Resin film for terminal and power storage device using the same
A three-layer resin film with specific polypropylene and adhesive layers maintains adhesion to both exterior and metal terminals, addressing adhesion loss in high-temperature environments and preventing foaming, ensuring reliable power storage device operation.
Patent Information
- Application Number
- JP2024117794
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The adhesion between the exterior material and the tab sealant in battery packs decreases in high-temperature environments due to electrolyte foaming, leading to potential insulation issues.
A resin film for terminals with a three-layer structure, comprising a first adhesive layer made of polypropylene with a long chain branched structure and a melting point of 80 to 155°C, a second adhesive layer, and an insulating layer, which maintains adhesion to both the exterior material and metal terminal even at high temperatures.
The resin film ensures excellent adhesion to both the exterior material and metal terminal at room temperature and maintains sufficient adhesion even in high-temperature environments, preventing foaming and curling, thus enhancing the reliability of power storage devices.
Smart Images

Figure 2024133377000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film for a terminal and an electricity storage device using the same. [Background technology]
[0002] In recent years, there has been an increasing demand for miniaturizing portable devices and making effective use of naturally generated energy, and research and development is being conducted on lithium-ion secondary batteries (a type of energy storage device) that can produce higher voltages and have higher energy density.
[0003] Conventionally, metal cans have been widely used as packaging materials for the lithium-ion secondary batteries. However, in response to demands for thinner and more diverse products to which the batteries are applied, packaging materials in the form of a bag made of a laminate of a metal layer (e.g., aluminum foil) and a resin film have come to be widely used because of their low manufacturing costs.
[0004] A laminated lithium ion secondary battery in which a battery body is housed and sealed inside the packaging material is provided with a current extraction terminal called a tab. The tab is connected to the negative or positive electrode of the battery body and has a metal terminal (sometimes called a "tab lead") that extends outside the packaging material (exterior material), and a terminal resin film (sometimes called a "tab sealant") that covers a part of the outer circumferential surface of the metal terminal (see, for example, Patent Documents 1 to 3). Usually, the terminal resin film is fused to the metal terminal. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2008-4316 A [Patent Document 2] JP 2010-218766 A [Patent Document 3] JP 2009-259739 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, battery packs are increasingly exposed to high-temperature environments due to rising chemical conversion temperatures in battery manufacturing, thermal runaway caused by rapid charging, etc. When a battery pack is exposed to a high-temperature environment, there is a problem that the adhesion between the exterior material and the tab sealant decreases.
[0007] The present disclosure aims to provide a resin film for terminals that has excellent adhesion to exterior materials and metal terminals in a room temperature environment and can sufficiently maintain adhesion to exterior materials even when exposed to a high-temperature environment, and an electricity storage device using the same. [Means for solving the problem]
[0008] In order to achieve the above object, the present disclosure provides a resin film for a terminal having three or more layers arranged so as to cover the outer peripheral surface of a portion of a metal terminal electrically connected to an electricity storage device main body that constitutes an electricity storage device, the resin film for a terminal comprising a first adhesive layer arranged on one surface, a second adhesive layer arranged on a surface opposite to the first adhesive layer, and an insulating layer arranged between the first adhesive layer and the second adhesive layer, wherein the first adhesive layer is a layer containing polypropylene having a structure with long chain branches and polypropylene having a melting point of 80 to 155°C and not having a structure with long chain branches.
[0009] As a result of intensive research by the present inventors, it was found that the reason why the adhesion between the exterior material and the tab sealant decreases when exposed to a high-temperature environment is that the electrolyte foams in the high-temperature environment, causing gaps between the exterior material and the tab sealant. It was also found that the foaming of the electrolyte occurs frequently, especially in the tab sealant on the exterior material side. As a result of further research by the present inventors, it was found that it is possible to suppress foaming originating from the tab sealant by disposing a layer containing a polypropylene having a long-chain branched structure and a polypropylene having a melting point of 80 to 155°C and not having a long-chain branched structure so as to be in contact with the exterior material.
[0010] In the resin film for terminal, the content of the polypropylene having a structure with long chain branches may be 1 to 50% by mass based on the total amount of the first adhesive layer. When the content of the polypropylene having a structure with long chain branches is 1 to 50% by mass based on the total amount of the first adhesive layer, the adhesion between the resin film for terminal and the exterior material is more excellent, and curling of the resin film for terminal can be more effectively suppressed.
[0011] In the resin film for terminal, the polypropylene having a structure with long chain branches may be polypropylene synthesized using a metallocene catalyst. When the polypropylene having a structure with long chain branches is polypropylene synthesized using a metallocene catalyst, the adhesion between the resin film for terminal and the exterior material is more excellent, and the adhesion between the resin film for terminal and the exterior material can be better maintained even when exposed to a high-temperature environment.
[0012] In the resin film for terminal, the ratio of the thickness of the second adhesive layer to the thickness of the first adhesive layer (second adhesive layer / first adhesive layer) may be 0.2 to 4.5. When the ratio of the thickness of the second adhesive layer to the thickness of the first adhesive layer is 0.2 to 4.5, curling of the resin film for terminal can be further suppressed.
[0013] In the resin film for a terminal, the absolute difference between the melting point of the first adhesive layer and the melting point of the second adhesive layer may be 0 to 15° C. When the absolute difference between the melting point of the first adhesive layer and the melting point of the second adhesive layer is 0 to 15° C., curling of the resin film for a terminal can be further suppressed.
[0014] In the resin film for a terminal, the first adhesive layer and / or the insulating layer may contain a filler. When the first adhesive layer and / or the insulating layer contains a filler, the adhesion between the resin film for a terminal and the exterior material can be further maintained even when exposed to a high-temperature environment.
[0015] In the resin film for terminal, the second adhesive layer may contain a resin having a polar group. When the second adhesive layer contains a resin having a polar group, the adhesion between the resin film for terminal and the metal terminal is more excellent.
[0016] The present disclosure can also provide an electricity storage device comprising: an electricity storage device main body, a metal terminal electrically connected to the electricity storage device main body, an exterior material that sandwiches the metal terminal and houses the electricity storage device main body, and a terminal resin film of the present disclosure that covers a part of the outer circumferential surface of the metal terminal and is disposed between the metal terminal and the exterior material, the first adhesive layer being in contact with the exterior material and the second adhesive layer being in contact with the metal terminal. Such an electricity storage device has excellent adhesion between the exterior material and the metal terminal in a room temperature environment, and can sufficiently maintain adhesion between the terminal resin film and the exterior material even when exposed to a high temperature environment. Effect of the Invention
[0017] According to the present disclosure, it is possible to provide a resin film for terminals that has excellent adhesion to exterior materials and metal terminals in a room temperature environment and can sufficiently maintain adhesion to exterior materials even when exposed to a high-temperature environment, and an electricity storage device using the same. [Brief description of the drawings]
[0018] [Figure 1] 1 is a perspective view showing a schematic configuration of an electricity storage device according to an embodiment of the present disclosure. [Diagram 2] 2 is a cross-sectional view showing an example of a cut surface of the exterior packaging material shown in FIG. 1. [Diagram 3] 2 is a cross-sectional view of the resin film for terminal and the metal terminal shown in FIG. 1 taken along the line AA. [Figure 4] FIG. 2 is a schematic diagram illustrating a method for preparing a sample for measuring heat seal strength in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0020] Fig. 1 is a perspective view showing a schematic configuration of an electricity storage device according to an embodiment of the present disclosure. In Fig. 1, a lithium ion secondary battery is illustrated as an example of an electricity storage device 10, and the following description will be given. Note that the lithium ion secondary battery configured as shown in Fig. 1 may be called a battery pack or a battery cell.
[0021] An electricity storage device 10 shown in FIG. 1 is a lithium ion secondary battery, and includes an electricity storage device body 11, an exterior material 13, a pair of metal terminals 14 (tab leads), and a terminal resin film 16 (tab sealant).
[0022] The power storage device body 11 is a battery body that performs charging and discharging. The exterior material 13 covers the surface of the power storage device body 11 and is disposed so as to be in contact with a part of the resin film 16 for terminals.
[0023] Fig. 2 is a cross-sectional view showing an example of a cut surface of the exterior material shown in Fig. 1. In Fig. 2, the same components as those in the structure shown in Fig. 1 are denoted by the same reference numerals.
[0024] Here, an example of the configuration of the exterior material 13 will be described with reference to Fig. 2. The exterior material 13 has a seven-layer structure in which, from the inside in contact with the electricity storage device body 11, an inner layer 21, an inner layer-side adhesive layer 22, a corrosion prevention treatment layer 23-1, a barrier layer 24 which is a metal layer, a corrosion prevention treatment layer 23-2, an outer layer-side adhesive layer 25, and an outer layer 26 are laminated in this order.
[0025] The inner layer 21 is a sealant layer that imparts heat sealing to the exterior material 13, and is a layer that is disposed on the inside and heat sealed (thermally fused) when assembling the electricity storage device 10. For example, a polyolefin resin or an acid-modified polyolefin resin obtained by graft-modifying a polyolefin resin with maleic anhydride or the like can be used as the base material of the inner layer (sealant layer) 21. For example, low-density, medium-density, and high-density polyethylene; ethylene-α-olefin copolymer; homo-, block-, or random polypropylene; propylene-α-olefin copolymer, and the like can be used as the polyolefin resin. Among these, it is preferable that the polyolefin resin contains polypropylene. These polyolefin resins may be used alone or in combination of two or more kinds.
[0026] The inner layer 21 may be formed using a single layer film or a multilayer film in which multiple layers are laminated, depending on the required function. Specifically, for example, a multilayer film in which a resin such as an ethylene-cyclic olefin copolymer or polymethylpentene is interposed may be used to impart moisture resistance. Furthermore, the inner layer 21 may contain, for example, various additives (for example, a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, etc.).
[0027] The thickness of the inner layer 21 is preferably set within a range of, for example, 10 to 150 μm, and more preferably 30 to 80 μm. If the thickness of the inner layer 21 is thinner than 10 μm, there is a risk of reduced heat seal adhesion between the exterior materials 13 and adhesion to the terminal resin film 16. Moreover, if the thickness of the inner layer 21 is thicker than 150 μm, this is not preferable because it will cause an increase in the cost of the exterior material 13.
[0028] As the inner adhesive layer 22, for example, a known adhesive such as a general dry lamination adhesive or an acid-modified heat-fusible resin can be appropriately selected and used.
[0029] As shown in Figure 2, it is preferable from the viewpoint of performance that the corrosion prevention treatment layers 23-1, 23-2 are formed on both sides of the barrier layer 24. However, taking cost into consideration, the corrosion prevention treatment layer 23-1 may be disposed only on the side of the barrier layer 24 located on the inner layer side adhesive layer 22 side.
[0030] The barrier layer 24 is, for example, a metal layer having electrical conductivity. Examples of the material of the barrier layer 24 include aluminum and stainless steel, and aluminum is preferable from the viewpoints of cost, mass (density), and the like.
[0031] For the outer adhesive layer 25, for example, a general polyurethane adhesive containing polyester polyol, polyether polyol, acrylic polyol or the like as a main component can be used.
[0032] The outer layer 26 may be, for example, a single layer film of nylon, polyethylene terephthalate (PET), or the like, or a multilayer film. The outer layer 26 may contain, for example, various additives (for example, a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, etc.) similarly to the inner layer 21. The outer layer 26 may also have a protective layer formed, for example, by laminating a resin insoluble in the electrolyte or coating a resin component insoluble in the electrolyte as a countermeasure against leakage.
[0033] Fig. 3 is a cross-sectional view taken along line AA of the resin film for terminal and the metal terminal shown in Fig. 1. In Fig. 3, the same components as those in the structure shown in Fig. 1 are denoted by the same reference numerals.
[0034] 1 and 3, a pair of metal terminals 14 (two in the case of FIG. 1) has a metal terminal body 14-1 and a corrosion prevention layer 14-2. Of the pair of metal terminal bodies 14-1, one metal terminal body 14-1 is electrically connected to the positive electrode of the electricity storage device body 11, and the other metal terminal body 14-1 is electrically connected to the negative electrode of the electricity storage device body 11. The pair of metal terminal bodies 14-1 extend in a direction away from the electricity storage device body 11, and a part of each of them is exposed from the exterior material 13. The shape of the pair of metal terminal bodies 14-1 may be, for example, a flat plate shape.
[0035] The material of the metal terminal body 14-1 may be a metal. The metal to be used for the metal terminal body 14-1 is preferably determined in consideration of the structure of the electricity storage device body 11, the materials of each component of the electricity storage device body 11, and the like.
[0036] For example, when the electricity storage device 10 is a lithium ion secondary battery, aluminum is used as the positive electrode current collector, and copper is used as the negative electrode current collector. In this case, it is preferable to use aluminum as the material of the metal terminal body 14-1 connected to the positive electrode of the electricity storage device body 11. In addition, in consideration of corrosion resistance to the electrolyte, it is preferable to use an aluminum material with a purity of 97% or more, such as 1N30, as the material of the metal terminal body 14-1 connected to the positive electrode of the electricity storage device body 11. Furthermore, when the metal terminal body 14-1 is bent, it is preferable to use an O material that has been tempered by sufficient annealing in order to add flexibility. It is preferable to use copper with a nickel plating layer formed on the surface, or nickel, as the material of the metal terminal body 14-1 connected to the negative electrode of the electricity storage device body 11.
[0037] The thickness of the metal terminal body 14-1 depends on the size and capacity of the lithium ion secondary battery. In the case of a small lithium ion secondary battery, the thickness of the metal terminal body 14-1 may be, for example, 50 μm or more. In the case of a large lithium ion secondary battery for power storage or vehicle use, the thickness of the metal terminal body 14-1 may be appropriately set within the range of, for example, 100 to 500 μm.
[0038] The corrosion prevention layer 14-2 is disposed so as to cover the surface of the metal terminal body 14-1. In the case of a lithium ion secondary battery, the electrolyte contains a corrosive component such as LiPF6. The corrosion prevention layer 14-2 is a layer for suppressing corrosion of the metal terminal body 14-1 caused by the corrosive component such as LiPF6 contained in the electrolyte.
[0039] 3, the resin film for terminal 16 is disposed so as to cover a portion of the outer peripheral surface of the metal terminal 14. In this embodiment, the resin film for terminal 16 is configured by laminating a second adhesive layer (hereinafter also referred to as the innermost layer) 31 in contact with the outer peripheral side surface of the metal terminal 14, a first adhesive layer (hereinafter also referred to as the outermost layer) 32 in contact with the exterior material 13, and an insulating layer (hereinafter also referred to as the intermediate layer) 33 disposed between the innermost layer 31 and the outermost layer 32. Note that the resin film for terminal 16 may include layers other than the innermost layer, the outermost layer, and the intermediate layer.
[0040] The innermost layer 31 is disposed so as to cover the outer peripheral surface of the metal terminal 14, thereby sealing the metal terminal 14 in the circumferential direction and bonding the terminal resin film 16 to the metal terminal 14. The outermost layer 32 is fused to the exterior material 13, thereby sealing the inside of the exterior material 13.
[0041] [Innermost layer] In this embodiment, the innermost layer 31 is a layer that is fused to the metal terminal. From the viewpoint of more excellent adhesion to the metal terminal, the innermost layer 31 preferably contains a resin having a polar group (hereinafter also referred to as a "polar resin"). Examples of the polar group include a hydroxyl group, a glycidyl group, an amide group, an imino group, an oxazoline group, an acid anhydride group, a carboxyl group, and an ester group. From the viewpoint of reactivity, the polar group is preferably an acid anhydride group (particularly a group derived from maleic anhydride). Examples of the polar resin include modified polyolefins having a polar group, polyhydroxypolyolefin oligomers, ethylene / acrylic acid / glycidyl methacrylate copolymers, and the like. From the viewpoint of reactivity, the polar resin is preferably a polyolefin modified with an acid anhydride such as maleic anhydride. Examples of the polyolefin include polypropylene, polyethylene, and polybutene.
[0042] As the polypropylene, homopolypropylene, random polypropylene, block polypropylene, low regular polypropylene, etc. can be used. Among these, random polypropylene and low regular polypropylene are preferred from the viewpoints of adhesion to metal terminals, ease of opening in a high temperature environment, and impact resistance. The modified polypropylene is a polypropylene having the polar group listed above, and is preferably an acid-modified polypropylene, and more preferably an acid-modified random polypropylene.
[0043] Specific examples of polar resin products include polar resins having hydroxyl groups such as "Poval" manufactured by Kuraray Co., Ltd. and "Mersen H" manufactured by Tosoh Corporation, polar resins having glycidyl groups such as "Modiper" manufactured by NOF Corporation, "LOTADER" and "BONDINE" manufactured by Arkema Co., Ltd., polar resins having amide groups such as "APOLHYA" manufactured by Arkema Co., Ltd., "Admer IP" manufactured by Mitsui Chemicals, Inc., polar resins having oxazoline groups such as "Epocross" manufactured by Nippon Shokubai Co., Ltd. The modified resins can be used alone or in combination of two or more types.
[0044] The melting point of the polar resin is preferably from 80 to 160°C, more preferably from 100 to 150°C, and even more preferably from 110 to 145°C, from the viewpoints of embeddability and heat resistance.
[0045] In this specification, the melting point of a resin can be measured with a differential scanning calorimeter (DSC) and determined by reading the peak top temperature, which is the main peak having the largest heat of dissolution.
[0046] In the innermost layer 31, the content of the polar resin is preferably 40% by mass or more based on the total amount of the innermost layer 31, from the viewpoint of better adhesion to the metal terminal. The upper limit of the content of the polar resin is not particularly limited, but may be 99% by mass or less, or may be 95% by mass or less.
[0047] The innermost layer 31 may contain a resin other than a polar resin. Examples of the resin other than a polar resin include polyolefins such as polypropylene, polyethylene, and polybutene.
[0048] In the innermost layer 31, the content of the resin other than the polar resin may be 1 to 20 mass % based on the total amount of the innermost layer 31. When the content of the resin other than the polar resin is 1 mass % or more, adhesion to the metal terminal tends to be better. When the content of the resin other than the polar resin is 20 mass % or less, a decrease in cohesive force is suppressed, and sufficient adhesion to the metal terminal can be maintained.
[0049] The innermost layer 31 may contain additives other than the above components. Examples of additives include antioxidants, slip agents, flame retardants, light stabilizers, dehydrating agents, coloring pigments, and tackifiers. These may be used alone or in combination of two or more. Examples of coloring pigments include carbon black, quinacridone pigments, polyazo pigments, and isoindolinone pigments.
[0050] The thickness of the innermost layer 31 is preferably 10 to 100 μm, and more preferably 15 to 50 μm. When the thickness of the innermost layer 31 is 10 μm or more, the adhesion to the metal terminal 14 is superior. Furthermore, when the thickness of the innermost layer 31 is 100 μm or less, an increase in the cost of the terminal resin film 16 can be suppressed.
[0051] [Outermost layer] In this embodiment, the outermost layer 32 is a layer that is fused to an exterior material. The outermost layer 32 contains polypropylene having a structure with long chain branches, and polypropylene having no long chain branches and a melting point of 80 to 155° C. The outermost layer contains polypropylene having a structure with long chain branches, and polypropylene having no long chain branches and a melting point of 80 to 155° C., so that the outermost layer has excellent adhesion to the exterior material in a room temperature environment, and can sufficiently maintain adhesion to the exterior material even when exposed to a high temperature environment.
[0052] Polypropylene having a long chain branching structure (hereinafter also referred to as long chain branched PP) means polypropylene having a branching structure due to molecular chains having several tens or more of carbon atoms in the main chain and an average molecular weight of several hundreds or more. The polypropylene having a long chain branching structure may be a propylene homopolymer or copolymer. In the case of a propylene copolymer, the comonomer is at least one olefin selected from the group consisting of ethylene and α-olefins having 4 to 10 carbon atoms, and the content of the comonomer in the long chain branched PP is preferably 3 mass% or less. The long chain branched PP is preferably a propylene homopolymer because of high heat resistance and rigidity.
[0053] The long-chain branched PP can be produced by a method using electronic crosslinking or synthesis using a metallocene catalyst. From the viewpoint of suppressing the generation of gel and obtaining sufficient strength, the long-chain branched PP is preferably one synthesized using a metallocene catalyst. Whether the long-chain branched PP has been synthesized using a metallocene catalyst can be confirmed by analyzing catalyst residues using analytical methods such as infrared spectroscopy (IR), NMR spectroscopy, mass spectrometry (MS), X-ray analysis, and Raman spectroscopy.
[0054] The melting point of the long-chain branched PP is preferably from 100 to 170°C, more preferably from 130 to 160°C, from the viewpoints of embeddability and heat resistance.
[0055] In the outermost layer 32, the content of the long-chain branched PP is preferably 1 to 50 mass%, more preferably 3 to 30 mass%, and even more preferably 5 to 20 mass%, based on the total amount of the outermost layer 32. When the content of the long-chain branched PP is 1 mass% or more, foaming in the outermost layer can be further suppressed. When the content of the long-chain branched PP is 50 mass% or less, the embeddability is more excellent, sufficient adhesion with the exterior material can be maintained, and curling of the resin film for terminal can be further suppressed.
[0056] The polypropylene having no long chain branches and a melting point of 80 to 155° C. means a polypropylene having a melting point of 80 to 155° C. that does not fall under the category of the polypropylene having long chain branches. The polypropylene having no long chain branches and a melting point of 80 to 155° C. may be a homopolypropylene, a random polypropylene, a block polypropylene, a low regularity polypropylene, or the like, each having a melting point of 80 to 155° C. The polypropylene having no long chain branches and a melting point of 80 to 155° C. may be modified.
[0057] The melting point of the polypropylene having no long chain branch structure and having a melting point of 80 to 155°C is more preferably 100 to 150°C, and further preferably 105 to 145°C, from the viewpoints of adhesion to the exterior material and heat resistance.
[0058] The outermost layer 32 preferably contains a filler from the viewpoint of further suppressing foaming in the outermost layer. Examples of the filler include inorganic fillers such as aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, calcium carbonate, zirconium silicate, zinc oxide, barium sulfate, copper oxide, cobalt oxide, titanium oxide, tin oxide, iron oxide, antimony oxide, boron nitride, aluminum nitride, and silicon nitride. These may be used alone or in combination of two or more. The average particle size of the filler is preferably 0.1 to 25 μm. The content of the filler is preferably 0.05 to 10 mass % based on the total amount of the outermost layer 32, and more preferably 0.1 to 5 mass %. When the content of the filler is 0.05 mass % or more, the decrease in adhesion due to foaming can be further suppressed. When the content of the filler is 10 mass % or less, sufficient adhesion to the exterior material can be maintained.
[0059] The outermost layer 32 may contain resins and additives other than the above-mentioned components. Examples of additives include antioxidants, slip agents, flame retardants, light stabilizers, dehydrating agents, coloring pigments, and tackifiers. These may be used alone or in combination of two or more. Examples of coloring pigments include carbon black, quinacridone pigments, polyazo pigments, and isoindolinone pigments.
[0060] The thickness of the outermost layer 32 is preferably 10 to 100 μm, and more preferably 15 to 50 μm. When the thickness of the outermost layer 32 is 10 μm or more, the adhesion to the exterior material 13 is superior. Furthermore, when the thickness of the outermost layer 32 is 100 μm or less, an increase in the cost of the resin film for terminal 16 can be suppressed.
[0061] The melting points of the innermost layer 31 and the outermost layer 32 can be determined by reading the peak top temperature, which is the main peak having the largest heat of dissolution measured by DSC. The absolute difference (difference in absolute value) between the melting points of the innermost layer 31 and the outermost layer 32 is preferably 0 to 15°C, more preferably 0 to 10°C, and even more preferably 0 to 5°C, from the viewpoint of further suppressing curling of the resin film for terminal.
[0062] [Middle layer] The intermediate layer 33 is disposed between the innermost layer 31 and the outermost layer 32. One surface of the intermediate layer 33 may be covered by the innermost layer 31, and the other surface may be covered by the outermost layer 32.
[0063] The intermediate layer 33 has an insulating layer. The insulating layer is a layer for preventing insulation deterioration caused by the sealant (the sealant layer of the exterior material and the innermost and outermost layers of the resin film for terminals) flowing out during heat sealing and contacting the exposed metal layer of the exterior material with the metal terminal. For this reason, the insulating layer is preferably formed using a resin having a high melting point or glass transition temperature that does not flow out during heat sealing.
[0064] Examples of resins that can be used to form the insulating layer include polyethylene terephthalate, polyethylene naphthalate, polyphenylene sulfide, polymethylpentene, polyacetal, cyclic polyolefin, polyamide, polycarbonate, polyphenylene ether, and polypropylene. Among these, polypropylene is preferably used from the viewpoints of film formability, interlayer adhesion, impact resistance, and the like, and block polypropylene is more preferably used. Furthermore, these resins preferably have a higher melting point or glass transition temperature (Tg) than the resins used in the innermost layer 31 and the outermost layer 32. These resins can be used alone or in combination of two or more.
[0065] Moreover, the insulating layer preferably contains a filler from the viewpoint of further suppressing foaming in the outermost layer. As the filler, the above-mentioned inorganic fillers that can be used in the outermost layer can be used in the same way. These can be used alone or in combination of two or more. The average particle size of the filler is preferably 0.1 to 25 μm. The content of the filler is preferably 0.1 to 30 mass % based on the total amount of the insulating layer (intermediate layer 33), and more preferably 1 to 15 mass %. When the content of the filler is 0.1 mass % or more, the decrease in adhesion due to foaming can be further suppressed. When the content of the filler is 30 mass % or less, sufficient embeddability can be maintained.
[0066] Also, the insulating layer may be colored by adding a coloring pigment to the insulating layer. By coloring the insulating layer, it is possible to improve the visibility of the terminal resin film 16. This improves the accuracy of the inspection of the terminal resin film 16 (specifically, for example, inspection of whether the terminal resin film 16 is attached to the metal terminal 14, inspection of the attachment position of the terminal resin film 16 relative to the metal terminal 14, etc.). Examples of the coloring pigment include copper oxide, cobalt oxide, zinc oxide, titanium oxide, carbon black, barium sulfate, quinacridone pigments, polyazo pigments, isoindolinone pigments, etc.
[0067] The intermediate layer 33 may further include a layer having a configuration other than the insulating layer described above. That is, the intermediate layer 33 may have a single-layer structure of only an insulating layer, or may have a multi-layer structure having a plurality of resin layers other than the insulating layer, for example, via an adhesive. The intermediate layer 33 may include, for example, a layer (crosslinked layer) containing a resin having a crosslinked structure, and a layer (reinforced layer) containing at least one selected from the group consisting of a filler and a fiber.
[0068] In the crosslinked layer, examples of the resin having a crosslinked structure include crosslinked acrylic resin, epoxy resin, phenol resin, urea resin, melamine resin, polyurethane resin, etc. These may be used alone or in combination of two or more.
[0069] The reinforcing layer may contain the same filler as the insulating layer, and the filler content is preferably 0.5 to 20 mass % based on the total amount of the reinforcing layer.
[0070] In the reinforcing layer, the fibers may be made of cellulose resin or the resin having a melting point of 200°C or higher used in the heat-resistant layer. These may be used alone or in combination of two or more. The fiber width is preferably 10 nm to 10 μm, and the fiber content is preferably 0.5 to 70 mass% based on the total amount of the reinforcing layer. The fibers may form a nonwoven fabric.
[0071] The reinforcing layer may be a layer in which the above-mentioned filler and / or fiber is dispersed in the above-mentioned polyolefin resin, a resin having a melting point of 200° C. or higher, a resin having a crosslinked structure, or the like.
[0072] The thickness of the intermediate layer 33 (the total thickness in the case of a multi-layer structure) can be set appropriately within a range of, for example, 10 to 200 μm, and is preferably 20 to 100 μm. Note that the balance between the thickness of the intermediate layer 33 and the thicknesses of the metal terminal 14 and the innermost layer 31 is important, and when the thickness of the innermost layer 31 or the metal terminal 14 is thick, the thickness of the intermediate layer 33 may be made thick accordingly.
[0073] The total thickness of the innermost layer 31, the outermost layer 32 and the intermediate layer 33 (the thickness of the resin film 16 for terminal) is preferably 10 to 500 μm, more preferably 15 to 300 μm, and even more preferably 30 to 200 μm, from the viewpoints of heat sealability, embeddability of the metal terminal and insulation properties.
[0074] When the intermediate layer 33 is an insulating layer, the thickness ratio of the innermost layer 31, the intermediate layer 33, and the outermost layer 32 (innermost layer 31:intermediate layer 33:outermost layer 32) may be, for example, 2:1:2, 1:2:1, 1:1:1, etc., such that the innermost layer 31 and the outermost layer 32 are uniform in thickness. In addition, the thickness ratio of the innermost layer 31, the intermediate layer 33, and the outermost layer 32 (innermost layer 31:intermediate layer 33:outermost layer 32) may be, for example, 3:1:1, 2:2:1, or 5:3:2, such that the thickness of the innermost layer 31 in contact with the metal terminal is thicker than the thickness of the outermost layer 32 from the viewpoint of embeddability of the metal terminal, or may be, for example, 1:1:3, 1:2:2, or 2:3:5, such that the thickness of the outermost layer 32 in contact with the exterior material is thicker than the thickness of the innermost layer 31 from the viewpoint of adhesion to the exterior material.
[0075] When the innermost layer 31 and the outermost layer 32 have the same thickness, the ratio of their thickness to the thickness of the intermediate layer 33 (innermost layer 31 or outermost layer 32:intermediate layer 33) may be 1:3 to 3:1, or 1:2 to 2:1. When the thickness of the innermost layer 31 and the thickness of the outermost layer 32 are different, the ratio of the thickness of the innermost layer 31 to the thickness of the intermediate layer 33 (innermost layer 31:intermediate layer 33) may be 4:1 to 1:1, or may be 3:1 to 1:1, the ratio of the thickness of the outermost layer 32 to the thickness of the intermediate layer 33 (outermost layer 32:intermediate layer 33) may be 1:3 to 3:1, or may be 1:2 to 2:1, and the ratio of the thickness of the innermost layer 31 to the thickness of the outermost layer 32 (innermost layer 31:outermost layer 32) is preferably 1:5 to 9:2, more preferably 3:10 to 7:2, and even more preferably 2:5 to 5:2, from the viewpoint of further suppressing curling of the resin film for terminal. That is, the ratio of the thickness of the innermost layer to the thickness of the outermost layer (innermost layer / outermost layer) is preferably 0.2 to 4.5, more preferably 0.3 to 3.5, and even more preferably 0.4 to 2.5, from the viewpoint of further suppressing curling of the resin film for a terminal.
[0076] Although the preferred embodiments of the present disclosure have been described in detail above, the present disclosure is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present disclosure as described in the claims.
[0077] For example, in FIG. 3, a terminal resin film 16 having a three-layer structure is described as an example, but a second intermediate layer made of insulating resin or the like may be disposed between the intermediate layer 33 and the innermost layer 31, and between the intermediate layer 33 and the outermost layer 32.
[0078] In this way, by disposing the second intermediate layer between the intermediate layer 33 and the innermost layer 31, and between the intermediate layer 33 and the outermost layer 32, respectively, to form a multilayer structure of four or more layers, it is possible to improve the insulation between the intermediate layer 33 and the barrier layer 24 (metal layer) constituting the exterior material 13, and the insulation between the intermediate layer 33 and the metal terminal 14. The second intermediate layer may be the above-mentioned bridging layer or reinforcing layer.
[0079] The innermost layer 31 and the outermost layer 32 may have the same structure or different structures. That is, in the resin film for a terminal of the present disclosure, at least one of the layers on the surface of the resin film for a terminal may be a layer that satisfies the requirements of the outermost layer, and the other layer may not be a layer that satisfies the requirements of the outermost layer. Therefore, one of the innermost layer 31 and the outermost layer 32 may be a layer that contains polypropylene having a long chain branching structure and polypropylene having a melting point of 80 to 155°C and not having a long chain branching structure, and the other may be a layer that does not contain either or both of the polypropylene having a long chain branching structure and the polypropylene having a melting point of 80 to 155°C and not having a long chain branching structure.
[0080] Next, a brief description will be given of a method for manufacturing the terminal resin film 16 of this embodiment. There is no particular limitation on the method for manufacturing the terminal resin film 16. The terminal resin film 16 can be manufactured using, for example, a film extrusion manufacturing device having a die such as a round die used in the inflation molding method or a T die used in the push die method, but from the viewpoint of film formation stability, a multi-layer inflation molding method is preferable.
[0081] In the following description, as an example of a method for producing the terminal resin film 16, a case in which the terminal resin film 16 is produced using an inflation molding method (in other words, an inflation molding device) will be described.
[0082] First, base materials for the innermost layer 31, the outermost layer 32, and the intermediate layer 33 are prepared. Next, the base materials for the innermost layer 31, the outermost layer 32, and the intermediate layer 33 are supplied to an inflation molding device. Next, the three base materials are extruded from the extrusion section of the inflation molding device to form a three-layer structure (a structure in which the innermost layer 31, the outermost layer 32, and the intermediate layer 33 are laminated), while air is supplied from inside the extruded laminate of the three-layer structure.
[0083] Then, while conveying the cylindrically inflated resin film for terminals 16, a guide section deforms the film into a flat shape, and a pair of pinch rolls folds the resin film for terminals 16 into a sheet shape. Both ends of the woven tube are slit, and a pair (two strips) of film are wound into a roll around a winding core, thereby producing the resin film for terminals 16 in a roll shape.
[0084] The extrusion temperature when manufacturing the resin film for terminal 16 is, for example, preferably in the range of 130 to 300°C, more preferably 130 to 250°C. If the extrusion temperature is less than 130°C, the resin constituting each layer will not melt sufficiently, resulting in a significant increase in melt viscosity, which may cause unstable extrusion from the screw. On the other hand, if the extrusion temperature exceeds 300°C, oxidation and deterioration of the resin constituting each layer will be severe, resulting in a decrease in the quality of the resin film for terminal 16.
[0085] The screw rotation speed, blow ratio, take-up speed, etc. can be appropriately set in consideration of the desired film thickness. In addition, the film thickness ratio of each layer of the resin film for terminal 16 can be easily adjusted by changing the rotation speed of each screw.
[0086] The resin film for terminal 16 of this embodiment may be manufactured by dry lamination using an adhesive, or by laminating formed insulating layers (insulating films) together by sandwich lamination.
[0087] Here, a fusion process for melt-bonding the resin film for terminal 16 and the exterior material 13 of the present embodiment will be described with reference to Fig. 3. In the fusion process, the resin film for terminal 16 and the exterior material 13 are thermally fused together while simultaneously melting the outermost layer 32 by heating and bonding the outermost layer 32 to the exterior material 13 by applying pressure.
[0088] In the fusion treatment, heating is performed to a temperature equal to or higher than the melting point of the resin constituting the outermost layer 32 in order to obtain sufficient adhesion and sealing properties between the resin film for terminal 16 and the exterior material 13 .
[0089] Specifically, the heating temperature of the terminal resin film 16 can be, for example, 140 to 170°C. The treatment time (the total time of the heating time and the pressing time) needs to be determined in consideration of the peel strength and productivity. The treatment time can be appropriately set within the range of, for example, 1 to 60 seconds.
[0090] When priority is given to the production takt time (productivity) of the terminal resin film 16, heat fusion may be performed with a short pressurizing time at a temperature exceeding 170° C. In this case, the heating temperature may be, for example, 170 to 230° C., and the pressurizing time may be, for example, 3 to 20 seconds.
[0091] 3, a fusion process for melt-bonding the terminal resin film 16 and the exterior material 13 of the present embodiment will be described. In the fusion process, the terminal resin film 16 and the metal terminal 14 are thermally fused together while simultaneously melting the innermost layer 31 by heating and bonding the innermost layer 31 and the metal terminal 14 by applying pressure.
[0092] In the fusion process, heating is performed to a temperature equal to or higher than the melting point of the resin constituting the innermost layer 31 in order to obtain sufficient adhesion and sealing properties between the terminal resin film 16 and the metal terminal 14 .
[0093] Specifically, the heating temperature of the terminal resin film 16 can be, for example, 140 to 170°C. The treatment time (the total time of the heating time and the pressing time) needs to be determined in consideration of the peel strength and productivity. The treatment time can be appropriately set within the range of, for example, 1 to 60 seconds.
[0094] When priority is given to the production takt time (productivity) of the terminal resin film 16, heat fusion may be performed with a short pressurizing time at a temperature exceeding 170° C. In this case, the heating temperature may be, for example, 170 to 230° C., and the pressurizing time may be, for example, 3 to 20 seconds. EXAMPLES
[0095] Hereinafter, the present disclosure will be described more specifically based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0096] [Materials used] The materials used in the examples and comparative examples are shown in Table 1 below. [Table 1]
[0097] [Preparation of resin film for terminals] (Examples 1 to 15 and Comparative Examples 1 to 4) The components shown in Table 2 were mixed in the amounts shown in the table (unit: mass%, abbreviated as "%" in the table) and dry blended to prepare the base material for each layer. When the heat of fusion of each layer was measured by DSC, a peak corresponding to the melting point of each resin component was detected. The absolute difference between the melting points of the outermost layer and the innermost layer is shown in Table 2.
[0098] Next, the base material of the first adhesive layer (outermost layer), the base material of the insulating layer (middle layer), and the base material of the second adhesive layer (innermost layer) were set in an inflation type film extrusion manufacturing device (Co-OI type) manufactured by Sumitomo Heavy Industries Modern Co., Ltd., and the above three base materials were extruded by the film extrusion manufacturing device to produce a three-layered resin film for terminals of outermost layer / middle layer / innermost layer (however, Comparative Example 4 is a two-layered resin film for terminals of middle layer / innermost layer). The melting temperature of each base material was 210°C. The thickness of each layer in the resin film for terminals of each Example was as shown in "Thickness [μm] outer / middle / inner" in Table 2. In addition, "outer / middle / inner" in Table 2 means outermost layer (outer) / middle layer (middle) / innermost layer (inner).
[0099] [Measurement of initial heat seal strength against lead (at room temperature)] A sample of a resin film for terminals cut to a size of 50 mm (TD) x 100 mm (MD) was folded in two so as to sandwich a chemically treated aluminum foil cut to a size of 50 mm x 50 mm, and the end opposite to the folded part was heat-sealed over a width of 10 mm at 165°C / 0.6 MPa / 10 seconds. Then, a 15 mm width was cut out from the center of the longitudinal direction of the heat-sealed part (see FIG. 4) to prepare a sample for measuring heat-seal strength. In this evaluation, the laminate 100 in FIG. 4 is a laminate consisting of a resin film for terminals / aluminum foil / resin film for terminals. A T-shaped peel test between the aluminum foil (lead) and the resin film for terminals was performed on the heat-sealed part of this sample using a tensile tester (manufactured by Shimadzu Corporation) under conditions of room temperature (25°C) environment and a tensile speed of 50 mm / min. From the obtained results, the initial heat-seal strength to the lead was evaluated based on the following evaluation criteria. Evaluations of A, B, or C are pass, and D is fail. The results are shown in Table 2. A: Heat seal strength is 25N / 15mm or more B: Heat seal strength is 20N / 15mm or more and less than 25N / 15mm C: Heat seal strength is 15N / 15mm or more and less than 20N / 15mm D: Heat seal strength is less than 15N / 15mm
[0100] [Measurement of initial heat seal strength (at room temperature) to exterior materials] A sample of the resin film for terminals cut to a size of 50 mm (TD) x 100 mm (MD) was folded in two so as to sandwich a chemically treated aluminum foil cut to a size of 50 mm x 50 mm, and the end opposite the folded part was heat sealed over a width of 10 mm at 165 ° C / 0.6 MPa / 10 seconds. Then, it was folded in two so that the sealant layer of the exterior material having a laminated structure of nylon film (thickness 25 μm) / adhesive / aluminum foil (thickness 40 μm) / polypropylene sealant layer (thickness 80 μm) was in contact with the resin film for terminals, and the end opposite the folded part (the same part as the part where the resin film for terminals and the aluminum foil were heat sealed) was heat sealed over a width of 10 mm at 190 ° C / 0.5 MPa / 5 seconds. Then, the center part of the heat seal part in the longitudinal direction was cut out to a width of 15 mm (see Figure 4) to prepare a sample for measuring heat seal strength. In this evaluation, the laminate 100 in Fig. 4 is a laminate consisting of an exterior material / resin film for terminal / aluminum foil / resin film for terminal / exterior material. A T-peel test between the exterior material and the resin film for terminal was performed on the heat-sealed portion of this sample at room temperature (25°C) and a tensile speed of 50 mm / min using a tensile tester (manufactured by Shimadzu Corporation). From the obtained results, the initial heat seal strength to the exterior material was evaluated based on the following evaluation criteria. A, B, or C indicates pass, and D indicates fail. The results are shown in Table 2. A: Heat seal strength is 100N / 15mm or more B: Heat seal strength is 90N / 15mm or more and less than 100N / 15mm C: Heat seal strength is 80N / 15mm or more and less than 90N / 15mm D: Heat seal strength is less than 80N / 15mm
[0101] [Heat seal strength against electrolyte in exterior material] A sample of the resin film for terminals cut to a size of 50 mm (TD) x 100 mm (MD) was folded in two so as to sandwich a chemically treated aluminum foil cut to a size of 50 mm x 50 mm, and the end opposite the folded part was heat sealed at 165 ° C / 0.6 MPa / 10 seconds over a width of 10 mm. Then, it was folded in two so that the sealant layer of the exterior material having a laminated structure of nylon film (thickness 25 μm) / adhesive / aluminum foil (thickness 40 μm) / polypropylene sealant layer (thickness 80 μm) was in contact with the resin film for terminals, and the end opposite the folded part (the same part as the part where the resin film for terminals and the aluminum foil were heat sealed) was heat sealed at 190 ° C / 0.5 MPa / 5 seconds over a width of 10 mm. Then, the remaining two ends other than the folded part were heat sealed in the same manner as the end opposite the folded part. First, one of the remaining two ends was heat-sealed, and then 1 mL of an electrolyte prepared by adding LiPF6 (lithium hexafluorophosphate) to a mixture of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) to adjust LiPF6 to 1M was injected, and the remaining one was heat-sealed to prepare a pouch. The prepared pouch was stored at 90°C for one week, and then the center of the lengthwise direction of the heat-sealed part at the end opposite to the folded part was cut out to a width of 15 mm (see FIG. 4) to prepare a sample for measuring heat seal strength. In this evaluation, the laminate 100 in FIG. 4 is a laminate consisting of an exterior material / resin film for terminals / aluminum foil / resin film for terminals / exterior material. A T-peel test was performed between the exterior material and the terminal resin film on the heat-sealed portion of this sample at room temperature (25°C) and a tensile speed of 50 mm / min using a tensile tester (manufactured by Shimadzu Corporation). From the results obtained, the heat seal strength of the exterior material against the electrolyte was evaluated based on the following evaluation criteria. A, B, or C indicates pass, and D indicates fail. The evaluation and seal strength results are shown in Table 2. A: Heat seal strength is 70N / 15mm or more B: Heat seal strength is 60N / 15mm or more and less than 70N / 15mm C: Heat seal strength is 50N / 15mm or more and less than 60N / 15mm D: Heat seal strength is less than 50N / 15mm
[0102] [Curling evaluation] A sample of the resin film for terminals was cut to a size of 50 mm (TD) x 100 mm (MD) and placed on a smooth surface, and the height of four vertices from the smooth surface was measured. The curling was evaluated based on the average height of the four points according to the following evaluation criteria. A rating of A, B, or C is pass, and D is fail. The results are shown in Table 2. A: Curl height is less than 15 mm B: Curl height is 15mm or more and less than 20mm C: Curl height is 20mm or more and less than 25mm D: Curl height is 25mm or more
[0103] [Table 2] [Explanation of symbols]
[0104] 10...electricity storage device, 11...electricity storage device main body, 13...exterior material, 14...metal terminal, 14-1...metal terminal main body, 14-2...corrosion prevention layer, 16...resin film for terminal, 21...inner layer, 22...inner layer side adhesive layer, 23-1, 23-2...corrosion prevention treatment layer, 24...barrier layer, 25...outer layer side adhesive layer, 26...outer layer, 31...innermost layer, 32...outermost layer, 33...intermediate layer.
Claims
1. A resin film for a terminal having three or more layers, which is arranged so as to cover a part of an outer peripheral surface of a metal terminal electrically connected to a main body of an electricity storage device constituting an electricity storage device, A first adhesive layer disposed on one surface, a second adhesive layer disposed on a surface opposite to the first adhesive layer, and an insulating layer disposed between the first adhesive layer and the second adhesive layer; The resin film for a terminal, wherein the first adhesive layer is a layer containing polypropylene having a long chain branching structure and polypropylene having no long chain branching structure and having a melting point of 80 to 155°C.
2. The resin film for terminals according to claim 1, wherein the content of the polypropylene having a long chain branched structure is 1 to 50 mass % based on the total amount of the first adhesive layer.
3. 3. The resin film for a terminal according to claim 1, wherein the polypropylene having a structure with long chain branches is synthesized using a metallocene catalyst.
4. The resin film for a terminal according to any one of claims 1 to 3, wherein a ratio of a thickness of the second adhesive layer to a thickness of the first adhesive layer is 0.2 to 4.
5.
5. The resin film for a terminal according to any one of claims 1 to 4, wherein an absolute difference between the melting point of the first adhesive layer and the melting point of the second adhesive layer is 0 to 15°C.
6. The resin film for a terminal according to any one of claims 1 to 5, wherein the first adhesive layer and / or the insulating layer contains a filler.
7. The resin film for a terminal according to any one of claims 1 to 6, wherein the second adhesive layer contains a resin having a polar group.
8. A power storage device body; A metal terminal electrically connected to the power storage device body; an exterior material that holds the metal terminals and accommodates the power storage device main body; The resin film for terminal according to any one of claims 1 to 7 is disposed between the metal terminal and the exterior material while covering a part of an outer peripheral surface of the metal terminal, The first adhesive layer is in contact with the exterior material, and the second adhesive layer is in contact with the metal terminal.
Citation Information
Patent Citations
Sealant for tab lead, tab lead and lithium ion secondary battery
JP2014225378A
Film for tab lead and tab lead using the same
JP2019220295A
Electrochromic composition
JP2020079387A
Terminal film for electricity storage devices, and electricity storage device
WO2015115371A1
Biaxially stretched polypropylene film, metallized film, and capacitor
WO2017221985A1