Water dispersion of polyurethane resin, and coating agent

JP2024132418AActive Publication Date: 2024-10-01DKS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023043168
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
2043-03-17

AI Technical Summary

Benefits of technology

【0008】 本発明の実施形態によれば、自己修復性及び耐溶剤性に優れ、かつタックを抑制することができ、更に防汚性にも優れるポリウレタン樹脂の水分散体を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132418000001
    Figure 2024132418000001
  • Figure 2024132418000002
    Figure 2024132418000002
  • Figure 2024132418000003
    Figure 2024132418000003
Patent Text Reader

Abstract

To provide a water dispersion of a polyurethane resin which improves self-repair property and solvent resistance, and can suppress tackiness.SOLUTION: A water dispersion of a polyurethane resin has a part derived from an isocyanate group-containing urethane prepolymer (A), and a part derived from a chain extender (B). The isocyanate group-containing urethane prepolymer (A) contains (A1) polycarbonate diol which contains a component of diol having 5 carbon atoms, and a component of diol having 6 carbon atoms, and has a number average molecular weight of 300 to 2,500, (A2) polyethylene glycol having a number average molecular weight of 500 to 2,500, (A3) carboxy group-containing polyol, and (A4) alicyclic polyisocyanate, as components. The amount of the polyethylene glycol with respect to 100 pts.mass of the polycarbonate diol is 5 to 30 pts.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to an aqueous dispersion of a polyurethane resin and a coating agent containing the same. [Background technology]

[0002] 2. Description of the Related Art Aqueous dispersions of polyurethane resins are widely used as raw materials for various coating agents for the interior and exterior coating of aircraft, automobiles, etc., and for the exterior walls and flooring of houses.

[0003] For example, Patent Document 1 discloses an aqueous dispersion of polyurethane resin obtained by reacting a urethane prepolymer with a chain extender, in which the weight average molecular weight of the urethane prepolymer is 2000 to 30000, the degree of crosslinking of the polyurethane resin is 0.03 to 0.15 mol / kg, and the amount of urea in the polyurethane resin is 0.5 mol / kg or less. Specifically, Patent Document 1 discloses an aqueous dispersion of polyurethane resin obtained by reacting the urethane prepolymer with an amine chain extender using polycarbonate diol, carboxyl group-containing polyol, and alicyclic polyisocyanate as components of the urethane prepolymer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 195964 Summary of the Invention [Problem to be solved by the invention]

[0005] According to the above-mentioned Patent Document 1, an aqueous dispersion of a polyurethane resin is obtained that can form a coating film having good self-repairing properties, suppressed tackiness, and good solvent resistance. However, market demands for these properties are increasing, and further improvements are required.

[0006] An object of an embodiment of the present invention is to provide an aqueous dispersion of a polyurethane resin that can improve self-repairability and solvent resistance and suppress tackiness. [Means for solving the problem]

[0007] The present invention includes the embodiments set forth below. [1] An aqueous dispersion of a polyurethane resin having a portion derived from an isocyanate group-containing urethane prepolymer (A) and a portion derived from a chain extender (B), wherein the isocyanate group-containing urethane prepolymer (A) comprises, as constituent components, (A1) a polycarbonate diol having a number average molecular weight of 300 to 2500, which contains a component derived from a diol having 5 carbon atoms and a component derived from a diol having 6 carbon atoms, (A2) a polyethylene glycol having a number average molecular weight of 500 to 2500, (A3) a carboxy group-containing polyol, and (A4) an alicyclic polyisocyanate, and the amount of the polyethylene glycol per 100 parts by mass of the polycarbonate diol is 5 to 30 parts by mass. [2] The aqueous dispersion of the polyurethane resin according to [1], wherein the isocyanate group-containing urethane prepolymer (A) is a urethane prepolymer having a terminal isocyanate group obtained by reacting an isocyanate group with a hydroxyl group at an equivalent ratio NCO / OH of 1.02 to 1.50. [3] An aqueous dispersion of the polyurethane resin according to [1] or [2], which has an acid value of 15 to 40 mgKOH / g. [4] The aqueous dispersion of the polyurethane resin according to any one of [1] to [3], wherein the chain extender (B) contains a triamine. [5] The aqueous dispersion of the polyurethane resin according to any one of [1] to [4], wherein the alicyclic polyisocyanate contains hydrogenated diphenylmethane diisocyanate. [6] A coating agent comprising an aqueous dispersion of the polyurethane resin according to any one of [1] to [5]. Effect of the Invention

[0008] According to an embodiment of the present invention, it is possible to provide an aqueous dispersion of a polyurethane resin which is excellent in self-repairing property and solvent resistance, can suppress tackiness, and further has excellent stain resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The aqueous dispersion of the polyurethane resin according to this embodiment (hereinafter sometimes simply referred to as aqueous dispersion) is a dispersion in water of the polyurethane resin obtained by reacting the isocyanate group-containing urethane prepolymer (A) with the chain extender (B). Therefore, the polyurethane resin has a portion derived from the isocyanate group-containing urethane prepolymer (A) and a portion derived from the chain extender (B).

[0010] [Isocyanate group-containing urethane prepolymer (A)] The isocyanate group-containing urethane prepolymer (A) is obtained by reacting a polyol component with a polyisocyanate component, and in this embodiment, the components include (A1) polycarbonate diol, (A2) polyethylene glycol, (A3) carboxy group-containing polyol, and (A4) alicyclic polyisocyanate. Thus, the polyol component includes (A1) polycarbonate diol, (A2) polyethylene glycol, and (A3) carboxy group-containing polyol, and the polyisocyanate component includes (A4) alicyclic polyisocyanate.

[0011] [(A1) Polycarbonate diol] The polycarbonate diol is a polyol having a repeating unit containing a carbonate group (-O-(C=O)-O-) in the molecule and having hydroxyl groups at both ends. In this embodiment, the polycarbonate diol used contains a component derived from a diol having 5 carbon atoms and a component derived from a diol having 6 carbon atoms.

[0012] The polycarbonate diol is, for example, one obtained by reacting a carbonate ester and / or phosgene with a diol, and a copolymer in which a diol having 5 carbon atoms and a diol having 6 carbon atoms are used in combination as the diol.

[0013] The diol having 5 carbon atoms is preferably an alkanediol having 5 carbon atoms, which may be linear or branched. Specific examples include 1,5-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 1,2-pentanediol, and 2-methyl-1,4-butanediol, and any one of these may be used alone or in combination of two or more. 1,5-pentanediol is preferred.

[0014] The diol having 6 carbon atoms is preferably an alkanediol having 6 carbon atoms, which may be linear or branched. Specific examples include 1,6-hexanediol, 1,5-hexanediol, 2,5-hexanediol, 2,4-hexanediol, 1,2-hexanediol, and 3-methyl-1,5-pentanediol, and any one of these may be used alone or in combination of two or more. 1,6-hexanediol is preferred.

[0015] Examples of the carbonate ester include dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, diphenyl carbonate, dinaphthyl carbonate, and phenyl naphthyl carbonate. These may be used alone or in combination of two or more.

[0016] The polycarbonate diol according to the embodiment may contain components other than the component derived from the diol having 5 carbon atoms and the component derived from the diol having 6 carbon atoms in its skeleton, as long as a person skilled in the art would recognize that it is generally a polycarbonate diol.

[0017] In one embodiment, the polycarbonate diol may be represented by the following general formula (1). [ka] In the formula, R 1 R represents a divalent hydrocarbon group having 5 carbon atoms (preferably an alkanediyl group, more preferably a pentamethylene group), and is a structural component derived from a diol having 5 carbon atoms. 2 R represents a divalent hydrocarbon group having 6 carbon atoms (preferably an alkanediyl group, more preferably a hexamethylene group), and is a structural component derived from a diol having 6 carbon atoms. 3 is R 1 or R 2 Each of m and n represents an integer of 1 or more. The arrangement of the monomers in the copolymer is not particularly limited.

[0018] As the polycarbonate diol, a diol obtained by reacting 1,6-hexanediol and 1,5-pentanediol with a carbonate ester and / or phosgene, that is, poly(hexamethylene carbonate / pentamethylene carbonate) diol, is preferably used.

[0019] The molar ratio of the component derived from a diol having 5 carbon atoms to the component derived from a diol having 6 carbon atoms (m / n in the above formula (1)) is not particularly limited and may be 75 / 25 to 25 / 75, or 65 / 35 to 35 / 65.

[0020] The number average molecular weight (Mn) of the polycarbonate diol is 300 to 2500, preferably 400 to 2200, more preferably 500 to 2000, and further preferably 700 to 1500, from the viewpoints of self-repairing property, suppression of tackiness, and solvent resistance.

[0021] In this specification, the number average molecular weight (Mn) is a value measured by GPC (gel permeation chromatography) and calculated using a calibration curve of standard polystyrene. In detail, the GPC conditions are as follows: column: "TSKgel G4000HXL+TSKgel G3000HXL+TSKgel G2000HXL+TSKgel G1000HXL+TSKgel G1000HXL" manufactured by Tosoh Corporation, mobile phase: THF (tetrahydrofuran), mobile phase flow rate: 1.0 mL / min, column temperature: 40°C, sample injection amount: 50 μL, sample concentration: 0.2 mass%.

[0022] [(A2) Polyethylene glycol] In this embodiment, polyethylene glycol is used as the polyol component together with the polycarbonate diol. By using polyethylene glycol, it is possible to improve the stain resistance and solvent resistance.

[0023] From the viewpoints of self-repairing property, suppression of tackiness, solvent resistance and stain resistance, the polyethylene glycol used has a number average molecular weight of 500 to 2500. The number average molecular weight of the polyethylene glycol is preferably 600 to 2300, more preferably 700 to 2000, and further preferably 800 to 1800.

[0024] [(A3) Carboxy group-containing polyol] In this embodiment, a carboxyl group-containing polyol is further used as the polyol component. By using the carboxyl group-containing polyol, it is possible to give the polyurethane resin an acid value.

[0025] The carboxyl group-containing polyol is a polyol having a carboxyl group in the molecule, and examples thereof include carboxylic acid-containing compounds such as dimethylolpropionic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolvaleric acid, dihydroxymaleic acid, 2,6-dihydroxybenzoic acid, and derivatives and salts thereof. Any of these may be used alone or in combination of two or more.

[0026] Here, the carboxyl group is a concept including not only the acid type (-COOH) but also the salt type, i.e., carboxylate group (-COOX, where X is a cation that forms a salt with a carboxylic acid), and the acid type and the salt type may be mixed. The carboxyl group can be neutralized to form a salt to make the finally obtained polyurethane resin water-dispersible. Therefore, in the aqueous dispersion of the polyurethane resin, the carboxyl group exists as a salt type. The type of salt type varies depending on the type of neutralizing agent described later, and may be an alkali metal salt such as a sodium salt, a tertiary amine salt such as a triethylamine salt, or an ammonium salt.

[0027] [(A4) Alicyclic polyisocyanate] In this embodiment, an alicyclic polyisocyanate is used as the polyisocyanate component. By using an alicyclic polyisocyanate, it is possible to provide the polyurethane resin with appropriate rigidity, and improve the self-repairing property while suppressing tack. In addition, it is possible to suppress yellowing of the polyurethane resin, which occurs when an aromatic polyisocyanate is used.

[0028] Examples of alicyclic polyisocyanates include hydrogenated diphenylmethane diisocyanate (hydrogenated MDI), hydrogenated xylylene diisocyanate, isophorone diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and modified and polynuclear products thereof. Examples of modified products include isocyanurate modified products, allophanate modified products, biuret modified products, adduct modified products, carbodiimide modified products, etc. These alicyclic polyisocyanates may be used alone or in combination of two or more.

[0029] Among these, hydrogenated MDI is preferred as the alicyclic polyisocyanate. Hydrogenated MDI is obtained by hydrogenating diphenylmethane diisocyanate (MDI), and examples of the hydrogenated MDI include dicyclohexylmethane 4,4'-diisocyanate.

[0030] [Polyol component] In the polyol component constituting the isocyanate group-containing urethane prepolymer (A), the amount of (A2) polyethylene glycol is 5 to 30 parts by mass relative to 100 parts by mass of (A1) polycarbonate diol. When the amount of (A2) polyethylene glycol is 5 parts by mass or more, it is possible to improve the antifouling property and the solvent resistance. Furthermore, when the amount of (A2) polyethylene glycol is 30 parts by mass or less, it is possible to suppress tackiness and improve the solvent resistance and the self-repairing property. The amount of (A2) polyethylene glycol relative to 100 parts by mass of (A1) polycarbonate diol is preferably 6 to 28 parts by mass, more preferably 8 to 25 parts by mass, and further preferably 10 to 20 parts by mass.

[0031] The amount of the (A1) polycarbonate diol in 100% by mass of the polyol component is not particularly limited, but is preferably from 65 to 95% by mass, more preferably from 70 to 93% by mass, and even more preferably from 75 to 90% by mass.

[0032] The amount of (A2) polyethylene glycol in 100% by mass of the polyol component is not particularly limited, but is preferably from 4.7 to 25% by mass, more preferably from 5 to 20% by mass, and even more preferably from 6 to 15% by mass.

[0033] The amount of the carboxy-containing polyol (A3) relative to 100% by mass of the polyol component is not particularly limited and may be, for example, 0.3 to 20% by mass, 2 to 15% by mass, or 4 to 10% by mass.

[0034] Here, the amount of each component constituting the polyol component is calculated based on 100% by mass of the polyol component, with the carboxy group of the carboxy group-containing polyol (A3) being in the acid form, and the amount of the carboxy group-containing polyol (A3) is also in the acid form.

[0035] The polyol component constituting the isocyanate group-containing urethane prepolymer (A) is basically composed of only the above-mentioned (A1) polycarbonate diol, (A2) polyethylene glycol, and (A3) carboxyl group-containing polyol, but may contain other polyols as long as the effects of this embodiment are achieved. The total amount of (A1) polycarbonate diol, (A2) polyethylene glycol, and (A3) carboxyl group-containing polyol in 100% by mass of the above polyol component is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.

[0036] Examples of other polyols include polyester polyols and polyether polyols other than polyethylene glycol. Other polyols include low molecular weight polyols such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, neopentyl glycol, glycerin, trimethylolpropane, ditrimethylolpropane, tritrimethylolpropane, pentaerythritol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, and bisphenol A.

[0037] [Polyisocyanate component] The polyisocyanate component constituting the isocyanate group-containing urethane prepolymer (A) is basically composed only of the above-mentioned (A4) alicyclic polyisocyanate, but may contain other polyisocyanates within the range in which the effects of the present embodiment are achieved. The amount of the (A4) alicyclic polyisocyanate in 100% by mass of the above-mentioned polyisocyanate component is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.

[0038] Examples of other polyisocyanates include aliphatic polyisocyanates such as tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate, and aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate, and xylylene diisocyanate.

[0039] [NCO / OH] The isocyanate group-containing urethane prepolymer (A) is preferably a urethane prepolymer having a terminal isocyanate group obtained by reacting an isocyanate group and a hydroxyl group at an equivalent ratio NCO / OH (index) of 1.02 to 1.50. NCO / OH is more preferably 1.05 to 1.35, even more preferably 1.08 to 1.25, and even more preferably 1.10 to 1.20.

[0040] Here, NCO / OH is the molar ratio of isocyanate groups contained in the polyisocyanate component to hydroxyl groups contained in the polyol component. NCO / OH is calculated using the hydroxyl value of the polyol component and the isocyanate value of the polyisocyanate component. The isocyanate value is calculated by the formula: Isocyanate value = {(isocyanate content) x 56110} / (42.02 x 100) using the isocyanate content measured in accordance with JIS K1603-1:2007, Method A.

[0041] [Chain extender (B)] Examples of the chain extender (B) include diamines, triamines, and tetramines. Examples of the diamines include ethylenediamine, trimethylenediamine, piperazine, and isophoronediamine. Examples of the triamines include diethylenetriamine and dipropylenetriamine. Examples of the tetramines include triethylenetetramine. These chain extenders may be used alone or in combination of two or more.

[0042] As the chain extender (B), it is preferable to use a triamine having three functional groups, and more preferably diethylenetriamine, because this has a superior effect of improving the self-repairing property.

[0043] The amount of the chain extender (B) is not particularly limited, and may be, for example, 0.1 to 3.0 parts by mass, 0.2 to 2.5 parts by mass, 0.3 to 2.0 parts by mass, 0.4 to 1.5 parts by mass, or 0.5 to 1.2 parts by mass relative to 100 parts by mass of the isocyanate group-containing urethane prepolymer (A).

[0044] [Water dispersion of polyurethane resin] The aqueous dispersion of the polyurethane resin is obtained by reacting an isocyanate group-containing urethane prepolymer (A) obtained by reacting a polyol component containing (A1) a polycarbonate diol, (A2) a polyethylene glycol, and (A3) a carboxy group-containing polyol with a polyisocyanate component containing (A4) an alicyclic polyisocyanate, with a chain extender (B).

[0045] The polyurethane resin preferably has an acid value of 15 to 40 mgKOH / g. When the acid value is 15 mgKOH / g or more, the effect of suppressing tackiness and solvent resistance tend to be improved. When the acid value is 40 mgKOH / g or less, the stain resistance and self-repairing property tend to be improved. The acid value of the polyurethane resin is more preferably 17 to 30 mgKOH / g, and further preferably 18 to 25 mgKOH / g. The acid value of the polyurethane resin can be adjusted, for example, by the type and amount of (A3) carboxyl group-containing polyol.

[0046] In this specification, the acid value can be determined in accordance with JIS K0070-1992 from the amount of KOH (mg) required to neutralize the free carboxy groups contained in 1 g of the solid content of the aqueous dispersion of the polyurethane resin (i.e., the polyurethane resin).

[0047] The number average molecular weight (Mn) of the polyurethane resin is not particularly limited, and may be, for example, 10,000 or more, or 50,000 or more. The average particle size of the aqueous dispersion of the polyurethane resin is not particularly limited, and may be, for example, 0.0005 to 0.5 μm. Here, the average particle size is the 50% cumulative particle size (d50) measured using "Microtrac UPA-UZ152" manufactured by Nikkiso Co., Ltd.

[0048] The method for producing the aqueous dispersion of the polyurethane resin is not particularly limited. For example, a method may be mentioned in which a polyol component and a polyisocyanate component are reacted to obtain an isocyanate group-containing urethane prepolymer (A), the urethane prepolymer (A) is neutralized with a neutralizing agent, emulsified and dispersed in water, and then the urethane prepolymer (A) is reacted with a chain extender (B).

[0049] In detail, the polyol component and the polyisocyanate component are reacted without a solvent or in an organic solvent not having an active hydrogen group to synthesize an isocyanate group-containing urethane prepolymer (A). At that time, NCO / OH is set as above. After synthesis of the isocyanate group-containing urethane prepolymer (A), the carboxyl group is neutralized with a neutralizing agent, and then emulsified and dispersed in water. Then, a chain extender (B) is added in an equivalent amount less than the remaining isocyanate group (for example, an equivalent ratio of the isocyanate group to the active hydrogen group of the chain extender (B) is 1:0.50 to 0.95), and the isocyanate group in the emulsion micelle and the chain extender (B) undergo an interfacial polymerization reaction to generate a urea bond. Then, the solvent used is removed as necessary to obtain an aqueous dispersion of the polyurethane resin.

[0050] Examples of the neutralizing agent include non-volatile bases such as sodium hydroxide and potassium hydroxide, tertiary amines such as trimethylamine, triethylamine, dimethylethanolamine, methyldiethanolamine and triethanolamine, and volatile bases such as ammonia. Neutralization can be carried out before, during, or after the urethanization reaction.

[0051] The organic solvent optionally used in the synthesis of the isocyanate group-containing urethane prepolymer (A) is an organic solvent that is inactive to the isocyanate group and can dissolve the resulting urethane prepolymer (A), such as dioxane, methyl ethyl ketone, acetone, dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, toluene, and propylene glycol monomethyl ether acetate.

[0052] The aqueous dispersion of polyurethane resin contains water and polyurethane resin dispersed in water, but may contain other components as long as the effects of the present embodiment are achieved, for example, may contain the above organic solvent together with water as a dispersion medium. The concentration of polyurethane resin in the aqueous dispersion is not particularly limited, and may be, for example, 10 to 50% by mass, or 20 to 45% by mass.

[0053] [Coating agent] The coating agent according to this embodiment contains the above-mentioned aqueous dispersion of polyurethane resin, and therefore contains water and polyurethane resin dispersed in water.

[0054] The coating agent may contain other aqueous resins together with the polyurethane resin, such as water-soluble or water-dispersible acrylic resins, water-soluble or water-dispersible polyester resins, water-soluble or water-dispersible alkyd resins, water-soluble or water-dispersible cellulose resins, and the like.

[0055] In addition, various additives that are generally used can be used in the coating agent as long as the effect of the present embodiment is achieved. Examples of such additives include weathering agents, antibacterial agents, antifungal agents, fillers, rust inhibitors, pigments, dyes, film-forming assistants, inorganic crosslinking agents, organic crosslinking agents (e.g., blocked isocyanate crosslinking agents, epoxy crosslinking agents, carbodiimide crosslinking agents, oxazoline crosslinking agents, melamine crosslinking agents), silane coupling agents, antiblocking agents, viscosity adjusters, leveling agents, defoamers, dispersion stabilizers, light stabilizers, antioxidants, ultraviolet absorbers, inorganic fillers, organic fillers, plasticizers, lubricants, antistatic agents, etc. EXAMPLES

[0056] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited thereto.

[0057] Details of each component used in the examples are as follows.

[0058] [(A1) Polycarbonate diol] Polycarbonate diol 1: Asahi Kasei Corporation's "DURANOL T5651" (number average molecular weight: 1000. 1,5-pentanediol and 1,6-hexanediol are used as diol components. Repeating units: pentamethylene carbonate / hexamethylene carbonate = 1 / 1 (molar ratio))

[0059] Polycarbonate diol 2: UBE Corporation's "ETERNACOLL PH-50" (number average molecular weight 500. 1,5-pentanediol and 1,6-hexanediol are used as diol components.)

[0060] Polycarbonate diol 3: Asahi Kasei Corporation's "DURANOL T5652" (number average molecular weight: 2000. 1,5-pentanediol and 1,6-hexanediol are used as diol components. Repeating units: pentamethylene carbonate / hexamethylene carbonate = 1 / 1 (molar ratio))

[0061] Polycarbonate diol C1: UBE Corporation's "ETERNACOLL UP-200" (number average molecular weight: 2000. Only 1,5-pentanediol is used as the diol component.)

[0062] Polycarbonate diol C2: UBE Corporation's "ETERNACOLL UH-200" (number average molecular weight: 2000. Only 1,6-hexanediol is used as the diol component.)

[0063] Polycarbonate diol C3: UBE Corporation's "ETERNACOLL PH-300" (number average molecular weight: 3000. 1,5-pentanediol and 1,6-hexanediol are used as diol components.)

[0064] [(A2) Polyethylene glycol] Polyethylene glycol 1: Sanyo Chemical Industries, Ltd. "PEG-1000" (number average molecular weight: 1000) Polyethylene glycol 2: Sanyo Chemical Industries, Ltd. "PEG-2000" (number average molecular weight: 2000) Polyethylene glycol C1: Sanyo Chemical Industries, Ltd. "PEG-3000" (number average molecular weight: 3000) Polyethylene glycol C2: Sanyo Chemical Industries, Ltd. "PEG-300" (number average molecular weight: 300)

[0065] [(A3) Carboxy group-containing polyol] Dimethylolpropionic acid: Perstorp's "Bis-MPA"

[0066] [Polyisocyanate component] Hydrogenated MDI: Dicyclohexylmethane 4,4'-diisocyanate ·MDI: 4,4'-diphenylmethane diisocyanate ·HDI: Hexamethylene diisocyanate

[0067] <Synthesis of aqueous dispersion of polyurethane resin> [Example 1] In a four-neck flask equipped with a stirrer, reflux condenser, thermometer and nitrogen blowing tube, 57.0 parts by mass of polycarbonate diol 1, 8.0 parts by mass of polyethylene glycol 1, 5.0 parts by mass of dimethylolpropionic acid (DMPA), and 100 parts by mass of methyl ethyl ketone were added and thoroughly stirred and dissolved, then 30.0 parts by mass of hydrogenated MDI were added, and the reaction was carried out at 75°C until the content of free isocyanate groups relative to the solid content reached 1.0% by mass, to obtain a methyl ethyl ketone solution of an isocyanate group-containing urethane prepolymer. This prepolymer solution was cooled to 45°C, neutralized by adding 3.8 parts by mass of triethylamine as a neutralizing agent, and then emulsified and dispersed by adding 300 parts by mass of distilled water while stirring using a homomixer. Next, 0.7 parts by mass of diethylenetriamine was added, and a chain extension reaction was carried out at 30°C for 30 minutes. This was heated under reduced pressure to distill off methyl ethyl ketone, to obtain an aqueous dispersion of polyurethane resin with a solid content of 25% by mass. The resulting polyurethane resin had an acid value of 21.0 mgKOH / g.

[0068] [Examples 2 to 13 and Comparative Examples 1 to 10] Aqueous dispersions of each polyurethane resin were obtained by the same synthesis as in Example 1, except that the type and amount of each raw material was changed as shown in Tables 1 and 2. In the table, the "blending ratio (A2) / (A1)" indicates the parts by mass of polyethylene glycol (A2) relative to 100 parts by mass of polycarbonate diol (A1).

[0069] <Evaluation of aqueous dispersion of polyurethane resin> [Creation of coating layer] A water dispersion of polyurethane resin was applied onto a polyethylene terephthalate substrate (PET manufactured by Toray Industries, Inc., model number: #100 T60) to a film thickness of approximately 20 μm, and then dried at 80° C. for 10 minutes to produce a coating layer.

[0070] [Anti-stain] Fingerprint resistance test The index finger was pressed against the coating surface for 3 seconds, and then the finger was gently removed to leave a fingerprint. The fingerprint was then wiped off by moving a nonwoven fabric ("Bencotto M-311" manufactured by Asahi Kasei Corporation) back and forth in one direction. The state after wiping was visually observed from a 45° angle above the coating film under a three-wavelength fluorescent lamp, and the number of times the finger was moved back and forth until the fingerprint was no longer visible was evaluated on the following three-point scale. ◯: Fingerprints were wiped off in less than 5 strokes. △: Fingerprints could be wiped off with 5 to less than 8 strokes. ×: Eight or more strokes were required to wipe off the fingerprint.

[0071] [Suppress tack] The coated surfaces were attached together under a load of 1 kg, and the condition of the coated surfaces when peeled off was visually observed to evaluate the effect of suppressing tack. If the coated surfaces did not adhere to each other, it was rated as "Excellent", if less than 50% of the attached area was adhered, it was rated as "△" (Good), and if 50% or more of the attached area was adhered, it was rated as "X" (Bad).

[0072] [Solvent resistance] The coating layer was rubbed 10 times with a toluene-soaked felt under a load of 1 kg, and the condition of the coating surface was visually observed. If the coating surface was unchanged, it was marked as "Good", if it was eroded, it was marked as "Good", and if the coating layer peeled off, it was marked as "Poor".

[0073] [Self-repairability] The coating surface was rubbed back and forth 15 times with a brass wire brush (No. 9, manufactured by Fujiwara Sangyo Co., Ltd.) loaded with a 500g load, and the degree of damage to the coating surface was visually observed. The evaluation was performed at room temperature of 23°C, and a mark was given for marks where the damage was restored in less than 1 minute, a mark was given for marks where the damage took 1 to 30 minutes to be restored, and a mark was given for marks where the damage was not restored after 30 minutes.

[0074] [Table 1]

[0075] [Table 2]

[0076] The results are shown in Tables 1 and 2. Comparative Example 1 is an example in which a polycarbonate diol whose diol component is composed only of a diol having 5 carbon atoms is used. Comparative Example 2 is an example in which a polycarbonate diol whose diol component is composed only of a diol having 6 carbon atoms is used. Comparative Example 3 is an example in which a polycarbonate diol whose diol component is a combination of a diol having 5 carbon atoms and a diol having 6 carbon atoms but whose Mn is larger than the specified value is used. In these comparative examples, one or more of the antifouling properties, tack suppression, solvent resistance, and self-repairing properties were poor.

[0077] Comparative Example 4 is an example in which a polyethylene glycol having a larger Mn than the standard was used, and the coating layer was too soft, resulting in poor tack suppression and self-repairing properties, and insufficient solvent resistance. Comparative Example 5 is an example in which a polyethylene glycol having a smaller Mn than the standard was used, and the coating layer was hard, resulting in poor self-repairing properties, and insufficient stain resistance.

[0078] Comparative Examples 6 and 7 were examples in which polyethylene glycol was not used or was used in a small amount, and were inferior in stain resistance and solvent resistance. Comparative Example 8 was an example in which the amount of polyethylene glycol was too high, and was inferior in tack suppression, solvent resistance, and self-repairing properties.

[0079] Comparative Example 9 is an example using an aromatic polyisocyanate, and the coating layer was too hard and had poor self-repairing properties and was also poor in antifouling properties. Comparative Example 10 is an example using an aliphatic polyisocyanate, and the coating layer was too soft and had poor tack suppression, and was also poor in antifouling properties, solvent resistance, and self-repairing properties.

[0080] In contrast, in Examples 1 to 13, the self-repairing property, tack suppression, and solvent resistance were excellent, and furthermore, the antifouling property was excellent. Comparing Example 1 with Example 6, the use of trifunctional diethylenetriamine as the chain extender was more excellent in tack suppression and self-repairing property than the use of bifunctional isophoronediamine.

[0081] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.

[0082] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. An aqueous dispersion of a polyurethane resin having a portion derived from an isocyanate group-containing urethane prepolymer (A) and a portion derived from a chain extender (B), The isocyanate group-containing urethane prepolymer (A) is (A1) a polycarbonate diol having a number average molecular weight of 300 to 2500, which contains a component derived from a diol having 5 carbon atoms and a component derived from a diol having 6 carbon atoms; (A2) polyethylene glycol having a number average molecular weight of 500 to 2500, (A3) a carboxy group-containing polyol, and (A4) Alicyclic polyisocyanate as a constituent component, and the amount of the polyethylene glycol is 5 to 30 parts by mass relative to 100 parts by mass of the polycarbonate diol. A water dispersion of polyurethane resin.

2. The aqueous dispersion of a polyurethane resin according to claim 1, wherein the isocyanate group-containing urethane prepolymer (A) is a urethane prepolymer having a terminal isocyanate group obtained by reacting an isocyanate group with a hydroxyl group at an equivalent ratio NCO / OH of 1.02 to 1.

50.

3. The aqueous dispersion of the polyurethane resin according to claim 1, having an acid value of 15 to 40 mgKOH / g.

4. The aqueous dispersion of a polyurethane resin according to claim 1 , wherein the chain extender (B) comprises a triamine.

5. The aqueous dispersion of a polyurethane resin according to claim 1 , wherein the alicyclic polyisocyanate comprises hydrogenated diphenylmethane diisocyanate.

6. A coating agent comprising the aqueous dispersion of the polyurethane resin according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Aqueous dispersion of carbonyl group-containing urethane urea resin

    JP2011157527A

  • Metal surface treatment agent

    JP2011231353A

  • Antistatic agent, antistatic laminate using the same, and method for manufacturing biaxially stretched antistatic film

    JP2014065869A

  • Aqueous gravure or flexographic ink, printed matter and laminate

    JP2020180271A

  • Aqueous ink for decorative material and decorative material using the same

    JP2021147428A