Alloy member, electrochemical module, solid oxide fuel battery, solid oxide electrolyte cell, and manufacturing method of the electrochemical module
The described method addresses the lack of synergistic effect in existing protective film formation by using batch heat treatment to form a Co or Co-Ni plating layer on alloy members, resulting in an electrochemical module with low resistance and improved durability for solid oxide fuel and electrolytic cells.
Patent Information
- Application Number
- JP2023043436
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing methods for forming protective films on alloy members in solid oxide fuel cells and electrolysis cells fail to achieve a synergistic effect between the adhesive layer and the protective film due to separate heat treatments, limiting performance improvement.
A method involving batch heat treatment at 650°C to 800°C forms a Co or Co-Ni plating layer on alloy members made of ferritic stainless steel, simultaneously bonding the alloy member with electrochemical elements, creating an oxide film and plating layer to suppress chromium volatilization and maintain low internal resistance.
This approach results in an electrochemical module with low resistance and improved durability by effectively suppressing chromium volatilization and maintaining low internal resistance over time, enhancing the performance of solid oxide fuel cells and electrolytic cells.
Smart Images

Figure 2024132600000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an alloy member for use in a solid oxide fuel cell or a solid oxide electrolysis cell, an electrochemical module, and a method for producing an electrochemical module. [Background technology]
[0002] Under the slogan of Goal 7 of the Sustainable Development Goals (SDGs), "Affordable and clean energy," electrochemical devices such as solid oxide electrolysis cells (SOECs), which generate hydrogen and oxygen through the electrolysis of water vapor and carbon dioxide, and solid oxide fuel cells (SOFCs), which generate electricity using fuel gases such as hydrogen and air, are attracting attention.
[0003] SOECs and SOFCs are configured to include single cells (electrochemical elements) each having a fuel electrode on one end and an air electrode on the other end of a solid electrolyte, and alloy members such as inter-cell connectors provided between the single cells. Specifically, for example, an electrochemical element is sandwiched between and electrically connected to a metallic fuel electrode-side alloy member arranged on the fuel electrode side of the electrochemical element and a metallic air electrode-side alloy member arranged on the air electrode, and the electrochemical elements are stacked in this order to form a cell stack.
[0004] Ferritic stainless steel is generally used as the base material of the alloy member. The alloy member is exposed to high temperatures during the cell manufacturing process and during use of the cell, so Cr contained in the ferritic stainless steel precipitates on the surface as Cr2O3. In order to prevent the volatilization of this Cr2O3 and Cr poisoning of the air electrode, attempts have been made to form a protective film.
[0005] Patent Document 1 describes a solid oxide fuel cell in which a protective film made of ZnCo2O4 is formed as a spinel-type oxide coating on the surface of a substrate of an interconnector. This solid oxide fuel cell is formed by coating a slurry that is the base of the protective film, heat treating it, and then applying an adhesive layer and heat treating it. It describes that this method of formation makes it possible to form a protective film that is highly resistant to peeling and suppresses an increase in resistance.
[0006] In Patent Document 2, x Mn 3-x The paper discloses an SOFC inter-cell connection member provided with a protective film of a spinel-type oxide made of O4. This inter-cell connection member is also formed by coating a slurry that is the base of the protective film, heat treating it, and then applying an adhesive layer and heat treating it. It is described that the inter-cell connection member having such a protective film can further suppress the volatilization of Cr2O3 that precipitates on the surface by having the protective film. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-118177 A [Patent Document 2] JP 2013-118178 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in these prior art documents, the protective film is formed by heat treatment, and then an adhesive layer is applied and heat treated in a stepwise manner. Therefore, the components of the adhesive layer do not diffuse into the protective film by heat treatment of the adhesive layer, and it is difficult to expect a synergistic effect between the raw materials of the adhesive layer and the raw materials of the protective film. Therefore, with such a method for producing electrochemical modules such as SOEC and SOFC, further improvement in the performance of these electrochemical modules cannot be expected.
[0009] The present invention aims to obtain an electrochemical module for SOEC and SOFC having low resistance performance by a lump-sum heat treatment at a relatively low temperature. [Means for solving the problem]
[0010] The method for producing an electrochemical module according to the present invention for achieving the above object comprises the steps of: a plating layer forming step of forming a plating layer made of a Co plating layer or a Co-Ni plating layer on the other side surface of the substrate of an alloy member made of ferritic stainless steel, the alloy member being used in a solid oxide fuel cell or a solid oxide electrolysis cell, in a state in which one side surface of the substrate is in an atmosphere in contact with a fuel gas and the other side surface of the substrate is in an atmosphere in contact with an oxygen-containing gas; The present invention has a stacking process in which a bonding material is interposed between the alloy member and an electrochemical element having a single cell formed by sandwiching an electrolyte layer between an electrode layer and a counter electrode layer, and a heat treatment is performed at a temperature of 650°C or more and 800°C or less.
[0011] According to this characteristic configuration, a plating layer made of a Co plating layer or a Co-Ni plating layer having electronic conductivity and an effect of suppressing Cr volatilization can be formed on the other side of the substrate at a relatively low cost and without requiring high-temperature heat treatment (for example, heat treatment at a temperature exceeding the temperature (for example, a temperature exceeding 800°C) at which the alloy member is used in a solid oxide fuel cell or a solid oxide electrolysis cell). Furthermore, according to the above-described characteristic configuration, by interposing a bonding material between the alloy member on which a plating layer is formed and an electrochemical element having a single cell formed by sandwiching an electrolyte layer between an electrode layer and a counter electrode layer, and performing heat treatment at a temperature of 650°C or higher and 800°C or lower, it is possible to simultaneously perform firing of the bonding material that bonds the alloy member and the electrochemical element and reaction of the bonding material with the plating layer. According to the above characteristic configuration, an alloy member can be obtained by a collective heat treatment at a relatively low temperature, which includes an oxide film having a thickness of 0.2 μm or more and 0.8 μm or less on the other side surface of the substrate, and a plating layer having a thickness of 2.0 μm or more and 3.0 μm or less on the oxide film. Therefore, as shown in the test results described later, it is possible to suppress the volatilization of Cr from the other side surface of the substrate and suppress the deterioration of performance over a long period of time, and even if an oxide film is present, it is possible to maintain the internal resistance at an acceptably low level. Therefore, according to the above characteristic configuration, an electrochemical module having an alloy member for SOEC and SOFC and an electrochemical element having low resistance performance can be obtained by a collective heat treatment at a relatively low temperature.
[0012] A further characteristic configuration of the manufacturing method of the electrochemical module according to the present invention is as follows: The heat treatment in the stacking process forms an oxide film having a thickness of 0.2 μm or more and 0.8 μm or less on the other side of the base material, and forms the plating layer having a thickness of 2.0 μm or more and 3.0 μm or less on the oxide film.
[0013] According to this characteristic configuration, as shown in the test results described below, it is possible to suppress the volatilization of Cr from the other side of the substrate over a long period of time, and even when an oxide film is present, it is possible to maintain the internal resistance at an acceptably low level.
[0014] A further characteristic configuration of the manufacturing method of the electrochemical module according to the present invention is as follows: The point is that after the heat treatment in the stacking step, the bonding material has a structure in which a plurality of fine particles having an average particle size of 0.1 μm or more and 0.2 μm or less are aggregated together in a state in which the alloy member and the unit cell are bonded together.
[0015] According to this characteristic configuration, after the heat treatment in the stacking process, the bonding material has a structure in which multiple microparticles having an average particle size of 0.1 μm or more and 0.2 μm or less are aggregated when the alloy member and the single cell are bonded together, so that low resistance performance and high adhesion performance can be ensured even with a batch heat treatment at a relatively low temperature.
[0016] A further characteristic configuration of the manufacturing method of the electrochemical module according to the present invention is as follows: The plating layer forming step includes a step of forming a strike plating layer of Co or Ni on the other side surface of the base material before forming the plating layer.
[0017] According to this characteristic configuration, a plating layer can be formed on top of a strike plating layer of Co or Ni, thereby effectively preventing the formed plating layer from peeling off from the other side surface of the substrate.
[0018] The alloy member according to the present invention for achieving the above object has the following characteristic configuration: An alloy member used in a solid oxide fuel cell or a solid oxide electrolysis cell, in a state where one side of a substrate is in an atmosphere in contact with a fuel gas and the other side of the substrate is in an atmosphere in contact with an oxygen-containing gas, comprising: an oxide coating having a thickness of 0.2 μm or more and 0.8 μm or less on the other side surface of the base material; The metal plated layer has a thickness of 2.0 μm or more and 3.0 μm or less and is provided on the oxide film.
[0019] According to this characteristic configuration, as shown in the test results described below, it is possible to suppress the volatilization of Cr from the other side of the substrate over a long period of time, thereby suppressing deterioration in performance, and even when an oxide coating is present, it is possible to maintain the internal resistance at an acceptably low level. Therefore, according to the above characteristic configuration, an alloy member for SOEC and SOFC having low resistance performance can be obtained. If the thickness of the oxide film is less than 0.2 μm, there is a risk of abnormal oxidation, such as the precipitation of iron oxide from the substrate, and if it is thicker than 0.8 μm, there is a risk of increased internal resistance. If the thickness of the plating layer is less than 2.0 μm, there is a risk of the Cr volatilization suppression effect being insufficient, and if it is thicker than 3.0 μm, there is a risk of increased resistance and reduced performance.
[0020] The electrochemical module according to the present invention for achieving the above object has the following characteristic configuration: The alloy member is bonded to an electrochemical element having a single cell formed by sandwiching an electrolyte layer between an electrode layer and a counter electrode layer, using a bonding material. Here, the oxide film of the alloy member may contain an oxide of Cr.
[0021] According to this characteristic configuration, as shown in the test results described below, it is possible to suppress the volatilization of Cr from the other side of the substrate to the electrode layer and electrolyte layer constituting the electrochemical element joined to the substrate over a long period of time, thereby suppressing the deterioration of performance, and even if an oxide film is present, it is possible to maintain the internal resistance at an acceptably low level. Therefore, according to the above characteristic configuration, an electrochemical module having an alloy member for SOEC and SOFC with low resistance performance and an electrochemical element can be obtained.
[0022] A further characteristic configuration of the electrochemical module according to the present invention is The bonding material has a structure in which a plurality of fine particles having an average particle size of 0.1 μm or more and 0.2 μm or less are aggregated when the alloy member and the unit cell are bonded together.
[0023] According to this characteristic configuration, the bonding material ensures high adhesion between the alloy member and the unit cell.
[0024] A further characteristic configuration of the electrochemical module according to the present invention is The plating layer contains Mn.
[0025] According to this characteristic configuration, the plating layer contains metals such as Mn diffused from the bonding material, making it a highly durable plating layer, which can suppress the volatilization of Cr from the other side surface of the base material and thus suppress the deterioration of performance over a long period of time.
[0026] In order to achieve the above object, a solid oxide fuel cell according to the present invention has a characteristic configuration in that it includes the above electrochemical module, and causes a power generation reaction in the unit cell.
[0027] According to the above-mentioned characteristic configuration, a power generation reaction can be carried out in a solid oxide fuel cell equipped with an electrochemical module that has excellent durability, reliability, and performance, so that a highly durable, high-performance solid oxide fuel cell can be obtained.
[0028] In order to achieve the above object, a solid oxide electrolysis cell according to the present invention has a characteristic configuration in that it includes the above electrochemical module and causes an electrolytic reaction in the single cell.
[0029] According to the above characteristic configuration, gas can be generated by an electrolytic reaction as a solid oxide electrolysis cell equipped with an electrochemical module that has excellent durability, reliability, and performance, so that a highly durable, high-performance solid oxide electrolysis cell can be obtained. [Brief description of the drawings]
[0030] [Figure 1] FIG. 1 is a schematic diagram of a solid oxide fuel cell. [Diagram 2] 1 is a cross-sectional view of an alloy member on which a strike plating layer and a plating layer are formed. FIG. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing a laminated state of an alloy member and an electrochemical element. [Figure 4] FIG. 4 is an enlarged view of the schematic cross-sectional view of FIG. [Diagram 5] FIG. 2 is an explanatory diagram of reactions during operation of a solid oxide fuel cell. [Figure 6] 1 shows SEM images and Cr mapping images obtained by an electron probe microanalyzer (EPMA) of the surfaces of the alloy members of (a) Example 1, (b) Example 2, and (c) Comparative Example 1. [Figure 7] 1 is a graph showing resistance values in a current test of electrochemical modules using the alloy members of Example 1, Example 2, and Comparative Example 1. [Figure 8]FIG. 2 is an explanatory diagram of reactions during operation of a solid oxide electrolysis cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The alloy member, electrochemical module, and manufacturing method of the electrochemical module used in the solid oxide fuel cell or solid oxide electrolysis cell according to the embodiment of the present invention will be described below. Note that although preferred embodiments are described below, each of these embodiments is described to more specifically illustrate the present invention, and various modifications are possible within the scope of the gist of the present invention, and the present invention is not limited to the following description.
[0032] FIG. 1 is a schematic diagram of a solid oxide fuel cell equipped with an electrochemical module C. FIG. 2 is a cross-sectional view of an inter-cell connection member 1 (an example of an alloy member) on which a strike plating layer 12 and a plating layer 13 are formed. FIG. 3 is a schematic explanatory diagram showing a stacked state of the inter-cell connection member 1 and an electrochemical element 3 (an example of a unit cell). FIG. 4 is an enlarged view of the schematic cross-sectional view of FIG. 3. FIG. 5 is an explanatory diagram of reactions during operation of a solid oxide fuel cell. 1 to 3, an electrochemical module C is configured by alternately joining inter-cell connection members 1 and electrochemical elements 3 configured by sandwiching an electrolyte membrane 30 (an example of an electrolyte layer) between a fuel electrode 31 (an example of an electrode layer) and an air electrode 32 (an example of a counter electrode layer). Specifically, the electrochemical elements 3 are formed by joining an air electrode 32 made of an oxygen ion and electron conductive porous body to one side of the electrolyte membrane 30 made of a dense body of oxygen ion conductive solid oxide, and joining a fuel electrode 31 made of an electron conductive porous body to the other side of the same electrolyte membrane 30.
[0033] The electrochemical module C has a structure in which an electrochemical element 3 is sandwiched between a pair of electronically conductive inter-cell connection members 1 in which grooves 2 are formed for donating and receiving electrons to the air electrode 32 or fuel electrode 31 and for supplying air (an example of an oxygen-containing gas) and hydrogen (an example of a fuel gas), with a gas seal held appropriately at the outer periphery. The air electrode 32 and the inter-cell connection members 1 are arranged in close contact with each other, so that the groove 2 on the air electrode 32 side functions as an air flow path 2b for supplying air to the air electrode 32. The fuel electrode 31 and the inter-cell connection members 1 are arranged in close contact with each other, so that the groove 2 on the fuel electrode 31 side functions as a fuel flow path 2a for supplying hydrogen to the fuel electrode 31.
[0034] In addition, to explain the general materials used for each element constituting the electrochemical element 3, for example, the material for the air electrode 32 can be a perovskite-type oxide of (La,AE)MO3 in which part of the La in LaMO3 (e.g., M=Mn, Fe, Co, Ni) is replaced with an alkaline earth metal AE (AE=Sr, Ca). The material of the fuel electrode 31 may be an electron-conductive porous material, such as a perovskite oxide of (La,AE)MO3 in which part of the La in LaMO3 (e.g., M=Mn, Fe, Co) is replaced with an alkaline earth metal AE (AE=Sr, Ca), or a cermet of Ni and yttria-stabilized zirconia (YSZ). Furthermore, the material of the electrolyte membrane 30 is preferably a dense body of a solid oxide having oxide ion conductivity, and examples of materials that can be used include ceria doped with a dopant such as gadolinia (GDC) and yttria-stabilized zirconia (YSZ).
[0035] Then, in a state where the electrochemical elements 3 are electrically connected to each other by the inter-cell connection members 1, i.e., in a state where the electrochemical elements 3 are stacked with the inter-cell connection members 1 sandwiched between them, the electrochemical elements 3 are clamped in the stacking direction by applying a pressing force with the bolts and nuts to form a cell stack. In this cell stack, the inter-cell connection members 1 arranged at both ends in the stacking direction need only have either the fuel flow path 2a or the air flow path 2b formed therein, and the other inter-cell connection members 1 arranged in the middle can have the fuel flow path 2a formed on one side and the air flow path 2b formed on the other side. In a cell stack having such a stacked structure, the inter-cell connection members 1 may be called separators, interconnectors, etc.
[0036] The cell stack is attached to a manifold that supplies fuel gas (hydrogen) by a bonding material such as a glass sealant. For example, crystallized glass is used as the glass sealant. The glass sealant is used for bonding the manifold and also for locations that require sealing, such as between the electrochemical element 3 and the inter-cell connection member 1. A solid oxide fuel cell having such a cell stack structure is generally called a flat plate solid oxide fuel cell. In this embodiment, a flat plate solid oxide fuel cell will be described as an example, but the present invention can also be applied to solid oxide fuel cells of other structures.
[0037] When a solid oxide fuel cell (cell stack) equipped with such an electrochemical module C and causing a power generation reaction in the electrochemical element 3 is in operation, as shown in FIG. 5, air is supplied to the air electrode 32 through the air flow path 2b formed in the adjacent inter-cell connection member 1, and hydrogen is supplied to the fuel electrode 31 through the fuel flow path 2a formed in the adjacent inter-cell connection member 1, and the cell stack operates at an operating temperature of, for example, about 800°C. Then, oxygen molecules O2 are converted into electrons e - reacts with oxygen ions O 2- is generated and its O 2- The O passes through the electrolyte membrane 30 and moves to the fuel electrode 31, and the H2 supplied at the fuel electrode 31 is converted to the O 2- reacts with H2O and e -As a result, an electromotive force E is generated between the pair of inter-cell connection members 1, and the electromotive force E can be extracted to the outside and utilized.
[0038] <Inter-cell connection material> The inter-cell connection member 1 is made of a metal substrate 11 (hereinafter, an example of a substrate) made of ferritic stainless steel, and has a groove 2 provided on its surface as shown in Fig. 1. The groove 2 includes a fuel flow path 2a that forms an atmosphere in which hydrogen comes into contact with one side surface of the metal substrate 11 (the surface facing the fuel electrode 31), and an air flow path 2b that forms an atmosphere in which air comes into contact with the other side surface of the metal substrate 11 (the surface facing the air electrode 32). Actually, the other side surface of the metal base 11 is bonded to the air electrode 32 via the bonding layer 15 (air electrode-side bonding layer 15b).
[0039] The metal substrate 11 is made of ferritic stainless steel, and generally contains metals such as Fe, Cr, and Mn.
[0040] A current collector may be provided on the inter-cell connection member 1. In this case, the current collector is disposed between the fuel electrode 31 and the inter-cell connection member 1, and the current collector is disposed between the air electrode 32 and the inter-cell connection member 1. As a result, the electrical connections between the inter-cell connection member 1 and the fuel electrode 31 and between the inter-cell connection member 1 and the air electrode 32 are reinforced.
[0041] <Oxide film on fuel electrode side> 3, one side surface (the surface facing the fuel electrode 31) of the metal substrate 11 of the cell-cell connection member 1 is provided with a fuel electrode-side oxide film 11a (not shown) formed inside the metal substrate 11. The fuel electrode-side oxide film 11a is a thin film layer containing an oxide of Cr and the like. As described later, the fuel electrode-side oxide film 11a is formed by firing at 650° C. or more and 800° C. or less in the heat treatment in the stacking step.
[0042] <Oxide film on the air electrode side> 3, the other side surface (the surface facing the air electrode 32) of the inter-cell connection member 1 is provided with an air electrode-side oxide coating 11b (an example of an oxide coating) formed inside the metal base material 11. The air electrode-side oxide coating 11b is a thin film layer containing oxides of Cr, Mn, etc. The thickness of the air electrode side oxide film 11b is 0.2 μm or more and 0.8 μm or less. As described later, the air electrode side oxide film 11b is formed by firing at 650° C. or more and 800° C. or less in the heat treatment in the stacking step.
[0043] <Strike plating layer> A strike plating layer 12 is provided on at least the other side surface of the metal base 11. The strike plating layer 12 is a thin plating layer containing Ni or Co. The strike plating layer 12 is provided to improve adhesion between a plating layer 13 formed on the strike plating layer 12 and the other side surface of the metal base 11. Therefore, when a plating layer described below can be plated with sufficient strength on the other side surface of the metal base 11, the strike plating layer 12 may be omitted. The strike plating layer 12 is generally obtained by a method in which the substrate is used as a cathode and immersed together with the anode in a bath containing Ni or Co with a low metal concentration, and plating is performed at a relatively high current density for a short period of time from a few seconds to a few minutes. The strike plating layer 12 may also be formed by vacuum deposition and sputtering of Ni, Co, etc. The strike plating layer 12 may contain Au, Ag, Cu, etc. in addition to Ni or Co.
[0044] <Plating layer> A plating layer 13 is provided on the strike plating layer 12 on the other side surface of the metal base 11. The plating layer 13 is a layer made of a Co plating layer or a Co-Ni plating layer. The plating layer 13 can be formed by immersing the metal base material 11 on which the strike plating layer 12 is provided as a cathode together with an anode such as SUS in a bath containing a salt such as Co, which serves as a precursor of the plating layer 13, or a salt of Co and a salt of Ni, and applying a voltage between the anode and the cathode to perform plating.
[0045] From the viewpoint of the possibility of abnormal oxidation such as precipitation of iron oxide from the base material and an increase in internal resistance, the thickness of the plating layer 13 is preferably 2.0 μm to 3.0 μm, more preferably 1.5 μm to 2.5 μm, and even more preferably 2.0 μm. If the plating layer is less than 2.0 μm thick, there is a risk that the effect of suppressing Cr volatilization may not be sufficiently obtained, and if it is thicker than 3.0 μm, there is a risk of increased resistance and reduced performance.
[0046] The plating layer 13 contains an oxide of Co and Mn, or an oxide of Co, Ni and Mn. It is considered that when the air electrode side bonding material contains Mn, which will be described later, the Mn in the air electrode side bonding material diffuses to the plating layer 13 side during the heat treatment in the stacking step and is oxidized, forming the oxide.
[0047] <Cathode side bonding layer> 3, on the other side surface of the metal base 11, an air electrode-side bonding layer 15b is provided on the plating layer 13 on the metal base 11. An enlarged view of this structure is shown in FIG. The air electrode-side bonding layer 15b is made of a composite material including NiO and LaCrO3 doped with at least one element selected from Sr, Ca, Mg, Ti, Zr, V, Mn, Fe, Co, Ni, Cu, Zn, Al, Ba, Mo, and Pb, and is provided to bond and electrically connect the metal substrate 11 and the electrochemical element 3. For the air electrode-side bonding layer 15b, an air electrode-side bonding material such as a perovskite-type oxide or a spinel-type oxide having a composition similar to that of the air electrode 32 can be used. In particular, the material of the bonding material of the air electrode side bonding layer 15b is preferably a material containing Co. Alternatively, the material of the bonding material is preferably a material containing Ni. Alternatively, the material of the bonding material is preferably a material containing a metal oxide containing at least two of Co, Mn, Cu, and Ni. Alternatively, the material of the bonding material is preferably a material containing a metal oxide containing Co and Mn as main components. Furthermore, the air electrode side bonding layer 15b (bonding material) has a structure in which a plurality of fine particles having an average particle size of 0.1 μm or more and 0.2 μm or less are assembled in a state in which the inter-cell connection member 1 and the electrochemical element 3 are bonded. In addition, the air electrode side bonding layer 15b (bonding material) preferably has a porosity of 60% or more in a state in which the inter-cell connection member 1 and the electrochemical element are bonded. Furthermore, it is more preferable that the porosity is 65% or more. In addition, the thickness of the air electrode side bonding layer 15b (bonding material) is not particularly limited, but from the viewpoint of cost-effectiveness, it is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less.
[0048] The air electrode side bonding layer 15b is formed by kneading the above-mentioned composite material with a solvent to prepare a slurry, applying the slurry to the other side of the metal substrate 11 to form the air electrode side bonding material layer 14b, and then firing the slurry at a temperature of 650°C or higher and 800°C or lower in the heat treatment of the stacking process, as described later.
[0049] <Electrochemical module> 1 is formed by alternately stacking multiple electrochemical elements 3 and metal substrates 11, with an air flow path 2b formed on the air electrode 32 side of the metal substrate 11 and a fuel flow path 2a formed on the fuel electrode 31 side of the metal substrate 11. Note that the metal substrates 11 arranged at both ends in the stacking direction need only have either the fuel flow path 2a or the air flow path 2b formed thereon, and the other intermediate metal substrates 11 may have the fuel flow path 2a formed on one side and the air flow path 2b formed on the other side. The electrochemical elements 3 constituting the electrochemical module C are stacked such that the fuel electrodes 31 and air electrodes 32 are arranged on the same side in the stacking direction. For example, when the metal substrates 11 and the electrochemical elements 3 are stacked alternately in the vertical direction, the fuel electrodes 31 are arranged on the upper side in the stacking direction, and the air electrodes 32 are arranged on the lower side in the stacking direction.
[0050] <Electrochemical module manufacturing process> Next, a method for manufacturing the electrochemical module C in this embodiment will be described. The manufacturing method of the electrochemical module C includes a plating layer formation step S101 of forming a plating layer 13 consisting of a Co plating layer or a Co-Ni plating layer on the other side of the metal substrate 11, and a stacking step S102 of performing a heat treatment at a temperature of 650°C or more and 800°C or less between the metal substrate 11 on which the plating layer 13 has been formed and the electrochemical element 3 having a single cell formed by sandwiching the electrolyte membrane 30 between the fuel electrode 31 and the air electrode 32, with a bonding material interposed between them.
[0051] More specifically, the plating layer formation step S101 includes a strike plating step of forming a strike plating layer 12 containing Co or Ni on at least the other side surface of the metal base material 11, and a step of forming a plating layer 13 consisting of a Co plating layer or a Co-Ni plating layer on the strike plating layer 12 on the other side surface of the metal base material 11.
[0052] Then, after the plating layer forming step S101, a stacking step S102 includes an air electrode side bonding material application step of applying an air electrode side bonding material onto the plating layer 13 on the other side of the metal base 11 to form an air electrode side bonding material layer 14b, and arranging an electrochemical element 3 on the anode side oxide film 11a on one side of the metal base 11 with the anode 31 in contact with the electrochemical element 3, and arranging another metal base 11 on the air electrode 32 of the electrochemical element 3 with the anode side bonding material layer 14b on the plating layer 13 on the other side of the metal base 11 in contact with the anode 32. This is repeated in sequence to stack a desired number of metal bases 11 and electrochemical elements 3 in sequence, and a step of heat treating at a temperature of 650°C to 800°C is performed. The electrochemical element 3 can be obtained by arranging the electrolyte membrane 30, the fuel electrode 31, and the air electrode 32 on one side and the other side of the electrolyte membrane 30, respectively, by a known method, and therefore a detailed description thereof will be omitted.
[0053] <Strike plating process> The strike plating process is a process for forming a strike plating layer 12 containing Co or Ni on at least the other surface of the cell-cell connection member 1. The strike plating layer 12 is formed by immersing the metal base material 11 in a solution containing a salt of Ni or Co, and performing plating treatment at a relatively high current density for a short period of time from a few seconds to a few minutes, using the metal base material 11 as the cathode and SUS or the like as the anode. Forming the strike plating layer 12 improves adhesion between the plating layer 13 formed on the strike plating layer 12 and the metal base material 11.
[0054] <Process for forming plating layer> A step of forming a plating layer 13 on the strike plating layer 12 on the other side surface of the inter-cell connection member 1 is performed. In this step, the metal base material 11 on which the strike plating layer 12 is provided is used as a cathode, and together with an anode such as SUS, it is immersed in a bath containing a salt such as Co, which serves as a precursor of the plating layer 13, or a salt of Co and a salt of Ni, and a voltage is applied between the anode and cathode to perform plating. As a result, the plating layer 13 consisting of a Co plating layer or a Co-Ni plating layer is obtained. In the process of forming the plating layer, the applied current, voltage, or application time, etc. are adjusted, and the material, concentration, etc. are selected so that the thickness of the plating layer 13 is 2.0 μm or more and 3.0 μm or less.
[0055] The Ni salt dissolved in the electrolyte is preferably water-soluble, and examples of the salt include Ni(NO3)2, NiSO4, etc. The Co salt dissolved in the electrolyte is preferably water-soluble, and examples of the salt include Co(NO3)2, CoSO4, etc.
[0056] <Cathode side bonding material application process> In the air electrode side bonding material application step performed after the step of forming the plating layer 13, an air electrode side bonding material is applied onto the plating layer 13 to form an air electrode side bonding material layer 14b. For example, the air electrode side bonding material is mixed with a solvent to prepare a slurry, which is then applied onto the plating layer 13. Examples of the method for applying the slurry that can be suitably used include a brush coating method, a screen printing method, a spray method, a dipping method, and a spin coater method.
[0057] <Heat treatment process> In the heat treatment step, first, an electrochemical element 3 is placed on the anode-side oxide film 11a on one side of the metal base 11 with the anode 31 in contact with it, and another metal base 11 is placed on the air electrode 32 of the electrochemical element 3 with the air electrode-side bonding material layer 14b on the plating layer 13 on the other side of the metal base 11 in contact with it. This is sequentially repeated to stack a desired number of metal bases 11 and electrochemical elements 3, and heat treatment is performed at a temperature of 650°C to 800°C. This allows the firing of the air electrode-side bonding material that bonds the inter-cell connection member 1 and the electrochemical element 3 and the reaction between the air electrode-side bonding material and the plating layer 13 to be carried out simultaneously by only the heat treatment at a relatively low temperature (600° C. or more and 800° C. or less) in the stacking step S102. Note that the air electrode-side bonding material layer 14b is baked by the above-mentioned heat treatment to become the air electrode-side bonding layer 15b.
[0058] The heat treatment temperature in the heat treatment step is preferably 600° C. or higher and 800° C. or lower. If the temperature is lower than 600° C., the anode-side oxide film 11a and the cathode-side oxide film 11b may not be formed to a sufficient thickness (for example, the cathode-side oxide film 11b may be less than 0.2 μm thick), which may result in insufficient suppression of Cr diffusion, insufficient baking of the cathode-side bonding material, and insufficient diffusion of metals such as Mn from the cathode-side bonding material to the plating layer 13. If the temperature is higher than 800° C., the anode-side oxide film 11a and the cathode-side oxide film 11b may become too thick (for example, the cathode-side oxide film 11b may be more than 0.8 μm thick), which may result in high resistance. The formation of the anode-side oxide film 11a and the air electrode-side oxide film 11b by heat treatment is preferably carried out in an air atmosphere, but may be carried out in a nitrogen atmosphere or a water vapor atmosphere as long as the anode-side oxide film 11a and the air electrode-side oxide film 11b can be formed.
[0059] As described above, by carrying out the manufacturing method for the electrochemical module C including the plating layer formation process S101 and the stacking process S102, it is possible to obtain an electrochemical module C in which the electrochemical elements 3 are electrically connected in series with the metal substrate 11 sandwiched between them.
[0060] Finally, a reducing gas such as hydrogen is passed through the fuel flow channel 2a to perform a reduction process on the electrochemical module C at a predetermined temperature. The predetermined temperature is preferably equal to or higher than about 750° C. and lower than 900° C. If it is lower than 750° C., there is a risk that the reduction of the fuel electrode 31 will not proceed sufficiently. If it is higher than 900° C., deterioration of the fuel electrode 31 will proceed too much, which is not preferable. Furthermore, in order to reinforce the adhesive strength between the electrochemical element 3 and the metal substrate 11 and to establish electrical connection, the electrochemical module C can be clamped by a number of bolts and nuts so that a pressing force is applied in the stacking direction from both ends of the electrochemical module C.
[0061] Next, examples and comparative examples of this embodiment will be described below.
[0062] Example 1 A strike plating layer containing Co was formed on a ferritic stainless steel having a size of 8 mm square and a thickness of 1 mm. The surface on the air electrode side was then immersed in an electrolyte containing dissolved Co salt to form a Co plating layer having a thickness of 2.0 μm. An air electrode side bonding material was then applied onto the plating layer to form an air electrode side bonding material layer made of Co-Mn oxide, and the resulting material was heat-treated at a temperature of 700°C to 800°C for 1 to 2 hours in an air atmosphere to obtain an alloy member A1. The thickness of the oxide film on the air electrode side was measured to find that the average thickness was 0.4 to 0.6 μm.
[0063] Example 2 Except for the fact that the plating layer was a Ni-Co plating layer, the ferritic stainless steel having the plating layer and the air electrode-side bonding material layer formed thereon was heat-treated under the same conditions as in Example 1 to obtain an alloy member A2. The average thickness of the oxide film on the air electrode side was 0.4 to 0.6 μm.
[0064] Comparative Example 1 A strike-plated layer containing Co was formed on a ferritic stainless steel piece measuring 8 mm square and 1 mm thick. A layer containing Co2MnO4 (approximately 10 μm thick) was then formed on the strike-plated layer by electrochemical coating, and sintered at a temperature of 1000°C in air. Next, the cathode-side bonding material was applied, and sintered at a temperature of 700°C to 800°C in air for 1 to 2 hours to obtain alloy member B. The average thickness of the oxide coating on the cathode side was 1.0 to 1.3 μm. The cathode-side bonding material used was the same as that used in Examples 1 and 2.
[0065] <Analysis of the oxide film on the air electrode side> The alloy members of Examples 1 and 2 and Comparative Example 1 were analyzed by a scanning electron microscope (SEM). In addition, Cr mapping was performed on the oxide film on the air electrode side by an electron probe microanalyzer (EPMA).
[0066] The results are shown in FIG. 6. In the alloy members of Examples 1 and 2, a very thin air electrode side oxide film of 0.40 to 0.60 μm was formed on the inner side of the alloy member at the interface between the alloy member and the plating layer. On the other hand, in the alloy member of Comparative Example 1, a relatively thick air electrode side oxide film of 1.0 to 1.3 μm was formed on the inner side of the alloy member at the interface between the alloy member and the layer containing Co2MnO4. These results show that the methods of Examples 1 and 2 can form an air electrode side oxide film that is about half as thin as the method of Comparative Example 1. These results are also suggested by the fact that EPMA analysis shows that relatively dark parts (parts containing a lot of Cr) are concentrated on the surface of each alloy member.
[0067] <Electrical test> The alloy members A1 and A2 of Examples 1 and 2 and the alloy member B of Comparative Example 1 were subjected to a current flow of 0.50 A / cm 2 The specimen was connected to an electrical current tester set to flow a current of 12,000 h at a temperature of 700°C. The results are shown in Figure 7.
[0068] The alloy member A1 had a resistance of about 50 (mΩcm 2 ) and remained stable, and the alloy member A2 showed a resistance value of about 70 (mΩcm) during the current test. 2 ) and remained stable. From this result, it is considered that since the resistance value remains low even after long-term use, it can be used in an electrochemical module and maintain high performance for a long period of time. On the other hand, alloy material B showed a resistance value of about 90 (mΩcm) immediately after the start of the current test. 2 ), and even after the current test was completed, the resistance was higher than the other alloy members. The reason why alloy member B showed a relatively high resistance immediately after the current test started is believed to be due to the existence of a thermal history of 1000°C and the relatively thick oxide film on the air electrode side (1 to 1.3 μm).
[0069] (Another embodiment) (1) In the above embodiment, a configuration has been described in which an electrochemical module C including a metal substrate 11 and an electrochemical element 3 is used as a solid oxide fuel cell to generate electricity. However, the present invention is not limited to this, and the electrochemical module C can also be used as a solid oxide electrolysis cell. A case will be described where a solid oxide electrolysis cell (SOEC) is realized in which an electrochemical reaction occurs in the electrochemical element 3 constituting the electrochemical module C. During operation of the solid oxide electrolysis cell, as shown in FIG. 8, a gas containing water vapor and carbon dioxide (an example of a fuel gas) is circulated through the fuel electrode 31 (an example of an electrode layer) as an electrode layer via the fuel flow channel 2a, and a voltage is applied between the fuel electrode 31 and the air electrode 32 (an example of a counter electrode layer). Then, electrons e - reacts with water molecules H2O and carbon dioxide molecules CO2 to produce hydrogen molecules H2, carbon monoxide CO, and oxygen ions O 2- (oxide ion). Oxygen ion O 2- The oxygen ions O 2 move through the electrolyte membrane 30 to the air electrode 32. 2- releases electrons and becomes oxygen molecules O2. Through the above reaction, water molecules H2O are electrolyzed into hydrogen molecules H2 and oxygen molecules O2, and when gas containing carbon dioxide molecules CO2 is circulated, it is electrolyzed into carbon monoxide CO and oxygen molecules O2.
[0070] (2) In the above embodiment, an example was shown in which the alloy member was used as the inter-cell connection member 1 that sandwiched both sides of the electrochemical element 3. However, the alloy member may also be used as a metal support that supports the electrochemical element 3, and used as a metal-supported solid oxide fuel cell or solid oxide electrolysis cell. Specifically, an electrochemical element 3 is disposed on an alloy member, and a metallic separator is disposed on the electrochemical element 3, and the alloy member, electrochemical element 3, and separator are sequentially stacked to form a cell stack, thereby forming an electrochemical module C. In this case, the fuel electrode-side oxide film 11a formed on one side surface of the alloy member is joined to the fuel electrode 31 of the electrochemical element 3, and the plating layer 13 formed on the other side surface of the alloy member is joined to the air electrode 32 of the other electrochemical element 3. In addition, the alloy member is provided with a plurality of through holes penetrating one side surface and the other side surface of the alloy member in the thickness direction, and is configured to be able to transmit gas between one side surface and the other side surface of the alloy member.
[0071] Furthermore, the configurations disclosed in the above embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided that no contradiction arises. Furthermore, the embodiments disclosed in this specification are merely examples, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Industrial Applicability]
[0072] The electrochemical module according to the present invention can be used as an electrochemical module for a solid oxide fuel cell or a solid oxide electrolysis cell. [Explanation of symbols]
[0073] 1: Alloy components 2: Groove 2a: Fuel flow path 2b: Air flow path 3: Electrochemical elements 11: Metal base material 11a: Fuel electrode side oxide film 11b: Oxide film on the air electrode side 12: Strike plating layer 13: Plating layer 14b: Air electrode side bonding material layer 15: Bonding layer 15b: Air electrode side bonding layer 30: Electrolyte membrane 31:Fuel electrode 32: Air electrode C: Cell S101: Plating layer formation process S102: Stacking process
Claims
1. a plating layer forming step of forming a plating layer made of a Co plating layer or a Co-Ni plating layer on the other side surface of a substrate of an alloy member made of ferritic stainless steel, the other side surface of the substrate being used in a solid oxide fuel cell or a solid oxide electrolysis cell, in a state in which one side surface of the substrate is in an atmosphere in contact with a fuel gas and the other side surface of the substrate is in an atmosphere in contact with an oxygen-containing gas; and a stacking step of heat treating the alloy member and an electrochemical element having a single cell formed by sandwiching an electrolyte layer between an electrode layer and a counter electrode layer, with a bonding material interposed between the alloy member and the electrochemical element, at a temperature of 650°C or higher and 800°C or lower.
2. 2. The method for manufacturing an electrochemical module according to claim 1, wherein the heat treatment in the stacking step forms an oxide film having a thickness of 0.2 μm or more and 0.8 μm or less on the other side surface of the base material, and the plating layer having a thickness of 2.0 μm or more and 3.0 μm or less is formed on the oxide film.
3. 3. The method for manufacturing an electrochemical module according to claim 2, wherein after the heat treatment in the stacking step, the bonding material has a structure in which a plurality of fine particles having an average particle size of 0.1 μm or more and 0.2 μm or less are aggregated in a state in which the alloy member and the single cell are bonded together.
4. 4. The method for manufacturing an electrochemical module according to claim 1, further comprising the step of forming a strike plating layer of Co or Ni on the other side surface of the base material before forming the plating layer in the plating layer forming step.
5. An alloy member used in a solid oxide fuel cell or a solid oxide electrolysis cell, in a state where one side of a substrate is in an atmosphere in contact with a fuel gas and the other side of the substrate is in an atmosphere in contact with an oxygen-containing gas, comprising: an oxide coating having a thickness of 0.2 μm or more and 0.8 μm or less on the other side surface of the base material; The alloy member is provided with a plating layer on the oxide film, the plating layer being made of a Co plating layer or a Co-Ni plating layer having a thickness of 2.0 μm or more and 3.0 μm or less.
6. 6. An electrochemical module comprising: the alloy member according to claim 5; and an electrochemical element having a single cell formed by sandwiching an electrolyte layer between an electrode layer and a counter electrode layer; and bonded together by a bonding material.
7. 7. The electrochemical module according to claim 6, wherein the bonding material has a structure in which a plurality of fine particles having an average particle size of 0.1 μm or more and 0.2 μm or less are assembled when the alloy member and the unit cell are bonded together.
8. The electrochemical module of claim 6 , wherein the oxide layer comprises an oxide of Cr.
9. The electrochemical module according to claim 6 , wherein the plating layer comprises Mn.
10. A solid oxide fuel cell comprising the electrochemical module according to claim 6 , wherein a power generating reaction occurs in the unit cell.
11. A solid oxide electrolysis cell comprising the electrochemical module according to claim 6 , wherein an electrolytic reaction occurs in the single cell.
Citation Information
Patent Citations
Fuel battery member and manufacturing method for the same
JP2016195101A
Bonding structure of SOFC, and conductive bonding material used therefor
JP2019212374A
Method for producing alloy member, alloy member, electrochemical element, electrochemical module, electrochemical device, energy system, and solid oxide fuel cell
WO2018181926A1
Solid oxide fuel cell
JP2013118177A
Solid oxide fuel cell
JP2013118178A