Optical member, image capturing device module, and image display device module

A transparent substrate with a fine uneven structure film and adhesive layer addresses reflection issues in both visible and near-infrared light regions, improving visibility and sensitivity in optical devices.

JP2024132915APending Publication Date: 2024-10-01MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2024027451
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2024-02-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Conventional antireflection techniques fail to prevent reflection in both visible light and near-infrared light transmission regions, leading to decreased visibility and detection sensitivity in optical devices with both types of sensors on a transparent substrate.

Method used

A transparent substrate with a film having a fine uneven structure on its surface, where the average distance between convex portions is less than the wavelength of visible light, covering both visible and near-infrared light transmission regions, and an adhesive layer to secure the film, achieving a reflectance of 0.5% or less in the visible light region and 5.0% or less in the near-infrared region.

Benefits of technology

The solution effectively prevents reflection in both visible and near-infrared light transmission regions, enhancing visibility and detection sensitivity by suppressing reflections, flare, and ghosts in optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132915000001_ABST
    Figure 2024132915000001_ABST
Patent Text Reader

Abstract

To provide an optical member capable of preventing reflection in both a visible light transmission area and near-infrared light transmission area.SOLUTION: An optical member 10A according to an exemplary embodiment comprises a transparent substrate 1 having a visible light transmission area 3 and near-infrared light transmission area 5 in the same plane, and a film 7 having a fine concavo-convex structure provided on a surface thereof, with an average inter-protrusion distance of less than or equal to a visible light wavelength, the film 7 being disposed on a surface 1a side of the transparent substrate 1 to cover both the visible light transmission area 3 and the near-infrared light transmission area 5.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical member, an imaging device module, and an image display device module. [Background technology]

[0002] A fine uneven structure having a periodic interval equal to or less than the wavelength of visible light exhibits an anti-reflection effect, a lotus effect, etc. In particular, a fine uneven structure called a moth-eye structure can be an effective anti-reflection means because the refractive index increases continuously from that of air to that of the material of the article (for example, Patent Documents 1 and 2).

[0003] Patent Document 1 discloses an infrared sensor cover having a substrate and an anti-reflection layer provided on at least one surface of the substrate. Patent Document 2 discloses an anti-reflective article having optical transparency. The anti-reflective article has a plurality of protrusions on a first surface located on the viewing side and a second surface opposite to the first surface. The average distance between the protrusions is 400 nm or less, the ratio (H1 / W1) of the height H1 of the protrusions on the first surface to the width W1 of the bottom of the protrusions is 1.3 or more, and the ratio (H2 / W2) of the height H2 of the protrusions on the second surface to the width W2 of the bottom of the protrusions is greater than H1 / W1.

[0004] Incidentally, a transparent front panel made of resin, glass or the like is often used to protect optical devices such as visible light cameras, displays, and near-infrared sensors. For example, Patent Document 3 discloses a transparent substrate having a light-shielding region in the peripheral portion of one of the main surfaces of the transparent substrate. The light-shielding region includes a first light-shielding region and a second light-shielding region. The transparent substrate is proposed to obtain a display device with excellent design by making the boundary between these regions unclear. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-124279 A [Patent Document 2] International Publication No. 2010 / 150514 [Patent Document 3] International Publication No. 2018 / 105602 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, an increasing number of optical devices, such as smartphones, have a visible light camera, a display, and a near-infrared sensor on the same surface of a transparent substrate. However, the formation of an air gap between the front panel and a visible light camera, display, near-infrared sensor, etc. causes interface reflection, resulting in reduced visibility and detection sensitivity. Conventional anti-reflection technologies cannot prevent reflection in both the visible light transmission range and the near-infrared light transmission range.

[0007] An object of the present invention is to provide an optical member capable of preventing reflection in both the visible light transmission range and the near-infrared light transmission range of a transparent substrate. [Means for solving the problem]

[0008] The present invention has the following aspects. [1] A transparent substrate having a visible light transmission range and a near-infrared light transmission range in the same plane; a film having a fine uneven structure on its surface, the average distance between convex portions being equal to or less than the wavelength of visible light; having An optical member, wherein the film is disposed on at least one surface side of the transparent substrate so as to cover both the visible light transmission region and the near-infrared light transmission region. [2] The luminous reflectance of the film is 0.5% or less, and The optical member according to [1], wherein the reflectance of the film at a wavelength of 900 nm is 1.0% or less. [3] The luminous reflectance of the film is 0.5% or less, and The optical member according to [1] or [2], wherein the reflectance of the film at 1550 nm is 5.0% or less. [4] The optical member according to any one of [1] to [3], further comprising an adhesive layer between the near-infrared light transmitting region of the transparent substrate and the film. [5] A photographing device module including a photographing device and a protective member, The protective member is an optical member according to any one of [1] to [4], an imaging device module, the imaging device being disposed in the visible light transmission area; [6] An image display device module including an image display device and a protective member, The protective member is an optical member according to any one of [1] to [4], The image display device module, wherein the image display device is disposed in the visible light transmission region. Effect of the Invention

[0009] According to the present invention, there is provided an optical member capable of preventing reflection in both the visible light transmission region and the near-infrared light transmission region. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a top view illustrating an example of an optical member. [Diagram 2] 2 is a cross-sectional view of the optical member shown in FIG. 1 along line II-II. [Diagram 3] FIG. 2 is a top view illustrating an example of an optical member. [Figure 4] 4 is a cross-sectional view of the optical member shown in FIG. 3 along line IV-IV. [Diagram 5] FIG. 2 is a top view illustrating an example of an optical member. [Figure 6] 6 is a cross-sectional view of the optical member shown in FIG. 5 along the line VI-VI. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The meanings of the terms are as follows: "Visible light" means light with a wavelength in the range of 400 to 780 nm. "Near infrared light" means light with a wavelength in the range of 800 to 2500 nm. The symbol "~" indicating a range of numerical values ​​means that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0012] Hereinafter, some embodiments of the present invention will be described with reference to the drawings. However, the following description is a representative example, and the present invention is not limited to the following description. The dimensional ratios in each drawing are for the convenience of explanation and may differ from the actual ones. In the following drawings, the same components are indicated by the same reference numerals, and the explanation of the overlapping components may be omitted.

[0013] The optical component 10A shown in Figures 1 and 2 has a transparent substrate 1 in which a visible light transmission range 3 and a near-infrared light transmission range 5 are in the same plane, a film 7 having a fine uneven structure on its surface in which the average spacing between convex portions is equal to or less than the wavelength of visible light, and an adhesive layer 9 between the transparent substrate 1 and the film 7. The film 7 is disposed on at least one surface 1 a of the transparent substrate 1 so as to cover both the visible light transmission region 3 and the near-infrared light transmission region 5 . In another example of the optical member, the film 7 may be disposed on the other surface 1b side of the transparent substrate 1. In still another example of the optical member, the film 7 may be disposed on both the surface 1a and the surface 1b of the transparent substrate 1.

[0014] (Transparent substrate) The material of the transparent substrate is not particularly limited as long as it transmits visible light, infrared light, and near-infrared light. Examples include resin materials such as acrylic resin, polycarbonate resin, styrene resin, cellulose resin, polyester resin, and polyolefin resin, and glass. Among them, glass and resin are preferred because they have excellent transmittance for visible light, infrared light, and near-infrared light. Glass is more preferred in terms of smoothness and less optical distortion. Resin is more preferred in terms of moldability to curved surfaces and light weight.

[0015] 1 and 2, in the optical component 10A, a printing process is partially performed on one surface 1a of the transparent substrate 1. The printed layer 8 partially provided on the surface 1a of the transparent substrate 1 is visible as shown in FIG. 1, and therefore can impart design features to the optical component 10A. The printed layer 8 between the transparent substrate 1 and the film 7 can be protected by adhering the transparent substrate 1 and the film 7 with the adhesive layer 9. This improves the durability of the printed layer 8.

[0016] In addition, the surface of the transparent substrate may be subjected to a coating treatment, a corona treatment, etc., for the purpose of improving properties such as adhesion, scratch resistance, etc. The shape of the transparent substrate can be appropriately selected depending on the application of the optical member.

[0017] The transparent substrate has a visible light transmission region and a near-infrared light transmission region in the same plane. In the optical member 10A, a visible light transmission region 3 and a near-infrared light transmission region 5, which are partitioned in the same plane, are formed on the surface 1b of the transparent substrate 1. The visible light transmission region and the near-infrared light transmission region can be formed in the same plane of the transparent substrate, for example, by partially providing a light-shielding layer that transmits near-infrared light on a visible light-transmitting transparent substrate.

[0018] 2, in the optical member 10A, a light-shielding layer 4 is partially provided on one surface 1a of the transparent substrate 1, thereby forming a visible light transmission region 3 and a near-infrared light transmission region 5. The light-shielding layer 4 partially provided on the surface 1a of the transparent substrate 1 is visually recognized as a near-infrared light transmission region 5 as shown in FIG. The light-shielding layer may be a single-layer structure or a multi-layer structure made up of a plurality of kinds of layers. The light-shielding layer may be formed on one side of the transparent substrate, or on both sides of the transparent substrate.

[0019] The light-shielding layer can be formed by curing a resin composition containing an infrared-transmitting material on a transparent substrate. The infrared-transmitting material can be a pigment having infrared-transmitting ability. The pigment can be either an inorganic pigment or an organic pigment. Examples of inorganic pigments include iron oxide, titanium oxide, and composite oxides. Examples of organic pigments include metal complex pigments such as phthalocyanine pigments, anthraquinone pigments, and azo pigments. The pigment may be used alone or in combination of two or more kinds. The content of the infrared transmitting material in the light-shielding layer can be freely changed according to the desired optical properties.

[0020] Depending on the curing method, the resin composition may be a photocurable type, a thermosetting type, a type that is cured by mixing two or more liquids, or a type that is cured by drying a solvent. Examples of the resin component include varnish (oil varnish and / or alcohol varnish), paint resin, general-purpose plastic, or engineering plastic. The resin component is preferably a material that absorbs little infrared rays. Examples of the paint resin include acrylic resin, polyurethane resin, acrylic silicone resin, silicone resin, and fluororesin. Examples of the general-purpose plastic or engineering plastic include ABS resin, polycarbonate resin, unsaturated polyester resin, polypropylene resin, modified PPO resin, and polyamide resin. The resin composition may contain a solvent or a dispersion medium. These materials are appropriately blended in the resin composition to improve the workability of applying the resin composition to a transparent substrate.

[0021] The thickness of the light-shielding layer is preferably 0.5 to 20 μm, more preferably 2 to 10 μm. When the thickness of the light-shielding layer is equal to or greater than the lower limit of the above-mentioned numerical range, unevenness in transmittance can be suppressed. When the thickness of the light-shielding layer is equal to or less than the upper limit of the above-mentioned numerical range, peeling between layers due to stress can be easily prevented.

[0022] The thickness of the transparent substrate excluding the light-shielding layer is preferably 1 to 50 mm, more preferably 2 to 30 mm. When the thickness of the transparent substrate is equal to or greater than the lower limit of the above-mentioned numerical range, an optical member having excellent mechanical strength is easily obtained. When the thickness of the transparent substrate is equal to or less than the upper limit of the above-mentioned numerical range, an optical member having excellent visibility is easily obtained.

[0023] The shape of the transparent substrate is not particularly limited, and may be a flat plate, a curved surface, or a flexible shape that can follow a curved surface.

[0024] (Film with a fine uneven structure) The film 7 has a fine uneven structure, a so-called moth-eye structure, on its surface 7a, in which the average distance between convex portions is equal to or less than the wavelength of visible light. The fine uneven structure imparts anti-reflection performance to the film 7. The fine uneven structure is made up of a plurality of convex portions and concave portions formed between the convex portions.

[0025] The average interval between adjacent convex portions of the fine uneven structure is equal to or less than the wavelength of visible light. The average interval is preferably 20 nm to 400 nm, more preferably 80 nm to 250 nm. When the average interval between adjacent convex portions of the fine uneven structure is 20 nm or more, it is easy to form convex portions when forming the convex portions by transferring a plurality of pores of anodized porous alumina. When the average interval between adjacent convex portions of the fine uneven structure is 400 nm or less, it is possible to suppress the voltage for increasing the pore interval when forming the convex portions by transferring a plurality of pores of anodized porous alumina, and it is easy to industrially manufacture anodized porous alumina. When the average interval between adjacent convex portions of the fine uneven structure is 250 nm or less, it is possible to suppress the generation of unnecessary diffracted light. The average distance between adjacent protrusions is determined by measuring the distance between adjacent protrusions (the distance from the center of a protrusion to the center of an adjacent protrusion) at 10 random points using an electron microscope and averaging these values.

[0026] The average height of the convex portions is preferably 150 nm to 1000 nm, more preferably 300 nm to 800 nm, and even more preferably 350 nm to 600 nm. When the average height of the convex portions is 150 nm or more, the increase in the minimum reflectance and the reflectance of visible light and near infrared light can be suppressed, and the antireflection performance is excellent. When the average height of the convex portions is 300 nm or more, the increase in the reflectance of near infrared light around 900 nm can be suppressed. Furthermore, when the average height of the convex portions is 350 nm or more, the increase in the reflectance of near infrared light up to around 1550 nm can be suppressed. When the average height of the convex portions is 1000 nm or less, the convex portions are easy to form, and the convex portions have excellent scratch resistance. The average height of the convex portions is determined by measuring the vertical distance between the top of a convex portion and the bottom of an adjacent concave portion at 10 random points using an electron microscope, and averaging these values.

[0027] The aspect ratio of the convex portions (average height of the convex portions / average distance between adjacent convex portions) is preferably 0.8 to 5.0, more preferably 1.2 to 4.0, and even more preferably 1.5 to 3.0. When the aspect ratio of the convex portions is 0.8 or more, the antireflection performance is excellent. Furthermore, when the aspect ratio of the convex portions is 5.0 or less, the convex portions are easy to form and have excellent scratch resistance.

[0028] Examples of the shape of the convex portion include a cone shape, a pyramid shape, a bell shape, and a cylinder shape. One of these convex shapes may be used alone, or two or more of them may be used in combination. Among these convex shapes, a shape in which the cross-sectional area of ​​the convex portion in the direction perpendicular to the height direction increases continuously from the apex in the depth direction is preferred, since it is possible to continuously increase the refractive index from the air to the surface of the material on which the fine uneven structure is formed, thereby achieving anti-reflection performance that combines low reflectance and low wavelength dependency, and a cone shape, a pyramid shape, and a bell shape are more preferred. The convex portion may be a single convex portion formed by merging a plurality of fine convex portions.

[0029] The luminous reflectance of the film is preferably 0.5% or less, more preferably 0.4% or less, even more preferably 0.3% or less, and particularly preferably 0.2% or less. When the luminous reflectance of the film is equal to or less than the upper limit, reflection in the visible light transmission range can be sufficiently prevented. The luminous reflectance of the film is a value determined by the method described in the Examples.

[0030] The reflectance at a wavelength of 900 nm is preferably 1.0% or less, more preferably 0.8% or less, even more preferably 0.5% or less, and particularly preferably 0.3% or less. When the reflectance at a wavelength of 900 nm of the film is the upper limit value or less, reflection in the near-infrared light transmission range can be sufficiently prevented. The reflectance at a wavelength of 900 nm is a value determined by the method described in the Examples.

[0031] The reflectance at a wavelength of 1550 nm is preferably 5.0% or less, more preferably 3.0% or less, even more preferably 2.0% or less, and particularly preferably 1.0% or less. When the reflectance at a wavelength of 1550 nm of the film is the upper limit value or less, reflection in the near-infrared light transmission range can be sufficiently prevented. The reflectance at a wavelength of 1550 nm is a value determined by the method described in the examples.

[0032] In a preferred embodiment, the film has a luminous reflectance of 0.5% or less, and a reflectance at a wavelength of 900 nm of 1.0% or less. In another preferred embodiment, the film has a luminous reflectance of 0.5% or less and a reflectance at 1550 nm of 5.0% or less.

[0033] The thickness of the film is preferably 10 to 500 μm, more preferably 30 to 100 μm. When the thickness of the film is equal to or greater than the lower limit of the above-mentioned numerical range, an optical component having excellent mechanical strength is easily obtained. When the thickness of the film is equal to or less than the upper limit of the above-mentioned numerical range, an optical component having excellent visibility is easily obtained.

[0034] Examples of methods for forming the fine uneven structure include the following methods A1 to A3. Method A1: A method in which a microrelief structure is formed directly on the surface of a substrate by injection molding or press molding using a mold having an inverted structure of the microrelief structure on its surface. Method A2: A method in which an active energy ray-curable composition is sandwiched between a mold having an inverted structure of a microrelief structure and a substrate, the active energy ray-curable composition is cured to form a cured resin layer, and then the cured resin layer and the mold are separated. Method A3: A method in which an active energy ray-curable composition is sandwiched between a mold having an inverted structure of a fine relief structure and a substrate, the fine relief structure of the mold is transferred to the active energy ray-curable composition, the mold is then separated, and the active energy ray-curable composition is cured to form a cured resin layer. Among the methods for producing a fine concave-convex structure, methods A2 and A3 are preferred, and method A2 is more preferred, because they are excellent in transferability of the fine concave-convex structure and have a high degree of freedom in surface composition.

[0035] Examples of the mold include a mold having a microrelief structure formed on its surface by lithography, a mold having a microrelief structure formed on its surface by laser processing, a mold having an anodized porous alumina having a plurality of pores formed on its surface, and a replica mold obtained by replicating a mother mold having a microrelief structure by electroforming or the like. Among these molds, a mold having an anodized porous alumina having a plurality of pores formed on its surface is preferred because it has excellent anti-reflection performance and is easy to form a large-area microrelief structure at low cost.

[0036] Examples of the lithography method include electron beam lithography and laser interference lithography. Examples of methods for producing a mold having an inverted microrelief structure on its surface by lithography include a method in which a photoresist film is applied to the surface of a substrate, and the photoresist film is exposed to an ultraviolet laser, an electron beam, an X-ray, or the like, and then developed to obtain a mold having a microrelief structure on its surface consisting of a resist pattern; and a method in which the substrate is selectively etched by dry etching or the like through the resist pattern, and the resist pattern is removed to obtain a mold having a microrelief structure formed directly on the surface of the substrate.

[0037] Examples of methods for manufacturing a mold having anodized porous alumina with a plurality of pores formed on its surface include a method in which aluminum is anodized at a predetermined voltage using an electrolyte such as oxalic acid, sulfuric acid, or phosphoric acid.

[0038] As a method for producing a mold having anodized porous alumina formed on the surface, for example, there is a method in which aluminum is anodized at a predetermined voltage using oxalic acid, sulfuric acid, phosphoric acid or the like as an electrolyte. According to a method of anodizing aluminum at a predetermined voltage using an electrolyte such as oxalic acid, sulfuric acid, or phosphoric acid, it is possible to form pores in high purity aluminum that are not rectangular in cross section but triangular or bell-shaped by combining anodizing and pore size expansion treatment. Furthermore, it is possible to make the angle of the innermost part of the pores sharp by appropriately adjusting the time, number of times, conditions, etc. of anodizing and pore size expansion treatment. An example of a method for producing a mold having anodized porous alumina formed on its surface is the method described in JP 2015-129706 A.

[0039] Examples of the shape of the mold include a flat plate, a belt, a roll, etc. Among these mold shapes, the belt and roll are preferred because they allow the fine concave-convex structure to be transferred continuously and are excellent in productivity of the substrate.

[0040] The fine unevenness is preferably made of a cured resin layer, since it is possible to form the fine unevenness more easily. The cured resin layer is a layer made of a cured product of an active energy ray-curable composition.

[0041] The active energy ray-curable composition is a composition that undergoes a polymerization reaction and is cured when irradiated with active energy rays. Examples of active energy rays include visible light, ultraviolet light, electron beams, plasma, heat rays (infrared rays, etc.), etc. Among these active energy rays, ultraviolet light and electron beams are preferred, and ultraviolet light is more preferred, since they provide excellent curing properties for the active energy ray-curable composition.

[0042] The active energy ray-curable composition preferably contains a polymerizable compound, a polymerization initiator, and, if necessary, other additives.

[0043] Examples of the polymerizable compound include monomers, oligomers, reactive polymers, etc., each of which contains at least one of a radical polymerizable bond and a cationic polymerizable bond in the molecule. These polymerizable compounds may be used alone or in combination of two or more.

[0044] Examples of the monomer having a radical polymerizable bond include monofunctional monomers having a (meth)acryloyl group, a vinyl group, etc., and polyfunctional monomers having a (meth)acryloyl group, a vinyl group, etc. These monomers having a radical polymerizable bond may be used alone or in combination of two or more kinds. (Meth)acrylic is a general term for acrylic and methacrylic.

[0045] Examples of the monomer having a cationic polymerizable bond include monomers having an epoxy group, an oxetanyl group, an oxazolyl group, a vinyloxy group, etc. These monomers having a cationic polymerizable bond may be used alone or in combination of two or more kinds.

[0046] Examples of oligomers or reactive polymers containing at least one of radically polymerizable bonds and cationic polymerizable bonds in the molecule include unsaturated polyester compounds such as condensates of unsaturated dicarboxylic acids and polyhydric alcohols; polyester (meth)acrylates; polyether (meth)acrylates; polyol (meth)acrylates; epoxy (meth)acrylates; urethane (meth)acrylates; cationic polymerization type epoxy compounds; homopolymers or copolymers of monomers having the above radically polymerizable bonds in their side chains, etc. These oligomers or reactive polymers containing at least one of radically polymerizable bonds and cationic polymerizable bonds in the molecule may be used alone or in combination of two or more.

[0047] Examples of the polymerization initiator include a photopolymerization initiator, an electron beam polymerization initiator, and a thermal polymerization initiator. These polymerization initiators may be used alone or in combination of two or more. The other additives are not particularly limited, but examples thereof include non-reactive polymers, antioxidants, release agents, lubricants, plasticizers, antistatic agents, light stabilizers, flame retardants, flame retardant assistants, polymerization inhibitors, ultraviolet absorbers, fillers, silane coupling agents, reinforcing agents, inorganic fillers, and impact resistance modifiers. The other additives may be used alone or in combination of two or more.

[0048] When imparting water repellency to the surface of the fine unevenness structure, it is preferable to use a fluorine-containing compound or a silicone-based compound as an active energy ray curable composition capable of forming a hydrophobic material. The term "imparting water repellency" refers to making the contact angle between the fine unevenness structure and water 120° or more. If the material is water repellent, when the material is used as an optical material for a photographing device or an image display device, even if clouding occurs due to temperature changes or in a high humidity environment, the material can be dried quickly to suppress a decrease in detection sensitivity and visibility.

[0049] When imparting hydrophilicity to the surface of the fine unevenness structure, it is preferable to use a combination of a tetrafunctional or higher polyfunctional (meth)acrylate and a difunctional or higher hydrophilic (meth)acrylate as an active energy ray curable composition capable of forming a hydrophilic material. The term "hydrophilicity" refers to making the contact angle between the fine unevenness structure and water 40° C. or less, preferably 30° or less. If the surface is hydrophilic, it is possible to suppress fogging under temperature changes or high humidity environments and to suppress deterioration in detection sensitivity and visibility when used as an optical member of a photographing device or an image display device.

[0050] The composition of the active energy ray-curable composition is not particularly limited. For example, the compositions described in JP-A-2013-175733 and JP-A-2015-129947 can be used as reference.

[0051] Examples of a method for sandwiching the active energy ray-curable composition between a mold and a substrate include a method in which the active energy ray-curable composition is placed between the mold and the substrate, and the mold and the substrate are pressed together to inject the active energy ray-curable composition into the fine uneven structure of the mold.

[0052] Examples of the material of the substrate include acrylic resins such as polymethyl methacrylate; polycarbonate resins; styrene resins such as polystyrene and methyl methacrylate-styrene copolymers; cellulose resins such as cellulose diacetate, cellulose triacetate, and cellulose acetate butyrate; polyester resins such as polyethylene terephthalate; polyamide resins; polyimide resins; polyethersulfone resins; polysulfone resins; polyolefin resins such as polypropylene, polymethylpentene, and alicyclic polyolefins; vinyl chloride resins such as polyvinyl chloride; polyvinyl acetal resins; polyether ketone resins; polyurethane resins; and glass. Among them, acrylic resins, polycarbonate resins, polyester resins, and cellulose resins are preferred because they have excellent transmittance for visible light and near-infrared light. Acrylic resins and cellulose resins with an in-plane phase difference of 20 nm or less are more preferred because they have excellent visibility when used in an image display device and excellent accuracy when used in a near-infrared sensor. When glass is used as a transparent substrate, polycarbonate resins and polyester resins are preferred because they can provide shatterproof properties.

[0053] The form of the substrate is not particularly limited. For example, the substrate may be in the form of a film, a sheet, etc. Among these, a film or a sheet is preferred because of its excellent productivity and ease of handling. Examples of the method for producing the substrate include injection molding, extrusion molding, cast molding, etc. Among these, extrusion molding and cast molding are preferred because of their excellent productivity.

[0054] The surface of the substrate may be subjected to a coating treatment, a corona treatment, a printing treatment, etc. for the purpose of improving properties such as adhesion, antistatic properties, scratch resistance, weather resistance, and design properties.

[0055] (Adhesive layer) As in the optical member 10A shown in Figs. 1 and 2, the optical member according to a preferred embodiment further includes an adhesive layer 9. The adhesive layer functions to bond the transparent substrate and the film. In one embodiment, the adhesive layer may also function to block a portion of visible light, in which case the transmittance of visible light is preferably 30% or more and 70% or less. The adhesive layer can be formed, for example, by curing an adhesive composition. A preferred adhesive composition includes an acrylic resin. The acrylic resin is not particularly limited, and various acrylic resins can be used. In order to apply the optical member to a curved surface, the pressure-sensitive adhesive composition may be capable of being cured in two or more stages, that is, may exhibit multi-stage curing properties.

[0056] (Mechanism of action) In the optical member described above using one example, a film having a fine uneven structure is disposed on at least one surface side of a transparent substrate so as to cover both the visible light transmission region and the near-infrared light transmission region. Therefore, reflection in both the visible light transmission region and the near-infrared light transmission region can be prevented. When used as a front panel of an optical device, the optical member can suppress reflection of light in both the visible light region and the near-infrared light region. Therefore, it contributes to improving visibility by the front panel, and can prevent a decrease in resolution, a decrease in detection sensitivity, reflection, flare, and ghosting.

[0057] (Application) The optical member is useful as a protective member for optical devices such as photographing devices such as cameras and image display devices. A photographing device such as a camera or an image display device is disposed in the visible light transmission region of the transparent substrate of the optical member. Also, a sensor such as an infrared sensor is disposed in the near-infrared light transmission region of the optical member.

[0058] For example, the optical member can be applied to a protective member of a photographing device module including a photographing device and a protective member, in which the photographing device is disposed in a visible light transmission region. In addition, the optical member can be applied to a protective member of an image display device module including an image display device and a protective member. In the image display device module, the image display device is disposed in the visible light transmission region.

[0059] (Other examples) 3 and 4 includes a transparent substrate 1, a film 7, and an adhesive layer 9. In the optical member 10B, a light-shielding layer 4 and a printed layer 8 are each partially provided on a surface 7b of the film 7 opposite to the fine uneven structure. The light-shielding layer 4 partially provided on the surface 7b of the film 7 is visually recognized as a near-infrared light transmitting region 5 as shown in FIG. The print layer 8 partially provided on the surface 7b of the film 7 is visible as shown in FIG. 3, and therefore can provide a design.

[0060] 5 and 6 includes a transparent substrate 1, a film 7, and an adhesive layer 9. In the optical member 10C, a printed layer 8 is partially provided on a surface 7a of the film 7 on which a fine uneven structure is formed. The print layer 8 partially provided on the surface 7a of the film 7 is visible as shown in FIG. 5, and therefore can impart design features to the optical component 10C.

[0061] The wettability (surface tension) of the surface 7a of the microrelief structure 7 is preferably 38 mN / m or more. If the wettability of the surface 7a is 38 mN / m or more, it is easy to prevent ink from repelling onto the microrelief structure when applying a printing layer 8 for the purpose of imparting design or light blocking properties. This makes printing easy and provides good adhesion between the ink and the microrelief structure.

[0062] Although one embodiment has been described above by showing several example embodiments, the present invention is not limited to the example embodiments disclosed in this specification, and can be appropriately modified and implemented without departing from the gist of the invention. The embodiment disclosed in this specification can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. EXAMPLES

[0063] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description.

[0064] <Manufacture of roll-shaped mold 1> An aluminum ingot with a purity of 99.99% was cut to an outer diameter of 200 mm, an inner diameter of 155 mm, and a length of 350 mm to prepare a cylindrical aluminum base material without rolling marks. The cylindrical outer peripheral surface of the aluminum base material was anodized for 10 minutes in a 0.3M oxalic acid aqueous solution at a DC voltage of 40 V and a temperature of 16° C. The aluminum base material on which the oxide film was formed was immersed in a 6% by mass phosphoric acid / 1.8% by mass chromic acid mixed solution to remove the oxide film (oxide film removal step). The aluminum base material obtained was anodized for 30 seconds in a 0.3M oxalic acid aqueous solution at a DC voltage of 40 V and a temperature of 16° C. (anodizing step). The aluminum base material on which the oxide film was formed was immersed in a 5% by mass phosphoric acid aqueous solution at 30° C. for 8 minutes to perform a pore size expansion treatment (pore size expansion treatment step). By repeating this anodizing process and pore size expansion process a total of five times, a roll-shaped mold 1 was obtained in which anodized alumina was formed on the surface, with approximately conical pores designed to be spaced 100 nm apart and 200 nm deep.

[0065] <Manufacture of disc-shaped molds 2, 3, 4, and 5> An aluminum ingot with a purity of 99.99% was cut into a disk shape with a diameter of 55 mm and a thickness of 3 mm, and the surface was polished to prepare a disk plate of an aluminum substrate without rolling marks. The disk surface of the aluminum substrate was anodized in a 0.3 M oxalic acid aqueous solution under conditions of a direct current voltage of 40 or 80 V and a temperature of 16°C (anodizing process). The aluminum substrate on which the oxide film was formed was immersed in a 9.55 mass% phosphoric acid aqueous solution at 30°C to perform a pore size expansion process (pore size expansion process). This anodizing process and pore size expansion process were repeated a total of five times to obtain a disk-shaped mold with anodized alumina formed on the surface. The direct current voltage of the anodizing process, the time and number of anodizing and pore size expansion processes were appropriately adjusted to obtain molds 2, 3, 4, and 5 with different average intervals and depths, respectively.

[0066] <Preparation of active energy ray-curable composition> 25 parts by mass of dipentaerythritol hexaacrylate, 25 parts by mass of pentaerythritol triacrylate, 25 parts by mass of polyethylene glycol diacrylate, and 25 parts by mass of an ethylene oxide modified compound of dipentaerythritol hexaacrylate were mixed, and then 1 part by mass of a first photopolymerization initiator (product name "Irgacure 184", manufactured by BASF) and 0.5 parts by mass of a second photopolymerization initiator (product name "Irgacure 819", manufactured by BASF) were added and mixed to prepare an active energy ray curable composition.

[0067] <Anti-reflection film with fine uneven structure (1)> A roll-shaped mold 1 was rotated, and a polyethylene terephthalate substrate (product name "U403" manufactured by Toray Industries, Inc., thickness 50 μm) was run along the outer peripheral surface of the mold in the rotation direction of the mold, while an active energy ray curable composition was supplied between the outer peripheral surface of the mold and the running substrate. The active energy ray curable composition was then cured by irradiating with ultraviolet light. The cured product was peeled off from the mold to produce an anti-reflection film (1) having a fine uneven structure (moth-eye structure). When the surface of the obtained anti-reflection film was observed with a scanning electron microscope, fine convex portions with a period of 100 nm and a height of 200 nm were formed.

[0068] <Anti-reflection film with fine uneven structure (2)> A roll-shaped mold 1 was rotated, and a triacetyl cellulose substrate (product name "KC4UA", manufactured by Konica Minolta, Inc., thickness 40 μm) was run along the outer peripheral surface of the mold in the direction of rotation of the mold, while an active energy ray curable composition was supplied between the outer peripheral surface of the mold and the running substrate. The active energy ray curable composition was then cured by irradiating with ultraviolet light. The cured product was peeled off from the mold to produce an antireflection film (2) having a fine uneven structure (moth-eye structure). When the surface of the obtained antireflection film was observed with a scanning electron microscope, fine convex portions with a period of 100 nm and a height of 200 nm were formed.

[0069] <Anti-reflection film with fine uneven structure (3)> A roll-shaped mold 1 was rotated, and an acrylic substrate (product name "ORV-40UT", manufactured by Okura Kogyo Co., Ltd., thickness 40 μm) was run along the outer peripheral surface of the mold in the direction of rotation of the mold, while an active energy ray curable composition was supplied between the outer peripheral surface of the mold and the running substrate. The active energy ray curable composition was cured by irradiating with ultraviolet rays. The cured product was peeled off from the mold to produce an anti-reflection film (3) having a fine uneven structure (moth-eye structure). When the surface of the obtained anti-reflection film was observed with a scanning electron microscope, fine convex portions with a period of 100 nm and a height of 200 nm were formed.

[0070] <Anti-reflection film with fine uneven structure (4)> A disk-shaped mold 2 and a polyethylene terephthalate substrate (product name "U403" manufactured by Toray Industries, Inc., thickness 50 μm) were overlapped, and an active energy ray curable composition was supplied between the mold and the substrate. The active energy ray curable composition was then cured by irradiating with ultraviolet light. The cured product was peeled off from the mold to produce an anti-reflection film (4) having a fine uneven structure (moth-eye structure). When the surface of the obtained anti-reflection film was observed with a scanning electron microscope, fine convex portions with a period of 100 nm and a height of 300 nm were formed.

[0071] <Anti-reflection film with fine uneven structure (5)> A disk-shaped mold 3 and a polyethylene terephthalate substrate (product name "U403" manufactured by Toray Industries, Inc., thickness 50 μm) were overlapped, and an active energy ray curable composition was supplied between the mold and the substrate. The active energy ray curable composition was then cured by irradiating with ultraviolet light. The cured product was peeled off from the mold to produce an anti-reflection film (5) having a fine uneven structure (moth-eye structure). When the surface of the obtained anti-reflection film was observed with a scanning electron microscope, fine convex portions with a period of 150 nm and a height of 350 nm were formed.

[0072] <Anti-reflection film with fine uneven structure (6)> A disk-shaped mold 4 and a polyethylene terephthalate substrate (product name "U403" manufactured by Toray Industries, Inc., thickness 50 μm) were overlapped, and an active energy ray curable composition was supplied between the mold and the substrate. The active energy ray curable composition was then cured by irradiating with ultraviolet light. The cured product was peeled off from the mold to produce an anti-reflection film (6) having a fine uneven structure (moth-eye structure). When the surface of the obtained anti-reflection film was observed with a scanning electron microscope, fine convex portions with a period of 150 nm and a height of 400 nm were formed.

[0073] <Anti-reflection film with fine uneven structure (7)> A disk-shaped mold 5 and a polyethylene terephthalate substrate (product name "U403" manufactured by Toray Industries, Inc., thickness 50 μm) were overlapped, and an active energy ray curable composition was supplied between the mold and the substrate. The active energy ray curable composition was then cured by irradiating with ultraviolet light. The cured product was peeled off from the mold to produce an anti-reflection film (7) having a fine uneven structure (moth-eye structure). When the surface of the obtained anti-reflection film was observed with a scanning electron microscope, fine convex portions with a period of 150 nm and a height of 500 nm were formed.

[0074] <Example 1> The anti-reflection film (1) having a fine uneven structure was attached to one side of a black acrylic resin plate (product name "Acrylite EX502", manufactured by Mitsubishi Chemical Corporation) via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0075] <Example 2> The anti-reflection film (2) with a fine uneven structure was attached to one side of a black acrylic resin plate via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0076] <Example 3> The anti-reflection film (3) with a fine uneven structure was attached to one side of a black acrylic resin plate via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0077] <Example 4> The anti-reflection film (4) with a fine uneven structure was attached to one side of a black acrylic resin plate via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0078] <Example 5> The anti-reflection film (5) with a fine uneven structure was attached to one side of a black acrylic resin plate via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0079] <Example 6> The anti-reflection film (6) with a fine uneven structure was attached to one side of a black acrylic resin plate via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0080] <Example 7> The anti-reflection film (7) with a fine uneven structure was attached to one side of a black acrylic resin plate via an adhesive layer. The reflectance was then measured. The results are shown in Table 1.

[0081] <Comparative Example 1> An anti-reflection film having an anti-reflection layer including a multi-layer structure (product name "FHC-FV4ARS+HN01A", manufactured by Higashiyama Film Co., Ltd.) was attached to one side of a black acrylic resin plate via an adhesive layer, and the reflectance was measured. The evaluation results obtained are shown in Table 1.

[0082] <Comparative Example 2> The reflectance of a black acrylic resin plate to which no anti-reflection film was attached was measured.

[0083] <Measurement method> The reflectance of the film with a fine uneven structure in the range of 190 to 900 nm was measured with a spectrophotometer (model name "UV-2450", Shimadzu Corporation) at an incident angle of 5° and regular reflection. The luminous reflectance was calculated in accordance with JIS R3106. Table 1 shows the reflectance at 900 nm and the luminous reflectance. The reflectance of the film having a fine uneven structure in the range of 300 to 2500 nm was measured with a spectrophotometer (model name "UH-4150", manufactured by Hitachi, Ltd.) at an incident angle of 8° and total reflection. Table 1 shows the reflectance at 1550 nm.

[0084] [Table 1]

[0085] As can be seen from Table 1, the films having a fine uneven structure obtained in Examples 1, 2, 3, 4, 5, 6, and 7 had excellent luminous reflectance, 900 nm reflectance, and 1550 nm reflectance. On the other hand, the AR film of Comparative Example 1 had poor reflectance at 900 nm and 1550 nm. [Industrial Applicability]

[0086] According to the present invention, there is provided an optical member capable of preventing reflection in both the visible light transmission region and the near-infrared light transmission region. [Explanation of symbols]

[0087] 1 Transparent substrate 3 Visible light transmission range 4 Light blocking layer 5 Near infrared light transmission range 7. Film with a micro-relief structure 8 printing layer 9 Adhesive layer 10 Optical components

Claims

1. a transparent substrate having a visible light transmission region and a near-infrared light transmission region in the same plane; a film having a fine uneven structure on its surface, the average distance between convex portions being equal to or less than the wavelength of visible light; having The film is disposed on at least one surface of the transparent substrate so as to cover both the visible light transmission region and the near-infrared light transmission region.

2. The luminous reflectance of the film is 0.5% or less, and 2. The optical member according to claim 1, wherein the film has a reflectance of 1.0% or less at a wavelength of 900 nm.

3. The luminous reflectance of the film is 0.5% or less, and The optical member according to claim 1 , wherein the reflectance of the film at 1550 nm is 5.0% or less.

4. The optical member according to claim 1 , further comprising an adhesive layer between the near-infrared light transmitting region of the transparent substrate and the film.

5. A photographing device module including a photographing device and a protective member, The protective member is an optical member according to any one of claims 1 to 4, an imaging device module, the imaging device being disposed in the visible light transmission area;

6. An image display device module including an image display device and a protective member, The protective member is an optical member according to any one of claims 1 to 4, The image display device module, wherein the image display device is disposed in the visible light transmission region.

Citation Information

Patent Citations

  • Infrared sensor cover, infrared sensor module, and camera

    JP2018124279A

  • Antireflection article and display device

    WO2010150514A1

  • Transparent substrate having light blocking region and display device

    WO2018105602A1

Cited By