Laminated film, laminate, and packaging material

The laminated film structure with a polyolefin base and controlled anchor coat layer ensures gas barrier and adhesive properties are maintained post-retort treatment, addressing the issues of conventional films.

JP2024133299AActive Publication Date: 2024-10-01TOYOBO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024114836
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

Conventional gas barrier laminated films experience a decrease in gas barrier properties and adhesive strength due to damage from high temperatures during processing and retort treatment, leading to content leakage.

Method used

A laminated film structure with a base layer of polyolefin, an anchor coat layer containing a resin composition, and an inorganic thin film layer, designed to maintain gas barrier and adhesive properties even after retort treatment, with specific moisture and adhesion controls.

Benefits of technology

The laminated film maintains excellent oxygen and water vapor barrier properties and interlayer adhesion, preventing delamination after retort treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133299000001
    Figure 2024133299000001
  • Figure 2024133299000002
    Figure 2024133299000002
  • Figure 2024133299000003
    Figure 2024133299000003
Patent Text Reader

Abstract

To provide a laminated film which is excellent in oxygen and water vapor barrier property even after retort treatment, and has such adhesion as to prevent in delamination after the retort treatment.SOLUTION: There is provided a laminated film in which an anchor coat layer and an inorganic thin film layer are laminated in this order on a surface layer (B) of a base material film in which a surface layer (C), a base material layer (A) and the surface layer (B) are laminated in this order, with or without another layer interposed therebetween, wherein the surface layer (B) is formed of a resin composition containing two or more resins, a deposition amount of the anchor coat layer is less than 0.50 g / m2, and a moisture content of the laminated film is 0.2 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging material that has excellent gas barrier properties and adhesive strength even after being subjected to moist heat treatment such as boiling sterilization or retort sterilization. The present invention also relates to a laminate that has excellent material recycling suitability, and a packaging material using the same. [Background technology]

[0002] Packaging materials used for food, medicines, etc. are required to have gas barrier properties, that is, properties that block gases such as oxygen and water vapor, in order to inhibit oxidation of proteins and fats and oils, maintain flavor and freshness, and maintain the efficacy of medicines. In addition, gas barrier materials used in solar cells, organic electroluminescence (EL) and other electronic devices, electronic components, etc., require higher gas barrier properties than food packaging materials.

[0003] Conventionally, gas barrier laminate films in which a thin metal film such as aluminum or a thin inorganic oxide film such as silicon oxide or aluminum oxide is formed on the surface of a plastic substrate film have been commonly used in food applications that require blocking various gases such as water vapor and oxygen. Among them, those in which a thin inorganic oxide film such as silicon oxide, aluminum oxide, or a mixture thereof is formed are widely used because they are transparent and allow the contents to be confirmed.

[0004] However, the above-mentioned gas barrier laminate film may become locally hot during the formation process, causing damage to the substrate, or defects, pinholes, etc. in the inorganic thin film layer due to decomposition or degassing of the low molecular weight portion or additive portion such as plasticizer, etc., resulting in a decrease in gas barrier properties. Furthermore, there is a problem that the inorganic thin film layer may crack during post-processing of the packaging material, such as printing, lamination, and bag making, resulting in a decrease in gas barrier properties. In particular, if the inorganic thin film layer is damaged by the above-mentioned process, the gas barrier properties may be significantly decreased by the subsequent retort treatment, and the interlayer adhesive strength between the inorganic thin film and the resin in contact therewith may decrease, resulting in leakage of the contents.

[0005] As a method for improving the deterioration of a gas barrier laminate film having an inorganic thin film formed thereon, a method is known in which a coating layer made of various aqueous polyurethane resins, polyester resins, or a mixture of polyurethane and polyester is provided between a polyester base film and an inorganic thin film layer formed, for example, by a vapor deposition method (for example, Patent Document 1).

[0006] In addition to the gas barrier laminate film, many gas barrier films have been proposed by coating a resin composition on a base film. In particular, coating agents using polyvinyl alcohol or ethylene-vinyl alcohol copolymers, which have high oxygen barrier properties by themselves, have been put to practical use.

[0007] Furthermore, a gas barrier film has been proposed in which a layer having gas barrier properties, which is made by blending the vinyl alcohol resin with an inorganic layered compound such as montmorillonite, is coated on a base film made of plastic. For example, a layer having gas barrier properties composed of polyvinyl alcohol, a crosslinking agent, and an inorganic layered compound is provided on a base film, and a layer having gas barrier properties composed of an ethylene-vinyl alcohol copolymer, a water-soluble zirconium crosslinking agent, and an inorganic layered compound is provided on a base film (see, for example, Patent Documents 2 and 3). These gas barrier films have crosslinked resins, so they are moisture-resistant and can withstand water resistance to the extent of boiling, but when used for retort, the gas barrier properties and laminate strength after retort treatment performed under pressure at 120 to 130°C are not fully satisfactory. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 2-50837 [Patent Document 2] JP 2005-349769 A [Patent Document 3] JP 2008-297527 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made against the background of the problems of the conventional technology, and an object of the present invention is to provide a laminated film that has excellent oxygen and water vapor barrier properties even after retort treatment and has adhesion that does not cause interlayer delamination after retort treatment. [Means for solving the problem]

[0010] The inventors have discovered that by designing a specific laminate film tailored to the required performance, it is possible to provide a film that maintains good gas barrier properties and adhesion even when subjected to retort treatment, and have thus completed the present invention.

[0011] That is, the present invention comprises the following: 1. A laminated film in which a surface layer (C), a base layer (A), and a surface layer (B) are laminated in this order on the surface layer (B) of a base film, and an anchor coat layer and an inorganic thin film layer are laminated in this order with or without other layers interposed therebetween, the surface layer (B) being made of a resin composition containing two or more types of resins, and the adhesion amount of the anchor coat layer is 0.50 g / m 2 and the moisture content of the laminate film is 0.2 mass% or less. 2. The laminate film according to 1., wherein the anchor coat layer contains at least one of polyester resin and polyurethane resin. 3. The laminate film according to either 1 or 2, wherein the inorganic thin film layer is made of a metal oxide. 4. The laminate film or laminate film according to any one of 1. to 3., wherein the base layer (A) is made of a resin containing polyolefin as a main component. 5. A laminate comprising the laminate film according to any one of 1. to 4. above, and an olefin-based sealant layer laminated on the side opposite to the surface layer (C). 6. The laminate according to 5., characterized in that the laminate has a lamination strength of 2.0 N / 15 mm or more. 7. The laminate according to 5. or 6., characterized in that, when the oxygen permeability value of the laminate measured under conditions of 23°C × 65% RH is (A) and the oxygen permeability value of the laminate measured under conditions of 23°C × 65% RH after performing retort treatment in which the laminate is kept in pressurized hot water at a temperature of 130°C for 30 minutes is (B), the barrier value deterioration rate after wet heat treatment, represented by the following formula, is 150% or less. Barrier value deterioration rate after heat and moisture treatment (%) = (B / A) × 100 Formula (1) 8. A packaging material comprising at least one layer of the laminate film according to any one of 1. to 4. above, or the laminate according to 5. to 7. above. Effect of the Invention

[0012] By using this technique, the present inventors have been able to provide a laminate that retains the necessary properties, such as barrier properties and adhesive properties, required for packaging materials even after retort treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. A laminated film in which an anchor coat layer and an inorganic thin film layer are laminated in this order on the surface layer (B) of a substrate film having a surface layer (C), a substrate layer (A), and a surface layer (B) laminated in this order, the surface layer (B) being made of a resin composition containing two or more types of resins, and the coating amount of the anchor coat layer is 0.50 g / m 2 and the moisture content of the laminate film is 0.2 mass % or less. Each layer of the laminate will now be described.

[0014] [Base film layer] (1) Base material layer (A) The base layer of the present invention is preferably made of a polyolefin such as polypropylene or polyethylene resin, in order to make the moisture content in the laminated film 0.20% by mass or less. The term "main component" means that the ratio of a specific component to the total components is 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The polypropylene used in the layer may be a polypropylene copolymerized with ethylene and / or an α-olefin having 4 or more carbon atoms at 0.5 mol % or less. Such copolymerized polypropylene is also included in the polypropylene of the present invention (hereinafter, polypropylene). The copolymerization component is preferably 0.3 mol % or less, more preferably 0.1 mol % or less, and a completely homopolypropylene containing no copolymerization component is most preferable. When ethylene and / or an α-olefin having 4 or more carbon atoms is copolymerized in an amount exceeding 0.5 mol %, the crystallinity and rigidity are too low, and the thermal shrinkage rate at high temperatures may become large. Such resins may be blended and used.

[0015] The mesopentad fraction ([mmmm]%) measured by 13C-NMR, which is an index of stereoregularity of the polypropylene constituting the base layer (A) of the laminated film of the present invention, is preferably 98 to 99.5%, more preferably 98.1% or more, and even more preferably 98.2% or more. If the mesopentad fraction of the polypropylene is small, the elastic modulus will be low and the heat resistance may be insufficient. 99.5% is the practical upper limit.

[0016] The mass average molecular weight (Mw) of the polypropylene constituting the base layer (A) of the laminated film of the present invention is preferably 180,000 to 500,000. If the Mw is less than 180,000, the melt viscosity is low, so the resin is not stable during casting, and film-forming properties may be poor. If the Mw is more than 500,000, the amount of components with a molecular weight of 100,000 or less becomes 35% by mass, and heat resistance is deteriorated. A more preferred lower limit of Mw is 190,000, even more preferably 200,000, and a more preferred upper limit of Mw is 320,000, even more preferably 300,000, and particularly preferably 250,000.

[0017] The number average molecular weight (Mn) of the polypropylene constituting the base layer (A) of the laminated film of the present invention is preferably 20,000 to 200,000. If it is less than 20,000, the melt viscosity is low, so that the film-forming property may be deteriorated due to instability during casting, whereas if it exceeds 200,000, the heat resistance is deteriorated. A more preferable lower limit of Mn is 30,000, even more preferably 40,000, and particularly preferably 50,000, and a more preferable upper limit of Mn is 80,000, even more preferably 70,000, and particularly preferably 60,000.

[0018] Furthermore, the Mw / Mn, which is an index of molecular weight distribution, of the polypropylene constituting the base layer (A) is preferably 2.8 to 10, more preferably 2.8 to 8, still more preferably 2.8 to 6, and particularly preferably 2.8 to 5.4. The lower limit is preferably 3 or more, and more preferably 3.3 or more. The molecular weight distribution of polypropylene can be adjusted by polymerizing components of different molecular weights in a series of plants in multiple stages, blending components of different molecular weights offline in a kneader, blending catalysts with different performance properties and polymerizing them, or using a catalyst that can achieve the desired molecular weight distribution.

[0019] When the polypropylene constituting the base layer (A) of the laminated film of the present invention has an Mw / Mn in the range of 2.8 to 5.4, it preferably has a melt flow rate (MFR; 230° C., 2.16 kgf) of 2 g / 10 min to 20 g / 10 min. The lower limit of the MFR of the polypropylene of the base layer (A) is more preferably 3 g / 10 min, further preferably 4 g / 10 min, and particularly preferably 5 g / 10 min. The upper limit of the MFR of the polypropylene constituting the base layer (A) is more preferably 15 g / 10 min, and further preferably 12 g / 10 min. When the Mw / Mn and MFR of the polypropylene constituting the base layer (A) are within this range, the polypropylene can withstand hot water treatment, and also has good adhesion to a cooling roll and excellent film formability.

[0020] (2) Surface layer (B) The surface layer (B) of the present invention is preferably composed mainly of polyolefin such as polypropylene or polyethylene resin, in order to make the moisture content in the laminated film 0.20% by mass or less. The term "main component" means that the proportion of a specific component in the total components is 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. Hereinafter, polypropylene will be taken as an example for explanation. The polypropylene resin composition constituting the surface layer (B) of the laminated film of the present invention is preferably a resin composition containing two or more resins, and has an MFR of 1.0 g / 10 min to 10.0 g / 10 min. The lower limit of the MFR of the polypropylene resin composition constituting the surface layer (B) is more preferably 2.0 g / 10 min, even more preferably 3.0 g / 10 min, and particularly preferably 4.0 g / 10 min. The upper limit of the MFR of the polypropylene resin composition constituting the surface layer (B) is more preferably 9.0 g / 10 min, even more preferably 8.0 g / 10 min, and particularly preferably 5.5 g / 10 min. Within this range, the film formability is good and the appearance is excellent. If the MFR of the polypropylene resin composition constituting the surface layer (B) is smaller than 1.0 g / 10 min, when the MFR of the polypropylene constituting the base layer (A) is large, the viscosity difference between the base layer (A) and the surface layer (B) becomes large, and unevenness (unevenness of the original roll) is likely to occur during film formation. If the MFR of the polypropylene resin composition constituting the surface layer (B) exceeds 10 g / 10 min, the adhesion to the cooling roll will be poor, air will be entrapped, the smoothness will be poor, and there is a risk that many defects will occur due to this.

[0021] As polypropylene resins with a smaller MFR, polypropylenes copolymerized with ethylene and / or α-olefins having 4 or more carbon atoms can be used. Examples of α-olefins having 4 or more carbon atoms include 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. In addition, polar maleic acid and the like can be used as other copolymerization components. The total amount of ethylene and / or α-olefins having 4 or more carbon atoms and other copolymerization components is preferably 8.0 mol% or less. If copolymerized in excess of 8.0 mol%, the film may whiten and have a poor appearance, or may become sticky, making film formation difficult.

[0022] Further, each of the resins to be blended may be copolymerized at more than 8.0 mol %, but it is preferable that the blend contains, on a monomer unit basis, 8.0 mol % or less of monomers other than propylene. As the polypropylene resin having a larger MFR, the above-mentioned copolymer polypropylene can be used, or a homopolypropylene resin can be used.

[0023] The polypropylene resin composition constituting the surface layer (B) of the laminated film of the present invention is preferably a mixture of resin compositions with different crystallinity. By mixing polypropylene resin compositions with different crystallinity, the degree of crystallinity can be partially changed on the film surface, and the surface roughness of the film can be controlled. In addition, the surface hardness can be controlled within a desired range, and it is presumed that these effects enable the adhesion to be maintained even after boiling or retort treatment.

[0024] The antiblocking agent can be appropriately selected from inorganic particles such as silica, calcium carbonate, kaolin, and zeolite, and organic particles such as acrylic, polymethacrylic, and polystyrene. Among these, it is particularly preferable to use silica or polymethacrylic particles. The preferred average particle size of the antiblocking agent is 1.0 to 3.0 μm, and more preferably 1.0 to 2.7 μm. The average particle size is measured by taking a photograph with a scanning electron microscope, measuring the Feret's diameter in the horizontal direction using an image analyzer, and expressing the average value. There are no particular limitations on the amount of anti-blocking agent added, so long as the amount added to the surface layer (B) and surface layer (C) is adjusted so that the haze, dynamic friction coefficient, center surface average roughness (SRa), and air release time are within the specified ranges.

[0025] The surface wetting tension of the surface layer (B) of the laminated film of the present invention is preferably 38 mN / m or more. The wetting tension represents the surface tension (mN / m) of a mixed liquid reagent determined to wet the film surface, and is related to the wettability of printing inks and adhesives. If the wetting tension is 38 mN / m or more, the adhesion to the adhesive used for deposition film, coating film, and lamination with other member films is improved. In order to make the wetting tension 38 mN / m or more, additives such as antistatic agents and surfactants are usually used, but these methods have the effect of reducing the surface resistance value, so it is preferable to carry out physicochemical surface treatments such as corona treatment and heat treatment. For example, in the corona treatment, it is preferable to use a preheat roll and a treatment roll and perform discharge in the air.

[0026] (3) Surface layer (C) The laminated film of the present invention may have a surface layer (C) on the opposite side of the substrate layer (A) to the surface layer (B). The surface layer (C) of the present invention is preferably composed mainly of a polyolefin such as polypropylene or polyethylene resin, so that the moisture content in the laminated film is 0.20% by mass or less. The term "main component" means that the proportion of a specific component in the total components is 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The polypropylene used in the layer may be a polypropylene copolymerized with 0.5 mol % or less of ethylene and / or an α-olefin having 4 or more carbon atoms. Such copolymerized polypropylene is also included in the polypropylene of the present invention (hereinafter, polypropylene). The copolymerization component is preferably 0.3 mol % or less, more preferably 0.1 mol % or less, and a completely homopolypropylene containing no copolymerization component is most preferred. When ethylene and / or an α-olefin having 4 or more carbon atoms is copolymerized in an amount exceeding 0.5 mol %, the crystallinity and rigidity are too low, and the thermal shrinkage rate at high temperatures may become large. Such resins may be blended and used.

[0027] The surface layer (C) preferably has a center surface average roughness (SRa) of 0.020 μm or more as measured by a three-dimensional surface roughness meter. The center surface average roughness (SRa) of the surface layer (C) is more preferably 0.022 μm or more, even more preferably 0.025 μm or more, and particularly preferably 0.028 μm or more. If the center surface average roughness (SRa) of the surface layer (C) is less than 0.020 μm, the surface unevenness is small, and the slipperiness of the film, the air release time between the films, and the blocking resistance are deteriorated. There are several methods for setting the center surface average roughness (SRa) of the surface layer (C) within the specified range, and it is possible to adjust it by the average particle size and the amount of the antiblocking agent added. The surface layer (C) of the laminate of the present invention preferably has a center surface average roughness (SRa) of 0.040 μm or less as measured by a three-dimensional roughness meter.

[0028] The polypropylene resin used in the present invention is obtained by polymerizing the raw material propylene using a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst. Among them, it is preferable to use a Ziegler-Natta catalyst in order to eliminate heterogeneous bonds, and to use a catalyst capable of polymerization with high stereoregularity. As a method for polymerizing the raw material propylene, a known method may be adopted, and examples thereof include a method of polymerizing in an inert solvent such as hexane, heptane, toluene, or xylene, a method of polymerizing in a liquid monomer, a method of adding a catalyst to a gaseous monomer and polymerizing in a gas phase state, or a method of polymerizing by combining these methods.

[0029] The base layer (A) and / or the surface layer (B) and / or the surface layer (C) of the laminated film of the present invention may contain additives or other resins. Examples of additives include antioxidants, ultraviolet absorbers, nucleating agents, adhesives, antifogging agents, flame retardants, inorganic or organic fillers, etc. Examples of other resins include polypropylene resins other than the polypropylene resin used in the present invention, random copolymers which are copolymers of propylene and ethylene and / or α-olefins having 4 or more carbon atoms, and various elastomers. These may be sequentially polymerized using a multi-stage reactor, blended with polypropylene resin using a Henschel mixer, master pellets prepared in advance using a melt kneader may be diluted with polypropylene to a predetermined concentration, or the entire amount may be melt kneaded and used. Furthermore, as long as the object of the present invention is not impaired, corona discharge treatment, glow discharge treatment, flame treatment, surface roughening treatment, and known anchor coat treatment, printing, decoration, etc. may be performed.

[0030] As a method for producing the base film of the present invention, a biaxially oriented film is preferably produced, and the film can be obtained by melt-extruding the polypropylene resin composition constituting the base layer (A), the polypropylene resin composition constituting the surface layer (B), and the polypropylene resin composition constituting the surface layer (C) using separate extruders, co-extruding them through a die, and cooling them with a cooling roll to form an unstretched sheet, stretching the unstretched sheet in the machine direction (MD) and the transverse direction (TD), and then subjecting it to a heat setting treatment. The melt extrusion temperature is preferably about 200 to 280°C. In order to obtain a laminate with good appearance without disturbing the layers within this temperature range, it is preferable that the viscosity difference (MFR difference) between the polypropylene raw material for the base layer (A) and the polypropylene raw material for the surface layer (B) is 6.0 g / 10 min or less. If the viscosity difference is more than 6 g / 10 min, the layers are likely to be disturbed and the appearance is likely to be poor. The viscosity difference is more preferably 5.5 g / 10 min or less, and even more preferably 5.0 g / 10 min or less. In addition, the surface temperature of the cooling roll is preferably 25 to 35°C, and more preferably 27 to 33°C.

[0031] The lower limit of the stretching ratio in the machine direction (MD) is preferably 3 times, more preferably 3.5 times. If it is less than the above, the film thickness may become uneven. The upper limit of the stretching ratio in the MD is preferably 8 times, more preferably 7 times. If it exceeds the above, the subsequent TD stretching may become difficult. The lower limit of the MD stretching temperature is preferably 120 ° C, more preferably 125 ° C, and even more preferably 130 ° C. If it is less than the above, the mechanical load may become large, the thickness unevenness may become large, and the surface roughness of the film may occur. The upper limit of the MD stretching temperature is preferably 160 ° C, more preferably 155 ° C, and even more preferably 150 ° C. A higher temperature is preferable because it reduces the dimensional change during the moist heat treatment and reduces the deterioration of the barrier property and adhesion, but it may adhere to the roll, making it impossible to stretch, or cause surface roughness.

[0032] The lower limit of the stretching ratio in the transverse direction (TD) is preferably 4 times, more preferably 5 times, and even more preferably 6 times. If it is less than the above, thickness unevenness may occur. The upper limit of the TD stretching ratio is preferably 20 times, more preferably 17 times, even more preferably 15 times, and particularly preferably 12 times. If it exceeds the above, the heat shrinkage rate may increase or the film may break during stretching. The preheating temperature in TD stretching is preferably set to be 5 to 15°C higher than the stretching temperature in order to quickly raise the film temperature to the vicinity of the stretching temperature. The lower limit of the TD stretching temperature is preferably 150°C, more preferably 155°C, even more preferably 158°C, and especially preferably 160°C. If it is less than the above, the film may break due to insufficient softening, or the dimensional change may be large during wet heat treatment, resulting in deterioration of barrier properties and adhesion. The upper limit of the TD stretching temperature is preferably 170°C, more preferably 168°C, and even more preferably 165°C. A higher temperature is preferred to reduce dimensional change, but if the temperature exceeds the upper limit, the low molecular weight components will melt and recrystallize, resulting in a decrease in orientation and possibly causing surface roughness and whitening of the film.

[0033] The stretched film is heat-set. The lower limit of the heat-set temperature is preferably 163°C, more preferably 165°C. If the temperature is lower than the above, the dimensional change during wet heat treatment is large, and the barrier property and adhesion may deteriorate. In addition, a long treatment time may be required to reduce the dimensional change, and the productivity may be poor. The upper limit of the heat-set temperature is preferably 176°C, more preferably 175°C. If the temperature exceeds the above, low molecular weight components may melt and recrystallize, causing surface roughness and whitening of the film.

[0034] It is preferable to relax the film during heat setting. The lower limit of the relaxation rate is preferably 2%, and more preferably 3%. If it is less than the above, the dimensions will change significantly during wet heat treatment, and the barrier properties and adhesion may deteriorate. The upper limit of the relaxation rate is preferably 10%, and more preferably 8%. If it exceeds the above, thickness unevenness may increase.

[0035] Furthermore, in order to reduce dimensional changes, the film produced by the above process can be wound into a roll and then annealed off-line.

[0036] The biaxially oriented polypropylene laminate thus obtained can be subjected to corona discharge, plasma treatment, flame treatment, etc., as required, and then wound up with a winder to obtain the biaxially oriented polypropylene film roll of the present invention.

[0037] [Anchor coat layer] In the present invention, an anchor coat layer is provided on the surface layer (B). By providing the anchor coat layer, it is possible to suppress the exposure of oligomers and antiblocking materials from the polypropylene resin. Furthermore, when other layers are laminated on the anchor coat layer, it is also possible to increase the adhesion between the layers. In particular, in the formation of an inorganic thin film layer, there is a problem not only of adhesion but also of the fact that a thin film cannot be formed at protruding parts due to surface unevenness, resulting in poor barrier properties. In addition, by using a material having gas barrier properties for the anchor coat layer itself, the gas barrier performance of the laminate can be greatly improved. Furthermore, by laminating a water-resistant anchor coat layer, the intrusion of hot water is prevented, and as a result, defects such as barrier properties and adhesion after boiling and retort treatment can be reduced. Since a resin component having a polar group or the like is introduced into the anchor coat layer to ensure the necessary adhesion, it is often composed of a material with a high moisture content. The present inventors have newly discovered that the defects after the wet heat treatment can be improved by controlling the moisture content of the entire laminate film to a predetermined amount. In order to control the moisture content of the laminated film within the preferred range described below, it is necessary to adopt a composition and / or processing conditions that exhibit adhesion and barrier properties in a small adhesion amount of the anchor coat layer described below.

[0038] In the present invention, the adhesion amount of the anchor coat layer is 0.01 to 0.50 g / m 2 This allows the anchor coat layer to be uniformly controlled during coating, resulting in a film with fewer coating irregularities and defects. The amount of the anchor coat layer is preferably 0.05 g / m 2 More preferably, 0.10 g / m 2 or more, preferably 0.47 g / m 2 Less than or equal to 0.45 g / m 2 The adhesion weight of the anchor coat layer is 0.50 g / m or less. 2If the thickness of the protective layer exceeds 0.01 g / m, the gas barrier property is improved, but the moisture content in the laminated film increases due to the thick film thickness. In terms of processability, the thick film thickness may cause blocking. Furthermore, there is a concern that it may have a negative effect on the recyclability and manufacturing costs of the film. On the other hand, 2 If it is less than this, there is a risk that sufficient gas barrier properties and interlayer adhesion cannot be obtained.

[0039] The resin composition used in the anchor coat layer of the present invention may be a resin such as a urethane-based, polyester-based, acrylic-based, titanium-based, isocyanate-based, imine-based, or polybutadiene-based resin to which a curing agent such as an epoxy-based, isocyanate-based, or melamine-based curing agent has been added. It may further contain a crosslinking agent such as a silicon-based crosslinking agent, an oxazoline compound, a carbodiimide compound, or an epoxy compound. In particular, the inclusion of a urethane resin is preferable because, in addition to the barrier performance due to the high cohesiveness of the urethane bond itself, the polar group interacts with the inorganic thin film layer, and the presence of amorphous parts gives flexibility, so that damage can be suppressed even when a load is applied due to a wet heat treatment. In addition, a polyester resin is also preferable because it can be expected to have the same effect. In the present invention, it is preferable to contain a polyurethane having polyester + isocyanate as constituent components, and it is more preferable to add a silicon-based crosslinking agent from the viewpoint of improving water-resistant adhesion.

[0040] (1) Urethane resin From the viewpoint of improving the barrier property by the cohesive force, the urethane resin used in the present invention preferably has a glass transition temperature (Tg) of 100°C or more, more preferably 110°C or more, and even more preferably 120°C or more. However, in order to develop adhesive force, a soft resin having excellent flexibility and a Tg of 100°C or less may be mixed and used. In that case, the addition ratio of the soft resin is preferably within the range of 0 to 80%, more preferably within the range of 10 to 70%, and even more preferably within the range of 20 to 60%. When the addition ratio is within the above range, it is possible to achieve both cohesive force and flexibility, and the barrier property and adhesive property are good. Note that, if the addition ratio exceeds 80%, the film becomes too soft, which may lead to a decrease in barrier performance.

[0041] From the viewpoint of improving gas barrier properties, it is more preferable to use a urethane resin containing an aromatic or araliphatic diisocyanate component as a main constituent component. Among these, it is particularly preferable to contain a metaxylylene diisocyanate component. By using the above resin, the cohesive strength of the urethane bond can be further increased due to the stacking effect between aromatic rings, and as a result, good gas barrier properties can be obtained.

[0042] In the present invention, the proportion of aromatic or araliphatic diisocyanate in the urethane resin is preferably 50 mol% or more (50 to 100 mol%) in 100 mol% of the polyisocyanate component (F). The proportion of the total amount of aromatic or araliphatic diisocyanate is preferably 60 to 100 mol%, more preferably 70 to 100 mol%, and even more preferably 80 to 100 mol%. If the proportion of the total amount of aromatic or araliphatic diisocyanate is less than 50 mol%, good gas barrier properties may not be obtained.

[0043] (2) Silicon-based crosslinking agents In the urethane resin used in the present invention, various crosslinking agents may be blended in order to improve the cohesive strength and the wet heat resistance adhesion of the film, as long as the gas barrier properties are not impaired. Examples of crosslinking agents include silicon-based crosslinking agents, oxazoline compounds, carbodiimide compounds, and epoxy compounds. Among them, silicon-based crosslinking agents are particularly preferred from the viewpoint that the water-resistant adhesion with the inorganic thin film layer can be improved by blending the silicon-based crosslinking agent. In addition, oxazoline compounds, carbodiimide compounds, and epoxy compounds may be used in combination as crosslinking agents.

[0044] As the silicon-based crosslinking agent, a silane coupling agent is preferred from the viewpoint of crosslinking between inorganic and organic substances. As the silane coupling agent, hydrolyzable alkoxysilane compounds, for example, halogen-containing alkoxysilanes (chloro C2-4 alkyl tri C1-4 alkoxysilanes such as 2-chloroethyl trimethoxysilane, 2-chloroethyl triethoxysilane, 3-chloropropyl trimethoxysilane, 3-chloropropyl triethoxysilane, etc.), alkoxysilanes having epoxy groups [2-glycidyloxyethyl trimethoxysilane, 2-glycidyloxyethyl triethoxysilane, 3-glycidyloxypropyl ... trimethoxysilane, glycidyloxy C2-4 alkyl tri C1-4 alkoxysilanes such as 3-glycidyloxypropyl triethoxysilane, glycidyloxy di C2-4 alkyl di C1-4 alkoxysilanes such as 3-glycidyloxypropyl methyl dimethoxysilane and 3-glycidyloxypropyl methyl diethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl triethoxysilane, 3-(3,4-epoxycyclohexyl)propyl (epoxycycloalkyl)C2-4 alkyltriC1-4 alkoxysilanes such as 2-aminoethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and other amino C2-4 alkyltriC1-4 alkoxysilanes, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, and other amino diC2-4 alkyldiC1-4 alkoxysilanes, 2-[N-(2-aminoethyl)amino (2-amino C2-4 alkyl) amino C2-4 alkyl tri C1-4 alkoxy silanes such as 3-[N-(2-aminoethyl)amino]ethyltrimethoxysilane, 3-[N-(2-aminoethyl)amino]propyltrimethoxysilane, and 3-[N-(2-aminoethyl)amino]propyltriethoxysilane; (amino C2-4 alkyl) amino di C2-4 alkyl di C1-4 alkoxy silanes such as 3-[N-(2-aminoethyl)amino]propylmethyldimethoxysilane and 3-[N-(2-aminoethyl)amino]propylmethyldiethoxysilane;Alkoxysilanes having a mercapto group (mercapto C2-4 alkyl tri C1-4 alkoxysilanes such as 2-mercaptoethyl trimethoxysilane, 3-mercaptopropyl trimethoxysilane, 3-mercaptopropyl triethoxysilane, mercapto di C2-4 alkyl di C1-4 alkoxysilanes such as 3-mercaptopropyl methyl dimethoxysilane, 3-mercaptopropyl methyl diethoxysilane, etc.), alkoxysilanes having a vinyl group (vinyl tri C1-4 alkoxysilanes such as vinyl trimethoxysilane, vinyl triethoxysilane, etc.), ethylene Examples of the silane coupling agents include alkoxysilanes having a reactive unsaturated bond group [(meth)acryloxy C2-4 alkyl tri C1-4 alkoxysilanes such as 2-(meth)acryloxyethyl trimethoxysilane, 2-(meth)acryloxyethyl triethoxysilane, 3-(meth)acryloxypropyl trimethoxysilane, and 3-(meth)acryloxypropyl triethoxysilane, and (meth)acryloxy di C2-4 alkyl di C1-4 alkoxysilanes such as 3-(meth)acryloxypropyl methyl dimethoxysilane and 3-(meth)acryloxypropyl methyl diethoxysilane, etc.]. These silane coupling agents can be used alone or in combination of two or more. Among these silane coupling agents, silane coupling agents having an amino group are preferred.

[0045] The silicon-based crosslinking agent is preferably added in an amount of 0.05 to 4.00% by mass in the coating layer, more preferably 0.10 to 3.50% by mass, and even more preferably 0.15 to 3.00% by mass. The addition of the silane coupling agent promotes the hardening of the film and improves the cohesive force, resulting in a film with excellent water-resistant adhesion, and is also expected to have the effect of preventing the exposure of oligomers. If the amount added exceeds 3.00% by mass, the hardening of the film progresses and the cohesive force improves, but some unreacted portions may be generated, and the adhesion between layers may decrease. On the other hand, if the amount added is less than 0.05% by mass, sufficient cohesive force may not be obtained.

[0046] (3) Polyester resin The polyester resin used in the present invention is produced by polycondensation of a polyvalent carboxylic acid component and a polyhydric alcohol component. The molecular weight of the polyester is not particularly limited as long as it can provide sufficient film toughness, coating suitability, and solvent solubility as a coating material, but is preferably 1000 to 50000 in number average molecular weight, more preferably 1500 to 30000. The functional group at the polyester end is also not particularly limited, and may be an alcohol end, a carboxylic acid end, or both. However, when an isocyanate-based curing agent is used in combination, it is necessary to use a polyester polyol mainly composed of alcohol ends.

[0047] The Tg of the polyester used in the present invention is preferably 15°C or higher. If the temperature is lower than this, the resin becomes sticky after the coating operation, tends to cause blocking, and makes the winding operation after coating difficult. If the Tg is 15°C or lower, it becomes difficult to prevent blocking even under conditions where the pressure near the winding core is high, even with the addition of an anti-blocking agent. The Tg temperature is more preferably 18°C ​​or higher, and even more preferably 25°C or higher.

[0048] The polyester used in the present invention is prepared by polycondensing a polyvalent carboxylic acid component and a polyhydric alcohol component. [Polycarboxylic acid component] The polycarboxylic acid component of the polyester used in the present invention is characterized by containing at least one of ortho-oriented aromatic dicarboxylic acids or their anhydrides. The ortho-orientation improves solubility in solvents, making it possible to uniformly coat the resin. The uniformly coated protective layer reduces the variation in barrier performance, which ultimately contributes to the suppression of oligo whitening. In addition, the ortho-orientation results in a film with excellent flexibility and improved interfacial adhesion, which reduces damage to the resin caused by wet heat treatment and leads to the suppression of oligomers. Examples of aromatic polycarboxylic acids or their anhydrides in which carboxylic acids are substituted at the ortho positions include orthophthalic acid or its anhydride, naphthalene 2,3-dicarboxylic acid or its anhydride, naphthalene 1,2-dicarboxylic acid or its anhydride, anthraquinone 2,3-dicarboxylic acid or its anhydride, and 2,3-anthracene carboxylic acid or its anhydride. These compounds may have a substituent on any carbon atom of the aromatic ring. Examples of the substituent include a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimide group, a carboxyl group, a carbamoyl group, an N-ethylcarbamoyl group, a phenyl group, a naphthyl group, etc. Furthermore, polyester polyols having a content of 70 to 100 mol% relative to 100 mol% of the total polycarboxylic acid components are particularly preferred because they have a high effect of improving the barrier properties and excellent solvent solubility, which is essential for a coating material.

[0049] In the present invention, other polybasic carboxylic acid components may be copolymerized within the range that does not impair the effects of the present invention. Specifically, examples of aliphatic polycarboxylic acids include succinic acid, adipic acid, azelaic acid, sebacic acid, and dodecanedicarboxylic acid; examples of unsaturated bond-containing polycarboxylic acids include maleic anhydride, maleic acid, and fumaric acid; examples of alicyclic polycarboxylic acids include 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid; examples of aromatic polycarboxylic acids include terephthalic acid, isophthalic acid, pyromellitic acid, trimellitic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, naphthalic acid, biphenyldicarboxylic acid, diphenic acid and its anhydride, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, and anhydrides or ester-forming derivatives of these dicarboxylic acids; p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, and ester-forming derivatives of these dihydroxycarboxylic acids; and the like, which can be used alone or in a mixture of two or more kinds. Among these, succinic acid, 1,3-cyclopentanedicarboxylic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalic acid, and diphenic acid are preferred from the viewpoints of solubility in organic solvents and gas barrier properties.

[0050] [Polyhydric alcohol component] The polyhydric alcohol component of the polyester used in the present invention is not particularly limited as long as it can synthesize a polyester that exhibits gas barrier compensation performance, but it is preferable to contain a polyhydric alcohol component containing at least one selected from the group consisting of ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol, cyclohexanedimethanol, and 1,3-bishydroxyethylbenzene. Among them, it is most preferable to use ethylene glycol as the main component, since it is presumed that the smaller the number of carbon atoms between oxygen atoms, the less the molecular chain will be excessively flexible and the less oxygen will permeate.

[0051] In the present invention, it is preferable to use the above-mentioned polyhydric alcohol component, but other polyhydric alcohol components may be copolymerized within the range that does not impair the effects of the present invention. Specifically, the diols include 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, methylpentanediol, dimethylbutanediol, butylethylpropanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, and tripropylene glycol, and the trihydric or higher alcohols include glycerol, trimethylolpropane, trimethylolethane, tris(2-hydroxyethyl)isocyanurate, 1,2,4-butanetriol, pentaerythritol, and dipentaerythritol. In particular, polyesters using glycerol and tris(2-hydroxyethyl)isocyanurate in combination among trihydric alcohols are particularly preferably used because they have a moderately high crosslinking density due to their branched structure, have good solubility in organic solvents, and have excellent barrier function.

[0052] Examples of catalysts used in the reaction to obtain the polyester of the present invention include tin catalysts such as monobutyltin oxide and dibutyltin oxide, titanium catalysts such as tetra-isopropyl-titanate and tetra-butyl-titanate, and acid catalysts such as zirconia catalysts such as tetra-butyl-zirconate. It is preferable to use the above titanium catalysts such as tetra-isopropyl-titanate and tetra-butyl-titanate, which have high activity in esterification reactions, in combination with the above zirconia catalyst. The amount of the catalyst is 1 to 1000 ppm, more preferably 10 to 100 ppm, based on the total mass of the reaction raw materials used. If the amount is less than 1 ppm, it is difficult to obtain the effect of the catalyst, and if the amount is more than 1000 ppm, a problem of inhibiting the urethane reaction may occur when an isocyanate curing agent is used.

[0053] (4) Isocyanate-based hardener In the present invention, when a polyester resin is used as the main agent of the coating agent constituting the anchor coat layer, it is preferable to use an isocyanate-based curing agent to form a urethane resin. In this case, the coating layer becomes a crosslinked system, which has the advantage of improving heat resistance, abrasion resistance, and rigidity. Therefore, it is easy to use for boiling and retort packaging. On the other hand, there is a problem that the liquid cannot be reused after mixing with the curing agent, and a curing (aging) process is necessary after coating. As an advantage, as a simple overcoat varnish, for example, there is no risk of thickening of the coating liquid, and the coating production is easy to manage, the coating liquid can be diluted and reused, and in addition, a curing process (so-called aging process) is not required. In this case, the end of the polyester used can be polyol or polycarboxylic acid, or a mixture of these two, without any problems. On the other hand, since the resin of the coating layer is linear, there are cases where the heat resistance and abrasion resistance are insufficient, and problems occur that make it difficult to use for boiling and retort packaging.

[0054] When a curing agent is used in the coating layer, an isocyanate curing system is preferred from the viewpoint of the heat resistance of the film, since it is a coating on a film, and in this case the resin component of the coating material must be polyester polyol. On the other hand, when an epoxy compound is used as a curing agent, it must be polyester polycarboxylic acid. In these cases, the coating layer becomes a crosslinked system, which has the advantage of improving heat resistance, abrasion resistance, and rigidity. Therefore, it is easy to use for boiling and retort packaging. On the other hand, there are problems with this, such as the liquid not being reusable after mixing with the curing agent, and the need for a curing (aging) process after coating.

[0055] When the polyester has a hydroxyl group, the polyisocyanate compound used in the present invention reacts at least partially to form a urethane structure, which makes the resin component highly polar, and the polymer chains are aggregated to further strengthen the gas barrier function. In addition, when the resin of the coating material is a straight-chain resin, crosslinking with a trivalent or higher polyisocyanate can impart heat resistance and abrasion resistance. The polyisocyanate compound used in the present invention may be any of diisocyanates, trivalent or higher polyisocyanates, low molecular weight compounds, and high molecular weight compounds, but it is preferable to contain an aromatic ring or an aliphatic ring in a part of the skeleton from the viewpoint of improving the gas barrier function. For example, examples of isocyanates having an aromatic ring include toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and naphthalene diisocyanate; examples of isocyanates having an aliphatic ring include hydrogenated xylylene diisocyanate, hydrogenated toluene diisocyanate, isophorone diisocyanate, norbornine diisocyanate, or trimers of these isocyanate compounds; and compounds containing terminal isocyanate groups obtained by reacting an excess amount of these isocyanate compounds with low molecular weight active hydrogen compounds such as ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, ethylenediamine, monoethanolamine, diethanolamine, and triethanolamine, or high molecular weight active hydrogen compounds such as various polyester polyols, polyether polyols, and polyamides.

[0056] The coating method of the resin composition for the anchor coat layer is not particularly limited as long as it is a method for forming a layer by coating on the film surface. For example, a conventional coating method such as gravure coating, reverse roll coating, wire bar coating, die coating, etc. can be adopted.

[0057] When forming the anchor coat layer, it is preferable to apply the resin composition for the anchor coat layer and then heat and dry it. The drying temperature is preferably 90 to 180 ° C, more preferably 100 to 170 ° C, and even more preferably 110 to 160 ° C. If the drying temperature is less than 90 ° C, the anchor coat layer may not be sufficiently dried, or the film formation of the anchor coat layer may not proceed, resulting in a decrease in cohesive strength and water-resistant adhesion, and as a result, the barrier properties and hand-cutting properties may be decreased. On the other hand, if the drying temperature exceeds 180 ° C, the film may be too hot, making it brittle and reducing the puncture strength, or shrinking and causing poor processability. In particular, by drying at 100 ° C or higher, preferably 110 ° C or higher, the film formation of the anchor coat layer can proceed effectively and the water-resistant adhesion can be improved. In addition, in addition to drying, it is also more effective to apply additional heat treatment at a temperature as low as possible in order to promote the film formation of the anchor coat layer.

[0058] In addition, by applying an additional heat treatment in a low temperature range, the moisture content in the laminated film can be controlled to a predetermined amount. The preferred temperature conditions for the heat treatment are 25°C to 80°C, more preferably 30°C to 70°C, and even more preferably 35°C to 60°C. If the heat treatment temperature is 20°C or lower, the effect of the heat treatment is small, and it becomes difficult to control the moisture content. On the other hand, if the heat treatment temperature exceeds 80°C, the laminated film is overheated, which causes poor appearance such as wrinkles. Furthermore, the preferred time for the heat treatment varies depending on the adhesion amount and temperature of the anchor coat layer, but for example, when the treatment is performed at 40°C, it is preferably 24 hours or more, more preferably 48 hours or more, and even more preferably 72 hours or more.

[0059] In the laminated film of the present invention, the ratio (P1 / P2) of the peak intensity (P1) having an absorption maximum in the region of 1250±50 cm-1 to the peak intensity (P2) having an absorption maximum in the region of 1070±10 cm-1 in the total reflection infrared absorption spectrum of the anchor coat layer is preferably in the range of 1.0 to 10.0. It is preferably in the range of 1.2 to 9.0, more preferably in the range of 1.5 to 8.0. The peak at 1250±50 cm-1 is a peak derived from a COC structure derived from an aromatic or unsaturated aliphatic skeleton, and is an index showing the degree of crosslinking of the polyester or polyurethane skeleton. In addition, the peak at 1070±10 cm-1 is a peak derived from C-OH, and is an index showing the amount of hydroxyl groups derived from the polyester or polyurethane skeleton in the anchor coat layer. (P1 / P2) represents the ratio of hydroxyl groups in the polyester or polyurethane skeleton. By keeping this ratio within the above range, the film becomes highly polarized while controlling the moisture content to a specified amount, and the adhesion between the anchor coat layer and the inorganic thin film layer increases, resulting in maximum gas barrier performance and adhesion even after wet heat treatment. If (P1 / P2) is less than 1.0, the amount of hydroxyl groups in the anchor coat layer is large, and the bonding strength with the inorganic thin film layer is strong, but crosslinking in the anchor coat layer does not progress, film formation properties decrease and the film becomes brittle, or the moisture content increases due to the remaining polar groups in the anchor coat layer. On the other hand, if (P1 / P2) exceeds 10.0, the amount of hydroxyl groups in the anchor coat layer is small, and the film formation of the inorganic thin film layer becomes sparse, making it difficult to obtain gas barrier properties and adhesion. In order to set the value of (P1 / P2) of the anchor coat layer to the specified numerical range, it is necessary to use the above-mentioned materials to achieve the above-mentioned specified adhesion amount, and further to set the compounding ratio of the materials to the above-mentioned suitable range, and to combine with the above-mentioned drying and heat treatment conditions.

[0060] [Inorganic thin film layer] The laminate of the present invention has an inorganic thin film layer. The inorganic thin film layer is preferably a metal oxide layer. There is no particular limitation on the material forming the metal oxide layer as long as it can be made into a thin film, but from the viewpoint of gas barrier properties, inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), and a mixture of silicon oxide and aluminum oxide are preferred. In this composite oxide, the mixing ratio of silicon oxide and aluminum oxide is preferably in the range of 20 to 70 mass% Al in terms of the mass ratio of the metal content. If the Al concentration is less than 20 mass%, the water vapor barrier properties may be reduced. On the other hand, if it exceeds 70 mass%, the metal oxide layer tends to become hard, and the film may be destroyed after wet heat treatment, resulting in a decrease in gas barrier properties. In addition, when the Al concentration is 100 mass%, the water vapor barrier performance is good, but since it is a single material, the surface tends to be smooth, and the slipperiness is poor, making it easy for processing defects (wrinkles, acne, etc.) to occur. The silicon oxide referred to here is various silicon oxides such as SiO and SiO2, or mixtures thereof, and the aluminum oxide is various aluminum oxides such as AlO and Al2O3, or mixtures thereof.

[0061] The mixture ratio of silicon oxide and aluminum oxide in this mixture can be determined by a monitor that measures the composition using fluorescent X-rays. The object being measured is irradiated with X-rays, the intensity of the characteristic X-rays emitted from the atoms contained in the object is measured, and the value is converted into a composition and output. The conversion is performed by measuring an object of known film thickness and composition, and using a calibration curve created in relation to the obtained fluorescent X-rays. When the plastic substrate film contains the same atoms as those contained in the inorganic thin film layer, for example, when the inorganic thin film layer contains SiOx, and when the plastic film contains silica powder as a lubricant, and contains Si atoms in common, a film is prepared in which inorganic thin film layers of different known thicknesses are formed on plastic substrate films containing the same concentration of the atoms in advance, and the film is measured with the monitor.The thickness of the unknown inorganic thin film layer can be obtained by the calibration curve prepared by calculating the relationship between the obtained fluorescent X-ray intensity and the film thickness.

[0062] The inorganic thin film layer has a thickness of usually 1 to 100 nm, preferably 5 to 50 nm. If the inorganic thin film layer has a thickness of less than 1 nm, it may be difficult to obtain satisfactory gas barrier properties, while if the inorganic thin film layer has a thickness exceeding 100 nm, the corresponding improvement in gas barrier properties cannot be obtained, and it is rather disadvantageous in terms of flex resistance and production costs.

[0063] The method for forming the inorganic thin film layer is not particularly limited, and any known deposition method such as physical deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, or chemical deposition (CVD) may be appropriately adopted. A typical method for forming the inorganic thin film layer will be described below using a silicon oxide / aluminum oxide thin film as an example. For example, when the vacuum deposition method is adopted, a mixture of SiO2 and Al2O3, or a mixture of SiO2 and Al, is preferably used as the deposition raw material. Particles are usually used as these deposition raw materials, and in this case, it is desirable that the size of each particle is large enough that the pressure during deposition does not change, and the preferred particle diameter is 1 mm to 7 mm. Heating can be performed by resistance heating, high-frequency induction heating, electron beam heating, laser heating, or other methods. It is also possible to introduce oxygen, nitrogen, hydrogen, argon, carbon dioxide, water vapor, or other reactive gases as reaction gases, or to adopt reactive deposition using means such as ozone addition and ion assist. Furthermore, the film formation conditions can be changed arbitrarily, such as applying a bias to the deposition target (a laminate to be subjected to deposition), or heating or cooling the deposition target. The deposition material, reaction gas, bias of the deposition target, heating / cooling, etc. can be changed in the same manner when the sputtering method or the CVD method is adopted.

[0064] [Laminated film] The moisture content of the laminated film of the present invention is preferably 0.20% by mass or less. More preferably, it is 0.18% by mass or less, further preferably, it is 0.15% by mass or less, and particularly preferably, it is 0.12% by mass or less. The preferable lower limit is 0.01% by mass or more. If the moisture content is more than 0.20% by mass, there is a tendency that the inorganic thin film cracks due to the penetration of moisture during the wet heat treatment, and the gas barrier property and adhesion are deteriorated. The moisture content here is measured by a heat-drying moisture meter. The detailed measurement method is as described in the Examples, but in short, the moisture content is calculated by the formula (amount of moisture [g] coming out of the sample) / (weight of the sample [g]).

[0065] [Protective layer] In the present invention, when gas barrier performance is required or processing such as printing is required, a protective layer can be provided on the inorganic thin film layer. The inorganic thin film layer is not a completely dense film, but has minute missing parts scattered therein. By forming a protective layer by applying a specific resin composition for protective layer described later on the inorganic thin film layer, the resin in the resin composition for protective layer penetrates into the missing parts of the inorganic thin film layer, resulting in an effect of stabilizing the gas barrier property. In addition, by using a material having gas barrier property for the protective layer itself, the gas barrier property of the laminate is also greatly improved. However, it is necessary to note that the provision of the protective layer increases the number of processes, resulting in an increase in cost and a burden on the environment depending on the material used. It is also necessary to note that the physical properties such as surface roughness change depending on the protective layer.

[0066] [Laminate] The laminate of the present invention uses a heat-sealable resin called a sealant. The heat-sealable resin layer is usually provided on the anchor coat layer or inorganic thin film layer side, but may also be provided on the outside of the resin film layer (the surface opposite to the surface on which the inorganic thin film is formed). The heat-sealable resin layer is usually formed by extrusion lamination or dry lamination. The thermoplastic polymer forming the heat-sealable resin layer may be any polymer capable of sufficiently exhibiting sealant adhesion, and may be, for example, polyethylene resins such as olefin-based HDPE, LDPE, and LLDPE, polypropylene resins, ethylene-vinyl acetate copolymers, ethylene-α-olefin random copolymers, and ionomer resins. Among these, LLDPE or polypropylene resins, which are highly versatile in terms of durability, seal strength, cost, and mono-materialization, are particularly preferred. The thickness of the sealant layer is preferably 20 to 100 μm, more preferably 30 to 90 μm, and even more preferably 40 to 80 μm. If the thickness is less than 20 μm, sufficient seal strength may not be obtained, or the sealant may lack stiffness and be difficult to handle. On the other hand, if the thickness exceeds 100 μm, the bag will feel stiff and will be difficult to handle, and the price may also become high.

[0067] The total thickness of the laminate of the present invention is preferably 9 μm or more and 200 μm or less, more preferably 10 μm or more and 170 μm or less, further preferably 12 μm or more and 150 μm or less, and particularly preferably 15 μm or more and 120 μm or less.

[0068] The haze of the laminate of the present invention is preferably 5% or less, more preferably 0.2% or more and 5.0% or less, even more preferably 0.3% or more and 4.5% or less, and particularly preferably 0.4% or more and 4.0% or less. When the haze is within the above range, it may be easy to use in applications where transparency is required. For example, the haze tends to deteriorate when the stretching temperature or heat setting temperature is too high, the cooling roll temperature is high and the cooling rate of the unstretched (raw) sheet is slow, or there is too much low molecular weight component, and the haze can be adjusted to within the above range by adjusting these.

[0069] The laminate of the present invention has an oxygen permeability of 25 cc / m under conditions of 23°C x 65% RH. 2 / d / atm or less, more preferably 20cc / m 2 / d / atm or less, more preferably 15cc / m 2 The preferred lower limit of oxygen permeability is 0.1 cc / m 2 / d / atm or more. In addition, the water vapor transmission rate under the conditions of 40℃ × 90% RH is 3.0g / m 2 / d or less. More preferably, it is 2.5 g / m 2 / d or less, more preferably 2.0 g / m 2 The preferred lower limit of the water vapor permeability is 0.1 g / m 2 / d or more. Furthermore, the barrier value deterioration rate of the laminate of the present invention after wet heat treatment represented by formula (1) is preferably 150% or less, more preferably 140% or less, and further preferably 130% or less.

[0070] The laminate of the present invention preferably has a laminate strength of 2.0 N / 15 mm or more under 23° C.×65% RH conditions, more preferably 2.3 N / 15 mm or more, and even more preferably 2.6 N / 15 mm or more, in both dry and wet evaluations described below. If the laminate strength is less than 2.0 N / 15 mm, peeling may occur due to the load generated during wet heat treatment, resulting in deterioration of barrier properties and leakage of contents. Furthermore, hand tearability may also be deteriorated.

[0071] [Adhesive layer] The adhesive layer used in the present invention can be a general-purpose adhesive for lamination. For example, (non-)solvent, water-based, or hot melt adhesives can be used that are mainly composed of poly(ester)urethane, polyester, polyamide, epoxy, poly(meth)acrylic, polyethyleneimine, ethylene-(meth)acrylic acid, polyvinyl acetate, (modified) polyolefin, polybutadiene, wax, or casein. Among these, urethane or polyester adhesives are preferred in consideration of heat resistance and flexibility that can follow the dimensional changes of each resin. The adhesive layer can be applied by, for example, direct gravure coating, reverse gravure coating, kiss coating, die coating, roll coating, dip coating, knife coating, spray coating, fountain coating, or other methods, and the coating amount after drying is 1 to 8 g / m in order to develop sufficient adhesion. 2 More preferably, the thickness is 2 to 7 g / m 2 , and more preferably 3 to 6 g / m 2 The coating amount is 1g / m 2 If it is less than 8g / m, it becomes difficult to bond the entire surface, and the adhesive strength decreases. 2 If the temperature exceeds this range, it will take a long time for the film to completely cure, unreacted material will be likely to remain, and adhesive strength will decrease.

[0072] [Print layer] Furthermore, in the laminate of the present invention, at least one printed layer or other plastic resin and / or paper resin layer may be laminated between the resin film layer and the heat-sealable resin layer or on the outer side thereof.

[0073] As the printing ink for forming the printing layer, water-based and solvent-based resin-containing printing inks can be preferably used. Examples of the resin used in the printing ink include acrylic resins, urethane resins, polyester resins, vinyl chloride resins, vinyl acetate copolymer resins, and mixtures thereof. The printing ink may contain known additives such as antistatic agents, light blocking agents, ultraviolet absorbers, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, defoamers, crosslinking agents, anti-blocking agents, and antioxidants. The printing method for providing the printing layer is not particularly limited, and known printing methods such as offset printing, gravure printing, and screen printing can be used. To dry the solvent after printing, known drying methods such as hot air drying, hot roll drying, and infrared drying can be used.

[0074] According to the present invention, it is possible to obtain a laminated film which has excellent oxygen barrier properties and water vapor barrier properties after retort treatment, and also has high interlayer adhesion and excellent laminate strength. EXAMPLES

[0075] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples. The films were evaluated by the following measurement methods.

[0076] The evaluation methods used in the present invention are as follows. (1) Creating a laminate A 70 μm-thick non-oriented polypropylene film (P1146, manufactured by Toyobo Co., Ltd.) was laminated as a thermal adhesive resin by dry lamination using a urethane-based two-liquid curing adhesive (Mitsui Chemicals' "Takelac A525S" and "Takenate A50" mixed in a ratio of 13.5:1) on the inorganic thin film layer of the laminated film obtained in the Examples and Comparative Examples, and aged at 40° C. for 4 days to obtain laminates of Examples 1 to 4 and Comparative Examples 1 to 2. The thickness of the adhesive layer was about 4 μm after drying in all cases.

[0077] (2) Thickness (μm) The thickness of each layer was measured by cutting out a cross section of the laminate of the present invention solidified with the modified urethane resin using a microtome and observing it with a differential interference microscope.

[0078] (3) Anchor coat layer adhesion In each example and comparative example, each laminate obtained at the stage of laminating an anchor coat layer onto a resin film was used as a sample, and a test piece of 100 mm x 100 mm was cut out from this sample, and the anchor coat layer was wiped off with acetone. The amount of adhesion was calculated from the change in mass of the film before and after wiping.

[0079] (4) Composition and thickness of inorganic thin film layer In each example and comparative example, each laminate obtained at the stage of laminating the inorganic thin film layer was used as a sample, and the film thickness composition was measured using a fluorescent X-ray analyzer ("ZSX100e" manufactured by Rigaku Corporation) based on a calibration curve prepared in advance. The excitation X-ray tube conditions were 50 kV and 70 mA.

[0080] (5) Moisture content The moisture content of the laminates obtained in each of the Examples and Comparative Examples was measured using a heat-drying moisture content meter ("MS-70" manufactured by A&D Co., Ltd.).

[0081] About 5g of the laminated film obtained in each Example and Comparative Example was stored for 72 hours or more under an environment of 25±2°C and 65±10% RH relative humidity, then cut into a 50×50 mm square, set on a measuring dish, and weighed. The sample weight [g] at this time was taken as (Wa). After that, the sample was heated to 140°C, and the weight of the sample was measured when the weight change was 0.02% / sec or less. The sample weight [g] at this time was taken as (Wb). The moisture content was calculated from the weight obtained at this time using the following formula (1). (Water content [%])=(Wa-Wb) / (Wa)×100...Equation (1) Each sample was measured three times, and the average value was used as the moisture content.

[0082] (6) Laminate strength The laminate prepared in (1) above was cut into a test piece with a width of 15 mm and a length of 200 mm, and the laminate strength was measured using a Tensilon universal material testing machine (Tensilon UMT-II-500, manufactured by Toyo Baldwin Co., Ltd.) under conditions of a temperature of 23° C. and a relative humidity of 65%. The laminate strength was measured at a tensile speed of 200 mm / min, the laminate layer and the heat-sealable resin layer of each laminate obtained in the examples and comparative examples were peeled off at a peel angle of 90 degrees, and the strength was measured when water was dripped onto the peeled part with a dropper (wet) and when water was not dripped (dry). On the other hand, the laminate produced above was subjected to retort treatment by holding it in pressurized hot water at a temperature of 130°C for 30 minutes, and immediately thereafter, a test piece was cut out from the resulting laminate after retort treatment in the same manner as described above, and the laminate strength (after retort treatment) was measured in the same manner as described above.

[0083] (7) Oxygen permeability The oxygen permeability of the laminate produced in (1) above was measured in accordance with JIS-K7126 Method B using an oxygen permeability measuring device ("OX-TRAN (registered trademark) 1 / 50" manufactured by MOCON) under an atmosphere at a temperature of 23°C and a humidity of 65% RH. The oxygen permeability was measured in the direction in which oxygen permeates from the surface layer (C) side. On the other hand, the evaluation laminate was subjected to retort treatment by holding it in pressurized hot water at a temperature of 130°C for 30 minutes, and then dried at 40°C for 24 hours. The oxygen permeability (after retort treatment) of the resulting laminate after retort treatment was measured in the same manner as described above.

[0084] (8) Water vapor permeability The water vapor permeability of the laminate produced in (1) above was measured in accordance with JIS-K7129 Method B using a water vapor permeability measuring device ("PERMATRAN-W 3 / 33MG" manufactured by MOCON) under an atmosphere of a temperature of 40°C and a humidity of 90% RH. The water vapor permeability was measured in the direction in which water vapor permeates from the surface layer (C) side. On the other hand, the evaluation laminate was subjected to retort treatment by holding it in pressurized hot water at a temperature of 130°C for 30 minutes, and then dried at 40°C for 24 hours. The water vapor permeability (after retort treatment) of the resulting laminate after retort treatment was measured in the same manner as described above.

[0085] (9) Laminate strength deterioration rate The value calculated by the following formula (2) relative to the value measured in the above (6) was defined as the deterioration rate of laminate strength. Laminate strength deterioration rate (%) = (laminate strength before retort treatment - laminate strength after retort treatment) / (laminate strength before retort treatment) × 100 Formula (2)

[0086] (10) Barrier value deterioration rate 7. The laminated film according to claim 5 or 6, wherein, with respect to the values ​​measured in (7) and (8), a barrier value deterioration rate after moist heat treatment, represented by the following formula (3), is 150% or less, where (A) is an oxygen permeability value measured under conditions of 23°C × 65% RH and (B) is an oxygen permeability value measured under conditions of 23°C × 65% RH after performing a retort treatment in which the film is kept in compressed hot water at a temperature of 130°C for 30 minutes. Barrier value deterioration rate after heat and moisture treatment (%) = (B / A) × 100 Equation (3)

[0087] (11) Total reflection infrared absorption spectrum of anchor coat layer In each example and comparative example, the total reflection infrared absorption spectrum was measured by total reflection absorption infrared spectroscopy using an infrared spectrometer (BRUKER's "ALPHA") for the surface of the anchor coat layer of each laminate film obtained at the stage of laminating the anchor coat layer on the base film, and the peak intensity (P1) having the absorption maximum in the region of 1250±50 cm-1 and the peak intensity (P2) having the absorption maximum in the region of 1070±10 cm-1 were obtained, and the intensity ratio (P1 / P2) was calculated. The calculation of each peak intensity was performed from the peak height vertically connecting the baseline of zero absorbance and each peak top.

[0088] [Preparation of base film layer] Tables 1 to 3 show the details of the resin raw materials used in the preparation of the substrate film, the film forming conditions, and the raw material blending ratios.

[0089] [Table 1]

[0090] [Table 2]

[0091] [Table 3]

[0092] (OPP-1) The base layer (A) was made of 100.0 wt% polypropylene homopolymer PP-2 shown in Table 1. The surface layer (B) was made of a mixture of 43.2 wt% polypropylene homopolymer PP-2 shown in Table 1, 52.0 wt% ethylene copolymerized polypropylene polymer PP-4 shown in Table 1, and 4.8 wt% antiblocking agent-containing master batch FTX0627G. The melt flow rate (g / 10 min) of the polypropylene resin composition constituting the surface layer (B) was 5.1. For the surface layer (C), a mixture of 93.6% by weight of polypropylene homopolymer PP-2 and 6.4% by weight of antiblocking agent-containing master batch FTX0627G shown in Table 1 was used. The base layer (A) was made using a 45 mm extruder, the surface layer (B) was made using a 25 mm extruder, and the surface layer (C) was made using a 20 mm extruder. The raw material resins were melted at 250 ° C. and co-extruded from a T-die into a sheet shape, and the surface layer (B) was cooled and solidified so that it contacted a cooling roll at 30 ° C., and then stretched 4.5 times in the machine direction (MD) at 125 ° C. Then, in a tenter, both ends of the film in the width direction (TD) were clamped with clips, preheated at 168 ° C., stretched 8.2 times in the width direction (TD) at 155 ° C., and heat-set at 165 ° C. while relaxing 6.7% in the width direction (TD). The film formation conditions at this time were film formation conditions a. In this way, a biaxially oriented polypropylene film having a structure of surface layer (B) / base layer (A) / surface layer (C) was obtained. The surface of the surface layer (B) of the biaxially oriented polypropylene film was corona-treated using a corona treatment machine manufactured by Softal Corona & Plasma GmbH at an applied current value of 0.75 A, and then wound up with a winder. The thickness of the obtained film was 20 μm (thickness of surface layer (B) / base layer (A) / surface layer (C) was 1.3 μm / 17.7 μm / 1.0 μm).

[0093] (OPP-2) For the base layer (A), a polypropylene homopolymer PP-1 shown in Table 1 was used. The surface layer (B) was made of a blend of 43.2% by weight of polypropylene homopolymer PP-2 shown in Table 1, 52.0% by weight of ethylene copolymerized polypropylene polymer PP-4 shown in Table 1, and 4.8% by weight of antiblocking agent-containing master batch FTX0627G. The surface layer (C) was made of a blend of 93.6% by weight of polypropylene homopolymer PP-1 shown in Table 1, and 6.4% by weight of antiblocking agent-containing master batch FTX0627G. The base layer (A) was made using a 45 mm extruder, the surface layer (B) was made using a 25 mm extruder, and the surface layer (C) was made using a 20 mm extruder. The raw material resins were melted at 250 ° C. and co-extruded from a T-die into a sheet shape, and the surface layer (B) was cooled and solidified so that it contacted a cooling roll at 30 ° C., and then stretched 4.5 times in the machine direction (MD) at 135 ° C. Then, in a tenter, both ends of the film in the width direction (TD) were clamped with clips, preheated at 173 ° C., stretched 8.2 times in the width direction (TD) at 164 ° C., and heat-set at 171 ° C. while relaxing 6.7% in the width direction (TD). The film formation conditions at this time were film formation conditions b. In this way, a biaxially oriented polypropylene film having a structure of surface layer (B) / base layer (A) / surface layer (C) was obtained. The surface of the surface layer (B) of the biaxially oriented polypropylene film was corona-treated using a corona treatment machine manufactured by Softal Corona & Plasma GmbH at an applied current value of 0.75 A, and then wound up with a winder. The thickness of the obtained film was 20 μm (thickness of surface layer (B) / base layer (A) / surface layer (C) was 1.3 μm / 17.7 μm / 1.0 μm).

[0094] (PET) The ester film E5100 manufactured by Toyobo Co., Ltd., having a thickness of 12 μm, was used.

[0095] [Creation of anchor coat layer] The method for producing the anchor coat layer used in each of the Examples and Comparative Examples will be described below.

[0096] [Coating Fluid 1] Silane coupling agent; N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM-603") 0.25 parts by mass was dissolved in 1.48 parts by mass of acetone, and 4.07 parts by mass of isocyanate; trimethylolpropane adduct of meta-xylylene diisocyanate (manufactured by Mitsui Chemicals, Inc., "Takenate D-110N": solid content 75%) was mixed and stirred for 10 minutes using a magnetic stirrer. The obtained mixed solution was diluted with 69.55 parts by mass of methyl ethyl ketone and 14.03 parts by mass of 1-methoxy-2-propanol (hereinafter referred to as PGM), and 10.62 parts by mass of polyester resin (manufactured by DIC Corporation, DF-COAT GEC-004C: solid content 30%) was added to obtain the target coating solution 1.

[0097] [Coating fluid 2] To a mixture of 42.83 parts by mass of purified water and 20.00 parts by mass of isopropanol, 6.67 parts by mass of a commercially available metaxylylene group-containing urethane resin dispersion (Mitsui Chemicals' "Takelac (registered trademark) WPB341"; solid content 30%) and 28.00 parts by mass of a commercially available polyester urethane resin dispersion (DIC's "Hydran (registered trademark) AP-80"; solid content 25%) were added, and the mixture was stirred for 10 minutes using a magnetic stirrer. To the obtained mixture, 2.50 parts by mass of a carbodiimide-based crosslinking agent (Nisshinbo Chemical's "Carbodilite SV-02"; solid content 40%) was further added to obtain the desired coating liquid 2.

[0098] [Coating fluid 3] To 90 parts by mass of purified water, 10 parts by mass of fully saponified polyvinyl alcohol resin (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: G Polymer OKS8049Q, (saponification degree 99.0% or more, average polymerization degree 450) was added, and the mixture was heated to 80°C with stirring, and then stirred for about 1 hour. The mixture was then cooled to room temperature, thereby obtaining a nearly transparent polyvinyl alcohol solution (PVA solution) with a solids content of 10%. 50.00 parts by mass of the above PVA solution was mixed with a mixed solution of 35.00 parts by mass of purified water and 15.00 parts by mass of 2-propanol, to obtain the target coating solution 2.

[0099] [Formation of inorganic thin film layer] The method for producing the inorganic thin film layer used in each of the Examples and Comparative Examples will be described below. A composite oxide layer of silicon dioxide and aluminum oxide was formed on the anchor coat layer by electron beam deposition. Particulate SiO2 (99.9% purity) and Al2O3 (99.9% purity) of about 3 mm to 5 mm were used as deposition sources. The inorganic thin film layer (SiO2 / A12O3 composite oxide layer) in the film thus obtained (film containing inorganic thin film layer / anchor coat layer) had a thickness of 13 nm. The composition of this composite oxide layer was A12O3 / SiO2 (mass ratio) = 30 / 70.

[0100] Example 1 OPP-1 was used for the base film, and Coating Solution 1 was used for the anchor coat layer. The surface layer (B) of the resin film was coated by gravure roll coating, and dried at 130° C. for 10 seconds. The adhesion amount of the anchor coat layer at this time was 0.40 g / m 2 Thereafter, a post-heat treatment was carried out at 40° C. for 2 days, and then an inorganic thin film layer was laminated thereon by the above-mentioned method to obtain the intended laminate film. Example 2 The target laminated film was obtained under the same conditions as in Example 1, except that the resin film was changed to OPP-2. Example 3 Anchor coat layer adhesion weight 0.20g / m 2 The target laminated film was obtained under the same conditions as in Example 1, except for changing the above. Example 4 The target laminated film was obtained under the same conditions as in Example 1, except that the composition of the inorganic thin film layer was changed to A12O3 / SiO2 (mass ratio) = 40 / 60. Example 5 The target laminated film was obtained under the same conditions as in Example 1, except that Coating Liquid 2 was used for the anchor coat layer. Comparative Example 1 The target laminated film was obtained under the same conditions as in Example 1, except that Coating Liquid 3 was used for the anchor coat layer. Comparative Example 2 The target laminated film was obtained under the same conditions as in Example 1, except that the base film was changed to PET.

[0101] A laminate film was produced in the manner described above. Furthermore, a laminate was produced from the obtained laminate film as described in (1) above, and the composition and the results of various evaluations were carried out for the laminate film and the laminate. The results are shown in Table 4.

[0102] [Table 4A]

[0103] [Table 4B] [Industrial Applicability]

[0104] According to the present invention, it is possible to provide a laminated film that has excellent oxygen and water vapor barrier properties even after retort treatment and has adhesion that does not cause interlayer delamination after retort treatment.

Claims

1. A laminated film in which an anchor coat layer and an inorganic thin film layer are laminated in this order on the surface layer (B) of a substrate film in which a surface layer (C), a substrate layer (A), and a surface layer (B) are laminated in this order, each layer containing 50% by mass of polyolefin, and the surface layer (B) is made of a resin composition containing two or more polyolefin resins having different crystallinity, and the anchor coat layer has a total reflection infrared absorption spectrum of 1250±50 cm. -1 The peak intensity (P1) with an absorption maximum in the region of 1070 ± 10 cm -1 The ratio (P1 / P2) of the peak intensity (P2) having an absorption maximum in the region is in the range of 1.0 to 10.0, and the coating amount is 0.50 g / m 2 a moisture content of the laminate film being less than 0.2 mass % and the moisture content of the laminate film being 0.2 mass % or less, and an olefin-based sealant layer being laminated on the surface opposite to the surface layer (C), wherein when an oxygen permeability value of the laminate measured under conditions of 23°C x 65% RH is (A) and an oxygen permeability value of the laminate measured under conditions of 23°C x 65% RH after performing a retort treatment in which the laminate is held in compressed hot water at a temperature of 130°C for 30 minutes is (B), the barrier value deterioration rate after moist heat treatment, which is represented by the following formula, is 150% or less: Barrier value deterioration rate (%) after moist heat treatment=(B / A)×100 Formula (1).

2. The laminate according to claim 1 , wherein the inorganic thin film layer is made of a metal oxide.

3. 3. The laminate according to claim 1, wherein the laminate has a lamination strength of 2.0 N / 15 mm or more.

4. A packaging material comprising at least one layer of the laminate according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Transparent gas barrier film

    JP1994023901A

  • Gas barrier laminate and packaging bag

    WO2021176948A1

  • Vapor deposited polyester film

    JP1990050837A

  • Laminated film

    JP2005349769A

  • Barrier coating composition for lamination, and barrier composite film for lamination

    JP2008297527A