Pressure device, manufacturing method of structural member, and fatigue strength improvement method of structural member

The pressing device addresses the challenge of applying compressive stress in welded joints by forming indentations, improving fatigue strength in structures like crane runway girders through efficient use of a compact, adjustable mechanism.

JP2024133027APending Publication Date: 2024-10-01NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2024041013
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing methods for improving fatigue strength in welded joints, such as those used in crane runway girders, are difficult to implement due to limited space and the need for large, heavy equipment, making it challenging to generate compressive residual stress effectively.

Method used

A pressing device with adjustable first and second support parts and pressing portions that can be inserted into notches of welded joints to apply compressive stress by forming indentations, using a mechanism with threaded parts and protrusions to facilitate easy installation and adjustment.

Benefits of technology

The device effectively applies compressive stress to welded joints, enhancing fatigue strength by reducing tensile residual stress and preventing crack propagation, even in constrained spaces like crane runway girders.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133027000001_ABST
    Figure 2024133027000001_ABST
Patent Text Reader

Abstract

To provide a technique capable of easily applying compression stress to metal members that constitute structures in the various structures.SOLUTION: A pressure device which presses a metal member to form an indentation includes: a first support part; a second support part which is opposed to the first support part in a first direction such that a gap is formed between the first support part and itself; a connection part which connects the first support part with the second support part; a first pressing part which is provided in the first support part and in which one tip protrudes to the second support part side; and a second pressing part which is provided in the second support part so as to be opposed to the first pressing part and in which one tip protrudes to the first support part side. A distance between the first pressing part and the second pressing part in the first direction can be adjusted.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressing device for pressing a metal member, a method for manufacturing a structural member, and a method for improving the fatigue strength of a structural member. [Background technology]

[0002] Various welded joints are used in structures such as buildings, bridges, ships, and cranes. Tensile welding residual stress is likely to occur in the welded parts of welded joints due to the shrinkage of the weld metal during welding. Furthermore, in such structures, when a load is repeatedly applied to the welded joint, fatigue cracks may occur due to stress concentration at the weld toe, etc. For this reason, when welded joints are used in such structures, it is necessary to improve the fatigue strength of the welded parts.

[0003] Therefore, techniques for improving the fatigue strength of welded joints have been proposed in the past. For example, Patent Document 1 discloses a method for generating compressive residual stress in advance in a stress concentration part of a welded joint by making an indentation with a punch. Patent Document 1 describes that by generating compressive residual stress in the stress concentration part, it is possible to suppress the occurrence and growth of fatigue cracks from the stress concentration part and minor defects in the stress concentration part. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-275913 A Summary of the Invention [Problem to be solved by the invention]

[0005] By utilizing the method disclosed in Patent Document 1, the fatigue strength of the welded joints constituting a structure can be improved. On the other hand, depending on the structure in which the welded joints are used, it may be difficult to apply the method disclosed in Patent Document 1. For example, it is not easy to appropriately generate compressive residual stress in the stress concentration part of the welded joint used in the crane runway girder (CRG) laid in the factory for running the overhead crane. That is, since the CRG is placed at a high place and the working space is limited, it is difficult to install heavy and large equipment and prepare utilities such as a power source, and the above construction to appropriately generate compressive residual stress is not easy.

[0006] Therefore, an object of the present invention is to provide a technique that can easily impart compressive stress to metal members that constitute various structures. [Means for solving the problem]

[0007] The present invention relates to a pressing device, a method for manufacturing a structural member, and a method for improving the fatigue strength of a structural member, as described below.

[0008] (1) A pressing device for pressing a metal member to form an indentation, A first support portion; a second support portion facing the first support portion in a first direction such that a gap is formed between the second support portion and the first support portion; a connecting portion that connects the first support portion and the second support portion; a first pressing portion provided on the first support portion and having one tip protruding toward the second support portion; a second pressing portion provided on the second support portion so as to face the first pressing portion, one tip of which protrudes toward the first support portion; Equipped with A pressing device, wherein the distance between the first pressing portion and the second pressing portion in the first direction is adjustable.

[0009] (2) The pressing device according to (1) above, wherein the first support portion, the second support portion, and the connecting portion are integrally formed.

[0010] (3) A first screw hole penetrating the first support portion in the first direction is formed, The pressing device according to (1) or (2) above, wherein the first pressing portion comprises a first screw portion screwed into the first screw hole, and a first protrusion portion provided at a tip of the first screw portion and protruding from the first support portion toward the second support portion in the gap.

[0011] (4) The pressing device described in (3) above, wherein a tip surface of the first protrusion has a flat shape perpendicular to the first direction and a circular shape having a diameter smaller than a diameter of the first screw portion when viewed from the first direction.

[0012] (5) The pressing device described in (3) above, wherein a tip of the first protrusion is rotationally symmetric about the axis of the first screw portion and has a curved surface that is convex toward the second support portion.

[0013] (6) The first support portion and the second support portion are provided to extend to one side in a second direction perpendicular to the first direction relative to the connecting portion, A pressing device as described in any one of (1) to (5) above, wherein, when viewed from the second direction, the gap extends in a direction perpendicular to the first direction and the distance in the first direction gradually increases on one side in the third direction.

[0014] (7) The pressing tool is used to press the metal member having a notch formed therein penetrating in a predetermined direction, The pressing device according to any one of (1) to (6) above, which can be inserted into the notch portion with the first direction aligned with the predetermined direction.

[0015] (8) When viewed from the first direction, a direction in which the connecting portion and the first pressing portion are aligned is defined as an X direction, and a direction perpendicular to the X direction is defined as a Y direction. The pressing device according to any one of (1) to (7) above, wherein, when viewed from the first direction, the first support portion and the second support portion each have a shape in which each corner of a virtual rectangle consisting of a pair of long sides parallel to the X direction and a pair of short sides parallel to the Y direction is cut off.

[0016] (9) The pressing device according to (8) above, wherein when viewed from the first direction, the first support portion and the second support portion each fall within a quadrant having a radius of 35 mm.

[0017] (10) A second screw hole penetrating the second support portion in the first direction is formed, The pressing device according to any one of (1) to (9) above, wherein the second pressing portion comprises a second screw portion screwed into the second screw hole, and a second protrusion provided at a tip of the second screw portion and protruding from the second support portion toward the first support portion in the gap.

[0018] (11) A portion of the connecting portion facing the gap has a first surface extending in a second direction perpendicular to the first direction, a second surface extending in a third direction perpendicular to the first direction and the second direction, and a third surface connecting the first surface and the second surface, the first surface is provided on one side in the third direction relative to the second surface, the second surface is provided on one side in the second direction relative to the first surface, and the third surface extends from an edge of the first surface on the one side in the second direction toward an edge of the second surface on the one side in the third direction, obliquely extending with respect to the second direction and the third direction; The pressing device according to any one of (1) to (10) above, wherein the first pressing portion and the second pressing portion protrude into the gap on the one side of the first surface in the third direction.

[0019] (12) The pressing device according to (1) above, wherein the first support portion, the second support portion, and the connecting portion are configured by separate members.

[0020] (13) The connecting portion includes a first bolt, a nut, and a second bolt having a curved tip portion, the first support portion has a first through hole penetrating in the first direction and a screw hole penetrating in the first direction, the second support portion has a second through hole that faces the first through hole in the first direction and penetrates in the first direction, and a curved recess that faces the screw hole in the first direction and is recessed toward the opposite side to the first support portion in the first direction, the first bolt is inserted into the first through hole and the second through hole; the nut is attached to a tip portion of the first bolt such that the first support portion and the second support portion are sandwiched between a head portion of the first bolt and the nut; The pressing device according to (12) above, wherein the second bolt is screwed into the screw hole from the outside of the first support part so that the tip part fits into the recess part.

[0021] (14) The first support portion has a first thin plate portion and a first thick plate portion that protrudes toward the second support portion in the first direction more than the first thin plate portion, the second support portion has a second thin plate portion and a second thick plate portion that protrudes toward the first support portion in the first direction relative to the second thin plate portion, the gap includes an insertion gap between the first thin plate portion and the second thin plate portion and an adjustment gap between the first thick plate portion and the second thick plate portion, The first thick plate portion has a first support surface facing the insertion gap, the second thick plate portion has a second support surface that is provided at the same position as the first support surface when viewed from the first direction so as to face the insertion gap, each of the first support surface and the second support surface has a first surface extending in a second direction perpendicular to the first direction, a second surface extending in a third direction perpendicular to the first direction and the second direction, and a third surface connecting the first surface and the second surface; the first surface is provided on one side in the third direction relative to the second surface, the second surface is provided on one side in the second direction relative to the first surface, and the third surface extends from an edge of the first surface on the one side in the second direction toward an edge of the second surface on the one side in the third direction, obliquely extending with respect to the second direction and the third direction; the first pressing portion and the second pressing portion protrude into the insertion gap on the one side of the first surface in the third direction, the first bolt and the second bolt are provided to pass through the adjustment gap in the first direction, The pressing device according to (13) above, wherein the first pressing portion, the first bolt, and the second bolt are arranged in this order in the third direction.

[0022] (15) The pressing device according to (2) above, wherein the first support portion, the connecting portion and the second support portion are integrally formed in an arc shape.

[0023] (16) The first support portion has a first screw hole formed therein and penetrating therethrough in the first direction, The second support portion has a second screw hole formed therein, the second screw hole penetrating in the first direction. the first pressing portion includes a first screw portion screwed into the first screw hole, and a first protruding portion provided at a tip of the first screw portion and protruding from the first support portion toward the second support portion in the gap, The pressing device described in (15) above, wherein the second pressing portion comprises a second screw portion screwed into the second screw hole, and a second protrusion portion provided at a tip of the second screw portion and protruding from the second support portion toward the first support portion in the gap.

[0024] (17) the first support portion and the second support portion are provided on one side of the connecting portion in a second direction perpendicular to the first direction, The pressing device described in (16) above, wherein, when viewed from a third direction perpendicular to the first direction and the second direction, an inner edge of the first support portion includes a straight portion extending in a straight line toward the tip of the one side in the second direction so as to move away from the second support portion in the first direction toward that side.

[0025] (18) A method for manufacturing a structural component having a plate-shaped metal member, the method comprising the step of pressing the metal member with a pressing device according to any one of (1) to (17) above.

[0026] (19) A method for improving fatigue strength of a structural component, comprising pressing the plate-shaped metal member of the structural component with the pressing device described in any one of (1) to (17) above. Effect of the Invention

[0027] According to the present invention, compressive stress can be easily applied to metal members in various structures. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a diagram showing a pressing device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a welded joint whose fatigue strength is improved by the pressing device. [Diagram 3] FIG. 3 is a diagram for explaining a method for improving fatigue strength using a pressing device. [Figure 4] FIG. 4 is a diagram for explaining a method for improving fatigue strength using a pressing device. [Diagram 5] FIG. 5 shows an example of a structure whose fatigue strength is improved by the pressing device. [Figure 6] FIG. 6 shows an example of a structure whose fatigue strength is improved by the pressing device. [Figure 7] FIG. 7 shows an example of a structure whose fatigue strength is improved by the pressing device. [Figure 8]FIG. 8 shows an example of a structure whose fatigue strength is improved by the pressing device. [Figure 9] FIG. 9 shows an example of a structure whose fatigue strength is improved by the pressing device. [Figure 10] FIG. 10 is a diagram showing another example of the shape of the tip of the protrusion of the first pressing portion. [Figure 11] FIG. 11 is a diagram showing a pressing device according to a second embodiment of the present invention. [Figure 12] FIG. 12 is a diagram for explaining a method for improving fatigue strength using a pressing device. [Figure 13] FIG. 13 is a diagram showing a pressing device according to a third embodiment of the present invention. [Figure 14] FIG. 14 is a diagram for explaining a method for improving fatigue strength using a pressing device. [Figure 15] FIG. 15 is a schematic diagram for explaining a pressing device according to a fourth embodiment of the present invention. [Figure 16] FIG. 16 is a diagram for explaining an example of a fatigue strength improving method using the pressing device according to this embodiment. [Figure 17] FIG. 17 is a diagram for explaining an example of a fatigue strength improving method using the pressing device according to this embodiment. [Figure 18] FIG. 18 is a diagram for explaining an example of a fatigue strength improving method using the pressing device according to this embodiment. [Figure 19] FIG. 19 is a diagram showing a pressing device according to a modified example. [Figure 20] FIG. 20 is a diagram for explaining a fatigue strength improving method using a pressing device. [Figure 21] FIG. 21 is a diagram showing another example of a structural member. [Figure 22] FIG. 22 is a diagram showing another example of a structural member. [Figure 23] FIG. 23 is a diagram showing a specific example of application of the pressing device to an out-of-plane gusset joint. [Figure 24] FIG. 24 is a diagram showing the welded structure specimen used in Test 1. [Diagram 25]FIG. 25 shows the results of Test 1. [Figure 26] FIG. 26 is a diagram showing the in-plane gusset welded joint used in Test 2. [Figure 27] FIG. 27 shows the results of Test 2. [Figure 28] FIG. 28 shows the results of Test 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A pressing device, a manufacturing method for a structural member, and a method for improving fatigue strength of a structural member according to embodiments of the present invention will be described below with reference to the drawings.

[0030] (First embodiment) (Configuration of the pressing device) FIG. 1 is a diagram showing a pressing device according to an embodiment of the present invention, where (a) is a plan view, (b) is a front view, (c) is a right side view, (d) is a left side view, and (e) is a rear view. Each view in FIG. 1 is marked with arrows indicating directions A, B, and C that are perpendicular to each other. In this embodiment, direction A corresponds to the first direction, direction B corresponds to the second direction, and direction C corresponds to the third direction. Hereinafter, direction A will be referred to as first direction A, direction B will be referred to as second direction B, and direction C will be referred to as third direction C.

[0031] Although details will be described later, the pressing device 10 according to this embodiment is a device that presses metal members to impart compressive stress to stress concentration portions in a welded joint having a plurality of plate-shaped metal members welded together. In this embodiment, the welded joint corresponds to a structural member.

[0032] 1, the pressing device 10 includes a first support portion 12, a second support portion 14, a connecting portion 16, a first pressing portion 18, and a second pressing portion 20. In this embodiment, the first support portion 12, the second support portion 14, and the connecting portion 16 are integrally formed. The first support portion 12, the second support portion 14, and the connecting portion 16 are made of, for example, a steel material having a tensile strength of 950 MPa or more.

[0033] The first support portion 12 and the second support portion 14 face each other in the first direction A such that a gap 22 is formed between them. The connecting portion 16 is provided between the first support portion 12 and the second support portion 14 so as to extend in the first direction A. In this embodiment, the first support portion 12 and the second support portion 14 are provided so as to extend to one side in the second direction B beyond the connecting portion 16. When viewed from the second direction B, the gap 22 is provided so as to extend in the third direction C, and such that the distance in the first direction A gradually increases on one side in the third direction C.

[0034] The first support portion 12 has a screw hole 12a formed therethrough in the first direction A. Similarly, the second support portion 14 has a screw hole 14a formed therethrough in the first direction A. The screw hole 14a is provided to face the screw hole 12a in the first direction A.

[0035] The first pressing portion 18 is provided on the first support portion 12 so as to protrude from the first support portion 12 to the second support portion 14 side at the gap 22. The second pressing portion 20 is provided on the second support portion 14 so as to face the first pressing portion 18 in the first direction A and so as to protrude from the second support portion 14 to the first support portion 12 side at the gap 22. The first pressing portion 18 and the second pressing portion 20 are supported by the first support portion 12 and the second support portion 14 so that the distance in the first direction A between the first pressing portion 18 and the second pressing portion 20 can be adjusted.

[0036] In this embodiment, the first pressing portion 18 is inserted into the screw hole 12a. Specifically, the first pressing portion 18 has a screw portion 18a screwed into the screw hole 12a so as to be movable in the first direction A, and a protruding portion 18b provided at the tip of the screw portion 18a and protruding from the first support portion 12 to the second support portion 14 side in the gap 22. In this embodiment, a bolt having a head portion 18c is used as the first pressing portion 18. In this embodiment, the first pressing portion 18 can be moved in the first direction A by rotating the head portion 18c.

[0037] The second pressing portion 20 is inserted into the screw hole 14a. Specifically, the second pressing portion 20 has a screw portion 20a screwed into the screw hole 14a so as to be movable in the first direction A, and a protruding portion 20b provided at the tip of the screw portion 20a and protruding from the second support portion 14 toward the first support portion 12 through the gap 22. A groove 20c is formed on the end face of the screw portion 20a opposite to the protruding portion 20b. In this embodiment, the second pressing portion 20 can be moved in the first direction A by inserting a flathead screwdriver into the groove 20c and rotating the screw portion 20a.

[0038] In this embodiment, screw hole 12a corresponds to the first screw hole, screw hole 14a corresponds to the second screw hole, threaded portion 18a corresponds to the first threaded portion, threaded portion 20a corresponds to the second threaded portion, protrusion 18b corresponds to the first protrusion, and protrusion 20b corresponds to the second protrusion.

[0039] In this embodiment, a flat surface 18d having a circular shape and perpendicular to the first direction A (axial direction of the threaded portion 18a) is formed at the tip of the protruding portion 18b. The diameter of the flat surface 18d is smaller than the diameter (nominal diameter) of the threaded portion 18a. The area of ​​the flat surface 18d is preferably set to 2 / 5 or less of the cross-sectional area (area of ​​a cross section perpendicular to the first direction A) of the threaded portion 18a, and more preferably set to 1 / 3 or less. By setting the area of ​​the flat surface 18d in this manner, when the metal member of the welded joint is pressed by the flat surface 18d, the metal member can be pressed with a small tightening load. The pressing position of the metal member by the pressing device 10 will be described later.

[0040] In this embodiment, a flat surface 20d having a circular shape and perpendicular to the first direction A (axial direction of the threaded portion 20a) is formed at the tip of the protruding portion 20b. As with the flat surface 18d, the area of ​​the flat surface 20d is preferably set to, for example, 2 / 5 or less of the cross-sectional area of ​​the threaded portion 20a (the area of ​​the cross section perpendicular to the first direction A), and more preferably set to 1 / 3 or less.

[0041] As shown in Figs. 1(c) and (d), in this embodiment, the connecting portion 16 and the first pressing portion 18 are arranged side by side in the second direction B. Also, as viewed from the first direction A, the first support portion 12 and the second support portion 14 each have a shape in which each corner of a virtual rectangle consisting of a pair of long sides parallel to the second direction B and a pair of short sides parallel to the third direction C is cut out. In this embodiment, the second direction B corresponds to the X direction, and the third direction C corresponds to the Y direction. Note that, in this embodiment, the connecting portion 16 is formed so as not to protrude from the first support portion 12 and the second support portion 14 as viewed from the first direction A. Note that, in the example shown in Fig. 1, as viewed from the first direction A, the first support portion 12 and the second support portion 14 each have a shape in which each corner of the virtual rectangle is cut out linearly, but the first support portion 12 and the second support portion 14 each may have a shape in which each corner of the virtual rectangle is cut out in an arc shape. That is, both ends of the first support portion 12 and the second support portion 14 in the second direction B may be chamfered into a U-shape.

[0042] (Methods for improving fatigue strength) The pressing device 10 according to the present embodiment is used to press metal members in order to impart compressive stress to the vicinity of a stress concentration portion in a welded joint having a plurality of plate-shaped metal members welded together. For example, in a welded joint having a notch such as a scallop, the pressing device 10 is disposed in the notch, and the vicinity of the weld toe of the weld (weld metal), which is the stress concentration portion (more specifically, the vicinity of the toe of the weld (including the box weld) at the gusset end), is pressed by the pressing device 10. As a result, compressive stress is imparted to the vicinity of the stress concentration portion (weld toe) of the welded joint, and the fatigue strength of the welded joint is improved. In this specification, improving fatigue strength means not only suppressing the occurrence of fatigue cracks, but also suppressing the further progression and enlargement of existing fatigue cracks.

[0043] An example of a method of using the pressing device 10 will be described below. Fig. 2 is a diagram showing an example of a welded joint whose fatigue strength is improved by the pressing device 10. Fig. 2 shows a steel deck as an example of a welded joint. Fig. 2 is also a diagram showing the steel deck as viewed obliquely from below.

[0044] 2, the steel deck 30 has a deck plate 32, a main girder 34, a horizontal rib 36, and a vertical rib 38. A plurality of cutouts 36a, 36b, and 36c are formed in the steel deck 30. In the steel deck 30 of FIG. 2, the deck plate 32, the main girder 34, the horizontal rib 36, and the vertical rib 38 are each an example of a plate-shaped metal member.

[0045] Welds 42a, 42b, and 42c are formed so as to pass through the notch 36a. Weld 42a joins the deck plate 32 to the main girder 34, weld 42b joins the deck plate 32 to the cross rib 36, and weld 42c joins the main girder 34 to the cross rib 36. Weld 42d joining the cross rib 36 to the vertical rib 38 is formed so as to pass through the notches 36b and 36c. Weld 42e joining the deck plate 32 to the vertical rib 38 and weld 42f joining the deck plate 32 to the cross rib 36 are formed so as to pass through the notch 36c.

[0046] In this embodiment, the pressing device 10 is disposed in each of the cutouts 36a, 36b, 36c, and the vicinity of the weld toes (weld toes at the gusset ends) of each of the welds 42b to 42d, 42f is pressed by the first pressing part 18 and the second pressing part 20, thereby imparting compressive residual stress to the weld toes. This makes it possible to improve the fatigue strength of the weld toes (stress concentration parts) of each of the welds 42b to 42d, 42f. As a result, the fatigue strength of the steel deck 30 can be improved.

[0047] The fatigue strength improving method will be described in more detail below, taking as an example a case where the pressing device 10 is disposed inside the cutout portion 36a.

[0048] 3 and 4 are diagrams for explaining a method for improving the fatigue strength of the steel deck 30 by using a pressing device 10 placed in the through hole 40a. As shown in Fig. 3, the welded portion 42b includes a box welded portion 44. The box welded portion 44 is a portion of the welded portion 42b that is formed so as to go around the end portion of the transverse rib 36 on the side of the notched portion 36a.

[0049] In this embodiment, as shown in FIG. 3(a), first, the pressing device 10 is placed in the cutout portion 36a. Note that FIG. 3(a) shows an ellipse inscribed in the cutout portion 36a. In this embodiment, the pressing device 10 is formed to a size that fits within the ellipse when the first direction A is aligned with the penetration direction of the cutout portion 36a (thickness direction of the transverse rib 36), for example. Note that in welded joints used in architectural structures, etc., a scallop is often formed to a size equivalent to a quadrant with a radius of about 35 mm. The pressing device 10 according to this embodiment is formed to a size that can be inserted into such a scallop, for example. Specifically, the first support portion 12 and the second support portion 14 are formed to fit within a quadrant with a radius of 35 mm, for example, when viewed from the first direction A. Note that the dimensions of the first support portion 12 and the second support portion 14 can be appropriately changed according to the structure (dimensions of the scallop, etc.) of the structural member (welded joint) to be improved in fatigue strength. Therefore, the first support portion 12 and the second support portion 14 may be formed to fit within a quadrant with a radius of 25 mm when viewed from the first direction A, or may be formed to fit within a quadrant with a radius of 20 mm.

[0050] Next, as shown in FIG. 3(b), the pressing device 10 is rotated to position the transverse rib 36 and the welded portion 42b between the first support portion 12 (see FIG. 1) and the second support portion 14. Specifically, the pressing device 10 is positioned so that the vicinity of the weld toe 44a on the transverse rib 36 side of the boxing welded portion 44 is positioned between the protruding portion 18b of the first pressing portion 18 and the protruding portion 20b of the second pressing portion 20 (see FIG. 1(d)). If the dimension of the connecting portion 16 is too large, the pressing device 10 cannot be smoothly rotated within the scallop. For this reason, in this embodiment, the connecting portion 16 is designed to have a dimension that allows the pressing device 10 to be smoothly rotated within the scallop.

[0051] In this state, the first pressing portion 18 is moved toward the second pressing portion 20, and the protruding portion 18b (flat surface 18d) and the protruding portion 20b (flat surface 20d (see FIG. 1)) press the transverse rib 36. As a result, a compressive load acts on the portion near the weld toe 44a, and as shown in FIG. 4, an indentation 46 due to plastic deformation can be formed on both sides of the transverse rib 36. As a result, the tensile residual stress generated near the weld toe 44a during welding can be reduced, or a compressive residual stress can be generated near the weld toe 44a. This can improve the fatigue strength of the steel deck 30. In this embodiment, the pressing depth of the first pressing portion 18 is set to, for example, about 5% of the thickness of the metal member to be pressed. Therefore, for example, when the thickness of the transverse rib 36 is 9 mm, the pressing depth of the first pressing portion 18 is about 0.5 mm. In this embodiment, by pressing the first pressing portion 18 in by about 0.5 mm, the protruding portion 18b and the protruding portion 20b form indentations 46 with a depth of about 0.25 mm on both sides of the transverse rib 36. The principle by which the fatigue strength of the welded joint is improved by forming indentations as described above is the same as the principle disclosed in the above-mentioned Patent Document 1.

[0052] When forming an indentation on the metal member, it is preferable to apply a lubricant to the protruding portion 18b (flat surface 18d) of the first pressing portion 18. This can reduce friction between the first pressing portion 18 and the metal member, and the first pressing portion 18 can be rotated smoothly. As a result, the indentation can be easily formed on the metal member. In order to properly form an indentation on the metal member, it is preferable that the tip of the protruding portion 20b of the second pressing portion 20 has a surface state that is not easily slippery against the metal member. Therefore, it is not necessary to apply a lubricant to the protruding portion 20b (flat surface 20d) of the second pressing portion 20. In this embodiment, the flat surface 20d is formed at the tip of the protruding portion 20b to increase the contact area between the protruding portion 20b and the metal member. This can prevent the protruding portion 20b from slipping against the metal member. In addition, the flat surface 20d may be formed with a protrusion or a recess in order to increase the frictional force generated between the protruding portion 20b and the metal member.

[0053] The dimensions of each part of the pressing device 10 are not particularly limited, and may be set appropriately according to the dimensions of each part of the welded joint to be improved in fatigue strength. In order to sufficiently improve the fatigue strength of the welded joint, it is preferable to cause plastic flow over almost the entire thickness of the metal member. In this regard, if the diameter of the flat surfaces 18d, 20d is too small, plastic flow will occur only on the surface of the metal member. For this reason, the diameter of the flat surfaces 18d, 20d is preferably 1 / 3 or more, more preferably 1 / 2 or more, of the thickness of the metal member on which the indentation is formed.

[0054] The fatigue strength improvement method according to the present embodiment is a method for improving the fatigue strength of a welded joint, but it can also be said to be a method for manufacturing a new welded joint having improved fatigue strength by using an existing welded joint as a base material. The same applies to the embodiments described below.

[0055] (Effects of this embodiment) As described above, with the pressing device 10 according to this embodiment, indentations can be easily formed in the metal member by the first pressing portion 18 and the second pressing portion 20 while the metal member is sandwiched between the first supporting portion 12 and the second supporting portion 14. Therefore, by using the pressing device 10 according to this embodiment, compressive stress can be easily applied near the stress concentration portion of a welded joint in various structures.

[0056] 1(b), in the pressing device 10 according to this embodiment, the gap 22 is provided such that the distance in the first direction A gradually increases on one side in the third direction C when viewed from the second direction B. In this case, by positioning the welded portion in the portion of the gap 22 where the distance in the first direction A increases, it is possible to prevent the welded portion from coming into contact with the pressing device 10 when forming an indentation in the metal member. This allows the indentation to be formed more smoothly in the metal member.

[0057] In addition, in the pressing device 10 according to this embodiment, the diameter of the flat surface 18d is smaller than the diameter (nominal diameter) of the threaded portion 18a. In this case, when the metal member is pressed by the flat surface 18d, it is possible to prevent excessive stress from being generated in the threaded portion 18a, and therefore it is possible to prevent damage to the threaded portion 18a. In particular, as described above, by setting the area of ​​the flat surface 18d to 2 / 5 or less (more preferably 1 / 3 or less) of the cross-sectional area of ​​the threaded portion 18a, it is possible to appropriately press the metal member by the protruding portion 18b with a small tightening load.

[0058] In the above embodiment, the case has been described in which the pressing device 10 is placed in the cutout 36a of the steel deck 30 in FIG. 2 to improve the fatigue strength of the weld toe. However, the pressing device 10 may also be placed in the cutout 36b or cutout 36c to improve the fatigue strength of the weld toe.

[0059] Also, for example, in a structure as shown in Figs. 5 to 8, the pressing device 10 may be used to improve the fatigue strength of the weld toe. The structure 50 shown in Fig. 5 includes a main girder web 51, a lower cross gusset 52, a main girder lower flange 53, and a vertical stiffener 54. The lower cross gusset 52, the main girder lower flange 53, and the vertical stiffener 54 are joined to the main girder web 51 by welds 55a, 55b, and 55c. The lower cross gusset 52 has a notch (scallop) 56 for passing the vertical stiffener 54 and the weld 55c through. When the pressing device 10 is used in the structure 50, for example, the pressing device 10 can be disposed in the notch 56 to form an indentation 46a on both sides of the lower cross gusset 52 in the vicinity of the weld toe on the lower cross gusset 52 side of the weld 55a. This improves the fatigue strength of the weld toe of the boxing weld on the side of the notch 56 of the weld 55a in the lower horizontal gusset 52. Note that a pressing device 10 may be disposed from the outside of the lower horizontal gusset 52 to form an indentation 46b in the vicinity of the weld toe of the boxing weld on the side opposite the notch 56 of the weld 55a.

[0060] The structure 60 shown in FIG. 6 includes a deck plate 61, a transverse rib 62, and a valve rib 63. The deck plate 61 and the transverse rib 62 are joined to the deck plate 61 by a plurality of welds 64. The transverse rib 62 is formed with a notch (scallop) 62a for passing the lower end of the valve rib 63. A part (a box weld) of the weld 64 joining the transverse rib 62 and the valve rib 63 is provided so as to pass through the notch 62a. When the pressing device 10 is used in the structure 60, for example, the pressing device 10 can be disposed in the notch 62a to form an indentation 46 on both sides of the transverse rib 62 in the vicinity of the weld toe of the box weld of the weld 64 on the transverse rib 62 side. This can improve the fatigue strength of the weld toe of the box weld of the weld 64 on the transverse rib 62 side.

[0061] The structure 65 shown in FIG. 7 includes a deck plate 66, a transverse rib 67, and a valve rib 68. The deck plate 66 and the transverse rib 67 are joined to the deck plate 66 by welds 69a and 69b. The transverse rib 67 is formed with a notch (scallop) 67a for passing the valve rib 68 and a pair of welds 69a. A part (a box weld) of the weld 69b joining the deck plate 66 and the transverse rib 67 is provided to pass through the notch 67a. When the pressing device 10 is used in the structure 65, for example, the pressing device 10 can be disposed in the notch 67a to form an indentation 46 on both sides of the transverse rib 67 in the vicinity of the weld toe of the box weld of the weld 69b on the transverse rib 67 side. This can improve the fatigue strength of the weld toe of the box weld of the weld 69b on the transverse rib 67 side.

[0062] The structure 70 shown in FIG. 8 has a first mold member 71 and a second mold member 72. In FIG. 8, (a) is a front view of the structure 70, and (b) is a side view of the structure 70 (viewed from the second mold member 72 side). The first mold member 71 and the second mold member 72 are, for example, I-shaped or H-shaped members. In this embodiment, the first mold member 71 has a flange portion 71a and a web portion 71b. Similarly, the second mold member 72 has a flange portion 72a and a web portion 72b. The thickness of the flange portion 72a is greater than that of the flange portion 71a.

[0063] Web portion 71b is joined to flange portion 71a by welded portion 71c. Web portion 72b is joined to flange portion 72a by welded portion 72c. Flange portion 71a and flange portion 72a are joined by welded portion 74a. Web portion 71b and web portion 72b are joined by welded portion 74b. A notch portion (rathole) 75 is formed so as to penetrate web portion 71b and web portion 72b in the thickness direction.

[0064] In the structure 70, when a force acts in a direction that separates the first and second mold members 71 and 72 from each other, cracks may occur in the weld toe 76a on the web portion 71b side of the welded portion 74b and in the weld toe 76b on the web portion 72b side of the welded portion 74b. Therefore, as shown in Fig. 9, it is considered to form an indentation 46 on both sides of the web portion 71b in the vicinity of the weld toe 76a by disposing a pressing device 10 in the notch 75. Similarly, it is considered to form an indentation 46 on both sides of the web portion 72b in the vicinity of the weld toe 76b. This makes it possible to improve the fatigue strength in the vicinity of the weld toe 76a and in the vicinity of the weld toe 76b.

[0065] In the above embodiment, as shown in FIG. 1, the case where the flat surface 18d is formed at the tip of the protruding portion 18b of the first pressing portion 18 has been described. However, the tip of the protruding portion 18b of the first pressing portion 18 may be formed with a curved surface that is rotationally symmetric about the axis of the threaded portion 18a and curved so as to be convex toward the second support portion 14. For example, as shown in FIG. 10(a), the tip surface 18e of the protruding portion 18b may have a spherical crown shape formed so that the apex is located on the axis of the threaded portion 18a. Also, as shown in FIG. 10(b), a spherical crown-shaped protrusion 18f may be provided at the center of the flat surface 18d of the protruding portion 18b. Note that the area of ​​the tip surface 18e as viewed from the first direction A is preferably set to 2 / 5 or less of the cross-sectional area of ​​the threaded portion 18a (the area of ​​the cross section perpendicular to the first direction A), and more preferably set to 1 / 3 or less. The height of the tip surface 18e in the first direction A is set to, for example, 1 / 100 or less of the diameter of the tip surface 18e as viewed from the first direction A. The height of the projection 18f in the first direction A is set to, for example, about 1 / 50 to 1 / 10 of the diameter of the flat surface 18d. Since the tip of the first pressing portion 18 has the above-mentioned shape, it is possible to prevent one-sided contact from occurring when the first pressing portion 18 (threaded portion 18a) is screwed in to press the protruding portion 18b into the metal member. In other words, it is possible to prevent the first pressing portion 18 from rotating around the outer edge of the tip surface 18e or the outer edge of the flat surface 18d as the rotation center due to the displacement of the fulcrum when the first pressing portion 18 (threaded portion 18a) is screwed in. This allows an indentation to be formed smoothly on the metal member. Note that the indentation formed by the protruding portion 18b shown in FIG. 10 has a shape with a concave center. Although not shown in the drawings, a conical tip surface may be provided instead of tip surface 18e shown in Fig. 10(b). In this case as well, the height of the tip surface in the first direction A is set to, for example, 1 / 100 or less of the diameter of the tip surface as viewed from the first direction A.

[0066] In the above-described embodiment, the second pressing portion 20 is provided on the second support portion 14 so as to be movable in the first direction A, but the second pressing portion may be fixed to the second support portion 14. For example, as the second pressing portion, a protruding portion protruding from the second support portion 14 toward the first support portion 12 side so as to face the protruding portion 18b of the first pressing portion 18 may be integrally formed with the second support portion 14.

[0067] Second embodiment (Configuration of the pressing device) 11 is a diagram showing a pressing device according to a second embodiment of the present invention, where (a) is a front view, (b) is a right side view, and (c) is a bottom view. Each view in FIG. 11 is marked with arrows indicating directions A, B, and C that are perpendicular to each other. In this embodiment, direction A corresponds to the first direction, direction B corresponds to the second direction, and direction C corresponds to the third direction. Hereinafter, direction A will be referred to as first direction A, direction B will be referred to as second direction B, and direction C will be referred to as third direction C.

[0068] Like the above-described pressing device 10, the pressing device according to this embodiment is a device for pressing metal members in a welded joint having a plurality of plate-shaped metal members welded to one another.

[0069] As shown in Fig. 11, the pressing device 80 includes a first support portion 82, a second support portion 84, a connecting portion 86, a first pressing portion 18, and a second pressing portion 20. The first pressing portion 18 and the second pressing portion 20 can be configured similarly to the first pressing portion 18 and the second pressing portion 20 in the above-mentioned first embodiment, and therefore detailed description will be omitted. In this embodiment, the first supporting portion 82, the second supporting portion 84, and the connecting portion 86 are integrally formed. The first supporting portion 82, the second supporting portion 84, and the connecting portion 86 are made of, for example, a steel material having a tensile strength of 950 MPa or more.

[0070] The first support portion 82 and the second support portion 84 face each other in the first direction A such that a gap 88 is formed between them. The connecting portion 86 is provided so as to extend in the first direction A between the first support portion 82 and the second support portion 84. In this embodiment, the first support portion 82 and the second support portion 84 are provided so as to extend further to one side in the second direction B and one side in the third direction C than the connecting portion 86.

[0071] The first support portion 82 has a screw hole 82a formed therethrough in the first direction A. Similarly, the second support portion 84 has a screw hole 84a formed therethrough in the first direction A. The screw hole 84a is provided to face the screw hole 82a in the first direction A.

[0072] The first pressing portion 18 is provided on the first support portion 82 so as to protrude from the first support portion 82 to the second support portion 84 side at the gap 88. The second pressing portion 20 is provided on the second support portion 84 so as to face the first pressing portion 18 in the first direction A and so as to protrude from the second support portion 84 to the first support portion 82 side at the gap 88.

[0073] In this embodiment, the first pressing portion 18 is inserted into the screw hole 82a. Also, the second pressing portion 20 is inserted into the screw hole 84a. In this embodiment, the screw hole 82a corresponds to the first screw hole, and the screw hole 84a corresponds to the second screw hole.

[0074] The portion of the connecting portion 86 facing the gap 88 has a first surface 86a extending in the second direction B, a second surface 86b extending in the third direction C, and a third surface 86c connecting the first surface 86a and the second surface 86b. In this embodiment, when viewed from the first direction A, the gap 88 is formed in an L-shape so as to pass through one side of the first surface 86a in the third direction C and one side of the second surface 86b in the second direction B. The second surface 86b is provided on one side in the second direction B and on the other side in the third direction C from the first surface 86a. The third surface 86c extends from one edge of the first surface 86a in the second direction B toward one edge of the second surface 86b in the third direction C, at an angle with respect to the second direction B and the third direction C. The first pressing portion 18 (protruding portion 18b) and the second pressing portion 20 (protruding portion 20b) protrude into the gap 88 on one side of the first surface 86a in the third direction C.

[0075] (Methods for improving fatigue strength) The pressing device 80 according to this embodiment can be suitably used to improve the fatigue strength of an in-plane gusset welded joint. FIG. 12 is a diagram for explaining a fatigue strength improvement method using the pressing device 80 according to this embodiment. FIG. 12 shows an in-plane gusset welded joint 90. The in-plane gusset welded joint 90 has a main plate portion 91 and a gusset portion 92. In this embodiment, the main plate portion 91 and the gusset portion 92 are examples of plate-shaped metal members. The gusset portion 92 is joined to the main plate portion 91 by a weld portion 93 extending along the edge of the main plate portion 91.

[0076] As described above, in the pressing device 80 according to this embodiment, an L-shaped gap 88 is formed between the first support portion 82 and the second support portion 84. This allows the pressing device 80 to be easily fitted into the joint between the main plate portion 91 and the gusset portion 92, as shown in Fig. 12(a). In this state, by pressing the main plate portion 91 with the first pressing portion 18 (projecting portion 18b) and the second pressing portion 20 (projecting portion 20b), the indentations 46 can be easily formed on both sides of the main plate portion 91, as shown in Fig. 12(b).

[0077] 11, in this embodiment, the first pressing portion 18 (protruding portion 18b) and the second pressing portion 20 (protruding portion 20b) are provided so as to protrude into the gap 88 on one side of the first surface 86a in the third direction C. Therefore, by attaching the pressing device 80 to the in-plane gusset welded joint 90 so that the first surface 86a faces the main plate portion 91 and the second surface 86b faces the gusset portion 92, it is possible to form an indentation 46 in the vicinity of the weld toe 93a on the main plate portion 91 side of the weld 93. This makes it possible to improve the fatigue strength of the weld toe 93a in the main plate portion 91. On the other hand, although not shown, by attaching the pressing device 80 to the in-plane gusset welded joint 90 so that the first surface 86a faces the gusset portion 92 and the second surface 86b faces the main plate portion 91, it is possible to form an indentation near the weld toe 93b on the gusset portion 92 side of the weld 93. This can also improve the fatigue strength of the weld toe 93b in the gusset portion 92.

[0078] In addition, in the pressing device 80 according to this embodiment, a third surface 86c inclined with respect to the first surface 86a and the second surface 86b is provided between the first surface 86a and the second surface 86b. This makes it possible to prevent the pressing device 80 from contacting the welded portion 93 when the pressing device 80 is attached to the in-plane gusset welded joint 90. However, the present invention is not limited to this embodiment. When viewed from the first direction A, the first surface 86a may be inclined with respect to the second direction B or may be curved. Also, when viewed from the first direction A, the second surface 86b may be inclined with respect to the third direction C or may be curved. Furthermore, the third surface 86c may not be provided, and the first surface 86a and the second surface 86b may be directly connected to each other.

[0079] Although detailed description is omitted, the indentation 46 may be formed in the in-plane gusset welded joint 90 using the pressing device 10 according to the first embodiment.

[0080] Third embodiment (Configuration of the pressing device) 13 is a diagram showing a pressing device according to a third embodiment of the present invention, where (a) is a front view, (b) is a right side view, and (c) is a bottom view. Each view in FIG. 13 is marked with arrows indicating directions A, B, and C that are perpendicular to each other. In this embodiment, direction A corresponds to the first direction, direction B corresponds to the second direction, and direction C corresponds to the third direction. Hereinafter, direction A will be referred to as first direction A, direction B will be referred to as second direction B, and direction C will be referred to as third direction C.

[0081] Like the above-described pressing devices 10 and 80, the pressing device according to this embodiment is a device for pressing metal members in a welded joint having a plurality of plate-shaped metal members welded to one another.

[0082] 13, the pressing device 100 includes a first support portion 102, a second support portion 104, a connecting portion 106, a first pressing portion 108, and a second pressing portion 110. The first support portion 102 and the second support portion 104 face each other in a first direction A such that a gap 112 is formed between them. In this embodiment, the first support portion 102, the second support portion 104, and the connecting portion 106 are separate members.

[0083] The connecting portion 106 is provided to extend in a first direction A. In this embodiment, the connecting portion 106 includes a first bolt 114, a nut 116, and a second bolt 118 having a curved tip portion 118a. The tip portion 118a is rotationally symmetric about the axis of the second bolt 118, and has a shape that is curved so as to be convex toward the second support portion 104 side (a spherical crown shape in this embodiment).

[0084] The first support portion 102 is formed with a first through hole 102a penetrating in the first direction A, and screw holes 102b and 102c penetrating in the first direction A. The second support portion 104 is formed with a second through hole 104a that faces the first through hole 102a in the first direction A and penetrates in the first direction A, a curved (in this embodiment, spherical crown-shaped) recess 104b that faces the screw hole 102b in the first direction A and is recessed on the opposite side to the first support portion 102 in the first direction A, and a screw hole 104c that faces the screw hole 102c in the first direction A and penetrates in the first direction A. As shown in FIG. 13(b), the length of the first through hole 102a in the third direction C is greater than the length in the second direction B. Similarly, the length of the second through hole 104a (see FIG. 13(a)) in the third direction C is greater than the length in the second direction B.

[0085] 13(a), in the present embodiment, when viewed from the second direction B, the outer surface of the first support portion 102 in the first direction A includes curved surfaces 103a and 103b that are curved in an arc outward in the first direction A. When viewed from the second direction B, the outer surface of the second support portion 104 in the first direction A includes a curved surface 103c that is curved in an arc outward in the first direction A. The first through hole 102a opens in the curved surface 103a, the screw hole 102b opens in the curved surface 103b, and the second through hole 104a opens in the curved surface 103c.

[0086] The first bolt 114 is inserted into the first through hole 102a and the second through hole 104a in the first direction A. A nut 116 is attached to the tip of the first bolt 114 so that the first support part 102 and the second support part 104 are sandwiched between the head 114a of the first bolt 114 and the nut 116. The second bolt 118 is screwed into the screw hole 102b from the outside of the first support part 102 in the first direction A so that the tip part 118a fits into the recess 104b.

[0087] The first pressing portion 108 has a thread groove on its outer circumferential surface and is screwed into the threaded hole 102c so as to be movable in the first direction A. Similarly, the second pressing portion 110 has a thread groove on its outer circumferential surface and is screwed into the second through hole 104a so as to be movable in the first direction A.

[0088] In this embodiment, the first support portion 102 has a first thin plate portion 200 and a first thick plate portion 202 that protrudes toward the second support portion 104 side more than the first thin plate portion 200 in the first direction A. Similarly, the second support portion 104 has a second thin plate portion 400 and a second thick plate portion 402 that protrudes toward the first support portion 102 side more than the second thin plate portion 400 in the first direction A.

[0089] The gap 112 includes an insertion gap 112a between the first thin plate portion 200 and the second thin plate portion 400, and an adjustment gap 112b between the first thick plate portion 202 and the second thick plate portion 402. The first thick plate portion 202 has a first support surface 202a facing the insertion gap 112a. Similarly, the second thick plate portion 402 has a second support surface 402a provided at the same position as the first support surface 202a when viewed from the first direction A so as to face the insertion gap 112a.

[0090] As shown in Fig. 13(a), the first support surface 202a has a first surface 206a, a second surface 206b, and a third surface 206c similar to the first surface 86a, the second surface 86b, and the third surface 86c shown in Fig. 11(a). Although detailed description is omitted, the second support surface 402a also has a first surface, a second surface, and a third surface similar to the first surface, the second surface, and the third surface shown in Fig. 11(a). Therefore, the insertion gap 112a is formed in an L-shape when viewed from the first direction A, similar to the gap 88 shown in Fig. 11.

[0091] The first pressing portion 108 and the second pressing portion 110 protrude into the insertion gap 112a on one side of the first surface 206a in the third direction C, and the first bolt 114 and the second bolt 118 are provided to pass through the adjustment gap 112b in the first direction A. The first pressing portion 108 (second pressing portion 110), the first bolt 114, and the second bolt 118 are provided to be aligned in this order in the third direction C.

[0092] (Methods for improving fatigue strength) The pressing device 100 according to this embodiment can be suitably used to improve the fatigue strength of an in-plane gusset welded joint, similarly to the pressing device 80 described above. Specifically, as shown in FIG. 14, the first bolt 114 is fastened in a state in which the joint between the main plate portion 91 and the gusset portion 92 is fitted into the insertion gap 112a of the pressing device 100. As a result, the first bolt 114 receives a tensile reaction force, and the second bolt 118 receives a compressive force. As a result, the amount of pressing of the first pressing portion 108 and the second pressing portion 110 (see FIG. 13) into the main plate portion 91 can be adjusted. As a result, as shown in FIG. 12(b), the indentation 46 can be formed in the main plate portion 91. Also, similarly to the pressing device 80, the indentation 46 can be formed in the gusset portion 92 by changing the orientation of the pressing device 100 with respect to the in-plane gusset welded joint 90.

[0093] In pressing device 100 according to this embodiment, head 114a of first bolt 114 is provided on curved surface 103a via a washer, and nut 116 is provided on curved surface 103c via a washer. This makes it possible to prevent bending load from being applied to first bolt 114 even if second support portion 104 is inclined relative to first support portion 102 when forming an indentation in the metal member. The same applies to second bolt 118.

[0094] Furthermore, in the pressing device 100 according to this embodiment, the first through hole 102a and the second through hole 104a into which the first bolt 114 is inserted are formed so that their lengths in the third direction C are greater than their lengths in the second direction B. As a result, even if the second support part 104 is tilted relative to the first support part 102 when forming an indentation in the metal member, the first bolt 114 can be tilted in the third direction C, so that the application of a bending load to the first bolt 114 can be suppressed.

[0095] Furthermore, in the pressing device 100 according to this embodiment, the curved tip 118a of the second bolt 118 is supported by the curved recess 104b. This makes it possible to prevent a bending load from being applied to the second bolt 118 even if the second support part 104 is inclined with respect to the first support part 102 when forming an indentation in the metal member.

[0096] (Fourth embodiment) (Configuration of the pressing device) FIG. 15 is a schematic diagram for explaining a pressing device according to a fourth embodiment of the present invention, in which (a) is a plan view of the pressing device, (b) is a front view of a support member of the pressing device, (c) is a left side view of the support member, and (d) is a right side view of the support member. Each view in FIG. 15 is provided with arrows indicating A direction, B direction, and C direction that are orthogonal to each other. In this embodiment, the A direction corresponds to the first direction, the B direction corresponds to the second direction, and the C direction corresponds to the third direction. Hereinafter, the A direction will be referred to as the first direction A, the B direction will be referred to as the second direction B, and the C direction will be referred to as the third direction C.

[0097] 15(a), the pressing device 150 includes a support member 160, a first pressing portion 18, and a second pressing portion 20. Note that the first pressing portion 18 and the second pressing portion 20 can be configured similarly to the first pressing portion 18 and the second pressing portion 20 in the above-described first embodiment, and therefore detailed description thereof will be omitted.

[0098] The support member 160 includes a first support portion 162, a second support portion 164, and a connecting portion 166 that connects the first support portion 162 and the second support portion 164. The first support portion 162 and the second support portion 164 face each other in the first direction A such that a gap 168 is formed between them. In this specification, the fact that the first support portion and the second support portion face each other in the first direction does not mean that the first support portion and the second support portion are provided completely parallel to each other, but means that the second support portion exists on a virtual straight line that passes through the first support portion and extends in the first direction A.

[0099] In this embodiment, the first support portion 162, the connecting portion 166, and the second support portion 164 are integrally formed in an arc shape. In this embodiment, the support member 160 has a shape in which the outer portions of both ends of a semi-torus-shaped member are cut away, and the connecting portion 166 has a circular cross section. However, the cross section of the connecting portion 166 is not limited to a circular shape, and may be a polygonal shape. The cross section of the first support portion 162 and the second support portion 164 is also not particularly limited. The support member 160 is made of, for example, a steel material having a tensile strength of 950 MPa or more.

[0100] In this embodiment, the first support portion 162 and the second support portion 164 are provided on one side in the second direction B relative to the connecting portion 166. In addition, the connecting portion 166 is curved in an arc shape so as to be convex toward the other side in the second direction B when viewed from the third direction C.

[0101] The first support portion 162 has a screw hole 162a formed therethrough in the first direction A. Similarly, the second support portion 164 has a screw hole 164a formed therethrough in the first direction A. The screw hole 164a is provided to face the screw hole 162a in the first direction A.

[0102] The first pressing portion 18 is provided on the first support portion 162 so as to protrude from the first support portion 162 to the second support portion 164 side in the gap 168. The second pressing portion 20 is provided on the second support portion 164 so as to face the first pressing portion 18 in the first direction A and so as to protrude from the second support portion 164 to the first support portion 162 side in the gap 168.

[0103] In this embodiment, the first pressing portion 18 is inserted into the screw hole 162a. Also, the second pressing portion 20 is inserted into the screw hole 164a. In this embodiment, the screw hole 162a corresponds to the first screw hole, and the screw hole 164a corresponds to the second screw hole.

[0104] (Methods for improving fatigue strength) The pressing device 150 according to this embodiment, like the pressing device 10 according to the first embodiment described above, can be used to improve fatigue strength by applying compressive stress to the vicinity of a stress concentration portion in a welded joint having a plurality of plate-shaped metal members welded together. Figures 16 to 18 are diagrams for explaining an example of a fatigue strength improvement method using the pressing device 150 according to this embodiment.

[0105] FIG. 16 is a schematic perspective view showing a welded joint to be improved in fatigue strength. The welded joint 170 shown in FIG. 16 has a plurality of plate-shaped metal members 171, 172, and 173 welded to each other. A scallop 174 is formed at the intersection of the metal members 171, 172, and 173. The metal members 171, 172, and 173 are joined to each other by a plurality of welds 175 to 178. A box weld 175a of the weld 175 joining the metal members 171 and 172 and a box weld 176a of the weld 176 joining the metal members 172 and 173 are formed so as to pass through the scallop 174. In addition, a weld 177 joining the metal members 171 and 173 is also formed so as to pass through the scallop 174. In the following, a case will be described in which the pressing device 150 is used to press the portions near the weld toe 175b of the box weld 175a on the metal member 172 side (portions indicated by dashed-dotted circles 179a, 179b: hereinafter referred to as pressing targets 179a, 179b).

[0106] In this embodiment, as shown in FIG. 17, first, the support member 160 with the first pressing portion 18 and the second pressing portion 20 removed is inserted into the scallop 174. As described above, in this embodiment, the support member 160 has an arc-shaped curved shape. Therefore, by inserting the support member 160 into the scallop 174 while rotating it around the weld toe 175b, the pressing target portions 179a, 179b can be easily positioned between the first support portion 162 and the second support portion 164. In addition, since the support member 160 can be inserted into the scallop 174 while rotating it as described above, the support member 160 can be smoothly inserted even if the dimension of the scallop 174 is small.

[0107] In this embodiment, the support member 160 is formed to a size that allows it to be inserted into a scallop having a size equivalent to a quadrant with a radius of 20 mm. In this embodiment, the cross-sectional shape of the support member 160 is set to a size equivalent to a circle with a diameter of 15 mm, for example.

[0108] Next, as shown in FIG. 18, the first pressing part 18 is attached to the first support part 162, and the second pressing part 20 is attached to the second support part 164. Then, the first pressing part 18 is moved toward the second pressing part 20, and the protruding part 18b and the protruding part 20b press the metal member 172 (more specifically, the pressing target parts 179a, 179b: see FIG. 17). As a result, a compressive load acts on the part in the vicinity of the weld toe 175b, and an indentation (not shown) due to plastic deformation can be formed on both sides of the metal member 172. As a result, the tensile residual stress generated in the vicinity of the weld toe 175b during welding can be reduced, or a compressive residual stress can be generated in the vicinity of the weld toe 175b. This can improve the fatigue strength of the welded joint 170. Although a detailed description is omitted, the pressing device 150 according to this embodiment can be used to improve the fatigue strength of various welded joints, similar to the pressing devices according to the first to third embodiments described above.

[0109] (Modification) Fig. 19 is a diagram showing a pressing device according to a modified example. Note that Fig. 19 is provided with arrows indicating directions A and B that are perpendicular to each other. In this embodiment, direction A corresponds to the first direction, and direction B corresponds to the second direction. Also, a direction perpendicular to directions A and B corresponds to a third direction. Hereinafter, direction A will be referred to as first direction A, and direction B will be referred to as second direction B. Also, hereinafter, when it is described as being in a plan view, it means being viewed from a direction (third direction) perpendicular to first direction A and second direction B.

[0110] 19, a pressing device 180 according to this embodiment includes a support member 190, a first pressing portion 18, and a second pressing portion 20. Note that the first pressing portion 18 and the second pressing portion 20 can be configured similarly to the first pressing portion 18 and the second pressing portion 20 in the above-described first embodiment, and therefore detailed description thereof will be omitted.

[0111] The support member 190 includes a first support portion 192, a second support portion 194, and a connecting portion 196 that connects the first support portion 192 and the second support portion 194. The first support portion 192 and the second support portion 194 face each other in the first direction A so that a gap 198 is formed between them. The first support portion 192, the connecting portion 196, and the second support portion 194 are integrally formed in an arc shape. In this embodiment, the connecting portion 196 has a circular cross section, similar to the connecting portion 166 of the support member 160 described above. However, the cross section of the connecting portion 196 is not limited to a circular shape, and may be a polygonal shape. The cross section of the first support portion 192 and the second support portion 194 is not particularly limited. The support member 190 is made of, for example, a steel material having a tensile strength of 950 MPa or more.

[0112] The first support portion 192 and the second support portion 194 are provided on one side in the second direction B of the connecting portion 196. Moreover, the connecting portion 196 is curved in an arc shape so as to be convex toward the other side in the second direction B in a plan view.

[0113] The pressing device 180 according to this embodiment has a shape in which a first support 192 having a shape in which a part of a cylinder is cut out is connected to one end of a connecting portion 196 forming a part of a torus. In this embodiment, a straight portion 192c is formed by the first support 192. That is, in a plan view, an inner edge 192a of the first support 192 includes a straight portion 192c that extends in a straight line toward a tip 192b on one side in the second direction B so as to be farther away from the second support 194 in the first direction A toward one side in the second direction B. In this specification, the inner edge of the first support in a plan view means an edge on the gap 198 side. The same applies to the inner edge of the second support 194 and the inner edge of the connecting portion 196 in a plan view. In this embodiment, the inner edge 194a of the second support 194 is curved in an arc shape so as to be convex toward the opposite side to the first support 192 in the first direction A. Moreover, an inner edge 196a of the connecting portion 196 is curved in an arc shape so as to be convex toward the other side in the second direction B.

[0114] Although detailed description is omitted, the first support portion 192 has a screw hole penetrating in the first direction A for mounting the first pressing portion 18, similar to the above-mentioned first support portion 162. Also, the second support portion 194 has a screw hole penetrating in the first direction A for mounting the second pressing portion 20, similar to the above-mentioned second support portion 164. The first pressing portion 18 is provided on the first support portion 192 so as to protrude from the first support portion 192 to the second support portion 194 side in the gap 198. The second pressing portion 20 is provided on the second support portion 194 so as to face the first pressing portion 18 in the first direction A and to protrude from the second support portion 194 to the first support portion 192 side in the gap 198.

[0115] In this embodiment, the straight portion 192c formed in a straight line is provided at the end of the first support portion 192, so that the pressing device 180 can be easily disposed within the scallop 174 (see FIG. 17). Specifically, after the straight portion 192c (first support portion 192) is inserted into the scallop 174, the pressing device 180 can be rotated to position the connecting portion 196 inside the scallop 174. This allows the pressing device 180 to be attached to a predetermined position.

[0116] FIG. 20 is a diagram for explaining a method for improving fatigue strength using a pressing device according to this embodiment, in which (a) shows the relationship between the pressing device 150 and the welded joint 170 when the fatigue strength of the welded joint 170 is improved using the above-mentioned pressing device 150, and (b) shows the relationship between the pressing device 180 and the welded joint 170 when the fatigue strength of the welded joint 170 is improved using the pressing device 180.

[0117] Although detailed description will be omitted, as shown in FIG. 20, when the pressing device 180 according to this embodiment is used, the fatigue strength of the welded joint can be improved by the same method as the pressing device 150 described above. Furthermore, in this embodiment, the inner edge 192a of the first support portion 192 is provided with a straight portion 192c that extends in a straight line toward the tip 192b of the inner edge 192a so that the one side in the second direction B is farther away from the second support portion 194 in the first direction A. With this shape, even if the length of the support member 190 in the second direction B is increased, the support member 190 can be appropriately positioned inside the scallop 174 by inserting the support member 190 into the scallop 174 (see FIG. 17) from the first support portion 192 side. As a result, as shown in FIG. 20, when the pressing device 180 is used, a position further away from the weld toe 175b can be pressed by the protruding portion 18b (see FIG. 19) and the protruding portion 20b compared to when the pressing device 150 is used. For example, if a fatigue crack has already occurred at the weld toe 175b, the crack can be closed by pressing a position away from the weld toe 175b with the pressing device 180. It also makes it possible to relax the residual stress at the weld root and reduce the acting stress when fillet welding is performed.

[0118] (Other examples of structural members) In the above embodiment, the pressing device is used to press the metal members of the welded joint to form the indentation, but the structural member pressed by the pressing device is not limited to the welded joint. Fig. 21 is a diagram showing another example of the structural member.

[0119] The structural member 300 shown in FIG. 21 is made of a single plate-shaped metal member. The structural member 300 includes a rectangular main body 302 and a pair of protruding portions 304 that protrude in the width direction at the center in the longitudinal direction of the main body 302. In the structural member 300 having such a shape, when a tensile load is applied in the longitudinal direction to the main body 302, stress concentration occurs at the corners 306a to 306d between the main body 302 and the protruding portions 304. Therefore, for example, as shown in FIG. 21, the above-mentioned pressing device is used to form indentations 46 on both sides of the main body 302 in the vicinity of the corners 306a to 306d. This makes it possible to apply compressive stress in the vicinity of the corners 306a to 306d, thereby improving the fatigue strength of the structural member 300, or to manufacture a structural member 300 with improved fatigue strength. Note that indentations may be formed on both sides of the protruding portions 304 in the vicinity of the corners 306a to 306d, as shown by the dashed lines in FIG. 21. It should be noted that the shape of the structural member 300 shown in FIG. 21 is merely one example, and the present invention can be utilized to improve the fatigue strength of structural members of various shapes having stress concentration portions.

[0120] Furthermore, the pressing device according to each of the above-mentioned embodiments can also improve the fatigue strength near the weld toes of the T-joint shown in Fig. 22(a) and the out-of-plane gusset joint shown in Fig. 22(b). In Fig. 22(a) and (b), the locations where fatigue cracks may occur are indicated by dashed circles, and indentations 46 formed by the pressing device to suppress the occurrence of fatigue cracks are also shown. In Fig. 22(a) and (b), the direction of the force acting on the joint is indicated by an arrow.

[0121] As a specific example of application of the pressing device according to each of the above-mentioned embodiments to an out-of-plane gusset joint, application to a reinforcing material of a lighting pole can be considered as shown in Fig. 23. In the example of Fig. 23, an indentation 46 is formed by the pressing device near the weld toe on the reinforcing material side of the welded part joining the reinforcing material and the base. Conventionally, measures have been taken to improve fatigue strength near the weld toe on the upper end side of the welded part joining the lighting pole and the reinforcing material, but the pressing device according to the present invention can also take measures near the weld toe on the reinforcing material side of the welded part joining the reinforcing material and the base, thereby further improving the fatigue life of the base part of the lighting pole. EXAMPLES

[0122] Tests 1, 2, and 3 described below were carried out to confirm the effects of the present invention.

[0123] (Test 1) Welded structure specimens having scallops of Example 1 and Comparative Example 1 were fabricated and subjected to fatigue testing. Fig. 24 shows the welded structure specimen of Example 1, where (a) is a front view, (b) is a side view, and (c) is an enlarged view showing the part surrounded by the dashed line in (a). Note that, although values ​​showing the dimensions of each part of the welded structure specimen 500 are shown in Fig. 24, the unit of the values ​​is "mm".

[0124] 24, the welded structure specimen 500 includes four plate-shaped metal members 502, 504, 506, and 508. A 490 MPa-class rolled steel material for welded structure (SM490B JIS G3106:2020) was used as the metal members 502, 504, 506, and 508. When the welded structure specimen 500 is viewed from above, the thickness direction of the metal member 504 and the thickness directions of the metal members 506 and 508 are perpendicular to each other.

[0125] Metal member 504 is joined to the upper surface of metal member 502 by welds 510 and 512. A scallop 504a is formed in the center of the lower part of metal member 504. Metal member 506 is provided so as to pass through scallop 504a. Metal member 506 is joined to the upper surface of metal member 502 by welds 514 and 516. Metal member 508 is joined to the lower surface of metal member 502 by welds 518 and 520.

[0126] As shown in Figure 24(c), an indentation 46 with a depth of about 0.25 mm was formed on both sides of the metal member 504 in the vicinity of the weld toe 510a of the weld 510 on the metal member 504 side, using the pressing device 10 shown in Figure 1. An indentation 46 was also formed in the vicinity of the weld toe 512a of the weld 512 on the metal member 504 side in a similar manner.

[0127] The welds 510 and 512 were fully penetrated in order to avoid fracture from the weld root. In the fatigue test, ultrasonic impact treatment (UIT) was applied to the weld toes other than the weld toes 510a and 512a of the weld 510 on the metallic member 504 side and the weld toe 512a of the weld 512 on the metallic member 504 side, respectively, to prevent cracks from occurring in the weld toes. The welded structure specimen of Comparative Example 1 had the same configuration as the welded structure specimen 500 of Example 1, except that the indentation 46 was not formed.

[0128] Three welded structure specimens 500 of Example 1 having the above configuration were fabricated, and fatigue tests (Tests Nos. 1 to 3) were conducted in which repeated tensile loads were applied in the vertical direction. Four welded structure specimens of Comparative Example 1 were fabricated, and similar fatigue tests (Tests Nos. 4 to 7) were conducted. In these fatigue tests, the minimum load was fixed at 3.5 kN, assuming a structure with a constant dead load such as a bridge. The maximum load was 50 kN for Tests Nos. 1, 2 and 4, 5, and 35 kN for Tests Nos. 3, 6, and 7. The test conditions are shown in Table 1 below, and the test results are shown in FIG. 25.

[0129] [Table 1]

[0130] The number of repetitions shown in FIG. 25 is the number of load repetitions when a crack initiates from the weld toe 510a or the weld toe 512a and the crack length reaches 10 mm on the surface of the metal member 504 or on the welds 510, 512.

[0131] In the fatigue test of the welded structure specimens of Test Nos. 1 and 2, where the maximum load was set to 50 kN, a crack occurred at the weld root, not the evaluation area (weld toes 510a and 512a), and the test was stopped at the point where the crack occurred. Even when evaluated at that point, the fatigue life was improved by more than 15 times compared to the welded structure specimens of Test Nos. 4 and 5, which were subjected to the same load conditions. In the fatigue test of the welded structure specimen of Test No. 3, where the maximum load was set to 35 kN, no sign of crack initiation was observed, so the test was stopped midway.

[0132] From the above test results, it has been found that by pressing the vicinity of the weld toe of a weld, which is a stress concentration area, using the pressing device according to the present invention, it is possible to significantly improve fatigue strength compared to an as-welded welded structure specimen.

[0133] (Test 2) In Test 2, in-plane gusset welded joints of Example 2, Comparative Example 2, and Reference Example were fabricated and subjected to fatigue testing. FIG. 26 is a diagram showing the in-plane gusset welded joint of Example 2. As shown in FIG. 26, the in-plane gusset welded joint 600 of Example 2 includes a plate-shaped metal member (main plate) 602 and plate-shaped metal members (gussets) 604, 606 joined to both side surfaces of the metal member 602. FIG. 26 shows a part of the metal member 602. General structural rolled steel (SS400 JIS G3101:2020) was used as the metal members 602, 604, 606. FIG. 26 shows numerical values ​​indicating the dimensions of each part of the in-plane gusset welded joint 600, but the unit is "mm". The total length of the metal member 602 is about 1000 mm. During the fatigue test described later, about 150 mm portions of both ends of the metal member 602 were gripped by hydraulic chucks. The metal members 604 and 606 have the same dimensions.

[0134] The metal member 604 is joined to one side of the metal member 602 by a weld 608, and the metal member 606 is joined to the other side of the metal member 602 by a weld 610. The welds 608 and 610 are fully welded from both sides to avoid fracture from the weld root. The thickness of the metal member 602 is 19 mm, and the thickness of the metal members 604 and 606 is 9 mm.

[0135] Indentations 46 with a diameter of about 10 mm and a depth of about 0.45 mm were formed on both sides of the metal member 602 near the weld toes 608a, 608b of the weld 608 on the metal member 602 side, using the pressing device 80 shown in Fig. 11. Indentations 46 were also formed similarly in the vicinity of the weld toes 610a, 610b of the weld 610 on the metal member 602 side.

[0136] The in-plane gusset welded joint of Comparative Example 2 had the same configuration as the in-plane gusset welded joint 600 of Example 2, except that no indentation 46 was formed. The in-plane gusset welded joint of Reference Example had the same configuration as the in-plane gusset welded joint 600 of Example 2, except that instead of forming the indentation 46, ultrasonic impact treatment (UIT) was performed on the weld toes 608a, 608b, 610a, and 610b.

[0137] A plurality of in-plane gusset welded joints of Example 2, Comparative Example 2, and Reference Example were fabricated, and fatigue tests were conducted by applying tensile stress in the vertical direction. The test results are shown in Fig. 27. The number of repetitions shown in Fig. 27 is the number of repetitions of the stress when a crack occurs at any one of the weld toes 608a, 608b, 610a, and 610b, and the crack length reaches 10 mm on the surface of the metal member 602.

[0138] From the results shown in Fig. 27, it was found that by pressing the vicinity of the weld toe of the weld (the vicinity of the weld toe at the gusset end), which is a stress concentration area, with the pressing device according to the present invention, the fatigue strength can be significantly improved compared to an as-welded in-plane gusset welded joint. It was also found that the pressing device according to the present invention can provide a fatigue strength improvement effect equal to or greater than that of ultrasonic impact treatment (UIT).

[0139] (Test 3) In Test 3, a fatigue test was performed on an in-plane gusset welded joint having the same configuration as in Comparative Example 2 described above. Specifically, the fatigue test was performed with a stress range of 155 MPa and a stress ratio of 0.05, and fatigue cracks were generated at the weld toes 608a, 608b, 610a, and 610b (see FIG. 26). When the generated fatigue cracks for each of the weld toes 608a, 608b, 610a, and 610b satisfied a predetermined condition (when the fatigue crack penetrated the metal member 602 in the thickness direction and propagated about 2 to 3 mm on the surface of the metal member 602), the fatigue test was temporarily stopped, and an indentation 46 with a diameter of 10 mm and a depth of about 0.45 mm was formed on both sides using the pressing device 80 shown in FIG. 11. After the indentation 46 was formed, the fatigue test was resumed. Since the fatigue cracks generated at each of the weld toes 608a, 608b, 610a, and 610b did not satisfy the above condition at the same time, the fatigue test was stopped, the indentation 46 was formed (fatigue strength improvement treatment), and the fatigue test was resumed four times. After the fatigue test was resumed for the fourth time, the fatigue test was continued until the number of repetitions reached 2.6 million. The indentation 46 was formed so that a part of the fatigue crack was closed. The position where the indentation 46 was formed is the same as the position shown in FIG. 26. The test results are shown in FIG. 28. In FIG. 28, "□" indicates the number of repetitions when the fatigue cracks generated at each of the weld toes 608a, 608b, 610a, and 610b satisfied the above condition (when the indentation for fatigue strength improvement was formed). In FIG. 28, "◯" indicates the number of repetitions for each of the weld toes 608a, 608b, 610a, and 610b after the fatigue strength improvement treatment. In addition, in Fig. 28, the number of repetitions (2.6 million times) for the four weld toes 608a, 608b, 610a, and 610b after the fatigue strength improvement treatment is plotted in one place, and is therefore shown as one "◯." In other words, in Fig. 28, four "◯"s indicating the number of repetitions for the four weld toes 608a, 608b, 610a, and 610b after the fatigue strength improvement treatment are shown overlapping each other.

[0140] In this test, none of the fatigue cracks that occurred at the weld toes 608a, 608b, 610a, and 610b caused fatigue failure. In other words, even if fatigue cracks occurred at each of the weld toes 608a, 608b, 610a, and 610b, by carrying out the fatigue strength improvement method according to the present invention, the cracks hardly propagate on the surface even at a number of repetitions that is one order of magnitude higher than the number of repetitions at which the cracks occurred, and therefore the cracks do not reach 10 mm, and fatigue failure of the in-plane gusset welded joint can be prevented. From this result, it was found that the fatigue strength improvement method according to the present invention can sufficiently suppress the further propagation and enlargement of fatigue cracks even when the fatigue cracks occur at the weld toes, which are stress concentration parts of the welded joint. [Industrial Applicability]

[0141] According to the present invention, compressive stress can be easily applied to the toes of welded joints in various structures, thereby making it possible to suppress the initiation of fatigue cracks from the weld toes and, even if a crack has already been initiated at the weld toes, to suppress the propagation of the cracks. [Explanation of symbols]

[0142] 10,80,100,150,180 Pressing device 12,82,102,162,192 1st support part 14,84,104,164,194 2nd support part 16,86,106,166,196 Connection part 18 First pressing part 20 Second pressing part 22,88,112,168,198 Gap

Claims

1. A pressing device for pressing a metal member to form an indentation, A first support portion; a second support portion facing the first support portion in a first direction such that a gap is formed between the second support portion and the first support portion; a connecting portion that connects the first support portion and the second support portion; a first pressing portion provided on the first support portion and having one tip protruding toward the second support portion; a second pressing portion provided on the second support portion so as to face the first pressing portion, the second pressing portion having one tip protruding toward the first support portion; Equipped with A pressing device, wherein a distance between the first pressing portion and the second pressing portion in the first direction is adjustable.

2. The pressing device according to claim 1 , wherein the first support portion, the second support portion and the connecting portion are integrally formed.

3. The first support portion has a first screw hole formed therein and penetrating therethrough in the first direction, 2. The pressing device according to claim 1, wherein the first pressing portion comprises: a first screw portion screwed into the first screw hole; and a first protrusion provided at a tip of the first screw portion and protruding from the first support portion toward the second support portion in the gap.

4. The pressing device according to claim 3 , wherein a tip surface of the first protrusion has a flat shape perpendicular to the first direction and a circular shape having a diameter smaller than a diameter of the first screw portion when viewed from the first direction.

5. 4. The pressing device according to claim 3, wherein a tip of the first protrusion is rotationally symmetric about an axis of the first screw portion and has a surface that is curved so as to be convex toward the second support portion.

6. the first support portion and the second support portion are provided to extend to one side in a second direction perpendicular to the first direction relative to the connecting portion, 2. The pressing device according to claim 1, wherein, when viewed from the second direction, the gap extends in a third direction perpendicular to the first direction, and the distance in the first direction gradually increases on one side in the third direction.

7. The pressing force is applied to the metal member having a notch formed therein penetrating in a predetermined direction, The pressing device according to claim 1 , wherein the pressing device can be inserted into the notch with the first direction being aligned with the predetermined direction.

8. When viewed from the first direction, a direction in which the connecting portion and the first pressing portion are aligned is defined as an X direction, and a direction perpendicular to the X direction is defined as a Y direction.

2. The pressing device according to claim 1, wherein, when viewed from the first direction, the first support portion and the second support portion each have a shape obtained by cutting out each corner of a virtual rectangle formed by a pair of long sides parallel to the X direction and a pair of short sides parallel to the Y direction.

9. The pressing device according to claim 8 , wherein, when viewed from the first direction, the first support portion and the second support portion each fall within a quadrant having a radius of 35 mm.

10. The second support portion has a second screw hole formed therein, the second screw hole penetrating in the first direction.

2. The pressing device according to claim 1, wherein the second pressing portion comprises: a second screw portion screwed into the second screw hole; and a second protruding portion provided at a tip of the second screw portion and protruding from the second support portion toward the first support portion in the gap.

11. A portion of the connecting portion facing the gap has a first surface extending in a second direction perpendicular to the first direction, a second surface extending in a third direction perpendicular to the first direction and the second direction, and a third surface connecting the first surface and the second surface, the first surface is provided on one side of the second surface in the third direction, the second surface is provided on one side of the first surface in the second direction, and the third surface extends from an edge of the first surface on the one side in the second direction toward an edge of the second surface on the one side in the third direction, obliquely extending with respect to the second direction and the third direction; The pressing device according to claim 1 , wherein the first pressing portion and the second pressing portion protrude into the gap on the one side of the first surface in the third direction.

12. The pressing device according to claim 1 , wherein the first support portion, the second support portion, and the connecting portion are configured by separate members.

13. The connecting portion includes a first bolt, a nut, and a second bolt having a curved tip portion, the first support portion has a first through hole penetrating in the first direction and a screw hole penetrating in the first direction, the second support portion has a second through hole that faces the first through hole in the first direction and penetrates in the first direction, and a curved recess that faces the screw hole in the first direction and is recessed toward the opposite side to the first support portion in the first direction, the first bolt is inserted into the first through hole and the second through hole; the nut is attached to a tip portion of the first bolt such that the first support portion and the second support portion are sandwiched between a head portion of the first bolt and the nut; The pressing device according to claim 12 , wherein the second bolt is screwed into the screw hole from the outside of the first support part so that the tip portion fits into the recess.

14. the first support portion has a first thin plate portion and a first thick plate portion that protrudes toward the second support portion in the first direction relative to the first thin plate portion, the second support portion has a second thin plate portion and a second thick plate portion that protrudes toward the first support portion in the first direction relative to the second thin plate portion, the gap includes an insertion gap between the first thin plate portion and the second thin plate portion and an adjustment gap between the first thick plate portion and the second thick plate portion, The first thick plate portion has a first support surface facing the insertion gap, the second thick plate portion has a second support surface provided at the same position as the first support surface when viewed from the first direction so as to face the insertion gap, each of the first support surface and the second support surface has a first surface extending in a second direction perpendicular to the first direction, a second surface extending in a third direction perpendicular to the first direction and the second direction, and a third surface connecting the first surface and the second surface; the first surface is provided on one side of the second surface in the third direction, the second surface is provided on one side of the first surface in the second direction, and the third surface extends from an edge of the first surface on the one side in the second direction toward an edge of the second surface on the one side in the third direction, obliquely extending with respect to the second direction and the third direction; the first pressing portion and the second pressing portion protrude into the insertion gap on the one side of the first surface in the third direction, the first bolt and the second bolt are provided to pass through the adjustment gap in the first direction, The pressing device according to claim 13 , wherein the first pressing portion, the first bolt, and the second bolt are arranged in this order in the third direction.

15. The pressing device according to claim 2 , wherein the first support portion, the connecting portion and the second support portion are integrally formed in an arc shape.

16. The first support portion has a first screw hole formed therein and penetrating therethrough in the first direction, The second support portion has a second screw hole formed therein, the second screw hole penetrating in the first direction. the first pressing portion includes a first screw portion screwed into the first screw hole, and a first protruding portion provided at a tip of the first screw portion and protruding from the first support portion toward the second support portion in the gap, 16. The pressing device according to claim 15, wherein the second pressing portion comprises: a second screw portion screwed into the second screw hole; and a second protruding portion provided at a tip of the second screw portion and protruding from the second support portion toward the first support portion in the gap.

17. the first support portion and the second support portion are provided on one side of the connecting portion in a second direction perpendicular to the first direction, 17. The pressing device according to claim 16, wherein, when viewed from a third direction perpendicular to the first direction and the second direction, an inner edge of the first support portion includes a straight portion that extends linearly toward a tip of the one side in the second direction so as to be away from the second support portion in the first direction toward the one side in the second direction.

18. A method for manufacturing a structural member having a plate-shaped metal member, comprising the steps of: A method for manufacturing a structural member, comprising the step of pressing the metal member with the pressing device according to claim 1 .

19. A method for improving fatigue strength of a structural member, comprising pressing said metal plate-shaped member of the structural member by the pressing device according to claim 1.

Citation Information

Patent Citations

  • Metallic plate member having different widths excellent in fatigue crack development and propagation suppressing characteristic, and metallic structure using the same

    JP2007275913A