Woven fabric and clothing

A polyester multifilament fabric with a core-sheath structure and specific twist coefficient addresses the issue of shine by creating three-dimensional irregularities, effectively reducing shine and maintaining fabric appearance during prolonged use.

JP2024132912APending Publication Date: 2024-10-01TORAY INDUSTRIES INC

Patent Information

Application Number
JP2024026217
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-02-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing fabrics fail to effectively suppress shine caused by long-term wear due to fiber smoothing, leading to visible light reflection and impaired appearance.

Method used

A polyester multifilament fabric with a core-sheath structure, where the sheath yarn is finer and shorter than the core yarn, and a specific twist coefficient, combined with a ratio of core to sheath yarns, creates a three-dimensional irregularity that reduces friction-induced shine.

Benefits of technology

The fabric effectively suppresses shine during long-term wear by dispersing frictional stress and maintaining a non-smooth surface, enhancing durability and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132912000001
    Figure 2024132912000001
  • Figure 2024132912000002
    Figure 2024132912000002
  • Figure 2024132912000003
    Figure 2024132912000003
Patent Text Reader

Abstract

To provide a woven fabric capable of suppressing shininess caused by wearing for a long period.SOLUTION: There is provided a woven fabric containing a polyester multifilament thread having a core-sheath structure including a core yarn and a sheath yarn, in which the core yarn has a yarn length shorter than that of the sheath yarn, the sheath yarn has a fineness smaller than that of the core yarn, a number ratio of the core yarn to the sheath yarn (the number of the core yarn: the number of the sheath yarn) is 1:6 to 1:24, and a twist coefficient K determined by the following formula 1 from the twist number T of the polyester multifilament thread and the fineness D of the multifilament thread is 0 to 100: K=T / (10000 / D)1 / 2...formula 1, where K: twist coefficient, T: twist number (T / m), and D: fineness (dtex).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fabric that suppresses shine that occurs when wearing clothing for a long period of time, and to clothing containing the same. [Background technology]

[0002] When clothing such as suits and school uniforms are worn for a long period of time, a particular shine, known as "glossiness," often occurs on parts of the clothing (elbows, buttocks, knees, etc.). It is said that shine occurs when the fiber surface is worn down and smoothed by friction and pressure generated when the clothing comes into contact with a chair or other textile product, causing visible light to be generated by specular reflection. When shine occurs, the clothing shows a sense of wear, and the noticeable localized gloss significantly impairs the appearance of quality, so it is desirable to suppress shine.

[0003] As a method for suppressing the shine of clothing, a method using a shine inhibitor for textile products has been proposed. However, the shine inhibitor only loosens the alignment of fibers and improves the surface slipperiness, so it does not fundamentally improve the fiber, and the shine inhibitor has poor durability. Furthermore, the effect is temporary, so repeated treatment is required.

[0004] On the other hand, as an approach to sustaining the effect of suppressing the occurrence of shine on clothing, it has been proposed to endow the fabric itself with a shine-suppressing function.

[0005] Patent Document 1 discloses an anti-shine fabric having specified elongation properties, which is produced by draw-twisting highly oriented undrawn polyester filament yarn having a 5-12-lobe modified cross section with a specified concave surface ratio.

[0006] Furthermore, Patent Document 2 proposes a false twist textured yarn obtained from an air-entangled yarn having a self-extensible polyester intermediate oriented yarn as a sheath yarn and a polyester-based high-shrinkage yarn having a boiling water shrinkage rate at least 3% higher than that of the intermediate oriented yarn as a core yarn, the false twist textured yarn being characterized in that the total crimp rate is at a low level of 5% or less, and discloses a method for suppressing the occurrence of shine by using the false twist textured yarn. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Unexamined Patent Publication No. 1-156542 [Patent Document 2] JP 2000-314038 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, in Patent Document 1, because the thick yarn is exposed on the outermost surface of the woven fabric, the fiber surface wears and becomes smooth when the garment is worn for a long period of time, and as a result, the shine-suppressing function of the modified cross-section yarn is not fully exerted, resulting in an issue of insufficient shine-suppressing function of the woven fabric.

[0009] In addition, in the woven fabric described in Patent Document 2, the sheath yarn is made finer than the core yarn in order to improve the shine-suppressing function, but since the thickness is between 2 denier and 4 denier, it is insufficient to suppress shine.

[0010] In view of the above problems, an object of the present invention is to provide a fabric that suppresses shine that occurs with long-term wear, and clothing including the fabric. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention has the following configuration. (1) A woven fabric comprising a polyester multifilament having a core-sheath structure comprising a core yarn and a sheath yarn, the core yarn having a shorter yarn length than the sheath yarn, the sheath yarn having a finer fiber size than the core yarn, a ratio of the number of the core yarn to the sheath yarn (number of the core yarns:number of the sheath yarns) being 1:6 to 1:24, and a twist coefficient K calculated from the number of twists T of the polyester multifilament and the fineness D of the multifilament according to the following formula 1 being 0 to 100. K = T / (10000 / D) 1 / 2 (Formula 1) (K: twist coefficient, T: number of twists (T / m), D: fineness (dtex)) (2) The woven fabric described in (1), wherein the sheath yarn is formed from two types of polyester. (3) The woven fabric according to (1) or (2), wherein the sheath yarn has a single yarn fineness of 0.1 to 2.0 dtex. (4) The woven fabric according to any one of (1) to (3), in which the warp or weft yarns are floating yarns, and the polyester multifilament having a core-sheath structure is arranged as the floating yarn. (5) The woven fabric according to any one of (1) to (4), having an initial water repellency of grade 3 or higher. (6) The woven fabric according to any one of (1) to (5), wherein the low pressure region compressibility Cr calculated by the following formula 2 is 5% to 30%: Cr=(T0-T1) / T0×100 (Formula 2) (Cr: compression ratio in low pressure region (%), T0: fabric thickness (mm) when a lower limit pressure of 0.2 kPa is applied, T1: fabric thickness (mm) when a constant pressure of 4.9 kPa is applied) (7) A woven fabric according to any one of (1) to (6), which has a light fastness of grade 4 or higher when measured with an ultraviolet carbon arc lamp. (8) The woven fabric according to any one of (1) to (7), comprising an azo disperse dye and a quinone disperse dye, the content of the quinone disperse dye being 30 to 70 mass% relative to the total content of the azo disperse dye and the quinone disperse dye. (9) Clothing comprising the fabric according to any one of (1) to (8). Effect of the Invention

[0012] According to the present invention, it is possible to provide a fabric that suppresses shine that occurs when wearing clothing for a long period of time, and clothing containing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below together with preferred embodiments.

[0014] The woven fabric of the present invention has a polyester multifilament having a core-sheath structure with a core yarn and a sheath yarn, the core yarn being shorter in length than the sheath yarn, the sheath yarn being finer than the core yarn, and the ratio of the number of core yarns to the number of sheath yarns (number of core yarns: number of sheath yarns) being 1:6 to 1:24.Furthermore, the woven fabric is characterized in that the twist coefficient K calculated from the number of twists T of the polyester multifilament and the fineness D of the multifilament by the following formula 1 is 0 to 100. K = T / (10000 / D) 1 / 2 (Formula 1) (K: twist coefficient, T: number of twists (T / m), D: fineness (dtex)).

[0015] <Fabric composition> The woven fabric of the present invention is made of a multifilament consisting of a core yarn and a sheath yarn. Here, the sheath yarn is wound around the core yarn, and multiple sheath yarns are wound around one core yarn. The woven fabric of the present invention is woven using the multifilament as a raw yarn.

[0016] <Polymer composition of core yarn and sheath yarn> The polymers constituting the core yarn and the sheath yarn of the multifilament according to the present invention are both made of polyester, and may be formed of a single component polyester or may be formed of multiple polyesters. Preferred examples of polyesters include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, and copolymers thereof with a dicarboxylic acid component, a diol component, or an oxycarboxylic acid component, or blends of these polyesters. In the present invention, polyesters with different melting points are considered to be different types of polyesters.

[0017] The polyester composition of the core yarn and the sheath yarn is not particularly limited as long as it satisfies the constitution of the present invention, and may be a combination that causes a shrinkage difference between the core yarn and the sheath yarn, as described below. For example, when the core yarn and the sheath yarn are each a single-component polyester, it is preferable that they are different polyesters. In addition, when the core yarn is a single component and the sheath yarn is formed of multiple polyesters, it is also preferable to select different polyesters for each, and one of the multiple polyesters of the sheath yarn may have the same composition as the polyester of the core yarn.

[0018] By forming the sheath yarn from multiple polyesters, as described below, the sheath yarn undergoes crimping during heat treatment, resulting in a structure in which three-dimensional unevenness is generated in the multifilament and the woven fabric using the same. When three-dimensional unevenness is generated in the woven fabric, the area of ​​contact between the frictional object and the woven fabric is reduced, thereby reducing the area where the fiber surface is smoothed. Therefore, the woven fabric of the present invention has a structure that is more effective in suppressing shine. When two types of polyesters with different melting points are combined, the polyester with the lower melting point shrinks first during heat treatment, and the shrinkage characteristics of each polyester are different, so that the shrinkage difference between the polymers is expressed and the sheath yarn can be given crimping. As the two types of polyesters with different melting points that constitute the sheath yarn, a combination of polyethylene terephthalate (PET) and polyethylene terephthalate copolymerized with isophthalic acid (IPA), in which the difference in melting points between the polyesters is large, is preferably used.

[0019] In addition, these polymers may contain inorganic fine particles, organic compounds, and carbon black as matting agents such as titanium oxide, flame retardants, lubricants, antioxidants, coloring pigments, etc., as necessary, within the scope of the invention.

[0020] <Length of core and sheath yarns> The core yarn according to the present invention has a shorter thread length than the sheath yarn. When the thread length of the core yarn is shorter than that of the sheath yarn, the sheath yarn of the woven fabric swells, thereby reducing stress when the woven fabric comes into contact with the frictional object, and thus exhibiting a further effect in suppressing shine. The thread length is measured by the method described in F. Thread Length and Thread Length Difference Ratio in the Examples below. One way to make the thread length of the core yarn shorter than that of the sheath yarn is to make the shrinkage rate of the core yarn greater than that of the sheath yarn. In other words, when the core yarn shrinks more than the sheath yarn, the core yarn becomes longer than the sheath yarn.

[0021] From the viewpoint of highlighting the shrinkage difference, it is preferable that the core yarn uses a polymer having a lower melting point than the sheath yarn. On the other hand, it is preferable that the sheath yarn uses a polymer having a higher melting point than the core yarn, and it is also more preferable to use a two-component sheath yarn that combines a low-melting polymer and a high-melting polymer. By using a two-component sheath yarn, it is possible to express crimps with different heights that are not expressed when the sheath yarn is a single component. That is, the shrinkage rate of the core yarn is greater than that of the sheath yarn, the core yarn is shorter than the sheath yarn, and the core yarn is covered by the sheath yarn. In addition, as described later, the sheath yarn of the multifilament of the present invention has a smaller fineness than the core yarn, i.e., a smaller fiber diameter. Therefore, even if the woven fabric of the present invention is subjected to friction, only the fine sheath yarn located on the outermost surface of the woven fabric is worn and smoothed. Therefore, the smoothed area is smaller than that of a woven fabric consisting of only normal thick fineness, and the occurrence of shine can be further suppressed.

[0022] When two types of polymer compositions are combined for the sheath yarn, they may be of the side-by-side type (bimetal type) or eccentric sheath-core type. When the sheath yarn is a side-by-side type composite fiber or an eccentric sheath-core type composite fiber, the fine spiral structure of the sheath yarn can produce complex crimps, further improving shine suppression.

[0023] <Core and sheath yarn fineness> The single yarn fineness of the sheath yarn according to the present invention is preferably 0.1 to 2.0 dtex, and more preferably 0.4 to 1.9 dtex. When the single yarn fineness of the sheath yarn is 0.1 dtex or more, the color development of the woven fabric is improved, which is preferable. On the other hand, when the single yarn fineness of the sheath yarn is 2.0 dtex or less, even if the woven fabric is subjected to friction and the fiber surface is smoothed, the smooth area becomes smaller, so that the occurrence of shine can be further suppressed.

[0024] The core yarn preferably has a single yarn fineness of 1.0 to 10.0 dtex, more preferably 2.0 to 5.0 dtex. When the core yarn has a single yarn fineness of 1.0 dtex or more, the color development of the woven fabric is improved. On the other hand, when the core yarn has a single yarn fineness of 10.0 dtex or less, the texture becomes soft, and the texture of the woven fabric can be improved.

[0025] It is important that the sheath yarn according to the present invention has a finer diameter than the core yarn. In the present invention, the sheath yarn having a finer diameter than the core yarn means that the single yarn fineness of the sheath yarn is lower, i.e., finer, than the single yarn fineness of the core yarn. If the fineness of the sheath yarn arranged on the outside is thinner than that of the core yarn arranged on the inside, the area smoothed by friction is reduced, which can provide a further effect in suppressing shine, and also, by not making the inner core yarn fine, the color development is not reduced, so the difference in fineness of the sheath yarn relative to the fineness of the core yarn (fineness of the core yarn - fineness of the sheath yarn) is preferably 1 dtex or more, more preferably 2 dtex or more.

[0026] <Ratio of core threads to sheath threads> The ratio of the number of core yarns to the sheath yarns (number of core yarns: number of sheath yarns) is 1:6 to 1:24. By setting the ratio of the number in the above range, the exposure of the core yarns having a larger fineness than the sheath yarns in the polyester multifilament can be suppressed, and the shine of the woven fabric can be suppressed. Here, if the ratio of the sheath yarns is lower than the ratio of the number of core yarns to the sheath yarns of 1:6, i.e., the ratio of the number of sheath yarns is low, the sheath yarns cannot completely cover the thick core yarns, and the core yarns having a larger fineness than the sheath yarns are exposed on the surface of the polyester multifilament, and when smoothed by friction, the smooth surface becomes large and shine occurs. On the other hand, if the ratio of the number of core yarns to the sheath yarns is higher than 1:24, i.e., the ratio of the number of sheath yarns is high, the sheath yarns having a smaller fineness than the core yarns are excessive, and the color development of the woven fabric decreases. More preferably, the ratio of the number of core yarns to the sheath yarns is 1:6 to 1:12.

[0027] <Structure of multifilament with core-sheath structure> The multifilament having a core-sheath structure contained in the woven fabric of the present invention may be a yarn obtained by a textured yarn made up of a plurality of yarns, or may be a yarn obtained by subjecting a sea-island composite fiber to a sea-removal treatment. In the case of textured yarn, the woven fabric is made from a multifilament obtained by intertwining a thick, high-shrinkage yarn with a thin, low-shrinkage yarn.

[0028] <Twist coefficient> When calculated from the following formula 1 using the fineness D of the multifilament and the twist number T of the multifilament obtained by the method described later, it is important that the twist factor K of the multifilament is 0 to 100, and more preferably 0 to 80. A twist factor of 0 means that there is no twist, and a twist factor of 80 or less means that the multifilament is not very twisted. If the twist factor is in the above range, the multifilament constituting the woven fabric can be made bulging. If the twist factor is greater than 100, that is, if the twist is strong, the multifilament is strongly restrained, and the stress dispersion effect due to the core-sheath structure decreases when friction occurs, so that the sheath yarn becomes smoother and more likely to become shiny. K = T / (10000 / D) 1 / 2 (Formula 1) (K: twist coefficient, T: number of twists (T / m), D: fineness (dtex)).

[0029] <Low pressure range compression rate> The low pressure region compressibility of a woven fabric (hereinafter sometimes referred to as Cr) is calculated according to the following formula 2 and Example H. Low pressure region compressibility described later, and is preferably 5% to 30%. Unlike the usual compressibility evaluation that evaluates the crushability of a woven fabric, the low pressure region compressibility can evaluate the ease with which a woven fabric disperses stress against frictional force. Cr=(T0-T1) / T0×100 (Formula 2) (Cr: compression rate in the low pressure region (%), T0: fabric thickness (mm) when a lower limit pressure of 0.2 kPa is applied, T1: fabric thickness (mm) when a constant pressure of 4.9 kPa is applied).

[0030] Here, the lower limit pressure in formula 2 refers to the initial load in the compression ratio test, and the constant pressure refers to the upper limit pressure applied to the woven fabric. From the start of pressure application to the woven fabric of the present invention up to a pressure of 0.2 kPa, mainly the fuzz present in the woven fabric is compressed, and due to this influence, it is not possible to evaluate the stress dispersion of the woven fabric against frictional force. Therefore, 0.2 kPa is set as the lower limit pressure. In addition, when the woven fabric of the present invention is used as clothing, the load applied when wearing the clothing is equivalent to a pressure of 4.9 kPa, so that this pressure is defined as a constant pressure and evaluated as the low pressure range compression ratio.

[0031] When the low pressure region compression rate is 5% or more, the stress of the woven fabric against frictional force is sufficiently dispersed, and the occurrence of shine can be further suppressed. On the other hand, when the low pressure region compression rate is 30% or less, the number of floating threads is reduced, and the occurrence of snagging and pilling of hooks and zippers can be suppressed. A more preferable range is 10% to 25%.

[0032] <Weaving structure> The weave of the woven fabric of the present invention is not particularly limited, but examples thereof include plain weave, twill weave, satin weave, varied plain weave, varied twill weave, varied satin weave, variegated weave, patterned weave, single-ply weave, double weave, multi-weave, warp pile weave, weft pile weave, and leno weave.

[0033] In order to arrange a polyester multifilament having a sheath-core structure with a shine-suppressing effect on the surface of the fabric of the garment, it is also possible to use polyester multifilament for both the warp and weft. Also, by using a multifilament having a sheath-core structure for either the warp or weft, and arranging a thread that imparts another function such as stretchability or antistatic properties for the other thread, it is possible to impart a function other than shine suppression. In this case, it is preferable that the weave structure is such that either the warp or weft is a floating thread, and that the polyester multifilament having a sheath-core structure is arranged as the floating thread. Also, the floating thread can be formed by arranging a plurality of polyester multifilaments in the warp or weft to give it bulk. That is, due to the above circumstances, it is preferable that the woven fabric of the present invention has a weave structure in which the warp or weft is a floating thread, and more preferably, it is a 1 / 3 twill (1 / 3 twill weave) or a 3 / 1 twill (3 / 1 twill weave).

[0034] <dye> The disperse dyes used in the woven fabric of the present invention are not particularly limited, but include azo dyes classified as benzene azo dyes and heterocyclic azo dyes, and quinone disperse dyes containing a condensed anthraquinone skeleton. Azo disperse dyes have excellent color development and are inexpensive. On the other hand, quinone disperse dyes, which have a stable color skeleton, are resistant to hydrolysis and reductive decomposition and have good light fastness.

[0035] Since the yarn of the present invention is fine, it is difficult to obtain color development compared to yarn of normal fineness, and it is easily faded by the influence of sunlight. Due to this characteristic, it is preferable to use azo-based disperse dyes and quinone-based disperse dyes in combination. When disperse dyes are used in combination, the content of the quinone-based disperse dye is preferably 30 to 70% by mass relative to the total content of the azo-based disperse dye and the quinone-based disperse dye. If the content of the quinone-based disperse dye is less than 30% by mass, the light resistance decreases, while if it is more than 70% by mass, the desired color development cannot be obtained.

[0036] The light fastness of the woven fabric of the present invention to ultraviolet carbon arc lamp light is preferably at least grade 4, and more preferably at least grade 5. For clothing to be worn outdoors as outerwear, a light fastness of less than grade 4 is not preferred because it will cause total or partial fading over time, resulting in a poor appearance.

[0037] <Water repellency of textiles> The woven fabric of the present invention is preferably subjected to a water-repellent treatment. When the initial water repellency is measured by the method described below, the initial water repellency of the woven fabric of the present invention is preferably grade 3 or higher. When the initial water repellency is grade 3 or higher, the woven fabric is lightly wetted even when it is wet with water in rainy weather or in a water area. From this viewpoint, it is preferable that the initial water repellency is grade 4 or higher, since the woven fabric is lightly wetted. The initial water repellency is the water repellency of the woven fabric before washing.

[0038] In addition, the woven fabric of the present invention preferably has a water repellency after washing of grade 2 or higher when measured by the method described below. When the water repellency after washing is grade 2 or higher, the woven fabric after washing maintains water repellency to the extent that the wetting is suppressed to about half. From this viewpoint, the water repellency is more preferably grade 3 or higher.

[0039] <Post-treatment of textiles> The woven fabric of the present invention can obtain the desired water repellency by selecting the water repellent. In addition, by using a crosslinking agent in the water repellent treatment, the water repellency after washing can be further improved. In addition, by using an antistatic agent in the water repellent treatment, antistatic properties can be imparted to the woven fabric. As the water repellent, a water repellent treatment agent for general fibers can be used, and for example, a fluorine-based water repellent made of a polymer having a perfluoroalkyl group, or a silicone-based, acrylic-based, or paraffin-based non-fluorine-based water repellent is preferably used.

[0040] In addition, as the crosslinking agent, a general crosslinking agent for fibers can be used, for example, a melamine-based crosslinking agent having methylolmelamine, an isocyanate-based crosslinking agent represented by a compound having one or more isocyanate groups or blocked isocyanate groups, etc. are listed. From the viewpoint of flexibility, an isocyanate-based crosslinking agent is preferred, and in particular, one having a blocked isocyanate group is preferred. Examples of the compound having one or more blocked isocyanate groups include compounds in which the isocyanate group of the compound having the isocyanate group is protected with a blocking agent. Examples of the blocking agent used at this time include organic blocking agents such as secondary or tertiary alcohols, active methylene compounds, phenols, oximes, and lactams, and bisulfites such as sodium bisulfite and potassium bisulfite. The above-mentioned crosslinking agents may be used alone or in combination of two or more types.

[0041] <Fabric uses and clothing> The woven fabric of the present invention has a function of suppressing shine, and therefore can be used in various applications where shine occurs due to friction of the woven fabric. Examples of applications include clothing, miscellaneous goods, shoes and bags, interior materials for vehicles, seating surfaces and headrests for chairs and sofas, floor mats, etc., which will be described later. In particular, it is preferable that the clothing of the present invention contains the above-mentioned woven fabric.

[0042] The clothing of the present invention can be suitably used for uniform clothing such as blazers, jackets, and slacks, formal clothing such as ceremonial vests, formal wear, and slacks, business clothing such as suits, coats, and slacks, casual clothing such as windbreakers, cloaks, capes, aprons, cloaks, slacks, jeans, and trousers, tops such as T-shirts, polo shirts, dress shirts, blouses, cache-coeurs, cut-and-sewn tops, vests, hoodies, sweatshirts, tank tops, and tube tops, dresses such as skirts, cocktail dresses, one-piece dresses, and gowns, and underwear. Among these, the woven fabric of the present invention can be suitably used as a fabric for clothing such as outerwear represented by uniform clothing, casual clothing, formal clothing, business clothing, and student clothing. The woven fabric of the present invention can be preferably used for the entire clothing, but it can also be preferably used for only a part of the local area such as elbows, buttocks, and knees, which are easily caused by friction when worn and become shiny.

[0043] In addition, the present invention can be suitably used for miscellaneous goods and shoe and bag applications, such as shoe uppers and trims, hats, bags, belts, scarves, neckties, and wallets.

[0044] <Fabric manufacturing method> Next, an example of a preferred method for producing the woven fabric of the present invention will be described, but the method is not limited thereto.

[0045] First, a polyester multifilament having a core-sheath structure is prepared by the following method. As a method for producing the polyester multifilament, as described above, the polyester multifilament may be a yarn obtained by subjecting a sea-island composite fiber to a sea-removal treatment, or a yarn obtained by combining a plurality of yarns into a textured yarn.

[0046] For example, when a sea-island composite fiber in which an easily soluble polymer is arranged in the sea part, a high shrinkage polymer in the center island part, and a normal polymer in the island part in the centrifugal part is formed by dissolving the sea part by an alkali weight reduction treatment during dyeing, the sheath yarn may be formed from a plurality of polymers, and in that case, the sheath yarn can be formed by using a plurality of polymers for the island part in the centrifugal part. In addition, the polymer composition is not particularly limited as long as it is a combination that causes a shrinkage difference by heat treatment, and a combination of polymers with different viscosities or melting points is possible, and from the viewpoint of easy control of the occurrence of crimp, a combination of polymers with different melting points is preferable. By using a combination of polymers with different melting points, the polymer with the lower melting point shrinks first when heat treatment is performed, so that a shrinkage difference between the polymers can be easily expressed. In addition, in the present invention, when the sheath yarn is formed from two-component polymers, the component with the higher shrinkage rate of the two components is defined as the high shrinkage polymer, and the component with the lower shrinkage rate is defined as the normal polymer.

[0047] Furthermore, when producing a multifilament using textured yarn, a core yarn having a larger fineness than the sheath yarn and a higher shrinkage rate than the sheath yarn and a sheath yarn having a smaller fineness than the core yarn and a lower shrinkage rate than the core yarn may be aligned and formed by air processing (interlace processing or taslan processing) or false twist processing. A more preferable method is a method using sea-island composite fibers, which can reduce protruding yarns that can cause hooks or zippers to get caught or cause pilling, and is also favorable from the viewpoint of productivity since it does not require yarn processing.

[0048] The method for weaving the woven fabric of the present invention is not particularly limited, and the fabric can be woven by a conventional method, for example, a method using a loom such as a water jet loom, an air jet loom, a rapier loom, or a jacquard loom.

[0049] The fabric obtained by the above weaving method can then be scoured, hot water treated, and dyed by the usual methods. The heat treatment accompanying these processes causes the core yarn, which is thicker than the sheath yarn and has a higher shrinkage rate than the sheath yarn, to shrink, causing the sheath yarn, which is thinner than the core yarn and has a lower shrinkage rate than the core yarn, to shrink, forming a bulge on the surface of the fabric. If the polyester multifilament constituting the above fabric contains sea-island composite fibers, it is necessary to carry out an alkali reduction treatment or the like to elute the sea component after the scouring treatment.

[0050] The woven fabric of the present invention may be subjected to finishing treatments for improving antistatic properties, flame retardancy, moisture absorption, antistatic properties, antibacterial properties, flexibility, etc., and other known post-treatments (including resin coating, film lamination, and other treatments for imparting functions, etc.), and the washing durability of functional finishing agents may be improved by using a crosslinking agent in combination. The water-repellent finishing process may be a bath treatment, a padding method, a spray method, a printing method, a coating method, a gravure method, etc., but is not particularly limited thereto, with the padding method being preferred in terms of penetrating the finishing agent into the interior of the woven fabric. EXAMPLES

[0051] The woven fabric of the present invention will be specifically described below with reference to examples, although the present invention is not limited to these.

[0052] The following measurements and evaluations were carried out for the examples and comparative examples.

[0053] A. Fineness The fineness was measured based on "8.3.1 Correct fineness (Method A)" ​​of JIS L 1013:2010 (Testing method for chemical fiber filament yarn).

[0054] B. Number of filaments The number of filaments in the multifilament was measured based on "8.4 Number of filaments" of JIS L 1013:2010 (Testing method for chemical fiber filament yarn).

[0055] C. Number of twists The number of twists of the multifilament yarn was measured based on "8.13 Number of twists" of JIS L 1013:2010 (Test method for chemical fiber filament yarn).

[0056] D. Twist modulus The twist factor K was calculated by applying the yarn fineness and the number of twists to Equation 1. K = T / (10000 / D) 1 / 2 (Formula 1) (K: twist coefficient, T: number of twists (T / m), D: fineness (dtex)).

[0057] E. Ratio of core yarn to sheath yarn in multifilament (number of core yarns: number of sheath yarns) For multifilaments with a sheath-core structure of woven fabrics, the number of each filament was measured using the method described above in B. The number of filaments in the sheath yarn was divided by the number of filaments in the core yarn to calculate the number ratio when the number of filaments in the core yarn was set at 1.

[0058] F. Yarn length and yarn length difference rate For multifilaments with a core-sheath structure in woven fabrics, the yarn length and yarn length difference rate were calculated using the following method. A 5 cm length of multifilament was cut from the woven fabric, and the core yarn and sheath yarn were each extracted. The "5.1 Initial Load" of JIS L 1013:2010 (Test Method for Chemical Fiber Filament Yarns) was applied, and the yarn lengths of the core yarn and sheath yarn were measured. The yarn length difference rate (%) between the core yarn and sheath yarn was then calculated using the following formula 3. Yarn length difference rate (%) = (sheath yarn length (mm) - core yarn length (mm)) / core yarn length (mm) × 100 (Equation 3).

[0059] G. Polymer Melting Point The melting point of the polymer was calculated for the multifilament sheath yarn by the following method. Approximately 5 mg of the multifilament sheath yarn was weighed, and a differential scanning calorimeter (DSC) Q2000 manufactured by TA Instruments was used to measure the DSC by heating from 0°C to 300°C at a heating rate of 16°C / min, and then holding at 300°C for 5 minutes. The apex of the melting peak observed during the heating process was taken as the melting point. When multiple melting peaks were observed, it was determined that multiple polymers were present, and the apex of each peak was taken as the melting point. Measurements were performed three times for each sample, and the average value was taken as the melting point.

[0060] H. Low pressure range compression ratio The test method of "8.20 Compressibility and compressive modulus" of JIS L 1096:2010 (Fabric test methods for woven and knitted fabrics) was applied, and the thickness of the woven fabric was measured with a lower limit pressure of 0.2 kPa and a constant pressure of 4.9 kPa. The low pressure range compressibility was calculated using the following formula 2. Cr=(T0-T1) / T0×100 (Formula 2) (Cr: compression rate in the low pressure region (%), T0: fabric thickness (mm) when a lower limit pressure of 0.2 kPa is applied, T1: fabric thickness (mm) when a constant pressure of 4.9 kPa is applied).

[0061] I. Initial water repellency The initial water repellency refers to the water repellency of the fabric before the washing treatment described in the next section. This initial water repellency was measured based on "7.2 Water repellency test (spray test)" of JIS L 1092 (2009) (Test method for waterproofing of textile products).

[0062] J. Water repellency after washing The post-wash water repellency was measured based on "7.2 Water repellency test (spray test)" in JIS L 1092:2009 (Test methods for waterproofing of textile products) after washing 20 times based on "Appendix F C4M method" in JIS L 1930:2014 (Test methods for home washing of textile products).

[0063] K. Shine Evaluation Using a Fabric Development Tests frosting tester, the sample was attached to the sample holder at the center of the top of the device, and the friction surface at the bottom of the device was measured at 0.33 N / cm 2 The fabric was rubbed for a certain period of time under a pressure of 10 ... The evaluation sample was rubbed, and the glossiness of the sample after rubbing was visually confirmed under a D65 light source and graded in comparison with the standard. If it was less glossy than the standard sample of grade 3 and more glossy than the standard sample of grade 5, it was rated as grade 4, and if it was less glossy than the standard sample of grade 1 and more glossy than the standard sample of grade 3, it was rated as grade 2.

[0064] L. Pilling The test was conducted based on "8.1.3 C Method" of JIS L 1076:2012 (Pilling test method for woven and knitted fabrics).

[0065] M.Lightness L * JIS Z8781-4:2013 (Colorimetry-Part 4: CIE 1976 L * a * b * L defined in "3.3 CIE1976 Lightness Index" of the Color Space * The value was measured using a Konica Minolta, Inc. multi-light source spectrophotometer (CM-3700d) with the total reflection method.

[0066] N. Light fastness The test was carried out based on JIS L 0842:2004 (Test method for color fastness to ultraviolet carbon arc lamp light).

[0067] [Example 1] We prepared normal PET containing 0.3 wt% titanium oxide as a semi-dull polymer (hereinafter referred to as P1), PET copolymerized with isophthalic acid (IPA) as a high-shrinkage polymer (hereinafter referred to as P2), and PET copolymerized with a compound copolymerized with 5-sodium sulfoisophthalic acid and polyethylene glycol (SSIA-PEG) as a readily soluble polymer (hereinafter referred to as P3).

[0068] These polymers were melted separately at 290°C, and then weighed out to a weight ratio of 60 / 30 / 10 P1 / P2 / P3. The polymers were fed into a spin pack equipped with a composite spinneret, and the polymers were discharged from the discharge hole. The discharged composite polymer stream was cooled and solidified, after which an oil agent was added, and the stream was taken up and drawn in a spinning machine to produce a sea-island composite fiber with 84 dtex-12 filaments. In the fiber cross section, the obtained sea-island composite fiber had eight flat segments with a side-by-side composite structure of the P1 and P2 polymers (P1 / P2) arranged around an eight-lobed segment formed by the high shrinkage polymer P2, and the periphery was surrounded by the easily soluble polymer P3.

[0069] A 1 / 3 twill fabric was obtained using a rapier loom with a round cross section yarn of P3 with untwisted and sized 56 dtex-24 filaments (56T-24F, hereinafter the same) as the warp yarn and the above sea-island composite fiber as the weft yarn, which was untwisted and arranged in two strands. The obtained fabric was scoured in a bath of 80°C for 20 minutes in an aqueous solution containing a surfactant at a bath ratio of 1:20 to the fabric. The fabric was then scoured in a bath of 80°C for 30 minutes in an aqueous solution containing 1% by weight of sodium hydroxide at a bath ratio of 1:20 to the fabric, to remove 99% or more by mass of the easily soluble polymer P3. The fabric was then treated in a bath of 130°C for 60 minutes in a batch dyeing machine at a bath ratio of 1:20 to the fabric, and then dry-heated and set using a pin tenter at 180°C for 1 minute with a tentering ratio of 5%.

[0070] Thereafter, the fabric was treated in a bath of 1:20 with an aqueous solution of Dianix Tuxedo Black F conc. Liquid (Dystar Co., Ltd., azo disperse dye) at 13% owf, 0.5 g / L of "IONET" (registered trademark) RAP-250 (Sanyo Chemical Industries Co., Ltd., leveling agent), and pH adjusted to 5.0 by adding acetic acid and sodium acetate as pH adjusters, at a temperature of 130°C for 60 minutes, and then rinsed with water. Next, the fabric was treated in a bath of 1:20 with an aqueous solution of 2.0 g / L of hydrosulfite and 2.0 g / L of caustic soda as reduction cleaning agents, at a temperature of 80°C for 20 minutes, and then rinsed with water and air-dried.

[0071] The fabric was then immersed in an aqueous solution containing 50 g / L of "Neoseed" (registered trademark) NR-158 (Nicca Chemical Co., Ltd., water repellent) (hereafter, water repellent A), 10 g / L of SU-268A (Meisei Chemical Industry Co., Ltd., isocyanate-based crosslinking agent) (hereafter, crosslinking agent a), and BG-290 (Nicca Chemical Co., Ltd., penetrating agent), and nipped with a mangle so that the amount of treatment solution adhered was 80%. Next, using a pin tenter, the fabric was treated with dry heat at 140°C for 2 minutes and dried. Furthermore, using a pin tenter, the fabric was treated with dry heat at 180°C for 1 minute and set.

[0072] The single yarn fineness of the core yarn in the weft multifilament of the obtained woven fabric was 2.8 dtex, and the single yarn fineness of the sheath yarn was 0.4 dtex, so that the sheath yarn was finer than the core yarn. The number of filaments in the core yarn was 24, and the number of filaments in the sheath yarn was 192, forming a multifilament having a core-sheath structure with a core-sheath ratio of 1:8. The yarn density at that time was 176 / 25.4 mm for the warp yarn and 128 / 25.4 mm for the weft yarn.

[0073] As shown in Table 1, the fabric composed of multifilament having a core-sheath structure had a yarn length difference of 10% between the core yarn and the sheath yarn of the weft yarn, and the core yarn was shorter than the sheath yarn due to shrinkage, and the core yarn was covered by the sheath yarn, so it was not exposed. Two peaks were confirmed in the polymer melting point of the sheath yarn of the multifilament having a core-sheath structure, 254°C and 232°C, respectively. The twist coefficient was 0, and the low pressure region compression rate was 21%, which were sufficiently high values ​​to disperse frictional forces. In addition, the initial water repellency was grade 4, and the water repellency after washing was grade 3, so it had good water repellency and washing durability. The shine property was grade 4, and it had high suppression performance against the occurrence of shine when worn for a long time. The pilling was size L, and it had high suppression performance against abrasion and snagging due to wearing. Lightness L * The value was 17, and the color development was without fading.

[0074] [Example 2] The same treatment as in Example 1 was carried out, except that the weft twist number was set to 200 T / m.

[0075] As shown in Table 1, the fabric composed of multifilaments with a core-sheath structure had a twist coefficient of 25 and a low pressure region compression rate of 17%, which were high enough to disperse frictional forces. The shine was grade 4, and the fabric had high performance in suppressing the occurrence of shine when worn for a long period of time.

[0076] [Example 3] The same treatment as in Example 1 was carried out, except that the weft twist number was set to 500 T / m.

[0077] As shown in Table 1, the fabric composed of multifilaments having a core-sheath structure had a twist coefficient of 62 and a low pressure region compression rate of 15%, which were moderate values ​​for dispersing frictional force. The shine property was grade 3, which was moderately effective in suppressing the occurrence of shine when worn for a long period of time.

[0078] [Example 4] The same treatment as in Example 1 was carried out, except that the twist number of the weft yarn was 800 T / m.

[0079] As shown in Table 1, the fabric composed of multifilament with a core-sheath structure had a twist count of 99 and a low pressure compression rate of 13%, indicating a decrease in the value indicating the dispersion of frictional force. Shininess was grade 2, indicating a decrease in the ability to suppress the occurrence of shine when worn for a long period of time.

[0080] [Comparative Example 1] The same treatment as in Example 1 was carried out, except that the twist number of the weft yarn was 1000 T / m.

[0081] As shown in Table 1, the fabric composed of multifilaments with a core-sheath structure had a twist count of 123 and a compression rate in the low pressure region of 9%, and showed a decrease in the value indicating the dispersibility of frictional force. The shine property was grade 1, and did not show any suppressive performance against the occurrence of shine when worn for a long period of time.

[0082] [Comparative Example 2] The spinning ratio of P1 / P2 / P3 was 45 / 45 / 10 by weight, and the obtained composite fiber had eight flat segments having a side-by-side composite structure of P1·P2 arranged on the outer periphery of an eight-lobed segment having a side-by-side composite structure of P1·P2, surrounded by P3. The same treatment as in Example 1 was carried out.

[0083] As the results are shown in Table 1, the woven fabric composed of multifilament with a core-sheath structure had a yarn length difference between the core yarn and sheath yarn of the weft of 0%, meaning that the core yarn was exposed and not covered by the sheath yarn. The compression rate in the low pressure region was 9%, and a decrease in the value indicating the dispersibility of frictional force was observed. The shine property was grade 1, and it did not show any ability to suppress the occurrence of shine when worn for a long period of time.

[0084] [Example 5] The spinning was carried out in the same manner as in Example 1, except that the weight ratio of P1 / P2 / P3 was 45 / 45 / 10, and the obtained composite fiber had eight flat segments of P1 arranged on the outer periphery of an eight-lobed segment of P2, which was surrounded by P3. The yarn length difference between the core yarn and the sheath yarn was 0.

[0085] As the results are shown in Table 1, the woven fabric composed of multifilament having a core-sheath structure had a yarn length difference between the core yarn and sheath yarn of the weft yarn of 22%, and the core yarn was shorter than the sheath yarn due to shrinkage, and the core yarn was covered by the sheath yarn, resulting in a structure in which it was not exposed. The polymer melting point of the sheath yarn of the multifilament having a core-sheath structure had one peak, at 254°C. The twist coefficient was 0, and the low pressure region compression rate was 31%, which were sufficiently high values ​​to disperse frictional forces. The shine property was grade 4, and the fabric had high suppression performance against the occurrence of shine when worn for a long period of time. The pilling property was size H, and a decrease in the suppression performance against chafing and snagging due to wear was observed.

[0086] [Comparative Example 3] An island-sea composite fiber of 84 dtex-24 filaments was produced by using P1 instead of P2 and weighing out P1 / P1 / P3 at a weight ratio of 45 / 45 / 10. The composite fiber obtained had a cross section in which eight flat-shaped segments formed from P1 were arranged on the outer periphery of an eight-lobe-shaped segment formed from P1, and P3 surrounded the periphery. The weft yarns of the obtained woven fabric were treated in the same manner as in Example 1, except that the core yarn had a single yarn fineness of 1.4 dtex and the sheath yarn had a single yarn fineness of 0.2 dtex, making the sheath yarn finer than the core yarn.

[0087] As the results are shown in Table 1, the woven fabric composed of multifilament having a core-sheath structure had a yarn length difference between the core yarn and sheath yarn of the weft yarn of 0%, and the core yarn was exposed and not covered by the sheath yarn. The polymer melting point of the sheath yarn of the multifilament having a core-sheath structure had one peak, at 254°C. The compression rate in the low pressure region was 9%, and a decrease in the value indicating the dispersibility of frictional force was observed. The shine property was Grade 1, and did not show any inhibitory performance against the occurrence of shine when worn for a long period of time. Lightness L * The value was 21, and due to the fineness of the yarn, the color had a faded appearance from the beginning.

[0088] [Comparative Example 4] Instead of the 84 dtex-12 filament sea-island composite fiber, an 84 dtex-24 filament yarn formed only from P1 was used, and the same treatment as in Example 1 was carried out, except that the bath treatment in an aqueous solution containing 1 wt% sodium hydroxide and the bath treatment at 130°C for 60 minutes in a batch dyeing machine were not carried out. The core yarn had 24 filaments, the sheath yarn had 24 filaments, and the single yarn fineness was 3.5 dtex for both the core yarn and the sheath yarn, with no difference in fineness, and a multifilament with a core / sheath ratio of 1:1 was formed.

[0089] The results are shown in Table 1. The compression rate in the low pressure region was 7%, and a decrease in the value indicating the dispersibility of frictional force was observed. Shininess was grade 1, and the product did not show any inhibitory performance against the occurrence of shine when worn for a long period of time.

[0090] [Example 6] A textured yarn was obtained by air entangling a 33 dtex-12 filament P2 yarn with a false twist of a 56 dtex-144 filament P1 yarn.

[0091] A 56 dtex-24 filament P1 round cross section yarn with no twist and size was used as the warp yarn, and the above textured yarn was used as the weft yarn in a non-twisted, two-stranded arrangement, and a 1 / 3 twill fabric was obtained using a rapier loom. The fabric obtained was treated in a bath containing a surfactant at a bath ratio of 1:20 with the fabric at 80°C for 20 minutes and scoured. Next, using a batch dyeing machine, the fabric was treated in a bath ratio of 1:20 with the fabric at 130°C for 60 minutes, and then dry-heated using a pin tenter at 180°C for 1 minute with a tentering ratio of 5%, and set.

[0092] Thereafter, the fabric was treated in a bath of 1:20 with an aqueous solution of Dianix Tuxedo Black F conc. Liquid (Dystar Co., Ltd., azo disperse dye) at 13% owf, 0.5 g / L of "IONET" (registered trademark) RAP-250 (Sanyo Chemical Industries Co., Ltd., leveling agent), and pH adjusted to 5.0 by adding acetic acid and sodium acetate as pH adjusters, at a temperature of 130°C for 60 minutes, and then rinsed with water. Next, the fabric was treated in a bath of 1:20 with an aqueous solution of 2.0 g / L of hydrosulfite and 2.0 g / L of caustic soda as reduction cleaning agents, at a temperature of 80°C for 20 minutes, and then rinsed with water and air-dried.

[0093] The fabric was then immersed in an aqueous solution containing 50 g / L of "NEOSEED" (registered trademark) NR-158 (Nicca Chemical Co., Ltd., water repellent), 10 g / L of SU-268A (Meisei Chemical Industry Co., Ltd., crosslinking agent), and BG-290 (Nicca Chemical Co., Ltd., penetrating agent), and nipped with a mangle so that the amount of treatment solution adhered was 80%. Next, the fabric was treated with dry heat at 140°C for 2 minutes using a pin tenter and dried. The fabric was further treated with dry heat at 180°C for 1 minute using a pin tenter and set.

[0094] The weft yarns of the obtained woven fabric had a core yarn with a single yarn fineness of 2.8 dtex and a sheath yarn with a single yarn fineness of 0.4 dtex, which made the sheath yarn finer than the core yarn. The number of filaments in the core yarn was 24 and the number of filaments in the sheath yarn was 288, forming a multifilament having a core-sheath structure with a core-sheath ratio of 1:12.

[0095] As shown in Table 2, the fabric composed of multifilament having a core-sheath structure had a yarn length difference of 15% between the core yarn and the sheath yarn of the weft yarn, and the core yarn was shorter than the sheath yarn due to shrinkage, and the core yarn was covered by the sheath yarn, resulting in a structure in which it was not exposed. The polymer melting point of the sheath yarn of the multifilament having a core-sheath structure had one peak, at 254°C. The twist coefficient was 0, and the low pressure region compression rate was 24%, which were sufficiently high values ​​to disperse frictional forces. In addition, the initial water repellency was grade 4, and the water repellency after washing was grade 3, indicating good water repellency and washing durability. The shine property was grade 4, indicating high suppression performance against the occurrence of shine when worn for a long period of time. The pilling was size M, indicating moderate suppression performance against abrasion and snagging due to wearing. Lightness L * The color developed was 19 and had no fading.

[0096] [Comparative Example 5] The same treatment as in Example 6 was carried out, except that the weft twist number was 1000 T / m.

[0097] As shown in Table 2, the fabric composed of multifilaments with a core-sheath structure had a twist count of 133 and a compression rate in the low pressure region of 9%, and showed a decrease in the value indicating the dispersion of frictional force. The shine property was grade 1, and did not show any suppression performance against the occurrence of shine when worn for a long period of time.

[0098] [Example 7] The same processing as in Example 6 was carried out, except that a textured yarn was obtained by air entangling one 33 dtex-12 filament P2-used yarn made of a high shrinkage polymer with two false-twisted 56 dtex-144 filament semi-dull polymer-used yarns. The weft yarn of the obtained woven fabric had 12 filaments in the core yarn and 288 filaments in the sheath yarn, forming a multifilament having a core-sheath structure with a core-sheath ratio of 1:24.

[0099] As shown in Table 2, the shine was graded at level 4, demonstrating high performance in suppressing shine when worn for extended periods. *The value was 21, and the fine yarn covered the thick yarn, resulting in a faded color from the beginning.

[0100] [Comparative Example 6] The same processing as in Example 6 was carried out, except that a textured yarn was obtained by air entangling one 33 dtex-12 filament P2 high shrinkage polymer yarn with three false twisted 56 dtex-144 filament semi-dull polymer yarns. The weft yarn of the obtained woven fabric had 12 filaments in the core yarn and 432 filaments in the sheath yarn, forming a multifilament having a core-sheath structure with a core-sheath ratio of 1:36.

[0101] As shown in Table 2, the shine was graded at level 4, demonstrating high performance in suppressing shine when worn for extended periods. * The value was 25, and the fine yarn completely covered the thick yarn, resulting in a cloudy white color from the beginning.

[0102] [Example 8] The same treatment as in Example 1 was carried out, except that 50 g / L of a fluorine-based water repellent "UNIDYNE" (registered trademark) TG-5546 (Daikin Corporation, water repellent) having a perfluoroalkyl group with a carbon number of 6 or less (hereinafter referred to as water repellent B) was used instead of water repellent A, and 3 g / L of a melamine-based crosslinking agent having trimethylol melamine "AMIDIA" (registered trademark) M-3 (DIC Corporation, crosslinking agent) (hereinafter referred to as crosslinking agent b) was used instead of crosslinking agent a.

[0103] As shown in Table 2, the fabric composed of multifilaments with a core-sheath structure had a low pressure compression rate of 12%, indicating a decrease in the value indicating the dispersibility of frictional force. The shine was grade 3, indicating a moderate level of ability to suppress the occurrence of shine when worn for an extended period of time. In addition, the initial water repellency was grade 4, and the water repellency after washing was grade 2, indicating a decrease in washing durability.

[0104] [Example 9] The same treatment as in Example 2 was carried out, except that no crosslinking agent was used.

[0105] As shown in Table 2, the initial water repellency was grade 4, and the water repellency after washing was grade 1, showing no durability to washing. The shine resistance was grade 4, showing high performance in suppressing the occurrence of shine when worn for a long period of time.

[0106] [Example 10] The same treatment as in Example 2 was carried out, except that the amount of crosslinking agent a used was increased to 15 g / L.

[0107] The results are shown in Table 2. The initial water repellency was grade 4, and the water repellency after washing was grade 4, indicating good water repellency and washing durability. The shine resistance was grade 2, indicating a decrease in the ability to inhibit shine when worn for a long period of time.

[0108] [Example 11] The same treatment as in Example 1 was carried out, except that 3 g / L of crosslinking agent b was used instead of crosslinking agent a.

[0109] The results are shown in Table 2. The initial water repellency was grade 4, and the water repellency after washing was grade 3, indicating good water repellency and washing durability. The shine resistance was grade 2, indicating a decrease in the ability to inhibit shine when worn for a long period of time.

[0110] [Example 12] The same process as in Example 2 was carried out, except that the sea-island composite fiber was used as the warp yarn, with a twist number of 200 T / m and two parallel fibers, and a non-twisted, unsized, 56 dtex-24 filament round cross section yarn using P3 was used as the weft yarn, and a 3 / 1 twill fabric was obtained using an air jet loom.

[0111] As the results are shown in Table 3, the woven fabric composed of multifilament with a core-sheath structure had a yarn length difference between the core yarn and sheath yarn of the weft yarn of 10%, and the core yarn had shrunk to become shorter than the sheath yarn, resulting in a structure in which the core yarn was covered by the sheath yarn and was not exposed. The twist coefficient was 25 and the low pressure region compression rate was 17%, which were sufficiently high values ​​to disperse frictional forces. The shine property was grade 4, and the fabric had high performance in suppressing the occurrence of shine when worn for long periods of time.

[0112] [Example 13] The same treatment as in Example 12 was carried out, except that the warp twist number was set to 500 T / m.

[0113] As shown in Table 3, the fabric composed of multifilaments having a core-sheath structure had a low pressure compression rate of 15%, which was a medium value for dispersing frictional force. The shine property was grade 3, which was a medium level of performance in suppressing the occurrence of shine when worn for a long period of time.

[0114] [Example 14] The same treatment as in Example 12 was carried out, except that the weave was changed to 2 / 2 twill. The results are shown in Table 3. The compression ratio in the low pressure region was 14%, which was a moderate value for dispersing frictional force. The shine resistance was grade 3, which was a moderate level of performance in suppressing the occurrence of shine when worn for a long period of time. [Example 15] The same processing as in Example 1 was carried out, except that Dianix Tuxedo Black F conc. Liquid (Dystar Co., Ltd., azo-based disperse dye) was used instead of 13% owf, and Dianix Navy S-2G (Dystar Co., Ltd., azo-based disperse dye) was used at 4% owf, and Dianix Navy AM-G (Dystar Co., Ltd., quinone-based disperse dye) was used at 6% owf.

[0115] The results are shown in Table 3. * The colorfastness was 18 and the lightfastness was 5, demonstrating high color development and high light fastness. [Example 16] The same treatment as in Example 1 was carried out, except that Dianix Navy S-2G (Dystar Co., Ltd., azo-based disperse dye) was used at 6% owf and Dianix Navy AM-G (Dystar Co., Ltd., quinone-based disperse dye) was used at 4% owf in combination.

[0116] The results are shown in Table 3. * The colorfastness was 18 and the lightfastness was 5, demonstrating high color development and high light fastness. [Example 17] The same treatment as in Example 1 was carried out, except that Dianix Navy S-2G (Dystar Co., Ltd., azo-based disperse dye) was used at 8% owf and Dianix Navy AM-G (Dystar Co., Ltd., quinone-based disperse dye) was used at 2% owf in combination.

[0117] The results are shown in Table 3. * The colorfastness was 17 and the lightfastness was grade 4, showing high color development, but showing a decrease in lightfastness compared to Example 1. [Example 18] The same treatment as in Example 1 was carried out, except that Dianix Navy AM-G (Dystar Co., Ltd., quinone-based disperse dye) was used alone at 10% owf.

[0118] The results are shown in Table 3. * The color fastness was 20, which indicated a decrease in color development compared to Example 1. Furthermore, the light fastness was grade 5, which indicated high light fastness.

[0119] [Table 1]

[0120] [Table 2]

[0121] [Table 3]

[0122] Although the present invention has been described in detail and with reference to specific embodiments as shown above, it is clear to those skilled in the art that various changes and modifications can be made without departing from the spirit of the present invention. This application is based on a Japanese patent application filed on March 14, 2023, the contents of which are incorporated herein by reference. [Industrial Applicability]

[0123] The woven fabric of the present invention can suppress the occurrence of shine even when worn for a long period of time. Such a woven fabric can be used for clothing and textile products, and can be suitably used for clothing such as outerwear, such as uniform clothing, casual clothing, formal clothing, business clothing, and student clothing, which are worn for a long period of time.

Claims

1. The polyester multifilament has a core-sheath structure including a core yarn and a sheath yarn, The core yarn has a length shorter than that of the sheath yarn, The sheath yarn has a finer thread size than the core yarn, the ratio of the number of the core yarn to the number of the sheath yarn (number of the core yarn:number of the sheath yarn) is 1:6 to 1:24; The woven fabric is characterized in that the twist coefficient K calculated from the number of twists T of the polyester multifilament and the fineness D of the multifilament by the following formula 1 is 0 to 100. K=T / (10000 / D) 1/2 (Formula 1) (K: twist coefficient, T: number of twists (T / m), D: fineness (dtex))

2. The woven fabric of claim 1 , wherein the sheath yarn is formed from two types of polyester.

3. 3. The woven fabric according to claim 1, wherein the sheath yarn has a single yarn fineness of 0.1 dtex or more and 2.0 dtex or less.

4. 3. The woven fabric according to claim 1 or 2, wherein the warp or weft yarns are floating yarns, and the polyester multifilament having a core-sheath structure is arranged as a floating yarn.

5. 3. The woven fabric according to claim 1, which has an initial water repellency of grade 3 or higher.

6. The woven fabric according to claim 1 or 2, wherein the low pressure region compression rate Cr calculated by the following formula 2 is 5% or more and 30% or less. Cr = (T 0 -T 1 ) / T 0 ×100 (Formula 2) (Cr: low pressure region compression ratio (%), T 0 : Fabric thickness (mm) when a lower limit pressure of 0.2 kPa is applied, T 1 : Fabric thickness (mm) when a constant pressure of 4.9 kPa is applied

7. 3. The woven fabric according to claim 1, which has a light fastness of grade 4 or higher when measured with an ultraviolet carbon arc lamp.

8. The woven fabric according to claim 1 or 2, comprising an azo-based disperse dye and a quinone-based disperse dye, wherein the content of the quinone-based disperse dye relative to the total content of the azo-based disperse dye and the quinone-based disperse dye is 30% by mass or more and 70% by mass or less.

9. A garment comprising the fabric according to claim 1 or 2.

Citation Information

Patent Citations

  • Shining preventing fabric

    JP1989156542A

  • Bulky composite false twist textured yarn and its production

    JP2000314038A

Cited By

  • Polyester core-sheath blended yarns and woven / knitted fabrics

    JP2026161940A