Thermoplastic elastomer composition
A thermoplastic elastomer composition with styrenic thermoplastic elastomer, propylene polymer, and isobutylene crosslinked thermoplastic elastomer addresses the shortcomings of existing compositions by providing superior leakage resistance and needle retention, suitable for medical applications.
Patent Information
- Application Number
- JP2023043251
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermoplastic elastomer compositions used in medical applications, such as rubber stoppers, lack both sufficient needle retention properties and liquid leakage resistance, failing to meet the performance standards of conventional vulcanized rubber.
A thermoplastic elastomer composition comprising styrenic thermoplastic elastomer, propylene polymer, mineral oil-based rubber softener, and isobutylene crosslinked thermoplastic elastomer, with specific proportions and properties, to enhance both leakage resistance and needle retention.
The composition achieves excellent leakage resistance and needle retention, making it suitable for medical rubber stoppers and other applications requiring similar properties.
Smart Images

Figure 2024132477000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic elastomer composition. The present invention also relates to a molded article and a sealing material made of the thermoplastic elastomer composition, and to an article using the thermoplastic elastomer composition. [Background technology]
[0002] In recent years, thermoplastic elastomers, which are soft materials having rubber elasticity, do not require a vulcanization process, and are moldable and recyclable similar to thermoplastic resins, have been used in a wide variety of industrial fields, such as automobile parts, medical parts, etc. In particular, for medical parts, where hygiene is essential, thermoplastic elastomers that do not contain vulcanizing agents or vulcanization accelerators are widely used as a substitute for vulcanized rubber.
[0003] In order to improve such thermoplastic elastomer compositions, aiming at a compression set equivalent to that of vulcanized rubber and liquid leakage resistance when made into stoppers such as cap liners, packings, and rubber stoppers, a styrene-based thermoplastic elastomer composition containing a modified polypropylene resin having a specific structure, a styrene-based thermoplastic elastomer having a specific molecular weight distribution, and a hydrocarbon-based rubber softener has been proposed (see Patent Document 1). Also, focusing on a crosslinked product of an isobutylene polymer having a reactive group, a composite elastomer composition for use in a medical container plug containing this in a relatively small proportion has been proposed (see Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2023 / 022028 [Patent Document 2] JP 2010-227285 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, according to detailed studies by the present inventors, the thermoplastic elastomer composition described in Patent Document 1 above is still insufficient in terms of the liquid leakage properties and needle retention properties required for medical rubber stoppers, as shown in Comparative Example 2 below, and does not reach the performance level required for conventional vulcanized rubber. As shown in Comparative Example 1 below, the elastomer composition described in Patent Document 2 also still lacks the needle retention properties required for medical rubber stoppers, and does not reach the performance level required for conventional vulcanized rubber.
[0006] The present invention has been made in consideration of the above-mentioned problems in the prior art. That is, an object of the present invention is to provide a thermoplastic elastomer composition which combines excellent leakage resistance and needle retention properties and is suitable as a molding material for medical rubber stoppers and the like, and to provide a molded body, a sealing material, and an article which use this thermoplastic elastomer composition. [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above problems, the inventors have found that an elastomer composition containing a styrene-based thermoplastic elastomer, a propylene-based polymer, a mineral oil-based or rubber softener having a specific kinetic viscosity, and an isobutylene-based crosslinked thermoplastic elastomer in specific ratios can achieve both excellent leakage resistance and needle retention properties, thereby solving the conventional problems. That is, the present invention relates to the following.
[0008] [1] A thermoplastic elastomer composition comprising the following components (A) to (D), wherein the content of component (D) in the total of components (A) to (D) is 35 mass% or more and 80 mass% or less, and component (C) is a mineral oil-based rubber softener: Component (A): Styrene-based thermoplastic elastomer Component (B): Propylene-based polymer Component (C): Rubber softener Component (D): Isobutylene-based crosslinked thermoplastic elastomer
[0009] [2] A thermoplastic elastomer composition comprising the following components (A) to (D), wherein the content of component (D) in the total of components (A) to (D) is 35% by mass or more and 80% by mass or less, and component (C) has a kinematic viscosity at 40°C of 20 cSt or more and 600 cSt or less: Component (A): Styrene-based thermoplastic elastomer Component (B): Propylene-based polymer Component (C): Rubber softener Component (D): Isobutylene-based crosslinked thermoplastic elastomer
[0010] [3] The thermoplastic elastomer composition according to [1] or [2], having a compression set of 30% or less.
[0011] [4] The thermoplastic elastomer composition according to any one of [1] to [3], having a melt flow rate (230°C, load 49 N) of 0.1 g / 10 min or more and 200 g / 10 min or less.
[0012] [5] The thermoplastic elastomer composition according to any one of [1] to [4], having a Duro hardness A of 10 or more and 55 or less.
[0013] [6] The thermoplastic elastomer composition according to any one of [1] to [5], which is used for a rubber stopper having a needle piercing portion.
[0014] [7] A molded article made of the thermoplastic elastomer composition according to any one of [1] to [6].
[0015] [8] A sealing material comprising the thermoplastic elastomer composition according to any one of [1] to [6].
[0016] [9] The sealing material according to [8], which is a rubber stopper.
[0017]
[10] The sealing material described in [9], wherein the rubber stopper is a rubber stopper having a needle puncture portion.
[0018]
[11] An article comprising a rubber stopper made of the thermoplastic elastomer composition according to any one of [1] to [6].
[0019]
[12] The article according to
[11] , which is a vial.
[0020]
[13] The article described in
[11] , which is an infusion bag.
[0021]
[14] The article described in
[11] , which is a vacuum blood collection tube. Effect of the Invention
[0022] The thermoplastic elastomer composition of the present invention has both excellent liquid leakage resistance and needle retention properties. Therefore, the thermoplastic elastomer composition of the present invention provides a molded article that has both excellent liquid leakage resistance and needle retention properties. The molded article of the present invention can be suitably used for rubber stoppers that require resistance to liquid leakage and needle retention, such as rubber stoppers for vials that can be pierced by medical needles, rubber stoppers for infusion bags, and rubber stoppers for vacuum blood collection tubes. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 shows an example of an embodiment of a rubber stopper having a needle piercing portion, where (a) is a plan view and (b) is a cross-sectional view taken along line BB in (a). [Diagram 2] FIG. 2 shows another embodiment of a rubber stopper having a needle piercing portion, where (a) is a plan view and (b) is a cross-sectional view taken along line BB in (a). [Diagram 3] FIG. 3 shows another embodiment of a rubber stopper having a needle piercing portion, where (a) is a plan view and (b) is a cross-sectional view taken along line BB in (a). [Figure 4] FIG. 4 shows yet another embodiment of a rubber stopper having a needle piercing portion, where (a) is a plan view and (b) is a cross-sectional view taken along line BB in (a). [Diagram 5]FIG. 5 shows yet another embodiment of a rubber stopper having a needle piercing portion, where (a) is a plan view and (b) is a cross-sectional view taken along line BB in (a). [Figure 6] FIG. 1 is an explanatory diagram showing the evaluation methods for leakage resistance, needle retention time, and operability in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. The following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not exceed the gist of the present invention. The present invention can be modified in any way as long as it does not deviate from the gist of the present invention. In the present invention, when "~" is used to express a numerical value or a physical property value, the values before and after the "~" are included.
[0025] [Thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention comprises the following components (A) to (D), and is characterized in that the content of component (D) in the total of components (A) to (D) is 35 mass % or more and 80 mass % or less. Component (A): Styrene-based thermoplastic elastomer Component (B): Propylene-based polymer Component (C): A rubber softener that satisfies the following requirement (i) or (ii): (i): A mineral oil-based rubber softener. (ii) The kinematic viscosity at 40°C is 20 cSt or more and 60 cSt or less. Component (D): Isobutylene-based crosslinked thermoplastic elastomer The rubber softener of component (C) may satisfy either one of the above requirements (i) and (ii), or may satisfy both. However, in order to more effectively obtain the effects of the present invention, it is preferable that the softener satisfies both requirements (i) and (ii).
[0026] <Mechanism> The thermoplastic elastomer composition of the present invention contains the above-mentioned components (A), (B), and (C) and a predetermined amount of component (D), and thus achieves both excellent leakage resistance and needle retention properties. The mechanism by which the thermoplastic elastomer composition of the present invention exerts such effects is considered to be as follows. The styrene-based thermoplastic elastomer of component (A) imparts rubber elasticity to the thermoplastic elastomer composition, making it possible to obtain a molded article with excellent operability that allows easy insertion and removal of a needle. The propylene polymer of component (B) makes it possible to obtain a thermoplastic elastomer composition having excellent moldability. In addition, component (C) can provide the thermoplastic elastomer composition with appropriate flexibility and moldability. In addition, the rubber softener is mineral oil-based or has a specific kinetic viscosity, so that a molded product with particularly excellent liquid leakage properties can be obtained. This is presumably because the mineral oil-based or specific kinetic viscosity prevents the molded product from becoming excessively sticky, and the hole closes quickly after the needle is removed, preventing liquid leakage. It is believed that the crosslinked structure contained in the isobutylene-based crosslinked thermoplastic elastomer of component (D) reduces the compression set of the thermoplastic elastomer composition, and is effective in improving the liquid leakage properties. In addition, the crosslinked structure of component (D) increases the holding power when a needle is inserted, and improves the needle retention properties. In addition, by including component (D) in the above specific ratio, it is believed that the sufficient distribution of component (D) within the thermoplastic elastomer composition can provide sufficient and stable effects on the liquid leakage properties and needle retention properties.
[0027] <Component (A): Styrene-based thermoplastic elastomer> The styrene-based thermoplastic elastomer of component (A) is not particularly limited, and may be a block copolymer selected from the group consisting of a block copolymer having at least one polymer block P derived from a vinyl aromatic compound and at least one polymer block Q derived from a conjugated diene, and a block copolymer obtained by hydrogenating the block copolymer (hydrogenated block copolymer).
[0028] The polymer block P is a polymer block of a monomer mainly composed of a vinyl aromatic compound, while the polymer block Q is a polymer block of a monomer mainly composed of a conjugated diene. Here, "mainly composed of" means that the content in the block is 50 mol % or more.
[0029] The vinyl aromatic compound as a monomer constituting the polymer block P is not limited, but is preferably a styrene derivative such as styrene, α-methylstyrene, or chloromethylstyrene. Of these, it is preferable to use styrene as the main component. These may be used alone or in combination of two or more. The polymer block P may contain a monomer other than the vinyl aromatic compound as a raw material.
[0030] The monomer constituting the polymer block Q is not limited, but preferably includes butadiene alone, isoprene alone, a mixture of butadiene and isoprene, etc. These may be used alone or in combination of two or more. Note that the polymer block Q may contain monomers other than butadiene and isoprene as raw materials.
[0031] Furthermore, the polymer block Q may be a hydrogenated derivative in which the double bonds contained therein are hydrogenated after polymerization, i.e., a hydrogenated block copolymer. The hydrogenation rate of the polymer block Q is not limited, but is preferably 50 to 100% by mass, and more preferably 80 to 100% by mass. By hydrogenating the polymer block Q within the above range, the thermal stability and weather resistance stability tend to be improved. The same applies to the case in which the polymer block P is made using a diene component as a raw material. The hydrogenation rate is, 13 It can be measured by C-NMR.
[0032] The styrene-based thermoplastic elastomer preferably has a styrene unit content of 8 to 45% by mass. When the styrene unit content of the styrene-based thermoplastic elastomer is equal to or higher than the lower limit, bleeding out of the rubber softener of component (C) from the thermoplastic elastomer composition can be effectively suppressed. On the other hand, when the styrene unit content is equal to or lower than the upper limit, the hardness of the styrene-based thermoplastic elastomer can be prevented from becoming too high. The styrene unit content of the styrene-based thermoplastic elastomer is more preferably 10 to 40% by mass. The term "styrene unit content" is used to mean not only the content of styrene units, but also the content of structural units in which an atom or atomic group other than a hydrogen atom is substituted on the aromatic ring of a styrene unit. 13 It can be measured by C-NMR.
[0033] The chemical structure of the copolymer having the polymer block P and the polymer block Q in the styrene-based thermoplastic elastomer may be any of linear, branched, radial, etc., but is preferably a block copolymer represented by the following formula (1) or (2).
[0034] Furthermore, the block copolymer represented by the following formula (1) or (2) is preferably a hydrogenated derivative (hydrogenated block copolymer). When the copolymer represented by the following formula (1) or (2) is a hydrogenated block copolymer, the heat resistance and weather resistance tend to be good. P-(QP) m (1) (PQ) n (2) (In the formula, P represents a polymer block P, Q represents a polymer block Q, m represents an integer of 1 to 5, and n represents an integer of 1 to 5.)
[0035] In formula (1) or (2), the larger the m and n, the better in terms of lowering the order-disorder transition temperature of the rubber-like polymer, but the smaller the m and n, the better in terms of ease of production and cost.
[0036] As the block copolymer and / or hydrogenated block copolymer of a styrene-based thermoplastic elastomer (hereinafter collectively referred to as "(hydrogenated) block copolymer"), the (hydrogenated) block copolymer represented by formula (1) is more preferable than the (hydrogenated) block copolymer represented by formula (2) because of its excellent rubber elasticity.
[0037] The upper limit of the mass average molecular weight (Mw) of the styrene-based thermoplastic elastomer is not limited, but is usually 700,000 or less, preferably 600,000 or less, more preferably 500,000 or less. The lower limit of the mass average molecular weight (Mw) of the styrene-based thermoplastic elastomer is not limited, but is usually 40,000 or more, preferably 60,000 or more, more preferably 100,000 or more. By setting the mass average molecular weight (Mw) of the styrene-based thermoplastic elastomer to the above upper limit or less, the moldability and the appearance of the molded product can be maintained in a good condition. In addition, by setting the mass average molecular weight (Mw) to the above lower limit or more, the rubber softener of component (C) can be suppressed from bleeding out from the thermoplastic elastomer composition, and the compression set can be reduced.
[0038] The upper limit of the number average molecular weight (Mn) of the styrene-based thermoplastic elastomer is not limited, but is usually 600,000 or less, preferably 500,000 or less, more preferably 400,000 or less. The lower limit of the number average molecular weight (Mn) of the styrene-based thermoplastic elastomer is not limited, but is usually 30,000 or more, preferably 50,000 or more, more preferably 80,000 or more. By making the number average molecular weight (Mn) of the styrene-based thermoplastic elastomer below the above upper limit, the moldability and the appearance of the molded product can be maintained well. In addition, by making the number average molecular weight (Mn) above the above lower limit, the rubber softener of component (C) can be suppressed from bleeding out from the thermoplastic elastomer composition, and the compression set can be reduced.
[0039] The mass average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (PDI) of the styrenic thermoplastic elastomer of component (A) are measured under the following conditions by gel permeation chromatography (GPC), converted to polystyrene, and determined by creating a differential molecular weight distribution diagram. The analysis range is for molecular weights of 10,000 or more. <Measurement Conditions for GPC> Equipment: HLC-8220 GPC manufactured by Tosoh Corporation Column: TSKgel Super HM-M manufactured by Tosoh Corporation Detector: Differential refractive index detector (RI / built-in) Solvent: Chloroform, special grade Temperature: 40 °C Flow rate: 0.3 mL / min Injection volume: 20 μL Concentration: 0.1 mass% Calibration sample: Monodisperse polystyrene Calibration method: Conversion to polystyrene
[0040] The production method of the styrenic thermoplastic elastomer may be any method as long as the above-described structure and physical properties are obtained, and is not particularly limited. For example, it can be obtained by performing block polymerization in an inert solvent using a lithium catalyst or the like. Further, for the hydrogenation (hydrogen addition) of the block copolymer, known methods such as performing it in the presence of a hydrogenation catalyst in an inert solvent can be adopted.
[0041] Among the above-described ones, as the styrenic thermoplastic elastomer, a styrene-conjugated diene block copolymer and / or its hydrogenated product is preferable, and a hydrogenated product in which the conjugated diene of the styrene-conjugated diene block copolymer is composed of one or more selected from isoprene and butadiene is suitable. The styrene-conjugated diene block copolymer and / or its hydrogenated product may have a polar group as necessary.
[0042] Examples of styrene-conjugated diene block copolymers and / or hydrogenated products thereof include styrene-butadiene block copolymers and / or hydrogenated products thereof, styrene-butadiene-styrene block copolymers and hydrogenated products thereof, styrene-isoprene block copolymers and / or hydrogenated products thereof, styrene-isoprene-styrene block copolymers and / or hydrogenated products thereof, styrene-butadiene-isoprene block copolymers and / or hydrogenated products thereof, styrene-isoprene-butadiene-styrene block copolymers and / or hydrogenated products thereof, etc.
[0043] Hydrogenated styrene-butadiene block copolymers include styrene-butadiene-butylene copolymers (SBB) and styrene-ethylene-butylene copolymers (SEB). An example of a hydrogenated styrene-butadiene-styrene block copolymer is styrene-ethylene-butylene-styrene copolymer (SEBS). Hydrogenated styrene-isoprene-styrene block copolymers include styrene-ethylene-propylene-styrene copolymers (SEPS). An example of a hydrogenated styrene-isoprene-butadiene-styrene block copolymer is styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS).
[0044] Among these, from the viewpoint of tensile strength and compression set, styrene-ethylene-butylene copolymer (SEB), which is a hydrogenated product of styrene-butadiene block copolymer, styrene-ethylene-butylene-styrene copolymer (SEBS), which is a hydrogenated product of styrene-butadiene-styrene block copolymer, styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), which is a hydrogenated product of styrene-isoprene-butadiene-styrene block copolymer, and styrene-ethylene-propylene-styrene copolymer (SEPS), which is a hydrogenated product of styrene-isoprene-styrene block copolymer, are preferred. These may be fully hydrogenated or partially hydrogenated.
[0045] The styrene-based thermoplastic elastomer may be a commercially available product, which may be appropriately selected from "Kraton" manufactured by Kraton Corporation, "Septon" and "Hybler" manufactured by Kuraray Co., Ltd., "Sibstar" manufactured by Kaneka Corporation, and "Tuftec (registered trademark)" series manufactured by Asahi Kasei Corporation.
[0046] The styrene-based thermoplastic elastomer may be used alone or in combination of two or more kinds having different physical properties, block structures, hydrogenation or the like.
[0047] <Component (B): Propylene-based polymer> The propylene-based polymer of component (B) is not particularly limited, and examples thereof include propylene homopolymers and propylene-based copolymers which are random or block copolymers of propylene and ethylene or an α-olefin.
[0048] As the propylene copolymer, one containing 90% by mass or more of propylene units is preferred in that it retains the crystallinity, rigidity, chemical resistance, and other characteristics of polypropylene.
[0049] Monomers copolymerizable with propylene that constitute the propylene copolymer include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene; and cyclic olefins, such as cyclopentene, norbornene, and tetracyclo[6,2,11,8,13,6]-4-dodecene. ; dienes such as 5-methylene-2-norbornene, 5-ethylidene-2-norbornene, 1,4-hexadiene, methyl-1,4-hexadiene, and 7-methyl-1,6-octadiene; vinyl chloride, vinylidene chloride, acrylonitrile, vinyl acetate, acrylic acid, methacrylic acid, maleic acid, ethyl acrylate, butyl acrylate, methyl methacrylate, maleic anhydride, styrene, methylstyrene, vinyltoluene, and divinylbenzene. These may be used alone or in combination of two or more. Among these, ethylene, 1-butene, and 1-hexene are preferred because they are inexpensive and easy to handle.
[0050] The propylene polymer of component (B) may be a hydrocarbon group-grafted propylene polymer in which a hydrocarbon group is grafted onto a propylene homopolymer or a propylene random copolymer. It is believed that the hydrocarbon group-grafted propylene polymer has a low compression set because the crystalline lamellae of the propylene polymer are strong and plastic deformation of the matrix is unlikely to occur. The hydrocarbon group-grafted propylene polymer is obtained by graft-modifying a propylene homopolymer or a propylene random copolymer with a diene compound.
[0051] Examples of diene compounds that can be used for the graft modification of the raw propylene polymer include conjugated diene compounds such as butadiene, isoprene, 1,3-heptadiene, 2,3-dimethylbutadiene, and 2,5-dimethyl-2,4-hexadiene. These compounds may be used alone or in any combination and ratio of two or more. Among these, butadiene and isoprene are preferred, and isoprene is particularly preferred.
[0052] Any method may be used for the modification to obtain a hydrocarbon group-grafted propylene-based polymer, and for example, the method described in JP 2015-98542 A can be used for production. In addition, a method of irradiating a propylene-based polymer with radiation, or a method of melt-mixing a propylene-based polymer, a diene compound, and a radical generator can be mentioned. Among these, the method of melt-mixing a propylene-based polymer, a diene compound, and a radical generator is preferred because it does not require expensive equipment and can produce a hydrocarbon group-grafted propylene-based polymer at low cost.
[0053] Examples of the apparatus for reacting the propylene polymer, the diene compound, and the radical generator include kneaders such as rolls, co-kneaders, Banbury mixers, Brabenders, single-screw extruders, and twin-screw extruders, horizontal stirrers such as twin-screw surface renewal machines and twin-screw multi-disk devices, and vertical stirrers such as double helical ribbon stirrers. Of these, it is preferable to use a kneader, and in particular, an extruder is preferable from the viewpoint of productivity.
[0054] There is no particular limitation on the order or method of mixing and kneading (stirring) the propylene-based polymer, diene compound, and radical generator. The propylene-based polymer, diene compound, and radical generator may be mixed and then melt-kneaded (stirred). The propylene-based polymer may be melt-kneaded (stirred) and then the diene compound or radical generator may be mixed simultaneously or separately, all at once or in portions. The propylene-based polymer and either one of the diene compound and the radical generator may be melt-kneaded (stirred) and then the other of the diene compound and the radical generator may be added and then melt-kneaded (stirred). The temperature of the kneader (agitator) is preferably 130° C. or more and 300° C. or less, in that the propylene-based polymer melts and does not undergo thermal decomposition. The kneading (agitation) time is generally preferably 1 to 60 minutes.
[0055] There is no limitation on the shape or size of the thus obtained hydrocarbon group-grafted propylene polymer, and it may be in the form of pellets.
[0056] The blending ratio of the diene compound to the propylene-based polymer is not particularly limited. The blending ratio of the diene compound to 100 parts by mass of the propylene-based polymer is usually 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and usually 30 parts by mass or less, preferably 10 parts by mass or less, more preferably 5 parts by mass or less.
[0057] One or more of the following monomers copolymerizable with the diene compound may be used in combination with the diene compound: vinyl chloride, vinylidene chloride, acrylonitrile, methacrylonitrile, acrylamide, methacrylamide, vinyl acetate, acrylic acid, methacrylic acid, maleic acid, maleic anhydride, metal acrylates, metal methacrylates, acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and stearyl acrylate; and methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and stearyl methacrylate.
[0058] The radical generator is not particularly limited, and peroxides, azo compounds, etc. can be used. Specifically, diacyl peroxides such as diperoxide and dilauroyl peroxide, dicumyl peroxide, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, α,α'-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, etc., dialkyl peroxides, tert-butyl peroxybenzoate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, cumyl peroxypivalate, etc. Examples of the peroxycarbonate include alkyl peroxy esters, peroxycarbonates such as tert-butylperoxyisopropyl carbonate, tert-butylperoxy 2-ethylhexyl carbonate, and tert-amylperoxyisopropyl carbonate, peroxyketals such as 1,1-bis(tert-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, n-butyl 4,4-bis(tert-butylperoxy)valerate, and 2,2-bis(tert-butylperoxy)butane, and azo compounds such as azobisisobutyronitrile and dimethylazoisobutyrate.
[0059] These radical generators can be appropriately selected depending on the type and MFR of the raw propylene polymer, the type of diene compound, reaction conditions, etc. The radical generators may be used alone or in any combination and ratio of two or more.
[0060] The amount of the radical generator is not particularly limited and is usually 0.001 to 20 parts by mass, preferably 0.005 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and further preferably 0.05 to 4 parts by mass, based on 100 parts by mass of the propylene polymer.
[0061] The melt flow rate (MFR) (JIS K7210, 230°C, 21.2N load) of the propylene polymer or hydrocarbon group-grafted propylene polymer of component (B) is not particularly specified, but is usually 0.05 to 200g / 10min, preferably 0.05 to 100g / 10min, and more preferably 0.1 to 80g / 10min. By setting the melt flow rate within the above range, excellent moldability and good appearance of the obtained molded product are obtained, and the mechanical properties, particularly the tensile breaking strength, can be controlled within the desired range.
[0062] The polypropylene-based polymer may be a commercially available product, such as Novatec (registered trademark) PP from Japan Polypropylene Corporation, Prime Polypro (registered trademark) from Prime Polymer Corporation, Sumitomo Noblen (registered trademark) from Sumitomo Chemical Co., Ltd., or polypropylene block copolymer from SunAllomer Corporation.
[0063] The hydrocarbon group-grafted propylene polymer is also available as a commercially available product. As the commercially available product, a suitable product can be selected from the "PP processability improver" series manufactured by Kaneka Corporation, the "Waymax (registered trademark)" series manufactured by JPP Co., Ltd., and the like.
[0064] The propylene polymer of component (B) may be used alone or in combination of two or more types having different physical properties, structures, etc.
[0065] <Component (C): Rubber softener> The rubber softener of component (C) is a mineral oil-based rubber softener and / or a rubber softener having a kinetic viscosity of 20 cSt or more and 600 cSt or less.
[0066] Mineral oil-based rubber softeners that satisfy the above requirement (i) are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons, and paraffinic hydrocarbons, and those in which 50% or more of the total carbon atoms are paraffinic hydrocarbons are called paraffinic oils, those in which 30-45% of the total carbon atoms are naphthenic hydrocarbons are called naphthenic oils, and those in which 35% or more of the total carbon atoms are aromatic hydrocarbons are called aromatic oils, respectively. Among these, paraffinic oils are preferred.
[0067] The kinematic viscosity at 40°C of a rubber softener satisfying the above requirement (ii) is 20 cSt or more, preferably 50 cSt or more, from the viewpoints of hygiene in terms of dissolution into chemical solutions and bleed-out, and is 600 cSt or less, preferably 550 cSt or less, from the viewpoint of liquid leakage resistance.
[0068] The rubber softener used in component (C) may be a commercially available product. Commercially available mineral oil-based rubber softeners include the PW series "Diana (registered trademark) Process Oil" manufactured by Idemitsu Kosan Co., Ltd.
[0069] The rubber softener of component (C) may be used alone or in combination of two or more kinds.
[0070] <Component (D): Isobutylene-based crosslinked thermoplastic elastomer> Examples of the isobutylene-based crosslinked thermoplastic elastomer of component (D) include a dynamic heat treatment product of a mixture containing (a) an isobutylene-based polymer having a reactive group, (b) a polyolefin, (c) a polybutene, and (d) a hydrosilyl group-containing compound.
[0071] For example, there may be mentioned a composition obtained by crosslinking (a) 100 parts by mass of an isobutylene-based polymer having a reactive group with (d) a hydrosilyl group-containing compound in a melt kneading system in the presence of (b) 5 to 30 parts by mass of a polyolefin which is at least one kind selected from the group consisting of polyethylene-based resins and polypropylene-based resins, and (c) 5 to 100 parts by mass of a polybutene having a number average molecular weight of 700 to 100,000.
[0072] (a) Isobutylene-Based Polymer Having Reactive Groups The isobutylene polymer having a reactive group (a) (hereinafter, sometimes referred to as "component (a)") can be crosslinked to produce a crosslinked product by having a reactive group, and the reactive group may be active in a crosslinking reaction by a crosslinking agent (d) hydrosilyl group-containing compound described below, and is not particularly limited. However, an alkenyl group having a carbon-carbon double bond is preferable, and from the viewpoint of reaction activity, the isobutylene polymer of component (a) preferably has a reactive group at its terminal. That is, the isobutylene polymer having a reactive group (a) is preferably an isobutylene polymer having an alkenyl group at its terminal. Specific examples of the alkenyl group of the reactive group include linear alkenyl groups such as vinyl group, allyl group, methylvinyl group, propenyl group, butenyl group, pentenyl group, and hexenyl group, and cycloalkenyl groups such as cyclopropenyl group, cyclobutenyl group, cyclopentenyl group, and cyclohexenyl group, and from the viewpoint of steric hindrance, an allyl group is preferable.
[0073] The amount of reactive groups such as alkenyl groups in component (a) can be arbitrarily selected depending on the required properties, but from the viewpoint of properties after crosslinking, it is preferable that at least 0.2 reactive groups per molecule are present at the end, that is, the reactive group content of component (a) is 0.2 / mol or more, more preferably 1.0 or more (1.0 / mol or more) per molecule, and even more preferably 1.5 or more (1.5 / mol or more) per molecule. If the amount of reactive groups is less than 0.2 per molecule, the crosslinking reaction may not proceed sufficiently. There is no particular limit to the upper limit of the amount of reactive groups, but it is usually 5 / mol or less. Here, the amount of reactive groups such as alkenyl groups is 1 It can be determined by H-NMR analysis.
[0074] The isobutylene polymer of component (a) is a polymer in which the content of isobutylene units relative to the total monomer units is more than 50% by mass. The type of isobutylene polymer is not particularly limited, and any of isobutylene homopolymers, isobutylene random copolymers, isobutylene block copolymers, etc. can be used.
[0075] When the isobutylene polymer is an isobutylene copolymer, examples of monomers copolymerized with isobutylene include one or more of ethylene, propylene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, styrene, etc.
[0076] The content of isobutylene units in the isobutylene polymer is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. The higher the content of isobutylene units is above the lower limit, the better the compatibility with (c) polybutene tends to be, so the isobutylene polymer is most preferably an isobutylene homopolymer with an isobutylene unit content of 100% by mass. The content of isobutylene units in the isobutylene polymer can be determined by infrared spectroscopy.
[0077] The mass average molecular weight (Mw) of the isobutylene polymer is preferably 5,000 to 500,000, particularly 10,000 to 200,000. When the mass average molecular weight of the isobutylene polymer is equal to or higher than the lower limit, mechanical properties and the like tend to be sufficiently exhibited, whereas when the mass average molecular weight is equal to or lower than the upper limit, melt-kneadability and crosslinking reactivity tend to be excellent.
[0078] The mass average molecular weight of the isobutylene polymer is a value calculated as polystyrene measured by GPC.
[0079] As a method for introducing an alkenyl group into the terminal of an isobutylene polymer, there may be mentioned a method disclosed in JP-A-3-152164 and JP-A-7-304909, in which a polymer having a functional group such as a hydroxyl group is reacted with a compound having an unsaturated group to introduce an unsaturated group into the polymer. In addition, in order to introduce an unsaturated group into a polymer having a halogen atom, there may be mentioned a method of carrying out a Friedel-Crafts reaction with an alkenylphenyl ether, a method of carrying out a substitution reaction with allyltrimethylsilane or the like in the presence of a Lewis acid, a method of carrying out a Friedel-Crafts reaction with various phenols to introduce a hydroxyl group, and then carrying out the above-mentioned alkenyl group introduction reaction. Among these, the method of introducing an allyl group into the terminal by a substitution reaction of allyltrimethylsilane with chlorine is preferred from the viewpoint of reactivity.
[0080] The component (a) may be used alone or in combination with two or more different types having different reactive groups, monomer compositions of isobutylene polymers, mass average molecular weights, and the like.
[0081] ((b) Polyolefin) The (b) polyolefin (hereinafter, may be referred to as "component (b)") is preferably selected from the group consisting of polyethylene-based resins and polypropylene-based resins, and component (b) not only functions as a crosslinking reaction field for component (a), but also has the function of imparting molding flowability, heat resistance, and mechanical strength to the thermoplastic elastomer composition of the present invention.
[0082] A polyethylene-based resin is a polyolefin having an ethylene unit content of more than 50 mass % relative to all monomer units.
[0083] The type of polyethylene resin is not particularly limited, and any of ethylene homopolymers, ethylene random copolymers, ethylene block copolymers, etc. can be used.
[0084] When the polyethylene resin is an ethylene copolymer, examples of monomers copolymerized with ethylene include one or more of propylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.
[0085] A polypropylene-based resin is a polyolefin having a propylene unit content of more than 50 mass % relative to all monomer units.
[0086] The type of polypropylene resin is not particularly limited, and any of propylene homopolymers, propylene random copolymers, propylene block copolymers, etc. can be used.
[0087] When the polypropylene-based resin is a propylene copolymer, examples of monomers copolymerized with propylene include one or more of ethylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.
[0088] The content of propylene units in the polypropylene-based resin is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. When the content of propylene units is equal to or more than the above lower limit, the crystallinity of the isobutylene-based crosslinked thermoplastic elastomer is improved, and the heat resistance of the obtained molded article tends to be good. On the other hand, there is no particular limit to the upper limit of the content of propylene units in the polypropylene-based resin, and it is usually 100% by mass or less. The content of propylene units in the polypropylene-based resin can be determined by infrared spectroscopy.
[0089] Preferred polyethylene resins include high density polyethylene, low density polyethylene, linear low density polyethylene, etc. Preferred polypropylene resins include homopolypropylene, random polypropylene, block polypropylene, etc. From the standpoint of heat resistance, it is preferable to use a polypropylene-based resin as the component (b).
[0090] The melt flow rate (MFR) of the (b) component is not particularly limited, but in the case of a polyethylene resin, the MFR measured according to JIS K7210 at a measurement temperature of 190°C and a measurement load of 21.2N is preferably 0.1 to 100g / 10min, more preferably 0.5 to 50g / 10min, and particularly preferably 1 to 30g / 10min. In the case of a polypropylene resin, the MFR measured according to JIS K7210 at a measurement temperature of 230°C and a measurement load of 21.2N is preferably 0.1 to 100g / 10min, more preferably 0.5 to 50g / 10min, and particularly preferably 1 to 30g / 10min. In either case, it is preferable that the MFR is not less than the lower limit from the viewpoint of molding flowability, and it is preferable that the MFR is not more than the upper limit from the viewpoint of improving the dispersibility of the isobutylene polymer during dynamic heat treatment.
[0091] The component (b) may be used alone or in combination of two or more types having different resin types or physical properties.
[0092] The (b) component is preferably used in an amount of 5 to 30 parts by mass per 100 parts by mass of the (a) component. If the (b) component is less than 5 parts by mass, not only is it not possible to obtain sufficient molding fluidity and other effects due to the use of the (b) component, but the dispersion of the (a) component becomes insufficient, and the dynamic heat treatment of the (a) component may not proceed uniformly. If the (b) component is more than 30 parts by mass, the amount of components exposed to the increase in resin temperature due to the dynamic heat treatment increases, so that the isobutylene-based crosslinked thermoplastic elastomer as a whole is more likely to undergo thermal degradation, and discoloration and stickiness of the obtained isobutylene-based crosslinked thermoplastic elastomer, generation of low molecular weight components, generation of foreign matter such as scorching may occur, and flexibility may be impaired, and the obtained thermoplastic elastomer composition may not have sufficient liquid leakage resistance and needle retention properties. The (b) component is more preferably used in an amount of 6 to 25 parts by mass, and even more preferably 7 to 20 parts by mass per 100 parts by mass of the (a) component.
[0093] ((c) Polybutene) (c) Polybutene having a number average molecular weight of 700 to 100,000 (hereinafter, sometimes referred to as "component (c)") functions as a softening agent for imparting flexibility and molding fluidity.
[0094] Bleeding out becomes noticeable when the number average molecular weight of the polybutene of the component (c) is less than 700. The number average molecular weight of the polybutene of the component (c) is preferably 800 to 100,000, and more preferably 850 to 80,000.
[0095] Here, the number average molecular weight of polybutene is a value calculated as polystyrene measured by GPC.
[0096] The (c) component is preferably used in an amount of 5 to 100 parts by mass per 100 parts by mass of the (a) component. If the (c) component is used in an amount of less than 5 parts by mass, the above-mentioned effect of using the (c) component cannot be fully obtained, and if the amount is more than 100 parts by mass, there is a risk of bleeding out. The (c) component is more preferably used in an amount of 10 to 80 parts by mass, and even more preferably 20 to 70 parts by mass, per 100 parts by mass of the (a) component.
[0097] ((d) Hydroxyl group-containing compounds) The (d) hydroxyl group-containing compound (hereinafter, sometimes referred to as "component (d)") functions as a crosslinking agent for the component (a).
[0098] There is no particular restriction on the hydrosilyl group-containing compound of component (d), but hydrosilyl group-containing polysiloxanes are preferred, and various compounds can be used. Among them, hydrosilyl group-containing polysiloxanes having 3 or more hydrosilyl groups and 3 to 500 siloxane units are preferred, hydrosilyl group polysiloxanes having 3 or more hydrosilyl groups and 10 to 200 siloxane units are more preferred, and hydrosilyl group polysiloxanes having 3 or more hydrosilyl groups and 20 to 100 siloxane units are even more preferred. If the number of hydrosilyl groups is less than 3, the network due to crosslinking does not grow sufficiently, and optimal rubber elasticity tends not to be obtained, and if the number of siloxane units is more than 500, the viscosity of the polysiloxane is high, dispersibility in component (a) is reduced, and the crosslinking reaction tends to proceed insufficiently.
[0099] The polysiloxane unit referred to here means a partial structure represented by the following general formula (I), (II), or (III). [Si(R 1 )2O] …(I) [Si(H)(R 2 )O] …(II) [Si(R 2 )(R 3 )O] …(III) (In the above formula, R 1 and R 2 represents an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 3 represents an alkyl group or an aralkyl group having 1 to 10 carbon atoms.
[0100] As the hydrosilyl group-containing polysiloxane, one or more of chain polysiloxanes represented by the following general formula (IV) or (V) and cyclic polysiloxanes represented by the following general formula (VI) can be used.
[0101] [ka]
[0102] (In the above formulas (IV) to (VI), R 1 and R 2 represents an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 3 represents an alkyl group or an aralkyl group having 1 to 10 carbon atoms; b represents an integer satisfying 3≦b, and a, b, and c represent integers satisfying 3≦a+b+c≦500; e represents an integer satisfying 3≦e, and d, e, and f represent integers satisfying d+e+f≦500.
[0103] The hydrosilyl group-containing compound of component (d) can be used in any ratio, but from the viewpoint of crosslinking speed, it is preferable to use it so that the amount of hydrosilyl groups relative to reactive groups such as alkenyl groups of component (a) (hydrosilyl groups / reactive groups) is in the range of a molar ratio of 0.5 to 10, and more preferably 1 to 5. If this molar ratio is less than 0.5, crosslinking tends to be insufficient, and if it is more than 10, a large amount of active hydrosilyl groups remains even after crosslinking, so that volatile matter tends to be generated.
[0104] (Hydrosilylation catalyst) The crosslinking reaction between components (a) and (d) proceeds by mixing and heating the two components, but in order to promote the reaction more rapidly, it is preferable to add a hydrosilylation catalyst. Such a hydrosilylation catalyst is not particularly limited, and examples thereof include radical generators such as organic peroxides and azo compounds, and transition metal catalysts.
[0105] The radical generator is not particularly limited, and examples thereof include dialkyl peroxides such as di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, dicumyl peroxide, t-butylcumyl peroxide, and α,α'-bis(t-butylperoxy)isopropylbenzene; diacyl peroxides such as benzoyl peroxide, p-chlorobenzoyl peroxide, m-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, and lauroyl peroxide; peroxy esters such as t-butyl perbenzoate; peroxydicarbonates such as diisopropyl percarbonate and di-2-ethylhexyl percarbonate; and peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane and 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane.
[0106] The transition metal catalyst is not particularly limited, and examples thereof include platinum alone, solid platinum dispersed on a carrier such as alumina, silica, or carbon black, chloroplatinic acid, complexes of chloroplatinic acid with alcohols, aldehydes, ketones, etc., platinum-olefin complexes, and platinum(0)-dialkenyltetramethyldisiloxane complexes. Examples of catalysts other than platinum compounds include RhCl(PPh3)3, RhCl3, RuCl3, IrCl3, FeCl3, AlCl3, PdCl2·H2O, NiCl2, and TiCl4 (wherein "Ph" stands for "phenyl group"). These catalysts may be used alone or in combination of two or more kinds. Of these, platinum vinyl siloxane is preferred in terms of crosslinking efficiency.
[0107] The amount of the hydrosilylation catalyst is not particularly limited, but it is preferable to use 10 -1 ~10 -8 It is preferable to use in the molar range of 10 -3 ~10 -6When the amount of the catalyst is equal to or more than the lower limit, the crosslinking reaction tends to proceed sufficiently, whereas when the amount of the catalyst is equal to or less than the upper limit, the crosslinking reaction tends to be sufficiently controlled by suppressing heat generation.
[0108] Component (D) is produced by subjecting a mixture containing components (a), (b), (c), and (d), and, if necessary, other components such as the hydrosilylation catalyst, to dynamic heat treatment. This dynamic heat treatment causes a crosslinking reaction in which component (a) is crosslinked by component (d) in the presence of components (b) and (c), resulting in a crosslinked product.
[0109] "Dynamic heat treatment" means kneading in a molten or semi-molten state. This dynamic heat treatment is preferably performed by melt kneading, and the heating and kneading device for this purpose is not particularly limited, but examples include single-screw extruders, twin-screw extruders, rolls, Banbury mixers, Brabenders, kneaders, high-shear mixers, etc. In addition, the order of addition is preferably such that after component (b) is melted, component (a) is added to the molten components (b) and (c), and other components are further added if necessary, and mixed uniformly, and then the crosslinking agent and hydrosilylation catalyst of component (d) are added to proceed with the crosslinking reaction. The hydrosilylation catalyst may be added by mixing it with the liquid component (c).
[0110] The melt-kneading temperature during the dynamic heat treatment is preferably 130 to 240°C. If this temperature is 130°C or higher, the (b) component tends to melt sufficiently and be uniformly kneaded. If this temperature is 240°C or lower, the (a) component can be prevented from thermal decomposition. The melt-kneading time is usually about 1 to 10 minutes.
[0111] In the thermoplastic elastomer composition of the present invention, in order to reliably obtain the effects of component (D) obtained by subjecting the aforementioned (a) isobutylene-based polymer having a reactive group to dynamic heat treatment with (d) a hydrosilyl group-containing compound in the presence of a predetermined amount of (b) at least one polyolefin selected from the group consisting of polyethylene-based resins and polypropylene-based resins, and (c) a polybutene having a number average molecular weight of 700 to 100,000, component (D) is preferably blended such that the total of components (a), (b), (c), (d) and the aforementioned hydrosilylation catalyst used as necessary is contained in the raw material mixture used to produce component (D) by dynamic heat treatment to 50% by mass or more, particularly 60% by mass or more, and even more preferably 80 to 100% by mass.
[0112] The isobutylene-based crosslinked thermoplastic elastomer of component (D) can be obtained as a commercially available product. Examples of commercially available products of component (D) include "Sibstar (registered trademark) TPV" manufactured by Kaneka Corporation, and the relevant product can be appropriately selected from these and used.
[0113] The thermoplastic elastomer composition of the present invention may contain only one type of component (D), or may contain two or more types of components (a) to (d) that differ in type or composition.
[0114] <Content rate> The thermoplastic elastomer composition of the present invention preferably contains 3% by mass or more of component (A) in 100% by mass of the total of components (A) to (D), more preferably 5% by mass or more, and even more preferably 8% by mass or more. If the content of component (A) is equal to or more than the above lower limit, the effect of rubber elasticity due to the inclusion of component (A) can be obtained more effectively. On the other hand, the thermoplastic elastomer composition of the present invention preferably contains 35% by mass or less of component (A) in 100% by mass of the total of components (A) to (D), more preferably 30% by mass or less, and even more preferably 25% by mass or less. If the content of component (A) is equal to or less than the above upper limit, the contents of other components can be secured and the effects of liquid leakage properties and needle retention properties can be obtained more effectively.
[0115] The thermoplastic elastomer composition of the present invention preferably contains 0.1% by mass or more of component (B) in 100% by mass of the total of components (A) to (D), more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. If the content of component (B) is equal to or higher than the above lower limit, the effect of moldability due to the inclusion of component (B) can be obtained more effectively. On the other hand, the thermoplastic elastomer composition of the present invention preferably contains 20% by mass or less of component (B) in 100% by mass of the total of components (A) to (D), more preferably 15% by mass or less, and even more preferably 10% by mass or less. If the content of component (B) is equal to or lower than the above upper limit, the contents of other components can be secured and the effects of liquid leakage properties and needle retention properties can be obtained more effectively.
[0116] The thermoplastic elastomer composition of the present invention preferably contains 5% by mass or more of component (C) in 100% by mass of the total of components (A) to (D), more preferably 8% by mass or more, and even more preferably 10% by mass or more. If the content of component (C) is equal to or higher than the above lower limit, the effect of flexibility and moldability due to the inclusion of component (C) can be obtained more effectively. On the other hand, the thermoplastic elastomer composition of the present invention preferably contains 50% by mass or less of component (C) in 100% by mass of the total of components (A) to (D), more preferably 45% by mass or less, and even more preferably 40% by mass or less. If the content of component (C) is equal to or lower than the above upper limit, the contents of other components can be secured and the effect of liquid leakage properties and needle retention properties can be obtained more effectively.
[0117] The thermoplastic elastomer composition of the present invention must contain 35% by mass or more of component (D) in 100% by mass of the total of components (A) to (D), and this content is preferably 37% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more. If the content of component (D) is above the lower limit, the effect of needle retention property due to the inclusion of component (D) can be obtained more effectively. On the other hand, the thermoplastic elastomer composition of the present invention must contain 80% by mass or less of component (D) in 100% by mass of the total of components (A) to (D), and this content is preferably 75% by mass or less, more preferably 70% by mass or less, and even more preferably 65% by mass or less. If the content of component (D) is below the upper limit, the contents of other components can be secured and the effect of liquid leakage property can be obtained more effectively.
[0118] The thermoplastic elastomer composition of the present invention preferably contains 80% by mass or more of components (A) to (D) in total, based on 100% by mass of the total amount of the thermoplastic elastomer composition of the present invention, in order to effectively obtain the effects of the present invention provided by containing these components. This content is more preferably 85% by mass or more, and even more preferably 90% by mass or more. There is no particular upper limit, and the content may be 100% by mass.
[0119] <Other ingredients> The thermoplastic elastomer composition of the present invention may contain components other than the above components (A) to (D) as necessary, provided that the object of the present invention is not impaired.
[0120] Examples of other components include various fillers such as talc and calcium carbonate, various antiblocking agents, heat stabilizers, antioxidants, lubricants, crystal nucleating agents, colorants, and resins other than components (A), (B), and (D).
[0121] Preferred examples of the antioxidant (hereinafter sometimes referred to as component (E)) include phenol-based antioxidants such as tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]pentaerythritol and 4,4',4"-[(2,4,6-trimethyl-1,3,5-benzenetriyl)tris(methylene)]tris[2,6-bis(1,1-dimethylethyl)phenol; phosphorus-based processing stabilizers such as tris(2,4-di-t-butylphenyl)phosphite; and hydroxylamine-based processing heat stabilizers such as oxidation products of alkylamines made from reduced beef tallow. When an antioxidant is used, the blending amount is preferably 0.01 to 1.0 mass %, and more preferably 0.05 to 0.5 mass %, relative to 100 mass % in total of the components (A) to (D).
[0122] Resins other than components (A), (B), and (D) that may be contained in the thermoplastic elastomer composition of the present invention include styrene-based elastomers other than component (A), polyolefin resins other than components (B) and (D), polyester resins, polyamide resins, acrylic resins, polycarbonate resins, polyvinyl chloride resins, polystyrene resins, liquid crystal resins, various elastomers (excluding those corresponding to components (A) and (D)), etc. The above-mentioned other resins may be contained alone or in combination of two or more.
[0123] When the thermoplastic elastomer composition of the present invention contains resins other than the components (A), (B), and (D), in order to fully obtain the effects of containing the components (A) to (D), the content of the other resins is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of the total of the components (A) to (D).
[0124] <Method of producing thermoplastic elastomer composition> The thermoplastic elastomer composition of the present invention is obtained as a solid such as pellets by mechanically mixing the above-mentioned components (A) to (D) and other components blended as necessary using a known method, for example, a Henschel mixer, a V blender, or a tumbler blender, mechanically melt-kneading the mixture using a known method, and extruding the mixture through a die. For the mechanical melt-kneading, a general melt-kneading machine such as a Banbury mixer, various kneaders, or a single-screw or twin-screw extruder can be used.
[0125] <Physical Properties> The thermoplastic elastomer composition of the present invention contains the above-mentioned components (A), (B), (C) and (D), and thus has excellent liquid leakage resistance and needle retention. The thermoplastic elastomer composition of the present invention preferably has the following physical properties.
[0126] (Melt Flow Rate (MFR)) In the present invention, the melt flow rate (MFR) measured at 230°C and a load of 49N (5kgf) with reference to ISO 1133-1 (2011) is used as an index of moldability of the thermoplastic elastomer composition. In order to make the thermoplastic elastomer composition of the present invention excellent in moldability, it is preferable that the melt flow rate (49N) is 0.1g / 10 minutes or more and 200g / 10 minutes or less. When the MFR of the thermoplastic elastomer composition is 0.1g / 10 minutes or more, the fluidity tends to be good, and when it is 200g / 10 minutes or less, it is preferable from the viewpoint of heat resistance. From the viewpoint of fluidity, the MFR of the thermoplastic elastomer composition is more preferably 0.2g / 10 minutes or more, even more preferably 0.3g / 10 minutes or more, and particularly preferably 1g / 10 minutes or more. On the other hand, from the viewpoint of heat resistance, the MFR of the styrene-based thermoplastic elastomer composition is more preferably 150g / 10 minutes or less, even more preferably 100g / 10 minutes or less.
[0127] (Compression set) The thermoplastic elastomer composition of the present invention preferably has a compression set (restoration rate) determined as follows of 40% or less, more preferably 35% or less, and even more preferably 30% or less. A compression set of 40% or less provides recovery similar to that of vulcanized rubber, and is suitable for liquid leakage resistance and sealing properties. With reference to ISO815-1, the thermoplastic elastomer composition of the present invention is injection molded into a plate, and six test pieces with a diameter of 29 mm are punched out, stacked, and the original thickness (t0) is measured. Then, the test pieces are compressed by 25% using a compression device and a spacer (thickness t1), and heat-treated for 22 hours in a gear oven maintained at 70°C. Then, immediately after removing from the oven, the test pieces are taken out of the compression device and released from compression in an environment of 23°C and 50% RH, and the thickness (t2) is measured after 30 minutes. The compression set is calculated according to the following formula.
[0128]
number
[0129] CS: Compression set (%) t0: original thickness of test piece (mm) t1: Spacer thickness (mm) t2: The thickness (mm) of the test piece after 30 minutes from the compression device
[0130] (Flexibility (Duro hardness A)) The thermoplastic elastomer composition of the present invention preferably has a hardness of 10 to 55 when three plates obtained by injection molding are stacked on top of each other and measured after 15 seconds using a durometer A (type A durometer) with reference to ISO 7619-1. When the durometer A of the thermoplastic elastomer composition is 55 or less, the compression set tends to be good. When the durometer A of the thermoplastic elastomer composition is 10 or more, it is preferable for the ease of assembly. From the viewpoint of the ease of assembly, the durometer A of the thermoplastic elastomer composition is more preferably 15 or more, and even more preferably 20 or more. From the viewpoints of the liquid leakage resistance and the compression set, the durometer A of the thermoplastic elastomer composition is more preferably 50 or less, even more preferably 35 or less, and particularly preferably 45 or less.
[0131] [Molded body of thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention can be used as a molded article by various molding methods. In particular, it is preferable to make a molded article by injection molding the thermoplastic elastomer composition of the present invention. The molding conditions for injection molding are as follows.
[0132] The molding temperature when the thermoplastic elastomer composition is injection molded is usually 150 to 300° C., preferably 180 to 280° C. The injection pressure is usually 5 to 100 MPa, preferably 10 to 80 MPa. The mold temperature is usually 0 to 80° C., preferably 20 to 60° C.
[0133] [Application] The thermoplastic elastomer composition of the present invention has excellent compression set, and in particular, excellent resistance to leakage and needle retention, and therefore can be applied to various sealing materials, specifically, rubber stoppers having needle piercing parts such as syringe gaskets, rubber stoppers for infusion bags, and rubber stoppers for vials, cap liners, packing, etc., which require leakage sealing. However, the applications are not limited to medical use. For example, the composition can be suitably used for non-medical syringes, droppers, water pitchers, bottle pumps, syringe-type feeders, gaskets for water guns, gaskets for cooking utensils, exterior moldings for automobiles, window wipers for automobiles, etc.
[0134] [Rubber stopper with needle piercing part] The molded article of the present invention made of the thermoplastic elastomer composition of the present invention is excellent in compression set and has excellent sealing properties against liquid leakage, and is therefore particularly useful as a rubber stopper having a needle pierce portion.
[0135] A rubber stopper having a needle piercing portion as one embodiment of the molded article of the present invention will be described below with reference to Figs. However, the rubber stopper according to the present invention is not limited to those shown in FIGS.
[0136] The rubber stopper 10 shown in Fig. 1 has a base portion 10A and needle piercing portions 11, 12, 13, and 14. The base portion 10A has a base portion (leg portion) 10a that is inserted into the mouth of a vial or the like, and a cap portion 10b. The needle piercing portions 11 to 14 are recessed and provided on the upper surface of the cap portion 10b. In this rubber plug 10, the needlestick portion is composed of needlestick portion 11 having a large diameter and needlestick portions 12 to 14 having smaller diameters provided at equal intervals around the same. In this way, by having needlestick portion 11 and needlestick portions 12 to 14 of different diameters, needles of different thicknesses can be inserted. For example, a plastic needle of a large diameter for an infusion set can be inserted into large-diameter needlestick portion 11. A mixing needle for injecting a medicinal liquid or a metal needle of a small diameter can be inserted into small-diameter needlestick portions 12 to 14.
[0137] The rubber stopper 20 shown in Fig. 2 has the same structure as the rubber stopper 10 shown in Fig. 1, except that needle puncture parts 21-23 having the same diameter are recessed at equal intervals into the upper surface of the lid part 20b of the base part 20A. In Fig. 2, 20a is the base part (leg part).
[0138] The rubber stopper 30 shown in Fig. 3 has the same configuration as the rubber stopper 20 shown in Fig. 2, except that, among the needlestick parts 31 to 33, a convex part 33A is provided around the periphery of the needlestick part 33. In Fig. 3, 30A is a base part, 30a is a base part (leg part), and 30b is a lid part. By providing the convex part 33A on the periphery of the needlestick part 33 as in this rubber stopper 30, it becomes easy to distinguish it from the other needlestick parts 31, 32, and it can be used as a marker for injecting the target medicinal liquid.
[0139] The rubber stopper 40 shown in Fig. 4 has a needle piercing part 41 and four convex ridges 40d on the upper surface of the lid part 40b of the base part 40A. A recess 40c is formed in the center of the base part (leg part) 40a of the base part 40A. In this rubber stopper 40, the recess 40c is formed in the base part (leg part) 40a and the base part (leg part) 40a is annular, so that the rubber stopper 40 can be easily inserted into the mouth of a vial bottle or the like. In addition, in this rubber stopper 40, the needle piercing part 41 is recessed into the center of the lid part 40b, and four convex ridges 40d extending radially are provided around the needle piercing part 41 at 90° intervals for identification of the rubber stopper 40, etc.
[0140] The rubber stopper 50 in Fig. 5 has the same configuration as the rubber stopper 40 shown in Fig. 4, except that there is no protruding portion and only a needle piercing portion 51 is provided in the center of the lid portion 50b. 50A is a base portion consisting of a base portion (leg portion) 50a in which a recess 50c is formed, and a lid portion 50b.
[0141] [Infusion bag] The rubber stopper made of the thermoplastic elastomer composition of the present invention as described above has excellent compression set and excellent sealing properties against liquid leakage, and is therefore useful as a rubber stopper for infusion bags. The shape, structure, material, etc. of an infusion bag having a rubber stopper made of the thermoplastic elastomer composition of the present invention are not limited, but it is usually composed of an infusion bag body, a port for injecting the medicinal solution, a rubber stopper, a cap, etc.
[0142] The shape of the rubber stopper of the infusion bag is not limited, but may be roughly cone-shaped, cylindrical, or disk-shaped, and the diameter is usually about 10 to 20 mm. The thickness of the rubber stopper of the infusion bag (thickness in the direction of piercing the injection needle) is also not limited, but is usually about 4 to 8 mm.
[0143] When removing the contents from an infusion bag having a rubber stopper made of the thermoplastic elastomer composition of the present invention, a metal injection needle, a plastic injection needle, or an injection needle made of other materials may be used. The diameter of the injection needle to be used is not limited. Furthermore, needles other than injection needles may be used. Generally, when a large-diameter injection needle is used, the liquid leakage resistance becomes poor. However, since the rubber stopper made of the thermoplastic elastomer composition of the present invention has good liquid leakage resistance, it is possible to use an injection needle with an outer diameter of 2 mm or more, or even 3 mm or more.
[0144] [Vial] The rubber stoppers made of the thermoplastic elastomer composition of the present invention as described above have excellent compression set and excellent sealing properties against liquid leakage, and are therefore useful as rubber stoppers for vials. There are no limitations on the shape, structure, material, etc. of a vial having a rubber stopper made of the thermoplastic elastomer composition of the present invention, but it usually consists of a vial body, a rubber stopper, a sealing member, a cap member, etc.
[0145] The shape of the rubber stopper of the vial is not limited, but may be roughly cylindrical or disk-like, and its diameter is usually about 5 to 30 mm. The thickness of the rubber stopper of the vial (thickness in the direction of insertion of the injection needle) is also not limited, but is usually about 5 to 10 mm.
[0146] When removing the contents from a vial having a rubber stopper made of the thermoplastic elastomer composition of the present invention, a metal injection needle, a plastic injection needle, or an injection needle made of other materials may be used. The diameter of the injection needle to be used is not limited. Furthermore, needles other than injection needles may be used. Generally, when a large-diameter injection needle is used, the liquid leakage resistance becomes poor. However, since the rubber stopper made of the thermoplastic elastomer composition of the present invention has good liquid leakage resistance, it is possible to use an injection needle with an outer diameter of 2 mm or more, or even 3 mm or more.
[0147] [Vacuum blood collection tube] The rubber stopper made of the thermoplastic elastomer composition of the present invention as described above has excellent compression set and excellent liquid leakage sealing properties, and is therefore useful as a rubber stopper for vacuum blood collection tubes. There are no limitations on the shape, structure, material, etc. of a vacuum blood collection tube having a rubber stopper made of the thermoplastic elastomer composition of the present invention, but it is usually composed of a bottomed tubular body that forms the main body of the vacuum blood collection tube, a rubber stopper, etc.
[0148] The shape of the rubber stopper of the vacuum blood collection tube is not limited, but examples include a roughly cap-like or cylindrical shape, and the diameter is usually about 10 to 20 mm. EXAMPLES
[0149] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values between the examples.
[0150] [raw materials] The raw materials used in the following Examples and Comparative Examples are shown below.
[0151] Component (A): Styrene-based thermoplastic elastomer A-1: Hydrogenated styrene-butadiene copolymer (styrene-ethylene-butylene-styrene copolymer (SEBS) and / or styrene-ethylene-butylene copolymer (SEB)) Asahi Kasei Corporation, product name: Tuftec (registered trademark) N527 Styrene unit content: 21.3% by mass 1,4-microstructure ratio of butadiene: 29.6% by mass Mass average molecular weight (Mw): 395,000 Number average molecular weight (Mn): 210,000 Molecular weight distribution (PDI): 1.9 A-2: Hydrogenated styrene-isoprene-styrene copolymer Manufactured by Kuraray Co., Ltd. Product name: Hybra (registered trademark) 7135R Mass average molecular weight (Mw): 279,000 Number average molecular weight (Mn): 210,000 Molecular weight distribution (PDI): 1.3 A-3: Styrene-ethylene-butylene-styrene copolymer (SEBS) Kraton Corporation Product name: Kraton (registered trademark) G1633EU Mass average molecular weight (Mw): 394,000 Number average molecular weight (Mn): 310,000 Molecular weight distribution (PDI): 1.3 A-4: Styrene-ethylene-butylene-styrene copolymer (SEBS) Kraton Corporation, product name: Kraton (registered trademark) G1651HU Mass average molecular weight (Mw): 246,000 Number average molecular weight (Mn): 140,000 Molecular weight distribution (PDI): 1.8 A-5: Styrene-ethylene-butylene-styrene copolymer (SEBS) Kraton Corporation, product name: Kraton (registered trademark) G1641HU Mass average molecular weight (Mw): 220,000 Number average molecular weight (Mn): 180,000 Molecular weight distribution (PDI): 1.2
[0152] Component (B): Polypropylene B-1: Hydrocarbon group grafted propylene-based polymer obtained by grafting isoprene onto polypropylene homopolymer Kaneka Corporation Product name: PP processability improver MFR (230℃, 21.2N load): 56g / 10 minutes B-2: Propylene homopolymer Made by Japan Polypropylene Corporation Product name: Novatec (registered trademark) PP FA3KM MFR (230℃, 21.2N load): 10g / 10 minutes
[0153] Component (C): Mineral oil-based rubber softener C-1: Paraffin oil Product name: Diana (registered trademark) Process Oil PW-90 manufactured by Idemitsu Kosan Co., Ltd. Kinematic viscosity at 40℃: 95cSt Flash point: 272℃
[0154] Component (D): Isobutylene-based crosslinked thermoplastic elastomer D-1: Dynamic heat treatment product of a mixture containing (a) an isobutylene polymer having a reactive group, (b) a polyolefin, (c) a polybutene, and (d) a hydrosilyl group-containing compound, as shown below. Kaneka Corporation Product name: Shibstar TPV P1140B Component (a): 100 parts by mass of polyisobutylene having an allyl group at its end (mass average molecular weight: 50,000, allyl group content: 2.0 / mol) (b) Component: Polypropylene (MFR (JIS K7210 (230°C, 21.2N load): 7g / 10min) 11 parts by mass (c) Component: Polybutene (number average molecular weight: 960): 40 parts by mass (d) Component: (CH3)3SiO-[Si(H)(CH3)O] 48 Hydrosilyl group-containing polysiloxane represented by -Si(CH3)3
[0155] Ingredient (E): Antioxidant E-1: Hindered phenol antioxidant ADEKA ADEKA STAB (registered trademark) AO-60 (Tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl) propionate] pentaerythritol)
[0156] Ingredient (X): Other X-1: Synthetic resin softener Manufactured by ENEOS, product name: Nippon Oil Polybutene HV300 Kinematic viscosity at 40℃: 26,000cSt Flash point: 230℃
[0157] [Evaluation method] The thermoplastic elastomer compositions obtained in the following Examples and Comparative Examples were evaluated by preparing sheets or rubber stopper molded products from pellets of the thermoplastic elastomer composition by the following method, and the pellets of the thermoplastic elastomer composition were evaluated in the following (1), the sheets of the thermoplastic elastomer composition were evaluated in the following (2) to (3), and the rubber stopper molded products of the thermoplastic elastomer composition were evaluated in the following (4) to (6).
[0158] <Preparation of Thermoplastic Elastomer Composition Pellets> The raw materials described in the Examples and Comparative Examples were mixed in the ratios shown in Tables 1 and 2, and the resulting mixture was melt-kneaded in a twin-screw kneader (cylinder temperature 180 to 200°C) to produce pellets of a thermoplastic elastomer composition. The resulting pellets were evaluated for the following evaluation item (1).
[0159] <Preparation of Thermoplastic Elastomer Composition Sheet> The obtained pellets were fed to an in-line screw type injection molding machine (IS130GN manufactured by Toshiba Machine Co., Ltd.) and injection molded under conditions of an injection pressure of 40 MPa, a cylinder temperature of 210° C., and a mold temperature of 40° C. to obtain a sheet of the thermoplastic elastomer composition having a thickness of 2 mm. Using this sheet, the following evaluation items (2) to (3) were evaluated.
[0160] <Preparation of Thermoplastic Elastomer Composition Rubber Stopper Molding> The obtained pellets were fed to an in-line screw type injection molding machine (J110AD-180H manufactured by Japan Steel Works, Ltd.) and injection molded under conditions of injection pressure of 30 MPa, cylinder temperature of 210°C, and mold temperature of 40°C to obtain a rubber stopper molded product of the thermoplastic elastomer composition (rubber stopper molded product 1 in Figure 6) having a maximum outer diameter of 20.98 mm and a central thickness of 7.14 mm. Using this rubber stopper molded product of the thermoplastic elastomer composition, the following evaluation items (4) to (6) were evaluated.
[0161] (1) Formability (MFR) The MFR of the pellets of the thermoplastic elastomer compositions obtained in the Examples and Comparative Examples was measured at 230°C and 49 N using a melt indexer (manufactured by Toyo Seiki Seisakusho) in accordance with ISO 1133. A higher MFR indicates higher fluidity and superior moldability.
[0162] (2) Compression set The compression set (CS) was measured at 70°C for 22 hours and 30 minutes after release using the method described above with reference to ISO815-1.
[0163] (3) Flexibility (Duro hardness A) Durohardness A (type A durometer) was measured (after 15 seconds) with reference to ISO 7619-1.
[0164] (4) Leak resistance The amount of liquid leakage (g) was measured by the following method. The rubber plug molded product 1 was fitted into a predetermined jig 2 shown in FIG. Next, the retaining ring 3 was fixed with another jig (not shown) so that it was in complete contact with the holder 4 in which the rubber stopper molded product 1 was fitted, and the product was steam sterilized at 121°C for 30 minutes at a steam pressure of 0.1 MPa using a high-pressure steam sterilizer CLS-32S manufactured by ALP Co., Ltd. Thereafter, the samples were removed from the high-pressure steam sterilizer and cooled in a constant temperature and humidity room at 23°C and 50% humidity for 12 hours or more. After that, with the rubber stopper molded product 1 fitted into the jig 2 in Fig. 6, a plastic needle with a diameter (maximum diameter at the base) of 5 mm was inserted into the center of the rubber stopper molded product 1 up to the maximum diameter of the needle. The plastic needle used was a plastic needle from Nipro's Nipro infusion set (50 pieces) ISA-600A00Z manufactured by Nipro Corporation. Next, in the state shown in FIG. 6, a metal cylinder of the same diameter was attached to the thread pitch portion 5, and this was filled with 130 g of water and fixed in place. The sample was left as it was for 4 hours, the needle was removed, and the time it took for the water leaking from the needle hole to stop was measured, which was recorded as the liquid leakage time (sec). The mass of the leaked water was also measured, which was recorded as the amount of leaked water (g). The number of measurements was three, and the simple average was used as the measured value. The smaller the amount of leakage, the better the leakage resistance was judged to be.
[0165] (5) Needle holding time The needle retention time (sec) was measured by the following method. The rubber plug molded product 1 was fitted into a predetermined jig 2 shown in FIG. Next, the retaining ring 3 was fixed with another jig (not shown) so that it was in complete contact with the holder 4 in which the rubber stopper molded product 1 was fitted, and the product was steam sterilized at 121°C for 30 minutes at a steam pressure of 0.1 MPa using a high-pressure steam sterilizer CLS-32S manufactured by ALP Co., Ltd. Thereafter, the samples were removed from the high-pressure steam sterilizer and cooled in a constant temperature and humidity room at 23°C and 50% humidity for 12 hours or more. Next, a 450 mm long connecting tube manufactured by Nipro was cut into two at the center of the tube, and a 600 g weight was attached to the tube side. With the rubber stopper molded product 1 fitted into the jig 2 in FIG. 6, water was added up to the top of the jig 2, and then the metal needle at the end of the connecting tube with a weight attached was inserted up to the maximum diameter of the needle. After releasing the weight, the time until the needle with the weight attached fell naturally was measured and recorded as the needle holding time (sec). Two pieces were measured, and the measured value was calculated by simply averaging and rounding off the first digit. The longer the needle retention time, the less likely the needle was to fall out, and the better the result was.
[0166] (6) Operability The needle penetration strength (N) and needle withdrawal strength (N) were measured using the following method. The rubber plug molded product 1 was fitted into a predetermined jig 2 shown in FIG. Next, the retaining ring 3 was fixed with another jig (not shown) so that it was in complete contact with the holder 4 in which the rubber stopper molded product 1 was fitted, and the product was steam sterilized at 121°C for 30 minutes at a steam pressure of 0.1 MPa using a high-pressure steam sterilizer CLS-32S manufactured by ALP Co., Ltd. Thereafter, the samples were removed from the high-pressure steam sterilizer and cooled in a constant temperature and humidity room at 23°C and 50% humidity for 12 hours or more. Thereafter, a jig was attached to the top of an autograph AG-Xplus manufactured by Shimadzu Corporation, with a resin needle fitted to the top and the rubber stopper molded product 1 fitted to the bottom. As the resin needle, a Terumo TI-U200L plastic bottle needle was used. After that, the crosshead of the AG-Xplus was lowered at 200 mm / min until the needle penetrated the specimen up to its maximum diameter. The maximum stress (N) at that time was taken as the needle penetration strength. After measuring the needle puncture strength, the needle was raised at 200 mm / min and the needle was removed from the rubber stopper. The maximum stress (N) at that time was recorded as the needle removal strength. Two measurements were taken, and the simple average was used as the measured value. The smaller the needle penetration and withdrawal strength, the better the operability and the better it was judged to be.
[0167] [Example 1] 22.4 parts by mass of A-1 as a styrene-based thermoplastic elastomer of component (A), 4 parts by mass of B-1 as a propylene-based polymer of component (B), 33.6 parts by mass of C-1 as a rubber softener of component (C), and 40 parts by mass of D-1 as an isobutylene-based crosslinked thermoplastic elastomer of component (D) were mixed to obtain a mixture. 0.1 parts by mass of E-1 as an antioxidant of component (E) was added to a unidirectional twin-screw extruder (Toshiba Machine Co., Ltd. "TEM26-SS", cylinder diameter mouth 26 mm) at a rate of 10 to 20 kg / hour, melt-kneaded at 180 to 220 ° C, extruded from a die in the form of a strand, and then cut to obtain pellets of a pellet-shaped thermoplastic elastomer composition. The pellets were used to perform the above-mentioned evaluation. The evaluation results are shown in Table 1.
[0168] [Examples 2 to 10 and Comparative Examples 1 to 4] Pellets made of a thermoplastic elastomer composition were obtained and evaluated in the same manner as in Example 1, except that the composition was changed as shown in Tables 1 and 2. The results are shown in Tables 1 and 2.
[0169] [Table 1]
[0170] [Table 2]
[0171] [Consideration] The following can be seen from Tables 1 and 2. The rubber stopper molded product obtained from the thermoplastic elastomer composition of Comparative Example 1, in which the blended amount of component (D) was small, had good leakage resistance but poor needle retention. The rubber stopper molded product obtained from the thermoplastic elastomer composition of Comparative Example 2, which did not contain component (D), was poor in both leakage resistance and needle retention. The rubber stopper molded products obtained from the thermoplastic elastomer compositions of Comparative Examples 3 and 4, in which the synthetic resin-based softener (X) was used instead of the mineral oil-based rubber softener (C), had good needle retention but poor leakage resistance. In contrast, the rubber stopper molded products obtained from the thermoplastic elastomer compositions of Examples 1 to 10 were excellent in operability and showed good evaluation results in both leakage resistance and needle retention. [Explanation of symbols]
[0172] 1 Rubber stopper molded products 2 Jig 3 Retaining Ring 4 Holder 5 Thread pitch 10,20,30,40,50 Rubber stopper 10A,20A,30A,40A,50A Base part 10a,20a,30a,40a,50a base (leg) 10b,20b,30b,40b,50b Lid 11,12,13,14,21,22,23,31,32,33,41,51 Needle insertion part
Claims
1. A thermoplastic elastomer composition comprising the following components (A) to (D), wherein the content of component (D) in the total of components (A) to (D) is 35 mass% or more and 80 mass% or less, and component (C) is a mineral oil-based rubber softener: Component (A): Styrenic thermoplastic elastomer Component (B): Propylene-based polymer Component (C): Rubber softener Component (D): Isobutylene-based crosslinked thermoplastic elastomer
2. A thermoplastic elastomer composition comprising the following components (A) to (D), wherein the content of component (D) in the total of components (A) to (D) is 35% by mass or more and 80% by mass or less, and component (C) has a kinetic viscosity at 40°C of 20 cSt or more and 600 cSt or less: Component (A): Styrenic thermoplastic elastomer Component (B): Propylene-based polymer Component (C): Rubber softener Component (D): Isobutylene-based crosslinked thermoplastic elastomer
3. The thermoplastic elastomer composition according to claim 1 or 2, which has a compression set of 30% or less.
4. The thermoplastic elastomer composition according to claim 1 or 2, having a melt flow rate (230°C, load 49 N) of 0.1 g / 10 min or more and 200 g / 10 min or less.
5. The thermoplastic elastomer composition according to claim 1 or 2, having a durometer hardness A of 10 or more and 55 or less.
6. The thermoplastic elastomer composition according to claim 1 or 2, which is used for a rubber stopper having a needle pierce portion.
7. A molded article comprising the thermoplastic elastomer composition according to claim 1 or 2.
8. A sealing material comprising the thermoplastic elastomer composition according to claim 1 or 2.
9. The sealing material according to claim 8, which is a rubber plug.
10. The sealing material according to claim 9 , wherein the rubber plug is a rubber plug having a needle piercing portion.
11. An article comprising a rubber stopper made of the thermoplastic elastomer composition according to claim 1 or 2.
12. The article of claim 11 , wherein the article is a vial.
13. The article of claim 11 , which is an infusion bag.
14. The article of claim 11 , which is an evacuated blood collection tube.
Citation Information
Patent Citations
Composite elastomer composition for medical container plug body
JP2010227285A
Thermoplastic elastomer composition
WO2023022028A1