Image recorded matter and method for manufacturing the same, as well as laminate body and method for manufacturing the same

By applying a pretreatment liquid and inks with controlled resin ratios and surface tensions, the method addresses lamination strength issues in image recording materials, achieving a stable and uniform laminate structure.

JP2024133075AActive Publication Date: 2024-10-01FUJIFILM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024104251
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-10-29
Filing Date
2024-06-27
Publication Date
2024-10-01
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Existing image recording methods on impermeable substrates face challenges in achieving strong lamination strength when a laminating base material is applied over the image, leading to issues with adhesion and unevenness.

Method used

A method involving the application of a pretreatment liquid containing a flocculant, followed by a first ink and a second ink with specific resin ratios and surface tensions, to create an image recording material with controlled resin aggregation, ensuring the lamination strength between the image and the laminating base material.

Benefits of technology

The method enhances the lamination strength and reduces surface irregularities, resulting in a stable laminate structure with improved adhesion and uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133075000001
    Figure 2024133075000001
  • Figure 2024133075000002
    Figure 2024133075000002
Patent Text Reader

Abstract

To provide an image recorded matter which is excellent in laminate strength when a base material for laminate is laminated on an image and a method for manufacturing the same, as well as a laminate body and a method for manufacturing the same.SOLUTION: There are provided: a method for manufacturing an image recorded matter which includes an image recording step of imparting a pretreatment liquid containing a coagulant and water, first ink containing a first pigment, a first resin, and water, and second ink which contains a second pigment, a second resin, and water and has surface tension smaller than surface tension of the first ink, in this order, onto a non-permeable base material, and recording an image, where the image recording step is performed in an overlapping region where a region where the pretreatment liquid is imparted, a region where the first ink is imparted and a region where the second ink is imparted overlap in plan view, under the condition that a ratio of the total imparting mass of the first resin and the second resin per unit area with respect to an imparting mass of the coagulant per unit area is 16.0 or more and 30.0 or less; an image recorded matter; and a laminate and a method for manufacturing the same.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an image recorded matter and a manufacturing method thereof, and a laminated body and a manufacturing method thereof. [Background technology]

[0002] In recent years, research has been conducted on a technique for recording an image using ink and a pretreatment liquid (also called a reaction liquid or the like) that contains an aggregating agent that aggregates components in the ink.

[0003] For example, Patent Document 1 discloses an inkjet recording method capable of reducing the odor of a reactant and obtaining a recorded matter of high image quality, the inkjet recording method comprising a recording step of adhering a reaction liquid and one or more inkjet ink compositions to a low-absorbency or non-absorbency recording medium, the reaction liquid containing a reactant which is a carboxylic acid or a carboxylate that reacts with a component of the inkjet ink composition, the inkjet ink composition containing a resin and water, and the reaction liquid and the inkjet ink composition are adhered such that, when the adhesion amount of a region with the greatest adhesion amount of the resin per unit area in an adhesion region of the inkjet ink composition on the low-absorbency or non-absorbency recording medium is taken as 100%, the mass ratio of the adhesion amount of the resin to the adhesion amount of the reactant (the resin / the reactant) in the adhesion region where the adhesion amount of the resin is 20% or more and 100% or less is 1.5 or more and 16 or less.

[0004] Patent Document 2 discloses an inkjet recording method capable of obtaining recorded matter with excellent image quality and abrasion resistance, the inkjet recording method comprising: a reaction liquid applying step of applying a reaction liquid containing an aggregating agent that aggregates components of an aqueous ink composition to a recording region of a recording medium; and an ink composition applying step of ejecting an aqueous ink composition containing a pigment dispersion containing a surface-treated pigment and water from an inkjet head to apply the aqueous ink composition to the recording region of the recording medium, the inkjet recording method having an area in which the amount of the aqueous ink composition applied is 2 to 20 times the amount of the reaction liquid applied. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-217591 A [Patent Document 2] JP 2018-165029 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, after an image is recorded on a non-permeable substrate to obtain an image recorded matter, a substrate for lamination may be laminated onto the image in the image recorded matter. In this case, it may be necessary to improve the lamination strength between the image recorded matter and the substrate for lamination.

[0007] An object of one embodiment of the present disclosure is to provide an image recorded material comprising a non-permeable substrate and an image recorded on the non-permeable substrate, the image recorded material having excellent lamination strength when a substrate for lamination is laminated onto the image, and a method for producing the image recorded material capable of producing the image recorded material. An object of another aspect of the present disclosure is to provide a laminated body comprising the image recorded matter and a substrate for lamination laminated onto the image of the image recorded matter, the laminated body having excellent lamination strength between the image and the substrate for lamination, and a method for producing the laminated body capable of producing the laminated body. [Means for solving the problem]

[0008] Specific means for solving the problems include the following aspects. <1> A step of preparing a pretreatment liquid containing water and at least one flocculant selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex; preparing a first ink containing a first pigment, a first resin, and water; preparing a second ink containing a second pigment, a second resin, and water, the second ink having a surface tension lower than that of the first ink; an image recording step of applying a pretreatment liquid, a first ink, and a second ink in this order onto a non-permeable substrate to record an image; Including, The image recording process is a method for producing an image recorded product, in which an image is recorded under conditions in which an overlapping region is generated in which an area to which a pretreatment liquid is applied, an area to which a first ink is applied, and an area to which a second ink is applied overlap in a planar view, and under conditions in which, in the overlapping region, the ratio of the total applied mass of the first resin and the second resin per unit area to the applied mass of the coagulant per unit area is 16.0 or more and 30.0 or less. <2> The above ratio is between 16.0 and 25.0. <1> 13. A method for producing the image recorded matter described in claim 12. <3> the content of organic solvents having a boiling point of 220° C. or higher relative to the total amount of the first ink is 5 mass % or less; The content of organic solvents having a boiling point of 220° C. or higher in the total amount of the second ink is 5% by mass or less. <1> or <2> 13. A method for producing the image recorded matter described in claim 12. <4> The pretreatment liquid contains a resin, the first resin comprises resin particles; The glass transition temperature of the resin contained in the pretreatment liquid is lower than the glass transition temperature of the resin particles contained in the first resin. <1> ~ <3> 13. A method for producing an image recorded matter according to any one of the above items. <5> the first resin comprises resin particles; the second resin comprises resin particles; In the overlapping region of the resin particles contained in the first resin and the resin particles contained in the second resin, the glass transition temperature of the resin particle having a larger applied mass per unit area is defined as Ta, and the glass transition temperature of the resin particle having a smaller applied mass per unit area is defined as Tb, where Ta and Tb satisfy the relationship 0°C≦Ta-Tb≦30°C. <1> ~ <4> 13. A method for producing an image recorded matter according to any one of the above items. <6> If the viscosity of the mixture of the pretreatment liquid and the first ink is A1, and the viscosity of the mixture of the pretreatment liquid and the second ink is A2, A1 and A2 satisfy A1-A2>0 mPa s. <1> ~ <3> 13. A method for producing an image recorded matter according to any one of the above items. <7> <1> ~ <6> obtaining an image recorded material by the method for producing an image recorded material according to any one of the above items; A step of laminating a substrate for lamination onto the side of the image recorded product on which the image is recorded to obtain a laminate; A method for producing a laminate comprising the steps of: <8> a non-permeable substrate; and an image recorded on the non-permeable substrate; the image includes a pretreatment layer in contact with the non-permeable substrate and containing a flocculant, a first layer in contact with the pretreatment layer and containing a first pigment and a first resin, and a second layer in contact with the first layer and containing a second pigment and a second resin, and includes an overlapping region in which the pretreatment layer, the first layer, and the second layer overlap in a planar view; The flocculant is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex; An image recorded matter, in which in the overlapping region, the ratio of the total mass of the first resin and the second resin per unit area to the mass of the flocculant per unit area is 16.0 or more and 30.0 or less. <9> <8> and an image recording material according to the above. a lamination substrate laminated onto an image of an image recording material; A laminate body comprising: Effect of the Invention

[0009] According to one aspect of the present disclosure, there is provided an image recorded material comprising a non-permeable substrate and an image recorded on the non-permeable substrate, the image recorded material having excellent lamination strength when a substrate for lamination is laminated onto the image, and a method for producing the image recorded material capable of producing the image recorded material. According to another aspect of the present disclosure, there is provided a laminated body comprising the above-mentioned image recorded matter and a lamination substrate laminated onto the image of the image recorded matter, the laminated body having excellent lamination strength between the image and the lamination substrate, and a method for producing the laminated body capable of producing the above-mentioned laminated body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the numerical ranges described in stages in this disclosure, the upper or lower limit value described in a certain numerical range may be replaced by the upper or lower limit value of another numerical range described in stages, or may be replaced by a value shown in the examples. In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In this disclosure, combinations of preferred aspects are more preferred aspects.

[0011] In this disclosure, the term "image" refers generally to a film formed by applying a pretreatment liquid, a first ink, and a second ink in this order onto a non-permeable substrate, and the terms "image recording" and "image recording" refer to film formation and film formation, respectively. Additionally, the concept of "image" in this disclosure also includes solid images.

[0012] [Method for producing image recording material] The method for producing an image recorded matter according to the present disclosure includes: A step of preparing a pretreatment liquid containing water and at least one flocculant selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex; preparing a first ink containing a first pigment, a first resin, and water; preparing a second ink containing a second pigment, a second resin, and water, the second ink having a surface tension lower than that of the first ink; an image recording step of applying a pretreatment liquid, a first ink, and a second ink in this order onto a non-permeable substrate to record an image; Including, In the image recording process, an image is recorded under conditions where an overlapping region is generated in which the region to which the pretreatment liquid is applied, the region to which the first ink is applied, and the region to which the second ink is applied overlap in a planar view, and where in the overlapping region, the ratio of the total applied mass of the first resin and the second resin per unit area to the applied mass of the coagulant per unit area (hereinafter also referred to as "application mass ratio [(first resin + second resin) / coagulant]" or "application amount ratio [resin / coagulant]") is 16.0 or more and 30.0 or less.

[0013] According to the manufacturing method of the image recording material disclosed herein, it is possible to produce an image recording material comprising a non-permeable substrate and an image recorded on the non-permeable substrate, and which has excellent lamination strength when a substrate for lamination is laminated onto the image. Here, the laminate strength refers to the peel strength when peeling off the substrate for lamination and the image recording material in a laminated body formed by the above-mentioned lamination (i.e., a laminated body having a layered structure of "substrate for lamination / image recording material" (more specifically, a layered structure of "substrate for lamination / image / non-permeable substrate")).

[0014] The reason why the method for producing an image recorded matter according to the present disclosure exhibits the above-mentioned effects is presumed to be as follows. In order to improve the laminate strength in a laminate, it is necessary to first improve the adhesion between the non-permeable substrate and the image, and then to improve the adhesion between the image and the substrate for lamination. In the image recording step in the manufacturing method of the image recorded matter of the present disclosure, the pretreatment liquid, the first ink, and the second ink are applied in this order onto the non-permeable substrate. That is, the pretreatment liquid is applied onto the non-permeable substrate, the first ink is applied onto the applied pretreatment liquid, and the second ink is applied onto the applied first ink. The pretreatment liquid, the first ink, and the second ink are applied under conditions (i.e., application arrangement) that generate an overlapping region in which the region to which the pretreatment liquid is applied, the region to which the first ink is applied, and the region to which the second ink is applied overlap in a plan view. As a result, on the non-permeable substrate, the components in the first ink (mainly the first resin) and the components in the second ink (mainly the second resin) applied onto the pretreatment liquid are aggregated by the action of the aggregating agent, which is a component of the pretreatment liquid, to obtain an image. Here, in the overlapping region, by setting the applied mass ratio [(first resin + second resin) / aggregant] to 30.0 or less, it is believed that insufficient aggregation of the first resin and the second resin is suppressed, and a decrease in adhesion between the non-permeable substrate and the image caused by insufficient aggregation is suppressed. In addition, in the overlapping region, by setting the applied mass ratio [(first resin + second resin) / aggregant] to 16.0 or more, it is considered that excessive aggregation of the first resin and the second resin is suppressed, and unevenness of the image surface and / or unevenness of the image thickness caused by excessive aggregation are suppressed. As a result, it is considered that a decrease in adhesion between the image and the lamination substrate caused by unevenness of the image surface and / or unevenness of the image thickness is suppressed. Furthermore, since the surface tension of the second ink is smaller than that of the first ink, the wetting and spreading property of the second ink on the first ink is improved in the overlapping region, and as a result, unevenness of the image surface and / or unevenness of the image thickness are suppressed, which is thought to suppress a decrease in adhesion between the image and the lamination substrate caused by unevenness of the image surface and / or unevenness of the image thickness. As described above, in the manufacturing method of the image recording material disclosed herein, adhesion between the non-permeable substrate and the image is ensured, and adhesion between the image and the substrate for lamination is also ensured, and as a result, it is believed that the lamination strength is ensured.

[0015] Hereinafter, each step that may be included in the method for producing an image recorded matter according to the present disclosure will be described.

[0016] <Preparing the pretreatment liquid> The process of preparing a pretreatment liquid (hereinafter also referred to as the "pretreatment liquid preparation process") is a process of preparing a pretreatment liquid containing water and a flocculant which is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex. The pretreatment liquid preparation step may be a step of simply preparing a pretreatment liquid that has been produced in advance, or may be a step of producing a pretreatment liquid. There is no particular limitation on the method for producing the pretreatment liquid, and any known method for mixing the components can be used.

[0017] (water) The pretreatment liquid contains water. The water content is preferably 50% by mass or more, and more preferably 60% by mass or more, based on the total amount of the pretreatment liquid. The upper limit of the water content depends on the amounts of other components, but is preferably 90 mass % or less based on the total amount of the pretreatment liquid.

[0018] (Flocculant) The pretreatment liquid is prepared by preparing a flocculant which is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex. The aggregating agent is a component that aggregates components (for example, the first resin and the second resin) in the inks (that is, the first ink and the second ink; the same applies below).

[0019] -Organic acid- The organic acid includes an organic compound having an acidic group. Examples of the acidic group include a phosphoric acid group, a phosphonic acid group, a phosphinic acid group, a sulfuric acid group, a sulfonic acid group, a sulfinic acid group, and a carboxy group. From the viewpoint of the aggregation rate of the ink, the acidic group is preferably a phosphate group or a carboxy group, and more preferably a carboxy group. It is preferable that the acidic groups are at least partially dissociated in the pretreatment liquid.

[0020] Preferred organic compounds having a carboxy group include polyacrylic acid, acetic acid, formic acid, benzoic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, fumaric acid, citric acid, tartaric acid, phthalic acid, adipic acid, pimelic acid, 4-methylphthalic acid, lactic acid, pyrrolidone carboxylic acid, pyrone carboxylic acid, pyrrole carboxylic acid, furan carboxylic acid, pyridine carboxylic acid, coumaric acid, thiophene carboxylic acid, nicotinic acid, pimelic acid, etc. These compounds may be used alone or in combination of two or more.

[0021] From the viewpoint of the aggregation speed of the ink, the organic compound having a carboxy group is preferably a divalent or higher carboxylic acid (hereinafter also referred to as a polyvalent carboxylic acid). Polycarboxylic acids include: Dicarboxylic or tricarboxylic acids are preferred, More preferred are glutaric acid, malonic acid, succinic acid, adipic acid, pimelic acid, malic acid, maleic acid, fumaric acid, tartaric acid, or citric acid; More preferably, the acid is glutaric acid, malonic acid, succinic acid, adipic acid, pimelic acid, malic acid, fumaric acid, tartaric acid, or citric acid; More preferred are glutaric acid, malonic acid, succinic acid, adipic acid, or pimelic acid.

[0022] The organic acid preferably has a low pKa (for example, 1.0 to 5.0). This reduces the surface charge of particles such as pigments and polymer particles in the ink, which are stabilized by weakly acidic functional groups such as carboxy groups, by contacting them with an organic acidic compound with a lower pKa, thereby lowering the dispersion stability.

[0023] The organic acid preferably has a low pKa, high solubility in water, and a valence of divalent or greater, and is more preferably a divalent or trivalent acidic substance that has a high buffering capacity in a pH range lower than the pKa of the functional group (e.g., a carboxy group) that stabilizes the dispersion of the particles in the ink.

[0024] -Organic acid salt- Examples of the organic acid salt include salts of the organic acids exemplified above. Organic acid salts include those containing alkaline earth metals from Group 2 of the periodic table (e.g., magnesium, calcium), transition metals from Group 3 of the periodic table (e.g., lanthanum), cations from Group 13 of the periodic table (e.g., aluminum), and lanthanides (e.g., neodymium). As the organic acid salt, an organic acid salt containing an alkaline earth metal is preferable, and an organic acid salt containing calcium (for example, calcium lactate, calcium acetate, etc.) or an organic acid salt containing magnesium (for example, magnesium lactate, magnesium acetate, etc.) is preferable.

[0025] -Polyvalent metal compounds- Examples of polyvalent metal compounds include salts (excluding organic acid salts) containing at least one selected from the group consisting of alkaline earth metals of Group 2 of the periodic table (e.g., magnesium, calcium), transition metals of Group 3 of the periodic table (e.g., lanthanum), cations from Group 13 of the periodic table (e.g., aluminum), and lanthanides (e.g., neodymium). The polyvalent metal compound is preferably a nitrate, chloride, or thiocyanate. Particularly preferred polyvalent metal compounds are calcium or magnesium nitric acid salts, calcium chloride, magnesium chloride, or calcium or magnesium thiocyanate salts. The polyvalent metal compound is preferably at least partially dissociated into polyvalent metal ions and counter ions in the pretreatment liquid.

[0026] -Metal complexes- The metal complex is preferably a metal complex containing, as a metal element, at least one selected from the group consisting of zirconium, aluminum, and titanium. The metal complex is preferably a metal complex containing, as a ligand, at least one selected from the group consisting of acetate, acetylacetonate, methyl acetoacetate, ethyl acetoacetate, octylene glycolate, butoxy acetylacetonate, lactate, lactate ammonium salt, and triethanolamine.

[0027] As the metal complex, various metal complexes are commercially available, and in the present disclosure, commercially available metal complexes may be used. In addition, various organic ligands, particularly various multidentate ligands that can form metal chelate catalysts, are commercially available. Therefore, a metal complex prepared by combining a commercially available organic ligand with a metal may be used.

[0028] The content of the flocculant is not particularly limited. From the viewpoint of the aggregation speed of the ink, the content of the aggregating agent relative to the total amount of the pretreatment liquid is preferably 0.1% by mass to 40% by mass, more preferably 0.1% by mass to 30% by mass, even more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 10% by mass.

[0029] (resin) The pretreatment liquid preferably contains at least one type of resin. When the pretreatment liquid contains a resin, the adhesion of the image is further improved.

[0030] When the pre-treatment liquid contains a resin, the glass transition temperature (Tg) of the resin contained in the pre-treatment liquid is preferably 0° C. or higher, more preferably 10° C. or higher, even more preferably 20° C. or higher, and even more preferably 30° C. or higher. When the pretreatment liquid contains a resin, the glass transition temperature (Tg) of the resin contained in the pretreatment liquid is preferably 120° C. or lower, more preferably 100° C. or lower, even more preferably 80° C. or lower, and even more preferably 70° C. or lower.

[0031] In this disclosure, the glass transition temperature of a resin means a value measured using differential scanning calorimetry (DSC). The glass transition temperature is specifically measured according to the method described in JIS K 7121 (1987) or JIS K 6240 (2011). The glass transition temperature in the present disclosure is the extrapolated glass transition onset temperature (hereinafter, sometimes referred to as Tig). The method for measuring the glass transition temperature will now be described more specifically. When determining the glass transition temperature, the temperature is maintained at about 50°C lower than the expected glass transition temperature of the resin until the apparatus stabilizes, and then the temperature is heated at a heating rate of 20°C / min to a temperature about 30°C higher than the temperature at which the glass transition ends, and a differential thermal analysis (DTA) curve or DSC curve is prepared. The extrapolated glass transition onset temperature (Tig), i.e., the glass transition temperature in the present disclosure, is determined as the temperature at the intersection of a straight line extending from the low-temperature side baseline of a DTA curve or DSC curve to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change in the glass transition is maximum.

[0032] When the pretreatment liquid contains two or more types of resins, the glass transition temperature (Tg) of the resins in the pretreatment liquid means the weighted average of the glass transition temperatures of the individual resins.

[0033] Examples of resins that can be contained in the pretreatment liquid include acrylic resins, polyester resins, polyolefin resins, polyurethane resins, polyurea resins, polyamide resins, polycarbonate resins, and polystyrene resins. The resin that can be contained in the pretreatment liquid preferably contains a polyester resin or an acrylic resin, and more preferably contains a polyester resin.

[0034] In the present disclosure, the acrylic resin refers to a polymer (homopolymer or copolymer) of raw material monomers including at least one selected from the group consisting of acrylic acid, derivatives of acrylic acid (e.g., acrylic acid esters, etc.), methacrylic acid, and derivatives of methacrylic acid (e.g., methacrylic acid esters, etc.). In the present disclosure, the polyester resin refers to a polymer compound containing an ester bond in the main chain. Examples of the polyester resin include a polycondensation product of a polycarboxylic acid (e.g., a dicarboxylic acid) and a polyalcohol (e.g., a diol). In the present disclosure, polyolefin resin means a polymer (homopolymer or copolymer) of raw material monomers containing olefin. Examples of polyolefin resin include a polymer of one type of olefin, a copolymer of two or more types of olefins, and a copolymer of one or more types of olefins and one or more types of other monomers. Examples of olefin include α-olefins having 2 to 30 carbon atoms. In the present disclosure, a polyurethane resin refers to a polymer compound containing a urethane bond. In the present disclosure, a polyurea resin means a polymer compound containing a urea bond. In the present disclosure, a polyamide resin refers to a polymer compound containing an amide bond. In the present disclosure, polycarbonate resin refers to a polymeric compound that contains carbonate bonds. In the present disclosure, polystyrene resin refers to a polymer of raw material monomers including styrene.

[0035] The resin that can be contained in the pretreatment liquid may be a water-soluble resin or a water-insoluble resin, with a water-insoluble resin being preferred.

[0036] In the present disclosure, "water solubility" refers to the property of dissolving 1 g or more in 100 g of water at 25° C. Preferably, "water solubility" refers to the property of dissolving 3 g or more (more preferably 10 g or more) in 100 g of water at 25° C. In the present disclosure, "water-insoluble" refers to the property of dissolving less than 1 g in 100 g of water at 25° C. Preferably, "water-insoluble" refers to the property of dissolving less than 0.5 g in 100 g of water at 25° C.

[0037] The pretreatment liquid preferably contains resin particles. The resin particles are preferably made of a water-insoluble resin. The resin particles are preferably acrylic resin particles, polyester resin particles, a mixture of acrylic resin particles and polyester resin particles, or composite particles containing an acrylic resin and a polyester resin. As the resin particles, those similar to the resin particles that can be contained in the first ink, which will be explained in the section "Step of preparing the first ink" below, are also preferred.

[0038] The weight average molecular weight (Mw) of the resin in the resin particles is preferably 1,000 to 300,000, more preferably 2,000 to 200,000, and further preferably 5,000 to 100,000.

[0039] In the present disclosure, the weight average molecular weight (Mw) means a value measured by gel permeation chromatography (GPC), unless otherwise specified. Measurement by gel permeation chromatography (GPC) was performed using an HLC (registered trademark)-8020GPC (Tosoh Corporation) as a measuring device, three TSKgel (registered trademark) Super Multipore HZ-H (4.6 mm ID x 15 cm, Tosoh Corporation) columns, and THF (tetrahydrofuran) as an eluent. The measurement conditions were a sample concentration of 0.45 mass%, a flow rate of 0.35 mL / min, a sample injection amount of 10 μL, and a measurement temperature of 40° C., and an RI detector was used. The calibration curve is prepared from eight samples of "Standard sample TSK standard, polystyrene" from Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".

[0040] The volume average particle size of the resin particles is preferably from 1 nm to 300 nm, more preferably from 3 nm to 200 nm, and further preferably from 5 nm to 150 nm.

[0041] When preparing the pretreatment liquid, a commercially available aqueous dispersion of resin particles may be used. Commercially available aqueous dispersions of resin particles include PESRESIN A124GP, PESRESIN A645GH, PESRESIN A615GE, PESRESIN A520 (all manufactured by Takamatsu Oil Co., Ltd.), Eastek 1100, Eastek 1200 (all manufactured by Eastman Chemical Co., Ltd.), Pluscoat RZ570, Pluscoat Z687, Pluscoat Z565, Pluscoat RZ570, Pluscoat Z690 (all manufactured by GOO Chemical Industry Co., Ltd.), Vylonal MD1200 (manufactured by Toyobo Co., Ltd.), and EM57DOC (manufactured by Daicel FineChem).

[0042] When the pretreatment liquid contains resin particles, the content of the resin particles relative to the total amount of the pretreatment liquid is preferably 0.5% by mass to 30% by mass, more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 15% by mass.

[0043] (Water-soluble organic solvent) The pretreatment liquid preferably contains at least one water-soluble organic solvent. As the water-soluble organic solvent, any known solvent can be used without any particular limitation. Examples of the water-soluble organic solvent include polyhydric alcohols such as glycerin, 1,2,6-hexanetriol, trimethylolpropane, alkanediols (e.g., ethylene glycol, propylene glycol (1,2-propanediol), 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2-butene-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, 1,2-octanediol, 1,2-hexanediol, 1,2-pentanediol, 4-methyl-1,2-pentanediol, etc.), and polyalkylene glycols (e.g., diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, dipropylene glycol, polyoxyethylene polyoxypropylene glycol, etc.); polyhydric alcohol ethers such as polyalkylene glycol ethers (e.g., diethylene glycol monoalkyl ether, triethylene glycol monoalkyl ether, tripropylene glycol monoalkyl ether, polyoxypropylene glyceryl ether, etc.); C1-C4 alkyl alcohols, glycol ethers, 2-pyrrolidone, and N-methyl-2-pyrrolidone; etc. Among these, from the viewpoint of suppressing transfer of components, polyhydric alcohols or polyhydric alcohol ethers are preferred, and alkanediols, polyalkylene glycols, or polyalkylene glycol ethers are more preferred.

[0044] When the pretreatment liquid contains a water-soluble organic solvent, the content of the water-soluble organic solvent relative to the total amount of the pretreatment liquid is preferably 0.5% by mass to 30% by mass, more preferably 1% by mass to 20% by mass, and particularly preferably 1% by mass to 15% by mass.

[0045] As the water-soluble organic solvent that can be contained in the pretreatment liquid, a water-soluble organic solvent having a boiling point of less than 220°C is also preferred. From the viewpoint of drying properties of the pre-treatment liquid, it is preferable that the pre-treatment liquid does not contain an organic solvent having a boiling point of 220° C. or higher, or the content of the organic solvent having a boiling point of 220° C. or higher is 5 mass % or less (more preferably 3 mass % or less, and even more preferably 1 mass % or less) relative to the total amount of the pre-treatment liquid. For specific examples of the water-soluble organic solvents having a boiling point of less than 220° C. and the organic solvents having a boiling point of 220° C. or higher, see the section "Step of Preparing First Ink" below.

[0046] (Other Ingredients) The pretreatment liquid may contain other components in addition to those described above, if necessary. Other components that can be contained in the pretreatment liquid include known additives such as surfactants, solid wetting agents, silicic acid compounds (e.g., colloidal silica), inorganic salts, anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, antifungal agents, pH adjusters, viscosity adjusters, rust inhibitors, chelating agents, and water-soluble polymer compounds other than water-soluble cationic polymers (e.g., the water-soluble polymer compounds described in paragraphs 0026 to 0080 of JP2013-001854A). As for other components that may be contained in the pretreatment liquid, reference may also be made to the components that may be contained in the first ink, which will be described later.

[0047] (Properties of pretreatment liquid) From the viewpoint of the aggregation speed of the ink, the pH of the pretreatment liquid at 25° C. is preferably 0.1 to 3.5. When the pH of the pretreatment liquid is 0.1 or more, the roughness of the non-permeable substrate is further reduced, and the adhesion of the image area is further improved. When the pH of the pretreatment liquid is 3.5 or less, the aggregation rate is further improved, the coalescence of ink dots (ink dots) on the surface of the non-permeable substrate is further suppressed, and roughness of the image is further reduced. The pH of the pretreatment liquid at 25° C. is more preferably 0.2 to 2.0. The conditions for measuring the pH of the pretreatment liquid at 25° C. are the same as the conditions for measuring the pH of the ink at 25° C. described above.

[0048] When the pretreatment liquid contains an aggregating agent, the viscosity of the pretreatment liquid is preferably in the range of 0.5 mPa·s to 10 mPa·s, and more preferably in the range of 1 mPa·s to 5 mPa·s, from the viewpoint of the aggregation speed of the ink.

[0049] In this disclosure, unless otherwise specified, the viscosity is a value measured using a viscometer at 25°C. As the viscometer, for example, a VISCOMETER TV-22 type viscometer (manufactured by Toki Sangyo Co., Ltd.) is used.

[0050] The surface tension of the pretreatment liquid is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m.

[0051] In this disclosure, the surface tension is a value measured at a temperature of 25° C., unless otherwise specified. The surface tension is measured, for example, using an Automatic Surface Tentiometer CBVP-Z (manufactured by Kyowa Interface Science Co., Ltd.).

[0052] <Step of Preparing First Ink> The step of preparing the first ink (hereinafter also referred to as the "first ink preparation step") is a step of preparing a first ink containing a first pigment, a first resin, and water. The first ink preparing step may be a step of simply preparing a first ink that has been manufactured in advance, or may be a step of manufacturing the first ink. There are no particular limitations on the method for producing the first ink, and any known method for mixing the components can be used.

[0053] (water) The first ink contains water. The content of water relative to the total amount of the first ink is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The upper limit of the water content depends on the amounts of other components, but is preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the first ink.

[0054] (First pigment) The first ink contains a first pigment. The first pigment refers to all pigment components contained in the first ink (that is, one or more types of pigments). The first pigment is not particularly limited, and may be either an organic pigment or an inorganic pigment.

[0055] Examples of organic pigments include azo pigments, polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, diketopyrrolopyrrole pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), dye chelates, nitro pigments, nitroso pigments, aniline black, and the like. Examples of inorganic pigments include white inorganic pigments, iron oxide, barium yellow, cadmium red, chrome yellow, carbon black, etc. Preferred embodiments of the white inorganic pigment will be described later. Examples of the first pigment include the pigments described in paragraphs 0096 to 0100 of JP-A No. 2009-241586.

[0056] The first ink containing a chromatic pigment or a black pigment as the first pigment can be used as, for example, a color ink (for example, a cyan ink, a magenta ink, a yellow ink, etc.) or a black ink.

[0057] Furthermore, when the first pigment contains a white pigment (for example, a white inorganic pigment), the first ink can also be used as a white ink (hereinafter, also referred to as a "white ink"). Furthermore, when the first pigment contains a white pigment and a pigment of a color other than white, the first ink can be used as an ink in which a chromatic color is added to white.

[0058] Examples of white inorganic pigments include titanium dioxide (TiO2), barium sulfate, calcium carbonate, aluminum hydroxide, silica, zinc oxide, zinc sulfide, mica, talc, pearl, etc. Among the white inorganic pigments, titanium dioxide, barium sulfate, calcium carbonate, or zinc oxide is preferred, and titanium dioxide is more preferred.

[0059] The average primary particle size of the white inorganic pigment is, for example, 150 nm to 400 nm. When the average primary particle size is 150 nm or more, the hiding power is further improved. Here, the hiding power means the property of covering and concealing the base with an image (for example, a white image). When the average primary particle size is 400 nm or less, the ejection properties of the first ink are further improved. The average primary particle size of the white inorganic pigment is preferably from 250 nm to 350 nm, and more preferably from 250 nm to 300 nm.

[0060] The average primary particle size of the white inorganic pigment is a value measured using a transmission electron microscope (TEM). For the measurement, a 1200EX transmission electron microscope manufactured by JEOL Ltd. can be used. Specifically, ink diluted 1,000 times was dropped onto a Cu200 mesh (manufactured by JEOL Ltd.) with a carbon film attached, and then dried. The circular equivalent diameters of 300 non-overlapping independent particles were measured from an image magnified 100,000 times with a TEM, and the simple average of the measured values ​​was used as the average primary particle diameter.

[0061] The content of the first pigment is preferably 1% by mass to 20% by mass, more preferably 1% by mass to 15% by mass, and even more preferably 1% by mass to 10% by mass, relative to the total amount of the first ink.

[0062] (First resin) The first ink contains a first resin. Here, the first resin refers to all the resin components contained in the first ink (that is, one or more types of resin). In the image recording process described below, when the first resin in the first ink comes into contact with the aggregating agent in the pretreatment liquid on the non-permeable substrate, the resin particles in the first ink aggregate, thereby improving the adhesion of the image.

[0063] The first resin is not particularly limited, but is preferably an acrylic resin, a polyester resin, a polyurethane resin, or a polyolefin resin.

[0064] The content of the first resin relative to the total amount of the first ink is preferably 1% by mass to 30% by mass, more preferably 2% by mass to 20% by mass, even more preferably 2% by mass to 15% by mass, and even more preferably 2% by mass to 10% by mass.

[0065] Specific examples of the first resin include a pigment dispersion resin for dispersing the first pigment, and resin particles which are particles made of resin.

[0066] -Pigment dispersion resin- The first resin may include a pigment dispersing resin. When the first resin contains a pigment dispersing resin, the first ink contains a resin-coated pigment having a structure in which at least a portion of the surface of the first pigment is coated with the pigment dispersing resin. The pigment dispersing resin is preferably a water-insoluble resin.

[0067] The pigment dispersing resin is preferably an acrylic resin. Examples of the pigment dispersing resin include those described in International Publication No. 2013 / 180074, Japanese Patent No. 5863600, JP 2018-28080 A, JP 2017-149906 A, and JP 2016-193981 A. The pigment dispersing resin is also called a "resin dispersant" or the like. Furthermore, as a combination of the first pigment and the pigment dispersing resin, for example, a resin-coated pigment in which a pigment is coated with a cross-linked water-soluble resin may be used, as described in Japanese Patent No. 5404669. In this case, the resin-coated pigment can be prepared by using, for example, an acrylic resin having a carboxy group as the water-soluble resin and a bifunctional or higher epoxy compound as the cross-linking agent.

[0068] From the viewpoint of adsorptivity to the pigment, the pigment dispersing resin preferably contains an alicyclic structure or an aromatic ring structure, and more preferably contains an aromatic ring structure. The alicyclic structure is preferably an alicyclic hydrocarbon structure having 5 to 10 carbon atoms, and a cyclohexane ring structure, a dicyclopentanyl ring structure, a dicyclopentenyl ring structure, a norbornane ring structure, an isobornane ring structure, a norbornene ring structure, an isobornene ring structure, or an adamantane ring structure is preferred. The aromatic ring structure is preferably a naphthalene ring or a benzene ring, and more preferably a benzene ring. The amount of the alicyclic structure or aromatic ring structure is, for example, preferably 0.01 mol to 1.5 mol, and more preferably 0.1 mol to 1 mol, per 100 g of resin contained in the resin particles.

[0069] From the viewpoint of the performance of dispersing the pigment, the pigment dispersing resin preferably has an ionic group in the structure. The ionic group may be either an anionic group or a cationic group, with an anionic group being preferred. The anionic group is not particularly limited, but is preferably a carboxy group, a salt of a carboxy group, a sulfo group, or a salt of a sulfo group.

[0070] The acid value of the resin dispersant is preferably from 30 mgKOH / g to 100 mgKOH / g, more preferably from 30 mgKOH / g to 85 mgKOH / g, and even more preferably from 50 mgKOH / g to 85 mgKOH / g, from the viewpoints of pigment dispersibility and storage stability. Here, the acid value is defined as the mass (mg) of KOH required to completely neutralize 1 g of resin, and is measured by the method described in the JIS standard (JIS K 0070, 1992).

[0071] The weight average molecular weight (Mw) of the pigment dispersion resin is preferably 30,000 or more, more preferably from 30,000 to 150,000, even more preferably from 30,000 to 100,000, and still more preferably from 30,000 to 80,000.

[0072] When the first resin contains a pigment dispersion resin, the content of the pigment dispersion resin is preferably 1% by mass to 25% by mass, more preferably 1% by mass to 20% by mass, even more preferably 1% by mass to 15% by mass, and even more preferably 1% by mass to 10% by mass, relative to the total amount of the first ink.

[0073] When the first resin contains a pigment dispersion resin, the ratio of the pigment dispersion resin (D) to the pigment (P) (i.e., the D / P ratio) is preferably 0.05 to 3, more preferably 0.05 to 2, even more preferably 0.05 to 1, and even more preferably 0.05 to 0.7.

[0074] -Resin particles- The first resin may include resin particles. Here, the resin particles are distinguished from the above-mentioned pigment dispersion resin in that they are particles made of resin. The resin constituting the resin particles is preferably a water-insoluble resin. When the first resin contains resin particles, when the resin particles in the first ink come into contact with the aggregating agent in the pretreatment liquid on the non-permeable substrate, the resin particles in the first ink aggregate, and the first ink thickens. Thus, when the first resin contains resin particles, the strength and adhesion of the image are improved compared to when the first resin does not contain resin particles. Furthermore, when the first resin contains resin particles, the increase in viscosity of the first ink is more suppressed and the deterioration of the ejection properties of the first ink is more suppressed compared to when the first resin contains the same mass of water-soluble resin.

[0075] The glass transition temperature of the resin particles (that is, the glass transition temperature of the resin in the resin particles) is not particularly limited. From the viewpoint of further improving the strength of the image, the glass transition temperature (Tg) of the resin particles is preferably 20° C. or higher, more preferably 50° C. or higher, and even more preferably 80° C. or higher. From the viewpoint of the manufacturability of the resin particles, the glass transition temperature (Tg) of the resin particles is preferably 150° C. or lower, and more preferably 130° C. or lower.

[0076] In the method for producing an image recorded matter according to the present disclosure, from the viewpoint of further improving the adhesion of the image, The pretreatment liquid contains a resin, the first resin in the first ink contains resin particles; The glass transition temperature of the resin contained in the pretreatment liquid is preferably lower than the glass transition temperature of the resin particles contained in the first resin. In this case, the value obtained by subtracting the glass transition temperature of the resin contained in the pretreatment liquid from the glass transition temperature of the resin particles contained in the first resin is preferably 20°C or higher, more preferably 30°C or higher, and even more preferably 40°C or higher. There is no particular upper limit to this value, but examples of the upper limit include 100°C, 150°C, and 200°C.

[0077] The resin particles are preferably particles made of an acrylic resin (hereinafter also referred to as acrylic resin particles), particles made of a polyester resin (hereinafter also referred to as polyester resin particles), particles made of a polyurethane resin (hereinafter also referred to as polyurethane resin particles), or particles made of a polyolefin resin (hereinafter also referred to as polyolefin resin particles).

[0078] From the viewpoint of further improving the adhesion and abrasion resistance of the image, it is preferable that the resin particles contained in the first ink contain acrylic resin particles. When the resin particles contained in the first ink include acrylic resin particles, the ratio of the acrylic resin particles to the resin particles contained in the first ink is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the ratio of the acrylic resin particles to the resin particles contained in the first ink is 60 mass % or more, the adhesion of the image is further improved.

[0079] The resin particles are preferably self-dispersing resin particles. Examples of the self-dispersing resin particles include the self-dispersing polymer particles described in paragraphs 0062 to 0076 of JP2016-188345A and paragraphs 0109 to 0140 of WO2013 / 180074A.

[0080] The resin in the resin particles preferably contains an alicyclic structure or an aromatic ring structure, and more preferably contains an alicyclic structure. The alicyclic structure is preferably an alicyclic hydrocarbon structure having 5 to 10 carbon atoms, and a cyclohexane ring structure, a dicyclopentanyl ring structure, a dicyclopentenyl ring structure, a norbornane ring structure, an isobornane ring structure, a norbornene ring structure, an isobornene ring structure, or an adamantane ring structure is preferred. The aromatic ring structure is preferably a naphthalene ring or a benzene ring, and more preferably a benzene ring. The amount of the alicyclic structure or aromatic ring structure is, for example, preferably from 0.01 mol to 1.5 mol, and more preferably from 0.1 mol to 1 mol, per 100 g of resin in the resin particles.

[0081] The resin in the resin particles preferably has an ionic group in the structure, from the viewpoint of further improving the water dispersibility of the resin particles. The ionic group may be either an anionic group or a cationic group, with an anionic group being preferred. The anionic group is not particularly limited, but is preferably a carboxy group, a salt of a carboxy group, a sulfo group, or a salt of a sulfo group.

[0082] As the resin in the resin particles, More preferably, the acrylic resin contains at least one selected from the group consisting of a benzyl (meth)acrylate unit, a phenoxyethyl (meth)acrylate unit, and an alicyclic structure-containing (meth)acrylate unit, and a (meth)acrylic acid unit, More preferably, it is an acrylic resin containing at least one selected from the group consisting of benzyl (meth)acrylate units, phenoxyethyl (meth)acrylate units, and alicyclic structure-containing (meth)acrylate units, (meth)acrylic acid units, alkyl (meth)acrylate units containing an alkyl group having 1 to 4 carbon atoms, and alkyl (meth)acrylate units containing an alkyl group having 5 to 12 carbon atoms.

[0083] The alicyclic structure-containing (meth)acrylate is preferably at least one selected from an alkyl (meth)acrylate having a cycloalkyl group having 3 to 10 carbon atoms (e.g., cyclohexyl (meth)acrylate), isobornyl (meth)acrylate, adamantyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; At least one selected from isobornyl (meth)acrylate, adamantyl (meth)acrylate, and dicyclopentanyl (meth)acrylate is more preferred.

[0084] The acid value of the resin in the resin particles is preferably 25 mgKOH / g to 100 mgKOH / g, more preferably 30 mgKOH / g to 90 mgKOH / g, and even more preferably 35 mgKOH / g to 80 mgKOH / g, from the viewpoints of self-dispersibility, aggregation during image recording, and the like.

[0085] The molecular weight of the resin in the resin particles is preferably from 1,000 to 300,000, more preferably from 2,000 to 200,000, and further preferably from 5,000 to 100,000, in terms of weight average molecular weight. The weight average molecular weight is measured by gel permeation chromatography (GPC). Details of GPC are as described above.

[0086] The volume average particle size of the resin particles is preferably from 1 nm to 200 nm, more preferably from 3 nm to 200 nm, and further preferably from 5 nm to 50 nm.

[0087] When the first ink contains resin particles, the content of the resin particles relative to the total amount of the first ink is preferably 1% by mass to 25% by mass, more preferably 2% by mass to 20% by mass, even more preferably 2% by mass to 15% by mass, and even more preferably 2% by mass to 10% by mass.

[0088] (Water-soluble organic solvent with a boiling point of less than 220°C) The first ink preferably contains at least one water-soluble organic solvent having a boiling point of less than 220°C. This further improves the lamination strength of the image recorded product. In this disclosure, boiling point means the boiling point at 1 atmosphere (101325 Pa).

[0089] Examples of water-soluble organic solvents with a boiling point of less than 220°C include 1,2-propanediol (also known as propylene glycol; PG) (boiling point 188°C), 1,3-propanediol (boiling point 213°C), propylene glycol monomethyl ether (boiling point 121°C), ethylene glycol (boiling point 197°C), ethylene glycol monomethyl ether (boiling point 124°C), propylene glycol monoethyl ether (boiling point 133°C), ethylene glycol monoethyl ether (boiling point 135°C), propylene glycol monopropyl ether ( boiling point 149°C), ethylene glycol monopropyl ether (boiling point 151°C), propylene glycol monobutyl ether (boiling point 170°C), ethylene glycol monobutyl ether (boiling point 171°C), 2-ethyl-1-hexanol (boiling point 187°C), dipropylene glycol monomethyl ether (boiling point 188°C), diethylene glycol dimethyl ether (boiling point 162°C), diethylene glycol diethyl ether (boiling point 188°C), dipropylene glycol dimethyl ether (boiling point 175°C), and the like.

[0090] When the first ink contains a water-soluble organic solvent having a boiling point of less than 220°C, the content of the water-soluble organic solvent having a boiling point of less than 220°C is preferably 1 mass % to 50 mass %, more preferably 5 mass % to 40 mass %, even more preferably 10 mass % to 40 mass %, and even more preferably 15 mass % to 35 mass %, relative to the total amount of the ink.

[0091] (Organic solvents with a boiling point of 220°C or higher) The content of the organic solvent having a boiling point of 220° C. or higher (hereinafter also referred to as a “high boiling point solvent”) in the first ink is preferably 5% by mass or less, which further improves the lamination strength of the image recording material and the adhesion of the image. Here, "the content of organic solvents with a boiling point of 220°C or higher in the first ink is 5% by mass or less" means that the first ink does not contain any organic solvents with a boiling point of 220°C or higher (i.e., the content of organic solvents with a boiling point of 220°C or higher in the first ink is 0% by mass), or, even if it does contain organic solvents, the content of organic solvents with a boiling point of 220°C or higher is 5% by mass or less relative to the total amount of the first ink. The content of organic solvents having a boiling point of 220° C. or higher in the first ink is more preferably 3% by mass or less, even more preferably 2% by mass or less, even more preferably 1% by mass or less, and even more preferably 0% by mass.

[0092] The meaning of "the content of organic solvents with a boiling point of 220°C or higher in the second ink is 5% by mass or less" described below is the same as "the content of organic solvents with a boiling point of 220°C or higher in the first ink is 5% by mass or less", and the preferred content of high boiling point solvents in the second ink is the same as the preferred content of high boiling point solvents in the first ink.

[0093] Examples of organic solvents having a boiling point of 220° C. or higher include glycerin (boiling point 290° C.), 1,2-hexanediol (HDO) (boiling point 223° C.), diethylene glycol (boiling point 245° C.), diethylene glycol monobutyl ether (boiling point 230° C.), triethylene glycol (boiling point 285° C.), dipropylene glycol (boiling point 232° C.), tripropylene glycol (boiling point 267° C.), trimethylolpropane (boiling point 295° C.), 2-pyrrolidone (boiling point 245° C.), tripropylene glycol monomethyl ether (boiling point 243° C.), and triethylene glycol monomethyl ether (boiling point 248° C.).

[0094] (Surfactant) The first ink may contain at least one surfactant. Examples of the surfactant include a nonionic surfactant, a cationic surfactant, an anionic surfactant, and a betaine surfactant.

[0095] Preferred surfactants include acetylene glycol surfactants, which are a type of nonionic surfactant. As the acetylene glycol surfactant, for example, the acetylene glycol surfactants described in paragraphs 0070 to 0080 of WO 2017 / 149917 can be used. Examples of acetylene glycol surfactants include: A polyalkylene oxide adduct (preferably a polyethylene oxide adduct) of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, A polyalkylene oxide adduct (preferably a polyethylene oxide adduct) of 3,6-dimethyl-4-octyne-3,6-diol, A polyalkylene oxide adduct (preferably a polyethylene oxide adduct) of 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol, Examples thereof include polyalkylene oxide adducts (preferably polyethylene oxide adducts) of 2,5-dimethyl-3-hexyne-2,5-diol. Commercially available acetylene glycol surfactants include the Surfynol series (e.g., Surfynol 420, Surfynol 440, Surfynol 465, Surfynol 485), Olfine series (e.g., Olfine E1010, Olfine E1020), and Dynol series (e.g., Dynol 604) manufactured by Air Products Inc. or Nissin Chemical Industry Co., Ltd.; and Acetylenol manufactured by Kawaken Fine Chemical Co., Ltd. Commercially available acetylene glycol surfactants are also provided by The Dow Chemical Company, General Aniline Company, and the like.

[0096] Examples of the surfactant include the compounds listed as surfactants on pages 37 to 38 of JP-A-59-157636 and Research Disclosure No. 308119 (1989). In addition, examples of the surfactant include fluorine (alkyl fluoride) surfactants and silicone surfactants described in JP-A-2003-322926, JP-A-2004-325707, and JP-A-2004-309806.

[0097] When the first ink contains a surfactant, the content of the surfactant in the first ink is appropriately adjusted taking into consideration the surface tension of the first ink. The content of the surfactant in the first ink is preferably 0.01% by mass to 5% by mass, more preferably 0.05% by mass to 3% by mass, and even more preferably 0.1% by mass to 2% by mass, relative to the total amount of the first ink.

[0098] (Silicate compounds) The first ink may contain at least one silicic acid compound. When the first ink contains a silicic acid compound, the ejection stability of the first ink from the inkjet head can be further improved. As the silicic acid compound, for example, the compounds described in paragraphs 0058 to 0075 of Japanese Patent No. 5430316 can be used. The silicate compounds are: Silicates (e.g., sodium silicate, potassium silicate, calcium silicate, magnesium silicate, ammonium salts of silicic acid, etc.) or anhydrous silicic acid (silica) are preferred; Silica is more preferred, Colloidal silica is more preferred. As the colloidal silica, a commercially available product may be used. Specific examples of commercially available products include Snowtex S, Snowtex XS, Snowtex 20, Snowtex 30, Snowtex 40, Snowtex N, Snowtex C, and Snowtex O (all manufactured by Nissan Chemical Industries, Ltd.).

[0099] The content of the silicic acid compound in the first ink is preferably 0.0001% by mass to 1% by mass, more preferably 0.0005% by mass to 0.5% by mass, even more preferably 0.001% by mass to 0.5% by mass, and even more preferably 0.01% by mass to 0.3% by mass, relative to the total amount of the first ink.

[0100] (Other Ingredients) The first ink may contain other components in addition to the above components. Examples of other components include known additives such as urea, urea derivatives, wax, anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, anti-fungal agents, pH adjusters, antifoaming agents, viscosity adjusters, dispersion stabilizers, and chelating agents.

[0101] (Preferable physical properties of the first ink) The viscosity of the first ink (25° C.) is preferably 1.2 mPa·s or more and 15.0 mPa·s or less, more preferably 2 mPa·s or more and less than 13 mPa·s, and even more preferably 2.5 mPa·s or more and less than 10 mPa·s.

[0102] The surface tension of the first ink (25° C.) is preferably 25 mN / m to 50 mN / m, more preferably 30 mN / m to 45 mN / m, and even more preferably 30 mN / m to 40 mN / m.

[0103] The pH of the first ink at 25°C is preferably from 6 to 11, more preferably from 7 to 10, and even more preferably from 7 to 9. The pH of the first ink at 25° C. is measured using a commercially available pH meter.

[0104] <Step of preparing the second ink> The process of preparing a second ink (hereinafter also referred to as the "second ink preparation process") is a process of preparing a second ink that contains a second pigment, a second resin, and water and has a surface tension lower than that of the first ink. The second ink preparing step may be a step of simply preparing a second ink that has been manufactured in advance, or may be a step of manufacturing the second ink.

[0105] The second ink is an ink similar to the first ink, except that the surface tension of the second ink is smaller than that of the first ink, and the preferred aspects of the second ink are also similar to the preferred aspects of the first ink.

[0106] Specific examples and preferred aspects of the second pigment contained in the second ink are the same as the specific examples and preferred aspects of the first pigment contained in the first ink. The hue of the second pigment is preferably different from the hue of the first pigment. In addition, it is preferable that the hue of the second ink is different from the hue of the first ink.

[0107] One specific embodiment of the method for producing an image recorded matter of the present disclosure comprises: The hue of the first ink is a hue other than white (preferably a chromatic color or black, for example, cyan, magenta, yellow, black, etc.), In this embodiment, the hue of the second ink is white (see Examples described later). In this embodiment, it is preferable that the first pigment contained in the first ink is a chromatic pigment and / or a black pigment, and the second pigment contained in the second ink is a white pigment. In this embodiment, for example, a substrate having transparency is used as the non-permeable substrate, a colored image (i.e., a chromatic image or a black image; for example, a pattern image such as a character or a figure) is recorded on the non-permeable substrate using the first ink, and a white image (e.g., a solid image) is recorded on the non-permeable substrate on which the colored image has been recorded, so as to cover the colored image. In this case, when observed from the non-image recorded side (i.e., the side on which an image is not recorded) of the non-permeable substrate, the colored image of the first ink against the white image of the second ink in the background can be seen through the non-permeable substrate. On the other hand, when observed from the image recorded side (i.e., the side on which an image is recorded) of the non-permeable substrate, the colored image and the non-permeable substrate are concealed by the white image of the second ink, making it difficult to see the colored image and the non-permeable substrate. In this embodiment, the area of ​​the white image formed by the second ink tends to be larger than the area of ​​the colored image formed by the first ink in order to cover up the colored image formed by the first ink. As a result, in this embodiment, the effect of suppressing unevenness of the image surface and / or unevenness in the image thickness (i.e., the effect of the surface tension of the second ink being smaller than that of the first ink, and the effect of the applied mass ratio [(first resin + second resin) / coagulant] being 16.0 or more) is more effectively exerted, and the laminate strength is further improved.

[0108] The above embodiment may also include an embodiment in which, for example, a plurality of colored inks (e.g., four types of cyan ink, magenta ink, yellow ink, and black ink) are applied to an area of ​​a non-permeable substrate to which a pretreatment liquid has been applied to record a multicolored colored image, and a white ink (white ink) is applied as a second ink to cover the multicolored colored image to record a white image. In this case, the relationship between all of the plurality of colored inks and the white ink as the second ink does not necessarily have to satisfy the conditions of the manufacturing method of the image recorded product of the present disclosure, but it is sufficient that the relationship between at least one of the plurality of colored inks and the white ink as the second ink satisfies the conditions of the manufacturing method of the image recorded product of the present disclosure. In this case, among the plurality of colored inks, the colored ink that satisfies the conditions of the manufacturing method of the image recorded product of the present disclosure corresponds to the first ink.

[0109] The content of high boiling point solvent (that is, organic solvent with a boiling point of 220° C. or higher) in the second ink is also preferably 5% by mass or less, which further improves the lamination strength of the image recorded product and the adhesion of the image. From the viewpoint of further improving the lamination strength and image adhesion of the image recorded material, it is more preferable that the content of organic solvents having a boiling point of 220°C or higher relative to the total amount of the first ink is 5 mass% or less, and that the content of organic solvents having a boiling point of 220°C or higher relative to the total amount of the second ink is 5 mass% or less.

[0110] (Surface tension difference [1st ink - 2nd ink]) As described above, the surface tension of the second ink is smaller than the surface tension of the first ink. As described above, the surface tension of the first ink and the surface tension of the second ink are both values ​​measured under a temperature condition of 25° C. Examples of the surface tension measuring device are also as described above. In other words, the value obtained by subtracting the surface tension of the second ink from the surface tension of the first ink (hereinafter referred to as the "surface tension difference [first ink - second ink]" or simply "surface tension difference") is greater than 0 mN / m. This improves the wetting and spreading of the second ink on the first ink applied to the non-permeable substrate, suppressing unevenness of the image surface and / or unevenness in the image thickness, thereby improving the adhesion between the image and the substrate for lamination and improving the lamination strength of the laminate. From the viewpoint of further improving the laminate strength, the surface tension difference [first ink - second ink] is preferably 2.0 mN / m or more, more preferably 3.0 mN / m or more, and even more preferably 4.0 mN / m or more. There is no particular upper limit to the surface tension difference [first ink - second ink], but the upper limit is, for example, 10.0 mN / m.

[0111] Specific examples and preferred aspects of the second resin contained in the second ink are the same as the specific examples and preferred aspects of the first resin contained in the first ink. For example, the second resin preferably contains resin particles, which improves the adhesion between the layer made of the second ink (hereinafter also referred to as the "second ink layer") and the layer made of the first ink (hereinafter also referred to as the "first ink layer") and / or the layer made of the pretreatment liquid (hereinafter also referred to as the "pretreatment layer"), thereby improving the laminate strength.

[0112] (Glass transition temperature difference (Ta-Tb)) A preferred embodiment of the method for producing an image recorded matter according to the present disclosure is one in which the first resin contains resin particles and the second resin contains resin particles. In this preferred embodiment, in an overlapping region (i.e. an overlapping region where a region to which the pretreatment liquid is applied, a region to which the first ink is applied, and a region to which the second ink is applied overlap in a planar view) of the resin particles contained in the first resin and the resin particles contained in the second resin, when the glass transition temperature of the particle having a larger applied mass per unit area is taken as Ta and the glass transition temperature of the particle having a smaller applied mass per unit area is taken as Tb, it is preferred that Ta and Tb satisfy the relationship 0°C≦Ta-Tb≦30°C. By ensuring that "0°C≦Ta-Tb" (i.e., Tb≦Ta), the film strength of the entire image (i.e., an image having a layer structure of second ink layer / first ink layer / pretreatment layer) is further improved, and as a result, the laminate strength is further improved. By satisfying "Ta-Tb≦30° C." (that is, "Ta-Tb" is 30° C. or less), the adhesion between the second ink layer and the first ink layer is improved, and as a result, the laminate strength is improved. "Ta-Tb" is preferably 25°C or lower, more preferably 20°C or lower.

[0113] (Mixture viscosity difference (A1-A2)) A preferred embodiment of the method for producing an image recorded matter according to the present disclosure is one in which, when the viscosity of a mixture obtained by mixing the pretreatment liquid and the first ink is A1 (hereinafter also referred to as the “mixture viscosity A1”) and the viscosity of a mixture obtained by mixing the pretreatment liquid and the second ink is A2 (hereinafter also referred to as the “mixture viscosity A2”), A1 and A2 satisfy A1-A2>0 mPa s. When A1-A2>0 mPa s is satisfied, the wetting and spreading properties of the second ink applied onto the first ink are improved, and as a result, unevenness of the image surface and / or unevenness in the image thickness are suppressed, leading to improved adhesion between the image and the lamination substrate and improved lamination strength.

[0114] From the viewpoint of further improving the laminate strength, "A1-A2" is preferably 10 mPa·s or more, more preferably 20 mPa·s or more, and even more preferably 25 mPa·s or more. There is no particular restriction on the upper limit of "A1-A2", but the upper limit is, for example, preferably 50 mPa·s or less, and more preferably 40 mPa·s or less.

[0115] Here, the mixture viscosity A1 refers to a value measured as follows. The pretreatment liquid and the first ink are mixed at a liquid temperature of 25° C. such that the mass ratio of the pretreatment liquid to the first ink (i.e., mass ratio [pretreatment liquid / first ink]) is 0.1. The viscosity of the resulting mixture is measured at a liquid temperature of 25° C. within 30 minutes after the completion of mixing the flocculant and the first ink. The viscosity is measured using a viscometer such as a VISCOMETER TV-22 type viscometer (manufactured by Toki Sangyo Co., Ltd.). The mixture viscosity A2 refers to a value measured in the same manner as the mixture viscosity A1, except that the first ink was changed to the second ink.

[0116] <Image recording process> The image recording step is a step of applying the pretreatment liquid, the first ink, and the second ink in this order onto a non-permeable substrate to record an image. In the image recording process, the pretreatment liquid, the first ink, and the second ink are applied in this order to record an image under conditions (i.e., application arrangement) such that an overlapping region is created in which the region to which the pretreatment liquid is applied, the region to which the first ink is applied, and the region to which the second ink is applied overlap in a planar view, and under conditions (i.e., application amounts) such that in the overlapping region, the ratio of the total applied mass of the first resin and the second resin per unit area to the applied mass of the coagulant per unit area (i.e., applied mass ratio [(first resin + second resin) / coagulant]) is 16.0 or more and 30.0 or less. The image recording process will be described in detail below.

[0117] (Order of application of pretreatment liquid, first ink, and second ink) In the image recording process, the pretreatment liquid, the first ink, and the second ink are applied in this order onto the non-permeable substrate. That is, in the image recording process, a pretreatment liquid is applied onto a non-permeable substrate, a first ink is applied onto the applied pretreatment liquid, and a second ink is applied onto the applied first ink. On a non-permeable substrate, the aggregating agent, which is a component of the pretreatment liquid, agglomerates components in a first ink (e.g., a first resin) applied onto the pretreatment liquid, and also agglomerates components in a second ink (e.g., a second resin) applied onto the first ink, via the first ink. As a result, an image having a layer structure of "second ink layer / first ink layer / pretreatment layer ( / non-permeable substrate)" is formed on the non-permeable substrate, where the pretreatment layer, the first ink layer, and the second ink layer refer to the layer derived from the pretreatment liquid, the layer derived from the first ink, and the layer derived from the second ink, respectively.

[0118] The first ink may be applied onto a pretreatment liquid that has been dried by heating (preferable conditions will be described later), or may be applied onto a pretreatment liquid that has not been dried by heating. From the viewpoint of suppressing bleeding, etc., it is preferable that the first ink is applied onto the pretreatment liquid that has been heated and dried. The preferable conditions for heating and drying the pretreatment liquid will be described later.

[0119] The second ink may be applied onto the first ink that has been dried by heating (preferable conditions will be described later), or may be applied onto the first ink that has not been dried by heating. Even in an embodiment in which the second ink is applied onto a first ink that has not been heated and dried, bleeding and color mixing are suppressed because the first ink has already been thickened by the action of the pretreatment liquid at the time the second ink is applied. From the viewpoints of suppressing bleeding and efficiency of image recording, the image recording step is preferably a step of applying a pretreatment liquid onto a non-permeable substrate, heating and drying the pretreatment liquid, and then applying the first ink and the second ink in this order onto the heated and dried pretreatment liquid.

[0120] (Application arrangement of pre-treatment liquid, first ink, and second ink) In the image recording process, the pretreatment liquid, the first ink, and the second ink are applied under conditions (i.e., application arrangement) such that an overlapping area is created where the area to which the pretreatment liquid is applied, the area to which the first ink is applied, and the area to which the second ink is applied overlap in a planar view, to record an image. In the image recording process, the pretreatment liquid, the first ink, and the second ink may be applied under conditions (that is, application arrangements) that result in overlapping regions and regions other than the overlapping regions. For example, a first ink may be applied in a pattern onto an area to which the pretreatment liquid has been applied to form a patterned first ink layer, and then a second ink may be applied (e.g., solidly) to an area spanning the first ink layer and an area other than the first ink layer (e.g., an area covering the entire first ink layer and its periphery) to form a second ink layer. In this case, the area where the first ink layer exists corresponds to the above-mentioned "overlapping area", and the area where the first ink layer does not exist but the second ink layer exists, and the area where neither the first ink layer nor the second ink layer exists correspond to the above-mentioned "area other than the overlapping area".

[0121] (Amounts of Pretreatment Liquid, First Ink, and Second Ink Applied) In the image recording process, in the overlapping region, the pretreatment liquid, the first ink, and the second ink are applied under conditions (i.e., application amounts) such that the ratio of the total applied mass of the first resin and the second resin per unit area to the applied mass of the coagulant per unit area (i.e., the applied mass ratio [(first resin + second resin) / coagulant]) is 16.0 or more and 30.0 or less to record an image. As described above, by setting the applied mass ratio [(first resin + second resin) / aggregant] in the overlapping region to 16.0 or more, the over-aggregation of the first resin and the second resin in the overlapping region is suppressed, and unevenness of the surface (i.e., the surface of the second ink layer) of the image (i.e., an image having a layer structure of the second ink layer / first ink layer / pretreatment layer; the same applies below) and / or unevenness in the thickness of the image due to over-aggregation are suppressed. As a result, the adhesion between the image and the lamination substrate is improved, and the lamination strength is improved. As described above, by setting the mass ratio [(first resin + second resin) / aggregating agent] in the overlapping region to 30.0 or less, insufficient aggregation of the first resin and the second resin in the overlapping region is suppressed, resulting in improved adhesion between the non-permeable substrate and the image, and improved laminate strength.

[0122] The applied mass ratio in the overlap region [(first resin + second resin) / coagulant] is calculated based on the applied mass of coagulant per unit area in the overlap region, the applied mass of the first resin per unit area in the overlap region, and the applied mass of the second resin per unit area in the overlap region. The mass of coagulant applied per unit area in the overlapping region (unit: g / m 2 ) is calculated, for example, based on the mass of the pretreatment liquid applied per unit area in the overlap region and the content (mass %) of the flocculant relative to the total amount of the pretreatment liquid. The applied mass of the first resin per unit area in the overlapping region (unit: g / m 2 ) is calculated, for example, based on the applied mass of the first ink per unit area in the overlap region and the content (mass %) of the first resin relative to the total amount of the first ink. The mass of the second resin per unit area in the overlapping region (unit: g / m 2) is calculated, for example, based on the applied mass of the second ink per unit area in the overlap region and the content (mass %) of the second resin relative to the total amount of the second ink.

[0123] From the viewpoint of further improving the laminate strength, the applied mass ratio [(first resin+second resin) / coagulant] is preferably 16.0 or more and 25.0 or less, and more preferably 16.0 or more and 20.0 or less. From the viewpoint of further improving the laminate strength, the lower limit of the applied mass ratio [(first resin+second resin) / coagulant] is preferably 16.1, and more preferably 16.2.

[0124] The mass of coagulant applied per unit area in the overlapping region (unit: g / m 2 ) is preferably 0.040 to 0.100, and more preferably 0.045 to 0.075. The applied mass of pretreatment liquid per unit area in the overlapping region (unit: g / m 2 ) is preferably 1.0 to 2.0, and more preferably 1.2 to 1.8.

[0125] The total applied mass of the first resin and the second resin per unit area in the overlapping region (unit: g / m 2 ) is preferably 1.00 to 2.50, and more preferably 1.00 to 2.00. The total applied mass of the first ink and the second ink per unit area in the overlapping region (unit: g / m 2 ) is preferably 14.0 to 30.0, and more preferably 14.5 to 28.0.

[0126] The applied mass of the first resin per unit area in the overlapping region (unit: g / m 2 ) is preferably 0.45 to 1.00, and more preferably 0.48 to 0.90. The applied mass of the first ink per unit area in the overlapping region (unit: g / m 2 ) is preferably 7.0 to 13.0, preferably 7.0 to 12.0, and more preferably 7.0 to 11.5.

[0127] The mass of the second resin per unit area in the overlapping region (unit: g / m 2 ) is preferably 0.40 to 2.00, preferably 0.40 to 1.30, and more preferably 0.50 to 1.10. The applied mass of the second ink per unit area in the overlapping region (unit: g / m 2 ) is preferably 7.0 to 20.0, preferably 7.0 to 18.0, and more preferably 7.0 to 16.0.

[0128] (Non-permeable base material) In the image recording process, the pretreatment liquid, the first ink, and the second ink are applied onto a non-permeable substrate. An impermeable substrate refers to a substrate that has a water absorption rate (mass %, 24 hr.) of less than 0.2 according to ASTM test method ASTM D570. The impermeable substrate is not particularly limited, but a resin substrate is preferred. The resin substrate is not particularly limited, and examples thereof include substrates made of thermoplastic resin. The resin substrate may be, for example, a substrate obtained by forming a thermoplastic resin into a sheet or film. As the resin substrate, a substrate containing polypropylene, polyethylene terephthalate, nylon, polyethylene, or polyimide is preferable.

[0129] The resin substrate may be a transparent resin substrate. Here, transparent means that the transmittance of visible light with a wavelength of 400 nm to 700 nm is 80% or more (preferably 90% or more). In the embodiment described above in which the hue of the first ink is a hue other than white (preferably a chromatic color or black, such as cyan, magenta, yellow, black, etc.) and the hue of the second ink is white, when the non-permeable substrate is a transparent resin substrate, a colored image made by the first ink against a white image made by the second ink can be viewed through the non-permeable substrate from the non-image recording side (i.e., the side on which no image is recorded) of the non-permeable substrate. The resin substrate may be colored.

[0130] The shape of the resin substrate is not particularly limited, but is preferably a sheet-like resin substrate, and from the viewpoint of productivity of the recording medium, is more preferably a sheet-like resin substrate that can be wound up into a roll. The thickness of the resin substrate is preferably from 10 μm to 200 μm, and more preferably from 10 μm to 100 μm.

[0131] The resin substrate may be subjected to a surface treatment in order to improve the surface energy. Examples of surface treatments include, but are not limited to, corona treatment, plasma treatment, flame treatment, heat treatment, abrasion treatment, light irradiation treatment (UV treatment), and flame treatment.

[0132] (Application of pre-treatment liquid) In the image recording process, the pretreatment liquid can be applied to the non-permeable substrate by applying a known method such as a coating method, an inkjet method, or a dipping method. Examples of the coating method include known coating methods using a bar coater (for example, a wire bar coater), an extrusion die coater, an air doctor coater, a blade coater, a rod coater, a knife coater, a squeeze coater, a reverse roll coater, a gravure coater, a flexo coater, and the like. The ink-jet method will be described in detail later.

[0133] In the image recording process, the non-permeable substrate may be heated before the pretreatment liquid is applied. The heating temperature is preferably from 20°C to 50°C, and more preferably from 25°C to 40°C, for the non-permeable substrate.

[0134] In the image recording process, after the application of the pretreatment liquid and before the application of the first ink, the pretreatment liquid may be dried by heating. Means for heating and drying the pretreatment liquid include known heating means such as a heater, known air blowing means such as a dryer, and a combination of these. Examples of the method for drying the pretreatment liquid by heating include: A method of applying heat by a heater or the like to the side opposite to the side of the non-permeable substrate to which the pretreatment liquid has been applied; A method of applying warm or hot air to a surface of a non-permeable substrate to which a pretreatment liquid has been applied; A method of applying heat by an infrared heater to the surface of the non-permeable substrate to which the pretreatment liquid has been applied or to the side opposite to the surface to which the pretreatment liquid has been applied; A combination of these methods, etc.

[0135] The heating temperature during heating and drying of the pretreatment liquid is preferably 35° C. or higher, and more preferably 40° C. or higher. There is no particular upper limit to the heating temperature, but the upper limit is preferably 100°C, more preferably 90°C, and even more preferably 70°C. The heat drying time is not particularly limited, but is preferably 0.5 seconds to 60 seconds, more preferably 0.5 seconds to 20 seconds, and particularly preferably 0.5 seconds to 10 seconds.

[0136] (Application of the first ink) In the image recording process, the first ink can be applied onto the pretreatment liquid (i.e., the pretreatment layer) by applying a known method such as a coating method, an inkjet method, or a dipping method, but is preferably applied by an inkjet method. The method for ejecting the first ink in the inkjet method is not particularly limited, and may be any of the well-known methods, such as a charge control method that uses electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element, an acoustic inkjet method in which an electrical signal is converted into an acoustic beam and irradiated onto the ink to eject the ink using radiation pressure, and a thermal inkjet (Bubble Jet (registered trademark)) method in which ink is heated to form bubbles and the resulting pressure is utilized. As an ink-jet method, in particular, the method described in JP-A-54-59936 can be effectively utilized, in which ink undergoes a sudden change in volume when exposed to thermal energy, and the force resulting from this change in state causes the ink to be ejected from a nozzle. As the inkjet method, the method described in paragraphs 0093 to 0105 of JP-A No. 2003-306623 can also be used.

[0137] The application of the first ink by the inkjet method is carried out by ejecting the first ink from the nozzles of an inkjet head. Inkjet head methods include the shuttle method, in which a short serial head is scanned across the width of the recording medium to perform recording, and the line method, which uses a line head in which recording elements are arranged to cover the entire area of ​​one side of the recording medium. In the line method, an image can be recorded on the entire surface of a recording medium by scanning the recording medium in a direction intersecting the arrangement direction of the recording elements. The line method does not require a transport system such as a carriage that scans a short head in the shuttle method. Furthermore, compared to the shuttle method, the line method does not require complex scanning control of the carriage movement and the recording medium, and only the recording medium moves. Therefore, the line method achieves faster image recording speeds than the shuttle method.

[0138] The first ink is preferably applied using an inkjet head having a resolution of 300 dpi or more (more preferably 600 dpi, and even more preferably 800 dpi), where dpi is an abbreviation for dots per inch, and 1 inch is 2.54 cm.

[0139] The amount of droplets of the first ink ejected from the nozzles of the inkjet head is preferably 1 pL (picoliter) to 10 pL, and more preferably 1.5 pL to 6 pL, from the viewpoint of obtaining a high-definition image. From the viewpoint of improving image unevenness and continuous gradation, it is also effective to eject a combination of different droplet amounts.

[0140] In the image recording process, the first ink applied onto the pretreatment liquid (i.e., the pretreatment layer) may be dried by heating, and then the second ink may be applied onto the first ink that has been dried by heating. The preferred conditions for the heat drying in the case of heat drying are the same as the preferred conditions for the heat drying after application of the second ink, which will be described later. As described above, in the image recording process, the second ink may be applied onto the first ink applied onto the pretreatment liquid (i.e., the pretreatment layer) without heating and drying the first ink, because at the stage of applying the second ink, the first ink has already been thickened by the action of the coagulant.

[0141] Furthermore, the non-permeable substrate may be heated in advance before the application of the first ink. This heating may also serve to heat and dry the pretreatment liquid. The heating temperature may be appropriately set, but the temperature of the non-permeable substrate is preferably 20°C to 50°C, and more preferably 25°C to 40°C.

[0142] (Application of the second ink) In the image recording process, the second ink can be applied onto the first ink (i.e., the first ink layer) by applying a known method such as a coating method, an inkjet method, or a dipping method, but is preferably applied by an inkjet method. The inkjet method that can be applied to apply the second ink is the same as the inkjet method that can be applied to apply the first ink described above, and the preferred embodiments are also the same.

[0143] In the image recording process, after the second ink is applied, the first ink (that is, the first ink layer) and the second ink (that is, the second ink layer) on the non-permeable substrate may be dried by heating. Means for carrying out the heating and drying include known heating means such as a heater, known air blowing means such as a dryer, and a combination of these. Examples of methods for performing heat drying include: A method of applying heat by a heater or the like to the side of the non-permeable substrate opposite to the side on which the first ink and the second ink are applied; a method of applying warm or hot air to the surface of the non-permeable substrate to which the first ink and the second ink have been applied; and a method of applying heat using an infrared heater from the surface of the non-permeable substrate to which the first ink and the second ink have been applied or the side opposite to the surface to which the inks have been applied. A combination of these methods, etc. The heating temperature during drying by heating is preferably 55° C. or higher, more preferably 60° C. or higher, and particularly preferably 65° C. or higher. There is no particular upper limit to the heating temperature, but the upper limit is, for example, 100° C., and preferably 90° C. The time for heating and drying is not particularly limited, but is preferably 3 to 60 seconds, more preferably 5 to 30 seconds, and particularly preferably 5 to 20 seconds.

[0144] [Method for producing laminate] As described above, according to the method for producing an image recorded material disclosed herein, it is possible to produce an image recorded material that comprises a non-permeable substrate and an image recorded on the non-permeable substrate, and that has excellent lamination strength when a substrate for lamination is laminated onto the image. Therefore, the method for producing an image recorded material disclosed herein is suitable for use in producing a laminated body comprising the above-mentioned image recorded material and a lamination substrate laminated to the side of the image recorded material on which the image is located. A method for producing the above laminate will now be described.

[0145] The method for producing a laminate according to the present disclosure includes: A step of obtaining an image recorded material by the method for producing an image recorded material according to the present disclosure; A step of laminating a substrate for lamination onto the side of the image recorded product on which the image is disposed to obtain a laminate; Includes.

[0146] According to the method for producing a laminated body of the present disclosure, it is possible to produce a laminated body having excellent lamination strength (i.e., peel strength) between an image-recorded material and a substrate for lamination.

[0147] For the process of obtaining an image recording material, the image recording method of the present disclosure described above can be referred to. The step of obtaining a laminate is a step of obtaining a laminate by laminating a substrate for lamination onto the side of the image recorded product on which the image is disposed.

[0148] The substrate for lamination is preferably a resin substrate. The resin substrate is not particularly limited, but examples thereof include substrates made of thermoplastic resins. An example of the resin substrate is a substrate obtained by molding a thermoplastic resin into a sheet shape. The resin substrate preferably comprises polypropylene, polyethylene terephthalate, nylon, polyethylene, or polyimide.

[0149] The shape of the resin substrate is not particularly limited, but a sheet-like resin substrate is preferred. The thickness of the resin substrate is preferably from 10 μm to 200 μm, and more preferably from 10 μm to 100 μm.

[0150] In this step, the substrate for lamination may be laminated directly onto the side of the image recorded product on which the image is disposed, or may be laminated via another layer (for example, an adhesive layer).

[0151] When the substrate for lamination is directly laminated onto the side of the image recorded product on which the image is disposed, the lamination can be carried out by a known method such as heat compression bonding or heat fusion bonding.

[0152] Furthermore, when laminating a substrate for lamination to the side of the image recorded material on which the image is arranged via an adhesive layer, the lamination can be carried out, for example, by a method in which an adhesive is applied to the side of the image recorded material on which the image is recorded, the substrate for lamination is then placed, and the image recorded material and the substrate for lamination are then bonded together. When laminating the image-recorded product on the image-positioned side via an adhesive layer, the lamination can also be performed by a method such as extrusion lamination (that is, sandwich lamination).

[0153] In the embodiment in which the image recorded product is laminated on the image-bearing side via an adhesive layer, the adhesive layer preferably contains an isocyanate compound. When the adhesive layer contains an isocyanate compound, the adhesion between the adhesive layer and the ink-derived layer of the image is further improved, so that the laminate strength can be further improved.

[0154] [Image Recording] An image recording according to an example of the present disclosure includes: a non-permeable substrate; and an image recorded on the non-permeable substrate; the image includes a pretreatment layer in contact with the non-permeable substrate and containing a flocculant, a first layer in contact with the pretreatment layer and containing a first pigment and a first resin, and a second layer in contact with the first layer and containing a second pigment and a second resin, and includes an overlapping region in which the pretreatment layer, the first layer, and the second layer overlap in a planar view; The flocculant is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex; In the overlapping region, the ratio of the total mass of the first resin and the second resin per unit area to the mass of the flocculant per unit area is 16.0 or more and 30.0 or less.

[0155] The image recorded matter according to this example has excellent lamination strength when a lamination substrate is laminated onto the image.

[0156] The image recorded matter according to this example is preferably manufactured by the manufacturing method of the image recorded matter of the present disclosure. In this case, the first layer corresponds to the first ink layer after drying, and the second layer corresponds to the second ink layer after drying. However, the first layer, the second layer, and the pretreatment layer may each contain residual solvent. The preferred aspects of each component in the image recorded matter according to this example are the same as the preferred aspects of each component explained in the section on the method for producing an image recorded matter of the present disclosure.

[0157] [Laminated body] A laminate according to one example of the present disclosure includes the image recorded matter of the present disclosure described above, and a lamination substrate laminated onto the image of the image recorded matter. The laminate according to this embodiment has excellent laminate strength.

[0158] In the laminate of this example, the lamination substrate may be laminated directly to the side of the image-recorded material on which the image is recorded, or may be laminated via another layer (adhesive layer). The laminate according to this example is preferably manufactured by the method for manufacturing a laminate according to the present disclosure. The preferred embodiments of the substrate for lamination and the adhesive layer are the same as those described in the section on the method for producing the laminate. EXAMPLES

[0159] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples. Hereinafter, unless otherwise specified, "%" and "parts" mean % by mass and parts by mass, respectively. "Tg" means the glass transition temperature, and the Tg difference (Ta-Tb) means the above-mentioned glass transition temperature difference (Ta-Tb). Ion-exchanged water was used as the "water."

[0160] <Preparation of pretreatment solution> Pretreatment solutions PC1, PC2, and PC3 were prepared as follows.

[0161] (Preparation of pretreatment solution PC1) The components shown below were mixed to prepare a pretreatment solution PC1.

[0162] -Composition of pretreatment solution PC1- Glutaric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.; flocculant (organic acid)) …4% by mass Resin particles PC1 (Tg50℃) … 5% by mass as the solid content of the resin particles PC1 shown below 1,2-propanediol (Fujifilm Wako Pure Chemical Industries, Ltd.; water-soluble organic solvent) …10% by mass ·water … The remaining amount that makes up 100% by mass

[0163] -Preparation of aqueous dispersion of resin particles PC1 (Tg50℃)- As an aqueous dispersion of resin particles PC1 (Tg 50° C.), “Pesresin A-520” (a 30 mass % aqueous dispersion of polyester resin particles (Tg 50° C.) as resin particles PC1) manufactured by Takamatsu Oil Co., Ltd. was prepared.

[0164] (Preparation of pretreatment solution PC2) Pretreatment solution PC2 was prepared in the same manner as pretreatment solution PC1, except that the glutaric acid used as the flocculant was changed to the same mass of calcium acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.; flocculant (organic acid salt)).

[0165] (Preparation of pretreatment solution PC3) A resin-free pretreatment liquid PC3 was prepared in the same manner as for preparing pretreatment liquid PC1, except that the aqueous dispersion of resin particles PC1 was not used and the amount of water was adjusted so that the glutaric acid content was 4 mass %.

[0166] <Preparation of the first and second inks> Inks A to H were prepared as the first inks, and inks I to M were prepared as the second inks. The first inks are all cyan inks, and the second inks are all white inks. Details are given below.

[0167] (Preparation of Ink A) The first ink, Ink A, was prepared as follows.

[0168] -Synthesis of pigment dispersing resin 1- 88g of methyl ethyl ketone was added to a 1000mL three-neck flask equipped with a stirrer and a cooling tube, and heated to 72°C under a nitrogen atmosphere. A solution of 0.85g of dimethyl 2,2'-azobisisobutyrate, 60g of benzyl methacrylate, 10g of methacrylic acid, and 30g of methyl methacrylate dissolved in 50g of methyl ethyl ketone was added dropwise over 3 hours. After the dropwise addition was completed and the mixture was allowed to react for another hour, a solution of 0.42g of dimethyl 2,2'-azobisisobutyrate dissolved in 2g of methyl ethyl ketone was added, and the temperature was raised to 78°C and heated for 4 hours. The resulting reaction solution was reprecipitated twice in a large excess of hexane, and the precipitated resin was dried. In this way, 96g of pigment dispersion resin 1, which is a benzyl methacrylate / methyl methacrylate / methacrylic acid copolymer (=60 / 30 / 10 [mass ratio]), was obtained. The composition of the resulting pigment dispersion resin 1 was: 1 The weight average molecular weight (Mw) was confirmed by H-NMR and calculated as polystyrene by GPC to be 44600. Furthermore, the acid value was determined by the method described in the JIS standard (JISK0070:1992) to be 65.2 mgKOH / g.

[0169] -Preparation of pigment dispersion C- CI Pigment Blue 15:3 (manufactured by Dainichi Seikagaku Kogyo Co., Ltd.) (4 parts) as a cyan pigment, the pigment dispersion resin 1 obtained as above (2 parts), methyl ethyl ketone (42 parts), 1N NaOH aqueous solution (5.5 parts), and water (87.2 parts) were mixed and dispersed in a bead mill using 0.1 mmφ zirconia beads at 2500 rpm (revolutions per minute, the same applies below) for 6 hours. The resulting dispersion was concentrated under reduced pressure at 55°C until methyl ethyl ketone was sufficiently distilled off, and after further removing some of the water, it was centrifuged (using a 50 mL centrifuge tube) at 8000 rpm for 30 minutes using a high-speed centrifugal chiller 7550 (manufactured by Kubota Seisakusho Co., Ltd.), the precipitate was removed, and the supernatant was collected. In this manner, pigment dispersion C containing a resin-coated pigment in which at least a portion of the cyan pigment was coated with pigment dispersing resin 1 was obtained.

[0170] -Preparation of aqueous dispersion of resin particles 1 (Tg 100°C)- A 2-liter three-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with 560.0 g of methyl ethyl ketone and heated to 87°C. Next, while maintaining the reflux state in the reaction vessel (hereinafter, the reflux state was maintained until the end of the reaction), a mixed solution consisting of 336.4 g of methyl methacrylate, 69.6 g of isobornyl methacrylate, 116.0 g of 2-ethylhexyl methacrylate, 58 g of methacrylic acid, 108 g of methyl ethyl ketone, and 2.32 g of "V-601" (a polymerization initiator manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.; dimethyl 2,2'-azobis(2-methylpropionate)) was added dropwise to the methyl ethyl ketone in the reaction vessel at a constant rate so that the drop was completed in 2 hours. After the dropwise addition was completed, the mixture was stirred for 1 hour, and then the operation of the following step (1) was performed on the solution after stirring for 1 hour. Step (1): A solution consisting of 1.16 g of "V-601" and 6.4 g of methyl ethyl ketone was added and stirred for 2 hours.

[0171] Next, the above step (1) was repeated four times, and then a solution consisting of 1.16 g of "V-601" and 6.4 g of methyl ethyl ketone was added and stirred for 3 hours (the operations up to this point are referred to as "reaction"). After the reaction was completed, the temperature of the solution was lowered to 65°C, 163.0 g of isopropanol was added, and the solution was allowed to cool to obtain a polymerization solution (solid concentration 41.0%) containing a methyl methacrylate / isobornyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid (=58 / 12 / 20 / 10 [mass ratio]) copolymer. The copolymer had a weight average molecular weight (Mw) of 35,000 and an acid value of 65.1 (mgKOH / g).

[0172] Next, 317.3 g of the obtained polymerization solution (solid concentration 41.0 mass%) was weighed out, and 46.4 g of isopropanol, 1.65 g of a 20% aqueous maleic anhydride solution (water-soluble acidic compound, equivalent to 0.3 mass% as maleic acid relative to the copolymer), and 40.77 g of a 2 mol / L aqueous NaOH solution were added thereto, and the temperature of the liquid in the reaction vessel was raised to 70°C. Next, 380 g of water was added dropwise to the solution heated to 70° C. at a rate of 10 mL / min to carry out aqueous dispersion (dispersion step). Then, the temperature of the liquid in the reaction vessel was kept at 70°C for 1.5 hours under reduced pressure to distill off 287.0 g of isopropanol, methyl ethyl ketone, and water (solvent removal step). 0.278 g of Proxel GXL(S) (Arch Chemicals Japan Co., Ltd.) (440 ppm as benzoisothiazolin-3-one relative to the polymer solid content) was added to the obtained liquid. The resulting liquid was filtered through a 1 μm filter, and the filtrate was collected to obtain an aqueous dispersion of resin particles 1 having a solid content concentration of 26.5% by mass. The Tg of the resin particles 1 was 100° C., and the volume average particle size was 10 nm.

[0173] -Preparation of Ink A- Ink A having the following composition was prepared using pigment dispersion C, an aqueous dispersion of resin particles 1, 1,2-propanediol (hereinafter also referred to as "PG"; a water-soluble organic solvent with a boiling point of less than 220°C), a surfactant (Olfine (registered trademark) E1010 manufactured by Nissin Chemical Industry Co., Ltd.), colloidal silica (Snowtex (registered trademark) XS (solid content 20% by mass) manufactured by Nissan Chemical Industries, Ltd.), and water.

[0174] -Composition of Ink A- Cyan pigment: 4% by weight Pigment dispersion resin 1... 2% by mass 1,2-propanediol (PG; water-soluble organic solvent with a boiling point of less than 220°C)... 25% by mass Surfactant (Olfine (registered trademark) E1010 manufactured by Nissin Chemical Industry Co., Ltd.)... 0.5% by mass ·Resin particles 1...5% by mass Colloidal silica (Nissan Chemical's Snowtex (registered trademark) XS (silica solid content 20% by mass))... 0.06% by mass as silica solid content Water: The balance that makes the total 100% by mass

[0175] (Preparation of Inks B to H) Inks B to H were prepared as first inks in the same manner as ink A, except that the ink compositions were changed as shown in Table 1. In Table 1, HDO is 1,2-hexanediol, which is a high boiling point solvent (i.e., an organic solvent with a boiling point of 220°C or higher); Resin particles 2 are resin particles synthesized as follows: The resin particles 3 are synthesized as follows.

[0176] -Preparation of aqueous dispersion of resin particles 2 (Tg 80°C)- An aqueous dispersion of resin particles 2 with a solids concentration of 26.5% by mass was obtained in the same manner as the aqueous dispersion of resin particles 1, except that the amount of each monomer was changed so that the copolymerization ratio [methyl methacrylate / isobornyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid] in the copolymer was 42 / 11 / 37 / 10 [mass ratio], the weight average molecular weight (Mw) was 35,000, and the acid value was 65.1 (mg KOH / g). The Tg of the resin particles 2 was 80° C., and the volume average particle size was 10 nm.

[0177] -Preparation of aqueous dispersion of resin particles 3 (Tg 120°C)- An aqueous dispersion of resin particles 3 with a solids concentration of 26.5% by mass was obtained in the same manner as the aqueous dispersion of resin particles 1, except that the amount of each monomer was changed so that the copolymerization ratio [methyl methacrylate / isobornyl methacrylate / 2-ethylhexyl methacrylate / methacrylic acid] in the copolymer was 70 / 16 / 4 / 10 [mass ratio], the weight average molecular weight (Mw) was 35,000, and the acid value was 65.1 (mg KOH / g). The Tg of the resin particles 3 was 120° C., and the volume average particle size was 10 nm.

[0178] (Preparation of Ink I) The second ink was prepared as follows.

[0179] -Synthesis of pigment dispersing resin 2- Pigment dispersing resin 2 was synthesized as shown below. Dipropylene glycol was added to a three-neck flask equipped with a stirrer and a condenser in an amount equal to the total amount of the monomers described below, and heated to 85° C. under a nitrogen atmosphere. Solution 1 was prepared by mixing 9.1 molar equivalents of stearyl methacrylate, 34.0 molar equivalents of benzyl methacrylate, 31.9 molar equivalents of hydroxyethyl methacrylate, 25.0 molar equivalents of methacrylic acid, and 0.8 molar equivalents of 2-mercaptopropionic acid, and solution 2 was prepared by dissolving 1% by mass of t-butylperoxy-2-ethylhexanoate (Perbutyl O manufactured by NOF Corp.) based on the total amount of monomers in 20% by mass of dipropylene glycol based on the total amount of monomers. Solution 1 was added dropwise to the three-neck flask over 4 hours, and solution 2 was added dropwise over 5 hours. After the dropwise addition, the mixture was allowed to react for another 2 hours, then the temperature was raised to 95°C and the mixture was heated and stirred for 3 hours to react all the unreacted monomer. The disappearance of the monomer was monitored by nuclear magnetic resonance ( 1 This was confirmed by H-NMR. The resulting reaction solution was heated to 70° C., and 20.0 molar equivalents of dimethylethanolamine was added as an amine compound, followed by the addition of propylene glycol and stirring to obtain a 30% by mass solution of pigment dispersing resin 2. The components of the resulting polymer are: 1 The weight average molecular weight (Mw) was determined by GPC and was found to be 22,000. The mass ratio of the constituent units in the pigment dispersion resin 2 was stearyl methacrylate-derived constituent units / benzyl methacrylate-derived constituent units / hydroxyethyl methacrylate-derived constituent units / methacrylic acid-derived constituent units=20 / 39 / 27 / 14. However, the above mass ratio does not include dimethylaminoethanol.

[0180] -Preparation of pigment dispersion W- A pigment dispersion W was prepared using a ready mill Model LSG-4U-08 (manufactured by Imex Co., Ltd.) as follows. In a zirconia container, 45 parts by mass of titanium dioxide particles (TiO2 particles; average primary particle diameter: 210 nm, product name: PF-690, manufactured by Ishihara Sangyo Kaisha, Ltd.) as a white pigment (white inorganic pigment), 15 parts by mass of a 30% by mass solution of the pigment dispersion resin 2, and 40 parts by mass of ultrapure water were added. Furthermore, 40 parts by mass of 0.5 mmφ zirconia beads (manufactured by TORAY, Toraceram beads) were added and mixed lightly with a spatula. The zirconia container containing the obtained mixture was placed in a ball mill and dispersed for 5 hours at a rotation speed of 1000 rpm. After the dispersion was completed, the beads were removed by filtration using a filter cloth, and a pigment dispersion W having a TiO2 concentration of 45% by mass was obtained.

[0181] -Preparation of Ink I- Ink I having the following composition was prepared using pigment dispersion W, an aqueous dispersion of resin particles 3, 1,2-propanediol (PG; a water-soluble organic solvent having a boiling point of less than 220°C), a surfactant (Olfine (registered trademark) E1010 manufactured by Nissin Chemical Industry Co., Ltd.), colloidal silica (Snowtex (registered trademark) XS (solid content 20% by mass) manufactured by Nissan Chemical Industries, Ltd.), and water.

[0182] - Composition of Ink I - ·White pigment (TiO2)…8% by mass Pigment dispersion resin 2... 0.5% by mass 1,2-propanediol (PG; water-soluble organic solvent with a boiling point of less than 220°C)... 25% by mass Surfactant (Olfine (registered trademark) E1010 manufactured by Nissin Chemical Industry Co., Ltd.)... 1.2% by mass ·Resin particles 3...6% by mass Colloidal silica (Nissan Chemical's Snowtex (registered trademark) XS (silica solid content 20% by mass))... 0.06% by mass as silica solid content Water: The balance that makes the total 100% by mass

[0183] (Preparation of Inks J to M) Inks J to M were prepared as second inks in the same manner as ink I, except that the ink compositions were changed as shown in Table 1.

[0184] [Table 1]

[0185] [Examples 1 to 21, Comparative Examples 1 to 8] The pretreatment liquid, the first ink, and the second ink were used in the combinations shown in Table 2, and the following measurements, image recording, and evaluations were carried out.

[0186] <Measurement of each ink> For the first inks (inks A to H), the surface tension and mixture viscosity A1 were measured by the method described above. In addition, the Tg (° C.) of the first resin in the first inks (inks A to H) was determined. The surface tension and mixture viscosity A2 of the second inks (inks I to M) were measured by the method described above. In addition, the Tg (° C.) of the second resin in the second inks (inks I to M) was determined. Based on the results obtained, the surface tension difference (i.e., the surface tension of the first ink minus the surface tension of the second ink), the mixture viscosity difference (A1-A2) (mPa s), and the Tg difference (Ta-Tb) (°C) for each example were calculated. The above results are shown in Table 2.

[0187] <Production of Image Recorded Material> A polyethylene terephthalate (PET) substrate ("FE2001" manufactured by Futamura Chemical Co., Ltd., thickness 12 μm, width 540 mm, length 4000 m) was prepared as a non-permeable substrate (hereinafter simply referred to as "substrate") on which an image was recorded.

[0188] A conveying mechanism for conveying the substrate; a wire bar coater for applying a pretreatment liquid, a first inkjet head for applying the first ink, and a second inkjet head for applying the second ink, which are arranged in this order from the upstream side in a transport direction of the substrate; An image recording device equipped with the above was prepared. Both the first inkjet head and the second inkjet head were 1200 dpi / 20 inch wide piezoelectric full line heads, where dpi stands for dots per inch. The first inkjet head and the second inkjet head were both arranged such that the nozzle arrangement direction was inclined at 75.7° with respect to the direction perpendicular to the transport direction of the substrate (ie, the width direction of the substrate). A liquid-repellent film containing a fluorine compound is provided on the ink ejection surface of each of the ink-jet heads (i.e., the first ink-jet head and the second ink-jet head). 17 It is a monolayer (SAM film) of C2H4SiCl3.

[0189] The substrate, the pretreatment liquid, the first ink, and the second ink were set in the image recording device, and the pretreatment liquid, the first ink, and the second ink were applied to the substrate under conditions (i.e., application arrangement) such that an overlapping region was generated in which the region to which the pretreatment liquid was applied, the region to which the first ink was applied, and the region to which the second ink was applied overlapped in a plan view, thereby recording an image. This resulted in a recorded image. Details are given below.

[0190] The pretreatment liquid was applied to the substrate using a wire bar coater while the substrate was moved at a constant speed of 500 mm / sec. The amount of the pretreatment liquid applied was the amount shown in the "Amount of pretreatment liquid applied" column in Table 2 (unit: g / m 2 The amount of flocculant added to the pretreatment liquid was the amount shown in the "Amount of flocculant added" column in Table 2 (unit: g / m 2 )

[0191] "Amount of pre-treatment liquid applied" (unit: g / m 2 ) is the value obtained by dividing the mass of the applied pretreatment liquid by the area of ​​the region to which the pretreatment liquid is applied. "Amount of flocculant applied" (unit: g / m 2 ) is the "amount of pretreatment liquid applied" (unit: g / m 2 ) and the content (mass %) of the flocculant relative to the total amount of the pretreatment liquid.

[0192] At the location where application of the pretreatment liquid was completed, drying of the pretreatment liquid was started using a dryer at 50° C. 1.5 seconds after application of the pretreatment liquid to this location was completed, and drying was completed 3.5 seconds after application of the pretreatment liquid was completed. The drying time at this time was 2 seconds.

[0193] While the substrate on which the pretreatment liquid had dried was moved at a constant stage speed of 50 mm / sec, the first ink was ejected from the first inkjet head onto the dried pretreatment liquid in the form of a solid image, and the second ink was ejected from the second inkjet head onto the applied first ink in the form of a solid image. At this time, the second ink was applied over the entire first ink applied onto the substrate. That is, the overlapping regions in the present examples and comparative examples coincide with the regions to which the first ink is applied and the regions to which the second ink is applied. The first ink and the second ink were then dried at 70° C. for 10 seconds. As a result, a solid image having a layered structure in which a white solid film made of the second ink film was laminated on a cyan solid film made of the first ink was obtained. That is, an image recorded product was obtained that had a substrate and the solid image provided on the substrate.

[0194] Here, the ejection conditions for both the first ink and the second ink were an ejection frequency of 24 kHz and a resolution of 1200 dpi×1200 dpi (dots per inch). The droplet volume of each of the first ink and the second ink when ejecting each of the first ink and the second ink was adjusted according to the application amount of each of the first ink and the second ink. For example, in Example 1, the droplet volume of the first ink was set to 3.0 pL (application amount of the first ink: 7.0 g / m 2 ), and the droplet volume of the second ink was 3.3 pL (corresponding to the application amount of the second ink of 7.8 g / m 2 (corresponding to). The first ink and the second ink were both deaerated through a degassing filter and had their temperature adjusted to 30° C. before use.

[0195] The application amount of the first ink and the application amount of the second ink are shown in the "Application amount of first ink" and "Application amount of second ink" columns in Table 2, respectively (units are g / m 2 The amounts of the first resin and the second resin applied were the amounts shown in the "Amount of the first resin applied" and "Amount of the second resin applied" columns in Table 2 (units are g / m for both). 2 )

[0196] "First ink application amount" (unit: g / m 2 ) is the mass of the first ink applied to the overlap region divided by the area of ​​the overlap region. "First resin application amount" (unit: g / m 2 ) is the "first ink application amount" (unit: g / m 2 ) and the content (mass %) of the first resin relative to the total amount of the first ink. "Amount of second ink applied" (unit: g / m 2 ) is the mass of the second ink applied to the overlap region divided by the area of ​​the overlap region. "Amount of second resin applied" (unit: g / m 2 ) is the "second ink application amount" (unit: g / m 2 ) and the content (mass %) of the second resin relative to the total amount of the second ink.

[0197] Based on the amount of flocculant applied, the amount of first resin applied, and the amount of second resin applied, the applied mass ratio [(first resin + second resin) / flocculant] (i.e., the ratio of the total applied mass of the first resin and the second resin per unit area to the applied mass of flocculant per unit area) was calculated. The obtained applied mass ratio [(first resin+second resin) / flocculant] is shown in the column "Applied amount ratio [resin / flocculant]" in Table 2.

[0198] <Evaluation> The above recorded image was evaluated as follows.

[0199] (Laminate strength (L strength)) From the image recorded product obtained above, a region of 500 mm length x 500 mm width in which a solid image was provided on the entire surface (hereinafter also referred to as a laminate strength evaluation region) was cut out to provide a laminate strength evaluation sample. A dry lamination adhesive (main agent TM-320 (isocyanate compound) / curing agent CAT-13B (alcohol compound), manufactured by Toyo-Morton Co., Ltd.) was applied onto the solid image of the laminate strength evaluation sample using a bar coater, and after drying at 70°C for 10 seconds, a non-oriented polypropylene film (CPP) film (product name: Pylen P1128, manufactured by Toyobo Co., Ltd., thickness 25 μm) was placed on top of it as a laminate substrate. In this state, the laminate substrate and the laminate strength evaluation sample were bonded together to obtain a laminate.

[0200] The resulting laminate was aged at 40° C. for 48 hours. A sample piece measuring 100 mm in length and 15 mm in width was cut out from the aged laminate. Next, the laminate substrate and the laminate strength evaluation sample were peeled off by hand in a region of 30 mm from one end in the longitudinal direction of the sample piece, while the laminate substrate and the laminate strength evaluation sample were left stuck together in the remaining region of 70 mm. Next, a tensile test was carried out in which the peeled portion of the laminate substrate and the laminate strength evaluation sample were pulled in opposite directions in the sample piece, perpendicular to the remaining 70 mm region (the region where the laminate substrate and the laminate strength evaluation sample remained attached). By this tensile test, the peel strength for peeling the laminate strength evaluation sample from the laminate substrate in the remaining region of 70 mm length was determined, and the obtained peel strength was regarded as the laminate strength. Based on the obtained laminate strength, the laminate strength between the laminate strength evaluation sample (i.e., the image recorded product) and the substrate for lamination was evaluated according to the following evaluation criteria, thereby evaluating the laminate strength between the image in the image recorded product and the substrate for lamination (hereinafter also referred to as "L strength"). The results are shown in Table 2. The tensile test was carried out using a tensile tester (TENSILON RTM-25, manufactured by Orientec Co., Ltd.).

[0201] -Evaluation criteria for laminate strength (L strength)- 5: The lamination strength between the image-recorded material and the lamination substrate is 2N / 15mm or more. 4: The lamination strength between the image-recorded material and the lamination substrate is 1.5 N / 15 mm or more and less than 2 N / 15 mm. 3: The lamination strength between the image-recorded material and the lamination substrate is 1 N / 15 mm or more and less than 1.5 N / 15 mm. 2: The lamination strength between the image-recorded material and the lamination substrate is 0.5 N / 15 mm or more and less than 1 N / 15 mm. 1: The lamination strength between the image-recorded material and the lamination substrate is less than 0.5 N / 15 mm.

[0202] <Evaluation of Adhesion> The adhesion of the image was evaluated by attaching a piece of Cellophane tape (registered trademark, No. 405, manufactured by Nichiban Co., Ltd., width 12 mm, hereinafter also referred to as "tape") to the solid image in the image recording material obtained above, and then peeling off the tape piece. Specifically, the tape was applied and peeled off in the following manner. The tape was removed at a constant speed and cut to a length of about 75 mm to obtain a tape strip. The obtained piece of tape was placed on the solid image, and a central area of ​​12 mm width and 25 mm length of the tape was applied with a finger and rubbed firmly with a fingertip. Within 5 minutes of applying the tape, the edge of the tape was grasped and peeled off at an angle as close to 60° as possible in 0.5–1.0 seconds. The presence or absence of any applied matter on the peeled tape piece and the presence or absence of peeling of the solid image on the recording medium were visually observed, and the adhesion of the image was evaluated according to the following evaluation criteria. The results are shown in Table 2. In the following evaluation criteria, the most excellent adhesion is ranked as "5".

[0203] -Adhesion evaluation criteria- 5: No deposits were found on the tape piece, and no peeling of the image on the recording medium was found. 4: A small amount of colored matter was observed on the tape piece, but no peeling of the image on the recording medium was observed. 3: A small amount of colored matter was found on the tape piece, and the image on the recording medium was slightly peeled off, but this was within the range that was practically acceptable. 2: Colored matter was found on the tape piece, and peeling was also found on the image on the recording medium, exceeding the practically acceptable range. 1: Colored matter was observed on the tape piece, the image on the recording medium was almost completely peeled off, and the recording medium was visible.

[0204] [Table 2]

[0205] -Explanation of Table 2- The units for the amount of pretreatment liquid applied, the amount of coagulant applied, the amount of first ink applied, the amount of first resin applied, and the amount of second ink applied are all g / m. 2 It is. The amount (%) of high boiling point solvent in the first ink means the content (mass %) of high boiling point solvent (specifically, 1,2-hexanediol (HDO)) relative to the total amount of the first ink, and the amount (%) of high boiling point solvent (specifically, 1,2-hexanediol (HDO)) in the second ink means the content (mass %) of high boiling point solvent relative to the total amount of the second ink. The surface tension difference refers to the surface tension of the first ink minus the surface tension of the second ink. The amount ratio [resin / coagulant] means the mass ratio [(first resin + second resin) / coagulant] (i.e., the ratio of the total mass of the first resin and the second resin per unit area to the mass of the coagulant per unit area). ·Ta-Tb is the value obtained by subtracting Tb from Ta, where Ta is the glass transition temperature of the resin particles contained in the first resin and the resin particles contained in the second resin that have a larger applied mass per unit area in the overlapping region, and Tb is the glass transition temperature of the resin particles contained in the first resin and the resin particles that have a smaller applied mass per unit area. A1-A2 is the value obtained by subtracting A2 from A1, where A1 is the viscosity of the mixture of the pretreatment liquid and the first ink, and A2 is the viscosity of the mixture of the pretreatment liquid and the second ink. The method for measuring A1-A2 is as described above.

[0206] As shown in Table 2, the image records of Examples 1 to 21 obtained by applying the pretreatment liquid, the first ink, and the second ink using a first ink and a second ink having a surface tension difference (i.e., the surface tension of the first ink minus the surface tension of the second ink) of more than 0 mN / m and under conditions in which the application amount ratio [resin / coagulant] was 16.0 or more and 30.0 or less, had excellent lamination strength (L strength) and image adhesion. In contrast, the image recording materials of Comparative Examples 1, 6 and 7, which were produced under conditions where the ratio of the amount of resin / aggregating agent applied was less than 16.0, had excellent image adhesion but had reduced laminate strength, presumably because excessive aggregation of the resin caused unevenness on the image surface and / or thickness variations. In addition, the image recording materials of Comparative Examples 2, 5, and 8, which were produced under conditions where the ratio of the amount of resin / coagulant applied was more than 30.0, showed reduced adhesion and laminate strength. This is believed to be because insufficient coagulation of the resin reduced the adhesion of the image, which is the basis of the laminate strength. In addition, the image records of Comparative Examples 3 and 4, which were produced using the first ink and the second ink with a surface tension difference of 0 mN / m or less, had excellent image adhesion but had reduced lamination strength. This is believed to be because the second ink did not spread sufficiently, causing unevenness on the image surface and / or thickness variations.

[0207] Among Examples 1, 2, 6 and 7, Examples 1 and 2 in which the ratio of the amount of resin / coagulant applied was 16.0 or more and 25.0 or less were superior in lamination strength and image adhesion.

[0208] Among Examples 1, 13, and 14, Example 1, in which the first ink did not contain a high-boiling point solvent (i.e., an organic solvent with a boiling point (bp) of 220°C or higher), and Example 13, in which the first ink contained a high-boiling point solvent but the content of the high-boiling point solvent was 5 mass% or less, had superior laminate strength and adhesion. Among Examples 1, 15, and 16, Example 1, in which the second ink did not contain a high-boiling point solvent (i.e., an organic solvent with a boiling point of 220°C or higher), and Example 15, in which the second ink contained a high-boiling point solvent but the content of the high-boiling point solvent was 5 mass% or less, had superior laminate strength and adhesion.

[0209] Comparing Examples 1 and 20, Example 1, in which the pretreatment liquid contained a resin and the Tg of the resin contained in the pretreatment liquid was lower than the Tg of the resin particles in the first resin, had superior laminate strength and adhesion compared to Example 20, in which the pretreatment liquid did not contain a resin. Comparing Examples 5 and 21, Example 5, in which the pretreatment liquid contained a resin and the Tg of the resin contained in the pretreatment liquid was lower than the Tg of the resin particles in the first resin, had superior laminate strength and adhesion.

[0210] Of Examples 1 and 18, Example 1, which satisfied the relationship 0° C.≦Ta−Tb≦30° C., was superior in lamination strength and adhesion.

[0211] Of Examples 1 and 19, Example 1, which satisfied A1-A2>0 mPa·s, was superior in laminate strength.

[0212] Although a group of examples in which cyan ink is used as the first ink and white ink is used as the second ink have been described above, the present disclosure is not limited to the aspects of these group of examples. For example, it goes without saying that the same effects as those of the above-mentioned embodiment group can be obtained if the first ink is changed to an ink other than cyan ink (e.g., magenta ink, yellow ink, black ink, etc.), if a multi-color image is recorded using cyan ink as the first ink and at least one ink other than cyan ink, and if at least one ink other than white ink is used as the second ink.

Claims

1. A step of preparing a pretreatment liquid containing a flocculant which is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex, a resin, and water; preparing a first ink containing a first pigment, a first resin, and water; preparing a second ink containing a second pigment, a second resin, and water, the second ink having a surface tension lower than that of the first ink; an image recording step of recording an image on a non-permeable substrate by applying the pretreatment liquid, the first ink, and the second ink in this order; Including, the resin contained in the pretreatment liquid is at least one selected from the group consisting of an acrylic resin, a polyester resin, a polyolefin resin, a polyurethane resin, a polyurea resin, a polyamide resin, a polycarbonate resin, and a polystyrene resin, and is a water-insoluble resin; The image recording process is a method for manufacturing an image recorded product, in which the image is recorded under conditions in which an overlapping region is generated in which an area to which the pretreatment liquid is applied, an area to which the first ink is applied, and an area to which the second ink is applied overlap in a planar view, and under conditions in which, in the overlapping region, a ratio of the total applied mass of the first resin and the second resin per unit area to the applied mass of the coagulant per unit area is 16.0 or more and 30.0 or less.

2. The method for producing an image recorded matter according to claim 1, wherein the ratio is 16.0 or more and 25.0 or less.

3. the first ink contains an organic solvent having a boiling point of 220° C. or higher in an amount of 5 mass % or less relative to the total amount of the first ink; 3 . The method for producing an image recorded matter according to claim 1 , wherein the second ink contains an organic solvent having a boiling point of 220° C. or higher in an amount of 5 mass % or less with respect to the total amount of the second ink.

4. the pretreatment liquid contains a resin, the first resin comprises resin particles; 4. The method for producing an image recorded matter according to claim 1, wherein the glass transition temperature of the resin contained in the pretreatment liquid is lower than the glass transition temperature of the resin particles contained in the first resin.

5. the first resin comprises resin particles; the second resin comprises resin particles; 5. The method for producing an image recorded matter according to claim 1, wherein, in the overlapping region, of the resin particles contained in the first resin and the resin particles contained in the second resin, a glass transition temperature of one having a larger applied mass per unit area is defined as Ta, and a glass transition temperature of one having a smaller applied mass per unit area is defined as Tb, where Ta and Tb satisfy a relationship of 0° C.≦Ta-Tb≦30° C.

6. 4. The method for producing an image recorded matter according to claim 1, wherein, when a viscosity of a mixture obtained by mixing the pretreatment liquid and the first ink is A1 and a viscosity of a mixture obtained by mixing the pretreatment liquid and the second ink is A2, A1 and A2 satisfy A1-A2>0 mPa s.

7. A step of obtaining an image recorded matter by the method for producing an image recorded matter according to any one of claims 1 to 6; a step of laminating a substrate for lamination onto the side of the image recorded product on which the image is recorded to obtain a laminate; A method for producing a laminate comprising the steps of:

8. a non-permeable substrate; and an image recorded on the non-permeable substrate; the image includes a pretreatment layer in contact with the non-permeable substrate, the pretreatment layer including a flocculant and a resin, a first layer in contact with the pretreatment layer, the first layer including a first pigment and a first resin, and a second layer in contact with the first layer, the second layer including a second pigment and a second resin, and includes an overlapping region in which the pretreatment layer, the first layer, and the second layer overlap in a planar view; The flocculant is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex; the resin contained in the pretreatment layer is at least one selected from the group consisting of an acrylic resin, a polyester resin, a polyolefin resin, a polyurethane resin, a polyurea resin, a polyamide resin, a polycarbonate resin, and a polystyrene resin, and is a water-insoluble resin; In the overlapping region, a ratio of a total mass of the first resin and the second resin per unit area to a mass of the aggregating agent per unit area is 16.0 or more and 30.0 or less.

9. The image recording material according to claim 8 , a lamination substrate laminated onto the image of the image recording material; A laminate body comprising:

Citation Information

Patent Citations

  • Image forming method

    JP2007125855A

  • Image forming method, image forming device and ink set

    JP2007331171A

  • Image forming method by inkjet recording device

    JP2013107224A

  • Inkjet recording method

    JP2015217591A

  • Printing method, printing apparatus, print set of pretreatment liquid, and ink and printed matter

    JP2017125158A