Microporous film
A PTFE-based microporous membrane with narrow pores and a thin skin layer addresses the trade-off between gas and liquid permeability, ensuring high gas permeability and liquid impermeability, particularly effective against low-surface-tension liquids, with improved flexibility and mechanical strength.
Patent Information
- Application Number
- JP2024037704
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-01
AI Technical Summary
Existing porous membranes face a trade-off between gas permeability and liquid permeability, with liquids like alcohol and oil easily penetrating due to capillary action, and there is a need for improved flexibility and mechanical strength.
A microporous membrane made of polytetrafluoroethylene (PTFE) with pore widths of 1 μm or less, a thin skin layer of 200 nm or less, porosity of 20% or less, and specific gravity of 1.96 or more, ensuring high gas permeability and liquid impermeability, particularly effective against low-surface-tension liquids.
The membrane achieves excellent gas permeation performance while preventing liquid permeation, including low-surface-tension liquids, with enhanced flexibility and mechanical strength, and maintains high gas permeability without liquid leakage.
Smart Images

Figure 2024132975000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a microporous membrane that is suitably used in degassing applications for removing dissolved gases such as oxygen contained in liquids such as chemical solutions and inks, aeration applications such as aerating carbon dioxide gas into water when producing functional water for cleaning, and gas separation applications for separating a specific gas from a gas mixture. [Background technology]
[0002] As separation membranes used for deaeration and aeration, various porous membranes made of fluororesin have been used up to now (Patent Documents 1 to 3).
[0003] In recent years, hollow fiber membranes have become known that have excellent water permeability and selectivity by defining the ratio of the average pore size on the inner peripheral surface to the average pore size on the outer peripheral surface of the filtration layer (Patent Document 4).
[0004] The porous tube of Patent Document 1 has closed-cell type air bubbles formed by foaming fluororesin, and therefore has poor gas permeability.
[0005] The pore size of the porous fluororesin thin film in Patent Document 2 is very small, but since the thin film is formed by coating a dispersion, it has low mechanical strength and poor water pressure resistance.
[0006] Patent Documents 3 and 4 have a skin layer, but there remains a problem in achieving both gas permeability and liquid permeability.
[0007] In addition to the above-mentioned patent documents, a separation membrane made of an amorphous fluororesin is also known. Although this membrane has excellent degassing performance, it has a problem in that it is poor in flexibility.
[0008] As described above, separation materials for degassing and aeration applications are required to have excellent gas permeability and to be impermeable to liquids, but there is a trade-off between these two properties; improving gas permeability makes it easier for liquids to permeate, and it has been extremely difficult to achieve both gas permeability and liquid permeability prevention. In particular, liquids with low surface tension such as alcohol and oil tend to easily permeate due to capillary action, and further improvements are desired. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2004-160291 A [Patent Document 2] JP 2010-94579 A [Patent Document 3] Japanese Patent Application Publication No. 10-202074 [Patent Document 4] WO2020 / 059344 publication Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a microporous membrane which is excellent in both gas permeability and liquid permeation prevention properties, and which also has excellent flexibility. [Means for solving the problem]
[0011] The gist of the microporous membrane of the present invention is as follows. (1) A microporous membrane made of a fluororesin whose main component is polytetrafluoroethylene, characterized in that the pore width of the microporous membrane is 1 μm or less. (2) It is preferable that the microporous membrane has a surface layer having a skin layer with a thickness of 200 nm or less. (3) The porosity of the microporous membrane is preferably 20% or less. (4) The specific gravity of the microporous membrane according to JIS Z 8807 is preferably 1.96 or more. (5) The gas permeability coefficient of nitrogen gas at 25°C is preferably 800×10-10cm3·cm / cm2·sec·cmHg or more and 1800×10-10cm3·cm / cm2·sec·cmHg or less. (6) When an internal pressure of 1 MPa is applied for 10 minutes, it is preferable that no methanol permeates through the membrane. (7) It is preferable that the device has a tubular shape. (8) It is preferable to use it for degassing or aeration. Effect of the Invention
[0012] According to the present invention, a microporous membrane having excellent gas permeability, excellent liquid permeability prevention, and excellent flexibility can be obtained. In addition, when the surface layer has a skin layer having a thickness of 200 nm or less, the membrane also has excellent buckling prevention properties. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram showing a cross-sectional view (observation point X) in a line direction of a tubular microporous membrane. [Diagram 2] 1 is a FE-SEM measurement image of a microporous membrane according to the present invention. [Diagram 3] Observation point X (near the center of the tube wall thickness) of a general-purpose PTFE porous tube. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, as an example of the microporous membrane of the present invention, the basic structure will be described with reference to the drawings.
[0015] The microporous membrane 1 of the present invention is characterized by being made of a fluororesin mainly composed of polytetrafluoroethylene (PTFE). It is preferably made of PTFE alone, and additives such as pigments for coloring and antistatic materials for preventing static electricity may be added in appropriate amounts depending on the purpose.
[0016] The pore width of the microporous membrane 1 is further characterized to be 1.0 μm or less, preferably 0.05 μm to 1.0 μm, and more preferably 0.10 μm to 0.50 μm. The pore width is measured from an FE-SEM measurement image (FIG. 2(a)) near the center of the tube wall thickness at observation point X in FIG. 1.
[0017] The FE-SEM measurement conditions for the pore width were as follows: the sample was platinum-vapor-deposited, the sample was surrounded by embedding resin, the acceleration voltage was 1.0 kV, and the observation magnification was 20,000. As shown in Fig. 2(a), the pores of the microporous membrane 1 of the present invention have a long and narrow shape similar to a cylindrical or bale shape, so the longest part of the pore width was taken as the pore width value.
[0018] The microporous membrane 1 of the present invention is characterized by the presence of very fine pores throughout the membrane. Adjacent pores are partially connected to each other, allowing gas to move through the pores.
[0019] As shown in the image of the skin layer located on the outside (surface layer) of the tube at observation point X in Figure 1 (Figure 2(b)) and the image of the skin layer located on the inside (surface layer) of the tube at observation point X (Figure 2(c)), it is preferable that the microporous membrane 1 has a skin layer with a thickness of 200 nm or less on the surface layer. It is more preferably 100 nm or less, and most preferably 50 nm or less. The measurement method used was FE-SEM measurement, as with the pore width, and the measurement conditions were changed to an accelerating voltage of 0.8 kV and an observation magnification of 100,000 times.
[0020] Here, the skin layer present on the surface refers to a layer with a smaller porosity than the inner layer. From the viewpoint of preventing liquid permeation, the porosity is preferably 0%, but from the viewpoint of preventing buckling, the presence of a very small number of holes is acceptable.
[0021] The porosity of the microporous membrane 1 is preferably 20% or less, more preferably 10% or less, and most preferably 7% or less. The porosity is measured according to the underwater displacement method described in JIS K 7112.
[0022] The specific gravity of the microporous membrane 1 is preferably 1.96 or more, and more preferably 2.0 or more. The specific gravity is measured according to the liquid weighing method described in JIS Z 8807.
[0023] The specific gravity of a typical industrial PTFE membrane (solid structure product) is often 2.0 to 2.2. The microporous membrane 1 of the present invention has a specific gravity equivalent to that of a solid structure product, but is characterized by excellent gas permeability. Since the specific gravity is not reduced but remains equivalent, and the gas permeability is excellent, it is possible to achieve both gas permeability and liquid permeation prevention performance.
[0024] The gas permeability coefficient of the microporous membrane 1 for nitrogen gas at 25°C is preferably 800×10-10cm3·cm / cm2·sec·cmHg or more and 1800×10-10cm3·cm / cm2·sec·cmHg or less.
[0025] The gas permeability coefficient is measured for nitrogen gas at an atmospheric pressure and at a temperature of 25°C in accordance with the gas chromatography test method described in JIS K 7126-2. The flow rate of the carrier gas is 10 ml / min.
[0026] The greatest feature of the microporous membrane 1 of the present invention is that it is excellent in gas permeability and does not allow liquid to pass through. In particular, it is effective in preventing liquid permeation even with liquids having low surface tension such as alcohol and oil.
[0027] No liquid permeation means that when an internal pressure of 1 MPa is applied to the microporous membrane 1 for 10 minutes, no liquid permeates through the microporous membrane 1. The types of liquid include, for example, water, alcohols such as ethanol, and oils, but in the present invention, methanol is used for the evaluation.
[0028] Among liquids, the surface tension of alcohol and oil is lower than that of water, with the surface tension of water being approximately 73 mN / m, ethanol and methanol being approximately 23 mN / m at 20°C, and paraffin oil having a surface tension of approximately 26 mN / m at 25°C.
[0029] A liquid with low surface tension easily penetrates into the pores of a porous body due to the capillary phenomenon. Therefore, in the case of a conventional porous membrane (tube), when a liquid with low surface tension is passed through the tube, the liquid penetrates into the pores in the tube wall and may leak out to the outside of the tube over a long period of use.
[0030] The microporous membrane 1 of the present invention has very small pores and a very thin skin layer, and therefore can prevent liquid permeation even with liquids having low surface tension while maintaining high gas permeability.
[0031] The shape of the microporous membrane 1 is not particularly limited and includes a sheet shape, a tube shape, a rod shape, etc. For the purpose of transporting liquid, the tube shape is preferred.
[0032] In the case of a sheet-shaped microporous membrane, the skin layer may be present in at least one of the top layer and bottom layer, and in the case of a tube-shaped microporous membrane, the skin layer may be present in at least one of the inner surface layer (the inner surface of the tube) and the outer surface layer (the outer surface of the tube). In the case of a rod-shaped microporous membrane, the skin layer may be present in the surface layer. The same applies to other shapes.
[0033] The inner diameter and thickness of the microporous membrane 1 are not particularly limited, but from the viewpoint of formability and deaeration / aeration applications, the inner diameter is preferably 0.20 to 2.0 mm, and the thickness is preferably 0.01 to 0.50 mm.
[0034] The elongation percentage of the microporous membrane 1 is not particularly limited, but is preferably 200% or more. The tensile strength is not particularly limited, but is preferably 80 MPa or more.
[0035] Although there is no particular limitation on the method for producing the microporous membrane 1, molding by a general paste extrusion process and stretching process is preferred. In the case of paste extrusion molding using PTFE fine powder, unlike molding by dispersion coating, a thick microporous membrane 1 having excellent mechanical strength and water pressure resistance can be obtained.
[0036] The microporous film 1 may be formed of only a single layer, but may also be combined with other layers to form a multi-layer structure, without any particular limitation.
[0037] There is no particular limitation on the application, but it is preferable that it is used for degassing and aeration. EXAMPLES
[0038] The microporous membrane 1 of the present invention will be described in more detail below with reference to examples and comparative examples, but the scope of the present invention is not limited to these.
[0039] Example 1 is a tubular microporous membrane 1 of the present invention made of 100% PTFE. The inner diameter of the tube is 0.82 mm, the wall thickness is 0.30 mm, and the pore width is 0.6 μm. The thickness of the skin layer present on the surface layer of the tube is 10 nm.
[0040] Comparative Example 1 is a general-purpose PTFE porous tube shown in Fig. 3, which has an inner diameter of 3.0 mm, a wall thickness of 0.5 mm, and a pore width of 17 µm. The tube surface layer does not have a skin layer.
[0041] Comparative Example 2 is a general-purpose PTFE tube (solid structure product) having an inner diameter of 0.90 mm, a wall thickness of 0.50 mm, and no holes. The tube surface layer does not have a skin layer.
[0042] Comparative Example 3 is an amorphous fluororesin tube, which has an inner diameter of 0.68 mm, a wall thickness of 0.08 mm, and is non-porous. The tube surface layer does not have a skin layer.
[0043] Comparative Example 4 is a commercially available deaeration silicone rubber tube, which has an inner diameter of 0.80 mm, a wall thickness of 0.20 mm, and is non-porous. The surface layer of the tube does not have a skin layer.
[0044] The above-mentioned Examples and Comparative Examples are evaluated for specific gravity, porosity, gas permeability coefficient, and liquid permeability.
[0045] The measurement methods for each evaluation are shown below.
[0046] (Method of measuring specific gravity) The method complies with the liquid weighing method described in JIS Z 8807. The standard substance is water, the measurement temperature is 25°C, and the sample length is 150 mm.
[0047] (Method of measuring porosity) The measurement is based on the underwater displacement method described in JIS K 7112. The measurement temperature is 25°C.
[0048] (Method of measuring gas permeability coefficient) The gas permeability coefficient of nitrogen gas at 25°C is measured according to the gas chromatography method described in JIS K 7126-2. The measurement device used is a gas permeability tester manufactured by GL Sciences Inc. The flow rate of the carrier gas is 10 ml / min, the atmospheric pressure during the test is 101.3 kPa, and the time from the gas flow until the equilibrium state is reached is 10 minutes.
[0049] (Method for evaluating the presence or absence of liquid permeation) Pour methanol into the tube and apply an internal pressure of 1.0 MPa for 10 minutes to check whether or not methanol seeps out from the inside of the tube to the outside.
[0050] The evaluation results of the examples and comparative examples are shown in Table 1 below.
[0051] [Table 1]
[0052] From Table 1, the microporous membrane 1 of the present invention (Example 1) is excellent in both high gas permeability and liquid permeation prevention performance. The general-purpose PTFE porous tube (Comparative Example 1) has a high porosity, so it has excellent gas permeability, but liquid leakage occurs. The general-purpose PTFE tube (Comparative Example 2) is non-porous, so it does not cause liquid leakage, but it also has low gas permeability. The amorphous fluororesin tube (Comparative Example 3) is excellent in both gas permeability and liquid permeation prevention performance, but its gas permeability coefficient is lower than that of Example 1 and is not as good as that of the microporous membrane 1 of the present invention. In addition, the amorphous fluororesin tube is a very expensive material, and is inferior to the Examples in terms of cost. The deaeration silicone rubber (Comparative Example 4) is generally inexpensive, but is inferior to the others in terms of gas permeability, liquid prevention performance, and chemical resistance.
[0053] The reason why the microporous membrane 1 (Example 1) of the present invention is very excellent in both gas permeability and liquid permeation prevention properties is that the pore width is very small. Since there are countless fine pores, liquid permeation can be prevented while maintaining high gas permeability. Furthermore, when an extremely thin skin layer is present on the surface layer of the microporous membrane 1, the liquid permeation prevention property is further improved while maintaining the gas permeability. The improvement in liquid permeation prevention property leads to a significant improvement in water pressure resistance. [Industrial Applicability]
[0054] The microporous membrane of the present invention can be suitably used for degassing and defoaming liquids and for supplying air, but is not particularly limited thereto. [Explanation of symbols]
[0055] 1. Tube-shaped microporous membrane 2. Skin layer X Observation point (cross section along the tube shape line) L hole width
Claims
1. A microporous membrane made of a fluororesin containing polytetrafluoroethylene as a main component, The microporous membrane has a pore width of 1 μm or less.
2. The microporous membrane has a surface layer having a skin layer having a thickness of 200 nm or less. The microporous membrane of claim 1.
3. The microporous membrane has a porosity of 20% or less. The microporous membrane of claim 1 or 2.
4. The microporous membrane has a specific gravity of 1.96 or more according to JIS Z 8807. The microporous membrane according to any one of claims 1 to 3.
5. The gas permeability coefficient of nitrogen gas at 25°C is 800 x 10-10 cm3 cm / cm2 sec cmHg or more and 1800 x 10-10 cm3 cm / cm2 sec cmHg or less. The microporous membrane according to any one of claims 1 to 3.
6. It is characterized in that no methanol permeates when an internal pressure of 1 MPa is applied for 10 minutes. The microporous membrane according to any one of claims 1 to 3.
7. Characterized in that it is made of a tube shape, The microporous membrane according to any one of claims 1 to 3.
8. Characterized in that it is used for degassing or aeration, The microporous membrane according to any one of claims 1 to 3.
Citation Information
Patent Citations
Asymmetric structural fluororesin tube, production thereof, deaerating method using the tube and device therefor
JP1998202074A
Fluororesin tube for degassing / dissolving treatment
JP2004160291A
Method of manufacturing porous fluororesin thin film and porous fluororesin thin film
JP2010094579A
Hollow-fiber membrane
WO2020059344A1