Polyvinyl alcohol-based polarizer and polarizing plate

A polyvinyl alcohol-based polarizer with a 60% esterification rate and controlled manufacturing processes addresses durability issues, ensuring high transmittance and clarity in displays under high temperature and humidity.

JP2024133756AInactive Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023043708
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyvinyl alcohol-based polarizing plates suffer from poor durability and performance under high temperature and high humidity conditions, leading to reduced contrast and clarity in displays.

Method used

A polyvinyl alcohol-based polarizer with an esterification rate of 60% or more, combined with specific manufacturing processes to control molecular weight, moisture content, and evaporation rates, ensuring durability and maintaining optical performance.

Benefits of technology

The solution results in a polarizing plate with excellent durability and balanced contrast and clarity under harsh environmental conditions, maintaining high transmittance at critical wavelengths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133756000001
    Figure 2024133756000001
  • Figure 2024133756000002
    Figure 2024133756000002
Patent Text Reader

Abstract

To provide a polyvinyl alcohol-based polarizer which is usable in a polarizing plate capable of obtaining a display that is excellent in a balance between a contrast and clearness even under a severe environmental condition such as high temperature and high humidity.SOLUTION: A polarizer contains a polyvinyl alcohol-based resin, and has a rate of esterification formed of a hydroxyl group of the polyvinyl alcohol-based resin and a boric acid calculated by the following expression (1) of 60% or more. Expression (1): A rate of esterification (unit%)=100×(1-a) / ((1-a)+b). In expression (1), when methyl of heavy dimethyl sulfoxide is set at 2.5 ppm and an integral value of main chain methylene (CH2) of 2.2 to 1.9 ppm is set at 2.00, in NMR measurement of a polarizer using a 4 mm HRMAS probe using the heavy dimethyl sulfoxide as a medium, an integral value of 5.0 to 4.2 ppm is represented by a, and an integral value of 7.5 to 6.8 ppm is represented by b.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl alcohol-based polarizer and a polarizing plate, and when used as a polarizing plate, Polyvinyl chloride is a material that can produce polarizing plates with little change in optical performance even when exposed to harsh environments such as high humidity. This relates to a vinyl alcohol-based polarizer. [Background technology]

[0002] Conventionally, polyvinyl alcohol films have been used in many applications as films with excellent transparency. One of the useful applications of polarizers is as a polarizing plate. It is used as a basic component of liquid crystal displays as a component of Its use is expanding to equipment that requires high quality and high reliability.

[0003] In this environment, the polarizing plates used in displays of LCD televisions and multi-function mobile terminals have There is a demand for LEDs to be high brightness, high definition, large area, and thin. The optical performance changes little even in harsh environments such as high humidity, and the lens is highly durable. This was what was required.

[0004] As a polarizing plate with such excellent durability, a polarizing plate manufactured using a dye-based polarizing film is By using a polarizing plate (see Patent Documents 1 and 2) or a polarizer with low transmittance, When used as a light plate, techniques are used to maintain a high degree of polarization even when used under harsh conditions. was. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-57909 A [Patent Document 2] JP 2021-101237 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the polarizing plates produced by the techniques disclosed in the above Patent Documents 1 and 2 are susceptible to high temperatures and Although it has excellent durability under high humidity conditions, it has a low degree of polarization and cannot achieve high brightness when used in displays. In addition, polarizing plates using polarizers with low transmittance have problems with high temperatures and high humidity. Although it has excellent durability under low light conditions, it is inferior in contrast and clarity when used as a display. It was.

[0007] In this invention, therefore, under such circumstances, it is desirable to develop a method for producing a condensation film that can be used even under harsh environmental conditions such as high temperature and high humidity. It is used in polarizing plates that can provide displays with a good balance of contrast and clarity. The object of the present invention is to provide a polyvinyl alcohol-based polarizer that can [Means for solving the problem]

[0008] However, the present inventors have found that the polyvinyl alcohol resin in the polyvinyl alcohol polarizer Focusing on the esterification rate formed by the hydroxyl groups of fats and boric acid, this value is set to a specific range higher than that of the conventional method. When the above problem is solved and the polarizing plate is used in the range of 100 nm to 150 nm, the contrast and clarity are improved. The present invention has been completed based on the findings that a display having a good balance between the above-mentioned characteristics can be obtained.

[0009] That is, the gist of the present invention is as follows. [1] A polarizer containing a polyvinyl alcohol resin, the poly(vinyl alcohol) content of which is calculated by the following formula (1): The esterification rate formed by the hydroxyl groups of polyvinyl alcohol resin and boric acid is 60% or more. A polyvinyl alcohol-based polarizer comprising: Equation (1): Esterification rate (unit %) = 100 × (1-a) / ((1-a) + b) (where a and b are the values ​​measured using a 4 mm HRMAS spectrometer with deuterated dimethyl sulfoxide as a medium) In the NMR measurement of a polarizer using a lobe, the methyl of deuterated dimethyl sulfoxide was 2.5 The integral value of the main chain methylene (CH2) from 2.2 to 1.9 ppm was set to 2.00. In this case, the integral value of 5.0 to 4.2 ppm is set as a, and the integral value of 7.5 to 6.8 ppm is set as b. (It is something) [2] The weight average molecular weight of the polyvinyl alcohol resin is 100,000 to 300,000 0. The polyvinyl alcohol-based polarizer according to [1]. [3] A polarizer comprising the polyvinyl alcohol-based polarizer according to [1] or [2]. A polarizing plate. Effect of the Invention

[0010] The polyvinyl alcohol-based polarizer of the present invention is a polarizing plate having excellent durability under high temperature and high humidity conditions. When the polarizer is used as a polarizing plate in a display, It is possible to obtain a display that has a good balance between reliability and clarity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The polyvinyl alcohol-based polarizer of the present invention is a polarizer containing a polyvinyl alcohol-based resin. The formula (1) below is calculated based on the hydroxyl group of polyvinyl alcohol resin and boric acid. The esterification rate (hereinafter referred to simply as "esterification rate") is 60%. The present invention is characterized in that: Equation (1): Esterification rate (unit %) = 100 × (1-a) / ((1-a) + b) (where a and b are the values ​​measured using a 4 mm HRMAS spectrometer with deuterated dimethyl sulfoxide as a medium) In the NMR measurement of a polarizer using a lobe, the methyl of deuterated dimethyl sulfoxide was 2.5 The integral value of the main chain methylene (CH2) from 2.2 to 1.9 ppm was set to 2.00. In this case, the integral value of 5.0 to 4.2 ppm is set as a, and the integral value of 7.5 to 6.8 ppm is set as b. (It is something)

[0012] The esterification rate of the polyvinyl alcohol polarizer of the present invention must be 60% or more. It is preferably 62% or more, and particularly preferably 65% ​​or more. By setting the esterification rate at 60% or more, the film can be made into a polarizing plate with a 60°C / 90R Cross transmittance at 700 nm and cross transmittance at 430 nm under high temperature and humidity conditions of H% This resulted in a polarizing plate with little change in the rate of change, making it possible to reduce the loss of both red and blue light. become.

[0013] The above-mentioned esterification rate can be controlled within a predetermined range by, for example, A method of using polyvinyl chloride resin with a weight average molecular weight of 150,000 or more. When producing a polyvinyl alcohol polarizer using an alcohol-based resin, a cast drum is used. A method to keep the moisture content of the film at 10% or less when peeling, and the evaporation rate of moisture on the cast mold at 1 0.6% / sec or more, and the drying temperature of the polarizer during manufacturing is 85°C or more. Among these, the esterification rate of the polarizer is improved to withstand harsh conditions of high temperature and high humidity. This allows you to obtain a display with a good balance of contrast and clarity even under various environmental conditions. In order to produce a polarizing plate that can be used with a polarizer, the drying temperature during polarizer production is set to 85°C or higher. In addition, it is also possible to combine this with a method that allows the evaporation rate of water on the cast mold to be 1.6% / second or more. Particularly preferred.

[0014] The polyvinyl alcohol polarizer of the present invention is first prepared by subjecting a polyvinyl alcohol film to After the film is produced, the base film is used to produce the product. First, we will explain in more detail the manufacturing process of the raw polyvinyl alcohol film. The polyvinyl alcohol-based film of the present invention will be described in detail, but it is not limited to these embodiments. It is not something that can be done.

[0015] The polyvinyl alcohol film of the present invention is produced through the following steps (A) to (C). It is preferable to also carry out step (D) as necessary. Step (A) A step of preparing an aqueous solution of a polyvinyl alcohol-based resin. Step (B) A step of casting an aqueous solution of a polyvinyl alcohol-based resin into a cast mold to form a membrane. Step (C) The formed film is heated and dried by contacting it with a plurality of heat rolls. The process. Step (D) A step of heat treating the obtained film using hot air.

[0016] <Process (A)> Step (A) is a step of preparing an aqueous solution of a polyvinyl alcohol-based resin. First, the polyvinyl alcohol resin which is the material of the polyvinyl alcohol film is and the aqueous polyvinyl alcohol resin solution will be described. In the present invention, the polyvinyl alcohol-based film is The resin is usually an unmodified polyvinyl alcohol resin, i.e., a resin polymerized from vinyl acetate. The resin produced by saponifying the polyvinyl acetate obtained by mixing the above two components is used. , vinyl acetate, and a small amount (usually 10 mol % or less, preferably 5 mol % or less) of vinyl acetate It is also possible to use a resin obtained by saponifying a copolymer with a copolymerizable component. Examples of components copolymerizable with the alkyl include unsaturated carboxylic acids (e.g., salts, esters, amides, nitriles, etc.), olefins having 2 to 30 carbon atoms (e.g., ethylene, pyrene, n-butene, isobutene, etc.), vinyl ethers, unsaturated sulfonates, etc. In addition, modified polyvinyl alcohol resins obtained by chemically modifying the hydroxyl groups after saponification are also available. Fats and oils can also be used. These can be used alone or in combination of two or more.

[0017] In addition, as a polyvinyl alcohol resin, a polyvinyl alcohol having a 1,2-diol structure in the side chain is Vinyl alcohol resins can also be used. The polyvinyl alcohol resin is, for example, (i) a copolymer of vinyl acetate and 3,4-diacetoxy (ii) a method of saponifying a copolymer of vinyl acetate and vinyl ethylene glycol with 1-butene; (iii) a method for saponifying and decarboxylating a copolymer of vinyl acetate and 2,2- Saponification and deketalization of copolymers with dialkyl-4-vinyl-1,3-dioxolane (iv) a method of saponifying a copolymer of vinyl acetate and glycerin monoallyl ether; The method can be obtained by the above method.

[0018] The weight average molecular weight of polyvinyl alcohol resin is 100,000 to 300,000. It is preferable that the molecular weight is 110,000 to 280,000, and more preferably 110,000 to 280,000. 120,000 to 260,000, particularly preferably 150,000 to 260,000 If the weight average molecular weight is too small, the polyvinyl alcohol resin may not be used as an optical filter. It is difficult to obtain sufficient optical performance when used as a film, and durability under high temperature and high humidity conditions is insufficient. When used as a display, it tends to have poor contrast and clarity, and if it is too large, When a vinyl alcohol film is used to manufacture a polarizer, the film tends to be difficult to stretch. The weight average molecular weight of the polyvinyl alcohol resin is measured by a GPC-MALS method. The weight average molecular weight is measured by

[0019] The average degree of saponification of the polyvinyl alcohol resin used in the present invention is usually 98 mol % or more. It is particularly preferred that the content is 99 mol % or more, and further preferably 99.5 mol % or more. More preferably, the average saponification degree is 99.8 mol % or more. If the average saponification degree is too low, the polyvinyl When an alcohol-based film is used as a polarizer, sufficient optical performance tends not to be obtained. Here, the average degree of saponification in the present invention is measured in accordance with JIS K 6726. That is why.

[0020] The polyvinyl alcohol resin used in the present invention is selected from the group consisting of modified species, modified amount, weight average molecular weight, Two or more types of polyvinyl alcohol having different average saponification degrees may be used in combination.

[0021] In addition to polyvinyl alcohol resin, the polyvinyl alcohol resin aqueous solution contains Depending on the type, glycerin, diglycerin, triglycerin, ethylene glycol, triethylene Commonly used ethylene glycol, trimethylolpropane, etc. and at least one of a nonionic, anionic, and cationic surfactant. It is more preferable from the viewpoint of film forming properties to contain these. These may be used alone or in combination of two or more. It can be used.

[0022] The resin concentration of the polyvinyl alcohol-based resin aqueous solution thus obtained is 15 to 60 % by weight, particularly preferably 17 to 55% by weight, and further preferably 20 to 55% by weight. If the resin concentration of the aqueous solution is too low, the drying load will be large, and the production If the temperature is too high, the viscosity will be too high and it will be difficult to dissolve uniformly. There is a tendency for

[0023] Next, the obtained aqueous polyvinyl alcohol resin solution is subjected to a degassing treatment. Examples of the defoaming method include static defoaming and defoaming using a multi-screw extruder. Any multi-screw extruder having a vent may be used, and usually a twin-screw extruder having a vent is used.

[0024] <Process (B)> Step (B) is a step of casting an aqueous solution of a polyvinyl alcohol resin into a cast mold to form a membrane. That's about it. After the degassing treatment, the polyvinyl alcohol resin aqueous solution was poured into a T-shaped slit in a fixed amount. The mixture is introduced into a die and discharged and cast onto a rotating casting drum for a continuous casting process. It is then formed into a film.

[0025] The resin temperature of the polyvinyl alcohol-based resin aqueous solution at the outlet of the T-type slit die is 80 to 10 The temperature is preferably 0°C, and particularly preferably 85 to 98°C. If the resin temperature of the aqueous polyvinyl alcohol resin solution is too low, the flow tends to be poor. If it is too high, it tends to foam.

[0026] The viscosity of the polyvinyl alcohol-based resin aqueous solution during discharge is 50 to 200 Pa·s. It is preferable that the viscosity is within a range from 70 to 150 Pa·s. If the viscosity of the aqueous solution is too high, the flow tends to be poor, and if the viscosity is too low, the casting of the film tends to be difficult. It tends to be difficult.

[0027] Aqueous polyvinyl alcohol resin solution discharged from a T-shaped slit die onto a casting drum The discharge speed is preferably 0.2 to 5 m / min, and more preferably 0.4 to 4 m / min. The speed is preferably 0.6 to 3 m / min. If the discharge speed is too slow, the productivity tends to decrease, whereas if it is too fast, casting becomes difficult. There is a tendency for

[0028] The diameter of the casting drum is preferably 2 to 5 m, particularly preferably 2.4 to 4.5 m. m, and more preferably 2.8 to 4 m. If the diameter is too small, the drying zone on the casting drum will be short, and the speed will increase. If the particle size is too large, transportability tends to decrease.

[0029] The width of the casting drum is preferably 4 m or more, and particularly preferably 4.5 m or more. The length is preferably 5 m or more, more preferably 5 to 8 m. If the width of the casting drum is too small, productivity tends to decrease.

[0030] The rotation speed of the casting drum is preferably 3 to 50 m / min, and particularly preferably The speed is preferably 7 to 40 m / min, and more preferably 10 to 35 m / min. If the rotation speed is too slow, the productivity tends to decrease, whereas if it is too fast, the drying is insufficient. There is a tendency for this to happen.

[0031] The upper limit of the surface temperature of the cast drum is 100°C or less to prevent foaming during drying. It is preferable in that the temperature can be suppressed and a film having excellent appearance can be obtained. Particularly preferable is 97° C. or less. It is more preferably 95°C or lower, and particularly preferably 92°C or lower. The lower limit of the temperature is 60°C or higher, which is necessary for peeling the film from the cast mold. It is particularly preferred that the temperature is 65° C. or higher, and even more preferred that the temperature is 70° C. or higher. It is preferably 75°C or higher, more preferably 80°C or higher.

[0032] The moisture content of the film immediately after being peeled off from the cast mold is preferably 23% or less. It is preferably 21% or less, particularly preferably 20% or less, and particularly preferably 10% or less. If the moisture content is too high, the residual crystallinity tends to increase, resulting in high production costs for polarizers. The tension is high and breakage tends to occur easily, so the extensibility is low, and as a result, boric acid and The crosslinking property of the material decreases, and the change in transmittance after durability test and the transmittance at wavelengths of 430 nm and 730 nm is observed. becomes larger. Here, the above "undissolved crystallinity" refers to the rate at which a polyvinyl alcohol film is immersed in water for 30 seconds. This refers to the percentage of crystals that remain when immersed in water. The moisture content immediately after peeling is preferably 3% or more, and particularly preferably 5% or more. If the moisture content is too low, the film tends to curl. .

[0033] The evaporation rate of water on the cast mold is preferably 1.4% / sec or more at the lower limit, Particularly preferably, the rate is 1.5% / sec or more, further preferably, 1.6% / sec or more, and particularly preferably, 1 .7% / sec or more. The upper limit is preferably 3.0% / sec or less, and more preferably 2.7% / sec or less. The rate is preferably 2.6% / sec or less, and more preferably 2.6% / sec or less. If the evaporation rate of water on the cast mold is too slow, the rate of undissolved crystals tends to be high. This results in high tension during the production of the polarizer, which makes it more likely to break, and also reduces extensibility. The crosslinking with urethane acid decreases, and the transmittance after durability and the transmittance at wavelengths of 430 nm and 730 nm are If the change is too fast, it tends to cause defects in appearance such as waviness.

[0034] <Process (C)> Step (C) is a step of heating and drying the formed film.

[0035] The film peeled off from the cast drum (the film formed above) is then passed through a nip roll. The film is transported in the machine direction (MD direction) using a thermal roller, and the front and back surfaces of the film are The heated roll is dried by contacting the heated roll with a hard cloth. It is a roll of 0.2 to 2 m in diameter, plated or mirror-finished, usually 2 to 30 rolls, preferably It is preferable to carry out drying using 10 to 25 pieces.

[0036] The surface temperature of the heat roll is not particularly limited, but is usually 60 to 150° C., and more preferably 70 If the surface temperature is too low, drying may be insufficient. If the temperature is too high, the coating will be too dry, which tends to result in poor appearance such as wavy edges.

[0037] The upper limit of the heat roll drying time is preferably 60 seconds or less, and particularly preferably The lower limit is 55 seconds or less, more preferably 50 seconds or less, and particularly preferably 45 seconds or less. It is preferably 20 seconds or more, particularly preferably 25 seconds or more, and further preferably 27 seconds or more. More preferably, the time is 30 seconds or more. If the heat roll drying time is too long, the dyeability during polarizer production tends to decrease. If the temperature becomes too high, the film is prone to wrinkles and folds during the swelling process in the manufacture of the polarizer, The child's appearance tends to deteriorate.

[0038] <Process (D)> Step (D) is a step of heat treating the obtained film with hot air. The film that has been subjected to the above step (C) is subjected to a heat treatment, for example, using a floating dryer. Just say it. The upper limit of the heat treatment temperature is preferably 140° C. or less, and particularly preferably 1 The temperature is preferably 37° C. or lower, more preferably 135° C. or lower, and particularly preferably 130° C. or lower. The limit is preferably 100° C. or higher, particularly preferably 103° C. or higher, and further preferably It is preferably 105°C or higher, and more preferably 110°C or higher. If the heat treatment temperature is too high, the dyeability during the production of the polarizer tends to decrease, and if it is too low, the polarizer During the swelling process in photon production, the film is prone to wrinkles and creases, which deteriorates the appearance of the polarizer. There is a tendency for The heat treatment time is preferably 20 to 100 seconds, and more preferably 40 to 7 It is 0 seconds.

[0039] [Polyvinyl alcohol film] Thus, a polyvinyl alcohol film is obtained through the above steps (A) to (D). Finally, it is wound onto a roll to become a finished product.

[0040] The thickness of the polyvinyl alcohol film thus obtained is 10 μm or more. In terms of the production stability of the polarizer, it is preferable that the thickness is 15 μm or more, and more preferably 15 μm or more. The thickness is preferably 20 μm or more, and more preferably 25 μm or more. The upper limit is 70 μm or less. The polarizers made from polyvinyl alcohol-based films were used in liquid crystal displays. It is preferable from the viewpoint of reducing warpage, particularly preferably 60 μm or less, and further preferably 50 μm or less. Particularly preferably, the thickness is 45 μm or less.

[0041] The length of the polyvinyl alcohol film is 4 km or more in order to increase the area of ​​the polarizer. It is preferable that the distance is 5 to 50 km from the viewpoint of the transport weight.

[0042] The width of the polyvinyl alcohol film should be 4m or more in order to widen the polarizer. It is preferable that the length is 5 m or more, and more preferable that the length is 5 m or more, from the viewpoint of avoiding breakage during the production of the polarizer. It is 5 to 6 meters. The polyvinyl alcohol film obtained by the above-mentioned production method is useful for optical purposes. In particular, the polyvinyl alcohol is very useful as a raw film for a polarizer. A method for producing a polarizer and a polarizing plate made of a polymer film will be described.

[0043] [Method for producing polyvinyl alcohol-based polarizer] The polyvinyl alcohol-based polarizer of the present invention is a polyvinyl alcohol-based polarizer obtained by the above-mentioned production method. Alcohol-based film is unwound from a roll and transported horizontally, where it is swollen, dyed, and crosslinked with boric acid. It is manufactured through processes such as bridging, stretching, washing, and drying.

[0044] The swelling process is carried out before the dyeing process. In addition to being able to clean dirt from the film surface, it also swells polyvinyl alcohol-based films. This also has the effect of preventing uneven dyeing. Usually, water is used. If the main component of the treatment liquid is water, it may contain iodide compounds, surfactants, etc. The temperature of the swelling bath is usually about 10 to 45°C. The immersion time in the swelling bath is usually about 0.1 to 10 minutes.

[0045] The dyeing process is carried out by contacting the film with a liquid containing iodine or a dichroic dye. Usually, an aqueous solution of iodine and potassium iodide is used, and the concentration of iodine is The appropriate concentration of potassium iodide is 1 to 100 g / L. A practical time is about 30 to 500 seconds. The temperature of the treatment bath is preferably 5 to 50°C. In addition to the water solvent, a small amount of an organic solvent compatible with water may be contained.

[0046] The boric acid crosslinking step is carried out using boron compounds such as boric acid and borax. The substance is used in the form of an aqueous solution or a water-organic solvent mixture at a concentration of about 10 to 100 g / L. It is preferable to add potassium iodide to the film in order to stabilize the polarization performance. The temperature is preferably about 30 to 70°C, and the treatment time is preferably about 0.1 to 20 minutes. A stretching operation may be carried out during processing.

[0047] In the stretching step, the film is stretched uniaxially by 3 to 10 times, preferably by 3.5 to 7 times. At this time, it is preferable to stretch the film slightly in the direction perpendicular to the stretching direction (to a degree sufficient to prevent shrinkage in the width direction). The temperature during stretching is 40 to 170°C. Furthermore, the stretching ratio may be finally set within the above range, and the stretching operation may be performed in one step. This may be performed not only once but multiple times in the manufacturing process.

[0048] The washing step may be performed by, for example, immersing the film in water or an aqueous solution of an iodide such as potassium iodide. This is done to remove any deposits that may occur on the surface of the film. When using an aqueous potassium iodide solution, the concentration of potassium iodide should be about 10 to 1000 g / L. The temperature during the treatment is usually 5 to 50° C., preferably 10 to 45° C. The treatment time is usually The time is 1 to 300 seconds, preferably 10 to 240 seconds. Washing with the aqueous solutions may be carried out in appropriate combination.

[0049] The drying step is typically performed using a dryer at 40 to 100° C. for 0.1 to 10 minutes. The drying temperature is preferably 70° C. or higher, and more preferably Preferably, the temperature is 75° C. or higher, particularly preferably 80° C. or higher, and particularly preferably 85° C. or higher.

[0050] Thus, a polarizer is obtained, and the degree of polarization of such a polarizer is preferably 99.90% or more. More preferably, the degree of polarization is 99.99% or more. If the degree of polarization is too low, the liquid crystal display may not be able to display images with high resolution. The contrast tends to decrease. The degree of polarization is generally measured by stacking two polarizers so that their orientation directions are in the same direction. The light transmittance (H 11 ) and two polarizers are arranged The light measured at wavelength λ is measured with the directions of the two beams overlapping each other so that they are perpendicular to each other. It is calculated from the linear transmittance (H1) according to the following formula (1). Degree of polarization = [(H 11 -H1) / (H 11 +H1) 1 / 2 (1)

[0051] Furthermore, the single transmittance of the polarizer of the present invention is preferably 42% or more. If the transmittance is too low, it tends not to be possible to achieve high brightness in the liquid crystal display. The single transmittance is a value obtained by measuring the light transmittance of a single polarizer using a spectrophotometer. do.

[0052] Next, a method for producing a polarizing plate of the present invention using the polarizer of the present invention will be described. The polarizer of the present invention is suitable for producing a polarizing plate having little color unevenness and excellent polarizing performance. do.

[0053] [Method of manufacturing polarizing plate] The polarizing plate of the present invention is provided by providing the polarizer of the present invention on one or both sides thereof with an adhesive to obtain an optically uniform polarizing film. It is produced by laminating a isotropic resin film as a protective film. Examples of the cellulose acetate include acetylcellulose, triacetylcellulose, diacetylcellulose, and the like. Cellulose-based resin film, polyethylene terephthalate, polyethylene naphtha a film made of a polyester resin such as polybutylene terephthalate; Polycarbonate resin film, cycloolefin resin film, acrylic resin film Examples of such a film include films made of linear olefin resins such as polypropylene resins.

[0054] The bonding method is carried out by a known method. For example, a liquid adhesive composition is applied to the polarizer, the protective film, and the like. After applying the coating evenly to the film or both, the two are laminated together and pressed, then heated or This is done by irradiating with active energy rays.

[0055] In addition, a resin such as a urethane resin, an acrylic resin, or a urea resin may be applied to one or both sides of the polarizer. A polarizing plate can also be produced by applying a curable resin and curing it to form a cured layer. Then, the cured layer serves as a substitute for the protective film, making it possible to reduce the thickness.

[0056] The polarizer and polarizing plate obtained by using the polyvinyl alcohol film of the present invention are It has excellent optical performance and is used in mobile information terminals, PCs, TVs, projectors, and signage. , electronic desk calculators, electronic clocks, word processors, electronic paper, game consoles, videos, cameras, Photo albums, thermometers, audio equipment, liquid crystal display devices such as gauges for automobiles and machines, and other devices. Glasses, anti-glare glasses, 3D glasses, wearable displays, foldable displays , anti-reflection layers for display elements (CRT, LCD, organic EL, electronic paper, etc.), optical communication devices, It is preferably used in medical equipment, building materials, toys, etc. EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples, but the present invention will not go beyond the gist of the invention. However, the present invention is not limited to the following examples. In the examples, "parts" and "%" are based on mass.

[0058] <Measurement conditions> <Esterification rate of polyvinyl alcohol-based polarizer> For NMR measurements, the polarizer was cut to 2 mm × 2 mm, weighed out 20 mg, and diluted with dehydrated DMSO (DMSO-d 6) was added and heated at 90°C for 10 minutes, after which AVANCE NEO40 (Bruker) was added. 0 spectrometer, equipped with a 4 mm MAS probe, 90° pulse width 5 μs, 23 °C, Single pulse, pulse interval 10 seconds, cumulative count 64, 10000Hz high speed machine The measurements were performed under gyro-angle spinning. The NMR measurement results showed that the methyl group of deuterated dimethyl sulfoxide was 2.5 ppm. If the integral value of the main chain methylene (CH2) from 2.2 to 1.9 ppm is set to 2.00, The integral value of 5.0 to 4.2 ppm is a, and the integral value of 7.5 to 6.8 ppm is b, and the following formula ( The esterification rate was calculated from 1). Equation (1): Esterification rate (unit %) = 100 × (1-a) / ((1-a) + b)

[0059] <Durability under high temperature and humidity> The polarizing plate was cut into a 3cm x 3cm piece, and then the polarizing plate and glass were attached to a double-sided adhesive film. After preparing a test specimen with the film attached, the initial cross transmittance was measured. After a 500-hour durability test in a thermo-hygrostat set at 0°C and 90% RH, the product was placed in a 24°C / 5°C / 1-hour The cross transmittance was measured after storage under 0% RH conditions. Change in cross transmittance at wavelengths of 700 nm and 430 nm (cross transmittance after durability test - initial The cross transmittance (φ1 / φ2) was calculated for each. <Polarizing plate with initial transmittance of 44%> (evaluation) ◯: The change in cross transmittance at TC 430 nm and TC 700 nm is 3 or less. ×: Either or both of the cross transmittance changes at TC430nm and TC700nm are greater than 3 It's bigger. <Polarizing plate with initial transmittance of 42.5%> (evaluation) ○: The change in cross transmittance at TC430nm and TC700nm is 0.2 or less. do. ×: Either or both of the cross transmittance changes at TC430nm and TC700nm are 0. Greater than 2.

[0060] <Example 1> (Preparation of polyvinyl alcohol film) In a 500L dissolving vessel, polyvinyl chloride with a weight average molecular weight of 123,000 and a saponification degree of 99.8 mol% was added. 100 kg of styrene-based resin, 300 kg of water, 11.5 kg of glycerin as a plasticizer 0.03 kg of sodium dodecyl sulfonate was added as a surfactant and the mixture was stirred. The temperature was raised from 0.1 to 150°C and pressure dissolution was performed, resulting in a polyvinyl alcohol resin concentration of 29.0% by mass. Thus, an aqueous solution of a vinyl resin was obtained. Next, the aqueous polyvinyl alcohol resin solution is fed to a twin-screw extruder having a vent to remove the solvent. After foaming, the temperature of the aqueous solution is raised to 95°C, and the mixture is poured into a rotating cast mold through the outlet of a T-shaped slit die. The film was formed by extrusion and casting at a temperature of 84°C and the evaporation rate of water was 1.8% / s. The moisture content of the film immediately after it was peeled off from the cast mold was 10% by mass. The film was dried by alternately contacting the front and back sides with a total of 10 heated rolls. After that, 121℃ hot air is blown on both sides of the film to heat it, and finally, it is slit. The film was then wound up to obtain a roll of polyvinyl alcohol film (film thickness: 30 μm, Width 0.6m, length 1km). (Preparation of polyvinyl alcohol-based polarizer) The resulting polyvinyl alcohol film is unwound from the roll and conveyed horizontally. Then, the fabric is immersed in a water bath at 25°C to swell, and the original roll is used as a reference in the machine direction (MD). The film was stretched 1.6 times. During this swelling process, no folds or wrinkles were generated in the film. The amount of iodine was adjusted so that the single transmittance of the final polarizer was 43.6%. The flow was measured while dyeing by immersing in an aqueous solution (28°C) containing 30g / L of potassium iodide. The film is stretched in the MD direction to 2.3 times its original size, and then it is washed with 30% boric acid. g / L, potassium iodide 30 g / L, and boric acid crosslinking was performed by immersing the specimen in an aqueous solution (57°C) containing 10 g / L of potassium iodide. The film was then uniaxially stretched in the machine direction (MD) up to 6.00 times the size of the original roll. The film was washed with an aqueous potassium iodide solution and dried at 80°C to obtain a polyvinyl alcohol polarizer. The polarization performance of the polarizer was as shown in Table 1. (Preparation of polarizing plate) A water-based adhesive was applied to the upper and lower sides of the obtained polyvinyl alcohol-based polarizer, and then a protective film was applied to the upper and lower sides of the polarizer. After laminating a 40μm TAC film, it was dried in a dryer at 80℃ to obtain a single-layer transparent A polarizing plate with a permeability of 44% was obtained. The durability of the obtained polarizing plate was evaluated. The results are shown in Table 2.

[0061] <Example 2> (Preparation of polyvinyl alcohol film) In a 500L dissolving vessel, a poly(propylene glycol) having a weight average molecular weight of 156,000 and a saponification degree of 99.8 mol% was placed. 100 kg of vinyl alcohol resin, 300 kg of water, 11.5 kg of glycerin as a plasticizer g and 0.03 kg of sodium dodecyl sulfonate as a surfactant, and stir. The temperature was then raised to 150°C and the mixture was pressurized and dissolved to obtain a polyvinyl alcohol resin concentration of 26.0% by mass. An aqueous solution of a glycol-based resin was obtained. Next, the aqueous polyvinyl alcohol resin solution is fed to a twin-screw extruder having a vent to remove the solvent. After foaming, the temperature of the aqueous solution is raised to 95°C, and the mixture is poured into a rotating cast mold through the outlet of a T-shaped slit die. The film was formed by extrusion and casting at a temperature of 69°C and the evaporation rate of water was 1.6% / s. The moisture content of the film immediately after it was peeled off from the cast mold was 20% by mass. The film was dried by alternately contacting the front and back sides with a total of 10 heated rolls. After that, 127℃ hot air is blown onto both sides of the film to heat it, and finally, it is slit. The film was then wound up to obtain a roll of polyvinyl alcohol film (film thickness: 30 μm, Width 0.6m, length 1km). (Preparation of polarizer) The resulting polyvinyl alcohol film is unwound from the roll and conveyed horizontally. Then, the fabric is immersed in a water bath at 25°C to swell, and the original roll is used as a reference in the machine direction (MD). The film was stretched 1.6 times. During this swelling process, no folds or wrinkles were generated in the film. The amount of iodine was adjusted so that the single transmittance of the final polarizer was 43.6%. The flow was measured while dyeing by immersing in an aqueous solution (28°C) containing 30g / L of potassium iodide. The film is stretched in the MD direction to 2.3 times its original size, and then it is washed with 30% boric acid. g / L, potassium iodide 30 g / L, and boric acid crosslinking was performed by immersing the sample in an aqueous solution (61°C) containing 20 g / L of potassium iodide. The film was then uniaxially stretched in the machine direction (MD) to 5.70 times the size of the original roll. The film was washed with an aqueous potassium iodide solution and dried at 80° C. to obtain a polarizer. The results were as shown in Table 1. (Preparation of polarizing plate) After applying a water-based adhesive to the top and bottom of the obtained polarizer, a 40 μm thick protective film was applied. After laminating the TAC, it was dried in a dryer at 80℃ to obtain a polarizing plate with a single transmittance of 44%. The obtained polarizing plate was used to evaluate durability. The results are shown in Table 2. there were.

[0062] <Comparative Example 1> (Preparation of polyvinyl alcohol film) In a 500L dissolving vessel, polyvinyl chloride with a weight average molecular weight of 123,000 and a saponification degree of 99.8 mol% was added. 100 kg of styrene-based resin, 300 kg of water, 11.5 kg of glycerin as a plasticizer 0.03 kg of sodium dodecyl sulfonate was added as a surfactant and the mixture was stirred. The temperature was raised from 0.1 to 150°C and pressure dissolution was performed, resulting in a polyvinyl alcohol resin concentration of 29.0% by mass. Thus, an aqueous solution of a vinyl resin was obtained. Next, the aqueous polyvinyl alcohol resin solution is fed to a twin-screw extruder having a vent to remove the solvent. After foaming, the temperature of the aqueous solution is raised to 95°C, and the mixture is poured into a rotating cast mold through the outlet of a T-shaped slit die. The film was formed by extrusion and casting at a temperature of 65°C and the evaporation rate of water was 1.5% / s. The moisture content of the film immediately after it was peeled off from the cast mold was 21% by mass. The film was dried by alternately contacting the front and back sides with a total of 10 heated rolls. After that, 127℃ hot air is blown onto both sides of the film to heat it, and finally, it is slit. The film was then wound up to obtain a roll of polyvinyl alcohol film (film thickness: 30 μm, Width 0.6m, length 1km). (Preparation of polarizer) The resulting polyvinyl alcohol film is unwound from the roll and conveyed horizontally. Then, the fabric is immersed in a water bath at 25°C to swell, and the original roll is used as a reference in the machine direction (MD). The film was stretched 1.6 times. During this swelling process, no folds or wrinkles were generated in the film. The amount of iodine was adjusted so that the single transmittance of the final polarizer was 43.6%. The flow was measured while dyeing by immersing in an aqueous solution (28°C) containing 30g / L of potassium iodide. The film is stretched in the MD direction to 2.3 times its original size, and then it is washed with 30% boric acid. g / L, potassium iodide 30 g / L, and boric acid crosslinking was performed by immersing the specimen in an aqueous solution (57°C) containing 10 g / L of potassium iodide. The film was then uniaxially stretched in the machine direction (MD) to 5.70 times the size of the original roll. The film was washed with an aqueous potassium iodide solution and dried at 80° C. to obtain a polarizer. The results were as shown in Table 1. (Preparation of polarizing plate) After applying a water-based adhesive to the top and bottom of the obtained polarizer, a 40 μm thick protective film was applied. After laminating the TAC, it was dried in a dryer at 80℃ to obtain a polarizing plate with a single transmittance of 44%. The obtained polarizing plate was used to evaluate durability. The results are shown in Table 2. there were.

[0063] <Example 3> The stretching ratio during polarizer production was changed to 5.85 times, the drying temperature was changed to 90°C, and the transmittance of the polarizing plate was also changed. A polyvinyl alcohol polarizing plate was prepared in the same manner as in Comparative Example 1, except that the polarizing efficiency was set to 42.5%. The polarizing performance of the obtained polarizer is as shown in Table 1. The durability of the polarizing plate was evaluated, and the results are shown in Table 2.

[0064] <Comparative Example 2> A polyvinyl chloride film was prepared in the same manner as in Example 3, except that the drying temperature during the preparation of the polarizer was changed to 80° C. The resulting polyol-based polarizer and polarizing plate were obtained. The polarizing performance of the obtained polarizer is shown in Table 1. The results of durability evaluation using the obtained polarizing plate are shown in Table 2. there were.

[0065] <Comparative Example 3> The stretching temperature during polarizer production was changed to 58.5°C, the stretching ratio to 6.0 times, and the drying temperature to 80°C. A polyvinyl alcohol-based polarizer and a polarizing plate were obtained in the same manner as in Example 3. The polarization performance of the obtained polarizer is shown in Table 1. The durability of the obtained polarizing plate was evaluated. The results are shown in Table 2.

[0066] [Table 1]

[0067] [Table 2]

[0068] By comparing Examples 1 and 2, in which the initial transmittance of the polarizing plate is 44%, with Comparative Example 1, The polyvinyl alcohol polarizers of Examples 1 and 2, whose refractive index is within the range specified in the present application, are used. Even under harsh environmental conditions of high temperature and humidity, the transmittance at wavelengths of 430 nm and 700 nm is This allows for a display with little variation and a well-balanced contrast and clarity. It can be seen that a polarizing plate having such a structure can be obtained. Similarly, in comparison between Example 3, in which the initial transmittance of the polarizing plate is 42.5%, and Comparative Examples 2 and 3, However, the polyvinyl alcohol polarizer of Example 3, in which the esterification rate is within the range specified in the present application, By using this, the transmittance at wavelengths of 430 nm and 700 nm can be achieved even under harsh environmental conditions of high temperature and high humidity. To obtain a display with little change in transmittance and a good balance between contrast and clarity. It can be seen that a polarizing plate capable of doing so can be obtained. [Industrial Applicability]

[0069] The polyvinyl alcohol-based polarizer of the present invention and the polarizing plate using the same have excellent polarization performance. It is used in mobile information terminals, personal computers, televisions, projectors, signage, electronic desk Calculators, electronic clocks, word processors, electronic paper, game consoles, videos, cameras, photo albums LCD display devices for cameras, thermometers, audio equipment, automobile and machine gauges, sunglasses, anti-glare devices Glasses, 3D glasses, wearable displays, foldable displays, rollerbugs LCD, rollable displays, display elements (CRT, LCD, organic EL, electronic paper) The present invention is preferably used in applications such as anti-reflection films for automobiles, optical communication devices, medical devices, building materials, toys, etc.

Claims

1. The polarizer contains a polyvinyl alcohol resin, and the polyvinyl The esterification rate formed by the hydroxyl group of the diol alcohol resin and boric acid is 60% or more. A polyvinyl alcohol-based polarizer. Equation (1): Esterification rate (unit %) = 100 × (1-a) / ((1-a) + b) (where a and b are the values ​​measured using a 4 mm HRMAS spectrometer in deuterated dimethyl sulfoxide as a medium.) In the NMR measurement using a polarizer with a lobe, the methyl of deuterated dimethyl sulfoxide was 2.5 Main chain methylene (CH 2 ) was set to 2.

00. In this case, the integral value from 5.0 to 4.2 ppm was defined as a, and the integral value from 7.5 to 6.8 ppm was defined as b. It is something.)

2. The weight average molecular weight of the polyvinyl alcohol resin is 100,000 to 300,000.

2. The polyvinyl alcohol polarizer according to claim 1,

3. A polarizing plate comprising the polyvinyl alcohol polarizer according to claim 1 or 2. 。

Citation Information

Patent Citations

  • Polyvinyl alcohol-based film, polarizing film using same, and polarizing plate

    JP2007137042A

  • Polarization film, polarization plate and manufacturing method of polarization film

    JP2019053278A

  • Polyvinyl alcohol polymer film and process for producing same

    WO2012132984A1

  • Polarizing element and polarizing plate

    JP2013057909A

  • Azo compound or salt thereof, and polarization film containing the same

    JP2021101237A