Removal of impurity in doped ald tantalum nitride

By forming a doped tantalum nitride layer and exposing it to helium or neon plasma, the method addresses the challenges of copper/ruthenium corrosion and in situ H nitride formation, improving the barrier properties and reliability of copper interconnects in semiconductor devices.

JP2024133454AActive Publication Date: 2024-10-02APPLIED MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024066962
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-06-28
Filing Date
2024-04-17
Publication Date
2024-10-02
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

The miniaturization of semiconductor circuit devices poses challenges in filling gaps between circuit elements due to the difficulty in forming barrier layers, particularly with ruthenium-doped tantalum nitride, which can cause copper/ruthenium corrosion and in situ H nitride formation during atomic layer deposition, leading to electromigration issues.

Method used

A method involving the formation of a doped tantalum nitride layer on a substrate, followed by exposure to helium or neon plasma to reduce dopant amounts and impurities, enhancing the barrier properties of copper interconnects by increasing etch selectivity and reducing carbon content.

Benefits of technology

The method improves the barrier properties of tantalum nitride films by reducing dopant levels and carbon impurities, thereby enhancing the reliability and integrity of copper interconnects in semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133454000001_ABST
    Figure 2024133454000001_ABST
Patent Text Reader

Abstract

To provide a method for forming a barrier layer for contact formation.SOLUTION: A treatment method forms a doped tantalum nitride layer 154 on a substrate 125, the doped tantalum nitride layer having a first dopant amount including one or more of ruthenium, tungsten, or cobalt. The substrate 125 has a surface on which a structure 135 is formed. The structure 135 extends certain distance into the substrate and has a sidewall and a bottom. The doped tantalum nitride layer 154 is exposed to a plasma containing one or more of helium and neon to form a treated doped tantalum nitride layer 154 that has a resistance lower than 600 μΩ cm and a second dopant amount lower than the first dopant amount. A metal film 156 is deposited on the treated doped tantalum nitride layer 154 to fill the structure 135.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE Embodiments of the present disclosure generally relate to methods of forming barrier layers, and more particularly, to methods of forming tantalum nitride barrier layers. [Background technology]

[0002] The miniaturization of semiconductor circuit elements has reached a point where feature sizes of 20 nm and below are being manufactured on a commercial scale. As the size of the critical dimensions continues to decrease, new challenges arise for process steps such as filling the gaps between circuit elements. As the width between elements continues to shrink, the gaps between elements often become taller and narrower, making it more difficult to fill the gaps and more difficult to make the contacts robust.

[0003] Ruthenium-doped tantalum nitride is being investigated as a copper barrier material for smaller node applications, but the integration of ruthenium-doped tantalum nitride into small features can result in copper / ruthenium corrosion due to, for example, copper electromigration in close proximity to the ruthenium, potentially resulting in disconnection.

[0004] Ruthenium (Ru) doped tantalum nitride (TaN) often contains high concentrations of carbon (C) that is not efficiently or easily removed by in situ H2 / Ar plasma during atomic layer deposition (ALD) tantalum nitride formation. Studies of ALD TaN densification in physical vapor deposition (PVD) chambers have shown that ALD TaN films can be densified by selectively removing nitrogen (N) in an Ar plasma treatment. Summary of the Invention [Problem to be solved by the invention]

[0005] Accordingly, there is a need for a method of forming a barrier layer for contact formation. [Means for solving the problem]

[0006] One or more embodiments of the present disclosure are directed to a method of forming an interconnect. A doped tantalum nitride layer is formed on a substrate. The doped tantalum nitride layer has a first dopant amount including one or more of ruthenium, tungsten, or cobalt. The doped tantalum nitride layer is exposed to a plasma including one or more of helium or neon to form a treated doped tantalum nitride layer having a second dopant amount less than the first dopant amount.

[0007] An additional embodiment of the present disclosure is directed to a cluster tool comprising one or more process chambers around a central transfer station. The one or more process chambers are configured to deposit a doped tantalum nitride film, anneal the doped tantalum nitride film, and expose the annealed doped tantalum nitride film to a plasma comprising one or more of helium or neon. At least one controller is connected to the one or more process chambers and the central transfer station. The at least one controller has one or more configurations selected from a configuration for depositing a tantalum nitride film, a configuration for depositing a dopant-containing film, a configuration for annealing a substrate, a configuration for moving a substrate between the one or more process chambers and the central transfer station, and a configuration for exposing a substrate to a neon plasma.

[0008] A further embodiment of the present disclosure is directed to a non-transitory computer-readable medium including instructions that, when executed by a controller of a processing chamber, cause the processing chamber to perform operations of depositing a tantalum nitride film on a substrate, depositing a dopant-containing film on the substrate, annealing the substrate, and exposing the substrate to a neon plasma.

[0009] So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure briefly summarized above can be obtained by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the present disclosure is open to other equally effective embodiments, and therefore, that the accompanying drawings only illustrate typical embodiments of the present disclosure and should not be considered as limiting the scope of the present disclosure. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic diagram of a substrate structure according to one or more embodiments of the present disclosure. [Diagram 2] 1 is a flow diagram of a method according to one or more embodiments of the present disclosure. [Figure 3A] FIG. 3 is a schematic diagram of an electronic device during the execution of the method of FIG. 2. [Figure 3B] FIG. 3 is a schematic diagram of an electronic device during the execution of the method of FIG. 2. [Figure 3C] FIG. 3 is a schematic diagram of an electronic device during the execution of the method of FIG. 2. [Figure 3D] FIG. 3 is a schematic diagram of an electronic device during the execution of the method of FIG. 2. [Figure 3E] FIG. 3 is a schematic diagram of an electronic device during the execution of the method of FIG. 2. [Figure 4] 1 is a schematic diagram of an electronic device according to one or more embodiments of the present disclosure. [Figure 5A] FIG. 3C is an enlarged view of region 5 of FIG. 3B according to one or more embodiments of the present disclosure. [Figure 5B] FIG. 3C is an enlarged view of region 5 of FIG. 3B according to one or more embodiments of the present disclosure. [Figure 6] 1 is a schematic diagram of a processing tool according to one or more embodiments of the present disclosure. [Figure 7] 1 is a schematic diagram of a processing tool according to one or more embodiments of the present disclosure. [Figure 8] FIG. 1 is a schematic diagram of a cluster tool according to one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Before describing certain exemplary embodiments of the present disclosure, it is to be understood that the present disclosure is not limited to the details of structure or process steps set forth in the following description as the present disclosure is capable of other embodiments and of being practiced or carried out in various ways.

[0012] As used herein and in the appended claims, the term "substrate" refers to a surface or a portion of a surface on which a process acts. Those skilled in the art will understand that a reference to a substrate may refer to only a portion of the substrate, unless the context clearly indicates otherwise. In addition, a reference to depositing on a substrate can refer to both a bare substrate and a substrate on which one or more films or features have been deposited or formed.

[0013] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment can be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), silicon oxide doped with carbon, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials, such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates can be exposed to pretreatment processes for polishing, etching, reducing, oxidizing, hydroxylating, annealing, UV curing, e-beam curing, and / or baking of the substrate surface. In addition to direct film treatment on the surface of the substrate itself, the present disclosure also provides for performing any of the disclosed film treatment steps on an underlayer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include such underlayers as the context dictates. Thus, for example, when a film / layer or partial film / layer is deposited onto a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.

[0014] One or more embodiments of the present disclosure advantageously provide a method for reducing ruthenium (Ru), tungsten (W), cobalt (Co), and / or carbon (C) in doped tantalum nitride (TaN) films. Some embodiments advantageously enhance the barrier properties of the films for copper (Cu) interconnects.

[0015] In some embodiments, a helium (He) or neon (Ne) plasma is used to reduce the etch rate of the TaN film. In some embodiments, the etch selectivity of nitrogen over tantalum is increased. Some embodiments provide additional process control by lowering the etch rate to increase the selectivity of the etch process. In some embodiments, a neon plasma treatment removes ruthenium from the TaN film, reducing the possibility of copper corrosion at the contacts. Some embodiments remove carbon impurities to improve film resistance. In some embodiments, the tantalum to nitrogen ratio is increased to improve barrier density.

[0016] FIG. 1 illustrates a structure used by one or more embodiments. The substrate 10 illustrated in FIG. 1 includes a material 15 (e.g., a dielectric) having a structure 20 formed on a surface 18 thereof. The structure 20 has a top 22, a bottom 26, and sides 24, 25. In the illustrated embodiment, the structure 20 is bounded by the material 15 at the bottom 26 and the sides 24, 25. In some embodiments, the bottom 26 of the structure 20 is bounded by a different material (not shown) than the sides 24, 25. For example, in some embodiments, the bottom 26 of the structure includes a conductive material and the sides 24, 25 include a dielectric. In some embodiments, the bottom 26 of the structure 20 includes a dielectric and the sides 24, 25 include a conductive material. In some embodiments, the bottom and sides are different materials, and both the bottom and sides are a dielectric or a conductive material.

[0017] The width W of the structure 20 is defined as the distance between the sides 24, 25. Those skilled in the art will appreciate that the structures shown are exemplary and that typical structures may not have square corners. The width of such a structure is measured as the average distance between the sidewalls measured parallel to the surface of the structure. The depth D of the structure is defined as the distance from the top 22 to the bottom 26 of the structure 20. The aspect ratio of the structure 20 is defined as the depth D:width W of the structure. In some embodiments, the aspect ratio is 5:1, 10:1, 15:1, 20:1, or 25:1 or greater.

[0018] In some embodiments, the material 15 comprises a dielectric. Suitable dielectrics include, but are not limited to, silicon oxide (SiO), silicon dioxide (SiO2), silicon nitride (SiN), silicon oxynitride (SiON), aluminum nitride (AlN), aluminum oxide (AlO), or high-k dielectric materials. In some embodiments, the material comprises a hard mask material (e.g., carbon (C)). As used herein and in the appended claims, unless otherwise specified by a subscript, chemical formulas represent elemental identities and are not intended to imply any particular stoichiometric ratio. For example, a titanium nitride (TiN) film can have any suitable combination of titanium and nitrogen atoms and is not limited to a single relationship.

[0019] Some embodiments of the method include depositing tantalum nitride, doped tantalum nitride, and tantalum nitride films by atomic layer deposition or chemical vapor deposition (CVD) processes. One or more embodiments of the method include sequentially depositing ruthenium-doped tantalum nitride, tantalum nitride, and ruthenium-doped tantalum nitride films by atomic layer deposition or chemical vapor deposition processes. In some embodiments, an in situ plasma is applied to reduce film impurities and incorporate doping layers into the TaN layer to improve barrier and / or adhesion properties.

[0020] In some embodiments, physical vapor deposition (PVD) processing with high density plasma and a biasable pedestal further improves one or more of the barrier performance, carbon, and / or ruthenium content without damaging the low-k dielectric.

[0021] In some embodiments, neon or helium plasma exposure increases the etch selectivity between tantalum and nitrogen (atomic selectivity). Some embodiments provide a way to control bevel damage (geometry selectivity). One or more embodiments reduce the deposition rate by about 30% or more, allowing for more process control. In some embodiments, an integrated hardware solution with a DC / RF coil process chamber is provided.

[0022] Figure 2 illustrates one embodiment of a method 100 for forming copper interconnects according to one or more embodiments of the present disclosure. Figures 3A-3E illustrate an electronic device 120 being processed using the method 100 of Figure 2. Those skilled in the art will appreciate that the illustrated embodiment is merely an exemplary embodiment, and that the present disclosure is not limited to the process shown.

[0023] 3A shows a substrate 125 having a first material 130 and a second material 132 forming a structure 135. The structure 135 shown is bounded by a surface 131 of the first material 130 at a sidewall 137 and by a top surface 133 of the second material 132 at a bottom 136.

[0024] The substrate 125, and any layers formed thereon, are exposed to one or more suitable deposition conditions in process 102 to form a doped (with ruthenium) tantalum nitride layer 140, as shown in FIG. 3B. The present disclosure will discuss these figures and refer to a film doped with ruthenium. However, the doped tantalum nitride layer 140 may be doped with ruthenium, tungsten, and / or cobalt. The present disclosure is not limited to films doped with ruthenium, and ruthenium may be replaced with or may further include tungsten and / or cobalt. FIGS. 5A and 5B show expanded views of region 5 of FIG. 3B in accordance with one or more embodiments of the present disclosure. Throughout this specification, references to "ruthenium" may be replaced with "cobalt" and / or "tungsten."

[0025] The first material 130 can be any suitable material or combination of materials. In some embodiments, the first material 130 comprises a dielectric. Suitable dielectrics include, but are not limited to, silicon oxide, silicon nitride, silicon oxynitride, low-k dielectrics (e.g., porous SiO 2 having a dielectric constant value of less than about 5). x or carbon-doped SiO x ). In some embodiments, the low-k dielectric comprises one or more of fluorine-doped silicon oxide, organosilicate glass, or porous silicon dioxide. In other embodiments, the dielectric layer is a multi-layer structure. For example, in one or more embodiments, the dielectric layer comprises a stack of an oxide layer and a nitride layer.

[0026] The doped tantalum nitride layer 140 of some embodiments includes a stack of multiple layers. In the embodiment shown in FIG. 2, FIG. 3B, and FIG. 5A, forming the doped tantalum nitride layer 140 is composed of a stack of a first tantalum nitride layer 142 formed by process 104, a dopant-containing layer 144 formed by process 106, and a second tantalum nitride layer 146 formed by process 108. The dopant of the dopant-containing layer 144 includes one or more of ruthenium, cobalt, or tungsten. Throughout this description, references to "ruthenium" can be replaced with "tungsten" and / or "cobalt." As used herein, dopant refers to ruthenium, cobalt, and / or tungsten. In some embodiments, forming the doped tantalum nitride layer includes forming a stack of tantalum nitride and dopant-containing layers by atomic layer deposition.

[0027] In some embodiments, the first tantalum nitride layer 142 is formed to a first layer thickness T1 (as shown in FIG. 5A) by any suitable deposition technique. In an exemplary embodiment, the tantalum nitride layer 142 is formed by atomic layer deposition to a first layer thickness in the range of 5 Å to 10 Å. In some embodiments, the first layer thickness is about 7 Å. In some embodiments, the first layer thickness is greater than or equal to 5 Å, 10 Å, 15 Å, or 20 Å and less than or equal to 40 Å, 35 Å, 30 Å, or 25 Å.

[0028] In some embodiments, atomic layer deposition of TaN includes sequential exposure of a tantalum precursor and a nitrogen reactant. The tantalum precursor can be any suitable tantalum species, including but not limited to pentakis(dimethylamino)tantalum (PDMAT), and the nitrogen reactant includes ammonia. Those skilled in the art will appreciate that the reaction with PDMAT and NH3 represents only one possible ALD reaction and should not be considered as limiting the scope of the present disclosure.

[0029] The temperature during formation of the tantalum nitride layer 142 can be any suitable temperature, depending, for example, on the reactants being used. In some embodiments, the substrate is maintained at a temperature in the range of 200°C to 350°C, or in the range of 225°C to 300°C, or in the range of 250°C to 275°C.

[0030] The dopant-containing layer 144 formed by process 106 can be any suitable material. In some embodiments, the dopant-containing layer 144 includes one or more of metallic ruthenium, metallic tungsten, or metallic cobalt. In some embodiments, the ruthenium-containing layer 144 consists essentially of one or more of metallic ruthenium, metallic tungsten, or metallic cobalt. When used in this manner, the term "consisting essentially of" means that the specified layer consists of 95%, 98%, 99%, or 99.5% or more of the recited species on an atomic basis.

[0031] In some embodiments, the dopant-containing layer 144 comprises tantalum nitride doped with one or more of ruthenium, tungsten, or cobalt. In some embodiments, the tantalum nitride doped with one or more of ruthenium, tungsten, or cobalt is formed by flash CVD. In some embodiments, the dopant-containing layer 144 is a thin conformal film deposited by CVD.

[0032] In some embodiments, the dopant-containing layer 144 has a pre-treatment thickness T in the range of 0.5 Å to 5 Å or in the range of about 1 Å to about 2 Å. R (See FIG. 5A). In some embodiments, the dopant-containing layer 144 is amorphous. In some embodiments, the dopant-containing layer 144 is substantially amorphous. When used in this manner, the term "substantially amorphous" means that greater than 90%, 95%, or 98% of the volume of the dopant-containing layer 144 is amorphous. In some embodiments, the dopant-containing layer 144 has a nanocrystalline structure.

[0033] In some embodiments, the dopant-containing layer is formed while the substrate is maintained at the same process temperature as during the formation of the first tantalum nitride layer 142.

[0034] The second tantalum nitride layer 146 deposited by process 108 in some embodiments is formed by the same process as the first tantalum nitride layer 142. In some embodiments, the second tantalum nitride layer 146 is formed by a process different from that of the first tantalum nitride layer 142. In some embodiments, the second tantalum nitride layer 146 is formed by ALD using PDMAT and ammonia. In some embodiments, the second tantalum nitride layer 146 is formed while the substrate is maintained at a temperature in the range of 200° C. to 350° C., or in the range of 225° C. to 300° C., or in the range of 250° C. to 275° C.

[0035] The thickness T2 (see FIG. 5A) of the second tantalum nitride layer 146 can be any suitable thickness. In some embodiments, the second thickness of the second tantalum nitride layer 146 is less than, equal to, or greater than the first thickness of the first tantalum nitride layer 142. In some embodiments, the second thickness of the second tantalum nitride layer 146 is in the range of 1 Å to 5 Å, or in the range of 2 Å to 4 Å, or about 3 Å. In some embodiments, the second thickness is 1 Å, 2 Å, 3 Å, 4 Å, or 5 Å or more and 10 Å, 9 Å, 8 Å, 7 Å, or 6 Å or less.

[0036] In some embodiments, the total thickness T of the doped tantalum nitride layer 140 is F (see FIG. 5A) is greater than 5 Å, 7.5 Å, 10 Å, 15 Å, or 20 Å. In an exemplary embodiment, the thickness of the doped (Ru, W, and / or Co) TaN layer 140 is in the range of about 10 Å to 15 Å or in the range of 11 Å to 12 Å.

[0037] In some embodiments, the doped tantalum nitride layer 140 includes at least one tantalum nitride layer and at least one dopant-containing layer. In some embodiments, the doped tantalum nitride layer 140 is deposited as a single layer. For example, in some embodiments, the tantalum nitride layer 140 is formed by ALD or CVD, where a dopant precursor is administered and reacted.

[0038] In some embodiments, after formation of the doped tantalum nitride layer 140 stack, the substrate is annealed in process 110. The stack of first tantalum nitride layer 142, dopant-containing layer 144, and second tantalum nitride layer 146 is annealed to form annealed doped tantalum nitride layer 150, as shown in Figure 3C. For illustrative purposes, dopant atoms 152 are marked as dots in these figures.

[0039] Annealing of the stack can be performed by any suitable technique known to those skilled in the art. In some embodiments, annealing is performed at temperatures of 300° C., 400° C., 500° C., 600° C., 700° C., 800° C., 900° C., or 1000° C. or higher. In some embodiments, annealing is performed in an atmosphere that includes one or more of an inert gas (e.g., molecular nitrogen (N2), argon (Ar)), a reducing gas (e.g., molecular hydrogen (H2) or ammonia (NH3)), or an oxidant (e.g., molecular oxygen (O2), ozone (O3), or a peroxide). Annealing can be performed for any suitable length of time. In some embodiments, the film is annealed for a predetermined time in the range of about 15 seconds to about 90 minutes or in the range of about 1 minute to about 60 minutes. In some embodiments, annealing the as-deposited film increases the density, decreases the resistivity, and / or increases the purity of the film.

[0040] In some embodiments, as shown in FIG. 3A, the structure 135 in the first material 130 has a bottom 136 and at least one sidewall 137. In some embodiments, the structure 135 is a circular via and has one cylindrical sidewall 137. In some embodiments, the structure 135 is a trench and has two or more sidewalls 137. In the exemplary embodiment shown, the doped tantalum nitride film 150 is a conformal film formed on the sidewalls and bottom of the structure. As used in this manner, a "conformal film" has a thickness that does not vary by more than 0.5%, 1%, 5%, 10%, or 15% relative to the average thickness. In some embodiments, each of the layers of the stack prior to annealing is a conformal film. In some embodiments, the first tantalum nitride layer 142 and the second tantalum nitride layer 146 are conformal films.

[0041] Referring back to method 100 of FIG. 2, annealed doped tantalum nitride layer 150 is exposed to a plasma in process 112 to form treated doped tantalum nitride layer 154. In some embodiments, annealed doped tantalum nitride layer 150 is an annealed ruthenium doped tantalum nitride layer, an annealed tungsten doped tantalum nitride layer, and / or an annealed cobalt doped tantalum nitride layer. In some embodiments, the plasma includes one or more of helium or neon. In some embodiments, the plasma includes neon. In some embodiments, the plasma includes helium.

[0042] As a result of the plasma exposure process 112, the treated doped tantalum nitride layer 154 has a reduced amount of dopant atoms 152 than the doped tantalum nitride layer 150. In some embodiments, as a result of the plasma exposure process 112, the treated ruthenium doped tantalum nitride layer has a reduced amount of ruthenium atoms than the ruthenium doped tantalum nitride layer. In some embodiments, as a result of the plasma exposure process 112, the treated tungsten doped tantalum nitride layer has a reduced amount of tungsten atoms than the tungsten doped tantalum nitride layer. In some embodiments, as a result of the plasma exposure process 112, the treated cobalt doped tantalum nitride layer has a reduced amount of cobalt atoms than the cobalt doped tantalum nitride layer.

[0043] The plasma exposure process 112 causes a decrease in the doping level from a first dopant amount before plasma exposure to a second dopant amount after plasma exposure that is less than the first dopant amount. In some embodiments, the plasma exposure process 112 causes a decrease in the ruthenium doping level from a first ruthenium amount before plasma exposure to a second ruthenium amount after plasma exposure that is less than the first ruthenium amount. In some embodiments, the plasma exposure process 112 causes a decrease in the tungsten doping level from a first tungsten amount before plasma exposure to a second tungsten amount after plasma exposure that is less than the first tungsten amount. In some embodiments, the plasma exposure process 112 causes a decrease in the cobalt doping level from a first cobalt amount before plasma exposure to a second cobalt amount after plasma exposure that is less than the first cobalt amount.

[0044] In some embodiments, as shown in Figures 5A and 5B, the doped tantalum nitride layer 140 is not annealed or maintains the structural appearance of the stack with different layers. Adjacent edges of the individual layers can be blurred from one another while maintaining the structural appearance of the stack. In the embodiment shown, the doped tantalum nitride layer 140 is exposed to a plasma containing one or more of helium or neon to form a processed doped tantalum nitride layer 154a having a striped layer structure.

[0045] The thickness T of the doped tantalum nitride layer 140 in some embodiments F is the treated thickness T as shown in Figure 5B. FT The processed thickness T FT Thickness T to F The reduction in the treated thickness T depends on a variety of factors, including, but not limited to, the length of plasma exposure, the power of the plasma exposure, the method of depositing the individual layers, and the composition of the individual layers. FT is the thickness before plasma exposure T F is less than 90%, 80%, 70%, or 60% of the

[0046] The thickness of the individual layers may be affected to different degrees by the plasma exposure. In some embodiments, the plasma exposure changes the thickness of the dopant-containing layer 144, but does not substantially change the thickness of the other layers. When used in this manner, the film thickness is not substantially changed if the thickness varies by less than ±5% of the pre-plasma thickness. In some embodiments, the thickness T1 of the first tantalum nitride layer 142 is approximately equal to the processed thickness T 1T The thickness T2 of the second tantalum nitride layer 146 is reduced to the processed thickness T 2T , and the thickness T R is the processed thickness T RT In some embodiments, the thickness T1 of the first tantalum nitride layer 142 decreases to a processed thickness T 1T tantalum nitride layer 146 is reduced to a processed thickness T2T or the thickness T of the dopant-containing layer 144. R is the processed thickness T RT In some embodiments, the thickness T of the dopant-containing layer 144 decreases to R is equal to or greater than 2 Å, 3 Å, or 4 Å and is less than 1 Å, 2 Å, 3 Å, or 4 Å; RT In some embodiments, the thickness T of the dopant-containing layer 144 is reduced to R is the processed thickness T greater than 2 Å, 3 Å, or 4 Å and less than 1 Å, 2 Å, 3 Å, or 4 Å RT is reduced to

[0047] 5A and 5B, as a result of the plasma exposure process 112, the treated doped tantalum nitride layer 154a has a reduced amount of dopant atoms than the doped tantalum nitride layer 150. The plasma exposure process 112 causes a decrease in the doping level from a first dopant amount before plasma exposure to a second dopant amount after plasma exposure that is less than the first dopant amount.

[0048] In some embodiments, the concentration of the dopant in the doped tantalum nitride layer 140 is in the range of 0.5-50 weight percent, or in the range of 1-45 weight percent, or in the range of 2-40 weight percent, or in the range of 3-35 weight percent, or in the range of 4-30 weight percent, or in the range of 5-25 weight percent of the total weight of the doped tantalum nitride layer 140. In some embodiments, the weight percentage of the dopant in the doped tantalum nitride layer 140 is reduced to an amount of 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10% or more and 50%, 45%, 40%, 35%, 30%, 25%, 20%, or 15% or less.

[0049] In one or more embodiments, after plasma exposure, the concentration of dopant in the treated doped tantalum nitride layer 154, 154a is reduced to an amount in the range of 0.05-20 wt %, or in the range of 0.1-15 wt %, or in the range of 0.2-10 wt %, or in the range of 0.3-8 wt %, or in the range of 0.4-6 wt %, or in the range of 0.5-5 wt % of the total mass of the treated doped tantalum nitride layer 154, 154a. In some embodiments, the mass percentage of dopant in the processed doped tantalum nitride layer 154, 154a is reduced to an amount of 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, or 5.0% or more and 20%, 17.5%, 15%, 12.5%, 10%, 9%, 8%, 7%, 6%, or 5% or less.

[0050] The resistivity of the doped tantalum nitride layer 154 is less than the resistivity of both thermal ALD TaN (without dopant) and doped thermal ALD TaN without helium or neon plasma exposure. In some embodiments, the resistivity of the doped tantalum nitride layer 150 is greater than or equal to 1000 μΩ·cm, 1100 μΩ·cm, 1200 μΩ·cm, 1300 μΩ·cm, 1400 μΩ·cm, 1500 μΩ·cm, or 1600 μΩ·cm. In some embodiments, the resistivity of the treated doped tantalum nitride layer 154 is less than or equal to 1000 μΩ·cm, 900 μΩ·cm, 800 μΩ·cm, 700 μΩ·cm, 600 μΩ·cm, or 500 μΩ·cm. In some embodiments, the helium and / or neon plasma exposure reduces the resistivity of the doped tantalum nitride layer 150 to less than 60%, 50%, 40%, or 30% of its pre-plasma (pre-treatment) amount. For example, in an exemplary process, the resistivity of the doped tantalum nitride film 150 is reduced from about 1700 μΩ·cm to about 500 μΩ·cm by exposure to a neon plasma.

[0051] In some embodiments, the doped tantalum nitride film has a pre-plasma carbon content and a post-plasma carbon content. In some embodiments, exposure to a helium or neon plasma reduces the pre-plasma carbon content to a post-plasma carbon content. In some embodiments, the pre-plasma carbon content of the doped tantalum nitride film 150 is greater than 0.8% on an atomic basis. In some embodiments, the post-plasma carbon content of the doped tantalum nitride film 154 is less than 0.6%, 0.5%, or 0.4% on an atomic basis. In some embodiments, exposure to a helium or neon plasma reduces the carbon content in the doped tantalum nitride film by 25%, 30%, 35%, 40%, 45%, or 50% or more.

[0052] The plasma can be any suitable plasma. In some embodiments, the helium or neon plasma is an inductively coupled plasma (ICP) and is generated by an ICP coil. ICP coils can operate at lower pressures with higher plasma densities. In some embodiments, the plasma density of the inductively coupled plasma is about 10 11 cm -3 , 10 12 cm -3 , or 10 13 cm -3or greater, or an order of magnitude greater than or equal to the stated order. In some embodiments, the plasma generated by the ICP coil has a frequency of 2 MHz. In some embodiments, RF source power of about 500 Watts to about 25 kW can be provided at a frequency of about 400 kHz to about 60 MHz. RF bias power of up to about 3000 Watts can be applied to the substrate support at a frequency of 13.56 MHz or 2 MHz. In some embodiments, RF source power of about 100 Watts to about 3000 Watts can be provided to the gas mixture at a frequency of about 400 kHz to about 60 MHz. In certain cases, dual or triple frequencies can be used to modulate the ion energy. DC bias power of about 1 kW to about 10 kW can be applied to the collimator in pulsed mode. Alternatively, DC bias power can be applied to the collimator in continuous mode. In some embodiments, the plasma pressure is in the range of 0.1 mTorr to 100 mTorr. In some embodiments, the substrate is maintained at a temperature in the range of -20°C to 400°C.

[0053] Referring back to method 100 of Figure 2, in some embodiments, process 114 deposits a metal film 156 on the treated tantalum nitride layer 154 to fill the structure, as shown in Figure 3E. In some embodiments, metal film 156 is a metal contact. In some embodiments, metal film 156 includes or consists essentially of one or more of copper (Cu), cobalt (Co), or copper doped with one or more of manganese (Mn), tungsten (W), or aluminum (Al).

[0054] The metal film 156 may be deposited by any suitable technique known to those of skill in the art, in some embodiments, the metal film 156 is deposited by atomic layer deposition, chemical vapor deposition, or physical vapor deposition.

[0055] 4 illustrates another electronic device 120 according to one or more embodiments of the present disclosure. The structure 135 of FIG. 4 is bounded on the sides by a first material 130 and on the bottom by a second material 132. In some embodiments, the first material 130 comprises a dielectric and the second material 132 comprises a conductive material. In some embodiments, the conductive material comprises a copper layer. In some embodiments, the first material 130 comprises a low-k dielectric material.

[0056] In some embodiments, the doped tantalum nitride film 150 is deposited as a conformal film having a first amount of dopant. In the embodiment shown, the substrate 125 is biased to form a directional plasma during the plasma exposure process 112. Biasing the substrate 125 causes ions in the neon plasma to move toward the substrate surface, resulting in a different removal pattern for the dopant atoms 152 than would be observed if no bias was applied to the substrate.

[0057] 4, the directional plasma removes dopant 152 from the tantalum nitride at the bottom 157 of the structure 135, leaving substantially all of the dopant in the tantalum nitride on the sidewalls 158. When used in this manner, the term "substantially all" means that about 85%, 90%, 95%, or more of the original dopant atoms in the sidewalls of the tantalum nitride film remain below the top surface of the first material 130. In the embodiment shown, dopant is also removed from the tantalum nitride top portion 155 of the conformal film.

[0058] A variety of hardware configurations can be used to implement the method 100. In some embodiments, the deposition, plasma exposure, and annealing of the tantalum nitride film are performed in the same process chamber. In some embodiments, the deposition, annealing, and plasma exposure are performed in separate process chambers.

[0059] 6 shows a schematic cross-sectional view of an exemplary processing chamber 200 (e.g., a PVD chamber) according to some embodiments of the present disclosure. Examples of suitable PVD chambers include ENCORE® II and ENCORE® III, available from Applied Materials, Inc., Santa Clara, Calif., as well as other PVD processing chambers. However, the disclosed methods can be used with processing chambers available from other manufacturers. In one embodiment, the process chamber 200 is capable of depositing, for example, metals, metal nitrides, metal fluorides, metal carbides, etc., on a substrate 218.

[0060] The process chamber 200 has a chamber body 205 that includes sidewalls 202, a bottom 203, and a lid assembly 204, all of which enclose an interior volume 206. A substrate support 208 is disposed at a lower portion of the interior volume 206 of the process chamber 200 opposite the target 214. A substrate transfer port 209 is formed in the sidewalls 202 for transferring a substrate into and out of the interior volume 206.

[0061] A gas source 210 is coupled to the process chamber 200 to supply a process gas into the interior volume 206. In one embodiment, the process gas may include an inert gas, a non-reactive gas, and a reactive gas, etc. Examples of process gases that may be provided by the gas source 210 include, but are not limited to, argon gas (Ar), helium (He), neon gas (Ne), nitrogen gas (N2), oxygen gas (O2), hydrogen gas (H2), and H2O, among others.

[0062] A pump 212 is coupled to the process chamber 200 in communication with the interior volume 206 for controlling the pressure of the interior volume 206. In one embodiment, the pressure of the process chamber 200 may be maintained at greater than 0 to about 10 millitorr or less. In another embodiment, the pressure in the process chamber 200 may be maintained at about 3 millitorr.

[0063] A backing plate 213 may support a target 214 on top of the interior volume 206. The backing plate 213 may be electrically insulated from the sidewall 202 by an insulator 215. The target 214 generally provides a source of material to be deposited on a substrate 218. The target 214 may be made from materials containing titanium (Ti) metal, tantalum metal (Ta), niobium (Nb) metal, tungsten (W) metal, cobalt (Co), nickel (Ni), copper (Cu), aluminum (Al), manganese (Mn), alloys thereof, combinations thereof, and the like. In the exemplary embodiment shown herein, the target 214 may be made from cobalt metal (Co).

[0064] The target 214 may be coupled to a source assembly 216 that includes a power supply 217 for the target 214. In some embodiments, the power supply 217 may be an RF generator. In some embodiments, the power supply 217 may alternatively be a DC source power supply. In some embodiments, the power supply 217 may include both a DC power source and an RF power source.

[0065] An additional RF power source 280 may also be coupled to the process chamber 200 through the substrate support 208 to provide bias power between the target 214 and the substrate support 208. In one embodiment, the RF power source 280 may provide power to the substrate support 208 to bias the substrate 218 at a frequency between about 1 MHz and about 100 MHz, for example about 13.56 MHz.

[0066] The substrate support 208 may be movable between an elevated position and a lowered position, as indicated by arrow 282. In the lowered position, a support surface 211 of the substrate support 208 may be aligned with or just below the substrate transfer port 209 to facilitate loading and unloading of the substrate 218 into and from the process chamber 200. The support surface 211 may have an edge deposition ring 236 sized to receive the substrate 218 while protecting the substrate support 208 from the plasma and deposition material. To process the substrate 218 in the process chamber 200, the substrate support 208 may be moved to an elevated position closer to the target 214. When the substrate support 208 is in the elevated position, a cover ring 226 may engage the edge deposition ring 236. The cover ring 226 may prevent deposition material from bridging between the substrate 218 and the substrate support 208. When the substrate support 208 is in the lowered position, the cover ring 226 floats above the substrate support 208 and the substrate 218 positioned thereon to allow for transfer of the substrate.

[0067] During transfer of a substrate to or from the process chamber 200, a robot blade (not shown) carrying a substrate 218 is extended through the substrate transfer port 209. Lift pins (not shown) extend through the support surface 211 of the substrate support 208 to lift the substrate 218 off of the support surface 211 of the substrate support 208, thus providing space for the robot blade to pass between the substrate 218 and the substrate support 208. The robot can then transport the substrate 218 through the substrate transfer port 209 into or out of the process chamber 200. The raising and lowering of the substrate support 208 and / or the lift pins can be controlled by a controller 298.

[0068] During sputter deposition, the temperature of the substrate 218 can be controlled by utilizing a thermal controller 238 disposed within the substrate support 208. The substrate 218 can be optionally heated to a desired temperature for processing. In some embodiments, optional heating can be used to bring the temperature of the substrate and / or film to a temperature of about 200 to about 400 degrees Celsius. In other embodiments, the substrate can be processed at room temperature (about 15 degrees Celsius to about 30 degrees Celsius). In other embodiments, the temperature is within the range of about 15 degrees Celsius to about 400 degrees Celsius. After processing, the substrate 218 can be rapidly cooled by utilizing a thermal controller 238 disposed within the substrate support 208. The thermal controller 238 controls the temperature of the substrate 218, and the thermal controller 238 can be used to change the temperature of the substrate 218 from a first temperature to a second temperature in a few seconds to about a minute.

[0069] An inner shield 220 may be positioned within the interior volume 206 between the target 214 and the substrate support 208. The inner shield 220 may be formed from aluminum or stainless steel, among others. In one embodiment, the inner shield 220 is formed from stainless steel. An outer shield 222 may be formed between the inner shield 220 and the sidewall 202. The outer shield 222 may be formed from aluminum or stainless steel, among others. The outer shield 222 may extend beyond the inner shield 220 and is configured to support a cover ring 226 when the substrate support 208 is in a lowered position.

[0070] In one embodiment, the inner shield 220 includes a radial flange 223 that includes an inner diameter that is greater than the outer diameter of the inner shield 220. The radial flange 223 extends from the inner shield 220 at an angle greater than about ninety degrees (90°) relative to an inner diameter surface of the inner shield 220. The radial flange 223 may be a circular ridge extending from a surface of the inner shield 220 and is generally adapted to fit into a recess formed in a cover ring 226 disposed on the substrate support 208. The recess may be a circular groove formed in the cover ring 226 that centrally aligns the cover ring 226 with respect to a longitudinal axis of the substrate support 208.

[0071] In some embodiments, the process chamber 200 may include an inductive coil 242. The inductive coil 242 of the process chamber 200 may have one or more turns. The inductive coil 242 may be located just inside the inner shield 220 and may be positioned above the substrate support 208. The inductive coil 242 may be positioned closer to the substrate support 208 than the target 214. The inductive coil 242 may be formed from a material of similar or equal composition to the target 214, such as cobalt, to act as a secondary sputtering target. The inductive coil 242 is supported from the inner shield 220 by a number of coil spacers 240. The coil spacers 240 may electrically insulate the inductive coil 242 from the inner shield 220 and other chamber components to protect it from sputtering in order to avoid shorting or creating an undesirable plasma excitation source.

[0072] The inductive coil 242 can be coupled to a power source 250. The power source 250 can have electrical leads that pass through the sidewall 202, the outer shield 222, the inner shield 220, and the coil spacer 240 of the process chamber 200. The electrical leads connect to an electrical hub 244 on the inductive coil 242 to provide electrical power to the inductive coil 242. The electrical hub 244 can have multiple insulated electrical connections to provide electrical power to the inductive coil 242. Additionally, the electrical hub 244 can be configured to support the inductive coil 242 in conjunction with the coil spacer 240. In one embodiment, the power source 250 applies a current to the inductive coil 242 to induce an RF field in the process chamber 200 and couple power to the plasma to increase the plasma density, i.e., the concentration of reactive ions. In some embodiments, the inductive coil 242 operates at an RF power frequency that is less than the RF power frequency of the RF power source 280. In one embodiment, the RF power frequency provided to the inductive coil 242 is about 2 MHz. In other embodiments, the RF power frequency can operate within a range of about 1.8 MHz to about 2.2 MHz. In other embodiments, the RF power frequency can range from about 0.1 MHz to 99 MHz. In some embodiments, the induction coil 242 is made from a material, such as a metallic material, that can be sputtered onto a substrate. The power supply 250 can then also apply DC power to the induction coil 242 while coupling RF power to the plasma to enable sputtering of the induction coil 242.

[0073] A controller (not shown) is coupled to the process chamber 200. The controller includes a central processing unit (CPU), memory, and supporting circuits. The controller is utilized to control the process sequence, regulate the gas flow from the gas source 210 into the process chamber 200, and control the ion bombardment of the target 214 and the inductive coil 242. In one embodiment, the controller adjusts a first RF power level of the first power supply (e.g., RF power supply 280), a second RF power level of the second power supply (e.g., power supply 250), a first DC power level of the second power supply (e.g., power supply 250), and a second DC power level of the third power supply (e.g., power supply 217), while sputtering the target and / or the inductive coil and regulating the flow of etching gas into the interior volume 206 of the process chamber 200. Additional aspects of the controller are described below.

[0074] FIG. 7 illustrates a processing tool 300 according to one or more embodiments. In one or more embodiments, the processing tool 300 comprises a processing chamber 301. The processing chamber comprises a lid 302 and at least one sidewall 304. In one or more embodiments, the lid 302 and at least one sidewall 304 define an interior volume 305 of the processing chamber 301. In one or more embodiments, the processing tool 300 comprises a remote plasma unit 306 within the interior volume 305 of the processing chamber 301. In one or more embodiments, a direct plasma unit 308 is located within the interior volume 305 of the processing chamber 301. In one or more embodiments, one of the remote plasma unit 306 generating a remote plasma and the direct plasma unit 308 generating a direct plasma occurs. In one or more embodiments, the remote plasma generation and the direct plasma generation occur sequentially. In some embodiments, the remote plasma generation occurs first, followed by the direct plasma generation. In other embodiments, the direct plasma generation occurs first, followed by the remote plasma generation. In one or more embodiments, the remote plasma generation and the direct plasma generation occur simultaneously.

[0075] In one or more embodiments, an ion filter 312 separates the remote plasma unit 306 and the direct plasma unit 308. In one or more embodiments, the ion filter 312 is used to filter ions from the plasma effluent during passage from the remote plasma unit 306 to the substrate processing region 315. In one or more embodiments, the ion filter 312 functions to reduce or remove ionically charged species traveling from the remote plasma unit 306 to the substrate 330. In one or more embodiments, uncharged neutral and radical species can pass through at least one aperture 318 in the ion filter 312 to react at the substrate 330. It should be noted that complete removal of ionically charged species in the reaction region 315 surrounding the substrate 330 is not always a desired goal. In one or more embodiments, ionic species are required to reach the substrate 330 to perform the etching and / or deposition process. In these examples, the ion filter 312 helps to control the concentration of ionic species in the reaction region 315 at a level useful for the treatment / cleaning and / or deposition process. In one or more embodiments, the ion filter 312 comprises a showerhead.

[0076] In one or more embodiments, the processing tool includes at least one electrode in the processing chamber. In one or more embodiments, the at least one electrode is disposed in the interior volume 305 of the processing chamber 301. In the embodiment shown in FIG. 6, the at least one electrode 316 is positioned in electrical communication with the pedestal 314.

[0077] In one or more embodiments, the processing chamber 301 includes a pedestal 314. In one or more embodiments, the pedestal 314 is configured to support a semiconductor substrate 330 in the processing region 315. In one or more embodiments, the pedestal 314 can have heat exchange channels (not shown) through which a heat exchange fluid flows to control the temperature of the substrate 330. In one or more embodiments, the temperature of the substrate 330 can be cooled or heated to maintain a relatively low temperature, such as between about -20°C and about 400°C, or between about 0°C and about 400°C. In one or more embodiments, the heat exchange fluid includes one or more of ethylene glycol or water. In other embodiments, the pedestal 314 is resistively heated to achieve a relatively high temperature, such as between about 100°C and about 1100°C, or between about 200°C and about 750°C, by use of an embedded resistive heating element (not shown). In one or more embodiments, the pedestal 314 is configured to rotate. In one or more embodiments, the pedestal 314 includes an electrode 316 therein, which is powered by an RF generator 350 and matched by an RF matcher 340. In one or more embodiments, the pedestal 314 is constructed from a metallic material and is itself an electrode. The electrode 316 can be polarized to bias the substrate or substrate support to form a directional plasma.

[0078] In one or more embodiments, at least one power source, such as an RF generator 350 , is electrically connected to the processing chamber 301 through an RF match 340 .

[0079] In one or more embodiments, two RF generators are electrically connected to the processing chamber 301. In such embodiments, a first RF generator 350 is electrically connected to the pedestal electrode 316 and a second RF generator 355 is electrically connected to an inductively coupled plasma (ICP) coil 370.

[0080] In one or more embodiments, the plasma is generated using radio frequency (RF) power remote plasma unit 306 and direct plasma unit 308. In one or more embodiments, alternating current (AC) power is rectified and switched to provide current to the RF amplifier. The RF amplifier operates at a reference frequency (e.g., 13.56 MHz) and drives a current that passes through an output matching network and then through a power measurement circuit to the output of the power supply. The output matching is typically designed to connect to a generator optimized to drive a specific impedance, e.g., 50 Ω, to have the same characteristic impedance as a coaxial cable commonly used in the industry. The power flow through the matched cable section is measured by a match controller and converted by a load matcher. Typically, the load matcher is an electronic auto-tuner, and therefore the load matching operation incurs a certain time delay until the system is properly configured. After passing through the load matcher, the power then enters a plasma excitation circuit that drives two electrodes in the exhaust treatment chamber. When treatment gas is introduced into the exhaust treatment chamber and driven by this circuit, a plasma is generated. Because the matching network or load matcher is electrically powered, the response time from the matching network is typically about 1 second or longer.

[0081] In some embodiments, the plasma power is in the range of about 10 W to about 1000 W, including about 200 W to about 600 W. In some embodiments, the plasma power is about 1000 W or less, or about 6500 W or less.

[0082] The plasma frequency can be any suitable frequency. In some embodiments, the plasma has a frequency in the range of about 200 kHz to 30 MHz. In some embodiments, the plasma frequency is about 20 MHz or less, about 10 MHz or less, about 5 MHz or less, about 1000 kHz or less, or about 500 kHz or less. In some embodiments, the plasma frequency is about 210 kHz or more, about 250 kHz or more, about 600 kHz or more, about 750 MHz or more, about 1200 kHz or more, about 2 MHz or more, about 4 MHz or more, about 7 MHz or more, about 12 MHz or more, about 15 MHz or more, or about 25 MHz or more. In one or more embodiments, the plasma has a frequency of about 13.56 MHz, or about 350 kHz, or about 400 kHz, or about 27 MHz, or about 40 MHz, or about 60 MHz.

[0083] In one or more embodiments, a controller 320 can be provided and coupled to various components of the processing tool 300 to control their operation. The controller 320 can be a single controller that controls the entire processing tool 300, or can be multiple controllers that control individual portions of the processing tool 300. For example, the processing tool 300 can include separate controllers for each of the processing chamber 301, the remote plasma unit 306, the direct plasma unit 308, and the power sources (e.g., RF generator 350).

[0084] In some embodiments, the process chamber 301 further comprises a controller 320. In one or more embodiments, the controller 320 controls the ignition of plasma by the remote plasma unit 306 and / or the direct plasma unit 308 in the process chamber 301.

[0085] In some embodiments, the controller 320 includes a central processing unit (CPU) 322, memory 324, input / output (I / O) 326, and support circuits 328. The controller 320 may control the processing tool 300 directly or via computers (or controllers) associated with particular process chambers and / or support system components.

[0086] The controller 320 can be one of any form of general-purpose computer processor that can be used in an industrial environment to control various chambers and sub-processors. The memory 324 or computer readable medium of the controller 320 can be one or more of readily available memories, such as non-transitory memory (e.g., random access memory (RAM)), read-only memory (ROM), floppy disk, hard disk, optical storage medium (e.g., compact disk or digital video disk), flash drive, or any other form of digital storage, local or remote. The memory 324 can hold a set of instructions operable by the processor (CPU 322) to control parameters and components of the processing tool 300.

[0087] The support circuits 328 are coupled to the CPU 322 to conventionally support the processor. These circuits include cache, power supplies, clock circuits, input / output circuits and subsystems, etc. One or more processes may be stored in the memory 324 as software routines that, when executed or invoked by the processor, cause the processor to control the operation of the processing tool 300 or individual processing units (e.g., the remote plasma unit 306 and the direct plasma unit 308) as described herein. The software routines may also be stored and / or executed by a second CPU (not shown) located remotely from the hardware being controlled by the CPU 322.

[0088] Some or all of the processes and methods of the present disclosure may also be performed in hardware. Thus, the processes may be implemented in software and executed using a computer system in hardware, for example as an application specific integrated circuit or other type of hardware implementation, or as a combination of software and hardware. The software routines, when executed by a processor, transform a general purpose computer into a special purpose computer (controller) that controls the chamber operation so that the processes are performed.

[0089] In some embodiments, the controller 320 has one or more configurations for executing individual processes or sub-processes to perform the method. The controller 320 can be connected to intermediate components and configured to operate the intermediate components to perform the functions of the method. For example, the controller 320 can be connected to and configured to control one or more of the remote plasma unit 306, the direct plasma unit 308, the pedestal 314, the at least one electrode 316, the ICP coil 370, or other components.

[0090] Additional embodiments of the present disclosure are directed to a processing system having one or more processing chambers, hi one or more embodiments, the processing chambers include the processing tools of FIG.

[0091] An additional embodiment of the present disclosure is directed to a processing tool and described methods for the formation of memory devices, as shown in Figure 7. The cluster tool 900 includes at least one central transfer station 921, 931 having multiple sides. A robot 925, 935 is positioned within the central transfer station 921, 931 and configured to move the robot blade and wafer to each of the multiple sides.

[0092] The cluster tool 900 comprises a number of processing chambers, also referred to as process stations, 902, 904, 906, 908, 910, 912, 914, 916, and 918, connected to a central transfer station. The various processing chambers provide separate processing regions isolated from adjacent process stations. The processing chambers can be any suitable chambers, including, but not limited to, pre-clean chambers, buffer chambers, transfer spaces, wafer orientation / degassing chambers, cryogenic cooling chambers, deposition chambers, annealing chambers, etch chambers, selective etch chambers, and the like. The particular arrangement of process chambers and components can vary depending on the cluster tool and should not be considered limiting to the scope of the present disclosure.

[0093] 8, a factory interface 950 is connected to the front of the cluster tool 900. The factory interface 950 includes a loading chamber 954 and an unloading chamber 956 at the front 951 of the factory interface 950. Although the loading chamber 954 is shown on the left and the unloading chamber 956 is shown on the right, one of ordinary skill in the art will understand that this represents only one possible configuration.

[0094] The size and shape of the loading chamber 954 and the unloading chamber 956 can vary depending on, for example, the substrate being processed in the cluster tool 900. In the embodiment shown, the loading chamber 954 and the unloading chamber 956 are sized to hold a wafer cassette with multiple wafers positioned within the cassette.

[0095] A robot 952 is located within the factory interface 950 and can move between a loading chamber 954 and an unloading chamber 956. The robot 952 can transfer wafers from a cassette in the loading chamber 954 through the factory interface 950 to a load lock chamber 960. The robot 952 can also transfer wafers from the load lock chamber 962 through the factory interface 950 to a cassette in the unloading chamber 956. As will be appreciated by those skilled in the art, the factory interface 950 can have more than one robot 952. For example, the factory interface 950 can have a first robot that transfers wafers between the loading chamber 954 and the load lock chamber 960 and a second robot that transfers wafers between the load lock chamber 962 and the unloading chamber 956.

[0096] The illustrated cluster tool 900 has a first section 920 and a second section 930. The first section 920 is connected to a factory interface 950 via load lock chambers 960, 962. The first section 920 includes a first transfer chamber 921 in which at least one robot 925 is positioned. The robot 925 is also referred to as a robotic wafer transport mechanism. The first transfer chamber 921 is centrally located relative to the load lock chambers 960, 962, the process chambers 902, 904, 916, 918, and the buffer chambers 922, 924. The robot 925 in some embodiments is a multi-arm robot capable of independently moving two or more wafers at a time. In some embodiments, the first transfer chamber 921 includes two or more robotic wafer transfer mechanisms. The robot 925 in the first transfer chamber 921 is configured to move wafers between chambers around the first transfer chamber 921. Individual wafers are transported on a wafer transport blade located at the distal end of the first robotic mechanism.

[0097] After processing the wafer in the first zone 920, the wafer can be moved through a pass-through chamber to the second zone 930. For example, the chambers 922, 924 can be one-way or two-way pass-through chambers. The pass-through chambers 922, 924 can be used, for example, to cryogenically cool the wafer before processing in the second zone 930 or to allow for cooling or post-processing of the wafer before returning to the first zone 920.

[0098] A system controller 990 is in communication with the first robot 925, the second robot 935, the first plurality of processing chambers 902, 904, 916, 918, and the second plurality of processing chambers 906, 908, 910, 912, 914. The system controller 990 can be any suitable component capable of controlling the processing chambers and robots. For example, the system controller 990 can be a computer including a central processing unit (CPU), memory, suitable circuitry, and storage.

[0099] Accordingly, one or more embodiments of the present disclosure are directed to a cluster tool comprising one or more process chambers around a central transfer station. The one or more process chambers of some embodiments are configured to deposit a tantalum nitride film doped with ruthenium, anneal the tantalum nitride film doped with ruthenium, and expose the annealed tantalum nitride film to neon plasma. At least one controller is connected to the one or more process chambers and the central transfer station. The at least one controller of some embodiments has one or more configurations selected from a configuration for depositing a tantalum nitride film, a configuration for depositing a ruthenium-containing film, a configuration for annealing a substrate, a configuration for moving a substrate between the one or more process chambers and the central transfer station, and a configuration for exposing a substrate to neon plasma.

[0100] Generally, the processes can be stored as software routines in the memory of the system controller 990, which, when executed by the processor, cause the process chamber to perform the processes of the present disclosure. The software routines can also be stored and / or executed by a second processor (not shown) located remotely from the hardware being controlled by the processor. Some or all of the methods of the present disclosure can also be performed in hardware. Thus, the processes can be implemented in software and executed using a computer system in hardware, for example as an application specific integrated circuit or other type of hardware implementation, or as a combination of software and hardware. The software routines, when executed by the processor, transform a general-purpose computer into a special-purpose computer (controller) that controls the chamber operation so that the processes are performed.

[0101] An additional embodiment of the present disclosure is directed to a non-transitory computer-readable medium including instructions that, when executed by a controller of a processing chamber, cause the processing chamber to perform operations of depositing a tantalum nitride film on a substrate, depositing a ruthenium-containing film on a substrate, annealing the substrate, and exposing the substrate to a neon plasma.

[0102] One or more embodiments are directed to a non-transitory computer-readable medium including instructions that, when executed by a controller of a processing chamber, cause the processing chamber to perform an operation of exposing a substrate including a surface structure having a metal bottom, a dielectric sidewall, and a dielectric region to a dual plasma treatment in the processing chamber to remove chemical residues and / or impurities from the metal bottom, the dielectric sidewall, and / or the dielectric region and / or repair surface defects of the dielectric sidewall and / or the dielectric region, the dual plasma treatment including a direct plasma followed by a remote plasma.

[0103] Spatially relative terms such as "beneath," "below," "lower," "above," and "upper" may be used herein to describe the relationship of one element or feature shown in the figures to another element or feature for ease of description. It will be understood that these spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation shown in the figures. For example, if the device in the figures were turned over, elements described as being "below" or "beneath" other elements or features would be oriented "above" the other elements or features. Thus, the exemplary term "below" can encompass both an upper and lower orientation. The device can be oriented in other ways (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein can be interpreted accordingly.

[0104] Throughout this specification, a reference to "one embodiment," "a particular embodiment," "one or more embodiments," or "an embodiment" means that a particular feature, structure, material, or characteristic described in connection with that embodiment is included in at least one embodiment of the disclosure. Thus, the appearances of phrases such as "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification do not necessarily refer to the same embodiment of the disclosure. Furthermore, in one or more embodiments, the particular features, structures, materials, or characteristics may be combined in any suitable manner.

[0105] Although the disclosure herein has been described with reference to specific embodiments, those skilled in the art will recognize that the described embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the disclosure. Thus, the disclosure may include modifications and variations that come within the scope of the appended claims and their equivalents.

Claims

1. 1. A method of forming an interconnect, comprising: forming a doped tantalum nitride layer on a substrate having a first dopant amount including one or more of ruthenium, tungsten, or cobalt; and exposing the doped tantalum nitride layer to a plasma comprising one or more of helium or neon to form a treated doped tantalum nitride layer having a second dopant amount less than the first dopant amount.

2. The method of claim 1 , wherein the first dopant amount is in the range of 0.5 to 50 weight percent of the doped tantalum nitride layer.

3. 3. The method of claim 2, wherein the second dopant amount is reduced from the first dopant amount and is in the range of 0.05 to 20 weight percent of the treated doped tantalum nitride layer.

4. 10. The method of claim 1, wherein forming the doped tantalum nitride layer comprises forming a stack of tantalum nitride and a dopant-containing layer by atomic layer deposition and then annealing the stack.

5. 2. The method of claim 1, wherein the doped tantalum nitride layer has a resistivity greater than 1200 μΩ·cm.

6. 2. The method of claim 1, wherein the treated doped tantalum nitride layer has a resistivity of less than 600 μΩ·cm.

7. The method of claim 1 , wherein the doped tantalum nitride has a carbon content of greater than 0.8% on an atomic basis.

8. The method of claim 7 , wherein the treated doped tantalum nitride layer has a carbon content of less than 0.6% on an atomic basis.

9. The method of claim 1 , wherein the plasma is an inductively coupled plasma and is generated by an ICP coil.

10. The method of claim 9 , wherein the plasma generated by the ICP coil has a frequency of 2 MHz.

11. The method of claim 1 , wherein the substrate is biased to produce a directional plasma.

12. 10. The method of claim 1, further comprising depositing a metal contact on the treated doped tantalum nitride layer.

13. The method of claim 12 , wherein the metal contacts comprise one or more of copper, cobalt, or copper doped with one or more of manganese, tungsten, or aluminum.

14. 10. The method of claim 1, wherein the substrate has a surface on which a structure is formed, the structure extending a distance into the substrate and having sidewalls and a bottom, the bottom comprising a copper layer.

15. The method of claim 14 , wherein the sidewalls of the structure comprise a low-k dielectric material.

16. 16. The method of claim 15, wherein the low-k dielectric material comprises one or more of fluorine-doped silicon oxide, organosilicate glass, or porous silicon dioxide.

17. 17. The method of claim 16, wherein the doped tantalum nitride layer is a conformal film formed on the sidewalls and bottom of the structure.

18. 20. The method of claim 17, wherein the substrate is biased to form a directional plasma that removes the dopant from the tantalum nitride on the bottom of the structure and leaves substantially all of the dopant in the tantalum nitride on the sidewalls.

19. one or more process chambers about a central transfer station configured to deposit a doped tantalum nitride film, anneal the doped tantalum nitride film, and expose the annealed doped tantalum nitride film to a plasma comprising one or more of helium or neon; at least one controller connected to the one or more process chambers and a central transfer station, the at least one controller having one or more configurations selected from a configuration for depositing a tantalum nitride film, a configuration for depositing a dopant-containing film, a configuration for annealing a substrate, a configuration for moving the substrate between the one or more process chambers and a central transfer station, and a configuration for exposing the substrate to a neon plasma; A cluster tool comprising:

20. A non-transitory computer readable medium containing instructions that, when executed by a controller of a processing chamber, depositing a tantalum nitride film on a substrate; depositing a dopant-containing film onto the substrate; annealing the substrate; and exposing the substrate to a neon plasma.

Citation Information

Patent Citations

  • Thin film manufacturing method, semiconductor device and manufacturing method thereof

    JP2005158761A

  • Method and apparatus for adjusting the barrier interface of copper wiring

    JP2010503204A

  • Methods for Enabling Seamless Cobalt Gap Filling

    JP2016540368A

  • Interconnect structure and method of manufacturing a damascene structure

    US20080142971A1

  • Doped Tantalum Nitride for Copper Barrier Applications

    US20130140698A1