Antibacterial laminate
A laminate with a cured coating layer of olefin polymer and cationic organosilane quaternary ammonium salt on polyolefin substrates addresses the challenge of immobilizing antibacterial agents on polypropylene films, maintaining efficacy through durability tests.
Patent Information
- Application Number
- JP2023043205
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polypropylene films lack the ability to effectively immobilize antibacterial agents due to their non-polar surface, and existing methods for immobilization do not ensure durability or antibacterial efficacy under water resistance and hot water conditions.
A laminate structure comprising a cured coating layer containing an olefin polymer and a cationic organosilane quaternary ammonium salt is applied to polyolefin substrates, with specific ratios and inclusion of hydrophilic polymers and graft polymers to enhance adhesion and durability.
The laminate maintains antibacterial properties even after durability tests such as water resistance, ensuring effective antibacterial activity on polyolefin surfaces like OPP films.
Smart Images

Figure 2024132445000001 
Figure 2024132445000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate having antibacterial properties. [Background technology]
[0002] Polypropylene film is the most widely used plastic film for flexible packaging because it has the lightest specific gravity among plastic films and is excellent in mechanical properties, heat resistance, water resistance, and transparency. However, polypropylene has low polarity because it does not have polar groups in its molecules, making it difficult to paint, adhere, or fix components to it.
[0003] In recent years, interest in safety and hygiene has increased in the wake of the global spread of the new coronavirus infection, and products with antibacterial and anti-coronavirus activity are being developed.
[0004] Dialkyldimethylammonium chloride is known as one of the materials having antibacterial and anticoronavirus activity (Non-Patent Document 1). Materials that can immobilize dialkyldimethylammonium chloride on a substrate include silane-based quaternary ammonium salts such as 3-(trihydroxysilyl)propyldimethyloctadecyl ammonium chloride. In the case of the above-mentioned material, the hydroxysilyl group forms a covalent bond with a carboxy group, a hydroxy group, etc. present on the substrate surface, thereby realizing the immobilization of the antibacterial and anticoronavirus components.
[0005] Flexible packaging materials that consumers often come into direct contact with are required to have antibacterial and anti-coronavirus activity. However, olefin films such as polypropylene films, which are widely used in such materials, generally do not have polar groups on their surfaces, making it difficult to immobilize components with antibacterial and anti-coronavirus activity.
[0006] Patent Document 1 discloses that a silane-based coating agent can be fixed onto a polyolefin substrate by using a primer containing polyacrylic acid for the silane-based coating agent. However, the polyolefin substrate used is SM340, an ICP (impact copolymer) PP with rubber components introduced, and it is unclear whether it is possible to fix it to PP that does not contain rubber components or biaxially oriented PP (OPP) film, etc., and issues remain.
[0007] Patent Document 2 discloses a method of fixing an antibacterial agent to the surface of an article by applying an antibacterial agent containing an ethoxysilane-based quaternary ammonium salt to a primer having a carboxy group. Specifically, it discloses that, as a method of fixing an antibacterial agent to a polypropylene resin molded body, an ethoxysilane-based quaternary ammonium salt remains even after an abrasion test by using maleic anhydride-modified polypropylene (acid value 3.0) as a binder for a 0.2 mm-thick polypropylene film. However, no evaluation of antibacterial performance has been performed when a polypropylene film is used as a substrate, and it is unclear whether sufficient antibacterial agent remains to exhibit antibacterial activity. In addition, the method described in Patent Document 2 has not been subjected to water resistance or hot water resistance tests. In other words, the presence or absence of antibacterial activity and durability are unknown, and problems remain. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2017-160311 A [Patent Document 2] International Publication No. 2013 / 047642 Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention is to provide a laminate for a poorly adherent polyolefin substrate, particularly an OPP film, in which an antibacterial agent containing an organosilane-based quaternary ammonium salt is fixed to the surface, and which maintains its antibacterial properties even after durability tests such as water resistance tests. [Means for solving the problem]
[0010] The present invention relates to the following items [1] to [7]. [1] A laminate having a cured coating layer (1) containing an olefin polymer (A) and a cured coating layer (2) containing a cationic organosilane quaternary ammonium salt. [2] The laminate according to [1], wherein the olefin-based polymer (A) has structural units derived from propylene and structural units derived from an olefin other than propylene, and a mass ratio of the structural units derived from propylene to the structural units derived from an olefin other than propylene is 60 / 40 to 95 / 5. [3] The laminate according to [1] or [2], wherein the cured coating layer (1) contains a hydrophilic polymer. [4] The laminate according to any one of [1] to [3], wherein the cured coating layer (1) contains a graft polymer in which a hydrophilic polymer is grafted onto the olefin polymer (A). [5] The laminate according to any one of [1] to [4], wherein the cured coating layer (1) contains a polymer (B) having a structural unit derived from a radically polymerizable monomer. [6] The laminate according to [5], wherein the polymer (B) has a structural unit derived from a radically polymerizable monomer having a hydroxyl group. [7] The laminate according to any one of [1] to [6], wherein the cured coating film layer (1) and the cured coating film layer (2) are provided in this order on a polyolefin substrate. [8] The laminate according to [7], wherein the polyolefin substrate is a biaxially oriented polypropylene substrate. Effect of the Invention
[0011] According to the present invention, it is possible to provide a laminate in which an antibacterial agent is immobilized on a polyolefin substrate such as an OPP film, and which is capable of maintaining antibacterial properties even after durability tests such as water resistance tests. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In this specification, the numerical range expressed by "to" means a range including the numbers before and after it as the lower and upper limits. In addition, "(meth)acrylic" is a general term for acrylic and methacrylic.
[0013] The laminate according to the embodiment is a laminate having a cured coating layer (1) containing an olefin polymer (A) and a cured coating layer (2) containing a cationic organosilane quaternary ammonium salt.
[0014] [Cured coating layer (1)] The cured coating layer (1) contains an olefin polymer (A). In addition to the olefin polymer (A), the cured coating layer (1) may contain at least one of a hydrophilic polymer and a polymer (B) having a structural unit derived from a radical monomer (excluding the olefin polymer (A)).
[0015] (Olefin Polymer (A)) The olefin polymer (A) is a polymer having an olefin-derived structural unit as a main structural unit, where the "main structural unit" means a structural unit that accounts for 50 mol % or more of the total structural units of the olefin polymer (A). The olefin polymer (A) may be a homopolymer of an olefin, or a copolymer having structural units derived from an olefin and structural units derived from a monomer other than an olefin.
[0016] The weight average molecular weight of the olefin polymer (A) is preferably 10,000 to 300,000. When the weight average molecular weight is within the above range, the handling property is good when applying and drying a coating material in which the olefin polymer (A) is dispersed or dissolved in a solvent or an organic solvent. From the viewpoint of environmental load, the coating material is preferably an aqueous resin dispersion in which the olefin polymer (A) is dispersed in an aqueous solvent.
[0017] A preferred embodiment of the olefin polymer (A) is an olefin polymer that satisfies the following (1) and (2). (1) It is a polymer composed of structural units derived from olefin monomers having 4 or less carbon atoms. (2) A polymer having a propylene content of 50 mol % or more. In order to improve adhesion to a polypropylene substrate, the propylene content is more preferably 60 mol % or more, and further preferably 70 mol % or more.
[0018] As the olefin-based polymer (A), various known olefin homopolymers and olefin-based copolymers can be used. Specific examples include, but are not limited to, the following polyolefins: homopolymers of ethylene or propylene; copolymers of ethylene and propylene; copolymers of ethylene and / or propylene with other monomers (for example, α-olefin monomers having 4 or more carbon atoms, such as 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, cyclopentene, cyclohexene, and norbornene); copolymers consisting of two or more types selected from the above-mentioned other monomers; copolymers of α-olefin monomers having 2 or more carbon atoms and comonomers such as vinyl acetate, acrylic esters, and methacrylic esters; copolymers of α-olefin monomers having 2 or more carbon atoms and comonomers such as aromatic vinyl monomers, or hydrogenated products thereof; conjugated diene block copolymers or hydrogenated products thereof, and the like. When the term "copolymer" is used simply, it may be a random copolymer or a block copolymer.
[0019] The α-olefin monomer having 2 or more carbon atoms is preferably an α-olefin monomer having 2 to 4 carbon atoms. Furthermore, the olefin polymer (A) may be a chlorinated polyolefin obtained by chlorinating the polyolefin. In this case, the chlorination degree of the chlorinated polyolefin is usually 5% by mass or more, preferably 10% by mass or more. In addition, the chlorination degree is usually 40% by mass or less, preferably 30% by mass or less.
[0020] Specific examples of the olefin polymer (A) include polyethylene, polypropylene, ethylene-butene copolymer, ethylene-propylene copolymer, propylene-butene copolymer, propylene-hexene copolymer, chlorinated polyethylene, chlorinated polypropylene, chlorinated ethylene-propylene copolymer, chlorinated propylene-butene copolymer, ethylene-vinyl acetate copolymer, hydrogenated styrene-butadiene-styrene block copolymer (SEBS), hydrogenated styrene-isoprene-styrene block copolymer (SEPS), etc. These polymers may be used alone or in combination of two or more.
[0021] The olefin polymer (A) is preferably a propylene homopolymer or a copolymer of propylene and an α-olefin other than propylene, which may be chlorinated. As the copolymer, an ethylene-propylene copolymer, a propylene-butene copolymer, a chlorinated ethylene-propylene copolymer, or a chlorinated propylene-butene copolymer is more preferred. From the viewpoint of environmental load, the olefin polymer (A) is more preferably one that does not contain chlorine atoms, and is particularly preferably a propylene homopolymer, an ethylene-propylene copolymer, or a propylene-butene copolymer that does not contain chlorine atoms.
[0022] The olefin polymer (A) is preferably a propylene polymer containing propylene as a constituent unit. The propylene content in the propylene polymer is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more. Usually, the higher the propylene content, the higher the adhesion to the polypropylene substrate tends to be. The olefin polymer (A) is particularly preferably a copolymer having structural units derived from propylene and structural units derived from an olefin other than propylene, in which the mass ratio of the structural units derived from propylene to the structural units derived from an olefin other than propylene is 60 / 40 to 95 / 5.
[0023] The weight average molecular weight (Mw) of the olefin polymer (A) is preferably 5,000 to 500,000 when measured using GPC (Gel Permeation Chromatography) and converted using the calibration curve of each polyolefin. The lower limit is more preferably 10,000, further preferably 20,000, and particularly preferably 30,000. The upper limit is more preferably 300,000. If Mw is 5,000 or more, the stickiness tends to be reduced and the adhesion to the substrate tends to increase. If Mw is 500,000 or less, the viscosity tends to be reduced and the preparation of the aqueous resin dispersion tends to be easier. The GPC measurement is performed by a conventionally known method using a commercially available device with orthodichlorobenzene as a solvent.
[0024] The method for producing the olefin polymer (A) is not particularly limited as long as it is a method capable of producing a polymer that satisfies the requirements of the present invention, and any method may be used. Examples of the method for producing the polymer include radical polymerization, cationic polymerization, anionic polymerization, and coordination polymerization. These methods may be living polymerization methods.
[0025] In the case of coordination polymerization, for example, a method of polymerization using a Ziegler-Natta catalyst or a method of polymerization using a single-site catalyst can be mentioned. A more preferred manufacturing method is a manufacturing method using a single-site catalyst. The reason for this is that single-site catalysts can generally sharpen the molecular weight distribution and stereoregularity distribution by designing the ligand. As single-site catalysts, those having symmetric types such as C1 symmetric type, C2 symmetric type, C2V symmetric type, and CS symmetric type are known. In the present invention, an appropriate metallocene catalyst may be selected and used depending on the stereoregularity of the polyolefin to be polymerized.
[0026] The production method may be any of solution polymerization, slurry polymerization, bulk polymerization, gas phase polymerization, etc. In the case of solution polymerization or slurry polymerization, examples of the solvent include aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as hexane, heptane, and octane, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, halogenated hydrocarbons, esters, ketones, and ethers. Among these, aromatic hydrocarbons, aliphatic hydrocarbons, and alicyclic hydrocarbons are preferred, and toluene, xylene, heptane, and cyclohexane are more preferred. These may be used alone or in combination of two or more.
[0027] The olefin polymer (A) may be linear or branched. Further, the olefin polymer (A) may have a reactive group. Specific examples thereof include a copolymer (Aa) obtained by copolymerizing an olefin with an unsaturated compound having a reactive group during polymerization, and a graft polymer (Ab) obtained by graft polymerizing a radically polymerizable unsaturated compound having a reactive group onto an olefin polymer.
[0028] The copolymer (Aa) is obtained by copolymerizing an olefin with an unsaturated compound having a reactive group, and is a copolymer in which the unsaturated compound having a reactive group is inserted into the main chain. For example, copolymers of α-olefins such as ethylene, propylene, and butene with α,β-unsaturated carboxylic acids or anhydrides such as acrylic acid and maleic anhydride can be mentioned. Specific examples of the copolymer (Aa) include ethylene-acrylic acid copolymers, ethylene-acrylic acid ester-maleic anhydride copolymers, and the like. These may be used alone or in combination of two or more. The copolymer (Aa) can be produced by the same method as that described above for the olefin polymer (A).
[0029] The graft polymer (Ab) is obtained by graft polymerizing an olefin-based polymer with a radical polymerizable unsaturated compound having a reactive group. The copolymer (Aa) can be used as the olefin-based polymer. The graft polymer (Ab) may also be graft polymerized with a radical polymerizable unsaturated compound having a reactive group.
[0030] Examples of the reactive group in the radically polymerizable unsaturated compound having a reactive group include a carboxy group and its anhydride, an amino group, an epoxy group, an isocyanato group, a sulfonyl group, a hydroxyl group, etc. Among these, a carboxy group and its anhydride are preferred. Examples of radically polymerizable unsaturated compounds having a reactive group include (meth)acrylic acid, fumaric acid, maleic acid or its anhydride, itaconic acid or its anhydride, crotonic acid, etc. These may be used alone or in combination of two or more.
[0031] The radical polymerization initiator used in the graft polymerization can be appropriately selected from ordinary radical polymerization initiators, and examples thereof include organic peroxides and azonitriles. Examples of the organic peroxides include peroxyketals such as di(t-butylperoxy)cyclohexane, hydroperoxides such as cumin hydroperoxide, dialkyl peroxides such as di(t-butyl)peroxide, and peroxyesters such as t-butylperoxyisopropyl monocarbonate. Examples of the azonitriles include azobisbutyronitrile and azobisisopropylnitrile. Among these, benzoyl peroxide and t-butylperoxyisopropyl monocarbonate are preferred. These may be used alone or in combination of two or more.
[0032] The ratio of the radical polymerization initiator to the graft copolymerization units of the graft polymer (Ab) is usually within the range of radical polymerization initiator:graft copolymerization units=1:100 to 2:1 (molar ratio), and preferably within the range of 1:20 to 1:1. The reaction temperature for the graft polymerization is usually 50°C or higher, and preferably in the range of 80 to 200°C. The reaction time for the graft polymerization is usually about 2 to 20 hours.
[0033] The method for producing the graft polymer (Ab) is not particularly limited as long as it is a method capable of producing a polymer that satisfies the requirements of the present invention, and any method may be used. Examples of the method for producing the graft polymer (Ab) include a method for producing the polymer by heating and stirring in a solution, a method for producing the polymer by melting and heating and stirring in a solvent-free state, and a method for producing the polymer by heating and kneading in an extruder. As a solvent for producing the polymer in a solution, the solvents exemplified in the method for producing the polymer (A) can be used in the same manner.
[0034] The content of the reactive group in the graft polymer (Ab) is preferably in the range of 0.01 to 1 mmol per 1 g of the graft polymer (Ab). A more preferred lower limit is 0.05 mmol / g, and even more preferred is 0.1 mmol / g. A more preferred upper limit is 0.5 mmol / g, and even more preferred is 0.3 mmol / g. If the content of the reactive group is 0.01 mmol / g or more, hydrophilicity increases, and thus the dispersed particle size tends to become smaller when the aqueous resin dispersion is prepared. In addition, if the content of the reactive group is 1 mmol / g or less, adhesion to a polypropylene substrate tends to increase.
[0035] When the reactive group in the graft polymer (Ab) is an acidic group such as a carboxyl group, its anhydride, or a sulfonyl group, the mechanical stability of the aqueous resin dispersion tends to be improved by neutralizing the acidic group with a basic compound. Examples of the basic compound include inorganic bases such as sodium hydroxide, potassium hydroxide, and ammonia, and organic bases such as triethylamine, diethylamine, ethanolamine, dimethylethanolamine, 2-methyl-2-amino-propanol, triethanolamine, morpholine, and pyridine. The neutralization rate by the basic compound is not particularly limited within the range of 1 to 100 mol% as long as dispersibility in water is obtained, but is preferably 50 mol% or more. If the neutralization rate is low, dispersibility in water tends to decrease.
[0036] In the present invention, the olefin polymer (A) may be used in the form of an aqueous resin dispersion. The method for producing the aqueous resin dispersion is not particularly limited, but examples thereof include a method in which a mixture of the olefin polymer (A), water, and a solvent other than water is prepared, and then the solvent is removed from the mixture to obtain a dispersion, and a method in which the olefin polymer (A) is melted and then water is added to obtain a dispersion.
[0037] The aqueous resin dispersion of the olefin polymer (A) can be prepared by dispersing the olefin polymer (A) by adding a surfactant to the olefin polymer (A), dispersing a graft polymer in which a hydrophilic polymer is bonded to the olefin polymer (A) via a covalent bond, or dispersing the graft polymer (Ab) by neutralizing the acidic group with a basic compound when the reactive group in the graft polymer (Ab) is an acidic group such as a carboxy group or its anhydride, or a sulfonyl group, etc. It is particularly preferable that the olefin polymer (A) and the hydrophilic polymer are bonded to each other via a covalent bond, since this provides excellent storage stability and water resistance.
[0038] (Hydrophilic polymer) In the present invention, the term "hydrophilic polymer" refers to a polymer that has an insoluble content of 1% by mass or less when dissolved in water at a concentration of 10% by mass at 25° C. There are no particular limitations on the hydrophilic polymer that can be used as long as it does not significantly impair the effects of the present invention, and any of synthetic polymers, semi-synthetic polymers, and natural polymers can be used, and they may further have a reactive group.
[0039] As the synthetic polymer, there is no particular limitation, but for example, poly(meth)acrylic resin, polyether resin, polyvinyl alcohol resin, polyvinylpyrrolidone resin, etc. can be used. As the natural polymer, there is no particular limitation, but for example, starches such as corn start wheat starch, sweet potato starch, potato starch, tapioca starch, rice starch, etc., seaweed such as funori, agar, sodium alginate, etc., plant mucilages such as gum arabic, gum tragacanth, konjac, etc., animal proteins such as glue, casein, gelatin, etc., fermented mucilages such as pullulan, dextrin, etc. can be used. As the semi-synthetic polymer, there is no particular limitation, but for example, starches such as carboxyl starch, cationic starch, dextrin, etc., celluloses such as viscose, methyl cellulose, ethyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, etc. can be used. These may be used alone or in combination of two or more.
[0040] Among them, synthetic polymers are preferred because the degree of hydrophilicity is easily controlled and the properties are stable. More preferred are acrylic resins such as poly(meth)acrylic resins, polyvinyl alcohol resins, polyvinylpyrrolidone resins, and polyether resins. Polyether resins, which have high hydrophilicity, are the most preferred. Polyether resins are usually obtained by ring-opening polymerization of cyclic alkylene oxides or cyclic alkyleneimines.
[0041] (Grafted polymer of olefin polymer (A) and hydrophilic polymer) The olefin polymer (A) and the hydrophilic polymer may form a graft polymer. In this case, the method for bonding the olefin polymer (A) and the hydrophilic polymer is not particularly limited, but examples thereof include a method of ring-opening polymerization of a cyclic alkylene oxide in the olefin polymer (A) having a reactive group, and a method of reacting a hydrophilic polymer having a reactive group, such as a polyether polyol or polyether amine obtained by ring-opening polymerization, with the olefin polymer (A) having a reactive group.
[0042] Polyetheramine is a compound having a primary amino group as a reactive group at one or both ends of a resin having a polyether skeleton. Polyetherpolyol is a compound having a hydroxyl group as a reactive group at both ends of a resin having a polyether skeleton. Preferred examples of hydrophilic polyalkylene oxides and polyalkyleneimines include polyethylene oxide, polypropylene oxide, and polyethyleneimine.
[0043] As the polyetheramine, Jeffamine M series, D series, ED series, etc. manufactured by Huntsman may be used. The hydrophilic polymer used in the present invention preferably has one or more reactive groups capable of reacting with the olefin polymer (A) before bonding with the olefin polymer (A). Examples of reactive groups that the hydrophilic polymer has include carboxylic acid groups, dicarboxylic anhydride groups, dicarboxylic anhydride monoester groups, hydroxyl groups, amino groups, glycidyl groups, isocyanate groups, etc., and preferably has at least an amino group. Since the amino group has high reactivity with various reactive groups such as carboxylic acid groups, carboxylic anhydride groups, glycidyl groups, isocyanate groups, etc., it is easy to bond with the olefin polymer (A). The amino group may be any of primary, secondary, and tertiary, but is more preferably a primary amino group.
[0044] The hydrophilic polymer may have one or more reactive groups, but more preferably has only one reactive group. If the hydrophilic polymer has two or more reactive groups, it may form a three-dimensional network structure when bonded to the olefin polymer (A), which may result in gelation. However, even if the hydrophilic polymer has multiple reactive groups, it is sufficient that there is only one reactive group that is more reactive than the others. For example, a hydrophilic polymer having multiple hydroxyl groups and one amino group that is more reactive than the hydroxyl groups is a preferred example. The above "reactivity" refers to reactivity with the reactive group of the olefin polymer (A).
[0045] (Polymer (B) Having a Constituent Derived from a Radical Polymerizable Monomer) The cured coating layer (1) may further contain a polymer (B) having a structural unit derived from a radically polymerizable monomer. From the viewpoint of environmental load, the polymer (B) is also preferably an aqueous resin dispersion. The polymer (A) and the polymer (B) may each be present as separate particles, or the polymer (A) and the polymer (B) may be present in the same particle. From the viewpoint of stability of the aqueous resin dispersion and the appearance of the cured coating layer, the latter is preferred.
[0046] Examples of radically polymerizable monomers used in the polymer (B) include (meth)acrylic acid monomers such as (meth)acrylic acid and (meth)acrylic acid esters, aromatic monomers such as styrene and α-methylstyrene, amide monomers such as (meth)acrylamide and dimethyl(meth)acrylamide, (meth)acrylonitrile, vinyl acetate, vinyl propionate, vinyl versatate, etc. Among these, (meth)acrylic acid monomers and aromatic monomers are preferred from the viewpoints of weather resistance and solvent resistance.
[0047] Specific examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and the like; and compounds having an aryl group or an aralkyl group having 6 to 12 carbon atoms, such as benzyl (meth)acrylate. Meth)acrylic acid esters; dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-aminoethyl (meth)acrylate, glycidyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, adducts of (meth)acrylic acid and polyethylene oxide, and the like; and (meth)acrylic acid esters having an alkyl group having 1 to 20 carbon atoms and a fluorine atom, such as trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, and 2-perfluoroethylethyl (meth)acrylate.
[0048] The polymer (B) preferably contains a structural unit derived from a radically polymerizable monomer having a hydroxyl group. When the cured coating layer (1) contains a polymer (B) having a structural unit derived from at least a radically polymerizable monomer having a hydroxyl group, the cured coating layer (2) can be fixed more effectively and a laminate having particularly excellent optical properties can be obtained.
[0049] Examples of the radically polymerizable monomer having a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 2-hydroxybutyl methacrylate, polypropylene glycol acrylate, and polypropylene glycol methacrylate.
[0050] The method for producing the polymer (B) is not particularly limited, but examples thereof include a method of polymerizing the raw material monomers of the polymer (B) in an aqueous resin dispersion of the olefin polymer (A), a method of dissolving the olefin polymer (A) and the raw material monomers of the polymer (B) to prepare an aqueous resin dispersion, and then polymerizing the resulting mixture, etc. From the viewpoint of the polymerizability of the raw material monomers of the polymer (B), the former method is preferred.
[0051] The ratio of the olefin polymer (A) to the polymer (B) contained in the aqueous resin dispersion (mass ratio of solid contents (A) / (B)) is preferably 0.25 to 4. Within this range, the smaller the ratio, the more stable the aqueous resin dispersion can be produced and the better the storage stability. Also, within the range, the larger the ratio, the better the initial adhesion between the coating film and the polyolefin substrate.
[0052] A surfactant may be added to the aqueous resin dispersion containing the polymer (B) in order to improve storage stability. As the surfactant, various anionic, cationic, or nonionic surfactants, or polymer surfactants can be used. Furthermore, so-called reactive surfactants having an ethylenically unsaturated bond in the surfactant component can also be used. Among these, it is preferable to use an anionic surfactant from the viewpoint of the storage stability of the obtained aqueous resin dispersion. As the anionic surfactant, there is no particular limitation, but for example, Adeka Reasoap SR (trade name, manufactured by ADEKA Corporation), which is a reactive surfactant, or Newcol (registered trademark) 707SF (trade name, manufactured by Nippon Nyukazai Co., Ltd.), which is a non-reactive surfactant, can be used.
[0053] The surfactant is preferably contained in an amount of 3 parts by mass or less, more preferably 2 parts by mass or less, per 100 parts by mass (solid content) of the polymer (B). By making the surfactant content 3 parts by mass or less, the storage stability of the aqueous resin dispersion is improved. In addition, the water resistance is not easily impaired, and the stability can be maintained when used in a coating composition.
[0054] Furthermore, as a method for producing an aqueous resin dispersion containing the polymer (B), bulk polymerization and / or drop polymerization can be used as long as the effect of the present invention is not impaired. Here, bulk polymerization is a method in which the entire amount of monomers is charged at once and polymerized. Drop polymerization is a method in which the monomers are dropped little by little to polymerize. From the viewpoint of polymerization stability and adhesion to a polypropylene substrate, bulk polymerization is preferred. For example, the bulk polymerization can be carried out by mixing an aqueous resin dispersion of an olefin polymer (A) with a radical polymerizable monomer, which is a raw material for the polymer (B), in an amount of 0.25 to 4 times the mass of the olefin polymer (A), and then carrying out radical polymerization with an initiator. For example, the drop polymerization can be carried out by dropping a radical polymerizable monomer, which is a raw material for the polymer (B), into the olefin polymer (A) under radical polymerization.
[0055] As the initiator used in the polymerization reaction, those generally used in radical polymerization can be used. Specific examples include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate; oil-soluble azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile; 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis{2-methyl-N-[2-(1-hydroxyethyl)]propionamide}, and 2,2'-azobis{2-methyl-N-[2-(1-hydroxybutyl)]propionamide}. water-soluble azo compounds such as 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] and its salts; 2,2'-azobis[2-(2-imidazolin-2-yl)propane] and its salts; 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} and its salts; 2,2'-azobis(2-methylpropynamidine) and its salts; 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]; and organic peroxides such as benzoyl peroxide, cumene hydroperoxide, t-butyl hydroperoxide, t-butyl peroxy-2-ethylhexanoate, and t-butyl peroxyisobutyrate. These initiators may be used alone or in combination of two or more.
[0056] In the present invention, a reducing agent may be further added to carry out a redox polymerization reaction. Preferred radical polymerization methods are a method of carrying out polymerization using a water-soluble initiator, or a method of carrying out polymerization by a redox reaction using an organic peroxide as an initiator and ferrous sulfate, isoascorbic acid, or the like as a reducing agent.
[0057] When carrying out the polymerization reaction, known chain transfer agents such as n-dodecyl mercaptan, t-dodecyl mercaptan, α-methylstyrene dimer, etc. can be used as a molecular weight regulator.
[0058] After the polymerization reaction is completed, when the aqueous resin dispersion is cooled and taken out, it is preferable to carry out a filtration operation in order to prevent foreign matter or cullet from being mixed in. As the filtration method, a known method can be used, and for example, a nylon mesh, a bag filter, filter paper, a metal mesh, etc. can be used.
[0059] The particle structure of aqueous resin dispersions can be observed using a transmission electron microscope after ultrathin sections prepared by a general gel embedding method or after a sample is diluted, dropped onto a grid, dried, and stained with RuO.
[0060] The aqueous resin dispersion is preferably further blended with various additives to form an aqueous coating composition, such as various pigments, resin beads, defoamers, pigment dispersants, leveling agents, UV absorbers, light stabilizers, antioxidants, heat resistance improvers, slip agents, preservatives, thickeners, wetting agents, and solvents, and one or more of these additives may be used.
[0061] The aqueous coating composition may further contain, as components other than the olefin polymer (A), hydrophilic polymer, and polymer (B), other polymer particles (for example, dispersed particles made of other polymers such as polyester resins, polyurethane resins, acrylic silicone resins, silicone resins, fluorine resins, epoxy resins, alkyd resins, etc.), water-soluble resins, viscosity control agents, amino resins, polyisocyanate compounds, blocked polyisocyanate compounds, melamine resins, urea resins, carboxy group-containing compounds, carboxy group-containing resins, epoxy group-containing resins, epoxy group-containing compounds, carbodiimide group-containing compounds, and other curing agents.
[0062] [Cured coating layer (2)] The cured coating layer (2) contains a cationic organosilane quaternary ammonium salt. The cationic organosilane quaternary ammonium salt is an antibacterial component.
[0063] (Cationic organic silane quaternary ammonium salt) The cationic organosilane quaternary ammonium salt has an ammonium group having a long-chain alkyl group that exhibits antibacterial properties, and an alkoxysilyl group or a hydroxysilyl group that can form a covalent bond with the surface of the cured coating layer (1). As the organosilane quaternary ammonium salt, a silicon-containing compound represented by the following general formula (1) is preferred.
[0064] [ka]
[0065] (In the formula, R 1 represents a long-chain alkyl group having 12 to 24 carbon atoms, and R 2 and R 3 each independently represents an alkyl group having 1 to 6 carbon atoms; - represents a halogen ion or an organic carbonyloxy ion, and R 4 , R 5 , R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0066] R in formula (1) 1 The long-chain alkyl group having 12 to 24 carbon atoms is not particularly limited, and examples thereof include a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, an eicosyl group, a heniicosyl group, a docosyl group, a tricosyl group, and a tetracosyl group.
[0067] R in formula (1) 2 and R 3 Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, and a cyclohexyl group.
[0068] Specific examples of the silicon-containing compound represented by formula (1) include octadecyldimethyl(3-trialkoxysilylpropyl)ammonium chloride, dodecyldimethyl(3-trialkoxysilylpropyl)ammonium chloride, dodecyldiisopropyl(3-trialkoxysilylpropyl)ammonium chloride, tetradecyldimethyl(3-trialkoxysilylpropyl)ammonium chloride, tetradecyldiethyl(3-trialkoxysilylpropyl)ammonium chloride, tetradecyldi-n-propyl(3-trialkoxysilylpropyl)ammonium chloride, pentadecyldimethyl(3-trialkoxysilylpropyl)ammonium chloride, pentadecyldiethyl(3-trialkoxysilylpropyl)ammonium chloride, pentadecyldi-n-propyl(3-trialkoxysilylpropyl)ammonium chloride, hexadecyldimethyl(3-trialkoxysilylpropyl)ammonium chloride, hexadecyldiethyl(3-trialkoxysilylpropyl)ammonium chloride, hexadecyldi-n-propyl(3-trialkoxysilylpropyl)ammonium chloride, propyl(3-trialkoxysilylpropyl)ammonium chloride, octadecyl diethyl(3-trialkoxysilylpropyl)ammonium chloride, octadecyl di-n-propyl(3-trialkoxysilylpropyl)ammonium chloride, octadecyl dimethyl(3-trihydroxysilylpropyl)ammonium chloride, dodecyl dimethyl(3-trihydroxysilylpropyl)ammonium chloride, dodecyl diisopropyl(3-trihydroxysilylpropyl)ammonium chloride, tetradecyl dimethyl(3-trihydroxysilylpropyl)ammonium chloride, tetradecyl diethyl(3-trihydroxysilylpropyl)ammonium chloride, tetradecyl di-n-propyl(3-trihydroxysilylpropyl)ammonium chloride, pentadecyl dimethyl(3-trihydroxysilylpropyl)ammonium chloride, pentadecyl diethyl(3-trihydroxysilylpropyl)ammonium chloride, pentadecyl di-n-propyl(3-trihydroxysilylpropyl)ammonium chloride,Examples of suitable ammonium chloride include hexadecyldimethyl(3-trihydroxysilylpropyl)ammonium chloride, hexadecyldiethyl(3-trihydroxysilylpropyl)ammonium chloride, hexadecyldi-n-propyl(3-trihydroxysilylpropyl)ammonium chloride, octadecyldiethyl(3-trihydroxysilylpropyl)ammonium chloride, and octadecyldi-n-propyl(3-trihydroxysilylpropyl)ammonium chloride. Among these, octadecyldimethyl(3-trialkoxysilylpropyl)ammonium chloride and octadecyldimethyl(3-trihydroxysilylpropyl)ammonium chloride are preferred, as they are less biotoxic and impose less of a burden on the environment during use and waste liquid.
[0069] The antibacterial agent used in the cured coating layer (2) may be one or more types of cationic organosilane quaternary ammonium salts, and may also be used in combination with other antibacterial agents. Cationic organosilane quaternary ammonium salts have antibacterial effects against gram-positive and gram-negative bacteria, and antiviral effects against enveloped viruses such as influenza virus, measles virus, and coronavirus (antibacterial effect and antiviral effect are collectively referred to as antibacterial effect). In addition to the antibacterial effect, they are also thought to have antistatic and deodorizing effects at the same time.
[0070] The cationic organic silane quaternary ammonium salt may be dissolved in water, alcohol, or an organic solvent to adjust the viscosity to be easily applied. In addition to the solvent, various additives may be further included as long as the effect of the present invention is not impaired. Examples of additives include various pigments, resin beads, defoamers, pigment dispersants, leveling agents, ultraviolet absorbers, light stabilizers, antioxidants, heat resistance improvers, slip agents, preservatives, thickeners, wetting agents, and solvents, and one or more of these may be used. In addition, catalysts such as acids, bases, metal alkoxides, and metal chelates may be used in combination to promote the reaction.
[0071] [Laminate] The laminate of the present invention has the above-mentioned cured coating layer (1) and cured coating layer (2). In order to fix the cured coating layer (2), the cured coating layer (1) and the cured coating layer (2) are laminated in that order, and it is preferable that the cured coating layer (2) is located on the outermost surface in order to exhibit antibacterial properties.
[0072] The cured coating layer (1) is preferably applied onto a substrate containing a polyolefin resin. Although polyolefin resin is generally a poorly adherent material, the presence of the cured coating layer (1) makes it possible to fix the cured coating layer (2) onto the substrate containing the polyolefin resin. Specific examples of the polyolefin resin contained in the substrate include polypropylene, polyethylene, cycloolefin polymer, etc. The present invention is particularly suitable for substrates containing polypropylene. The substrate may be in the form of a film or sheet, an injection molded body, or a fiber substrate. The cured coating layer (1) in the present invention has strong adhesion to polypropylene and is highly transparent, so a biaxially oriented polypropylene substrate is preferred, and a biaxially oriented polypropylene (OPP) film is particularly suitable.
[0073] The surface of the substrate containing the polyolefin resin may be modified by corona treatment, plasma treatment, flame treatment or the like for the purpose of improving the wettability and adhesion of the topcoat layer.
[0074] The cured coating layer (1) and the cured coating layer (2) can be formed by a conventional coating method. Specific examples include gravure and microgravure methods, slot die methods, knife coating, gap coating, curtain coating, spray coating, brush coating, dip coating, roll coating, etc. In addition, the step of laminating the aqueous resin dispersion and the antibacterial component may be performed by sequentially coating and drying the layers, or by simultaneously coating and laminating the layers using a multilayer slot die or a multilayer curtain coater, etc.
[0075] The thickness of the cured coating layer (1) is preferably 0.1 to 30 μm, more preferably 0.1 to 20 μm, and even more preferably 1 to 15 μm. If the thickness of the cured coating layer (1) is 0.1 μm or more, the variation in thickness is small, and the cured coating layer (2) can be easily fixed. If the thickness of the cured coating layer (1) is 30 μm or less, it can be dried in a shorter time, which is economically advantageous. The drying temperature when forming the cured coating layer (1) is preferably 60° C. or higher. If the temperature is 60° C. or higher, drying can be completed in a short time. There is no particular upper limit, but it is preferable to dry within a range that does not exceed the heat resistance temperature of the substrate.
[0076] The thickness of the cured coating layer (2) is preferably 0.01 to 1 μm. During the coating and drying process, the antibacterial component undergoes hydrolysis and dehydration condensation, causing the coating to shrink, but if the thickness is 0.01 μm or more, it is easy to form a uniform cured coating layer (2). On the other hand, if the thickness of the cured coating layer (2) is 1 μm or less, it is economically advantageous. The drying temperature when forming the cured coating layer (2) is preferably 60°C or higher. If it is 60°C or higher, drying can be completed in a short time. In order to promote the hydrolysis reaction and dehydration condensation reaction of the antibacterial component, it is more preferably 90°C or higher, and even more preferably 120°C or higher. There is no particular upper limit, but it is preferable to dry within a range that does not exceed the heat resistance temperature of the substrate or the decomposition temperature of the antibacterial component.
[0077] The laminate obtained by the present invention can be used for flexible packaging materials, home appliances such as air conditioners, refrigerators, and washing machines, toilets, kitchen sinks, bathroom fixtures, and automobile interiors. EXAMPLES
[0078] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples, "parts" refers to "parts by mass." Evaluations were performed by the methods shown below.
[0079] [Physical property measurement and evaluation methods] (1) Method for measuring weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of olefin polymer (A) 5 mg of a sample of olefin polymer (A) was collected in a 10 mL vial, and 5 g of tetrahydrofuran containing 250 mass ppm of dibutylhydroxytoluene as a stabilizer was added, and completely dissolved at 50 ° C. After cooling to room temperature, the mixture was filtered through a filter with a pore size of 0.45 μm to prepare a sample solution with a polymer concentration of 0.1 mass %. Next, GPC measurement was performed using a GPC HLC-8020 manufactured by Tosoh Corporation, which was equipped with a guard column TSKguardcolumnHXL-H on a TSKgel GMHXL-L (30 cm × 2 columns) as a column. The measurement conditions were as follows: injection amount of sample solution: 50 μL, column temperature: 40 ° C, solvent: tetrahydrofuran, and flow rate: 1.0 mL / min. A commercially available monodisperse polystyrene standard sample was measured as a standard sample, and a calibration curve was prepared from the retention time and molecular weight of the standard sample to calculate the weight average molecular weight [Mw] and molecular weight distribution [Mw / Mn] of the olefin polymer (A).
[0080] (2) Method for measuring melting point (Tm) of olefin polymer (A) The measurement was performed using a differential scanning calorimeter (DSC 220C) manufactured by Seiko Instruments Inc. 5±1 mg of a sample of the olefin polymer (A) was placed in an aluminum pan and covered with an aluminum lid, and an empty aluminum pan was placed on the detector as a reference. The temperature was raised to 200°C at a rate of 100°C / min. After holding at 200°C for 5 minutes, the temperature was cooled at a rate of 10°C / min, and the amount of heat was detected at 0.5 second intervals to -10°C. After holding at -10°C for 1 minute, the temperature was raised to 200°C at a rate of 10°C / min, and the amount of heat was detected at 0.5 second intervals. For each sample, one exothermic peak was observed during the cooling process, and one endothermic peak was observed during the final heating process. The peak top temperature during the final heating process was determined as the melting point (°C) of the olefin polymer (A).
[0081] (3) Method for measuring the average particle size (d) of aqueous resin dispersions The aqueous resin dispersion was diluted to 1% by mass with deionized water, and the average particle size (nm) was determined by the cumulant method using a concentrated particle size analyzer (FPAR-1000, manufactured by Otsuka Electronics Co., Ltd.).
[0082] (4) Optical property evaluation Using a spectroscopic haze meter (SH 7000, manufactured by Nippon Denshoku Industries Co., Ltd.), the total light transmittance (Tt) and haze of the laminates described in Examples 1 to 3 and Comparative Examples 1 and 2 were measured. The results are shown in Table 1.
[0083] (5)BPB color reaction The presence or absence of the antibacterial component remaining after the durability test was confirmed by the color reaction of bromophenol blue (BPB) with quaternary ammonium cations. Several 5 cm square test pieces were cut out from the laminates (processed samples) prepared in the examples and comparative examples. Some of the test pieces were subjected to the water resistance test shown below. (Water resistance test) Water resistance treatment category 1: Immerse in room temperature water for 16 hours Water resistance treatment category 2: Immerse in hot water at 50℃±5℃ for 16 hours
[0084] Test pieces that had not been subjected to the water resistance test and test pieces that had been subjected to the water resistance test (water resistance treatment category 1 or 2) were fixed with tape in a container and immersed in a 1% by mass BPB aqueous solution for 20 minutes. Bromophenol blue was used as a reagent express grade manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. After the color reaction, the test pieces were washed three times with a large amount of deionized water and dried. The degree of coloration before and after the water resistance test was visually confirmed and evaluated according to the following criteria. (Evaluation Criteria) ++: Almost no change in color between samples before and after durability test +: The color of the sample after the durability test is lighter than before the durability test. -: Almost no color change in samples after durability test
[0085] (6) Antibacterial evaluation The antibacterial properties of the antibacterial laminate were evaluated according to the following procedure based on JIS Z 2801:2012 (film adhesion method). Escherichia coli (E. Coli NBRC 3972) was used as the test strain. As in the above "(5) BPB color reaction", multiple test pieces were prepared from the laminates (processed samples) prepared in the examples and comparative examples, and some of the test pieces were subjected to the water resistance test or light resistance test shown below. (Water resistance test) Water resistance treatment category 1: Immerse in room temperature water for 16 hours Water resistance treatment category 2: Immerse in hot water at 50℃±5℃ for 16 hours (Light resistance test) Light resistance treatment category 1: Xenon arc lamp 10 hours
[0086] A test piece that had not been tested (untreated) and test pieces that had been tested were placed in separate petri dishes, and 0.4 mL of the test bacteria liquid was dropped onto the test piece (5 cm x 5 cm) in each petri dish, and the test piece was covered with a film (4 cm x 4 cm), and the petri dish was then covered with a lid. Each petri dish was cultured for 24 hours at 35°C and 90% RH or higher. After the culture, 10 mL of SCDLP medium was added to wash out the test bacteria attached to the film and test piece. The number of bacteria in the washed out solution was measured using the agar plate culture method. The same procedure was performed on test pieces made from untreated samples (OPP film) to measure the number of bacteria, and the antibacterial activity values were calculated according to the following formula for the untreated test pieces, the test pieces after the water resistance test (water resistance treatment category 1 or 2), and the test pieces after the light resistance test. Antibacterial activity value = logN A -logN B In the above formula, the symbols have the following meanings. N A : Unprocessed sample 1cm 2 Number of live bacteria per culture N B : Processed sample 1cm 2 Number of live bacteria per culture The antibacterial evaluation was performed with n=3, and the average value was taken as the antibacterial activity value. In addition, when the antibacterial activity value was 2.0 or more, it was evaluated as having antibacterial properties.
[0087] [Production Example 1: Production of Olefin Polymer (A) (Acid-Modified Polyolefin Resin)] 200 kg of "Tafmer (registered trademark) XM-7070" (manufactured by Mitsui Chemicals, Inc., melting point 75°C, propylene content 74 mol%, weight average molecular weight [Mw] 250,000, molecular weight distribution [Mw / Mn] 2.2), a propylene-butene copolymer polymerized by a metallocene catalyst, and 5 kg of maleic anhydride were dry-blended in a super mixer. Thereafter, using a twin-screw extruder (manufactured by Nippon Seiko Co., Ltd., "TEX54αII"), t-butylperoxyisopropyl monocarbonate (manufactured by Nippon Oil & Fats Co., Ltd., "Perbutyl I") was fed in the middle with a liquid addition pump so that 1 part per 100 parts of the propylene-butene copolymer was obtained, and the mixture was kneaded under the conditions of a cylinder temperature of 200°C in the kneading section, a screw rotation speed of 125 rpm, and a discharge rate of 80 kg / hour, to obtain a pellet-shaped maleic anhydride-modified propylene-butene copolymer. The content (graft ratio) of maleic anhydride groups in the obtained maleic anhydride-modified propylene-butene copolymer was 1% by mass. The weight average molecular weight (polystyrene equivalent) [Mw] was 160,000, and the number average molecular weight [Mn] was 80,000.
[0088] [Production Example 2: Production of a graft polymer by grafting a hydrophilic polymer onto an olefin polymer (A)] In a glass flask equipped with a reflux condenser, a thermometer, and a stirrer, 40 g of propylene-butene copolymer "Tafmer (registered trademark) XM-7070" and 60 g of the maleic anhydride-modified propylene-butene copolymer obtained in Production Example 1 were dissolved in 66.6 g of toluene, and the inside of the container was replaced with nitrogen gas. The inside of the flask was heated to 90°C, 1.5 g of maleic anhydride was added, and the temperature was raised to 110°C. 0.75 g of t-butylperoxyisopropyl monocarbonate ("Perbutyl I" manufactured by NOF Corporation) was added, reacted for 7 hours, and further modified with maleic anhydride. Then, 71.4 g of toluene was added. The temperature inside the flask was set to 70°C, and a solution in which 20 g of methoxypoly(oxyethylene / oxypropylene)-2-propylamine "Jeffamine M-2005: manufactured by Huntsman" was dissolved in 130 g of 2-propanol was dropped into the flask over 1 hour, and the reaction was continued for another 1.5 hours. Then, 10 g of methoxypoly(oxyethylene / oxypropylene)-2-propylamine "Jeffamine M-1000: manufactured by Huntsman" was dissolved in 70 g of 2-propanol, and the solution was dropped over 1 hour. Then, the reaction was continued for another 1 hour. 1.5 g of dimethylethanolamine was dissolved in 62 g of deionized water and 45 g of 2-propanol, dropped into the flask, and stirred at 70°C for 30 minutes. The temperature of the obtained reaction liquid was kept at 50°C, heated and stirred, and deionized water was added dropwise while the degree of vacuum in the system was reduced to remove toluene and 2-propanol under reduced pressure. When the amount of distillate reached 500 g, the reduction in pressure was stopped to obtain a milky white aqueous resin dispersion. The average particle size of the obtained aqueous resin dispersion (solid content concentration 30% by mass) was 90 nm.
[0089] [Production Example 3: Production of aqueous resin dispersion containing olefin polymer (A) and polymer (B)] A flask equipped with a stirrer, a reflux condenser, and a temperature controller was charged with 222.2 parts of the aqueous resin dispersion obtained in Production Example 2, 118.8 parts of deionized water, and 3.3 parts of Newcol 707SF (trade name, Nippon Nyukazai Co., Ltd.: solid content 30 mass %) as a surfactant, and nitrogen was passed through at 40 mL / min, and the temperature was raised to 55°C. 6.7 parts of Newcol 707SF were added to 40 parts of deionized water, and then 38 parts of 2-ethylhexyl acrylate (manufactured by Mitsubishi Chemical Corporation), 52 parts of isobutyl methacrylate (manufactured by Mitsubishi Chemical Corporation), and 10 parts of 4-hydroxybutyl acrylate (manufactured by Mitsubishi Chemical Corporation) were added as radical polymerizable monomers. The mixture was then stirred at about 2000 rpm using a homogenizer MARKII to emulsify the radical polymerizable monomers. The emulsified radical polymerizable monomer was put into a flask, heated to 55° C., and then held for 1 hour with stirring. Further, 0.1 part of Perbutyl (registered trademark) H69 (trade name, NOF Corp., solid content 69 mass%) as an initiator, 0.0002 parts of ferrous sulfate as a reducing agent, 0.00027 parts of ethylenediaminetetraacetic acid (EDTA), 0.08 parts of sodium isoascorbate monohydrate, and 1 part of deionized water were added dropwise over 30 minutes to initiate polymerization. After the dropwise addition, the temperature was raised to 70°C, 0.1 parts of Perbutyl H69, 2 parts of deionized water, 0.04 parts of sodium isoascorbate monohydrate, and 2 parts of deionized water were added, and the mixture was aged for 60 minutes. After aging, the heating was stopped and the mixture was cooled to room temperature. The average particle size of the obtained aqueous resin dispersion (solid content concentration 30% by mass) was 90 nm.
[0090] [Example 1] The aqueous resin dispersion obtained in Production Example 2 was applied to an OPP film (Pylen P2108, Toyobo Co., Ltd.) using a bar coater #22, and dried for 5 minutes in a hot air dryer set at 100°C. At this time, the dry film thickness was 10 μm. As an antibacterial component, Biosafe HE4005 Antimicrobial (3-(Trihydroxysilyl)propyldimethyloctadecylammonium chloride: 5 mass% aqueous solution, Gelest, Inc.) diluted to 1 mass% with isopropanol (IPA) was applied to the coating film coated with the aqueous resin dispersion of Production Example 2 using a bar coater #9, and dried for 5 minutes in a hot air dryer set at 130°C to obtain a laminate.
[0091] [Example 2] A laminate was obtained in the same manner as in Example 1, except that a #22 bar coater was used when applying the antibacterial component.
[0092] [Example 3] A laminate was obtained in the same manner as in Example 2, except that the aqueous resin dispersion obtained in Production Example 3 was applied onto the OPP film instead of Production Example 2.
[0093] [Comparative Example 1] A laminate was obtained in the same manner as in Example 1, except that the antibacterial component was directly applied onto the OPP film.
[0094] [Comparative Example 2] A laminate was obtained in the same manner as in Example 2, except that the antibacterial component was directly applied onto the OPP film.
[0095] [Table 1]
[0096] The laminates of Examples 1 to 3 in which the cured coating layer (1) and the cured coating layer (2) were laminated had superior antibacterial activity compared to the laminates of Comparative Examples 1 and 2 in which the cured coating layer (1) was not included, and the antibacterial activity was maintained even after the water resistance test and the light resistance test.
Claims
1. A laminate comprising a cured coating layer (1) containing an olefin polymer (A) and a cured coating layer (2) containing a cationic organosilane quaternary ammonium salt.
2. The laminate according to claim 1, wherein the olefin-based polymer (A) has a structural unit derived from propylene and a structural unit derived from an olefin other than propylene, and a mass ratio of the structural unit derived from propylene to the structural unit derived from an olefin other than propylene is 60 / 40 to 95 / 5.
3. The laminate according to claim 1 or 2, wherein the cured coating layer (1) comprises a hydrophilic polymer.
4. 3. The laminate according to claim 1, wherein the cured coating layer (1) comprises a graft polymer in which a hydrophilic polymer is grafted onto the olefin polymer (A).
5. The laminate according to claim 1 or 2, wherein the cured coating layer (1) comprises a polymer (B) having a structural unit derived from a radically polymerizable monomer.
6. The laminate according to claim 5 , wherein the polymer (B) has a structural unit derived from a radically polymerizable monomer having a hydroxyl group.
7. 3. The laminate according to claim 1 or 2, wherein the cured coating layer (1) and the cured coating layer (2) are provided in this order on a polyolefin substrate.
8. 8. The laminate of claim 7, wherein the polyolefin substrate is a biaxially oriented polypropylene substrate.
Citation Information
Patent Citations
Coating agent, coating agent set, and water-related member
JP2017160311A
Article comprising immobilized antibacterial agent and method for producing same
WO2013047642A1
Cited By
Antibacterial modified cycloolefin polymer, preparation method thereof and cycloolefin polymer antibacterial modified film
CN121426998A