Compound, resin composition, cured product, molding, and optical material
A compound with a specific structure enhances the refractive index of resin compositions, addressing the limitations of resin materials in optical applications by improving their performance in optical materials.
Patent Information
- Application Number
- JP2023044413
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Resin materials used as optical materials face challenges due to their heavy and brittle nature and limitations in processing, requiring high refractive indices.
Development of a compound with a specific structure, represented by general formula (1), which exhibits a high refractive index, and its incorporation into resin compositions to enhance optical materials.
The compound improves the refractive index of resin compositions, resulting in improved optical materials suitable for various applications, including optical lenses and coatings.
Smart Images

Figure 2024134216000001 
Figure 2024134216000002 
Figure 2024134216000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound, a resin composition, a cured product, a molded article, and an optical material. [Background technology]
[0002] Inorganic glass is widely used as an optical material because of its excellent properties such as total light transmittance, weather resistance, and chemical resistance. However, due to its heavy and brittle nature and limitations in its processing, resin materials are also used as optical materials. When these resin materials are used as optical materials, they are required to have a high refractive index.
[0003] Hexathiaadamantane compounds are known as high refractive index compounds. As a technique relating to such a hexathiaadamantane compound, for example, there is a technique described in Patent Document 1.
[0004] Patent Document 1 describes a method for producing a hexathiaadamantane compound in high yield by a method that can be easily carried out industrially, and is characterized by condensing a thiocarboxylic acid compound represented by a specific chemical formula in the presence of iodine and a solvent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-209005 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a novel compound having an improved refractive index, as well as a resin composition, a cured product, a molded article, and an optical material each using the novel compound having an improved refractive index. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and as a result have found that a compound having a specific structure exhibits a high refractive index, thereby completing the present invention.
[0008] According to the present invention, there are provided a compound, a resin composition, a cured product, a molded article, and an optical material as shown below.
[0009] [1] A compound (A) represented by the following general formula (1): [ka] (In general formula (1), R 1 ~R 4 each independently represents a hydrocarbon group having 2 to 12 carbon atoms which may contain an unsaturated bond, M represents Si, Ge or Sn, and E represents S or Se. [2] R in the general formula (1) 1 ~R 4 at least one of the above is a hydrocarbon group containing an unsaturated bond. [3] R in the general formula (1) 1 ~R 4 are each independently an ethyl group, a vinyl group, an allyl group or a phenyl group. [4] R in the general formula (1) 1 ~R 4 The compound (A) according to any one of the above [1] to [3], wherein is an allyl group. [5] The compound (A) according to any one of the above [1] to [4], wherein M in the above general formula (1) is Si. [6] The compound (A) according to any one of the above [1] to [5], wherein E in the above general formula (1) is S. [7] The compound (A) according to any one of the above [1] to [6], which has a refractive index (nD) at 25° C. for sodium D lines of 1.60 or more. [8] The compound (A) according to any one of the above [1] to [7], which can be used as an optical material. [9] A resin composition comprising the compound (A) according to any one of the above [1] to [8].
[10] The resin composition according to [9] above, further comprising a resin (B).
[11] The resin composition according to item
[10] , wherein the resin (B) comprises one or more selected from the group consisting of an epoxy resin, a curable acrylic resin, a diallyl phthalate resin, an unsaturated polyester resin, a styrene resin, a polyester resin, a polycarbonate resin, a polyphenylene ether resin, a polyamide resin, a polyurethane resin, a polythiourethane resin, a cycloolefin copolymer, and a (meth)acrylic resin.
[12] The resin composition according to any one of the above [9] to
[11] , further comprising a polymerization initiator.
[13] The resin composition according to any one of [9] to
[12] above, wherein the content of the compound (A) is 0.1 parts by mass or more and 50 parts by mass or less, when the total amount of the resin composition is 100 parts by mass.
[14] The resin composition according to any one of the above [9] to
[13] , which can be used as an optical material.
[15] A cured product obtained by curing the resin composition according to any one of the above [9] to
[14] .
[16] A molded article comprising the resin composition according to any one of the above items [9] to
[14] or the cured product according to the above item
[15] .
[17] An optical material comprising the compound (A) according to any one of the above [1] to [8] or the molded article according to the above
[16] .
[18] The optical material according to
[17] above, which is an optical lens. Effect of the Invention
[0010] According to the present invention, it is possible to provide a novel compound having an improved refractive index, as well as a resin composition, a cured product, a molded article, and an optical material using the novel compound having an improved refractive index. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the present invention will be described based on an embodiment.
[0012] In this embodiment, the numerical range "A to B" indicates A or more and B or less, unless otherwise specified.
[0013] <Compound (A)> The compound (A) of this embodiment is represented by the following general formula (1).
[0014] [ka]
[0015] In general formula (1), R 1 ~R 4 each independently represents a hydrocarbon group having 2 to 12 carbon atoms which may contain an unsaturated bond, M represents Si, Ge or Sn, and E represents S or Se. R 1 ~R 4 The hydrocarbon group in may be a hydrocarbon group in which some of the hydrogen atoms are substituted with a substituent, or may be an unsubstituted hydrocarbon group, but is preferably an unsubstituted hydrocarbon group.
[0016] In general formula (1), R 1 ~R 4 may each independently contain an unsaturated bond, and from the viewpoint of further improving the curability of the resin composition containing the compound (A), preferably R 1 ~R 4 At least one of R 1 ~R 4At least two of R 1 ~R 4 At least three of R 1 ~R 4 All of the above contain unsaturated bonds.
[0017] In general formula (1), R 1 ~R 4 From the viewpoint of further improving the refractive index of compound (A), each independently represents a hydrocarbon group having 2 to 12 carbon atoms, preferably a hydrocarbon group having 2 to 8 carbon atoms, more preferably a hydrocarbon group having 2 to 6 carbon atoms, even more preferably an ethyl group, a vinyl group, an allyl group, or a phenyl group, and even more preferably a phenyl group. In general formula (1), R 1 ~R 4 Among these, it is preferable that at least two of them represent the same hydrocarbon group, it is more preferable that at least three of them represent the same hydrocarbon group, and it is even more preferable that all of them represent the same hydrocarbon group. In addition, in the general formula (1), R 1 ~R 4 From the viewpoint of further improving the curability of the resin composition containing the compound (A), preferably represents a vinyl group or an allyl group, and more preferably represents an allyl group.
[0018] In the general formula (1), M represents Si, Ge or Sn, and preferably represents Si from the viewpoint of further improving the refractive index of the compound (A). In the general formula (1), E represents S or Se, and preferably represents S from the viewpoint of further improving the refractive index and solubility of the compound (A).
[0019] From the viewpoint of further improving the refractive index of compound (A), the molecular weight of compound (A) in this embodiment is preferably 300 or more, more preferably 400 or more, even more preferably 450 or more, and is preferably 1200 or less, more preferably 1000 or less, even more preferably 800 or less, even more preferably 700 or less.
[0020] From the viewpoint of further improving the refractive index of compound (A) and further improving the curability of a resin composition containing compound (A), compound (A) of the present embodiment preferably contains a compound represented by the following formula (2):
[0021] [ka]
[0022] The compound (A) of the present embodiment has a refractive index (nD) of sodium D line at 25° C. of preferably 1.60 or more, more preferably 1.63 or more, even more preferably 1.66 or more, even more preferably 1.68 or more, even more preferably 1.70 or more, and even more preferably 1.73 or more. The upper limit of the refractive index is not particularly limited, and may be, for example, 3.00 or less, 2.50 or less, 2.00 or less, or 1.76 or less. In this embodiment, compound (A) is dissolved in THF to prepare solutions of predetermined concentrations, and the refractive index of sodium D line at 25°C is measured for each solution of each concentration. The refractive index (nD) of sodium D line of compound (A) at 25°C is determined by extrapolating the measurement results of each concentration to a concentration of 100%.
[0023] The compound (A) of this embodiment has an improved refractive index and can therefore be suitably used in optical materials. In addition, since the compound (A) of this embodiment has good solubility in organic solvents, when used in optical materials, it is possible to suppress the occurrence of light scattering and haze due to insolubility in organic solvents.
[0024] <Resin composition> The resin composition of the present embodiment contains the above-mentioned compound (A).
[0025] From the viewpoint of further improving the refractive index of the resulting resin composition and cured product, the content of compound (A) in the resin composition of this embodiment is, when the total amount of the resin composition is 100 parts by mass, preferably 0.1 part by mass or more, more preferably 1.0 part by mass or more, even more preferably 5.0 parts by mass or more, even more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less, even more preferably 35 parts by mass or less, and even more preferably 30 parts by mass or less.
[0026] The resin composition of this embodiment has an improved refractive index due to the inclusion of the compound (A) of this embodiment, and therefore can be suitably used as an optical material.
[0027] The resin composition of the present embodiment may further contain a resin (B).
[0028] The resin (B) is not particularly limited, but from the viewpoint of further improving the refractive index of the resulting resin composition and cured product, it preferably contains one or more types selected from the group consisting of epoxy resins, curable acrylic resins, diallyl phthalate resins, unsaturated polyester resins, styrene resins, polyester resins, polycarbonate resins, polyphenylene ether resins, polyamide resins, polyurethane resins, polythiourethane resins, cycloolefin copolymers, and (meth)acrylic resins.
[0029] From the viewpoint of further improving the refractive index of the obtained resin composition and cured product, the content of resin (B) in the resin composition of this embodiment is, when the total amount of the resin composition is 100 parts by mass, preferably 50 parts by mass or more, more preferably 55 parts by mass or more, even more preferably 60 parts by mass or more, even more preferably 65 parts by mass or more, even more preferably 70 parts by mass or more, and is preferably 99.9 parts by mass or less, more preferably 99.0 parts by mass or less, even more preferably 95.0 parts by mass or less, even more preferably 90 parts by mass or less, even more preferably 85 parts by mass or less, and even more preferably 80 parts by mass or less.
[0030] The resin composition of the present embodiment may further include a polymerization initiator. The polymerization initiator includes, for example, one or more selected from the group consisting of a thermal radical polymerization initiator and a photoradical polymerization initiator.
[0031] Examples of thermal radical polymerization initiators include dialkyl peroxides such as dicumyl peroxide, t-butylcumyl peroxide, 2,5-bis(t-butylperoxy)2,5-dimethylhexane, 2,5-bis(t-butylperoxy)2,5-dimethylhexyne-3, di-t-butyl peroxide, isopropylcumyl-t-butyl peroxide, and bis(α-t-butylperoxyisopropyl)benzene; 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclododecane, n-butyl-4,4-bis(t-butylperoxy)valerate, and ethyl-3,3-bis(t-butylperoxy). peroxyketals such as bis(t-butylperoxy)isophthalate, t-butylperoxybenzoate, t-butylperoxyacetate, and the like; hydroperoxides such as t-butyl hydroperoxide, t-hexyl hydroperoxide, cumin hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, and the like; bibenzyl compounds such as 2,3-dimethyl-2,3-diphenylbutane, and the like; 3,3,5,7,7-pentamethyl-1,2,4-trioxepane, and the like.
[0032] Examples of the photoradical polymerization initiator include benzoin alkyl ether, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzophenone, methylbenzoyl formate, isopropyl thioxanthone, and mixtures of two or more of these. In addition, a sensitizer can be used together with these photoradical polymerization initiators. Examples of the sensitizer include carbonyl compounds such as anthraquinone, 1,2-naphthoquinone, 1,4-naphthoquinone, benzanthrone, p,p'-tetramethyldiaminobenzophenone, and chloranil; nitro compounds such as nitrobenzene, p-dinitrobenzene, and 2-nitrofluorene; aromatic hydrocarbons such as anthracene and chrysene; sulfur compounds such as diphenyl disulfide; and nitrogen compounds such as nitroaniline, 2-chloro-4-nitroaniline, 5-nitro-2-aminotoluene, and tetracyanoethylene.
[0033] From the viewpoint of further improving the refractive index of the obtained resin composition and cured product, the content of the polymerization initiator in the resin composition of this embodiment is, when the content of compound (A) in the resin composition is 100 parts by mass, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1.0 parts by mass or more, even more preferably 1.5 parts by mass or more, even more preferably 2.0 parts by mass or more, even more preferably 2.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8.0 parts by mass or less, even more preferably 5.0 parts by mass or less, and even more preferably 4.0 parts by mass or less.
[0034] <Method of producing resin composition> The resin composition of the present embodiment can be obtained by mixing the compound (A) with the resin (B), a polymerization initiator, and other components, as necessary, by a conventionally known method.
[0035] In the resin composition of this embodiment, the total content of compound (A) and resin (B) is, when the total amount of the resin composition is taken as 100 parts by mass, preferably 80 parts by mass or more, more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, and is preferably 99.5 parts by mass or less, more preferably 99 parts by mass or less, even more preferably 98 parts by mass or less, from the viewpoint of further improving the refractive index of the obtained cured product.
[0036] <Cured product> The cured product of the present embodiment is obtained by curing the resin composition of the present embodiment. The cured product of the present embodiment has an improved refractive index and is therefore suitable for use as an optical material.
[0037] <Molded body> The molded article of the present embodiment is a molded article containing the cured product of the present embodiment, and can be obtained, for example, by molding the resin composition of the present embodiment into a predetermined shape while curing it. The molded article of the present embodiment has an improved refractive index due to the inclusion of the cured product of the present embodiment, and therefore can be suitably used as an optical material.
[0038] From the viewpoint of further improving the refractive index of the molded body, the content of the cured product of this embodiment in the molded body of this embodiment is, when the entire molded body is taken as 100 parts by mass, preferably 50 parts by mass or more, more preferably 70 parts by mass or more, even more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, even more preferably 97 parts by mass or more, and preferably 100 parts by mass or less.
[0039] <Optical materials> The optical material of the present embodiment includes the molded article of the present embodiment, and can be obtained, for example, by molding the resin composition of the present embodiment into a predetermined shape while curing it. The optical material of the present embodiment has an improved refractive index due to the inclusion of the cured product or molded article of the present embodiment, and therefore can be used, for example, in various optical lenses such as lenses for various sensors, pickup lenses, lenses for projectors, prisms, fθ lenses, lenses for imaging, camera lenses, light guide plates, lenses for head-mounted displays, plastic eyeglass lenses, goggles, eyeglass lenses for vision correction, lenses for imaging devices, Fresnel lenses for liquid crystal projectors, lenticular lenses, and contact lenses; sealing materials for light-emitting diodes (LEDs); optical waveguides; optical adhesives used for bonding wafer-level optical components (WLO) and optical waveguides; anti-reflection films used for optical lenses and the like; transparent coatings used for liquid crystal display device components (substrates, light guide plates, films, sheets, and the like); sheets or films attached to car windshields and motorcycle helmets; transparent substrates, and the like. The optical material of the present embodiment has an improved refractive index and can therefore be suitably used as various optical lenses.
[0040] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0041] <Example 1: Synthesis of 1,3,5,7-tetraethyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane> Under a nitrogen atmosphere, 3.3 g of anhydrous lithium sulfide (0.072 mol: manufactured by Sigma-Aldrich) was dispersed in 50 mL of THF and cooled to 0°C. Next, 7.7 g of ethyltrichlorosilane (0.048 mol: manufactured by Tokyo Chemical Industry Co., Ltd.) was diluted with 150 mL of THF and added dropwise over 120 minutes. After the dropwise addition, the mixture was stirred at 0°C for 30 minutes and at room temperature for another 9 hours. The resulting solution was concentrated, and the resulting pale yellow solid was extracted with 120 mL of toluene, and the precipitate was filtered off. The filtrate was concentrated to obtain 3.5 g of the desired white solid 1,3,5,7-tetraethyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane. The yield was 70%. The obtained solid was confirmed to be soluble in common organic solvents such as toluene, tetrahydrofuran, dichloromethane, and chloroform, and no precipitate was formed. The identification data of the obtained compounds are shown below. 1 H-NMR (solvent: CDCl3, internal standard: TMS) δ:1.19(t,12H),1.38(q,8H)
[0042] <Example 2: Synthesis of 1,3,5,7-tetravinyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane> Under a nitrogen atmosphere, 2.8 g of anhydrous lithium sulfide (0.060 mol: manufactured by Sigma-Aldrich) was dispersed in 90 mL of THF and cooled to 0°C. Next, 6.3 g of vinyltrichlorosilane (0.040 mol: manufactured by Tokyo Chemical Industry Co., Ltd.) was diluted with 50 mL of THF and added dropwise over 120 minutes. After the dropwise addition, the mixture was stirred at 0°C for 30 minutes and at room temperature for another 9 hours. The resulting solution was concentrated, and the resulting pale yellow solid was extracted with 100 mL of toluene, and the precipitate was filtered off. The filtrate was concentrated to obtain 2.8 g of the desired white solid 1,3,5,7-tetravinyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane. The yield was 69%. The obtained solid was soluble in common organic solvents such as toluene, tetrahydrofuran, dichloromethane, and chloroform, and it was confirmed that no precipitate was formed. The identification data of the obtained compounds are shown below. 1 H-NMR (solvent: CDCl3, internal standard: TMS) δ:6.20-6.26(dd,4H),6.32-6.37(dd,4H),6.37-6.46(dd,4H)
[0043] <Example 3: Synthesis of 1,3,5,7-tetraallyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane> Under a nitrogen atmosphere, 1.5 g of anhydrous lithium sulfide (0.034 mol: manufactured by Sigma-Aldrich) was dispersed in 50 mL of THF and cooled to 0°C. Subsequently, 3.7 g of allyltrichlorosilane (0.021 mol: manufactured by Sigma-Aldrich) was diluted with 100 mL of THF and added dropwise over 120 minutes. After the dropwise addition, the mixture was stirred at 0°C for 30 minutes and then at room temperature for another 9 hours. The resulting solution was concentrated, and the resulting pale yellow solid was extracted with 100 mL of toluene, and the precipitate was filtered off. The filtrate was concentrated to obtain 1.6 g of the desired white solid of 1,3,5,7-tetraallyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane. The yield was 64%. The solid obtained was confirmed to be soluble in common organic solvents such as toluene, tetrahydrofuran, dichloromethane, and chloroform, and no precipitate was formed. The identification data for the obtained compound are shown below. 1 H-NMR (solvent: CDCl3, internal standard: TMS) δ:2.30-2.36(m,8H),5.12-5.19(m,8H),5.75-5.86(m,4H)
[0044] <Example 4: Synthesis of 1,3,5,7-tetraphenyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane> Under a nitrogen atmosphere, 1.5 g of anhydrous lithium sulfide (0.034 mol: manufactured by Sigma-Aldrich) was dispersed in 200 mL of THF and cooled to 0°C. Subsequently, 4.4 g of phenyltrichlorosilane (0.021 mol: manufactured by Sigma-Aldrich) was diluted with 100 mL of THF and added dropwise over 120 minutes. After the dropwise addition, the mixture was stirred at 0°C for 60 minutes and then at room temperature for another 9 hours. The resulting solution was concentrated, and the resulting white solid was extracted with 120 mL of toluene, and the precipitate was filtered off. The filtrate was gradually concentrated under a nitrogen atmosphere to obtain 0.9 g of the desired white crystals of 1,3,5,7-tetraphenyl-2,4,6,8,9,10-hexathia-1,3,5,7-tetrasilaadamantane. The yield was 26%. The solid obtained was confirmed to be soluble in common organic solvents such as toluene, tetrahydrofuran, dichloromethane, and chloroform, and no precipitate was formed. The identification data for the obtained compound are shown below. 1 H-NMR (solvent: CDCl3, internal standard: TMS) δ:7.49-7.94(m,20H)
[0045] <Comparative Example 1: Synthesis of 1,3,5,7-tetramethyl-2,4,6,8,9,10-hexathiaadamantane> 2.1g of thioacetic acid (0.028mol: Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 3mL of chloroform, 1.4g of iodine (0.006mol: Sigma-Aldrich) was added, and the mixture was stirred at room temperature for one day. 10mL of chloroform was added to the reaction solution, and the mixture was washed three times with water and three times with an aqueous solution of sodium thiosulfate. The organic layer was concentrated, and the resulting yellow solid was purified by silica gel chromatography (developing solvent dichloromethane:hexane = 2:1), to obtain 1.1g of the desired white solid 1,3,5,7-tetramethyl-2,4,6,8,9,10-hexathiaadamantane. The yield was 53%. The obtained solid was confirmed to be soluble in common organic solvents such as toluene, tetrahydrofuran, dichloromethane, and chloroform, and no precipitate was formed. The identification data of the obtained compound are shown below. 1H-NMR (solvent: CDCl3, internal standard: TMS) δ:2.16(s,12H)
[0046] < 1 H-NMR measurement> The structure of the compound obtained is shown below. 1 The compound was analyzed by H-NMR spectroscopy. Measuring equipment: JNM-ECZ400S manufactured by JEOL Ltd. Solvent: Deuterated chloroform Sample concentration: 10mg / 0.7mL Pulse repetition time: 5.5 seconds Number of times: 8 Measurement temperature: 25℃
[0047] <Refractive index measurement> The compounds obtained in the Examples and Comparative Examples were each dissolved in THF to prepare solutions of a given concentration, and the refractive index of the sodium D line of each solution at 25°C was measured using Anton Paar's Abbemat 550. The value obtained by extrapolating the measurement results of each concentration to a concentration of 100% was taken as the refractive index (nD) of the compounds obtained in the Examples and Comparative Examples.
[0048] [Table 1]
Claims
1. A compound (A) represented by the following general formula (1): [Case 1] (In general formula (1), R 1 ~R 4 each independently represents a hydrocarbon group having 2 to 12 carbon atoms which may contain an unsaturated bond, M represents Si, Ge or Sn, and E represents S or Se.
2. R in the general formula (1) 1 ~R 4 The compound (A) according to claim 1, wherein at least one of the following is a hydrocarbon group containing an unsaturated bond:
3. R in the general formula (1) 1 ~R 4 The compound (A) according to claim 1 or 2, wherein each of the is independently an ethyl group, a vinyl group, an allyl group or a phenyl group.
4. R in the general formula (1) 1 ~R 4 The compound (A) according to any one of claims 1 to 3, wherein is an allyl group.
5. The compound (A) according to any one of claims 1 to 4, wherein M in the general formula (1) is Si.
6. The compound (A) according to any one of claims 1 to 5, wherein E in the general formula (1) is S.
7. The compound (A) according to any one of claims 1 to 6, having a refractive index (nD) at 25°C for sodium D line of 1.60 or more.
8. The compound (A) according to any one of claims 1 to 7, which can be used as an optical material.
9. A resin composition comprising the compound (A) according to any one of claims 1 to 8.
10. The resin composition according to claim 9 , further comprising a resin (B).
11. The resin (B) is one or more selected from the group consisting of epoxy resins, curable acrylic resins, diallyl phthalate resins, unsaturated polyester resins, styrene resins, polyester resins, polycarbonate resins, polyphenylene ether resins, polyamide resins, polyurethane resins, polythiourethane resins, cycloolefin copolymers and (meth)acrylic resins. The resin composition according to claim 10.
12. The resin composition according to any one of claims 9 to 11, further comprising a polymerization initiator.
13. The content of the compound (A) is 0.1 parts by mass or more and 50 parts by mass or less when the total amount of the resin composition is 100 parts by mass. The resin composition according to any one of claims 9 to 12.
14. The resin composition according to any one of claims 9 to 13, which can be used as an optical material.
15. A cured product obtained by curing the resin composition according to any one of claims 9 to 14.
16. A molded article comprising the resin composition according to any one of claims 9 to 14 or the cured product according to claim 15.
17. An optical material comprising the compound (A) according to any one of claims 1 to 8 or the molded article according to claim 16.
18. 18. The optical material according to claim 17, which is an optical lens.
Citation Information
Patent Citations
Manufacturing method of hexathiaadamantane compound
JP2010209005A