Laminate and display device comprising the same

The laminate structure with a wavelength conversion, light absorption, and overcoat layers addresses light leakage and unevenness issues, improving color gamut and emission intensity in display devices by controlling layer thickness and refractive indices.

JP2024127828APending Publication Date: 2024-09-20SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024033140
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-08
Filing Date
2024-03-05
Publication Date
2024-09-20

AI Technical Summary

Technical Problem

Display devices face challenges in widening their color gamut due to light leakage through wavelength conversion layers, which can lead to in-plane unevenness in light emission intensity, and existing solutions like light absorption layers often result in structural irregularities.

Method used

A laminate structure is introduced with a wavelength conversion layer, a light absorption layer, and an overcoat layer, where the overcoat layer is 15 μm or less thick, and the refractive indices are carefully controlled to minimize in-plane unevenness.

Benefits of technology

The laminate structure effectively suppresses in-plane unevenness in the light absorption layer, enhancing the color gamut and maintaining consistent light emission intensity by adjusting the thickness and refractive indices of the layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024127828000001
    Figure 2024127828000001
Patent Text Reader

Abstract

To provide a laminate capable of suppressing in-plane unevenness of a light absorbing layer.SOLUTION: A laminate of the present invention comprises a wavelength conversion layer containing luminescent inorganic semiconductor particles, a light absorbing layer, and an overcoat layer provided between the wavelength conversion layer and the light absorbing layer, the overcoat layer having a thickness of 15 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate including an overcoat layer and a display device including the laminate. [Background technology]

[0002] Patent Document 1 describes a curable resin composition containing quantum dots, and a wavelength conversion film formed using the curable resin composition. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-065178 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been a demand for wider color gamuts in display devices. For example, the recommendation Rec. ITU-R BT.2020, which specifies the video format for Super Hi-Vision (SHV), has been published, and there is a demand to further expand the color gamut and thereby increase the coverage rate of the Rec. ITU-R BT.2020 color gamut (the ratio of the color gamut that can be expressed within the Rec. ITU-R BT.2020 color gamut).

[0005] In a display device having a wavelength conversion layer that absorbs primary light from a primary light source and emits wavelength-converted (color-converted) light, not all of the primary light irradiated to the wavelength conversion layer is usually absorbed by the wavelength conversion layer, and some of the light passes through the wavelength conversion layer and leaks to the viewing side. This can be one of the factors that hinder the display device from having a wide color gamut. One solution to this problem is to place a light absorbing layer on the wavelength conversion layer that absorbs the primary light that has passed through the wavelength conversion layer. However, the laminated structure makes it easy for in-plane unevenness to form in the light absorbing layer, and suppressing this is important from the viewpoint of unevenness in the luminous intensity of the entire display device. An object of the present invention is to provide a laminate that can suppress in-plane unevenness in the light absorbing layer. [Means for solving the problem]

[0006] The gist of the present invention is as follows. [1] A wavelength conversion layer containing luminescent inorganic semiconductor particles and a light absorbing layer, an overcoat layer is provided between the wavelength conversion layer and the light absorbing layer; The overcoat layer has a thickness of 15 μm or less. [2] The laminate according to [1], wherein a thickness ratio calculated by (thickness of overcoat layer+thickness of light absorbing layer) / thickness of wavelength conversion layer is 0.100 or more and 5 or less. [3] The laminate according to [1] or [2], wherein the thickness ratio of the light absorbing layer to the thickness of the laminate (light absorbing layer / laminate) is 0.030 or more and 0.300 or less. [4] The laminate according to any one of [1] to [3], which satisfies the following i) and ii): i) the refractive index of the overcoat layer is smaller than the refractive index of the wavelength conversion layer; ii) the refractive index of the overcoat layer is smaller than the refractive index of the light absorbing layer; [5] The laminate according to any one of [1] to [4], wherein the wavelength conversion layer, the light absorbing layer and the overcoat layer have a value represented by Formula 1 of 0.30 or less. {Q 20 / (T 20 +T 30 )} / {Q10 / T 10} …(Formula 1) [In formula 1, Q 10 : Total amount of luminescent inorganic semiconductor particles and organic ligands in the wavelength conversion layer (g) Q 20 :Total amount of colorant in the light absorbing layer (g) T 10 :Thickness of wavelength conversion layer (μm) T 20 : Thickness of light absorbing layer (μm) T 30 : thickness of overcoat layer (μm)] [6] A display device comprising the laminate according to any one of [1] to [5]. Effect of the Invention

[0007] According to the present invention, the laminate further includes an overcoat layer between the wavelength conversion layer and the light absorbing layer, and the thickness of the overcoat layer is adjusted to 15 μm or less, thereby making it possible to suppress in-plane unevenness in the light absorbing layer. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a laminate according to the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the laminate according to the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing an example of a display device according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Laminate> The laminate (preferably an optical laminate) according to the present invention is characterized in that it includes a wavelength converting layer and a light absorbing layer, and an overcoat layer is provided between the wavelength converting layer and the light absorbing layer.

[0010] FIG. 1 is a schematic cross-sectional view showing an example of a laminate according to the present invention. The laminate shown in FIG. 1 includes a wavelength conversion layer 10 and a light absorbing layer 20, and has an overcoat layer 30 between the wavelength conversion layer 10 and the light absorbing layer 20. As in the laminate shown in FIG. 1, the overcoat layer 30 may be directly laminated on the wavelength conversion layer 10, and the overcoat layer 30 and the wavelength conversion layer 10 may be in contact with each other. The light absorbing layer 20 may be directly laminated on the overcoat layer 30, and the light absorbing layer 20 and the overcoat layer 30 may be in contact with each other. Although not shown in FIG. 1, other layers (however, layers different from the wavelength conversion layer 10, the overcoat layer 30, and the light absorbing layer 20) may be present between the overcoat layer 30 and the wavelength conversion layer 10, between the overcoat layer 30 and the light absorbing layer 20, or on the light absorbing layer 20. The light absorbing layer 20 is disposed, for example, on the light extraction direction side of the wavelength conversion layer 10.

[0011] FIG. 2 is a schematic cross-sectional view showing another example of the laminate according to the present invention. As shown in FIG. 2, the laminate according to the present invention may include a first wavelength conversion layer 11 that emits red light and a second wavelength conversion layer 12 that emits green light. In this case, as shown in FIG. 2, the laminate includes the first wavelength conversion layer 11, the first overcoat layer 31, and the first light absorbing layer 21 in this order, and the second wavelength conversion layer 12, the second overcoat layer 32, and the second light absorbing layer 22 in this order. In FIG. 2, instead of providing the first overcoat layer 31 and the second overcoat layer 32, one (integral) overcoat layer may be provided. Similarly, instead of providing the first light absorbing layer 21 and the second light absorbing layer 22, one (integral) light absorbing layer may be provided.

[0012] The thickness of the laminate according to the present invention (hereinafter also referred to as "total thickness") is, for example, 4.0 μm or more and 30 μm or less, preferably 5.0 μm or more and 27 μm or less, and more preferably 6.0 μm or more and 15 μm or less.

[0013] The refractive index of each layer constituting the laminate according to the present invention preferably satisfies at least one of the following relationships i) to iii). In a preferred embodiment, the refractive index of each layer preferably satisfies the following i) and ii), and more preferably satisfies all of the following i) to iii). i) The refractive index of the overcoat layer 30 is smaller than the refractive index of the wavelength conversion layer 10 ii) The refractive index of the overcoat layer 30 is smaller than the refractive index of the light absorbing layer 20. iii) The refractive index of the wavelength conversion layer 10 is greater than the refractive index of the light absorbing layer 20 The refractive index can be measured according to the measurement method described in the Examples section below, and the refractive index of each layer is evaluated at a wavelength of 550 nm.

[0014] In the wavelength ranges of 400 to 465 nm and 530 to 1690 nm, the refractive indexes of the layers constituting the laminate according to the present invention preferably satisfy the relationship wavelength conversion layer>light absorbing layer>overcoat layer. In addition, in the wavelength range of more than 465 nm and less than 530 nm, the refractive indexes of the layers constituting the laminate according to the present invention preferably satisfy the relationship: light absorbing layer>wavelength converting layer>overcoat layer. The refractive index can be measured according to the measurement method described in the Examples section below.

[0015] The laminate according to the present invention can be suitably used as a color conversion member disposed on a primary light source (eg, a blue light source) of a display device.

[0016] 1. Wavelength conversion layer The wavelength conversion layer is a layer that absorbs primary light from a primary light source and emits green or red light, and is preferably a layer that converts the wavelength of the primary light, that is, blue light, into the wavelength of green light or the wavelength of red light.

[0017] The thickness of the wavelength conversion layer is, for example, 1 μm to 20 μm, preferably 1.5 μm to 18 μm, more preferably 1.8 μm to 14 μm, even more preferably 2 μm to 12 μm, and even more preferably 2 μm to 10 μm. If the thickness of the wavelength conversion layer is too small, when the wavelength conversion layer is irradiated with primary light, a proportion of the primary light that is not sufficiently absorbed or scattered by the wavelength conversion layer and transmits through the wavelength conversion layer tends to increase.

[0018] The thickness ratio of the wavelength converting layer to the total film thickness (wavelength converting layer / total film thickness) is, for example, 0.250 or more and 0.990 or less, preferably 0.350 or more and 0.900 or less, and more preferably 0.450 or more and 0.850 or less.

[0019] The refractive index of the wavelength conversion layer is preferably 1.55 or more, more preferably 1.60 or more, even more preferably 1.65 or more, and is preferably 1.85 or less, more preferably 1.80 or less, even more preferably 1.75 or less.

[0020] 2. Light absorbing layer The light absorbing layer is a layer that transmits light in a specific wavelength range and absorbs light in at least a part of the other wavelength ranges. The light emitted from the wavelength conversion layer is emitted from the display device as green light or red light by transmitting through the light absorbing layer. By providing the light absorbing layer, leakage of primary light to the viewing side of the light absorbing layer can be suppressed, thereby enabling the display device to have a wide color gamut. It is particularly desirable for the light absorbing layer to be a color resist layer.

[0021] The wavelength range of light transmitted through the light absorbing layer is a green or red wavelength range. The green wavelength range is, for example, a wavelength range from 495 nm to 585 nm. The red wavelength range is, for example, a wavelength range from 585 nm to 780 nm. The wavelength range of light absorbed by the light absorbing layer is preferably a blue wavelength range, more preferably a wavelength range including 450 nm, for example, a wavelength range from 380 nm to less than 495 nm. 2, the first light absorbing layer 21 transmits light in the red wavelength range. The second light absorbing layer 22 transmits light in the green wavelength range. The wavelength range of light absorbed by the first light absorbing layer 21 and the second light absorbing layer 22 is preferably the blue wavelength range, more preferably a wavelength range including 450 nm, for example, a wavelength range included in the range of 380 nm or more and less than 495 nm.

[0022] The light absorbing layer preferably has an average light transmittance of 98% or more in the wavelength region of 520 nm or more and 780 nm or less. By having an average light transmittance of 98% or more, the emission intensity can be further increased.

[0023] The thickness of the light absorbing layer is, for example, 0.1 μm or more and 30 μm or less, and from the viewpoint of effectively suppressing leakage of primary light (blue light) to the viewing side of the light absorbing layer, it is preferably 0.5 μm or more and 20 μm or less, more preferably 0.7 μm or more and 10 μm or less, even more preferably 0.9 μm or more and 5 μm or less, and still more preferably 1.0 μm or more and 2 μm or less.

[0024] The thickness ratio of the light absorbing layer to the total film thickness (light absorbing layer / total film thickness) is, for example, 0.030 or more and 0.400 or less, preferably 0.030 or more and 0.300 or less, more preferably 0.050 or more and 0.200 or less, and further preferably 0.090 or more and 0.175 or less.

[0025] The refractive index of the light absorbing layer is preferably 1.45 or more, more preferably 1.50 or more, and even more preferably 1.55 or more, and is preferably 1.75 or less, more preferably 1.70 or less, and even more preferably 1.65 or less.

[0026] 3. Overcoat layer The overcoat layer is a layer that can suppress the decrease in luminescence intensity. When a light absorbing layer is arranged, the problem of the decrease in luminescence intensity occurs compared to when the light absorbing layer is not arranged. However, the present inventors have found that by laminating an overcoat layer between the wavelength conversion layer and the light absorbing layer, the decrease in luminescence intensity can be significantly suppressed even with the light absorbing layer. It is particularly preferable that the overcoat layer is a resin layer.

[0027] The thickness of the overcoat layer is 15 μm or less, preferably 12 μm or less. There is a correlation between the thickness of the overcoat layer and the film formability of the light absorbing layer, and by making the thickness of the overcoat layer 15 μm or less, it is possible to suppress the in-plane unevenness of the light absorbing layer. In particular, from the viewpoint of suppressing the film thickness unevenness in the overcoat layer, the thickness of the overcoat layer is more preferably 9 μm or less, even more preferably 7 μm or less, and even more preferably 5 μm or less. The thickness of the overcoat layer is, for example, 0.1 μm or more, preferably 0.4 μm or more, more preferably 0.7 μm or more, even more preferably 1.2 μm or more, and even more preferably 1.8 μm or more. By making the thickness of the overcoat layer 0.1 μm or more, it becomes easy to form an overcoat layer having a uniform thickness, and the unevenness of the film thickness in the overcoat layer can be reduced.

[0028] The thickness ratio of the overcoat layer to the light absorbing layer (overcoat layer / light absorbing layer) is, for example, 0.10 or more and 15 or less, preferably 0.50 or more and 12 or less, and more preferably 0.8 or more and 10 or less.

[0029] The thickness ratio of the overcoat layer to the wavelength converting layer (overcoat layer / wavelength converting layer) is, for example, 0.020 or more and 3 or less, preferably 0.100 or more and 2 or less, and more preferably 0.150 or more and 1 or less.

[0030] The thickness ratio of (overcoat layer+light absorbing layer) / wavelength conversion layer is, for example, 0.100 or more and 5 or less, preferably 0.200 or more and 3 or less, and more preferably 0.250 or more and 1.500 or less.

[0031] The value calculated by (thickness of overcoat layer)×(thickness of light absorbing layer) / (thickness of wavelength conversion layer) is, for example, 0.030 μm or more and 5 μm or less, preferably 0.080 μm or more and 3 μm or less, and more preferably 0.100 μm or more and 2 μm or less.

[0032] The thickness ratio of the overcoat layer to the total film thickness (overcoat layer / total film thickness) is, for example, 0.010 or more and less than 1, preferably 0.050 or more and 0.600 or less, and more preferably 0.100 or more and 0.400 or less.

[0033] The refractive index of the overcoat layer is preferably 1.35 or more, more preferably 1.40 or more, and even more preferably 1.45 or more, and is preferably 1.65 or less, more preferably 1.60 or less, and even more preferably 1.55 or less.

[0034] In the wavelength converting layer, the light absorbing layer and the overcoat layer in the present invention, the value shown in Formula 1 is preferably 0.30 or less, more preferably 0.010 to 0.28, even more preferably 0.015 to 0.25, still more preferably 0.020 to 0.20, and particularly preferably 0.022 to 0.15. Blue light leaking from the wavelength converting layer is usually absorbed by the light absorbing layer. The amount of colorant in the laminate (specifically, the total amount of luminescent inorganic semiconductor particles and organic ligands in the wavelength converting layer (Q 10 ) and the total amount of colorant in the light absorbing layer (Q 20 Controlling the balance between the above is effective from the viewpoints of suppressing blue light leakage and maintaining luminous intensity. In other words, by adjusting the value shown in formula 1 to fall within the above range, it is possible to easily obtain a laminate in which blue light leakage is suppressed and luminous intensity is appropriately maintained. In formula 1, the luminescent inorganic semiconductor particles and organic ligands in the wavelength conversion layer, and the colorant in the light absorbing layer refer to the luminescent inorganic semiconductor particles (A), organic ligands (G) and colorant (I) described later, as appropriate. {Q 20 / (T 20 +T 30 )} / {Q 10 / T 10} …(Formula 1) [In formula 1, Q 10 : Total amount of luminescent inorganic semiconductor particles and organic ligands in the wavelength conversion layer (g) Q 20 :Total amount of colorant in the light absorbing layer (g) T 10 :Thickness of wavelength conversion layer (μm) T 20 : Thickness of light absorbing layer (μm) T 30 : thickness of overcoat layer (μm)]

[0035] <Composition> The wavelength conversion layer can be formed from a composition for forming a wavelength conversion layer (hereinafter also referred to as “composition I”) containing luminescent inorganic semiconductor particles (A) (hereinafter also referred to as “semiconductor particles (A)”). Composition I may contain an organic ligand (G). Composition I may contain a light scattering agent (B). The composition I may contain a resin (C). The composition I may contain a polymerizable compound (D). The composition I may contain a polymerization initiator (E). Composition I may contain a polymerization initiation aid (E1). Composition I may contain an antioxidant (F). Composition I may contain a solvent (J). Composition I may contain a leveling agent (H).

[0036] The light-absorbing layer can be formed from a composition for forming a light-absorbing layer (hereinafter, also referred to as "composition II"). Composition II contains a colorant (I). The composition II may contain a resin (C). The composition II may contain a polymerizable compound (D). Composition II may contain a polymerization initiator (E). Composition II may contain a polymerization initiator coagent (E1). Composition II may contain an antioxidant (F). Composition II may contain a solvent (J). Composition II may contain a leveling agent (H).

[0037] The overcoat layer can be formed from a composition for forming an overcoat layer (hereinafter, also referred to as "composition III"). The composition III may contain a resin (C). The composition III may contain a polymerizable compound (D). The composition III may contain a polymerization initiator (E). The composition III may contain a polymerization initiation aid (E1). Composition III may contain an antioxidant (F). The composition III may contain a solvent (J). Composition III may contain a leveling agent (H). Composition III may contain an ultraviolet absorber. Composition III is substantially free of semiconductor particles (A) and colorant (I). "Substantially free of semiconductor particles (A) and colorant (I)" means that the content of semiconductor particles (A) or colorant (I) relative to the total amount of solids in composition III is preferably 1 mass % or less, more preferably 0.5 mass % or less, still more preferably 0.1 mass % or less, and particularly preferably 0 mass %.

[0038] In this specification, the compounds exemplified as each component may be used alone or in combination of two or more, unless otherwise specified.

[0039] <Luminescent inorganic semiconductor particles (A)> The semiconductor particles (A) absorb the primary light and emit green or red light, and preferably convert the wavelength of blue light, which is the primary light, to a red light wavelength or a green light wavelength.

[0040] In this specification, "blue" refers to all light that is visually recognized as blue (all light having intensity in the blue wavelength range, for example, 380 nm to 495 nm), and is not limited to light of a single wavelength. "Green" refers to all light that is visually recognized as green (all light having intensity in the green wavelength range, for example, 495 nm to 585 nm), and is not limited to light of a single wavelength. "Red" refers to all light that is visually recognized as red (all light having intensity in the red wavelength range, for example, 585 nm to 780 nm), and is not limited to light of a single wavelength. "Yellow" refers to all light that is visually recognized as yellow (all light having intensity in the yellow wavelength range, for example, 560 nm to 610 nm), and is not limited to light of a single wavelength.

[0041] The emission spectrum of the semiconductor particles (A) emitting green light preferably includes a peak having a maximum value in a wavelength range of 500 nm to 560 nm, more preferably includes a peak having a maximum value in a wavelength range of 520 nm to 545 nm, and even more preferably includes a peak having a maximum value in a wavelength range of 525 nm to 535 nm. This can further improve the emission intensity of green light from the display device. The peak preferably has a full width at half maximum of 15 nm to 80 nm, more preferably 15 nm to 60 nm, even more preferably 15 nm to 50 nm, and particularly preferably 15 nm to 45 nm. This can further improve the emission intensity of green light from the display device.

[0042] The emission spectrum of the semiconductor particles (A) emitting red light preferably includes a peak having a maximum value in a wavelength range of 610 nm to 750 nm, more preferably includes a peak having a maximum value in a wavelength range of 620 nm to 650 nm, and even more preferably includes a peak having a maximum value in a wavelength range of 625 nm to 645 nm. This can further improve the emission intensity of red light from the display device. The peak preferably has a full width at half maximum of 15 nm to 80 nm, more preferably 15 nm to 60 nm, even more preferably 15 nm to 50 nm, and particularly preferably 15 nm to 45 nm. This can further improve the emission intensity of red light from the display device.

[0043] Examples of the semiconductor particles (A) include quantum dots and particles composed of a compound having a perovskite crystal structure (hereinafter also referred to as a "perovskite compound"), and quantum dots are preferred. Quantum dots are luminescent semiconductor particles having a particle diameter of 1 nm to 100 nm, which utilize the band gap of a semiconductor to absorb ultraviolet light or visible light (e.g., blue light) and emit light.

[0044] Examples of quantum dots include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, CdHgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZn compounds between group 12 elements and group 16 elements, such as SeTe and HgZnSTe; compounds between group 13 elements and group 15 elements, such as GaN, GaP, GaAs, AlN, AlP, AlAs, InN, InP, InAs, GaNP, GaNAs, GaPAs, AlNP, AlNAs, AlPAs, InNP, InNAs, InPAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, InAlNP, InAlNAs, InAlPAs; and compounds between group 14 elements and group 16 elements, such as PdS and PbSe.

[0045] When the quantum dots contain S or Se, quantum dots whose surfaces are modified with a metal oxide or an organic substance may be used. By using surface-modified quantum dots, it is possible to prevent S or Se from being extracted by a reactive component that is or may be contained in composition I.

[0046] The quantum dots may also have a core-shell structure formed by combining the above compounds, such as particles having a CdSe core and a ZnS shell, or particles having an InP core and a ZnSeS shell.

[0047] Since the energy state of quantum dots depends on their size, it is possible to freely select the emission wavelength by changing the particle diameter. In addition, the emission light from quantum dots has a narrow spectral width, which is advantageous for widening the color gamut of display devices. Furthermore, quantum dots have a high response rate, which is advantageous in terms of the utilization efficiency of primary light.

[0048] The perovskite compound is a compound having a perovskite type crystal structure, which is composed of A, B and X.

[0049] A is a component located at each vertex of a hexahedron with B at the center in the perovskite crystal structure, and is a monovalent cation.

[0050] X represents a component located at each vertex of an octahedron with B at the center in the perovskite crystal structure, and is at least one type of ion selected from the group consisting of halide ions and thiocyanate ions.

[0051] B is a component located at the center of a hexahedron with A at its vertex and an octahedron with X at its vertex in the perovskite crystal structure, and is a metal ion.

[0052] The perovskite compound containing A, B, and X as components is not particularly limited, and may be a compound having any of a three-dimensional structure, a two-dimensional structure, and a pseudo-two-dimensional structure.

[0053] In the case of a three-dimensional structure, perovskite compounds are classified as ABX (3+δ) It is expressed as:

[0054] In the case of the two-dimensional structure, the perovskite compound is A2BX (4+δ) It is expressed as:

[0055] Here, δ is a number that can be appropriately changed depending on the charge balance of B, and is equal to or greater than −0.7 and equal to or less than 0.7.

[0056] A perovskite compound, ABX (3+δ) Preferable specific examples of the compound having a three-dimensional perovskite-type crystal structure represented by the formula: CH3NH3PbBr3, CH3NH3PbCl3, CH3NH3PbI3, CH3NH3PbBr (3-y) I y (0 <y<3)、CH3NH3PbBr (3-y) Cl y (0 <y<3)、(H2N=CH-NH2)PbBr3、(H2N=CH-NH2)PbCl3、(H2N=CH-NH2)PbI3、 CH3NH3Pb (1-a) Ca a Br3(0 <a≦0.7)、CH3NH3Pb (1-a) Sr a Br3(0 <a≦0.7)、CH3NH3Pb (1-a) La a Br (3+δ) (0 <a≦0.7,0<δ≦0.7)、CH3NH3Pb (1-a) Ba a Br3(0 <a≦0.7)、CH3NH3Pb (1-a) Dy a Br (3+δ) (0 <a≦0.7,0<δ≦0.7)、 CH3NH3Pb (1-a) Na a Br (3+δ) (0 <a≦0.7,-0.7≦δ<0)、CH3NH3Pb (1-a) Li a Br (3+δ) (0 <a≦0.7,-0.7≦δ<0)、 CsPb (1-a) Na a Br (3+δ) (0 <a≦0.7,-0.7≦δ<0)、CsPb (1-a) Li a Br (3+δ) (0 <a≦0.7,-0.7≦δ<0)、 CH3NH3Pb (1-a) Na a Br (3+δ-y) I y (0<a≦0.7,-0.7≦δ<0,0<y<3)、CH3NH3Pb (1-a) Li a Br (3+δ-y) I y (0<a≦0.7,-0.7≦δ<0,0<y<3)、CH3NH3Pb (1-a) Na a Br (3+δ-y) Cl y (0<a≦0.7,-0.7≦δ<0,0<y<3)、CH3NH3Pb (1-a) Li a Br (3+δ-y) Cl y (0<a≦0.7,-0.7≦δ<0,0<y<3)、 (H2N=CH-NH2)Pb (1-a) Na a Br (3+δ) (0<a≦0.7,-0.7≦δ<0)、(H2N=CH-NH2)Pb (1-a) Li a Br (3+δ) (0<a≦0.7,-0.7≦δ<0)、(H2N=CH-NH2)Pb (1-a) Na a Br (3+δ-y) I y (0<a≦0.7,-0.7≦δ<0,0<y<3)、(H2N=CH-NH2)Pb (1-a) Na a Br (3+δ-y) Cl y (0<a≦0.7,-0.7≦δ<0,0<y<3)、 CsPbBr3、CsPbCl3、CsPbI3、CsPbBr (3-y) I y (0<y<3)、CsPbBr (3-y) Cl y (0<y<3)、CH3NH3PbBr (3-y) Cl y (0<y<3)、 CH3NH3Pb (1-a) Zn a Br3(0<a≦0.7)、CH3NH3Pb (1-a) Al a Br (3+δ)(0<a≦0.7,0≦δ≦0.7)、CH3NH3Pb (1-a) Co a Br3(0<a≦0.7)、CH3NH3Pb (1-a) Mn a Br3(0<a≦0.7)、CH3NH3Pb (1-a) Mg a Br3(0<a≦0.7)、 CsPb (1-a) Zn a Br3(0<a≦0.7)、CsPb (1-a) Al a Br (3+δ) (0<a≦0.7,0<δ≦0.7)、CsPb (1-a) Co a Br3(0<a≦0.7)、CsPb (1-a) Mn a Br3(0<a≦0.7)、CsPb (1-a) Mg a Br3(0<a≦0.7)、 CH3NH3Pb (1-a) Zn a Br (3-y) I y (0<a≦0.7,0<y<3)、CH3NH3Pb (1-a) Al a Br (3+δ-y) I y (0<a≦0.7,0<δ≦0.7,0<y<3)、CH3NH3Pb (1-a) Co a Br (3-y) I y (0<a≦0.7,0<y<3)、CH3NH3Pb (1-a) Mn a Br (3-y) I y (0<a≦0.7,0<y<3)、CH3NH3Pb (1-a) Mg a Br (3-y) I y (0<a≦0.7,0<y<3)、CH3NH3Pb (1-a) Zn a Br (3-y) Cl y (0<a≦0.7,0<y<3)、CH3NH3Pb (1-a) Al a Br (3+δ-y) Cl y(0 < a ≤ 0.7, 0 < δ ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Co a Br (3+δ-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Mn a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), CH3NH3Pb (1-a) Mg a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), (H2N = CH - NH2)Zn a Br3(0 < a ≤ 0.7), (H2N = CH - NH2)Mg a Br3(0 < a ≤ 0.7), (H2N = CH - NH2)Pb (1-a) Zn a Br (3-y) I y (0 < a ≤ 0.7, 0 < y < 3), (H2N = CH - NH2)Pb (1-a) Zn a Br (3-y) Cl y (0 < a ≤ 0.7, 0 < y < 3), etc. can be mentioned.

[0057] A perovskite compound, A2BX (4+δ) As preferable specific examples of the compound having a two - dimensional perovskite - type crystal structure represented by (C4H9NH3)2PbBr4, (C4H9NH3)2PbCl4, (C4H9NH3)2PbI4, (C7H 15 NH3)2PbBr4, (C7H 15 NH3)2PbCl4, (C7H 15 NH3)2PbI4, (C4H9NH3)2Pb (1-a) Li a Br (4+δ) (0 < a ≤ 0.7, - 0.7 ≤ δ < 0), (C4H9NH3)2Pb (1-a) Na a Br (4+δ) (0 < a ≤ 0.7, - 0.7 ≤ δ < 0), (C4H9NH3)2Pb (1-a) Rb a Br(4+δ) (0<a≦0.7,-0.7≦δ<0)、 (C7H 15 NH3)2Pb (1-a) Na a Br (4+δ) (0<a≦0.7,-0.7≦δ<0)、(C7H 15 NH3)2Pb (1-a) Li a Br (4+δ) (0<a≦0.7,-0.7≦δ<0)、(C7H 15 NH3)2Pb (1-a) RbaBr (4+δ) (0<a≦0.7,-0.7≦δ<0)、 (C4H9NH3)2Pb (1-a) Na a Br (4+δ-y) I y (0<a≦0.7,-0.7≦δ<0,0<y<4)、(C4H9NH3)2Pb (1-a) Li a Br (4+δ-y) I y (0<a≦0.7,-0.7≦δ<0,0<y<4)、(C4H9NH3)2Pb (1-a) Rb a Br (4+δ-y) I y (0<a≦0.7,-0.7≦δ<0,0<y<4)、 (C4H9NH3)2Pb (1-a) Na a Br (4+δ-y) Cl y (0<a≦0.7,-0.7≦δ<0,0<y<4)、(C4H9NH3)2Pb (1-a) Li a Br (4+δ-y) Cl y (0<a≦0.7,-0.7≦δ<0,0<y<4)、(C4H9NH3)2Pb (1-a) Rb a Br (4+δ-y) Cl y (0<a≦0.7,-0.7≦δ<0,0<y<4)、 (C4H9NH3)2PbBr4、(C7H 15 NH3)2PbBr4、 (C4H9NH3)2PbBr (4-y) Cl y(0<y<4)、(C4H9NH3)2PbBr (4-y) I y (0<y<4)、 (C4H9NH3)2Pb (1-a) Zn a Br4(0<a≦0.7)、(C4H9NH3)2Pb (1-a) Mg a Br4(0<a≦0.7)、(C4H9NH3)2Pb (1-a) Co a Br4(0<a≦0.7)、(C4H9NH3)2Pb (1-a) Mn a Br4(0<a≦0.7)、 (C7H 15 NH3)2Pb (1-a) Zn a Br4(0<a≦0.7)、(C7H 15 NH3)2Pb (1-a) Mg a Br4(0<a≦0.7)、(C7H 15 NH3)2Pb (1-a) Co a Br4(0<a≦0.7)、(C7H 15 NH3)2Pb (1-a) Mn a Br4(0<a≦0.7)、 (C4H9NH3)2Pb (1-a) Zn a Br (4-y) I y (0<a≦0.7,0<y<4)、(C4H9NH3)2Pb (1-a) Mg a Br (4-y) I y (0<a≦0.7,0<y<4)、(C4H9NH3)2Pb (1-a) Co a Br (4-y) I y (0<a≦0.7,0<y<4)、(C4H9NH3)2Pb (1-a) Mn a Br (4-y) I y (0<a≦0.7,0<y<4)、 (C4H9NH3)2Pb (1-a) Zn a Br (4-y) Cl y(0 < a ≤ 0.7, 0 < y < 4), (C4H9NH3)2Pb (1-a) Mg a Br (4-y) Cl y (0 < a ≤ 0.7, 0 < y < 4), (C4H9NH3)2Pb (1-a) Co a Br (4-y) Cl y (0 < a ≤ 0.7, 0 < y < 4), (C4H9NH3)2Pb (1-a) Mn a Br (4-y) Cl y Examples include (0 < a ≤ 0.7, 0 < y < 4), etc.

[0058] The semiconductor particles (A) that absorb primary light and emit green light can be used alone or in combination of two or more. Also, the semiconductor particles (A) that absorb primary light and emit red light can be used alone or in combination of two or more.

[0059] The content of the semiconductor particles (A) in Composition I is, for example, 1% by mass or more and 60% by mass or less, preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 50% by mass or less, still more preferably 20% by mass or more and 50% by mass or less, and even more preferably 25% by mass or more and 45% by mass or less, based on the total amount of the solid content of Composition I.

[0060] In this specification, the total amount of the solid content of the composition means the total of the components contained in the composition excluding the solvent (J). The content in the solid content of the composition can be measured by known analytical means such as liquid chromatography or gas chromatography. The content of each component in the solid content of the composition may be calculated from the formulation at the time of preparing the composition.

[0061] In this specification, the content or content ratio of each component means the total content or total content ratio when two or more of these components are contained.

[0062] It is preferable that composition II is substantially free of semiconductor particles (A). "Substantially free of semiconductor particles (A)" means that the content of semiconductor particles (A) relative to the total amount of solids in composition II is preferably 1 mass% or less, more preferably 0.5 mass% or less, even more preferably 0.1 mass% or less, and particularly preferably 0 mass%.

[0063] Composition III does not substantially contain semiconductor particles (A), and the content of semiconductor particles (A) relative to the total amount of solids in composition III is preferably 1 mass % or less, more preferably 0.5 mass % or less, even more preferably 0.1 mass % or less, and particularly preferably 0 mass %.

[0064] <Organic ligand (G)> The semiconductor particles (A) may be present in the composition in a state where the organic ligand (G) is coordinated. The organic ligand (G) is, for example, an organic compound having a polar group that exhibits coordination ability with the semiconductor particles (A). The organic ligand (G) can be coordinated, for example, to the surface of the semiconductor particles (A). The composition can contain one or more types of organic ligands (G).

[0065] It is preferable that at least a part of the molecules of the organic ligand (G) is coordinated to the semiconductor particle (A), and all or almost all of the molecules may be coordinated to the semiconductor particle (A). The inclusion of the organic ligand (G) coordinated to the semiconductor particle (A) can be advantageous from the viewpoint of improving the stability and dispersibility of the semiconductor particle (A) and the luminescence intensity of the wavelength conversion layer.

[0066] The polar group of the organic ligand (G) is, for example, at least one group selected from the group consisting of a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH2). A polar group selected from the group can be advantageous in increasing the coordination ability to the semiconductor particles (A). High coordination ability can contribute to improving the stability and dispersibility of the semiconductor particles (A) in the composition, and improving the luminescence intensity of the wavelength conversion layer. Among them, it is more preferable that the polar group is at least one group selected from the group consisting of a thiol group and a carboxyl group. The organic ligand (G) can have one or more polar groups.

[0067] The organic ligand (G) is, for example, a compound represented by the following formula (x): X A -R X (x) In the formula, X A is the polar group as above, and R X is a monovalent hydrocarbon group which may contain a heteroatom (N, O, S, halogen atom, etc.). The hydrocarbon group may have one or more unsaturated bonds such as a carbon-carbon double bond. The hydrocarbon group may have a linear, branched, or cyclic structure. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 40, and may be 1 to 30. The methylene group contained in the hydrocarbon group may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc.

[0068] base R X may contain a polar group. Specific examples of the polar group include the polar group X A Reference is made to the above description.

[0069] polar group ASpecific examples of organic ligands having a carboxyl group as the carboxyl group include formic acid, acetic acid, and propionic acid, as well as saturated or unsaturated fatty acids. Specific examples of saturated or unsaturated fatty acids include saturated fatty acids such as butyric acid, pentanoic acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid; monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, oleic acid, icosenoic acid, erucic acid, and nervonic acid; and polyunsaturated fatty acids such as linoleic acid, α-linolenic acid, γ-linolenic acid, stearic acid, dihomo-γ-linolenic acid, arachidonic acid, eicosatetraenoic acid, docosadienoic acid, and adrenic acid (docosatetraenoic acid).

[0070] polar group A Specific examples of organic ligands having a thiol group or an amino group as the polar group X include the above-exemplified organic ligands having a thiol group or an amino group as the polar group X A The organic ligand includes an organic ligand in which the carboxy group of an organic ligand having a carboxy group as the substituent is replaced with a thiol group or an amino group.

[0071] In addition to the above, examples of the organic ligand represented by the above formula (x) include compound (G-1) and compound (G-2).

[0072] [Compound (G-1)] The compound (G-1) is a compound having a first functional group and a second functional group. The first functional group is a carboxy group (-COOH), and the second functional group is a carboxy group or a thiol group (-SH). Since the compound (G-1) has a carboxy group and / or a thiol group, it can be a ligand that coordinates to the semiconductor particles (A). The composition may contain only one type of compound (G-1), or may contain two or more types.

[0073] An example of the compound (G-1) is a compound represented by the following formula (G-1a): The compound (G-1) may be an acid anhydride of the compound represented by the formula (G-1a).

[0074] [ka]

[0075] [In the formula, R B represents a divalent hydrocarbon group. B When present, they may be the same or different. The above-mentioned hydrocarbon group may have one or more substituents. When a plurality of substituents are present, they may be the same or different, and they may be bonded to each other to form a ring together with the atom to which they are bonded. -CH2- contained in the above-mentioned hydrocarbon group may be replaced by at least one of -O-, -S-, -SO2-, -CO- and -NH-. and p represents an integer of 1 to 10. R B Examples of the divalent hydrocarbon group represented by the formula (I) include linear hydrocarbon groups, alicyclic hydrocarbon groups, aromatic hydrocarbon groups, and combinations of these groups.

[0076] Examples of the chain hydrocarbon group include a linear or branched alkanediyl group, the number of carbon atoms of which is usually 1 to 50, preferably 1 to 20, and more preferably 1 to 10. Examples of the alicyclic hydrocarbon group include a monocyclic or polycyclic cycloalkanediyl group, the number of carbon atoms of which is usually 3 to 50, preferably 3 to 20, and more preferably 3 to 10. Examples of the aromatic hydrocarbon group include a monocyclic or polycyclic arenediyl group, the number of carbon atoms of which is usually 6 to 20.

[0077] Examples of the substituent that the above-mentioned hydrocarbon group may have include an alkyl group having 1 to 50 carbon atoms, a cycloalkyl group having 3 to 50 carbon atoms, an aryl group having 6 to 20 carbon atoms, a carboxy group, an amino group, a halogen atom, etc. The substituent that the above-mentioned hydrocarbon group may have is preferably a carboxy group, an amino group or a halogen atom.

[0078] When -CH2- contained in the above-mentioned hydrocarbon group is replaced by at least one of -O-, -CO- and -NH-, -CH2- is preferably replaced by at least one of -CO- and -NH-, more preferably -NH-. p is preferably 1 or 2.

[0079] Examples of the compound represented by formula (G-1a) include compounds represented by the following formulas (1-1) to (1-9).

[0080] [ka]

[0081] Specific examples of the compound represented by formula (G-1a) by chemical name include mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutanoic acid, 4-mercaptobutanoic acid, mercaptosuccinic acid, mercaptostearic acid, mercaptooctanoic acid, 4-mercaptobenzoic acid, 2,3,5,6-tetrafluoro-4-mercaptobenzoic acid, L-cysteine, N-acetyl-L-cysteine, 3-mercaptopropionic acid 3-methoxybutyl, 3-mercapto-2-methylpropionic acid, etc. Among them, 3-mercaptopropionic acid and mercaptosuccinic acid are preferred.

[0082] Another example of compound (G-1) is a polycarboxylic acid compound, preferably a compound (G-1b) represented by the above formula (G-1a), in which -SH in formula (G-1a) is replaced with a carboxy group (-COOH).

[0083] Examples of the compound (G-1b) include the following compounds.

[0084] Succinic acid, glutaric acid, adipic acid, octafluoroadipic acid, azelaic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, dodecafluorosuberic acid, 3-ethyl-3-methylglutaric acid, hexafluoroglutaric acid, trans-3-hexenedioic acid, sebacic acid, hexadecafluorosebacic acid, acetylenedicarboxylic acid, trans-aconitic acid, 1,3-adamantanedicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, cis-4-cyano Cyclohexene-1,2-dicarboxylic acid, 1,1-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, cis- or trans-1,3-cyclohexanedicarboxylic acid, cis- or trans-1,4-cyclohexanedicarboxylic acid, 1,1-cyclopentanediacetic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, decahydro-1,4-naphthalenedicarboxylic acid, 2,3-norbornanedicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, phthalic acid, 3-fluorophthalic acid, isophthalic acid, tetrafluoroisophthalic acid Phthalic acid, terephthalic acid, tetrafluoroterephthalic acid, 2,5-dimethylterephthalic acid, 2,6-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,1'-ferrocenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 2,5-furandicarboxylic acid, benzophenone-2,4'-dicarboxylic acid monohydrate, benzophenone-4,4'-dicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-Pyridinedicarboxylic acid, 2,5-Pyridinedicarboxylic acid, 2,6-Pyridinedicarboxylic acid, 3,4-Pyridinedicarboxylic acid, Pyrazole-3,5-dicarboxylic acid monohydrate, 4,4'-Stilbenedicarboxylic acid, Anthraquinone-2,3-dicarboxylic acid, 4-(carboxymethyl)benzoic acid, Chelidonic acid monohydrate, Azobenzene-4,4'-dicarboxylic acid, Azobenzene-3,3'-dicarboxylic acid, Chlorendic acid, 1H-Imidazole-4,5-dicarboxylic acid, 2,2-Bis(4-carboxyphenyl)hexafluoropropane, 1,10-bis(4-carboxyphenoxy)decane, dipropylmalonic acid, dithiodiglycolic acid, 3,3'-dithiodipropionic acid, 4,4'-dithiodibutanoic acid, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfone, ethylene glycol bis(4-carboxyphenyl)ether, 3,4-ethylenedioxythiophene-2,5-dicarboxylic acid, 4,4'-isopropylidenediphenoxyacetic acid, 1,3-acetonedicarboxylic acid, methylenedisalicylic acid, 5,5'-thiodisalicylic acid, tris(2-carboxyethyl)isocyanurate, tetrafluorosuccinic acid, α,α,α',α'-tetramethyl-1,3-benzenedipropionic acid, 1,3,5-benzenetricarboxylic acid, etc.

[0085] From the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, the molecular weight of the compound (G-1) is preferably 3000 or less, more preferably 2500 or less, even more preferably 2000 or less, still more preferably 1000 or less, particularly preferably 800 or less, and most preferably 500 or less. The molecular weight of the compound (G-1) is usually 100 or more.

[0086] The molecular weight may be a number average molecular weight or a weight average molecular weight, where the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight, respectively, measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0087] When composition I contains compound (G-1), the content ratio of compound (G-1) to semiconductor particles (A) in composition I is preferably 0.001 to 1, more preferably 0.01 to 0.5, and even more preferably 0.02 to 0.45, in terms of mass ratio. A content ratio within this range can be advantageous in terms of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer.

[0088] When composition I contains compound (G-1), the content of compound (G-1) in composition I is, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, preferably from 0.1 mass% to 20 mass%, more preferably from 0.2 mass% to 20 mass%, even more preferably from 0.2 mass% to 10 mass%, still more preferably from 0.5 mass% to 10 mass%, and particularly preferably from 0.5 mass% to 8 mass%, relative to the total amount of solids in composition I.

[0089] [Compound (G-2)] Compound (G-2) is a compound different from compound (G-1), which contains a polyalkylene glycol structure and has a polar group at the molecular end. The molecular end is preferably the end of the longest carbon chain (the carbon atom in the carbon chain may be replaced with another atom such as an oxygen atom) in compound (G-2).

[0090] The composition may contain only one type of compound (G-2), or may contain two or more types. The composition may contain compound (G-1) or compound (G-2), or may contain compound (G-1) and compound (G-2).

[0091] A compound that contains a polyalkylene glycol structure and has the above-mentioned first functional group and second functional group is considered to belong to the compound (G-1).

[0092] The polyalkylene glycol structure is represented by the following formula:

[0093] [ka]

[0094] (n is an integer of 2 or more). In the formula, R C is an alkylene group, for example, an ethylene group, a propylene group, etc.

[0095] A specific example of the compound (G-2) is a polyalkylene glycol compound represented by the following formula (G-2a).

[0096] [ka]

[0097] In formula (G-2a), X is a polar group, Y is a monovalent group, and Z C is a divalent or trivalent group. n is an integer of 2 or more. m is 1 or 2. R C is an alkylene group.

[0098] The polar group X is preferably at least one group selected from the group consisting of a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH2). A polar group selected from this group can be advantageous in terms of enhancing coordination with the semiconductor particles (A). Among these, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity of the wavelength conversion layer, it is more preferable that the polar group X is at least one group selected from the group consisting of a thiol group and a carboxyl group.

[0099] The group Y is a monovalent group. The group Y is not particularly limited, and examples thereof include monovalent hydrocarbon groups which may have a substituent (N, O, S, halogen atom, etc.). The -CH2- contained in the hydrocarbon group may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc. The number of carbon atoms in the hydrocarbon group is, for example, 1 or more and 12 or less. The hydrocarbon group may have an unsaturated bond.

[0100] Examples of the group Y include an alkyl group having a carbon number of 1 to 12 and a straight-chain, branched-chain or cyclic structure; an alkoxy group having a carbon number of 1 to 12 and a straight-chain, branched-chain or cyclic structure. The number of carbon atoms in the alkyl group and alkoxy group is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. The -CH2- contained in the alkyl group and alkoxy group may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc. Among them, the group Y is preferably a straight-chain or branched-chain alkoxy group having a carbon number of 1 to 4, and more preferably a straight-chain alkoxy group having a carbon number of 1 to 4.

[0101] The group Y may contain a polar group. The polar group may be at least one group selected from the group consisting of a thiol group (-SH), a carboxyl group (-COOH) and an amino group (-NH2). However, as described above, a compound that contains a polyalkylene glycol structure and has the first functional group and the second functional group is considered to belong to the compound (G-1). The polar group is preferably located at the end of the group Y.

[0102] Base Z C is a divalent or trivalent radical. The radical Z C is not particularly limited, and examples thereof include divalent or trivalent hydrocarbon groups which may contain heteroatoms (N, O, S, halogen atoms, etc.). The number of carbon atoms in the hydrocarbon group is, for example, 1 to 24. The hydrocarbon group may have an unsaturated bond.

[0103] The divalent group Z CExamples of the alkyl group include an alkylene group having 1 to 24 carbon atoms and a linear, branched or cyclic structure; and an alkenylene group having 1 to 24 carbon atoms and a linear, branched or cyclic structure. The number of carbon atoms in the alkyl group and the alkenylene group is preferably 1 to 12, more preferably 1 to 8, and further preferably 1 to 4. -CH2- contained in the alkyl group and the alkenylene group may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -C(=O)-NH-, -NH-, etc. The trivalent group Z C Examples of the divalent group Z C Examples of groups obtained by removing one hydrogen atom from the above include:

[0104] Base Z C may have a branched structure. C may have a polyalkylene glycol structure other than the polyalkylene glycol structure represented by the above formula (G-2a) in a branched chain other than the branched chain containing the polyalkylene glycol structure represented by the above formula (G-2a).

[0105] Among them, the group Z C is preferably a linear or branched alkylene group having 1 or more and 6 or less carbon atoms, and more preferably a linear alkylene group having 1 or more and 4 or less carbon atoms.

[0106] R C is an alkylene group, preferably a linear or branched alkylene group having 1 or more and 6 or less carbon atoms, and more preferably a linear alkylene group having 1 or more and 4 or less carbon atoms.

[0107] In formula (G-2a), n is an integer of 2 or more, preferably 2 or more and 540 or less, more preferably 2 or more and 120 or less, and further preferably 2 or more and 60 or less.

[0108] The molecular weight of the compound (G-2) may be, for example, about 150 or more and 10,000 or less, but from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity of the wavelength conversion layer, it is preferably 150 or more and 5,000 or less, and more preferably 150 or more and 4,000 or less. The molecular weight may be a number average molecular weight or a weight average molecular weight. In this case, the number average molecular weight and the weight average molecular weight are number average molecular weight and weight average molecular weight, respectively, measured by GPC in terms of standard polystyrene.

[0109] When composition I contains compound (G-2), the content ratio of compound (G-2) to semiconductor particles (A) in composition I, in terms of mass ratio, is preferably from 0.001 to 2, more preferably from 0.01 to 1.5, and even more preferably from 0.1 to 1. A content ratio within this range can be advantageous from the viewpoints of improving the stability and dispersibility of semiconductor particles (A) and the luminous intensity of the wavelength conversion layer.

[0110] When composition I contains compound (G-2), the content of compound (G-2) in composition I is, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, preferably from 0.1 mass % to 40 mass %, more preferably from 0.1 mass % to 20 mass %, even more preferably from 1 mass % to 15 mass %, and still more preferably from 2 mass % to 12 mass %, relative to the total amount of solids in composition I.

[0111] When the composition I contains an organic ligand (G), the ratio of the content of the organic ligand (G) to the semiconductor particles (A) in the composition I is preferably 0.001 to 1, more preferably 0.01 to 0.8, and even more preferably 0.02 to 0.5, in terms of mass ratio. When the content ratio is within this range, it can be advantageous in terms of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer. The content of the organic ligand (G) here refers to the total content of all organic ligands contained in the composition I.

[0112] From the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminous intensity of the wavelength conversion layer, the total content of the semiconductor particles (A) and the organic ligands (G) in the composition I is preferably from 10 mass % to 75 mass %, more preferably from 12 mass % to 70 mass %, and even more preferably from 15 mass % to 65 mass %, relative to the total amount of solids in the composition I.

[0113] It is preferable that Composition II and Composition III are substantially free of organic ligand (G). "Substantially free of organic ligand (G)" means that the content of organic ligand (G) is preferably 1 mass% or less, more preferably 0.5 mass% or less, further preferably 0.1 mass% or less, and particularly preferably 0 mass% based on the total amount of solids in Composition II or Composition III.

[0114] <Light scattering agent (B)> Examples of the light scattering agent (B) include inorganic particles such as metal or metal oxide particles and glass particles. Examples of metal oxides include TiO2, SiO2, BaTiO3, ZnO, etc., and TiO2 particles are preferred because they efficiently scatter light. The particle size of the light scattering agent (B) is, for example, about 0.03 μm to 20 μm, preferably 0.05 μm to 1 μm, and more preferably 0.05 μm to 0.5 μm.

[0115] The light scattering agent (B) may be a dispersion in advance in a part or the whole of the solvent (J) using a dispersant. Commercially available dispersants can be used. Examples of commercially available dispersants include: DISPERBYK-101, 102, 103, 106, 107, 108, 109, 110, 111, 116, 118, 130, 140, 154, 161, 162, 163, 164, 165, 166, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 192, 20 00, 2001, 2020, 2025, 2050, 2070, 2095, 2150, 2155;ANTI-TERRA-U, U100, 203, 204, 250;BY K-P104, P104S, P105, 220S, 6919; BYK-LPN6919, 21116; LACTIMON, LACTIMON-WS; Bykumen, etc.; Lubrizol Japan SOLSPERSE-3000, 9000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000, 26000, 27000, 28000, 31845, 32000, 32500, 32550, 33500, 32600, 34750, 35100, 36600, 38500, 41000, 41090, 53095, 55000, 76500, etc. BASF EFKA-46, 47, 48, 452, 4008, 4009, 4010, 4015, 4020, 4047, 4050, 4055, 4060, 4080, 4400, 4401, 4402, 4403, 4406, 4408, 4300, 4310, 4320, 4330, 4340, 450, 451, 453, 4540, 4550, 4560, 4800, 5010, 5065, 5066, 5070, 7500, 7554, 1101, 120, 150, 1501, 1502, 1503, etc.; Examples of such polyvinyl chloride resins include Ajisper PA111, PB711, PB821, PB822, and PB824 manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0116] The content of the light scattering agent (B) in composition I is, for example, 0.001 mass% or more and 50 mass% or less, relative to the total amount of solids in composition I, and from the viewpoint of improving the light scattering ability and luminous intensity of the wavelength conversion layer, is preferably 1 mass% or more and 30 mass% or less, more preferably 2 mass% or more and 20 mass% or less, even more preferably 2 mass% or more and 15 mass% or less, and still more preferably 3 mass% or more and 10 mass% or less.

[0117] It is preferable that Composition II and Composition III are substantially free of light scattering agent (B). "Substantially free of light scattering agent (B)" means that the content of light scattering agent (B) is preferably 1 mass% or less, more preferably 0.5 mass% or less, further preferably 0.1 mass% or less, and particularly preferably 0 mass% based on the total amount of solids in Composition II or Composition III.

[0118] <Colorant (I)> The colorant (I) may be a pigment or a dye. As the pigment, a known pigment may be used, for example, a pigment classified as a pigment in the Color Index (published by The Society of Dyers and Colourists). The pigment may be used alone or in combination of two or more kinds. As the dye, a known dye may be used, for example, a dye described in the Color Index (published by The Society of Dyers and Colourists) and Dyeing Notes (Ikisensha). The dye may be used alone or in combination of two or more kinds.

[0119] The colorant (I) is preferably a pigment, and preferably contains at least one colorant selected from the group consisting of a yellow colorant, a green colorant, and a red colorant.

[0120] Examples of yellow colorants include yellow pigments such as CI Pigment Yellow 1, 3, 12, 13, 14, 15, 16, 17, 20, 24, 31, 53, 83, 86, 93, 94, 109, 110, 117, 125, 128, 129, 137, 138, 139, 147, 148, 150, 153, 154, 166, 173, 185, 194, 214, and 231. Other examples of yellow colorants are the following dyes. CI Solvent Dyes such as CI Solvent Yellow 4, 14, 15, 23, 24, 25, 38, 62, 63, 68, 79, 81, 82, 83, 89, 94, 98, 99, 117, 162, 163, 167, 189; CI Acid Yellow 1, 3, 7, 9, 11, 17, 23, 25, 29, 34, 36, 38, 40, 42, 54, 65, 72, 73, 76, 79, 98, 99, 111, 112, 113, 114, 116, 119, 123, 128, 134, 135, 138, 139, 140, 144, 150, 155, 157, 1 CI acid dyes such as 60, 161, 163, 168, 169, 172, 177, 178, 179, 184, 190, 193, 196, 197, 199, 202, 203, 204, 205, 207, 212, 214, 220, 221, 228, 230, 232, 235, 238, 240, 242, 243, 251, etc.; CI Direct Dyes such as CI Direct Yellow 2, 4, 28, 33, 34, 35, 38, 39, 43, 44, 47, 50, 54, 58, 68, 69, 70, 71, 86, 93, 94, 95, 98, 102, 108, 109, 129, 132, 136, 138, 141; CI Disperse dyes such as CI Disperse Yellow 51, 54, 76; CI Reactive dyes such as CI Reactive Yellow 2, 76, 116; CI Mordant dyes such as CI Mordant Yellow 5, 8, 10, 16, 20, 26, 30, 31, 33, 42, 43, 45, 56, 61, 62, 65; etc.

[0121] Green colorants include green pigments such as CI Pigment Green 7, 36, 58, 59, 62, and 63. Other examples of green colorants are the following dyes. CI Solvent Dyes such as CI Solvent Green 1, 3, 4, 5, 7, 28, 29, 32, 33, 34, 35; CI Acid dyes such as CI Acid Green 1, 3, 5, 6, 7, 8, 9, 11, 13, 14, 15, 16, 22, 25, 27, 28, 41, 50, 50:1, 58, 63, 65, 80, 104, 105, 106, 109; CI Direct Dyes such as CI Direct Green 25, 27, 31, 32, 34, 37, 63, 65, 66, 67, 68, 69, 72, 79, 82; CI Basic dyes such as CI Basic Green 1; CI Mordant dyes such as CI Mordant Green 1, 3, 4, 5, 10, 13, 15, 19, 21, 23, 26, 29, 31, 33, 34, 35, 41, 43, 53; CI Vat dyes such as CI Vat Green 1.

[0122] Examples of red colorants include red pigments such as CI Pigment Red 9, 97, 105, 122, 123, 144, 149, 166, 168, 176, 177, 178, 179, 180, 190, 192, 209, 215, 216, 224, 242, 254, 255, 264, 265, 266, 268, 269, and 273. Other examples of red colorants are the following dyes. CI Solvent Dyes such as CI Solvent Red 24, 45, 49, 90, 91, 111, 118, 119, 122, 124, 125, 127, 130, 132, 143, 145, 146, 150, 151, 155, 160, 168, 169, 172, 175, 181, 207, 218, 222, 227, 230, 245, 247; CI Acid Red 1, 4, 8, 14, 17, 18, 26, 27, 29, 31, 33, 34, 35, 37, 40, 42, 44, 50, 51, 52, 57, 66, 73, 76, 80, 87, 88, 91, 92, 94, 95, 97, 98, 103, 106, 111, 114, 129, 133, 134, 138, 143, 145, 150, 151, 155, 158, 160, 172, 176, 182, 18 CI acid dyes such as 3, 195, 198, 206, 211, 215, 216, 217, 227, 228, 249, 252, 257, 258, 260, 261, 266, 268, 270, 274, 277, 280, 281, 289, 308, 312, 315, 316, 339, 341, 345, 346, 349, 382, ​​383, 388, 394, 401, 412, 417, 418, 422, 426; CI Direct Dyes such as CI Direct Red 79, 82, 83, 84, 91, 92, 96, 97, 98, 99, 105, 106, 107, 172, 173, 176, 177, 179, 181, 182, 184, 204, 207, 211, 213, 218, 220, 221, 222, 232, 233, 234, 241, 243, 246, 250; CI Basic dyes such as CI Basic Red 1, 9, 10; CI Mordant dyes such as CI Mordant Red 1, 2, 3, 4, 9, 11, 12, 14, 17, 18, 19, 22, 23, 24, 25, 26, 27, 29, 30, 32, 33, 36, 37, 38, 39, 41, 42, 43, 45, 46, 48, 52, 53, 56, 62, 63, 71, 74, 76, 78, 85, 86, 88, 90, 94, 95, etc.

[0123] The colorant (I) more preferably contains a yellow colorant, even more preferably contains a yellow pigment, and even more preferably contains at least one selected from the group consisting of CI Pigment Yellow 138, 150, and 231.

[0124] The colorant (I) may be subjected, as necessary, to a rosin treatment, a surface treatment using a colorant derivative having an acidic or basic group introduced therein, a graft treatment onto the colorant surface using a polymer compound, a microparticulation treatment using a sulfuric acid microparticulation method, a washing treatment using an organic solvent or water to remove impurities, a removal treatment of ionic impurities using an ion exchange method, etc. The particle size of the colorant (I) is preferably approximately uniform.

[0125] When composition II contains a green colorant and / or a red colorant, the colorant (I) contained in composition II is preferably a green colorant when the wavelength-converting layer is a layer that emits green light, and is preferably a red colorant when the wavelength-converting layer is a layer that emits red light. The green colorant and the red colorant may each be used alone or in combination of two or more kinds.

[0126] The content of colorant (I) in composition II is, for example, 0.01 mass% or more and 99.99 mass% or less, preferably 0.1 mass% or more and 99.9 mass% or less, more preferably 1 mass% or more and 99 mass% or less, even more preferably 10 mass% or more and 90 mass% or less, and still more preferably 15 mass% or more and 70 mass% or less, based on the total amount of solids in composition II.

[0127] It is preferable that composition I is substantially free of colorant (I). "Substantially free of colorant (I)" means that the content of colorant (I) relative to the total amount of solids in composition I is preferably 1 mass% or less, more preferably 0.5 mass% or less, even more preferably 0.1 mass% or less, and particularly preferably 0 mass%.

[0128] Composition III is substantially free of colorant (I), and the content of colorant (I) relative to the total amount of solids in composition III is preferably 1 mass% or less, more preferably 0.5 mass% or less, even more preferably 0.1 mass% or less, and particularly preferably 0 mass%.

[0129] <Resin (C)> Examples of the resin (C) include the following resins [K1] to [K6].

[0130] Resin [K1]: a copolymer having a structural unit derived from at least one type (a) (hereinafter also referred to as "(a)") selected from the group consisting of unsaturated carboxylic acids and unsaturated carboxylic anhydrides, and a structural unit derived from a monomer (c) (however different from (a)) (hereinafter also referred to as "(c)") copolymerizable with (a); Resin [K2]: a copolymer having a structural unit derived from the (a), a structural unit derived from the (c), and a structural unit derived from a monomer (b) (hereinafter also referred to as "(b)") having a cyclic ether structure having 2 to 4 carbon atoms and an ethylenically unsaturated bond; Resin [K3]: a copolymer having a structural unit derived from the (a) to which the (b) has been added, and a structural unit derived from the (c); Resin [K4]: a copolymer having a structural unit obtained by adding the (b) to a structural unit derived from the (a) and further ester-bonding a carboxylic acid anhydride thereto, and a structural unit derived from the (c); Resin [K5]: a copolymer having a structural unit derived from the (b) to which the (a) has been added, and a structural unit derived from the (c); Resin [K6]: A copolymer having a structural unit obtained by adding the (a) to a structural unit derived from the (b) and further ester-bonding a carboxylic acid anhydride, and a structural unit derived from the (c).

[0131] Examples of (a) include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, and p-vinylbenzoic acid; Unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, 3-vinylphthalic acid, 4-vinylphthalic acid, 3,4,5,6-tetrahydrophthalic acid, 1,2,3,6-tetrahydrophthalic acid, dimethyltetrahydrophthalic acid, and 1,4-cyclohexenedicarboxylic acid; Bicyclounsaturated compounds containing a carboxy group, such as methyl-5-norbornene-2,3-dicarboxylic acid, 5-carboxybicyclo[2.2.1]hept-2-ene, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene, 5-carboxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-ethylbicyclo[2.2.1]hept-2-ene, etc. Unsaturated dicarboxylic acid anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride, etc.; Unsaturated mono[(meth)acryloyloxyalkyl] esters of divalent or higher polyvalent carboxylic acids, such as mono[2-(meth)acryloyloxyethyl] succinate and mono[2-(meth)acryloyloxyethyl] phthalate; Examples include unsaturated (meth)acrylates containing a hydroxy group and a carboxy group in the same molecule, such as α-(hydroxymethyl)(meth)acrylic acid.

[0132] Among these, (meth)acrylic acid, mono[2-(meth)acryloyloxyethyl] succinate, maleic anhydride, and the like are preferred from the viewpoint of copolymerization reactivity, etc.

[0133] In this specification, (meth)acrylic acid means acrylic acid and / or methacrylic acid. The same applies to "(meth)acryloyl", "(meth)acrylate", etc.

[0134] (b) is, for example, a monomer having a cyclic ether structure having 2 to 4 carbon atoms (for example, at least one selected from the group consisting of an oxirane ring, an oxetane ring, and a tetrahydrofuran ring) and an ethylenically unsaturated bond. (b) is preferably a monomer having a cyclic ether structure having 2 to 4 carbon atoms and a (meth)acryloyloxy group.

[0135] Examples of (b) include a monomer (b1) having an oxiranyl group and an ethylenically unsaturated bond (hereinafter sometimes referred to as "(b1)"), a monomer (b2) having an oxetanyl group and an ethylenically unsaturated bond (hereinafter sometimes referred to as "(b2)"), and a monomer (b3) having a tetrahydrofuryl group and an ethylenically unsaturated bond (hereinafter sometimes referred to as "(b3)").

[0136] Examples of (b1) include a monomer (b1-1) (hereinafter sometimes referred to as "(b1-1)") having a structure in which a linear or branched aliphatic unsaturated hydrocarbon is epoxidized, and a monomer (b1-2) (hereinafter sometimes referred to as "(b1-2)") having a structure in which an alicyclic unsaturated hydrocarbon is epoxidized.

[0137] Examples of (b1-1) include glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, β-ethyl glycidyl (meth)acrylate, glycidyl vinyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, α-methyl-o-vinylbenzyl glycidyl ether, α-methyl-m-vinylbenzyl glycidyl ether, α-methyl-p-vinylbenzyl glycidyl ether, 2,3-bis(glycidyl Examples of such styrene include 2,4-bis(glycidyloxymethyl)styrene, 2,5-bis(glycidyloxymethyl)styrene, 2,6-bis(glycidyloxymethyl)styrene, 2,3,4-tris(glycidyloxymethyl)styrene, 2,3,5-tris(glycidyloxymethyl)styrene, 2,3,6-tris(glycidyloxymethyl)styrene, 3,4,5-tris(glycidyloxymethyl)styrene, and 2,4,6-tris(glycidyloxymethyl)styrene.

[0138] Examples of (b1-2) include vinylcyclohexene monoxide, 1,2-epoxy-4-vinylcyclohexane (e.g., Celloxide 2000; manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl (meth)acrylate (e.g., Cyclomer A400; manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl (meth)acrylate (e.g., Cyclomer M100; manufactured by Daicel Corporation), compounds represented by formula (BI) and compounds represented by formula (BII).

[0139] [ka]

[0140] [In formula (BI) and formula (BII), R e and R f represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the hydrogen atom contained in the alkyl group may be substituted with a hydroxy group. X e and X fis a single bond, *-R g -, *-R g -O-, *-R g -S- or *-R g -NH-. R g represents an alkanediyl group having 1 to 6 carbon atoms. * represents a bond to O.]

[0141] Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, and a tert-butyl group. Examples of the alkyl group in which a hydrogen atom is substituted with a hydroxy group include a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, a 1-hydroxypropyl group, a 2-hydroxypropyl group, a 3-hydroxypropyl group, a 1-hydroxy-1-methylethyl group, a 2-hydroxy-1-methylethyl group, a 1-hydroxybutyl group, a 2-hydroxybutyl group, a 3-hydroxybutyl group, and a 4-hydroxybutyl group. R e and R f Preferred examples of the alkyl group include a hydrogen atom, a methyl group, a hydroxymethyl group, a 1-hydroxyethyl group, and a 2-hydroxyethyl group, and more preferred examples include a hydrogen atom and a methyl group.

[0142] Examples of the alkanediyl group include a methylene group, an ethylene group, a propane-1,2-diyl group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, and a hexane-1,6-diyl group. X e and X f Preferred examples of the group include a single bond, a methylene group, an ethylene group, *-CH2-O-, and *-CH2CH2-O-, and more preferred examples include a single bond and *-CH2CH2-O- (* represents a bond to O).

[0143] The compound represented by formula (BI) includes compounds represented by any one of formulas (BI-1) to (BI-15), etc. Among them, compounds represented by formulas (BI-1), (BI-3), (BII-5), (BI-7), (BI-9) or (BI-11) to (BI-15) are preferred, and compounds represented by formulas (BI-1), (BI-7), (BI-9) or (BI-15) are more preferred.

[0144] [ka]

[0145] The compound represented by formula (BII) includes compounds represented by any of formulas (BII-1) to (BII-15), etc. Among them, compounds represented by formulas (BII-1), (BII-3), (BII-5), (BII-7), (BII-9) or (BII-11) to (BII-15) are preferred, and compounds represented by formulas (BII-1), (BII-7), (BII-9) or (BII-15) are more preferred.

[0146] [ka]

[0147] The compound represented by formula (BI) and the compound represented by formula (BII) may be used alone or in combination of two or more. When the compound represented by formula (BI) and the compound represented by formula (BII) are used in combination, the content ratio thereof [compound represented by formula (BI) : compound represented by formula (BII)] is preferably 5:95 to 95:5, more preferably 20:80 to 80:20 on a molar basis.

[0148] As (b2), a monomer having an oxetanyl group and a (meth)acryloyloxy group is more preferable. As (b2), 3-methyl-3-methacryloyloxymethyloxetane, 3-methyl-3-acryloyloxymethyloxetane, 3-ethyl-3-methacryloyloxymethyloxetane, 3-ethyl-3-acryloyloxymethyloxetane, 3-methyl-3-methacryloyloxyethyloxetane, 3-methyl-3-acryloyloxyethyloxetane, 3-ethyl-3-methacryloyloxyethyloxetane, 3-ethyl-3-acryloyloxyethyloxetane, and the like can be mentioned.

[0149] As (b3), a monomer having a tetrahydrofuryl group and a (meth)acryloyloxy group is more preferable. Specific examples of (b3) include tetrahydrofurfuryl acrylate (e.g., Viscoat V#150, manufactured by Osaka Organic Chemical Industry Co., Ltd.), tetrahydrofurfuryl methacrylate, etc.

[0150] As (b), (b1) is preferable in that it is possible to further increase reliability in terms of heat resistance, chemical resistance, and the like.

[0151] A monomer having an oxirane ring and an ethylenically unsaturated bond is preferred as (b) since the reactivity during production of the resins [K3] to [K6] is high and unreacted (b) is unlikely to remain.

[0152] Examples of (c) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0 2,6]decan-8-yl(meth)acrylate (commonly known in the art as "dicyclopentanyl(meth)acrylate" and sometimes called "tricyclodecyl(meth)acrylate"), tricyclo[5.2.1.0 2,6 ](meth)acrylic acid esters such as decene-8-yl (meth)acrylate (commonly known in the art as "dicyclopentenyl (meth)acrylate"), dicyclopentanyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, allyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, and benzyl (meth)acrylate; hydroxy group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; dicarboxylic acid diesters such as diethyl maleate, diethyl fumarate, and diethyl itaconate; Bicyclo[2.2.1]hept-2-ene, 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxybicyclo[2.2.1]hept-2-ene, 5-hydroxymethylbicyclo[2.2.1]hept-2-ene, 5-(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5-methoxybicyclo[2.2.1]hept-2-ene Cyclo[2.2.1]hept-2-ene, 5-ethoxybicyclo[2.2.1]hept-2-ene, 5,6-dihydroxybicyclo[2.2.1]hept-2-ene, 5,6-di(hydroxymethyl)bicyclo[2.2.1]hept-2-ene, 5,6-di(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5,6-dimethoxybicyclo[2.2.1]hept 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxymethyl-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-diethoxybicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2-ene, bicyclounsaturated compounds such as -ene, 5-cyclohexyloxycarbonylbicyclo[2.2.1]hept-2-ene, 5-phenoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-bis(tert-butoxycarbonyl)bicyclo[2.2.1]hept-2-ene, and 5,6-bis(cyclohexyloxycarbonyl)bicyclo[2.2.1]hept-2-ene; dicarbonyl imide derivatives such as N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, N-succinimidyl-3-maleimidobenzoate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidocaproate, N-succinimidyl-3-maleimidopropionate, and N-(9-acridinyl)maleimide; Examples of the copolymer include styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-methoxystyrene, acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylamide, methacrylamide, vinyl acetate, 1,3-butadiene isoprene, and 2,3-dimethyl-1,3-butadiene.

[0153] Among the above, from the viewpoints of copolymerization reactivity and heat resistance of the resin (C), methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, benzyl (meth)acrylate, styrene, vinyltoluene, N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, bicyclo[2.2.1]hept-2-ene, and the like are preferred.

[0154] In the resin [K1], the ratio of structural units derived from each of them is as follows among all structural units constituting the resin [K1]: Structural units derived from (a): 2 mol % or more and 60 mol % or less Structural units derived from (c): 40 mol % or more and 98 mol % or less It is preferred that Structural units derived from (a): 10 mol % or more and 50 mol % or less Structural units derived from (c): 50 mol % or more and 90 mol % or less It is more preferable that:

[0155] When the ratio of the structural units in the resin [K1] is within the above range, the storage stability and solvent resistance tend to be excellent.

[0156] Resin [K1] can be produced, for example, by referring to the method described in the literature "Experimental Methods of Polymer Synthesis" (written by Takayuki Otsu, published by Kagaku Dojin Co., Ltd., 1st edition, 1st printing, published on March 1, 1972) and the cited references described in said literature.

[0157] Specifically, a method in which predetermined amounts of (a) and (c), a polymerization initiator, a solvent, and the like are placed in a reaction vessel, and the atmosphere is made deoxygenated, for example by replacing oxygen with nitrogen, and the mixture is heated and kept warm while being stirred, can be mentioned.

[0158] The polymerization initiator and solvent used are not particularly limited, and those generally used in the field can be used. For example, the polymerization initiator can be an azo compound (2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile) etc.) or an organic peroxide (benzoyl peroxide etc.), and the solvent can be any one that dissolves each monomer, such as the solvent (J) described below.

[0159] The obtained copolymer may be used as a solution after the reaction as it is, or may be a concentrated or diluted solution, or may be extracted as a solid (powder) by a method such as reprecipitation. If a solvent (J) described below is used as a solvent during polymerization, the solution after the reaction can be used as it is for the preparation of the composition, and therefore the production process of the composition can be simplified.

[0160] In the resin [K2], the ratio of structural units derived from each of them is as follows among all structural units constituting the resin [K2]: Structural units derived from (a): 2 to 45 mol% Structural units derived from (b): 2 to 95 mol% Structural units derived from (c): 1 to 65 mol% It is preferred that Structural units derived from (a): 5 to 40 mol% Structural units derived from (b): 5 to 80 mol% Structural units derived from (c): 5 to 60 mol% It is more preferable that:

[0161] When the ratio of the structural units in the resin [K2] is within the above range, the compositions I to III tend to have excellent storage stability and developability when forming a colored pattern.

[0162] Resin [K2] can be produced, for example, in the same manner as described above as the method for producing resin [K1].

[0163] Resin [K3] can be produced by adding a cyclic ether having 2 to 4 carbon atoms contained in (b) to a carboxylic acid and / or a carboxylic acid anhydride contained in (a) to a copolymer of (a) and (c).

[0164] First, a copolymer of (a) and (c) is produced in the same manner as described for the production method of resin [K1]. In this case, the ratio of the structural units derived from each is preferably the same as that described for resin [K1].

[0165] Next, a part of the carboxylic acid and / or carboxylic acid anhydride derived from (a) in the copolymer is reacted with a cyclic ether having 2 to 4 carbon atoms contained in (b).

[0166] Following the production of the copolymer of (a) and (c), the atmosphere in the flask is replaced with air from nitrogen, and (b) is reacted in the presence of a reaction catalyst (e.g., an organic phosphorus compound, a metal complex, an amine compound, etc.) between a carboxylic acid or a carboxylic acid anhydride and a cyclic ether and a polymerization inhibitor (e.g., hydroquinone, etc.) at a temperature of, for example, 60°C or higher and 130°C or lower for 1 hour or longer and 10 hours or shorter, to produce resin [K3].

[0167] The amount of (b) used is preferably 5 to 80 mol, more preferably 10 to 75 mol, per 100 mol of (a). By setting it within this range, the storage stability of the composition and the balance of the solvent resistance, heat resistance, and mechanical strength of each layer tend to be good.

[0168] The organic phosphorus compound as the reaction catalyst may be, for example, triphenylphosphine. The amine compound as the reaction catalyst may be, for example, an aliphatic tertiary amine compound or an aliphatic quaternary ammonium salt compound, and specific examples thereof include, for example, tris(dimethylaminomethyl)phenol, triethylamine, tetrabutylammonium bromide, and tetrabutylammonium chloride. The reaction catalyst is preferably an organic phosphorus compound.

[0169] The amount of the reaction catalyst used is preferably 0.001 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the total amount of (a), (b) and (c).

[0170] The amount of the polymerization inhibitor used is preferably 0.001 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the total amount of (a), (b) and (c).

[0171] The reaction conditions such as the charging method, reaction temperature and time can be appropriately adjusted in consideration of the production equipment, the amount of heat generated by the polymerization, etc. As with the polymerization conditions, the charging method and reaction temperature can be appropriately adjusted in consideration of the production equipment, the amount of heat generated by the polymerization, etc.

[0172] Resin [K4] is a resin obtained by further reacting resin [K3] with a carboxylic acid anhydride. The hydroxyl group generated by the reaction of a carboxylic acid or a carboxylic acid anhydride with a cyclic ether is reacted with a carboxylic acid anhydride. Examples of carboxylic acid anhydrides include succinic anhydride, maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride. The amount of the carboxylic acid anhydride used is preferably 0.5 moles or more and 1 mole or less per mole of the amount of (b) used.

[0173] Resin [K5] is produced in the first step by the same method as the above-mentioned resin [K1] to obtain a copolymer of (b) and (c). As in the above, the obtained copolymer may be used as it is in the form of a solution after the reaction, or may be a concentrated or diluted solution, or may be extracted as a solid (powder) by a method such as reprecipitation.

[0174] The ratios of the structural units derived from (b) and (c) to the total number of moles of all structural units constituting the copolymer are, respectively, Structural units derived from (b): 5 mol % or more and 95 mol % or less Structural units derived from (c): 5 mol % or more and 95 mol % or less It is preferred that Structural units derived from (b): 10 mol % or more and 90 mol % or less Structural units derived from (c): 10 mol % or more and 90 mol % or less It is more preferable that:

[0175] Resin [K5] can be obtained by reacting a cyclic ether derived from (b) contained in a copolymer of (b) and (c) with a carboxylic acid or carboxylic anhydride contained in (a) under the same conditions as in the production method of resin [K3].

[0176] The amount of (a) used to react with the copolymer is preferably 5 moles or more and 80 moles or less per 100 moles of (b).

[0177] Resin [K6] is a resin obtained by further reacting resin [K5] with a carboxylic acid anhydride. The hydroxyl group generated by the reaction of a cyclic ether with a carboxylic acid or a carboxylic acid anhydride is reacted with the carboxylic acid anhydride.

[0178] Examples of carboxylic acid anhydrides include succinic anhydride, maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride.

[0179] The amount of the carboxylic acid anhydride used is preferably 0.5 to 1 mole per mole of the amount of (a) used.

[0180] Examples of the resin [K1], resin [K2], resin [K3], resin [K4], resin [K5] and resin [K6] include resin [K1] such as benzyl (meth)acrylate / (meth)acrylic acid copolymer, styrene / (meth)acrylic acid copolymer, (meth)acrylic acid / mono[2-(meth)acryloyloxyethyl] succinate / dicyclopentanyl (meth)acrylate / methyl (meth)acrylate copolymer; Glycidyl (meth)acrylate / benzyl (meth)acrylate / (meth)acrylic acid copolymer, glycidyl (meth)acrylate / styrene / (meth)acrylic acid copolymer, 3,4-epoxytricyclo[5.2.1.0 2,6 ] Decyl acrylate / (meth)acrylic acid / methyl (meth)acrylate copolymer, 3,4-epoxytricyclo[5.2.1.0 2,6 ]decyl acrylate / (meth)acrylic acid / N-cyclohexylmaleimide copolymer, 3,4-epoxytricyclo[5.2.1.0 2,6 ] Decyl acrylate / (meth)acrylic acid / benzyl (meth)acrylate copolymer and other resins [K2]; Resins such as a resin obtained by adding glycidyl (meth)acrylate to a benzyl (meth)acrylate / (meth)acrylic acid copolymer, a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / styrene / (meth)acrylic acid copolymer, a resin obtained by adding glycidyl (meth)acrylate to a tricyclodecyl (meth)acrylate / benzyl (meth)acrylate / (meth)acrylic acid copolymer, and a resin obtained by adding glycidyl (meth)acrylate to a dicyclopentanyl (meth)acrylate / methyl (meth)acrylate / (meth)acrylic acid copolymer [K3]; Resins in which glycidyl (meth)acrylate is added to a benzyl (meth)acrylate / (meth)acrylic acid copolymer, and then tetrahydrophthalic anhydride or succinic anhydride is ester-bonded to the resin; resins in which glycidyl (meth)acrylate is added to a tricyclodecyl (meth)acrylate / benzyl (meth)acrylate / (meth)acrylic acid copolymer, and then tetrahydrophthalic anhydride or succinic anhydride is ester-bonded to the resin; resins in which glycidyl (meth)acrylate is added to a dicyclopentanyl (meth)acrylate / methyl (meth)acrylate / (meth)acrylic acid copolymer, and tetrahydrophthalic anhydride or succinic anhydride is further bonded via an ester bond to the resin; and resins in which glycidyl (meth)acrylate is added to a dicyclopentanyl (meth)acrylate / 2-ethylhexyl (meth)acrylate / (meth)acrylic acid copolymer, and tetrahydrophthalic anhydride or succinic anhydride is further bonded via an ester bond to the resin [K4]; Resins such as a resin obtained by adding (meth)acrylic acid to a copolymer of tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate, and a resin obtained by adding (meth)acrylic acid to a copolymer of tricyclodecyl (meth)acrylate / styrene / glycidyl (meth)acrylate [K5]; Examples of such resins include a resin obtained by adding (meth)acrylic acid to a copolymer of tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate, and then ester-bonding tetrahydrophthalic anhydride or succinic anhydride to the resin; and a resin obtained by adding (meth)acrylic acid to a copolymer of dicyclopentanyl (meth)acrylate / 2-ethylhexyl (meth)acrylate / glycidyl (meth)acrylate, and then ester-bonding tetrahydrophthalic anhydride or succinic anhydride to the resin [K6].

[0181] The resin (C) contained in the composition I and the composition III preferably includes at least one selected from the group consisting of the resin [K1], the resin [K2], the resin [K3], the resin [K4], the resin [K5] and the resin [K6], more preferably includes at least one selected from the group consisting of the resin [K1] and the resin [K2], and even more preferably includes the resin [K1]. The resin (C) contained in composition II preferably includes at least one selected from the group consisting of resin [K1], resin [K2], resin [K3], resin [K4], resin [K5] and resin [K6], more preferably includes at least one selected from the group consisting of resin [K1] and resin [K2], and even more preferably includes resin [K1] and resin [K2].

[0182] Further examples of the resin (C) include the resins described in JP 2018-123274 A. Examples of the resin include a polymer (hereinafter also referred to as "resin (Ca)") having a double bond in a side chain, containing a structural unit (α) represented by the following formula (I) and a structural unit (β) represented by the following formula (II) in the main chain, and further containing an acid group.

[0183] The acid group can be introduced into the resin (Ca) by, for example, including a structural unit (γ) derived from an acid group-containing monomer (e.g., (meth)acrylic acid, etc.). The resin (Ca) preferably includes the structural units (α), (β), and (γ) in the main chain skeleton.

[0184] [ka]

[0185] [In the formula, R A and R B are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms. n represents the average number of repeating units of the structural unit represented by formula (I) and is a number of 1 or more.]

[0186] [ka]

[0187] [In the formula, R C R may be the same or different and represents a hydrogen atom or a methyl group. D are the same or different and represent a linear or branched hydrocarbon group having 4 to 20 carbon atoms. m represents the average number of repeating units of the structural unit represented by formula (II) and is a number of 1 or more.] In resin (Ca), the content of structural unit (α) is, for example, 0.5% by mass or more and 50% by mass or less, preferably 1% by mass or more and 40% by mass or less, more preferably 5% by mass or more and 30% by mass or less, based on the total amount of all monomer units that give the main chain skeleton of resin (Ca), from the viewpoint of heat resistance and storage stability of resin (Ca). n in formula (I) represents the average number of repeating units of structural unit (α) in resin (Ca), and n can be set so that the content of structural unit (α) falls within the above range.

[0188] From the viewpoint of the solvent resistance of each layer, the content of the structural unit (β) is, for example, 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 75% by mass or less, based on the total amount of all monomer units that give the main chain skeleton of the resin (Ca) being 100% by mass. m in the formula (II) represents the average number of repeating units of the structural unit (β) in the resin (Ca), and m can be set so that the content of the structural unit (β) falls within the above-mentioned range.

[0189] The content of the structural unit (γ) is, from the viewpoint of the solubility of the resin (Ca) in the solvent (J) and the like, for example, 0.5% by mass or more and 50% by mass or less, preferably 2% by mass or more and 50% by mass or less, and more preferably 5% by mass or more and 45% by mass or less, relative to 100% by mass of the total amount of all monomer units that provide the main chain skeleton of the resin (Ca).

[0190] Resin (C) has a weight average molecular weight Mw of, for example, 1000 to 100000 in terms of standard polystyrene measured by GPC, and from the viewpoint of the developability and luminescence intensity of the composition, it is preferably 2000 to 50000, more preferably 3000 to 20000. Mw of resin (C) can be adjusted by appropriately combining reaction conditions such as the selection of raw materials used, the charging method, the reaction temperature and time. Mw of resin (C) can be measured according to the measurement method described in the Examples section below. Alternatively, Mw of resin (C) contained in the composition may be measured using GPC.

[0191] The molecular weight distribution [weight average molecular weight (Mw) / number average molecular weight (Mn)] of the resin (C) measured by GPC is, for example, 1.0 or more and 6.0 or less, and from the viewpoint of improving the luminescence intensity, preferably 1.2 or more and 4.0 or less.

[0192] From the viewpoint of the developability of the composition and the solvent resistance of each layer, the acid value of the resin (C) is, for example, 30 mgKOH / g or more, preferably 90 mgKOH / g to 150 mgKOH / g, more preferably 95 mgKOH / g to 140 mgKOH / g, and even more preferably 100 mgKOH / g to 130 mgKOH / g. The acid value of the resin (C) can be adjusted by the content of a monomer component having an acid group (e.g., the above (a)) or the content of a carboxylic acid anhydride to be reacted with a hydroxyl group generated by the reaction of a carboxylic acid or a carboxylic acid anhydride with a cyclic ether.

[0193] The acid value of the resin (C) is a value measured as the amount (mg) of potassium hydroxide required to neutralize 1 g of the resin (C), and can be determined, for example, by titration using an aqueous potassium hydroxide solution. Specifically, it can be measured according to the measurement method described in the Examples section below. Alternatively, the acid value of the resin (C) contained in the composition can be determined, for example, by performing a structural analysis of the resin (C).

[0194] From the viewpoint of improving the emission intensity, the resin (C) preferably contains a resin having a double bond equivalent of 300 g / eq or more and 2000 g / eq or less, and more preferably contains a resin having a double bond equivalent of 500 g / eq or more and 1500 g / eq or less. An example of a resin having a double bond equivalent of 300 g / eq or more and 2000 g / eq or less is a (meth)acrylic resin. The resin (C) is preferably made of a (meth)acrylic resin.

[0195] The content of resin (C) in composition I is, for example, 5% by mass or more and 80% by mass or less, preferably 10% by mass or more and 70% by mass or less, more preferably 13% by mass or more and 60% by mass or less, and even more preferably 17% by mass or more and 55% by mass or less, relative to the total amount of solids in composition I. When the content of resin (C) is within the above range, the semiconductor particles (A) become more easily dispersed, and the luminous intensity of the wavelength conversion layer tends to be increased.

[0196] The content of resin (C) in composition II is, for example, 0.00001 mass% or more and 99.99999 mass% or less, preferably 1 mass% or more and 99 mass% or less, more preferably 1 mass% or more and 97 mass% or less, even more preferably 1 mass% or more and 95 mass% or less, still more preferably 3 mass% or more and 90 mass% or less, particularly preferably 5 mass% or more and 80 mass% or less, and most preferably 10 mass% or more and 70 mass% or less, based on the total amount of solids in composition II.

[0197] The content of resin (C) in composition III is, for example, 0.00001 mass% or more and 99.99999 mass% or less, preferably 1 mass% or more and 99 mass% or less, more preferably 1 mass% or more and 97 mass% or less, even more preferably 1 mass% or more and 95 mass% or less, still more preferably 3 mass% or more and 90 mass% or less, particularly preferably 5 mass% or more and 80 mass% or less, and most preferably 10 mass% or more and 70 mass% or less, based on the total amount of solids in composition III.

[0198] In the composition I, the mass ratio (solid content ratio) of the resin (C) to the polymerizable compound (D) is, for example, 1 or more, and from the viewpoints of the developability of the composition I and the luminous intensity of the wavelength conversion layer, it is preferably 1.5 or more, more preferably 2 or more, and is preferably 5 or less, more preferably 4 or less.

[0199] In the composition II, the mass ratio (solid content ratio) of the resin (C) to the polymerizable compound (D) is, for example, 0.5 or more, and from the viewpoint of the developability of the composition II, it is preferably 0.8 or more, more preferably 1.2 or more, and is preferably 5 or less, more preferably 4 or less.

[0200] In the composition III, the mass ratio (solid content ratio) of the resin (C) to the polymerizable compound (D) is, for example, 1 or more, and from the viewpoints of the developability and luminescence intensity of the composition III, it is preferably 1.5 or more, more preferably 2 or more, and is preferably 5 or less, more preferably 4 or less.

[0201] <Polymerizable compound (D)> The polymerizable compound (D) is a compound that can be polymerized by an active radical, an acid, or the like generated from a polymerization initiator (E) described later. Examples of the polymerizable compound (D) include photopolymerizable compounds such as compounds having an ethylenically unsaturated bond, such as (meth)acrylic acid ester compounds. Another example of the polymerizable compound (D) is a thermally polymerizable compound. The composition may contain two or more types of polymerizable compounds (D).

[0202] The polymerizable compound (D) is preferably a photopolymerizable compound having three or more ethylenically unsaturated bonds in the molecule. The weight average molecular weight of the polymerizable compound (D) is preferably 150 or more and 2900 or less, more preferably 250 or more and 1500 or less.

[0203] Examples of the polymerizable compound (D) include a compound (Da) having three or more (meth)acryloyloxy groups in the molecule and an acidic functional group, and a compound (Db) having three or more (meth)acryloyloxy groups in the molecule and no acidic functional group. The photopolymerizable compound preferably contains at least one of the compounds (Da) and (Db), and may contain two or more of the compounds (Da), two or more of the compounds (Db), or at least one of the compounds (Da) and at least one of the compounds (Db). Examples of the acidic functional group include a carboxy group, a sulfonic acid group, a phosphoric acid group, and the like. Among them, the acidic functional group is preferably a carboxy group.

[0204] The polymerizable compound (D) in the composition I contains the compound (Da), which can improve the dispersibility of the semiconductor particles (A) and can improve the luminescence intensity of the wavelength conversion layer. In addition, the polymerizable compound (D) contains the compound (Da), which can improve the curability and heat resistance of the composition.

[0205] The number of (meth)acryloyloxy groups in one molecule of compound (D) is, for example, 3 or more and 6 or less, preferably 3 or more and 5 or less, and more preferably 3. The number of acidic functional groups in one molecule of compound (Da) is 1 or more, and preferably 1. When two or more acidic functional groups are present, the respective acidic functional groups may be different or the same, but it is preferable that the compound (Da) has at least one carboxy group.

[0206] Examples of the compound (Da) include compounds obtained by esterifying a compound having three or more (meth)acryloyloxy groups and hydroxyl groups, such as pentaerythritol tri(meth)acrylate or dipentaerythritol penta(meth)acrylate, with a dicarboxylic acid. Examples of the compound include a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate with succinic acid, a compound obtained by monoesterifying dipentaerythritol penta(meth)acrylate with succinic acid, a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate with maleic acid, and a compound obtained by monoesterifying dipentaerythritol penta(meth)acrylate with maleic acid. Among these, a compound obtained by monoesterifying pentaerythritol tri(meth)acrylate with succinic acid is preferred.

[0207] Examples of commercially available products of compound (Da) include "ARONIX M-510" manufactured by Toagosei Co., Ltd., which contains a dibasic acid anhydride adduct of pentaerythritol tri(meth)acrylate as the main component, and "ARONIX M-520D" manufactured by Toagosei Co., Ltd., which contains a dibasic acid anhydride adduct of dipentaerythritol penta(meth)acrylate as the main component. These commercially available products have a carboxy group as the acidic functional group.

[0208] The ethylenically unsaturated bond contained in the compound (Db) is preferably a (meth)acryloyloxy group. The number of ethylenically unsaturated bonds contained in one molecule of the compound (Db) is preferably 3 to 6.

[0209] Examples of the compound (Db) include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, tris( 2-(meth)acryloyloxyethyl)isocyanurate, ethylene glycol modified pentaerythritol tetra(meth)acrylate, ethylene glycol modified dipentaerythritol hexa(meth)acrylate, propylene glycol modified pentaerythritol tetra(meth)acrylate, propylene glycol modified dipentaerythritol hexa(meth)acrylate, caprolactone modified pentaerythritol tetra(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, etc. Among them, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. are preferred.

[0210] From the viewpoint of improving the developability of the composition, it is preferable that the composition I and the composition III contain a compound (Da). The compound (Da) is contained in an amount of preferably 50% by mass or more, more preferably 70% by mass or more, based on 100% by mass of the polymerizable compound (D) contained in the composition I or the composition III. On the other hand, from the viewpoint of improving the curability, it is preferable that the composition II contains a compound (Db). The compound (Db) is contained in an amount of preferably 50% by mass or more, more preferably 70% by mass or more, based on 100% by mass of the polymerizable compound (D) contained in the composition II.

[0211] The content of the polymerizable compound (D) in composition I is preferably from 7 to 60% by mass, more preferably from 10 to 45% by mass, and even more preferably from 13 to 30% by mass, based on the total amount of solids in composition I. When the content of the polymerizable compound (D) is within the above range, the developability of composition I and the solvent resistance of the wavelength converting layer tend to be improved.

[0212] The content of the polymerizable compound (D) in composition II is, for example, 0.00001 mass% or more and 99.99999 mass% or less, preferably 1 mass% or more and 99 mass% or less, more preferably 1 mass% or more and 97 mass% or less, even more preferably 1 mass% or more and 95 mass% or less, still more preferably 1 mass% or more and 90 mass% or less, particularly preferably 2 mass% or more and 80 mass% or less, and most preferably 3 mass% or more and 70 mass% or less, relative to the total amount of solids in composition II.

[0213] The content of the polymerizable compound (D) in the composition III is, for example, 0.00001% by mass or more and 99.99999% by mass or less, preferably 1% by mass or more and 99% by mass or less, more preferably 1% by mass or more and 97% by mass or less, even more preferably 1% by mass or more and 95% by mass or less, still more preferably 1% by mass or more and 90% by mass or less, particularly preferably 2% by mass or more and 80% by mass or less, especially preferably 3% by mass or more and 70% by mass or less, preferably 7% by mass or more and 60% by mass or less, more preferably 10% by mass or more and 55% by mass or less, and even more preferably 15% by mass or more and 50% by mass or less, based on the total amount of solids in the composition III. When the content is within the above range, it is advantageous in suppressing the decrease in the luminous intensity of the wavelength conversion layer due to heat.

[0214] <Polymerization initiator (E)> The polymerization initiator (E) is a compound that generates active radicals, acids, etc. by the action of light or heat, and can initiate polymerization of the polymerizable compound (D). The composition can contain one or more polymerization initiators (E).

[0215] Examples of the polymerization initiator (E) include photopolymerization initiators such as oxime compounds, biimidazole compounds, triazine compounds and acylphosphine compounds, and thermal polymerization initiators such as azo compounds and organic peroxides.

[0216] An example of the oxime compound is an oxime compound having a first molecular structure represented by the following formula (1): Hereinafter, this oxime compound is also referred to as "oxime compound (1)".

[0217] [ka]

[0218] Inclusion of oxime compound (1) as polymerization initiator (E) can be advantageous in terms of improving the emission intensity. One of the reasons for such an effect is presumably that the absorption wavelength of oxime compound (1) changes significantly before and after cleavage (decomposition) of oxime compound (1), which is necessary for oxime compound (1) to initiate photopolymerization, due to the unique molecular structure of oxime compound (1), and thus oxime compound (1) has a high photoradical polymerization initiation ability.

[0219] In formula (1), R 1 is R 11 , OR 11 , C.O.R. 11 , S.R. 11 ,CONR 12 R 13 Or CN.

[0220] R 11 , R 12 and R 13 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0221] R 11 , R 12 or R 13 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21, S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom, or COOR 21 may be substituted with.

[0222] R 21 , R 22 and R 23 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0223] R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group.

[0224] R 11 , R 12 , R 13 , R 21 , R 22 or R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-.

[0225] R 24 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0226] R 11 , R 12 , R 13 , R 21 , R 22 or R 23 When the group represented by R 12 and R 13 and R 22 and R 23 may be joined together to form a ring.

[0227] * represents a bond to a second molecular structure, which is a molecular structure other than the first molecular structure that the oxime compound (1) has.

[0228] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the alkyl group having 1 to 20 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a tert-octyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an icosyl group, a cyclopentyl group, a cyclohexyl group, a cyclohexylmethyl group, and a cyclohexylethyl group.

[0229] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24Examples of the aryl group having 6 to 30 carbon atoms represented by the formula (I) include a phenyl group, a tolyl group, a xylyl group, an ethylphenyl group, a naphthyl group, an anthryl group, a phenanthryl group, a phenyl group substituted with one or more of the above-mentioned alkyl groups, a biphenylyl group, a naphthyl group, and an anthryl group.

[0230] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the aralkyl group having 7 to 30 carbon atoms represented by the following formula include a benzyl group, an α-methylbenzyl group, an α,α-dimethylbenzyl group, and a phenylethyl group.

[0231] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 Examples of the heterocyclic group having 2 to 20 carbon atoms represented by the formula (I) include a pyridyl group, a pyrimidyl group, a furyl group, a thienyl group, a tetrahydrofuryl group, a dioxolanyl group, a benzoxazol-2-yl group, a tetrahydropyranyl group, a pyrrolidyl group, an imidazolidyl group, a pyrazolidyl group, a thiazolidyl group, an isothiazolidyl group, an oxazolidyl group, an isoxazolidyl group, a piperidyl group, a piperazyl group, and a morpholinyl group, and are preferably 5- to 7-membered heterocyclic rings.

[0232] R in formula (1) 12 and R 13 and R 22 and R 23 may be joined together to form a ring, R 12 and R 13 and R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached.

[0233] R in formula (1)12 and R 13 and R 22 and R 23 Examples of the ring that can be formed by combining with each other include a cyclopentane ring, a cyclohexane ring, a cyclopentene ring, a benzene ring, a piperidine ring, a morpholine ring, a lactone ring, and a lactam ring, and preferably a 5- to 7-membered ring.

[0234] R in formula (1) 11 , R 12 , R 13 , R 21 , R 22 and R 23 Examples of the halogen atom which may be contained as a substituent include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0235] R in formula (1) 1 is preferably R 11 and more preferably an alkyl group having 1 to 20 carbon atoms, even more preferably an alkyl group having 1 to 10 carbon atoms, and even more preferably an alkyl group having 1 to 6 carbon atoms.

[0236] An example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (2): The second molecular structure means a molecular structure portion other than the first molecular structure possessed by the oxime compound (1).

[0237] The bond represented by "*" in formula (2) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (2), the benzene ring having "-*" in formula (2) and the carbonyl group having "-*" in formula (1) are directly bonded.

[0238] [ka]

[0239] In formula (2), R 2 and R 3 are each independently R 11, OR 11 , S.R. 11 , C.O.R. 11 ,CONR 12 R 13 , N.R. 12 COR 11 , O.C.O.R. 11 , COOR 11 , SCOR 11 , OCSR 11 , C.O.S.R. 11 , C.S.O.R. 11 , CN or a halogen atom.

[0240] R 2 When multiple are present, they may be the same or different.

[0241] R 3 When multiple are present, they may be the same or different.

[0242] R 11 , R 12 and R 13 has the same meaning as above.

[0243] s and t each independently represent an integer of 0 to 4.

[0244] L is a sulfur atom, CR 31 R 32 , CO or NR 33 Represents.

[0245] R 31 , R 32 and R 33 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms.

[0246] R 31 , R 32 or R 33 When the group represented by R 31 , R 32 and R 33may each independently form a ring together with either adjacent benzene ring.

[0247] R 4 is a hydroxy group, a carboxy group, or a group represented by the following formula (2-1):

[0248] [ka]

[0249] (In formula (2-1), L 1 -O-, -S-, -NR 22 -, -NR 22 It represents CO-, -SO2-, -CS-, -OCO- or -COO-.

[0250] R 22 has the same meaning as above.

[0251] L 2 represents a group obtained by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms, a group obtained by removing v hydrogen atoms from an aryl group having 6 to 30 carbon atoms, a group obtained by removing v hydrogen atoms from an aralkyl group having 7 to 30 carbon atoms, or a group obtained by removing v hydrogen atoms from a heterocyclic group having 2 to 20 carbon atoms.

[0252] L 2 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 22 -, -NR 22 COO-, -OCONR 22 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-, and the alkylene portion may be branched or cyclic.

[0253] R 4a OR 41 , S.R. 41 ,CONR 42 R 43 , N.R. 42 COR 43 , O.C.O.R. 41 , COOR41 , SCOR 41 , OCSR 41 , C.O.S.R. 41 , C.S.O.R. 41 , CN or a halogen atom.

[0254] R 4a When multiple are present, they may be the same or different.

[0255] R 41 , R 42 and R 43 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms; R 41 , R 42 and R 43 When the group represented by R 42 and R 43 may be joined together to form a ring. v represents an integer from 1 to 3. It represents a group represented by the following formula:

[0256] * represents a bond to the first molecular structure of the oxime compound (1).

[0257] R in Equation (2) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 , R 31 , R 32 and R 33 and R in the above formula (2-1) 22 , R 41 , R 42 and R 43 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, and the aralkyl group having 7 to 30 carbon atoms are represented by R 11 , R 12 , R 13 , R 21 , R 22 , R23 and R 24 The example for is similar.

[0258] R in Equation (2) 11 , R 12 , R 13 , R 21 , R 22 , R 23 , R 24 and R in the above formula (2-1) 22 Examples of the heterocyclic group having 2 to 20 carbon atoms represented by the formula (1) include R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.

[0259] R in Equation (2) 31 , R 32 and R 33 may each independently form a ring together with either adjacent benzene ring, R 31 , R 32 and R 33 means that each of them may independently form a ring together with either adjacent benzene ring and the nitrogen atom to which it is connected.

[0260] R in Equation (2) 31 , R 32 and R 33 Examples of rings that may be formed by combining with either adjacent benzene ring include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.

[0261] L in the above formula (2-1) 2 represents a group in which v hydrogen atoms have been removed from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0262] Examples of the group obtained by removing v hydrogen atoms from an alkyl group having 1 to 20 carbon atoms, when v is 1, include alkylene groups such as a methylene group, an ethylene group, a propylene group, a methylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a 1,2-dimethylpropylene group, a 1,3-dimethylpropylene group, a 1-methylbutylene group, a 2-methylbutylene group, a 3-methylbutylene group, a 4-methylbutylene group, a 2,4-dimethylbutylene group, a 1,3-dimethylbutylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, an ethane-1,1-diyl group, and a propane-2,2-diyl group.

[0263] Examples of the group in which v hydrogen atoms have been removed from an aryl group having 6 to 30 carbon atoms, when v is 1, include arylene groups such as a 1,2-phenylene group, a 1,3-phenylene group, a 1,4-phenylene group, a 2,6-naphthylene group, a 1,4-naphthylene group, a 2,5-dimethyl-1,4-phenylene group, a diphenylmethane-4,4'-diyl group, a 2,2-diphenylpropane-4,4'-diyl group, a diphenylsulfide-4,4'-diyl group, and a diphenylsulfone-4,4'-diyl group.

[0264] Examples of the group in which v hydrogen atoms have been removed from an aralkyl group having 7 to 30 carbon atoms, when v is 1, include groups represented by the following formula (a) and groups represented by the following formula (b).

[0265] [ka] [In formulas (a) and (b), L 3 and L 5 represents an alkylene group having 1 to 10 carbon atoms; L 4 and L 6 represents a single bond or an alkylene group having 1 to 10 carbon atoms.]

[0266] Examples of the alkylene group having 1 to 10 carbon atoms include a methylene group, an ethylene group, a propylene group, a methylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a 1,2-dimethylpropylene group, a 1,3-dimethylpropylene group, a 1-methylbutylene group, a 2-methylbutylene group, a 3-methylbutylene group, a 4-methylbutylene group, a 2,4-dimethylbutylene group, a 1,3-dimethylbutylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, and a decylene group.

[0267] Examples of the group in which v hydrogen atoms have been removed from a heterocyclic group having 2 to 20 carbon atoms, when v is 1, include divalent heterocyclic groups such as a 2,5-pyridinediyl group, a 2,6-pyridinediyl group, a 2,5-pyrimidinediyl group, a 2,5-thiophenediyl group, a 3,4-tetrahydrofurandiyl group, a 2,5-tetrahydrofurandiyl group, a 2,5-furandiyl group, a 3,4-thiazolediyl group, a 2,5-benzofurandiyl group, a 2,5-benzothiophenediyl group, an N-methylindole-2,5-diyl group, a 2,5-benzothiazolediyl group, and a 2,5-benzoxazolediyl group.

[0268] R in Equation (2) 2 and R 3 and R in the above formula (2-1) 4a Examples of the halogen atom represented by the formula (I) include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0269] From the viewpoint of solubility in the solvent (J) and / or developability of the composition, a preferred example of the structure represented by formula (2) is a structure represented by the following formula (2a).

[0270] [ka]

[0271] [In formula (2a), L′ is a sulfur atom or NR 50 R 50represents a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms; R 2 , R 3 , R 4 , s and t have the same meanings as above.] From the same viewpoint as above, another preferable example of the structure represented by formula (2) is a structure represented by the following formula (2b).

[0272] [ka]

[0273] [In formula (2b), R 44 is a hydroxy group, a carboxy group, or a group represented by the following formula (2-2)

[0274] [ka]

[0275] (In formula (2-2), L 11 represents *-O- or *-OCO-, and * represents L 12 represents a bond with L 12 represents an alkylene group having 1 to 20 carbon atoms, which may be interrupted by 1 to 3 -O-; R 44a OR 55 or COOR 55 R 55 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. It represents a group represented by the following formula: R 44 is preferably a group represented by formula (2-2). In this case, it is advantageous in terms of the solubility of the oxime compound (1) in the solvent (J) and the developability of the composition.

[0276] L 12 The alkylene group represented by the following formula (1) preferably has 1 to 10 carbon atoms, and more preferably has 1 to 4 carbon atoms.

[0277] R 44ais preferably a hydroxy group or a carboxy group, and more preferably a hydroxy group.

[0278] The method for producing the oxime compound (1) having the second molecular structure represented by formula (2) is not particularly limited, but it can be produced, for example, by the method described in JP-A-2011-132215.

[0279] Another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (3).

[0280] The bond represented by "*" in formula (3) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (3), the benzene ring having "-*" in formula (3) and the carbonyl group having "-*" in formula (1) are directly bonded.

[0281] [ka]

[0282] In formula (3), R 5 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0283] R 5 When the group represented by the formula (I) has an alkyl portion, the alkyl portion may be branched or cyclic.

[0284] R 5 The hydrogen atoms of the group represented by R 21 , OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR23 , N.R. 22 COR 21 , O.C.O.R. 21 , COOR 21 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , SCOR 21 , OCSR 21 , C.O.S.R. 21 , C.S.O.R. 21 , hydroxyl group, nitro group, CN, halogen atom, or COOR 21 may be substituted with.

[0285] R 21 , R 22 and R 23 has the same meaning as above.

[0286] R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group.

[0287] R 21 , R 22 and R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-.

[0288] R 24 has the same meaning as above.

[0289] R 21 , R 22 and R 23 When the group represented by R 22 and R 23may be joined together to form a ring.

[0290] R 6 , R 7 , R 8 and R 9 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom.

[0291] R 61 , R 62 , R 63 , R 64 and R 65 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0292] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom, or COOR 21may be substituted with.

[0293] R 6 and R 7 , R 7 and R 8 and R 8 and R 9 may be joined together to form a ring.

[0294] * represents a bond to the first molecular structure of the oxime compound (1).

[0295] R in Equation (3) 5 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.

[0296] R in Equation (3) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached.

[0297] R in Equation (3) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.

[0298] R in Equation (3) 6 , R 7 , R 8 and R 9 Halogen atoms represented by R 5 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0299] In one preferred embodiment, from the viewpoint of solubility in the solvent (J) and / or developability of the composition, R 5 is a group represented by the following formula (3-1).

[0300] [ka]

[0301] [In formula (3-1), Z represents a group in which one hydrogen atom has been removed from an alkyl group having 1 to 20 carbon atoms, a group in which one hydrogen atom has been removed from an aryl group having 6 to 30 carbon atoms, a group in which one hydrogen atom has been removed from an aralkyl group having 7 to 30 carbon atoms, or a group in which one hydrogen atom has been removed from a heterocyclic group having 2 to 20 carbon atoms, When the group represented by Z has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 COO-, -OCONR 24 may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-, and the alkylene moiety may be branched or cyclic; R 21 , R 22 and R 24 has the same meaning as above.] From the same viewpoint as above, Z in formula (3-1) is preferably a methylene group, an ethylene group, or a phenylene group.

[0302] R in formula (3-1) 21 and R 22 From the same viewpoint as above, is preferably an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 30 carbon atoms, and more preferably a methyl group, an ethyl group, or a phenyl group.

[0303] From the same viewpoint as above, in another preferred embodiment, R 7 is a nitro group.

[0304] The method for producing the oxime compound (1) having the second molecular structure represented by formula (3) is not particularly limited, but it can be produced by, for example, the methods described in JP-A-2000-80068 and JP-A-2011-178776.

[0305] Yet another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (4).

[0306] The bond represented by "*" in formula (4) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (4), the benzene ring having "-*" in formula (4) and the carbonyl group having "-*" in formula (1) are directly bonded.

[0307] [ka]

[0308] In formula (4), R 71 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0309] R 71 When the group represented by the formula (I) has an alkyl portion, the alkyl portion may be branched or cyclic.

[0310] R 71 The hydrogen atoms of the group represented by R 21 , OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , N.R. 22 COR 21 , O.C.O.R. 21 , COOR 21 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , SCOR 21 , OCSR 21 , C.O.S.R. 21 , C.S.O.R. 21 , hydroxyl group, nitro group, CN, halogen atom, or COOR 21 may be substituted with.

[0311] R 21 , R 22 and R 23 has the same meaning as above.

[0312] R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group.

[0313] R 21 , R 22 and R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-.

[0314] R 24 has the same meaning as above.

[0315] R 21 , R 22 and R 23 When the group represented by R 22 and R 23 may be joined together to form a ring.

[0316] R 72 , R 73 and 3 R 74 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom.

[0317] R 61 , R 62 , R 63 , R 64 and R 65 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0318] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom, or COOR 21 may be substituted with.

[0319] R 72 and R 73 and two R 74 may be joined together to form a ring.

[0320] * represents a bond to the first molecular structure of the oxime compound (1).

[0321] R in Equation (4) 71 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.

[0322] R in Equation (4) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached.

[0323] R in Equation (4) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.

[0324] R in Equation (4) 72 , R 73 and R 74 Halogen atoms represented by R 71 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0325] The method for producing the oxime compound (1) having the second molecular structure represented by formula (4) is not particularly limited, and it can be produced, for example, by the methods described in WO 2017 / 051680 and WO 2020 / 004601.

[0326] Yet another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (5).

[0327] The bond represented by "*" in formula (5) is directly bonded to the bond represented by "*" in formula (1). That is, when the second molecular structure is a structure represented by formula (5), the pyrrole ring having "-*" in formula (5) and the carbonyl group having "-*" in formula (1) are directly bonded.

[0328] [ka]

[0329] In formula (5), R81 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0330] R 81 When the group represented by the formula (I) has an alkyl portion, the alkyl portion may be branched or cyclic.

[0331] R 81 The hydrogen atoms of the group represented by R 21 , OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , N.R. 22 COR 21 , O.C.O.R. 21 , COOR 21 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , SCOR 21 , OCSR 21 , C.O.S.R. 21 , C.S.O.R. 21 , hydroxyl group, nitro group, CN, halogen atom, or COOR 21 may be substituted with.

[0332] R 21 , R 22 and R 23 has the same meaning as above.

[0333] R 21 , R 22 or R 23 The hydrogen atom of the group represented by the formula (I) may be substituted by CN, a halogen atom, a hydroxy group or a carboxy group.

[0334] R 21 , R22 and R 23 When the group represented by the formula (I) has an alkylene portion, the alkylene portion is preferably -O-, -S-, -COO-, -OCO-, -NR 24 -, -NR 24 CO-, -NR 24 COO-, -OCONR 24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS- or -CSO-.

[0335] R 24 has the same meaning as above.

[0336] R 21 , R 22 and R 23 When the group represented by R 22 and R 23 may be joined together to form a ring.

[0337] R 82 , R 83 , R 84 , R 85 and R 86 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom.

[0338] R 61 , R 62 , R 63 , R 64 and R 65each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0339] R 61 , R 62 , R 63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom, or COOR 21 may be substituted with.

[0340] R 83 and R 84 , R 84 and R 85 and R 85 and R 86 may be joined together to form a ring.

[0341] * represents a bond to the first molecular structure of the oxime compound (1).

[0342] R in Equation (5) 81 , R 21 , R 22 , R 23 , R 24 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R11 , R 12 , R 13 , R 21 , R 22 , R 23 and R 24 The example for is similar.

[0343] R in Equation (5) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached.

[0344] R in Equation (5) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.

[0345] R in Equation (5) 82 , R 83 , R 84 , R 85 and R 86 Halogen atoms represented by R 81 , R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0346] The method for producing the oxime compound (1) having the second molecular structure represented by formula (5) is not particularly limited, but can be produced, for example, by the methods described in WO 2017 / 051680 and WO 2020 / 004601.

[0347] Yet another example of the second molecular structure linked to the first molecular structure represented by formula (1) is a structure represented by the following formula (6).

[0348] The bond represented by "*" in formula (6) is directly bonded to the bond represented by "*" in formula (1). In other words, when the second molecular structure is a structure represented by formula (6), the benzene ring having "-*" in formula (6) and the carbonyl group having "-*" in formula (1) are directly bonded.

[0349] [ka]

[0350] In formula (6), four R 91 , R 92 , R 93 , R 94 , R 95 , R 96 and R 97 are each independently R 61 , OR 61 , S.R. 61 , C.O.R. 62 ,CONR 63 R 64 , N.R. 65 COR 61 , O.C.O.R. 61 , COOR 62 , SCOR 61 , OCSR 61 , C.O.S.R. 62 , C.S.O.R. 61 , a hydroxyl group, a nitro group, CN or a halogen atom.

[0351] R 61 , R 62 , R 63 , R 64 and R 65 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms.

[0352] R 61 , R 62 , R63 , R 64 or R 65 The hydrogen atoms of the group represented by OR 21 , C.O.R. 21 , S.R. 21 , N.R. 22 R 23 ,CONR 22 R 23 , -NR 22 -OR 23 , -N(COR 22 )-OCOR 23 , -C(=N-OR 21 )-R 22 , -C(=N-OCOR 21 )-R 22 , CN, halogen atom, or COOR 21 may be substituted with.

[0353] R 21 , R 22 and R 23 has the same meaning as above.

[0354] R 92 and R 93 , R 94 and R 95 , R 95 and R 96 and R 96 and R 97 may be joined together to form a ring.

[0355] * represents a bond to the first molecular structure of the oxime compound (1).

[0356] R in Equation (6) 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of the alkyl group having 1 to 20 carbon atoms, the aryl group having 6 to 30 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, and the heterocyclic group having 2 to 20 carbon atoms, which are represented by the formula (1), are R 11 , R 12 , R 13 , R 21, R 22 and R 23 The example for is similar.

[0357] R in Equation (6) 22 and R 23 may be joined together to form a ring, R 22 and R 23 means that they may be taken together to form a ring with the nitrogen atom, carbon atom or oxygen atom to which they are attached.

[0358] R in Equation (6) 22 and R 23 Examples of rings that may be formed by combining with each other include R 12 and R 13 and R 22 and R 23 The same is true for the ring which may be formed by combining with each other.

[0359] R in Equation (6) 91 , R 92 , R 93 , R 94 , R 95 , R 96 and R 97 Halogen atoms represented by R 21 , R 22 , R 23 , R 61 , R 62 , R 63 , R 64 and R 65 Examples of halogen atoms which may replace the hydrogen atoms of include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0360] The method for producing the oxime compound (1) having the second molecular structure represented by formula (6) is not particularly limited, but can be produced, for example, by the methods described in WO 2017 / 051680 and WO 2020 / 004601.

[0361] Another example of the oxime compound (excluding the oxime compound (1)) is a compound represented by the formula (EA).

[0362] [ka] [In the formula, R ea1 represents a branched hydrocarbon group having 3 to 20 carbon atoms which may have a substituent. R ea2 ~R ea5 each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. and n represents an integer of 0 to 4. The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO- or -OCO-.

[0363] R ea1 Examples of the branched hydrocarbon group having 3 to 20 carbon atoms represented by the formula (I) include a branched saturated hydrocarbon group having 3 to 20 carbon atoms and a branched unsaturated hydrocarbon group having 3 to 20 carbon atoms.

[0364] R ea1Examples of the branched saturated hydrocarbon group having 3 to 20 carbon atoms represented by the formula (I) include a 1-methylethyl group (isopropyl group), a 1-methylpropyl group (sec-butyl group), a 2-methylpropyl group (isobutyl group), a 1,1-dimethylethyl group (tert-butyl group), a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylbutyl group, and a 2,2-dimethylbutyl group. , 3,3-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 3,3-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 2,3-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3 -ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 1,1-dimethylhexyl group, 2,2-dimethylhexyl group, 3,3-dimethylhexyl group, 1,2-dimethylhexyl group, 1,3-dimethylhexyl group, 2,3-dimethylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 4-methylheptyl group, 1,1-dimethylhexyl group butyl group, 2,2-dimethylheptyl group, 3,3-dimethylheptyl group, 1,2-dimethylheptyl group, 1,3-dimethylheptyl group, 2,3-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 3-ethylheptyl group, 1-methyloctyl group, 2-methyloctyl group, 3-methyloctyl group, 4-methyloctyl group, 1,1-dimethyloctyl group, 2,2-dimethyloctyl group, 3,3-dimethyloctyl group, 1,2-dimethyloctyl group, 1,3-dimethyloctyl group, 2,Branched alkyl groups such as 3-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, dimethylnonyl group, ethylnonyl group, methyldecyl group, dimethyldecyl group, ethyldecyl group, methylundecyl group, dimethylundecyl group, ethylundecyl group, and methyldodecyl group are included. R ea1 The branched alkyl group represented by the formula (I) may be a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. R ea1 The number of carbon atoms in the branched saturated hydrocarbon group represented by the formula (I) is preferably 4 or more, more preferably 5 or more, and is preferably 16 or less, more preferably 12 or less, and further preferably 10 or less.

[0365] R ea1 The branched unsaturated hydrocarbon group represented by the above-mentioned R ea1 Examples of the branched saturated hydrocarbon group include those in which at least one carbon-carbon single bond contained in the branched saturated hydrocarbon group represented by the following formula (I) is replaced with a carbon-carbon double bond or a carbon-carbon triple bond. R ea1 Examples of the branched unsaturated hydrocarbon group represented by the formula (I) include alkenyl groups such as an isopropenyl group, an isobutenyl group, an isopentenyl group, an isohexenyl group, an isoheptenyl group, an isooctenyl group, an isononyl group, and an isodecenyl group; and alkynyl groups such as an isopropynyl group, an isobutynyl group, an isopentynyl group, an isohexynyl group, an isoheptynyl group, an isooctynyl group, an isononynyl group, and an isodecynyl group. R ea1 The branched unsaturated hydrocarbon group represented by the formula (I) has preferably 4 or more, more preferably 5 or more, and preferably 16 or less, more preferably 12 or less, and further preferably 10 or less.

[0366] R ea2 , R ea3 , R ea4 and R ea5Examples of the hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) include a saturated hydrocarbon group having 1 to 20 carbon atoms, an unsaturated hydrocarbon group having 2 to 20 carbon atoms, and an aromatic hydrocarbon group having 6 to 20 carbon atoms. ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon groups represented by the following formula may be the same or different.

[0367] Examples of the saturated hydrocarbon group having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and icosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.

[0368] Examples of the unsaturated hydrocarbon group having 2 to 20 carbon atoms include alkenyl groups such as vinyl group, allyl group, butenyl group, pentenyl group, hexenyl group, heptenyl group, octenyl group, nonenyl group, decenyl group, undecenyl group, dodecenyl group, hexadecenyl group, octadecenyl group, and icosenyl group; alkynyl groups such as ethynyl group, propynyl group, hexynyl group, decynyl group, and icosenyl group; cycloalkenyl groups such as cyclopentenyl group, cyclohexenyl group, and cycloheptenyl group; etc. The number of carbon atoms in the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.

[0369] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a xylyl group, a trimethylphenyl group, a dipropylphenyl group, a di(2,2-dimethylpropyl)phenyl group, a naphthyl group, a benzyl group, a phenylethyl group, a phenylbutyl group, etc. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and further preferably 6 to 12.

[0370] R ea1 , R ea2 , R ea3 , R ea4 and R ea5 Examples of the substituent that the hydrocarbon group represented by the formula (I) may have include a halogen atom, a cyano group, and a nitro group. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom.

[0371] The -CH2- contained in the hydrocarbon group may be replaced by -O-, -S-, -CO- or -OCO-, provided that adjacent -CH2- are not simultaneously replaced by the same type of group, and the terminal -CH2- is not replaced.

[0372] n represents an integer of 0 to 4, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, further preferably an integer of 0 or 1, and even more preferably 0.

[0373] *-OCO-R ea4 The bonding position of the group (* represents a bond to the phenyl group) is the *-OCO-R ea4 The group may be bonded to any of the 2-, 3- or 4-positions of the phenyl group, but is preferably bonded to the 3- or 4-position, more preferably to the 4-position.

[0374] R ea1 The branched hydrocarbon group having 3 to 20 carbon atoms represented by the formula: A branched saturated hydrocarbon group having 3 to 20 carbon atoms is preferred. A branched alkyl group having 3 to 20 carbon atoms is more preferable. A branched alkyl group having 3 to 10 carbon atoms is more preferable. It is preferable that the alkyl group is one or more selected from the group consisting of a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1-ethylpentyl group, a 2-ethylpentyl group, a 3-ethylpentyl group, a 1-methylhexyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 1-ethylhexyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, a 1-methylheptyl group, a 2-methylheptyl group, a 3-methylheptyl group, a 1-ethylheptyl group, a 2-ethylheptyl group, and a 3-ethylheptyl group.

[0375] R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group having 1 to 20 carbon atoms represented by the formula: A saturated hydrocarbon group having 1 to 20 carbon atoms and an unsaturated hydrocarbon group having 2 to 20 carbon atoms are preferred. A saturated hydrocarbon group having 1 to 20 carbon atoms is more preferable. A chain-like saturated hydrocarbon group having 1 to 10 carbon atoms is more preferable. A chain alkyl group having 1 to 8 carbon atoms is even more preferred. R ea2 is preferably a chain alkyl group having 1 to 8 carbon atoms, and more preferably a chain alkyl group having 1 to 6 carbon atoms. R ea3 is preferably a chain alkyl group having 1 to 8 carbon atoms, and more preferably a chain alkyl group having 1 to 3 carbon atoms. R ea4 is preferably a chain alkyl group having 1 to 8 carbon atoms, and more preferably a chain alkyl group having 1 to 3 carbon atoms. R ea5 is preferably a linear or branched alkyl group having 1 to 8 carbon atoms, and more preferably a linear or branched alkyl group having 1 to 6 carbon atoms.

[0376] Other examples of the photopolymerization initiator include photopolymerization initiators other than the oxime compound (1) and the compound represented by formula (EA). Examples of the other photopolymerization initiators include oxime compounds other than the oxime compound (1) and the compound represented by formula (EA), biimidazole compounds, triazine compounds, and acylphosphine compounds.

[0377] Examples of oxime compounds other than the oxime compound (1) and the compound represented by formula (EA) include oxime compounds having a partial structure represented by the following formula (d1): * represents a bond.

[0378] [ka]

[0379] Examples of the oxime compound having a partial structure represented by formula (d1) include N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropan-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-imine, N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2-phenyl)ethyl]ethane-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2-phenyl)ethyl]ethane-1-imine. ,4-dioxacyclopentanylmethyloxy)benzoyl}-9H-carbazol-3-yl]ethane-1-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-3-cyclopentylpropan-1-imine, N-benzoyloxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-3-cyclopentylpropan-1-one-2-imine; compounds described in JP 2011-132215 A, WO 2008 / 78678, WO 2008 / 78686, and WO 2012 / 132558. Commercially available products such as Irgacure OXE01 (N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine), OXE02 (N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-imine) (both manufactured by BASF), and N-1919 (manufactured by ADEKA) may also be used.

[0380] Among them, the oxime compound having a partial structure represented by formula (d1) is preferably at least one selected from the group consisting of N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-imine and N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropan-1-one-2-imine, and more preferably N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine or N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-imine.

[0381] An example of the biimidazole compound is a compound represented by the formula (d5).

[0382] [ka]

[0383] [In formula (d5), R E ~R J represents an aryl group having 6 to 10 carbon atoms which may have a substituent.] Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group, a toluyl group, a xylyl group, an ethylphenyl group, and a naphthyl group, and preferably a phenyl group.

[0384] Examples of the substituent include a halogen atom and an alkoxy group having 1 to 4 carbon atoms. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and preferably a chlorine atom. Examples of the alkoxy group having 1 to 4 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group, and preferably a methoxy group.

[0385] Examples of the biimidazole compound include 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole (see, for example, JP-A-06-75372 and JP-A-06-75373), 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(alkoxyphenyl) 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(dialkoxyphenyl)biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(trialkoxyphenyl)biimidazole (see, for example, JP-B-48-38403 and JP-A-62-174204), biimidazole compounds in which the phenyl groups at the 4,4',5,5'-positions are substituted with carboalkoxy groups (see, for example, JP-A-7-10913), etc. Among these, the compounds represented by the following formula or mixtures thereof are preferred.

[0386] [ka]

[0387] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[ 2-(5-methylfuran-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine, etc. Among them, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine is preferred.

[0388] Examples of the acylphosphine compound include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and (2,4,6-trimethylbenzoyl)diphenylphosphine oxide.

[0389] Other examples of photopolymerization initiators other than the oxime compound (1) and the compound represented by formula (EA) include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenone compounds such as benzophenone, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, and 4,4'-bis(diethylamino)benzophenone; quinone compounds such as 9,10-phenanthrenequinone, 2-ethylanthraquinone, and camphorquinone; 10-butyl-2-chloroacridone, benzyl, methyl phenylglyoxylate, and titanocene compounds.

[0390] The content of the polymerization initiator (E) in the composition I is preferably 0.1 parts by mass or more and 300 parts by mass or less, more preferably 0.1 parts by mass or more and 200 parts by mass or less, based on 100 parts by mass of the polymerizable compound (D). The content of the polymerization initiator (E) in the composition I is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, based on 100 parts by mass of the total amount of the resin (C) and the polymerizable compound (D). When the content of the polymerization initiator (E) is within the above range, the sensitivity of the composition I tends to be increased and the exposure time tends to be shortened, so that the productivity of the wavelength conversion layer tends to be improved.

[0391] The content of the polymerization initiator (E) in the composition II is preferably 0.001 mass % or more and 60 mass % or less, more preferably 0.01 mass % or more and 50 mass % or less, based on the total amount of the resin (C) and the polymerizable compound (D).

[0392] The content of the polymerization initiator (E) in the composition III is preferably 0.001 mass% or more and 60 mass% or less, more preferably 0.01 mass% or more and 50 mass% or less, even more preferably 0.05 mass% or more and 30 mass% or less, and even more preferably 0.1 mass% or more and 10 mass% or less, based on the total amount of the resin (C) and the polymerizable compound (D).

[0393] From the viewpoint of improving the luminescence intensity, the content of the oxime compound (1) in the polymerization initiator (E) is preferably 30% by mass or more and 100% by mass or less, more preferably 50% by mass or more and 100% by mass or less, even more preferably 80% by mass or more and 100% by mass or less, still more preferably 90% by mass or more and 100% by mass or less, particularly preferably 95% by mass or more and 100% by mass or less, and most preferably 100% by mass, based on the total amount of the polymerization initiator (E).

[0394] <Polymerization initiator aid (E1)> The composition may further contain a polymerization initiation aid (E1) together with the polymerization initiator (E). The polymerization initiation aid (E1) is a compound used to promote the polymerization of the polymerizable compound (D) initiated by the polymerization initiator (E), or a sensitizer. Examples of the polymerization initiation aid (E1) include photopolymerization initiation aids such as amine compounds, alkoxyanthracene compounds, thioxanthone compounds, and carboxylic acid compounds, as well as thermal polymerization initiation aids. The composition may contain two or more types of polymerization initiation aids (E1).

[0395] Examples of the amine compound include triethanolamine, methyldiethanolamine, triisopropanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-dimethylaminoethyl benzoate, 2-ethylhexyl 4-dimethylaminobenzoate, N,N-dimethyl-p-toluidine, 4,4'-bis(dimethylamino)benzophenone (commonly known as Michler's ketone), 4,4'-bis(diethylamino)benzophenone, and 4,4'-bis(ethylmethylamino)benzophenone.

[0396] Examples of the alkoxyanthracene compound include 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 2-ethyl-9,10-diethoxyanthracene, 9,10-dibutoxyanthracene, and 2-ethyl-9,10-dibutoxyanthracene.

[0397] Examples of thioxanthone compounds include 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone.

[0398] Examples of the carboxylic acid compound include phenylsulfanylacetic acid, methylphenylsulfanylacetic acid, ethylphenylsulfanylacetic acid, methylethylphenylsulfanylacetic acid, dimethylphenylsulfanylacetic acid, methoxyphenylsulfanylacetic acid, dimethoxyphenylsulfanylacetic acid, chlorophenylsulfanylacetic acid, dichlorophenylsulfanylacetic acid, N-phenylglycine, phenoxyacetic acid, naphthylthioacetic acid, N-naphthylglycine, and naphthoxyacetic acid.

[0399] When the composition I contains the polymerization initiation aid (E1), the content of the polymerization initiation aid (E1) in the composition I is preferably 0.1 parts by mass or more and 300 parts by mass or less, more preferably 0.1 parts by mass or more and 200 parts by mass or less, based on 100 parts by mass of the polymerizable compound (D). The content of the polymerization initiation aid (E1) in the composition I is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 1 part by mass or more and 20 parts by mass or less, based on 100 parts by mass of the total amount of the resin (C) and the polymerizable compound (D). When the content of the polymerization initiation aid (E1) is within the above range, the sensitivity of the composition I can be further increased.

[0400] When the polymerization initiator aid (E1) is used, the content of the polymerization initiator aid (E1) in the composition II is preferably 0.00001 mass% or more and 60 mass% or less, more preferably 0.0001 mass% or more and 50 mass% or less, based on the total amount of the resin (C) and the polymerizable compound (D). The content of the polymerization initiator aid (E1) in the composition II is preferably 0.1 mass% or more and 30 mass% or less, more preferably 1 mass% or more and 20 mass% or less, based on 100 mass parts of the total amount of the resin (C) and the polymerizable compound (D).

[0401] When the polymerization initiation aid (E1) is used, the content of the polymerization initiation aid (E1) in the composition III is preferably 0.00001 mass% or more and 60 mass% or less, more preferably 0.0001 mass% or more and 50 mass% or less, based on the total amount of the resin (C) and the polymerizable compound (D). The content of the polymerization initiation aid (E1) in the composition III is preferably 0.1 mass% or more and 30 mass% or less, more preferably 1 mass% or more and 20 mass% or less, based on 100 mass% of the total amount of the resin (C) and the polymerizable compound (D).

[0402] <Antioxidants (F)> The antioxidant (F) is not particularly limited as long as it is an antioxidant generally used industrially, and examples of the antioxidant that can be used include phenol-based antioxidants, phosphorus-based antioxidants, phosphorus / phenol complex antioxidants, and sulfur-based antioxidants. The composition may contain two or more types of antioxidants (F).

[0403] The phosphorus / phenol complex type antioxidant is, for example, a compound having one or more phosphorus atoms and one or more phenol structures in the molecule. Among them, from the viewpoint of the developability and luminescence intensity of the composition, it is preferable that the antioxidant (F) contains a phosphorus / phenol complex type antioxidant.

[0404] Examples of phenol-based antioxidants include Irganox (registered trademark) 1010 (Irganox 1010: pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], manufactured by BASF Ltd.), Irganox 1076 (Irganox 1076: octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, manufactured by BASF Ltd.), Irganox 1330 (Irganox 1330: 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4,6-triyl) tri-p-cresol, manufactured by BASF Ltd.), and Irganox 3114 (Irganox 3114: 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Co., Ltd.), 3790 (Irganox 3790: 1,3,5-tris((4-tert-butyl-3-hydroxy-2,6-xylyl)methyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, manufactured by BASF Co., Ltd.), 1035 (Irganox 1035: thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], manufactured by BASF Co., Ltd.), 1135 (Irganox 1135: 3,5-bis(1,1-dimethylethyl)-4-hydroxy-C7-C9 side chain alkyl ester of benzenepropanoic acid, manufactured by BASF Co., Ltd.), 1520L (Irganox 1520L: 4,6-bis(octylthiomethyl)-o-cresol, manufactured by BASF Co., Ltd.), 3125 (Irganox 3125, manufactured by BASF Co., Ltd.), 565 (Irganox 565: 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, manufactured by BASF Co., Ltd.), Adeka STAB (registered trademark) AO-80 (Adeka STAB AO-80: 3,9-bis(2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5) Undecane (manufactured by ADEKA Co., Ltd.), Sumilizer (registered trademark) BHT, Sumilizer GA-80, and Sumilizer GS (all manufactured by Sumitomo Chemical Co., Ltd.), Cyanox (registered trademark) 1790 (manufactured by Cytec Co., Ltd.), and Vitamin E (manufactured by Eisai Co., Ltd.).

[0405] Examples of phosphorus-based antioxidants include Irgafos (registered trademark) 168 (Irgafos 168: tris(2,4-di-tert-butylphenyl)phosphite, manufactured by BASF Co., Ltd.), Irgafos 12 (Irgafos 12: tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphine-6-yl]oxy]ethyl]amine, manufactured by BASF Co., Ltd.), Irgafos 38 (Irgafos 38: bis(2,4-bis(1,1-dimethylethyl)-6-methylphenyl)ethyl ester phosphorous acid, manufactured by BASF Co., Ltd.), Adeka STAB (registered trademark) 329K, Adeka STAB PEP36, Adeka STAB PEP-8 (all manufactured by ADEKA Co., Ltd.), Sandstab Examples of such antibacterial agents include P-EPQ (manufactured by Clariant), Weston (registered trademark) 618, Weston 619G (all manufactured by GE), and Ultranox 626 (manufactured by GE).

[0406] Examples of phosphorus / phenol complex antioxidants include Sumilizer (registered trademark) GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1.3.2]dioxaphosphepine) (manufactured by Sumitomo Chemical Co., Ltd.).

[0407] Examples of the sulfur-based antioxidant include dialkyl thiodipropionate compounds such as dilauryl, dimyristyl, and distearyl thiodipropionate, and β-alkyl mercaptopropionate compounds of polyols such as tetrakis[methylene(3-dodecylthio)propionate]methane.

[0408] The content of the antioxidant (F) in the composition I is, for example, 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the resin (C), and from the viewpoints of luminescence intensity and heat resistance, it is preferably 5 parts by mass or more and 40 parts by mass or less, and more preferably 7 parts by mass or more and 30 parts by mass or less.

[0409] The content of the antioxidant (F) in the composition II is, for example, 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the resin (C), and from the viewpoints of luminescence intensity and heat resistance, it is preferably 5 parts by mass or more and 40 parts by mass or less, and more preferably 7 parts by mass or more and 30 parts by mass or less.

[0410] The content of the antioxidant (F) in the composition III is, for example, 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the resin (C), and from the viewpoints of luminescence intensity and heat resistance, it is preferably 5 parts by mass or more and 40 parts by mass or less, and more preferably 7 parts by mass or more and 30 parts by mass or less.

[0411] <Solvent (J)> The solvent (J) is preferably one that dissolves the resin (C), the polymerizable compound (D) and the polymerization initiator (E). Examples of the solvent (J) include an ester solvent (a solvent containing -COO- in the molecule and not containing -O-), an ether solvent (a solvent containing -O- in the molecule and not containing -COO-), an ether ester solvent (a solvent containing -COO- and -O- in the molecule), a ketone solvent (a solvent containing -CO- in the molecule and not containing -COO-), an alcohol solvent (a solvent containing OH in the molecule and not containing -O-, -CO- and COO-), an aromatic hydrocarbon solvent, an amide solvent, and dimethyl sulfoxide.

[0412] Examples of the ester solvent include methyl lactate, ethyl lactate, n-butyl lactate, methyl 2-hydroxyisobutanoate, ethyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, isopropyl butyrate, ethyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, cyclohexyl acetate, and γ-butyrolactone.

[0413] Examples of the ether solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, 3-methoxy-1-butanol, 3-methoxy-3-methylbutanol, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, anisole, phenetole, and methylanisole.

[0414] The ether ester solvents include methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate, methyl 2-methoxy-2-methyl ... Examples of the alkyl ether acetates include ethyl methoxy-2-methylpropionate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0415] Examples of ketone solvents include 4-hydroxy-4-methyl-2-pentanone, acetone, 2-butanone, 2-heptanone, 3-heptanone, 4-heptanone, 4-methyl-2-pentanone, cyclopentanone, cyclohexanone, and isophorone.

[0416] Examples of the alcohol solvent include methanol, ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, propylene glycol, and glycerin.

[0417] Aromatic hydrocarbon solvents include benzene, toluene, xylene, and mesitylene.

[0418] Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0419] The solvent (J) preferably contains one or more solvents selected from the group consisting of propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, cyclohexyl acetate, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone, and aromatic hydrocarbon solvents.

[0420] The solvent (J) is preferably propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, cyclohexyl acetate, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone or toluene, or a mixture of two or more of these.

[0421] The solvent (J) is a component other than the solid content, and for example, the solvent contained in the dispersion of the semiconductor particles (A) and the solution of the resin (C) is also included in the solvent (J).

[0422] The content of solvent (J) in composition I is the ratio of the total mass of all solvents contained in the composition to the total amount of composition I, and is, for example, from 40% by mass to 95% by mass, and preferably from 55% by mass to 90% by mass, relative to the total amount of composition I. In other words, the solid content of composition I is, for example, from 5% by mass to 60% by mass, and preferably from 10% by mass to 45% by mass. When the content of solvent (J) is within the above range, the flatness of the composition layer during application is improved, and a wavelength conversion layer of an appropriate thickness tends to be easily formed.

[0423] The solid content of composition II is preferably 0.01% by mass or more and 100% by mass or less, more preferably 0.1% by mass or more and 99.9% by mass or less, even more preferably 0.1% by mass or more and 99% by mass or less, still more preferably 1% by mass or more and 90% by mass or less, even more preferably 1% by mass or more and 80% by mass or less, particularly preferably 1% by mass or more and 70% by mass or less, extremely preferably 1% by mass or more and 60% by mass or less, and most preferably 1% by mass or more and 50% by mass or less, based on the total amount of composition II.

[0424] The solid content of composition III is, relative to the total amount of composition III, preferably 0.01% by mass or more and 100% by mass or less, more preferably 0.1% by mass or more and 99.9% by mass or less, even more preferably 0.1% by mass or more and 99% by mass or less, still more preferably 1% by mass or more and 90% by mass or less, even more preferably 1% by mass or more and 80% by mass or less, particularly preferably 1% by mass or more and 70% by mass or less, extremely preferably 1% by mass or more and 60% by mass or less, and most preferably 1% by mass or more and 50% by mass or less.

[0425] <Leveling Agent (H)> The leveling agent (H) may be a silicone surfactant, a fluorine surfactant, or a silicone surfactant having a fluorine atom. These may have a polymerizable group in the side chain. From the viewpoint of the developability and luminescence intensity of the composition, the leveling agent (H) is preferably a fluorine surfactant. The composition may contain two or more types of leveling agents (H).

[0426] Examples of silicone surfactants include surfactants having a siloxane bond in the molecule.Specific examples include Toray Silicone DC3PA, SH7PA, DC11PA, SH21PA, SH28PA, SH29PA, SH30PA, and SH8400 (trade name: manufactured by Toray Dow Corning Co., Ltd.), KP321, KP322, KP323, KP324, KP326, KP340, and KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF4446, TSF4452, and TSF4460 (manufactured by Momentive Performance Materials Japan LLC).

[0427] Examples of fluorine-based surfactants include surfactants having a fluorocarbon chain in the molecule.Specific examples include Fluorad (registered trademark) FC430, FC431 (manufactured by Sumitomo 3M Limited), Megafac (registered trademark) F142D, F171, F172, F173, F177, F183, F554, F575, R30, RS-718-K (manufactured by DIC Corporation), F-top (registered trademark) EF301, EF303, EF351, EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Surflon (registered trademark) S381, S382, SC101, SC105 (manufactured by Asahi Glass Co., Ltd.), and E5844 (manufactured by Daikin Fine Chemicals Research Institute Co., Ltd.).

[0428] Examples of silicone surfactants having fluorine atoms include surfactants having a siloxane bond and a fluorocarbon chain in the molecule, such as Megafac (registered trademark) R08, BL20, F475, F477, and F443 (manufactured by DIC Corporation).

[0429] When composition I contains the leveling agent (H), the content of the leveling agent (H) in composition I is, for example, 0.001 mass % or more and 1.0 mass % or less, preferably 0.005 mass % or more and 0.75 mass % or less, and more preferably 0.01 mass % or more and 0.5 mass % or less, relative to the total amount of composition I. When the content of the leveling agent (H) is within the above range, the flatness of the wavelength conversion layer can be improved.

[0430] When composition II contains a leveling agent (H), the content of the leveling agent (H) in composition II is, for example, 0.001 mass% or more and 1.0 mass% or less, preferably 0.005 mass% or more and 0.75 mass% or less, and more preferably 0.01 mass% or more and 0.5 mass% or less, relative to the total amount of composition II.

[0431] When composition III contains a leveling agent (H), the content of the leveling agent (H) in composition III is, for example, 0.001 mass% or more and 1.0 mass% or less, preferably 0.005 mass% or more and 0.75 mass% or less, and more preferably 0.01 mass% or more and 0.5 mass% or less, relative to the total amount of composition III.

[0432] <Other ingredients> Compositions I, II and III may further contain additives known in the art, such as ultraviolet absorbers, polymerization inhibitors, fillers, other polymer compounds, adhesion promoters, light stabilizers, chain transfer agents, etc., as necessary.

[0433] Examples of the ultraviolet absorber include benzotriazole-based compounds such as 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole and (2-(2,4-dihydroxyphenyl)-2H-benzotriazole; benzophenone-based compounds such as 2-hydroxy-4-octyloxybenzophenone; benzoate-based compounds such as 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate; and triazine-based compounds such as 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol.

[0434] <Method of producing the composition> Compositions I, II, and III can be produced by a method including a step of mixing the prescribed components and other components used as necessary. The method of producing compositions I, II, and III can further include a step of preparing resin (C).

[0435] When using the colorant (I), it is preferable to use the colorant (I) in the form of a colorant dispersion liquid in which the colorant (I) is mixed in advance with a part or all of the solvent (J) and dispersed using a bead mill or the like until the average particle size of the colorant (I) is about 0.2 μm or less. In this case, a dispersant and a part or all of the resin (C) may be mixed as necessary. As for the dispersant, the description of the dispersant described in the section on the light scattering agent (B) is cited.

[0436] <Method of manufacturing laminate> 1. Wavelength-Converting Layer (Composition I) The wavelength conversion layer may be, for example, Method a, comprising the step of applying composition I to a substrate and then drying it; or A method b in which a wavelength-converting layer is produced by a method including a step of applying composition I to a support and then drying the applied composition, and then the wavelength-converting layer is peeled off from the support and attached to a substrate via an adhesive layer. The coating can be provided on the substrate by the above-mentioned methods.

[0437] In one embodiment, the composition I is a resin composition R1 further containing a resin (C). The wavelength conversion layer (resin film) formed from the resin composition R1 can be formed by applying the composition I to a substrate or support and then drying it. In another embodiment, the composition I is a curable composition R2 further comprising a polymerizable compound (D) and a polymerization initiator (E). The curable composition R2 may further comprise a resin (C). The wavelength conversion layer formed from the curable composition R2 is a cured film. The cured film can be obtained by applying the curable composition R2 to a substrate or support, drying the composition, and curing the composition by the action of light and / or heat. One embodiment of the curable composition R2 is a photocurable composition R3 containing a photopolymerizable compound and a photopolymerization initiator. The photocurable composition R3 may further contain a resin (C).

[0438] 2. Overcoat Layer (Composition III) In one embodiment, the composition III is a resin composition R4 further containing a resin (C). The overcoat layer (resin film) formed from the resin composition R4 can be formed by applying the composition III to a substrate and then drying it. In another embodiment, the composition III is a curable composition R5 further comprising a polymerizable compound (D) and a polymerization initiator (E). The curable composition R5 may further comprise a resin (C). The overcoat layer formed from the curable composition R5 is a cured film. The cured film can be obtained by applying the curable composition R5 to a substrate, drying the composition, and curing the composition by the action of light and / or heat. One embodiment of the curable composition R5 is a photocurable composition R6 containing a photopolymerizable compound and a photopolymerization initiator. The photocurable composition R6 may further contain a resin (C).

[0439] 3. Light-absorbing layer (composition II) In one embodiment, the composition II is a resin composition R7 further containing a resin (C). The light absorbing layer (resin film) formed from the resin composition R7 can be formed by applying the composition II to a substrate and then drying it. In another embodiment, the composition II is a curable composition R8 further comprising a polymerizable compound (D) and a polymerization initiator (E). The curable composition R8 may further comprise a resin (C). The light absorbing layer formed from the curable composition R8 is a cured film. The cured film can be obtained by applying the curable composition R8 to a substrate, drying the composition, and curing the composition by the action of light and / or heat. One embodiment of the curable composition R8 is a photocurable composition R9 containing a photopolymerizable compound and a photopolymerization initiator. The photocurable composition R9 may further contain a resin (C).

[0440] 4.Base material Examples of the substrate on which the wavelength conversion layer is formed include glass plates such as quartz glass, borosilicate glass, alumina silicate glass, and soda lime glass with a silica-coated surface; resin plates such as polycarbonate, polymethyl methacrylate, and polyethylene terephthalate; silicon; aluminum, silver, and silver / copper / palladium alloy thin films formed on these substrates; and members that are or can be included in the display device. Examples of the members that are or can be included in the display device include a primary light source (e.g., a blue light source), a light guide plate, a diffusion film (diffusion layer), a light reflecting member (such as a reflection film), a brightness enhancing member, a prism sheet, a barrier layer, and a protective layer.

[0441] The substrate on which the overcoat layer is formed is the wavelength converting layer or another layer formed on the wavelength converting layer (however, a layer different from the wavelength converting layer, the overcoat layer, and the light absorbing layer).

[0442] The substrate on which the light absorbing layer is formed is an overcoat layer or another layer formed on the overcoat layer (however, a layer different from the wavelength converting layer, the overcoat layer, and the light absorbing layer).

[0443] The wavelength conversion layer, the overcoat layer, and the light absorbing layer may be provided on the entire surface of each substrate, or may be provided in a pattern on a part of the substrate. Methods for forming each layer (wavelength conversion layer, overcoat layer, or light absorbing layer) in a pattern on the substrate include photolithography, inkjet, and printing. Examples of printing methods include stencil printing, screen printing, and printing and coating using an applicator.

[0444] 5. Manufacturing method The patterned resin film (wavelength conversion layer) formed from the resin composition R1, the patterned resin film (overcoat layer) formed from the resin composition R4, and the patterned resin film (light absorbing layer) formed from the resin composition R7 can be formed on the substrate corresponding to each of the above-mentioned layers, for example, as follows. First, the resin composition R1, R4, or R7 is applied to the substrate corresponding to each of the above-mentioned layers through a mask to form a patterned composition layer. Examples of the method for applying the resin composition include spin coating, slit coating, and slit and spin coating.

[0445] Next, the composition layer is dried (volatile components such as solvent are removed) to obtain a resin film (wavelength conversion layer, overcoat layer, or light absorbing layer). Examples of the drying method include heat drying, reduced pressure drying, and a combination of these. The temperature when heat drying is performed is preferably 30°C or more and 250°C or less, more preferably 50°C or more and 235°C or less. The heating time is preferably 10 seconds or more and 180 minutes or less, more preferably 30 seconds or more and 90 minutes or less. When reduced pressure drying is performed, it is preferably performed under a pressure of 50 Pa or more and 150 Pa or less. The drying of the composition layer may be performed in multiple stages, for example, by performing multiple drying steps with different drying temperatures.

[0446] The patterned cured film (wavelength conversion layer) formed from the photocurable composition R3, the patterned cured film (overcoat layer) formed from the photocurable composition R6, and the patterned cured film (light absorbing layer) formed from the photocurable composition R9 can be formed on the substrate corresponding to each of the above-mentioned layers, for example, by using a photolithography method as follows. First, the photocurable composition R3, R6, or R9 is applied onto the substrate corresponding to each of the above-mentioned layers, and volatile components such as solvents are removed by heating and drying (pre-baking) and / or drying under reduced pressure to obtain a composition layer. The coating method can be the same as that described above.

[0447] The temperature in the case of heat drying is preferably 30° C. to 120° C., more preferably 50° C. to 110° C. The heating time is preferably 10 seconds to 60 minutes, more preferably 30 seconds to 30 minutes. In the case of reduced pressure drying, it is preferably performed under a pressure of 50 Pa to 150 Pa at a temperature range of 20° C. to 25° C.

[0448] Next, the composition layer is exposed through a photomask to form a desired pattern shape. The light source used for exposure is preferably a light source that generates light with a wavelength of 250 nm or more and 450 nm or less. For example, from the light with the wavelength, light with a wavelength of around 436 nm, around 408 nm, or around 365 nm may be selectively extracted by a bandpass filter according to the absorption wavelength of the photopolymerization initiator. Specific examples of the light source include a mercury lamp, a light-emitting diode, a metal halide lamp, and a halogen lamp.

[0449] It is preferable to use an exposure device such as a mask aligner or a stepper, since it is possible to uniformly irradiate the entire exposure surface with parallel light rays and to accurately align the photomask with the substrate on which the composition layer is formed. The exposed composition layer is cured by polymerization of the photopolymerizable compound and the like contained in the composition layer.

[0450] By contacting the composition layer after exposure with a developer and developing it, the unexposed parts of the composition layer are dissolved in the developer and removed, and a patterned cured film (wavelength conversion layer, overcoat layer, or light absorbing layer) is obtained. Examples of the developer include aqueous solutions of alkaline compounds such as potassium hydroxide, sodium bicarbonate, sodium carbonate, and tetramethylammonium hydroxide, and organic solvents. The concentration of the alkaline compound in the aqueous solution is preferably 0.01% by mass or more and 10% by mass or less, and more preferably 0.03% by mass or more and 5% by mass or less. Examples of the organic solvent include the same as the above-mentioned solvent (J). The developer may contain a surfactant.

[0451] The developing method may be any of a puddle method, a dipping method, a spray method, etc. Furthermore, the substrate may be inclined at any angle during the developing.

[0452] It is preferable to further heat (post-bake) the patterned film obtained by development. The heating temperature is preferably 150°C or more and 250°C or less, more preferably 160°C or more and 235°C or less. The heating time is preferably 1 minute or more and 120 minutes or less, more preferably 10 minutes or more and 60 minutes or less. By heating after development, the polymerization of unreacted photopolymerizable compounds contained in the film can be promoted, so that a cured film with better chemical resistance can be obtained. Even when development is not performed, it is preferable to further heat (post-bake) the exposed composition layer.

[0453] On the other hand, examples of a method for forming a cured film (wavelength converting layer, overcoat layer, or light absorbing layer) on the entire surface of a substrate include a method in which a curable composition is applied to a substrate corresponding to each of the above-mentioned layers, and dried as necessary to form a composition layer, and the composition layer is heated and / or the entire surface of the composition layer is exposed to light.

[0454] The cured films formed from the curable compositions R2, R5, and R7 contain a cured reaction product of the polymerizable compound and the polymerization initiator contained in the curable compositions R2, R5, and R7. The cured reaction product is a substance containing a structure resulting from the structure of the polymerizable compound and the polymerization initiator. The structure resulting from the structure of the polymerizable compound and the polymerization initiator is, for example, a skeletal structure or a part thereof other than the curing reaction site of the polymerizable compound and the polymerization initiator.

[0455] The shapes and dimensions of the patterned wavelength conversion layer, overcoat layer and light absorbing layer are not particularly limited. The patterned wavelength conversion layer, overcoat layer and light absorbing layer may have, for example, a rectangular shape in plan view.

[0456] The wavelength conversion layer according to one embodiment is a layer that absorbs primary light from a primary light source and emits green light, and is preferably a layer that converts the wavelength of the primary light, that is, blue light, into the wavelength of green light. The green light emitted by the wavelength conversion layer preferably includes a peak having a maximum value in a wavelength range of 500 nm to 560 nm, more preferably includes a peak having a maximum value in a wavelength range of 520 nm to 555 nm, and even more preferably includes a peak having a maximum value in a wavelength range of 525 nm to 550 nm. The peak preferably has a full width at half maximum of 15 nm to 80 nm, more preferably 15 nm to 60 nm, even more preferably 15 nm to 50 nm, and particularly preferably 15 nm to 45 nm.

[0457] The wavelength conversion layer according to another embodiment is a layer that absorbs the primary light from the primary light source and emits red light, and is preferably a layer that converts the wavelength of the primary light, that is, blue light, into the wavelength of red light. The red light emitted by the wavelength conversion layer preferably includes a peak having a maximum value in the wavelength range of 610 nm to 750 nm, more preferably includes a peak having a maximum value in the wavelength range of 620 nm to 650 nm, and even more preferably includes a peak having a maximum value in the wavelength range of 625 nm to 645 nm. The peak preferably has a full width at half maximum of 15 nm to 80 nm, more preferably 15 nm to 60 nm, even more preferably 15 nm to 50 nm, and particularly preferably 15 nm to 45 nm.

[0458] The laminates and displays described below can include both a green-emitting wavelength conversion layer and a red-emitting wavelength conversion layer.

[0459] The wavelength conversion layer may be a layer that absorbs a part of the primary light and transmits the remaining part of the primary light. From the viewpoint of widening the color gamut and energy efficiency of the display device, the wavelength conversion layer has a light transmittance at a wavelength of 450 nm of preferably 90% or less, more preferably 85% or less, even more preferably 75% or less, even more preferably 60% or less, particularly preferably 40% or less, more particularly preferably 30% or less, and most preferably 20% or less. It is desirable that the amount of primary light that transmits through the wavelength conversion layer is small, but according to the present invention having a light absorbing layer, even if a part of the primary light transmits through the wavelength conversion layer, leakage of the primary light to the viewing side can be suppressed, and the provision of the light absorbing layer can suppress a decrease in luminous intensity. From this viewpoint, the wavelength conversion layer may have a light transmittance at a wavelength of 450 nm of 10% or more, further 15% or more, and even 20% or more.

[0460] The luminescence intensity maintenance rate of the laminate according to the present invention is preferably 60% or more, more preferably 65% ​​or more, and even more preferably 69% or more. The upper limit is not particularly limited, and 100% is ideal, but 95% or less, even 90% or less is acceptable. The luminescence intensity maintenance rate, which was reduced in the two-layer structure of the wavelength conversion layer and the light absorbing layer, is greatly improved by configuring the laminate to further include an overcoat layer between the wavelength conversion layer and the light absorbing layer. The luminescence intensity maintenance rate can be measured according to the measurement method described in the Examples section below.

[0461] The blue intensity cut rate of the laminate according to the present invention is preferably 40% or more, more preferably 60% or more, even more preferably 80% or more, and even more preferably 90% or more. The upper limit is not particularly limited, and 100% is ideal, but 99.5% or less, or even 90% or less is acceptable. By laminating the light absorbing layer, the blue intensity cut rate can be significantly improved. The blue intensity cut rate can be measured according to the measurement method described in the Examples section below.

[0462] <Display device> A display device according to the present invention includes a primary light source and the laminate according to the present invention. The display device is a device that irradiates a wavelength conversion layer with primary light from the primary light source to cause the wavelength conversion layer to emit light, and extracts the emitted light via a light absorbing layer.

[0463] FIG. 3 is a schematic cross-sectional view showing an example of a display device according to the present invention. The display device shown in FIG. 3 includes the laminate shown in FIG. 2, and includes a blue light source 40, which is a primary light source having a first region, a second region, and a third region that are different from each other. On the first region of the blue light source 40, a first wavelength conversion layer 11 that emits red light, a first overcoat layer 31 disposed thereon, and a first light absorption layer 21 disposed thereon are provided. On the second region of the blue light source 40, a second wavelength conversion layer 12 that emits green light, a second overcoat layer 32 disposed thereon, and a second light absorption layer 22 disposed thereon are provided. The display device has a red light emission region (i.e., the first region), a green light emission region (i.e., the second region), and a blue light emission region (i.e., the third region). Thus, the display device has a blue light source, a wavelength conversion layer, an overcoat layer, and a light absorption layer in this order in the optical path of light from the blue light source 40.

[0464] The first wavelength conversion layer 11 and the second wavelength conversion layer 12 may be arranged directly on the blue light source 40, or may be arranged on a light guide plate arranged between the blue light source 40 and the first wavelength conversion layer 11 and the second wavelength conversion layer 12 in the optical path of light from the blue light source 40.

[0465] The display device may further include a transparent layer or a layer containing a light diffusing agent that is disposed on the third region of the blue light source 40 and transmits blue light, and a third light absorbing layer that is disposed on the transparent layer and transmits blue light and absorbs light other than blue light.

[0466] Known light sources such as light emitting diodes (LEDs) such as blue light emitting diodes, lasers, EL, etc. can be used as the blue light source 40. From the viewpoints of color gamut and energy efficiency, the blue light source 40 is a light source that emits light having a peak preferably at 495 nm or less, and more preferably a light source that emits light having a peak at 425 nm or more and 495 nm or less.

[0467] The display device may further include, for example, a light guide plate, a diffusion film (diffusion layer), a light reflecting member (such as a reflective film), a brightness enhancing member, a prism sheet, a barrier layer, and the like.

[0468] As the light guide plate, any appropriate light guide plate can be used, for example, a light guide plate having a lens pattern formed on the back surface side so as to be able to deflect light from the lateral direction in the thickness direction, or a light guide plate having a prism shape or the like formed on the back surface side and / or the viewing side can be used.

[0469] The diffusion film is a film for diffusing the primary light or the light emitted from the wavelength conversion layer, and may be an amplifying diffusion film, etc. The light reflecting member is a member for reflecting the primary light toward the wavelength conversion layer, and may be, for example, a reflecting mirror, a film of reflecting particles, a reflecting metal film, or a reflector, etc. The brightness enhancing member is a member for reflecting a portion of the light back toward the direction from which the light was transmitted.

[0470] Typically, the prism sheet has a base portion and a prism portion. The base portion may be omitted depending on the adjacent member. The prism sheet can be attached to the adjacent member via any suitable adhesive layer (e.g., an adhesive layer, a pressure-sensitive adhesive layer). The prism sheet is configured by arranging a plurality of unit prisms that are convex on the opposite side (back side) from the viewing side in parallel. By arranging the convex portion of the prism sheet facing the back side, the light that passes through the prism sheet is easily concentrated. Furthermore, by arranging the convex portion of the prism sheet facing the back side, less light is reflected without entering the prism sheet compared to the case where the convex portion is arranged facing the viewing side, and a display device with high luminous intensity can be obtained.

[0471] The barrier layer is a layer for protecting the wavelength conversion layer from water vapor in the outside air and oxygen in the atmosphere.

[0472] The display device may include a layer of one or more media materials in the optical path between adjacent elements (layers), which may include any suitable material, including, but not limited to, vacuum, air, gas, optical material, adhesive, optical adhesive, glass, polymer, solid, liquid, gel, curable material, optical bonding material, index matching or index mismatching material, index gradient material, cladding or anti-cladding material, spacer, silica gel, brightness enhancing material, scattering or diffusing material, reflective or anti-reflective material, wavelength selective material, wavelength selective anti-reflective material, or other suitable media known in the art.

[0473] Specific examples of the display device include those equipped with a wavelength conversion material for an EL display or a liquid crystal display. The display device is not limited to the example shown in FIG. 3, and may be, for example, A display device in which a wavelength conversion layer is disposed between a blue light source and a light guide plate along the end face (side face) of the light guide plate to form a backlight that emits white light (on-edge type backlight), and a light absorbing layer is disposed on the light guide plate side; A display device in which a wavelength conversion layer is placed on a light guide plate, and a backlight (surface mount type backlight) is formed in which light irradiated from a blue light source placed on an end face (side face) of the light guide plate to the wavelength conversion layer through the light guide plate is emitted as white light, and an overcoat layer and a light absorbing layer are placed on the wavelength conversion layer; A display device in which a wavelength conversion layer is disposed near a light emitting portion of a blue light source, and a backlight (on-chip type backlight) is formed that emits irradiated light as white light, and an overcoat layer and a light absorbing layer are disposed on the wavelength conversion layer; etc. EXAMPLES

[0474] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0475] <Measurement> (1) Thickness measurement of the wavelength conversion layer, overcoat layer, and light absorbing layer The thickness was measured using a film thickness measuring device (DEKTAKXT; manufactured by Bruker).

[0476] (2) Measurement of luminescence intensity maintenance rate A light diffusion plate was placed on a backlight using a blue LED lamp with a peak emission wavelength of 450 nm as a point light source to form a backlight unit. The backlight unit was placed with the light diffusion plate facing upward, and a spectroradiometer (Topcon Corporation's "SR-UL1R") was installed at a height of 60 cm from the surface of the light diffusion plate. A laminate of a wavelength conversion layer, an overcoat layer, and a light absorbing layer formed on a glass substrate (a wavelength conversion layer formed on a glass substrate in Comparative Example 1, and a laminate of a wavelength conversion layer and a light absorbing layer formed on a glass substrate in Comparative Example 2) was used as a measurement sample, and the measurement sample was placed on the surface of the light diffusion plate with the laminate facing upward. In this state, the backlight was turned on, and the spectral radiance spectrum of the light emitted from the laminate was measured using the spectroradiometer, and the emission intensity EI (μW) at the maximum peak wavelength of the green emission peak was calculated from this spectrum. The maximum peak wavelength of the above-mentioned green emission peak was 530 nm, which is the maximum peak wavelength of the green emission peak in the emission spectrum of the semiconductor particles (A) contained in the wavelength conversion layer, and the full width at half maximum of the green emission peak was 42 nm. The emission spectrum of the semiconductor particles (A) was measured using an absolute PL quantum yield measurement device (Hamamatsu Photonics "C9920-02", excitation light 450 nm, room temperature, under atmospheric air) by using a semiconductor particle (A) dispersion solution diluted to an absorbance of 0.4 at a wavelength of 450 nm as a measurement sample. Emission intensity EI of the measured sample a The emission intensity of Comparative Example 1 was measured as EI b The maintenance rate of the luminous intensity EI before and after lamination of the overcoat layer was calculated according to the following formula. The results are shown in Table 6. Luminescence intensity EI maintenance rate (%) = [EI a / EI b ] x 100

[0477] (3) Blue intensity cut rate The spectral radiance spectrum was measured in the same manner as in "(2) Measurement of luminous intensity maintenance rate", and the luminous intensity EI' (μW) at a wavelength of 450 nm was calculated from this spectrum. Emission intensity EI' of the measured sample a The emission intensity of Comparative Example 1 was measured as EI' b The blue intensity cut rate was calculated according to the following formula. The results are shown in Table 6. Blue intensity cut rate (%) = [1-EI' a / EI' b ] x 100

[0478] (4) Condition of the overcoat layer The thickness of the laminate (a cured film consisting of a wavelength conversion layer, an overcoat layer, and a light absorbing layer) was measured at four arbitrary points using a thickness measuring device (DEKTAKXT; manufactured by Bruker). The maximum thickness Tmax, minimum thickness Tmin, and average thickness Tave of the four measured points were calculated, and the thickness unevenness was calculated according to the following formula, and the state of the overcoat layer was evaluated based on the following criteria. Film thickness unevenness (%) = (Tmax-Tmin) / Tave x 100 ◎ Film thickness unevenness is within 5% ○ Film thickness unevenness is more than 5% and less than 10% △ Film thickness unevenness exceeds 10%

[0479] (5) Film-forming ability of the light-absorbing layer The light absorbing layer was visually observed, and the film formability of the light absorbing layer was evaluated based on the following criteria. A light absorbing layer is formed on almost the entire surface of the overcoat layer. × There is a portion on the overcoat layer where the light absorbing layer is not formed (when the laminate is viewed from the light absorbing layer side, the area of ​​the overcoat layer occupies 10% or more of the observation area).

[0480] (6) Measurement of refractive index The laminate of the wavelength conversion layer, the overcoat layer, and the light absorbing layer was measured with a spectroscopic ellipsometer to determine the refractive index of each layer at a wavelength of 550 nm. The ellipsometer settings were as follows: Equipment: JA Woollam M-2000 Measurement wavelength: 400~1690nm Exposure time: 5 seconds Incident angle: 50, 60, 70 degrees

[0481] (7) Measurement of weight average molecular weight (Mw) of resin The polystyrene-equivalent weight average molecular weight (Mw) of the resin (C) was measured by GPC under the following conditions.

[0482] Equipment: HLC-8120GPC (Tosoh Corporation) Column: TSK-GELG2000HXL Column temperature: 40℃ Solvent: Tetrahydrofuran Flow rate: 1.0mL / min Solid concentration of the analytical sample: 0.001 to 0.01% by mass Injection volume: 50μL Detector: RI Calibration standard materials: TSK STANDARD POLYSTYRENE F-40, F-4, F-288, A-2500, A-500 (manufactured by Tosoh Corporation)

[0483] <Synthesis Example 1: Synthesis of Resin (C1)> A suitable amount of nitrogen was flowed into a flask equipped with a reflux condenser, a dropping funnel and a stirrer to replace the atmosphere with nitrogen, 80 parts of propylene glycol monomethyl ether acetate (PGMEA) was added, and the mixture was heated to 85°C while stirring. Next, a mixed solution prepared by dissolving 6 parts of methacrylic acid, 25 parts of dicyclopentanyl methacrylate, 40 parts of methyl methacrylate, and 29 parts of 1-[2-(methacryloyloxy)ethyl] succinate in 20 parts of PGMEA was dropped into the flask over 4 hours. Meanwhile, a solution prepared by dissolving 9 parts of polymerization initiator 2,2-azobis(2,4-dimethylvaleronitrile) in 40 parts of PGMEA was dropped over 5 hours. After the dropwise addition of the initiator solution, the mixture was kept at 85°C for 4 hours and then cooled to room temperature to obtain a copolymer (resin (C1)) solution. The solid content of the resin (C1) solution was 40%, and the weight average molecular weight Mw was 11,500.

[0484] <Synthesis Example 2: Synthesis of Resin (C2)> A suitable amount of nitrogen was poured into a flask equipped with a reflux condenser, a dropping funnel, and a stirrer to replace the atmosphere with nitrogen, 371 parts of PGMEA was added, and the mixture was heated to 85°C with stirring. Next, 54 parts of acrylic acid, 3,4-epoxytricyclo[5.2.1.0 2,6 ]decan-8-yl acrylate and 3,4-epoxytricyclo[5.2.1.0 2,6 ] A mixture of 225 parts of decan-9-yl acrylate (content ratio 50:50 by molar ratio) and 81 parts of vinyltoluene (mixture of isomers) was dissolved in 80 parts of PGMEA to prepare a mixed solution, which was dropped into the flask over 4 hours. Meanwhile, a solution of 30 parts of polymerization initiator 2,2-azobis(2,4-dimethylvaleronitrile) dissolved in 160 parts of PGMEA was dropped over 5 hours. After the dropwise addition of the initiator solution was completed, the mixture was kept at 85°C for 4 hours and then cooled to room temperature to obtain a copolymer (resin (C2)) solution. The solid content of the resin (C2) solution was 37%, and the weight average molecular weight Mw was 10600.

[0485] <Preparation Example 1: Preparation of semiconductor particle (A1) dispersion> A toluene dispersion a of semiconductor particles (A1) [green-emitting InP / ZnSeS quantum dots] containing oleic acid as an organic ligand (G1) was prepared. As described above, the maximum peak wavelength of the green emission peak of the quantum dots was 530 nm, and the full width at half maximum of the green emission peak was 42 nm.

[0486] After removing toluene from the toluene dispersion a by vacuum distillation, 70 parts of cyclohexyl acetate (J3) was added to 30 parts of the total amount of the semiconductor particles (A1) and the organic ligand (G1) to obtain a semiconductor particle (A1) dispersion b. The composition of the semiconductor particle (A1) dispersion b is shown in Table 1.

[0487] [Table 1]

[0488] The composition ratio of the semiconductor particles (A1) and the organic ligand (G1) was determined by measuring the amount of the organic ligand (G1) remaining when the mixture after removing the toluene was heated to 550°C at a heating rate of 5°C / min by TG-DTA measurement, and calculating the weight of the organic ligand (G1).

[0489] <Preparation Example 2: Preparation of wavelength-converting layer-forming composition (I)> The semiconductor particle (A1) dispersion b and each component were mixed to prepare a wavelength conversion layer forming composition (I) having the composition shown in Table 2. In Table 2, the parts of the components other than the solvent (J) are shown as solid content equivalents.

[0490] [Table 2]

[0491] Details of the abbreviations of the components shown in Table 2 are as follows.

[0492] Light scattering agent (B1): 60 parts of titanium oxide particles are mixed with 10 parts of resin C1 (solid content equivalent) and 30 parts of PGMEA, and the titanium oxide particles are thoroughly dispersed using a bead mill. The number of parts of light scattering agent (B1) listed in Table 2 is the number of parts of titanium oxide particles. Polymerizable compound (D1): Carboxy group-containing polyfunctional (meth)acrylate (product name "Aronix (registered trademark) M-510" manufactured by Toagosei Co., Ltd.) Polymerization initiator (E1): "Irgacure (registered trademark) OXE-02" manufactured by BASF Antioxidant (F1): Trade name "Sumilizer (registered trademark) GP" manufactured by Sumitomo Chemical Co., Ltd. Leveling agent (H1): Polyether modified silicone oil (product name "Toray Silicone SH8400" manufactured by Toray Dow Corning Co., Ltd.) Solvent (J1): Propylene glycol monomethyl ether acetate Solvent (J3): Cyclohexyl acetate

[0493] <Preparation Example 3: Preparation of overcoat layer-forming composition (III)> The components were mixed to prepare a composition (III) for forming an overcoat layer having the composition shown in Table 3. In Table 3, the parts of the components other than the solvent (J) are shown as solid content equivalents.

[0494] [Table 3]

[0495] <Preparation Example 4: Preparation of pigment dispersion (Ph)> The components in Table 4 were mixed, and the pigment, which is the colorant (I), was thoroughly dispersed using a bead mill to prepare a pigment dispersion (Ph-1).

[0496] [Table 4]

[0497] Details of the abbreviations of the components shown in Table 4 are as follows:

[0498] Pigment (P1): CI Pigment Yellow 138 Pigment dispersant: Solvent-based pigment dispersant Resin (C3): Methacrylic acid / benzyl methacrylate copolymer (copolymerization ratio (mass ratio): 30 / 70, Mw: 1.2 × 10 4 Solvent (J1): Propylene glycol monomethyl ether acetate Solvent (J2): Propylene glycol monomethyl ether (PGME)

[0499] <Preparation Example 5: Preparation of light-absorbing layer-forming composition (II)> A light-absorbing layer-forming composition (II) was obtained by mixing the components in Table 5. In Table 5, the parts of the resin are shown as solid content values.

[0500] [Table 5]

[0501] Details of the abbreviations of the components shown in Table 5 are as follows:

[0502] Polymerizable compound (D2): Dipentaerythritol hexaacrylate (trade name "KAYARAD (registered trademark) DPHA" manufactured by Nippon Kayaku Co., Ltd.) Polymerization initiator (E2): N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine (trade name "Irgacure (registered trademark) OXE-01" manufactured by BASF) Leveling agent (H1): Polyether modified silicone oil (product name "Toray Silicone SH8400" manufactured by Toray Dow Corning Co., Ltd.) Solvent (J1): Propylene glycol monomethyl ether acetate

[0503] <Example 1> The wavelength conversion layer-forming composition (I) was applied by spin coating onto a 5 cm square glass substrate ("Eagle XG" manufactured by Corning Incorporated) so that the thickness of the layer after post-baking would be 7 μm, and then pre-baked at 100° C. for 3 minutes to form a composition layer. The substrate on which this composition layer was formed was exposed to light at 80 mJ / cm 2 in the air using an exposure machine ("TME-150RSK" manufactured by Topcon Corporation). 2 After development, the resultant was post-baked at 180° C. for 30 minutes to form a wavelength conversion layer. The weight of the formed wavelength conversion layer was calculated from the difference in weight before and after the formation of the wavelength conversion layer, and was 0.043 g.

[0504] Next, the composition for forming an overcoat layer (III) was applied onto the wavelength conversion layer by spin coating so that the thickness of the layer after post-baking would be 0.3 μm, and then pre-baked at 100° C. for 3 minutes to form a composition layer. The substrate having the composition layer formed on the wavelength conversion layer was exposed to light at 100 mJ / cm 2 in the air using an exposure machine (Topcon Corporation's "TME-150RSK"). 2 After development, the resist was post-baked at 180° C. for 30 minutes to form a laminate of the wavelength conversion layer and the overcoat layer.

[0505] Next, the light absorbing layer forming composition (II) was applied onto this overcoat layer by spin coating so that the thickness of the layer after post-baking would be 1.5 μm, and then pre-baked at 100° C. for 3 minutes to form a composition layer. The substrate on which the composition layer was formed on the overcoat layer was exposed to light at 100 mJ / cm 2 in the air using an exposure machine (Topcon Corporation's "TME-150RSK"). 2 After development, the laminate was post-baked at 180° C. for 30 minutes to form a laminate of the wavelength conversion layer, the overcoat layer, and the light absorbing layer. The weight of the light absorbing layer formed was 0.004 g, as determined from the difference in weight before and after the formation of the light absorbing layer. The refractive indices of the wavelength conversion layer, the overcoat layer and the light absorbing layer were measured, and the wavelength conversion layer was 1.70, the overcoat layer was 1.53 and the light absorbing layer was 1.62. In addition, when calculating the value shown in Equation 1, Q 10 (wavelength conversion layer) and Q 20 (Light absorbing layer) was determined from the weight of each layer and the colorant concentration in each layer as follows. The content of the semiconductor particles (A1) and the organic ligand (G1) was 35.0 mass% based on the total solid content of the composition for forming a wavelength conversion layer (I). The content of the pigment (P1) was 26.4 mass% based on the total solid content of the composition for forming a light absorbing layer (II). Q 10 = Weight of wavelength conversion layer × (35.0 / 100) Q 20 =Weight of light absorbing layer × (26.4 / 100)

[0506] <Examples 2 to 8, Comparative Example 3> A laminate was formed in the same manner as in Example 1, except that the thickness of each layer was changed as shown in Table 6. The weight of each layer of the light absorbing layer of Example 7 and the wavelength converting layer of Example 8, which had a different thickness from that of Example 1, was determined in the same manner as in Example 1. The weight of the light absorbing layer of Example 7 was 0.001 g, and the weight of the wavelength converting layer of Example 8 was 0.01 g.

[0507] <Comparative Example 1> The wavelength conversion layer-forming composition (I) was applied by spin coating onto a 5 cm square glass substrate ("Eagle XG" manufactured by Corning Incorporated) so that the thickness of the layer after post-baking would be 7 μm, and then pre-baked at 100° C. for 3 minutes to form a composition layer. The substrate on which this composition layer was formed was exposed to light at 80 mJ / cm 2 in the air using an exposure machine ("TME-150RSK" manufactured by Topcon Corporation). 2 After development, the resist was post-baked at 180° C. for 30 minutes to form a wavelength conversion layer.

[0508] <Comparative Example 2> On the wavelength conversion layer obtained in Comparative Example 1, the composition for forming a light absorbing layer (II) was applied by spin coating so that the thickness of the layer after post-baking would be 1.5 μm, and then pre-baked at 100° C. for 3 minutes to form a composition layer. The substrate having the composition layer formed on the wavelength conversion layer was exposed to light at 100 mJ / cm 2 in the air using an exposure machine (Topcon Corporation's "TME-150RSK"). 2 After development, the resist was post-baked at 180° C. for 30 minutes to form a laminate of the wavelength conversion layer and the light absorbing layer.

[0509] [Table 6] [Explanation of symbols]

[0510] 10 Wavelength conversion layer 11 First wavelength conversion layer 12 Second Wavelength Conversion Layer 20 Light absorbing layer 21 First light absorbing layer 22 Second light absorbing layer 30 Overcoat layer 31 First overcoat layer 32 Second overcoat layer 40 blue light source

Claims

1. A wavelength conversion layer containing luminescent inorganic semiconductor particles and a light absorbing layer, an overcoat layer is provided between the wavelength conversion layer and the light absorbing layer; The overcoat layer has a thickness of 15 μm or less.

2. 2. The laminate according to claim 1, wherein a thickness ratio calculated by (thickness of the overcoat layer+thickness of the light absorbing layer) / thickness of the wavelength converting layer is 0.100 or more and 5 or less.

3. 2. The laminate according to claim 1, wherein a ratio of a thickness of the light absorbing layer to a thickness of the laminate (light absorbing layer / laminate) is 0.030 or more and 0.300 or less.

4. The laminate according to claim 1, which satisfies the following i) and ii): i) the refractive index of the overcoat layer is smaller than the refractive index of the wavelength conversion layer; ii) the refractive index of the overcoat layer is smaller than the refractive index of the light absorbing layer;

5. The laminate according to claim 1 , wherein the wavelength conversion layer, the light absorbing layer and the overcoat layer have a value represented by Formula 1 of 0.30 or less. {Q 20 / (T 20 +T 30 ) ) ) / {Q 10 / T 10} ...(Formula 1) [In formula 1, Q 10 : total amount of luminescent inorganic semiconductor particles and organic ligands in the wavelength conversion layer (g) Q 20 : total amount of colorant in light absorbing layer (g) T 10 : Thickness of wavelength conversion layer (μm) T 20 : Thickness of light absorbing layer (μm) T 30 : Thickness of overcoat layer (μm)]

6. A display device comprising the laminate according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Curable resin composition, cured film, wavelength conversion film, light-emitting element, and method for forming light-emitting layer

    JP2016065178A