Pattern forming method of thin film and processing apparatus thereof
The method of dividing the etching process into multiple stages with resist property modification and stabilization processes effectively suppresses side etching, ensuring accurate thin film pattern formation by enhancing adhesion and reducing dimensional inaccuracies.
Patent Information
- Application Number
- JP2023204300
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-16
- Filing Date
- 2023-12-02
- Publication Date
- 2024-10-01
AI Technical Summary
Conventional methods for forming thin film patterns using organic masks face challenges in suppressing side etching during the etching process, particularly for thin patterns, leading to dimensional inaccuracies and potential loss of the base film pattern.
A method involving multiple stages of etching, each followed by resist property modification and stabilization processes, including heat treatment and organic solvent exposure, to enhance adhesion and control side etching, combined with a processing apparatus that includes units for resist property change, substrate stabilization, and etching.
Significantly reduces side etching by dividing the etching process into multiple stages, maintaining pattern accuracy and adhesion, and ensuring consistent dimensions, even for fine patterns.
Smart Images

Figure 2024132849000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a pattern on a thin film using an organic mask, and a processing apparatus thereof. All of the patents, patent applications, patent publications, scientific articles, etc. cited or identified in this application are incorporated by reference in their entirety in order to more fully describe the current state of the art to which this invention pertains. [Background technology]
[0002] As an example of a mask formed by an organic film (hereinafter referred to as an organic mask or an organic film pattern, but also including a resist mask, a resist film mask, and a resist pattern mask as examples in the category), a resist pattern mask (hereinafter referred to as a resist mask, a resist pattern mask, a resist film mask, a resist film pattern mask, or a mask of a pattern using a resist film, but all are synonymous) will be described below. The process of etching an undercoat film using a resist mask is an essential process when forming a semiconductor device. Etching includes isotropic etching represented by wet etching and anisotropic etching represented by dry etching. The term "isotropic etching" as used in this specification refers to a case where etching proceeds not only up and down but also left and right, and includes a case where etching does not necessarily proceed at the same rate up, down, left and right. Furthermore, the term "anisotropic etching" as used in this specification refers to a case where the etching rates in the up, down and left and right directions are different to such an extent that etching hardly proceeds at the bottom of the organic mask. However, among dry etching, the nature varies depending on the type of plasma discharge, processing pressure, material to be etched, and type of processing gas, and there are cases where the tendency is relatively strong to be isotropic (hereinafter referred to as isotropic dry etching) and cases where the tendency is strong to be anisotropic (hereinafter referred to as anisotropic dry etching). Of these different types of etching, the more appropriate one is selected in consideration of the conditions when performing the etching. When etching an underlayer using a resist pattern as a mask, there is a problem that the underlayer is formed with different dimensions from the resist pattern at the end of the resist pattern (the boundary between the part with the resist pattern and the part without the resist pattern) due to a phenomenon called side etching (or undercut). In particular, in the case of a pattern with a strong tendency or a fine pattern (for example, 1 μm or less), not only is the underlayer pattern formed with a significantly different dimension, but the underlayer pattern itself disappears and is not formed. For this reason, even in any of the above etching methods, it is strongly required to suppress side etching (or undercut) of the underlayer as much as possible.
[0003] A conventional technique for suppressing side etching (or undercutting) of an underlying film when etching is performed using wet etching is disclosed in Patent Document 1 (JP Patent Publication 50-37374). In the etching method, a photoresist film is partially formed on the main surface of the object to be treated, and the object is selectively etched using this as a mask. After a thermoplastic photoresist film is partially formed on the main surface of the object to be treated, the object is etched using this as a mask to form a groove, and then the object is heated to soften the photoresist film and cover the side of the groove, and then further etched, and the softening of the photoresist film and the etching of the object are performed one or more times to form a through hole.
[0004] Patent Document 2 (JP Patent Publication 60-234982 A) describes a method of heating the resist on the layer to be etched in the same manner as Patent Document 1, and heating the resist to a temperature at which the resist cures (a temperature at which resist flow occurs, and is separately described as curing), and suppressing side etching by partially etching before and after the heat treatment.
[0005] Patent Document 3 (JP Patent Publication No. 05-327179), like Patent Documents 1 and 2, describes a method in which a layer to be etched is half-etched, a resist layer provided on the layer to be etched is softened, and then the remaining etching is performed. The method for softening the resist is usually softened by heat treatment (paragraph number 0016 in the same document).
[0006] Patent Document 4 (JP Patent Publication No. 11-214826), like Patent Documents 1 and 2, describes a method in which a resist film is partially formed on a layer to be etched (a conductor layer in this document), a part of the layer to be etched is etched, and then the resist film at the etched edge is heated and bent with a cushion plate of a vacuum pressure bonding device, and it is described (from paragraphs 0010, 0011, 0021, and 0032 of the same document) that the heating is performed up to the softening temperature.
[0007] Patent Document 5 (JP Patent Publication 77848 / 1978) describes a method of softening the resist film during etching similar to Patent Documents 1, 2, 3, and 4, in which the resist film is immersed in an organic solvent to cause it to swell. Furthermore, examples of the organic solvent used for immersion include hydrocarbons, ketones, alcohols, and esters.
[0008] Patent Document 6 (JP Patent Publication 16169 / 1982) employs a method of folding a mask layer (the mask layer in this document is similar to the resist film in the other documents) during etching, similar to Patent Documents 1, 2, 3, and 4, but also employs a method of immersing the mask layer in a swelling liquid such as paraffin-based hydrocarbons, so-called white kerosene or aromatic hydrocarbons, xylene, toluene, etc., to cause it to swell.
[0009] Furthermore, Patent Document 7 (JP Patent Publication No. 2002-334830) describes a method in which a chemical solution that dissolves an organic film (including a resist film and a resist mask) is penetrated into the organic film (i.e., the organic film is at least immersed in the chemical solution that dissolves the organic film or exposed to the vapor of the organic solvent), causing the organic film to dissolve and reflow (also called chemical solution dissolution reflow (or chemical solution gas exposure) or chemical solution gas exposure, etc.), and an underlying film is etched after the organic film is dissolved.
[0010] The above-mentioned conventional techniques disclosed in Patent Documents 1 to 4 all employ a method of heating the resist film to soften or flow the resist film, but the treatment temperature is near the temperature at which the resist film cures. The treatment temperature is higher than the pre-bake or post-bake temperature of the resist film, and most of the solvent components in the resist film evaporate, so the resist film hardens after the treatment, making it difficult to peel off, and it is almost impossible to soften the resist film again. Therefore, it must be said that it is difficult to soften the resist film after the first softening of the photoresist film (synonymous with resist film) described in Patent Document 1 and the second etching of the base film.
[0011] In all of the above-mentioned conventional techniques disclosed in Patent Documents 5 and 6, the resist film is swelled by immersing the resist film in an organic solvent. However, swelling only expands the resist film, and since the resist film is in liquid, it is difficult to achieve the effect of flowing and protecting the surface of the base film. There is a high possibility that the resist film will not adhere well to the side-etched portion of the base film due to buoyancy. In addition, immersion in the organic solvent may cause a portion of the surface of the resist film to dissolve. In that case, rather than flowing over the surface of the base film, the resist film may disappear by partially dissolving in the liquid.
[0012] Hereinafter, the process of immersing the resist film in a chemical solution to cause it to dissolve and flow will be referred to as chemical immersion dissolution reflow, and the process of exposing the resist film to the vapor of the chemical solution to cause it to dissolve and flow will be referred to as chemical vapor dissolution reflow.
[0013] The above-mentioned conventional technology disclosed in Patent Document 7 adopts a method of soaking in a chemical solution to dissolve and reflow as the first method, or a method of soaking in a chemical solution to dissolve and reflow as the second method, as a method of soaking in a chemical solution to dissolve and reflow the resist film in an organic solvent. In this case, the first method (soaking in a chemical solution to dissolve and reflow the resist film) has the same problems as Patent Documents 5 and 6 (resist film dissolves and disappears in the liquid, etc.), and the other method (chemical solution to dissolve and reflow the resist film) dissolves and flows the surface of the resist film by exposing the organic solvent in a gaseous state, but the method involves reflowing the resist film to a size of 1 to 4 μm or more to etch the undercoat film, which is the first problem that the undercoat film has a significantly different dimension from the resist film, and there is no description of baking after reflow to improve the adhesion between the reflowed resist film and the undercoat film, which makes the state prone to side etching, and in addition, the undercoat film is only reflowed twice in total, once before and once after the reflow of the resist film, so the side etching suppression effect is small.
[0014] The above-mentioned conventional technology disclosed in Patent Document 8 adopts a method of soaking in a chemical solution to dissolve and reflow as the first method, or a method of dissolving in a chemical solution to dissolve and reflow as the second method, as a method of soaking in a chemical solution to dissolve and reflow as the second method, as a method of soaking in a chemical solution to dissolve and reflow as the second method, as in Patent Documents 5 and 6. In this case, the first method (soaking in a chemical solution to dissolve and reflow) has the same problems as Patent Documents 5 and 6, and the other method (chemical solution to dissolve and reflow) dissolves the surface of the resist film and allows it to flow by exposing the organic solvent in a gaseous state, but the adhesiveness between the flowed resist film and the base film is made worse than the adhesiveness between the original resist film and the base film when the base film is etched, intentionally causing side etching of the base film to make the edge of the base film tapered, which is the opposite of the purpose of the present invention, and furthermore, since the etching is performed only once, there is a problem that side etching is more likely to occur than usual.
[0015] Therefore, it has been desired to provide a method for forming a pattern on a thin film, which is an underlying film, that is free from the drawbacks and problems associated with the above-mentioned conventional techniques (by suppressing side etching), and a processing apparatus therefor. [Prior art documents] [Patent documents]
[0016] [Patent Document 1] JP-A-50-37374 (column 3, lines 4 to 15, column 8, lines 4 to 9, Figures 1 and 2) [Patent Document 2] JP-A-60-234982 (column 3, lines 4 to 14, column 3, line 13 to column 4, line 12, Figures 1, 2 and 3) [Patent Document 3] JP-A-05-327179 (paragraphs 0008, 009, 0016 and FIG. 1) [Patent Document 4] JP-A-11-214826 (paragraphs 0013, 0014 and FIG. 4) [Patent Document 5] JP-A-53-77848 (column 3, lines 1 to 10, column 5, line 14 to column 6, line 8, Figure 2) [Patent Document 6] JP 57-16169 A (column 7, line 10 to column 8, line 9 and figures 1 to 5) [Patent Document 7] JP 2002-334830 A (paragraphs 0039, 0041, 0043 to 0053 and Figs. 1 and 2) [Patent Document 8] JP2005-303151A (paragraphs 0017, 0018, 0019, 0020, 0021, 0022, 0023, 0043 and Figures 1, 2, 3, and 4) DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0017] Therefore, a first object is to provide a method for forming a pattern on a thin film, which is an underlying film, that is free from the drawbacks and problems associated with the above-mentioned conventional techniques (by suppressing side etching).
[0018] A second object of the present invention is to provide a processing apparatus for implementing the method of the present invention for forming a pattern on a thin film that is an undercoat film (with suppressed side etching). [Means for solving the problem]
[0019] [Method of forming thin film patterns by etching] The first object of the present invention is to form a thin film pattern by suppressing side etching of the underlayer at the edge of an organic film pattern containing at least one organic substance formed on the underlayer or a mask of a pattern using a resist film, by dividing the total etching time, which is the sum of the shortest time required to etch and remove the entire underlayer at the part not covered with the resist film and the overetching time of 5 to 30% (or 0 to 100%) of the total etching time, into three or more times, and optimally, 4 to 10 times. In addition, in the case of processing a finer pattern (3 μm or less, etc.), a method of dividing the number of etching times into 11 to several tens of times may be used.
[0020] However, the etching can also be divided not by the total processing time but by the total thickness of the base film to be etched. As in the above, the etching can be divided into three or more steps, optimally four to ten steps, and in the case of finer patterns, eleven or several tens of steps, based on the thickness of the base film to be etched.
[0021] Before the first etching process, a post-bake process after development (which is also a pre-bake process before etching) is performed, and before each etching process from the second onwards (before each etching process from the second onwards through the final etching process), at least a resist characteristic modification process and a resist stabilization process are performed, and if necessary, a re-development process of the resist mask or an ashing process (mainly a process in an O2 gas plasma atmosphere) is added before each etching process.
[0022] However, a heat bake process (at 90 to 130° C. or less, which is lower than the curing temperature) and a temperature adjustment (cooling) process may be added before the etching process after the resist property changing process and resist stabilization process.
[0023] Here, the resist characteristic modification process refers to any one of the following four types: a) a process that has the effect of recovering or increasing the contact area between the resist mask and the base film after etching or recovering even a little the areas where adhesion has deteriorated: resist adhesion strengthening process; b) a process that changes the shape of the resist mask (at least a part of it remains solid, or is softened without liquefying, thereby bending or curving) to recover or increase the contact area between the base film and the resist film: resist deformation process 1; c) a process that changes the shape of the resist mask (at least a part of it is liquefied, dissolved, reflowed, or fluidized) to recover or increase the contact area between the base film and the resist film: resist deformation process 2; and d) a combination of any of a), b), or c).
[0024] In addition, substrate stabilization processing refers to any one of the following four types of processing: a) processing in which the temperature of the substrate is brought to room temperature or an optimum temperature, or is cooled: substrate temperature adjustment processing; b) processing in which liquids and the like adhering to the substrate are removed and dried by blowing hot or cold air, dry air, N2, etc.: substrate drying processing; c) processing in which liquids and the like adhering to the substrate are removed and dried by placing the substrate in a vacuum: substrate vacuum processing; and d) any combination of a), b), or c).
[0025] Furthermore, the redevelopment or ashing process of the resist mask, which is added as necessary, is either 1) a dissolution process that has some development effect on the resist mask (a dissolution effect with a difference in dissolution speed due to exposure / non-exposure), or 2) a so-called ashing process on the resist mask (a process of removing at least a part of the resist mask mainly by treatment in a plasma atmosphere of O2 gas). However, in the case of the redevelopment process 1), since the photosensitivity of the resist mask is affected by the environment after exposure, it is more effective to keep it in a state that is not exposed to light even after exposure.
[0026] The etching used here may be either wet etching or dry etching. In particular, in the case of dry etching, isotropic etching is effective.
[0027] [Thin film pattern formation processing equipment by etching] The pattern formation processing apparatus, which is the second object of the present invention, is a processing apparatus that realizes the thin film pattern formation method suppressing side etching of the undercoat film, which is the first object of the present invention, and is a processing apparatus composed of 1) an etching processing unit, 2) a resist property modification processing unit, and 3) a substrate stabilization processing unit as the minimum necessary processing units.
[0028] In addition, a substrate stabilization processing unit is either 1) a processing unit that has the effect of adjusting the temperature of a resist mask to room temperature or an optimal temperature before etching, 2) a processing unit that has the effect of removing liquid adhering to a resist mask or drying it, or a processing unit that has the combined effect of 1) and 2).
[0029] Furthermore, the resist mask redevelopment processing unit or ashing processing unit that is added as necessary is either 1) a dissolution processing unit that has some development effect on the resist mask (dissolution effect with a difference in dissolution speed due to exposure / non-exposure to light), or 2) a so-called ashing processing unit for the resist mask (processing to remove at least a part of the resist mask mainly by processing in a plasma atmosphere of O2 gas). However, in the case of the redevelopment processing unit 1), since the photosensitivity of the resist mask is affected by the environment after exposure, it is more effective to keep it in a state that is not exposed to light even after exposure.
[0030] Furthermore, the processing apparatus is configured as either 1) an apparatus with a multi-unit processing function or 2) an apparatus with a continuous unit processing function based on the processing sequence and processing conditions of the thin film pattern formation method that suppresses side etching of the underlying film, which is the first object of the present invention.
[0031] However, a heat bake processing unit (90 to 130° C. or less, which is lower than the cure temperature) and a temperature adjustment (cooling) processing unit may be added before the etching processing unit after the resist property modification processing unit and the resist stabilization processing unit. Effect of the Invention
[0032] The first object of the present invention is to suppress the side etching of the undercoat film by dividing the etching time of the undercoat film into at least three times, and optimally into about 4 to 10 times when considering the processing capacity (effective number of processes per hour). In addition, before each etching process, a resist characteristic change process is performed on the resist mask, and the adhesion between the resist mask and the undercoat film, which is separated and deteriorated by etching, is restored to an adhesion state and lateral dimension adhesion position almost equal to those before etching (the processing method and processing conditions are J1 conditions), or only the adhesion state is almost equal (the processing method and processing conditions are J2 conditions). In other words, it is possible to recover or increase the adhesion area between the undercoat film and the resist film. Therefore, the amount of side etching in each process is greatly suppressed, and the total (total) amount of side etching can be suppressed to only the first divided amount (under J1 conditions) or at least two divided amounts (under J2 conditions).
[0033] Therefore, if the amount of side etching in the conventional case where all etching is performed in one time is S1, and the number of divided etchings in the present invention is n times, then the total (total) amount of side etching in the present invention is Sn, Example 1) When the processing method and processing conditions for resist characteristic change processing are J1 conditions Sn≒(S1 / n) (≒ means approximately equal) Example 2) When the processing method and processing conditions for resist characteristic change processing are J2 conditions (S1 / n)≦Sn≦ (2×S1 / n) (≦ means the following) The larger the number of n, the more effectively the total (sum) amount of side etching can be suppressed. This calculation also shows that a number n of two is insufficient, and that it is important and necessary to set the number n to at least three in order to suppress side etching more than before.
[0034] Furthermore, when forming fine patterns (3µm or less) by wet etching, if emphasis is placed on fine pattern formation capability rather than processing capability, dividing the number of etching steps into 11 or even several tens of steps can have the effect of realizing finer pattern formation.
[0035] That is, in the case of the conventional process in which the base film in FIG. 1 is etched once, the total etching amount is E1y and the total side etching amount is E1x, and in the case of the process in which the base film in FIG. 2 is etched twice, the total etching amount is E2y and the total side etching amount is E2x, The total etching amount: E1x = E2x is the same, Total amount of etching on each side: E2y ≒ 1 / 2E2y (≒ means equal) This becomes a relationship.
[0036] The pattern formation processing apparatus, which is the second object of the present invention, is a processing apparatus which realizes the thin film pattern formation method suppressing side etching of the underlying film, which is the first object of the present invention, and is configured as a multi-processing unit apparatus or a continuous repetitive processing unit apparatus including the repetitive processing parts, i.e., at least 1) a resist property modification processing unit, 2) a substrate stabilization processing unit, and 3) an etching processing unit, and multi-processing or continuous repetitive processing is performed in each unit based on the processing order and processing conditions of the pattern formation method, which is the first object of the present invention, and has the effect of efficiently performing the processing of the pattern formation method, which is the first object of the present invention, and shortening the overall processing time.
[0037] However, in this apparatus, other processing units may be added as necessary, and processing may be added. Furthermore, as the processing method and processing conditions JI and J2 of the resist characteristic changing processing of the present invention, for example, J1 condition: The resist mask on the substrate is exposed to an organic solvent (the resist mask is partially dissolved and reflowed, and the resist mask dimensions expand by about 1 / 10 to 2 / 10) and baked at 110 to 130°C for 3 to 10 minutes, after which the entire substrate is cooled to room temperature (approximately 25°C). J2 condition: The resist mask on the substrate is exposed to an organic solvent (the resist mask is partially dissolved and reflowed, but the resist mask dimensions remain almost unchanged or expand to within 1 / 10 of their original size) and baked at 110-130°C for 3-10 minutes, after which the entire substrate is cooled to room temperature (approximately 25°C). However, under the above J1 and J2 conditions, if the resist mask material can be repeatedly dissolved and reflowed at or below the cure temperature (returns to original state when cooled), exposure to organic solvent vapor is not necessary, and heating and cooling alone are sufficient.
[0038] The conventional techniques will be described below with reference to the drawings. FIG. 1 shows an example of wet etching, which is an isotropic etching, as the conventional technique 1. First, a resist film is applied onto an undercoat film T0, and after pre-baking (pre-heating), exposure, development, and post-baking (post-heating), a resist mask pattern P1 is formed, and then the undercoat film T0 is etched to form an undercoat film pattern T1. In this case, the undercoat film is, for example, a 0.5 μm copper (Cu) film, and a positive resist film made of a novolac resin and a photosensitive agent is applied to a thickness of 1 to 3 μm using a spin coater or the like, and is pre-baked by heating at 100 to 110° C. for 1 to 3 minutes, and then exposed and developed (with an alkaline aqueous solution) to form a resist pattern P1 with a pattern width of 2 μm. Further, post-baking is performed by heating at 110 to 120° C. for 3 to 5 minutes to obtain the state shown in FIG. 1(a).
[0039] Next, as an etching solution for the copper (Cu) film of the base film T0, for example, a ferric chloride solution, a cupric chloride solution, an alkaline ammonia (alkaline ammonia) solution, a sulfuric acid hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution, etc. are used, and the etching rate is, for example, a composition that gives an etching rate of 0.25 to 0.5 μm / min at 25°C. In this case, the base film pattern T1 is formed by processing for 66 seconds (just etching 60 seconds + overetching 6 seconds) with a composition that gives an etching rate of 0.5 μm / min, resulting in the state shown in Figure 1(b).
[0040] In the case of this prior art 1, etching of a film thickness of 0.5 μm is performed for 66 seconds at an etching rate of 0.5 μm / min. Since this is isotropic etching, the side etching is at least 0.5 μm or more from both ends, and the upper part of the base film pattern T1 is 1.0 μm or less.
[0041] FIG. 2 shows a conventional technique 2 in which the undercoat film T0 is etched twice, as described in Patent Documents 1 to 8, and each etching time is divided equally into 1 / 2 of the time required for the entire etching (in this case, the total is 66 seconds, so each etching time is 33 seconds). In this case, the undercoat film T0 is a 0.5 μm copper (Cu) film as in Conventional Technique 1, and a positive resist film made of a novolac resin and a photosensitive agent is applied to a thickness of 1 to 3 μm using a spin coater or the like, and is prebaked by heating at 100 to 110° C. for 1 to 3 minutes, and then exposed and developed (in an alkaline aqueous solution) to form a resist pattern P1 with a pattern width of 2 μm. Further, postbaked by heating at 110 to 120° C. for 3 to 5 minutes, the state shown in FIG. 2(a) is obtained.
[0042] Next, the copper (Cu) film of the base film T0 is etched. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution similar to that of the conventional technique 1, and has a composition that results in an etching rate of 0.5 μm / min at 25° C. The base film pattern T1 is formed by processing for 33 seconds, resulting in the state shown in FIG. 2(b).
[0043] Next, the resist pattern P1 is heated at a high temperature (cures and flows the resist film: 140°C to 200°C near the softening point), or is immersed in an organic solvent chemical, or is exposed to steam for chemical dissolution reflow (or chemical gas exposure) processing, causing the resist pattern P1 to flow and transform into resist pattern P2. However, the amount and shape of flow are different in the case of high-temperature heating processing and in the case of chemical dissolution reflow (or chemical gas exposure) processing, and the latter has the characteristic of being more likely to become a more liquid and fluid flow at a lower temperature. This is because the former evaporates and removes the solvent in the resist pattern 1, while the latter penetrates the resist pattern 1 and actually liquefies and transforms at least a part of its surface to form resist pattern P2.
[0044] Next, the former high-temperature heat treatment is left as is, and only in the latter case where chemical dissolution reflow (or exposure to chemical gas) is performed, a post-bake heat treatment is performed at 110-120°C for 3-5 minutes to reach the state shown in Figure 2(c).
[0045] Next, the copper (Cu) film of the base film pattern T1 is etched for the second time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution similar to that used in the prior art 1, and is a composition that results in an etching rate of 0.5 μm / min at 25° C. The etching is performed for 33 seconds to form a base film pattern T2, resulting in the state shown in FIG. 2(d).
[0046] In the case of conventional technique 2, the etching of the 0.5 μm thick undercoat film T0 is performed at an etching rate of 0.5 μm / min for a total of 66 seconds, with two processes of 33 seconds each. Since this is isotropic etching, side etching proceeds, but the amount of side etching each time is less than the amount of etching performed once, so the final amount of side etching is only half of the usual amount.
[0047] However, what is important here is that the amount of side etching in the first and second steps is still large and the etching rate is also fast, so the etching solution easily penetrates into the resist interface, resulting in larger side etching than expected, which is not as large as in prior art 1, but is larger than the amount of side etching described in paragraph 0035 above.
[0048] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Here, a method for forming a pattern on a thin film by etching according to the present invention will be described. Example 1
[0049] FIG. 3 shows Example 1 of the present invention. In this Example 1, the undercoat film T0 is etched three times, and each etching time is divided equally into 1 / 3 depending on the number of etchings (in this case, the total etching time is 66 seconds, so each etching time is about 22 seconds). However, if the etching time per etching is too short, the controllability of the etching deteriorates, so the composition of the etching solution is adjusted and the etching rate is reduced to 1 / 2 to 1 / 5. In this case, the etching rate is set to 1 / 5, and the etching is performed for a total of 330 seconds (just etching 300 seconds + overetching 30 seconds), and each etching time is 110 seconds.
[0050] In this case, the undercoat film T0 is a 0.5 μm copper (Cu) film, and a positive resist film made of novolac resin and photosensitive agent is applied to a thickness of 1 to 3 μm using a spin coater or the like, and then pre-baked at 100 to 110°C for 1 to 3 minutes, exposed, and developed (with an alkaline aqueous solution) to form a resist pattern P1 with a pattern width of 2 μm.Furthermore, post-baked at 110 to 120°C for 3 to 5 minutes, the temperature of the substrate is then adjusted (cooled) to bring the substrate temperature to room temperature (around 25°C), resulting in the state shown in FIG. 3(a).
[0051] Next, the copper (Cu) film of the base film T0 is etched. The etching solution is an etching solution such as a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution, as described in paragraph 0039 above, which is formulated to give an etching rate of 0.1 μm / min at 25° C. After treatment for 110 seconds, a base film pattern T1 is formed, resulting in the state shown in FIG. 3(b).
[0052] Next, a resist characteristic change process is performed on the resist mask pattern (hereinafter, may be called a resist mask or a resist pattern) P1. As shown in FIG. 11-7, the resist characteristic change process is as follows: (a) Resist adhesion strengthening treatment: A treatment that has the effect of restoring even a little the adhesion between the resist mask and the base film that has deteriorated after etching, i.e., a treatment that restores or increases the adhesion area between the base film and the resist film. (b) Resist deformation process 1: A process in which at least a part of the resist mask pattern remains solid or is softened without being liquefied, and is bent or curved, etc., to recover or increase the contact area between the base film and the resist film. (c) Resist transformation process 2: A process that has the effect of liquefying, dissolving, reflowing, fluidizing, or the like at least a part of the resist mask pattern, thereby recovering or increasing the contact area between the base film and the resist film. (d) is a combination of (a), (b), and (c). However, in terms of dimensions, in resist deformation process 2, where at least a portion of the resist is liquefied, there may be a large change in any of the dimensions of length, width, or thickness after deformation, but in resist deformation process 1, where the resist remains solid or is not liquefied, there is also a feature that the total dimensions of length, width, and thickness do not change significantly even after deformation.
[0053] Thereafter, the resist mask pattern P1 is subjected to a substrate stabilization process. As shown in FIG. (a) Substrate temperature control process: A process that adjusts the temperature of the resist mask to room temperature or to an optimal temperature before etching. (b) Substrate drying process: A process that has the effect of removing liquid adhering to the resist mask and drying it. (c) Substrate vacuum drying process: A process of vacuum drying to remove liquid adhering to the resist mask and to dry it. (d) A combination of (a), (b), and (c). However, the resist characteristic changing process and the substrate state stabilizing process are not limited to the following examples shown in the first embodiment.
[0054] However, in this Example 1, an example of a chemical dissolving reflow (or chemical gas exposure) process is shown as an example of (c) resist deformation process 2 in the resist property changing process of Figure 11-7, in which the resist mask pattern P1 is exposed to the vapor of an organic solvent chemical, and the solvent is penetrated into the resist mask pattern P1, and at least a part of the surface is actually liquefied and deformed to form a resist mask pattern P2.Furthermore, as an (a) resist adhesion strengthening process, a post-bake heating process is performed at 110 to 120°C for 3 to 5 minutes, and then, as an (a) substrate temperature adjustment process in the substrate state stabilization process of Figure 11-8, the substrate is placed on a plate at room temperature so that the substrate temperature is brought to room temperature, and left for 3 to 5 minutes until it cools to room temperature, resulting in the state of Figure 3(c).
[0055] Next, the copper (Cu) film of the base film pattern T1 is etched for the second time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, which is used at 25°C and has an etching rate of 0.1 μm / min. The etching is performed for 110 seconds to form the base film pattern T2, as shown in Figure 3(d).
[0056] Next, the resist mask pattern P2 is subjected to a process similar to that described in paragraphs 0052 to 0054 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P3, which is shown in FIG. 3(e).
[0057] Next, the copper (Cu) film of the base film pattern T2 is etched for the third time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like with a composition that results in an etching rate of 0.1 μm / min at 25°C. The etching is performed for 110 seconds to form the base film pattern T3, resulting in the state shown in Figure 3(f).
[0058] In the case of Example 1 of the present invention, the etching of the 0.5 μm-thick undercoat film T0 is performed at an etching rate of 0.1 μm / min for a total of 330 seconds, three times for 110 seconds each. Since this is isotropic etching, side etching proceeds, but the amount of side etching each time is less than the amount of etching in one time, so the final amount of side etching in Example 1 is only 1 / 3 of the usual amount.
[0059] However, what is important here is that, when the etching thickness is divided into three layers of the upper, middle and lower layers, the etching of the base film T0 is divided into three steps, and after each etching process, a chemical dissolution reflow (or chemical gas exposure) process and a post-bake process are performed. Therefore, in the second and third etchings, the adhesion of the resist mask patterns P1, P2 to the base films T1, T2 is strong, and the etching rate is kept low. Also, the processing time is limited to the amount of etching for each layer equal to the etching thickness, so that at least in the third etching of the lower layer, the etching area of the first upper layer is not affected.
[0060] This is the reason why the amount of side etching in Example 1 of the present invention is kept low compared to the amounts of side etching in Conventional Techniques 1 and 2. Furthermore, it is shown that the etching divided into three or more steps, which is a feature of the present invention, is important, and that there is a large significant difference compared to etching two or less steps.
[0061] Furthermore, if necessary, a redevelopment process or an ashing process of the resist mask may be added during the above process, which is either 1) a dissolution process that has some development effect on the resist mask (a dissolution effect with a difference in dissolution rate due to exposure / non-exposure), or 2) a so-called ashing process on the resist mask (a process of removing at least a part of the resist mask mainly by processing in a plasma atmosphere of O2 gas). However, in the case of the redevelopment process 1), since the photosensitivity of the resist mask due to the environment after exposure affects it, it is more effective to keep it in a state where it is not exposed to light even after exposure. This is added in order to suppress, reduce, or return the dimensional expansion of the resist mask due to the resist deformation processes 1 and 2 (especially large in the case of the resist deformation process 2) to the original dimensions (i.e., suppress, reduce, or return the dimensional expansion of the underlying film pattern after etching due to the dimensional expansion of the mask pattern to the original dimensions). Example 2
[0062] 4 shows Example 2 of the present invention. In this Example 2, the undercoat film T0 is etched four times, and the time required for the entire etching is divided equally into 1 / 4 depending on the number of etchings. However, in Example 2, as in Example 1, if the etching time per etching is too short, the controllability of the etching deteriorates, so the composition of the etching solution is adjusted to 1 / 5 and the etching time is adjusted to 330 seconds in total (just etching 300 seconds + overetching 30 seconds), and each etching is performed for 82.5 seconds.
[0063] In this case, the undercoat film T0 is a 0.5 μm copper (Cu) film, and a positive resist film made of novolac resin and photosensitive agent is applied to a thickness of 1 to 3 μm using a spin coater or the like, and then pre-baked at 100 to 110°C for 1 to 3 minutes, exposed, and developed (with an alkaline aqueous solution) to form a resist mask pattern P1 with a pattern width of 2 μm.Furthermore, post-baked at 110 to 120°C for 3 to 5 minutes, the temperature of the substrate is then adjusted (cooled) to bring the substrate temperature to room temperature (around 25°C), resulting in the state shown in FIG. 4(a).
[0064] Next, the copper (Cu) film of the base film T0 is etched. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, as described in paragraph number 0051 above, and is formulated to give an etching rate of 0.1 μm / min at 25° C. The base film pattern T1 is formed by treating for 82.5 seconds, resulting in the state shown in Figure 4(b).
[0065] Next, a resist characteristic change process is performed on the resist mask pattern (hereinafter, may be called a resist mask or a resist pattern) P1. As shown in FIG. 11-7, the resist characteristic change process is as follows: (a) Resist adhesion strengthening treatment: A treatment that has the effect of restoring even a little the adhesion between the resist mask and the base film that has deteriorated after etching, i.e., a treatment that restores or increases the adhesion area between the base film and the resist film. (b) Resist deformation process 1: A process in which at least a part of the resist mask pattern remains solid or is softened without being liquefied, and is bent or curved, etc., to recover or increase the contact area between the base film and the resist film. (c) Resist transformation process 2: A process that has the effect of liquefying, dissolving, reflowing, fluidizing, or the like at least a part of the resist mask pattern, thereby recovering or increasing the contact area between the base film and the resist film. (d) A combination of (a), (b), and (c). However, in terms of dimensions, in resist deformation process 2, where at least a portion of the resist is liquefied, there may be a large change in any of the dimensions of length, width, or thickness after deformation, but in resist deformation process 1, where the resist remains solid or is not liquefied, there is also a feature that the total dimensions of length, width, and thickness do not change significantly even after deformation.
[0066] Thereafter, the resist mask pattern P1 is subjected to a substrate stabilization process. As shown in FIG. (a) Substrate temperature control process: A process that adjusts the temperature of the resist mask to room temperature or to an optimal temperature before etching. (b) Substrate drying process: A process that has the effect of removing liquid adhering to the resist mask and drying it. (c) Substrate vacuum drying process: A process of vacuum drying to remove liquid adhering to the resist mask and to dry it. (d) A combination of (a), (b), and (c). However, the resist characteristic changing process and the substrate state stabilizing process are not limited to the following examples shown in the second embodiment.
[0067] However, in this embodiment 2, as the resist deformation process 2 in the resist characteristic change process of FIG. 11-7, an example of exposing to the vapor of an organic solvent chemical solution to chemical solution reflow (or exposure to chemical gas) is shown, and the solvent is penetrated into the resist mask pattern P1, and at least a part of the surface is actually liquefied and deformed to form a resist mask pattern P2. Furthermore, as the resist adhesion strengthening process of (a), a post-bake is performed at 110 to 120° C. for 3 to 5 minutes, and then, as the substrate temperature control process in the substrate state stabilization process of FIG. 11-8, the substrate is placed on a plate at room temperature so that the substrate temperature is kept at room temperature, and is left for 3 to 5 minutes until it cools to room temperature, resulting in the state of FIG. 4(c).
[0068] Next, the copper (Cu) film of the base film pattern T1 is etched for the second time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, which is formulated to give an etching rate of 0.1 μm / min at 25°C, and is treated for 110 seconds to form the base film pattern T2, resulting in the state shown in Figure 4(d).
[0069] Next, the resist mask pattern P2 is subjected to a process similar to that described in paragraphs 0065 to 0067 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P3, resulting in the state shown in Figure 4(e).
[0070] Next, the copper (Cu) film of the base film pattern T2 is etched for the third time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like with a composition that results in an etching rate of 0.1 μm / min at 25°C, and the treatment is performed for 82.5 seconds to form the base film pattern T3, resulting in the state shown in Figure 4(f).
[0071] Next, the resist mask pattern P3 is subjected to a similar process to that described in paragraphs 0065 to 0067 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P4, as shown in Figure 4(g).
[0072] Next, the copper (Cu) film of the base film pattern T3 is etched for the fourth time. As described in paragraph 0064 above, the etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, which is formulated to give an etching rate of 0.1 μm / min at 25° C., and the etching is performed for 82.5 seconds to form the base film pattern T4, resulting in the state shown in FIG. 4(h).
[0073] In the case of Example 2 of the present invention, the etching of the 0.5 μm-thick undercoat film T0 is performed at an etching rate of 0.1 μm / min for a total of 330 seconds, four times for 82.5 seconds each. Since this is isotropic etching, side etching proceeds, but the amount of side etching each time is less than the amount of etching in one time, so the final amount of side etching in Example 2 is only 1 / 4 of the usual amount.
[0074] However, what is important here is that when the etching thickness is divided into four layers, i.e., layers 1, 2, 3, and 4, the etching of the base film T0 is divided into four steps, and after each etching process, as a resist characteristic modification process (Figure 11-7), an example of a chemical dissolution reflow (or chemical gas exposure) process is shown in which the resist is exposed to the vapor of an organic solvent chemical as (c) resist deformation process 2, and further, a post-bake process is also performed as a resist adhesion strengthening process (a). Therefore, in the second, third, and fourth etchings, the adhesion of the resist mask patterns P1, P2, and P3 to the bases T1, T2, and T3 is strong, and the etching rate is kept low. Also, since the etching amount for each layer is only the amount of etching for the etching thickness during the processing time, there is no effect on the etching area of layer 1 at least in the third etching, and on the etching areas of layers 1 and 2 in the fourth etching.
[0075] This is the reason why the amount of side etching in Example 2 of the present invention is kept low compared to the amounts of side etching in Conventional Techniques 1 and 2. Furthermore, it is shown that the etching divided into three or more steps, which is a feature of the present invention, is important, and that there is a large significant difference compared to etching two or less steps.
[0076] Furthermore, if necessary, a redevelopment process or an ashing process of the resist mask may be added during the above process, which is either 1) a dissolution process that has some development effect on the resist mask (a dissolution effect with a difference in dissolution rate due to exposure / non-exposure), or 2) a so-called ashing process on the resist mask (a process of removing at least a part of the resist mask mainly by processing in a plasma atmosphere of O2 gas). However, in the case of the redevelopment process 1), since the photosensitivity of the resist mask due to the environment after exposure affects it, it is more effective to keep it in a state where it is not exposed to light even after exposure. This is added in order to suppress, reduce, or return the dimensional expansion of the resist mask due to the resist deformation processes 1 and 2 (especially large in the case of the resist deformation process 2) to the original dimensions (i.e., suppress, reduce, or return the dimensional expansion of the underlying film pattern after etching due to the dimensional expansion of the mask pattern to the original dimensions). Example 3
[0077] Figures 5-1 and 5-2 show Example 3 of the present invention. In this Example 3, the undercoat film T0 is etched seven times, and each etching time is divided equally into 1 / 7 of the time required for the entire etching depending on the number of etchings. However, in Example 3, as in Examples 1 and 2, if the etching time per etching is too short, the etching controllability becomes poor, so the composition of the etching solution is adjusted to 1 / 10 of the rate, and the etching is performed for a total of 660 seconds (just etching 600 seconds + overetching 60 seconds), and each etching is performed for 94.3 seconds.
[0078] In this case, the undercoat film T0 is a 0.5 μm copper (Cu) film, and a positive resist film made of novolac resin and photosensitive agent is applied to a thickness of 1 to 3 μm using a spin coater or the like, and then pre-baked at 100 to 110°C for 1 to 3 minutes, exposed, and developed (with an alkaline aqueous solution) to form a resist pattern P1 with a pattern width of 2 μm.Furthermore, post-baked at 110 to 120°C for 3 to 5 minutes, the temperature of the substrate is adjusted (cooled) to bring the substrate temperature to room temperature (around 25°C), resulting in the state shown in Figure 5-1(a).
[0079] Next, the copper (Cu) film of the base film T0 is etched. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, as described in paragraph number 0072 above, and is formulated to give an etching rate of 0.05 μm / min at 25°C. The base film pattern T1 is formed by treating the base film for 94.3 seconds, resulting in the state shown in Figure 5-1(b).
[0080] Next, a resist characteristic changing process is performed on the resist mask pattern P1. As shown in FIG. (a) Resist adhesion strengthening treatment: A treatment that has the effect of restoring even a little the adhesion between the resist mask and the base film that has deteriorated after etching, i.e., a treatment that restores or increases the adhesion area between the base film and the resist film. (b) Resist deformation process 1: A process in which at least a part of the resist mask pattern remains solid or is softened without being liquefied, and is bent or curved, etc., to recover or increase the contact area between the base film and the resist film. (c) Resist transformation process 2: A process that has the effect of liquefying, dissolving, reflowing, fluidizing, or the like at least a part of the resist mask pattern, thereby recovering or increasing the contact area between the base film and the resist film. (d) A combination of (a), (b), and (c). It can be one of the following.
[0081] Thereafter, the resist mask pattern P1 is subjected to a substrate stabilization process. As shown in FIG. (a) Substrate temperature control process: A process that adjusts the temperature of the resist mask to room temperature or to an optimal temperature before etching. (b) Substrate drying process: A process that has the effect of removing liquid adhering to the resist mask and drying it. (c) Substrate vacuum drying process: A process of vacuum drying to remove liquid adhering to the resist mask and to dry it. (d) A combination of (a), (b), and (c). However, the resist characteristic changing process and the substrate state stabilizing process are not limited to the following examples shown in the third embodiment.
[0082] However, in this Example 3, as the resist characteristic changing process in FIG. 11-7, an example of a chemical dissolving reflow (or chemical gas exposure) process by exposing to the vapor of an organic solvent chemical is shown as (c) resist deformation process 2, and further, as an example of (a) resist adhesion strengthening process, a post-bake process is also shown in combination, and a solvent is penetrated into the resist mask pattern P1, and at least a part of the surface is actually liquefied and deformed to form a resist mask pattern P2. Further, as the (a) resist adhesion strengthening process, a post-bake heat treatment is performed at 110 to 120°C for 3 to 5 minutes, and then, as the (a) substrate temperature adjustment process in the substrate state stabilization process in FIG. 11-8, the substrate is placed on a plate at room temperature so that the substrate temperature is kept at room temperature, and left for 3 to 5 minutes until it cools to room temperature, and the state in FIG. 5-1(c) is achieved.
[0083] Next, the copper (Cu) film of the base film pattern T1 is etched for the second time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, which is formulated to give an etching rate of 0.1 μm / min at 25°C, and is treated for 110 seconds to form the base film pattern T2, resulting in the state shown in Figure 5-1(d).
[0084] Next, the resist mask pattern P2 is subjected to a process similar to that described in paragraphs 0080 to 0082 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P3, resulting in the state shown in Figure 5-1(e).
[0085] Next, the copper (Cu) film of the base film pattern T2 is etched for the third time. As described in paragraph number 0079 above, the etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like with a composition that results in an etching rate of 0.05 μm / min at 25° C., and the etching is performed for 94.3 seconds to form the base film pattern T3, resulting in the state shown in Figure 5-1(f).
[0086] Next, the resist mask pattern P3 is subjected to a process similar to that described in paragraphs 0080 to 0082 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P4, resulting in the state of Figure 5-1(g).
[0087] Next, the copper (Cu) film of the base film pattern T3 is etched for the fourth time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like with a composition that results in an etching rate of 0.05 μm / min at 25°C. The etching is performed for 94.3 seconds to form the base film pattern T4, resulting in the state shown in Figure 5-1(h).
[0088] Next, the resist mask pattern P4 is subjected to a process similar to that described in paragraphs 0080 to 0082 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P5, which is shown in Figure 5-2(i).
[0089] Next, the copper (Cu) film of the base film pattern T4 is etched for the fifth time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like with a composition that results in an etching rate of 0.05 μm / min at 25°C. The etching is performed for 94.3 seconds to form the base film pattern T5, resulting in the state shown in Figure 5-2(j).
[0090] Next, the resist mask pattern P5 is subjected to a process similar to that described in paragraphs 0080 to 0082 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P6, which is shown in FIG. 5-2(k).
[0091] Next, the copper (Cu) film of the base film pattern T5 is etched for the sixth time. The etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, which is formulated to give an etching rate of 0.05 μm / min at 25°C, and is processed for 94.3 seconds to form the base film pattern T6, which is in the state shown in Figure 5-2(l).
[0092] Next, the resist mask pattern P6 is subjected to a process similar to that described in paragraphs 0080 to 0082 above, which is a process for changing the resist mask pattern P1 to P2, thereby changing it into the resist mask pattern P7, resulting in the state of FIG. 5-2(m).
[0093] Next, the copper (Cu) film of the base film pattern T6 is etched for the seventh time. As described in paragraph number 0085 above, the etching solution is a sulfuric acid / hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution or the like, which is formulated to give an etching rate of 0.05 μm / min at 25° C., and the etching is performed for 94.3 seconds to form the base film pattern T7, resulting in the state shown in Figure 5-2(n).
[0094] In the case of Example 3 of the present invention, the etching of the 0.5 μm-thick undercoat film T0 is performed at an etching rate of 0.05 μm / min for a total of 660 seconds, seven times for 94.3 seconds each. Since this is isotropic etching, side etching proceeds, but the amount of side etching each time is less than the amount of etching in one time, so the final amount of side etching in Example 3 is 1 / 7 of the usual amount.
[0095] However, what is important here is that when the etching thickness of layers 1 to 7 is divided into seven layers, the etching of the base film T0 is divided into seven times, and after each etching process, a chemical solution reflow (or chemical gas exposure) process and a post-bake process are performed, so that in the second to seventh etchings, the resist patterns P2 to P7 have strong adhesion to the base films T1 to T6, and the etching rate is kept low. Since the etching time is only the amount of etching for each layer, at least from the third etching onwards, there is no effect on the etching area of the layer two or more above each etching layer. In this way, the more times the etching of the base film is divided into three or more times, the smaller the degree of influence on the side of the base film is, so that the overall amount of side etching is significantly suppressed.
[0096] This is the reason why the amount of side etching is suppressed to be lower in Example 3 of the present invention than in Examples 1 and 2 of the present invention, compared with the amount of side etching in the conventional techniques 1 and 2, and furthermore, shows that it is important to perform etching in three or more steps, which is a feature of the present invention, and that there is a large significant difference from etching in two or less steps.
[0097] Furthermore, if necessary, a redevelopment process or an ashing process of the resist mask may be added during the above process, which is either 1) a dissolution process that has some development effect on the resist mask (a dissolution effect with a difference in dissolution rate due to exposure / non-exposure), or 2) a so-called ashing process on the resist mask (a process of removing at least a part of the resist mask mainly by processing in a plasma atmosphere of O2 gas). However, in the case of the redevelopment process 1), since the photosensitivity of the resist mask due to the environment after exposure affects it, it is more effective to keep it in a state where it is not exposed to light even after exposure. This is added in order to suppress, reduce, or return the dimensional expansion of the resist mask due to the resist deformation processes 1 and 2 (especially large in the case of the resist deformation process 2) to the original dimensions (i.e., suppress, reduce, or return the dimensional expansion of the underlying film pattern after etching due to the dimensional expansion of the mask pattern to the original dimensions).
[0098] In the resist characteristic modification process used in the present invention, (a) resist adhesion strengthening process: specific examples of a process that has the effect of recovering even a little the adhesion between the resist mask and the base film that has deteriorated after etching, i.e., recovering or increasing the adhesion area between the base film and the resist film, include heating (baking) process at a temperature lower than the cure temperature of the resist mask (e.g., 100 to 130°C), coating, immersion, and steam exposure of a chemical solution (organic solvent, solution containing an adhesion strengthener, or aqueous solution), and irradiation process with electromagnetic waves, infrared rays, ultraviolet rays, etc.
[0099] (b) Resist deformation process 1: Specific examples of processes that have the effect of slightly changing (softening, curving, etc.) the shape of the resist mask include a process in which a resist material is selected that softens and curves repeatedly by heating (baking) at temperatures below the cure temperature (e.g., 100 to 130°C) due to the characteristics of the resist material itself, and a heating (baking) process in which the film thickness of the resist mask is thinned (e.g., 1 µm or less, 1 / 2 or less of the film thickness of the base film).
[0100] (c) Resist deformation process 2: Specific examples of processes that have the effect of even slightly changing (dissolving, reflowing, fluidizing, etc.) the shape of the resist mask include immersion in an organic solvent or other chemical that has the effect of reflowing the resist, vapor exposure to the chemical, etc. Here, a more specific example of the chemical dissolution reflow (or chemical gas exposure) process is described in detail below from paragraph number 0104 onwards.
[0101] In addition, in the substrate stabilization process, (a) Substrate temperature adjustment process: Specific examples of processes that have the effect of adjusting the temperature of the resist mask to room temperature or an optimal temperature before etching include leaving it on a plate that is at room temperature or cooled (20 to 30°C), and cooling the substrate temperature to room temperature by blowing low-temperature or room-temperature N2, air, or other gas.
[0102] (b) Substrate drying process: Examples of processes that are effective in removing or drying liquid adhering to the resist mask include gas blowing with N2 or air at room temperature to slightly higher temperatures (e.g., 30 to 80°C), drying by air knife blowing, etc. In addition, this also includes processes for improving the hydrophilicity of the substrate, or conversely, for decreasing the hydrophilicity.
[0103] (c) Substrate vacuum drying process: A specific example of a process for vacuum drying to remove liquid adhering to a resist mask or to dry it is to use a gas blow such as N2 or air at room temperature to a slightly higher temperature (e.g., 30 to 80°C) or an air knife blow, followed by drawing a vacuum in the room in which the substrate is placed and drying it.
[0104] Here, as an example of a chemical dissolution reflow (or chemical gas exposure) process in which the resist is exposed to the vapor of an organic solvent as the (c) resist deformation process 2 in the resist characteristic change process of Figure 11-7, a chemical dissolution reflow (or chemical gas exposure) process using an organic solvent is described in detail below.
[0105] The organic solvents used in the chemical dissolution reflow (or chemical gas exposure) treatment of the present invention are mainly solvents used in organic masks, and resist materials, such as thinners, but the following chemicals and mixtures thereof can be used as long as they are organic solvents. Specifically, acetone, propylene glycol monoethyl ether, tripropylene glycol monoethyl ether, N-methyl-2-pyrrolidone, and further, the organic solvents are divided into organic solvents as higher-level concepts and organic solvents as lower-level concepts that embody them below. (R represents an alkyl group or a substituted alkyl group, and Ar represents a phenyl group or an aromatic ring other than a phenyl group) Organic solvents: Alcohols (R-OH) Alkoxy alcohols Ethers (ROR, Ar-OR, Ar-O-Ar) Esters Ketones Glycols Alkylene glycols Glycol ethers Specific examples of the above organic solvents: CH3OH, C2H5OH,CH3(CH2)XOH·Isopropyl alcohol (IPA)·Ethoxyethanol·Methoxy alcohol·Long chain alkyl esters·Monoethanolamine (MEA)·Acetone·Acetylacetone·Dioxane·Ethyl acetate·Butyl acetate·Toluene·Methyl ethyl ketone (MEK)·Diethyl ketone·Dimethyl sulfoxide (DMSO)·Methyl isobutyl ketone (MIBK)·Butyl carbitol·n-Butyl acetate (nBA)·Gamma-butyrolactone·Ethyl cellosolve acetate (ECA)·Ethyl lactate·Ethyl pyruvate·2-Heptanone (MAK)·3-Methoxybutyl acetate·Ethylene glycol·Propylene glycol·Butylene glycol·Ethylene glycol monoethyl ether·Diethylene glycol monoethyl ether·Ethylene glycol monoethyl ether acetate·Ethylene glycol monomethyl ether·Ethylene glycol monomethyl ether acetate·Ethylene glycol mono-n-butyl ether·Polyethylene glycol Polypropylene glycol Polybutylene glycol Polyethylene glycol monoethyl ether Polydiethylene glycol monoethyl ether Polyethylene glycol monoethyl ether acetate Polyethylene glycol monomethyl ether Polyethylene glycol monomethyl ether acetate Polyethylene glycol mono-n-butyl ether Methyl 3-methoxypropionate (MMP) Propylene glycol monomethyl ether (PGME) Propylene glycol monomethyl ether acetate (PGMEA) Propylene glycol monopropyl ether (PGP) Propylene glycol monoethyl ether (PGEE) Ethyl 3-ethoxypropionate (FEP) Dipropylene glycol monoethyl ether Tripropylene glycol monoethyl ether Polypropylene glycol monoethyl ether Propylene glycol monomethyl ether propionate Methyl 3-methoxypropionate 3-ethoxypropionate Ethyl acetate, N-methyl-2-pyrrolidone (NMP), pentanone, cyclopropane, cyclopentanone, 2-heptylcyclopentanone, 2-pentylcyclopentanone, 2-methyl-3-2-pentanone, 4-methyl-2-pentanone, methyl isobutyl ketone,Methyl propyl ketone, etc.
[0106] The step of subjecting the resist film or resist pattern to the organic solvent reflow treatment may be a step of exposing the organic film pattern to an organic solvent-containing gas containing the organic solvent. The organic solvent-containing gas may be a vapor gas of the organic solvent or a mixed gas in which an organic solvent is mixed with an inert gas (N2, Ar, etc.).
[0107] The method of exposure to chemical vapor can be a method of exposing the chemical (including the organic solvent) to a gas in which an inert gas such as N2 (or Ar) is bubbled into the chemical, or a method of exposing the chemical to a gas sprayed simultaneously with an inert gas such as N2 (or Ar).
[0108] The etched portion of the base film is reflow-deformed so as to cover at least a part of it to the entirety thereof, and the degree of reflow deformation covering the base film is controlled by managing the time of exposure to the chemical vapor, and the degree of reflow deformation depends on the penetration depth, i.e., the penetration amount, of the organic solvent into the organic film pattern and the properties of the organic solvent.
[0109] The penetration depth, i.e., the penetration amount, of an organic solvent into a resist film pattern (hereinafter, an example of an organic film pattern) containing an organic solvent depends on the material constituting the organic film pattern, the concentration of the organic solvent in an organic solvent-containing gas, and the contact time, i.e., the processing time, during which the organic film pattern is in contact with the organic solvent. It is highly likely that the material constituting the organic film pattern is determined by a factor other than the penetration depth of the organic solvent into the organic film pattern. Therefore, the penetration depth, i.e., the penetration amount, of the organic solvent into the organic film pattern can be adjusted by adjusting the concentration of the organic solvent in the organic solvent-containing gas and the contact time, i.e., the processing time, during which the organic film pattern is in contact with the organic solvent.
[0110] When the amount of penetration of the organic solvent into the organic film pattern is small, dissolution reflow does not occur. On the other hand, when the amount of penetration of the organic solvent into the organic film pattern is large, dissolution reflow occurs. The critical value of the penetration amount at which dissolution reflow occurs depends on conditions including the physical properties and concentration of the organic solvent and the physical properties of the organic film pattern. In any case, when the amount of penetration of the organic solvent into the organic film pattern is less than the critical value, dissolution reflow does not occur, and when the amount of penetration exceeds the critical value, dissolution reflow occurs. Therefore, when the required horizontal dimension of the bottom of the organic solvent penetration region in which the adhesion to the undercoat film is adjusted is about the organic solvent penetration depth, and a predetermined deformation of the organic film pattern occurs due to dissolution reflow and no more is required, dissolution reflow can be stopped by stopping the contact of the organic film pattern with the organic solvent.
[0111] During the divided etching process, the resist film is reflowed and deformed by using the chemical vapor dissolution reflow method so as to cover at least a part of the etched part of the undercoat film to cover the whole, and the part is also heated and baked to improve the adhesion between the resist film and the undercoat film, so that the next side etching of the undercoat film starts from the position of the reflowed resist film, and for example, if the reflow amount is always reflowed to fill the side etching of the undercoat film, the side etching amount can be reset every time. The time management of the reflow amount is important, and by managing it, the side etching amount and the dimensions of the finished undercoat film can be controlled.
[0112] The processing steps of the present invention will be described below in Examples 1, 2, and 3. Figures 11-1 to 11-4 show four examples of processing steps of Examples 1, 2, and 3 of the method for forming a pattern on a thin film by etching of the present invention. Figure 11-5 shows an example of a processing step in which a redevelopment process and an additional etching process are added to Figure 11-1 or Figure 11-2 as an additional process only when necessary as an example of the first processing step of Example 4. Figure 11-6 shows a schematic example of a processing step in which a redevelopment process and an additional etching process are added to Figure 11-3 or Figure 11-4 as an additional process only when necessary as an example of the second processing step of Example 4.
[0113] In all of the embodiments, the processes in common are resist (film) coating process S1, heating (pre)bake process S2, temperature adjustment (cooling) process S3, resist exposure process S4, resist development process S5, heating (post)bake process S6, and temperature adjustment (cooling) process S7.
[0114] In the process steps of Examples 1, 2, and 3 in FIG. 11-1, after the common process, resist characteristic changing process RH1, resist stabilization process RH2, and etching process S12 are performed in that order, and the processes RH1, RH2, and S12 are repeated a divided number of times for etching, and then a resist stripping process S13 is performed.
[0115] In the process steps of Examples 1, 2, and 3 in FIG. 11-2, after the common process, an etching process S12, a resist characteristic changing process RH1, and a resist stabilization process RH2 are performed in that order, and the processes of S12, RH1, and RH2 are repeated a divided number of times for etching, and then a resist stripping process S13 is performed.
[0116] In the process steps of Examples 1, 2, and 3 in FIG. 11-3, after the common process, resist characteristic changing process RH1, resist stabilization process RH2, and etching process S12 are performed in that order, and the processes of RH1, RH2, and S12, including the common processes S6 and S7, are repeated a divided number of times for etching, and then a resist stripping process S13 is performed.
[0117] In the process steps of Examples 1, 2, and 3 in FIG. 11-4, after the common process, an etching process S12, a resist characteristic changing process RH1, and a resist stabilization process RH2 are performed in that order, and the processes of S12, RH1, and RH2, including the common processes S6 and S7, are repeated a divided number of times for etching, and then a resist stripping process S13 is performed.
[0118] In the process steps of Example 4 in FIG. 11-5, after the above-mentioned common process, resist characteristic changing process RH1, resist stabilization RH2, and etching process S12 are performed in that order, and if necessary, a re-development process S14 and an additional etching process S15 are added. This shows an example in which the processes of RH1, RH2, and S12, and S14 and S15 are added if necessary, and etching is repeated a divided number of times, and then a resist stripping process S13 is performed.
[0119] In the process steps of Example 4 in FIG. 11-6, after the common processes, resist property changing process RH1, resist stabilization RH2, and etching process S12 are performed in that order, and if necessary, a re-development process S14 and an additional etching process S15 are added. This shows an example in which the processes of RH1, RH2, and S12, including the common processes S6 and S7, and S14 and S15 are added if necessary, and etching is repeated a divided number of times, and then a resist stripping process S13 is performed.
[0120] However, in the above-described embodiments, in the liquid etching process and the process using a liquid, a water washing process and a drying process are essential, and they are either included in the same process or omitted in the case of separate processes.
[0121] Further application examples of the present invention will be described below in Examples 1, 2, 3, and 4. In the above-mentioned Examples 1, 2, 3, and 4 and the processing steps, the etching process is described based on wet etching, but either wet etching or dry etching is acceptable. In particular, in the case of dry etching, isotropic etching is effective, and it is also effective in a chemical dry etching process in which only the radical gas portion is extracted from the so-called plasma state of the etching gas and processed separately. That is, in the processing of the above-mentioned Examples 1, 2, and 3, the case where the processing after the development processing of the resist film is replaced with processing in a vacuum is also included in the application range of the examples.
[0122] The processing methods and details of the above-mentioned Examples 1, 2, 3, and 4 will be explained in more detail below. The following cases where various processing conditions are different are also within the scope of the Examples 1, 2, 3, and 4. 1) A method of forming an organic film pattern (hereinafter, resist mask, resist pattern, and resist mask pattern are also included as examples) containing at least one type of organic substance on an underlying film to be etched, and then etching the underlying film to be etched at least three times, and optimally four times or more. In addition, a process for changing the characteristics and shape of the organic film pattern may be performed at least before each etching from the second onward. The process for changing the characteristics and shape may be a process for exposing the organic film pattern to an organic solvent to cause softening or reflow (fluidization). 2) A method for forming a thin film pattern, in which an underlying film to be etched is etched at least three times, and optimally four times or more, the total amount of etching of the underlying film to be etched each time, or the total of the product of the etching rate of each time and the processing time of each time (i.e., synonymous with the amount of etching of each time) is at least 100 to 200%, and optimally 110 to 150%, assuming that the value equal to the film thickness of the underlying film to be etched is 100%. 3) A method for forming a thin film pattern in which the underlying film to be etched is etched at least three times, and optimally four times or more, the amount of etching of the underlying film to be etched each time, or the product of the etching rate for each time and the processing time for each time (i.e., equivalent to the amount of etching for each time) is at least 100±50%, and optimally within the range of 100±20%, when the amount of etching is 100% when the entire underlying film to be etched is etched evenly by the number of etchings (i.e., the value obtained by dividing the total thickness of the underlying film by the number of etchings). 4) A method for forming a thin film pattern in which an underlying film to be etched is etched at least three times, and optimally four times or more, the amount of etching of the underlying film to be etched each time, or the product of the etching rate of each time and the processing time of each time (i.e., synonymous with the amount of etching each time), when the etching amount when the entire underlying film to be etched is etched evenly by the number of etchings (i.e., the value obtained by dividing the total thickness of the underlying film by the number of etchings) is taken as 100%, is at least 100±20%, optimally 100±10%, except for the final etching, and is at least 100+0 to 100%, optimally 100+0 to 50%. 5) A method of exposing an organic film pattern to an organic solvent to soften or reflow (fluidize) it is a method of forming a thin film pattern in which at least the surface area of the organic film pattern or the contact area with the underlying film is increased. 6) A method for forming a thin film pattern, characterized in that the method for exposing the organic film pattern to an organic solvent chemical is to expose it to vapor of the organic solvent chemical, to simultaneously spray the organic solvent chemical and an inert gas such as N2 or Ar, or to a gas in which an inert gas such as N2 or Ar is bubbled into the organic solvent chemical. Example 4
[0123] Example 4 of the present invention is an example in which redevelopment and additional etching are added to Examples 1, 2, and 3 as additional processes only when necessary. FIG. 12 shows the change in the cross section when this additional process step (redevelopment and additional etching) is performed. FIG. 12(a1) is the same as the state of FIG. 3(f) of Example 1. After this, as the redevelopment process of S14 in FIG. 11-5 and 6, the same chemical (or its diluted solution or other developer) as in the normal resist development process of S14 in FIG. 11-5 and 6 is used for an optimal processing time so that at least a part of the unexposed part of the resist part is removed. As a result, at least a part of the unexposed part of the resist pattern P3 in FIG. 12(b1) is selectively removed, and a new resist pattern SP3 as shown in FIG. 8(a2) remains. Next, the additional etching process of S15 in FIG. 11-5 and 6 is performed. This treatment is equivalent to the etching treatment S12 in Figures 11-5 and 11-6, or is performed for an optimal treatment time sufficient to remove unevenness on the side of the base film pattern T3 in Figure 12(c1) and at least a part of the surrounding residue (or a treatment with a dilute solution thereof or an etching solution of another composition with the same effect is also possible). As a result, a base film pattern such as base film pattern ST3, which is slightly narrower than base film pattern T3 but has smooth sides and no residue, is formed.
[0124] Fig. 12(a2) shows an example in which a resist pattern P3b and an undercoat film pattern T3b, which are expanded more than the resist pattern P3 in Fig. 12(a1), are formed by the resist characteristic change process (particularly including the resist deformation process 2) in Fig. 11-7 in the state of Fig. 3(f) in Example 1. In this case, by performing the process of removing at least a part of the unexposed part of the resist in the redevelopment process in S14 in Fig. 11-5 and 6 so that the resist part is removed more than in the case of Fig. 12(b1) or by performing the additional etching process in S15 more, the remaining resist pattern SP3b as in Fig. 12(b2) and the undercoat film pattern ST3b as in Fig. 12(c2) can be reduced more than the original P3b and T3b, which shows the effect of reducing the resist pattern and undercoat film pattern that expanded too much before the redevelopment process in S14 in Fig. 11-5 and 6.
[0125] Figure 12(a3) shows a larger expansion than Figure 12(a2). In this example, a resist pattern P3c and an undercoat film pattern T3c are formed. In this case, by performing the redevelopment process of S14 in Fig. 11-5 and 6 and the additional etching process of S15 more frequently, the remaining resist pattern SP3c as shown in Fig. 12(b3) and the undercoat film pattern ST3c as shown in Fig. 12(c3) can be further reduced from the original P3b and T3b. Therefore, the effect of controlling the dimensions by the two processes of expansion by the deformation process of the resist pattern and reduction by this redevelopment process is large, and the fact that the dimensions can be controlled by plus or minus (±) shows that more precise dimension control can be achieved.
[0126] In addition, although the above paragraphs 0123 to 0125 show the case where the process is performed at the end of the etching process, the present invention is not limited to this. The re-development process of S14 and the additional etching process of S15 can also be performed in the middle of the repetitive process as shown in Figures 11-5 and 11-6. By controlling the dimensions in the middle, it is possible to realize more accurate dimensions and to control in response to fluctuations in each process, which has the advantage of being very effective in controlling the final dimensions.
[0127] In addition, in the process steps of the above-mentioned embodiment, the etching process is described based on wet etching process, but either wet etching or dry etching can be used. In particular, in the case of dry etching, isotropic etching is effective, and it is also effective in a chemical dry etching process in which only radical gas part is extracted from the plasma state of the etching gas and processed separately. That is, in the processes of the above-mentioned embodiments 1, 2, 3, and 4, the cases where S5 to S9 after the development process of the resist film are replaced with processes in a vacuum are also included in the scope of application of the embodiments.
[0128] Here, the necessity and effectiveness of dividing the etching into three or more steps in the present invention will be described. This shows that dividing the etching into three or more steps, which is a feature of the present invention, is important, and that there is a significant difference compared to etching into two or less steps. However, as an example, these divided etchings are all in the case of equal divided time and divided etching amount, and although there are significant differences and advantages in other cases, all cases will be omitted.
[0129] FIG. 6 shows detailed dimensions of the underlayer T0 when etching is completed in only one step using a resist mask pattern P1 of the conventional example. (a) shows the resist mask pattern and underlayer before etching. (b) shows the state after etching, and assuming that etching (such as isotropic) proceeds from the end E1-1Point of the resist mask pattern P1, the dimensions of E1x1 as the side etching in the lateral direction (X direction) of the underlayer in the first etching, the etching amount (Y direction) and E1y1 are shown. (c) shows the pattern dimensions of the underlayer after resist peeling, and assuming that the total side etching amount is E1x and the total etching amount is E1y, E1x=E1x1 and E1y=E1y1 since the number of times is only one.
[0130] FIG. 7 shows a detailed view of dimensions when etching is completed by dividing the base film T0 by the resist mask pattern P1 of the conventional example into two parts. (a) shows the resist mask pattern and the base film before etching. (b) shows the state after the first etching process, and if it is assumed that etching (such as isotropic) proceeds from the end E2-1Point of the resist mask pattern P1, the dimensions of E2x1, the etching amount (Y direction), and E2y1 are shown as the side etching of the base film in the lateral direction (X direction) in the first etching. (c) shows the case where the resist mask pattern P2 is changed by heating (baking) processing at the curing temperature. (d) shows the state after the second etching process, and if it is assumed that etching (such as isotropic) proceeds from the end E2-2Point of the resist mask pattern P2, the dimensions of E2x2, the etching amount (Y direction), and E2y2 are shown as the side etching of the base film in the lateral direction (X direction) in the second etching. (e) shows the pattern dimensions of the undercoat film after resist stripping. If the total side etching amount is E2x and the total etching amount is E2y, then since the number of etchings is two, E2x=E2x1+E2x2 and E2y=E2y1+E2y2.
[0131] FIG. 8 shows a detailed view of dimensions when etching is completed by dividing the undercoat film T0 by the resist mask pattern P1 of Example 1 of the present invention into three times. (a) shows the resist mask pattern and the undercoat film before etching. (b) shows the state after the first etching process, and assuming that etching (such as isotropic) proceeds from the end E3-1Point of the resist mask pattern P1, the dimensions of E3x1 as the side etching of the undercoat film in the lateral (X direction) direction in the first etching, the etching amount (Y direction) and E3y1 are shown. (c) shows the case where the resist mask pattern P1 is changed to the resist mask pattern P2 by performing the resist deformation process 2 (e.g., organic solvent chemical solution dissolution reflow process) + resist adhesion strengthening process (e.g., 3-5 minutes heating process at 1120-130°C) as the resist adhesion strengthening process of the present invention, and then performing the substrate temperature adjustment process (e.g., placing on a plate at room temperature) + substrate drying process (e.g., dry air blow) as the substrate stabilization process. (d) shows the state after the second etching process, and assuming that etching (such as isotropic) starts from the end E3-2Point of the resist mask pattern P2, the dimensions of E3x2, the etching amount (Y direction), and E3y2 are shown as the side etching of the lateral (X direction) of the base film in the second etching. (e) shows the case where the resist mask pattern P2 has changed to the resist mask pattern P3 by the same process as (c). (f) shows the state after the third etching process, and assuming that etching (such as isotropic) starts from the end E3-3Point of the resist mask pattern P3, the dimensions of E3x3, the etching amount (Y direction), and E3y3 are shown as the side etching of the lateral (X direction) of the base film in the third etching. (g) shows the pattern dimensions of the undercoat film after resist removal, and assuming that the total side etching amount is E3x and the total etching amount is E3y, since the number of times is three, E3x=E3x1+E3x2(+E3x3) and E3y=E3y1+E3y2+E3y3. However, as can be seen from the figure, E3x3 is - (minus), which means that the third side etching hardly progresses (in fact, it becomes less), and does not affect the total side etching amount.
[0132] 9-1 and 9-2 show detailed dimensional diagrams of the resist mask pattern P1 of Example 1 of the present invention when etching is completed by dividing the undercoat film T0 into four parts. (a) shows the resist mask pattern and undercoat film before etching. (b) shows the state after the first etching process, and assuming that etching (such as isotropic) proceeds from the end E4-1Point of the resist mask pattern P1, the dimensions of E4x1 as the side etching (X direction) of the undercoat film in the first etching, the etching amount (Y direction) and E4y1 are shown. (c) shows the case where the resist mask pattern P1 is changed to the resist mask pattern P2 by performing the resist deformation process 2 (e.g., organic solvent chemical solution dissolution reflow process) + resist adhesion strengthening process (e.g., 3-5 minutes heating process at 1120-130°C) as the resist adhesion strengthening process of the present invention, and then performing the substrate temperature control process (e.g., placing on a plate at room temperature) + substrate drying process (e.g., dry air blow) as the substrate stabilization process. (d) shows the state after the second etching process, and assuming that etching (such as isotropic) proceeds from the end E4-2Point of the resist mask pattern P2, the dimensions of E4x2, the etching amount (Y direction), and E4y2 are shown as the side etching of the lateral (X direction) of the base film in the second etching. (e) shows the case where the resist mask pattern P2 is changed to the resist mask pattern P3 by the same process as (c). (f) shows the state after the third etching process, and assuming that etching (such as isotropic) proceeds from the end E4-3Point of the resist mask pattern P3, the dimensions of E4x3, the etching amount (Y direction), and E4y3 are shown as the side etching of the lateral (X direction) of the base film in the third etching. (g) shows the case where the resist mask pattern P3 is changed to the resist mask pattern P4 by the same process as (e). (h) shows the state after the fourth etching process. Assuming that (isotropic, etc.) etching proceeds from the end E4-4Point of the resist mask pattern P4, the fourth etching shows E4x4 as the side etching of the base film in the lateral direction (X direction), and the etching amount (Y direction) and E4y4 dimensions.(i) shows the pattern dimensions of the undercoat film after resist peeling, and assuming that the total side etching amount is E4x and the total etching amount is E4y, since the number of times is four, E4x=E4x1+E4x2(+E4x3)(+E4x4), E4y=E4y1+E4y2+E4y3+E4y4. However, as can be seen from the figure, E4x3 and E4x4 are - (minus), which means that the third and fourth side etchings hardly progress (in fact, they become less), and do not affect the total side etching amount.
[0133] From the above description of the dimensions in Figures 6, 7, 8, 9-1 and 9-2, when the etching is divided into three or more steps (however, the divided time and divided etching amount are equal), the third or more side etching amount does not affect the whole, so in the divided etching of the present invention, if the side etching amount in the case of the division number (n) is Enx, and the first and second side etching amounts in that case are Enx1 and Enx2, then Enx = Enx1 + Enx2 only, and if n is at least three or more, Enx becomes smaller than the total side etching amount E1x or E2x in the case where all etching is completed in only one or two divisions in the past (i.e., n ≥ 3, Enx ≤ E1x, E2x). Therefore, it is important and effective to etch by dividing into three or more steps.
[0134] In the above paragraphs 0128 to 0133, the etching is divided into equal times and amounts. However, FIGS. 10-1, 10-2, and 10-3 explain the case where the division of each etching is not equal in time and amount when completing two separate etchings of the base film T0 using the resist mask pattern P1.
[0135] Figure 10-1 shows detailed dimensions when the first etching division time and amount are small and the second etching division time and amount are large. (a) shows the resist mask pattern and the underlayer before etching. (b) shows the state after the first etching process. Assuming that etching (isotropic, etc.) proceeds from the end E2a-1Point of the resist mask pattern P1, the dimensions of E2ax1, etching amount (Y direction), and E2ay1 are shown as the side etching of the underlayer in the lateral direction (X direction) in the first etching. (c) shows the case where the resist mask pattern is changed to P2 by heating (baking) at the curing temperature. (d) shows the state after the second etching process. Assuming that etching (isotropic, etc.) proceeds from the end E2a-2Point of the resist mask pattern P2, the dimensions of E2ax2, etching amount (Y direction), and E2ay2 are shown as the side etching of the underlayer in the lateral direction (X direction) in the second etching. (e) shows the pattern dimensions of the base film after resist stripping. If the total side etching amount is E2ax and the total etching amount is E2ay, then since the number of etchings is two, E2ax=E2ax1+E2ax2 and E2ay=E2ay1+E2ay2.
[0136] Figure 10-2 shows detailed dimensions when the first etching division time and amount are the same as the second etching division time and amount. (a) shows the resist mask pattern and the underlayer before etching. (b) shows the state after the first etching process, and if it is assumed that etching (isotropic, etc.) proceeds from the end E2b-1Point of the resist mask pattern P1, the dimensions of E2bx1, etching amount (Y direction), and E2by1 are shown as the side etching of the underlayer in the lateral direction (X direction) in the first etching. (c) shows the case where the resist mask pattern is changed to P2 by heating (baking) processing at the curing temperature. (d) shows the state after the second etching process, and if it is assumed that etching (isotropic, etc.) proceeds from the end E2b-2Point of the resist mask pattern P2, the dimensions of E2bx2, etching amount (Y direction), and E2by2 are shown as the side etching of the underlayer in the lateral direction (X direction) in the second etching. (e) shows the pattern dimensions of the undercoat film after resist stripping. If the total side etching amount is E2bx and the total etching amount is E2by, then since the number of times is two, E2bx=E2bx1+E2bx2 and E2by=E2by1+E2by2.
[0137] Figure 10-3 shows detailed dimensions when the first etching division time and amount are large and the second etching division time and amount are small. (a) shows the resist mask pattern and the underlayer before etching. (b) shows the state after the first etching process. If it is assumed that etching (isotropic, etc.) proceeds from the end E2c-1Point of the resist mask pattern P1, the dimensions of E2cx1, etching amount (Y direction), and E2cy1 are shown as the side etching of the underlayer in the lateral direction (X direction) in the first etching. (c) shows the case where the resist mask pattern is changed to P2 by heating (baking) at the curing temperature. (d) shows the state after the second etching process. If it is assumed that etching (isotropic, etc.) proceeds from the end E2c-2Point of the resist mask pattern P2, the dimensions of E2cx2, etching amount (Y direction), and E2cy2 are shown as the side etching of the underlayer in the lateral direction (X direction) in the second etching. (e) shows the pattern dimensions of the undercoat film after resist stripping. If the total side etching amount is E2cx and the total etching amount is E2cy, then since the number of etchings is two, E2cx=E2cx1+E2cx2 and E2cy=E2cy1+E2cy2.
[0138] Comparing the states of FIG. 10-1, FIG. 10-2, and FIG. 10-3, as can be seen from the figures, if the etching amount of each time is larger than the others, as in FIG. 10-1, the effect of the side etching amount is large, and if etching is performed uniformly, the total side etching amount is smaller. That is, if the total side etching amount is E2ax in the case of FIG. 10-1, the total side etching amount is E2bx in the case of FIG. 10-2, and the total side etching amount is E2cx in the case of FIG. 10-3, then E2ax≧E2bx≦E2cx. From this, the total side etching amount can be minimized by making the etching time and amount of each etching in the divided etching equal. Therefore, it is complemented that the division into three or more times for the equal divided etching time and amount described in the above paragraphs 0127 to 0132 is important and effective in suppressing the side etching amount, and further indicates that it is a necessary important element. This indicates that it is important to divide the etching into three or more times, which is a feature of the present invention, and that there is a large significant difference from etching two or less times. Example 5
[0139] Next, a processing apparatus for forming a pattern on a thin film by etching according to the present invention for achieving the method for forming a pattern on a thin film by etching according to the present invention will be described as Example 5. As an example of each processing unit used in the processing apparatus for forming a pattern on a thin film by etching according to the present invention and its processing order, a resist (film) coating processing unit Y1, a heating and baking processing unit Y2, a temperature adjustment (cooling) processing unit Y3, a resist exposure processing unit Y4, a resist development processing unit Y5, a heating and baking processing unit Y6, and a temperature adjustment (cooling) processing unit Y7 are units that perform processing in a common order.
[0140] FIG. 13-1 shows an example 1 of Example 5 (Example 5-1), in which after the common processing units Y1 to Y7, processing is carried out in the order of a resist characteristic changing processing unit YRH1, a resist stabilization unit YRH2, and an etching processing unit Y12, and after the processing in the processing units YRH1, YRH2, and Y12 is repeated the number of times for etching, processing is carried out in a resist stripping processing unit Y13.
[0141] In Example 2 (Example 5-2) of Example 5 in Figure 13-2, after the common processing units Y1 to Y7, processing is performed in the order of an etching unit Y12, a resist characteristic changing processing unit YRH1, and a resist stabilization unit YRH2, and after the processing in the processing units Y12, YRH1, and YRH2 is repeated the number of times for etching, processing is performed in a resist stripping processing unit Y13.
[0142] In Example 3 (Example 5-3) of Example 5 in Figure 13-3, after the common processing units Y1 to Y5, a heating bake processing unit Y6, a temperature adjustment (cooling) processing unit Y7, a resist characteristic changing processing unit YRH1, a resist stabilization processing unit YRH2, and an etching processing unit Y12 are performed in that order, and after the processes of YRH1, YRH2, and Y12, including the common processes Y6 and Y7, are repeated the number of etching divisions, a resist stripping process Y13 is performed.
[0143] In Example 4 (Example 5-4) of Example 5 in Figure 13-4, after the common processing units Y1 to Y5, a heating bake processing unit Y6, a temperature adjustment (cooling) processing unit Y7, an etching processing unit Y12, a resist characteristic changing processing unit YRH1, and a resist stabilization processing unit YRH2 are performed in that order, and after the processes of Y12, YRH1, and YRH2, including the common processes Y6 and Y7, are repeated the number of times for etching, a resist stripping process Y13 is performed.
[0144] In Example 5 (Example 5-5) of Figure 13-5, after the common processing units Y1 to Y5, processing is performed in the order of the resist characteristic changing processing unit YRH1, the resist stabilization processing unit YRH2, and the etching processing unit Y12, and if necessary, processing is added in the order of the re-development processing unit Y14 and the additional etching processing unit Y15.This shows an example in which processing in the YRH1, YRH2, and Y12 units, and if necessary, processing in the re-development processing unit Y14 and the additional etching processing unit Y15 are added, and etching is repeated a divided number of times, and then processing is performed in the resist stripping processing unit Y13.
[0145] In Example 6 (Example 5-6) of Example 5 in Figure 13-6, after the common processing units Y1 to Y5, a heating bake processing unit Y6, a temperature adjustment (cooling) processing unit Y7, an etching processing unit Y12, a resist characteristic changing processing unit YRH1, and a resist stabilization processing unit YRH2 are performed in that order, and if necessary, a re-development processing unit Y14 and an additional etching processing unit Y15 are added, and after repeating the etching divided number of times, processing is performed in the resist stripping processing unit Y13.
[0146] However, in the above-described embodiment 5, in the liquid etching processing unit and the processing unit using a liquid, the water washing processing and drying processing are essential, and they are either included in the same processing unit or omitted in the case of a separate processing unit.
[0147] The resist characteristic change processing unit is, as shown in FIG. 13-7, (a) Resist adhesion strengthening processing unit: A processing unit that has the effect of recovering even a little the adhesion between the resist mask and the base film that has deteriorated after etching, i.e., recovering or increasing the adhesion area between the base film and the resist film. (b) Resist deformation processing unit 1: A processing unit having an effect of restoring or increasing the contact area between the base film and the resist film by softening, bending, curving, or the like, at least a part of the resist mask pattern without being liquefied or remaining solid. (c) Resist transformation processing unit 2: A processing unit having the effect of liquefying, dissolving, reflowing, fluidizing, or the like at least a part of the resist mask pattern, thereby recovering or increasing the contact area between the base film and the resist film. (d) is a processing unit that combines (a), (b), and (c). It can be one of the following.
[0148] After that, the resist mask pattern is further processed in a substrate stabilization processing unit. As shown in FIG. 13-8, the substrate stabilization processing unit is (a) Substrate temperature control processing unit: A processing unit that controls the temperature of the resist mask to room temperature or to an optimal temperature before etching. (b) Substrate drying processing unit: A processing unit that has the effect of removing liquid adhering to the resist mask and drying it. (c) Substrate vacuum drying processing unit: A processing unit that performs vacuum drying to remove liquid adhering to the resist mask and to dry it. (d) A processing unit combining (a), (b), and (c). However, although the resist property change processing unit and the substrate state stabilization processing unit are exemplified by the examples in paragraphs 0147 to 0148 in this embodiment 5, they are not limited thereto.
[0149] 14 shows examples of each processing unit, a transport system robot, and a processing substrate cassette as a multi-processing unit device as an example A of a device realizing the embodiment 5 of the processing device for forming a pattern on a thin film by etching according to the present invention. That is, it is composed of a heating bake processing unit Y6, a temperature adjustment (cooling) processing unit Y7, a resist property changing processing unit YRH1, a substrate stabilization processing unit YRH2, an etching processing unit Y12 (Y15) (or an additional etching processing unit, which may also be used for both), a redevelopment processing unit Y14, substrate cassettes C1 to C4 that store substrates, a transport robot R1 that takes substrates in and out of the substrate cassettes C1 to C4, and a transport robot R2 that receives substrates from the transport robot R1 and transports them to each unit.
[0150] However, the multi-unit apparatus, which is a processing apparatus for forming a thin film pattern by etching according to the present invention, is not limited to the apparatus example A for realizing the above-mentioned embodiment 5, but may be provided with three minimum processing units: a resist property change processing unit YRH1, a substrate stabilization processing unit YRH2, and an etching processing unit Y12 (Y15) (or an additional etching processing unit, or both). Furthermore, depending on the need for improved processing capacity and additional processing (for example, a resist property change processing unit YRH1), it is possible to add the processing units Y1 to Y5 and Y13, and this is also included in the apparatus example A for realizing the embodiment 5 of the present invention.
[0151] FIG. 15 shows examples of each processing unit, a transport robot, and a processing substrate cassette as a multi-processing unit apparatus as an example B of an apparatus for realizing the fifth embodiment of the processing apparatus for forming a thin film pattern by etching according to the present invention. However, Example B in this case differs from Example A in that all units are dry units, that is, processing units in a vacuum. That is, the heating and baking processing unit Y6, the temperature adjustment (cooling) processing unit Y7, the resist property changing processing unit YRH1, the substrate stabilization processing unit YRH2, the etching processing unit Y12 (Y15) (or additional etching processing unit, also used for both), the redevelopment processing unit Y14, the substrate cassettes C1 to C4 storing substrates, the transport robot R1 which takes substrates in and out of the substrate cassettes C1 to C4, and the transport robot R2 which receives substrates from the transport robot R1 and transports them to each unit are all processes performed in a vacuum and are composed of vacuum units. For example, the etching process is a so-called dry etching process. Redevelopment is also performed by dry development processing or ashing processing (mainly processing in a plasma atmosphere of O2 gas).
[0152] FIG. 16 shows an example of an apparatus C for implementing embodiment 5 of the thin film pattern formation processing apparatus by etching of the present invention, in which substrates are transported by a conveyor system (continuous, intermittent or discontinuous tact feed), and in the etching processing unit, the application of processing liquid is performed by a shower system, and examples of each processing unit, a transport system robot and a processed substrate cassette are shown.
[0153] In this case, in the Y12 conveyor-type etching processing unit, in which the substrate is transported by a conveyor system (continuous, intermittent, or discontinuous) and the processing liquid is applied by a shower system, since this is a liquid etching process, a water washing process and a drying process for removing the etching liquid are essential, and they will be included in the same process, or will be omitted if they are separate processes.
[0154] Also, this is an apparatus capable of processing the conveyor-type etching processing unit Y12, the resist property change processing unit YRH1, and the substrate stabilization processing unit YRH2 in succession, and an example of installation in this case is to install the conveyor-type etching processing unit Y12 on the lower level (or left line), and install the resist property change processing unit YRH1 and the substrate stabilization processing unit YRH2 on the upper level (or right line), with the transfer robots R1 and R2 transferring substrates between the upper and lower levels, and the transfer between the resist property change processing unit YRH1 and the substrate stabilization processing unit YRH2 being performed by a conveyor or a transfer robot similar to R1 and R2. However, this is not limited to this installation example, and as long as the processing order is the same, it also includes cases where the upper and lower levels, left and right lines, and transfer robots and conveyors along the way are different.
[0155] FIG. 17 shows an example of an apparatus D for implementing embodiment 5 of the thin film pattern formation processing apparatus by etching of the present invention, in which substrates are transported by a conveyor system (continuous, intermittent or discontinuous tact feed), and in the etching processing unit, the application of processing liquid is performed by a shower system, and examples of each processing unit, a transport system robot and a processed substrate cassette are shown as an example of an apparatus in which processing units are connected.
[0156] In this case, in the Y12 conveyor-type etching processing unit, in which the substrate is transported by a conveyor system (continuous, intermittent, or discontinuous) and the processing liquid is applied by a shower system, since this is a liquid etching process, a water washing process and a drying process for removing the etching liquid are essential, and they will be included in the same process, or will be omitted if they are separate processes.
[0157] In addition, this is an apparatus capable of processing the conveyor-type etching processing unit Y12, the resist property change processing unit YRH1, the substrate stabilization processing unit YRH2, and the redevelopment processing unit Y14 in succession, and an example of the installation in this case is to install the conveyor-type etching processing unit Y12 in the lower tier (or left line), and the resist property change processing unit YRH1, the substrate stabilization processing unit YRH2, and the redevelopment processing unit Y14 in the upper tier (or right line), and the substrates are moved between the upper and lower tiers by the transport robots R1 and R2, and transport is performed between the resist property change processing unit YRH1, the substrate stabilization processing unit YRH2, and the redevelopment processing unit Y14 by a conveyor or a transport robot similar to R1 and R2. However, this is not limited to this installation example, and as long as the processing order is the same, it also includes cases where the upper tier, lower tier, left and right lines, and the transport robots and conveyors along the way are different.
[0158] FIG. 18 shows an example of an apparatus E for implementing embodiment 5 of the thin film pattern formation processing apparatus by etching of the present invention, in which substrates are transported by a conveyor system (continuous, intermittent or discontinuous tact feed), and in the etching processing unit, the application of processing liquid is performed by a shower system, and examples of each processing unit, a transport system robot and a processed substrate cassette are shown as an example of an apparatus connected to the processing unit.
[0159] In this case, in the Y12 conveyor-type etching processing unit, in which the substrate is transported by a conveyor system (continuous, intermittent, or discontinuous) and the processing liquid is applied by a shower system, since this is a liquid etching process, a water washing process and a drying process for removing the etching liquid are essential, and they will be included in the same process, or will be omitted if they are separate processes.
[0160] This is also an apparatus capable of successively processing the conveyor-type etching processing unit Y12, the heating bake processing unit Y7, the temperature adjustment (cooling) processing unit Y8, the resist property change processing unit YRH1, and the substrate stabilization processing unit YRH2.As an example of an installation in this case, the conveyor-type etching processing unit Y12 is installed on the lower tier (or left line), and the heating bake processing unit Y7, the temperature adjustment (cooling) processing unit Y8, the resist property change processing unit YRH1, and the substrate stabilization processing unit YRH2 are installed on the upper tier (or right line), and substrates are moved between the upper and lower tiers by the transport robots R1 and R2, and transport is performed between the heating bake processing unit Y7, the temperature adjustment (cooling) processing unit Y8, the resist property change processing unit YRH1, and the substrate stabilization processing unit YRH2 by a conveyor or a transport robot similar to R1 and R2. However, this is not limited to this installation example, and includes cases where the processing order is the same, such as upper and lower levels, left and right lines, and different transport robots and conveyors along the way.
[0161] FIG. 19 shows an example of an apparatus F for implementing embodiment 5 of the thin film pattern formation processing apparatus by etching of the present invention, in which substrates are transported by a conveyor system (continuous, intermittent or discontinuous tact feed), and in the etching processing unit, the application of processing liquid is performed by a shower system, and examples of each processing unit, a transport system robot and a processed substrate cassette are shown as an example of an apparatus in which processing units are connected.
[0162] In this case, in the Y12 conveyor-type etching processing unit, in which the substrate is transported by a conveyor system (continuous, intermittent, or discontinuous) and the processing liquid is applied by a shower system, since this is a liquid etching process, a water washing process and a drying process for removing the etching liquid are essential, and they will be included in the same process, or will be omitted if they are separate processes.
[0163] This is also an apparatus capable of continuously processing the conveyor-type etching processing unit Y12, the heating bake processing unit Y7, the temperature adjustment (cooling) processing unit Y8, the resist property modification processing unit YRH1, the substrate stabilization processing unit YRH2, and the re-development processing unit Y14.As an example of an installation in this case, the conveyor-type etching processing unit Y12 is installed on the lower tier (or left line), and the heating bake processing unit Y7, the temperature adjustment (cooling) processing unit Y8, the resist property modification processing unit YRH1, the substrate stabilization processing unit YRH2, and the re-development processing unit Y14 are installed on the upper tier (or right line), and substrates are moved between the upper and lower tiers by the transport robots R1 and R2, and transport is performed between the heating bake processing unit Y7, the temperature adjustment (cooling) processing unit Y8, the resist property modification processing unit YRH1, the substrate stabilization processing unit YRH2, and the re-development processing unit Y14 by a conveyor or a transport robot similar to R1 and R2. However, this is not limited to this installation example, and includes cases where the processing order is the same, such as upper and lower levels, left and right lines, and different transport robots and conveyors along the way.
[0164] However, the apparatus for implementing the fifth embodiment of the etching processing apparatus for a thin film according to the present invention is not limited to the apparatus examples A, B, C, D, E, and F, but may include three minimum processing units, namely, an etching processing unit Y12, a resist property changing processing unit YRH1, and a substrate stabilization processing unit YRH2. Furthermore, depending on the need for improved processing capacity and additional processing, it is possible to add the processing units Y6 to Y9, or to configure the apparatus to include two or more of the same processing units, and these are also included in the apparatus examples for implementing the fifth embodiment of the etching processing apparatus for a thin film according to the present invention.
[0165] Example of processing using the resist characteristic change processing unit shown in Figure 13-7 The resist mask is a processing unit corresponding to the resist characteristic modification processing of Fig. 11-7 shown in paragraph number 0104. For example, in (a) resist adhesion strengthening processing unit, a heating process is performed at a temperature equal to or lower than the curing temperature (e.g., 100 to 130°C), in (b) resist deformation processing 1 unit, a special heating process temperature, time, and atmosphere process is performed at a temperature equal to or lower than the curing temperature (e.g., 100 to 130°C) in order to soften, bend, and curve the resist mask while keeping it solid or without liquefying it, and in (c) resist deformation processing 2 unit, a chemical solution dissolution reflow (or chemical solution gas exposure) process is performed by exposing the resist mask to the vapor of an organic solvent chemical solution as a process for liquefying, dissolving, reflowing, and fluidizing it.
[0166] The unit for performing the chemical dissolution reflow (or chemical gas exposure) process may be any process unit that performs a process for softening, dissolving and flowing an organic film pattern, such as exposing the pattern to vapor of a chemical containing at least an organic solvent, simultaneously spraying the pattern with an inert gas (N2, Ar gas, etc.), or exposing the pattern to gas in which an inert gas (N2, Ar gas, etc.) is bubbled through a chemical containing an organic solvent, as described in the first to fifth embodiments.
[0167] The other processing units in Fig. 13-7 are also units corresponding to the processing in Fig. 11-7, and the processing unit in Fig. 13-8 is also a unit corresponding to the processing in Fig. 11-8.
[0168] In addition, the processing conditions other than the heat treatment include, for example, in the case of wet etching, (1) the composition of the etching solution, (2) the temperature of the etching solution, (3) the spraying conditions of the etching solution (in the case of the shower method: the shower pressure, the shower oscillation operation, etc.), (4) the etching processing time, (5) the water rinsing processing method, (6) the water rinsing processing time, and (7) the drying method (temperature, time), and in the case of isotropic dry etching, so-called chemical dry etching, the processing conditions include, for example, (1) the processing pressure (degree of vacuum), (2) the discharge power, (3) the type and gas flow rate of the processing gas, (4) the processing time, and (5) the temperature of the processing substrate (temperature of the substrate stage).
[0169] The treatment temperature range for resist adhesion strengthening treatment (FIG. 11-7(a)), which is a heat treatment for adjusting the adhesion of the resist, and other heat baking treatments are not particularly limited, but may be, for example, a temperature range of about 80° C. to 150° C., which is a temperature range in which the resist pattern does not cure, and is optimally performed in a range of about 90° C. to 120° C. In the chemical solution reflow (or chemical gas exposure) treatment, treatment is basically performed at room temperature of 25° C., but it also includes treatment at temperatures higher than room temperature, such as 25 to 40° C., as well as temperatures of about room temperature or below room temperature, which can be selected depending on the treatment speed and characteristics.
[0170] Here, as an additional explanation, Examples 1, 2, 3, and 4 of the present invention The following describes in detail an example of resist deformation process 1 (FIG. 11-7(b)), which is a resist characteristic changing process, in which the resist remains solid or is softened without being liquefied and is bent or curved.
[0171] As a specific processing example, the case of Example 1 of the present invention in FIG. 3 is shown in paragraph number 0049 above. As the resist property changing process used here, an example of a case where resist deformation process 1 is selected: a process in which the shape of the resist mask hardly expands and at least a part of it remains solid, or the resist mask is softened without liquefying and is bent, curved, etc. is shown in FIG. 20.
[0172] The difference between resist deformation process 2 in Fig. 11-7(c) and resist deformation process 1 in Fig. 11-7(b) is that in resist deformation process 2, at least a part of the resist mask pattern is liquefied and dissolved, or reflows, becomes fluid, etc., whereas in resist deformation process 1, at least a part of the material remains solid, or does not liquefy but softens and becomes bent or curved, etc. Furthermore, in terms of dimensions, in resist deformation process 2, there may be a large change in any of the dimensions of length, width, or thickness after deformation, whereas in resist deformation process 1, there is also a characteristic that the total dimensions of length, width, and thickness do not change significantly even after deformation.
[0173] However, while FIG. 20 is an additional explanation of Example 1, it is not limited to this, and is a specific example that can be applied to any case where the resist characteristic change process in Examples 1, 2, 3, and 4 is performed as the resist deformation process 1, 2, or a combination thereof.
[0174] Here, a resist pattern P1 and an undercoat film T0 formed by normal coating, exposure, and development are shown. Starting from the innermost part where side etching occurs along with the etching of the undercoat film, the resist mask pattern bends or curves, and adheres to fill the gaps of the side etching. As the undercoat film changes from T0 to T1, T1 to T2, and T2 to T3 due to three etchings, the resist mask pattern changes from P1 to P2, P2 to P3, and P3 to P4.
[0175] In this example, in the case of each etching of the base film, the resist pattern is heated to a temperature equal to or lower than the cure temperature of the resist pattern (e.g., 100 to 130°C) so that at least a portion of the resist mask pattern remains solid or softens without liquefying, and is bent or curved starting from the deepest part of the gap between each resist mask pattern and the base film, thereby deforming so as to fill the gap, or to deform so as to cover at least a portion, or optimally, all, of the part of the base film where side etching has occurred, and in each resist mask pattern P2, P3, P4, the gap part or the part corresponding to the part where side etching has occurred in the base film becomes an interface M1, M2, M3 where the adhesion between the base film T1, T2, T3 and the resist pattern is strengthened, and the adhesion is restored to at least a strength equal to or greater than the adhesion between the base film T0 and the resist pattern P1 before the side etching.
[0176] FIG. 20(a) shows a state in which a resist pattern P1 is formed on the undercoat film T0 of FIG. 3(a) of the first embodiment.
[0177] Fig. 20 is similar to the state of Fig. 3 of Example 1, but the difference is that in the resist property changing process performed after etching, resist deformation process 2 of Fig. 11-7 is performed in Fig. 3 of Example 1, whereas resist deformation process 1 of Fig. 11-7(b) is performed in Fig. 20. In this case, as described in paragraphs 0170-173, in resist deformation process 1, the shape of the resist mask hardly expands and at least a part of it remains solid, or it does not liquefy but softens, and is bent or curved. That is, in Figure 20(b) and its enlarged view, the first etching of the base film T0 creates a gap due to side etching between the resist mask pattern P1 and the etched base film T1, resulting in a eaves-shaped resist mask pattern P1. However, by heating the resist pattern to a temperature below its cure temperature (e.g., 100 to 130°C), the resist mask pattern P1 is bent or curved starting from the innermost part where the side etching has occurred, and the resist mask pattern adheres to fill the gap due to the side etching, forming an M1 interface with strengthened adhesion, and the resist mask pattern P2 is adhered to the base film T1.
[0178] In Figure 20(c) and its enlarged view, a gap due to side etching is created between the resist mask pattern P2 and the etched base film T2 due to the second etching of the base film T1, and the resist mask pattern P2 has become shaped like a canopy. However, by heating the resist pattern to a temperature below the cure temperature (e.g., 100 to 130°C), the resist mask pattern P2 is bent or curved starting from the innermost part where the side etching has occurred, and the resist mask pattern adheres to fill the gap due to the side etching, forming an M2 interface with strengthened adhesion, and the resist mask pattern P3 is adhered to the base film T2.
[0179] In Figure 20(d) and its enlarged view, the third etching of the base film T2 creates gaps due to side etching between the resist mask pattern P3 and the etched base film T3, resulting in a eaves-shaped resist mask pattern P3. However, by heating the resist pattern to a temperature below its cure temperature (e.g., 100 to 130°C), the resist mask pattern P3 is bent or curved starting from the innermost part where the side etching has occurred, and the resist mask pattern adheres to fill the gaps caused by the side etching, forming an M3 interface with strengthened adhesion, and the resist mask pattern P4 is adhered to the base film T3.
[0180] As a more detailed processing method of the resist deformation process 1, 1) The resist mask is formed thin (e.g., 1 / 2 or less, optimally 1 / 4 or less, or 0.5µm or less, optimally 0.25µm or less) so that it remains solid under its own weight or deforms by bending, curving, etc. without liquefying, and furthermore, a heating (baking) treatment is performed below the curing temperature (e.g., 100 to 130°C) to assist the deformation and to recover and strengthen the adhesion. 2) Even if the resist pattern is not formed thin as in 1), a material that is easily deformed under its own weight as a characteristic of the resist material itself, or a material that remains solid or deforms by bending, curving, etc. without liquefying when heated (baked) below the curing temperature (e.g., 100 to 130°C), and furthermore, a resist material that softens and deforms by bending, curving, etc. repeatedly even when treated at the same temperature is selected. 3) Even if the resist pattern is not formed thin as in 1), the resist material itself has a property that, even when various resist property changing processes are repeated many times, the mask material has a property that can restore or at least increase the adhesion with the underlayer each time, and can repeatedly undergo deformations such as softening, bending, curving, liquid flowing, reflowing, and deformations that cover at least a part of the part of the underlayer where side etching has occurred, optimally all of it (this is called self-aligned deformation to the underlayer). However, this self-aligned deformation and improvement in adhesion may be realized by performing a single resist property changing process, but two separate resist property changing processes may also be performed, and are performed using a resist material having such properties. This can be realized by adopting a method such as the above. The resist pattern in this case is the same for the organic film pattern and resist mask.
[0181] In the case of resist deformation process 1 as a resist characteristic change process (Figure 11-7 (b)), the resist remains solid or is not liquefied, so compared to resist deformation process 2 (Figure 11-7 (c)), which causes the resist pattern to expand and deform due to dissolution, reflow, fluidization, etc. due to liquefaction of the resist pattern, there is the disadvantage that the etching dimensions will be larger, and there is the advantage that there is no need to control the expansion, making it easier to control the dimensions and simplifying the process.
[0182] An example of the resist modification process 1 as the resist characteristic change process shown in paragraphs 0170 to 0181 above is applicable not only to the case of the embodiment 1 in FIG. 3 but also to the embodiments 2, 3, 4, and 5 above.
[0183] Furthermore, in the above-mentioned Examples 1, 2, 3, 4, and 5, the number of divided etching steps is 3 to 7, but the embodiments of the present invention are not limited to this, and cases in which the number of divided etching steps is greater than this are also included in the application examples.
[0184] As an example of the etching used in all the embodiments of the present invention, as an example of the wet etching, when the base film is a copper (Cu) film, the etching solution is adjusted to a composition that provides the required etching rate, for example, a ferric chloride solution, a cupric chloride solution, an alkaline ammonia (alkaline ammonia) solution, a sulfuric acid hydrogen peroxide (sulfuric acid + hydrogen peroxide) solution, etc. As another example of wet etching, when the base film is a metal, semiconductor, or insulating film, an etching solution for the metal film is used in the case of a metal film, an NaOH-based, KOH-based, or alkaline-based etching solution is used in the case of a semiconductor film (Si, etc.), and an HF-based (BHF, etc.) solution is used in the case of an insulating film, with the composition adjusted to provide the required etching rate.
[0185] In the case of dry etching, for metal films such as Al (aluminum), Al alloys, Cr (chromium), In, and ITO, mainly Cl-based gases, BCl, HCl, etc. are used. For semiconductor films (Si, Ga, etc.) and insulating films (SiO2, Si3N4, etc.), PFC-based gases (CxFy such as CF4: x, y are arbitrary) gases, HFC-based gases (CxHyFz such as CHF3: x, y, z are arbitrary) gases, CFC-based gases (CxClyFz such as CCl2F2: x, y, z are arbitrary) gases, inorganic gases, etc. are used. It uses halogen gas (SF6, NF3, SiF4, HF, Cl2, BCl3, Br, HBr, HI, IBr, etc.) alone or in combination with gases such as H2, O2, N2, Ar, O3, NH3, H2O, CH4 (CxHv: x and y are optional) and controls the flow rate according to the required etching rate and uniformity, creating a plasma state, and uses the ions and radicals to perform dry etching while controlling the impact energy and chemical reaction with potential difference power and pressure. It is particularly effective in the case of isotropic dry etching, and is used effectively in chemical dry etching processes in which only the radical gas portion is extracted from the plasma state of the etching gas and processed separately. [Industrial Applicability]
[0186] The present invention can be applied to anything related to a method for forming a pattern on a thin film, a wet etching method, an anisotropic dry etching method, an isotropic dry etching method, and a chemical dry etching method using the processing apparatus, and the processing apparatus, and is not limited in its applicability. The present invention has been described in relation to several preferred embodiments and examples, but it is understood that these embodiments and examples are merely for illustrative purposes and are not meant to be limiting. After reading this specification, it will be apparent to those skilled in the art that numerous modifications and substitutions using equivalent elements and techniques are readily possible, and such modifications and substitutions are within the true scope and spirit of the appended claims. [Brief description of the drawings]
[0187] [Figure 1] FIG. 1 is a cross-sectional view showing an example of wet etching, which is an isotropic etching, as a conventional technique 1 in the order of processing. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a process in which wet etching, which is an isotropic etching, is performed twice as a conventional technique 2. In FIG. [Diagram 3] FIG. 3 is a cross-sectional view showing an example in which wet etching (or dry etching), which is isotropic etching, is performed three times according to the first embodiment of the present invention in the order of processing. [Figure 4] FIG. 4 is a cross-sectional view showing an example in which wet etching (or dry etching), which is isotropic etching, is performed four times according to the second embodiment of the present invention, in the order of processing. [Figure 5-1] FIG. 5-1 is a cross-sectional view showing an example of the first to fourth wet etching (or dry etching) cycles among seven cycles of isotropic etching according to the third embodiment of the present invention in the order of processing. [Figure 5-2] FIG. 5-2 is a cross-sectional view showing an example of the fifth to seventh cycles of wet etching (or dry etching), which is isotropic etching, in the order of processing, according to the third embodiment of the present invention. [Figure 6] FIG. 6 shows detailed dimensions of a conventional resist mask pattern when the underlying film is etched in a single step. [Figure 7] FIG. 7 shows detailed dimensions of a conventional resist mask pattern when etching is completed in two separate steps on an underlying film. [Figure 8] FIG. 8 shows detailed dimensions of the undercoat film according to the resist mask pattern of the first embodiment of the present invention after etching is completed in three separate steps. [Figure 9-1] FIG. 9-1 is a detailed dimensional diagram showing the fourth etching step performed after dividing the base film into four steps using a resist mask pattern according to the second embodiment of the present invention. [Figure 9-2] FIG. 9-2, subsequent to FIG. 9-1, shows detailed dimensions of the undercoat film formed by the resist mask pattern according to the second embodiment of the present invention after etching is completed in four separate steps. [Figure 10-1] FIG. 10-1 shows detailed dimensions of a conventional resist mask pattern that etches an underlying film in two separate steps, with the first etching time and amount being small and the second etching time and amount being large. [Figure 10-2] FIG. 10-2 shows detailed dimensions when etching an undercoat film using a conventional resist mask pattern in two separate steps, with the first etching divided time and amount being the same as the second etching divided time and amount. [Figure 10-3] FIG. 10-3 shows detailed dimensions when etching an underlying film using a resist mask pattern in two separate steps in a conventional example, where the first etching split time and amount are large and the second etching split time and amount are small. [Figure 11-1] FIG. 11-1 diagrammatically illustrates one of four examples of the process steps in Examples 1, 2, and 3 of the present invention. [Figure 11-2] FIG. 11-2 diagrammatically illustrates one of four examples of the process steps in Examples 1, 2, and 3 of the present invention. [Figure 11-3]FIG. 11-3 illustrates one of four examples of the process steps in Examples 1, 2, and 3 of the present invention. [Figure 11-4] FIG. 11-4 illustrates one of four examples of the process steps in Examples 1, 2, and 3 of the present invention. [Figure 11-5] FIG. 11-5 illustrates diagrammatically one of two examples of the process steps in Example 4 of the present invention. [Figure 11-6] FIG. 11-6 illustrates diagrammatically one of two examples of the process steps in Example 4 of the present invention. [Figure 11-7] FIG. 11-7 is a diagram showing three specific examples of the resist characteristic changing process in the first, second, third and fourth embodiments of the present invention and examples of their combinations. [Figure 11-8] FIG. 11-8 is a diagram showing three specific examples and combinations of the substrate stabilization processing in the first, second and third embodiments of the present invention. [Figure 12] FIG. 12 is a cross-sectional view showing a case where additional processing steps (re-development processing and additional etching processing) are carried out as a fourth embodiment of the present invention. [Figure 13-1] FIG. 13-1 shows a unit processing sequence of a processing apparatus for forming a thin film pattern by etching as a first subexample (Example 5-1) of the fifth embodiment of the present invention. [Figure 13-2] FIG. 13-2 shows the unit processing sequence of a processing apparatus for forming a thin film pattern by etching as a second subexample (Example 5-2) of the fifth embodiment of the present invention. [Figure 13-3] FIG. 13-3 shows the unit processing sequence of a processing apparatus for forming a thin film pattern by etching as a third subexample (Example 5-3) of the fifth embodiment of the present invention. [Figure 13-4] FIG. 13-4 shows the unit processing sequence of a processing apparatus for forming a thin film pattern by etching as a fourth subexample (Example 5-4) of the fifth embodiment of the present invention. [Figure 13-5] FIG. 13-5 shows the unit processing sequence of a processing apparatus for forming a thin film pattern by etching as a fifth subexample (fifth example) of the fifth embodiment of the present invention (fifth example 5-5). [Figure 13-6]FIG. 13-6 shows the unit processing sequence of a processing apparatus for forming a thin film pattern by etching as a sixth subexample (fifth example) of the fifth embodiment of the present invention. [Figure 13-7] FIG. 13-7 is a diagram showing three specific examples and combinations thereof for the resist property change processing unit according to the fifth embodiment of the present invention. [Figure 13-8] FIG. 13-8 is a diagram showing three specific examples and a combination thereof of the substrate stabilization processing unit according to the fifth embodiment of the present invention. [Figure 14] FIG. 14 shows an example of a multi-processing unit apparatus as an example A of an apparatus for realizing the embodiment 5 of the etching-based thin film pattern forming apparatus of the present invention. [Figure 15] FIG. 15 shows an example of an apparatus B for realizing the fifth embodiment of the thin film pattern forming apparatus by etching of the present invention, which is an example of an apparatus including all dry units, that is, a multi-processing unit apparatus in a vacuum. [Figure 16] FIG. 16 shows an example of an apparatus in which substrates are transported by a conveyor system (continuous, intermittent, or discontinuous tact feed) as an example of an apparatus C for realizing the fifth embodiment of the apparatus for forming a thin film pattern by etching according to the present invention. [Figure 17] FIG. 17 shows an example of an apparatus in which substrates are transported by a conveyor system (continuous, intermittent, or discontinuous tact feed) as an example of an apparatus D for realizing the embodiment 5 of the apparatus for forming a thin film pattern by etching according to the present invention. [Figure 18] FIG. 18 shows an example of an apparatus E for implementing the fifth embodiment of the etching thin film pattern forming apparatus of the present invention, in which the substrate is transported by a conveyor system (continuous, intermittent or discontinuous tact feed). [Figure 19] FIG. 19 shows an example of an apparatus in which substrates are transported by a conveyor system (continuous, intermittent, or discontinuous tact feed) as an example of an apparatus F for realizing the fifth embodiment of the apparatus for forming a thin film pattern by etching according to the present invention. [Figure 20]FIG. 20 shows, as an additional explanation for the first, second, third and fourth embodiments of the present invention, an example of resist softening and curving process, which is an example of resist deformation process 1, which is a resist characteristic changing process, in which the resist mask is formed thin or a material that is easily deformed under its own weight is selected, and the resist is softened and curved at a temperature below the cure temperature. [Explanation of symbols]
[0188] P1 Resist mask pattern (initial) P2 Resist mask pattern (after the first resist characteristic change process) P3 Resist mask pattern (after second resist characteristic change process) P4 Resist mask pattern (after the third resist characteristic change process) P5 Resist mask pattern (after 4th resist characteristic change process) P6 Resist mask pattern (after 5th resist characteristic change process) P7 Resist mask pattern (after 6th resist characteristic change process) T0 base film T1 Undercoat pattern (after 1st etching) T2 Undercoat film pattern (after second etching) T3 Undercoat pattern (after the third etching) T4 Undercoat pattern (after 4th etching) T5 Undercoat pattern (after 5th etching) T6 Base film pattern (after 6th etching) T7 Undercoat pattern (after 7th etching) E1x1: The amount of side etching of the base film in the lateral direction (X direction) in the first etching when the base film is etched in only one step E1y1: The amount of side etching of the base film in the lateral direction (Y direction) in the first etching when the base film is etched in only one step E1-1Point The edge of the resist mask pattern P1 when the undercoat film is etched in only one step E1x is the total amount of side etching of the underlayer in the lateral direction (X direction) in all etchings when the underlayer is etched in only one step E1y is the amount of side etching (in the Y direction) of the underlayer in all etchings when the underlayer is etched in only one step E2x1: The amount of side etching of the base film in the lateral direction (X direction) in the first etching when the base film is etched twice E2y1: The amount of side etching of the base film in the lateral direction (Y direction) in the first etching when the base film is etched twice E2-1Point Edge of resist mask pattern P1 when etching of the undercoat film is completed in two steps E2x2: The amount of side etching of the base film in the lateral direction (X direction) in the second etching when the base film is completely etched in two steps E2y2 is the amount of side etching (Y direction) of the base film in the second etching when the base film is completely etched in two steps E2-2Point Edge of resist mask pattern P2 when etching of the undercoat film is completed in two steps E2x is the total amount of side etching of the base film in the lateral direction (X direction) in all etchings when the base film is etched in two steps E2y is the amount of side etching of the base film in the lateral direction (Y direction) in all etchings when the base film is etched in two steps E3x1: The amount of side etching of the base film in the lateral direction (X direction) in the first etching when the base film is etched three times E3y1 The amount of side etching of the base film in the lateral direction (Y direction) in the first etching when the base film is etched three times E3-1Point Edge of resist mask pattern P1 when etching of the undercoat film is completed in three steps E3x2: The amount of side etching of the base film in the lateral direction (X direction) in the second etching when the base film is etched three times E3y2 The amount of side etching of the base film in the lateral direction (Y direction) in the second etching when the base film is etched three times E3-2Point Edge of resist mask pattern P2 when etching of the undercoat film is completed in three steps E3x3: The amount of side etching of the base film in the lateral direction (X direction) in the third etching when the base film is etched three times E3y3: The amount of side etching (Y direction) of the base film in the third etching when the base film is etched three times E3-3Point Edge of resist mask pattern P3 when etching of the undercoat film is completed in three steps E3x is the total amount of side etching of the underlayer in the lateral direction (X direction) in all etchings when the underlayer is etched three times. E3y: The amount of side etching (in the Y direction) of the base film in all etchings when the base film is etched three times E4x1: The amount of side etching of the base film in the lateral direction (X direction) in the first etching when the base film is etched four times E4y1: The amount of side etching of the base film in the lateral direction (Y direction) in the first etching when the base film is etched four times E4-1Point End of resist mask pattern P1 when etching of the undercoat film is completed in four steps E4x2: The amount of side etching of the base film in the lateral direction (X direction) in the second etching when the base film is etched four times E4y2: The amount of side etching of the base film in the lateral direction (Y direction) in the second etching when the base film is etched four times E4-2Point Edge of resist mask pattern P2 when etching of the undercoat film is completed in three steps E4x3: The amount of side etching (X direction) of the base film in the third etching when the base film is etched four times E4y3: The amount of side etching of the base film in the lateral direction (Y direction) in the third etching when the base film is etched four times E4-3Point End of resist mask pattern P3 when etching of the undercoat film is completed in four steps E4x4: The amount of side etching of the base film in the lateral direction (X direction) in the fourth etching when the base film is etched four times E4y4: The amount of side etching (Y direction) of the base film in the fourth etching when the base film is etched four times E4-4Point The edge of the resist mask pattern P4 when the undercoat film is etched four times. E4x is the total amount of side etching of the base film in the lateral direction (X direction) in all etchings when the base film is etched four times. E4y: The amount of side etching (in the Y direction) of the base film in all etchings when the base film is etched four times E2ax1 The amount of side etching (X direction) of the base film in the first etching when the base film is etched twice and the amount of the first etching is smaller than that of the second etching E2ay1 The amount of side etching (Y direction) of the base film in the first etching when the base film is etched twice and the amount of the first etching is smaller than that of the second etching E2a-1Point The edge of the resist mask pattern P1 when the undercoat film is etched twice and the amount of etching in the first time is smaller than that in the second time. E2ax2 The amount of side etching (X direction) of the base film in the second etching when the base film is etched twice and the amount of etching in the first etching is smaller than that in the second etching E2ay2 The amount of side etching (Y direction) of the base film in the second etching when the base film is etched twice and the amount of etching in the first etching is smaller than that in the second etching E2a-2Point The edge of the resist mask pattern P2 when the undercoat film is etched twice and the amount of etching in the first time is smaller than that in the second time. E2ax The total amount of side etching (X direction) of the base film in all etchings when the base film is etched twice and the amount of etching in the first step is smaller than that in the second step E2ay The amount of side etching (Y direction) of the base film in all etchings when the base film is etched twice and the amount of etching in the first step is smaller than that in the second step E2ax1 The amount of side etching (X direction) of the base film in the first etching when the base film is etched twice and the amount of etching in the first and second etchings is the same E2by1 The amount of side etching (Y direction) of the base film in the first etching when the base film is etched twice and the amount of etching in the first and second etchings is the same E2b-1Point The edge of the resist mask pattern P1 when the undercoat film is etched twice and the amount of etching in the first and second times is the same. E2bx2 The amount of side etching (X direction) of the base film in the second etching when the base film is etched twice and the amount of etching in the first and second etchings is the same E2by2 The amount of side etching (Y direction) of the base film in the second etching when the base film is etched twice and the amount of etching in the first and second etchings is the same E2b-2Point The edge of the resist mask pattern P2 when the undercoat film is etched twice and the amount of etching in the first and second times is the same. E2bx The total amount of side etching (X direction) of the base film in all etchings when the base film is etched twice and the amount of etching in the first and second times is the same E2by The amount of side etching (Y direction) of the base film in all etchings when the base film is etched twice and the amount of etching in the first and second times is the same E2ax1 The amount of side etching (X direction) of the base film in the first etching when the base film is etched twice and the amount of the first etching is greater than the amount of the second etching E2ay1 The amount of side etching (Y direction) of the base film in the first etching when the base film is etched twice and the amount of the first etching is greater than the amount of the second etching. E2a-1Point The edge of the resist mask pattern P1 when the undercoat film is etched twice and the amount of etching in the first time is greater than that in the second time. E2ax2 The amount of side etching (X direction) of the base film in the second etching when the base film is etched twice and the amount of etching in the first etching is greater than the amount of etching in the second etching E2ay2 The amount of side etching (Y direction) of the base film in the second etching when the base film is etched twice and the amount of etching in the first etching is greater than the amount of etching in the second etching E2a-2Point The edge of the resist mask pattern P2 when the undercoat film is etched twice and the amount of etching in the first step is greater than that in the second step. E2ax The total amount of side etching (X direction) of the base film in all etchings when the base film is etched twice and the amount of etching in the first step is greater than the amount of etching in the second step E2ay The amount of side etching (Y direction) of the base film in all etchings when the base film is etched twice and the amount of etching in the first step is greater than the amount of etching in the second step. S1 Resist coating process S2 Heat bake processing S3 Temperature control (cooling) processing S4 Resist exposure processing S5 Resist development process S6 Heat bake processing S7 Temperature control (cooling) processing RH1 Resist property change processing RH2 Substrate stabilization treatment S12 Etching process S13 Resist stripping process S14 Redevelopment S15 Additional etching process Y1 Resist coating processing unit Y2 Heat bake processing unit Y3 Temperature control (cooling) processing unit Y4 Resist exposure processing unit Y5 Resist Development Unit Y6 Heating and baking processing unit Y7 Temperature control (cooling) processing unit YRH1 Resist property modification processing unit YRH2 Substrate stabilization unit Y12 Etching Processing Unit Y13 Resist stripping unit Y14 Redevelopment Processing Unit Y15 additional etching processing unit C1, C2, C3, C4 Substrate cassettes (cassettes containing substrates to be processed) R1 Transport robot (takes substrates in and out of the substrate cassettes C1 to C4) R2 Transport robot (receives substrates from the R1 transport robot and transports them to each unit) LL1 Load Lock Chamber 1 (vacuum chamber for R1 transfer robot and entire path) LL2 Load Lock Chamber 2 (vacuum chamber for R2 transfer robot and entire path) R3 Transport robot (moves from the lower line to the upper line, or from the left line to the right line) R4 Transport robot (moves from the upper line to the lower line, or from the right line to the left line) M1: In the resist mask pattern P2, the interface where the base film T0 and the resist pattern are separated by etching becomes the new interface where the base film T1 and the resist pattern P2 come into contact, and the adhesion therebetween is at least equal to or greater than the adhesion between the base film T0 and the resist pattern P1 before side etching. M2: In the resist mask pattern P3, the interface where the base film T1 and resist pattern P2 are separated by etching becomes the new interface where the base film T2 and resist pattern P3 come into contact, and the adhesion therebetween is at least equal to or greater than the adhesion between the base film T1 and resist pattern P2 before side etching. M3: In the resist mask pattern P4, the interface where the base film T2 and resist pattern P3 are separated by etching becomes the new interface where the base film T3 and resist pattern P4 come into contact, and the adhesion therebetween is at least equal to or greater than the adhesion between the base film T2 and resist pattern P3 before side etching.
Claims
1. A method for forming a thin film pattern, comprising the steps of: forming an organic film pattern containing at least one type of organic substance on an underlying film to be etched; or forming a mask of a pattern using a resist film; and then etching the underlying film to be etched at least three times, and optimally four times or more, to remove all of the underlying film at least in the portion not covered by the organic film pattern, and a processing apparatus therefor.
2. The method for forming a thin film pattern and the processing apparatus thereof according to claim 1, characterized in that, when the etching of the base film to be etched is performed at least three times, and optimally four times or more, the total amount of etching of the base film to be etched in each etching or the total amount of etching of each etching calculated from the product of the etching rate of each etching and the processing time of each etching is at least within a ratio of 100 to 200%, and optimally within a ratio of 110 to 150%, when the value equal to the thickness of the base film to be etched is taken as 100%.
3. 3. The method for forming a thin film pattern and the processing apparatus thereof according to claim 1, wherein, when the etching of the underlying film to be etched is performed at least three times, and optimally four times or more, the etching amount of the underlying film to be etched each time, or the product of the etching rate of each time and the processing time of each time, is at least a value within a range of 100±50%, and optimally 100±20%, when the value obtained by dividing the total thickness of the underlying film by the number of times of etching is taken as 100%.
4. 4. The method for forming a thin film pattern and the processing apparatus thereof according to claim 1, wherein, when the etching of the base film to be etched is performed at least three times, and optimally four times or more, the etching amount of the base film to be etched each time, or the product of the etching rate of each time and the processing time of each time, when the total thickness of the base film divided by the number of times of etching is taken as a percentage of 100%, is at least 100±20%, and optimally 100±10%, except for the final etching, and is at least 100+0 to 100%, and optimally 100+0 to 50% for the final etching only.
5. 5. The method for forming a thin film pattern and the processing apparatus thereof according to claim 1, further comprising the step of performing a process for changing the characteristics or shape of the mask of the organic film pattern or the resist film pattern at least before each etching process from the second onward.
6. 6. The method for forming a thin film pattern according to claim 1, wherein a mask of an organic film pattern containing at least one kind of organic substance or a pattern using a resist film recovers or at least increases adhesion to an underlying film by a process for changing the characteristics or shape of the mask of the organic film pattern or the resist film pattern.
7. 7. The method for forming a thin film pattern according to claim 1, wherein the organic film pattern containing at least one kind of organic substance or the mask of the pattern using a resist film is deformed by softening, bending, curving, liquid-fluidizing (reflowing), or the like, through a process for changing the characteristics or shape of the mask of the organic film pattern or the resist film pattern.
8. 8. The method for forming a thin film pattern according to claim 1, wherein the organic film pattern containing at least one kind of organic substance or the mask of the pattern using a resist film is deformed by a process for changing the characteristics or shape of the organic film pattern or the mask of the resist film pattern, such as softening, bending, curving, or liquid-like fluidization (reflow), and then the adhesion with the underlying film is restored or at least increased.
9. 9. The method for forming a thin film pattern according to claim 1, characterized in that a mask of the organic film pattern containing at least one kind of organic substance or a pattern using a resist film is deformed so as to cover and conceal at least a part, and optimally, all of the part where side etching of the base film has occurred, by a process for changing the characteristics and shape of the mask of the organic film pattern or the resist film pattern.
10. 10. The method for forming a thin film pattern according to claim 1, further comprising selecting and using a material capable of recovering or at least increasing adhesion to an underlying film each time, and repeating deformations such as softening, bending, curving, and liquid-like fluidization (reflow), and of covering at least a part of, or optimally, all of, a portion of the underlying film where side etching has occurred, even when various resist property changing processes are repeatedly performed on the organic film pattern containing at least one kind of organic substance, or a mask of a pattern using a resist film, as a characteristic of the mask material.
11. 11. The method for forming a thin film pattern according to claim 1, wherein a mask of the organic film pattern containing at least one kind of organic substance or a pattern using a resist film is formed to a thickness of 1 / 2 or less of the thickness of the base film, optimally 1 / 4 or less, or 0.5 μm or less, optimally 0.25 μm or less.
12. 12. The method for forming a thin film pattern and the processing apparatus thereof according to any one of claims 1 to 11, characterized in that, in the method for forming a thin film pattern and the processing apparatus thereof, a process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film is carried out at least before each etching process from the second onwards, and then a re-development process or an ashing process, which is the second onwards development process, is carried out.
13. 13. The method for forming a thin film pattern according to claim 1, wherein the process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film includes a process for recovering or increasing the adhesion or adhesion area of at least a part of the mask of the organic film pattern or the pattern using a resist film to an underlying film.
14. 14. The method for forming a thin film pattern according to claim 1, characterized in that the process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film includes a process for improving adhesion to an underlying film or recovering or increasing an adhesion area by only softening or curving at least a part of the mask of the organic film pattern or the pattern using a resist film without dissolving or becoming liquid (reflow).
15. 15. The method for forming a thin film pattern according to claim 1, wherein the process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film includes a process for dissolving or fluidizing (reflowing) at least a part of the mask of the organic film pattern or the pattern using a resist film, thereby improving adhesion to an underlying film or recovering or increasing an adhesion area.
16. 16. The method for forming a thin film pattern according to claim 1, wherein the process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film is simply a heat bake process performed on the mask of the organic film pattern or the pattern using a resist film.
17. 17. The method for forming a thin film pattern according to claim 1, wherein the process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film is a process for exposing the mask of the organic film pattern or the pattern using a resist film to an organic solvent chemical.
18. 18. The method for forming a thin film pattern according to claim 1, wherein the process for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film is a process that combines a process of exposing the mask of the organic film pattern or the pattern using a resist film to an organic solvent chemical and a heat bake process.
19. 19. The method for forming a thin film pattern and its processing apparatus according to any one of claims 1 to 18, characterized in that the method for exposing the organic film pattern or the mask of the pattern using a resist film to the organic solvent chemical is a method of exposing it to the vapor of the organic solvent chemical, a method of simultaneously spraying the organic solvent chemical and an inert gas such as N2, Ar, or the like, or a method of exposing it to a gas in which an inert gas such as N2, Ar, or the like is bubbled into the organic solvent chemical.
20. 20. The method for forming a thin film pattern according to claim 1, wherein the redevelopment process is a process in which the amount of removal varies depending on the exposure sensitivity of the organic film pattern or the mask of the pattern using a resist film.
21. 21. The method for forming a thin film pattern and the processing apparatus therefor according to claim 1, wherein the redevelopment is performed using a chemical solution whose concentration is lower than that of the chemical solution used in the development.
22. 22. The method for forming a thin film pattern according to any one of claims 1 to 21, characterized in that the treatment for changing the characteristics or shape of the mask of the organic film pattern or the pattern using a resist film comprises a heating bake treatment for the mask of the organic film pattern or the pattern using a resist film, the heating bake treatment being performed at a temperature equal to or lower than a cure temperature of the mask of the organic film pattern or the mask of the pattern using a resist film, or 100 to 130°C or lower.
23. 23. The method for forming a thin film pattern and the processing apparatus therefor according to any one of claims 1 to 22, characterized in that the etching is wet etching or dry etching, particularly chemical dry etching in which only the radical gas portion is extracted from the plasma state of the etching gas and processed separately.
24. 24. The thin film pattern processing apparatus according to claim 1, wherein the processing units include at least three units: a processing unit for changing the shape or characteristics of a resist, a processing unit for drying or cooling or stabilizing temperature, and a processing unit for etching.
25. 25. The thin film pattern processing apparatus according to claim 1, wherein the processing unit for changing the shape or characteristics of the resist is a processing unit that heats and bakes the substrate, or a processing unit that combines a process of exposing the substrate to an organic solvent chemical and a process of heat baking.
26. In the thin film pattern processing apparatus described in any one of claims 1 to 25, a processing unit for drying or cooling or stabilizing temperature is a unit that performs only cooling processing to bring the substrate temperature to room temperature or the like, only drying processing, or a unit that combines drying processing and cooling processing.
27. A method for forming a thin film pattern, and the processing apparatus thereof, characterized in that in the processing apparatus of the thin film pattern described in any one of claims 1 to 26, processing in a processing unit for changing the shape or characteristics of the resist, a processing unit for drying or cooling or stabilizing the temperature, and a processing unit for etching are repeated at least two times, and optimally three times or more.
28. 28. A method for forming a thin film pattern, comprising the steps of: in the processing apparatus for a thin film pattern according to any one of claims 1 to 27, repeating the processing at least twice, and optimally three times, in the order of a processing unit for changing the shape or characteristics of a resist, a processing unit for drying or cooling or stabilizing the temperature, and a processing unit for etching, and the method and apparatus for forming the thin film pattern.
Citation Information
Patent Citations
JP1975037374A
Etching method that prevent side etch
JP1978077848A
Chemical etching process
JP1982016169A
Formation of pattern
JP1985234982A
Manufacture of printed circuit board
JP1993327179A
Cited By
Method for forming three-dimensional microstructures using etching and etching mask used therefor
JP2026512764A