Aqueous coating material, can lid, and beverage can
A polymer emulsion combining specific monomers and a nonionic surfactant addresses curability and sterilization issues in water-based paints for can lids, achieving rapid curing and high resistance to steam sterilization without BPA or styrene.
Patent Information
- Application Number
- JP2024114436
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Existing water-based paints for can lids fail to provide sufficient curability in high-temperature, short-time baking processes, compromise steam sterilization resistance due to ionic surfactants, and cannot meet the demand for avoiding styrene use.
A polymer emulsion formed by combining specific ethylenically unsaturated monomers with a nonionic surfactant and radical polymerization initiator, along with a basic compound, to create a coating film with excellent steam sterilization resistance, processability, and adhesion, using a surfactant that does not reduce retort resistance.
The solution enables a coating film that can be cured quickly, exhibits excellent steam sterilization resistance, and maintains adhesion, even without using BPA or styrene, suitable for coating can lids.
Smart Images

Figure 2024133276000001 
Figure 2024133276000002 
Figure 2024133276000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-based paint, more particularly to a water-based paint suitable for use in coating the inner and outer surfaces of can lids for containing beverages or foods. More particularly, the present invention relates to a water-based paint capable of forming a coating film having excellent steam sterilization resistance (also called "retort resistance"), processability, and adhesion, and further to a coated can obtained by coating the inner and outer surfaces of the lid with the water-based paint. [Background technology]
[0002] Bisphenol A (hereinafter referred to as BPA) and epichlorohydrin are used as raw materials to synthesize BPA-type epoxy resins. BPA-type epoxy resins are suitable for use in coatings for the inside and outside of can lids because they have the ability to form coating films that are excellent in steam sterilization resistance, processability, and adhesion. Conventionally, organic solvent-based paints containing BPA-type epoxy resin and phenolic resin as a hardener have been commonly used as can paints, but due to the problem of global environmental pollution caused by organic solvents emitted from paints, organic solvent-based paints have been replaced by water-based paints. For this reason, the use of water-dispersible acrylic-modified epoxy resins, which are made by modifying BPA-type epoxy resins with acrylic resins and introducing carboxyl groups into the molecules, has become more widespread than ever before.
[0003] Generally, can lids are often painted by the so-called coil coating method, in which paint is continuously applied to a metal coil such as a coiled steel sheet or aluminum sheet (including aluminum alloy sheet) and then baked. Conventionally, the speed of painting lines has been increased to reduce production costs, and the painting method used is the reverse coat method, in which the applicator roll rotates in the opposite direction to the flow direction of the metal coil to paint. In recent years, with the further increase in line speed, baking is performed at higher temperatures and in shorter times than before in the paint baking process, and there is an increasing demand for paint that hardens when baked in an increasingly short time.
[0004] In view of this, Patent Document 1 discloses an aqueous coating material containing a resin obtained by emulsion polymerization of an aqueous dispersion of monomers including amide monomers, using an aqueous acrylic polymer having a carboxyl group as a high molecular weight emulsifier. Furthermore, Patent Document 2 discloses a water-based coating material that is characterized by containing core-shell type acrylic resin particles in which ammonium persulfate is suitably used as a polymerization initiator. Furthermore, Patent Document 3 discloses a water-based coating material that is characterized by containing core-shell type acrylic resin particles using an azo-based water-soluble initiator in addition to ammonium persulfate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-193834 A [Patent Document 2] Patent No. 5649763 [Patent Document 3] JP 2016-113561 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0006] However, the paint disclosed in Patent Document 1 cannot obtain sufficient hardening properties with recent high-temperature short-time baking. In addition, in the paint disclosed in Patent Document 2, an ionic water-soluble initiator such as ammonium persulfate is incorporated into the emulsion resin in the polymerization reaction and behaves as a type of surfactant, which causes a decrease in the steam sterilization resistance of the cured coating film. In addition, the paint disclosed in Patent Document 3 contains, as a monomer constituting the acrylic resin, substantially Generally, styrene is an essential component, and it is not possible to meet the demand for not using styrene.
[0007] The present invention aims to provide an aqueous paint that is suitable for use in coating the inner and outer surfaces of lids, which is capable of forming a coating film that has excellent retort resistance while using a surfactant that has conventionally been thought to be a factor in reducing retort resistance, and which can harden in a short period of time and form a coating film that has excellent steam sterilization resistance, processability and adhesion, and to provide a coated can whose inner and outer surfaces are coated with the aqueous paint. [Means for solving the problem]
[0008] In order to solve the above problems, the inventors conducted extensive research and discovered that a polymer emulsion obtained by polymerizing a specific combination of ethylenically unsaturated monomers in an aqueous medium in the presence of a surfactant is capable of forming a coating film that is excellent in steam sterilization resistance, processability and adhesion, even when a surfactant is used, and that the polymer emulsion can be suitably used as a water-based paint for coating the inside and outside of a lid, leading to the present invention.
[0009] That is, the present invention relates to an aqueous paint characterized by containing a polymer emulsion (D) obtained by polymerizing 100 parts by mass of a mixture (A) of ethylenically unsaturated monomers including a monofunctional (meth)acrylic acid ester monomer (A-1) having no carboxyl group, a monomer (A-2) having a carboxyl group, and at least one amide monomer (A-3) selected from the group consisting of N-alkoxyalkyl (meth)acrylamide, N-hydroxyalkyl (meth)acrylamide, and (meth)acrylamide, using 0.01 to 1 part by mass of a nonionic water-soluble radical polymerization initiator (C) in the presence of water and a surfactant (B), and a basic compound (E).
[0010] The present invention also relates to the above water-based coating material, which contains 1 to 20 mass % of a monomer (A-2) having a carboxyl group in 100 mass % of the mixture (A) of ethylenically unsaturated monomers.
[0011] The present invention also relates to the above water-based coating material, which contains 0.01 to 10 mass % of the amide monomer (A-3) in 100 mass % of the mixture (A) of ethylenically unsaturated monomers.
[0012] The present invention also relates to the above aqueous coating material, wherein the surfactant (B) is an anionic surfactant, and the aqueous coating material contains 0.01 to 5 parts by mass of the anionic surfactant per 100 parts by mass of the mixture of ethylenically unsaturated monomers (A).
[0013] The present invention also relates to the above water-based coating material, wherein the basic compound (E) is contained in an amount such that the neutralization rate is 1 to 50 mol % relative to the carboxyl groups of the polymer emulsion (D).
[0014] The present invention also relates to the above-mentioned water-based paint, characterized in that it contains either the phenol resin (F) or the amino resin (G).
[0015] Furthermore, the present invention relates to a can lid having at least one surface of a can lid member coated with the above-mentioned water-based paint.
[0016] Furthermore, the present invention relates to a beverage can comprising the above-mentioned can lid and a can body member. Effect of the Invention
[0017] The present invention does not use any BPA or styrene-derived components, and has excellent retort resistance while using surfactants, which have been considered to be a factor in reducing retort resistance. It has now become possible to provide an aqueous paint that is suitable for use in coating the inner and outer surfaces of lids, capable of forming a coating film that can be easily cured in a short period of time and that has excellent steam sterilization resistance, processability and adhesion, and a coated can whose lids have inner and outer surfaces coated with the aqueous paint. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The polymer emulsion (D) contained in the aqueous coating material of the present invention is obtained by radical polymerization of a specific monomer mixture in an aqueous medium using a nonionic water-soluble radical polymerization initiator (C) in combination with a surfactant, by a method that may be called an "emulsion polymerization method."
[0019] Next, various components used in the present invention will be described in detail. "Monomer" refers to a monomer having an ethylenically unsaturated double bond. "(Meth)acrylic" refers to acrylic and methacrylic. "(Meth)acrylate" refers to acrylate and methacrylate.
[0020] In the present invention, the mixture of ethylenically unsaturated monomers (A) contains a monofunctional (meth)acrylic acid ester monomer (A-1) having no carboxyl group, a monomer (A-2) having a carboxyl group, and at least one amide monomer (A-3) selected from the group consisting of N-alkoxyalkyl (meth)acrylamide, N-hydroxyalkyl (meth)acrylamide, and (meth)acrylamide.
[0021] <Monofunctional (meth)acrylic acid ester monomer (A-1) not having a carboxyl group> Examples of the monofunctional (meth)acrylic acid ester monomer (A-1) having no carboxyl group include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; Hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate Examples of the ethylenically unsaturated monomer include ethylenically unsaturated monomers having a hydroxyl group, such as acrylate, hydroxypentyl (meth)acrylate, and hydroxyhexyl (meth)acrylate. The mixture (A) of ethylenically unsaturated monomers is preferably composed of 70 to 98% by mass, more preferably 80 to 90% by mass of monomer (A-1). If it is 70% by mass or more, the appearance, adhesion and sanitation after retort are excellent, while if it is 98% by mass or less, the polymerization stability and hardness are excellent.
[0022] <Monomer having a carboxyl group (A-2)> Next, the monomer (A-2) having a carboxyl group will be described. Examples of the monomer (A-2) having a carboxyl group include (meth)acrylic acid, crotonic acid, (anhydrous) itaconic acid, (anhydrous) maleic acid, fumaric acid, citraconic acid, and cinnamic acid, and among these, (meth)acrylic acid is preferred. The monomer (A-2) having a carboxyl group is preferably contained in an amount of 1 to 20 mass% and more preferably 5 to 15 mass% of the mixture (A) of ethylenically unsaturated monomers (100 mass%). If it is 1 mass% or more, the polymerization stability and adhesion are excellent, while if it is 20 mass% or less, the appearance after retort is excellent. The monomer (A-2) having a carboxyl group, together with the surfactant (B), forms monomer droplets containing monomers other than (A-2) during radical polymerization of the monomer mixture (A), or can form other monomers in micelles consisting of the monomer having a carboxyl group. The monomer (A-2) having a carboxyl group, together with the surfactant (B), provides a site for polymerization in water for the ethylenically unsaturated monomer that is insoluble or poorly soluble in water. Therefore, the carboxyl group-containing monomer (A-2) has a large effect on the polymerization rate, molecular weight, emulsion particle size, emulsion stability, coating film properties, etc., and is therefore positioned as one of the most important components in the present invention.
[0023] <Amide Monomer (A-3)> Ethylenically unsaturated monomers include N-alkoxyalkyl(meth)acrylamides. , consisting of N-hydroxyalkyl (meth)acrylamide and (meth)acrylamide It is important that the composition contains at least one amide monomer (A-3) selected from the group consisting of: By including the amide monomer (A-3), a crosslinkable functional group can be introduced into the polymer dispersed in the polymer emulsion (D) obtained by radical polymerization of the emulsified component (A). By introducing a crosslinkable functional group, the coating material containing the polymer emulsion (D) can undergo self-crosslinking during the baking process after application, forming a strong coating film.
[0024] Examples of the amide monomer (A-3) include N-alkoxyalkyl(meth)acrylamides, N-hydroxyalkyl(meth)acrylamides, and (meth)acrylamides. Examples of N-alkoxyalkyl(meth)acrylamides include N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, N-(n-iso)butoxymethyl(meth)acrylamide ("Nn-butoxymethyl(meth)acrylamide" and "N-isobutoxymethyl(meth)acrylamide" are collectively referred to as "N-(n-iso)butoxymethyl(meth)acrylamide". The same applies below.), N-methoxyethyl(meth)acrylamide, N-ethoxyethyl(meth)acrylamide, and N-(n-iso)butoxyethyl(meth)acrylamide. Examples of the N-hydroxyalkyl(meth)acrylamide include N-hydroxymethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and N-hydroxybutyl(meth)acrylamide. Among the monomers (A-3), N-alkoxyalkyl(meth)acrylamides and N-hydroxyalkyl(meth)acrylamides are particularly preferred because they have higher reactivity than (meth)acrylamide.
[0025] In the ethylenically unsaturated monomer mixture (A) (100 mass%), the amide monomer (A-3) is preferably contained in an amount of 0.01 to 10 mass%, more preferably 2 to 5 mass%. If it is 0.01 mass% or more, the appearance and adhesion after retort are excellent, while if it is 10 mass% or less, the hygiene is excellent.
[0026] If necessary, for example, polyester resin, acrylic modified polyester resin, cellulose resin, polyvinyl alcohol or a derivative thereof, etc. may be added to the mixture (A) of ethylenically unsaturated monomers in the present invention and subjected to polymerization together with the monomers.
[0027] <Surfactant (B)> The surfactant (B) is preferably used in an amount of 0.01 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the mixture of ethylenically unsaturated monomers (A).
[0028] The surfactant is preferably anionic, but nonionic surfactants may also be used.
[0029] Examples of the anionic surfactant include higher fatty acid salts such as sodium oleate, alkylarylsulfonates such as dodecylbenzenesulfonic acid, alkyl sulfates such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate, alkyl sulfosuccinates such as sodium monooctyl sulfosuccinate, sodium dioctyl sulfosuccinate, and sodium polyoxyethylene lauryl sulfosuccinate, and derivatives thereof, and polyoxyethylene distyrenated phenyl ether sulfate.
[0030] <Nonionic water-soluble radical polymerization initiator (C)> Next, the nonionic water-soluble radical initiator (C) will be described. The nonionic radical polymerization initiator in the present invention has a solubility in water of less than 1.0% by mass. is treated as "water insoluble." In the present invention, the term "nonionic" refers to a property in which no cationic or anionic moieties exist in the molecular structure in water.
[0031] In the polymerization of the ethylenically unsaturated monomer mixture (A), it is important to use a nonionic water-soluble radical polymerization initiator. By using a nonionic water-soluble radical polymerization initiator, the water resistance and retort resistance of the coating film can be improved.
[0032] The nonionic water-soluble radical polymerization initiator (C) is preferably a peroxide or an azo initiator. Examples of the peroxide include hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, and p-menthane hydroperoxide. Examples of the azo initiator include 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and the like. Pionamide], etc. Among these, peroxides are preferable, and hydrogen peroxide and tert-butyl hydroperoxide are more preferable. The nonionic water-soluble radical polymerization initiator (C) can be used alone or in combination of two or more kinds.
[0033] The nonionic water-soluble radical polymerization initiator (C) is used in an amount of 0.01 to 1 part by mass, and preferably 0.02 to 0.5 parts by mass, per 100 parts by mass of the mixture of ethylenically unsaturated monomers (A). If the amount is 0.01 parts by mass or more, the mixture (A) of ethylenically unsaturated monomers reacts sufficiently to obtain a polymer, whereas if the amount is 1 part by mass or less, the molecular weight of the obtained polymer becomes sufficiently large to obtain a coating film having excellent processability and water resistance.
[0034] When polymerizing the monomer mixture, a reducing agent can be used in combination with the polymerization initiator. This can accelerate the polymerization reaction. Examples of such reducing agents include reducing organic compounds such as ascorbic acid, erythorbic acid, tartaric acid, citric acid, glucose, and metal salts of formaldehyde sulfoxylate, and reducing inorganic compounds such as sodium sulfite, sodium bisulfite, sodium metabisulfite (SMBS), sodium hyposulfite, and ferrous sulfate.
[0035] <Polymer Emulsion (D)> As described above, the polymer emulsion (D) in the present invention is prepared by dissolving a monofunctional (meth)acrylic acid ester monomer (A-1) having no carboxyl group, a monomer (A-2) having a carboxyl group, and an N-alkoxyalkoxyalkyl ester (A-3) in the presence of water and a surfactant (B). and at least one amide monomer (A-3) selected from the group consisting of N-hydroxyalkyl(meth)acrylamide, N-hydroxyalkyl(meth)acrylamide, and (meth)acrylamide. A) is polymerized.
[0036] In the present invention, the glass transition temperature (hereinafter also referred to as "Tg") of the polymer (hereinafter also referred to as dispersed resin) dispersed in the polymer emulsion (D) is preferably 0°C to 100°C, and more preferably 20°C to 80°C. In general, the processability of the coating film can be improved by lowering the Tg of the resin constituting the coating material. That is, when an aqueous coating material containing a polymer emulsion whose dispersed resin has a Tg of 0°C or more is used for coating the inside and outside surfaces of a can lid, it becomes easy to obtain a coating film that is not scratched during processing. In addition, the use of an aqueous coating material containing a polymer emulsion whose dispersed resin has a Tg of 100°C or less makes it easy to obtain a coating film with high extensibility that follows the molding processing of the lid. The above Tg is a value calculated from the weight fraction of each monomer to be polymerized and the Tg of a homopolymer of each monomer according to the FOX formula.
[0037] <Basic Compounds (E)> The basic compound (E) is used in the present invention to neutralize a part or all of the carboxyl groups in the carboxyl group-containing monomer (A-2) and improve the particle stability of the polyemulsion (D).
[0038] The basic compound (E) used in the present invention includes organic amine compounds, ammonia, and hydroxides of alkali metals. Examples of organic amine compounds include monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, monopropylamine, dipropylamine, monoethanolamine, diethanolamine, triethanolamine, N,N-dimethyl-ethanolamine, N,N-diethyl-ethanolamine, 2-dimethylamine, -2-Methyl-1-propanol, 2-ethanolamine, monoisopropanolamine, Examples include diisopropanolamine and triisopropanolamine. Examples of the hydroxides of alkali metals include lithium hydroxide, sodium hydroxide, and potassium hydroxide. These basic compounds (E) are neutralized at a rate of 1 to 50 mol % relative to the total amount (100 mol %) of the carboxyl groups of the dispersion resin in the polymer emulsion (D). It is preferable to use it in combination. If it is 1 mol % or more, the stability of the polymer emulsion (D) is excellent, and if it is 50 mol % or less, a coating material having a viscosity excellent in coatability can be obtained.
[0039] In addition to the above-mentioned polymer emulsion, one or more curing agents such as phenolic resin (F), amino resin (G), polyvinyl alcohol, and derivatives of polyvinyl alcohol may be added to the aqueous coating material of the present invention in order to improve the curing property and adhesion of the coating film. The phenol resin (F) and the amino resin (G) may undergo a self-crosslinking reaction, and may also react with the hydroxyl groups of the resin in the polymer emulsion (D) if such resin has such hydroxyl groups, and may also react with the crosslinkable functional groups derived from the amide monomer (A-3). In the present invention, the phenolic resin (F) used may be a trifunctional phenolic compound such as carbolic acid, m-cresol, or 3,5-xylenol, or an o-cresol or p-cresol. , p-tert-butylphenol or other bifunctional phenolic compounds and formaldehyde are reacted to form aldehydes. Examples include those reacted in the presence of a potassium catalyst. The phenol resin (F) is preferably added in an amount of 0.5 to 20 parts by mass, and more preferably 1 to 10 parts by mass, per 100 parts by mass of the solid content of the polymer emulsion (D) (that is, 100 parts by mass of the dispersed resin).
[0040] Examples of the amino resin (G) include compounds obtained by addition reaction of urea, melamine or benzoguanamine with formaldehyde. The amino resin (G) is added in an amount of preferably 0.5 to 20 parts by mass, and more preferably 1 to 10 parts by mass, per 100 parts by mass of the solid content of the polymer emulsion (D).
[0041] A hydrophilic organic solvent may be added to the water-based coating material of the present invention for the purpose of improving the coating properties. Examples of hydrophilic organic solvents include ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol mono(iso)propyl ether, ethylene glycol di(iso)propyl ether, ethylene glycol mono(iso)butyl ether, ethylene glycol di(iso)butyl ether, ethylene glycol mono-tert-butyl ether, ethylene glycol monohexyl ether, ethylene glycol monohexyl ether, 1,3 -butylene glycol-3-monomethyl ether, 3-methoxybutanol, 3-methyl-3-methoxybutanol, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol mono(iso)propyl ether, diethylene glycol di(iso)propyl ether, diethylene glycol mono(iso)butyl ether, diethylene glycol di(iso)butyl ether, diethylene glycol monohexyl ether, diethylene glycol dihexyl ether, triethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol Various ether alcohols or ethers such as glycol mono(iso)propyl ether, propylene glycol mono(iso)butyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol di(iso)propyl ether, propylene glycol di(iso)butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono(iso)propyl ether, dipropylene glycol mono(iso)butyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, diethylene glycol di(iso)propyl ether, and dipropylene glycol di(iso)butyl ether; Methyl alcohol, ethyl alcohol, propyl alcohol, isopropyl alcohol, butyl alcohol, sec-butyl alcohol, tert-butyl alcohol, furfuryl alcohol Alcoholic drinks such as cole; Ketones such as methyl ethyl ketone, dimethyl ketone, and diacetone alcohol; Glycols such as ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol; Examples of such alkoxy esters include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, 1-methoxy-2-propyl acetate, and propylene glycol monomethyl ether acetate. These may be used alone or in combination of two or more.
[0042] In addition, various auxiliary agents such as hydrophobic organic solvents, surfactants, and antifoaming agents may be added to the water-based paint of the present invention for the purpose of improving the coatability.
[0043] The water-based paint of the present invention can be used not only for the can lids described below but also for a wide range of general metal materials and metal products, but is preferably used as a paint for coating the inner and outer surfaces of can lids that contain beverages or food, and is particularly suitable for coating the outer surfaces of lids. Can lid materials include aluminum, tin-plated steel, chrome-treated steel, and nickel-treated steel. Plates and the like are used, and these materials may be subjected to surface treatments such as zirconium treatment or phosphate treatment.
[0044] The water-based paint of the present invention is preferably applied by roll coater coating, but it can also be applied by spray coating such as air spray, airless spray, electrostatic spray, dip coating, electrodeposition coating, or the like. The water-based paint of the present invention can form a film simply by volatilizing the volatile components after application, but in order to obtain excellent steam sterilization resistance, workability, and adhesion, it is better to add a baking process. The baking conditions are preferably baked at a temperature of 210°C to 300°C for 10 seconds to 20 minutes.
[0045] A can is obtained by combining a can lid coated with the water-based paint of the present invention with a can body member, and is preferably used for storing beverages and food, and is particularly useful as a beverage can. EXAMPLES
[0046] The present invention will be described in more detail below with reference to examples. Unless otherwise specified, "parts" simply means "parts by mass" and "%" means "% by mass".
[0047] [Synthesis Example 1] Synthesis of polymer emulsion (D-1) A reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, dropping vessel 1, dropping vessel 2, dropping vessel 3, and a nitrogen gas inlet tube was charged with 110 parts of deionized water, and the contents were heated to 50°C while stirring under a nitrogen stream. The temperature rose. A mixture of 61 parts of methyl methacrylate, 25 parts of butyl methacrylate, 9 parts of methacrylic acid, 5 parts of N-butoxymethylacrylamide, 0.2 parts of sodium dodecylbenzenesulfonate as a surfactant, and 40 parts of ion-exchanged water was mixed using a mixer to prepare a monomer pre-emulsion, and was charged into dropping tank 1 of the reaction vessel. Furthermore, 5 parts of 1% hydrogen peroxide solution was charged into the dropping tank 2, and 5 parts of 1% sodium erythorbate aqueous solution was charged into the dropping tank 3. While maintaining the temperature inside the reaction vessel at 50° C., the solution was continuously dropped from each dropping tank over a period of 2 hours. One hour and 1.5 hours after the dropping, 0.01 parts of 1% hydrogen peroxide solution and 1% sodium erythorbate aqueous solution were added, respectively, and the reaction was continued for 2.5 hours after the end of the dropping, to obtain a polymer emulsion (D-1) of an acrylic copolymer with a glass transition temperature of 70° C. (non-volatile content concentration was 39%). In addition, Table 1 does not list the additional polymerization initiator and reducing agent.
[0048] "Synthesis Examples 2-15, Comparative Synthesis Examples 1-4" Polymer emulsions (D-2) to (D-3) were prepared in the same manner as in Synthesis Example 1, except that the composition of the monomer pre-emulsion of polymer emulsion (D-1) was changed as shown in Tables 1 and 2. D-18) was obtained. In Comparative Synthesis Example 4, polymerization was attempted according to the composition shown in Table 1, but the polymerization stability was poor and a polymer emulsion (D-19) could not be obtained.
[0049] [Comparative Synthesis Example 5a] Synthesis of acrylic copolymer aqueous solution (D-20a) A reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube was charged with 8 parts of ethylene glycol monobutyl ether and 18.2 parts of ion-exchanged water, and heating was started to reflux at about 100° C. While maintaining reflux, a mixture of 10 parts of methacrylic acid, 6 parts of methyl methacrylate, 4 parts of ethyl acrylate, and 0.3 parts of benzoyl peroxide was continuously dropped from the dropping tank over a period of 4 hours to polymerize. 0.03 parts of benzoyl peroxide was added 1 hour and 2 hours after the end of the dropwise addition, and the reaction was continued for 3 hours after the end of the dropwise addition. An acrylic copolymer solution (non-volatile content 41%) with a glass transition temperature of 70°C was obtained. Next, 5.2 parts of dimethylethanolamine was added, and the mixture was stirred for 10 minutes, after which 46.3 parts of ion-exchanged water was added to dissolve the acrylic copolymer in water. As a result, an acrylic copolymer aqueous solution (D-20a) with a non-volatile content of 20% was obtained.
[0050] [Comparative Synthesis Example 5] Synthesis of polymer emulsion (D-20) A reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, dropping vessel 1, dropping vessel 2, dropping vessel 3, and a nitrogen gas inlet tube was charged with 32 parts of deionized water, and the content was heated to 50°C while stirring under a nitrogen stream. A mixture consisting of 47 parts of methyl methacrylate, 47 parts of butyl methacrylate, 6 parts of N-butoxymethylacrylamide, and 225 parts of the acrylic copolymer aqueous solution (D-20a) was mixed using a mixer to prepare a monomer pre-emulsion, which was then charged into the dropping tank 1 of the reaction vessel. Furthermore, 10 parts of 1% hydrogen peroxide solution was charged into the dropping tank 2, and 10 parts of 1% aqueous sodium erythorbate solution was charged into the dropping tank 3. While maintaining the temperature inside the reaction vessel at 50° C., the mixture was continuously added dropwise from each dropping tank for 2 hours. One hour and 1.5 hours after the addition, 0.01 parts of 1% hydrogen peroxide solution and 1% sodium erythorbate aqueous solution were added, respectively, and the reaction was continued for 2.5 hours after the end of the addition, to obtain a polymer emulsion (D-20) of an acrylic copolymer with a glass transition temperature of 27° C. (non-volatile content concentration 39%).
[0051] <Polymerization stability> The polymerization stability of the polymer emulsion (D) was evaluated as follows: The polymer emulsions obtained in Synthesis Examples and Comparative Synthesis Examples were filtered through a 180 mesh polyester filter cloth, and the amount of residue was visually evaluated. : Almost no residue is observed. ○: A small amount of residue was observed. △: A lot of residue was observed. ×: Coagulation occurred during polymerization, and no emulsion was obtained.
[0052] [Example 1] 100 parts of the polymer emulsion (D-1) obtained in Synthesis Example 1, 160 parts of ion-exchanged water The neutralization rate of the carboxyl group of the polymer emulsion (D-1) corresponds to 15 mol %. A certain amount of dimethylaminoethanol (DMAE) was mixed as a basic compound, and 4 parts of n-butanol and 6 parts of ethylene glycol monobutyl ether were further added to obtain a water-based paint (E-1) with a non-volatile content of 25%.
[0053] [Examples 2 to 17, Comparative Examples 1 to 4] Based on the formulations in Tables 3 and 4, the water-based paints (E-2) to (E-21) were obtained in the same manner as in Example 1.
[0054] <Evaluation of coating film> Each of the water-based paints obtained in Examples 1 to 17 and Comparative Examples 1 to 4 was applied to an aluminum plate having a thickness of 0.26 mm to a dry film thickness of 45 mg / dm 2The coating was then baked in a gas oven at an atmospheric temperature of 280° C. for 3 seconds to obtain a test panel for evaluation, and the performance of the coating film was evaluated as follows. Each evaluation method is explained below.
[0055] <Appearance of initial coating> The test panels are visually evaluated. ◎: The coating is smooth and free of bumps and bubbles. ○: There are a few tiny particles, but they do not cause any problems in practical use. △: The coating film has many bumps, which is problematic for practical use. ×: Significant bumps are present over the entire surface of the coating film. Not suitable for practical use.
[0056] <Appearance after retort> The test panel was immersed in water and retorted in a retort oven at 125°C for 30 minutes, and the appearance of the coating was visually evaluated. ◎: No change from untreated coating 〇: Very lightly whitened △: Slightly whitened ×: Significant whitening
[0057] <Adhesion after retort> The test panel was immersed in water and retorted in a retort oven at 125°C for 30 minutes. The coating surface was then cut into a grid pattern with a cutter, and cellophane adhesive tape was attached and peeled off firmly to evaluate the coating surface. ⊚: No peeling at all. ○: Less than 5% peeling. △: 5 to 50% peeling. ×: More than 50% peeling
[0058] <Evaluation of bending processability> The test panel was cut to a size of 30 mm x 50 mm and pre-folded by hand with the coating facing outward so that the test area was 30 mm wide. Five 0.26 mm thick aluminum plates were placed between the two folded test pieces and a 3 kg load was dropped from a height of 40 cm on the folded part to completely fold it. Next, the bent tip of the test piece was immersed in 1% saline solution, and a current of 6.0 V was passed between the metal part of the test piece that was not immersed in the saline solution and the saline solution for 4 seconds, and the current value was measured. If the coating has poor workability, the coating will crack in the bent area, exposing the underlying metal plate and increasing the electrical conductivity, resulting in a high current value. ◎: Less than 10mA ○: 10mA or more and less than 20mA △: 20mA or more and less than 50mA ×: 50mA or more
[0059] <Pencil hardness> This indicates the maximum hardness at which the coating does not peel off when measured using Mitsubishi Pencil Co., Ltd.'s "UNI" (registered trademark) in an environment of 25°C. ◎:5H or more 〇:3H-4H △:H-2H ×: F or less
[0060] <Hygiene> The test panel was immersed in water and retorted in a retort cooker at 125℃ for 30 minutes. The water after retort treatment was analyzed using a "TOC-LCPH" (Shimadzu Corporation) to measure the total organic carbon (TOC) content. The TOC content is the total amount of organic matter present in the water, expressed as the amount of carbon in the organic matter. ◎: Less than 2 ppm (good) ○: 2 ppm or more and less than 5 ppm (usable) ×: 5ppm or more (defective, unusable)
[0061] [Table 1]
[0062] [Table 2]
[0063] [Table 3]
[0064]
Table 4
Claims
1. The aqueous coating material comprises: a polymer emulsion (D) obtained by polymerizing, in the presence of water and a surfactant (B), 100 parts by mass of a mixture (A) of ethylenically unsaturated monomers, the mixture (A) containing a monofunctional (meth)acrylic acid ester monomer (A-1) having no carboxyl group, a monomer (A-2) having a carboxyl group, and at least one amide monomer (A-3) selected from the group consisting of N-alkoxyalkyl (meth)acrylamide, N-hydroxyalkyl (meth)acrylamide, and (meth)acrylamide, using 0.01 to 1 part by mass of a nonionic water-soluble radical polymerization initiator (C); and a basic compound (E).
2. 2. The aqueous coating material according to claim 1, comprising 1 to 20% by mass of a monomer (A-2) having a carboxyl group, based on 100% by mass of the mixture (A) of ethylenically unsaturated monomers.
3. 3. The aqueous coating material according to claim 1, comprising 0.01 to 10 mass% of the amide monomer (A-3) relative to 100 mass% of the mixture (A) of ethylenically unsaturated monomers.
4. The aqueous coating material according to any one of claims 1 to 3, wherein the surfactant (B) is an anionic surfactant and contains 0.01 to 5 parts by mass of the anionic surfactant per 100 parts by mass of the mixture (A) of ethylenically unsaturated monomers.
5. 5. The aqueous coating material according to claim 1, wherein the basic compound (E) is contained in an amount such that the neutralization rate is 1 to 50 mol % based on the carboxyl groups of the polymer emulsion (D).
6. 6. The water-based paint according to claim 1, which contains either a phenolic resin (F) or an amino resin (G).
7. A can lid member, at least one surface of which is coated with the water-based paint according to any one of claims 1 to 6.
8. A beverage can comprising the can lid according to claim 7 and a can body member.
Citation Information
Patent Citations
Acrylic emulsion composition
JP1999080485A
Polymer emulsion-containing aqueous coating material
JP2008255204A
Polymer emulsion-containing aqueous coating material
JP2008255205A
Water based paint, manufacturing method of water based paint, and coated can
JP2015193834A
Aqueous coating material and coated can
JP2019094428A