Discoloration inhibitor for trivalent chromium chemical conversion coating and method for treating metal material including trivalent chromium chemical conversion coating using the same
A discoloration inhibitor using silicon compounds and carboxylic acids at pH 7.0 to 13.0 addresses trivalent chromium coating discoloration issues, ensuring efficient processing and maintaining coating integrity under adverse conditions.
Patent Information
- Application Number
- JP2023044663
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Trivalent chromium chemical conversion coatings suffer from discoloration issues, leading to reduced processing efficiency and product value, especially when exposed to high temperature and humidity environments, and existing solutions like colloidal silica treatments at low pH cause gelling and inefficiencies.
A discoloration inhibitor comprising silicon compounds and carboxylic acids with a pH of 7.0 to 13.0, specifically silicic acid, sodium silicate, and monocarboxylic or dicarboxylic acids, is used to form a trivalent chromium chemical conversion coating, suppressing discoloration while maintaining treatment efficiency.
The inhibitor effectively suppresses discoloration of trivalent chromium coatings, maintaining corrosion resistance and appearance under harsh conditions, with a discolored area ratio of 10% or less, and prevents gelation at higher pH, enhancing processing efficiency.
Smart Images

Figure 2024134392000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an inhibitor for inhibiting discoloration of a trivalent chromium chemical conversion coating, and a method for treating a metal material having a trivalent chromium chemical conversion coating with the inhibitor. [Background technology]
[0002] Chromate treatment using hexavalent chromium was widely used for plating films such as zinc plating to improve corrosion resistance and scratch resistance. However, due to concerns about environmental issues and effects on the human body, trivalent chromium conversion coating treatment is now mainstream (Patent Document 1).
[0003] The formation of a trivalent chromium chemical conversion film can improve the corrosion resistance and scratch resistance of the plating film while reducing the environmental load and the impact on the human body, but on the other hand, the trivalent chromium chemical conversion film has the problem that the surface discolors immediately after treatment in humid environments such as the rainy season. If the surface of the plating film discolors, the appearance of the plated product changes, and there is a risk of losing its value as a product. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-9319 A [Patent Document 2] JP 2003-313675 A Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Document 2, in order to address the problem of discoloration of trivalent chromium chemical conversion coatings, a discoloration prevention treatment for trivalent chromium chemical conversion coatings is carried out using a composition liquid containing colloidal silica and having a pH of 1.8 to 2.2 (Examples of Patent Document 2).
[0006] However, as disclosed in Patent Document 2, when the treatment solution is acidic, silicon compounds such as colloidal silica gel, making it difficult to perform surface treatment of the trivalent chromium chemical conversion coating by immersion treatment. As a result, there is a problem that the treatment efficiency of the trivalent chromium chemical conversion coating decreases. In addition, there is still room for development regarding the effect of suppressing discoloration of the trivalent chromium chemical conversion coating.
[0007] An object of the present invention is to provide a discoloration inhibitor for a trivalent chromium chemical conversion coating that has a good treatment efficiency and can effectively inhibit discoloration of a trivalent chromium chemical conversion coating, and a method for treating a metal material having a trivalent chromium chemical conversion coating using the same. [Means for solving the problem]
[0008] As a result of intensive research into solving the above problems, the inventors have found that the above problems can be solved by using a discoloration inhibitor containing a silicon compound and a specified carboxylic acid and having a pH controlled to 7.0 to 13.0.
[0009] The present invention, which was completed based on the above findings, is defined by the following (1) to (7). (1) One or more silicon compounds, one or more selected from the group consisting of a monocarboxylic acid having 1 to 10 carbon atoms or a salt thereof, and a dicarboxylic acid having 2 to 10 carbon atoms or a salt thereof; Including, A discoloration inhibitor for trivalent chromium conversion coatings with a pH of 7.0 to 13.0. (2) The discoloration inhibitor for a trivalent chromium conversion coating according to (1) above, wherein the silicon compound is silicic acid, sodium silicate, or colloidal silica. (3) The discoloration inhibitor for a trivalent chromium conversion coating according to (1) or (2) above, wherein the monocarboxylic acid is formic acid, acetic acid, propionic acid, acrylic acid, glycolic acid, or benzoic acid. (4) The discoloration inhibitor for a trivalent chromium chemical conversion coating according to any one of (1) to (3), wherein the dicarboxylic acid is oxalic acid, adipic acid, malonic acid, succinic acid, glutaric acid, maleic acid, fumaric acid, tartaric acid, malic acid, or phthalic acid. (5) The discoloration inhibitor for a trivalent chromium chemical conversion coating according to any one of (1) to (4), wherein the silicon compound has a silicate ion concentration of 0.01 to 40 g / L in the discoloration inhibitor for a trivalent chromium chemical conversion coating. (6) The discoloration inhibitor for a trivalent chromium chemical conversion coating according to any one of (1) to (5), wherein the monocarboxylic acid having 1 to 10 carbon atoms or its salt, and the dicarboxylic acid having 2 to 10 carbon atoms or its salt in the discoloration inhibitor for a trivalent chromium chemical conversion coating has a carboxylate ion concentration of 0.01 to 30 g / L. (7) preparing a metal material having a zinc or zinc alloy plated surface on which a trivalent chromium conversion coating is formed; a step of immersing the metal material in a bath provided with the discoloration inhibitor for a trivalent chromium chemical conversion coating film according to any one of (1) to (6); removing the immersed metal material from the bath and drying it; A method for treating a metal material having a trivalent chromium conversion coating, comprising: Effect of the Invention
[0010] According to the present invention, it is possible to provide a discoloration inhibitor for a trivalent chromium chemical conversion coating that can effectively inhibit discoloration of a trivalent chromium chemical conversion coating with good treatment efficiency, and a method for treating a metal material having a trivalent chromium chemical conversion coating using the same. [Brief description of the drawings]
[0011] [Figure 1] 1 shows binarized images of Examples 2 to 4 and 9 and Comparative Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, the embodiments for carrying out the present invention will be described in detail. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.
[0013] <Anti-discoloration agent for trivalent chromium conversion coating> The discoloration inhibitor for trivalent chromium chemical conversion coating according to an embodiment of the present invention contains one or more silicon compounds and one or more compounds selected from the group consisting of monocarboxylic acids having 1 to 10 carbon atoms or their salts, and dicarboxylic acids having 2 to 10 carbon atoms or their salts, and has a pH controlled to 7.0 to 13.0. With this configuration, discoloration of the trivalent chromium chemical conversion coating can be effectively inhibited with good treatment efficiency.
[0014] Trivalent chromium chemical conversion coatings are formed on plating films such as zinc plating in order to improve corrosion resistance and scratch resistance. Such trivalent chromium chemical conversion coatings have a problem of discoloration of the surface when exposed to high temperature and high humidity environments during the rainy season or summer, or when passing through the equator for export overseas. The discoloration inhibitor for trivalent chromium chemical conversion coatings according to the embodiment of the present invention effectively inhibits such discoloration of trivalent chromium chemical conversion coatings. Specific examples of the discoloration inhibition effect of the discoloration inhibitor for trivalent chromium chemical conversion coatings according to the embodiment of the present invention are shown below. First, a metal material having a zinc or zinc alloy plated surface on which a trivalent chromium conversion coating is formed is left to stand for 168 hours in a thermo-hygrostat chamber at 60°C and a relative humidity of 95%, after which the test piece is removed from the chamber and an appearance observation test is carried out as follows. (Appearance Observation Test) The appearance observation test involves taking an image of one surface of the test piece and binarizing it to determine the area that was originally white and is now displayed as black, which is the discolored area. The evaluation area is 4000 mm 2 The area of the discolored area is obtained using image processing software, etc., and the discolored area ratio (%) is calculated by dividing the area of the discolored area by the evaluation area. When the discolored area ratio is 10% or less, the discoloration inhibition effect is good.
[0015] (Silicon compounds) The silicon compound contained in the discoloration inhibitor for trivalent chromium conversion coating according to the embodiment of the present invention is preferably silicic acid, sodium silicate, or colloidal silica, with sodium silicate being particularly preferred.
[0016] (Colloidal Silica) The colloidal silica may be spherical colloidal silica, may be chain colloidal silica, or may be both spherical colloidal silica and chain colloidal silica. The spherical colloidal silica may be a normal one. The chain colloidal silica is a compound in which several to several tens of primary particles are bonded in a chain shape. The chain colloidal silica may be a straight chain or a branched chain. The particle size of the chain colloidal silica may be a particle having a diameter of 3 to 30 nm and a length of 30 to 500 nm. The spherical colloidal silica and the chain colloidal silica may be known ones, and may be available as a commercially available colloidal silica. Specific examples of chain colloidal silica include SNOWTEX (registered trademark) UP (solid content 20% by mass) and SNOWTEX (registered trademark) OUP (solid content 15% by mass) manufactured by Nissan Chemical Industries, Ltd. Specific examples of spherical colloidal silica include SNOWTEX (registered trademark) XS (solid content 20% by mass), SNOWTEX (registered trademark) CXS (solid content 14% by mass), SNOWTEX (registered trademark) OXS (solid content 10% by mass), SNOWTEX (registered trademark) S (solid content 30% by mass), SNOWTEX (registered trademark) OS (solid content 20% by mass), SNOWTEX (registered trademark) C (solid content 20% by mass), SNOWTEX (registered trademark) 30 (solid content 30% by mass), and SNOWTEX (registered trademark) O (solid content 20% by mass) manufactured by JGC Catalysts and Chemicals Co., Ltd., and CATALOID SI-30 (solid content 30% by mass) and CATALOID SI-550 (solid content 20% by mass) manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0017] The silicate ion (SiO3 2-) concentration is preferably 0.01 to 40 g / L. When the silicate ion concentration is 0.01 g / L or more, the discoloration suppression effect is further improved. Also, when the silicate ion concentration is 40 g / L or less, it is possible to suppress the white crystals (salts) remaining on the treated test piece, which would impair the appearance. The silicate ion concentration in the silicon compound discoloration inhibitor for trivalent chromium chemical conversion coating is more preferably 0.05 to 10 g / L, and even more preferably 0.05 to 2 g / L. When the silicon compound is colloidal silica, the SiO2 concentration in the discoloration inhibitor for trivalent chromium chemical conversion coating is preferably 0.01 to 40 g / L, and more preferably 0.05 to 10 g / L.
[0018] (Monocarboxylic acid, dicarboxylic acid or salt thereof) The monocarboxylic acid having 1 to 10 carbon atoms or its salt contained in the discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention is preferably formic acid, acetic acid, propionic acid, acrylic acid, glycolic acid, or benzoic acid, or its salt. The dicarboxylic acid having 2 to 10 carbon atoms or its salt contained in the discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention is preferably oxalic acid, adipic acid, malonic acid, succinic acid, glutaric acid, maleic acid, fumaric acid, tartaric acid, malic acid, or phthalic acid, or its salt. When the discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention contains these monocarboxylic acids, dicarboxylic acids, or their salts, the discoloration inhibitor for trivalent chromium chemical conversion coating is further improved in its discoloration inhibitory effect.
[0019] The carboxylate ion concentration in the discoloration inhibitor for trivalent chromium chemical conversion coating, which is a monocarboxylic acid having 1 to 10 carbon atoms or its salt, and a dicarboxylic acid having 2 to 10 carbon atoms or its salt, is preferably 0.01 to 30 g / L. When the carboxylate ion concentration is 0.01 g / L or more, the effect of inhibiting discoloration of the trivalent chromium chemical conversion coating is improved. When the carboxylate ion concentration is 30 g / L or less, it is possible to prevent white crystals (salts) from remaining on the treated test piece, which would impair the appearance. The carboxylate ion concentration is more preferably 0.1 to 10 g / L.
[0020] (aqueous medium) The discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention is obtained by dissolving the above-mentioned silicon compound, monocarboxylic acid or its salt, and dicarboxylic acid or its salt in an aqueous medium. Examples of the aqueous medium include water. By using the discoloration inhibitor obtained by dissolving the above-mentioned silicon compound, monocarboxylic acid or its salt, and dicarboxylic acid or its salt in an aqueous medium, it is possible to efficiently perform an immersion treatment of a metal material having a trivalent chromium chemical conversion coating formed on its surface.
[0021] The discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention may be composed only of one or more silicon compounds and one or more compounds selected from the group consisting of monocarboxylic acids having 1 to 10 carbon atoms or salts thereof, and dicarboxylic acids having 2 to 10 carbon atoms or salts thereof, or may further contain an aqueous medium and / or other components.
[0022] (pH) The discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention has a pH controlled to 7.0 to 13.0. With this configuration, the effect of inhibiting discoloration of the trivalent chromium chemical conversion coating is improved. Furthermore, when the pH is 7.0 or more, the discoloration inhibitor does not gel, and the immersion treatment of the metal material having the trivalent chromium chemical conversion coating formed on the surface can be performed more efficiently. Furthermore, when the pH is 13.0 or less, it is possible to inhibit the corrosion resistance from decreasing due to the remarkable dissolution of the trivalent chromium chemical conversion coating. It is more preferable that the discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention has a pH controlled to 8.0 to 12.0.
[0023] (metal material) Metal materials to be treated with the discoloration inhibitor for trivalent chromium conversion coating according to the embodiment of the present invention include zinc, or zinc alloys such as zinc-nickel alloy, zinc-iron alloy, tin-zinc alloy, zinc die-casting, etc. Furthermore, the metal material may be, for example, a plating of zinc, or zinc alloys such as zinc-nickel alloy, zinc-iron alloy, tin-zinc alloy, zinc die-casting, etc., formed on the surface of a metal substrate such as an iron-based material or an iron-based part.
[0024] (Trivalent chromium conversion coating) The trivalent chromium chemical conversion film on the surface of a metal material, the discoloration of which is inhibited by the discoloration inhibitor for trivalent chromium chemical conversion film according to the embodiment of the present invention, is not particularly limited. The trivalent chromium chemical conversion film may be, for example, a film containing 1) a trivalent chromium compound, 2) chloride ions, nitrate ions, sulfate ions, 3) an organic acid, 4) colloidal silica, 5) a pH adjuster made of sulfuric acid, nitric acid, hydrochloric acid, or sodium hydroxide, or the like.
[0025] <Method for treating metal material having trivalent chromium conversion coating> In the method for treating a metal material having a trivalent chromium chemical conversion coating according to the embodiment of the present invention, first, a metal material having a trivalent chromium chemical conversion coating formed on its surface is prepared. The metal material may have a zinc or zinc alloy plated surface. Next, the metal material is immersed in a bath containing the discoloration inhibitor for trivalent chromium chemical conversion coating according to the embodiment of the present invention. At this time, the bath temperature is preferably 10 to 50°C, and more preferably room temperature from the viewpoint of treatment efficiency. The immersion time is preferably 10 to 60 seconds. With this configuration, discoloration of the trivalent chromium chemical conversion coating can be more effectively inhibited. The immersion time is more preferably 20 to 40 seconds. Next, the immersed metal material is removed from the bath and dried using a thermostatic bath etc. Drying is preferably carried out at 70 to 90° C. for 10 to 30 minutes, and more preferably at 75 to 85° C. for 15 to 25 minutes. In this way, a discoloration suppression effect can be imparted to the trivalent chromium conversion coating on the metal material. EXAMPLES
[0026] Examples of the present invention are given below, but these are provided for a better understanding of the present invention and are not intended to limit the present invention.
[0027] (Examples 1 to 9, Comparative Examples 1 to 4) The test piece is 4000 mm on one side. 2 A flat steel plate having a surface area of 100 mm was prepared.
[0028] Next, the surface of the test piece was subjected to Zn electroplating under the following conditions. (Electrolytic zinc plating conditions) Metallic zinc concentration: 10g / L Caustic soda concentration: 120g / L Polishing agent concentration (Hyperzinc 9000A manufactured by Nippon Hyomen Kagaku Co., Ltd.): 12mL / L Polishing agent concentration (Hyper Zinc 9000BS manufactured by Nippon Hyomen Kagaku Co., Ltd.): 1mL / L - Water softener concentration (Hypersoft manufactured by Nippon Hyomen Kagaku Co., Ltd.): 10mL / L Impure metal inhibitor concentration (H-0624, manufactured by Nippon Hyomen Kagaku Co., Ltd.): 4mL / L ·Cathode current density: 1A / dm 2 - Plating bath temperature: 25℃ Plating time: 40 minutes Plating thickness: 5~7μm
[0029] Next, a trivalent chromium chemical conversion coating was formed on the Zn-plated surface of the test piece. Specifically, a trivalent chromium chemical conversion coating agent (TR-175SR manufactured by Nippon Hyomen Kagaku Co., Ltd.) containing chromium sulfate and colloidal silica was prepared, and the test piece was immersed in a bath containing the trivalent chromium chemical conversion coating agent at 30°C for 30 seconds. Next, the test piece was removed from the bath and dried at 80°C for 20 minutes using a thermostatic chamber, thereby forming a trivalent chromium chemical conversion coating on the Zn-plated surface of the test piece.
[0030] Next, the compounds shown in Table 1 were added to a bathtub containing pure water so as to obtain the compositions shown in Table 1 to prepare discoloration inhibitors. The test pieces on which the trivalent chromium conversion coatings were formed were then immersed in the discoloration inhibitors in the bathtub for 30 seconds. The bath temperature was about 25°C. The test pieces were then removed from the bathtub and dried in a thermostatic chamber at 80°C for 20 minutes.
[0031] The test piece thus subjected to the discoloration inhibition treatment of the trivalent chromium conversion coating was left to stand in a thermo-hygrostat chamber at 60° C. and a relative humidity of 95% for 168 hours. Thereafter, the test piece was taken out of the thermo-hygrostat chamber and subjected to an appearance observation test as follows. (Appearance Observation Test) The appearance observation test was carried out by taking an image of one surface of the test piece and binarizing it to determine the area that was originally white and was displayed as black, which was the discolored area. 2 The area of the discolored region was obtained using image processing software (ImageJ), and the discolored area percentage (%) was calculated by dividing the area of the discolored region by the evaluation area. The evaluation results are shown in Table 1. Moreover, the binarized images described above for Examples 2 to 4 and 9 and Comparative Examples 1 to 4 are shown in FIG.
[0032] [Table 1]
[0033] (Consideration) The samples of Examples 1 to 9 contained one or more silicon compounds and one or more compounds selected from the group consisting of monocarboxylic acids having 1 to 10 carbon atoms or their salts, and dicarboxylic acids having 2 to 10 carbon atoms or their salts, and had a pH of 7.0 to 13.0, so that the discoloration area ratio of the trivalent chromium conversion coating was good, being 10% or less. The sample of Comparative Example 1 did not contain carboxylate ions, and the discolored area ratio of the trivalent chromium conversion coating was poor. The samples of Comparative Examples 2 and 3 did not contain silicon ions and had poor discolored area ratios of the trivalent chromium conversion coating. The sample of Comparative Example 4, which did not contain either silicon ions or carboxylate ions, had the poorest discolored area ratio of the trivalent chromium chemical conversion coating.
Claims
1. One or more silicon compounds, one or more selected from the group consisting of a monocarboxylic acid having 1 to 10 carbon atoms or a salt thereof, and a dicarboxylic acid having 2 to 10 carbon atoms or a salt thereof; Including, A discoloration inhibitor for trivalent chromium conversion coatings having a pH of 7.0 to 13.
0.
2. 2. The discoloration inhibitor for a trivalent chromium conversion coating according to claim 1, wherein the silicon compound is silicic acid, sodium silicate, or colloidal silica.
3. 2. The discoloration inhibitor for a trivalent chromium conversion coating according to claim 1, wherein the monocarboxylic acid is formic acid, acetic acid, propionic acid, acrylic acid, glycolic acid, or benzoic acid.
4. 2. The discoloration inhibitor for a trivalent chromium conversion coating according to claim 1, wherein the dicarboxylic acid is oxalic acid, adipic acid, malonic acid, succinic acid, glutaric acid, maleic acid, fumaric acid, tartaric acid, malic acid, or phthalic acid.
5. 2. The discoloration inhibitor for trivalent chromium chemical conversion coating according to claim 1, wherein the silicon compound has a silicate ion concentration of 0.01 to 40 g / L in the discoloration inhibitor for trivalent chromium chemical conversion coating.
6. 2. The discoloration inhibitor for a trivalent chromium chemical conversion coating according to claim 1, wherein the monocarboxylic acid having 1 to 10 carbon atoms or its salt, and the dicarboxylic acid having 2 to 10 carbon atoms or its salt have a carboxylate ion concentration of 0.01 to 30 g / L in the discoloration inhibitor for a trivalent chromium chemical conversion coating.
7. A step of preparing a metal material having a trivalent chromium conversion coating formed on a zinc or zinc alloy plated surface; A step of immersing the metal material in a bath provided with the discoloration inhibitor for a trivalent chromium chemical conversion coating according to any one of claims 1 to 6; removing the immersed metal material from the bath and drying it; A method for treating a metal material having a trivalent chromium conversion coating, comprising:
Citation Information
Patent Citations
Agent for forming rust preventive film on metal, and forming method
JP2003313675A
Composition for forming protective film, method for manufacturing metal-molded body, and metal-molded body
JP2007009319A