Manufacturing method of tool for hot working

The method optimizes the composition of hot forging dies with a solid solution-strengthened Ni-based alloy intermediate layer and build-up layer to enhance wear resistance and weldability, addressing the limitations of conventional Ni-based alloys in hot forging tools.

JP2024133491AActive Publication Date: 2024-10-02PROTERIAL LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024094592
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-02
Estimated Expiration
2040-06-10

AI Technical Summary

Technical Problem

Conventional hot forging dies with precipitation-strengthened Ni-based alloys face issues with insufficient abrasion resistance, leading to rapid wear and deformation, affecting shape accuracy and requiring costly repairs, while alloys with high precipitation-strengthening elements suffer from poor weldability and cracking during overlay welding.

Method used

A hot working tool manufacturing method involving a base material of alloy tool steel, an intermediate layer of solid solution-strengthened Ni-based alloy, and a build-up layer with specific compositions of C, Cr, W, Mo, Co, Al, Ti, Nb, and B, optimized to enhance wear resistance and weldability by incorporating more solid solution strengthening elements.

Benefits of technology

The method improves wear resistance and extends the service life of hot working tools by maintaining strength over a wide temperature range, reducing wear, and preventing cracking, thus enhancing productivity and reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133491000001_ABST
    Figure 2024133491000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of tool for hot working that optimizes a chemical composition of weld metal used for a build-up layer, and has excellent abrasion resistance when being used in the build-up layer of a work surface of the tool for hot working without degrading weldability in build-up welding.SOLUTION: There is provided a manufacturing method of tool for hot working, the tool comprising a base material made of an alloy tool steel, a build-up layer made of a nickel (Ni) group alloy on a work surface, and an intermediate layer made of a solid-solution strengthened type Ni alloy in the middle between the base material and the build-up layer. The method comprises: forming the intermediate layer made of the solid-solution strengthened type Ni alloy on the base material made of the alloy tool steel; and sequentially repeating build-up welding for stacking to form the build-up layer, a composition of which contains, by mass%, 0.010-0.030% of C, 13.0-18.0% of Cr, 3.0-5.0% of W, 5.0-7.0% of Mo, 12.0-15.0% of Co, 1.0-2.8% of Al, 2.0-3.7% of Ti, 0.5-1.5% of Nb, 0.0010-0.0070% of B, and a balance Ni with inevitable impurities.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a hot working tool used in hot plastic working such as hot forging. [Background technology]

[0002] Hot working tools have been used to perform hot plastic working on workpieces. For example, hot forging dies used in hot forging are used with an alloy having high high-temperature strength and excellent wear resistance welded overlay on the striking surface (hereinafter referred to as the striking surface or working surface) in order to extend the service life of the dies. For example, in JP 2001-71086 A (Patent Document 1), the applicant of the present application has proposed a hot forging die in which an alloy equivalent to JIS-SKT4 is used as the base material of the die, and a precipitation-strengthened Ni-based alloy is overlaid and welded onto the base material to form a striking surface. In addition, in JP 2001-62541 A (Patent Document 2), the applicant has proposed a method in which the entire die including the base material is made of a precipitation-strengthened Ni-based alloy, or a base material made of a Ni-based alloy is used and a precipitation-strengthened Ni-based alloy is overlaid and welded to form a striking surface. In the hot forging dies proposed in Patent Documents 1 and 2, precipitation-strengthened Ni-based alloys such as Alloy713C, Alloy718, and Alloy U520 are given as overlaid weld metals. Incidentally, Ni-based alloys with improved high-temperature strength due to increased amounts of precipitation strengthening elements such as Al and Ti compared to the above-mentioned precipitation strengthened Ni-based alloys have been developed as heat-resistant materials for aircraft engines and heat-resistant materials for gas turbines. However, in the case of Ni-based alloys, it is said that the more precipitation strengthening elements there are, the more likely hot cracking and reheat cracking are to occur during overlay welding (Non-Patent Document 1), and from the viewpoint of weldability, Ni-based alloys that contain an excessive amount of precipitation strengthening elements are generally not considered suitable as overlay weld metals for hot forging dies. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2001-71086 A [Patent Document 2] JP 2001-62541 A [Non-patent literature]

[0004] [Non-Patent Document 1] "Welding of Superalloys (Guidebook for Welding of Heat-Resistant and Corrosion-Resistant Alloys)" edited by the Special Materials Welding Research Committee of the Japan Welding Society, Sanpo Publishing, p.36, p.46-48 Summary of the Invention [Problem to be solved by the invention]

[0005] Although the hot forging die having a striking surface formed by overlay welding of the above-mentioned precipitation-strengthened Ni-based alloy such as Alloy U520 has excellent high-temperature strength, when the material to be forged is a difficult-to-process material such as a Ni-based alloy, the abrasion resistance of the striking surface is insufficient, and the striking surface is plastically deformed and worn during forging, resulting in a significantly shortened service life of the die. If the hot forging die is used with the striking surface deformed, the shape accuracy of the material to be forged is extremely deteriorated. Therefore, repair work for the plastically deformed striking surface is required, which requires a large amount of labor and cost and reduces productivity. In addition, when an alloy with increased precipitation strengthening elements is used as a weld metal for overlay welding in order to improve the wear resistance of the impact surface, although the high-temperature strength increases as mentioned above, there is a problem that the weldability deteriorates and it is not suitable as a weld metal for overlay welding. In the case of Ni-based alloys, if the alloy contains an excessive amount of precipitation strengthening elements, the occurrence of high-temperature cracking and reheat cracking during overlay welding becomes prominent. Reheat cracking is a crack that occurs during heat treatment after welding or during use, but even in the case of weld metal for overlay welding, reheat cracking can occur because the lower overlay layer is thermally affected during overlay welding. If hot forging is performed using a hot forging die that contains even a small crack on its striking surface, stress will be concentrated in the cracked area during forging, and the crack will propagate from the striking surface of the die to the base material. Depending on the extent of the propagated crack, it may be necessary to replace the entire die, including the base material. From the above viewpoints, it has been difficult in the prior art to achieve both good weldability and wear resistance in an overlay layer using an overlay weld metal on the striking surface of a hot forging die. An object of the present invention is to provide a method for producing a hot working tool that has excellent wear resistance when used in an overlay layer on the working surface of a hot working tool such as an anvil or die for hot forging, by optimizing the chemical composition of the overlay weld metal that constitutes the overlay, without deteriorating the weldability during overlay welding. [Means for solving the problem]

[0006] The present inventors have investigated the problem of insufficient wear resistance of an overlay layer and the deterioration of weldability caused by improving the wear resistance when the overlay layer is used on the working surface of a hot working tool such as the striking surface of a hot forging die or anvil for hot forging, and have found that the wear resistance of the striking surface can be greatly improved by adding precipitation strengthening elements to the alloy within a range that does not deteriorate the weldability of the overlay alloy powder, and further by making the alloy contain more solid solution strengthening elements than conventional overlay weld metals, thereby arriving at the present invention. That is, the present invention relates to a method for manufacturing a hot working tool having a base material made of alloy tool steel, an overlay layer made of a Ni-based alloy on a working surface, and an intermediate layer made of a solid-solution strengthened Ni-based alloy between the base material and the overlay layer, the intermediate layer made of a solid-solution strengthened Ni-based alloy being formed on the base material made of alloy tool steel, and overlay welding is sequentially repeated on the intermediate layer to form an overlay layer, the composition of the overlay layer being, in mass %, C: 0.010-0.030%, Cr: 13.0-18.0%, W: 3.0-5.0%, Mo: 5.0-7.0%, Co: 12.0-15.0%, Al: 1.0-2.8%, Ti: 2.0-3.7%, Nb: 0.5-1.5%, B: 0.0010-0.0070%, with the balance being Ni and unavoidable impurities. The build-up layer is preferably an alloy powder obtained by mixing two types of alloy powders having different compositions, and the hot working tool is preferably a hot forging die or a hot forging anvil. Effect of the Invention

[0007] The alloy composition of the build-up layer used on the working surface of the hot working tool of the present invention has excellent weldability and wear resistance, making it possible to suppress the occurrence of cracks when build-up welding is performed on the working surface of the hot working tool. Furthermore, a hot working tool having a build-up layer made of this alloy composition has the effect of reducing the amount of wear on the working surface when hot working a difficult-to-work material, thereby extending the service life of the hot working tool. [Brief description of the drawings]

[0008] [Figure 1] 1 shows the results of a tensile test showing 0.2% yield strength at various temperatures for comparing the strength of an example of the present invention with that of a conventional example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] As described above, an important feature of the present invention is the adoption of an alloy composition that does not deteriorate weldability and has excellent wear resistance when used as an overlay alloy on the working surfaces of hot forging dies and hot forging anvils. Specifically, it has been discovered that by including, as an alloy element, a solid-solution strengthening element that does not excessively deteriorate weldability, it is possible to increase the strength of the build-up layer that constitutes the striking surface over a wide temperature range, thereby improving the wear resistance of the striking surface of a hot working tool. For example, among hot working tools, hot forging dies (anvils) are required to have high wear resistance, and in the thermally saturated state during hot forging, when the material to be forged is about 1000°C, the striking surface of the hot forging die is used in a high temperature range with a maximum temperature of about 800°C. However, the temperature of the striking surface at the beginning of forging is not so high, and as the forging time progresses, the temperature gradually rises from the initial temperature to a high temperature and reaches a thermally saturated state. Even at the thermally saturated state, the entire area of ​​the buildup layer constituting the striking surface does not reach the maximum temperature, and in areas with few opportunities for contact with the material to be forged, areas outside the die where heat is easily dissipated, and areas inside the surface, the buildup layer constituting the striking surface is maintained at a temperature lower than the maximum temperature. Therefore, in order to improve the wear resistance of the striking surface of a hot forging die, it is necessary to increase not only the high temperature strength but also the strength over a wide temperature range. Therefore, in the present invention, the alloy powder for overlay contains more solid solution strengthening elements such as Mo and W, which can increase strength over a wide temperature range, than conventional overlay weld metals, thereby improving the wear resistance of the overlay layer that constitutes the impact surface. Compared to precipitation strengthening elements, solid solution strengthening elements do not contribute to reheat cracking caused by strain due to precipitation of the gamma prime phase (hereinafter referred to as γ' phase). In addition, since they do not significantly expand the solidification temperature range, they are unlikely to contribute to high-temperature cracking. Therefore, if the alloy powder for overlay contains more solid solution strengthening elements than conventional precipitation strengthened Ni-based alloy overlay weld metals, it is possible to improve the wear resistance of the impact surface without deteriorating the weldability.

[0010] In the build-up layer used on the working surface of the present invention, the reasons for specifying the additive elements and the ranges of each additive element are as follows. Note that unless otherwise specified, the amounts are expressed as mass %. <C:0.010~0.030%> C has the effect of forming carbides at grain boundaries in the build-up layer, strengthening the grain boundaries, increasing the strength of the build-up layer, and improving the wear resistance. To obtain this effect, C needs to be in the range of 0.010 to 0.030%. If C is less than 0.010%, the strength of the build-up layer is insufficient and sufficient wear resistance cannot be obtained. On the other hand, if C exceeds 0.030%, coarse carbides are formed, making the build-up layer embrittled and reducing toughness and ductility. Therefore, C is set to the range of 0.010 to 0.030%. The preferable upper limit of C is 0.025%, and the preferable lower limit is 0.015%. <Cr:13.0~18.0%> Cr forms a Cr2O3 coating on the surface of the build-up layer to improve oxidation resistance, and further dissolves in the austenite phase (hereinafter referred to as γ phase) which is the base of the build-up layer to increase the strength of the build-up layer in a wide temperature range by solid solution strengthening, and has the effect of improving wear resistance. In order to obtain this effect, it is necessary to set Cr in the range of 13.0 to 18.0%. If Cr is less than 13.0%, sufficient oxidation resistance cannot be obtained. On the other hand, if it exceeds 18.0%, it forms a sigma phase (hereinafter referred to as σ phase), which is an embrittlement phase, or forms coarsening Cr-based carbides, which reduce the toughness and ductility of the build-up layer. Therefore, Cr is set in the range of 13.0 to 18.0%. The preferable upper limit of Cr is 17.0%, and the preferable lower limit is 14.0%.

[0011] <W:3.0~5.0%> W has the effect of increasing the strength of the build-up layer over a wide temperature range by dissolving in the γ phase, which is the base of the build-up layer, and improving the wear resistance through solid solution strengthening. To obtain this effect, W needs to be in the range of 3.0 to 5.0%. If W is less than 3.0%, the strength of the build-up layer is insufficient and sufficient wear resistance cannot be obtained. On the other hand, if W exceeds 5.0%, a brittle phase, the mu phase (hereinafter referred to as μ phase), is formed, and the toughness and ductility of the build-up layer are reduced. Therefore, W is set to the range of 3.0 to 5.0%. The preferable upper limit of W is 4.5%, and the preferable lower limit is 3.5%. <Mo:5.0~7.0%> Mo has the effect of increasing the strength of the build-up layer over a wide temperature range by solid solution strengthening due to its solid solution dissolution in the γ phase, and improving the wear resistance. To obtain this effect, Mo needs to be in the range of 5.0 to 7.0%. If Mo is less than 5.0%, the strength of the build-up layer is insufficient and sufficient wear resistance cannot be obtained. On the other hand, if Mo exceeds 7.0%, the build-up layer forms brittle phases such as μ phase and σ phase, which reduce the toughness and ductility of the build-up layer. Therefore, Mo is set to the range of 5.0 to 7.0%. The preferable upper limit of Mo is 6.5%, and the preferable lower limit is 5.5%.

[0012] <Co:12.0~15.0%> Co is dissolved in the γ phase, and thus has the effect of increasing the strength of the build-up layer in a wide temperature range by solid solution strengthening, and improving the wear resistance. To obtain this effect, Co needs to be in the range of 12.0 to 15.0%. If Co is less than 12.0%, the strength of the build-up layer is insufficient and sufficient wear resistance cannot be obtained. On the other hand, if Co exceeds 15.0%, the build-up layer is formed with brittle phases such as μ phase and σ phase, and the toughness and ductility of the build-up layer are reduced. In addition, since Co is an expensive element, the manufacturing cost of the alloy powder for build-up increases. Therefore, Co is set to the range of 12.0 to 15.0%. The preferable upper limit of Co is 14.0%, and the preferable lower limit is 13.0%. <Al:1.0~2.8%> Al combines with Ni to form a coherent precipitation of the γ' phase consisting of Ni3Al, and has the effect of increasing strength and improving wear resistance, particularly in high temperature regions, through precipitation strengthening. To obtain this effect, it is necessary to set Al in the range of 1.0 to 2.8%. If Al is less than 1.0%, the strength of the overlay layer in high temperature regions is insufficient and sufficient wear resistance cannot be obtained. On the other hand, if it exceeds 2.8%, the susceptibility to high temperature cracking during overlay welding and reheat cracking on the lower layer side during overlay welding increases, and weldability deteriorates. Therefore, Al is set in the range of 1.0 to 2.8%. The preferable upper limit of Al is 2.5%, and the preferable lower limit is 2.0%.

[0013] <Ti:2.0~3.7%> Ti has the effect of increasing strength and improving wear resistance, particularly in high temperature ranges, by substitutional solid solution in the Al site of the γ' phase of Ni3Al and precipitation strengthening. To obtain this effect, Ti needs to be in the range of 2.0 to 3.7%. If Ti is less than 2.0%, the strength of the overlay layer is insufficient in high temperature ranges and sufficient wear resistance cannot be obtained. On the other hand, if Ti exceeds 3.7%, the susceptibility to high temperature cracking during overlay welding and reheat cracking on the lower layer side during overlay welding increases, and weldability deteriorates. In addition, eta phase (η phase) is precipitated, reducing the strength of the overlay layer. Therefore, Ti is set to the range of 2.0 to 3.7%. The preferable upper limit of Ti is 3.5%, and the preferable lower limit is 3.0%. <Nb:0.5~1.5%> Nb dissolves in the Al site of the γ' phase of Ni3Al, and has the effect of increasing the strength and improving the wear resistance, particularly in the high temperature range, by precipitation strengthening. To obtain this effect, Nb needs to be in the range of 0.5 to 1.5%. If Nb is less than 0.5%, the strength of the overlay layer is insufficient in the high temperature range, and sufficient wear resistance cannot be obtained. On the other hand, if Nb exceeds 1.5%, it segregates significantly during solidification during overlay welding, increasing the susceptibility to hot cracking and deteriorating the weldability. In addition, it precipitates delta phase (δ phase) and reduces the strength of the overlay layer. Therefore, Nb is set to the range of 0.5 to 1.5%. The preferable upper limit of Nb is 1.3%, and the preferable lower limit is 0.8%.

[0014] <B:0.0010~0.0070%> B has the effect of strengthening the grain boundaries and increasing the strength and ductility at high temperatures. To obtain this effect, B needs to be in the range of 0.0010 to 0.0070%. If B is less than 0.0010%, sufficient grain boundary strengthening effect cannot be obtained. On the other hand, if B exceeds 0.0070%, it excessively segregates at the grain boundaries during solidification during overlay welding to form low-melting point compounds, which increase the susceptibility to hot cracking and deteriorate the weldability. Therefore, B is set to the range of 0.0010 to 0.0070%. The preferable upper limit of B is 0.0050%, and the preferable lower limit is 0.0020%. <Remainder: Ni and inevitable impurities> The balance is essentially Ni, but it does contain impurities that are unavoidably mixed in during manufacturing. In particular, Si, Mn, P, S, and Zr increase the susceptibility to hot cracking, Fe reduces the amount of γ' phase precipitation, O causes oxide scale to be entrained during overlay welding, and N causes blowholes, so it is preferable to have less of these impurity elements. Below are the preferred allowable ranges for the above impurity elements and other representative unavoidable impurity elements. Si≦1.0%, Mn≦1.0%, P≦0.01%, S≦0.01%, Fe≦1.0%, Zr≦0.03%, Mg≦0.005%, O≦0.03%, N≦0.05%.

[0015] The build-up layer used on the working surface of the hot working tool used in the present invention described above has the effect of providing good weldability during build-up welding due to its alloy composition, and also providing good wear resistance as a build-up metal, and is therefore suitable as a weld metal to be build-up welded onto the working surface of a hot working tool. In the present invention, the term "hot working tool" refers to a tool used to contact and press a workpiece heated to a hot working temperature to plastically deform the workpiece, and includes various rolls used for rolling, drawing, etc. Preferred forms of the hot working tool of the present invention include a hot forging die used in free forging or radial forging, a jig for partially pressing a workpiece, and a hot forging die used in hot die forging. The alloy composition of the buildup layer according to the present invention is particularly suitable for the buildup weld metal that is buildup welded to the part constituting the striking surface of a hot forging die or a hot forging die.

[0016] <Method of manufacturing hot working tools> Next, an example of forming a build-up layer having the above-mentioned composition to produce a hot working tool will be described. The following is for producing a hot forging die or hot forging anvil. Hot forging dies and hot forging anvils are composed of a base material and a build-up layer that constitutes the striking surface. The base material, which is the majority of the hot forging die, is an alloy tool steel having high rigidity, and its material may be, for example, an alloy for "hot die" as described in JIS-G4404 or an improved alloy thereof. The alloy tool steel that is the base material is, for example, quenched at 800 to 1100 ° C and tempered at 500 to 700 ° C, and is usually adjusted to a hardness of about 330 to 380 HBW. In addition, in the present invention, one or two types of solid solution strengthened Ni-based alloy intermediate layers can be provided between the base material made of alloy tool steel and the buildup layer having the above composition. By providing this intermediate layer, the alloy composition and mechanical properties of each layer do not change abruptly compared to forming the buildup layer directly on the base material (buildup welding), and therefore weldability can be improved. Furthermore, the effect of mitigating the stress generated between the base material and the buildup layer constituting the striking surface can be obtained, and the service life of the hot forging die can be further improved. This intermediate layer can be laminated by a general welding method such as MIG welding.

[0017] In the present invention, there are several methods for forming an overlay on the striking surface. The first method is a method in which two types of alloy powders with different compositions are prepared, and the different types of alloy powders are mixed or the mixed alloy powder is used as a weld metal for overlay welding, and the overlay is formed while adjusting the composition of the overlay. In this first method, one type of alloy powder is an alloy powder of an available existing alloy, and the composition after overlay welding can be adjusted by adjusting the composition and blending ratio of the other type of alloy powder, and the raw material cost can be reduced by using the alloy powder of an existing alloy. In addition, by using two types of alloy powders with different compositions, a synergistic effect of the properties of each alloy powder can be expected. The second method is to prepare an alloy powder whose composition is adjusted to fall within the above-mentioned range of chemical composition, and use the alloy powder as a weld metal for overlay welding. The overlay layer may be formed by appropriately selecting the first or second method.

[0018] In the present invention, to form an overlay layer on the striking surface, overlay welding is sequentially repeated to build up a predetermined thickness. As the overlay welding method for this purpose, a known technique such as powder plasma welding can be adopted. Powder plasma welding allows for faster welding than TIG welding or gas welding, and the weld structure becomes fine and dense, so it is suitable as a welding method for precipitation hardened Ni-based alloys such as those of the present invention, whose weldability is likely to be a problem, since the powder plasma welding method is a difficult-to-process material while having excellent high-temperature strength, and therefore it is difficult to manufacture welding materials such as wires. However, if the alloy is in powder form, it has the advantage that it can be manufactured relatively easily by gas atomization. A hot forging die or hot forging anvil with a buildup layer formed on the striking surface (work surface) by buildup welding can be used for hot forging as is. However, if stress generated during buildup welding needs to be reduced, it is possible to reduce the stress by performing heat treatment at 500 to 620°C for 1 to 10 hours. In addition, in order to prevent heat cracks, overlay welding may be performed in a state where the base material is preheated, so long as the temperature is lower than the annealing temperature of the base material. EXAMPLES

[0019] Example 1 The present invention will be described in more detail in the following examples. Example 1 illustrates weldability. An alloy equivalent to JIS-SKT4 was prepared as the base material for a hot forging die for radial forging, and was heat treated to a hardness of approximately 330 to 380 HBW. Next, an intermediate layer was formed on the substrate by MIG welding using a solid-solution strengthened Ni-based alloy equivalent to Hastelloy (registered trademark) C. At this time, the oxide scale on the surface of the intermediate layer was removed with a grinder in order to improve the weldability between the intermediate layer and the buildup layer, which will later become the striking surface (working surface). Two types of mixed alloy powders were prepared as alloy powders for overlay welding on the intermediate layer, and the mixing ratios of each were changed. The alloys prepared were a commercially available alloy equivalent to Alloy U520 (C 0.016%, Cr 19.2%, W 1.0%, Mo 6.0%, Co 12.3%, Al 2.0%, Ti 3.2%, Nb less than 0.01%, B 0.0067%, Ni and unavoidable impurities) and Alloy A (C 0.024%, Cr 13.5%, W 5.8%, Mo 6.0%, Co 14.2%, Al 2.2%, Ti 3.4%, Nb 1.9%, B 0.0005%, Ni and unavoidable impurities).

[0020] A build-up layer having the chemical composition shown in Table 1 was formed by gas atomization on the intermediate layer by powder plasma welding, with each layer being 2 mm thick, to form the build-up layer that constitutes the striking surface. The alloy powder produced by gas atomization was classified to obtain a particle size suitable for powder plasma welding, with a particle size range of 63 to 250 μm. The build-up layer on the intermediate layer was build-up welded in three layers (approximately 6 mm thick), and after each layer, the oxide scale on the surface of the build-up layer was ground off with a grinder to prevent cracking and the inclusion of oxide scale. In this example, when the overlay weld metal was welded up to the third layer by the powder plasma welding method, if even one visually visible crack was found on the surface of each layer, the overlay weld metal was judged to have poor weldability (symbol "x" in the table). On the other hand, if no crack was found up to the third layer, the overlay weld metal was judged to have good weldability (symbol "o" in the table).

[0021] The results of the evaluation of the weldability of the examples of the present invention, the conventional example, and the comparative example are shown in Table 2. No cracks were found on the surface of the overlay layer of the examples of the present invention and the conventional example, and the weldability of the examples of the present invention and the conventional example was evaluated as good. On the other hand, cracks were found in the second or third layer of the comparative example, and the weldability was evaluated as poor. In the case of the comparative example, it is believed that high-temperature cracking or reheat cracking occurred during overlay welding because some elements that deteriorate weldability were contained in the alloy in excess of the range of the chemical composition specified in the present invention. From the above results, it was found that the use of the build-up weld metal for the build-up layer of the invention example provided good weldability during build-up welding.

[0022] [Table 1]

[0023] [Table 2]

[0024] Example 2 In Example 2, the wear resistance will be described. In Example 1, an anvil for hot forging was prepared by overlay welding an overlay having the composition of the inventive examples No. 1 and 2 and the conventional example No. 11, which were judged to have good weldability, onto the striking surface (working surface), and hot forging was carried out using this anvil. The method of preparing the anvil for hot forging was the same as in Example 1, but the number of welded layers was two. The thickness of the overlay on the striking surface in this case was about 4 mm. Hot forging was carried out using a high-speed four-sided forging machine (radial forging machine). High-speed four-sided forging is a forging method in which the material to be forged is rotated intermittently while being forged from four directions simultaneously with four anvils arranged in an X-shape, and the material is stretched only in the axial direction by moving them relative to one another. First, the wear resistance of hot forging anvils overlaid with the overlay weld metal of No. 1, an example of the present invention, and No. 11, a conventional example, was evaluated. In order to accurately compare the wear resistance of the examples of the present invention and the conventional examples, of the four hot forging dies arranged in a high-speed four-sided forging machine, the anvils with the overlay layer of No. 1, an example of the present invention, were arranged in two dies diagonally opposite each other (dies 1 and 2), and the anvils with the overlay layer of No. 11, a conventional example, were arranged in the other two dies (dies 3 and 4). The wear resistance was evaluated by measuring the amount of wear on the striking surface of the hot forging anvil. At the most worn position on the striking surface, the wear depth was measured with a depth gauge based on the surface position of the striking surface before wear, and this was defined as the amount of wear. The forging conditions were as follows: four pieces of alloy equivalent to Alloy 718, a precipitation-strengthened Ni-based alloy, were forged as the forged material, followed by 15 pieces of alloy equivalent to Alloy U520, the same alloy as the conventional example. The forging load during forging was 700-750 tons. The temperature of the striking surface of the hot forging anvil rose from the initial temperature to a maximum of approximately 800°C during forging. The results of the wear amount of each hot forging anvil after forging are shown in Table 3. A total of 19 pieces of precipitation hardened Ni-based alloy were forged as the forged material, and the wear amount per forging of the inventive example and conventional example was calculated by dividing the average wear amount by the total number of forgings.

[0025] [Table 3]

[0026] A comparison was also made between the example of the present invention (No. 2) and the conventional example (No. 11) in the same manner. The method of preparing the hot forging anvil and the method of evaluating the wear amount were exactly the same as those described above. On the other hand, the forging conditions were different, and the material to be forged in this case was only one type, 13 pieces of Alloy718, a precipitation-strengthened Ni-based alloy. The forging load during forging was 700 to 750 tons. In addition, the temperature of the impact surface of the hot forging anvil rose from the initial temperature to a maximum of about 800°C during forging. The results of the wear amount of each hot forging anvil after forging are shown in Table 4.

[0027] [Table 4]

[0028] From the results of Tables 3 and 4, it is clear that the wear amount per forging of the examples of the present invention is less than that of the conventional examples, and that the wear resistance of the examples of the present invention is good. Considering that the wear amount is proportional to the number of forgings, it can be said that the service life of the hot forging anvil is greatly improved. In addition, when comparing No. 1 and No. 2, which are examples of the present invention, the wear amount per forging is slightly better in No. 2, which is thought to be due to the fact that No. 1 has a higher content of solid solution strengthening elements and precipitation strengthening elements than No. 2.

[0029] Example 3 In Example 3, the strength at each temperature of an example of the present invention and a conventional example will be described. Of the chemical compositions shown in Table 1, No. 1, the inventive example, and No. 11, the conventional example, were overlay welded to a thickness of 20 mm in the same manner as in Example 1. A number of tensile test pieces were taken from this overlay layer, and tensile tests were carried out at various temperatures from room temperature (22°C) to high temperature (900°C). The results of the 0.2% proof stress at each temperature from the tensile test are shown in Figure 1. Compared to the conventional example, the 0.2% proof stress of the inventive example is higher at all temperatures, and it is clear that the inventive example has increased strength over a wide temperature range. The conventional example, an alloy equivalent to Alloy U520, also contains a large amount of Mo, a solid solution strengthening element, so it does not have a strength peak at high temperatures and has high strength from low temperatures, but the inventive example exceeds that strength at all measurement temperatures. As mentioned above, hot forging dies and hot forging anvils need to provide high strength not only in the high temperature range at the time of thermal saturation, but also in the low temperature range up to the time of thermal saturation, and it can be seen that this can be achieved by using the examples of the present invention.

[0030] From the results of the above examples, it was confirmed that the examples of the present invention had good weldability without hot cracking or reheat cracking during overlay welding. In addition, it was confirmed that when the overlay weld metal of the examples of the present invention was used as the striking surface of a hot forging die, it had better wear resistance than the alloy equivalent to Alloy U520 of the conventional example. Furthermore, the results of the tensile test showed that the strength of the examples of the present invention was higher over a wide temperature range than that of the alloy equivalent to Alloy U520 of the conventional example. Therefore, when the overlay welding using the overlay weld metal of the present invention is applied to a work surface, it can be said that the weldability during overlay welding is not deteriorated, the strength of the overlay metal is increased over a wide temperature range, and the wear resistance is improved, thereby extending the service life of various hot working tools, including hot forging dies.

Claims

1. A method for manufacturing a hot working tool having a base material made of alloy tool steel, a build-up layer made of a Ni-based alloy on a working surface, and an intermediate layer made of a solid-solution strengthened Ni-based alloy between the base material and the build-up layer, comprising: forming an intermediate layer made of a solid-solution strengthened Ni-based alloy on the base material made of the alloy tool steel, and overlay welding is sequentially repeated on the intermediate layer to form an overlay layer; The composition of the buildup layer is, in mass%, C: 0.010-0.030%, Cr: 13.0-18.0%, W: 3.0-5.0%, Mo: 5.0-7.0%, Co: 12.0-15.0%, Al: 1.0-2.8%, Ti: 2.0-3.7%, Nb: 0.5-1.5%, B: 0.0010-0.0070%, and the balance being Ni and unavoidable impurities.

2. 2. The method for manufacturing a hot working tool according to claim 1, wherein the build-up layer is made of an alloy powder obtained by mixing two types of alloy powders having different compositions as a build-up weld metal.

3. 3. The method for producing a hot working tool according to claim 1, wherein the hot working tool is a hot forging die or a hot forging anvil.

Citation Information

Patent Citations

  • Hot forging die

    JP2015155115A

  • Metal powder, tool for hot working and method for manufacturing tool for hot working

    WO2014126086A1

  • Anvil for fast four faces forging device and fast four faces forging device using it, and manufacture of anvil in question

    JP2001062541A

  • Anvil for high speed four-surface forging apparatus and high speed four-surface forging apparatus

    JP2001071086A