Cover tape for packaging electronic component and package

The cover tape for electronic components addresses strong adhesion issues by optimizing layer configurations and materials, ensuring antistatic and heat sealing performance while facilitating easy peeling, thus preventing component ejection.

JP2024134232APending Publication Date: 2024-10-03DAI NIPPON PRINTING CO LTD

Patent Information

Application Number
JP2023044431
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing cover tapes for electronic component packaging face issues with strong adhesion between the end tape and the cover tape, leading to unintended peeling and potential ejection of components during handling, while maintaining antistatic and heat sealing performance.

Method used

A cover tape design with a specific configuration of layers, including an antistatic layer, base layer, and heat seal layer, optimized for low surface resistivity and controlled peeling forces, using conductive polymers and surfactants to enhance antistatic performance and facilitate easy peeling.

Benefits of technology

The cover tape achieves high antistatic performance, maintains heat sealing integrity, and ensures easy peeling of the end tape, preventing component ejection during handling and storage under varying environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134232000001_ABST
    Figure 2024134232000001_ABST
Patent Text Reader

Abstract

To provide a cover tape for packaging electronic components that has high antistatic performance and has an end tape easy to peel.SOLUTION: The surface resistivity of the antistatic layer side is less than 1×1010 Ω / sq, the peel strength to the end tape manufactured by NIPPO is 2.0 N or less, and the peel strength to the end tape is 2.0 N or less after being stored for 100 hours at 40°C, 90%RH with the end tape attached to the antistatic layer side of the cover tape for packaging electronic components. The peel strength of the cover tape for packaging electronic components to the carrier tape is greater than 0.15 N after being stored for 100 hours at 40°C and 90%RH with the surface of the heat seal layer side of the cover tape for packaging electronic components and the surface of the antistatic layer of the cover tape for packaging electronic components being superimposed while applying 125 kN / m2 of pressure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a cover tape for packaging electronic components and a package using the same. [Background technology]

[0002] In recent years, electronic components such as ICs, resistors, transistors, diodes, capacitors, and piezoelectric resistors are packaged in tape for surface mounting. In tape packaging, electronic components are stored in a carrier tape that has multiple storage compartments for storing electronic components, and then the carrier tape is heat-sealed with a cover tape to obtain a package for storing and transporting the electronic components. When mounting the electronic components, the cover tape is peeled off from the carrier tape, and the electronic components are automatically removed and surface mounted on a substrate. The cover tape is also called a top tape.

[0003] In taping packaging, static electricity may be generated by friction or contact between the electronic components and the carrier tape or cover tape. Static electricity may also be generated by peeling the cover tape from the carrier tape when mounting the electronic components. Static electricity may cause the electronic components to adhere to the cover tape during mounting, making it impossible to properly remove the electronic components, or causing the electronic components to jump out of the storage section of the carrier tape. This leads to a decrease in mounting efficiency. Furthermore, static electricity may cause deterioration and destruction of the electronic components. Therefore, various cover tapes having antistatic properties have been proposed to suppress the generation of static electricity (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4159979 Summary of the Invention [Problem to be solved by the invention]

[0005] In taping packaging, the package is usually wound up with the carrier tape on the inside and the cover tape on the outside, and then stored and transported with a seal affixed to the end where the winding ends. The seal is a temporary fixing tape that is peeled off when the package is unwound. The seal is also called end tape.

[0006] However, if the adhesion between the end tape and the cover tape is too strong, when the end tape is peeled off from the package, the end tape and the cover tape may peel off from the carrier tape, rather than the end tape peeling off from the cover tape, which may cause the electronic components contained therein to fall off.

[0007] For example, when the cover tape has a heat seal layer on one side of the base layer and an antistatic layer on the other side of the base layer, the antistatic layer is known to contain an antistatic agent and a binder resin. As the binder resin, a resin with high polarity may be used to improve adhesion to the base layer. In addition, the antistatic layer containing the binder resin has poor slipperiness, low surface roughness, and good flatness. Therefore, the adhesion between the end tape and the cover tape tends to be strong.

[0008] The present disclosure has been made in consideration of the above circumstances, and has an object to provide a cover tape for packaging electronic components that has high antistatic performance and allows the end tape to be easily peeled off. [Means for solving the problem]

[0009] In order to achieve the above-mentioned objective, the inventors of the present disclosure conducted extensive research into the peeling performance of an end tape in a cover tape having a heat seal layer on one side of a base layer and an antistatic layer on the other side of the base layer.

[0010] Surfactants such as quaternary ammonium salts are commonly used as antistatic agents. Such surfactants tend to bleed out. As a result, it is possible to realize light peeling and improve the peeling performance of the end tape. On the other hand, the cover tape is usually stored in a rolled state. Therefore, during storage, a part of the surfactant contained in the antistatic layer may migrate to the heat seal layer, which may cause a decrease in antistatic performance and heat seal performance. Therefore, when a surfactant is used as an antistatic agent, it is difficult to satisfy all of the antistatic performance, heat seal performance, and peeling performance of the end tape.

[0011] Conductive polymers are also known as antistatic agents. Conductive polymers are less likely to bleed out. This makes it possible to suppress the deterioration of antistatic performance and heat sealing performance during storage. However, because the conductive polymer does not bleed out, the peeling force of the end tape tends to be high. Therefore, even when a conductive polymer is used as an antistatic agent, it is difficult to satisfy all of the antistatic performance, heat sealing performance, and peeling performance of the end tape.

[0012] The present disclosure is based on these findings.

[0013] One embodiment of the present disclosure is a cover tape for packaging electronic components, comprising an antistatic layer, a base layer, an intermediate layer, and a heat seal layer in this order, the surface resistivity of the surface on the antistatic layer side being 1×10 10 The peel strength against the end tape manufactured by NIPPO is 2.0 N or less, and when the end tape is applied to the surface of the antistatic layer of the cover tape for packaging electronic components, the peel strength against the end tape after storage for 100 hours in an environment of 40°C and 90% RH is 2.0 N or less, and when the surface of the heat seal layer side of the cover tape for packaging electronic components and the surface of the antistatic layer side of the cover tape for packaging electronic components are overlapped, the peel strength against the end tape is 125 kN / m in an environment of 40°C and 90% RH. 2and storing the cover tape for packaging electronic components for 100 hours under a pressure of 0.15 N or more, the peel strength of the surface of the cover tape on the heat seal layer side from the carrier tape being greater than 0.15 N.

[0014] Another embodiment of the present disclosure provides a package comprising a carrier tape having a plurality of storage sections for storing electronic components, the electronic components stored in the storage sections, and the above-mentioned cover tape for packaging electronic components arranged to cover the storage sections. Effect of the Invention

[0015] The present disclosure has an effect of providing a cover tape for packaging electronic components that has high antistatic performance and from which the end tape can be easily peeled off. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view illustrating a cover tape for packaging electronic components according to the present disclosure. [Diagram 2] 1A and 1B are schematic plan and cross-sectional views illustrating a packaging body according to the present disclosure. [Diagram 3] 1A and 1B are schematic perspective and cross-sectional views illustrating a packaging body according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The following describes the embodiments of the present disclosure with reference to the drawings. However, the present disclosure can be implemented in many different forms, and is not to be construed as being limited to the description of the embodiments exemplified below. In addition, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the actual form in order to make the explanation clearer, but these are merely examples and do not limit the interpretation of the present disclosure. In addition, in this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.

[0018] In this specification, when describing an aspect in which another component is disposed on a certain component, the term "above" or "below" includes both cases in which another component is disposed directly above or below a certain component so as to be in contact with the component, and cases in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing an aspect in which another component is disposed on the surface of a certain component, the term "on the surface side" or "on the surface" includes both cases in which another component is disposed directly above or below a certain component so as to be in contact with the component, and cases in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified.

[0019] The cover tape for packaging electronic components and the package according to the present disclosure will be described in detail below. In this specification, the "cover tape for packaging electronic components" may be simply referred to as the "cover tape".

[0020] A. Cover tape for packaging electronic components The cover tape according to the present disclosure has an antistatic layer, a base layer, an intermediate layer, and a heat seal layer in this order, and the surface resistivity of the surface on the antistatic layer side is 1×10 10 The peel strength against the end tape manufactured by NIPPO is 2.0 N or less, and when the end tape is applied to the surface of the antistatic layer of the cover tape for packaging electronic components, the peel strength against the end tape after storage for 100 hours in an environment of 40°C and 90% RH is 2.0 N or less, and when the surface of the heat seal layer side of the cover tape for packaging electronic components and the surface of the antistatic layer side of the cover tape for packaging electronic components are overlapped, the peel strength against the end tape is 125 kN / m in an environment of 40°C and 90% RH. 2 and a peel strength of the surface of the heat seal layer of the cover tape for packaging electronic devices against a carrier tape of more than 0.15 N after storage for 100 hours while applying a pressure of 0.15 N.

[0021] The cover tape in the present disclosure will be described with reference to the drawings. Fig. 1 is a schematic cross-sectional view showing an example of the cover tape in the present disclosure. As shown in Fig. 1, the cover tape 1 has an antistatic layer 2, a base layer 3, an intermediate layer 4, and a heat seal layer 5 in this order. In the cover tape 1, the surface resistivity of the surface 1A on the antistatic layer 2 side is less than a predetermined value.

[0022] 2(a) and (b) are schematic plan views and cross-sectional views showing an example of a package using the cover tape of the present disclosure, and FIG. 2(b) is a cross-sectional view taken along line AA in FIG. 2(a). As shown in FIG. 2(a) and (b), the package 10 includes a carrier tape 11 having a plurality of storage sections 12 for storing electronic components 13, the electronic components 13 stored in the storage sections 12, and a cover tape 1 arranged to cover the storage sections 12. The cover tape 1 is heat-sealed to the carrier tape 11, and a heat-sealed portion 5h is provided in a line shape with a predetermined width at both ends of the heat-sealed layer 5 of the cover tape 1. In addition, in the package 10, the carrier tape 11 can have a feed hole 14.

[0023] As illustrated in Figures 3(a) and (b), the package 10 is usually wound up with the carrier tape 11 on the inside and the cover tape 1 on the outside, and then stored with an end tape 21 attached to the end where the winding ends.

[0024] In the cover tape of the present disclosure, the surface resistivity of the surface on the antistatic layer side is less than a predetermined value, so that the cover tape has high antistatic performance. In addition, in the cover tape of the present disclosure, the peel strength against the end tape is less than a predetermined value, so that the peel performance of the end tape is good. Furthermore, the peel strength of the end tape after storage for 100 hours in an environment of 40°C and 90% RH is also less than a predetermined value, so that the peel performance of the end tape can be maintained even when stored at a temperature and humidity higher than normal temperature and normal humidity. Therefore, when the end tape is peeled off in the package, it is possible to easily peel the end tape from the cover tape. This makes it possible to suppress the cover tape from peeling off from the carrier tape when the end tape is peeled off, and to suppress the electronic components from jumping out of the storage pocket. In addition, in the cover tape of the present disclosure, the peel strength against the carrier tape is greater than a predetermined value, so that the heat seal performance is good. In particular, when the heat seal layer side surface of the cover tape and the antistatic layer side surface of the cover tape are overlapped, the heat seal performance of the cover tape is 125 kN / m under an environment of 40°C and 90% RH. 2 Since the peel strength against the carrier tape after storage for 100 hours under pressure is equal to or greater than a predetermined value, the heat seal performance can be maintained even when the cover tape is stored under pressure at a temperature and humidity higher than normal temperature and humidity. In other words, the deterioration of the heat seal performance due to blocking of the cover tape can be suppressed. Therefore, in the package, unintended peeling of the cover tape can be suppressed, and the falling off of electronic components can be suppressed.

[0025] Therefore, the present disclosure can provide a cover tape that satisfies all of the requirements for antistatic performance, heat sealing performance, and end tape peeling performance.

[0026] Each component of the cover tape according to the present disclosure will be described below.

[0027] 1. Physical properties of cover tape (1)Surface resistivity In the cover tape of the present disclosure, the surface resistivity of the surface on the antistatic layer side is 1×10 10 Ω / □ or less than 1×109 Ω / □ or less is preferable, 1×10 8 It is more preferable that the surface resistivity is in the above range, and thus sufficient antistatic performance can be obtained. On the other hand, the lower limit of the surface resistivity is not particularly limited, but it is, for example, 1×10 5 If the surface resistivity is too low, a sudden voltage change occurs when electrostatic discharge (ESD; Electro Static Discharge) occurs, which may lead to damage to the contents.

[0028] The surface resistivity was measured using a resistivity meter "Hiresta UP MCP-HT450" manufactured by Nitto Seiko Analytech Co., Ltd. under the following test conditions. <Test conditions> Probe: UA probe Applied voltage: 10 10 Ω / □ Less than 10V 10 10 Ω / □ or more 10 12 Ω / □ Less than 500V 10 13 Ω / □ or more 1000V Sample size: 5.5mm x 100mm Measurement point: Center of sample Measurement value: 5 points are measured with no overlapping, and the average value is used. - Measurement time: Display after 10 seconds · Sample storage before measurement: Store for at least 24 hours in an environment of 25℃ and 40% RH ·Measurement environment: 25±2℃, 40±5%RH environment

[0029] In the cover tape of the present disclosure, methods for adjusting the surface resistivity of the surface on the antistatic layer side include, for example, a method of adjusting the type or content of an antistatic agent, a method of adjusting the type, physical properties, structure or content of a specific additive described below, and a method of adjusting the thickness of the antistatic layer.

[0030] (2) Peel strength against end tape In the cover tape of the present disclosure, the peel strength against the end tape manufactured by NIPPO Corporation is 2.0N or less, preferably 1.8N or less, and more preferably 1.5N or less. The above peel strength is the peel strength before the first environmental test described later, and is the initial peel strength. When the above peel strength is in the above range, the heat seal part of the cover tape can be prevented from peeling off from the carrier tape in the package when the end tape is peeled off from the package. As a result, the electronic components can be prevented from jumping out of the storage pocket. On the other hand, the above peel strength is, for example, preferably 0.8N or more, and more preferably 1.3N or more. When the above peel strength is in the above range, the end tape can be prevented from peeling off from the package.

[0031] In addition, in the cover tape of the present disclosure, the peel strength of the end tape after storing for 100 hours in an environment of 40°C and 90% RH in a state where the end tape is attached to the surface of the antistatic layer of the cover tape is 2.0N or less, preferably 1.8N or less, and may be 1.5N or less. In this specification, a test in which the end tape is attached to the surface of the antistatic layer of the cover tape and stored for 100 hours in an environment of 40°C and 90% RH may be referred to as a first environmental test. Since the peel strength after the first environmental test is in the above range, blocking between the surface of the antistatic layer side of the cover tape and the end tape can be suppressed. This makes it possible to suppress the heat seal portion of the cover tape from peeling off from the carrier tape in the package when the end tape is peeled off from the package. As a result, it is possible to suppress the electronic component from jumping out of the storage pocket. On the other hand, the peel strength after the first environmental test is, for example, preferably 0.8N or more, more preferably 1.3N or more. When the peel strength after the first environmental test is within the above range, peeling of the end tape from the package can be suppressed.

[0032] The peel strength of the cover tape against the end tape is measured by the following method. First, a cover tape with a width of 5.5 mm or more and an end tape with a width of 6 mm manufactured by NIPPO are prepared. The cover tape is cut to a length of 70 mm, and the surface of the cover tape on the heat seal layer side is attached to a glass plate via double-sided tape. The glass substrate is "S7213" (76 mm x 26 mm) manufactured by Matsunami Glass Industry Co., Ltd. The double-sided tape is double-sided tape No. 777 manufactured by Teraoka Seisakusho Co., Ltd. Next, the end tape is attached to the surface of the antistatic layer side of the cover tape by rolling a pressure roller back and forth twice to form a laminate. Then, the laminate is left to stand at 23 ± 2 ° C and 50 ± 10% RH for 60 minutes. Next, the end tape is peeled off from the cover tape using a Tensilon universal testing machine at a peel speed of 6000 mm / min and a peel angle of 180 °. The peel strength is then measured at four points, from 20 mm from the peel start point to 65 mm from the peel start point, and the average of the four measured values ​​is taken as the peel strength. Note that care is taken not to allow the end tape to stick to the double-sided tape when preparing the sample and during measurement. The Tensilon universal testing machine used is the "RTF-1150-H" manufactured by A&D.

[0033] In the first environmental test, the end tape is attached to the surface of the antistatic layer of the cover tape and stored for 100 hours in an environment of 40°C and 90% RH. The peel strength after the first environmental test is the peel strength when peeling the end tape from the cover tape after storing the laminate for 100 hours in an environment of 40°C and 90% RH and then leaving it to stand for 60 minutes in an environment of 23±2°C and 50±10% RH.

[0034] In the cover tape of the present disclosure, methods for adjusting the peel strength relative to the end tape include, for example, adjusting the type of binder resin, adjusting the type of antistatic agent, adjusting the type, physical properties, structure or content of a specific additive described below, adding a filler, and providing irregularities on the surface of the antistatic layer.

[0035] (3) Peel strength from carrier tape In the cover tape of the present disclosure, when the surface of the heat seal layer side of the cover tape and the surface of the antistatic layer side of the cover tape are overlapped, the cover tape has a compressive strength of 125 kN / m under an environment of 40° C. and 90% RH. 2 After storing for 100 hours while applying a pressure of 125 kN / m, the peel strength of the heat seal layer side of the cover tape to the carrier tape is greater than 0.15 N, preferably 0.18 N or more, and more preferably 0.20 N or more. In this specification, the peel strength of the heat seal layer side of the cover tape to the carrier tape after storing for 100 hours while applying a pressure of 125 kN / m under an environment of 40° C. and 90% RH in a state where the heat seal layer side of the cover tape and the antistatic layer side of the cover tape are overlapped. 2 The test in which the cover tape is stored for 100 hours while applying a pressure of 100 mm may be referred to as the second environmental test. Since the peel strength after the second environmental test is within the above range, it is possible to suppress a decrease in the peel strength due to blocking of the cover tape. Therefore, it is possible to suppress the peeling of the heat seal portion of the cover tape from the carrier tape before the cover tape is peeled from the carrier tape by a peeling device when mounting electronic components. As a result, it is possible to suppress the electronic components from falling off.

[0036] The upper limit of the peel strength after the second environmental test is not particularly limited, but is preferably 0.7 N or less, and more preferably 0.6 N or less. If the peel strength after the second environmental test is within the above range, the carrier tape can be prevented from vibrating when the cover tape is peeled off from the carrier tape. As a result, the electronic components can be prevented from jumping out of the storage pocket.

[0037] In addition, in the cover tape of the present disclosure, the peel strength to the carrier tape is, for example, preferably 0.15N or more, preferably 0.18N or more, and more preferably 0.20N or more. The above peel strength is the peel strength before the second environmental test, and is the initial peel strength. If the peel strength is within the above range, for example, even when the cover tape is heat-sealed to the carrier tape immediately after production, the heat-sealed portion of the cover tape can be prevented from peeling off from the carrier tape. As a result, the electronic components can be prevented from falling off. On the other hand, the upper limit of the peel strength is not particularly limited, but is, for example, preferably 0.7N or less, more preferably 0.6N or less. If the peel strength is within the above range, the carrier tape can be prevented from vibrating when the cover tape is peeled off from the carrier tape. As a result, the electronic components can be prevented from jumping out of the storage pocket.

[0038] The peel strength of the cover tape against the carrier tape is the peel strength of the cover tape against the paper carrier tape. Carrier tapes are broadly classified into plastic carrier tapes made of plastic and paper carrier tapes made of paper, but paper carrier tapes are generally more likely to absorb moisture than plastic carrier tapes. Therefore, the peel strength is more likely to decrease. Therefore, in this disclosure, the peel strength of the cover tape against the paper carrier tape is adopted.

[0039] The paper carrier tape used is "PCT31" manufactured by Hokuetsu Corporation. This paper carrier tape is 0.31 mm thick, 8 mm wide, and made of virgin paper.

[0040] The peel strength of the initial cover tape against the carrier tape is measured by the following method. First, the carrier tape and cover tape are heat-sealed under the following conditions using a taping machine "NST-35" manufactured by Nitto Kogyo Co., Ltd., and approximately 40 m of the tape is wound into a roll on a reel with a core diameter of 3 inches to prepare a reel sample. Next, the reel sample is stored in a tilted state under an environment of 25°C and 40% RH for 24 hours. Next, the peel strength is measured when peeling the cover tape from the carrier tape under the following conditions using an embossed tape peel strength tester "PTS-5000" manufactured by EPI Co., Ltd.

[0041] <Taping conditions> Carrier tape feed hole pitch: 2mm Taping temperature: adjustable from 0.25N to 0.35N, for example 180℃ Taping speed: 3500 tacts Taping iron size: 0.6mm x 2 lines Taping iron length (seal length in one stroke): 8±1mm

[0042] <Peel strength measurement conditions> Cover tape width: 5.25±0.2mm ·Measurement length: 150mm Peeling speed: 300mm / min Peeling angle: 165° to 175° Measurement environment: 25±3℃, 40±10%RH Measurement value: Average value when measuring 150 mm

[0043] The peel strength of the cover tape to the carrier tape after the second environmental test is measured by the following method. First, a 5.5 mm wide cover tape is prepared, and the cover tape is cut into two pieces with a length of 30 cm, and the second environmental test is performed. In the second environmental test, the heat seal layer side of the cover tape and the antistatic layer side of the cover tape are overlapped, and the peel strength is measured at 125 kN / m under an environment of 40°C and 90% RH. 2The laminate is stored for 100 hours while applying a pressure of 125 kN / m. When overlapping the heat seal layer side of the cover tape with the antistatic layer side of the cover tape, the heat seal layer side of the first cover tape and the antistatic layer side of the second cover tape are overlapped to form a laminate. When applying pressure, a blocking tester with a pressure section size of 60 mm square is used, and a pressure of 125 kN / m is applied to any area of ​​the laminate. 2 A pressure of 10 ...

[0044] <Taping conditions> Carrier tape feed hole pitch: 2mm Taping temperature: adjustable from 0.25N to 0.35N, for example 180℃ Taping speed: 3500 tacts Taping iron size: 0.6mm x 2 lines Taping iron length (seal length in one stroke): 8±1mm

[0045] <Peel strength measurement conditions> Cover tape width: 5.5mm Measurement length: 50mm Peeling speed: 300mm / min Peeling angle: 165° to 175° Measurement environment: 25±3℃, 40±10%RH Measurement value: Average value when measuring 50 mm

[0046] In the cover tape of the present disclosure, methods for adjusting the peel strength from the carrier tape include, for example, a method of adjusting the type of antistatic agent, a method of adjusting the type, physical properties, structure or content of a specific additive described below, and a method of adjusting the thickness of the antistatic layer.

[0047] (4) Haze The haze of the cover tape in the present disclosure is, for example, preferably 55% or less, more preferably 50% or less. If the cover tape has such optical properties, the cover tape will have good visibility. The haze is measured using a haze meter "NDH 7000" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K7136:2000.

[0048] (5) Total light transmittance The total light transmittance of the cover tape in the present disclosure is, for example, preferably 80% or more, more preferably 85% or more. If the cover tape has such optical properties, the cover tape has good visibility. The total light transmittance is measured using a haze meter "NDH 7000" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K7361-1:1997.

[0049] 2.Antistatic layer The antistatic layer in the present disclosure is a layer for preventing the cover tape from being charged. By having the antistatic layer in the cover tape, damage to the chip caused by peeling charge when peeling the cover tape from the carrier tape and mounting failure caused by static electricity can be suppressed. In addition, the generation of static electricity due to contact with other surfaces can be suppressed. Furthermore, the adhesion of dirt, dust, etc. to the cover tape surface due to static electricity can be suppressed.

[0050] (1) Antistatic layer material The antistatic layer preferably contains a binder resin and an antistatic agent, more preferably contains a conductive polymer or a metal oxide as the antistatic agent, and even more preferably contains a conductive polymer as the antistatic agent. That is, the antistatic layer preferably contains a binder resin and a conductive polymer or a metal oxide, and more preferably contains a binder resin and a conductive polymer.

[0051] Conventionally, surfactants such as quaternary ammonium salts have been widely used as antistatic agents. Such surfactants tend to bleed out, and they migrate to the surface of the antistatic layer to exhibit antistatic performance. On the other hand, as described below, the antistatic layer preferably contains a polyetheramine surfactant or a polymeric compound having a long-chain alkyl group on the side chain. When the antistatic layer contains a polyetheramine surfactant, it is considered that the polyetheramine surfactant also migrates to the surface of the antistatic layer to exhibit releasability. In addition, when the antistatic layer contains a polymeric compound having a long-chain alkyl group on the side chain, it is considered that the long-chain alkyl group of this polymeric compound is oriented on the surface of the antistatic layer or migrates to the surface of the antistatic layer to exhibit releasability. Therefore, when a surfactant is used as an antistatic agent, it is considered that the expression of antistatic performance by the surfactant as the antistatic agent and the expression of releasability by the polyetheramine surfactant or the polymeric compound having a long-chain alkyl group on the side chain become competitive, and the antistatic effect is difficult to exhibit.

[0052] On the other hand, conductive polymers are less likely to bleed out, and the inclusion of conductive polymers reduces the resistance of the entire antistatic layer, thereby exerting antistatic performance. Similarly, metal oxides are less likely to bleed out, and the inclusion of metal oxides reduces the resistance of the entire antistatic layer, thereby exerting antistatic performance. Therefore, even if the antistatic layer contains a polyetheramine surfactant or a polymer compound having a long-chain alkyl group on the side chain, the antistatic performance can be prevented from decreasing. Therefore, it is possible to achieve both antistatic performance and end tape peeling performance.

[0053] (a) Binder resin The antistatic layer preferably contains a binder resin. In order to improve adhesion to the substrate layer, a resin with high polarity may be used as the binder resin. In addition, the antistatic layer containing the binder resin has poor slipperiness, low surface roughness, and good flatness. Therefore, the adhesion between the end tape and the cover tape tends to be strong. Therefore, the effect of the present disclosure can be obtained significantly. In addition, by containing the binder resin in the antistatic layer, not only adhesion to the substrate but also optical properties, mechanical properties, etc. are imparted.

[0054] The binder resin is not particularly limited, but is preferably a resin with high polarity, i.e., a water-based resin, and more specifically, is preferably an acrylic resin, an epoxy resin, a polyester resin, or a urethane resin.

[0055] Examples of the acrylic resin include acrylic resins obtained by polymerizing one or more of the following monomers: a monomer containing a hydroxyl group, a monomer containing an amide group, a monomer containing a carboxyl group, and other monomers; and crosslinked acrylic resins obtained by crosslinking these resins with a crosslinking agent. Examples of the monomer containing a hydroxyl group include 2-hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, and hydroxybutyl acrylate. Examples of the monomer containing an amide group include acrylamide and N-methylol acrylamide. Examples of the monomer containing a carboxyl group include acrylic acid, methacrylic acid, itaconic acid, and maleic anhydride. Examples of the other monomers include methyl acrylate, ethyl acrylate, N-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, and 2-ethylhexyl methacrylate. Examples of the crosslinking agent include melamine-based crosslinking agents, urea-based crosslinking agents, epoxy-based crosslinking agents, isocyanate-based crosslinking agents, aziridine-based crosslinking agents, ethyleneimine-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, and silane coupling agents. In particular, from the viewpoints of mechanical properties, water resistance, and adhesion, acrylic resins having carboxyl groups and crosslinked acrylic resins in which acrylic resins having carboxyl groups are crosslinked with aziridine-based crosslinking agents are preferred. The acrylic resins may be used alone or in combination of two or more.

[0056] Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, etc. The epoxy resins may be used alone or in combination of two or more.

[0057] The polyester resin is composed of a polycarboxylic acid component and a polyol component. The polycarboxylic acid component includes at least one of an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid. The aromatic dicarboxylic acid includes at least one component selected from the group consisting of, for example, terephthalic acid, isophthalic acid, phthalic acid, diphenic acid, naphthalic acid, 1,2-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid. The aliphatic dicarboxylic acid may be linear, branched, or alicyclic. The aliphatic dicarboxylic acid includes at least one component selected from the group consisting of oxalic acid, malonic acid, succinic acid, maleic acid, itaconic acid, glutaric acid, adipic acid, pimelic acid, 2,2-dimethylglutaric acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, 1,3-cyclopentanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, diglycolic acid, and thiodipropionic acid. The polyol component includes, for example, ethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1,3-propanediol, 2,2,4-trimethyl-1,6-hexanediol, The mixture contains at least one component selected from the group consisting of 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 4,4'-dihydroxybiphenol, 4,4'-methylenediphenol, 1,5-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), and bisphenol S.The polyethylene glycol includes at least one component selected from the group consisting of, for example, diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, hexaethylene glycol, heptaethylene glycol, and octaethylene glycol. The polypropylene glycol includes at least one component selected from the group consisting of, for example, dipropylene glycol, tripropylene glycol, and tetrapropylene glycol.

[0058] The content of the binder resin in the antistatic layer is preferably 45% by mass or more, more preferably 60% by mass or more. On the other hand, the content of the binder resin is preferably 98% by mass or less, more preferably 95% by mass or less. That is, the content of the binder resin is preferably 45% by mass or more and 98% by mass or less, more preferably 60% by mass or more and 95% by mass or less. If the content of the binder resin is too low, the antistatic layer may easily peel off. On the other hand, if the content of the binder resin is too high, the content of the antistatic agent and the content of the specific additive described below are relatively periodically reduced, so that the antistatic agent and the specific additive may not be able to fully exert their effects.

[0059] (b) Antistatic agent As described above, the antistatic layer in the present disclosure preferably contains a conductive polymer or a metal oxide as an antistatic agent, and more preferably contains a conductive polymer. The antistatic layer may also contain a conductive polymer and a metal oxide as antistatic agents.

[0060] (i) Conductive polymer In this specification, the term "conductive polymer" refers to a polymer that itself exhibits electrical conductivity, such as polythiophene, which will be described later.

[0061] Examples of the conductive polymer include polythiophene, polyaniline, polypyrrole, polyacetylene, polyparaphenylene, polyphenylenevinylene, and polyvinylcarbazole.

[0062] Among them, the conductive polymer is preferably one or more selected from the group consisting of polythiophene, polyaniline, and polypyrrole. This is because the polymer itself exhibits conductivity, and therefore sufficient antistatic properties and transparency can be obtained without depending on humidity. For example, PEDOT / PSS ((poly(3,4-ethylenedioxythiophene)) / polystyrenesulfonic acid) is preferably used as the polythiophene. For example, sulfonated polyaniline is preferably used as the polyaniline. If the antistatic layer contains these conductive polymers, a low surface resistivity can be obtained even if the thickness is thin. The thin thickness of the antistatic layer can improve the light transmittance of the cover tape. In addition, the thin thickness of the antistatic layer can reduce the light absorption rate of the cover tape. Therefore, the visibility of the cover tape can be improved.

[0063] The content of the conductive polymer in the antistatic layer may be an amount that satisfies the above-mentioned surface resistivity. The content of the conductive polymer is preferably 5% by mass or more, more preferably 7% by mass or more. On the other hand, the content of the conductive polymer is preferably 15% by mass or less, more preferably 12% by mass or less. That is, the content of the conductive polymer is preferably 5% by mass or more and 15% by mass or less, more preferably 7% by mass or more and 12% by mass or less. If the content of the conductive polymer is too small, the antistatic effect may be difficult to exhibit. On the other hand, if the content of the conductive polymer is too large, the dispersibility may be poor, and the adhesion, optical properties, and mechanical properties may be poor.

[0064] (ii) Metal oxides Examples of metal oxides include antimony-doped tin oxide (ATO), fluorine-doped tin oxide, phosphorus-doped tin oxide (PTO), aluminum-doped tin oxide, niobium-doped tin oxide, tantalum-doped tin oxide, tungsten-doped tin oxide, indium-doped tin oxide, tin oxide, tin-doped indium oxide (ITO), fluorine-doped indium oxide, cadmium-doped indium oxide, indium-doped zinc oxide, fluorine-doped zinc oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, magnesium-doped zinc oxide, silicon-doped zinc oxide, tin-doped zinc oxide, boron-doped zinc oxide, zinc oxide, zinc antimonate (AZO), and niobium-doped titanium oxide. Metal oxides may be used alone or in combination of two or more. From the viewpoint of stabilizing the surface resistivity, antimony-doped tin oxide, tin-doped indium oxide, phosphorus-doped tin oxide, tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide and zinc antimonate are preferred.

[0065] The shape of the metal oxide may be any of spherical, needle-like, and lamellar, but from the viewpoints of transparency, surface resistivity, and dispersibility, spherical and needle-like are preferred. The average particle size of the metal oxide is, for example, 0.01 μm or more and 1 μm or less, and from the viewpoint of transparency, 0.01 μm or more and 0.5 μm or less is preferred.

[0066] The content of the metal oxide in the antistatic layer may be any amount that allows the surface resistivity to fall within a predetermined range, for example, from 30% by mass to 70% by mass.

[0067] (iii) Other antistatic agents The antistatic layer may contain an antistatic agent other than the conductive polymer and the metal oxide. Examples of the other antistatic agent include surfactants. The surfactants include cationic, anionic, and nonionic surfactants.

[0068] (c) Specific additives The antistatic layer preferably contains a polyetheramine surfactant or a polymeric compound having a long-chain alkyl group on the side chain. In this specification, the polyetheramine surfactant and the polymeric compound having a long-chain alkyl group on the side chain may be referred to as a specific additive. This is because the antistatic agent contains a specific additive, which makes it easier to obtain the above-mentioned physical properties of the cover tape. In addition, the inclusion of the specific additive can improve the slipperiness of the antistatic layer. This can suppress blocking. Furthermore, it can suppress the antistatic layer from being scraped off due to friction with the taping device.

[0069] (i) Polyetheramine surfactants Examples of polyetheramine surfactants include polyoxyalkylene alkylamines. Examples of polyoxyalkylene alkylamines include polyoxyethylene alkylamines. Examples of polyoxyethylene alkylamines include polyoxyethylene laurylamine, polyoxyethylene alkyl (coconut)amine, polyoxyethylene tallow alkylamine, polyoxyethylene stearylamine, polyoxyethylene oleylamine, and polyoxyethylene alkyl propylene diamine. The polyetheramine surfactants may be used alone or in combination of two or more.

[0070] In the polyoxyalkylene alkylamine, the carbon number of the alkyl group may be, for example, 10 or more, and may be, for example, 12 or more. The carbon number of the alkyl group may be, for example, 20 or less, and may be, for example, 18 or less. That is, the carbon number of the alkyl group may be, for example, 10 or more and 20 or less, and may be, for example, 12 or more and 18 or less. If the carbon number of the alkyl group is within the above range, it is easy to adjust the HLB value and the freezing point described later to be within a preferred range.

[0071] In the polyoxyalkylene alkylamine, examples of the oxyalkylene group include an oxyethylene group and an oxypropylene group. Among these, the oxyalkylene group is preferably an oxyethylene group, because it is easy to adjust the HLB value described below to fall within a preferred range.

[0072] In addition, in the polyoxyalkylene alkylamine, the number of moles of alkylene oxide added is, for example, from 1 to 10, and may be from 1 to 5. If the number of moles added is within the above range, the HLB value described below can be easily adjusted to be in a preferred range.

[0073] In the polyoxyalkylene alkylamine, the number of carbon atoms in the alkyl group, the oxyalkylene group, and the number of moles of alkylene oxide added are analyzed by gas chromatography mass spectrometry (GC-MS).

[0074] The HLB value (Hydrophilic-Lipophilic Balance) of the polyetheramine surfactant is preferably, for example, 3 or more and 7 or less. In general, it is assumed that the larger the HLB value, the higher the hydrophilicity and the better the compatibility with the binder resin. When the HLB value of the polyetheramine surfactant is a predetermined value or less, the compatibility with the binder resin is not too good, and the polyetheramine surfactant is likely to be localized on the surface of the antistatic layer. Therefore, the peel strength with respect to the end tape can be reduced, and the end tape can be easily peeled off. In addition, when the HLB value of the polyetheramine surfactant is large and the compatibility with the binder resin is too good, the polyetheramine surfactant may be well dissolved or dispersed in the binder resin in the antistatic layer, and may be difficult to bleed onto the surface of the antistatic layer. In addition, when the HLB value of the polyetheramine surfactant is a predetermined value or more, the compatibility with the binder resin is good, and the transparency can be increased.

[0075] In this specification, the HLB value is a value that indicates the degree of affinity of a surfactant for water and oil, and takes a value from 0 to 20, with the closer to 0 the higher the lipophilicity and the closer to 20 the higher the hydrophilicity. The HLB value is a value calculated by the Griffin method and is found by the following formula. HLB value = 20 × sum of hydrophilic moieties / molecular weight

[0076] The freezing point of the polyetheramine surfactant is preferably, for example, 5° C. or higher and 40° C. or lower. When the freezing point is a predetermined value or lower, the fluidity is increased and the dispersibility is improved, so that the transparency can be increased. In addition, when the freezing point is a predetermined value or higher, the fluidity is not too high, so that the occurrence of bias in antistatic performance and end tape peeling performance can be suppressed.

[0077] The freezing point is the phase transition temperature from liquid to solid. The freezing point is measured by differential scanning calorimetry (DSC). Specifically, in differential scanning calorimetry (DSC), the measurement start point is set to a temperature below the temperature at which the measurement sample freezes, and the freezing point is set to a temperature at which the measurement sample begins to melt as the temperature increases and reaches an endothermic peak.

[0078] The content of the polyetheramine surfactant in the antistatic layer is, for example, preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the total of the binder resin and the antistatic agent. The content of the polyetheramine surfactant is, for example, preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the total of the binder resin and the antistatic agent. That is, the content of the polyetheramine surfactant is, for example, preferably 5 parts by mass or more and 30 parts by mass or less, more preferably 8 parts by mass or more and 25 parts by mass or less, and even more preferably 10 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total of the binder resin and the antistatic agent. If the content of the polyetheramine surfactant is too low, the effect of improving the peeling performance of the end tape may not be sufficiently obtained. On the other hand, if the content of the polyetheramine surfactant is too high, the antistatic performance may be reduced.

[0079] (ii) Polymer compounds having long-chain alkyl groups on the side chains A polymer compound having a long-chain alkyl group on a side chain is used as a release agent for improving the peeling performance of an end tape. Hereinafter, a polymer compound having a long-chain alkyl group on a side chain may be referred to as a long-chain alkyl group-containing polymer compound.

[0080] In the long-chain alkyl group-containing polymer compound, the long-chain alkyl group is a linear or branched alkyl group. The carbon number of the long-chain alkyl group is, for example, preferably 6 or more, more preferably 8 or more, even more preferably 12 or more, and particularly preferably 15 or more. The carbon number of the long-chain alkyl group is, for example, preferably 30 or less, more preferably 25 or less. By having the carbon number of a predetermined value or more, the long-chain alkyl group of the long-chain alkyl group-containing polymer compound is easily oriented on the surface of the antistatic layer or easily bleeds, and the peeling performance of the end tape can be improved. In addition, by having the carbon number of a predetermined value or less, the compatibility with the binder resin is improved and the transparency can be increased. In addition, the decrease in antistatic performance can be suppressed. Examples of long-chain alkyl groups include hexyl, octyl, decyl, lauryl, octadecyl, behenyl, myristyl, palmityl, stearyl, oleyl, elaidyl, erucyl, zomaryl, lylyl, lylnyl, eleostearyl, and lysylyl groups.

[0081] In the long-chain alkyl group-containing polymer compound, the basic skeleton of the main chain is not particularly limited and is appropriately selected depending on the synthesis method. Examples of the basic skeleton of the main chain include polyester, polyamide, polyurethane, acrylic polymer, methacrylic polymer, acrylic acid ester copolymer, acrylamide copolymer, polyvinyl alcohol, polyethyleneimine, polyethyleneamine, etc.

[0082] The long-chain alkyl group-containing polymer compound can be obtained by reacting a polymer compound having a reactive group with a compound having an alkyl group capable of reacting with the reactive group. Examples of the reactive group include hydroxyl group, amino group, carboxy group, and acid anhydride. Examples of the polymer compound having a reactive group include polyvinyl alcohol, saponified vinyl acetate polymer, saponified vinyl acetate-ethylene copolymer, saponified vinyl acetate-acrylic acid copolymer, polyethyleneimine, polyethyleneamine, reactive group-containing polyester resin, and reactive group-containing poly(meth)acrylic resin. Among them, polyvinyl alcohol, saponified vinyl acetate polymer, saponified vinyl acetate-ethylene copolymer, and saponified vinyl acetate-acrylic acid copolymer are preferred in consideration of releasability and ease of handling. The saponification degree of the saponified vinyl acetate polymer is preferably 50% or more, more preferably 60% or more. The saponification degree of the saponified vinyl acetate polymer is preferably 90% or less, more preferably 80% or less. That is, the degree of saponification of the saponified vinyl acetate polymer is preferably 50% or more and 90% or less, and more preferably 60% or more and 80% or less.

[0083] Examples of compounds having an alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates, long-chain alkyl group-containing acid chlorides, long-chain alkyl group-containing amines, and long-chain alkyl group-containing alcohols. Examples of long-chain alkyl group-containing isocyanates include hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, and behenyl isocyanate. Examples of long-chain alkyl group-containing acid chlorides include hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, and behenyl chloride. Among these, in consideration of releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred.

[0084] The long-chain alkyl group-containing polymer compound can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of the long-chain alkyl (meth)acrylate include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.

[0085] In particular, the long-chain alkyl group-containing polymeric compound is a reaction product of a saponification product of a vinyl acetate polymer having a degree of saponification of 50% or more and 90% or less, particularly 60% or more and 80% or less, with a long-chain alkyl group-containing isocyanate, and it is preferable that the long-chain alkyl group has a carbon number of 20 or more and 25 or less.

[0086] In the long-chain alkyl group-containing polymer compound, the degree of polymerization of the main chain is, for example, 200 or more and 6,000 or less.

[0087] The number of carbon atoms in the long-chain alkyl group, the basic structure of the main chain, the degree of polymerization of the main chain, and the fact that the long-chain alkyl group-containing polymeric compound is a reaction product of a saponified vinyl acetate polymer and a long-chain alkyl group-containing isocyanate are analyzed by Fourier transform infrared spectroscopy (FT-IR).

[0088] The content of the long-chain alkyl group-containing polymer compound in the antistatic layer is, for example, preferably 30 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more, relative to 100 parts by mass of the binder resin and the antistatic agent in total. The content of the long-chain alkyl group-containing polymer compound is, for example, preferably 100 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 80 parts by mass or less, relative to 100 parts by mass of the binder resin and the antistatic agent in total. That is, the content of the long-chain alkyl group-containing polymer compound is, for example, preferably 30 parts by mass or more and 100 parts by mass or less, more preferably 40 parts by mass or more and 90 parts by mass or less, and even more preferably 50 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the binder resin and the antistatic agent in total. If the content of the long-chain alkyl group-containing polymer compound is too low, the effect of improving the peeling performance of the end tape may not be sufficiently obtained. On the other hand, if the content of the long-chain alkyl group-containing polymer compound is too high, the peel strength to the carrier tape may decrease, or the transparency may decrease.

[0089] (d) Additives The antistatic layer may contain additives, if necessary. Examples of the additives include a filler.

[0090] (3) Other aspects of the antistatic layer The thickness of the antistatic layer is, for example, 0.02 μm or more and 3 μm or less. If the thickness of the antistatic layer is within the above range, the cover tape can be provided with antistatic properties.

[0091] The method for forming the antistatic layer may be, for example, a method in which an antistatic layer composition in which a binder resin, an antistatic agent, a specific additive, etc. are dispersed or dissolved in a solvent is used, the composition is applied to the surface of the base layer opposite to the heat seal layer, and then dried. The method for applying the composition for the antistatic layer may be a known application method such as air doctor, blade coat, knife coat, rod coat, bar coat, direct roll coat, reverse roll coat, gravure coat, slide coat, etc.

[0092] 3.Base material layer The substrate layer in the present disclosure is a layer that supports the antistatic layer, the intermediate layer, and the heat seal layer. As the substrate layer, various materials can be applied as long as they have mechanical strength to withstand external forces during storage and transportation, and heat resistance to withstand manufacturing and taping packaging. For example, polyester, polyamide, polyolefin, etc. can be mentioned. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-isophthalate copolymer, terephthalic acid-cyclohexane dimethanol-ethylene glycol copolymer, etc. Examples of polyamide include nylon 6, nylon 66, nylon 610, etc. Examples of polyolefin include polyethylene, polypropylene, polymethylpentene, etc. Among them, polyester is preferred, and polyethylene terephthalate and polyethylene naphthalate are more preferred. These materials are low cost and have good mechanical strength.

[0093] Furthermore, the base layer may contain additives as necessary, such as fillers, plasticizers, colorants, and antistatic agents.

[0094] The substrate layer may be a single layer or a laminate of the same or different layers. The substrate layer may be a stretched film or an unstretched film. In particular, the substrate layer may be a film stretched uniaxially or biaxially for the purpose of improving the strength.

[0095] The thickness of the base layer is, for example, 2.5 μm or more, may be 6 μm or more, or may be 12 μm or more. The thickness of the base layer is, for example, 300 μm or less, may be 100 μm or less, or may be 50 μm or less. That is, the thickness of the base layer is, for example, 2.5 μm or more and 300 μm or less, may be 6 μm or more and 100 μm or less, or may be 12 μm or more and 50 μm or less. If the thickness of the base layer is too thick, the rigidity during tape packaging becomes strong, which is disadvantageous in terms of handling and cost. If the thickness of the base layer is too thin, the water vapor barrier property may decrease and the mechanical strength may be insufficient.

[0096] 4. Heat seal layer When a package is produced using the cover tape of the present disclosure, the heat seal layer of the present disclosure is heat sealed to the carrier tape, thereby adhering the cover tape to the carrier tape.

[0097] The heat seal layer contains a thermoplastic resin. The thermoplastic resin is preferably any one of an ethylene-based polymer, an acrylic resin, a polyester resin, a polyurethane resin, and a vinyl chloride-vinyl acetate copolymer, or a resin containing these as a main component. Among them, the heat seal layer preferably contains an ethylene-based polymer.

[0098] An ethylene-based polymer is a polymer containing a structural unit derived from ethylene. Examples of the ethylene-based polymer include an ethylene homopolymer and an ethylene copolymer of ethylene and another monomer.

[0099] Examples of ethylene homopolymers include low density polyethylene (LDPE), linear low density polyethylene (L-LDPE), medium density polyethylene (MDPE), and high density polyethylene (HDPE).

[0100] Examples of other monomers constituting the ethylene copolymer include olefin monomers, unsaturated carboxylic acids, unsaturated carboxylic acid esters, vinyl esters, and styrene. Examples of olefin monomers include propylene, butene, pentene, hexene, and octene. Examples of unsaturated carboxylic acids include acrylic acid and methacrylic acid. Examples of unsaturated carboxylic acid esters include methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, and diethyl maleate. Examples of vinyl esters include vinyl acetate, vinyl propionate, fumaric acid, maleic anhydride, and maleic acid monoester. These may be used alone or in combination of two or more.

[0101] The ethylene copolymer is preferably an ethylene-vinyl acetate copolymer (EVA resin) or an acrylic-styrene copolymer. In particular, the heat seal layer preferably contains an EVA resin. When the heat seal layer contains an EVA resin, the heat sealability to the carrier tape is improved. Therefore, unintended peeling of the cover tape during transportation or storage of the package can be suppressed.

[0102] An EVA resin is a copolymer containing at least an ethylene monomer unit and a vinyl acetate monomer unit. The ethylene monomer unit refers to a structural unit derived from an ethylene monomer, and the vinyl acetate monomer unit refers to a structural unit derived from a vinyl acetate monomer.

[0103] The EVA resin may contain a third monomer unit in addition to the ethylene monomer unit and the vinyl acetate monomer unit. The third monomer unit may have a functional group having antistatic properties.

[0104] The content of the EVA resin in the heat seal layer is not particularly limited. The content of the EVA resin is, for example, 50% by mass or more, and may be 60% by mass or more. On the other hand, the content of the EVA resin is, for example, 100% by mass or less, and may be 80% by mass or less. That is, the content of the EVA resin is, for example, 50% by mass or more and 100% by mass or less, and may be 60% by mass or more and 80% by mass or less. When the content of the EVA resin is high, the heat sealability is improved.

[0105] When the heat seal layer contains an EVA resin, it may further contain a polyethylene resin, which can suppress deterioration in a high-humidity and high-heat environment while maintaining good heat sealability.

[0106] Examples of the polyethylene resin include low density polyethylene, linear low density polyethylene, medium density polyethylene, high density polyethylene, etc. Among these, low density polyethylene and linear low density polyethylene are preferred from the viewpoint of dispersibility.

[0107] In this specification, the classifications of various polyethylenes refer to those defined in the old JIS K6748:1995 and JIS K6899-1:2000.

[0108] The content of the polyethylene resin in the heat seal layer is, for example, 50% by mass or less, and may be 40% by mass or less. On the other hand, the content of the polyethylene resin is, for example, 0% by mass or more, and may be 20% by mass or more. That is, the content of the polyethylene resin is, for example, 0% by mass or more and 50% by mass or less, and may be 20% by mass or more and 40% by mass or less. If the content of the polyethylene resin is high, the heat sealability may be reduced.

[0109] The heat seal layer may contain additives such as a tackifier, an antistatic agent, a dispersant, a filler, a plasticizer, a colorant, and an antiblocking agent, if necessary.

[0110] The thickness of the heat seal layer is not particularly limited. The thickness of the heat seal layer is, for example, 1 μm or more, and may be 10 μm or more. On the other hand, the thickness of the heat seal layer is, for example, 30 μm or less, and may be 20 μm or less. That is, the thickness of the heat seal layer is, for example, 1 μm or more and 30 μm or less, and may be 10 μm or more and 20 μm or less. If the thickness of the heat seal layer is too thin, the heat sealability may be poor or a uniform film may not be obtained. On the other hand, if the thickness of the heat seal layer is too thick, the transparency of the cover tape may be reduced.

[0111] The method for forming the heat seal layer is not particularly limited, and known methods can be used. For example, a method (extrusion lamination method) can be used in which the raw material of the heat-melted film is extruded onto the base layer or intermediate layer using a T-die or the like, and then pressed onto the base layer or intermediate layer using a cooling roll. In addition, a method can be used in which a pre-manufactured film is attached to the base layer or intermediate layer using an adhesive. For example, a polyester adhesive, a polyurethane adhesive, an acrylic adhesive, etc. can be used as the adhesive.

[0112] Another method for forming the heat seal layer includes, for example, a method of applying a composition for heat seal layer, which is prepared by dispersing or dissolving a thermoplastic resin and an additive in a solvent, onto a substrate layer and drying the composition. Examples of the method for applying the composition for heat seal layer include known application methods such as roll coating, reverse roll coating, gravure coating, gravure reverse coating, comma coating, bar coating, wire bar coating, rod coating, kiss coating, knife coating, die coating, flow coating, dip coating, and spray coating.

[0113] 5. Middle tier In the present disclosure, the intermediate layer is disposed between the base material layer and the heat seal layer, thereby improving the adhesion between the base material layer and the heat seal layer. In addition, when the cover tape of the present disclosure is heat sealed to the carrier tape, the intermediate layer improves the cushioning property. Therefore, heat can be applied to the heat seal layer more uniformly.

[0114] The resin material used for the intermediate layer can be appropriately selected depending on the materials of the base layer and the heat seal layer, and examples thereof include polyolefin, polyurethane, and polyester. Examples of polyolefin include polyethylene, polypropylene, and ethylene-methacrylate copolymer.

[0115] The thickness of the intermediate layer is, for example, 5 μm or more and 50 μm or less. A film can be used as the intermediate layer. In this case, the lamination method of the base layer and the intermediate layer is not particularly limited, and a known method can be used. For example, a method (extrusion lamination method) can be mentioned in which the raw material of the heat-melted film is extruded onto the base layer with a T-die or the like, quenched and solidified with a cooling roll, and pressure-bonded to the base layer. As a result, the intermediate layer is formed on one side of the base layer. It is preferable that an anchor coat layer is formed in advance on the surface of the base layer on which the intermediate layer is to be disposed. Another example is a method in which a pre-manufactured film is attached to the base layer with an adhesive.

[0116] 6.Adhesive layer The cover tape of the present disclosure may have an adhesive layer between the base layer and the intermediate layer, or between the intermediate layer and the heat seal layer. By disposing the adhesive layer, the adhesion between the base layer and the intermediate layer, or between the intermediate layer and the heat seal layer, can be improved.

[0117] The adhesive layer may be appropriately selected depending on the materials used for the base layer, intermediate layer, and heat seal layer, and is not particularly limited. For example, an olefin-based adhesive, an acrylic-based adhesive, an isocyanate-based adhesive, a urethane-based adhesive, or an ester-based adhesive may be used for the adhesive layer.

[0118] The adhesive layer can be formed by coating an adhesive composition. The method for coating the adhesive composition is not particularly limited, and examples of the method include gravure coating and roll coating.

[0119] The thickness of the adhesive layer is not particularly limited as long as it can improve the adhesion between the base layer and the intermediate layer, or between the intermediate layer and the heat seal layer, and may be adjusted as appropriate.

[0120] B. Packaging The packaging body of the present disclosure comprises a carrier tape having a plurality of storage sections for storing electronic components, the electronic components stored in the storage sections, and the above-mentioned cover tape arranged to cover the storage sections.

[0121] 2(a) and (b) are a schematic plan view and a cross-sectional view showing an example of a package according to the present disclosure. Note that since Fig. 2(a) and (b) are described in the above section "A. Cover tape for packaging electronic components," a description thereof will be omitted here.

[0122] Each component of the packaging body of the present disclosure will be described below.

[0123] 1.Cover tape The cover tape in this disclosure has been described above in the section "A. Cover tape for packaging electronic components," so description thereof will be omitted here.

[0124] In the package of the present disclosure, the heat seal layer of the cover tape and the carrier tape are bonded by a heat seal portion. The heat seal portion can be disposed, for example, in a part of the portion where the heat seal layer of the cover tape contacts the carrier tape. That is, the heat seal layer may have a heat seal portion and a non-heat seal portion. This can improve the peeling performance of the cover tape from the carrier tape.

[0125] 2. Carrier tape The carrier tape in the present disclosure is a member having a plurality of storage sections for storing electronic components.

[0126] The carrier tape may be any tape having a plurality of storage sections, and may be, for example, an embossed carrier tape (also called an embossed tape), a punched carrier tape (also called a punched tape), or a pressed carrier tape (also called a pressed tape). Among these, an embossed carrier tape is preferably used from the viewpoints of cost, moldability, dimensional accuracy, etc.

[0127] Examples of materials for the carrier tape include plastics such as polyvinyl chloride, polystyrene, polyester, polypropylene, polycarbonate, polyacrylonitrile, ABS resin, etc., and paper, etc. In this specification, paper refers to a material containing cellulose as a main component and may further contain a resin component.

[0128] The thickness of the carrier tape is appropriately selected depending on the material of the carrier tape, the thickness of the electronic components, etc. The thickness of the carrier tape is, for example, 30 μm or more and 1500 μm or less. If the thickness of the carrier tape is too thick, the moldability may be deteriorated. On the other hand, if the thickness of the carrier tape is too thin, the strength may be insufficient.

[0129] The carrier tape has a plurality of storage sections. The storage sections are usually arranged at predetermined intervals in the longitudinal direction of the carrier tape. The size, depth, pitch, etc. of the storage sections are appropriately adjusted according to the size, thickness, etc. of the electronic components.

[0130] As a method for forming a carrier tape having a storage portion, a general molding method for a carrier tape can be applied and is appropriately selected depending on the type and material of the carrier tape, etc. Examples of the method include press molding, vacuum molding, compressed air molding, punching, and compression processing.

[0131] 3. Electronic Components The electronic components used in the package of the present disclosure are not particularly limited, and examples thereof include ICs, resistors, capacitors, inductors, transistors, diodes, LEDs (light-emitting diodes), liquid crystal, piezoelectric element resistors, filters, crystal oscillators, crystal vibrators, connectors, switches, volumes, relays, etc. The type of IC is also not particularly limited.

[0132] 4.Other The package in the present disclosure is used for storing and transporting electronic components. The electronic components are stored and transported in the package and are then mounted on a substrate or the like. During mounting, the cover tape is peeled off, and the electronic components stored in the storage section of the carrier tape are removed and mounted on a substrate or the like.

[0133] The package in the present disclosure is usually wound with the cover tape on the outside and the carrier tape on the inside, and is stored with an end tape affixed to the end where the winding ends. A general end tape can be used.

[0134] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0135] The present disclosure will be described in further detail below with reference to examples and comparative examples.

[0136] [material] Polyetheramine surfactants 1 NOF Corp.'s Nymeen L-201 (Polyoxyethylene laurylamine) Polyetheramine surfactants 2 NOF Corp., Nimean T2-202 (Polyoxyethylene Beef Tallow Alkylamine) Polyetheramine surfactants 3 NOF Corp.'s Nymeen L-202 (Polyoxyethylene Laurylamine) Polyetheramine surfactants 4 NOF Corp.'s Nymeen S-204 (Polyoxyethylene Stearylamine) Ester surfactants NOF Corp. Nonion OP-85R (sorbitan trioleate) Ether surfactants 1 NOF Corp. Nonion S-202 (polyoxyethylene stearyl ether) Ether surfactants 2 NOF Corp. Dispanol LS-100 (polyoxyalkylene ether)

[0137] Long-chain alkyl-containing polymer compound 1 Lion Specialty Chemicals Piroil 406 Long-chain alkyl-containing polymer compound 2 Resem P-677 (polyvinyl alcohol with long-chain alkyl groups on the side chains) manufactured by Chukyo Yushi Co., Ltd.

[0138] [Example 1] First, an antistatic composition was prepared. A conductive coating agent ("U690" manufactured by Chukyo Yushi Co., Ltd.) containing polyester resin and PEDOT / PSS was dissolved in isopropyl alcohol and water (isopropyl alcohol / water = 6 / 4) to obtain a solution with a solid content of 0.6% by mass. 10 parts by mass of the polyetheramine surfactant 1 (Nimeen L-201 manufactured by NOF Corp., polyoxyethylene laurylamine) was added to the above solution per 100 parts by mass of polyester resin and PEDOT / PSS in total to prepare an antistatic composition. The conductive coating agent ("U690" manufactured by Chukyo Yushi Co., Ltd.) is a solution with a solid content of 3.5% by mass, containing about 3.4% by mass of polyester resin and about 0.1% by mass of PEDOT / PSS.

[0139] As a substrate layer, a biaxially oriented polyethylene terephthalate film ("FE2002" manufactured by Futamura Chemical Co., Ltd.) having a thickness of 25 μm and having been subjected to corona treatment on both sides (hereinafter referred to as PET film) was prepared. The above-mentioned antistatic composition was applied to one side of the above-mentioned PET film to form an antistatic layer having a thickness of 0.02 μm.

[0140] Next, polyurethane adhesives "Takenate A-3075" manufactured by Mitsui Chemicals Inc. and "Takelac A-3210" manufactured by Mitsui Chemicals Inc. were mixed in a mass ratio of 3:1 and diluted with ethyl acetate to a solid content of 5 mass% to prepare an adhesive composition. The adhesive composition was applied to the surface of the PET film opposite the antistatic layer to form an adhesive layer.

[0141] Next, polyethylene resin (Novatec LD LC600A manufactured by Japan Polyethylene Corporation, density 0.918 g / cm 3 ) was melted and extruded onto the surface of the adhesive layer, and an intermediate layer having a thickness of 15 μm was formed by extrusion lamination using a cooling roll.

[0142] Next, a heat seal composition ("MELTHENE MX74E" manufactured by Tosoh Corporation) was melted and extruded onto the surface of the intermediate layer, and a heat seal layer having a thickness of 15 μm was formed by extrusion lamination using a cooling roll.

[0143] This resulted in a cover tape having an antistatic layer, a base layer, an adhesive layer, an intermediate layer, and a heat seal layer.

[0144] [Comparative Example 1] A cover tape was produced in the same manner as in Example 1, except that the specific additive was not added in the preparation of the antistatic composition.

[0145] [Examples 2 to 9 and Comparative Examples 2 to 4] A cover tape was produced in the same manner as in Example 1, except that in preparing the antistatic composition, the specific additive used was changed and the amount of the specific additive added was changed.

[0146] [Comparative Example 5] A cover tape was prepared in the same manner as in Example 1, except that an antistatic layer was formed as described below.

[0147] An antistatic composition was prepared by diluting a quaternary ammonium salt type acrylic polymer ("1sx-1090" manufactured by Taisei Fine Chemical Co., Ltd.) with methanol to a solid content of 3% by mass. The antistatic composition was applied to one side of a PET film to form an antistatic layer having a thickness of 1.0 μm.

[0148] [Comparative Example 6] A cover tape was prepared in the same manner as in Example 1, except that in preparing the antistatic composition, a release agent (NOF Corporation's "Modiper F226", a block copolymer having a fluorine-based polymer component and an acrylic polymer component) was used as an additive, and the amount of additive added was changed.

[0149] [Comparative Example 7] A cover tape was prepared in the same manner as in Example 1, except that in preparing the antistatic composition, a release agent (NOF Corporation's "Modiper FS770", a block copolymer having a silicone polymer component and an acrylic polymer component) was used as an additive, and the amount of additive added was changed.

[0150] [evaluation] (1)Surface resistivity The surface resistivity of the surface of the cover tape on the antistatic layer side was measured by the method described above in the section "A. Cover tape for packaging electronic components: 1. Physical properties of the cover tape."

[0151] (2) Peel strength against end tape The peel strength to the end tape was measured by the method described above in the section "A. Cover tape for packaging electronic components 1. Physical properties of the cover tape."

[0152] (3) Peel strength from carrier tape The peel strength to the carrier tape was measured by the method described above in the section "A. Cover tape for packaging electronic components: 1. Physical properties of the cover tape."

[0153] (4) Haze In the examples and comparative examples, the haze of the laminate in which an antistatic layer was formed on one surface of the base layer was measured using a haze meter "NDH 7000" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K7136:2000.

[0154] (5) Evaluation of end tape peeling (5-1) Early period A reel sample was prepared using the cover tape. Using a Nitto Kogyo taping machine "NST-35," the paper carrier tape and the cover tape were heat-sealed under the following conditions, and approximately 40 m of the tape was wound onto a reel with a core diameter of 3 inches to obtain a reel sample.

[0155] <Taping conditions> Paper carrier tape: Hokuetsu Corporation, thickness 0.31 mm, width 8 mm, virgin paper Carrier tape feed hole pitch: 2mm Taping temperature: 190℃ Taping speed: 3500 tacts Seal width: 0.6mm Taping iron size: 0.6mm x 2 lines Taping iron length (seal length in one stroke): 8±1mm

[0156] An end tape manufactured by NIPPO was attached to the end of the reel sample using a pressure roller. The reel sample was then left to stand at 23±2°C and 50±10% RH for 60 minutes. The end tape was then peeled off from the reel sample by hand at a peeling speed of 12 m / min and a peeling angle of 120° to 170°. The peeling of the end tape was evaluated according to the following criteria. A: The heat-sealed portion did not peel off from the carrier tape. B: A portion of the heat-sealed area was peeled off from the calibrator tape by approximately 4 to 50 mm.

[0157] (5-2) After the second environmental test As described in the above section "A. Cover tape for packaging electronic components 1. Physical properties of the cover tape," the cover tape was subjected to a second environmental test. After the second environmental test, the first cover tape was peeled off from the second cover tape, and then a taping sample was produced using the first cover tape. Using a taping machine "NST-35" manufactured by Nitto Kogyo Co., Ltd., the surface of the heat seal layer side of the first cover tape was heat sealed to the carrier tape under the following conditions, to obtain a taping sample.

[0158] <Taping conditions> Paper carrier tape: Hokuetsu Corporation, thickness 0.31 mm, width 8 mm, virgin paper Carrier tape feed hole pitch: 2mm Taping temperature: 190℃ Taping speed: 3500 tacts Seal width: 0.6mm Taping iron size: 0.6mm x 2 lines Taping iron length (seal length in one stroke): 8±1mm

[0159] Next, an end tape manufactured by NIPPO Corporation was attached to the surface of the cover tape of the taping sample on the antistatic layer side by rolling a pressure roller twice back and forth, and then left to stand for 60 minutes at 23±2°C and 50±10% RH. Next, the end tape was peeled off from the taping sample by hand at a peeling speed of 12 m / min and a peeling angle of 120° to 170°. The peeling of the end tape was evaluated according to the following criteria. A: The heat-sealed portion did not peel off from the carrier tape. B: A portion of the heat-sealed area was peeled off from the calibrator tape by approximately 4 to 50 mm.

[0160] [Table 1]

[0161] [Table 2]

[0162] As can be seen from Tables 1 and 2, in Examples 1 to 9, the surface resistivity of the antistatic layer side of the cover tape, the initial peel strength from the end tape, the peel strength from the end tape after the first environmental test, and the peel strength from the carrier tape after the second environmental test were all within the specified ranges, so that the antistatic performance was high and the end tape was easy to peel off.

[0163] On the other hand, in Comparative Examples 1, 3, 4, 6, and 7, the initial peel strength from the end tape and the peel strength from the end tape after the first environmental test were high, and the end tape was difficult to peel off. In Comparative Example 5, a quaternary ammonium salt, which is a conventionally widely used antistatic agent, was used, and therefore the peel strength from the carrier tape after the second environmental test was high. This is thought to be because even quaternary ammonium salt-type polymers tend to bleed out, and blocking reduces the heat seal performance.

[0164] Examples 1 to 6 and Comparative Examples 1, 3 and 4 show that the antistatic layer preferably contains a polyetheramine surfactant. Examples 7 to 9 and Comparative Examples 1, 6 and 7 show that the antistatic layer also preferably contains a polymer compound having a long-chain alkyl group on the side chain.

[0165] In Comparative Example 2, the ester surfactant was not mixed into the solution containing the binder resin and PEDOT / PSS, so the properties could not be measured. This is because the HLB value of the ester surfactant is low.

[0166] In the present disclosure, for example, the following inventions are provided. [1] A cover tape for packaging electronic components, comprising an antistatic layer, a base layer, an intermediate layer, and a heat seal layer in this order, The surface resistivity of the surface on the antistatic layer side is 1×10 10 Less than Ω / □ The peel strength against NIPPO end tape is 2.0N or less. With the end tape attached to the surface of the antistatic layer of the cover tape for packaging electronic components, the peel strength of the end tape after storage for 100 hours under an environment of 40°C and 90% RH is 2.0 N or less; In a state where the surface of the cover tape for packaging electronic components on the heat seal layer side and the surface of the cover tape for packaging electronic components on the antistatic layer side are overlapped, the tape is subjected to a strength of 125 kN / m 2 the peel strength of the surface of the cover tape for packaging electronic components on the heat seal layer side from the carrier tape is greater than 0.15 N after storage for 100 hours while applying a pressure of 0.15 N. [2] The cover tape for packaging electronic components according to [1], wherein the antistatic layer contains a binder resin and a conductive polymer. [3] The cover tape for packaging electronic components according to [1] or [2], wherein the antistatic layer contains a polyetheramine type surfactant. [4] The cover tape for packaging electronic components according to [1] or [2], wherein the antistatic layer contains a polymer compound having a long-chain alkyl group on the side chain. [5] a carrier tape having a plurality of storage sections for storing electronic components; An electronic component stored in the storage unit; A cover tape for packaging electronic components according to any one of [1] to [4], which is arranged to cover the storage section; A packaging body comprising: [Explanation of symbols]

[0167] 1 … Cover tape 2 … Antistatic layer 3...Base material layer 4. Middle class 5 ... Heat seal layer 10 … Packaging 11 ... Carrier tape 12 … Storage area 13 … Electronic Components 21 … End tape

Claims

1. A cover tape for packaging electronic components, comprising an antistatic layer, a base layer, an intermediate layer, and a heat seal layer in this order, The surface resistivity of the surface on the antistatic layer side is 1×10 10 is less than Ω / □, The peel strength against NIPPO end tape is 2.0 N or less. In a state where the end tape is attached to a surface of the antistatic layer of the cover tape for packaging electronic components, the cover tape has a peel strength of 2.0 N or less after storage for 100 hours under an environment of 40° C. and 90% RH; In a state where the surface of the cover tape for packaging electronic components on the heat seal layer side and the surface of the cover tape for packaging electronic components on the antistatic layer side are overlapped, the tape is subjected to a strength of 125 kN / m under an environment of 40° C. and 90% RH. 2 The cover tape for packaging electronic components has a peel strength of more than 0.15 N from a carrier tape on the surface of the heat seal layer side of the cover tape for packaging electronic components after storage for 100 hours while applying a pressure of 0.15 N.

2. 2. The cover tape for packaging electronic components according to claim 1, wherein the antistatic layer comprises a binder resin and a conductive polymer.

3. 2. The cover tape for packaging electronic components according to claim 1, wherein the antistatic layer contains a polyetheramine type surfactant.

4. 2. The cover tape for packaging electronic components according to claim 1, wherein the antistatic layer comprises a polymer compound having a long-chain alkyl group on the side chain.

5. a carrier tape having a plurality of storage sections for storing electronic components; An electronic component stored in the storage section; A cover tape for packaging electronic components according to any one of claims 1 to 4, which is disposed so as to cover the storage section; A packaging body comprising:

Citation Information

Patent Citations

  • Cover tape for electronic parts packaging

    JP4159979B2

Cited By

  • Cover tape and packaging for electronic components

    JP2026137495A

  • Cover tape and packaging for electronic components

    JP7899910B1

  • Cover tape and packaging for electronic components

    JP7907710B1

  • Cover tape and packaging for electronic components

    JP7907711B1

  • Cover tape for packaging electronic components, and electronic component package

    WO2026172791A1