Steel sheet for hot press and manufacturing method thereof

A laminated Fe-Al alloyed and intermetallic compound layer in the hot press steel plate addresses cracking and adhesion issues, ensuring the steel plate's integrity and formability during hot pressing.

JP2024133498AInactive Publication Date: 2024-10-02HYUNDAE STEEL CO LTD

Patent Information

Application Number
JP2024096145
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2024-06-13
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

High-strength steel used in hot press forming is prone to surface oxidation and cracking due to alloying of the aluminum plating layer, leading to reduced corrosion resistance and mold adhesion during the hot press process.

Method used

A hot press steel plate with a laminated Fe-Al alloyed layer and Fe-Al intermetallic compound layer, where the first layer has a lower hardness than the second layer, and the Fe-Al intermetallic compound layer has an area fraction of 84.5% to 98.0%, with specific thickness and composition ranges to prevent cracking and improve adhesion.

Benefits of technology

The laminated structure effectively prevents cracks and improves adhesion, maintaining the integrity and formability of the steel plate during hot pressing, enhancing corrosion resistance and mold stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133498000001_ABST
    Figure 2024133498000001_ABST
Patent Text Reader

Abstract

To provide a steel sheet for hot press capable of preventing or reducing the occurrence of cracks in a plating layer during hot press forming, and a method of manufacturing the steel sheet.SOLUTION: Disclosed is a steel sheet for hot press 10, which includes: a base steel sheet 100; and a plating layer 200 disposed on the base steel sheet and including a diffusion layer 210 and a surface layer 220 that are sequentially laminated, wherein the diffusion layer includes an Fe-Al alloy layer 212 and an Fe-Al intermetallic compound layer 214 that are sequentially disposed on the base steel sheet and each include silicon, and the area fraction of the Fe-Al intermetallic compound layer with respect to the diffusion layer is 84.5% to 98.0%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel sheet for hot press use and a manufacturing method thereof. [Background technology]

[0002] Recently, as environmental regulations and safety standards in the automotive industry have become stricter, the use of high-strength steel has increased to reduce the weight and improve stability of automobiles. Meanwhile, high-strength steel can ensure high strength characteristics relative to weight, but it is difficult to form products with complex and precise shapes because the material breaks during processing and springback occurs. Therefore, the use of hot press forming has become widespread as a method to solve such problems.

[0003] In hot press forming, a steel sheet is heated at a high temperature and pressed, so that the steel material can be easily formed, and the strength of the formed product can be ensured by performing quenching through a die. However, since the steel sheet is heated at a high temperature for hot press forming, there is a problem that the steel sheet surface is oxidized. To solve such a problem, the invention of U.S. Patent No. 6,296,805 proposes a method of hot press forming an aluminum-plated steel sheet. According to the invention of U.S. Patent No. 6,296,805, since an aluminum-plated layer exists on the surface of the steel sheet, it is possible to prevent the surface of the steel sheet from being oxidized by heating the steel sheet.

[0004] However, when the steel sheet is heated, Fe is diffused from the steel sheet into the aluminum plating layer, and the aluminum plating layer is alloyed, and when such an aluminum-plated steel sheet is hot-pressed, cracks may occur in the plating layer, which becomes brittle due to the alloying. Note that since the aluminum plating layer does not have sacrificial corrosion protection, if cracks occur in the plating layer and the steel sheet surface is exposed, the corrosion resistance of the hot-pressed product will be rapidly reduced.

[0005] Meanwhile, the invention of 10-2019-0077928 discloses an iron-aluminum alloy-plated steel sheet that includes an Fe-Al alloy plating layer formed on the surface of a base steel sheet, but when the Fe-Al alloy plating layer is divided into four equal layers in the thickness direction to form four layers, the hardness of the remaining layers excluding the outermost layer is lower than the hardness of the outermost layers, thereby suppressing the occurrence of cracks on the surface. However, since the hardness of the Fe-Al alloy plating layer decreases toward the outer periphery, there is a concern that the Fe-Al alloy plating layer will adhere to the die during the hot pressing process and be peeled off. Summary of the Invention [Problem to be solved by the invention]

[0006] The embodiments of the present invention provide a steel sheet for hot press forming, which can prevent or minimize the occurrence of cracks in a coating layer during hot press forming, and a manufacturing method thereof. [Means for solving the problem]

[0007] One embodiment of the present invention discloses a steel sheet for hot pressing, comprising: a base steel sheet; and a plating layer located on the base steel sheet, the plating layer having a diffusion layer and a surface layer which are laminated in sequence, the diffusion layer being located in sequence on the base steel sheet and comprising an Fe-Al alloyed layer and an Fe-Al intermetallic compound layer each containing silicon, the area fraction of the Fe-Al intermetallic compound layer relative to the diffusion layer being 84.5% to 98.0%.

[0008] In this embodiment, the Fe-Al intermetallic compound layer includes a first layer and a second layer stacked in sequence, and the hardness of the Fe-Al alloyed layer is higher than a first hardness of the first layer and a second hardness of the second layer, and the second hardness is higher than the first hardness.

[0009] In this embodiment, the area ratio of the diffusion layer to the plating layer is 10% to 35%.

[0010] In this embodiment, in the Fe-Al alloyed layer, the first layer, and the second layer, the aluminum content is the lowest in the first layer, and the silicon content is also the highest in the first layer.

[0011] In this embodiment, the first layer has an average thickness of 50 nm to 500 nm and the second layer has an average thickness of 1 μm to 16 μm. In this embodiment, the average thickness of the Fe-Al alloyed layer is also between 50 nm and 500 nm.

[0012] In this embodiment, the area fraction of the Fe-Al alloyed layer to the diffusion layer is also 2.0% to 15.5%.

[0013] In this embodiment, the base steel plate contains carbon (C) 0.01 wt% to 0.5 wt%, silicon (Si) 0.01 wt% to 1.0 wt%, manganese (Mn) 0.5 wt% to 3.0 wt%, phosphorus (P) more than 0 and not more than 0.05 wt%, sulfur (S) more than 0 and not more than 0.01 wt%, aluminum (Al) more than 0 and not more than 0.1 wt%, nitrogen (N) more than 0 and not more than 0.001 wt%, the balance being iron (Fe), and other unavoidable impurities.

[0014] In this embodiment, the base steel plate further contains one or more of niobium (Nb), titanium (Ti), chromium (Cr), molybdenum (Mo) and boron (B).

[0015] Another embodiment of the present invention discloses a method for manufacturing a steel plate for hot pressing, comprising: immersing the base steel plate, which has been subjected to cold rolling or hot rolling, in a coating bath having a temperature of 650°C to 700°C to form a hot-dip coating layer on a surface of the base steel plate; and cooling the base steel plate on which the hot-dip coating layer has been formed to form the coating layer, wherein the coating bath contains 4 wt% to 12 wt% silicon, 1.0 wt% to 4.0 wt% iron, and the balance aluminum. The cooling step includes a first cooling step of cooling the base steel plate to 550°C at a first average cooling rate, and a second cooling step of cooling the base steel plate to room temperature at a second average cooling rate, wherein the first average cooling rate is faster than the second average cooling rate.

[0016] In this embodiment, the first average cooling rate is also greater than or equal to 20° C. / s.

[0017] In this embodiment, the base steel sheet passes through the coating bath and is immersed in the coating bath, and the passing speed of the base steel sheet through the coating bath is also 1 mpm to 250 mpm.

[0018] In this embodiment, the method further includes, before the cooling step, a step of injecting air or gas onto the base substrate to adjust the thickness of the hot-dip plating layer. Effect of the Invention

[0019] According to the embodiment of the present invention, since the coating layer includes an Fe-Al intermetallic compound layer, it is possible to more effectively prevent or minimize the occurrence of cracks in the hot-press steel sheet during the hot-press process.

[0020] In addition, the first layer in which the Fe-Al intermetallic compound layers are sequentially laminated and the second layer having a higher hardness than the first layer are included, so that the adhesion of the plating layer can be improved. [Brief description of the drawings]

[0021] [Figure 1] 1 is a cross-sectional view illustrating a cross section of a steel sheet for hot press according to an embodiment of the present invention. [Diagram 2] 2 is a flow chart that illustrates a method for manufacturing the steel plate for hot press use in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and will be described in detail by the detailed description. The advantages, features, and methods of achieving the present invention will become clear by referring to the embodiments described in detail below together with the drawings. However, the present invention is not limited to the embodiments disclosed below, but may be embodied in various forms.

[0023] In the following examples, terms such as "first" and "second" are not used in a limiting sense but are used to distinguish one component from another component. In the following examples, the singular expression includes the plural expression unless the context clearly indicates otherwise.

[0024] In the following examples, terms such as "comprise" or "have" mean the presence of features or components described in the specification, without precluding the possibility that one or more other features or components may also be added.

[0025] In the following examples, when a part such as a film, region, or component is said to be "on" or "above" another part, this does not only mean that it is directly on top of the other part, but also means that there is another film, region, component, etc. between them.

[0026] In the drawings, the size of components may be exaggerated or reduced for the convenience of explanation. For example, the size and thickness of each component shown in the drawings are arbitrarily shown for the convenience of explanation, and the present invention is not necessarily limited to what is shown in the drawings.

[0027] When an embodiment can be implemented differently, the order of certain steps may be performed differently than that described. For example, two steps described in succession may be performed substantially simultaneously or may be performed in the reverse order from that described.

[0028] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. When referring to the drawings, the same or corresponding elements will be denoted by the same reference numerals.

[0029] FIG. 1 is a cross-sectional view illustrating a cross section of a steel sheet for hot press according to an embodiment of the present invention.

[0030] Referring to FIG. 1, a steel plate 10 for hot pressing according to an embodiment of the present invention includes a base steel plate 100 and a plating layer 200 disposed on the base steel plate 100 .

[0031] The base steel plate 100 is also a steel plate manufactured by hot rolling and cold rolling a steel slab that is cast to contain a predetermined content of a predetermined alloy element. As an example, the base steel plate 100 contains carbon (C), silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), aluminum (Al), nitrogen (N), the balance being iron (Fe), and other unavoidable impurities. The base steel plate 100 further contains one or more of niobium (Nb), titanium (Ti), chromium (Cr), molybdenum (Mo), and boron (B).

[0032] Carbon (C) is a main element that determines the strength and hardness of the base steel plate 100, and is added for the purpose of ensuring the tensile strength and hardenability characteristics of the base steel plate 100 after the hot pressing process. Such carbon may be contained in an amount of 0.01 wt% to 0.5 wt% based on the total weight of the base steel plate 100. If the carbon content is less than 0.01 wt%, it is difficult to ensure the mechanical strength of the base steel plate 100, while if the carbon content exceeds 0.5 wt%, a decrease in toughness or a problem in controlling brittleness of the base steel plate 100 may occur.

[0033] Silicon (Si) acts as a ferrite stabilizing element in the base steel plate 100. Silicon (Si) is a solid solution strengthening element, which improves the softness of the base steel plate 100 and suppresses the formation of low temperature region carbides, thereby improving the carbon concentration in the austenite. Silicon (Si) is a key element for homogenizing the hot rolling, cold rolling, and hot pressing structure (control of pearlite and manganese segregation zones) and finely dispersing ferrite. Such silicon is contained in an amount of 0.01wt% to 1.0wt% based on the total weight of the base steel sheet 100. If the silicon content is less than 0.01wt%, it is difficult to obtain the above-mentioned effects. Conversely, if the silicon content exceeds 1.0wt%, the hot rolling load and cold rolling load increase, hot rolling red scale becomes excessive, and the plating properties of the base steel sheet 100 are deteriorated.

[0034] Manganese (Mn) is added to increase hardenability and strength during heat treatment. Manganese can be included in amounts of 0.5wt% to 3.0wt% based on the total weight of the base steel plate 100. If the manganese content is less than 0.5wt%, the crystal grain refinement effect is insufficient, and the hard phase fraction in the formed product after hot pressing is insufficient. On the other hand, if the manganese content exceeds 3.0wt%, softness and toughness are reduced due to manganese segregation or pearlite bands, which causes a decrease in bending performance and creates a non-uniform fine structure.

[0035] Phosphorus (P) is contained in an amount of more than 0 and not more than 0.05 wt% based on the total weight of the base steel plate 100 in order to prevent a decrease in the toughness of the base steel plate 100. If the phosphorus content of the base steel plate 100 exceeds 0.05 wt%, iron phosphide compounds are formed, which decreases the toughness and induces cracks in the base steel plate 100 during the manufacturing process.

[0036] Sulfur (S) is contained in an amount of more than 0 and not more than 0.01 wt% based on the total weight of the base steel plate 100. If the sulfur content exceeds 0.01 wt%, hot workability is reduced and large inclusions are formed, causing surface defects such as cracks.

[0037] Aluminum (Al) acts as a deoxidizer to remove oxygen from the base steel plate 100. Aluminum is contained in an amount of more than 0 and not more than 0.1 wt% based on the total weight of the base steel plate 100. If the aluminum content exceeds 0.1 wt%, it can cause nozzle clogging during steelmaking, and aluminum oxides and the like can cause hot brittleness during casting, resulting in cracks in the base steel plate 100 and reduced softness.

[0038] On the other hand, if the base steel plate 100 contains a large amount of nitrogen (N), the amount of dissolved nitrogen increases, which reduces the impact properties and elongation of the base steel plate 100 and reduces the toughness of the joints. Therefore, it is preferable that the nitrogen content of the base steel plate 100 be more than 0 and 0.001 wt% or less based on the total weight of the base steel plate 100.

[0039] Niobium (Nb) is added to increase strength and toughness by reducing martensite packet size. Niobium may be included in the base steel plate in an amount of 0.005wt% to 0.1wt% based on the total weight of 100. When niobium is included in the above range, it has an excellent effect of refining the crystal grains of the steel material in the hot rolling process and the cold rolling process, and can prevent cracks in the slab and brittle fracture of the product during steelmaking / continuous casting, and minimize the generation of coarse precipitates during steelmaking.

[0040] Titanium (Ti) can be added to form precipitates after hot press heat treatment to strengthen hardenability and improve material properties. It also forms precipitate phases such as Ti(C,N) at high temperatures, effectively contributing to refinement of austenite grains. Titanium can be included in an amount of 0.005wt% to 0.1wt% based on the total weight of the base steel sheet 100. If titanium is included within the above content range, continuous casting defects and coarsening of precipitates can be prevented, the physical properties of the steel can be easily secured, and defects such as cracks on the steel surface can be prevented.

[0041] Chromium (Cr) is added for the purpose of improving the hardenability and strength of the base steel plate 100. Chromium is contained in an amount of 0.01 wt% to 0.5 wt% based on the total weight of the base steel plate 100. When chromium is contained in the above range, the hardenability and strength of the base steel plate 100 can be improved, and an increase in production costs and a decrease in the toughness of the steel material can be prevented.

[0042] Molybdenum (Mo) can contribute to improving the strength of the base steel plate 100 by suppressing the coarsening of precipitates and increasing hardenability during hot rolling and hot pressing. Such molybdenum (Mo) is contained in an amount of 0.001 wt% to 0.008 wt% based on the total weight of the base steel plate 100.

[0043] Boron (B) is added to ensure the hardenability and strength of the base steel sheet 100 by ensuring a martensite structure, and has a grain refinement effect by increasing the austenite grain growth temperature. Boron is also included in an amount of 0.001wt% to 0.008wt% based on the total weight of the base steel sheet 100. When boron is included in the above range, it is possible to prevent the occurrence of hard phase grain boundary embrittlement and ensure high toughness and bendability.

[0044] The plating layer 200 is formed on at least one surface of the base steel sheet 100 to a thickness of 10 μm to 50 μm and contains aluminum (Al). Here, the thickness of the plating layer 200 means the average thickness of the plating layer 200 over the entire area of ​​the plating layer 200. If the thickness of the plating layer 200 is less than 10 μm, the corrosion resistance is reduced, and if the thickness of the plating layer 200 exceeds 50 μm, the productivity of the hot-press steel sheet 10 is reduced, and the plating layer 200 is attached to a roller or a die during the hot-press process, and the plating layer 200 is peeled off from the base steel sheet 100.

[0045] The plating layer 200 also includes a diffusion layer 210 and a surface layer 220 which are laminated in this order on the base steel sheet 100 .

[0046] The surface layer 220 is a layer containing 80wt% or more of aluminum (Al) and prevents oxidation of the base steel sheet 100. The diffusion layer 210 is formed by interdiffusion of the Fe of the base steel sheet 100 and the Al of the plating layer 200, and also contains an aluminum-iron (Al-Fe) compound and an aluminum-iron-silicon (Al-Fe-Si) compound. The diffusion layer 210 also contains 20wt% to 60wt% of iron (Fe), 30wt% to 80wt% of aluminum (Al), and 0.1wt% to 40wt% of silicon (Si).

[0047] Since such a diffusion layer 210 has a higher melting point than the surface layer 220, it is possible to prevent the surface layer 220 from melting during the hot pressing process and the Al from penetrating into the structure of the base steel plate 100, which is known as liquid metal embrittlement.

[0048] Therefore, the area fraction of the diffusion layer 210, which is the ratio of the cross-sectional area of ​​the diffusion layer 210 to the cross-sectional area of ​​the plating layer 200 (cross-sectional area of ​​the diffusion layer 210 ÷ cross-sectional area of ​​the plating layer 200), is 10% to 35%. Here, the cross-sectional area of ​​the plating layer 200 and the cross-sectional area of ​​the diffusion layer 210 refer to the cross-sectional area at the same arbitrary position. This can be applied to the area fractions of other layers in the following description.

[0049] The diffusion layer 210 is disposed in sequence on the base steel sheet 100 and includes an Fe-Al alloyed layer 212 and an Fe-Al intermetallic compound layer 214, each of which contains silicon.

[0050] The Fe-Al alloyed layer 212 contains 50 wt% to 75 wt% Al, 10 wt% to 50 wt% Fe, and 0.1 wt% to 15 wt% Si, and has a density of 4.0 g / cm 3 or 4.8g / cm 3 As an example, the Fe-Al alloyed layer 212 may have a density of Al 5 Fe 2 and may have a higher hardness than the diffusion layer 210.

[0051] Such an Fe-Al alloyed layer 212 serves to prevent liquid metal embrittlement. However, since the Fe-Al alloyed layer 212 is made of a hard phase and maintains high hardness even during the hot pressing process, it induces cracks during the hot pressing process and causes a decrease in formability of the steel sheet 10 for hot pressing. Therefore, in order to prevent the liquid metal embrittlement and the decrease in formability of the steel sheet 10 for hot pressing, the Fe-Al alloyed layer 212 is formed to an average thickness of 50 nm to 500 nm, preferably 50 nm to 300 nm. Moreover, the area ratio of the Fe-Al alloyed layer 212 to the diffusion layer 210 is also 2.0% to 15.5%.

[0052] The Fe-Al intermetallic compound layer 214 contains 35 wt% to 85 wt% Al, 25 wt% to 45 wt% Fe, and 8 wt% to 30 wt% Si, and has a density of 2.9 g / cm 3 or 5.6g / cm 3 The Fe-Al intermetallic compound layer 214 has a lower hardness than the Fe-Al alloyed layer 212 and acts to buffer the compression force during the hot pressing process of the steel sheet 10 for hot pressing, thereby preventing cracks from occurring in the plating layer 200.

[0053] More specifically, during heating for hot pressing, further interdiffusion occurs between the plating layer 200 and the base steel sheet 100, and at this time, the Fe-Al alloyed layer 212 maintains a relatively high hardness, but the Fe-Al intermetallic compound layer 214 forms a tau phase and / or AlFe, resulting in a decrease in hardness. Therefore, the diffusion layer 210 includes the Fe-Al intermetallic compound layer 214, which can act as a buffer against the compression force during the hot pressing process, and thus the crack resistance can be improved.

[0054] The Fe-Al intermetallic compound layer 214 has an area fraction of 84.5% to 98.0% with respect to the diffusion layer 210. If the cross-sectional area of ​​the Fe-Al intermetallic compound layer 214 with respect to the cross-sectional area of ​​the diffusion layer 210 is 84.5% or more, the Fe-Al intermetallic compound layer 214 can effectively absorb external forces that induce cracks in the plating layer 200 during the hot pressing process. However, if the area fraction of the Fe-Al intermetallic compound layer 214 with respect to the diffusion layer 210 exceeds 98.0%, the average thickness of the Fe-Al alloyed layer 212 becomes relatively thin, making it difficult to prevent liquid metal embrittlement, and making it extremely difficult to secure the Fe-Al intermetallic compound layer 214 with an area fraction exceeding 98.0% in the temperature range of the plating bath for melting Al, which will be described later.

[0055] The Fe-Al intermetallic compound layer 210 also includes a first layer 215 and a second layer 217 that are sequentially laminated. Although the first layer 215 and the second layer 217 are each formed of an Fe-Al intermetallic compound containing Si, the first hardness of the first layer 215 may be lower than the second hardness of the second layer 217. That is, the Fe-Al alloyed layer 212, the second layer 217, and the first layer 215 may have higher hardness values ​​in this order. Therefore, even if a phase change occurs in each layer or the position of each layer is changed during the hot pressing process, a layer structure that can absorb an external force that induces crack generation or deterioration of formability can be provided.

[0056] The Fe-Al intermetallic compound layer 214 is formed on the Fe-Al alloyed layer 212, which has a low solid solubility of Si. Therefore, the first layer 215 faces the surface of the plating layer 200 and has a gradually increasing Si content. The second layer 215 has a relatively higher Al content and a lower Si content than the first layer 215.

[0057] For example, the first layer 215 contains 35 wt% to 51 wt% Al, 25 wt% to 45 wt% Fe, and 15 wt% to 30 wt% Si, and has a density of 4.6 g / cm 3 or 5.6g / cm 3 The second layer 217 may have a density of 2.9 g / cm3, including 55 wt% to 85 wt% Al, 10 wt% to 30 wt% Fe, and 8 wt% to 25 wt% Si. 3 or 3.9g / cm 3 The Fe-Al alloyed layer 212, the second layer 217, and the first layer 215 may have a high Al content (wt%) in this order, and the second layer 217, the first layer 215, and the Fe-Al alloyed layer 212 may have a high Si content (wt%) in this order. Therefore, even if a phase change occurs in each layer or the position of each layer is changed during the hot pressing process, it is possible to have a layer structure that can absorb an external force that induces crack generation or deterioration of formability.

[0058] That is, among the Fe-Al alloyed layer 212, the first layer 215 and the second layer 217, the Al content is the lowest in the first layer 215 and the Si content is the highest in the first layer 215, so that the hardness of the first layer 215 can be formed to be the lowest.

[0059] The first layer 215 can absorb an external force that induces cracks in the plating layer 200 during the hot press process, and can prevent cracks from occurring in the plating layer 200. In addition, even if cracks occur in the second layer 217 or the Fe-Al alloyed layer 212, which have a relatively higher hardness than the first layer 215, during the hot press process, the soft first layer 215 not only acts as a buffer, but also blocks the crack propagation at the interface formed during the hot press process, effectively blocking the transmission of the cracks generated in the second layer 217 or the Fe-Al alloyed layer 212 to the base steel sheet 100 or the plating layer 200. Therefore, if the Fe-Al intermetallic compound layer 214 has a laminated structure of the first layer 215 and the second layer 217, it is possible to more effectively prevent or minimize the occurrence of cracks in the hot press steel sheet 10 during the hot press process.

[0060] The second layer 217 absorbs external forces during the hot pressing process and can improve the adhesion of the plating layer 200. The second layer 217 has a higher Al content and a lower Si content than the first layer 215, and therefore has a composition more similar to that of the surface layer 220 than the Fe-Al alloyed layer 212 and the first layer 215. However, the second layer 217 can improve the adhesion of the plating layer 200.

[0061] On the other hand, if the average thickness of the first layer 215 is thinner than 50 nm, the effect of absorbing external forces that induce cracks in the plating layer 200 during the hot pressing process is rapidly reduced, and on the other hand, if the average thickness of the first layer 215 is thicker than 500 nm, Kirkendall voids may occur due to the difference in diffusion speed between Al and Fe, which may reduce performance such as weldability. Therefore, the average thickness of the first layer 215 may be formed to be 50 nm to 500 nm, preferably 50 nm to 300 nm.

[0062] In addition, if the average thickness of the second layer 217 is thinner than 1 μm, the highly brittle Fe will be dispersed due to the diffusion of Fe during the hot pressing process. 2 Al 5If the average thickness of the second layer 217 is greater than 16 μm, the stress remaining in the plating layer 200 after the hot pressing process increases, which may cause cracks to form in the plating layer 200 or peeling off of the plating layer 200. Therefore, the average thickness of the second layer 217 may be formed to be in the range of 1 μm to 16 μm.

[0063] Thus, when the Fe-Al intermetallic compound layer 214 has a laminated structure of the first layer 215 and the second layer 217, not only is it possible to more effectively prevent cracks from occurring in the plating layer 200, but also the bonding strength of the surface layer 220 is improved, resulting in excellent stability of the plating layer 200.

[0064] Fig. 2 is a flow chart that illustrates a method for manufacturing a steel sheet for hot press use in Fig. 1. In the following, the method for manufacturing a steel sheet for hot press use will be described with reference to both Figs. 1 and 2.

[0065] The method for manufacturing a steel plate for hot pressing according to an embodiment of the present invention also includes a hot rolling step (S310) of a steel slab, a cooling / coiling step (S320), a cold rolling step (S330), an annealing heat treatment step (S340), and a hot-dip galvanizing step (S350).

[0066] First, a semi-finished steel slab to be subjected to a process for forming a plated steel sheet is prepared. The steel slab contains 0.01wt% to 0.5wt% carbon (C), 0.01wt% to 1.0wt% silicon (Si), 0.5wt% to 3.0wt% manganese (Mn), more than 0 and up to 0.05wt% phosphorus (P), more than 0 and up to 0.01wt% sulfur (S), more than 0 and up to 0.1wt% aluminum (Al), more than 0 and up to 0.001wt% nitrogen (N), the balance being iron (Fe), and other unavoidable impurities. The steel slab also includes one or more of the following components: 0.005 wt% to 0.1 wt% niobium (Nb), 0.005 wt% to 0.1 wt% titanium (Ti), 0.01 wt% to 0.5 wt% chromium (Cr), 0.001 wt% to 0.008 wt% molybdenum (Mo), and 0.001 wt% to 0.008 wt% boron (B).

[0067] A reheating step of the steel slab is carried out for hot rolling. In the steel slab reheating step, the steel slab obtained through the continuous casting process is reheated to a predetermined temperature to redissolve the elements segregated during casting. In one embodiment, the slab reheating temperature (SRT) is 1,200°C to 1,400°C. If the slab reheating temperature (SRT) is lower than 1,200°C, the elements segregated during casting are not sufficiently redissolved, making it difficult to increase the homogenization effect of the alloy elements and to increase the dissolution effect of titanium (Ti). The higher the slab reheating temperature (SRT), the more favorable it is for homogenization. However, if the SRT exceeds 1,400°C, the austenite grain size increases, making it difficult to ensure strength, and the manufacturing cost of the steel plate increases due to the excessive heating process.

[0068] In the hot rolling step (S310), the reheated steel slab is hot rolled at a predetermined finishing delivery temperature (FDT). In one embodiment, the finishing delivery temperature (FDT) is 880°C to 950°C. If the finishing delivery temperature (FDT) is lower than 880°C, a duplex structure due to abnormal region rolling is generated, making it difficult to ensure the workability of the steel sheet, and there is a problem that the workability is reduced due to the uneven microstructure. In addition, a problem of sheet threadability occurs during hot rolling due to a sudden phase change. If the finishing delivery temperature (FDT) exceeds 950°C, austenite grains are coarsened. In addition, there is a risk that TiC precipitates are coarsened, resulting in a reduction in final part performance.

[0069] In the cooling / coiling step (S320), the hot-rolled steel sheet is cooled to a predetermined coiling temperature (CT) and coiled. In one embodiment, the coiling temperature is 550°C to 800°C. The coiling temperature affects the redistribution of carbon (C). If the coiling temperature is 550°C, the low-temperature phase fraction increases due to overcooling, increasing the strength, and there is a concern that the rolling load during cold rolling increases, and the softness is rapidly reduced. On the other hand, if the coiling temperature exceeds 800°C, there is a problem that abnormal grain growth or excessive grain growth causes deterioration of formability and strength.

[0070] In the cold rolling step (S330), the coiled steel sheet is uncoiled, pickled, and then cold rolled. The pickling is carried out for the purpose of removing scale from the coiled steel sheet, i.e., the hot-rolled coil manufactured through the above-mentioned hot rolling process.

[0071] The annealing heat treatment step (S340) is a step of annealing the cold-rolled steel sheet at a temperature of 700° C. or more. In one embodiment, the annealing heat treatment includes the steps of heating the cold-rolled sheet material and cooling the heated cold-rolled sheet material at a predetermined cooling rate.

[0072] The hot-dip galvanizing step (S350) is a step of forming a plating layer on the annealed heat-treated steel sheet. In one embodiment, in the hot-dip galvanizing step (S350), an Al-Si plating layer 200 may be formed on the annealed heat-treated steel sheet, i.e., the base steel sheet 100.

[0073] Specifically, the hot-dip plating step (S350) includes a step of immersing the base steel sheet 100 in a plating bath having a temperature of 650°C to 700°C to form a hot-dip plating layer on the surface of the base steel sheet 100, and a cooling step of cooling the base steel sheet 100 with the hot-dip plating layer formed thereon to form a plating layer 200.

[0074] The plating bath also contains 4wt% to 12wt% Si, 1.0wt% to 4.0wt% Fe, and the balance Al. In particular, Si contained in the plating bath can suppress the growth of the Fe-Al alloyed layer 212 during the formation of the plating layer 200. Therefore, if the Si content is less than 4wt%, the Fe-Al alloyed layer 212 is formed too thick, which reduces the formability of the steel sheet 10 for hot press processing and makes it easy for cracks to occur in the steel sheet 10 for hot press processing. On the other hand, if the Si content is more than 12wt%, the growth of the Fe-Al intermetallic compound layer 214, especially the second layer 217, becomes dominant. Therefore, by adjusting the content of Si in the plating bath, the area fraction of the Fe-Al alloyed layer 212 relative to the diffusion layer 210 can be limited to 2.0% to 15.5%, and the Fe-Al intermetallic compound layer 214 is formed to have an area fraction of 84.5% to 98.0% relative to the diffusion layer 210, which can effectively prevent or minimize the occurrence of cracks in the plating layer 200 during the hot pressing process.

[0075] In addition, the plating bath may contain additive elements such as Mn, Cr, Mg, Ti, Zn, Sb, Sn, Cu, Ni, Co, In, and Bi.

[0076] The cooling step of cooling the base steel sheet 100 on which the hot-dip galvanized layer is formed may include a first cooling step of cooling the base steel sheet 100 from the temperature of the galvanizing bath to 550°C at a first average cooling rate, and a second cooling step of cooling the base steel sheet 100 from 550°C to room temperature at a second average cooling rate, in which the first average cooling rate is faster than the second average cooling rate. For example, the first average cooling rate is 20°C / s or more, and the overall average cooling rate from the temperature of the galvanizing bath to room temperature is 1°C / s to 50°C / s.

[0077] In order to form a hot-dip coating layer on the base steel sheet 100, the base steel sheet 100 can pass through a coating bath, and at this time, the passing speed of the base steel sheet 100 through the coating bath is 1 mpm to 250 mpm.

[0078] In this manner, the base steel sheet 100 passes through the plating bath at a speed of 1 mpm to 250 mpm, and then undergoes a first cooling step and a second cooling step, so that the Fe-Al intermetallic compound layer 214 is formed to include a first layer 215 and a second layer 217 that are laminated in sequence.

[0079] The formed plating layer 200 is also an Al-Si plating layer, and has a thickness of 40 g / m on both sides of the base steel sheet 100. 2 or 200g / m 2 The hot-dip plating layer may be formed by plating the base substrate 100 with a thickness of 10 μm to 50 μm. To this end, before cooling the base substrate 100 on which the hot-dip plating layer is formed, air or gas may be sprayed onto the base substrate 100 to wipe the hot-dip plating layer, thereby adjusting the thickness of the hot-dip plating layer.

[0080] The present invention will be described in more detail below through examples. However, the following examples are intended to more specifically explain the present invention, and the scope of the present invention is not limited by the following examples. The following examples may be appropriately modified or altered by those skilled in the art within the scope of the present invention.

[0081] <Manufacturing of steel sheets for hot pressing> A steel slab having the following composition was subjected to hot rolling, cooling / coiling, cold rolling and annealing heat treatment to form a base steel plate (plate thickness 1.2 mm), and then the surface of the base steel plate was subjected to hot-dip galvanizing to form a plating layer, thereby producing a steel plate for hot pressing.

[0082] [Table 1]

[0083] Hot-dip aluminum plating is carried out using a non-oxidizing furnace / reducing furnace type line, and after plating, gas wiping is used to keep the adhesion of the hot-dip plating layer at 50g / m2 on one side. 2 or 90g / m 2 The plating bath was set to contain 7 wt% Si, 2.5 wt% Fe, and the balance Al in a temperature range of 600°C to 700°C. The base steel sheet was passed through the plating bath at a speed of 100 mpm to 200 mpm, and then cooled to room temperature at an average cooling rate of 25°C / s to produce a steel sheet for hot pressing.

[0084] <Inspection of cracks in coating layer after hot pressing process> Wiping of the hot-dip coating layer, coating bath temperature and / or passing speed (immersion time) of the base steel sheet through the coating bath were adjusted to produce test specimens having different coating layer average thicknesses, area fractions of diffusion layer in comparison with the coating layer, area fractions of Fe-Al alloyed layer in comparison with the diffusion layer and area fractions of Fe-Al intermetallic compound layer in comparison with the diffusion layer as shown in Table 2 below. These test specimens were then heated to a temperature of Ac3 or higher, and then rapidly cooled while applying an external force using a press, and the number of cracks generated in the coating layer was measured. Specifically, samples were taken from the test pieces, and the area fraction of the diffusion layer relative to the coating layer, the area fraction of the Fe-Al alloyed layer relative to the diffusion layer, and the area fraction of the Fe-Al intermetallic compound layer relative to the diffusion layer were measured. The test pieces were then heated to a temperature of Ac3 or higher at an average heating rate of 3°C / s or more, and then rapidly cooled to 300°C or lower at an average rate of 30°C / s or more while applying external force using a press. The number of cracks generated in the coating layer per unit length (mm) was then measured at any three points on the test pieces.

[0085] [Table 2]

[0086] As can be seen from Table 2 above, in the cases of Examples 1 to 7 in which the area fraction of the Fe-Al intermetallic compound layer relative to the diffusion layer is formed within the range of 84.5% to 98.0%, the number of cracks generated in the coating layer is much smaller than that in the cases of Comparative Examples 1 to 6 in which the area fraction of the Fe-Al intermetallic compound layer relative to the diffusion layer is formed lower than 84.5%. This is because the area fraction of the Fe-Al intermetallic compound layer relative to the diffusion layer is formed to be 84.5% or more, and effectively absorbs external forces that induce cracks in the coating layer during the hot pressing process, and as a result, the generation of cracks in the coating layer can be prevented or minimized. Meanwhile, as described above, if the area fraction of the Fe-Al intermetallic compound layer exceeds 98.0%, the average thickness of the Fe-Al alloyed layer becomes relatively thin, making it difficult to prevent liquid metal embrittlement, and it is extremely difficult to secure an Fe-Al intermetallic compound layer with an area fraction exceeding 98.0% in the temperature range of the coating bath as described above.

[0087] Table 3 below shows the results of measuring the number of cracks generated in the coating layer in the case where a base steel sheet other than those in Examples 1 to 7 in Table 2 was passed through a coating bath under the same conditions as those in Examples 1 to 7 in Table 2, cooled to 550°C at an average cooling rate of 15°C / s, and cooled from 550°C to room temperature at an average cooling rate of 30°C / s to produce a steel sheet for hot pressing, and then prepared a test piece under the same conditions as those in Table 2. The test piece was heated to a temperature of Ac3 or higher, and then quenched while applying an external force by pressing.

[0088] [Table 3]

[0089] As can be seen from Table 3 above, in Examples 1 to 7 in which the base steel sheet was cooled from the coating bath temperature to room temperature at an average cooling rate of 25°C / s, the Fe-Al intermetallic compound layer structure was formed in one layer, whereas in Examples 8 to 17 in which the base steel sheet was cooled to 550°C at an average cooling rate of 15°C / s and then cooled from 550°C to room temperature at an average cooling rate of 30°C / s, the Fe-Al intermetallic compound layer structure had a two-layer structure in which a first layer and a second layer were laminated. It can be seen that when the Fe-Al intermetallic compound layer has a two-layer structure, the number of cracks generated in the coating layer is further reduced.

[0090] This is because, as mentioned above, the first and second layers not only act as a buffer to absorb external forces that induce cracks, but also, even if cracks occur in the hard Fe-Al alloyed layer, the interface formed during the hot pressing process prevents the cracks from propagating in the Fe-Al alloyed layer and being transmitted to the plating layer. In addition, since the Fe-Al intermetallic compound layer has a two-layer structure, the plating layer can be formed with excellent bonding strength.

[0091] As described above, the present invention has been described with reference to the embodiment shown in the drawings, but these are merely illustrative, and those skilled in the art will understand that various modifications and variations of the embodiment are possible therefrom. Therefore, the true technical scope of the present invention is defined by the technical ideas of the claims.

Claims

1. A steel plate for hot pressing, A base steel plate; a plating layer located on the base steel plate and having a diffusion layer and a surface layer laminated in sequence, the diffusion layer is disposed on the base steel sheet in sequence and includes an Fe-Al alloyed layer and an Fe-Al intermetallic compound layer, each of which includes silicon; an area fraction of the Fe-Al intermetallic compound layer relative to the diffusion layer is 84.5% to 98.0%; The base steel plate is a steel plate for hot pressing containing, in wt%, carbon (C): 0.01 wt% to 0.5 wt%, silicon (Si): 0.01 wt% to 1.0 wt%, manganese (Mn): 0.5 wt% to 3.0 wt%, phosphorus (P): more than 0 and not more than 0.05 wt%, sulfur (S): more than 0 and not more than 0.01 wt%, aluminum (Al): more than 0 and not more than 0.1 wt%, with the balance being iron (Fe) and other unavoidable impurities.

2. 2. The steel sheet for hot press use according to claim 1, wherein an area ratio of the diffusion layer to the plating layer is 10% to 35%.

3. The Fe-Al intermetallic compound layer includes a first layer and a second layer that are laminated in sequence, the first layer has a first hardness and the second layer has a second hardness that is greater than the first hardness; The steel sheet for hot press use according to claim 1 , wherein the hardness of the Fe—Al alloyed layer is higher than the first hardness and the second hardness.

4. 4. The steel sheet for hot press use according to claim 3, wherein the aluminum content in the Fe-Al alloyed layer, the first layer and the second layer is lowest in the first layer, and the silicon content is highest in the first layer.

5. 4. The steel sheet for hot press according to claim 3, wherein the first layer has an average thickness of 50 nm to 500 nm and the second layer has an average thickness of 1 μm to 16 μm.

6. The steel sheet for hot press use according to claim 1, wherein the average thickness of the plating layer is 10 μm to 50 μm.

7. The steel sheet for hot press use according to claim 1, wherein the average thickness of the Fe-Al alloyed layer is 50 nm to 500 nm.

8. 2. The steel sheet for hot press use according to claim 1, wherein an area fraction of the Fe-Al alloyed layer relative to the diffusion layer is 2.0% to 15.5%.

9. The steel plate for hot press use according to claim 1, wherein the base steel plate further contains one or more components selected from the group consisting of niobium (Nb), titanium (Ti), chromium (Cr), molybdenum (Mo) and boron (B).

Citation Information

Patent Citations

  • A high-strength hot-dip aluminized steel sheet and its manufacturing method

    CN105506509B

  • HPF molded member excellent in peeling resistance and its manufacturing method

    JP2018518600A

  • Aluminum-iron alloy plated steel sheet for hot forming having excellent hydrogen delayed fracture resistance, peeling resistance and weldability, and hot formed member using the same

    JP2019506523A

  • HOT-DIP Al-PLATED STEEL SHEET

    JP2020084224A

  • Hot-dip aluminum-plated steel material with excellent corrosion resistance and workability and its manufacturing method

    JP2020509205A

Cited By

  • Steel sheet for hot press and manufacturing method thereof

    JP2024133497A

  • Steel sheet for hot pressing and method for manufacturing the same

    JP7922084B2