Thermosetting resin composition, resin sheet, metal base substrate, and electronic device
By integrating a dihydroxy compound and bifunctional epoxy compound with a mesogenic skeleton, the thermal conductivity of thermosetting resin compositions is enhanced, addressing the insufficiency of existing resin compositions for heat dissipation in electronic components.
Patent Information
- Application Number
- JP2023044518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing thermosetting resin compositions, particularly those based on epoxy resins, do not achieve sufficient thermal conductivity for effective heat dissipation in electronic components.
Incorporation of a dihydroxy compound and bifunctional epoxy compound with a mesogenic skeleton, along with a curing accelerator and thermally conductive fillers, to enhance the thermal conductivity and heat resistance of the resin composition.
The resulting thermosetting resin composition achieves high thermal conductivity, making it suitable for heat dissipation in electronic devices and components.
Smart Images

Figure 2024134291000040 
Figure 2024134291000041 
Figure 2024134291000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, a resin sheet made of the thermosetting resin composition, an electronic device comprising a cured product of the resin sheet as a thermally conductive sheet, a metal base substrate comprising the cured product of the resin sheet, and an electronic device comprising the metal base substrate. [Background technology]
[0002] With the high integration of semiconductors and the rapid improvement of the processing power of electronic devices, electronic components with high processing power generate a lot of heat. Therefore, heat countermeasures to effectively dissipate heat from electronic components to the outside have become a very important issue. As a countermeasure for such heat dissipation, thermally conductive members made of heat dissipating materials such as metals, ceramics, and polymer compositions are used for heat dissipation members such as printed wiring boards, semiconductor packages, housings, heat pipes, heat sinks, and heat diffusion plates.
[0003] Among these heat dissipation members, thermally conductive epoxy resin molded products molded from epoxy resin compositions are excellent in electrical insulation properties, mechanical properties, heat resistance, chemical resistance, adhesive properties, etc., and are therefore widely used mainly in the electrical and electronic fields as castings, laminates, sealing materials, thermally conductive sheets, adhesives, etc.
[0004] Epoxy resin compositions constituting thermally conductive epoxy resin molded bodies are known to contain a thermally conductive filler with high thermal conductivity blended into a polymer matrix material such as resin, rubber, etc. Examples of thermally conductive fillers that have been used include metal oxides such as aluminum oxide, magnesium oxide, zinc oxide, and quartz, metal nitrides such as boron nitride and aluminum nitride, metal carbides such as silicon carbide, metal hydroxides such as aluminum hydroxide, metals such as gold, silver, and copper, carbon fibers, and graphite.
[0005] When even higher thermal conductivity is required, thermally conductive epoxy resin compositions and thermally conductive epoxy resin molded bodies in which a special thermally conductive filler is blended with epoxy resin have been proposed (for example, Patent Document 1). It has also been proposed to improve the thermal conductivity and heat resistance of the epoxy resin itself (for example, Patent Document 2). In Patent Document 2, an insulating composition with improved thermal conductivity is obtained by polymerizing a liquid crystal epoxy resin having a mesogen group. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-193504 A [Patent Document 2] Patent Application No. 2004-331811 Summary of the Invention [Problem to be solved by the invention]
[0007] However, as a result of investigations by the present inventors, it was found that the resin composition described in Patent Document 2 has room for further improvement in terms of thermal conductivity. [Means for solving the problem]
[0008] The present invention has been made in consideration of the above problems, and has been completed based on the discovery that a compound having a specific mesogenic skeleton has high thermal conductivity.
[0009] According to the present invention, there are provided a thermosetting resin composition, a resin sheet, a metal base substrate, and an electronic device, as shown below. [1] A dihydroxy compound represented by formula (1-1), A bifunctional epoxy compound having two epoxy groups represented by the formula (d-EP), A thermosetting resin composition comprising: [ka] In formula (1-1), Z represents -C(=O)-, -CH2-, or -NH-; [ka] In formula (d-EP), X is a divalent group having a mesogenic skeleton. Thermosetting resin composition. [2] The thermosetting resin composition according to item [1], In the formula (d-EP), X contains a divalent group represented by formula (2). [ka] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position. [3] The thermosetting resin composition according to item [2], In the group represented by the formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom. [4] The thermosetting resin composition according to item [2], In the group represented by the formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom. [5] The thermosetting resin composition according to item [2], In the group represented by the formula (2), R 1 ~R 8 are all hydrogen atoms. [6] The thermosetting resin composition according to any one of items [1] to [5], The thermosetting resin composition further comprises a curing accelerator. [7] The thermosetting resin composition according to any one of items [1] to [6], The thermosetting resin composition further comprises a thermally conductive filler. [8] A resin sheet comprising the thermosetting resin composition according to any one of items [1] to [7]. [9] A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, The thermally conductive sheet is made of a cured resin sheet according to item [8].
[10] A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal-based substrate made of a cured resin sheet according to item [8].
[11] An electronic device comprising the metal base substrate according to item
[10] .
[12] A thermosetting resin composition comprising an epoxy compound represented by formula (1-2): [ka] In formula (1-2), Z represents -C(=O)-, -CH2-, or -NH-. Thermosetting resin composition.
[13] The thermosetting resin composition according to item
[12] , The thermosetting resin composition further comprises a curing accelerator.
[14] The thermosetting resin composition according to item
[12] or
[13] , The thermosetting resin composition further comprises a thermally conductive filler.
[15] A resin sheet comprising the thermosetting resin composition according to any one of items
[12] to
[14] .
[16] A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, The thermally conductive sheet is made of a cured resin sheet according to item
[15] .
[17] A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate made of a cured resin sheet according to item
[15] .
[18] An electronic device comprising the metal base substrate according to item
[17] .
[19] A thermosetting resin composition comprising a phenoxy resin represented by formula (3): [ka] In formula (3), n is a number representing a repeating unit and represents an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), [ka] In formula (1-3), Z represents -C(=O)-, -CH2-, or -NH-; * indicates a linking position. Thermosetting resin composition.
[20] The thermosetting resin composition according to item
[19] , X in the formula (3) contains a divalent group represented by the formula (2), [ka] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position.
[21] The thermosetting resin composition according to item
[20] , In the group represented by formula (2), R1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
[22] The thermosetting resin composition according to item
[20] , In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, and R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
[23] The thermosetting resin composition according to item
[20] , In the group represented by formula (2), R 1 ~R 8 are all hydrogen atoms.
[24] The thermosetting resin composition according to any one of items
[19] to
[23] , The thermosetting resin composition further comprises a curing accelerator.
[25] The thermosetting resin composition according to any one of items
[19] to
[24] , The thermosetting resin composition further comprises a thermally conductive filler.
[26] The thermosetting resin composition according to any one of items
[19] to
[25] , The thermosetting resin composition further comprises an epoxy resin that is solid at room temperature.
[27] A resin sheet comprising the thermosetting resin composition according to any one of items
[19] to
[26] .
[28] A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, The thermally conductive sheet is made of a cured resin sheet according to item
[27] .
[29] A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate made of a cured resin sheet according to item
[27] .
[30] An electronic device comprising the metal base substrate according to item
[29] . According to the present invention, there is provided a thermosetting resin composition that can be used to produce a thermally conductive sheet having high thermal conductivity. Effect of the Invention
[0010] According to the present invention, there is provided a thermosetting resin composition that can be used to produce a thermally conductive sheet having high thermal conductivity. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view showing a structure of a metal base substrate according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a configuration of an electronic device using a metal base substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference symbols and their description will be omitted as appropriate. In addition, "~" indicates "above" to "below" unless otherwise specified.
[0013] [First embodiment] The thermosetting resin composition according to the first embodiment of the present invention comprises: A dihydroxy compound represented by formula (1-1), and a difunctional epoxy compound having two epoxy groups, represented by the formula (d-EP).
[0014] [ka]
[0015] In formula (1-1), Z represents -C(=O)-, -CH2-, or -NH-.
[0016] [ka]
[0017] In formula (d-EP), X is a divalent group having a mesogenic skeleton.
[0018] The thermosetting resin composition of the present embodiment contains a dihydroxy compound represented by the above formula (1-1). The compound represented by formula (1-1) has high planarity and high rigidity. Therefore, the cured product of the thermosetting resin composition containing this has high thermal conductivity.
[0019] The thermosetting resin composition of the present embodiment contains a bifunctional epoxy compound having a mesogenic skeleton represented by formula (d-EP). By containing such an epoxy compound having a mesogenic skeleton, the thermosetting resin composition of the present embodiment has high thermal conductivity when it is cured.
[0020] Hereinafter, the components used in the thermosetting resin composition in the first embodiment will be described.
[0021] (Dihydroxy Compounds) Examples of the compound represented by the above formula (1-1) used in the thermosetting resin composition of this embodiment include 2,7-dihydroxyfluorenone (2,7-dihydroxy-9H-fluoren-9-one) (a compound in which Z in formula (1-1) is -C(=O)-), 2,7-dihydroxyfluorene (a compound in which Z in formula (1-1) is -CH2-), and 2,7-dihydroxycarbazole (a compound in which Z in formula (1-1) is -NH-). Among these, it is preferable to use 2,7-dihydroxyfluorenone because it has high thermal conductivity and is easy to handle.
[0022] The compound represented by the above formula (1-1) may be a commercially available product or may be synthesized by a method known in the art. For example, the synthesis method of 2,7-dihydroxyfluorenone is described in Tetrahedron (2019), 75(2), 236-245.
[0023] The amount of the dihydroxy compound represented by the formula (1-1) in the thermosetting resin composition of the present embodiment is, for example, 2% by mass or more and 25% by mass or less, and preferably 5% by mass or more and 20% by mass or less, based on the total solid content of the thermosetting resin composition. By adding the dihydroxy compound within the above range, the fluidity of the resulting resin composition can be adjusted to a desired level, and the thermal conductivity of the cured product can be improved.
[0024] (Difunctional epoxy compound) The difunctional epoxy compound used in the thermosetting resin composition of the present embodiment is a compound represented by the formula (d-EP).
[0025] [ka]
[0026] In the formula (d-EP), X is a divalent group having a mesogenic skeleton. The thermosetting resin composition of the present embodiment contains a bifunctional epoxy compound having a mesogenic skeleton, and thus the obtained cured product has high thermal conductivity and high heat resistance.
[0027] Examples of the mesogenic skeleton of the X group in formula (d-EP) include a biphenyl skeleton, a naphthalene skeleton, a phenylbenzoate skeleton, an azobenzene skeleton, a stilbene skeleton, a cyclohexylbenzene skeleton, and derivatives thereof. When the X group has the above-mentioned mesogenic skeleton, the cured product of the obtained thermosetting resin composition can have high thermal conductivity.
[0028] In one embodiment, at least one of the X groups in formula (d-EP) is a group represented by formula (2). By using a bifunctional epoxy compound in which the X group in formula (d-EP) is a mesogenic skeleton represented by formula (2), the cured product of the thermosetting resin composition of this embodiment has high thermal conductivity and excellent heat resistance.
[0029] [ka]
[0030] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents the linking position.
[0031] In one embodiment, the bifunctional epoxy compound is a compound in which R1, R4, R5, and R8 in formula (2) are alkyl groups having 1 to 4 carbon atoms, and R2, R3, R6, and R7 are hydrogen atoms. Among them, the bifunctional epoxy compound is an epoxy compound in which R1, R4, R5, and R8 in formula (2) are alkyl groups having 1 carbon atom (methyl group), and R2, R3, R6, and R7 are hydrogen atoms (X group is a "tetramethylbiphenyl group"). By using such a bifunctional epoxy compound, the cured product of the obtained thermosetting resin composition can have a good balance between thermal conductivity and heat resistance.
[0032] In one embodiment, the bifunctional epoxy compound is an epoxy compound in which R1, R4, R5, and R8 in formula (2) are alkyl groups having one carbon atom, and R2, R3, R6, and R7 are hydrogen atoms (X group is a "biphenyl group"). By using such a bifunctional epoxy compound, the cured product of the obtained thermosetting resin composition has excellent thermal conductivity and heat resistance.
[0033] In one embodiment, the bifunctional epoxy compound represented by formula (d-EP) is preferably a compound containing a tetramethylbiphenyl group and a biphenyl group as the X group. By containing such a combination of bifunctional epoxy compounds, the cured product of the obtained thermosetting resin composition can have an excellent balance between thermal conductivity and heat resistance.
[0034] The bifunctional epoxy compounds may be used alone or in combination of two or more.
[0035] The amount of the bifunctional epoxy compound represented by the formula (d-EP) in the thermosetting resin composition of the present embodiment is, for example, 2% by mass or more and 40% by mass or less, and preferably 4% by mass or more and 30% by mass or less, based on the total solid content of the thermosetting resin composition. By blending the bifunctional epoxy compound within the above range, the curing properties of the resulting resin composition can be adjusted to an appropriate level.
[0036] (Cure accelerator) The thermosetting resin composition of the present embodiment may contain a curing accelerator. The type and amount of the curing accelerator are not particularly limited, and an appropriate one can be selected from the viewpoints of reaction speed, reaction temperature, storage property, etc.
[0037] Examples of the curing accelerator that can be used include imidazoles, organic phosphorus compounds, tertiary amines, phenolic compounds, organic acids, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of increasing the heat resistance of the resulting resin composition, it is preferable to use a nitrogen atom-containing compound such as imidazoles.
[0038] Examples of the imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-diethylimidazole, 2-phenyl-4-methyl-5-hydroxyimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-phenylimidazolium trimellitate.
[0039] Examples of the organic phosphorus compound include triphenylphosphine, tri-p-tolylphosphine, tetraphenylphosphonium tetraphenylborate, triphenylphosphine triphenylborane, and 1,2-bis-(diphenylphosphino)ethane. Examples of the tertiary amines include triethylamine, tributylamine, 1,4-diazabicyclo[2.2.2]octane, and 1,8-diazabicyclo(5,4,0)undecene-7. Examples of the phenol compound include phenol resin, bisphenol A, nonylphenol, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, and allylphenol. Examples of the organic acid include acetic acid, benzoic acid, salicylic acid, and p-toluenesulfonic acid.
[0040] The amount of the curing accelerator to be added is, for example, 0.01 to 10 mass%, preferably 0.02 to 5 mass%, and more preferably 0.05 to 1.5 mass%, based on the total solid content of the thermosetting resin composition.
[0041] (Thermal conductive filler) The thermosetting resin composition of the present embodiment may contain a thermally conductive filler. By blending the thermally conductive filler, the thermosetting resin composition of the present embodiment can be used as a material for producing a heat dissipation member. The thermally conductive filler may contain, for example, highly thermally conductive inorganic particles having a thermal conductivity of 20 W / m·K or more. Examples of highly thermally conductive inorganic particles include alumina, aluminum nitride, boron nitride, silicon nitride, silicon carbide, and magnesium oxide. These may be used alone or in combination of two or more.
[0042] When boron nitride is used as the thermally conductive filler, the boron nitride may contain monodisperse particles, agglomerated particles, or a mixture thereof, of scaly boron nitride. The scaly boron nitride may be granulated. By using agglomerated particles of scaly boron nitride, the thermal conductivity of the resulting thermosetting resin composition can be further increased. The agglomerated particles may be sintered particles or non-sintered particles.
[0043] The amount of the thermally conductive filler is, for example, 40% by mass to 90% by mass, preferably 50% by mass to 80% by mass, based on the total solid content of the thermosetting resin composition. By using the thermally conductive filler in the amount within the above range, the thermal conductivity of the cured product can be improved while maintaining the handleability of the obtained resin composition. The thermally conductive filler may be surface-treated with a silane coupling agent.
[0044] (Silane coupling agent) The thermosetting resin composition of the present embodiment may contain a silane coupling agent. This can improve the compatibility of the thermally conductive filler in the thermosetting resin composition. The coupling agent may be added to the thermosetting resin composition, or may be used by treating the surface of the thermally conductive filler.
[0045] The amount of the silane coupling agent to be added is from 0.05% by mass to 3% by mass, and preferably from 0.1% by mass to 2% by mass, based on the mass of the thermally conductive filler.
[0046] (Other Ingredients) The thermosetting resin composition of the present embodiment may contain other components in addition to the above-mentioned components. Examples of the other components include an antioxidant and a leveling agent.
[0047] (Method for producing thermosetting resin composition) The thermosetting resin composition of the present embodiment can be prepared as a resin varnish (a varnish-like thermosetting resin composition) by dissolving, mixing, and stirring the above-mentioned components other than the thermally conductive filler in a solvent. This mixing can be performed using various mixers such as an ultrasonic dispersion type, a high-pressure collision dispersion type, a high-speed rotation dispersion type, a bead mill type, a high-speed shear dispersion type, and a rotation-revolution dispersion type.
[0048] The solvent is not particularly limited, but examples thereof include acetone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone.
[0049] A thermosetting resin composition in a B-stage state can be obtained by adding a thermally conductive filler to the resin varnish and kneading the mixture using a three-roll mill or the like. By adding the filler during kneading, it is possible to disperse the inorganic filler more uniformly in the thermosetting resin, but this is not limited thereto. The thermally conductive filler may be added during kneading, or may be added during mixing of the resin varnish. After kneading, the mixture may be cooled and solidified, and the kneaded product may be processed into a granular, tablet, or sheet shape.
[0050] [Second embodiment] The thermosetting resin composition according to the second embodiment of the present invention contains an epoxy compound represented by formula (1-2). [ka]
[0051] In formula (1-2), Z represents -C(=O)-, -CH2-, or -NH-.
[0052] The epoxy compound represented by the above formula (1-2) has high planarity and high rigidity, and therefore the cured product of the thermosetting resin composition containing this has high thermal conductivity.
[0053] Hereinafter, the components used in the thermosetting resin composition in the second embodiment will be described.
[0054] (Epoxy compounds) Examples of the epoxy compound having a glycidyloxy group and represented by the above formula (1-2) used in the thermosetting resin composition of the present embodiment include a fluorenone derivative in which Z in formula (1-2) is -C(=O)-, a fluorene derivative in which Z in formula (1-2) is -CH2-, and a carbazole derivative in which Z in formula (1-2) is -NH-. Among these, it is preferable to use fluorenone derivatives because they have high thermal conductivity and good handleability.
[0055] The epoxy compound represented by the above formula (1-2) can be synthesized by reacting the dihydroxy compound represented by the above formula (1-1) with epihalohydrin in the presence of an alkali metal hydroxide to glycidylate the dihydroxy compound.
[0056] As the epihalohydrin used in the synthesis of the above epoxy compound, epichlorohydrin, α-methylepichlorohydrin, γ-methylepichlorohydrin, epibromohydrin, etc. can be used. Epichlorohydrin is preferably used because it is easily available. The amount of epihalohydrin used is, for example, 2 to 20 moles, preferably 4 to 10 moles, per mole of hydroxyl group of the dihydroxy compound of formula (1-1).
[0057] Examples of alkali metal hydroxides that can be used in the above reaction include sodium hydroxide and potassium hydroxide. These may be in the form of a solid or an aqueous solution thereof. When an aqueous solution is used, it is preferable to continuously add the aqueous solution of the alkali metal hydroxide to the reaction system, continuously distill water and epihalohydrin under reduced pressure or normal pressure, and then separate the mixture to remove water, and continuously return epihalohydrin to the reaction system. The amount of the alkali metal hydroxide used is, for example, 0.3 to 10.0 mol, preferably 1.0 to 5.0 mol, and more preferably 1.2 to 3.0 mol, relative to 1 mol of the hydroxyl group of the dihydroxy compound of formula (1-1).
[0058] The reaction temperature for the glycidylation reaction of a dihydroxy compound using the epihalohydrin is usually 30 to 90° C., preferably 35 to 80° C. The reaction time is usually 0.5 to 10 hours, preferably 1 to 8 hours. After completion of the reaction, the reaction mixture thus produced is purified by known means such as washing with water and / or distillation to obtain the desired epoxy compound.
[0059] (Cure accelerator) The thermosetting resin composition of the present embodiment may contain a curing accelerator. The curing accelerator that can be used and the amount of the curing accelerator that can be used are the same as the curing accelerator used in the thermosetting resin composition according to the first embodiment.
[0060] (Thermal conductive filler) The thermosetting resin composition of the present embodiment may contain a thermally conductive filler. The thermally conductive filler that can be used and the amount of the filler to be added are the same as those used in the thermosetting resin composition according to the first embodiment.
[0061] (Silane coupling agent) The thermosetting resin composition of the present embodiment may contain a silane coupling agent. The silane coupling agent that can be used and the amount of the silane coupling agent that can be used are the same as the silane coupling agent used in the thermosetting resin composition according to the first embodiment.
[0062] (Method for producing thermosetting resin composition) The thermosetting resin composition of this embodiment can be prepared as a resin varnish (a varnish-like thermosetting resin composition) by dissolving, mixing, and stirring the above-mentioned components other than the thermally conductive filler in a solvent. The mixing method and the solvent used are the same as those in the method for producing the thermosetting resin composition according to the first embodiment.
[0063] [Third embodiment] The thermosetting resin composition according to the third embodiment of the present invention contains a phenoxy resin represented by formula (3). [ka]
[0064] In formula (3), n is a number representing a repeating unit, and represents an integer of 2 to 50, preferably an integer of 5 to 40, more preferably an integer of 6 to 30, and further more preferably an integer of 8 to 20. X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), [ka] In formula (1-3), Z represents -C(=O)-, -CH2-, or -NH-; * indicates the linkage position.
[0065] The phenoxy resin represented by the above formula (3) contains a structural unit that is highly planar and rigid, and therefore a cured product of a resin composition containing such a phenoxy resin has high thermal conductivity.
[0066] The components used in the third thermosetting resin composition will be described below.
[0067] (Phenoxy resin) In the phenoxy resin represented by the above formula (3) used in the thermosetting resin composition of this embodiment, X in formula (3) is a divalent group having a mesogenic skeleton. The phenoxy resin used in the thermosetting resin composition of this embodiment contains the structural unit (X) having a mesogenic skeleton, and thus the cured product thereof has high thermal conductivity and high heat resistance.
[0068] Examples of the mesogenic skeleton of the X group in formula (3) include a biphenyl skeleton, a naphthalene skeleton, a phenylbenzoate skeleton, an azobenzene skeleton, a stilbene skeleton, a cyclohexylbenzene skeleton, and derivatives thereof. Since the X group has the above-mentioned mesogenic skeleton, the phenoxy resin can have high thermal conductivity.
[0069] In one embodiment, at least one of the X groups in formula (3) is a group represented by formula (2). By including a structure having a mesogenic skeleton represented by formula (2), the phenoxy resin has high thermal conductivity and excellent heat resistance, and therefore the thermosetting resin of this embodiment containing the phenoxy resin can have high thermal conductivity.
[0070] [ka]
[0071] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents the linking position.
[0072] In one embodiment, the group represented by formula (2) is preferably a group in which R1, R4, R5, and R8 are alkyl groups having 1 to 4 carbon atoms, and R2, R3, R6, and R7 are hydrogen atoms. Among them, a group in which R1, R4, R5, and R8 are alkyl groups having 1 carbon atom, and R2, R3, R6, and R7 are hydrogen atoms in formula (2) (referred to as a "tetramethylbiphenyl group") is preferred because the phenoxy resin containing it can achieve a good balance between thermal conductivity and heat resistance.
[0073] In one embodiment, the group represented by formula (2) may be a group in which R1, R4, R5, and R8 are alkyl groups having one carbon atom, and R2, R3, R6, and R7 are hydrogen atoms (referred to as a "biphenyl group"). By including such a group, the phenoxy resin has excellent thermal conductivity and heat resistance.
[0074] In one embodiment, the phenoxy resin represented by formula (3) preferably contains a tetramethylbiphenyl group and a biphenyl group as the X group. A phenoxy resin containing a combination of these groups can have a good balance between thermal conductivity and heat resistance.
[0075] The phenoxy resin represented by formula (3) contains a divalent group represented by the above formula (1-3) as the Y group. The group represented by formula (1-3) has high planarity and high rigidity. Therefore, the phenoxy resin containing such a group has high thermal conductivity, and as a result, the cured product obtained from the thermosetting resin composition containing it has high thermal conductivity.
[0076] The weight average molecular weight (Mw) of the phenoxy resin represented by formula (3) is, for example, 1,000 to 10,000, preferably 2,000 to 8,000, more preferably 3,000 to 7,000, and even more preferably 3,500 to 6,500. Mw is a value measured by gel permeation chromatography and converted using a standard polystyrene calibration curve. By setting Mw in the above range, the thermal conductivity of the phenoxy resin can be further improved.
[0077] In this embodiment, the weight average molecular weight (Mw) of the phenoxy resin represented by formula (3) can be measured by obtaining a molecular weight distribution curve using GPC (Gel Permeation Chromatography). The weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity (PDI: Mw / Mn) of the phenoxy resin are calculated using polystyrene-equivalent values obtained from a calibration curve of standard polystyrene (PS) obtained by GPC measurement.
[0078] The measurement conditions for GPC are, for example, as follows. Tosoh Corporation gel permeation chromatography device HLC-8320GPC Column: TSK-GEL GMH, G2000H, SuperHM-M manufactured by Tosoh Corporation Detector: UV detector for liquid chromatography Measurement temperature: 40℃ Solvent: THF Sample concentration: 2.0 mg / ml
[0079] The polydispersity (Mw / Mn) of the phenoxy resin represented by formula (3) is, for example, 1.00 to 7.00, preferably 2.00 to 6.00, and more preferably 3.50 to 5.50. By setting the polydispersity within the above range, the thermal conductivity and flowability of the phenoxy resin can be further improved.
[0080] The phenoxy resin represented by formula (3) may contain a low molecular weight phenoxy resin having a weight average molecular weight (Mw) of 1000 or less. When the phenoxy resin contains a low molecular weight phenoxy resin, the low molecular weight phenoxy resin is, for example, 5% or more and 60% or less, preferably 5% or more and 50% or less, as a ratio of the total area of components corresponding to a weight average molecular weight Mw of 1,000 or less to the total area 100% of the entire molecular weight distribution obtained by GPC measurement. The phenoxy resin containing the low molecular weight phenoxy resin in the above range has improved fluidity and excellent handleability. Therefore, for example, the processing stability is improved when the resin composition of the present embodiment is processed into the form of a sheet or film.
[0081] The epoxy equivalent of the phenoxy resin represented by formula (3) is, from the viewpoint of the effects of the present invention, for example, 300 to 6,000 g / eq, preferably 350 to 5,000 g / eq, and more preferably 400 to 4,500 g / eq.
[0082] The phenoxy resin represented by formula (3) has the above-mentioned structure, and thus the cured product has high thermal conductivity. The thermal conductivity of the cured product of the phenoxy resin is, for example, 0.3 W / (m·K) or more. Since the phenoxy resin itself has high thermal conductivity, the cured product of the thermosetting resin composition containing it can also have high thermal conductivity.
[0083] (Production of phenoxy resin) The phenoxy resin represented by formula (3) used in this embodiment can be synthesized by reacting a bifunctional epoxy compound represented by formula (d-EP) with a dihydroxy compound represented by formula (1-1). The bifunctional epoxy compound represented by formula (d-EP) is the same as the bifunctional epoxy compound represented by formula (d-EP) in the first embodiment. The dihydroxy compound represented by formula (1-1) is the same as the dihydroxy compound represented by formula (1-1) in the first embodiment.
[0084] [ka]
[0085] [ka]
[0086] The above reaction can be carried out in the absence of a solvent or in the presence of a reaction solvent using a reaction catalyst.
[0087] Suitable reaction solvents include aprotic organic solvents such as methyl ethyl ketone, dioxane, tetrahydrofuran, acetophenone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, sulfolane, propylene glycol monomethyl ether, cyclohexanone, etc. The use of a reaction solvent can reduce the initial viscosity and improve the reactivity of the raw material monomers.
[0088] As the reaction catalyst, a conventionally known polymerization catalyst can be used, and alkali metal hydroxides, tertiary amine compounds, quaternary ammonium compounds, tertiary phosphine compounds, quaternary phosphonium compounds, and imidazole compounds are preferably used.
[0089] Specifically, a bifunctional epoxy compound represented by formula (d-EP), a dihydroxy compound represented by formula (1-1), a reaction catalyst, and optionally a reaction solvent are added and melt-mixed under stirring. The heating temperature during melt-mixing is about 90 to 150°C, the mixing time is about 30 minutes to 2 hours, and the reaction pressure is normal pressure. After melt-mixing, the mixed solution is heated and a polymerization reaction is carried out at a predetermined reaction temperature under reduced pressure or normal pressure. The reaction temperature is about 140 to 180°C, the reaction time is about 2 hours to 10 hours, and the reaction pressure is about 1 to 760 Torr.
[0090] After the reaction is completed, the phenoxy resin can be obtained as a resin dissolved in a suitable solvent by performing solvent replacement, etc. In addition, the phenoxy resin obtained by the solvent reaction can be obtained as a solid resin that does not contain the solvent by performing a solvent removal treatment using an evaporator, etc.
[0091] In the above synthesis method, a phenoxy resin having a desired weight average molecular weight can be obtained by adjusting the degree of polymerization by appropriately selecting reaction conditions such as the amounts of starting materials used, the reaction temperature, and the reaction time.
[0092] (Cure accelerator) The thermosetting resin composition of the present embodiment may contain a curing accelerator. The curing accelerator that can be used and the amount of the curing accelerator that can be used are the same as the curing accelerator used in the thermosetting resin composition according to the first embodiment.
[0093] (Thermal conductive filler) The thermosetting resin composition of the present embodiment may contain a thermally conductive filler. The thermally conductive filler that can be used and the amount of the filler that can be added are the same as the thermally conductive filler used in the thermosetting resin composition according to the first embodiment.
[0094] (Silane coupling agent) The thermosetting resin composition of the present embodiment may contain a silane coupling agent. The silane coupling agent that can be used and the amount of the silane coupling agent that can be used are the same as the silane coupling agent used in the thermosetting resin composition according to the first embodiment.
[0095] (Epoxy resin) In one embodiment, the thermosetting resin composition may contain another epoxy resin in addition to the phenoxy resin. Specifically, it is preferable that a part or all of the epoxy resin is a solid epoxy resin at room temperature (25° C.).
[0096] In one embodiment, the other epoxy resin includes an epoxy resin that is liquid at room temperature or an epoxy resin that is semi-solid at room temperature in addition to an epoxy resin that is solid at room temperature, which improves the moldability of the resulting thermosetting resin composition.
[0097] When the thermosetting resin composition of the present embodiment contains the epoxy resin that is solid at room temperature, the blending amount of the epoxy resin is, for example, 5% by mass or more and 40% by mass or less, and preferably 10% by mass or more and 30% by mass or less, based on the components (resin content) of the thermosetting resin composition excluding the thermally conductive filler. This can improve the curability of the thermosetting resin composition and can further improve the thermal conductivity and insulating properties of the obtained cured product.
[0098] (Method for producing thermosetting resin composition) The thermosetting resin composition of this embodiment can be prepared as a resin varnish (a varnish-like thermosetting resin composition) by dissolving, mixing, and stirring the above-mentioned components other than the thermally conductive filler in a solvent. The mixing method and the solvent used are the same as those in the method for producing the thermosetting resin composition according to the first embodiment.
[0099] [Resin sheet] The resin sheet of the present embodiment is a sheet-like product obtained by curing the first, second or third thermosetting resin composition. The specific form of the resin sheet includes a carrier substrate and a resin layer formed on the carrier substrate and made of the thermosetting resin composition of the above embodiment.
[0100] The resin sheet of the present embodiment can be obtained, for example, by applying a varnish-like thermosetting resin composition onto a carrier substrate to obtain a coating film (resin layer) and then carrying out a solvent removal treatment. The solvent content in the resin sheet can be 10 mass% or less based on the entire thermosetting resin composition. For example, the solvent removal treatment can be carried out under conditions of 80°C to 200°C and 1 minute to 30 minutes.
[0101] The resin sheet (resin layer) of this embodiment is preferably in a B-stage state.
[0102] In this embodiment, the carrier substrate may be, for example, a polymer film or a metal foil. Examples of the polymer film include, but are not limited to, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonates, release papers such as silicone sheets, and heat-resistant thermoplastic resin sheets such as fluorine-based resins and polyimide resins. Examples of the metal foil include, but are not limited to, copper and / or copper-based alloys, aluminum and / or aluminum-based alloys, iron and / or iron-based alloys, silver and / or silver-based alloys, gold and gold-based alloys, zinc and zinc-based alloys, nickel and nickel-based alloys, and tin and tin-based alloys.
[0103] The resin substrate of the present embodiment has an insulating layer made of the cured product of the thermosetting resin composition. This resin substrate can be used as a material for a printed circuit board on which electronic components such as LEDs and power modules are mounted.
[0104] [Electronic equipment] The cured resin sheet is used as a thermally conductive sheet interposed between a heat generating body and a heat dissipating body.
[0105] Examples of the heating element include a semiconductor element, an LED element, a substrate on which a semiconductor element or an LED element is mounted, a Central Processing Unit (CPU), a power semiconductor, a lithium ion battery, and a fuel cell. Examples of the heat dissipator include a heat sink, a heat spreader, and a heat dissipation (cooling) fin. The heat dissipation insulating member may be partially composed of the thermosetting resin composition of this embodiment, and specific examples include a heat dissipation sheet obtained by curing the thermosetting resin composition, and a laminate in which the heat dissipation sheet and a substrate are laminated (for example, the metal base substrate 100 in FIG. 1). The substrate is not particularly limited as long as it is a heat dissipating metal substrate, and may be, for example, a copper substrate, a copper alloy substrate, an aluminum substrate, or an aluminum alloy substrate, with a copper substrate or an aluminum substrate being preferred, and a copper substrate being more preferred. By using a copper substrate or an aluminum substrate, the heat dissipation properties of the heat dissipation insulating member can be improved. The heat dissipating and insulating member is partially composed of the thermosetting resin composition of this embodiment, and has a thermal conductivity of preferably 12 W / m·K or more, and more preferably 15 W / m·K or more. The heat dissipating insulation member and the heat sink may be formed on one side or both sides of the heating element. In addition, various base materials or layers may be provided between the heating element and the heat dissipating insulation member, or between the heat dissipating insulation member and the heat sink, as long as they do not affect the heat dissipation properties.
[0106] In this embodiment, the heat generating body, the heat dissipation and insulation member, and the heat dissipation body can be appropriately combined from those described above to obtain a laminated structure. The laminated structure can be used for various applications requiring heat dissipation and insulation, such as semiconductor devices, smartphones, LED bulbs and lights, power modules, lithium ion batteries, fuel cells, wireless base stations, and uninterruptible power supplies. Hereinafter, the components contained in the thermosetting resin composition of the present embodiment will be described.
[0107] [Metal base board] A metal base substrate (heat dissipating resin member) 100 of this embodiment will be described with reference to FIG. FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a metal base substrate 100. As shown in FIG.
[0108] 1, the metal base substrate 100 may include a metal substrate 101, an insulating layer 102 provided on the metal substrate 101, and a metal layer 103 provided on the insulating layer 102. The insulating layer 102 may be made of one material selected from the group consisting of a resin layer made of the above-mentioned thermosetting resin composition, a cured product of the thermosetting resin composition, and a laminate. Each of the resin layer and the laminate may be made of a thermosetting resin composition (resin sheet) in a B-stage state before the circuit processing of the metal layer 103, and may be a cured product obtained by curing the resin composition after the circuit processing.
[0109] The metal layer 103 is provided on the insulating layer 102 and is subjected to circuit processing. Examples of metals constituting the metal layer 103 include one or more selected from copper, copper alloys, aluminum, aluminum alloys, nickel, iron, tin, and the like. Among these, the metal layer 103 is preferably a copper layer or an aluminum layer, and is particularly preferably a copper layer. By using copper or aluminum, the circuit processing property of the metal layer 103 can be improved. The metal layer 103 may be a metal foil available in a plate shape, or a metal foil available in a roll shape.
[0110] The lower limit of the thickness of the metal layer 103 is, for example, 0.01 mm or more, and preferably 0.035 mm or more, so long as it is applicable to applications requiring a high current. The upper limit of the thickness of the metal layer 103 is, for example, 10.0 mm or less, and preferably 5 mm or less. If the thickness is less than this value, the circuit processability can be improved, and the substrate as a whole can be made thinner.
[0111] The metal substrate 101 has a role of dissipating heat accumulated in the metal base substrate 100. The metal substrate 101 is not particularly limited as long as it is a heat dissipating metal substrate, but may be, for example, a copper substrate, a copper alloy substrate, an aluminum substrate, or an aluminum alloy substrate, with a copper substrate or an aluminum substrate being preferred, and a copper substrate being more preferred. By using a copper substrate or an aluminum substrate, the heat dissipation properties of the metal substrate 101 can be improved. The thickness of the metal substrate 101 can be appropriately set as long as it does not impair the object of the present invention.
[0112] The upper limit of the thickness of the metal substrate 101 is, for example, 20.0 mm or less, and preferably 5.0 mm or less. If the thickness is less than this value, the workability of the metal base substrate 100 in the contour processing, cutting processing, and the like can be improved.
[0113] The lower limit of the thickness of the metal substrate 101 is, for example, 0.01 mm or more, and preferably 0.6 mm or more. By using a metal substrate 101 having a thickness of this value or more, the heat dissipation properties of the metal base substrate 100 as a whole can be improved.
[0114] In this embodiment, the metal base substrate 100 can be used for various substrate applications, but because of its excellent thermal conductivity and heat resistance, it can be used as a printed circuit board that uses an LED or a power module.
[0115] The metal base substrate 100 may have a metal layer 103 that is circuitized by etching or the like into a pattern. In this metal base substrate 100, a solder resist (not shown) may be formed on the outermost layer, and connection electrodes may be exposed so that electronic components can be mounted thereon by exposure and development.
[0116] [Semiconductor Devices] The metal base substrate (heat dissipation and insulation member) 100 of the embodiment can be used in various applications requiring heat dissipation and insulation properties, for example, in electronic devices such as semiconductor devices. FIG. 2 is a schematic cross-sectional view showing an example of a semiconductor device using the metal base substrate 100. As shown in FIG. A semiconductor element 201 is mounted on a metal layer 103 of a metal base substrate 100 via an adhesive layer 202 (die attach material). The semiconductor element 201 is connected to a connection electrode portion formed on the metal base substrate 100 via a bonding wire 203, and is mounted on the metal base substrate 100. The semiconductor element 201 is then encapsulated on the metal base substrate 100 by an encapsulation resin layer 205 .
[0117] A heat sink 207 is provided on the metal substrate 101 side of the metal base substrate 100 via a thermally conductive layer 206 (thermal interface material (TIM)). The heat sink 207 is made of a material with excellent thermal conductivity, such as aluminum, iron, or copper.
[0118] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES
[0119] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these.
[0120] <Example A1, Comparative Example A1> (Preparation of Thermosetting Resin Composition Containing Dihydroxy Compound) A resin composition was obtained by mixing the components according to the composition shown in Table 1. Details of each component in Table 1 are as follows. The amount of each component in Table 1 is expressed in parts by mass.
[0121] (Phenol compounds) Phenol compound 1: 2,7-dihydroxyfluorenone represented by the following formula (1-4) (manufactured by Tokyo Chemical Industry Co., Ltd.) [ka] Phenolic compound 2: Novolac type phenolic resin (Sumitomo Bakelite Co., Ltd., PR-55617)
[0122] (Difunctional epoxy compound) Bifunctional epoxy compound 1: a tetramethylbiphenyl type epoxy compound represented by the following formula (4) (manufactured by Mitsubishi Chemical Corporation, YX-4000H, solid at room temperature) [ka]
[0123] (Cure accelerator) Curing accelerator 1: 2-methyl-imidazole
[0124] (Measurement of physical properties of thermosetting resin composition) (Measurement of thermal conductivity) The resin composition of Example A1 or Comparative Example A1 was set in a mold coated with a release agent, and compression molding was performed at 180°C for 30 minutes to obtain a resin molded product of 10 mm square x 1 mm thick. Then, curing was performed in an oven at 180°C for 180 minutes to obtain a resin molded product 1 (a sample for measuring thermal conductivity). From the obtained resin molded body, a test piece was cut to 10 mm square x 1 mm thick for thickness direction measurement. Next, the thermal diffusion coefficient (α) of the plate-shaped test piece in the thickness direction was measured by the Xe flash method using a Xe flash analyzer LFA467 HyperFlash manufactured by NETZSCH. The measurement was performed under the condition of air atmosphere and 25°C. The thermal conductivity of the resin molded body was calculated from the measured values of thermal diffusion coefficient (α), specific heat (Cp), and density (Sp) according to the following formula. The results are shown in Table 1 below. Thermal conductivity [W / m K]=α[m 2 / s]×Cp[J / kg K]×Sp[g / cm 3 ]
[0125] [Table 1]
[0126] <Example B1, Comparative Example B1> (Preparation of Thermosetting Resin Composition Containing Epoxy Compound) A resin composition was obtained by mixing the components according to the composition shown in Table 2. Details of each component in Table 2 are as follows. The amount of each component in Table 2 is expressed in parts by mass.
[0127] (Epoxy compounds) Epoxy compound 1: a fluorenone-skeleton epoxy compound represented by the following formula (1-5), obtained by the following method: (Synthesis of epoxy compound 1) In a flask equipped with a stirrer, a reflux condenser, and a stirring device, 12.6 parts by weight of 2,7-dihydroxyfluorenone, 68.5 parts by weight of epichlorohydrin, 0.1 parts by weight of tetrabutylammonium chloride, and 2.5 parts by weight of dimethyl sulfoxide were added, and the mixture was heated to 60°C under stirring and reacted for 2 hours. 16.2 parts by weight of a 50% aqueous sodium hydroxide solution was added dropwise over 60 minutes, and the reaction was further carried out at 80°C for 6 hours. After the reaction was completed, the solvent such as excess epichlorohydrin was distilled off under reduced pressure using a rotary evaporator. THF was added to the residue so that the solid content was about 30%, and the residue was washed with water until the washing water became neutral, and the resulting solution was dried under reduced pressure to obtain the desired epoxy compound 1 with a yield of 84%. The obtained epoxy compound 1 was a red to reddish brown viscous epoxy resin, and was obtained as a crystalline resin-like solid by leaving it at room temperature. [ka]
[0128] Epoxy compound 2: a tetramethylbiphenyl type epoxy compound represented by the following formula (4) (manufactured by Mitsubishi Chemical Corporation, YX-4000H, solid at room temperature) [ka] (Cure accelerator) Curing accelerator 1: 2-methyl-imidazole
[0129] (Measurement of physical properties of thermosetting resin composition) (Measurement of thermal conductivity) The resin composition of Example B1 or Comparative Example B1 was set in a mold coated with a release agent, and compression molding was performed at 180°C for 30 minutes to obtain a resin molded product of 10 mm square x 1 mm thickness. Then, curing was performed in an oven at 180°C for 180 minutes to obtain a resin molded product 1 (a sample for measuring thermal conductivity). From the obtained resin molded body, a test piece was cut to 10 mm square x 1 mm thick for thickness direction measurement. Next, the thermal diffusion coefficient (α) of the plate-shaped test piece in the thickness direction was measured by the Xe flash method using a Xe flash analyzer LFA467 HyperFlash manufactured by NETZSCH. The measurement was performed under the condition of air atmosphere and 25°C. The thermal conductivity of the resin molded body was calculated from the measured values of thermal diffusion coefficient (α), specific heat (Cp), and density (Sp) according to the following formula. The results are shown in Table 1 below. Thermal conductivity [W / m K]=α[m 2 / s]×Cp[J / kg K]×Sp[g / cm 3 ]
[0130] [Table 2]
[0131] <Examples C1 to C5 and Comparative Examples C1 to C2> (Preparation of phenoxy resin) Using the following method, phenoxy resins 1 to 7 were prepared. The raw material monomers used in the preparation of the phenoxy resins are shown below. Epoxy monomer 1: a tetramethylbiphenyl type epoxy compound represented by the following formula (4) (manufactured by Mitsubishi Chemical Corporation, YX-4000H, solid at room temperature) [ka]
[0132] Epoxy monomer 2: an epoxy compound represented by the following formula (5) (manufactured by DIC Corporation, HP-4032D, liquid at room temperature) [ka]
[0133] Phenol monomer 1: 2,7-dihydroxyfluorenone represented by the following formula (1-4) (manufactured by Tokyo Chemical Industry Co., Ltd.) [ka]
[0134] Phenol monomer 2: 4,4'-biphenol (Tokyo Chemical Industry Co., Ltd.)
[0135] (Preparation of phenoxy resin 1) Epoxy monomer 1 (73.9 parts by weight), phenol monomer 1 (24.1 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were dropped into a reactor and melt-mixed at 110°C to 120°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 1 to phenol monomer 1 was 1.75. The obtained mixed liquid was heated to 170°C, and reacted while removing the solvent under reduced pressure at that temperature. It was confirmed by GPC that the molecular weight was the target, and the reaction was stopped to obtain phenoxy resin 1. The reaction was carried out for 5 hours. After the reaction, it was cooled to room temperature, and the obtained solid was pulverized and collected as a reddish brown powdery solid. 91 parts by weight of phenoxy resin 1 represented by the following formula (3) was obtained (the average value of the number of repeating units n in formula (3) is 1.9, X is a structural unit derived from epoxy monomer 1, Y is a structural unit derived from phenol monomer 1, and the weight average molecular weight Mw measured by GPC is 2240). [ka]
[0136] (Preparation of phenoxy resin 2) Epoxy monomer 1 (76.2 parts by weight), phenol monomer 1 (21.7 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were dropped into a reactor and melt-mixed at 110°C to 120°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 1 to phenol monomer 1 was 2.0. The obtained mixed liquid was heated to 160°C, and reacted while removing the solvent under reduced pressure at that temperature. It was confirmed by GPC that the molecular weight was the target, and the reaction was stopped to obtain phenoxy resin 2. The reaction was carried out for 5 hours. After the reaction, it was cooled to room temperature, and the obtained solid was pulverized and collected as a reddish brown powdery solid. 92 parts by weight of phenoxy resin 2 represented by formula (3) was obtained (the average value of the number of repeating units n in formula (3) is 2.1, X is a structural unit derived from epoxy monomer 1, Y is a structural unit derived from phenol monomer 1, and the weight average molecular weight Mw measured by GPC is 3600).
[0137] (Preparation of phenoxy resin 3) Epoxy monomer 1 (74.4 parts by weight), phenol monomer 1 (23.6 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were dropped into a reactor and melt-mixed at 110°C to 120°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 1 to phenol monomer 1 was 1.8. The obtained mixed liquid was heated to 160°C, and reacted while removing the solvent under reduced pressure at that temperature. It was confirmed by GPC that the target molecular weight was reached, and the reaction was stopped to obtain phenoxy resin 3. The reaction was carried out for 7 hours. After the reaction, it was cooled to room temperature, and the obtained solid was pulverized and collected as a reddish brown powdery solid. 91 parts by weight of phenoxy resin 3 represented by formula (3) was obtained (the average value of the number of repeating units n in formula (3) is 2.9, X is a structural unit derived from epoxy monomer 1, Y is a structural unit derived from phenol monomer 1, and the weight average molecular weight Mw measured by GPC is 7145).
[0138] (Preparation of phenoxy resin 4) Epoxy monomer 1 (75.4 parts by weight), phenol monomer 1 (22.6 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were dropped into a reactor and melt-mixed at 100°C to 110°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 1 to phenol monomer 1 was 1.9. The obtained mixed liquid was heated to 160°C, and reacted while removing the solvent under reduced pressure at that temperature. It was confirmed by GPC that the molecular weight was the target, and the reaction was stopped to obtain phenoxy resin 4. The reaction was carried out for 7 hours. After the reaction, it was cooled to room temperature, and the obtained solid was pulverized and collected as a reddish brown powdery solid. 88 parts by weight of phenoxy resin 4 represented by formula (3) was obtained (the average value of the number of repeating units n in formula (3) is 2.0, X is a structural unit derived from epoxy monomer 1, Y is a structural unit derived from phenol monomer 1, and the weight average molecular weight Mw measured by GPC is 4000).
[0139] (Preparation of phenoxy resin 5) Epoxy monomer 2 (72.6 parts by weight), phenol monomer 1 (25.3 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were added to a reactor and melt-mixed at 110°C to 120°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 2 to phenol monomer 1 was 1.9. The resulting mixture was heated to 160°C and reacted at that temperature while removing the solvent under reduced pressure. It was confirmed by GPC that the desired molecular weight was obtained, and the reaction was stopped to obtain phenoxy resin 5. The reaction was carried out for 5 hours. After the reaction, the mixture was cooled to room temperature, and the resulting solid was pulverized and collected as a reddish brown powdery solid. 93 parts by weight of phenoxy resin 5 represented by the above formula (3) (in formula (3), the average value of the number of repeating units n is 2.1, X is a structural unit derived from epoxy monomer 2, Y is a structural unit derived from phenol monomer 1, and the weight average molecular weight Mw by GPC is 2980) was obtained.
[0140] (Preparation of Phenoxy Resin 6) A bisphenol A type phenoxy resin represented by the following formula (6) (manufactured by Mitsubishi Chemical Corporation, YP-55) was used as phenoxy resin 6.
[0141] [ka]
[0142] (Preparation of phenoxy resin 7) Epoxy monomer 1 (75.9 parts by weight), phenol monomer 2 (22.1 parts by weight), triphenylphosphine (TPP) (0.04 parts by weight), and solvent (cyclohexanone) (2 parts by weight) were added to a reactor and melt-mixed at 110°C to 120°C for 1 hour. The equivalent ratio (Ep / Ph) of epoxy monomer 1 to phenol monomer 2 was 2.0. The resulting mixture was heated to 160°C, and reacted at that temperature while removing the solvent under reduced pressure. It was confirmed by GPC that the desired molecular weight was obtained, and the reaction was stopped to obtain phenoxy resin 1. The reaction was carried out for 10 hours. After the reaction, it was cooled to room temperature, and the resulting solid was pulverized and collected as a reddish brown powdery solid. 3.7 parts by weight of phenoxy resin 7 represented by the following formula (3) was obtained. (In formula (3), the average value of the number of repeating units n is 2.6, X is a structural unit derived from epoxy monomer 1, Y is a structural unit derived from phenol monomer 2, and the weight average molecular weight Mw measured by GPC is 4200.)
[0143] (Physical property measurement of phenoxy resin) The solvent solubility of the phenoxy resins 1 to 7 obtained in the above Examples C1 to C5 and Comparative Examples C1 to C2 was measured. The results are shown in Table 3-1.
[0144] (Solvent soluble (THF)) Each of the phenoxy resins 1 to 7 obtained in the above Examples C1 to C5 and Comparative Examples C1 to C2 was mixed with tetrahydrofuran (THF) and heated to 60°C to completely dissolve, thereby obtaining a THF solution with a non-volatile content of 30%. The solvent solubility of the phenoxy resin was evaluated based on the presence or absence of turbidity in the THF solution when cooled to room temperature (25°C). When the THF solution was transparent when cooled to room temperature, it was evaluated as "A", and when the THF solution was even slightly turbid when cooled to room temperature, it was evaluated as "B". The results are shown in Table 3-1.
[0145] (Solvent soluble (DMF)) Each of the phenoxy resins 1 to 7 obtained in the above Examples C1 to C5 and Comparative Examples C1 to C2 was mixed with DMF and heated to 60°C to completely dissolve, thereby obtaining a DMF solution with a non-volatile content of 30%. The solvent solubility of the phenoxy resin was evaluated based on the presence or absence of turbidity in the DMF solution when cooled to room temperature (25°C). When the DMF solution was transparent when cooled to room temperature, it was evaluated as "A", and when the DMF solution was even slightly turbid when cooled to room temperature, it was evaluated as "B". The results are shown in Table 3-1.
[0146] (Thermal diffusivity) The phenoxy resins 1 to 7 obtained in the above Examples C1 to C5 and Comparative Examples C1 to C2 and the curing accelerator 1 (2-methyl-imidazole) were mixed in the amounts shown in Table 3-1 to prepare resin compositions. The obtained resin compositions were set in a mold coated with a release agent, and compression molded at 180°C for 30 minutes to obtain a resin molded product of 10 mm square and 1 mm thick. Then, the product was cured in an oven at 180°C for 180 minutes to obtain a resin molded product 1 (a sample for measuring thermal conductivity). From the obtained resin molded body, a test piece was cut to 10 mm square x 1 mm thick for thickness direction measurement. Next, the thermal diffusion coefficient (α) of the plate-shaped test piece in the thickness direction was measured by the Xe flash method using a Xe flash analyzer LFA467 HyperFlash manufactured by NETZSCH. The measurement was performed under the condition of air atmosphere and 25°C. The measurements were performed in an air atmosphere at 25°C. A higher thermal diffusivity value indicates higher thermal conductivity. The measurement results are shown in Table 3-1.
[0147] [Table 3] (
[0148] <Example C6, Comparative Examples C3 to C4> (Preparation of thermosetting resin composition containing phenoxy resin) The components were mixed according to the ratio shown in Table 3-2 to obtain a resin composition. The details of each component in Table 3-2 are as follows. The amount of each component in Table 3-2 is expressed in parts by mass. (Phenoxy resin) Phenoxy resin 2: Phenoxy resin 2 obtained in the above "Preparation of phenoxy resin 2" (Epoxy resin) Epoxy resin 1: Dicyclopentadiene type epoxy resin (DIC, EPICLON HP-7200, solid at room temperature) (hardening agent) Hardener 1: Cyanate resin (Lonza, Primaset "PT-30") (Cure accelerator) Curing accelerator 1: Novolac resin (Sumitomo Bakelite, PR-55617) (Thermal conductive filler) Thermally conductive filler 1: Agglomerated boron nitride (HP40, manufactured by Mizushima Ferroalloy Co., Ltd.)
[0149] (Measurement of physical properties of cured product) The cured products of the thermosetting resin compositions obtained above were measured for the following physical properties.
[0150] (Thermal Conductivity) -Making resin molded products The obtained thermosetting resin composition containing the thermally conductive filler was sandwiched between 0.018 mm copper foil and compression molded at 10 MPa, 180°C, and 90 minutes to obtain a resin molded body (thermal conductivity measurement sample 1). A 10 mm square sample for thermal diffusivity measurement was cut out from the obtained molded body and used for thermal diffusivity measurement.
[0151] Density (specific gravity) of resin molded body The density (specific gravity) measurement was performed in accordance with JIS K 6911 (general test method for thermosetting plastics). Test pieces were cut from the above resin molded bodies to a size of 2 cm length x 2 cm width. The unit of density (specific gravity) (ρ) is g / cm. 3 Let us assume that.
[0152] -Specific heat of resin molded body The specific heat (Cp) of the resin molded article obtained above was measured by a DSC method.
[0153] -Measurement of thermal conductivity of resin molded products From the obtained resin molded body, a test piece of 10 mm square was cut out for thickness direction measurement. Next, the thermal diffusion coefficient (α) of the plate-shaped test piece in the thickness direction was measured by the unsteady method using a Xe flash analyzer LFA467 HyperFlash manufactured by NETZSCH. The measurement was performed under the condition of air atmosphere and 25°C. The thermal conductivity of the resin molded body was calculated from the measured values of thermal diffusion coefficient (α), specific heat (Cp), and density (ρ) according to the following formula. The results are shown in Table 3-2. Thermal conductivity [W / m K]=α[m 2 / s]×Cp[J / kg K]×ρ[g / cm 3 ]
[0154] (glass transition temperature) After removing the copper foil from the obtained molded body, a test piece was cut into a rectangular shape with a width of 8 mm. The test piece was subjected to thermomechanical analysis using a dynamic viscoelasticity measuring device (Seiko Instruments Inc., DMS6100) under the conditions of a measurement temperature range of 0°C to 400°C and a heating rate of 5°C / min, to measure the glass transition temperature. The unit of glass transition temperature is °C.
[0155] (5% weight loss temperature) Each of the thermosetting resin compositions obtained above was cured at 180°C for 90 minutes to obtain a cured product. The cured product was pulverized in a small pulverizer to obtain a sample, and the 5% weight loss temperature Td5 (°C) was measured using TG-DTA with a sample amount of 10 mg, a heating rate of 10°C / min, a measurement temperature range of 30 to 600°C, and an air atmosphere. A higher 5% weight loss temperature indicates higher heat resistance. The results are shown in Table 3-2.
[0156] (Volume resistivity) Each of the thermosetting resin composition molded bodies with copper foil obtained above was etched to prepare a circular electrode with a guard, and the volume resistivity at 25°C and at 175°C was measured. The unit of volume resistivity is Ω·m. A higher volume resistivity value indicates higher insulation. The results are shown in Table 3-2.
[0157] [Table 4] [Explanation of symbols]
[0158] 100 Metal base board 101 Metal Substrate 102 Insulating layer 103 Metal layer 200 Semiconductor device 201 Semiconductor elements 202 Adhesive layer 203 Bonding Wire 205 Sealing resin layer 206 Thermal Conduction Layer 207 Heatsink
Claims
1. A dihydroxy compound represented by formula (1-1), A bifunctional epoxy compound having two epoxy groups, represented by the formula (d-EP), A thermosetting resin composition comprising: [Formula 1] In formula (1-1), Z is -C(=O)-, -CH 2 represents - or -NH-; [Case 2] In formula (d-EP), X represents a divalent group having a mesogenic skeleton. Thermosetting resin composition.
2. The thermosetting resin composition according to claim 1, In the formula (d-EP), X contains a divalent group represented by formula (2). [C3] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position.
3. The thermosetting resin composition according to claim 2, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms; R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
4. The thermosetting resin composition according to claim 2, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
5. The thermosetting resin composition according to claim 2, In the group represented by formula (2), R 1 ~R 8 are all hydrogen atoms.
6. The thermosetting resin composition according to claim 1, The thermosetting resin composition further comprises a curing accelerator.
7. The thermosetting resin composition according to claim 1, The thermosetting resin composition further comprises a thermally conductive filler.
8. A resin sheet comprising the thermosetting resin composition according to claim 1 .
9. A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, An electronic device, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 8.
10. A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate comprising a cured product of the resin sheet according to claim 8.
11. An electronic device comprising the metal base substrate according to claim 10.
12. A thermosetting resin composition comprising an epoxy compound represented by formula (1-2): [C4] In formula (1-2), Z is -C(=O)-, -CH 2represents - or -NH-; Thermosetting resin composition.
13. The thermosetting resin composition according to claim 12, The thermosetting resin composition further comprises a curing accelerator.
14. The thermosetting resin composition according to claim 12, The thermosetting resin composition further comprises a thermally conductive filler.
15. A resin sheet comprising the thermosetting resin composition according to any one of claims 12 to 14.
16. A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, An electronic device, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 15.
17. A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, The thermally conductive sheet is a metal base substrate comprising a cured product of the resin sheet according to claim 15.
18. An electronic device comprising the metal base substrate of claim 17.
19. A thermosetting resin composition comprising a phenoxy resin represented by formula (3), [C5] In formula (3), n is a number representing a repeating unit and is an integer of 2 to 50; X is a divalent group having a mesogenic skeleton, Y is a divalent group represented by formula (1-3), [C6] In formula (1-3), Z is -C(=O)-, -CH 2 represents - or -NH-; * indicates a linking position. Thermosetting resin composition.
20. 20. The thermosetting resin composition according to claim 19, X in the formula (3) contains a divalent group represented by the formula (2), [C7] In formula (2), R 1 ~R 8 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and * represents a linking position.
21. The thermosetting resin composition according to claim 20, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is an alkyl group having 1 to 4 carbon atoms; R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
22. The thermosetting resin composition according to claim 20, In the group represented by formula (2), R 1 , R 4 , R 5 , and R 8 is a methyl group, R 2 , R 3 , R 6 , and R 7 is a hydrogen atom.
23. The thermosetting resin composition according to claim 20, In the group represented by formula (2), R 1 ~R 8 are all hydrogen atoms.
24. 20. The thermosetting resin composition according to claim 19, The thermosetting resin composition further comprises a curing accelerator.
25. 20. The thermosetting resin composition according to claim 19, The thermosetting resin composition further comprises a thermally conductive filler.
26. 20. The thermosetting resin composition according to claim 19, The thermosetting resin composition further comprises an epoxy resin that is solid at room temperature.
27. A resin sheet comprising the thermosetting resin composition according to any one of claims 19 to 26.
28. A heat generating member; A heat dissipation member; a thermally conductive sheet provided between the heat generating component and the heat dissipating component, 28. An electronic device, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 27.
29. A metal substrate; A thermally conductive sheet; A metal base substrate comprising, in this order, 28. A metal base substrate, wherein the thermally conductive sheet is made of a cured product of the resin sheet according to claim 27.
30. 30. An electronic device comprising the metal base substrate of claim 29.
Citation Information
Patent Citations
Imide skeleton-containing epoxy resin and curable epoxy resin composition containing the same
JP2000026572A
Epoxy compound and epoxy resin cured product
JP2005206678A
Epoxy resin, epoxy resin composition and cured product thereof
JP2007326982A
New bismaleimide having phenolic hydroxyl group, thermosetting resin composition using the same as essential component and its cured product
JP2009161605A
Resin-coated inorganic particle, thermosetting resin composition, semiconductor device, manufacturing method of resin-coated inorganic particle