Lithium battery
By using an electrolyte solution with a lithium electrolyte salt, ethylene carbonate, and a phosphazene compound, the discharge characteristics of lithium batteries are enhanced, addressing the issue of premature depletion in low-temperature environments.
Patent Information
- Application Number
- JP2023043901
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional lithium batteries do not exhibit sufficient discharge characteristics, particularly pulse discharge characteristics, in low-temperature environments such as -40°C, leading to premature battery depletion due to low voltage values and significant voltage drops when suddenly connected to a load.
Incorporating an electrolyte solution containing a lithium electrolyte salt, ethylene carbonate solvent, and a phosphazene compound with an -OR group bonded to a phosphorus atom, such as monoethoxypentafluorocyclotriphosphazene, into the battery design to enhance discharge characteristics at low temperatures.
The addition of the phosphazene compound improves discharge characteristics, increasing voltage values and reducing voltage drops during sudden discharges in low-temperature conditions, preventing premature battery depletion.
Smart Images

Figure 2024133895000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to lithium batteries. [Background technology]
[0002] Known types of batteries that use an electrolyte include lithium ion batteries (also called "lithium secondary batteries") and lithium batteries (also called "lithium primary batteries"). For example, with regard to lithium ion batteries (lithium secondary batteries), a technology is known in which a phosphazene derivative is contained in the electrolyte to enhance the flame retardancy or self-extinguishing properties of the electrolyte in order to improve safety against fire or the like in the event of an abnormality (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-16107 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, a lithium battery (lithium primary battery), which is one type of battery using an electrolyte, has a configuration in which a battery element having a positive electrode using manganese dioxide, a negative electrode using lithium, and a separator provided between the positive electrode and the negative electrode is housed in an exterior body such as a film or a can together with an electrolyte. Lithium batteries are used for various purposes such as meter communication and various backup power sources, and are used in a wide temperature range, and it is desired that high discharge characteristics are exhibited in a wide temperature range. However, conventional lithium batteries using an electrolyte may not be able to obtain sufficient discharge characteristics in low temperature environments, for example, low temperature environments below 0°C, such as -40°C.
[0005] In one aspect, the present invention aims to provide a lithium battery that has excellent discharge characteristics at low temperatures. [Means for solving the problem]
[0006] In one embodiment, there is provided a lithium battery comprising: a battery element having a positive electrode using manganese dioxide, a negative electrode using lithium, and a separator provided between the positive electrode and the negative electrode; an exterior body in which the battery element is housed; and an electrolyte solution housed within the exterior body, the electrolyte solution including a component including a lithium electrolyte salt and a solvent containing ethylene carbonate, and a phosphazene compound having an -OR group (R is a hydrocarbon) bonded to a phosphorus atom. Effect of the Invention
[0007] In one aspect, it becomes possible to realize a lithium battery with excellent discharge characteristics at low temperatures. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram illustrating an example of a lithium battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] First, an example of a lithium battery will be described. Lithium batteries (lithium primary batteries) are known as one type of battery. The lithium battery has a configuration in which a battery element for a lithium battery, which has, for example, a positive electrode using manganese dioxide, a negative electrode using lithium, and a separator provided between the positive electrode and the negative electrode, is housed in an exterior body together with an electrolyte. Known forms of lithium batteries include a thin battery using a bag-shaped laminate film as the exterior body, and a coin battery, cylindrical battery, square battery, etc. using a can of a specific shape as the exterior body.
[0010] FIG. 1 is a diagram for explaining an example of a lithium battery. FIG. 1(A) is a schematic plan view of a main part of an example of a lithium battery. FIG. 1(B) is a schematic cross-sectional view of a main part of an example of a lithium battery. FIG. 1(B) is a schematic cross-sectional view of II in FIG. 1(A).
[0011] 1(A) and 1(B) is an example of a thin lithium battery. The lithium battery 100 includes a battery element 10, an electrolyte 20, and an exterior body 30. The battery element 10 is a battery element for a lithium battery, and as shown in FIG. 1(B), has a positive electrode 11, a negative electrode 12, and a separator 13 provided between them.
[0012] The positive electrode 11 is made of a positive electrode material including a positive electrode active material. Manganese dioxide is used as the positive electrode active material. The positive electrode material may include a conductive agent such as a carbon material, and organic components such as a binder and a solvent, in addition to the positive electrode active material. Such materials may be kneaded together with the positive electrode active material to form a positive electrode material (positive electrode mixture). The positive electrode 11 may include a current collector such as a stainless steel expanded metal, and a positive electrode material may be laminated thereon. For example, the positive electrode 11 is formed by applying a slurry-like positive electrode material to the current collector, drying it, and pressing it. To the positive electrode 11, a positive electrode tab 11a using a strip-shaped metal or the like is connected for external connection, as shown in FIG. 1(A) and FIG. 1(B).
[0013] The negative electrode 12 uses a negative electrode material including a negative electrode active material. The negative electrode active material uses lithium, for example, metallic lithium or a lithium alloy. The negative electrode 12 may include a current collector such as copper foil, on which lithium, which is a negative electrode material, is laminated. For example, the negative electrode 12 is formed by attaching lithium, which is a negative electrode material, to a current collector. To the negative electrode 12, as shown in FIG. 1(A) and FIG. 1(B), a negative electrode tab 12a using a strip-shaped metal or the like is connected for external connection.
[0014] As shown in Fig. 1(B), the positive electrode 11 and the negative electrode 12 are provided so as to face each other with a separator 13 interposed therebetween. The facing positive electrode 11 and the negative electrode 12 are separated by the separator 13. For the separator 13, a polyolefin-based or cellulose-based porous film, a woven fabric, a nonwoven fabric, or the like is used. Alternatively, for the separator 13, ceramics or the like may be used.
[0015] 1(A) and 1(B), the positive electrode 11, the negative electrode 12, and the separator 13 of the battery element 10 are housed in an exterior body 30, for example, an exterior body 30 formed into a bag shape by bonding the edges of two exterior films 30a, so that the tips of the positive electrode tab 11a and the negative electrode tab 12a protrude. For the exterior film 30a of the exterior body 30, a laminate film is used in which insulating layers of polyamide, polypropylene, or the like are laminated on both sides of a metal layer of aluminum, stainless steel, or the like.
[0016] The exterior body 30 contains the battery element 10 and an electrolyte solution 20 that serves as a conductive medium for lithium ions. For example, the battery element 10 is housed together with the electrolyte 20 in a bag-shaped exterior body 30 having three edges of two rectangular exterior films 30a welded together to open one side, so that the positive electrode tab 11a and the negative electrode tab 12a protrude outside the exterior body 30, and the open side is welded. Using such a method, a lithium battery 100 as shown in Figures 1(A) and 1(B) is obtained, that is, a lithium battery 100 in which the battery element 10 and the electrolyte 20 are housed in the exterior body 30 and the positive electrode tab 11a and the negative electrode tab 12a protrude outside the exterior body 30.
[0017] Here, as an example of a lithium battery, a lithium battery 100 in the form of a thin battery is illustrated, but other lithium batteries are also known, such as a coin-shaped battery in which a battery element having a positive electrode, a negative electrode, and a separator between them is accommodated in a coin-shaped outer can together with an electrolyte, and a cylindrical battery or a prismatic battery in which a battery element is accommodated in a cylindrical or rectangular outer can together with an electrolyte. In any form of lithium battery, the battery element may include two or more layers of separators, and may be arranged so that the positive electrode and the negative electrode face each other via each separator (i.e., two or more layers of positive electrodes or negative electrodes). The battery element may be one in which a predetermined number of layers of positive electrodes, negative electrodes, and separators are stacked in one direction in a predetermined order, or one in which the stacked layers are wound or folded.
[0018] Conventionally, as electrolytes for lithium batteries, such as the electrolyte 20 of the lithium battery 100, those containing a lithium electrolyte salt, such as lithium trifluoromethanesulfonate, and a solvent, such as ethylene carbonate, propylene carbonate, 1,2-dimethoxyethane, etc., have been known. However, lithium batteries using such conventional electrolytes sometimes fail to provide sufficient discharge characteristics in low-temperature environments, for example, in low-temperature environments below 0°C, such as -40°C.
[0019] Here, the discharge characteristics of a lithium battery include, for example, continuous discharge characteristics and pulse discharge characteristics. The continuous discharge characteristics are characteristics of a lithium battery when it is continuously discharged at a constant current, that is, when it is connected to a load through which a predetermined current flows continuously. The continuous discharge characteristics can also be said to be characteristics of a lithium battery when it is continuously discharged at a low rate. The pulse discharge characteristics are characteristics of a lithium battery when it is discharged in a pulsed or sudden manner from a no-load state, that is, when it is connected to a load through which a predetermined current flows in a pulsed or sudden manner from a no-load state in which it is not connected to a load. The pulse discharge characteristics can also be said to be characteristics of a high-rate pulsed or sudden discharge.
[0020] In lithium batteries using the above-mentioned conventional electrolyte, sufficient pulse discharge characteristics cannot be obtained in a low-temperature environment, and the voltage value when the battery is suddenly transferred from an unloaded state in which the battery is not connected to a load to a loaded state in which the battery is suddenly connected to a load, i.e., the voltage value when discharging is suddenly started from the unloaded state, tends to be low, resulting in a large voltage drop.
[0021] In general, when the voltage value during discharge becomes lower and the voltage drop becomes larger, the possibility of the lithium battery falling below the reference voltage value of the product in which it is used increases, and the product is more likely to determine that the battery is dead. Therefore, in a low-temperature environment, if the voltage value during discharge that is suddenly started from a no-load state falls below the reference voltage value, it is likely that the lithium battery will be determined to be dead early on the product side. For example, it is conceivable that this will lead to a situation in which the battery is determined to be dead early in the initial stage of starting the product in a low-temperature environment.
[0022] In order to avoid early battery depletion judgment on the product side in a low-temperature environment, it is effective to improve the pulse discharge characteristics of the lithium battery at low temperatures, that is, to increase the voltage value during discharge from a no-load state and to reduce the voltage drop. However, with lithium batteries using conventional electrolytes, the pulse discharge characteristics at such low temperatures are not sufficient, and it is sometimes difficult to avoid early battery depletion judgment on the product side.
[0023] In view of these points, the following electrolyte is used in the lithium battery to realize a lithium battery with excellent discharge characteristics at low temperatures. That is, in this embodiment, an electrolyte solution containing a component including a lithium electrolyte salt and a predetermined solvent, and a predetermined phosphazene compound is used as the electrolyte solution for the lithium battery.
[0024] The lithium electrolyte salt of the electrolyte solution may be, for example, lithium trifluoromethanesulfonate, which is a type of lithium salt. In addition, various lithium salts such as lithium bis(fluorosulfonyl)imide may be used as the lithium electrolyte salt of the electrolyte solution. One type of lithium salt may be used as the lithium electrolyte salt of the electrolyte solution, or two or more types of lithium salts may be used.
[0025] The solvent of the electrolytic solution contains ethylene carbonate. The solvent of the electrolytic solution may further contain other compounds such as propylene carbonate and 1,2-dimethoxyethane in addition to ethylene carbonate. The solvent of the electrolytic solution may contain two or more compounds including at least ethylene carbonate. Hereinafter, the solvent of the electrolytic solution containing at least ethylene carbonate in this way is also referred to as "ethylene carbonate-containing solvent".
[0026] The phosphazene compound used in the electrolyte has an -OR group (R is a hydrocarbon) bonded to a phosphorus atom. The phosphazene compound used in the electrolyte is, for example, a cyclic phosphazene compound represented by the following formula (1).
[0027] (NPX2)3...(1) In the above formula (1), of the six X's, five are halogen elements and one is an -OR group (R is a hydrocarbon). The halogen element is, for example, fluorine. The -OR group is, for example, an alkoxy group such as an ethoxy group, or an aryloxy group such as a phenoxy group. As an example, the phosphazene compound of the electrolyte may be monoethoxypentafluorocyclotriphosphazene as shown in the following formula (1a), or monophenoxypentafluorocyclotriphosphazene as shown in the following formula (1b).
[0028] [ka]
[0029] [ka]
[0030] The phosphazene compound in the electrolyte is not limited to these, and various phosphazene compounds can be used. As the phosphazene compound in the electrolyte, one type of phosphazene compound may be used, or two or more types of phosphazene compounds may be used.
[0031] The above-mentioned electrolyte, i.e., the electrolyte containing a component including a lithium electrolyte salt and an ethylene carbonate-containing solvent, and a phosphazene compound having an -OR group (R is a hydrocarbon), is adjusted to have a viscosity of, for example, 2.0 mPa s or less at 25° C. By making the viscosity of the electrolyte relatively low, such as 2.0 mPa s or less, in a lithium battery using the electrolyte, a decrease in lithium ion conductivity and an increase in cell resistance, etc., can be effectively suppressed.
[0032] In the above-mentioned electrolytic solution, the phosphazene compound is further added to the component containing the lithium electrolyte salt and the ethylene carbonate-containing solvent in an amount equivalent to 2% by volume or more and 50% by volume or less of the component. In other words, when the ratio of the volume V1 of the component containing the lithium electrolyte salt and the ethylene carbonate-containing solvent to the volume V2 of the phosphazene compound is V1:V2=100:X, the phosphazene compound is added to the component so that X is 2 or more and 50 or less. Note that the component may contain other substances different from the lithium electrolyte salt and the ethylene carbonate-containing solvent, such as a solvent or inevitable impurities, as long as the component mainly contains the lithium electrolyte salt and the ethylene carbonate-containing solvent.
[0033] As described above, the electrolyte of the lithium battery contains a component containing a lithium electrolyte salt and an ethylene carbonate-containing solvent, and a phosphazene compound having an -OR group (R is a hydrocarbon). By using an electrolyte containing such a specific phosphazene compound, the discharge characteristics of the lithium battery at low temperatures are improved compared to when an electrolyte containing no phosphazene compound is used. For example, the discharge characteristics in a low-temperature environment below 0°C, such as -40°C, and the pulse discharge characteristics in such a low-temperature environment are improved. That is, the voltage value during discharge that starts suddenly from a no-load state in a low-temperature environment is increased, and the voltage drop during such a sudden discharge from a no-load state is suppressed. As a result, even if a product using a lithium battery is placed in a low-temperature environment, it is possible to effectively suppress the voltage value of the lithium battery from falling below the reference voltage value of the product at the initial stage, such as when the product is started, and thus the product side from determining that the battery is dead early. The electrolyte realizes a lithium battery with excellent discharge characteristics at low temperatures.
[0034] The electrolyte solutions and lithium batteries of Examples and Comparative Examples, as well as the results of their characteristic evaluations, will be described below. <Example 1> (positive electrode) Manganese dioxide was used as the positive electrode active material, and this was mixed with a conductive agent, a binder, etc. to obtain a slurry-like positive electrode material. The obtained positive electrode material was applied to a sheet-like stainless steel expand metal that would become a positive electrode current collector, and after drying and pressing, a positive electrode part and a positive electrode terminal part were cut out, and a positive electrode tab with a heat-sealing resin was resistance-welded to the positive electrode terminal part to obtain a positive electrode with a positive electrode tab connected.
[0035] (Negative electrode) A lithium attachment portion and a negative electrode terminal portion were cut out from the copper foil serving as the negative electrode current collector, cut pieces of metallic lithium were attached to the lithium attachment portion as the negative electrode material or negative electrode active material, and a negative electrode tab with a heat fusion resin was resistance welded to the negative electrode terminal portion to obtain a negative electrode with a negative electrode tab connected.
[0036] (Separator) A polypropylene separator was used as the separator. (electrolyte) Lithium trifluoromethanesulfonate was used as the lithium electrolyte salt, and ethylene carbonate (also called "EC"), propylene carbonate (also called "PC"), and 1,2-dimethoxyethane (also called "DME") were used as the solvent. The phosphazene compound used was the one shown in formula (1a) above, i.e., monoethoxypentafluorocyclotriphosphazene.
[0037] In preparing the electrolyte solution, first, a solvent containing EC, PC, and DME (one example of the above-mentioned ethylene carbonate-containing solvent) was prepared. The volume ratio of EC, PC, and DME in the solvent can be, for example, 5% to 20% by volume for EC, 5% to 20% by volume for PC, and 60% to 90% by volume for DME. Here, as an example, a solvent was prepared with 10% by volume for EC, 10% by volume for PC, and 80% by volume for DME. Next, lithium trifluoromethanesulfonate, a lithium electrolyte salt, was dissolved in the prepared solvent so that the salt concentration was 0.6 M (mol / L), to prepare a solution containing the lithium electrolyte salt and the solvent. Then, a phosphazene compound was further added to the prepared solution in an amount equivalent to 2% by volume of the prepared solution. As a result, the electrolyte solution of Example 1 was obtained, which contains a component containing a predetermined lithium electrolyte salt and a solvent (100% by volume) and a predetermined phosphazene compound (2% by volume) equivalent to 2% by volume of the component.
[0038] (Cell Preparation) A laminate in which a positive electrode with a positive tab, a separator, and a negative electrode with a negative tab are laminated in this order was accommodated together with an electrolyte in a separately prepared exterior body made of a laminate film so that the positive and negative electrode tabs protrude, and the exterior body was sealed. The procedure for accommodating the laminate and electrolyte in the exterior body and sealing the exterior body so that the positive and negative electrode tabs protrude outside the exterior body can be, for example, as follows. That is, three sides of two rectangular laminate films (exterior films) facing each other are welded to prepare a bag-shaped exterior body with one side open, and the laminate is accommodated in the bag-shaped exterior body so that the positive and negative electrode tabs protrude, and the electrolyte is further injected and accommodated, and the open side of the bag-shaped exterior body on the positive and negative electrode tab protruding side is sealed. For example, such a procedure is adopted, and the laminate and electrolyte are accommodated in the exterior body so that the positive and negative electrode tabs protrude outside the exterior body.
[0039] The assembly was carried out according to the above-mentioned procedure to obtain the lithium battery of Example 1. The cell size of the lithium battery was 7 mm long x 7 mm wide x 1 mm thick. <Example 2> To a solution containing lithium trifluoromethanesulfonate, a lithium electrolyte salt with a salt concentration of 0.6M, and a solvent containing EC, PC and DME (volume ratio of EC:PC:DME=10:10:80), a phosphazene compound, monoethoxypentafluorocyclotriphosphazene, was further added in an amount equivalent to 5% by volume of the solution. This resulted in an electrolyte solution of Example 2, which contains a component containing a specific lithium electrolyte salt and a solvent (100% by volume), and a specific phosphazene compound (5% by volume) equivalent to 5% by volume of the component. A lithium battery of Example 2 was obtained in the same manner as in Example 1, except that such an electrolyte solution was used.
[0040] <Example 3> To a solution containing lithium trifluoromethanesulfonate, a lithium electrolyte salt with a salt concentration of 0.6M, and a solvent containing EC, PC and DME (volume ratio of EC:PC:DME=10:10:80), a phosphazene compound, monoethoxypentafluorocyclotriphosphazene, was further added in an amount equivalent to 10% by volume of the solution. This resulted in the electrolytic solution of Example 3, which contains a component containing a specific lithium electrolyte salt and a solvent (100% by volume), and a specific phosphazene compound (10% by volume) equivalent to 10% by volume of the component. A lithium battery of Example 3 was obtained in the same manner as in Example 1, except that such an electrolytic solution was used.
[0041] <Example 4> To a solution containing lithium trifluoromethanesulfonate, a lithium electrolyte salt with a salt concentration of 0.6M, and a solvent containing EC, PC and DME (EC:PC:DME=10:10:80 in volume ratio), a phosphazene compound, monoethoxypentafluorocyclotriphosphazene, was further added in an amount equivalent to 20% by volume of the solution. This resulted in the electrolytic solution of Example 4, which contains a component containing a specific lithium electrolyte salt and a solvent (100% by volume), and a specific phosphazene compound (20% by volume) equivalent to 20% by volume of the component. A lithium battery of Example 4 was obtained in the same manner as in Example 1, except that such an electrolytic solution was used.
[0042] <Example 5> To a solution containing lithium trifluoromethanesulfonate, a lithium electrolyte salt with a salt concentration of 0.6M, and a solvent containing EC, PC and DME (volume ratio of EC:PC:DME=10:10:80), a phosphazene compound, monoethoxypentafluorocyclotriphosphazene, was further added in an amount equivalent to 50% by volume of the solution. This resulted in the electrolytic solution of Example 5, which contains a component containing a predetermined lithium electrolyte salt and a solvent (100% by volume), and a predetermined phosphazene compound (50% by volume) in an amount equivalent to 50% by volume of the component. A lithium battery of Example 5 was obtained in the same manner as in Example 1, except that such an electrolytic solution was used.
[0043] <Comparative Example 1> A solution containing lithium trifluoromethanesulfonate, a lithium electrolyte salt with a salt concentration of 0.6 M, and a solvent containing EC, PC, and DME (EC:PC:DME=10:10:80 in volume ratio) was used as the electrolyte of Comparative Example 1. That is, the electrolyte of Comparative Example 1 was obtained by containing a predetermined lithium electrolyte salt and solvent (100% by volume) and not containing a phosphazene compound (0% by volume). A lithium battery of Comparative Example 1 was obtained in the same manner as in Example 1 above, except for using such an electrolyte.
[0044] <Characteristics evaluation> (Pulse discharge characteristics of lithium batteries) The open circuit voltage value [V] was measured for each of the lithium batteries (undischarged) using the electrolytes of Examples 1-5 and Comparative Example 1. Furthermore, pulse discharge (low temperature pulse discharge) was performed for each of the lithium batteries (undischarged) using the electrolytes of Examples 1-5 and Comparative Example 1 under the conditions of a current value of 16.1 mA, a time of 1 s (second), and a temperature of -40°C. During low temperature pulse discharge, the lithium battery exhibits a discharge behavior in which the voltage drops during the load period (1 second from the start of discharge). For each of the lithium batteries using the electrolytes of Examples 1-5 and Comparative Example 1, the voltage value [V] during low temperature pulse discharge (load period) was obtained from the discharge behavior (discharge graph) when low temperature pulse discharge was performed under the above conditions. Furthermore, for each of the lithium batteries using the electrolytes of Examples 1-5 and Comparative Example 1, the voltage difference between the open circuit voltage value and the voltage value during low temperature pulse discharge, i.e., the voltage drop [V] during low temperature pulse discharge from the open circuit voltage value was obtained.
[0045] (Electrolyte viscosity) The electrolyte solutions of Examples 1 to 5 and Comparative Example 1 were each measured in a thermostatic chamber at 25° C. using an E-type viscometer at a shear rate of 10 s -1 The viscosity [mPa s] was measured under the following conditions.
[0046] <Characteristics evaluation results> Table 1 shows the compositions [vol %] of the electrolytes in Examples 1 to 5 and Comparative Example 1, the open-circuit voltages [V] of the lithium batteries using the electrolytes, the voltages [V] and voltage drops [V] during low-temperature pulse discharge, and the viscosities [mPa s] of the electrolytes.
[0047] [Table 1]
[0048] First, the voltage values during low-temperature pulse discharge (current value 16.1 mA, time 1 s, temperature -40°C) and the voltage drop from the open-circuit voltage value of the voltage values are compared when the electrolyte of Comparative Example 1 is used in a lithium battery and when the electrolyte of Examples 1-5 is used.
[0049] As seen from Table 1, the voltage value during low-temperature pulse discharge of the lithium battery using the electrolyte of Comparative Example 1 was 2.39 V, whereas the voltage value during low-temperature pulse discharge of the lithium battery using the electrolyte of Example 1-5 was in the range of 2.45 V to 2.46 V. It was confirmed that the voltage value during low-temperature pulse discharge of the lithium battery using the electrolyte of Example 1-5 containing a phosphazene compound was higher than that of the lithium battery using the electrolyte of Comparative Example 1 containing no phosphazene compound.
[0050] Also, from Table 1, the voltage drop during low-temperature pulse discharge from the open-circuit voltage value of the lithium battery using the electrolyte of Comparative Example 1 was 0.76 V, whereas the voltage drop during low-temperature pulse discharge from the open-circuit voltage value of the lithium battery using the electrolyte of Example 1-5 was in the range of 0.70 V to 0.72 V. It was confirmed that the voltage drop during low-temperature pulse discharge from the open-circuit voltage value of the lithium battery using the electrolyte of Example 1-5 containing a phosphazene compound was suppressed to a small value compared to the lithium battery using the electrolyte of Comparative Example 1 containing no phosphazene compound.
[0051] Next, the viscosity at 25° C. of the electrolyte solution of Comparative Example 1 and the electrolyte solutions of Examples 1-5 will be compared. From Table 1, the viscosity of the electrolyte of Comparative Example 1 at 25°C was 0.9 mPa·s, whereas the viscosity of the electrolyte of Examples 1-5 at 25°C was in the range of 1.0 mPa·s to 1.3 mPa·s. The electrolyte of Examples 1-5 containing the phosphazene compound tended to have a slightly higher viscosity at 25°C than the electrolyte of Comparative Example 1 not containing the phosphazene compound. However, the electrolyte of Examples 1-5 exhibited a viscosity of 2.0 mPa·s or less, which is sufficiently low for a lithium battery electrolyte, and was not a viscosity that would cause a decrease in the performance of the lithium battery, such as a decrease in lithium ion conductivity or an increase in cell resistance. It was confirmed that a sufficiently low viscosity of 2.0 mPa·s or less was achieved even when a phosphazene compound was added, as in the electrolyte of Examples 1-5.
[0052] From the results of the above characteristic evaluation, a high-performance lithium battery can be realized by using the electrolyte of Examples 1-5 (electrolyte containing 2% by volume to 50% by volume of the phosphazene compound) in which a phosphazene compound is further added to components including lithium trifluoromethanesulfonate, a lithium electrolyte salt, and a solvent containing EC, PC, and DME.
[0053] That is, even if a phosphazene compound is added to the electrolyte, the electrolyte is prevented from becoming highly viscous, and the lithium ion conductivity is prevented from decreasing, and the cell resistance is prevented from increasing. In addition, by adding a phosphazene compound to the electrolyte, the voltage value during low-temperature pulse discharge of a lithium battery using the electrolyte is increased, and the voltage drop from the open circuit voltage value is suppressed. In other words, the voltage value during discharge that starts suddenly from a no-load state in a low-temperature environment is increased, and the voltage drop during such sudden discharge from a no-load state is suppressed. As a result, even if a product using a lithium battery is placed in a low-temperature environment, the voltage value of the lithium battery at the initial stage, such as when the product is started, is effectively prevented from falling below the reference voltage value of the product, and the product is therefore prevented from determining that the battery is dead early. According to the electrolyte, a lithium battery having excellent discharge characteristics at low temperatures is realized.
[0054] Here, an electrolyte solution containing monoethoxypentafluorocyclotriphosphazene (formula (1a)) as a phosphazene compound and a lithium battery using the same are exemplified, but the same effect as above can be obtained from an electrolyte solution containing monophenoxypentafluorocyclotriphosphazene (formula (1b)) as a phosphazene compound and a lithium battery using the same. It is considered that the same effect as above can be expected from an electrolyte solution containing both monoethoxypentafluorocyclotriphosphazene and monophenoxypentafluorocyclotriphosphazene and a lithium battery using the same.
[0055] In addition, although an electrolyte solution containing lithium trifluoromethanesulfonate as the lithium electrolyte salt and a lithium battery using the same have been exemplified here, it is believed that the same effects as described above can be expected for electrolyte solutions containing lithium salts other than lithium trifluoromethanesulfonate and lithium batteries using the same.
[0056] In addition, although an electrolyte solution containing a solvent containing EC, PC, and DME and a lithium battery using the same are exemplified here, it is believed that the same effects as above can be expected from an electrolyte solution containing a solvent that contains only EC and DME out of EC, PC, and DME, or a solvent that contains only EC and DME, and a lithium battery using the same. It is believed that the same effects as above can be expected from an electrolyte solution containing a solvent that contains EC and compounds other than PC and DME, and a lithium battery using the same. [Explanation of symbols]
[0057] 10 Battery elements 11 Positive electrode 11a Positive tab 12 Negative electrode 12a Negative tab 13 Separator 20 Electrolyte 30 Exterior body 30a exterior film 100 Lithium Batteries
Claims
1. A battery element having a positive electrode using manganese dioxide, a negative electrode using lithium, and a separator provided between the positive electrode and the negative electrode; an exterior body in which the battery element is housed; An electrolyte solution contained in the exterior body; Including, The electrolyte solution is A component including a lithium electrolyte salt and a solvent including ethylene carbonate; a phosphazene compound having an -OR group (R is a hydrocarbon) bonded to a phosphorus atom; Including, lithium batteries.
2. 2. The lithium battery according to claim 1, wherein the phosphazene compound is a cyclic phosphazene compound represented by the following formula (1): (NPX) 2 ) 3 ・・・(1) [In the formula (1), of the six X's, five are fluorine, and one is the -OR group which is an ethoxy group or a phenoxy group.]
3. 2. The lithium battery according to claim 1, wherein the electrolyte has a viscosity of 2.0 mPa·s or less at 25° C.
4. 2. The lithium battery according to claim 1, wherein the phosphazene compound is further added to the component in an amount equivalent to 2% by volume or more and 50% by volume or less of the component.
5. 2. The lithium battery of claim 1, wherein the solvent further contains propylene carbonate and 1,2-dimethoxyethane.
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP2009016107A