Zwitterionic polymers, printing medium, inkjet recording medium, inkjet ink, and composition
An amphoteric polymer with controlled solubility is used in inkjet recording media to enable print removal by hot water immersion, addressing the lack of elution in existing technologies and facilitating medium recyclability.
Patent Information
- Application Number
- JP2023043353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing inkjet recording media do not effectively allow for the removal of printed characters by immersion in hot water, lacking the ability to elute ink and detach prints from the medium without applying pressure.
Development of an amphoteric polymer with specific molecular weight and light transmittance properties, allowing it to dissolve in hot water while remaining insoluble in cold water, integrated into inkjet recording media to facilitate print removal.
Enables the inkjet recording medium to be eluted by immersion in hot water, effectively removing printed characters and allowing for recyclability of the medium.
Smart Images

Figure 2024132545000001 
Figure 2024132545000002 
Figure 2024132545000003
Abstract
Description
[Technical field]
[0001] The present invention relates to zwitterionic polymers, print recording media, ink-jet recording media, ink-jet inks and compositions. [Background technology]
[0002] It is known that amphoteric polymers of a specific structure exhibit UCST-type phase separation (a behavior in which the polymer dissolves at high temperatures and separates into phases at low temperatures). For example, Patent Document 1 describes that by utilizing this property, an inkjet recording medium containing a polymer compound exhibiting UCST-type phase separation exhibits a fast drying time, excellent image quality, low glycol staining, low color fusion, and excellent light fastness. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2009-500187 Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, Patent Document 1 states that it is possible to provide an inkjet recording medium that exhibits a fast drying time, excellent image quality, low glycol staining, low color fusion, and excellent light fastness. However, Patent Document 1 does not describe an inkjet recording medium or print recording medium in which the ink printed on the inkjet recording medium can be dissolved by immersing it in hot water at a certain temperature or higher, or an inkjet ink in which the print is detached from the print medium simply by immersing it in hot water at a certain temperature or higher after printing, and the elution property of the ink and the detachment property of the print from the print medium are unclear.
[0005] An object of the present invention is to provide an amphoteric polymer that can be dissolved by immersion in hot water at a certain temperature or higher, and to provide an inkjet recording medium or a print recording medium that can be dissolved by immersing ink printed on the inkjet recording medium in hot water at a certain temperature or higher by using the amphoteric polymer. Another object of the present invention is to provide an inkjet ink that uses an amphoteric polymer and allows the print to be detached from the print medium by simply immersing the medium in hot water at a certain temperature or higher after printing. [Means for solving the problem]
[0006] That is, the present invention relates to the following [1] to
[15] . [1] An amphoteric polymer having one or more types of constituent units derived from amphoteric monomer A, the weight average molecular weight being 1,000,000 or more and 10,000,000 or less, the transmittance of a 1% by mass aqueous solution of the amphoteric polymer at 30°C for light with a wavelength of 550 nm being 0% or more and 5.0% or less, and the transmittance of a 1% by mass aqueous solution of the amphoteric polymer at 80°C for light with a wavelength of 550 nm being 40% or more and 100% or less. [2] The amphoteric polymer according to [1], wherein the amphoteric monomer A is represented by the following formula (1):
[0007] [ka]
[0008] (In formula (1), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and X is -O- or -NR 2 - and Y + -S + R 3 -or-N + R 4 R 5 - and Z - Ha-SO3 - OR-PO2(OR 6 ) -where n is an integer from 1 to 8, m is an integer from 1 to 5, and R 2 , R 3 , R 4 , R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. [3] The amphoteric polymer according to [1] or [2], wherein the amphoteric monomer A is represented by the following formula (2):
[0009] [ka]
[0010] (In formula (2), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and X is -O- or -NR 2 -, n is an integer from 1 to 8, m is an integer from 1 to 5, and R 2 , R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. [4] The amphoteric polymer according to any one of [1] to [3], further comprising a constituent unit derived from an ethylenically unsaturated monomer B other than the amphoteric monomer A. [5] The amphoteric polymer according to [4], wherein the ethylenically unsaturated monomer B is at least one of (meth)acrylate and (meth)acrylamide having a hydroxy group or a tertiary amide bond. [6] The amphoteric polymer according to any one of [1] to [5], which contains 80 to 100 mass% of structural units derived from the amphoteric monomer A based on the total mass of the amphoteric polymer. [7] The amphoteric polymer according to any one of [1] to [6], which contains 0 to 20 mass% of a constituent unit derived from an ethylenically unsaturated monomer B other than the amphoteric monomer A, based on the total mass of the amphoteric polymer. [8] The amphoteric polymer according to any one of [1] to [7], which is for use in an inkjet recording medium. [9] An inkjet recording medium having, on a support, one or more composition layers each comprising a composition containing the amphoteric polymer according to any one of [1] to [8].
[10] The inkjet recording medium according to [9], wherein the composition layer is at least one layer selected from the group consisting of an inkjet ink receiving layer and a protective coating layer.
[11] At least one of the composition layers is an ink-jet ink-receiving layer; The inkjet recording medium according to [9] or
[10] , further comprising a barrier layer between the support and the inkjet ink receiving layer.
[12] The inkjet recording medium according to any one of [9] to
[11] , wherein the support comprises at least one material selected from the group consisting of cellulose ester, cellulose acetate, polyester, polystyrene, polyethylene, poly(vinyl acetate), polypropylene, polycarbonate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyamide, polyimide, polyether, polyvinyl chloride, polysulfonamide, silicone, glass, and stainless steel.
[13] The amphoteric polymer according to any one of [1] to [8], which is for use in a print recording medium.
[14] An inkjet ink containing the amphoteric polymer according to any one of [1] to [8].
[15] A composition comprising the amphoteric polymer according to any one of [1] to [8], wherein when a support having a composition layer formed from the composition on a surface thereof is immersed in warm water having a temperature of 80°C or higher and 100°C or lower for 30 minutes, the composition layer dissolves from the support. Effect of the Invention
[0011] According to the present invention, it is possible to provide an amphoteric polymer that can be dissolved by immersion in hot water at a certain temperature or higher. By using the amphoteric polymer of the present invention, it is possible to provide an inkjet recording medium that can be dissolved by immersing ink printed on the inkjet recording medium in hot water at a certain temperature or higher. Furthermore, by using the amphoteric polymer of the present invention, it is possible to provide an inkjet ink in which the print is detached from the printing medium by simply immersing the medium in hot water at a certain temperature or higher after printing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In this specification, the symbol "~" means to include the numbers before and after it. In the present specification and claims, "(meth)acrylic" is a general term for acrylic and methacrylic.
[0013] <Ampholytic polymer> The amphoteric polymer of the present invention is an amphoteric polymer having one or more types of constituent units derived from amphoteric monomer A, having a weight average molecular weight of 1,000,000 or more and 10,000,000 or less, and having a 1% by mass aqueous solution of the polymer having a light transmittance of 0% or more and 5.0% or less at 30°C for light with a wavelength of 550 nm, and having a 1% by mass aqueous solution of the polymer having a light transmittance of 40% or more and 100% or less at 80°C for light with a wavelength of 550 nm. When the amphoteric polymer has one or more types of constitutional units derived from the amphoteric monomer A, the amphoteric polymer exhibits solubility in warm water.
[0014] The weight average molecular weight of the amphoteric polymer is 1,000,000 or more and 10,000,000 or less, and more preferably 1,000,000 to 5,000,000. When the weight average molecular weight of the amphoteric polymer is within the above range, the solubility of the amphoteric polymer in cold water (water at 30° C.) is low, improving the practical applicability at room temperature. In this specification, the weight average molecular weight can be measured by the method described in the Examples.
[0015] The transmittance of a 1% by mass aqueous solution of the polymer at 30° C. for light with a wavelength of 550 nm is 0% or more and 5.0% or less, and preferably 0% or more and 4.0% or less. When the transmittance of a 1% by mass aqueous solution of the polymer at 30°C for light with a wavelength of 550 nm is within the above range, the solubility of the amphoteric polymer in cold water (water at 30°C) is reduced, improving the practical use at room temperature.
[0016] The transmittance of a 1% by mass aqueous solution of the polymer at 80° C. for light with a wavelength of 550 nm is 40% or more and 100% or less, and preferably 45% or more and 100% or less. When the transmittance of a 1% by mass aqueous solution of the polymer at 80° C. for light with a wavelength of 550 nm is within the above range, the dissolution rate of the amphoteric polymer in warm water is increased. In this specification, the light transmittance can be measured by the method described in the Examples.
[0017] The difference in transmittance, expressed as [transmittance of light with a wavelength of 550 nm at 80°C] - [transmittance of light with a wavelength of 550 nm at 30°C] of a 1% by mass aqueous solution of the polymer, is preferably 40% or more and 100% or less, and more preferably 45% or more and 100% or less. If the difference in transmittance is within the above range, when a composition layer is formed on a support using a composition containing the polymer, a sufficient difference in solubility in cold water and solubility in hot water can be provided, which makes the composition insoluble in cold water but easily soluble in hot water, thereby preventing inconvenience such as dissolution in cold water during use of the composition layer at room temperature, and enabling the support to be recycled by a simple method using hot water.
[0018] (Zwitterionic Monomer A) The amphoteric monomer A is preferably a monomer represented by the following formula (1), since the polymer obtained by polymerization exhibits solubility in warm water.
[0019] [ka]
[0020] (In formula (1), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and X is -O- or -NR 2 - and Y + -S + R 3 -or-N + R 4 R 5 - and Z - Ha-SO3 - OR-PO2(OR 6 ) - where n is an integer from 1 to 8, m is an integer from 1 to 5, and R 2 , R 3 , R 4 , R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Y + and Z - are selected from the viewpoint of availability, respectively. + R 4 R 5 - and -SO3 - is preferred.
[0021] In view of easy availability, the amphoteric monomer A is preferably a monomer represented by the following formula (2).
[0022] [ka]
[0023] (In formula (2), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and X is -O- or -NR 2 -, n is an integer from 1 to 8, m is an integer from 1 to 5, and R 2 , R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. The amphoteric monomer A may be used alone or in combination of two or more kinds.
[0024] In order to increase the transmittance of light with a wavelength of 550 nm of a 1% by mass aqueous solution of the amphoteric polymer at 80°C, the amphoteric polymer preferably contains 80 to 100% by mass, more preferably 90 to 100% by mass, and even more preferably 95 to 100% by mass of structural units derived from the amphoteric monomer A relative to the total mass of the amphoteric polymer.
[0025] Since a 1% by mass aqueous solution of the amphoteric polymer has a high transmittance for light having a wavelength of 550 nm at 80°C, it is preferable that the amphoteric polymer further contains a structural unit derived from an ethylenically unsaturated monomer B other than the amphoteric monomer A. In terms of easy availability, the amphoteric polymer is preferably at least one of (meth)acrylates and (meth)acrylamides in which the ethylenically unsaturated monomer B has a hydroxy group or a tertiary amide bond. During polymerization of the amphoteric monomer A, the ethylenically unsaturated monomer B can be copolymerized in a ratio described below.
[0026] (Ethylenically unsaturated monomer B) The ethylenically unsaturated monomer B is a monomer other than the zwitterionic monomer A. As the ethylenically unsaturated monomer B, general (meth)acrylates and vinyl monomers can be used. Among them, ethylenically unsaturated monomers having a hydroxy group or a tertiary amide bond, which are highly soluble in water, are preferred because water can be used as a solvent when copolymerizing with the amphoteric monomer A. The number of hydroxy groups and tertiary amide bonds in one molecule of the ethylenically unsaturated monomer B is preferably 1 to 5, more preferably 1 to 3. Examples of the ethylenically unsaturated monomer B include (meth)acrylamides such as (meth)acryloylmorpholine; hydroxypropyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 3-hydroxypropyl (meth)acrylate; hydroxybutyl (meth)acrylate; glycerol mono(meth)acrylate; neopentyl glycol mono(meth)acrylate; hexamethylene glycol mono(meth)acrylate; trimethylolpropane mono(meth)acrylate; trimethylolethane mono(meth)acrylate; trimethylolpropane mono(meth)methacrylate; trimethylolethane mono(meth)methacrylate; (meth)acrylates such as acrylate, tetraethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, tetraethylene glycol mono(meth)acrylate, pentaerythritol mono(meth)acrylate, dipentaerythritol mono(meth)acrylate, tripentaerythritol mono(meth)acrylate, 1,3-butanediol mono(meth)acrylate, sorbitol mono(meth)acrylate, pentaerythritol-modified mono(meth)acrylate, and 1-hydroxy-4-cyclohexyl (meth)acrylate; and vinyl monomers such as butanediol monovinyl ether and pentaerythritol monovinyl ether. Among these, (meth)acryloylmorpholine and 2-hydroxyethyl (meth)acrylate are preferred because of their good solubility in water. These ethylenically unsaturated monomers B may be used alone or in combination of two or more.
[0027] Since a 1% by mass aqueous solution of the amphoteric polymer has a high transmittance for light with a wavelength of 550 nm at 80° C., the amphoteric polymer preferably contains 0 to 20% by mass, more preferably 0 to 15% by mass, and even more preferably 0 to 10% by mass of a structural unit derived from an ethylenically unsaturated monomer B other than the amphoteric monomer A, relative to the total mass of the amphoteric polymer.
[0028] The ratio of amphoteric monomer A to ethylenically unsaturated monomer B in the polymerization of the amphoteric polymer of the present invention is preferably 80 to 100 mass%, more preferably 90 to 100 mass%, of the amphoteric monomer A relative to the total mass of amphoteric monomer A and ethylenically unsaturated monomer B, from the viewpoint of increasing the visible light (wavelength 550 nm) transmittance at 80° C. of the aqueous dispersion of the amphoteric polymer. When the ratio of amphoteric monomer A relative to the total mass of amphoteric monomer A and ethylenically unsaturated monomer B is within the above range, the visible light (wavelength 550 nm) transmittance at 80° C. of the aqueous dispersion of the amphoteric polymer tends to be increased.
[0029] In the present invention, the weight average molecular weight means the absolute molecular weight obtained by separating a polymer using a size exclusion chromatograph and detecting the eluted components using a light scattering detector and a differential refractive index detector. The absolute molecular weight at each elution position (elution time or elution volume) is determined by using a light scattering detector and a differential refractive index detector in combination.
[0030] The weight average molecular weight in the present invention means a value measured by connecting a size exclusion chromatograph, a light scattering detector, and a differential refractive index detector all in series.
[0031] The amphoteric polymer is preferably for use in inkjet recording media or print recording media, since the print can be removed from the recording medium and the recording medium can be recycled.
[0032] ≪Composition≫ The composition of the present invention includes the zwitterionic polymer of the present invention. In addition to the zwitterionic polymer, the composition of the present invention may further include a solvent such as water or a mixture of water and a water-miscible organic solvent, and an ink. In addition, the composition may include other components described below as necessary.
[0033] The composition of the present invention, when prepared as a 1% by mass aqueous solution of the polymer, preferably has a transmittance at 30° C. of light with a wavelength of 550 nm of 0% or more and 5.0% or less, more preferably 0% or more and 4.0% or less. When the transmittance of the composition of the present invention for light with a wavelength of 550 nm at 30° C. is within the above range, the solubility of the amphoteric polymer in cold water (water at 30° C.) is reduced, improving the practicality at room temperature.
[0034] The composition of the present invention, when prepared as a 1% by mass aqueous solution of the polymer, preferably has a transmittance at 80° C. of light with a wavelength of 550 nm of 40% or more and 100% or less, more preferably 45% or more and 100% or less. When the transmittance of the composition of the present invention for light with a wavelength of 550 nm at 80°C is within the above range, the dissolution rate of the amphoteric polymer in warm water is increased, and when a composition layer is formed on a support using the composition, the support can be recycled by a simple process.
[0035] When the composition of the present invention is prepared as a 1% by mass aqueous solution of the polymer, the difference in transmittance, expressed as [transmittance of light with a wavelength of 550 nm at 80°C] - [transmittance of light with a wavelength of 550 nm at 30°C], is preferably 40% or more and 100% or less, and more preferably 45% or more and 100% or less. If the difference in transmittance is within the above range, when a composition layer is formed on a support using the composition, a sufficient difference can be provided between the solubility in cold water and the solubility in hot water, which makes the composition insoluble in cold water but easily soluble in hot water, thereby preventing inconvenience such as dissolution in cold water during use of the composition layer at room temperature, and enabling the support to be recycled by a simple method using hot water.
[0036] (solvent) Examples of water-miscible organic solvents include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; polyalkylene glycols such as ethylene glycol, diethylene glycol, and propylene glycol; alkyl ethers such as polyalkylene glycol; and lactams such as N-methyl-2-pyrrolidone.
[0037] (ink) The ink may contain a colorant, such as a pigment or a dye.
[0038] (Other ingredients) Other ingredients may be added to the compositions of the present invention. Such other ingredients include, for example, fillers, amorphous silica, crystalline silica, aluminum trihydrate, kaolin, talc, chalk, bentonite, zeolite, glass beads, calcium carbonate, potassium sodium aluminum silicate, diatomaceous earth, aluminum and magnesium silicates, and mixtures thereof. Titanium dioxide may also be used for some applications. Organic particulates that may be used include polyolefins, polystyrene, polyurethanes, starch, poly(methyl methacrylate), and polytetrafluoroethylene.
[0039] Furthermore, within the scope not impairing the effects of the present invention, plasticizers, weathering agents, antioxidants, heat stabilizers, lubricants, antistatic agents, brightening agents, colorants, conductive agents, release agents, surface treatment agents, viscosity adjusters, fillers, and the like may be blended as necessary.
[0040] In terms of obtaining good solubility of the composition in warm water, the content of the amphoteric polymer in the composition of the present invention is preferably 0.01 to 99 mass%, more preferably 0.05 to 95 mass%, and even more preferably 0.1 to 90 mass%, of the total amount of the composition. In order to improve the dispersion stability of the zwitterionic polymer, when the composition of the present invention contains a solvent, the content of the solvent is preferably 1 to 99 mass %, more preferably 5 to 95 mass %, and even more preferably 10 to 90 mass %, of the total amount of the composition. In order to improve the dispersion stability of the zwitterionic polymer, when the composition of the present invention contains water as a solvent, the content of water is preferably 5 to 99 mass%, more preferably 10 to 95 mass%, and even more preferably 20 to 90 mass%, of the total amount of the composition. In order to improve the dispersion stability of the zwitterionic polymer, when the composition of the present invention contains a water-miscible organic solvent as a solvent, the content of the water-miscible organic solvent is preferably 1 to 99 mass%, more preferably 5 to 95 mass%, and even more preferably 10 to 90 mass%, of the total amount of the composition. In order to improve the dispersion stability of the amphoteric polymer, when the composition of the present invention contains ink, the content of the ink is preferably 0.0001 to 5 mass %, more preferably 0.001 to 3 mass %, and even more preferably 0.01 to 1 mass %, of the total amount of the composition. In order to improve the dispersion stability of the zwitterionic polymer, when the composition of the present invention contains other components, the total content of the other components is preferably 0.0001 to 5 mass%, more preferably 0.001 to 3 mass%, and even more preferably 0.01 to 1 mass%, of the total amount of the composition. In the composition of the present invention, the total content of each component does not exceed 100% by mass of the total amount of the composition.
[0041] ≪Composition layer≫ The composition layer of the present invention is a layer formed from a composition containing the zwitterionic polymer of the present invention.
[0042] Inkjet recording medium The zwitterionic polymer of the present invention may be used in any layer of the inkjet recording medium. By inkjet recording medium is meant the entire composition that receives the inkjet ink, any individual layer or combination of individual layers of the entire composition, prints of these compositions with the inkjet ink, and the inkjet ink. The inkjet recording medium of the present invention may also have one or more than one ink-receiving layer. The zwitterionic polymer of the present invention may be used in one or more than one receiving layer. The ink jet recording medium of the present invention may have an ink-receiving layer, a protective coating layer, a support, and a barrier layer.
[0043] <Print recording media> The zwitterionic polymers of the present invention can be used in any layer of the print recording medium. The print recording medium includes the entire composition that receives the printing ink, any individual layer or combination of individual layers of the entire composition, the print of the printing ink, and the printing ink. The print recording medium of the present invention can also have one or more than one ink-receiving layer. The zwitterionic polymers of the present invention can be used in one or more than one receiving layer. The print recording medium of the present invention may have an ink-receiving layer, a protective coating layer, a support, and a barrier layer. The print recording medium of the present invention can be used as a print recording medium for gravure printing, flexographic printing, and offset printing.
[0044] (Ink Receiving Layer) In the present invention, the ink-receiving layer means a layer that receives ink or an image-forming layer.
[0045] (Protective film layer) A protective coating layer in the present invention refers to a top coating or overcoat layer of inkjet and print recording media that can be used to provide specific properties as outlined above. The protective coating layer can usually be thin compared to the ink-receiving layer. The protective coating layer is usually present as the outermost layer, can allow ink penetration, and can be applied in subsequent lamination steps.
[0046] (Support) The support in the present invention means the base material of the inkjet recording medium. The support may be a naturally occurring or synthetic material, such as cellulose ester, cellulose acetate, polyester, polystyrene, polyethylene, poly(vinyl acetate), polypropylene, carbonate, polymethacrylic acid, and methyl and ethyl esters, polyamides such as nylon, polyesters such as poly(ethylene terephthalate), polyimides, polyethers, polyvinyl chloride, polysulfonamides, silicones, glass, and stainless steel. The support itself may also be an inkjet ink receiving layer. In this case, the amphoteric polymer may be directly coated on the support.
[0047] (Barrier layer) The barrier layer in the present invention is used between the support and the ink receiving layer. The barrier layer may be, for example, a polyolefin or a metal foil such as an aluminum foil.
[0048] (Application method) The amphoteric polymers of the present invention can be applied to a substrate for use in an ink jet recording medium by any known method, including, for example, Mayer bar coating, reverse roll coating, roller coating, wire bar coating, dip coating, air knife coating, slide coating, curtain coating, knife coating, flexographic coating, wound wire coating, slot coating, slide hopper coating and gravure coating.
[0049] The zwitterionic polymers or copolymers thereof of the present invention can be used in admixture with a wide variety of polymers or oligomers, neutral, anionic and cationic polyvinyl alcohols, and gelatin, for example, used in ink jet recording media.
[0050] Polymers used in inkjet recording media and commonly used in ink-receiving layers include gelatin, starch, styrene butadiene rubber latex, nitrile butadiene rubber latex, polyethylene glycol, polyacrylamide, polyvinyl alcohol, vinyl alcohol / vinyl acetate copolymers, methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl ethyl cellulose, hydroxymethyl cellulose, carboxymethyl cellulose, and poly(N-vinylpyrrolidone).
[0051] The zwitterionic polymers of the present invention can also be used as components of ink-jet inks.
[0052] Inks for inkjet printing are well known. These inks comprise a liquid vehicle and a dye or pigment dissolved or suspended therein. The liquid vehicles used include water or mixtures of water and water-miscible organic solvents. The ink may also be a vehicle for additives or other components to be incorporated into the recording medium.
[0053] <Method for producing amphoteric polymer> The amphoteric polymer of the present invention can be obtained by polymerizing a monomer containing one or more types of amphoteric monomer A. The polymerization method for the amphoteric polymer in the present invention is not particularly limited, and can be carried out by a known method such as solution polymerization, emulsion polymerization, suspension polymerization, etc. The polymerization reaction is not particularly limited as long as it is carried out under conditions in which radicals are generated.
[0054] When solution polymerization is carried out, it is preferable to use water as the solvent from the viewpoint of the solubility of the amphoteric monomer A. When an ethylenically unsaturated monomer B having low solubility in water is copolymerized, an alcohol solvent such as methanol or ethanol may be used in combination with water.
[0055] The method of generating radicals is not particularly limited, and may be, for example, a method of irradiating with radiation such as ultraviolet rays, gamma rays, or electron beams, or may be a method of using a radical initiator used in normal radical polymerization. The reaction temperature of the polymerization reaction is also not particularly limited, and is usually, for example, about 15 to 150°C. When using a radical initiator, examples of the radical initiator include bis(fluoroacyl)peroxides, bis(chlorofluoroacyl)peroxides, dialkyl peroxydicarbonates, diacyl peroxides, peroxyesters, azo compounds, and persulfates. Since the solvent in which the amphoteric monomer A dissolves is mainly water, it is preferable to use a radical initiator that has high solubility, dispersibility, and stability in water.
[0056] <Method for producing composition> The method for producing the composition of the present invention is not particularly limited, and for example, a production method in which each component is stirred with a conventional stirrer can be mentioned.
[0057] <<Method for producing composition layer>> The method for producing the composition layer of the present invention is not particularly limited, and any known method can be used. Examples of known methods include a method of coating the composition of the present invention on a support by Mayer bar coating, reverse roll coating, roller coating, wire bar coating, dip coating, air knife coating, slide coating, curtain coating, knife coating, flexo coating, wound wire coating, slot coating, slide hopper coating, and gravure coating, and then drying to produce a composition layer.
[0058] ≪How to use≫ The method of using the composition layer of the present invention is not particularly limited, and for example, when a support having the composition layer of the present invention on its surface is immersed in warm water at 80°C or more and 100°C or less for 30 minutes, only the composition layer dissolves, and the composition layer is removed from the support. This allows the support to be recycled. The recycled regenerated support may be reused as a support in the method for producing the composition layer.
[0059] ≪Applications≫ In order to impart solubility in warm water to the inkjet recording medium, the inkjet recording medium of the present invention preferably has a coating layer (protective coating layer) containing the amphoteric polymer. Since the print can be removed by immersing the inkjet recording medium in warm water, it is preferable that the inkjet recording medium of the present invention has one or more of an inkjet ink receiving layer and a protective coating layer on a support, and that one or more of the inkjet ink receiving layer and the protective coating layer contain the amphoteric polymer. In order to prevent the ink-jet ink-receiving layer from penetrating into the support and reducing its solubility in warm water, it is preferable that the ink-jet recording medium of the present invention has a barrier layer between the support and the ink-jet ink-receiving layer. In view of being a versatile material, the support of the inkjet recording medium and print recording medium of the present invention preferably comprises one or more of cellulose ester, cellulose acetate, polyester, polystyrene, polyethylene, poly(vinyl acetate), polypropylene, polycarbonate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyamide, polyimide, polyether, polyvinyl chloride, polysulfonamide, silicone, glass, and stainless steel. The inkjet recording medium and print recording medium of the present invention can be produced by any known method, such as Mayer bar coating, reverse roll coating, roller coating, wire bar coating, dip coating, air knife coating, slide coating, curtain coating, knife coating, flexographic coating, wound wire coating, slot coating, slide hopper coating, and gravure coating. The ink-jet ink of the present invention preferably contains the amphoteric polymer, since this makes it possible to impart solubility in warm water to the ink. The ink-jet ink of the present invention can be produced, for example, by stirring the composition of the present invention with the above-mentioned vehicle, dye and pigment using a conventional stirrer. From the viewpoint of recycling the support, it is preferable that the composition of the present invention is such that when a support having a composition layer containing the amphoteric polymer on its surface is immersed in warm water of 80°C or higher and 100°C or lower for 30 minutes, the composition layer dissolves from the support.
[0060] <Reasons why the present invention is effective> The reason why the present invention is effective is presumed to be as follows. In the present invention, since an amphoteric polymer exhibiting UCST-type phase separation is used, when the polymer coating is immersed in water at or above its critical point, the polymer coating dissolves, and the ink printed on the coating can be applied. The critical point depends on the molecular weight and composition of the amphoteric polymer, and the smaller the molecular weight, the lower the critical point. Therefore, in consideration of using the polymer without dissolving in water in a general living environment, it is preferable for the polymer to have a molecular weight that is not soluble in water at 30°C. Therefore, the amphoteric polymer of the present invention has a weight-average molecular weight within a specific range, and is therefore difficult to dissolve in water at 30°C, and is easily soluble in warm water at 80°C. EXAMPLES
[0061] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The measurement methods and evaluations of various measured values shown in this specification were performed as follows.
[0062] (1) Weight average molecular weight Mw The weight average molecular weight Mw was measured using a size exclusion chromatograph (GPC) (Viscotek, GPCmax-TDA302) equipped with a light scattering detector and a differential refractive index detector under the following conditions. Guard column: Shodex OHpak SB-G 6B (6.0mmI.D. x 50mm). Column: Shodex OHpak SB-806M HQ (8.0mmI.D. x 300mm). Mobile phase: 0.1M aqueous sodium nitrate solution. Column and detector temperature: 40°C. Flow rate: 0.5mL / min. Sample concentration: 1 mg / mL (mobile phase). Injection volume 100 μL. The weight-average molecular weight (Mw) was measured by weighing 20 mg of sample into a 20 mL measuring flask, adding mobile phase up to 80% of the volume, and leaving it to stand overnight to dissolve the sample. The sample was confirmed to have dissolved by visual inspection, and mobile phase was added up to the marked line. The sample was filtered through an aqueous disk filter with a pore size of 0.45 μm, placed in a vial, and subjected to measurement. In addition, 10 mL of the mobile phase was added to a vial containing polyethylene oxide standard (Viscotek, molecular weight 24,000) for calibration of the apparatus using a whole pipette, and the mixture was left to dissolve at room temperature overnight or longer.
[0063] (2) Coating adhesion to substrate The evaluation sample was prepared as follows. 1 g of the polymer prepared based on the examples and comparative examples described later and 9 g of ion-exchanged water were added to a glass bottle equipped with a stirrer, and the mixture was stirred for 10 minutes while being heated to 80°C. The prepared solution was bar-coated (wet film thickness 150 μm) onto a slide glass (76 mm x 26 mm) that had been treated with ultraviolet light / ozone for 30 minutes using a UV-208 ultraviolet ozone cleaning device manufactured by Technovision Co., Ltd. The bar-coated slide glass was dried on a hot plate at 60°C for 30 minutes to prepare an evaluation sample. The sample was cooled to room temperature to prepare an evaluation sample. The adhesion to the substrate was evaluated according to the cross-cut method according to JIS K 5600. When no peeling of the coating was observed, it was marked as "good", and when peeling of the coating was observed, it was marked as "x".
[0064] (3) Visible light transmittance of aqueous polymer solution The visible light transmittance of the polymer aqueous solution was measured using a UV-3100PC manufactured by Shimadzu Corporation equipped with a cell temperature regulator. The sample for measurement was prepared by adding 1 g of a polymer prepared based on the Examples and Comparative Examples described below and 9 g of ion-exchanged water to a glass bottle equipped with a stirrer, stirring for 10 minutes while heating to 80°C, and then cooling to room temperature to prepare a sample for evaluation. 0.7 mL of the sample was added to a quartz cell with a lid, and the cell was attached to a UV-3100PC manufactured by Shimadzu Corporation. The chiller for temperature control was set to a predetermined measurement temperature (30°C or 80°C), and the sample was allowed to settle within a range where the variation in the visible light transmittance was within ±5%, after which the cell was taken out once, shaken, and then attached to the device again before measurement. The value at a wavelength of 550 nm was read from the obtained visible light transmittance.
[0065] (4) Total light transmittance of polymer coating The total light transmittance of the polymer coating film was measured in accordance with JIS K 7136 using a haze meter manufactured by Nippon Denshoku Industries Co., Ltd., under the trade name "NDH2000."
[0066] (5) Removability of ink from polymer coating The ink shedding on the polymer coating was evaluated as follows. After measuring the total light transmittance of a glass slide (76 mm x 26 mm), an evaluation sample was prepared in the same manner as in (2) Adhesion of the coating to the substrate, and the total light transmittance was measured. Then, a 25 mm square was drawn on the polymer coating with a black oil-based pen, and the total light transmittance of the blackened area was measured. The glass slide was immersed in hot water at 60°C, and the water bath was stirred with a magnetic stirrer. After 1 hour, the glass slide was removed, and the total light transmittance of the blackened area where the blackened square was drawn with a black oil-based pen was measured. If the total light transmittance after immersion in the water bath was 90% or more of the total light transmittance of the glass slide, it was marked as "good", and if it was less than 90%, it was marked as "bad".
[0067] (6) Overall evaluation If all three of the following conditions were met, it was marked as "O", and if any one of them was not met, it was marked as "X". (i) The transmittance of a 1% by mass aqueous solution of the polymer at 30° C. for light with a wavelength of 550 nm is in the range of 0% to 5.0%, and therefore the solubility of the amphoteric polymer is low and favorable. (ii) The transmittance of a 1% by mass aqueous solution of the polymer at 80° C. for light with a wavelength of 550 nm is 40% or more and 100% or less, and therefore the dissolution rate of the amphoteric polymer is fast and favorable. (iii) Ink removal rating: “Good”.
[0068] The abbreviations for the raw materials used in the examples and comparative examples are as follows. DMAPS: 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid (Tokyo Chemical Industry Co., Ltd.). HEMA: 2-hydroxyethyl methacrylate (Tokyo Chemical Industry Co., Ltd.). ACMO: acryloylmorpholine (KJ Chemicals, Inc.). APS: Ammonium persulfate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0069] Example 1 7.5g of DMAPS and 50.7g of ion-exchanged water were weighed into a 100mL three-neck flask, and DMAPS was dissolved by adding a stirrer and stirring with a magnetic stirrer. Dry nitrogen was bubbled at 150mL / min for 30 minutes, and then 0.037g of APS was added to the flask and stirred until APS was dissolved. The flask was then immersed in a water bath at 60°C and stirred for 6 hours. The reaction solution obtained was then reprecipitated in 1L of methanol, and the precipitated white viscous solid was filtered off. The white viscous solid obtained was air-dried and then dried at 80°C to obtain an amphoteric polymer. Various evaluations were performed on the obtained amphoteric polymer. The results are shown in Table 1.
[0070] Example 2 An amphoteric polymer was obtained and various evaluations were carried out in the same manner as in Example 1, except that 0.2 g of HEMA was further added. The evaluation results are shown in Table 1.
[0071] Example 3 An amphoteric polymer was obtained and various evaluations were carried out in the same manner as in Example 1, except that 0.4 g of HEMA was further added. The evaluation results are shown in Table 1.
[0072] Example 4 An amphoteric polymer was obtained and various evaluations were carried out in the same manner as in Example 1, except that 0.2 g of ACMO was further added. The evaluation results are shown in Table 1.
[0073] Example 5 An amphoteric polymer was obtained and various evaluations were carried out in the same manner as in Example 1, except that 0.4 g of ACMO was further added. The evaluation results are shown in Table 1.
[0074] Comparative Example 1 A polymer was obtained and various evaluations were performed in the same manner as in Example 1, except that 10 g of HEMA was used instead of 7.5 g of DMAPS, the amount of ion-exchanged water used was 153.7 g, the amount of APS used was 0.105 g, and the amount of methanol used in the reprecipitation was 3 L. The evaluation results are shown in Table 2.
[0075] Comparative Example 2 A polymer was obtained and various evaluations were performed in the same manner as in Example 1, except that 10 g of ACMO was used instead of 7.5 g of DMAPS, the amount of ion-exchanged water used was 147.7 g, the amount of APS used was 0.101 g, and the amount of methanol used in the reprecipitation was 3 L. The evaluation results are shown in Table 2.
[0076] Comparative Example 3 An amphoteric polymer was obtained and various evaluations were carried out in the same manner as in Example 1, except that 1.1 g of DMAPS, 4.2 g of acrylamide, and 1.8 g of methoxy PEG350 methacrylate were used instead of 7.5 g of DMAPS in Example 1, the amounts of ion-exchanged water and APS used were 50.1 g and 0.042 g, respectively, and the amount of methanol used in the reprecipitation was 3 L. The evaluation results are shown in Table 2.
[0077] [Table 1]
[0078] [Table 2]
[0079] From Table 1, it can be seen that Examples 1 to 5, which used amphoteric polymers consisting of components specified in the present invention, were excellent in all evaluations. In contrast, it can be confirmed that those that do not satisfy the elements specified in the present invention have poor adhesion to the substrate, high solubility of the amphoteric polymer in water at 30°C, or a slow dissolution rate in water at 80°C, and are inferior in the evaluation of water immersion peelability of the ink on the amphoteric polymer coating film (Comparative Examples) (Comparative Examples 1 to 3).
[0080] As shown in Table 2, Comparative Example 1 used a polymer that had a low transmittance of light with a wavelength of 550 nm when dissolved in a 1% by mass aqueous solution at 80° C., so the polymer became insoluble in hot water and a coating film could not be produced, and the removability of the ink on the polymer coating film could not be evaluated. Comparative Examples 2 and 3 used a polymer that had a high transmittance of light with a wavelength of 550 nm when dissolved in a 1% by mass aqueous solution at 30° C., so the solubility of the amphoteric polymer in water at 30° C. was high and poor, and the overall evaluation was poor. [Industrial Applicability]
[0081] According to the amphoteric polymer defined in the present invention, oil-based inks printed on a substrate coated with the amphoteric polymer can be removed by immersing the substrate in warm water. This means that the substrate can be deinked and recycled, which is extremely important from the industrial point of view.
Claims
1. A zwitterionic polymer having one or more types of structural units derived from zwitterionic monomer A, the zwitterionic polymer having a weight average molecular weight of 1,000,000 or more and 10,000,000 or less, a 1% by mass aqueous solution of the zwitterionic polymer having a light transmittance of 0% or more and 5.0% or less at 30°C for light with a wavelength of 550 nm, and a 1% by mass aqueous solution of the zwitterionic polymer having a light transmittance of 40% or more and 100% or less at 80°C for light with a wavelength of 550 nm.
2. The amphoteric polymer according to claim 1 , wherein the amphoteric monomer A is represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and X is -O- or -NR 2 - and Y + Ha-S + R 3 -or-N + R 4 R 5 - and Z - Ha-SO 3 - Or -PO 2 (OR 6 ) - where n is an integer from 1 to 8, m is an integer from 1 to 5, and R 2 , R 3 , R 4 , R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
3. The amphoteric polymer according to claim 1 or 2, wherein the amphoteric monomer A is represented by the following formula (2): 【Chemistry 2】 (In formula (2), R 1 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and X is -O- or -NR 2 -, n is an integer from 1 to 8, m is an integer from 1 to 5, and R 2 , R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
4. The amphoteric polymer according to claim 1 or 2, further comprising a constituent unit derived from an ethylenically unsaturated monomer B other than the amphoteric monomer A.
5. The amphoteric polymer according to claim 4, wherein the ethylenically unsaturated monomer B is at least one of (meth)acrylates and (meth)acrylamides having a hydroxy group or a tertiary amide bond.
6. 3. The amphoteric polymer according to claim 1, which comprises 80 to 100% by mass of structural units derived from the amphoteric monomer A based on the total mass of the amphoteric polymer.
7. 3. The amphoteric polymer according to claim 1, which comprises 0 to 20 mass% of a constituent unit derived from an ethylenically unsaturated monomer B other than the amphoteric monomer A, based on the total mass of the amphoteric polymer.
8. 3. The amphoteric polymer according to claim 1, which is for use in an inkjet recording medium.
9. 13. An inkjet recording medium comprising at least one composition layer comprising a composition containing the amphoteric polymer according to claim 1 on a support.
10. 10. The inkjet recording medium according to claim 9, wherein the composition layer is at least one layer selected from the group consisting of an inkjet ink receiving layer and a protective coating layer.
11. at least one of the composition layers is an ink-jet ink-receiving layer; The inkjet recording medium of claim 10, further comprising a barrier layer between the support and the inkjet ink receiving layer.
12. The inkjet recording medium according to any one of claims 9 to 11, wherein the support comprises at least one material selected from the group consisting of cellulose ester, cellulose acetate, polyester, polystyrene, polyethylene, poly(vinyl acetate), polypropylene, polycarbonate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyamide, polyimide, polyether, polyvinyl chloride, polysulfonamide, silicone, glass, and stainless steel.
13. 3. The amphoteric polymer according to claim 1, which is for use in a print recording medium.
14. An ink-jet ink comprising the amphoteric polymer according to claim 1 or 2.
15. 3. A composition comprising the amphoteric polymer according to claim 1 or 2, wherein when a support having a composition layer formed from the composition on its surface is immersed in warm water having a temperature of 80°C or higher and 100°C or lower for 30 minutes, the composition layer dissolves from the support.
Citation Information
Patent Citations
Modification of Solid Surfaces with Polymer Combinations
JP2009528440A
Hydrophilic sheet
JP2019130667A
Hydrophilic structure and production method for hydrophilic structure