Photosensitive resin composition
The photosensitive resin composition addresses the limitations of high-temperature baking and substrate integrity by using a temperature-responsive polymer with an azide group, enabling patterning on plastics at lower temperatures and avoiding substrate dissolution.
Patent Information
- Application Number
- JP2023043186
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional cell culture methods using plastics face issues with low heat resistance and chemical resistance, and glass substrates used for temperature-responsive polymers require high-temperature baking, leading to alkali elution and reproducibility problems.
A photosensitive resin composition containing a temperature-responsive polymer without a carbon-carbon triple bond and an azide group, allowing for patterning at room temperature or below 50°C without high-temperature baking, using solvents that do not dissolve plastics.
Enables the production of temperature-responsive patterns on plastic substrates without high-temperature baking, ensuring the composition can be cured at lower temperatures and maintains the integrity of the plastic substrate.
Smart Images

Figure 2024132434000026 
Figure 2024132434000001 
Figure 2024132434000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition using a temperature-responsive polymer, and further to a film made of a cured or partially cured product formed from the composition, a laminate having the film, and a method for producing the laminate. [Background technology]
[0002] Poly(N-isopropylacrylamide) (PNIPAAm) is known as a temperature-responsive polymer. PNIPAAm can be easily obtained by polymerizing N-isopropylacrylamide (NIPAAm) with a radical initiator. Aqueous solutions of PNIPAAm undergo phase separation due to temperature changes, dissolving in water below 31°C, and becoming insoluble and precipitating at temperatures above that. NIPAAm is also known to copolymerize with other functional monomers, and copolymerization can produce polymers that respond to temperature changes. A technique is known for producing a chip having a dot pattern formed by photolithography using a photosensitive resin composition containing such a temperature-responsive polymer. The photolithography technique used for substrates and the like can produce a fine pattern structure. Such a fine pattern structure is useful for handling microscopic cells and the like.
[0003] The following are documents on the temperature-responsive polymer and documents on the use of the temperature-responsive polymer in cell culture, etc. Patent Document 1 describes, in an example, the production of a binary copolymer obtained by polymerizing monomers N-isopropylacrylamide and N-(2-hydroxyethyl)acrylamide, and a ternary copolymer obtained by further polymerizing a monomer having a C=C-CO-NRR' structure, and that various different temperature-responsive patterned substrates (particularly cell culture supports) are produced by patterning using a photolithography method from a photosensitive resin composition containing a temperature-responsive polymer. Patent Document 1 also describes that the substrate is baked after exposure (PEB) for 20 hours in an oven at 80°C, and in the example, a cell culture support is produced on a glass substrate. Patent Document 2 describes a ligand-attached substrate coated with a polymer containing a structural unit exhibiting cell non-adhesiveness and a structural unit exhibiting cell adhesiveness, and a coating material that exhibits excellent cell selective culture and separation capabilities without impairing cell selectivity due to non-specific adhesion of cells to the polymer or the substrate itself. In the examples of Patent Document 2, a synthesis example of a polymer having a zwitterion and a click reaction site is shown. Patent Document 2 also describes that the polymer coating on the surface of a glass substrate is heated on a hot plate heated to 100° C. for 1 minute. Non-Patent Document 1 describes the synthesis of a temperature-responsive hydrogel using photolithography, specifically, poly(N-isopropylacrylamide-acrylic acid) (PIA) and azidophenyl-derivatized PIA (AzPh-PIA) are synthesized, and an aqueous solution of this synthesis is eluted onto a glass plate, and a photomask is used to produce temperature-responsive microgels with several pattern structures. However, since the synthesis in Non-Patent Document 1 is an aqueous solution, a lot of heat is required to evaporate the water when producing a pattern on the glass plate. Furthermore, the aqueous solution in this document may not be uniformly applied. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 068271 [Patent Document 2] International Publication No. 2019 / 013148 [Non-patent literature]
[0005] [Non-Patent Document 1] macromolecules 1998,31,4397-4381 Summary of the Invention [Problem to be solved by the invention]
[0006] Conventionally, plastics such as polystyrene have been used for cell culture because they are inexpensive, lightweight, and have excellent impact resistance, but they also have problems such as low heat resistance and low chemical resistance. When applying a temperature-responsive polymer to cell culture, baking after exposure must be performed at high temperatures, so a glass substrate is used instead of a plastic substrate. However, when using a glass substrate for cell culture, the cured layer on the substrate becomes a thin film, so it is significantly affected by alkaline elution of the glass substrate, making it difficult to achieve reproducibility.
[0007] Therefore, it has been desired to use plastic substrates for cell culture, instead of glass ones. However, when using plastics, some cannot be used at high temperatures, and it is desirable to use them at room temperature or at most 50°C or less, and furthermore, it has been desired to use organic solvents that do not dissolve plastics. The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a photosensitive resin composition using a temperature-responsive polymer that can be used in the field of cell culture to produce a temperature-responsive pattern having a desired response temperature by a photolithography method. Another object of the present invention is to provide a photosensitive resin composition using a temperature-responsive polymer that does not require high-temperature baking after exposure so that a plastic substrate can be used, can be processed at room temperature or below 50°C, uses a solvent that does not dissolve plastics, and does not use an acid for processing, etc. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that if a photosensitive resin composition containing a temperature-responsive polymer having no carbon-carbon triple bond and a low molecular weight compound, etc., and a photosensitive resin composition having an azide group is used, a cured product can be prepared by exposure without the need for high-temperature baking, processing can be performed at 50° C. or less, and a temperature-responsive pattern having a desired response temperature can be produced by patterning using a photolithography method, thereby completing the invention. Furthermore, they have found that an organic solvent that does not dissolve plastics can be used as a solvent for the photosensitive resin composition.
[0009] That is, the present invention relates to the following. According to a first aspect, there is provided a photosensitive resin composition comprising a temperature-responsive polymer (A) having no carbon-carbon triple bond, and a solvent (B), and optionally comprising a low molecular weight compound (C) having an azide group, The photosensitive resin composition relates to a photosensitive resin composition in which, when the low molecular weight compound (C) is not contained, the temperature-responsive polymer (A) has an azide group, and, when the low molecular weight compound (C) is contained, the temperature-responsive polymer (A) may have an azide group. As a second aspect, the present invention relates to the photosensitive resin composition according to the first aspect, in which the temperature-responsive polymer (A) is a polymer having a structural unit represented by the following formula (1): [ka] (In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an optionally substituted alkyl group having 1 to 10 carbon atoms. As a third perspective, The photosensitive resin composition according to a first aspect, wherein the temperature responsive polymer (A) is a polymer having a structural unit represented by the following formula (2): [ka] (In formula (2), R 3 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R4 represents an optionally substituted alkyl group having 1 to 10 carbon atoms, R 5 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 6 represents a group containing an azide group, x and y are each any number satisfying x + y ≤ 1, 0 < x < 1, and 0 < y < 1.) As a fourth aspect, R in the formula (2) 6 In addition to the azide group, it may contain one or more selected from the group consisting of a carbonyl group, a hydroxy group, an ether group, an arylene group, an alkylene group having 1 to 10 carbon atoms, a hydrocarbon ring group having 3 to 10 carbon atoms, a 3- to 10-membered heterocyclic group, and a 3- to 10-membered hetero-condensed ring group, and relates to the photosensitive resin composition according to the third aspect. As a fifth aspect, in the formula (2), it relates to the photosensitive resin composition according to the third aspect, which satisfies 0.01 ≤ y / x ≤ 0.2. As a sixth aspect, the solvent (B) is selected from an optionally substituted alcohol having 2 to 10 carbon atoms or an ester which is a reaction product of the alcohol and a carboxylic acid, and relates to the photosensitive resin composition according to the first aspect. As a seventh aspect, the photosensitive resin composition according to the first aspect, wherein the low molecular compound (C) contains two or more azide groups and has a molecular weight of 1000 or less. As an eighth aspect, it relates to a film comprising a cured product or a partially cured product of the photosensitive resin composition according to any one of the first to seventh aspects. As a ninth aspect, it relates to a laminate having a substrate and the film according to the eighth aspect. As a tenth aspect, it relates to the laminate according to the eighth aspect, wherein the film is a patterned film. As an eleventh aspect, the substrate is a plastic having a glass transition temperature of 105°C or lower and relates to the laminate according to the ninth aspect. As a twelfth aspect, the substrate is a plastic having a glass transition temperature of 105°C or lower, and relates to the laminate according to the tenth aspect. According to a thirteenth aspect, the present invention relates to a method for producing a laminate, the method including a step of forming a cured or partially cured product of the photosensitive resin composition according to any one of the first to seventh aspects on a surface of a substrate. As a fourteenth aspect, the present invention relates to a method for producing a laminate, the method including the steps of applying the photosensitive resin composition according to any one of the first to seventh aspects onto a surface of a substrate to form a coating film, irradiating the coating film with light, and developing the coating film after exposure. Effect of the Invention
[0010] By using the photosensitive resin composition having an azide group of the present invention, high-temperature baking after exposure is not required, and a curing process can be performed at 50° C. or less, a process that does not generate acid is possible, and a process that partially cures the resin can be performed. If the solvent of the present invention is used, it is possible to use plastics and the like without dissolving them. According to the production method using the photosensitive resin composition having an azide group of the present invention, a simple production method using a photolithography method that does not require baking after exposure can be provided. According to the production method of the present invention using the photosensitive resin composition having an azide group, it is possible to provide a film made of a temperature-responsive cured or partially cured product and a patterned film on a plastic substrate having a glass transition temperature of 105° C. or less, and further to provide a laminate made of the substrate and the film. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the results of measuring the sensitivity of the photosensitive resin compositions obtained in Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Photosensitive resin composition> The photosensitive resin composition using the temperature-responsive polymer of the present invention is a photosensitive resin composition that contains a temperature-responsive polymer (A) that does not have a carbon-carbon triple bond, and a solvent (B), and may contain a low molecular weight compound (C) having an azide group, in which when the low molecular weight compound (C) is not contained, the temperature-responsive polymer (A) has an azide group, and when the low molecular weight compound (C) is contained, the temperature-responsive polymer (A) may have an azide group. Therefore, the photosensitive resin composition of the present invention is (1) a temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group, a solvent (B) and a low molecular weight compound (C) having an azide group, (2) a temperature-responsive polymer (A) having no carbon-carbon triple bond and no azide group, a solvent (B), and a low molecular weight compound (C) having an azide group; (3) a temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group, and a solvent (B); It consists of either However, the following photosensitive resin composition will also be described. (4) A temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group, a solvent (B), and a low molecular weight compound (C) having no azide group. The above components will be described below.
[0013] <Temperature-responsive polymer (A) having no carbon-carbon triple bond and no azide group> Examples of the temperature-responsive polymer (A) that does not have a carbon-carbon triple bond and does not have an azide group include polymers having structural units represented by the following formula (1), and formulas (1-1-1) and (1-1-2). [ka] (In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an optionally substituted alkyl group having 1 to 10 carbon atoms. The above-mentioned "alkyl group having 1 to 3 carbon atoms" includes those having a straight or branched chain, such as a methyl group, an ethyl group, an n-propyl group, and an isopropyl group.
[0014] The "alkyl group having 1 to 10 carbon atoms" includes those having a straight chain or a branched chain, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2 ... Examples of such alkyl groups include butyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl and 1-ethyl-2-methyl-n-propyl groups.
[0015] Examples of the substituent that the "optionally substituted alkyl group having 1 to 10 carbon atoms" may have include a halogen atom, an amino group, a mono- or di-alkylamino group having 1 to 4 carbon atoms, a nitro group, a cyano group, an oxo group, a hydroxy group, a sulfanyl group, an alkoxy group having 1 to 4 carbon atoms, an alkoxycarbonyl group having 1 to 4 carbon atoms, a formyl group, and an aryl group having 6 to 14 carbon atoms.
[0016] The aforementioned "halogen atom" includes fluorine, chlorine, bromine and iodine. Examples of the "mono- or di-alkylamino group having 1 to 4 carbon atoms" include a methylamino group, an ethylamino group, a propylamino group, an isopropylamino group, a butylamino group, a dimethylamino group, a diethylamino group, a dipropylamino group, a dibutylamino group, and an n-ethyl-n-methylamino group.
[0017] The alkoxy group may be either linear or branched. Examples of the "alkoxy group having 1 to 4 carbon atoms" include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, and a tert-butoxy group. The alkoxycarbonyl group having 1 to 4 carbon atoms is an organic group in which a carbonyl group -C(=O)- is bonded to the "alkoxy group having 1 to 4 carbon atoms."
[0018] Examples of the "aryl group having 6 to 14 carbon atoms" include a phenyl group, a 1-naphthyl group, Examples of the anthryl group include an anthryl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, and a 9-anthryl group. The above description of "having no carbon-carbon triple bond" indicates that in the present invention, a cycloaddition reaction between a carbon-carbon triple bond and a compound containing an azide group and a reaction for forming a 1,2,3-triazole ring are excluded. Examples of the temperature-responsive polymer (A) that does not have a carbon-carbon triple bond and does not have an azide group include polymers that contain the structural units represented by the following formulae (1-1-1) and (1-1-2). [ka] (In formula (1-1-1), R 11 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 12 represents an optionally substituted alkyl group having 1 to 10 carbon atoms, In formula (1-1-2), R 13 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 14 represents a group that does not contain an azide group but contains an epoxy group, In Formula (1-1-1) and Formula (1-1-2), x1 and y1 are each any number satisfying x1 + y1 ≤ 1, 0 < x1 < 1, and 0 < y1 < 1. In the above Formula (1-1-1) and Formula (1-1-2), x1 and y1 are each any number satisfying x1 + y1 ≤ 1, 0 < x1 < 1, and 0 < y1 < 1. Further, x1 and y1 can satisfy 0.01 ≤ y1 / x1 ≤ 0.2, preferably satisfy 0.02 ≤ y1 / x1 ≤ 0.18, and more preferably satisfy 0.03 ≤ y1 / x1 ≤ 0.15. The "alkyl group having 1 to 3 carbon atoms" and the "optionally substituted alkyl group having 1 to 10 carbon atoms" are the same as the content described above in Formula (1). Also, when there is a description of the "alkyl group having 1 to 3 carbon atoms", the "optionally substituted alkyl group having 1 to 10 carbon atoms", or "optionally substituted" below, unless otherwise specified, it is the same as the content described above.
[0019] The "R 14 ", and the "group containing no azide group and containing an epoxy group" include monovalent groups represented by the following Formulas (1-2) and (1-3).
Chemical Formula
Chemical Formula
Chemical Formula
[0020] <Synthesis of temperature-responsive polymer (A) having no carbon-carbon triple bond and no azide group> [ka] (In formula (1-4), R 11 , R 12 , R 13 , R 14 , x1 and y1 are the same as in formula (1-1-1) and formula (1-1-2), respectively. The monomer shown on the left side of the formula (1-4) and the monomer shown on the right side are dissolved in a molar ratio of x1:y1 in a solvent (B), and then reacted, for example, at 50°C or higher for 10 hours or more to obtain a solution of a temperature-responsive polymer of the monomer shown on the left side of the formula (1-4) and the monomer shown on the right side of the formula (1-4). The weight average molecular weight (mw) of the obtained temperature-responsive polymer in terms of standard polystyrene should preferably be 5,000 or more, more preferably 6,000 or more, 7,000 or more, 8,000 or more, 9,000 or more, 10,000 or more, 11,000 or more, or 12,000 or more, because if it is low, the sensitivity of the temperature response will be low. On the other hand, if it is high, there is a high possibility that the solubility and resolution will decrease. Therefore, it is preferably 300,000 or less, more preferably 250,000 or less, 200,000 or less, 150,000 or less, 100,000 or less, 90,000 or less, 80,000 or less, or 70,000 or less. The value of mw in the present invention is measured by gel permeation chromatography (GPC).
[0021] <Temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group> Examples of the temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group include a polymer having a structural unit represented by the following formula (2), i.e., the temperature-responsive polymer (A). [Chemical formula] (In formula (2), R 3 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 4 represents an optionally substituted alkyl group having 1 to 10 carbon atoms, R 5 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 6 represents a group containing an azide group, x and y are each any number satisfying x + y ≤ 1, 0 < x < 1, and 0 < y < 1.)
[0022] The "R 6 " and the "group containing an azide group" include, in addition to the azide group, a carbonyl group, a hydroxy group, an ether group, an arylene group, an alkylene group having 1 to 10 carbon atoms, a hydrocarbon ring group having 3 to 10 carbon atoms, a 3- to 10-membered heterocyclic group, and a 3- to 10-membered hetero-condensed ring group. It is a group which may contain one or more selected from the group. The "alkylene group having 1 to 10 carbon atoms" is a linear or branched alkylene group having 1 to 10 carbon atoms, and examples of such a divalent group include a divalent group obtained by removing one hydrogen atom from any carbon atom of the group exemplified above as the linear or branched alkyl group having 1 to 10 carbon atoms. The "hydrocarbon ring group having 3 to 10 carbon atoms" is also referred to as a cyclic alkyl group having 3 to 10 carbon atoms, and examples thereof include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, and a cyclodecyl group.
[0023] Examples of the "3- to 10-membered heterocyclic group" include aromatic heterocyclic groups such as a thienyl group, a furyl group, a pyrrolyl group, an imidazolyl group, a pyrazolyl group, a thiazolyl group, an isothiazolyl group, an oxazolyl group, an isoxazolyl group, a pyridyl group, a pyrazinyl group, a pyrimidinyl group, and a pyridazinyl group; and an aziridinyl group, an epoxy group, an oxiranyl group, a thiiranyl group, an azetidinyl group, an oxetanyl group, a thietanyl group, a tetrahydrothienyl group, a tetrahydrofuranyl group, a pyrrolinyl group, a pyrrolidinyl group, an imidazolinyl group, an imidazolidinyl group, an oxazolinyl group, an oxazolidinyl group, a pyrazolinyl group, Examples of non-aromatic heterocyclic groups include a pyrazolidinyl group, a thiazolinyl group, a thiazolidinyl group, a tetrahydroisothiazolyl group, a tetrahydrooxazolyl group, a tetrahydroisoxazolyl group, a piperidinyl group, a piperazinyl group, a tetrahydropyridinyl group, a dihydropyridinyl group, a dihydrothiopyranyl group, a tetrahydropyrimidinyl group, a tetrahydropyridazinyl group, a dihydropyranyl group, a tetrahydropyranyl group, a tetrahydrothiopyranyl group, a morpholinyl group, a thiomorpholinyl group, an azepanyl group, a diazepanyl group, an azepinyl group, an oxepanyl group, an azocanyl group, and a diazocanyl group.
[0024] The above-mentioned "3- to 10-membered fused heterocyclic group" includes a group represented by the following formula (2-1). [ka] Specific examples of the structural unit of the organic group shown on the right side of the formula (2) are the structural units of the organic groups shown in the above formulas (1-11) to (1-26) and the reaction product of 4-azidobenzoic acid. However, the structural unit of the organic group shown on the right side of the formula (2) is not limited to the reaction product of the organic groups shown in the above formulas (1-11) to (1-26) and 4-azidobenzoic acid. The phrase “may contain one or more kinds” means that, for example, a group containing a portion where a plurality of two or more kinds of groups are bonded, such as “-(ether group)-(alkylene group)-(ether group)-(alkylene group)-”, may be included.
[0025] The temperature-responsive polymer (A) is, for example, a polymer having a structural unit represented by the above formula (2). In the formula (2), two kinds of structural units are shown, and x and y are the molar ratios of the constituent units. The temperature-responsive polymer (A) may contain structural units other than the structural unit represented by the formula (2). In the formula (2), x and y are each any number satisfying x + y ≤ 1, 0 < x < 1, and 0 < y < 1. The ratio of the number of moles of x to the number of moles of y is represented by y / x. When y / x is greater than 0.2, the temperature responsiveness deteriorates, and when it is less than 0.01, the exposure sensitivity deteriorates. Therefore, it is preferable that y / x satisfies 0.01 ≤ y / x ≤ 0.2, more preferably 0.02 ≤ y / x ≤ 0.18, and still more preferably 0.03 ≤ y / x ≤ 0.15. is preferably satisfied. For example, what “0.03 ≤ y / x ≤ 0.15” means indicates that the number of moles of y is 3 mol% to 15 mol% with respect to the number of moles of x. This shows that for the left-side constituent unit represented by the formula (2), the right-side constituent unit suffices at 3 mol% to 15 mol%. That is, although the left-side constituent unit of the formula (2) is important as the temperature-responsive polymer, the right-side constituent unit of the formula (2) is necessary to promote crosslinking by light. In the present invention, under the constraints of the substrate, solvent, temperature, etc., the degree of film curing can be adjusted by the exposure amount and the ratio of x:y, and it can be determined whether to form a film with a cured product or a film by partial curing. Therefore, this ratio of x:y becomes an important index. Furthermore, the above "x+y≦1" can be "x+y=1" or "x+y<1". When "x+y=1", the polymer is composed only of the left and right structural units shown in formula (2). When "x+y<1", the "temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group" includes other polymer structural units in addition to the polymer structural units shown on the right and left sides of formula (2). A specific example of this case is the structural unit in a polymer polymerized from the "low molecular weight compound (C) having no azide group" below. From the above, examples of "temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group" include polymers obtained by polymerizing one or more compounds selected from the group consisting of the monomer before polymerization of the structural unit shown on the left side of the following formula (2), the monomer before polymerization of the structural unit shown on the right side of the above formula (2), and "low molecular weight compound (C) having no azide group."
[0026] <Synthesis of temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group> For example, 4-azidobenzoic acid and a solvent (B) are added to a solution having the temperature-responsive polymers represented by the formulas (1-1-1) and (1-1-2) and reacted for, for example, 20 hours or more at 50° C. or higher. Then, excess 4-azidobenzoic acid is removed by ion exchange to obtain a solution of a temperature-responsive polymer (A) having no carbon-carbon triple bond and having an azide group. Also, for example, any of the monomers shown in the following formulas (5-11) to (5-26), 4-azidobenzoic acid, and solvent (B) are added and reacted, for example, at 50° C. or higher for 20 hours or more. Then, excess 4-azidobenzoic acid is removed by ion exchange to obtain a solution of a monomer having an azide group. The monomer shown on the left of the above formula (1-4) and the monomer having an azide group are dissolved in a molar ratio of x1:y1 in a solvent (B), and then reacted, for example, at 50°C or higher for 10 hours or more to obtain a solution of a temperature-responsive polymer of the monomer shown on the left of the above formula (1-4) and the monomer having an azide group. The weight average molecular weight (mw) of the obtained temperature-responsive polymer (A) having no carbon-carbon triple bond and an azide group, calculated based on standard polystyrene standards, is preferably 5,000 or more, more preferably 6,000 or more, 7,000 or more, 8,000 or more, 9,000 or more, 10,000 or more, 11,000 or more, or 12,000 or more, because a low weight average molecular weight leads to a low sensitivity of temperature responsiveness, and is preferably 300,000 or less, more preferably 250,000 or less, 200,000 or less, 150,000 or less, 100,000 or less, 90,000 or less, 80,000 or less, or 70,000 or less, because a high weight average molecular weight leads to a high possibility of a low solubility or resolution. The mw value in the present invention is measured by gel permeation chromatography (GPC).
[0027] <Content of temperature-responsive polymer (A)> In order to achieve good patterning characteristics, the content of the temperature-responsive polymer may be 50 to 99 parts by mass, 60 to 98 parts by mass, or even 70 to 97 parts by mass or less per 100 parts by mass of the total mass of the solid content of the photosensitive resin composition excluding the solvent.
[0028] <Solvent (B)> The solvent (B) is selected from an optionally substituted alcohol having 2 to 10 carbon atoms or an ester which is a reaction product of such an alcohol with a carboxylic acid. The "alcohol having 2 to 10 carbon atoms" may be linear or branched. Specific examples include ethanol, 1-propanol, 2-propanol, 1-butanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-2-butanol, 2-ethyl-1-butanol, 2,3-dimethyl-2-butanol, 2-methyl-2-pentanol, 4-methyl-2-pentanol, tert-pentyl alcohol, propylene glycol monopropyl ether, tert-butyl cellosolve, cyclohexanol, 4-tert-butylhexanol, α-terpineol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, diethylene glycol mono-tert-butyl ether, and diacetone alcohol. In addition, the "ester which is a reaction product of the alcohol and the carboxylic acid" is a product of the reaction of the "alcohol having 2 to 10 carbon atoms" with a carboxylic acid, and is a bond formed by removing one hydrogen atom from any carbon atom of the group shown in the "alcohol having 2 to 10 carbon atoms". 7 " is a combination of The above "R 7 " is the above-mentioned "alkyl group having 1 to 10 carbon atoms."
[0029] The substituent that the "alcohol having 2 to 10 carbon atoms which may be substituted" may have is the same as the substituent that the "alkyl group having 1 to 10 carbon atoms which may be substituted" may have. In particular, when the substituent is a hydroxyl group, the alcohol becomes a polyhydric alcohol. Examples of the polyhydric alcohol include dihydric polyhydric alcohols such as ethylene glycol, propylene glycol, butanediol, pentanediol, dimethylbutanediol, hexanediol, octanediol, and decanediol, and trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, and trimethylolpropane. The present invention is not limited to only these examples. These alcohols may be used alone or in combination of two or more kinds.
[0030] In order to control the film thickness and obtain good patterning characteristics, the content of the solvent is preferably 50 to 99.5 parts by mass, more preferably 55 to 95 parts by mass or 60 to 90 parts by mass, and even more preferably 70 to 80 parts by mass, relative to 100 parts by mass of the total mass of the photosensitive resin composition.
[0031] <Low molecular weight compound having an azide group (C)> Examples of the low molecular weight compound (C) having an azide group include the compounds represented by the following formulae (3-1) and (3-2). HOOC-R 31 -N3(3-1) (In formula (3-1), R 31 represents a carbonyl group, an ether group, an arylene group, or an alkylene group having 1 to 10 carbon atoms. A specific example of the compound represented by the formula (3-1) is 4-azidobenzoic acid. C=CR 32 -COO-R 33 -N3(3-2) (In formula (3-2), R 32 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 33 is an organic group which may contain one or more selected from the group consisting of a carbonyl group, an ether group, an optionally substituted arylene group, and an optionally substituted alkylene group having 1 to 10 carbon atoms. The substituents which the "optionally substituted" may have are the same as the substituents which the "optionally substituted alkyl group having 1 to 10 carbon atoms" may have.
[0032] <Low molecular weight compound (C) having two or more azide groups> Examples of the low molecular weight compound (C) having two or more azide groups include the compounds represented by the following formulae (4-1), (4-2) and (4-3). HOOC-C(R 41 -N3)-R 42 -N3(4-1) (In formula (4-1), R 41 and R42 represents a carbonyl group, an ether group, an arylene group, or an alkylene group having 1 to 10 carbon atoms. C=CR 43 -COO-C(R 44 -N3)-R 45 -N3(4-2) (In formula (4-2), R 43 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 44 and R 45 are each an organic group which may contain one or more groups independently selected from the group consisting of a carbonyl group, an ether group, an optionally substituted arylene group, and an optionally substituted alkylene group having 1 to 10 carbon atoms. N3-R 46 -N3(4-3) (In formula (4-3), R 46 is an organic group which may contain one or more selected from the group consisting of a carbonyl group, an ether group, a sulfonyl group, an optionally substituted arylene group, an optionally substituted alkylene group having 1 to 10 carbon atoms, an optionally substituted alkenylene group having 1 to 10 carbon atoms, and an optionally substituted divalent hydrocarbon ring group having 3 to 10 carbon atoms. The substituent that the "optionally substituted" may have is the same as the substituent that the above-mentioned "optionally substituted alkyl group having 1 to 10 carbon atoms" may have. Specific examples include formulas (4-11) to (4-17). [ka] The molecular weight of the low molecular weight compound having two or more azide groups is preferably 1,000 or less, more preferably 800 or less, and even more preferably 500 or less.
[0033] <Low molecular weight compound (C) not having an azide group> Examples of the low molecular weight compound (C) not having an azide group include the compounds represented by the following formulae (5), (5-1) and (5-2). [ka] (In formula (5), R 51 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 52 and R 53 each independently represents a hydrogen atom or an optionally substituted alkyl group having 1 to 10 carbon atoms. Specific examples of the above formula (5) include the group consisting of (meth)acrylamide, n-methyl(meth)acrylamide, n-ethyl(meth)acrylamide, n-isopropyl(meth)acrylamide, n-propyl(meth)acrylamide, n-butyl(meth)acrylamide, n-(tert-butyl)(meth)acrylamide, hexyl(meth)acrylamide, heptyl(meth)acrylamide, n-methyl-n-isopropyl(meth)acrylamide, n-(2-hydroxy-1-methylethyl)(meth)acrylamide, n,n-dimethyl(meth)acrylamide, n,n-diethyl(meth)acrylamide, n-ethyl-n-methyl(meth)acrylamide, and n-(2-hydroxyethyl)(meth)acrylamide. In this specification, "(meth)acrylate" and the like mean "acrylate and methacrylate" and the like.
[0034] [ka] (In the formula, R 54 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 55 represents a divalent organic group represented by the following formula (I), formula (II) or formula (III). [ka] (In the formula, c represents an integer of 0 to 3, d represents an integer of 1 to 3, and e each independently represents an integer of 2 to 6.) Specific examples of the compounds (monomers) represented by the formulas (5-1) and (5-2) include the monomers represented by the following formulas (5-11) to (5-26). These monomers may be used alone or in combination of two or more. [ka]
[0035] Further, in addition to the compounds represented by the above formulas (5), (5-1) and (5-2), examples of the low molecular weight compound (C) not having an azide group include, for example, the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate and 1,4-cyclohexanedimethanol mono(meth)acrylate. Further examples include aminoalkyl (meth)acrylates such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; diaminoalkyl (meth)acrylates such as diaminomethyl (meth)acrylate and diaminoethyl (meth)acrylate; alkoxy (meth)acrylates such as methoxy(meth)acrylate; alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate; (meth)acrylamide derivatives such as N-(meth)acryloylpyrrolidine, N-(meth)acryloylpiperidine, and N-(meth)acryloylmorpholine; and the like. In addition, these monomers as well as two or more compounds selected from the group of compounds represented by the above formulas (5), (5-1) and (5-2) can be used as the "low molecular weight compound (C) not having an azide group".
[0036] <Crosslinking agent> The photosensitive resin composition of the present invention may contain a crosslinking agent within the range not impairing the effects of the present invention. Examples of the crosslinking agent include glycoluril compounds, melamine compounds, and bisazide compounds. Examples of glycoluril compounds include 1,3,4,6-tetrakis(methoxymethyl)glycoluril, 1,3,4,6-tetrakis(ethoxymethyl)glycoluril, 1,3,4,6-tetrakis(propoxymethyl)glycoluril, and 1,3,4,6-tetrakis(butoxymethyl)glycoluril. Examples of the melamine compound include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, and hexabutoxymethylmelamine. can be done.
[0037] Examples of the bisazide compound include crosslinking agents represented by the following formulas (6-1) to (6-12). [ka] When a crosslinking agent is used, the content thereof can usually be blended in a ratio of 50 parts by mass or less, 30 parts by mass or less, or even 10 parts by mass or less relative to 100 parts by mass of the total mass of the temperature-responsive polymer (A) (resin component) in order to obtain sufficient temperature responsiveness. In addition, when two or more reactive groups that react with each other are present in the photosensitive resin composition, the photosensitive resin composition can be crosslinked without a crosslinking agent (self-crosslinking). In such a case, the photosensitive resin composition of the present invention does not need to contain a crosslinking agent.
[0038] <Other additives> The photosensitive resin composition of the present invention may contain other additives commonly used in the art, as long as the effects of the present invention are not impaired. Examples of the other additives include antireflection agents, ultraviolet absorbers, antioxidants, light stabilizers, sensitizers, surfactants, leveling agents, silane coupling agents, and the above-mentioned "low molecular weight compound (C) having no azide group." When these other additives are used, they are usually added to the temperature-responsive polymer (A) (resin composition). The amount of the binder may be 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, or even 5 parts by mass or less, based on 100 parts by mass of the total mass of the binder and the binder (component).
[0039] <Base material> The substrate may be made of, for example, a resin. The resin may be any of natural resin, modified natural resin, and synthetic resin. Examples of natural resins include cellulose. Examples of modified natural resins include cellulose triacetate and cellulose immobilized with dextran sulfate. Examples of synthetic resins include polyethylene, polypropylene, polyvinyl chloride, polystyrene, ABS, polyamide 6, polyamide 66, polyurethane, polylactic acid, polyacrylonitrile, polyvinylidene fluoride, polybutylene terephthalate, polyethylene terephthalate, polyvinyl acetate, polybutyl acrylate, polyethyl acrylate, polymethyl acrylate, polymethyl methacrylate, polyester polymer alloy, polyvinyl alcohol, polyester, and polyethersulfone.
[0040] The substrate used in the present invention may be a plastic having a glass transition temperature of 105° C. or lower. In particular, examples of "plastic having a glass transition temperature of 105° C. or lower" include polyethylene, polypropylene, polyvinyl chloride, polystyrene, ABS, polyamide 6, polyamide 66, polylactic acid, polyacrylonitrile, polyvinylidene fluoride, polybutylene terephthalate, polyethylene terephthalate, polyvinyl acetate, polybutyl acrylate, polyethyl acrylate, polymethyl acrylate, polymethyl methacrylate, etc. Among these plastics, polystyrene is preferable.
[0041] <Film made of a cured or partially cured product of a photosensitive resin composition, a laminate having the film and a substrate, and a laminate having a patterned film and a substrate> The present invention also provides a film made of a cured or partially cured product obtained from the photosensitive resin composition, a laminate having the film and a substrate, and a laminate having a patterned film and a substrate. The patterned film of the present invention can be produced by the following pattern forming method. Furthermore, the laminate can be produced by the following laminate production method. The present invention also provides a laminate having a temperature-responsive patterned film having a desired response temperature and a substrate, which is formed by patterning the photosensitive resin composition of the present invention by a photolithography method. The laminate of the present invention has a film and a substrate. Therefore, the substrate may have a film on both sides, not just one side. The film constituting the laminate of the present invention may be a film made of a plurality of cured products, or a film made of a plurality of partially cured products.
[0042] The term "partially cured product" refers to a product that would become a cured product if the amount of exposure was increased, but is not cured in part because the amount of exposure is small. Also, for example, a product is partially cured when y1 / x1 in the above formula (1-4) or y / x in formula (2) is small.
[0043] There is no particular limit to the shape of the pattern formed in the patterned film, and examples of such shapes include square, round, linear, and line-and-space shapes when observed from above the substrate. There is no particular limit to the size of the pattern observed from above and its thickness (height) observed from the cross section of the pattern. The size of one side of the pattern is, for example, 0.1 μm to 1,000 mm, and the thickness (height) of the pattern is, for example, 5 nm to 1,000 μm. These pattern shapes can be controlled by using multiple masks with different shapes of transmitted light during the exposure process.
[0044] <Method of manufacturing a laminate having a film and a substrate> A film made of a cured or partially cured product of the photosensitive resin composition of the present invention and a laminate having the film and a substrate are obtained. The film is then patterned to obtain a patterned film and a laminate having the film and a substrate. The laminate can be produced, for example, by the method described below. i) A step of applying a photosensitive resin composition to a surface of a substrate to form a coating film. The photosensitive resin composition of the present invention is applied to a substrate by a method such as spin coating or slit coating, and the solvent is removed to form a coating film. ii) a step of irradiating the coating film with light When the coating is irradiated with light of a certain wavelength through a mask using an aligner to obtain a desired pattern, crosslinking (curing) occurs only in the exposed areas. iii) A step of developing the coating film after exposure The exposed coating is developed with a developer or the like to remove the unexposed areas (uncured areas of the coating). According to the above-described manufacturing method, it is possible to produce a film consisting of a cured product or a partially cured product of the photosensitive resin composition, a patterned film, and also to produce a laminate having the film and a substrate, and a laminate having a patterned film and a substrate.
[0045] In the above-mentioned production method, if the exposure dose is reduced in the "ii) step of irradiating the coating film with light", a partially cured product that is not completely cured can be produced. When producing a partially cured product, the degree of curing of the partially cured product varies depending on the film thickness, the type of solvent, the concentration of the solvent, etc., so the exposure dose is adjusted according to the desired degree of curing. The light to be irradiated is preferably ultraviolet light or visible light of 500 nm or less, more preferably ultraviolet light. The exposure dose is preferably 1 to 10,000 mj / cm. 2 , more preferably 10 to 5,000 mj / cm 2 , and more preferably 20 to 3,000 mj / cm 2 It is.
[0046] <Cell culture support and method for producing same> The cell culture support of the present invention is a film made of a temperature-responsive cured product, a film made of a partially cured product, or a patterned film, which is formed on a substrate using a photosensitive resin composition containing a temperature-responsive polymer, and is a laminate formed of the film. The present invention also provides a method for producing the cell culture support, and a cell culture support obtained by the production method. The method for producing a cell culture support in the present invention is the same as the method for producing a laminate having a film and a substrate, which uses a photosensitive resin composition containing a temperature-responsive polymer. The method is characterized by including a step of forming a coating film on a substrate and irradiating the coating film with light to form a film made of a cured product, a film made of a partially cured product, or a patterned film. It is preferable that the photosensitive resin composition does not contain an acid generator and is not subjected to high-temperature baking after light irradiation. The photosensitive resin composition may also contain a crosslinking agent or other additives. The thickness (height) of the membrane as a cell culture support is preferably 1 to 100 nm, more preferably 2 to 50 nm, and even more preferably 3 to 30 nm, so that the cells are attached to the membrane during culture and the cultured cells are detached from the membrane by changing the temperature of the culture system when the cultured cells are recovered. There is no particular limitation on the size of the membrane observed from above, and the size of one side of the cured layer is, for example, 0.1 to 1,000 mm. The base material as the cell culture support may be the same as the above-mentioned <base material>.
[0047] <Lower critical point temperature> In the present invention, the cell culture support has a lower critical solution temperature (LCST) in order to attach cells to the membrane during culture, and to detach the cultured cells from the membrane by changing the temperature of the culture system when recovering the cultured cells. The lower critical solution temperature is the temperature at which a solution separates into two phases above a certain temperature. In other words, in a system having a lower critical solution temperature, it is said that at temperatures below that temperature, multiple components exist in one phase regardless of their composition. The lower critical point temperature (LCST) was determined by dissolving the polymer in phosphate buffered saline (Phos The solution was dissolved in phosphate buffered saline (Sigma-Aldrich) at a concentration of 2 wt %. Under a nitrogen atmosphere, the temperature of the aqueous solution was lowered at 1° C. / min, and the differential heat was measured against the air using a differential scanning calorimetry (DSC) (DSC7020, SII Nano Technology Co., Ltd.), and the temperature showing the peak top of the measurement curve was calculated as the lower critical point temperature (LCST) of the polymer. The cell culture support of the present invention can be manufactured by changing the constituent units of the temperature-responsive polymer, so that the cell culture support has a lower critical temperature (LCST) of 15°C or more and less than 45°C. The cell culture support is a photosensitive resin composition using a temperature-responsive polymer containing two or more kinds of constituent units having different temperature responsiveness, and may have a pattern with two or more kinds of response temperatures. The cell culture support of the present invention can be any of the above cell culture supports.
[0048] <Cell culture method for cell culture support, etc.> In the present invention, the method and conditions for culturing cells on the cell culture support are not particularly limited, and cells can be cultured by a method known per se. The method for culturing cells involves using a cell culture support having a membrane formed on a substrate from a photosensitive resin composition containing a temperature-responsive polymer, seeding cells on the cell culture support on the membrane, and culturing the cells by incubating the cells at a temperature suitable for culture and higher than the lower critical point temperature of the cell culture support, and then adjusting the temperature of the cured material layer to a temperature lower than the lower critical point temperature of the temperature-responsive polymer, thereby detaching the cells from the cell culture support and recovering the cells.
[0049] In the present invention, the cells are not particularly limited, and various cells can be cultured. Examples of the cells include epithelial cells and endothelial cells that constitute each tissue and organ in the body; skeletal muscle cells, smooth muscle cells, and cardiomyocytes that exhibit contractility; neurons and glial cells that constitute the nervous system; fibroblasts; hepatocytes, non-parenchymal liver cells, and adipocytes related to metabolism in the body; stem cells present in various tissues, as well as bone marrow cells and ES cells, etc. In the present invention, there is no particular limitation on the method of seeding cells or the method of recovering cultured cells detached from a cell culture support, and a method known per se can be used.
Example
[0050] Hereinafter, the present invention will be described more specifically with reference to examples. However, the present invention is not limited by the following examples, and it is of course possible to appropriately modify and implement the invention within the scope that conforms to the above and below gists, and all of them are included in the technical scope of the present invention.
[0051] <a. Synthesis of Polymer and Monomer> <Synthesis Example 1> After dissolving 20 g of N-isopropylacrylamide and 2.8 g of glycidyl methacrylate in 81.4 g of 1-propanol, the temperature was raised to 75°C. Then, while maintaining the reaction solution at 75°C, 0.5 g of azobisisobutyronitrile was added and reacted at 75°C for 24 hours to obtain a solution of a polymer of N-isopropylacrylamide and glycidyl methacrylate. When GPC analysis of the obtained polymer was performed, the weight average molecular weight was 34,000 in terms of standard polystyrene conversion. To 50 g of a solution having 11.1 g of the polymer, 2.3 g of 4-azidobenzoic acid, 0.1 g of triethylamine, and 2.2 g of 1-propanol were added and reacted at 80°C for 48 hours. Then, excess 4-azidobenzoic acid was removed by ion exchange to obtain a solution of the polymer of formula (11). When GPC analysis of the obtained polymer was performed, the weight average molecular weight was 51,000 in terms of standard polystyrene conversion.
Chemical formula
[0052] <Synthesis Example 2> 20g of N-isopropylacrylamide and 1.3g of glycidyl methacrylate were dissolved in 76.1g of 1-propanol, and the temperature was raised to 75°C. Then, 0.4g of azobisisobutyronitrile was added while keeping the reaction solution at 75°C, and the reaction was carried out at 75°C for 24 hours to obtain a solution of a polymer of N-isopropylacrylamide and glycidyl methacrylate. When the obtained polymer was analyzed by GPC, the weight average molecular weight was 29000 in terms of standard polystyrene. 1.2g of 4-azidobenzoic acid, 0.05g of triethylamine, and 0.8g of 1-propanol were added to 50g of a solution containing 11.1g of the polymer, and the reaction was carried out at 80°C for 48 hours. Then, excess 4-azidobenzoic acid was removed by ion exchange, and a solution of the polymer of formula (12) was obtained. When the obtained polymer was analyzed by GPC, the weight average molecular weight was 36000 in terms of standard polystyrene. [ka]
[0053] <Synthesis Example 3> 20g of N-isopropylacrylamide and 3.9g of 4-hydroxybutyl acrylate glycidyl ether were dissolved in 56.9g of 1-propanol, and the temperature was raised to 75°C. Then, 0.5g of azobisisobutyronitrile was added while keeping the reaction solution at 75°C, and the mixture was reacted at 75°C for 24 hours to obtain a solution of a copolymerized polymer compound of N-isopropylacrylamide and 4-hydroxybutyl acrylate glycidyl ether. When the obtained copolymerized polymer compound was analyzed by GPC, the weight average molecular weight was 30800 in terms of standard polystyrene. 4.2g of 4-azidobenzoic acid, 0.2g of triethylamine, and 52.8g of 1-propanol were added to 70g of the solution containing 21.4g of the polymer compound, and the mixture was reacted at 80°C for 48 hours. Then, the excess 4-azidobenzoic acid was removed by ion exchange, and a solution of the polymer compound of formula (13) was obtained. The copolymerized polymer was analyzed by GPC and found to have a weight average molecular weight of 36,000 in terms of standard polystyrene. [ka]
[0054] <Synthesis Example 4> 10 g of N-isopropylacrylamide and 0.73 g of 4-benzoylphenyl methacrylate were dissolved in 43.3 g of 1-propanol, and the temperature was raised to 70°C. Then, while maintaining the reaction solution at 70°C, 0.11 g of azobisisobutyronitrile was added, and the reaction was carried out at 70°C for 24 hours to obtain a solution of a copolymerized polymer compound (formula (14)) of N-isopropylacrylamide and 4-benzoylphenyl methacrylate. When the obtained copolymerized polymer compound was subjected to GPC analysis, the weight average molecular weight was 55,200 in terms of standard polystyrene. [ka]
[0055] <Comparative Synthesis Example 1> After dissolving 20 g of N-isopropylacrylamide and 2.8 g of glycidyl methacrylate in 81.4 g of propylene glycol monomethyl ether, the temperature was raised to 75°C. Then, while maintaining the reaction solution at 75°C, 0.5 g of azobisisobutyronitrile was added and reacted at 75°C for 24 hours to obtain a solution of a copolymeric high molecular compound of N-isopropylacrylamide and glycidyl methacrylate. When GPC analysis of the obtained copolymeric high molecular compound was performed, the weight average molecular weight in terms of standard polystyrene was 38,900. To 50 g of a solution having 11.1 g of the high molecular compound, 2.3 g of 4-azidobenzoic acid, 0.1 g of triethylamine, and 2.2 g of 1-propanol were added and reacted at 80°C for 48 hours. Then, excess 4-azidobenzoic acid was removed by ion exchange to obtain a solution of the high molecular compound of formula (15). When GPC analysis of the obtained copolymeric high molecular compound was performed, the weight average molecular weight in terms of standard polystyrene was 59,800.
Chemical formula
[0056] <Comparative Synthesis Example 2> After dissolving 20 g of N-isopropylacrylamide and 5.13 g of 2-hydroxyethyl acrylate in 101.5 g of 1-propanol, the temperature was raised to 80°C. Then, while maintaining the reaction solution at 80°C, 0.25 g of azobisisobutyronitrile was added and reacted at 80°C for 24 hours to obtain a solution of a copolymeric high molecular compound (formula (16)) of N-isopropylacrylamide and 2-hydroxyethyl acrylate. When GPC analysis of the obtained copolymeric high molecular compound was performed, the weight average molecular weight in terms of standard polystyrene was 23,000.
Chemical formula
[0057] <b. Preparation of Composition> <Examples 1 to 3> After adding 6.4 g of 1-propanol to 3.6 g of a solution containing 0.7 g of the reaction product obtained in Synthesis Examples 1 to 3, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a solution of the photosensitive resin composition (Compositions 1 to 3). <Example 4> After adding 0.13 g of 1,11-diazido-3,6,9-trioxoundecane (Formula (17)) and 16.63 g of 1-propanol to 3.24 g of a solution containing 0.67 g of the reaction product obtained in Synthesis Example 4, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a solution of the photosensitive resin composition (Composition 4). [Chemical formula] <Comparative Example 1> After adding 6.4 g of propylene glycol monomethyl ether to 3.6 g of a solution containing 0.7 g of the reaction product obtained in Comparative Synthesis Example 1, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a solution of the photosensitive resin composition (Comparative Composition 1). <Comparative Example 2> After adding 0.1 g of α-(methylsulfonyloxyimino)-4-methoxybenzyl cyanide (trade name: PAI-1001, manufactured by Midori Chemical Co., Ltd.), 0.03 g of 1,3,4,6-tetrakis(methoxymethyl) glycoluril, and 0.52 g of 1-propanol to 10 g of a solution containing 2 g of the reaction product obtained in Comparative Synthesis Example 2, the mixture was filtered using a polyethylene microfilter with a pore size of 1.0 μm to prepare a solution of the photosensitive resin composition (Comparative Composition 2).
[0058] <c. Measurement of optical parameters> The photosensitive resin composition solutions prepared in Examples 1 to 2 were applied onto a silicon wafer using a spinner. The coating film was formed by baking at 100 °C for 1 minute on a hot plate. Then, the attenuation coefficient (k value) at a wavelength of 275 nm of these films was measured using a spectroscopic ellipsometer (VUV-VASE manufactured by J.A. Woollam). 275 nm is the absorption contributed by the 4-azidobenzoic acid moiety. As a result, since it changed to 0.034 in Example 1 and 0.019 in Example 2, it was suggested that the desired 4-azidobenzoic acid was grafted onto the polymer.
[0059] <d. Sensitivity measurement> The photosensitive resin composition solutions prepared in Examples 1 to 4 were applied onto a silicon wafer and a polystyrene substrate using a spinner. They were baked on a hot plate at 50°C for 1 minute to form a coating film with a film thickness of 300 nm. After irradiating with 254 nm light using an aligner while changing the exposure dose and then developing with 1-propanol, photocured films could also be formed on the silicon wafer and on a polystyrene petri dish (35 mm Non treated Dish manufactured by IWAKI). A difference in sensitivity was observed depending on the graft amount of 4-azidobenzoic acid. Also, a similar sensitivity behavior was seen with the addition of a diazide compound as a crosslinking agent. However, in Comparative Composition Example 2, it was applied onto a polystyrene substrate. After baking on a hot plate at 50°C for 1 minute and irradiating with 365 nm light using an aligner (PLA-501 manufactured by Canon) while changing the exposure dose, post-exposure bake (PEB) was performed, and a photocured film was formed by developing with 1-propanol. However, a temperature of 100°C or higher was required for PEB, exceeding the heat resistance temperature of the polystyrene petri dish, so deformation of the polystyrene petri dish was observed during PEB. The results of the sensitivity measurement are shown in FIG. 1.
[0060] <e. Erosion test of polystyrene petri dish> Comparative Composition 1 was put into a polystyrene petri dish (35 mm Non treated Dish manufactured by IWAKI), and an attempt was made to coat it, but the petri dish dissolved. The petri dishes were not dissolved with Compositions 1 to 3 in which propylene glycol monomethyl ether was changed to 1-propanol.
Claims
1. A photosensitive resin composition comprising a temperature-responsive polymer (A) having no carbon-carbon triple bond, a solvent (B), and optionally a low molecular weight compound (C) having an azide group, When the low molecular weight compound (C) is not contained, the temperature-responsive polymer (A) may have an azide group, and when the low molecular weight compound (C) is contained, the temperature-responsive polymer (A) may have an azide group.
2. The photosensitive resin composition according to claim 1 , wherein the temperature-responsive polymer (A) is a polymer having a structural unit represented by the following formula (1): [Formula 1] (In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an optionally substituted alkyl group having 1 to 10 carbon atoms.
3. The photosensitive resin composition according to claim 1 , wherein the temperature-responsive polymer (A) is a polymer having a structural unit represented by the following formula (2): [Case 2] (In formula (2), R 3 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 4 represents an optionally substituted alkyl group having 1 to 10 carbon atoms, R 5 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 6 represents a group containing an azide group, x and y are any numbers satisfying x+y≦1, 0<x<1, and 0<y<1.)
4. R in the formula (2) 6may contain, in addition to an azide group, one or more selected from the group consisting of a carbonyl group, a hydroxyl group, an ether group, an arylene group, an alkylene group having 1 to 10 carbon atoms, a hydrocarbon ring group having 3 to 10 carbon atoms, a 3- to 10-membered heterocyclic group, and a 3- to 10-membered fused heterocyclic group.
5. The photosensitive resin composition according to claim 3 , wherein in the formula (2), 0.01≦y / x≦0.2 is satisfied.
6. 2. The photosensitive resin composition according to claim 1, wherein the solvent (B) is selected from an optionally substituted alcohol having 2 to 10 carbon atoms or an ester which is a reaction product of the alcohol with a carboxylic acid.
7. The photosensitive resin composition according to claim 1 , wherein the low molecular weight compound (C) contains two or more azide groups and has a molecular weight of 1,000 or less.
8. A film comprising a cured or partially cured product of the photosensitive resin composition according to any one of claims 1 to 7.
9. A laminate comprising a substrate and the film according to claim 8.
10. The laminate of claim 8 , wherein the film is a patterned film.
11. The laminate according to claim 9, wherein the substrate is a plastic having a glass transition temperature of 105° C. or lower.
12. The laminate according to claim 10, wherein the substrate is a plastic having a glass transition temperature of 105°C or lower.
13. A method for producing a laminate, comprising a step of forming a cured or partially cured product of the photosensitive resin composition according to claim 1 on a surface of a substrate.
14. 8. A method for producing a laminate, comprising the steps of: applying the photosensitive resin composition according to claim 1 to a surface of a substrate to form a coating film; irradiating the coating film with light; and developing the coating film after exposure.
Citation Information
Patent Citations
Photosensitive composition, patterned substrate, cell culture support, and cultured cell production method
WO2016068271A1
Substrate covered with polymers for selective separation of cells or for cell culturing
WO2019013148A1