oxynitride film were formed by a plasma CVD method, and the substrate temperature during the film formation was set to 350°C.
[0492] Through the above steps, sample A was obtained.
[0493] <Cross-section observation of sample> Next, sample A was sliced using a focused ion beam (FIB), and the cross section of sample A was observed using a STEM.
[0494] STEM images of the cross section of sample A are shown in Figures 27(A) and 27(B). Figure 27(A) is a transmission electron image (TE image) at 100,000x magnification. Figure 27(B) is a Z contrast image (ZC image) at 100,000x magnification of the same location as Figure 27(A). In a Z contrast image, materials with higher atomic numbers appear brighter. As shown in Figures 27(A) and 27(B), it was confirmed that no undercuts occurred and that the shape was good. EXAMPLES
[0495] In this example, a transistor (sample B1) corresponding to the transistor 100B shown in Fig. 3 was fabricated and its electrical characteristics were evaluated. In addition, a transistor (sample B2) which does not include the conductive layer 106 serving as the first gate electrode of the transistor 100B was also fabricated and its electrical characteristics were similarly evaluated.
[0496] <Sample preparation> The structure of the fabricated transistor can be that of the transistor 100B illustrated in FIG.
[0497] The description of the second embodiment can be applied to the formation of the fourth silicon nitride film, which is a protective layer, and the fifth silicon oxynitride film, so detailed description thereof will be omitted.
[0498] Next, a part of the protective layer covering the transistor was opened, and a 100 nm thick molybdenum film was formed by sputtering, which was then processed to obtain source and drain electrodes. After that, an acrylic resin film with a thickness of about 1.5 μm was formed as a planarizing layer, and a heat treatment was performed under conditions of a nitrogen atmosphere at a temperature of 250°C for 1 hour.
[0499] Through the above steps, a transistor was formed on a glass substrate.
[0500] <Transistor Id-Vg characteristics> Next, the Id-Vg characteristics of the transistor fabricated as described above were measured.
[0501] As for the measurement conditions of the Id-Vg characteristics of the transistor, the voltage applied to the first gate electrode (hereinafter also referred to as the gate voltage (Vg)) and the voltage applied to the second gate electrode (hereinafter also referred to as the voltage (Vbg)) were applied in steps of 0.25 V from -15 V to +20 V. In addition, the voltage applied to the source electrode (hereinafter also referred to as the source voltage (Vs)) was set to 0 V (common), and the voltage applied to the drain electrode (hereinafter also referred to as the drain voltage (Vd)) was set to 0.1 V and 5.1 V.
[0502] FIG. 28 shows the Id-Vg characteristics of the transistor. In FIG. 28, sample B1 having a first gate electrode is shown in the upper row, and sample B2 not having a first gate electrode is shown in the lower row. Also, conditions with different transistor channel lengths are shown in the horizontal direction, and three types of transistors with channel lengths of 2 μm, 3 μm, and 6 μm and channel widths of 50 μm are shown. In FIG. 28, the horizontal axis shows gate voltage (Vg), the left vertical axis shows drain current (Id), and the right vertical axis shows saturation mobility (μFE) at Vd=5.1 V. In FIG. 28, the horizontal axis is shown in a linear scale, with Vg=-15 V at the left end and Vg=20 V at the right end. The left vertical axis is shown in a log scale, with Id=1×10 -12 A, and the upper end is Id=1×10 -2 A. The vertical axis on the right is a linear scale, with the bottom end at μFE=0 cm 2 / Vs, and the upper limit is μFE=100cm 2 / Vs. For each sample, the Id-Vg characteristics of 20 transistors were measured.
[0503] As shown in FIG. 28, good electrical characteristics were obtained in all samples. EXAMPLES
[0504] In this example, a sample (sample C) corresponding to the transistor 100E shown in FIG. 7 was fabricated, and the cross-sectional shape was evaluated.
[0505] <Sample preparation> First, a titanium film having a thickness of 30 nm and a copper film having a thickness of 100 nm were formed in this order on a glass substrate by sputtering, and then processed to obtain a first gate electrode.
[0506] Next, a first silicon nitride film having a thickness of 50 nm, a second silicon nitride film having a thickness of 200 nm, a third silicon nitride film having a thickness of 50 nm, and a first silicon oxynitride film having a thickness of 3 nm were deposited in this order as a first gate insulating layer. The first gate insulating layer was deposited by plasma CVD, and the substrate temperature during deposition was 350°C.
[0507] Next, a first metal oxide film having a thickness of 30 nm was formed on the first gate insulating layer. The first metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was room temperature. A mixed gas of oxygen gas and argon gas was used as the film formation gas, and the oxygen flow rate ratio was set to 10%.
[0508] Next, heat treatment was performed at 370°C for 1 hour in a nitrogen atmosphere, and then heat treatment was performed at 370°C for 1 hour in a mixed gas atmosphere of nitrogen and oxygen (nitrogen gas flow rate: oxygen gas flow rate = 1:1). An oven was used for the heat treatment.
[0509] Next, the first metal oxide film was processed into islands to form a first metal oxide layer.
[0510] Next, a second silicon oxynitride film with a thickness of 5 nm, a third silicon oxynitride film with a thickness of 125 nm, and a fourth silicon oxynitride film with a thickness of 10 nm were deposited in this order as a second gate insulating layer. The second gate insulating layer was deposited by plasma CVD, and the substrate temperature during deposition was set to 350°C.
[0511] The second silicon oxynitride film was formed under the film formation condition 1 shown in Example 2, the third silicon oxynitride film was formed under the film formation condition 2, and the fourth silicon oxynitride film was formed under the film formation condition 3.
[0512] Subsequently, a heat treatment was carried out for 1 hour at 370° C. in a nitrogen atmosphere using an oven.
[0513] Next, a second metal oxide film having a thickness of 20 nm was formed on the fourth silicon oxynitride film. The second metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was 200°C. Oxygen gas (oxygen flow rate ratio 100%) was used as the film formation gas.
[0514] Next, an ITSO film having a thickness of 10 nm and a copper film having a thickness of 100 nm were formed in this order on the second metal oxide film. The ITSO film and the copper film were formed by a sputtering method. The ITSO film was formed using an ITSO target (In 2 O 3 :SnO 2 :SiO 2 = 85:10:5 [weight ratio]) was used. A Cu target was used for depositing the copper film.
[0515] Next, a resist mask was formed on the copper film, and the second metal oxide film, the ITSO film, and the copper film were processed to form a second metal oxide layer, an ITSO layer, and a copper layer. A wet etching method was used for the processing. The etchant can be referred to in the description of Example 1 above, so a detailed description is omitted.
[0516] Next, the second silicon oxynitride film was etched using the resist mask to form a second gate insulating layer. The etching was performed by dry etching. After that, the resist mask was removed.
[0517] Next, a fourth silicon nitride film having a thickness of 100 nm and a fifth silicon oxynitride film having a thickness of 300 nm were formed in this order as a protective layer covering the transistor. The fourth silicon nitride film and the fifth silicon oxynitride film were formed by a plasma CVD method, and the substrate temperature during the film formation was set to 350°C.
[0518] Through the above steps, sample C was obtained.
[0519] <Cross-section observation of sample> Next, sample C was sliced by a focused ion beam (FIB), and the cross section of sample C was observed by STEM.
[0520] STEM images of the cross section of sample C are shown in Figures 29(A) and 29(B). Figure 29(A) is a transmission electron image (TE image) at a magnification of 100,000 times. Figure 29(B) is a Z-contrast image (ZC image) at a magnification of 100,000 times at the same location as Figure 29(A). As shown in Figures 29(A) and 29(B), it was confirmed that no undercut occurred and that the shape was good. It was also confirmed that the ends of the metal oxide layer, ITSO layer, and copper layer were located inside the ends of the silicon oxynitride layer, and that the ends of the copper layer were located inside the ends of the ITSO layer and copper layer. It was also confirmed that the width of the region corresponding to region 108L shown in Figure 7(B) was about 200 nm. EXAMPLES
[0521] In this example, a transistor (sample D) corresponding to the transistor 100E shown in FIG. 7 was fabricated, and its electrical characteristics were evaluated.
[0522] <Sample preparation> The structure of the fabricated transistor can be that of the transistor 100E illustrated in FIG.
[0523] The description of the fourth embodiment can be applied to the formation of the fourth silicon nitride film, which is a protective layer, and the fifth silicon oxynitride film, so detailed description thereof will be omitted.
[0524] Next, a part of the protective layer covering the transistor was opened, and a 30 nm thick titanium film and a 100 nm thick copper film were formed in that order by sputtering, and then processed to obtain source and drain electrodes. After that, an acrylic resin film with a thickness of about 1.5 μm was formed as a planarizing layer, and a heat treatment was performed under conditions of a nitrogen atmosphere at a temperature of 250°C for 1 hour.
[0525] Through the above steps, a transistor was formed on a glass substrate.
[0526] <Transistor Id-Vg characteristics> Next, the Id-Vg characteristics of the transistor fabricated as described above were measured.
[0527] As for the measurement conditions of the Id-Vg characteristics of the transistor, the voltage applied to the first gate electrode (hereinafter also referred to as the gate voltage (Vg)) and the voltage applied to the second gate electrode (hereinafter also referred to as the voltage (Vbg)) were applied in steps of 0.25 V from -15 V to +20 V. In addition, the voltage applied to the source electrode (hereinafter also referred to as the source voltage (Vs)) was set to 0 V (common), and the voltage applied to the drain electrode (hereinafter also referred to as the drain voltage (Vd)) was set to 0.1 V and 5.1 V.
[0528] The Id-Vg characteristics of the transistor are shown in Figure 30. In Figure 30, conditions with different transistor channel lengths are shown vertically, and four types of transistors with channel lengths of 1.5 μm, 2 μm, 3 μm, and 6 μm and channel widths of 50 μm are shown. In Figure 30, the horizontal axis is shown in a linear scale, with Vg = -15 V at the left end and Vg = 20 V at the right end. The left vertical axis is shown in a log scale, with Id = 1 x 10 -12 A, and the upper end is Id=1×10 -2 A. The vertical axis on the right is a linear scale, with the bottom end at μFE=0 cm 2 / Vs, and the upper limit is μFE=100cm 2 / Vs. For each sample, the Id-Vg characteristics of 20 transistors were measured.
[0529] As shown in FIG. 30, good electrical characteristics were obtained even in a transistor with a short channel length. EXAMPLES
[0530] In this example, samples (sample E1 and sample E2) with a laminated structure of an insulating film, a metal oxide film, a functional film, and a conductive film were prepared, and the absorbed water of the insulating film was evaluated. The cross-sectional structure of sample E1 is shown in Figure 31(A), and the cross-sectional structure of sample E2 is shown in Figure 31(B).
[0531] <Sample preparation> First, a first silicon oxynitride film 210A having a thickness of 5 nm, a second silicon oxynitride film 210B having a thickness of 130 nm, and a third silicon oxynitride film 210C were formed in this order as an insulating film 210 on a glass substrate 200. The first silicon oxynitride film 210A was formed under the film formation condition 1 shown in Example 2, the second silicon oxynitride film 210B was formed under the film formation condition 2, and the third silicon oxynitride film 210C was formed under the film formation condition 3. In addition, the thickness of the third silicon oxynitride film 210C of sample E1 was 5 nm, and the thickness of the third silicon oxynitride film 210C of sample E2 was 10 nm.
[0532] Subsequently, a heat treatment was carried out for 1 hour at 370° C. in a nitrogen atmosphere using an oven.
[0533] Subsequently, a metal oxide film 214 having a thickness of 20 nm was formed on the third silicon oxynitride film 210C. The metal oxide film 214 was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was 200° C. Oxygen gas (oxygen flow rate ratio 100%) was used as the film formation gas.
[0534] Next, an ITSO film 213 having a thickness of 10 nm and a copper film 212 having a thickness of 100 nm were formed in this order on the metal oxide film 214. The ITSO film 213 and the copper film 212 were formed by a sputtering method. The ITSO film 213 was formed using an ITSO target (In 2 O 3 :SnO 2 :SiO 2=85:10:5 [by weight]) was used. For the formation of the copper film 212, a Cu target was used.
[0535] Subsequently, the metal oxide film 214, the ITSO film 213, and the copper film 212 were removed by a wet etching method. For both sample E1 and sample E2, the etchant temperature during wet etching was set to 30 °C, and the etching time was set to 60 sec. Since the description of the etchant in Example 1 above can be referred to, a detailed explanation is omitted.
[0536] Subsequently, the film thickness was measured. From the measurement results of the film thickness, it was confirmed that in sample E1, a part of the surface side of the third silicon oxynitride film 210C and the second silicon oxynitride film 210B was also removed by the above wet etching treatment, and the surface of the second silicon oxynitride film 210B was exposed. Similarly, it was confirmed that in sample E2, a part of the surface side of the third silicon oxynitride film 210C was removed, and the surface of the third silicon oxynitride film 210C was exposed.
[0537] Through the above steps, sample E1 and sample E2 were obtained.
[0538] <TDS analysis> Subsequently, the desorbed gas from sample E1 and sample E2 was evaluated using thermal desorption spectrometry (TDS). In the TDS measurement, the substrate temperature was raised from about 50 °C to about 550 °C at a heating rate of 30 °C / min.
[0539] The TDS analysis results of sample E1 are shown in Fig. 32(A), and those of sample E2 are shown in Fig. 32(B). In Fig. 32(A) and Fig. 32(B), the horizontal axis represents the substrate temperature (Tsub), and the vertical axis represents the detection intensity (Intensity) of the mass-to-charge ratio 18 (M / z = 18). The gas with a mass-to-charge ratio of 18 (M / z = 18) is mainly water (H 2 2O) molecules.
[0540] As shown in Fig. 32(A), in sample E1, a peak with a mass-to-charge ratio of 18 (M / z = 18) was observed near Tsub = 100°C. The peak observed near Tsub = 100°C is considered to be due to adsorbed water on the sample surface. It is considered that the surface of the second silicon oxynitride film 210B was exposed, and thus water in the atmosphere was adsorbed on the surface of the second silicon oxynitride film 210B.
[0541] 32(B), the peak at a mass-to-charge ratio of 18 (M / z=18) in sample E2 was very small. Although the surface of the third silicon oxynitride film 210C was exposed, it is considered that the adsorption of water from the atmosphere was suppressed because a film that is difficult for water to adsorb was used for the third silicon oxynitride film 210C. EXAMPLES
[0542] In this example, the effect of impurities including hydrogen on metal oxides was evaluated.
[0543] For the evaluation, a sample was used in which a metal oxide film with a thickness of 200 nm was formed on a glass substrate. The metal oxide film was made of In-Ga-Zn oxide.
[0544] The metal oxide film used in this embodiment was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.4 Pa and a power supply of 0.2 kW (DC). The substrate temperature during film formation was 350°C. A mixed gas of oxygen gas and argon gas was used as the film formation gas, and the oxygen flow rate ratio was 33%. The film composition of the sample formed using a target with a composition of In:Ga:Zn=4:2:4.1 [atomic ratio] is approximately In:Ga:Zn=4:2:3 [atomic ratio]. The glass substrate was heated immediately before the metal oxide film was formed to remove water adsorbed on the glass substrate. The glass substrate was heated at 350°C for 5 minutes in a vacuum atmosphere.
[0545] After the metal oxide film was formed, the surface of the metal oxide film was exposed to a clean room atmosphere for about one week.
[0546] Next, the samples were subjected to heat treatment at 13 different temperatures: none, 250°C for 10 min, 250°C for 20 min, 250°C for 30 min, 250°C for 60 min, 300°C for 10 min, 300°C for 20 min, 300°C for 30 min, 300°C for 60 min, 350°C for 10 min, 350°C for 20 min, 350°C for 30 min, and 350°C for 60 min. The heat treatment was performed in a vacuum atmosphere.
[0547] <Evaluation of hydrogen concentration> The hydrogen concentration in the metal oxide film of the above-mentioned sample was evaluated using secondary ion mass spectrometry. The SIMS measurement was performed using a CAMECA IMS-6f, and the primary ion species was Cs + The primary acceleration voltage was 5.0 kV, and the detection area was 30 μm in diameter. The detection limit (BG) was approximately 5 × 10 17 atoms / cm 3 It was.
[0548] Figure 33(A) shows the hydrogen concentration profiles of the sample not subjected to heat treatment (labeled "none") and the samples heat-treated at 250°C for 10, 20, 30, and 60 min. Figure 33(B) shows the hydrogen concentration profiles of the sample not subjected to heat treatment and the samples heat-treated at 300°C for 10, 20, 30, and 60 min. Figure 34(A) shows the hydrogen concentration profiles of the sample not subjected to heat treatment and the samples heat-treated at 350°C for 10, 20, 30, and 60 min.
[0549] In FIG. 33(A), FIG. 33(B) and FIG. 34(A), the horizontal axis indicates the depth from the surface of the metal oxide film, and the vertical axis indicates the hydrogen concentration (H Concentration).
[0550] As shown in Figure 33(A), the hydrogen concentration on the surface side of the metal oxide film was higher under the condition of 250°C for 10 minutes compared to the condition without heat treatment. It is believed that water was adsorbed onto the metal oxide film surface by exposing the metal oxide film surface to the clean room atmosphere, and the hydrogen contained in the adsorbed water was diffused into the metal oxide film by the heat treatment. In addition, the hydrogen concentration in the metal oxide film tended to increase as the heat treatment time at 250°C was longer. It is believed that the amount of hydrogen diffusing into the metal oxide film increased as the heat treatment time was longer.
[0551] As shown in Figure 33(B), compared to the condition without heat treatment, the hydrogen concentration in the metal oxide film tended to be higher under the condition of heat treatment at 300°C. In addition, no particular difference was observed depending on the heat treatment time.
[0552] As shown in Figure 34(A), the hydrogen concentration in the metal oxide film was higher at 350°C for 10 minutes compared to the condition without heat treatment. Also, the hydrogen concentration tended to be lower on the surface side of the metal oxide film compared to the glass substrate side. It is believed that the heat treatment at 350°C caused hydrogen that had once diffused into the metal oxide film to be desorbed from the metal oxide surface side. Also, the longer the heating time at 350°C was, the lower the hydrogen concentration in the metal oxide film, and in particular the hydrogen concentration on the surface side of the metal oxide film. It is believed that the longer the heat treatment time, the more hydrogen was desorbed from the metal oxide surface side.
[0553] <Evaluation of carrier density> The carrier density was evaluated for the sample under the above-mentioned 250°C 10 min condition.
[0554] In this example, the carrier density in the thickness direction of the metal oxide film was evaluated. Specifically, the thickness and resistance were measured, and then the surface side was partially etched away to reduce the thickness, and the thickness and resistance were measured again.
[0555] The carrier density was calculated from the resistivity obtained by the resistance measurement. When calculating the carrier density, the mobility μ of the metal oxide was set to 16.50 cm2 / V s, and the charge q of the electron is 1.602×10 -19 I chose C.
[0556] The carrier density and hydrogen concentration in the metal oxide film are shown in Figure 34(B). In Figure 34(B), the horizontal axis indicates the depth from the surface of the metal oxide film, and the vertical axis indicates the carrier density and the hydrogen concentration (H Concentration). Note that the hydrogen concentration shown in Figure 34(B) is the same data as the hydrogen concentration shown in Figure 33(A).
[0557] As shown in Figure 34(B), the hydrogen concentration and carrier density in the thickness direction of the metal oxide film are almost the same, which suggests that hydrogen in the metal oxide film generates carriers. Therefore, it was found that when a metal oxide is used as the semiconductor layer, it is preferable to form a gate insulating layer immediately after forming the semiconductor layer. EXAMPLES
[0558] In this example, samples were fabricated using different heat treatment conditions after the formation of the first metal oxide film, and their electrical characteristics were evaluated. In this example, a transistor (samples F1 to F4) corresponding to the transistor 100A shown in FIG. 2 and a transistor (samples G1 to G4) corresponding to the transistor 100 shown in FIG. 1 were fabricated.
[0559] <Sample preparation> First, a tungsten film having a thickness of about 100 nm was formed on a glass substrate by sputtering, and then processed to obtain a first gate electrode.
[0560] Next, a first silicon nitride film having a thickness of 50 nm, a second silicon nitride film having a thickness of 200 nm, a third silicon nitride film having a thickness of 50 nm, and a first silicon oxynitride film having a thickness of 3 nm were deposited in this order as a first gate insulating layer. The first gate insulating layer was deposited by plasma CVD, and the substrate temperature during deposition was 350°C.
[0561] Next, a first metal oxide film having a thickness of 30 nm was formed on the first gate insulating layer. The first metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was room temperature. A mixed gas of oxygen gas and argon gas was used as the film formation gas, and the oxygen flow rate ratio was set to 10%.
[0562] Next, a heat treatment was performed using an oven. Samples F1 and G1 were heated in a nitrogen atmosphere at 370°C for 1 hour, and then heated in a nitrogen and oxygen mixed gas atmosphere (nitrogen gas flow rate: oxygen gas flow rate = 1:1) at 370°C for 1 hour. Samples F2 and G2 were heated in a nitrogen atmosphere at 370°C for 2 hours. Samples F3 and G3 were heated in a nitrogen and oxygen mixed gas atmosphere (nitrogen gas flow rate: oxygen gas flow rate = 1:1) at 370°C for 2 hours. Samples F4 and G4 were heated in a CDA atmosphere at 370°C for 2 hours.
[0563] Next, the first metal oxide film was processed into islands to form a first metal oxide layer.
[0564] Next, a second silicon oxynitride film with a thickness of 5 nm, a third silicon oxynitride film with a thickness of 125 nm, and a fourth silicon oxynitride film with a thickness of 10 nm were deposited in this order as a second gate insulating layer. The second gate insulating layer was deposited by plasma CVD, and the substrate temperature during deposition was set to 350°C.
[0565] The second silicon oxynitride film was formed under the film formation condition 1 shown in Example 2, the third silicon oxynitride film was formed under the film formation condition 2, and the fourth silicon oxynitride film was formed under the film formation condition 3.
[0566] Subsequently, a heat treatment was carried out for 1 hour at 370° C. in a nitrogen atmosphere using an oven.
[0567] Next, a second metal oxide film having a thickness of 20 nm was formed on the fourth silicon oxynitride film. The second metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) under conditions of a pressure of 0.6 Pa and a power supply of 2.5 kW. The substrate temperature during film formation was 200°C. Oxygen gas (oxygen flow rate ratio 100%) was used as the film formation gas.
[0568] Subsequently, a 50 nm-thick molybdenum film, a 200 nm-thick aluminum film, and a 50 nm-thick titanium film were formed in this order on the second metal oxide film. The molybdenum film, the aluminum film, and the titanium film were formed by a sputtering method.
[0569] The aluminum film used in this embodiment was formed by sputtering using an Al target under conditions of a pressure of 0.3 Pa and a power supply of 10 kW (DC). The substrate temperature during film formation was 70° C. Argon gas was used as the film formation gas. The molybdenum film and titanium film formation can be performed as described in Example 1 above, and detailed explanations will be omitted.
[0570] Then, a resist mask was formed on the titanium film, and the second metal oxide film, the molybdenum film, the aluminum film, and the titanium film were processed to form a second metal oxide layer, a molybdenum layer, an aluminum layer, and a titanium layer. A wet etching method was used for the processing. The etchant can be referred to in the description of the above-mentioned Example 1, so a detailed description is omitted.
[0571] Next, the second silicon oxynitride film was etched using the resist mask to form a second gate insulating layer. The etching was performed by dry etching. After that, the resist mask was removed.
[0572] Next, a fourth silicon nitride film having a thickness of 100 nm and a third silicon oxynitride film having a thickness of 300 nm were formed in this order as a protective layer covering the transistor. The fourth silicon nitride film and the third silicon oxynitride film were formed by a plasma CVD method, and the substrate temperature during the film formation was set to 350°C.
[0573] Next, a part of the protective layer covering the transistor was opened, and a 100 nm thick molybdenum film was formed by sputtering, which was then processed to obtain source and drain electrodes. After that, an acrylic resin film with a thickness of about 1.5 μm was formed as a planarizing layer, and a heat treatment was performed under conditions of a nitrogen atmosphere at a temperature of 250°C for 1 hour.
[0574] Through the above steps, a transistor was formed on a glass substrate.
[0575] <Transistor Id-Vg characteristics> Next, the Id-Vg characteristics of the transistor fabricated as described above were measured.
[0576] As for the measurement conditions of the Id-Vg characteristics of the transistor, the voltage applied to the first gate electrode (hereinafter also referred to as the gate voltage (Vg)) and the voltage applied to the second gate electrode (hereinafter also referred to as the voltage (Vbg)) were applied in steps of 0.25 V from -15 V to +20 V. In addition, the voltage applied to the source electrode (hereinafter also referred to as the source voltage (Vs)) was set to 0 V (common), and the voltage applied to the drain electrode (hereinafter also referred to as the drain voltage (Vd)) was set to 0.1 V and 5.1 V.
[0577] FIG. 35 shows the Id-Vg characteristics of the transistors in samples F1 to F4, and FIG. 36 shows the Id-Vg characteristics of the transistors in samples G1 to G4. In FIG. 35 and FIG. 36, the heat treatment conditions after the formation of the first metal oxide film are shown in the horizontal direction. Also, the conditions of different channel lengths of the transistors are shown in the vertical direction, and three types of transistors with channel lengths of 2 μm, 3 μm, and 6 μm and channel widths of 50 μm are shown. In FIG. 35 and FIG. 36, the horizontal axis shows the gate voltage (Vg), the left vertical axis shows the drain current (Id), and the right vertical axis shows the saturation mobility (μFE) at Vd=5.1 V. In FIG. 35 and FIG. 36, the horizontal axis is shown on a linear scale, with Vg=−15 V at the left end and Vg=20 V at the right end. The left vertical axis is shown on a log scale, with Id=1×10 -12 A, and the upper end is Id=1×10 -2 A. The vertical axis on the right is a linear scale, with the bottom end at μFE=0 cm 2 / Vs, and the upper limit is μFE=100cm 2 / Vs. For each sample, the Id-Vg characteristics of 20 transistors were measured.
[0578] As shown in FIGS. 35 and 36, good electrical characteristics were obtained in all samples.
[0579] <Transistor reliability> Next, the reliability of the transistor fabricated as described above was evaluated.
[0580] A gate bias stress test (GBT test) was conducted to evaluate the reliability. In the GBT test, the substrate on which the transistor was formed was kept at 60°C, and a voltage of 0.1 V was applied to the drain of the transistor and 20 V to the gate, and this condition was maintained for one hour. The test environment was dark.
[0581] The threshold voltage change (ΔVth) was evaluated before and after the gate bias stress test. For transistors with a channel length of 3 μm and a channel width of 50 μm, the threshold voltage change (ΔVth) of samples F1 to F4 is shown in FIG. 37A, and the threshold voltage change (ΔVth) of samples G1 to G4 is shown in FIG. 37B.
[0582] As shown in FIGS. 37A and 37B, it was confirmed that the variation in threshold voltage of the fabricated transistor was extremely small.
[0583] From the above, it was confirmed that the transistor of one embodiment of the present invention has favorable electrical characteristics and high reliability. [Explanation of symbols]
[0584] 100: transistor, 100A: transistor, 100B: transistor, 100C: transistor, 100D: transistor, 100E: transistor, 102: substrate, 103: insulating layer, 106: conductive layer, 108: semiconductor layer, 108L: region, 108N: region, 110: insulating layer, 110a: insulating layer, 110b: insulating layer, 110c: insulating layer, 110f: insulating film, 112: conductive layer, 112f: conductive film, 113: functional layer, 113 f: functional film, 114: metal oxide layer, 114f: metal oxide film, 115: resist mask, 116: insulating layer, 118: insulating layer, 120a: conductive layer, 120b: conductive layer, 141a: opening, 141b: opening, 142: opening, 200: glass substrate, 210: insulating film, 210A: silicon oxynitride film, 210B: silicon oxynitride film, 210C: silicon oxynitride film, 212: copper film, 213: ITSO film, 214: metal oxide film
Claims
1. A method for manufacturing a semiconductor device having a transistor, comprising the steps of: forming a first conductive layer on a substrate; forming a first insulating film on the first conductive layer; forming a semiconductor layer containing indium, gallium, and zinc on the first insulating film; forming a second insulating film on the semiconductor layer; forming a first metal oxide film containing indium on the second insulating film at an oxygen flow rate of 65% or more and 100% or less; After forming the first metal oxide film, a heat treatment is performed; After the heat treatment, a second metal oxide film containing indium tin oxide is formed on the first metal oxide film; forming a conductive film containing copper on the second metal oxide film; forming a resist mask on the copper-containing conductive film; After the resist mask is formed, the second insulating film, the first metal oxide film, the second metal oxide film, and the copper-containing conductive film are etched by a wet etching method to form an island-shaped insulating layer, a first metal oxide layer, a second metal oxide layer, and a second conductive layer containing copper; forming a third insulating film having an area located above the second conductive layer having copper after the etching; the semiconductor layer has a higher indium composition than the first metal oxide layer; the first metal oxide film and the second metal oxide film have an etching rate in one etchant that is slower than the conductive film containing copper; a third insulating film having a region in contact with a top surface of the semiconductor layer, a region in contact with a side surface of the island-shaped insulating layer, a region in contact with a side surface of the first metal oxide layer, a region in contact with a side surface of the second metal oxide layer, and a region in contact with a side surface and a top surface of the copper-containing conductive layer.
2. A method for manufacturing a semiconductor device having a transistor, comprising: forming a first conductive layer on a substrate; forming a first insulating film on the first conductive layer; forming a semiconductor layer containing indium, gallium, and zinc on the first insulating film; forming a second insulating film on the semiconductor layer; forming a first metal oxide film containing indium on the second insulating film at an oxygen flow rate of 65% or more and 100% or less; After forming the first metal oxide film, a heat treatment is performed; After the heat treatment, a second metal oxide film containing indium tin oxide is formed on the first metal oxide film; forming a conductive film containing copper on the second metal oxide film; forming a resist mask on the copper-containing conductive film; After forming the resist mask, the first metal oxide film, the second metal oxide film, and the copper-containing conductive film are etched by a wet etching method to form a first metal oxide layer, a second metal oxide layer, and a second conductive layer containing copper, which are located inside an outline of the resist mask in a cross-sectional view; forming an island-shaped insulating layer by etching the second insulating film using the resist mask after forming the first metal oxide layer, the second metal oxide layer, and the second conductive layer having copper; forming a third insulating film having a region located above the second conductive layer having copper after forming the island-shaped insulating layer; the semiconductor layer has a higher indium composition than the first metal oxide layer; the first metal oxide film and the second metal oxide film have an etching rate in one etchant that is slower than the conductive film containing copper; a third insulating film having a region in contact with a top surface of the semiconductor layer, a region in contact with a side surface and a top surface of the island-shaped insulating layer, a region in contact with a side surface of the first metal oxide layer, a region in contact with a side surface of the second metal oxide layer, and a region in contact with a side surface and a top surface of the copper-containing conductive layer.
3. A method for manufacturing a semiconductor device having a transistor, comprising: forming a first conductive layer on a substrate; forming a first insulating film on the first conductive layer; forming a semiconductor layer containing indium, gallium, and zinc on the first insulating film; forming a second insulating film on the semiconductor layer; forming a first metal oxide film containing indium on the second insulating film at an oxygen flow rate of 65% or more and 100% or less; After forming the first metal oxide film, a heat treatment is performed; After the heat treatment, a second metal oxide film containing indium tin oxide is formed on the first metal oxide film; forming a conductive film containing copper on the second metal oxide film; forming a resist mask on the copper-containing conductive film; After forming the resist mask, the first metal oxide film, the second metal oxide film, and the copper-containing conductive film are etched by a wet etching method to form a first metal oxide layer, a second metal oxide layer, and a second conductive layer containing copper, which are located inside an outline of the resist mask in a cross-sectional view; forming an island-shaped insulating layer by etching the second insulating film using the resist mask after forming the first metal oxide layer, the second metal oxide layer, and the second conductive layer having copper; forming a third insulating film having a region located above the second conductive layer having copper after forming the island-shaped insulating layer; the semiconductor layer has a higher indium composition than the first metal oxide layer; the conductive film containing copper has an etching rate in one etchant slower than the first metal oxide film and the second metal oxide film; a third insulating film having a region in contact with a top surface of the semiconductor layer, a region in contact with a side surface and a top surface of the island-shaped insulating layer, a region in contact with a side surface of the first metal oxide layer, a region in contact with a top surface of the second metal oxide layer, and a region in contact with a side surface and a top surface of the copper-containing conductive layer.