Adhesive sheet, laminate, and display body
The pressure-sensitive adhesive sheet with a layered structure addresses deformation and optical unevenness issues by ensuring effective adherence to uneven surfaces, improving display module design and image quality.
Patent Information
- Application Number
- JP2023044364
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing adhesive layers in display modules deform to follow uneven surfaces, leading to optical unevenness and blistering issues, which affect image quality and design unity.
A pressure-sensitive adhesive sheet with a layered structure that includes an adhesive layer with specific physical properties, such as unevenness tracking rates and total light transmittance, to effectively follow irregularities while maintaining optical clarity and blister resistance.
The adhesive sheet ensures excellent blister resistance and suppresses optical unevenness, enhancing the design unity and image quality of display modules by effectively adhering to uneven surfaces.
Smart Images

Figure 2024134184000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive sheet, a laminate, and a display. [Background technology]
[0002] In recent years, automobile instrument panels, car navigation systems, various instruments installed in consoles, and various mobile electronic devices such as smartphones and tablet terminals are equipped with displays (displays) that use display modules having liquid crystal elements, light-emitting diodes (LED elements), organic electroluminescence (organic EL) elements, etc.
[0003] Such a display module, or a laminate of a display module and another member, is generally formed by bonding the display component and the other member with the adhesive layer of an adhesive sheet.
[0004] For such displays, there is a demand for improving the design of the display by providing a sense of unity between the display and peripheral members of the display, such as a frame material, when the display is turned off.
[0005] Patent Document 1 discloses that an optical filter laminated on a plasma display panel body has a colored layer, and the colored layer has an adhesive and a coloring dye. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-234028 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the invention described in Patent Document 1, the colored layer is provided so as to be in contact with the transparent substrate and the concealing layer formed in a frame shape on the transparent substrate. Therefore, the adhesive constituting the colored layer needs to sufficiently conform to the irregularities caused by the concealing layer and fill the irregularities so that no gaps or the like are generated near the irregularities.
[0008] However, when the adhesive conforms to the unevenness, the adhesive may be deformed. When such deformation occurs, the optical properties of the adhesive change, causing optical unevenness (e.g., color unevenness) in the light passing through the adhesive layer. As a result, optical unevenness also occurs in the image displayed on the display.
[0009] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide an adhesive sheet having an adhesive layer that conforms well to unevenness, has excellent blister resistance, and is free of optical unevenness. [Means for solving the problem]
[0010] The aspects of the present invention are as follows.
[0011] [1] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding a first member and a second member, The total light transmittance of the pressure-sensitive adhesive layer is 85% or less, When one main surface of the pressure-sensitive adhesive layer is designated as side A and the other main surface is designated as side B, when side A is bonded to an adherend having an uneven surface, the side A unevenness-following rate (%), which indicates the ability of side A to conform to the unevenness, is different from the side B unevenness-following rate (%), which indicates the ability of side B to conform to the unevenness when side B is bonded to an adherend having an uneven surface, The pressure-sensitive adhesive sheet has an A-side unevenness conforming rate and a B-side unevenness conforming rate of more than 0%.
[0012] [2] The pressure-sensitive adhesive sheet according to [1], wherein the pressure-sensitive adhesive layer is composed of two or more layers.
[0013] [3] The pressure-sensitive adhesive sheet according to [1] or [2], wherein the value obtained by subtracting the B-side unevenness tracking rate from the A-side unevenness tracking rate is -20 points or more and -1 point or less.
[0014] [4] The pressure-sensitive adhesive sheet according to any one of [1] to [3], wherein the pressure-sensitive adhesive layer contains a coloring component.
[0015] [5] The pressure-sensitive adhesive sheet according to any one of [1] to [4], wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive having a crosslinked structure.
[0016] [6] A laminate comprising a first member, a second member, and a pressure-sensitive adhesive layer that bonds the first member and the second member to each other, At least one of the first member and the second member has projections and recesses; The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to any one of [1] to [5].
[0017] [7] A display comprising the laminate described in [6]. Effect of the Invention
[0018] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet including a pressure-sensitive adhesive layer which conforms well to irregularities, has excellent blister resistance, and is free of optical unevenness. [Brief description of the drawings]
[0019] [Figure 1A] FIG. 1A is a cross-sectional view of an example of a pressure-sensitive adhesive sheet according to the present embodiment. [Figure 1B] FIG. 1B is a cross-sectional view of another example of the pressure-sensitive adhesive sheet according to the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the laminate according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, the present invention will be described in detail based on specific embodiments.
[0021] (1. Adhesive sheet) As shown in Fig. 1A, the adhesive sheet 1 according to this embodiment has an adhesive layer 10 and release sheets 21 and 22. The adhesive layer bonds a first member and a second member. In this embodiment, the first member and the second member are members that constitute a display body (display body constituent members).
[0022] The display body is constructed by laminating display body components having a predetermined function, and each display body component is bonded via an adhesive layer. In this case, the display body component itself may have unevenness, or unevenness may be formed on the display body component. If the adhesive layer cannot follow the unevenness, the adhesive layer will rise near the unevenness, causing gaps, etc., resulting in a decrease in the image quality of the display body. Therefore, the adhesive layer is required to be bonded while sufficiently following the unevenness.
[0023] In addition, some of the display component parts are made of plastic, rather than glass. When the material is changed to plastic, there is a problem that when the display component parts bonded with the adhesive layer are exposed to a high-temperature and high-humidity environment, outgassing from the plastic occurs, causing blisters such as air bubbles, lifting, and peeling. Therefore, the adhesive layer is also required to have blister resistance.
[0024] On the other hand, in order to improve the design of a display, for example, the boundaries between the components of the display are made less visible, giving a sense of unity between the frame material of the display and the display when the display is turned off. Such a sense of unity is given by controlling the optical properties (for example, total light transmittance) of the pressure-sensitive adhesive layer.
[0025] However, in the vicinity of the unevenness, the adhesive layer may deform to follow the unevenness. When such deformation occurs, the optical properties of the adhesive layer may change, and the optical properties may differ between the deformed portion and the non-deformed portion. As a result, the light passing through the adhesive layer may be affected, and optical unevenness may occur in the display. An example of such optical unevenness is color unevenness when the adhesive layer is colored. When optical unevenness such as color unevenness occurs, the design and image quality of the display may be reduced, which is not preferable.
[0026] In order to address the above problems, in this embodiment, the pressure-sensitive adhesive layer is as follows: The pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment can sufficiently conform to the irregularities while suppressing optical unevenness even in the vicinity of the irregularities, and can also provide good blister resistance.
[0027] (2. Adhesive Layer) The adhesive layer of the adhesive sheet according to this embodiment is composed of an adhesive described below. The adhesive layer may be composed of one layer (single layer) or may be composed of two or more layers. In this embodiment, from the viewpoint of easily achieving the physical properties described below, it is preferable that the adhesive layer is composed of two or more layers.
[0028] The thickness of the pressure-sensitive adhesive layer is preferably 1 to 2000 μm, more preferably 10 to 1200 μm, even more preferably 40 to 900 μm, particularly preferably 80 to 600 μm, even more preferably 100 to 400 μm, and most preferably 150 to 250 μm. When the pressure-sensitive adhesive layer is composed of multiple layers, the above thickness is the total thickness of the multiple layers.
[0029] When the pressure-sensitive adhesive layer is composed of multiple layers, the thickness of each pressure-sensitive adhesive layer is preferably 1 to 1000 μm, more preferably 10 to 600 μm, further preferably 20 to 300 μm, and particularly preferably 25 to 200 μm.
[0030] (2.1. Physical properties of adhesive layer) The pressure-sensitive adhesive layer according to this embodiment has the following physical properties. When the pressure-sensitive adhesive layer is a multi-layer structure, the following physical properties are those of the entire pressure-sensitive adhesive layer.
[0031] (2.1.1. Contour rate of adhesive layer) In this embodiment, of the main surfaces of the adhesive layer, one of the main surfaces is surface A and the other is surface B. In Fig. 1A, main surface 10a of adhesive layer 10 is surface A, and main surface 10b is surface B. Surfaces A and B are surfaces to be attached to a display member.
[0032] In this embodiment, the unevenness tracking rate on side A (side A unevenness tracking rate) and the unevenness tracking rate on side B (side B unevenness tracking rate) are controlled. The unevenness tracking rate is an index of the extent to which the adhesive layer tracks unevenness such as steps of an adherend when it is attached to the adherend (a display member constituting member). The higher the unevenness tracking rate, the more the unevenness is embedded in the adhesive layer even in the vicinity of unevenness with a large height difference, and the adhesive layer can be attached without forming gaps or the like at the interface between the adhesive layer and the unevenness. The unevenness tracking rate can be calculated by the following formula. Unevenness conformance rate (%) = {(height of step that remains filled without bubbles, lifting, peeling, etc. after a specified durability test (μm)) / (thickness of adhesive layer (μm))} × 100
[0033] The method for testing the unevenness-conforming rate is as shown in the test examples described later. When the pressure-sensitive adhesive layer is composed of an active energy ray-curable pressure-sensitive adhesive, the unevenness-conforming rate is the unevenness-conforming rate when the pressure-sensitive adhesive layer is attached to an adherend and then cured with active energy rays.
[0034] In this embodiment, the A-side unevenness conforming rate of the pressure-sensitive adhesive layer is different from the B-side unevenness conforming rate of the pressure-sensitive adhesive layer, and the A-side unevenness conforming rate and the B-side unevenness conforming rate are greater than 0%. The A-side unevenness conforming rate and the B-side unevenness conforming rate of the pressure-sensitive adhesive layer satisfy the above relationship, so that the pressure-sensitive adhesive layer can sufficiently conform to the unevenness while suppressing unevenness in optical properties caused by the unevenness. Furthermore, blister resistance is also improved.
[0035] The A-side unevenness conforming rate and the B-side unevenness conforming rate are preferably 1% to 50%, more preferably 2% to 40%, further preferably 3% to 30%, and particularly preferably 4% to 20%.
[0036] Furthermore, the difference between the A-side unevenness tracking rate and the B-side unevenness tracking rate (A-side unevenness tracking rate-B-side unevenness tracking rate) is preferably -20 to -1 points, more preferably -15 to -1.5 points, and even more preferably -10 to -2 points.
[0037] (2.1.2. Total light transmittance of adhesive layer) The pressure-sensitive adhesive layer according to this embodiment has a total light transmittance of 85% or less, which improves the design of the display.
[0038] From the viewpoint of visibility, the total light transmittance is preferably 3% or more, more preferably 10% or more, even more preferably 25% or more, particularly preferably 30% or more, and more preferably 35% or more. From the viewpoint of design, the total light transmittance is preferably 75% or less, more preferably 65% or less, even more preferably 55% or less, and particularly preferably 50% or less. In this specification, the total light transmittance is a value measured in accordance with JISK7361-1:1997. In addition, when the adhesive layer is composed of an active energy ray-curable adhesive, the total light transmittance is the total light transmittance when the adhesive layer is cured with active energy rays after being attached to the adherend.
[0039] (2.1.3. Haze value of adhesive layer) The haze value of the pressure-sensitive adhesive layer according to the present embodiment is preferably 0 to 80%, more preferably 0.1 to 60%, even more preferably 0.5 to 40%, particularly preferably 1 to 20%, and more preferably 1.5 to 10%, from the viewpoint of easily achieving a desired total light transmittance and achieving both concealment and visibility. The haze value in this specification is a value measured in accordance with JISK7136:2000. In addition, when the pressure-sensitive adhesive layer is composed of an active energy ray-curable pressure-sensitive adhesive, the haze value is the haze value when the pressure-sensitive adhesive layer is cured with active energy rays after being attached to an adherend.
[0040] (2.1.4. Adhesive strength of adhesive layer) In this embodiment, the adhesive strength of the A-side of the adhesive layer to soda lime glass (hereinafter also referred to as the A-side adhesive strength) is preferably 1 N / 25 mm or more and 100 N / 25 mm or less. This ensures sufficient adhesion to the adherend to be bonded, and makes it easy to achieve good step conformability and good blister resistance.
[0041] From the above viewpoints, the A-side adhesive strength is more preferably 5 to 70 N / 25 mm, and further preferably 10 to 50 N / 25 mm.
[0042] In this embodiment, the adhesive strength of the B side of the adhesive layer to soda lime glass (hereinafter also referred to as the B side adhesive strength) is preferably 1 N / 25 mm or more and 100 N / 25 mm or less. This ensures sufficient adhesion to the adherend to be bonded, and makes it easy to achieve good step conformability and good blister resistance.
[0043] From the above viewpoints, the B-side adhesive strength is more preferably from 5 to 70 N / 25 mm, and even more preferably from 10 to 50 N / 25 mm.
[0044] The adhesive strength may be measured by a 180-degree peeling method in accordance with JIS Z0237: 2009. A specific measurement method is as shown in the test examples described later.
[0045] (2.2. When the adhesive layer is two layers) As described above, the adhesive layer according to the present embodiment preferably has two or more layers. Therefore, the case where the adhesive layer has two layers will be described below. When the adhesive layer has two layers, the adhesive sheet 1 according to the present embodiment has an adhesive layer 10 (a first adhesive layer 11 and a second adhesive layer 12) and release sheets 21 and 22, as shown in FIG. 1B.
[0046] The first pressure-sensitive adhesive layer 11 and the second pressure-sensitive adhesive layer 12 are laminated to form the pressure-sensitive adhesive layer 10. In this embodiment, the main surface 11a of the first pressure-sensitive adhesive layer 11 that is bonded to an adherend is referred to as side A, and the main surface 12a of the second pressure-sensitive adhesive layer 12 that is bonded to an adherend is referred to as side B.
[0047] (2.3. Physical Properties of the First Adhesive Layer and the Second Adhesive Layer) The physical properties of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are not particularly limited so long as the physical properties of the pressure-sensitive adhesive layer as a whole satisfy the above-mentioned physical properties.
[0048] (2.3.1.Total light transmittance) In this embodiment, when the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are layers for making it easier to satisfy the visibility of the entire pressure-sensitive adhesive layer, the total light transmittance is preferably 85 to 100%, more preferably 88 to 96%, and even more preferably 90 to 93%. When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are layers for making it easier to satisfy the design of the entire pressure-sensitive adhesive layer, the total light transmittance is preferably 3 to 85%, more preferably 10 to 80%, even more preferably 30 to 75%, particularly preferably 50 to 70%, and of these, preferably 55 to 68%. When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are active energy ray curable, the total light transmittance before and after active energy ray irradiation is preferably within the above range. This makes it easier to satisfy the optical properties required for the entire pressure-sensitive adhesive layer.
[0049] (2.3.2. Haze Value) In this embodiment, the haze value of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer is preferably 0 to 80%, more preferably 0.01 to 40%, even more preferably 0.05 to 10%, and even more preferably 0.1 to 2%. When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are active energy ray curable, the haze value before and after the active energy ray irradiation is preferably within the above range. This makes it easier to satisfy the optical properties required for the entire pressure-sensitive adhesive layer.
[0050] (2.3.3. Storage Modulus) In this embodiment, the storage modulus G' at 25°C of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer is preferably 0.01 to 10 MPa, more preferably 0.04 to 5 MPa, even more preferably 0.08 to 2 MPa, particularly preferably 0.1 to 1.5 MPa, and of these, preferably 0.15 to 1.1 MPa.
[0051] When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are active energy ray-curable, the storage modulus Gb' at 25°C before active energy ray irradiation is preferably 0.01 to 1 MPa, more preferably 0.03 to 0.5 MPa, and even more preferably 0.05 to 0.2 MPa. On the other hand, the storage modulus Ga' at 25°C after active energy ray irradiation is preferably 0.01 to 10 MPa, more preferably 0.04 to 5 MPa, even more preferably 0.08 to 1 MPa, and particularly preferably 0.1 to 0.5 MPa.
[0052] This allows the first and second pressure-sensitive adhesive layers to have suitable viscoelasticity and good adhesion to the adherend such as a display member, and also makes it easy to adjust the above-mentioned adhesive strength to a desired range, thereby exhibiting good irregularity-following ability and blister resistance. In particular, it is easy to satisfy the storage modulus ratio described later, and in the vicinity of the irregularities, optical unevenness is suppressed while the layers follow the irregularities well.
[0053] Furthermore, when one of the first and second adhesive layers contains a coloring component described below and the other does not contain a coloring component, the ratio (G1b' / G2b') of the storage modulus G1b' of the adhesive layer containing the coloring component at 25°C before active energy ray irradiation to the storage modulus G2b' of the adhesive layer not containing the coloring component at 25°C before active energy ray irradiation is preferably 1.1 to 10,000, more preferably 1.2 to 1,000, even more preferably 1.3 to 100, and even more preferably 1.4 to 50, and among these, preferably 1.5 to 25 and most preferably 1.6 to 15.
[0054] When one of the first and second adhesive layers contains a coloring component described below and the other does not contain a coloring component, the ratio (G1a' / G2a') of the storage modulus G1a' of the adhesive layer containing the coloring component at 25°C after irradiation with active energy rays to the storage modulus G2a' of the adhesive layer not containing the coloring component at 25°C before irradiation with active energy rays is preferably 1.11 to 10,000, more preferably 1.15 to 1,000, even more preferably 1.2 to 100, and even more preferably 1.24 to 50, and of these, preferably 1.28 to 25 and most preferably 1.3 to 15.
[0055] By satisfying the above-mentioned ranges for G1b' / G2b' and G1a' / G2a', the resulting pressure-sensitive adhesive sheet is more likely to exhibit the desired physical properties, and exhibits good irregularity-following ability and blister resistance. In particular, in the vicinity of the irregularities, optical unevenness is suppressed while the sheet conforms well to the irregularities.
[0056] (2.3.4. Gel Fraction) In this embodiment, the gel fraction of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer is preferably 30 to 99%, more preferably 40 to 90%, even more preferably 45 to 85%, and particularly preferably 50 to 80%.
[0057] When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are active energy ray-curable, the gel fraction before active energy ray irradiation is preferably 20 to 80%, more preferably 30 to 70%, even more preferably 40 to 60%, and particularly preferably 45 to 53%, while the gel fraction after active energy ray irradiation is preferably 40 to 99%, more preferably 50 to 95%, even more preferably 55 to 90%, and particularly preferably 60 to 80%.
[0058] This allows the first and second pressure-sensitive adhesive layers to have suitable cohesiveness, and the adhesive strength and storage modulus described above can be easily adjusted to the desired range, resulting in good conformability to irregularities and blister resistance. In addition, the storage modulus ratio described above can be easily satisfied, and optical unevenness can be suppressed in the vicinity of the irregularities while good conformability to the irregularities.
[0059] (2.3.5.Adhesion) In this embodiment, as described above, side A is the main surface of the first adhesive layer and side B is the main surface of the second adhesive layer, so it is preferable that the adhesive strength of the first adhesive layer satisfies the above-mentioned range of side A adhesive strength, and it is preferable that the adhesive strength of the second adhesive layer satisfies the above-mentioned range of side B adhesive strength.
[0060] (2.4. Composition of the first adhesive layer and the second adhesive layer) As long as the adhesive layer according to the present embodiment is configured to have the above-mentioned physical properties, the composition of the first adhesive layer and the second adhesive layer is not particularly limited. For example, acrylic adhesives, polyester adhesives, polyurethane adhesives, rubber adhesives, and silicone adhesives are exemplified. The adhesive may be any of emulsion type, solvent type, and solventless type. Furthermore, the adhesive may be active energy ray curable or active energy ray non-curable. Furthermore, the adhesive may have a crosslinked structure or may not have a crosslinked structure. And, as the material constituting the adhesive, from the viewpoint of SDGs, a material with a high biomass degree may be used, a material that can be recycled or reused may be used, or a recycled or reused material may be used. The adhesives constituting the first adhesive layer and the second adhesive layer may be the same or different.
[0061] In this embodiment, from the viewpoint of ease of achieving the above-mentioned physical properties and from the viewpoints of adhesive properties, optical properties, etc., the adhesive constituting the first adhesive layer and the second adhesive layer is preferably an acrylic adhesive, and more preferably an acrylic adhesive having a crosslinked structure.
[0062] However, from the viewpoint of controlling the A-side unevenness conformance rate and the B-side unevenness conformance rate to be different, it is preferable that the adhesive constituting the first adhesive layer and the adhesive constituting the second adhesive layer have different adhesive compositions, and it is even more preferable that the monomer compositions of the main polymers are different.
[0063] The acrylic adhesive having a crosslinked structure is preferably an adhesive obtained by crosslinking an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A) and a crosslinking agent (B). Such an adhesive is likely to satisfy the above-mentioned physical properties and is likely to provide good adhesive strength. In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. In addition, the term "polymer" is also intended to include the concept of "copolymer."
[0064] (2.4.1. (Meth)acrylic acid ester polymers) The (meth)acrylic acid ester polymer (A) preferably contains, as a monomer unit constituting the polymer, a reactive functional group-containing monomer having in the molecule a reactive functional group that reacts with a crosslinking agent (B) described below. The reactive functional group derived from the reactive functional group-containing monomer reacts with the crosslinking agent (B) to form a crosslinked structure (three-dimensional network structure), and a pressure-sensitive adhesive having the desired cohesive strength can be obtained.
[0065] (2.4.1.1. Monomers containing reactive functional groups) As the reactive functional group-containing monomer, a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer) and the like are preferably mentioned. Among these, a hydroxyl group-containing monomer or a carboxyl group-containing monomer having excellent reactivity with the crosslinking agent (B) is preferable. In addition, a hydroxyl group-containing monomer and a carboxyl group-containing monomer may be used in combination.
[0066] Among these, from the viewpoint of the reactivity of the hydroxyl group in the resulting (meth)acrylic acid ester polymer (A) with the crosslinking agent (B) and copolymerizability with other monomers, a (meth)acrylic acid hydroxyalkyl ester having a hydroxyalkyl group having 1 to 4 carbon atoms is preferred. Specifically, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. are preferred, and 2-hydroxyethyl acrylate or 4-hydroxybutyl acrylate are particularly preferred. These may be used alone or in combination of two or more.
[0067] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among these, acrylic acid is preferred in terms of the reactivity of the carboxyl group in the resulting (meth)acrylic acid ester polymer (A) with the crosslinking agent (B) and copolymerizability with other monomers. These may be used alone or in combination of two or more.
[0068] Examples of the amino group-containing monomer include aminoethyl (meth)acrylate and n-butylaminoethyl (meth)acrylate. These may be used alone or in combination of two or more. The amino group-containing monomer excludes the nitrogen atom-containing monomer described below.
[0069] When the (meth)acrylic acid ester polymer (A) contains a reactive functional group-containing monomer as a monomer unit constituting the polymer, the (meth)acrylic acid ester polymer (A) preferably contains 1 to 40 mass %, more preferably 2 to 35 mass %, of the reactive functional group-containing monomer. In particular, when the reactive functional group-containing monomer is a hydroxyl group-containing monomer, the (meth)acrylic acid ester polymer (A) preferably contains 5 to 32 mass %, more preferably 10 to 30 mass %, even more preferably 15 to 28 mass %, and particularly preferably 18 to 26 mass % of the hydroxyl group-containing monomer. In addition, when the reactive functional group-containing monomer is a carboxyl group-containing monomer, the (meth)acrylic acid ester polymer (A) preferably contains 3 to 25 mass %, more preferably 4 to 15 mass %, and even more preferably 5 to 10 mass % of the carboxyl group-containing monomer. As a result, a good crosslinked structure is formed in the obtained pressure-sensitive adhesive, and a pressure-sensitive adhesive having a relatively high cohesive strength is obtained, and the pressure-sensitive adhesive has excellent blister resistance. Furthermore, the resulting pressure-sensitive adhesive is more likely to satisfy the desired adhesive properties, optical characteristics, and the like, and in particular, in the vicinity of the irregularities, the pressure-sensitive adhesive conforms well to the irregularities while suppressing optical unevenness.
[0070] It is also preferred that the (meth)acrylic acid ester polymer (A) does not contain a carboxyl group-containing monomer as a monomer unit constituting the polymer. Since a carboxyl group is an acid component, by not containing a carboxyl group-containing monomer, even if the target to which the pressure-sensitive adhesive is applied includes a material that may be damaged by acid, such as a transparent conductive film or a metal film, the damage (corrosion, change in resistance, etc.) caused by acid can be suppressed.
[0071] Here, "not containing a carboxyl group-containing monomer" means that the carboxyl group-containing monomer is not substantially contained, and in addition to not containing any carboxyl group-containing monomer at all, the carboxyl group-containing monomer may be contained to an extent that the carboxyl group does not cause corrosion of the transparent conductive film, metal wiring, etc. Specifically, the (meth)acrylic acid ester polymer (A) is allowed to contain the carboxyl group-containing monomer as a monomer unit in an amount of less than 0.1 mass%, preferably 0.05 mass% or less, more preferably 0.01 mass% or less.
[0072] (2.4.1.2. (Meth)acrylic acid alkyl esters) The (meth)acrylic acid ester polymer (A) preferably contains, as a monomer unit constituting the polymer, a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms. This allows the adhesive to exhibit preferred adhesiveness. In addition, the (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms preferably has a linear or branched chain structure from the viewpoint of exhibiting more preferred adhesiveness.
[0073] Examples of (meth)acrylic acid alkyl esters having an alkyl group with 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate.
[0074] Among these, from the viewpoint of further improving adhesion, (meth)acrylic acid esters having an alkyl group with 1 to 12 carbon atoms are preferred, and (meth)acrylic acid esters having an alkyl group with 1 to 8 carbon atoms are more preferred. Specifically, methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (meth)acrylate are preferred, and methyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate are particularly preferred. These may be used alone or in combination of two or more.
[0075] The (meth)acrylic acid ester polymer (A) preferably contains 30 to 99 mass % of (meth)acrylic acid alkyl ester having an alkyl group carbon number of 1 to 20 as a monomer unit constituting the polymer, more preferably 40 to 90 mass %, further preferably 50 to 80 mass %, and particularly preferably 55 to 70 mass %. This allows other monomer components for expressing desired properties to be introduced into the (meth)acrylic acid ester polymer (A) in a desired amount, making it easy to impart suitable adhesive properties, optical properties, etc. to the resulting pressure-sensitive adhesive. In particular, it has excellent unevenness-following ability and blister resistance, and in the vicinity of the unevenness, it follows the unevenness well while suppressing optical unevenness.
[0076] It is also preferable that the (meth)acrylic acid ester polymer (A) contains a monomer having an alicyclic structure in the molecule (an alicyclic structure-containing monomer) as a monomer unit constituting the polymer. Since the alicyclic structure-containing monomer is bulky, it is presumed that the presence of this in the polymer increases the distance between the polymers, and the resulting adhesive can have excellent flexibility. This makes it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, and improves unevenness-following ability.
[0077] The carbon ring of the alicyclic structure in the alicyclic structure-containing monomer may be a saturated structure or may have an unsaturated bond in a part thereof. The alicyclic structure may be a monocyclic alicyclic structure or a polycyclic alicyclic structure (polycyclic structure) such as a bicyclic or tricyclic structure. From the viewpoint of making the distance between the obtained (meth)acrylic acid ester polymer (A) appropriate and imparting high stress relaxation properties to the adhesive, the alicyclic structure is preferably a polycyclic structure. Furthermore, in consideration of the compatibility of the (meth)acrylic acid ester polymer (A) with other components, the polycyclic structure is particularly preferably a bicyclic to tetracyclic structure. Also, from the viewpoint of imparting stress relaxation properties and compatibility as described above, the carbon number of the alicyclic structure (meaning the total carbon number of the portion forming the ring, and when multiple rings exist independently, the total carbon number) is usually preferably 5 to 15, more preferably 7 to 10.
[0078] Specific examples of the alicyclic structure-containing monomer include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, etc. Among them, dicyclopentanyl (meth)acrylate (alicyclic structure carbon number: 10), adamantyl (meth)acrylate (alicyclic structure carbon number: 10) or isobornyl (meth)acrylate (alicyclic structure carbon number: 7) are preferred, with isobornyl (meth)acrylate being particularly preferred, and isobornyl acrylate being even more preferred. These may be used alone or in combination of two or more.
[0079] When the (meth)acrylic acid ester polymer (A) contains an alicyclic structure-containing monomer as a monomer unit constituting the polymer, the alicyclic structure-containing monomer is preferably contained in an amount of 1 to 30 mass%, more preferably 3 to 26 mass%, further preferably 6 to 22 mass%, and particularly preferably 9 to 18 mass%. This makes it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, and improves the unevenness-following ability. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the unevenness is followed well.
[0080] It is also preferred that the (meth)acrylic acid ester polymer (A) contains a nitrogen atom-containing monomer as a monomer unit constituting the polymer. By making the nitrogen atom-containing monomer exist as a constituent unit in the polymer, a predetermined polarity is imparted to the adhesive, and it can be made to have excellent affinity even for an adherend having a certain degree of polarity. As the nitrogen atom-containing monomer, from the viewpoint of imparting an appropriate rigidity to the (meth)acrylic acid ester polymer (A), a monomer having a nitrogen-containing heterocycle is preferred. In addition, from the viewpoint of increasing the degree of freedom of the portion derived from the nitrogen atom-containing monomer in the higher-order structure of the adhesive that is constituted, it is preferred that the nitrogen atom-containing monomer does not contain a reactive unsaturated double bond group other than one polymerizable group used in polymerization to form the (meth)acrylic acid ester polymer (A).
[0081] Examples of monomers having a nitrogen-containing heterocycle include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Among these, N-(meth)acryloylmorpholine, which exhibits superior adhesion, is preferred, and N-acryloylmorpholine is particularly preferred. These may be used alone or in combination of two or more.
[0082] When the (meth)acrylic acid ester polymer (A) contains a nitrogen atom-containing monomer as a monomer unit constituting the polymer, the nitrogen atom-containing monomer is preferably contained in an amount of 1 to 20 mass%, more preferably 2 to 16 mass%, further preferably 3 to 12 mass%, and particularly preferably 4 to 8 mass%. This makes it easier to satisfy the physical properties such as the unevenness-following rate and adhesive strength described above, and improves the unevenness-following ability. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the unevenness is followed well.
[0083] The (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting the polymer, if desired. As the other monomers, monomers not containing reactive functional groups are preferred so as not to inhibit the above-mentioned action of the reactive functional group-containing monomer. Examples of such monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.
[0084] The (meth)acrylic acid ester polymer (A) is preferably a linear polymer, which is expected to facilitate entanglement of molecular chains and improve cohesive strength, making it easier to satisfy the physical properties such as the conformability and adhesive strength described above, resulting in good conformability.
[0085] The (meth)acrylic acid ester polymer (A) is preferably a solution polymer obtained by a solution polymerization method. This makes it easier to obtain a high molecular weight polymer, and is expected to improve the cohesive force, making it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, resulting in good unevenness-following ability. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the unevenness is well followed.
[0086] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.
[0087] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 100,000 to 3,000,000, and more preferably 200,000 to 2,500,000. When the monomer unit constituting the (meth)acrylic acid ester polymer (A) does not contain a carboxyl group but contains a hydroxyl group-containing monomer, the weight average molecular weight is preferably 300,000 to 1,800,000, more preferably 350,000 to 1,200,000, even more preferably 400,000 to 900,000, and particularly preferably 450,000 to 750,000. When the monomer unit constituting the (meth)acrylic acid ester polymer (A) does not contain a hydroxyl group-containing monomer but contains a carboxyl group, the weight average molecular weight is preferably 500,000 to 2,300,000, more preferably 1,000,000 to 2,200,000, and even more preferably 1,500,000 to 2,100,000. This makes it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, and the unevenness-following ability is improved. In particular, optical unevenness is suppressed while following the unevenness well in the vicinity of the unevenness. In this specification, the weight average molecular weight is a value measured by gel permeation chromatography (GPC) and converted into standard polystyrene.
[0088] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more kinds.
[0089] (2.4.2. Crosslinker (B)) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) by heating the pressure-sensitive adhesive composition P, and can form a three-dimensional network structure well. This improves the cohesive strength of the resulting pressure-sensitive adhesive, making it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, and improves the unevenness-following ability. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the unevenness is well followed.
[0090] The crosslinking agent (B) may be any that reacts with the reactive group of the (meth)acrylic acid ester polymer (A). For example, isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, ammonium salt-based crosslinking agents, etc. are exemplified. When the reactive functional group of the (meth)acrylic acid ester polymer (A) is a hydroxyl group, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with the hydroxyl group. On the other hand, when the reactive functional group of the (meth)acrylic acid ester polymer (A) is a carboxyl group, it is preferable to use an epoxy-based crosslinking agent that has excellent reactivity with the carboxyl group, and it is also preferable to use an isocyanate-based crosslinking agent from the viewpoint of easily obtaining a desired crosslinked structure. The crosslinking agent (B) may be used alone or in combination of two or more.
[0091] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and their biuret and isocyanurate forms, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate and trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.
[0092] Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. Among these, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane is preferred from the viewpoint of reactivity with carboxy groups.
[0093] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition P is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, even more preferably 0.08 to 1 part by mass, and particularly preferably 0.12 to 0.5 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This allows the resulting pressure-sensitive adhesive to exhibit good cohesive strength, making it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, resulting in good unevenness-following ability. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the unevenness is well followed.
[0094] (2.4.3. Active energy ray-curable component (C)) In this embodiment, when the adhesive constituting the first adhesive layer and the second adhesive layer is active energy ray curable, the adhesive composition P preferably contains an active energy ray curable component (C). In the adhesive obtained by crosslinking the adhesive composition P and further curing the adhesive by active energy rays, it is presumed that the active energy ray curable component (C) polymerized with each other is entangled in the crosslinked structure (three-dimensional network structure) formed by crosslinking the (meth)acrylic acid ester polymer (A) and the crosslinking agent (B). The adhesive having such a high-order structure is easy to satisfy the above-mentioned physical properties such as unevenness-following rate and adhesive strength, and is excellent in unevenness-following property and blister resistance. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while following the unevenness well.
[0095] The active energy ray curable component (C) is not particularly limited as long as it is a component that cures by irradiation with active energy rays and can obtain the above-mentioned effects, and may be any of a monomer, an oligomer, or a polymer, or a mixture thereof. Among these, polyfunctional acrylate monomers are preferred from the viewpoint of easily satisfying the physical properties such as the above-mentioned unevenness tracking rate and adhesive strength, and from the viewpoint of easily improving blister resistance. In addition, from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A), the polyfunctional acrylate monomer is preferably one having a molecular weight of less than 1000.
[0096] As the polyfunctional acrylate monomer, a difunctional, trifunctional, tetrafunctional, pentafunctional or hexafunctional acrylate monomer is preferable.
[0097] Examples of bifunctional acrylate monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene.
[0098] Examples of trifunctional acrylate monomers include trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate.
[0099] Examples of tetrafunctional acrylate monomers include diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate. Examples of pentafunctional acrylate monomers include propionic acid modified dipentaerythritol penta(meth)acrylate. Examples of hexafunctional acrylate monomers include dipentaerythritol hexa(meth)acrylate and caprolactone modified dipentaerythritol hexa(meth)acrylate.
[0100] Among these, from the viewpoint of the blister resistance of the resulting pressure-sensitive adhesive, preferred are polyfunctional acrylate monomers containing an isocyanurate structure in the molecule, such as di(acryloxyethyl)isocyanurate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, or polyfunctional acrylate monomers containing a cyclic structure (particularly a cycloalkane structure) in the molecule, such as tricyclodecane dimethanol (meth)acrylate. Polyfunctional acrylate monomers having three or more functionalities and containing an isocyanurate structure in the molecule are also preferred. More preferred are acrylate monomers, or polyfunctional acrylate monomers having two or more functionalities and containing a polycyclic structure (particularly a polycyclic structure of a cycloalkane) in the molecule, particularly preferred are ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate or tricyclodecane dimethanol (meth)acrylate, further preferred are ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate or tricyclodecane dimethanol acrylate, and most preferred are ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate. These may be used alone or in combination of two or more.
[0101] The content of the active energy ray curable component (C) in the adhesive composition P is preferably 1 to 40 parts by mass, more preferably 3 to 32 parts by mass, even more preferably 6 to 24 parts by mass, and particularly preferably 9 to 16 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This improves the cohesive force after irradiation with active energy rays, making it easier to satisfy the physical properties such as the above-mentioned unevenness-following rate and adhesive strength, resulting in more excellent blister resistance and unevenness-following ability. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the unevenness is well followed.
[0102] (2.4.4. Photopolymerization initiator (D)) In this embodiment, when the adhesive composition P contains an active energy ray curable component (C) and ultraviolet light is used as the active energy ray, the adhesive composition P preferably contains a photopolymerization initiator (D), which allows the active energy ray curable component (C) to be cured efficiently and reduces the polymerization curing time and the ultraviolet light irradiation dose.
[0103] Examples of the photopolymerization initiator (D) include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4 '-Diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1[4-(1-methylvinyl)phenyl]propanone], 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, etc. These may be used alone or in combination of two or more.
[0104] Among the above, phosphine oxide-based photopolymerization initiators are preferred from the viewpoint of being easily cleaved when irradiated with ultraviolet light and being easy to reliably cure the adhesive. Specifically, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, etc. are preferred. Some optical components that serve as adherends have ultraviolet light shielding properties, but even when ultraviolet light is irradiated through such ultraviolet light shielding components that are difficult for ultraviolet light to pass through, the above-mentioned phosphine oxide-based photopolymerization initiators can promote the curing of the active energy ray curable component (C).
[0105] The content of the photopolymerization initiator (D) in the adhesive composition P is preferably 1 to 30 parts by mass, more preferably 4 to 22 parts by mass, and even more preferably 8 to 15 parts by mass, relative to 100 parts by mass of the active energy ray curable component (C). This makes it easier for the resulting adhesive sheet to satisfy the desired physical properties and to have excellent irregularity-following ability and blister resistance. In particular, in the vicinity of the irregularities, optical unevenness is suppressed while the sheet follows the irregularities well.
[0106] (2.4.5. Coloring component (E)) In this embodiment, at least one of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer preferably contains a coloring component (E). When a plurality of layers contain the coloring component (E), the coloring components may be the same or different. By containing the coloring component (E), the total light transmittance and haze value of the pressure-sensitive adhesive layer can be adjusted to a desired range, and the design of the display to which the pressure-sensitive adhesive layer is attached can be improved. When the pressure-sensitive adhesive layer is a single layer, it is preferable that the pressure-sensitive adhesive layer contains a coloring component (E). When the pressure-sensitive adhesive layer is composed of three or more layers, it is preferable that at least one layer contains a coloring component (E).
[0107] The coloring component (E) may be a pigment or a dye. The pigment may be an inorganic pigment or an organic pigment. From the viewpoint of the durability of the resulting adhesive, inorganic pigments are preferred. The color of the coloring component (E) can be appropriately selected depending on the purpose, but generally, a dark or deep color such as black, brown, navy blue, purple, or blue is preferred, and black is particularly preferred.
[0108] Examples of inorganic pigments include carbon black, cobalt-based pigments, iron-based pigments, chromium-based pigments, titanium-based pigments, vanadium-based pigments, zirconium-based pigments, molybdenum-based pigments, ruthenium-based pigments, platinum-based pigments, ITO (indium tin oxide)-based pigments, and ATO (antimony tin oxide)-based pigments.
[0109] Examples of organic pigments and organic dyes include aminium-based dyes, cyanine-based dyes, merocyanine-based dyes, croconium-based dyes, squalium-based dyes, azulenium-based dyes, polymethine-based dyes, naphthoquinone-based dyes, pyrylium-based dyes, phthalocyanine-based dyes, naphthalocyanine-based dyes, naphtholactam-based dyes, azo-based dyes, condensed azo-based dyes, indigo-based dyes, perinone-based dyes, perylene-based dyes, dioxazine-based dyes, quinacridone-based dyes, isoindolinone-based dyes, quinophthalone-based dyes, pyrrole-based dyes, thioindigo-based dyes, metal complex-based dyes (metal complex dyes), dithiol metal complex-based dyes, indolephenol-based dyes, triarylmethane-based dyes, anthraquinone-based dyes, dioxazine-based dyes, naphthol-based dyes, azomethine-based dyes, benzimidazolone-based dyes, pyranthrone-based dyes, and threne-based colors.
[0110] Examples of black pigments include carbon black, copper oxide, iron oxide, manganese dioxide, aniline black, activated carbon, etc. Examples of black dyes include high-concentration vegetable dyes and azo dyes.
[0111] The above pigments or dyes can be used in appropriate mixtures so as to obtain the desired physical properties in the pressure-sensitive adhesive layer.
[0112] Among the above coloring components (E), carbon black, nigrosine-based black dyes, and chromate-based black dyes are preferred from the viewpoint of easily satisfying the above-mentioned physical properties and enhancing the design of the display body. The carbon black may or may not be subjected to a predetermined treatment (for example, a solvent-philic treatment) on its surface.
[0113] From the viewpoint of optical properties, the coloring component (E) preferably satisfies the following properties.
[0114] The coloring component (E) is preferably one in which the average haze, which is the average value of the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, of a solution obtained by diluting the coloring component 10,000 times with ethyl acetate, is 1 to 60%, more preferably 2 to 40%, even more preferably 3 to 20%, and particularly preferably 4 to 10%. By using an appropriate amount of such a coloring component (E), the optical properties (total light transmittance, haze value, etc.) of the pressure-sensitive adhesive layer described above are easily satisfied.
[0115] Furthermore, the coloring component (E) is preferably one in which the difference between the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm of a solution obtained by diluting the coloring component 10,000 times with ethyl acetate is 0 to 30 points, more preferably 0.1 to 22 points, particularly preferably 0.5 to 14 points, and further preferably 1 to 8 points. By using an appropriate amount of such a coloring component, the optical properties (total light transmittance, haze value, etc.) of the pressure-sensitive adhesive layer described above are easily satisfied.
[0116] The haze value at a wavelength of 780 nm of a solution obtained by diluting the coloring component (E) 10,000 times with ethyl acetate is preferably 0.1 to 50%, more preferably 0.5 to 35%, particularly preferably 1 to 20%, and even more preferably 2 to 10%. The haze value at a wavelength of 380 nm of a solution obtained by diluting the coloring component 10,000 times with ethyl acetate is preferably 1 to 60%, more preferably 3 to 45%, particularly preferably 6 to 30%, and even more preferably 10 to 20%. This makes it easier for the optical properties (total light transmittance, haze value, etc.) of the pressure-sensitive adhesive layer to be satisfied.
[0117] Furthermore, the standard deviation of the haze value at each wavelength at 5 nm intervals in the wavelength range of 380 nm to 780 nm (i.e., 380 nm, 385 nm, 390 nm, . . ., 775 nm, 780 nm) of a solution obtained by diluting the coloring component (E) 10,000 times with ethyl acetate is preferably 0.1 to 10, more preferably 0.5 to 6, and particularly preferably 1 to 3. This makes it easier for the pressure-sensitive adhesive layer to satisfy the optical properties (total light transmittance, haze value, etc.) described above.
[0118] The content of the coloring component (E) is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, even more preferably 0.1 to 1 part by mass, and particularly preferably 0.2 to 0.5 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier to satisfy the above-mentioned optical properties, and also makes it easier to satisfy the irregularity tracking rate since the desired adhesive strength and cohesive strength are maintained. In particular, in the vicinity of the irregularities, optical unevenness is suppressed while the irregularities are tracked well.
[0119] (2.4.6. Other Additives) The adhesive composition P may contain other additives as necessary. Examples of such additives include silane coupling agents, ultraviolet absorbers, antistatic agents, tackifiers, antioxidants, light stabilizers, rust inhibitors, infrared absorbers, softeners, fillers, and refractive index adjusters. Note that polymerization solvents and dilution solvents described below are not included in the additives constituting the adhesive composition P.
[0120] (2.5. Other configurations of the adhesive layer) 1A, when the adhesive layer 10 is composed of one layer, the adhesive constituting the adhesive layer 10 may be composed of the above-mentioned adhesive composition P. In addition, an example of a method for making the A-side unevenness conforming rate and the B-side unevenness conforming rate different from each other is a method of forming a gradient structure in which the hardness of the adhesive changes in the thickness direction from the A-side side to the B-side side.
[0121] In addition, as an example of a case where the adhesive layer is composed of two layers, the configuration in which the first adhesive layer and the second adhesive layer are in contact with each other as shown in FIG. 1B has been described, but the first adhesive layer and the second adhesive layer may not be in contact with each other. An example of such a configuration is, for example, a configuration in which the first adhesive layer and the second adhesive layer are laminated via a non-adhesive member. Specifically, an example is a configuration in which the first adhesive layer is formed on one main surface of a base material composed of a resin film or the like, and the second adhesive layer is formed on the other main surface.
[0122] When the adhesive layer is composed of three or more layers, the adhesive constituting each layer may be formed using the adhesive composition P described above so that the adhesive layer as a whole satisfies the above-mentioned physical properties.
[0123] (2.6. Release Sheet) The release sheets 21 and 22 protect the adhesive layer 10 until the adhesive sheet 1 is used, and are peeled off when the adhesive sheet 1 is used. In the adhesive sheet 1 according to this embodiment, one or both of the release sheets 21 and 22 are not necessarily required.
[0124] Examples of the release sheet include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these are also used. Furthermore, laminated films of these may be used. From the viewpoint of the SDGs, the material constituting the release sheet may be a material with a high biomass content, a material that can be recycled or reused, or a recycled or reused material.
[0125] The release surface of the release sheet (particularly the surface in contact with the adhesive layer) is preferably subjected to a release treatment. Examples of the release agent used in the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents. It is preferable that one of the release sheets is a heavy release type release sheet with a large release force, and the other is a light release type release sheet with a small release force.
[0126] There is no particular limitation on the thickness of the release sheet, but it is usually about 20 to 150 μm.
[0127] (3. Production of adhesive composition) The pressure-sensitive adhesive composition P can be produced, for example, by first producing a (meth)acrylic acid ester polymer (A) and mixing the resulting (meth)acrylic acid ester polymer (A) with a crosslinking agent (B). If necessary, the pressure-sensitive adhesive composition P can be produced by mixing an active energy ray-curable component (C), a photopolymerization initiator (D), and a coloring component (E).
[0128] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a normal radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) can be carried out by a solution polymerization method or the like, using a polymerization initiator as desired. Examples of the polymerization solvent include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, methyl ethyl ketone, and the like, and two or more types may be used in combination. Examples of the polymerization initiator include azo compounds, organic peroxides, and the like, and two or more types may be used in combination. In addition, in the above polymerization step, the weight average molecular weight of the obtained polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.
[0129] When the (meth)acrylic acid ester polymer (A) is obtained, the crosslinking agent (B) and, if necessary, the active energy ray curable component (C), the photopolymerization initiator (D), the coloring component (E), other additives, the dilution solvent, etc. are added to the solution of the (meth)acrylic acid ester polymer (A) and mixed thoroughly to obtain a solvent-diluted adhesive composition P (coating solution). In addition, when a solid component is used in any of the above components, or when precipitation occurs when mixed with other components in an undiluted state, the component may be dissolved or diluted alone in a dilution solvent before mixing with other components.
[0130] Examples of dilution solvents that can be used include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.
[0131] The concentration and viscosity of the coating solution thus prepared are not particularly limited as long as they are within the range that allows coating, and can be appropriately selected according to the situation. For example, the adhesive composition P is diluted so that the concentration becomes 10 to 60 mass %. In addition, when obtaining the coating solution, the addition of a dilution solvent or the like is not a necessary condition, and if the adhesive composition P has a viscosity that allows coating, it is not necessary to add a dilution solvent. In this case, the adhesive composition P becomes a coating solution in which the polymerization solvent of the (meth)acrylic acid ester polymer (A) itself serves as the dilution solvent.
[0132] (4. Manufacture of adhesives) The adhesive constituting the adhesive layer is preferably obtained by crosslinking the above-mentioned adhesive composition P. The crosslinking of the adhesive composition P can usually be carried out by a heat treatment. This heat treatment can also serve as a drying treatment for volatilizing a diluting solvent or the like from a coating film of the adhesive composition P applied to a desired object. In addition, such an adhesive layer can also be preferably formed by applying the adhesive composition P to a desired object, subjecting it to a heat treatment, and then curing the adhesive composition P by irradiating it with active energy rays.
[0133] The heating temperature in the heat treatment is preferably 50 to 150° C., and more preferably 70 to 120° C., in the case of the pressure-sensitive adhesive composition P. The heating time is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes, in the case of the pressure-sensitive adhesive composition P.
[0134] Here, the active energy ray refers to an electromagnetic wave or a charged particle ray having an energy quantum, specifically, ultraviolet rays and electron beams. Among the active energy rays, ultraviolet rays are particularly preferable because they are easy to handle. The irradiation of ultraviolet rays can be performed by a high pressure mercury lamp, a Heraeus H lamp, a xenon lamp, etc.
[0135] When the adhesive composition P is cured by irradiation with active energy rays after the heat treatment, the amount of ultraviolet light irradiation is set to an illuminance of 50 to 1000 mW / cm 2The light intensity is preferably about 50 to 10,000 mJ / cm. 2 is preferably 80 to 5000 mJ / cm 2 More preferably, it is 200 to 2000 mJ / cm 2 On the other hand, the irradiation with the electron beam can be carried out by an electron beam accelerator or the like, and the irradiation dose of the electron beam is preferably about 10 to 1000 krad.
[0136] If necessary, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, relative humidity 50%). When curing is required, the adhesive having a crosslinked structure is obtained after the curing period has elapsed. When curing is not required, the adhesive having a crosslinked structure is obtained after the end of the heat treatment.
[0137] (5. Manufacturing of adhesive sheets) The method for producing the adhesive sheet is not particularly limited, and it may be produced by a known method. For example, the above-mentioned coating solution of the adhesive composition P is applied to the release surface of one release sheet, and the adhesive composition P is crosslinked by heat treatment to form a coating layer having a predetermined thickness. The release surface of the other release sheet is superimposed on the formed coating layer. If curing is required, the coating layer becomes the adhesive layer after a predetermined curing period. Also, if curing is not required, the coating layer becomes the adhesive layer as it is. This results in a pressure-sensitive adhesive sheet.
[0138] When the adhesive layer is two layers, for example, a coating liquid of adhesive composition P for forming one adhesive layer (for example, a first adhesive layer) is applied to the release surface of one release sheet, a heat treatment is performed to crosslink the adhesive composition, and a coating layer is formed to obtain a release sheet with a coating layer. A coating liquid of adhesive composition P for forming another adhesive layer (for example, a second adhesive layer) is applied to the release surface of the other release sheet, and a heat treatment is performed to crosslink the adhesive composition, and a coating layer is formed to obtain a release sheet with a coating layer. Then, the release sheet with the coating layer and the release sheet with the coating layer are attached together so that the two coating layers are in contact with each other.
[0139] When the pressure-sensitive adhesive layer is three or more layers, a plurality of release sheets with coating layers may be prepared, and the desired number of coating layers may be laminated in a desired stacking order.
[0140] When curing is required, the coating layer becomes the adhesive layer after a predetermined curing period. When curing is not required, the coating layer becomes the adhesive layer as it is. When the adhesive layer is active energy ray curable, the adhesive layer may be cured by irradiating the adhesive layer with active energy rays as necessary. Through the above steps, the adhesive sheet 1 is obtained.
[0141] Examples of the method for applying the coating solution of the adhesive composition P include a bar coating method, a knife coating method, a roll coating method, a blade coating method, a die coating method, and a gravure coating method.
[0142] (6. Use of adhesive sheets) The pressure-sensitive adhesive sheet according to this embodiment is used as follows. First, one release sheet is removed from the pressure-sensitive adhesive sheet, and the exposed pressure-sensitive adhesive layer is attached to a first member (or a second member). Next, the other release sheet is peeled off, and the exposed pressure-sensitive adhesive layer is attached to a second member. This results in a laminate in which the first member and the second member are laminated and integrated via the pressure-sensitive adhesive layer.
[0143] Furthermore, when the pressure-sensitive adhesive layer is active energy ray-curable, the pressure-sensitive adhesive layer of the obtained laminate may be irradiated with a predetermined active energy ray as necessary to cure the pressure-sensitive adhesive layer and form a cured pressure-sensitive adhesive layer.
[0144] When the adhesive constituting the adhesive layer contains an active energy ray-curable component, the adhesive layer is attached to a first member or a second member before being irradiated with active energy rays. Therefore, the adhesive layer contains a cross-linked structure but is relatively soft, and even if unevenness is formed on the first member and / or the second member, it conforms to the unevenness sufficiently, preventing gaps, floating, etc. from occurring near the unevenness.
[0145] Then, after the pressure-sensitive adhesive layer is attached to the optical member in a relatively soft state, the pressure-sensitive adhesive layer is irradiated with a predetermined active energy ray to cure the pressure-sensitive adhesive layer. Therefore, the cohesive force of the cured pressure-sensitive adhesive layer can be increased while maintaining good conformability to the unevenness, so that both conformability to the unevenness and blister resistance can be achieved. In particular, in the vicinity of the unevenness, optical unevenness is suppressed while the pressure-sensitive adhesive layer can conform to the unevenness well.
[0146] (7. Laminate) As shown in FIG. 2, the laminate 3 of this embodiment is composed of a first member 31 (one display member) having an unevenness 41, a second member 32 (another display member), and an adhesive layer 10 located between them and bonding the first member 31 and the second member 32 to each other.
[0147] The adhesive layer 10 in the laminate 3 is the adhesive layer 10 of the adhesive sheet 1 described above or a cured adhesive layer, and is therefore bonded while sufficiently conforming to the irregularities 41. Therefore, the conformability to the irregularities and the blister resistance are excellent. In addition, optical unevenness is suppressed even in the vicinity of the irregularities.
[0148] The laminate 3 is preferably a display itself or a member constituting a part of a display. Examples of the display include in-vehicle displays such as automobile instrument panels, car navigation systems, and various instruments provided in consoles, general user smartphones, tablet terminals, and other displays, commercial tablet terminals and digital signage, and outdoor digital signage. Examples of types of display include organic electroluminescence (organic EL) displays, electrophoretic displays (electronic paper), liquid crystal displays using a plastic substrate (film) as a substrate, and light-emitting diode (LED) displays. These may be touch panels equipped with position input means.
[0149] Moreover, these display bodies may be flexible displays. The flexible display may be a display including a member that is bent once during manufacturing and maintains the bent state, or a display including a member that can be repeatedly bent (including folded). Examples of flexible displays include foldable displays, rollable displays, and stretchable displays.
[0150] When the laminate 3 is a display body itself or a member constituting a part of a display body (a display body component), the unevenness 41 in the laminate 3 may be unevenness of the display body component itself, or unevenness caused by other components formed on the display body component. Examples of unevenness caused by such other components include steps caused by a printed layer, steps caused by a light-emitting body, etc.
[0151] When the unevenness is a step caused by a printing layer, examples of the display component on which the printing layer is formed include a glass plate, a plastic plate, and a protective panel made of a laminate containing them. The printing layer is generally formed in a frame shape on the protective panel. The material constituting the printing layer is not particularly limited, and a known material for printing is used. The thickness of the printing layer, that is, the height of the step, is preferably 3 to 40 μm, more preferably 5 to 35 μm, more preferably 7 to 30 μm, and even more preferably 10 to 25 μm. This allows the adhesive layer to sufficiently follow the step.
[0152] The glass plate is not particularly limited, and examples thereof include chemically strengthened glass, alkali-free glass, quartz glass, soda-lime glass, barium-strontium-containing glass, aluminosilicate glass, lead glass, borosilicate glass, barium borosilicate glass, etc. The thickness of the glass plate is not particularly limited, but is usually 0.1 to 5 mm, and preferably 0.2 to 2 mm.
[0153] The plastic plate is not particularly limited, and examples thereof include an acrylic plate, a polycarbonate plate, etc. The thickness of the plastic plate is not particularly limited, but is usually 0.2 to 5 mm, and preferably 0.4 to 3 mm.
[0154] In addition, on one or both sides of the above glass plate or plastic plate, various functional layers (transparent conductive film, metal layer, silica layer, hard coat layer, anti-glare layer, anti-reflection layer, light diffusing layer, optical adjustment layer, ultraviolet absorbing layer, writing feeling improving layer, etc.) may be provided, or optical members may be laminated. In addition, the transparent conductive film and the metal layer may be patterned.
[0155] The display component is preferably an optical member, a display module (e.g., a liquid crystal (LCD) module, a light emitting diode (LED) module, an organic electroluminescence (organic EL) module, an electrophoretic display, etc.), an optical member as a part of a display module, or a laminate including a display module. Preferred examples of the optical member include shatterproof films, polarizing plates (polarizing films), polarizers, retardation plates (retardation films), viewing angle compensation films, brightness improvement films, contrast improvement films, liquid crystal polymer films, diffusion films, semi-transmissive reflective films, transparent conductive films, etc. Examples of shatterproof films include hard coat films in which a hard coat layer is formed on one side of a substrate film.
[0156] When the unevenness is a step caused by the light emitter, the display component on which the light emitter is formed is exemplified by a substrate equipped with the light emitter. Such a substrate may be a direct-type backlight. For example, a backlight of a liquid crystal display is exemplified. Examples of the light emitter include a light-emitting diode (LED), a laser diode (LD), an organic electroluminescence light-emitting element, and an inorganic electroluminescence light-emitting element. Among these, from the viewpoint of sealing by the adhesive layer, an LED is preferred, and a mini LED or a micro LED is particularly preferred.
[0157] The thickness of the light emitter is preferably 10 to 300 μm, more preferably 30 to 200 μm, further preferably 50 to 150 μm, and particularly preferably 80 to 120 μm. When a plurality of light emitters are provided, the width of the gap between adjacent light emitters is preferably 0.01 to 100 mm, more preferably 0.1 to 10 mm, and further preferably 0.5 to 4 mm. The shape of the light emitter is not particularly limited, but is usually a rectangular parallelepiped, hemispherical, or the like. The size of the light emitter is also not particularly limited, but from the viewpoint of light emitter sealing, one side or diameter in a planar view is preferably 0.01 to 100 mm, more preferably 0.1 to 10 mm.
[0158] An example of manufacturing the laminate 3 will be described below. First, one release sheet 21 of the adhesive sheet 1 is peeled off, and the exposed adhesive layer 10 of the adhesive sheet 1 is attached to one surface of the first member 31.
[0159] Thereafter, the other release sheet 22 is peeled off from the adhesive layer 10 of the adhesive sheet 1, and the exposed adhesive layer 10 of the adhesive sheet 1 is bonded to a second member 32 to obtain a laminate 3. As another example, the order in which the first member 31 and the second member 32 are bonded may be reversed.
[0160] Furthermore, when the pressure-sensitive adhesive layer 10 is active energy ray-curable, the pressure-sensitive adhesive layer 10 is laminated with the first member 31 and the second member 32 as necessary, and then the pressure-sensitive adhesive layer 10 is irradiated with active energy rays. This causes the active energy ray-curable component (C) in the pressure-sensitive adhesive layer 10 to polymerize, and a laminate 3 in which the pressure-sensitive adhesive layer 10 is cured is obtained.
[0161] (8.Display body) The display according to the present embodiment includes the laminate, and may be composed of only the laminate, or may include one or more laminates and other members. When laminating one laminate with another laminate, or when laminating a laminate with another member, it is preferable to laminate them via the adhesive layer of the adhesive sheet. Therefore, the display according to the present embodiment has excellent unevenness-following properties, blister resistance, and design, and optical unevenness is suppressed.
[0162] In this specification, when it is written "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is written "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is written "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.
[0163] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention.
[0164] (Production Example 1) 1. Preparation of (meth)acrylic acid ester polymers 25 parts by mass of n-butyl acrylate, 30 parts by mass of 2-ethylhexyl acrylate, 5 parts by mass of N-acryloylmorpholine, 10 parts by mass of isobornyl acrylate, 5 parts by mass of methyl methacrylate, and 25 parts by mass of 2-hydroxyethyl acrylate were copolymerized to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of the obtained (meth)acrylic acid ester polymer (A) was measured by the method shown below, and the weight average molecular weight (Mw) was 500,000.
[0165] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). (Measurement conditions) GPC measuring device: Tosoh HLC-8020 GPC columns (passed in the following order): Tosoh Corporation TSK guard column HXL-H TSK gel GMHXL (×2) TSK gel G2000HXL Measurement solvent: Tetrahydrofuran ·Measurement temperature: 40℃
[0166] 2. Preparation of adhesive composition 100 parts by mass (solid content equivalent; same below) of the (meth)acrylic acid ester copolymer (A) obtained above, 0.2 parts by mass of an isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E", isocyanate type: tolylene diisocyanate, modified form: trimethylolpropane adduct) as the crosslinking agent (B), and 0.25 parts by mass of a black pigment as the coloring component (E) were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.
[0167] 3. Preparation of adhesive layer The obtained adhesive composition coating solution was applied by a knife coater to a release-treated surface of a release sheet, one side of which was a polyethylene terephthalate film treated with a silicone-based release agent, and the coating layer was then heated at 90°C for 1 minute to promote a crosslinking reaction, thereby forming a coating layer.
[0168] Next, the coating layer on the release sheet obtained above was attached to the release-treated surface of a polyethylene terephthalate film, one side of which had been release-treated with a silicone-based release agent, so that the coating layer was in contact with the release-treated surface of the release sheet, and the film was cured for 7 days under conditions of 23°C and a relative humidity of 50%, to produce a 25 μm-thick adhesive layer (non-curable with active energy rays).
[0169] The thickness of the adhesive layer is a value measured using a constant pressure thickness measuring instrument (PG-02, manufactured by Teclock Corporation) in accordance with JIS K7130.
[0170] (Production Examples 2 to 7) The adhesive layer was produced in the same manner as in Production Example 1, except that the composition of the meth)acrylic acid ester polymer (A), the type and amount of the crosslinking agent (B), the type and amount of the active energy ray curable component (C), the type and amount of the photopolymerization initiator (D), the amount of the coloring component (E) and the thickness of the adhesive layer were changed as shown in Table 1. In Production Examples 4 and 5, the coating layer was cured by irradiating it with active energy rays (ultraviolet rays; UV) through a release sheet. The irradiation conditions of the active energy rays are shown below. For convenience, the dyed PET film is also shown in Table 1. <Activation energy ray irradiation conditions (hereinafter referred to as "Condition A")> -Uses high pressure mercury lamp ·Illuminance 200mW / cm 2 ,Light intensity 2000mJ / cm 2 The UV illuminance and light intensity meter used is the "UVPF-A1" manufactured by Eye Graphics.
[0171] In Table 1, the amounts of the crosslinking agent (B), active energy ray curable component (C), photopolymerization initiator (D) and coloring component (E) were calculated based on 100 parts by mass (solid content) of the (meth)acrylic acid ester polymer (A). The pressure sensitive adhesives of Production Examples 1, 4, 5 and 7 were not active energy ray curable, while the pressure sensitive adhesives of Production Examples 2, 3 and 6 were active energy ray curable.
[0172] [Table 1]
[0173] Details of the abbreviations and the like in Table 1 are as follows. As for the coloring component (E), Table 2 shows the optical properties of a solution obtained by diluting the coloring component E1 in Table 1 by 10,000 times with ethyl acetate. The optical properties shown in Table 2 were calculated from the haze value (%) obtained for the above-mentioned diluted solution using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7136:2000. The difference from the haze value is the difference between the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, the average haze is the average value of the haze value at a wavelength of 780 nm and the haze value at a wavelength of 380 nm, and the standard deviation of the haze value is the standard deviation of the haze value at each wavelength at a 5 nm pitch in the wavelength range of 380 nm to 780 nm. ((Meth)acrylic acid ester polymer (A)) BA: n-butyl acrylate 2EHA: 2-ethylhexyl acrylate ACMO: N-Acryloylmorpholine IBXA: Isobornyl acrylate MMA: Methyl methacrylate HEA: 2-hydroxyethyl acrylate 4HBA: 4-hydroxybutyl acrylate AAc: acrylic acid (Crosslinking agent (B)) B1: Isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, product name "Takenate D-101E", isocyanate type: tolylene diisocyanate, modified form: trimethylolpropane adduct) B2: Isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, product name "Takenate D-110N", isocyanate type: xylylene diisocyanate, modified form: trimethylolpropane adduct) (Active energy ray-curable component (C)) C1: ε-caprolactone-modified tris-(2-acryloxyethyl) isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "NK Ester A-9300-1CL") C2: Tris-(2-acryloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "NK Ester A-9300") (Photopolymerization initiator (D)) D1: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide D2: 1-hydroxycyclohexyl phenyl ketone and benzophenone mixed in a 1:1 mass ratio (Coloring component (E)) E1: Carbon black based black pigment
[0174] [Table 2]
[0175] (Measurement of total light transmittance) The pressure-sensitive adhesive layers obtained in Production Examples 1 to 7 were attached to glass to prepare measurement samples. After background measurement was performed on the glass, the measurement samples were measured for total light transmittance (%) using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7361-1:1997. The results are shown in Table 3. For Production Examples 2, 3, and 6, the total light transmittance was measured before and after irradiation with active energy rays (ultraviolet rays; UV) by the same method as above. The irradiation conditions for active energy rays were set to Condition A above.
[0176] (Haze value measurement) For the adhesive layers obtained in Production Examples 1 to 7, the haze value (%) was measured from the adhesive layer side using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SH-7000") in accordance with JIS K7136:2000. The obtained haze values (%) are shown in Table 3. For Production Examples 2, 3, and 6, the haze values were measured before and after irradiation with active energy rays (ultraviolet rays; UV) by the same method as above. The active energy ray irradiation conditions were Condition A above.
[0177] (Measurement of adhesive strength of adhesive layer) The release sheet was peeled off from the adhesive layer obtained in Production Examples 1 to 7, and the exposed adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 100 μm) having an easy-adhesion layer to obtain a release sheet / adhesive layer / PET film laminate. The obtained laminate was cut into a width of 25 mm and a length of 100 mm to prepare a sample.
[0178] The release sheet was peeled off from the sample under an environment of 23°C and 50% relative humidity, and the exposed adhesive layer was attached to soda lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressurized for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Seisakusho Co., Ltd. After that, the sample was left for 24 hours under conditions of 23°C and 50% relative humidity, and the adhesive strength (N / 25mm) was measured using a tensile tester (manufactured by Orientec Co., Ltd., product name "Tensilon") at a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurements were performed under conditions other than those described here in accordance with JISZ0237:2009. The results are shown in Table 3. For Production Examples 2, 3, and 6, the adhesive strength was measured before and after irradiation with active energy rays (ultraviolet rays; UV) by the same method as above. The active energy ray irradiation conditions were the above-mentioned condition A.
[0179] (Storage modulus of adhesive layer) A laminate having a thickness of 3 mm was prepared by laminating a plurality of the pressure-sensitive adhesive layers obtained in Production Examples 1 to 7. A cylindrical body having a diameter of 8 mm (height of 3 mm) was punched out from the obtained pressure-sensitive adhesive layer laminate to prepare a sample for measuring storage elastic modulus.
[0180] The storage modulus of the measurement samples was measured by a torsional shear method using a viscoelasticity measuring device (MCR301, manufactured by Anton Paar) at a measurement temperature of 25°C and a measurement frequency of 1 Hz in accordance with JIS K7244-6. The results are shown in Table 3. For Production Examples 2, 3, and 6, the storage modulus was measured before and after irradiation with active energy rays (ultraviolet rays; UV) by the same method as above. The active energy ray irradiation conditions were Condition A described above.
[0181] (Evaluation of gel fraction of adhesive) The adhesive layers obtained in Production Examples 1 to 7 were cut to a size of 80 mm x 80 mm, and the colored adhesive layers were wrapped in a polyester mesh (product name: Tetron mesh #200), and the mass was weighed on a precision balance. The mass of the adhesive alone was calculated by subtracting the mass of the mesh alone from the weighed value. The mass at this time was designated as M1.
[0182] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The mesh was then removed and air-dried for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%, and then dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance. The mass of the adhesive alone was calculated by subtracting the mass of the mesh alone from the weighed value. The mass at this time was designated as M2. The gel fraction was calculated from the obtained M1 and M2 using the following formula. The results are shown in Table 3. Gel fraction (%) = (M2 / M1) x 100 In addition, for Production Examples 2, 3, and 6, the gel fraction was measured before and after irradiation with active energy rays (ultraviolet rays; UV) in the same manner as in the measurement of the total light transmittance. The active energy ray irradiation conditions were the above-mentioned Condition A.
[0183] [Table 3]
[0184] Example 1 Two sheets of the adhesive layer obtained in Production Example 2 were laminated to form a first adhesive layer having a thickness of 50 μm. Then, six sheets of the adhesive layer obtained in Production Example 6 were laminated to form a second adhesive layer having a thickness of 150 μm. The main surface of the obtained first adhesive layer and the main surface of the second adhesive layer were bonded together to obtain an adhesive sheet having the configuration shown in Table 4.
[0185] (Examples 2 to 5 and Comparative Examples 1 to 3) The adhesive layers of Production Examples 1 to 7 were selected so that the first adhesive layer and the second adhesive layer were in the combination shown in Table 4, and laminated to the thickness shown in Table 4 to obtain an adhesive sheet. Example 5 had three adhesive layers. Comparative Example 3 had a configuration in which the adhesive layers of Production Example 3 were formed on both main surfaces of a dyed PET film (dyed PET). For the sake of convenience, the thickness of the dyed PET is shown in Table 1, and the storage modulus, total light transmittance, haze, and gel fraction are shown in Table 3.
[0186] [Table 4]
[0187] (Unevenness tracking rate) A UV-curable ink (Teikoku Ink Co., Ltd., product name "POS-911 Sumi") was screen-printed in the shape of a picture frame (outer dimensions: 90 mm long x 50 mm wide, 5 mm thick) on the surface of a glass plate (NSG Precision Co., Ltd., product name "Corning Glass Eagle XG", 90 mm long x 50 mm wide x 0.5 mm thick). Then, UV light (80 W / cm 2 The printed ultraviolet-curable ink was cured using a laser printer (two metal halide lamps, lamp height 15 cm, belt speed 10-15 m / min) to produce a stepped glass plate having printed steps (step height: one of 5 μm, 10 μm, 15 μm, 20 μm, and 25 μm).
[0188] The release sheet was peeled off from the adhesive sheets prepared in the examples and comparative examples so that the main surface of the second adhesive layer was exposed. The exposed second adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 100 μm) having an easy-adhesion layer. Next, the other release sheet was peeled off to expose the main surface (side A) of the first adhesive layer. Then, using a laminator (manufactured by Fujipla Co., Ltd., product name "LPD3214"), the adhesive layer was laminated on each stepped glass plate so that the main surface (side A) of the first adhesive layer covered the entire frame-shaped print, and this was used as an evaluation sample.
[0189] The obtained evaluation sample was autoclaved for 30 minutes under conditions of 50°C and 0.5 MPa, and then left to stand for 24 hours at normal pressure, 23°C, and a relative humidity of 50%. The pressure-sensitive adhesive sheets produced in Examples 1 and 3 and Comparative Examples 1 to 3 were irradiated with active energy rays through the PET film under the above-mentioned condition A to cure the pressure-sensitive adhesive layer.
[0190] The sample was then stored for 72 hours under high temperature and high humidity conditions of 85°C and 85% relative humidity (durability test), after which the conformability of side A was evaluated. Conformability was determined by whether the printed step was completely filled by the adhesive layer, and if air bubbles, lifting, peeling, etc. were observed at the interface between the printed step and the adhesive layer, it was determined that the adhesive layer was unable to conform to the unevenness of the printed step. Here, conformability was evaluated as the conformability rate (%) shown by the following formula. The results are shown in Table 5. Unevenness conformance rate (%) = {(height of the step that remains filled without bubbles, lifting, peeling, etc. after durability test (μm)) / (thickness of adhesive layer)} × 100
[0191] The unevenness tracking ability of side B was evaluated in the same manner as above. The results are shown in Table 5. Furthermore, the difference in unevenness tracking rate (side A unevenness tracking rate - side B unevenness tracking rate) was calculated from the obtained side A unevenness tracking rate and side B unevenness tracking rate. The results are shown in Table 5.
[0192] (Total light transmittance) The total light transmittance was measured for the pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples using the same method as in the measurement of the total light transmittance described above. The results are shown in Table 5. The pressure-sensitive adhesive sheets produced in Examples 1 and 3 and Comparative Examples 1 to 3 were irradiated with active energy rays through the PET film under the above-mentioned Condition A to cure the pressure-sensitive adhesive layers.
[0193] (Haze value) The total light transmittance was measured for the pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples using the same method as in the measurement of the total light transmittance described above. The results are shown in Table 5. The pressure-sensitive adhesive sheets produced in Examples 1 and 3 and Comparative Examples 1 to 3 were irradiated with active energy rays through the PET film under the above-mentioned Condition A to cure the pressure-sensitive adhesive layers.
[0194] (Ratio of storage modulus of colored adhesive layer to storage modulus of transparent adhesive layer) For the adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples, the ratio of the storage modulus (G1b') of the colored adhesive layer (adhesive layer containing carbon black) to the storage modulus (G2b') of the transparent adhesive layer (adhesive layer not containing carbon black) was calculated. The results are shown in Table 5. For the adhesive sheets produced in Examples 1 and 3 and Comparative Examples 1 to 3, the above ratio was also calculated for the storage moduli (G1a' and G2a') after the adhesive layer was cured by irradiating it with active energy rays through a PET film under the above-mentioned condition A.
[0195] (Evaluation of conformability and color unevenness 1) As adherends, a stepped glass (step height: 25 μm) made in the same manner as the stepped glass plate made in the measurement of the unevenness-following rate, and a glass plate without a step (manufactured by NSG Precision, product name "Corning Glass Eagle XG", length 90 mm × width 50 mm × thickness 0.5 mm) were prepared. In Table 5, the stepped glass is referred to as the uneven plate, and the glass plate without a step is referred to as the smooth plate.
[0196] The release sheet was peeled off from the pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples, and the exposed first pressure-sensitive adhesive layer was attached to a smooth plate. Next, the release sheet was peeled off from the pressure-sensitive adhesive sheet, and the exposed second pressure-sensitive adhesive layer was attached to a concave-convex plate.
[0197] The thus obtained structure was placed on a tablet device (Apple Inc., product name "iPad (registered trademark)", resolution: 264 ppi) with the uneven plate side facing down. The entire tablet device was displayed in white, and the vicinity of the step was visually observed for this sample, and the unevenness followability was evaluated according to the following criteria. The results are shown in Table 5. ○: No lifting or peeling ×: Lifting or peeling has occurred
[0198] Furthermore, the vicinity of the step was visually observed and color unevenness was evaluated according to the following criteria. The results are shown in Table 5. ◎: No color unevenness is visible when observed from a 60 degree angle or from the front ○: Color unevenness is visible when viewed from a 60-degree angle, but not visible from the front ×: Color unevenness is visible from the front
[0199] (Evaluation of conformability and color unevenness 2) The unevenness conformability and color unevenness were evaluated in the same manner as above, except that the second adhesive layer was attached to the uneven plate before the first adhesive layer was attached to the smooth plate. The results are shown in Table 5.
[0200] (Evaluation of blister resistance) The release sheet was peeled off from the adhesive sheets obtained in the Examples and Comparative Examples, and the exposed adhesive layer was attached to an ITO vapor deposition film (manufactured by Oike Industrial Co., Ltd., product name "Tetlite TCFKH150NMH2-125-U6 / T2"). Furthermore, the release sheet was peeled off from the adhesive sheet, and the exposed adhesive layer was attached to the polycarbonate side of a resin plate (manufactured by Mitsubishi Gas Chemical Co., Ltd., product name "Iupilon Sheet MR58U", containing ultraviolet absorber, thickness: 1 mm) in which a polymethyl methacrylate resin layer was laminated on a polycarbonate resin plate, to obtain an evaluation sample. Note that, for the adhesive sheets produced in Examples 1 and 3 and Comparative Examples 1 to 3, the adhesive layer was irradiated with active energy rays through the plastic plate under the same conditions as in Production Example 1, and the adhesive layer was cured.
[0201] The evaluation sample was then autoclaved for 20 minutes under conditions of 50°C and 0.5 MPa, left at normal pressure, 23°C and 50% relative humidity for 12 hours, and then stored under high temperature and humidity conditions of 85°C and 85% relative humidity for 72 hours. The condition of the interface between the pressure-sensitive adhesive layer and the adherend was then visually inspected, and the blister resistance was evaluated according to the following criteria. The results are shown in Table 5. ◎…No bubbles, lifting or peeling ○: No lifting or peeling, slight air bubbles occurred, but not to a problem level ×: Lifting or peeling has occurred
[0202] [Table 5]
[0203] From Table 5, it was confirmed that the pressure-sensitive adhesive sheets of Examples 1 to 5 were able to suppress color unevenness caused by unevenness, while achieving both unevenness-following ability and blister resistance. [Industrial Applicability]
[0204] The pressure-sensitive adhesive sheet of the present invention can be suitably used, for example, for bonding members constituting a display body. [Explanation of symbols]
[0205] 1...Adhesive sheet 10...Adhesive layer 11...First adhesive layer 12…Second adhesive layer 10a(11a)…A side 10b(12a)…B side 21, 22...Release sheet 3...Laminate 31...First member 32...Second member
Claims
1. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding a first member and a second member, The total light transmittance of the pressure-sensitive adhesive layer is 85% or less, when one main surface of the pressure-sensitive adhesive layer is designated as side A and the other main surface is designated as side B, a side A unevenness following rate (%), which indicates the ability of side A to follow the unevenness when side A is attached to an adherend having unevenness, is different from a side B unevenness following rate (%), which indicates the ability of side B to follow the unevenness when side B is attached to an adherend having unevenness, A pressure-sensitive adhesive sheet, wherein the A-side irregularity conforming rate and the B-side irregularity conforming rate are greater than 0%.
2. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer is composed of two or more layers.
3. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein a value obtained by subtracting the B-side unevenness following rate from the A-side unevenness following rate is −20 points or more and −1 point or less.
4. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer contains a coloring component.
5. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive having a crosslinked structure.
6. A laminate comprising a first member, a second member, and a pressure-sensitive adhesive layer that bonds the first member and the second member to each other, At least one of the first member and the second member has projections and recesses, The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to claim 1 .
7. A display comprising the laminate according to claim 6 .
Citation Information
Patent Citations
Adhesive sheet and display body
JP2020169262A
Optical laminate body
WO2021200732A1
Adhesive sheet and method for manufacturing structure
WO2022201613A1
Optical filter and display device
JP2012234028A