Coating agent, braid with coating, and method for manufacturing fishing line

A copolymer-based coating agent enhances filament adhesion in fishing lines, preventing air knots and maintaining flight distance by using specific monomers and resins.

JP2024132662APending Publication Date: 2024-10-01HARDBITE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023043520
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Fishing lines tend to loosen and form air knots when cast, leading to entanglement and reduced flight distance, especially with stronger and more abrasion-resistant synthetic fibers.

Method used

A coating agent comprising a copolymer with specific monomers and an adhesive resin is applied to the braid, enhancing adhesion and preventing air knots.

Benefits of technology

The coating agent effectively prevents air knots and maintains the flying distance of fishing lines by improving adhesion between filaments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132662000001
    Figure 2024132662000001
  • Figure 2024132662000002
    Figure 2024132662000002
Patent Text Reader

Abstract

To provide a coating agent which is excellent in air knot prevention of a fishing line.SOLUTION: A coating agent contains a copolymer including a constitutional unit composed of a first monomer having an aliphatic group having 10 or more carbon atoms, and a constitutional unit composed of a second monomer having any one of an amino group, an epoxy group and an ether group, and an adhesive resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating agent, a coated braid, and a method for producing a fishing line. [Background technology]

[0002] Generally, fishing lines are broadly divided into fishing lines made of monofilament and fishing lines made of braided yarn. However, due to recent trends in fishing methods and fishing equipment, the use of fishing lines braided with synthetic fibers and the like has been increasing in order to improve strength and abrasion resistance.

[0003] For example, Patent Document 1 discloses a fishing line that has a synthetic fiber multifilament yarn as a core yarn and a synthetic fiber multifilament twisted yarn as a sheath yarn wrapped around it in a predetermined manner as a covering yarn, with the aim of providing a fishing line with excellent breaking strength, knot strength, etc. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-103737 Summary of the Invention [Problem to be solved by the invention]

[0005] However, when casting such fishing lines using a spinning reel, the braided cord is prone to loosening due to various factors, and the cord is prone to tangling and forming knots called air knots. When air knots occur, expensive lures and other items can be lost. In addition, loosening of the braided cord increases air resistance, reducing the casting distance of the lure.

[0006] Therefore, the present invention has been made in consideration of the above problems, and has an object to provide a coating agent that is excellent in preventing air knots in fishing lines and maintaining casting distance. [Means for solving the problem]

[0007] As a result of intensive research into achieving the above object, the inventors have found that the above problems can be solved, particularly by using a coating agent containing a specific copolymer, and have thus completed the present invention.

[0008] That is, the present invention is as follows. [1] A copolymer including a structural unit made of a first monomer having an aliphatic group having 10 or more carbon atoms and a structural unit made of a second monomer having any one of an amino group, an epoxy group, or an ether group; and an adhesive resin, Coating agent. [2] The first monomer constituting the copolymer includes at least one selected from the group consisting of behenyl acrylate, behenyl methacrylate, stearyl acrylate, stearyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, lauryl acrylate, and lauryl methacrylate. The coating agent according to [1]. [3] the second monomer constituting the copolymer includes one or more selected from the group consisting of 2-(dimethylamino)ethyl acrylate, 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl acrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl acrylate, 2-(tert-butylamino)ethyl methacrylate, N,N-dimethylacrylamide, N,N-diethylacrylamide, and N,N-dimethylaminopropylacrylamide; The coating agent according to [1] or [2]. [4] The copolymer is a block copolymer, The weight average molecular weight of the first monomer block is 2000 or more. The coating agent according to any one of [1] to [3]. [5] The concentration of the copolymer is 0.01 to 10.0% by mass with respect to the total amount of the coating agent. The coating agent according to any one of [1] to [4]. [6] The adhesive resin contains at least one of an acrylic resin and a water-soluble urethane resin. The coating agent according to any one of [1] to [5]. [7] [1] to [6] are applied to a braided cord. Covered braid. [8] The braided cord contains ultra-high molecular weight polyethylene fibers. [7] A coated braid as described in [8]. [9] Used for fishing lines, The coated braid according to [7] or [8].

[10] a braiding step of braiding the filaments to obtain a braid; [1] to [6] include a coating step of coating the braided cord with the coating agent to obtain a coated braided cord. A method for manufacturing fishing line.

[11] Further comprising a twisting step of twisting the filaments to obtain a twisted yarn;

[10] A method for manufacturing a fishing line according to the present invention.

[12] The coated braid is further dried at a temperature of 40 to 120 ° C. A method for manufacturing a fishing line according to

[10] or

[11] .

[13] The twisting is 10 to 500 times / m. A method for manufacturing a fishing line according to

[11] or

[12] . Effect of the Invention

[0009] According to the present invention, a coating agent that is excellent in preventing air knots in fishing line and maintaining casting distance can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. However, the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.

[0011] 1. Coating agent The coating agent of the present embodiment includes a copolymer including a constituent unit made of a first monomer having an aliphatic group having 10 or more carbon atoms and a constituent unit made of a second monomer having any one of an amino group, an epoxy group, and an ether group, and an adhesive resin. The coating agent of the present embodiment may also include other components within a range that does not impair the effects of the present invention.

[0012] The technical mechanism by which the coating agent of the present embodiment has excellent air knot prevention properties is not particularly limited, but may be, for example, as follows. The coating agent of the present embodiment includes a structural unit made of a predetermined first monomer and a structural unit made of a predetermined second monomer. The structural unit made of the first monomer is hydrophobic and has side chain crystallinity, and strongly interacts with the surface of the filament, which is generally hydrophobic. On the other hand, the structural unit made of the second monomer is a structural unit with an excellent balance of hydrophilicity and hydrophobicity, and has excellent interaction with general adhesive resins for filaments. Therefore, the filament surface is surface-modified by the copolymer so that the adhesive resin is easily adsorbed, and the adhesion between the filaments is stronger than when an adhesive resin is simply used, and the braid does not loosen, and it is considered that the braid has excellent air knot prevention properties and maintenance of flight distance.

[0013] 1.1.Copolymer The copolymer used in this embodiment has a constitutional unit made of a first monomer having an aliphatic group having 10 or more carbon atoms, and a constitutional unit made of a second monomer having any one of an amino group, an epoxy group, and an ether group. The copolymer may be a random copolymer or a block copolymer, but is preferably a block copolymer from the viewpoint of exerting the effects of this embodiment.

[0014] The carbon number of the aliphatic group of the first monomer is 10 or more, preferably 14 or more, more preferably 16 or more, even more preferably 18 or more, and particularly preferably 20 or more. When the carbon number of the aliphatic group is within the above range, the adsorption strength to the braided cord surface tends to be further improved. In addition, the upper limit of the carbon number of the aliphatic group is not particularly limited, but is preferably 30 or less. When the carbon number of the aliphatic group is within the above range, the solubility in a solvent tends to be further improved.

[0015] Examples of the aliphatic group include linear aliphatic groups, branched aliphatic groups, and cyclic aliphatic groups. Among these, linear aliphatic groups are preferred from the viewpoint of the adsorption strength to the braided cord surface.

[0016] The first monomer is not particularly limited, but is preferably, for example, a vinyl monomer. By using a vinyl monomer, it is possible to relatively easily produce a block copolymer by various living polymerizations. In addition, this tends to have excellent interaction with the adhesive resin.

[0017] Specific examples of such a first monomer include, but are not limited to, behenyl acrylate, behenyl methacrylate, stearyl acrylate, stearyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, myristyl acrylate, myristyl methacrylate, lauryl acrylate, and lauryl methacrylate. The first monomer may be used alone or in combination of two or more kinds.

[0018] Among these, at least one selected from the group consisting of behenyl acrylate, behenyl methacrylate, stearyl acrylate, stearyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, lauryl acrylate, and lauryl methacrylate is preferred. By using such a first monomer, the adsorption strength to the braided cord surface tends to be further improved.

[0019] The content (copolymerization ratio) of the first monomer constituting the copolymer is preferably 5 to 95 mass %, more preferably 10 to 90 mass %, based on 100 mass % of the copolymer. When the content of the first monomer is within the above range, the adsorption strength to the braided cord surface tends to be further improved.

[0020] When the copolymer of the present embodiment is a block copolymer, the weight average molecular weight of the block of the first monomer constituting the copolymer is preferably 2000 or more, more preferably 3000 or more. The upper limit of the weight average molecular weight of the first monomer constituting the copolymer is not particularly limited, but is 100000 or less. When the weight average molecular weight of the first monomer constituting the copolymer is 2000 or more, that is, the long-chain alkane chain portion that can contribute to entanglement becomes longer, the proportion of bonds derived from co-crystal interactions tends to increase. This allows the copolymer to be more strongly bonded to the surface of a filament made of high-density polyethylene or ultra-high molecular weight polyethylene. The method for measuring the weight average molecular weight of the first monomer is not particularly limited as long as it is a conventionally known method, but for example, a method of measuring by GPC after completing polymerization of the block of the first monomer and before starting polymerization of the block of the second monomer can be mentioned.

[0021] The second monomer is not particularly limited as long as it has an amino group, an epoxy group, or an ether group, but is preferably a vinyl monomer having an amino group, an epoxy group, or an ether group. By using a vinyl monomer, it is relatively easy to produce a block copolymer by various living polymerizations, and it tends to have excellent interaction with the adhesive resin. In addition, the functional group of the second monomer is not particularly limited as long as it is an amino group, an epoxy group, or an ether group, and it may have two or more of these functional groups in combination.

[0022] Specific examples of such second monomers are not particularly limited, but include, for example, monomers having an amino group such as 2-(dimethylamino)ethyl acrylate, 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl acrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl acrylate, 2-(tert-butylamino)ethyl methacrylate, N,N-dimethylacrylamide, N,N-diethylacrylamide, and N,N-dimethylaminopropylacrylamide; monomers having an epoxy group such as glycidyl acrylate and glycidyl methacrylate; monomers having an ether group and a hydroxyl group terminal such as polyethylene glycol monoacrylate and polyethylene glycol monomethacrylate; and monomers having an ether group and an alkoxy group terminal such as di(ethylene glycol)ethyl ether acrylate. The second monomer may be used alone or in combination of two or more types.

[0023] Among these, one or more selected from the group consisting of 2-(dimethylamino)ethyl acrylate, 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl acrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl acrylate, 2-(tert-butylamino)ethyl methacrylate, N,N-dimethylacrylamide, N,N-diethylacrylamide, and N,N-dimethylaminopropylacrylamide are preferred. By using such a second monomer, the effect of modifying the braided cord surface tends to be further improved.

[0024] The content (copolymerization ratio) of the second monomer constituting the copolymer is preferably 5 to 95 mass %, more preferably 10 to 90 mass %, based on 100 mass % of the copolymer. When the content of the second monomer is within the above range, the effect of modifying the braid surface tends to be further improved.

[0025] The content of the copolymer is preferably 0.01 to 10.0% by mass, more preferably 0.1 to 5.0% by mass, even more preferably 0.3 to 3.0% by mass, and even more preferably 0.5 to 2.0% by mass, based on the total amount of the coating agent. When the content of the copolymer is 0.01% by mass or more based on the total amount of the coating agent, the air knot prevention property tends to be further improved, and similarly, when the content of the copolymer is 10.0% by mass or less based on the total amount of the coating agent, the air knot prevention property tends to be further improved.

[0026] The ratio of the copolymer content to the adhesive resin content is preferably 0.01 to 0.7, more preferably 0.03 to 0.5, even more preferably 0.05 to 0.3, and even more preferably 0.07 to 0.1. When the ratio of the copolymer content to the adhesive resin content is 0.01 or more, the hydrophobic structural unit of the copolymer is adsorbed on the surface of the braid, thereby improving the adhesiveness of the adhesive resin, and the air knot prevention tends to be more excellent. In addition, when the ratio of the copolymer content to the adhesive resin content is 0.7 or less, the adhesiveness of the braid by the adhesive resin can be fully exhibited, and the air knot prevention tends to be more excellent.

[0027] 1.2.Adhesive resin The adhesive resin of the present embodiment is not particularly limited as long as it improves the adhesion between the filaments and reduces the tendency for the filaments to sag. Note that the adhesive resin of the present embodiment does not include the copolymer of the present embodiment.

[0028] Such adhesive resins are not particularly limited, but include, for example, acrylic resins, modified polyethylene resins, modified polypropylene resins, polyester resins, modified nylon resins, water-soluble urethane resins, phenolic resins, silicone resins, and epoxy resins. These may be used alone or in combination of two or more. Among them, from the viewpoint of further improving the adhesiveness, one or more selected from the group consisting of acrylic resins, water-soluble urethane resins, modified polyethylene resins, and modified polypropylene resins are preferred, and it is more preferred to include at least one of acrylic resins and water-soluble urethane resins.

[0029] The adhesive resin may be produced by a conventional method, or may be a commercially available product. Examples of commercially available products include, but are not limited to, PLUS SIZE J-96 (manufactured by GOO KAGAKU KAGAKU KOGYO CO., LTD.), HYDRAN AP-40N (manufactured by DAI-NIPPON INK & CHEMICALS CO., LTD.), HYDRAN AP-40F (manufactured by DAI-NIPPON INK & CHEMICALS CO., LTD.), HYDRAN AP-X101H (manufactured by DAI-NIPPON INK & CHEMICALS CO., LTD.), ARROW BASE SB-1200 (manufactured by UNITIKA LTD.), ARROW BASE SD-1200 (manufactured by UNITIKA LTD.), POLYMENT NK100PM (manufactured by Nippon Shokubai Co., Ltd.), EPOCROS WS-300 (manufactured by Nippon Shokubai Co., Ltd.), and POLYSTRON 1280 (manufactured by Arakawa Chemical Industries Co., Ltd.).

[0030] The adhesive resin content is preferably 2.0 to 30 mass%, more preferably 5.0 to 25 mass%, and even more preferably 8.0 to 20 mass% relative to the total amount of the coating agent. When the adhesive resin content is 2.0 mass% or more relative to the total amount of the coating agent, the air knot prevention property tends to be further improved, and when the adhesive resin content is 30 mass% or less relative to the total amount of the coating agent, the mechanical properties tend to be further improved.

[0031] 2. Covered braid The coated braid of the present embodiment is a braid to which the coating agent of the present embodiment is applied. Note that the braid means a braid made by weaving a plurality of filaments. The coated braid of the present embodiment is suitably used for a fishing line.

[0032] The filaments used for the braided cord are not particularly limited, but examples thereof include polyolefin-based fibers, polyparaphenylene benzobisoxazole fibers, polyarylate fibers, polyamide-based fibers, polyester-based fibers, and fluorocarbon-based fibers. The polyolefin-based fibers are not particularly limited, but examples thereof include polyethylene-based fibers and polypropylene-based fibers. Among them, from the viewpoint of further improving the air knot prevention property, it is preferable to include polyolefin-based fibers, more preferably to include polyethylene-based fibers, even more preferably to include high molecular weight polyethylene-based fibers, and even more preferably to include ultra-high molecular weight polyethylene-based fibers.

[0033] The polyethylene fiber refers to a homopolymer or copolymer having at least 50 mole percent of ethylene units as a constituent monomer ratio. Here, high molecular weight polyethylene refers to polyethylene having a weight average molecular weight of 40,000 or more. Furthermore, ultra-high molecular weight polyethylene refers to polyethylene having a weight average molecular weight of 1,000,000 or more. Examples of polyethylene fibers include, but are not limited to, IZANAS (manufactured by Toyobo Co., Ltd.), Dyneema (manufactured by DSM Co., Ltd.), and Spectra (manufactured by Honeywell Co., Ltd.).

[0034] The polypropylene-based fiber means a homopolymer or copolymer having at least 50 mole percent of propylene units as a constituent monomer ratio. The polypropylene-based fiber is not particularly limited, but an example thereof is Marvess (manufactured by Phillips Fibers).

[0035] The thickness of the filaments used in the braid is preferably 33 to 880 dtex, more preferably 740 to 330 dtex, and further preferably 148 to 185 dtex. From the Izanas website

[0036] The braid is not particularly limited, but may be braided, for example, using a conventionally known braiding machine (braiding machine). The number of filaments to be braided is not particularly limited, but may be, for example, 2, 4, 8, or 16, and the braid angle is also optional.

[0037] The method for applying the coating agent of this embodiment to the braided cord will be described later.

[0038] 3. Fishing line manufacturing method The method for manufacturing a fishing line of this embodiment includes a braiding step of braiding filaments to obtain a braided cord, and an attachment step of applying the coating agent of this embodiment to the braided cord to obtain a coated braided cord, and may include other steps as necessary.

[0039] The braiding method in the braiding step is not particularly limited, but examples thereof include flat braiding, round braiding, and square braiding. After the multifilament is braided, a heat treatment may be performed.

[0040] The method of application in the application step is not particularly limited, but examples thereof include a method of spraying the coating agent onto the surface of the braided cord, a method of applying the coating agent to the surface of the braided cord, and a method of immersing the braided cord in the coating agent.

[0041] The fishing line manufacturing method of this embodiment may further include, as an additional step, a twisting step of twisting the filaments to obtain a twisted yarn.

[0042] The twisting in the twisting step is not particularly limited, but may be performed by a conventionally known twisting machine, for example. The twisting machine is not particularly limited, but examples thereof include a ring twisting machine, a double twister twisting machine, and an aroma twisting machine.

[0043] In the twisting step, the twisting is preferably 10 to 500 times / m, more preferably 20 to 400 times / m, and further preferably 40 to 300 times / m. By twisting at 10 times / m or more, the occurrence of fluff and knots tends to be further prevented. Furthermore, by twisting at 500 times / m or less, the prevention of air knots tends to be further improved.

[0044] The fishing line manufacturing method of this embodiment may further include, as an additional step, a drying step in which the covered braid is dried at a temperature of 40 to 120° C. When the drying temperature is 40° C. or higher, the air knot prevention property tends to be further improved, and when the drying temperature is 100° C. or lower, the mechanical properties of the braid tend to be further improved. The drying time is not particularly limited, but is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes, and even more preferably 30 seconds to 2 minutes. EXAMPLES

[0045] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0046] 1. Copolymer Preparation 1.1.Copolymer 1 (STA-DEAEMA) 5.0 g of stearyl acrylate, 5.0 g of butyl acetate, and 0.38 g of BlocBuilderR MA (manufactured by ARKEMA) (initiator) were put into a stirring polymerization apparatus, and the inside of the apparatus was replaced with a nitrogen atmosphere. Then, polymerization was performed for 24 hours while heating in an oil bath (110 ° C.). Next, 5.0 g of 2-(diethylamino)ethyl methacrylate and 5.0 g of butyl acetate were further put into the stirring polymerization apparatus, and polymerization was performed for 24 hours while heating in an oil bath (110 ° C.). After polymerization, the reaction solution was dropped into methanol to precipitate a block copolymer of stearyl acrylate and 2-(diethylamino)ethyl methacrylate, and the precipitate was filtered to obtain a copolymer. The weight average molecular weight of the block consisting of stearyl acrylate in the copolymer was 5000, and the weight average molecular weight of the block consisting of 2-(diethylamino)ethyl methacrylate in the copolymer was 5000.

[0047] 1.2.Copolymer 2 (STA-DEEA) 5.0 g of stearyl acrylate, 5.0 g of butyl acetate, and 0.38 g of BlocBuilder MA (manufactured by ARKEMA) (initiator) were put into a stirring polymerization apparatus, and the inside of the apparatus was replaced with a nitrogen atmosphere. Then, polymerization was carried out for 24 hours while heating in an oil bath (110°C). Next, 5.0 g of di(ethylene glycol) ethyl ether acrylate and 5.0 g of butyl acetate were further put into the stirring polymerization apparatus, and polymerization was carried out for 24 hours while heating in an oil bath (110°C). After polymerization, the reaction solution was dropped into methanol to precipitate a block copolymer of stearyl acrylate and di(ethylene glycol) ethyl ether acrylate, and the precipitate was filtered to obtain a copolymer. The weight average molecular weight of the block composed of stearyl acrylate in the copolymer was 5,000, and the weight average molecular weight of the block composed of di(ethylene glycol) ethyl ether acrylate in the copolymer was 5,000.

[0048] 1.3.Copolymer 3 (BHA-TBAEMA) 5.0 g of behenyl acrylate, 5.0 g of butyl acetate, and 0.38 g of BlocBuilderR MA (manufactured by ARKEMA) (initiator) were charged into a stirring polymerization apparatus, and the inside of the apparatus was replaced with a nitrogen atmosphere. Then, polymerization was performed for 24 hours while heating in an oil bath (110°C). Next, 5.0 g of 2-(tert-butylamino)ethyl methacrylate and 5.0 g of butyl acetate were further charged into the stirring polymerization apparatus, and polymerization was performed for 24 hours while heating in an oil bath (110°C). After polymerization, the reaction solution was dropped into methanol to precipitate a block copolymer of behenyl acrylate and 2-(tert-butylamino)ethyl methacrylate, and the precipitate was filtered to obtain a copolymer. The weight average molecular weight of the block consisting of behenyl acrylate in the copolymer was 5000, and the weight average molecular weight of the block consisting of 2-(tert-butylamino)ethyl methacrylate in the copolymer was 5000.

[0049] 2. Preparation of Coating Agent The coating agents of the Examples and Comparative Examples were obtained by mixing the copolymers 1 to 3 obtained as described above with adhesive resins to obtain the compositions shown in Tables 1 and 2. In addition, in the compositions in Tables 1 and 2, unless otherwise specified, the percentages are by mass, and "SB / WS" refers to a mixture of SB-1200 and WS-300, which will be described later, in a ratio of 100:2.

[0050] [Table 1]

[0051] [Table 2]

[0052] Details of each component shown in Table 1 are as follows. J-96: Product name "Plussize J-96", manufactured by GOO Chemical Industry Co., Ltd., acrylic resin, solid content concentration 22% by mass Hydran: Product name "Hydran AP-40N", manufactured by Dainippon Ink and Chemicals, Inc., water-based urethane resin, solid content concentration 35% by mass SB: Product name: Arrowbase SB-1200, manufactured by Unitika Ltd., modified polyethylene resin, solid content concentration 25% by mass WS: Product name "Epocross WS-300", manufactured by Nippon Shokubai Co., Ltd., water-soluble acrylic resin containing oxazoline groups, solid content concentration 10% by mass

[0053] 2. Making fishing line A ring twister was used to twist the filaments (IZANAS (registered trademark), manufactured by Toyobo Co., Ltd., 165 dtex) to 70 turns / m to obtain a twisted yarn. The twisted yarn was then twisted into a braid by twisting eight strands at a time to obtain a braided cord. The braided cord was immersed in the coating agent of each Example and Comparative Example, and then dried in an atmosphere at 65°C for 1 minute to produce a fishing line as a covered braided cord.

[0054] 3. Evaluation Using each of the obtained fishing lines, a rod (Ultimo 82, manufactured by RippleFisher), a reel (Stella 14000xG, manufactured by Shimano), and a lure (Wild Response 137g, manufactured by Shimano), a skilled person in the art performed casting and evaluated the casting distance and the number of air knots. The results are shown in Tables 1 and 2.

[0055] 4. Discussion Comparing each of the Examples and Comparative Examples, it was found that when the coating agent contained a copolymer, it had excellent air knot prevention properties regardless of the type of adhesive resin. Comparing Examples 2 to 5, it was found that the air knot prevention property was particularly excellent when the content of the copolymer was 0.5 to 2.0 mass % relative to the total amount of the coating agent. Similarly, a comparison of Examples 2 to 7 revealed that when the ratio of the copolymer content to the adhesive resin content was 0.07 to 0.1, the air knot prevention properties were particularly excellent. Comparison of Examples 2, 8, and 9 reveals that when the second monomer in the copolymer is a specific compound, the copolymer is particularly excellent in air knot properties. [Industrial Applicability]

[0056] INDUSTRIAL APPLICABILITY The present invention can be used for fishing lines and has industrial applicability.

Claims

1. A copolymer including a structural unit made of a first monomer having an aliphatic group having 10 or more carbon atoms and a structural unit made of a second monomer having any one of an amino group, an epoxy group, or an ether group; and an adhesive resin, Coating agent.

2. the first monomer constituting the copolymer includes one or more selected from the group consisting of behenyl acrylate, behenyl methacrylate, stearyl acrylate, stearyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, lauryl acrylate, and lauryl methacrylate; The coating agent according to claim 1.

3. the second monomer constituting the copolymer includes one or more selected from the group consisting of 2-(dimethylamino)ethyl acrylate, 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl acrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl acrylate, 2-(tert-butylamino)ethyl methacrylate, N,N-dimethylacrylamide, N,N-diethylacrylamide, and N,N-dimethylaminopropylacrylamide; The coating agent according to claim 1.

4. The copolymer is a block copolymer, The weight average molecular weight of the first monomer block is 2000 or more. The coating agent according to claim 1.

5. The concentration of the copolymer is 0.01 to 10.0% by mass based on the total amount of the coating agent; The coating agent according to claim 1.

6. The adhesive resin contains at least one of an acrylic resin and a water-soluble urethane resin. The coating agent according to claim 1.

7. A braided cord comprising the coating agent according to claim 1 attached thereto. Covered braid.

8. The braided cord contains ultra-high molecular weight polyethylene fibers. The covered braid according to claim 7.

9. Used for fishing lines, The covered braid according to claim 7 or 8.

10. a braiding step of braiding the filaments to obtain a braid; A coating step of applying the coating agent according to any one of claims 1 to 6 to the braided cord to obtain a coated braided cord. A method for manufacturing fishing line.

11. Further comprising a twisting step of twisting the filaments to obtain a twisted yarn; A method for manufacturing a fishing line according to claim 10.

12. The coated braid is dried at a temperature of 40 to 120° C. A method for manufacturing a fishing line according to claim 10.

13. The twist is 10 to 500 times / m. A method for manufacturing a fishing line according to claim 11.

Citation Information

Patent Citations

  • Fishing line

    JP2006129867A

  • Coating agent for thread and thread coated with the same

    JP2010077569A

  • Surface-modified material, composition for surface modification, and restoration method

    JP2015229725A

  • Surface modification composition, modified article and manufacturing method therefor

    JP2019070091A

  • Fishline

    JP1999103737A