High-strength zeolite molding and method for manufacturing the same
A high-strength zeolite molded body is produced using a low-acidity clay binder and controlled manufacturing process, addressing the complexity and strength issues of existing methods, ensuring durability and minimizing side reactions for effective adsorption and separation.
Patent Information
- Application Number
- JP2024117974
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-20
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing zeolite molded bodies with sufficient strength are complex, economically disadvantageous, and result in lower strength than binder-containing zeolite molded bodies, leading to potential equipment failure due to powdering.
A high-strength zeolite molded body is produced using a low-acidity clay binder, with specific ratios of zeolite and clay, and a manufacturing process involving kneading, drying, and firing at controlled temperatures to achieve a compressive strength of 20 N or more.
The resulting zeolite molded body maintains high strength, reducing the risk of powdering and equipment failure, while minimizing side reactions with organic substances, making it suitable for adsorption and separation applications.
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength zeolite shaped body and a method for producing the same, and more particularly to a high-strength zeolite shaped body using a low-acid clay binder and a method for producing the same. The high-strength zeolite shaped body of the present invention is useful for applications such as an adsorption / separation agent. [Background technology]
[0002] In recent years, VOC emissions, which are considered to be one of the causative substances of suspended particulate matter and photochemical oxidants, have been restricted, and attention has been focused on technologies to control VOC emissions. Zeolite has been attracting attention as a VOC adsorbent. Its skeleton is made of heat-resistant silicon dioxide, so it is easy to adsorb and desorb VOCs at high temperatures, and it has a high specific surface area. Zeolite's pores are also uniform, making it possible to adsorb and separate specific VOCs. When using zeolite for adsorption and separation, it is difficult to handle in powder form, so it is molded into pellets, beads, honeycombs, etc. When using zeolite for adsorption and separation, it is necessary to use a molded body with sufficient physical strength, as it is filled into a column or fluidized bed. In particular, molded bodies with weak strength that will powder after long-term use are not desirable because they will cause equipment failure. Zeolite alone has low plasticity, making it difficult to mold into the desired shape or to create a high-strength molded body, so a binder is often used. Clay, silica sol, alumina, etc. are used as binders. Although these binders are not used for adsorption separation, they may cause a decrease in the adsorption separation ability. For example, when aromatic hydrocarbons are adsorbed and separated, if clay or alumina having acid sites is used as a binder, the aromatic hydrocarbons may react, and the desired aromatic hydrocarbons may not be separated. As a method for preventing the decrease in adsorption separation ability due to the binder, methods such as making the molded body binderless or converting the binder into zeolite have been adopted. For example, in Patent Document 1, a molded body made of a kaolin clay binder and an FAU type zeolite is prepared, and then the kaolin clay binder is converted into a metakaolin clay binder by performing a heat treatment, and further a hydroxide source is added and subjected to a hydrothermal treatment to convert the non-zeolite components into FAU type zeolite, thereby obtaining a binderless zeolite adsorbent.
[0003] In addition, in Patent Document 2, raw materials containing an aluminum component, an alkali metal component, and a tetraalkylammonium component are supported on a silica molded body, and then the silica component is converted into zeolite by contacting it with saturated steam and a zeolite precursor, thereby obtaining a binderless zeolite molded body.
[0004] However, these methods all have problems in that the steps are extremely complicated and economically disadvantageous. Furthermore, these binderless zeolite shaped bodies have lower strength than binder-containing zeolite shaped bodies, and there is a possibility that the pulverization may cause equipment failure. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2019-501766 [Patent Document 2] JP 2006-334454 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a high-strength zeolite shaped body using a clay binder with a low acid content, which can be produced by a method that is simpler and less expensive than conventional methods, and a method for producing the same. The high-strength zeolite shaped body of the present invention can be used in various adsorption and separation applications. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved, leading to the completion of the present invention. That is, the present invention relates to a zeolite molded body containing 10 to 40 parts by weight of clay per 100 parts by weight of zeolite and having a compressive strength of 20 N or more, wherein the zeolite has a Si / Al ratio of 100 to 400 parts by weight of clay. 2 The clay contains one or more zeolites having a molecular weight of 300 or more and 100,000 or less, and a water adsorption amount of 10 (g / 100g) or less under the conditions of 25°C and a relative pressure of 0.5, 3- A high-strength zeolite molded body containing one or more clays having a solid acidity of 0.15 mmol / g or less by a TPD method, which is obtained by mixing and kneading 10 parts by weight of zeolite with 10 to 40 parts by weight of clay, 1 to 5 parts by weight of a molding aid, 0.5 to 5 parts by weight of a water-soluble sodium salt, and 60 to 100 parts by weight of water, and then forming and drying the kneaded mixture. The obtained zeolite molded body is crushed and then fired at 400°C to 700°C, and the zeolite is Si / Al 2 The clay contains one or more zeolites having a molecular weight of 300 or more and 100,000 or less, and a water adsorption amount of 10 (g / 100g) or less under the conditions of 25°C and a relative pressure of 0.5, 3 -A method for producing a high-strength zeolite molded body containing one or more clays having a solid acidity of 0.15 mmol / g or less by the TPD method.
[0008] The present invention will be described in detail below.
[0009] The high-strength zeolite molded article of the present invention contains 10 parts by weight or more and 40 parts by weight or less of clay based on 100 parts by weight of zeolite.
[0010] The zeolite contained in the high-strength zeolite molded body is Si / Al 2 The zeolite has a molecular weight of 300 or more and 100,000 or less, and has a water adsorption amount of 10 (g / 100g) or less under the conditions of 25°C and a relative pressure of 0.5. 2 If the ratio is less than 300, the affinity between zeolite and water is high, and the adsorption of VOCs, etc. may be inhibited. If the amount of water adsorption exceeds 10 (g / 100g) under conditions of 25°C and relative pressure 0.5, the affinity between zeolite and water is high, and the adsorption of VOCs, etc. may be inhibited. 2is preferably 500 or more and 10,000 or less, and more preferably 1,000 or more and 2,000 or less. The water adsorption amount under conditions of 25° C. and a relative pressure of 0.5 is preferably 5 (g / 100 g) or less. Examples of the type of zeolite include beta zeolite, Y zeolite, L zeolite, ferrierite zeolite, mordenite zeolite, and ZSM-5 zeolite, with ZSM-5 zeolite being preferred.
[0011] The amount of clay contained in the high-strength zeolite molded body is 10 parts by weight or more and 40 parts by weight or less per 100 parts by weight of zeolite (anhydrous equivalent). If it is less than 10 parts by weight, the pressure resistance strength is low, and even if it is more than 40 parts by weight, the pressure resistance strength is not improved and the amount of zeolite contained in the zeolite molded body is reduced, which causes a decrease in the adsorption separation ability. In order to increase the pressure resistance strength, it is preferable to use 12 parts by weight or more and 30 parts by weight or less, and more preferably 15 parts by weight or more and 25 parts by weight or less. The particle size of the clay is not particularly limited, but is preferably 0.5 μm or more and 30 μm or less as an average particle size, and more preferably 1 μm or more and 25 μm or less as an average particle size. Examples of clay include bentonite clay, sepiolite clay, attapulgite clay, palygorskite clay, synthetic layered silicate (smectite clay), etc., and bentonite clay is preferred.
[0012] The clay contained in the high-strength zeolite compact is NH 3 -Clay having a solid acidity of 0.15mmol / g or less by TPD method, and containing one or more of these. 3 -When the solid acidity by the TPD method exceeds 0.15 mmol / g, there is a possibility that the clay-derived acid sites react with the adsorbate. 3 The solid acid amount measured by the -TPD method is preferably 0.10 mmol / g or less, and more preferably 0.05 mmol / g or less.
[0013] In the present invention, the NH 3 -The amount of solid acid by the TPD method is measured by the NH3 - is a value measured by the TPD method. 3 The solid acidity measured by the TPD method is a value obtained by measuring the amount of ammonia desorbed at 100°C to 700°C from a sample saturated with ammonia at room temperature. Specifically, ammonia is saturated and adsorbed on a sample at room temperature, and the sample is heated to 100°C to remove any ammonia remaining in the measurement atmosphere. The amount of ammonia measured during the temperature rise process up to 700°C at a rate of 10°C / min is regarded as the solid acidity. The amount of ammonia can be measured using a TCD detector. More specifically, as described below, <NH 3 -Measurement of solid acidity by TPD method.
[0014] The high-strength zeolite shaped body of the present invention has a compressive strength measured with a Koyashiki hardness tester of at least 20 N. If the compressive strength is less than 20 N, it is likely to be pulverized, which may cause pressure loss and a decrease in adsorption efficiency.
[0015] The method for producing a high-strength zeolite molded body of the present invention (hereinafter also referred to as the "production method of the present invention") is characterized in that 100 parts by weight of zeolite are mixed with 10 to 40 parts by weight of clay, 1 to 5 parts by weight of a molding aid, 0.5 to 5 parts by weight of a water-soluble sodium salt, and 60 to 100 parts by weight of water, and then kneaded to obtain a kneaded product containing these, which is molded and dried, and the obtained zeolite molded body is crushed and then fired at 400 to 700°C.
[0016] The zeolite contained in the kneaded material used in the production method of the present invention is Si / Al 2 The zeolite has a molecular weight of 300 or more and 100,000 or less, and has a water adsorption amount of 10 (g / 100g) or less under the conditions of 25°C and a relative pressure of 0.5. 2If the ratio is less than 300, the affinity between zeolite and water is high, and the adsorption of VOCs, etc. may be inhibited. If the amount of water adsorption exceeds 10 (g / 100g) under conditions of 25°C and relative pressure 0.5, the affinity between zeolite and water is high, and the adsorption of VOCs, etc. may be inhibited. 2 is preferably 500 or more and 10,000 or less, and more preferably 1,000 or more and 2,000 or less. The water adsorption amount under conditions of 25° C. and a relative pressure of 0.5 is preferably 5 (g / 100 g) or less. Examples of the type of zeolite include beta zeolite, Y zeolite, L zeolite, ferrierite zeolite, mordenite zeolite, and ZSM-5 zeolite, with ZSM-5 zeolite being preferred.
[0017] The clay contained in the kneaded material used in the manufacturing method of the present invention is NH 3 -The solid acidity by TPD method is 0.15mmol / g or less. NH 3 -When the solid acidity by the TPD method exceeds 0.15 mmol / g, there is a possibility that the clay-derived acid sites react with the adsorbate. 3 The solid acid amount measured by the -TPD method is preferably 0.10 mmol / g or less, and more preferably 0.05 mmol / g or less.
[0018] Examples of clay include bentonite clay, sepiolite clay, attapulgite clay, palygorskite clay, synthetic layered silicate (smectite clay), etc., with bentonite clay being preferred.
[0019] The amount of clay is 10 parts by weight or more and 40 parts by weight or less per 100 parts by weight of zeolite (anhydrous equivalent). If it is less than 10 parts by weight, moldability decreases, and even if it is more than 40 parts by weight, no improvement in moldability is observed. In order to further improve moldability, it is preferably 12 parts by weight or more and 30 parts by weight or less, and more preferably 15 parts by weight or more and 25 parts by weight or less. The particle size of the clay is not particularly limited, but is preferably 0.5 μm or more and 30 μm or less as an average particle size, and more preferably 1 μm or more and 25 μm or less as an average particle size.
[0020] The kneaded material used in the manufacturing method of the present invention contains a molding aid. The molding aid is one that improves moldability, and examples thereof include cellulose, alcohol, lignin, starch, and guar gum. Of these, cellulose and alcohol are preferred because they are easy to handle. Examples of cellulose include crystalline cellulose, hydroxypropylmethylcellulose, and sodium carboxymethylcellulose (CMC). Examples of alcohol include polyvinyl alcohol and ethylene glycol. The amount of the molding aid is 1 part by weight or more and 5 parts by weight or less, and preferably 2 parts by weight or more and 4 parts by weight or less, relative to 100 parts by weight of zeolite (anhydrous equivalent). If it is less than 1 part by weight, moldability decreases, and if it exceeds 5 parts by weight, pressure resistance decreases.
[0021] The kneaded material used in the manufacturing method of the present invention contains a water-soluble sodium salt. Examples of the water-soluble sodium salt include inorganic acid sodium and organic acid sodium. The water-soluble sodium salt preferably contains at least one of inorganic acid sodium and organic acid sodium. Although the reason is unclear, the use of a water-soluble sodium salt significantly increases the pressure resistance. The amount of the water-soluble sodium salt is 0.5 parts by weight or more and 5 parts by weight or less with respect to 100 parts by weight of zeolite (anhydrous equivalent). If it is less than 0.5 parts by weight, the effect is insufficient, and if it is more than 5 parts by weight, the effect does not change. In order not to increase the amount of sodium derived from the water-soluble sodium salt, it is preferably 0.5 parts by weight or more and 3 parts by weight or less, and more preferably 0.5 parts by weight or more and 2 parts by weight or less.
[0022] The inorganic sodium salt may be any water-soluble sodium salt, such as sodium phosphate, sodium silicate, and sodium aluminate. Of these, sodium phosphate is preferably used because it is easy to handle. As the sodium phosphate, for example, sodium monophosphate, sodium diphosphate, sodium triphosphate, sodium pyrophosphate, sodium acid pyrophosphate, sodium tripolyphosphate, sodium tetrapolyphosphate, and sodium hexametaphosphate can be used.
[0023] The organic acid sodium salt may be any water-soluble sodium salt, such as general organic carboxylic acids, aminocarbonates, ether carboxylates, vinyl polymer sodium salts, etc. Examples of general organic carboxylic acids that can be used include sodium citrate, sodium gluconate, sodium oxalate, sodium tartrate, etc. Examples of aminocarbonates that can be used include sodium ethylenediaminetetraacetate, sodium diethylenetriaminopentaacetate, etc. Examples of ether carboxylates that can be used include sodium carboxymethyltartronate, sodium carboxymethyloxysuccinate, etc. Examples of vinyl polymer sodium salts that can be used include sodium polyacrylate, sodium salt of acrylic acid / maleic acid copolymer, etc.
[0024] The amount of water contained in the kneaded product used in the production method of the present invention is 60 parts by weight or more and 100 parts by weight or less, and preferably 60 parts by weight or more and 90 parts by weight or less, relative to 100 parts by weight of zeolite (anhydrous equivalent). If the amount is less than 60 parts by weight or more than 100 parts by weight, molding may become difficult.
[0025] The kneaded material used in the manufacturing method of the present invention preferably contains a pore-forming agent in order to improve the accessibility of the molded body itself. The pore-forming agent increases the macropore volume, and water-soluble salts such as sodium carbonate and sodium hydrogen carbonate can be used. In addition, combustible powders such as crystalline cellulose, hydroxypropylmethylcellulose, sodium carboxymethylcellulose (CMC), polyvinyl alcohol, etc. can be used. The pore-forming agent is removed by washing with water, burning, etc. in a process after molding, and contributes to an increase in the macropore volume of the molded body. The amount of the pore-forming agent is 20 parts by weight or less, preferably 4 parts by weight or more and 10 parts by weight or less, relative to 100 parts by weight of zeolite (anhydrous equivalent). As the amount of the pore-forming agent is increased, the pressure resistance strength decreases slightly, but the macropore volume increases, so it is important to balance the two.
[0026] The kneaded product used in the manufacturing method of the present invention is obtained by mixing 10 to 40 parts by weight of a specific clay, 1 to 5 parts by weight of a molding aid, 0.5 to 5 parts by weight of a water-soluble sodium salt, and 60 to 100 parts by weight of water (or further 20 parts by weight of a pore-forming agent) with respect to 100 parts by weight of zeolite, and then kneading the mixture. There are no particular limitations on the method of kneading the mixture after mixing, and for example, a roll mixer, a Henschel mixer which is a blade stirring type, a batch type or continuous type kneader, etc. can be used.
[0027] The manufacturing method of the present invention is to mold the kneaded product obtained as described above. There is no particular limitation on the molding method, and for example, it can be molded by rolling granulation, stirring granulation, extrusion molding, spray granulation, or a combination of two or more of these methods. There is no particular limitation on the shape of the molded product, but spherical, cylindrical, elliptical, bale-shaped, trefoil-shaped, ring-shaped, etc. are preferred, and cylindrical is more preferred. There is no particular limitation on the length of the molded product, but it is preferably 1 mm or more and 5 mm or less.
[0028] The shaped zeolite body is dried. There is no particular limitation on the drying method, and for example, a box dryer, a continuous dryer, etc. can be used. The drying temperature can be 50°C or higher and 200°C or lower. The drying atmosphere can be air or nitrogen atmosphere under atmospheric pressure. The dried zeolite body is crushed to a desired size.
[0029] The dried zeolite molded body is calcined. The calcination method is not particularly limited, and can be performed, for example, in a box-type muffle furnace, a rotary kiln, a shaft kiln, or the like. The calcination temperature is a temperature at which the fibrous clay can be sintered to develop strength, and is 400°C to 700°C. If the calcination temperature is less than 400°C, the binder is not sintered and the strength decreases, and even if the temperature exceeds 700°C, there is no change in the degree of sintering. The calcination can be performed in an air or nitrogen atmosphere under atmospheric pressure. Effect of the Invention
[0030] The high-strength zeolite shaped body of the present invention is particularly useful for adsorption separation applications, since the binder has a low acid content and is low in reactivity with organic substances, without causing side reactions. Furthermore, since the high-strength zeolite shaped body of the present invention has high strength, it is unlikely to be powdered even when used in adsorption separation, and is unlikely to cause equipment failure. EXAMPLES
[0031] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0032] <NH 3 -Measurement of solid acidity by TPD method> 0.1 g of sample (clay) was left to stand under helium flow at 500 ° C. as a pretreatment. A mixed gas containing 10 vol. % ammonia and 90 vol. % helium was passed through the sample after 1 hour of pretreatment at room temperature to saturate and adsorb ammonia to the sample. After passing the mixed gas for 1 hour, the sample was heated to 100 ° C. while passing helium gas instead of the mixed gas. After the temperature increase, the ammonia remaining in the atmosphere was removed by passing helium gas at 100 ° C. for 1 hour. After the removal of the remaining ammonia, the sample was heated to 700 ° C. at a heating rate of 10 ° C. / min under helium flow at a flow rate of 50 mL / min, and the amount of ammonia measured during the heating process using a TCD detector was taken as the amount of ammonia adsorbed on the sample. The amount of ammonia adsorbed per unit mass of the sample was taken as the solid acid amount (mmol / g).
[0033] <Measurement of the average particle size of clay> 0.5g of the sample (clay) was added to 50g of water being stirred at high speed and dispersed by stirring for a while. The average particle size was measured using a Microtrack particle size distribution analyzer (MT3000II: manufactured by Microtrack Bell). The average particle size here refers to the D50 diameter.
[0034] <Measurement of compressive strength> The compressive strength was measured using a Kiya hardness tester (KHT-20N, manufactured by Fujiwara Seisakusho). The average value of 25 pieces was taken as the compressive strength.
[0035] Example 1 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2 100 parts by weight (103 g; moisture content: 3%) of bentonite clay (Kunipia F: manufactured by Kunimine Industries) (22.2 g; moisture content: 10%, NH 3-Solid acid amount by TPD method (hereinafter, sometimes simply referred to as "solid acid amount"): 0.009 mmol / g, average particle size: 1.8 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: manufactured by Daiichi Kogyo Seiyaku), and 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai) were weighed out and mixed for 5 minutes in a kneader (Hibismix: manufactured by Primix). 68 parts by weight (68 g) of water were added and kneaded until the kneaded material was solidified. The kneaded material obtained was molded into a cylindrical shape with a diameter of 1.5 mm. It was then dried at 100°C for 12 hours or more and crushed to about 1 to 3 mm. It was then fired at 650°C for 3 hours to obtain a zeolite molded body (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al of zeolite: 1.0% by weight). 2 The results were: 1500, zeolite water adsorption: 4 (g / 100g), clay solid acidity: 0.009mmol / g, clay average particle size: 1.8μm. The compressive strength was 37N.
[0036] Example 2 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2 100 parts by weight (103 g, moisture content: 3%) of bentonite clay (Kunibond: manufactured by Kunimine Industries) were weighed out, 20 parts by weight (23.0 g, moisture content: 13%, solid acidity: 0.134 mmol / g, average particle size: 23 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: manufactured by Daiichi Kogyo Seiyaku), and 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai) were weighed out and mixed for 5 minutes with a kneader (Hibismix: manufactured by Primix). 70 parts by weight (70 g) of water were added and the kneaded material was kneaded until it was solidified. The obtained kneaded material was molded into a cylindrical shape with a diameter of 1.5 mm. After that, it was dried at 100 ° C for more than 12 hours and crushed to about 1 to 3 mm. Then, it was fired at 650°C for 3 hours to obtain a zeolite molded body (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite: 1.0). 2The results were: 1500, zeolite water adsorption: 4 (g / 100g), clay solid acidity: 0.134mmol / g, clay average particle size: 23μm. The compressive strength was 28N.
[0037] Example 3 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2 100 parts by weight (103 g; moisture content: 3%) of bentonite clay (Neokunibond: manufactured by Kunimine Industries) were weighed out, 20 parts by weight (22.6 g; moisture content: 12%, solid acidity: 0.045 mmol / g, average particle size: 8.8 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: manufactured by Daiichi Kogyo Seiyaku), and 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai) were weighed out and mixed in a kneader (Hibismix: manufactured by Primix) for 5 minutes. 67 parts by weight (67 g) of water were added and the kneaded material was kneaded until it was solidified. The obtained kneaded material was molded into a cylindrical shape with a diameter of 1.5 mm. After that, it was dried at 100 ° C for more than 12 hours and crushed to about 1 to 3 mm. Then, it was fired at 650°C for 3 hours to obtain a zeolite molded body (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite: 1.0). 2 The results were: 1500, zeolite water adsorption: 4 (g / 100g), clay solid acidity: 0.045mmol / g, clay average particle size: 8.8μm. The compressive strength was 28N.
[0038] Example 4 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2100 parts by weight (103 g, moisture content: 3%) of bentonite clay (OPTIGEL-CK: manufactured by BYK-Chemie GmbH) were weighed out, 20 parts by weight (24 g, moisture content: 17%, solid acidity: 0.01 mmol / g, average particle size: 6.4 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, cellogen: manufactured by Daiichi Kogyo Seiyaku), and 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai) were weighed out and mixed in a kneader (Hibismix: manufactured by Primix) for 5 minutes. 66 parts by weight (66 g) of water were added and the kneaded material was kneaded until it was solidified. The obtained kneaded material was molded into a cylindrical shape with a diameter of 1.5 mm. After that, it was dried at 100 ° C for more than 12 hours and crushed to about 1 to 5 mm. Then, it was fired at 650°C for 3 hours to obtain a zeolite molded body (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite: 1.0). 2 The results were: 1500, zeolite water adsorption amount 4 (g / 100g), clay solid acid amount: 0.01mmol / g, clay average particle size: 6.4μm. The compressive strength was 39N.
[0039] Example 5 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2100 parts by weight (103 g, moisture content: 3%) of bentonite clay (Kunipia F: manufactured by Kunimine Industries) 20 parts by weight (22.2 g, moisture content: 10%, solid acidity: 0.009 mmol / g, average particle size: 1.8 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: manufactured by Daiichi Kogyo Seiyaku), 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai), and 2 parts by weight (2 g) of crystalline cellulose (pore-forming agent, Ceolas (registered trademark) RC-591: manufactured by Asahi Kasei Chemicals) were measured and mixed for 5 minutes with a kneader (Hibismix: manufactured by Primix). 74 parts by weight (74 g) of water was added and kneaded until the kneaded product was consolidated. The obtained kneaded product was molded into a cylindrical shape with a diameter of 1.5 mm. It was then dried at 100°C for 12 hours or more and crushed into pieces of about 1 to 3 mm. It was then fired at 650°C for 3 hours to obtain a zeolite molded product (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite). 2 The results were: 1500, zeolite water adsorption: 4 (g / 100g), clay solid acidity: 0.009mmol / g, clay average particle size: 1.8μm. The compressive strength was 42N.
[0040] Example 6 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2100 parts by weight (103 g, moisture content: 3%) of bentonite clay (Kunipia F: manufactured by Kunimine Industries) 20 parts by weight (22.2 g, moisture content: 10%, solid acidity: 0.009 mmol / g, average particle size: 1.8 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: manufactured by Daiichi Kogyo Seiyaku), 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai), and 4 parts by weight (4 g) of crystalline cellulose (pore-forming agent, Ceolas (registered trademark) RC-591: manufactured by Asahi Kasei Chemicals) were measured and mixed for 5 minutes with a kneader (Hibismix: manufactured by Primix). 74 parts by weight (74 g) of water was added and kneaded until the kneaded product was consolidated. The obtained kneaded product was molded into a cylindrical shape with a diameter of 1.5 mm. It was then dried at 100°C for 12 hours or more and crushed into pieces of about 1 to 3 mm. It was then fired at 650°C for 3 hours to obtain a zeolite molded product (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite). 2 The results were: 1500, zeolite water adsorption: 4 (g / 100g), clay solid acidity: 0.009mmol / g, clay average particle size: 1.8μm. The compressive strength was 38N.
[0041] Example 7 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2100 parts by weight (103 g; moisture content 3%) of bentonite clay (Kunipia F: manufactured by Kunimine Industries) 20 parts by weight (22.2 g, moisture content 10%, solid acid amount: 0.009 mmol / g, average particle size: 1.8 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: manufactured by Daiichi Kogyo Seiyaku), 1 part by weight (1 g) of sodium polyacrylate (DL-40S: manufactured by Nippon Shokubai), and 8 parts by weight (8 g) of crystalline cellulose (pore-forming agent, Ceolas (registered trademark) RC-591: manufactured by Asahi Kasei Chemicals) were measured and mixed for 5 minutes with a kneader (Hibismix: manufactured by Primix). 82 parts by weight (82 g) of water was added and kneaded until the kneaded product was consolidated. The obtained kneaded product was molded into a cylindrical shape with a diameter of 1.5 mm. It was then dried at 100°C for 12 hours or more and crushed into pieces of about 1 to 3 mm. It was then fired at 650°C for 3 hours to obtain a zeolite molded product (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite). 2 The results were: 1500, zeolite water adsorption amount 4 (g / 100g), clay solid acid amount: 0.009mmol / g, clay average particle size: 1.8μm. The compressive strength was 33N.
[0042] Comparative Example 1 MFI type zeolite powder (HSZ (registered trademark)-891HOA: manufactured by Tosoh Corporation (Si / Al 2100 parts by weight (103 g; moisture content 3%) of attapulgite clay (Minigel MB: Active Minerals) 20 parts by weight (25.5 g, moisture content 22%, solid acidity 0.197 mmol / g, average particle size 11.6 μm), 3 parts by weight (3 g) of sodium carboxymethylcellulose (molding aid, Cellogen: Daiichi Kogyo Seiyaku), and 1 part by weight (1 g) of sodium polyacrylate (DL-40S: Nippon Shokubai) were weighed out and mixed in a kneader (Hibismix: Primix) for 5 minutes. 94 parts by weight (94 g) of water were added and the kneaded material was kneaded until it was solidified. The obtained kneaded material was molded into a cylindrical shape with a diameter of 1.5 mm. It was then dried at 100 ° C for more than 12 hours and crushed to about 1 to 3 mm. Then, it was fired at 650°C for 3 hours to obtain a zeolite molded body (clay: 20 parts by weight per 100 parts by weight of zeolite, Si / Al ratio of zeolite: 1.0). 2 The results were: 1500, zeolite water adsorption amount 4 (g / 100g), clay solid acid amount: 0.197mmol / g, clay average particle size: 11.6μm. The compressive strength was 15N. [Industrial Applicability]
[0043] The high-strength zeolite molded body of the present invention can be effectively used in adsorption / separation applications without causing side reactions because the binder has a low acid content and has low reactivity with organic substances. Furthermore, because of its high strength, it is less likely to powder even when used in adsorption / separation, and is less likely to cause equipment failures.
Claims
1. A zeolite molded body containing 10 parts by weight or more and 40 parts by weight or less of clay relative to 100 parts by weight of zeolite and having a compressive strength of 20 N or more, wherein the zeolite is Si / Al 2 The clay contains one or more zeolites having a NH 3 A high-strength zeolite molded body, characterized in that it contains one or more clays having a solid acidity of 0.15 mmol / g or less by the TPD method and an average particle size of 0.5 μm or more and 30 μm or less.
2. 2. The high-strength zeolite molded article according to claim 1, wherein the zeolite is a ZSM-5 type zeolite.
3. 3. The high-strength zeolite molded article according to claim 1, wherein the clay is bentonite clay.
4. 4. The high-strength zeolite molded article according to claim 1, wherein the zeolite has a water adsorption amount of 5 (g / 100 g) or less under conditions of 25° C. and a relative pressure of 0.5.
Citation Information
Patent Citations
Oxidizing agent composition
JP1989120247A
Molding containing dealminized zeolite y, method for its production and adsorbing body consisting of said molding
JP1993138016A
Calcium x type zeolite forming product and its production
JP1998081511A
Molded product containing x-type zeolite, manufacture and use application thereof
JP2000210557A
Molded microporous material catalyst for manufacturing dialkanol amine
JP2001321673A