Method for producing recycled plastic material, and recycled plastic material
By measuring and adjusting input amounts of recycled resin materials and inorganic fillers, the method addresses quality inconsistencies in recycled plastics, producing materials with consistent properties suitable for various applications.
Patent Information
- Application Number
- JP2023189690
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-11-06
- Publication Date
- 2024-10-03
AI Technical Summary
The quality of recycled plastic materials varies due to differences in origin, leading to inconsistencies in material properties, and it is challenging to produce products of consistent quality using recycled plastics, especially those covered by the Packaging and Recycling Law, which also faces challenges in pricing and market availability.
A method to produce recycled plastic materials by measuring and adjusting the input amounts of recycled resin materials and inorganic fillers to achieve specific performance criteria, including density, polyethylene content, and flexural modulus, ensuring the final product meets specified ranges.
The method enables the production of recycled plastic materials with consistent quality and improved physical properties, making them suitable for a wide range of applications while being environmentally friendly.
Smart Images

Figure 2024134500000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing recycled plastic material by producing recycled resin (hereinafter sometimes referred to as "R resin") obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law (hereinafter abbreviated as "Container and Packaging Recycling Law") applies, and to the recycled plastic material. [Background technology]
[0002] In recent years, in the development of plastic products, it is desirable to use recycled materials rather than virgin materials. In particular, since the establishment of the Containers and Packaging Recycling Law, the use of recycled materials covered by this law has been recommended. This is because, as described in Non-Patent Document 1 ("Use of Waste Plastics in 2020"), packaging containers / containers account for 47.5% (3.9 million tons) of the "total amount of waste plastic generated," and packaging containers / containers account for 77.1% (3.16 million tons) of the "general waste by category," and the volume of waste (waste plastic) related to packaging containers / containers in circulation is large. Therefore, if recycling of R resin subject to the Containers and Packaging Recycling Law progresses, the recycling of all waste plastics will also progress, so there is a strong demand for the use of recycled plastic materials to which the Containers and Packaging Recycling Law applies. [Prior art documents] [Non-patent literature]
[0003] [Non-Patent Document 1] Japan Plastics Industry Federation Magazine Plastics June 2022 Issue Pages 79-83 Author Masashi Hanba Publisher Japan Industrial Publishing Co., Ltd. Published June 10, 2022 Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, recycled plastic materials (hereinafter sometimes referred to as "RP materials") have a bias in quality depending on the origin of the material. In addition, while there is a considerable amount of unshipped and unused RP materials due to production losses and processing losses of RP materials, there is also a considerable amount of used waste (used waste may be contaminated with foreign matter even after cleaning). Therefore, unlike virgin materials with a constant material quality, various resins, foreign matter, etc. are mixed into RP materials, and the material properties tend to be easily deteriorated, biased, and varied. This is particularly noticeable for RP materials to which the Containers and Packaging Recycling Law applies. Therefore, various ingenuity and effort are required to manufacture products of a certain level of quality using RP materials to which the Containers and Packaging Recycling Law applies, and it is not necessarily easy to promote the use of RP materials to which the Containers and Packaging Recycling Law applies. In addition, regarding the distribution of RP materials, if the selling price is the same as that of virgin materials, businesses will not be motivated to purchase RP materials and manufacture them. Furthermore, if the price of products using RP materials does not fall, general consumers may not be motivated to purchase products using RP materials, even if they recognize the importance of recycling. Therefore, in order to promote the use of RP materials, it is important that the price falls compared to that of virgin materials. Furthermore, while those who wish to purchase plastic-related virgin materials can purchase them stably by placing an order with a company that manufactures and sells them, those who wish to purchase RP materials cannot purchase them if the company that supplies them cannot obtain recycled raw materials. Therefore, companies that purchase RP materials have strong ties with sales companies, and there are situations where companies that wish to purchase RP materials cannot obtain the desired amount from the market when they wish. Furthermore, when promoting the use of RP materials to which the Containers and Packaging Recycling Law applies, there is a strong demand for environmentally friendly recycling. The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a method for producing an excellent RP material, which can be expanded in use while being environmentally friendly by making good use of R resin obtained from RP materials to which the Container and Packaging Recycling Law is applied, and the RP material, and in particular, a material performance that has a density of 1.00 g / cm 3 The present invention provides a method for producing an RP material that satisfies a specific range set to be less than 100%, and the RP material. [Means for solving the problem]
[0005] In order to solve the above problems, the manufacturing method of the present invention has the following means. That is, as a means 1, a density of 1.00 g / cm3 is set as a material property. 3 A method for producing a recycled plastic material with a specific range of less than 100%, comprising: a first measurement step for measuring the material performance of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; a second measurement step for measuring the material performance of a second recycled resin material (which may contain an inorganic filler component) obtained from used plastics mainly composed of polypropylene; a calculation step for calculating the input amounts of the first recycled resin material and the second recycled resin material based on the material performances of the first recycled resin material and the second recycled resin material measured in the first measurement step and the second measurement step; and an input amount calculation step for determining the input amount of a new inorganic filler material based on the calculated input amounts of the first recycled resin material and the second recycled resin material so that the material performance of the recycled plastic material after melt-kneading falls within the specific range. Note that the first recycled resin material and the second recycled resin material may contain an inorganic filler component, so that it is calculated whether the material properties of the recycled plastic material after melt-kneading exceed the upper limit of the specific range for the inorganic filler component.
[0006] As a second measure, in the first measure, when the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range in the input amount calculation step, the input of new inorganic filler material is stopped.
[0007] As a third measure, in the first or second measure, when the material properties of the recycled plastic after molding are set to a specific range, it is preferable to set a high or low priority application order to be applied preferentially, and to stipulate that the "high priority application" is that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and that the "low priority application" is to include at least that the MFR (based on JIS standard K7210) is 3.0 g / 10 min or more.
[0008] As a fourth method, in either the first or third method, when the amount of polyethylene contained in the first recycled resin material is higher than the estimated polyethylene amount in the recycled plastic material after molding, it is preferable to provide an input amount adjustment step of reducing the input amount of the first recycled resin material below a predetermined estimated input amount and increasing the input amounts of the second cycle resin material and the inorganic filler material above the predetermined estimated input amounts.
[0009] The invention of the present invention has the following means. That is, as means 5, the density is 1.00 g / cm3 as a material property. 3 The recycled plastic material has a specific range of less than or equal to the specific content, and is characterized in that it comprises a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and whose input amount is calculated based on measured material performance; a second recycled resin material (which may contain an inorganic filler component) obtained from used plastic whose main component is polypropylene, and whose input amount is calculated based on measured material performance; and an inorganic filler material whose input amount is calculated based on the calculated input amounts of the first recycled resin material and the second recycled resin material so that the material performance after melt-kneading of the recycled plastic material falls within the specific range, and the first recycled resin material, the second recycled resin material, and the inorganic filler material whose input amounts are calculated are melt-kneaded together.
[0010] As a sixth aspect, in the fifth aspect, it is preferable that the polyethylene content in the molded recycled plastic material is adjusted and blended to be 30% by weight or less based on the total weight of the recycled plastic material.
[0011] As the seventh measure, in the fifth or sixth measures, it is preferable that the amount of the inorganic filler added is 15% by weight or less based on the total amount of the recycled plastic material before melt-kneading.
[0012] As an eighth aspect, in any one of the fifth to seventh aspects, it is preferable that the specific range of material performance satisfies all of the following conditions (1) to (3). (1) MFR (based on JIS standard K 7210) is 3.0g / 10min or more, (2) Flexural modulus (in accordance with JIS standard K 7171) of 1100 MPa or more; (3) Izod impact strength (JIS standard K 7110 compliant) is 5.0 kJ / m 2 End
[0013] Means 9: A product in which the recycled plastic material according to any one of means 6 to 8 is used as a raw material. Effect of the Invention
[0014] According to the present invention, by effectively utilizing recycled resin obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, it is possible to provide a manufacturing method for a recycled plastic material having excellent strength and other properties, which can be expanded in use while being environmentally friendly, and a recycled plastic material, and in particular, a material having a density of 1.00 g / cm3. 3 It is possible to provide a method for producing an excellent RP material and the RP material, in which the resistance of the RP material falls within a specific range set to less than 100%. [Brief description of the drawings]
[0015] [Figure 1] 1A to 1C are schematic diagrams showing a manufacturing process of an embodiment of the present invention. [Diagram 2] 4 is a graph showing the relationship between the polyethylene content and the weld strength in the embodiment. [Diagram 3] 4 is a flowchart showing a manufacturing process in the embodiment. [Figure 4] FIG. 4 is an explanatory diagram showing component values and physical property values of a resin material in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Next, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 shows a schematic diagram of the RP material being melt-kneaded and molded in the embodiment. Fig. 2 shows a graph showing the relationship between the PE content and the weld strength in the embodiment. Fig. 3 is a flow chart showing the manufacturing process for producing the RP material, and Fig. 4 shows the component values and physical property values of the resin material in the embodiment. The extrusion molding machine 37 shown in FIG. 1 can feed pellet material 42 (comprised of a first resin material 41, a second (home appliance recycling) resin material 42A, a second (automobile recycling) resin material 42B, a second (general material recycling) resin material 42C, or an inorganic filler material 43, etc., which will be described later) into its hopper 36, and the pellet material 42 is conveyed in a conveying section 38 equipped with an internal screw. The extrusion molding machine 37 can melt-knead and mold the fed pellet material 42 inside, and discharge the pellet material 42 from a discharge port 39 as new pellet material. For the melt-kneading method, a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer, etc. can be used. In the pellet material 42 of this embodiment, a recycled resin material 41 (hereinafter, this recycled resin material 41 will be referred to as "first resin material 41") obtained from used plastic container packaging to which the Container Recycling Law applies is an essential component. In addition, as a component of the pellet material 42, a recycled resin material obtained from used plastic to which the Home Appliance Recycling Law applies (hereinafter, this recycled resin material will be referred to as "second (home appliance recycling) resin material 42A") can be included. In addition, as another component of the pellet material 42, a recycled resin material obtained from used plastic to which the Automobile Recycling Law applies (hereinafter, this recycled resin material will be referred to as "second (automobile recycling) resin material 42B") can be included.
[0017] Furthermore, as a component of the pellet material 42, recycled resin material obtained from general used RP materials to which none of the Containers and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law apply (hereinafter, this recycled resin material will be referred to as "second (general material recycled) resin material 42C") can be included. As shown in FIG. 4, the first resin material 41, the second (home appliance recycling) resin material 42A, the second (automobile recycling) resin material 42B, and the second (general material recycling) resin material 42C contain a polypropylene (hereinafter referred to as "PP") component, a polyethylene (hereinafter referred to as "PE") component, an inorganic filler component, and other components (hereinafter referred to as "others"), and are characterized by bias in the amount of components, etc. depending on the origin of the product, etc., and variations in physical properties. In addition, an inorganic filler material 43 can be added to the pellet material 42 as an optional component to improve rigidity or increase specific gravity (density). The first resin material 41, the second (home appliance recycling) resin material 42A, the second (automobile recycling) resin material 42B, and the second (general material recycling) resin material 42C contain an inorganic filler component, and have the effect of improving rigidity according to the amount of the component. If the desired rigidity is insufficient, additional inorganic filler material 43 can be added. The inorganic filler material 43 may be any known material that does not affect the properties of the plastic material and improves rigidity. Examples of inorganic filler materials include carbonates, sulfates, silicates, phosphates, borates, oxides, and hydrates of calcium, magnesium, titanium, aluminum, iron, zinc, etc., or powders of these hydrates. Specific examples include calcium carbonate, magnesium carbonate, zinc oxide, titanium oxide, silica, alumina, clay, talc, kaolin, aluminum hydroxide, magnesium hydroxide, aluminum silicate, magnesium silicate, calcium silicate, aluminum sulfate, magnesium sulfate, calcium sulfate, magnesium phosphate, barium sulfate, silica sand, carbon black, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium sulfite, sodium sulfate, potassium titanate, bentonite, wollastonite, dolomite, graphite, etc. These may be contained alone or in combination of two or more kinds. The first resin material 41, the second (home appliance recycling) resin material 42A, the second (automobile recycling) resin material 42B, the second (general material recycling) resin material 42C (hereinafter, these may be collectively referred to as the second resin material 42) or the inorganic filler material 43 (a mixture of these) shown in Fig. 1 are illustrated in the form of pellets for ease of understanding, but this form is not necessarily limited to pellets. Also, the form of the resin material discharged from the discharge port 39 of the extrusion molding machine 37 may be pellets or may be other forms.
[0018] The inventors and researchers of the present application have studied the material properties, component analysis, market trends, and application fields of RP materials for many years. As a result, they have found that the presence of various resins in RP materials makes them susceptible to deterioration, deviation, bias, and variation in physical properties. They have also found that differences in the product origins of RP materials tend to cause specific trends in material properties and component analysis, which can be roughly categorized into the following (1) to (4). (1) A first resin material 41 obtained from used plastic containers and packaging to which the Containers and Packaging Recycling Law applies (in this case, the first resin material 41 (first recycled resin material) can be said to be a resin material derived from the Containers and Packaging Recycling Law). (2) A second (home appliance recycling) resin material 42A obtained from RP materials that are not subject to the Container Recycling Law but are subject to the Home Appliance Recycling Law (hereinafter, referred to as the second (home) resin material 42A, which can be said to be a resin material derived from the Home Appliance Recycling Law). (3) A second (automobile recycling) resin material 42B obtained from an RP material that is not subject to the application of the Containers and Packaging Recycling Law but is subject to the Automobile Recycling Law (hereinafter, referred to as the second (own) resin material 42B, which can be said to be a resin material derived from the Automobile Recycling Law). (4) A second (general recycled) resin material 42C obtained from a general RP material to which none of the Container Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law applies (hereinafter, abbreviated as the second (first) resin material 42C, but unlike the second (home) resin material 42A and the second (self) resin material 42B, the second (first) resin material 42C can be said to be a resin material derived from a general material). The official name of the Packaging Recycling Law is the Law Concerning Promotion of Separate Collection and Recycling of Containers and Packaging (the provisions and definitions of the Law will be cited as necessary). Specific targets include, for example, packaging film and food trays, but the items covered by the Law are limited. (R resin materials obtained from items covered by the Law are resin materials derived from packaging recycling materials and correspond to No. 1 Resin Material 41, but the content is subject to change in accordance with amendments to the Law, etc.) The official name of the Home Appliance Recycling Law is the Law Concerning the "Law Concerning the Recycling of Specified Household Appliances" (the provisions and definitions of the law will be cited as necessary). The items covered are four types of home appliances (air conditioners, televisions, refrigerators, freezers, washing machines, and clothes dryers), but the used plastics to which the law applies are limited to those discarded from ordinary households and offices. Therefore, even if the four types of home appliances are covered by the law, there are cases in which the law does not apply due to differences in the source of disposal. (R resin materials obtained from items covered by the law are resin materials derived from home appliance materials and correspond to Type 2 (household) resin materials 42A, but the content is subject to change in accordance with amendments to the Home Appliance Recycling Law, etc.) The official name of the Automobile Recycling Law is the "Law Concerning Recycling, etc. of End-of-Life Automobiles" (the provisions and definitions of the Law will be cited as necessary). The Law defines "automobiles," and the specific objects of the Law are limited to, for example, automobile bumpers and automobile interior materials. (The R resin material obtained from the objects covered by the Law is a resin material derived from automobile materials and corresponds to the second (auto) resin material 42B, but the content is subject to change in accordance with amendments to the Automobile Recycling Law, etc.) In addition, there are R resin materials obtained from general used RP materials to which the Container Recycling Law, Home Appliance Recycling Law, and Automobile Recycling Law do not apply. For example, there are (1) R resin materials obtained from RP materials of items other than the four types of home appliances to which the Home Appliance Recycling Law applies, and (2) resin materials obtained from RP materials of motorcycles, etc. to which the Automobile Recycling Law does not apply. (These R resin materials are resin materials derived from general materials and correspond to Section 2(1) Resin Material 42C, but their contents are subject to change in accordance with changes to the Container Recycling Law, Home Appliance Recycling Law, and Automobile Recycling Law, etc.) Due to such legal treatment, while the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C have similarities in their ingredients and material properties, there are differences in their ingredients and material properties due to the origin of the products related to the applicable laws, resulting in certain trends.
[0019] 4 shows Tables 1 to 4. Table 1 shows the component values by weight % of PP, PE, inorganic filler, and other components (hereinafter referred to as "others") for four groups of materials (material 1, material 2, material 3, and material 4) of the first resin material 41, and further shows four physical property values (in this case, density, melt flow rate (hereinafter referred to as "MFR"), flexural modulus, and Izod impact strength). Tables 2 to 4, like Table 1, show the weight percent values of the components (PP components, PE components, inorganic filler components, other components) of each material (material 1, material 2, material 3, material 4) for the second (home) resin material 42A, the second (self) resin material 42B, and the second (first) resin material 42C, as well as four physical property values (in this case, density, MFR, flexural modulus, Izod impact strength). The indication of materials 1 to 4 for each resin material (41, 42A, 42B, 42C) may be four or less or more. In addition, the four physical properties to be measured may include other physical properties as necessary.
[0020] Next, a method for measuring the material properties of a resin material will be described. The melt flow rate (hereinafter referred to as "MFR"), which represents one of the material properties of a resin material, can be measured using a Melt Indexer G-02 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the MFR measurement method (JIS K7210, 230 degrees Celsius, load 2.16 kg). The flexural modulus, which represents one of the material properties of a resin material, can be measured using a Bentograph B-2 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the flexural property measurement method (JIS K7171). The Izod impact strength, which represents one of the material properties of a resin material, can be measured using an impact tester IT (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the Izod impact measurement method (JIS K7110). The material density, which represents one of the material properties of a resin material, can be measured using an electronic specific gravity meter SD-200L (manufactured by Alpha Mirage Co., Ltd.) by the density and specific gravity measurement method (JIS K7112). The MFR of the material 1 of the first resin material 41 shown in the table is 3.1 g / 10 min. The flexural modulus of the material 1 of the first resin material 41 is 666 MPa. The Izod impact strength of the material 1 of the first resin material 41 is 4.6 kJ / m 2The material density of the material 1 of the first resin material 41 is 0.96 g / cm 3 The component values of PP, PE, other resins, and inorganic fillers that have been subjected to component analysis are listed in the columns for Material 2, Material 3, and Material 4 of the first resin material 41. For example, an infrared spectrophotometer FT / IR-4X manufactured by JASCO Corporation can be used to measure PP, PE, and other resins in the resin material, but other devices may also be used. The amount of inorganic filler is measured using the amount of combustion residue. For example, an electric crucible furnace FUC030FB manufactured by Advantec Toyo Co., Ltd. can be used. These values are shown in the columns of Tables 1 to 4 (Material 1, Material 2, Material 3, Material 4) in FIG.
[0021] Next, the resin materials shown in Tables 1 to 4 in Fig. 4 will be described. First, the first resin material 41 (materials 1 to 4) will be described. The first resin material 41 is characterized in that it has a large PE content and a small PP content, and also has a small content of other substances and inorganic filler. The densities of materials 1 to 4 are 0.94 to 0.97 g / cm 3 The MFR value is in the range of 3.0 to 3.8 g / 10 min, the flexural modulus is in the range of 666 to 937 MPa, and the Izod impact strength is in the range of 4.6 to 8.4 kJ / m 2 They are scattered within a range of about The first resin material 41 has a density of 0.90 to 0.98 g / cm 3 The range of 0.93 to 0.96 g / cm is the approximate practical range. 3 A suitable practical range for the MFR of the first resin material 41 is 1.0 to 10.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 3.0 to 7.0 g / 10 min. A suitable practical range for the flexural modulus of the first resin material 41 is 400 to 1200 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 600 to 1100 MPa. A suitable practical range for the Izod impact strength of the first resin material 41 is 3.0 to 20.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product.2 The range is roughly practical, and further, 5.0 to 15.0 kJ / m 2 This range is a suitable practical range.
[0022] The second (house) resin material 42A (materials 1 to 4) shown in Table 2 of Fig. 4 is characterized in that the PP content is extremely large and the PE content is extremely small, and the other contents and inorganic filler contents are also small. The density of the second (house) resin material 42A is 0.91 to 0.92 g / cm 3 The MFR value is in the range of 25.4 to 28.7 g / 10 min, the flexural modulus is in the range of 1259 to 1370 MPa, and the Izod impact strength is in the range of 6.0 to 7.3 kJ / m 2 As a result, the second (house) resin material 42A (materials 1 to 4) has superior values of MFR, flexural modulus, and Izod impact strength compared to the first resin material 41 (materials 1 to 4). The properties of the second resin material 42A alone are density of 0.91 to 0.97 g / cm 3 The range of 0.91 to 0.94 g / cm is the approximate practical range. 3 The preferred practical range for the MFR of the second (family) resin material 42A is 10.0 to 35.0 g / 10 min from the viewpoint of moldability during injection molding, and 15.0 to 30.0 g / 10 min is a more preferred practical range. The preferred practical range for the flexural modulus of the second (family) resin material 42A is 1000 to 1600 MPa from the viewpoint of product rigidity (strength), and 1100 to 1400 MPa is a more preferred practical range. The preferred practical range for the Izod impact strength of the second (family) resin material 42A is 4.0 to 15.0 kJ / m from the viewpoint of product impact resistance (avoidance of cracking). 2 The range is the approximate practical range, and further, 6.0 to 12.0 kJ / m 2 This range is a suitable practical range.
[0023] In addition, the second (own) resin material 42B (materials 1 to 4) shown in Table 3 of FIG. 4 is characterized by a large PP content and a small PE content, and is characterized by a large inorganic filler content compared to the first resin material 41, the second (home) resin material 42A, and the second (first) resin material 42C. Therefore, when using the second (own) resin material 42B (materials 1 to 4), since the second (own) resin material 42B (materials 1 to 4) itself contains a large amount of inorganic filler components, there are cases where no additional inorganic filler material 43 is used. However, if the inorganic filler components of the second (own) resin material 42B (materials 1 to 4) itself are less than expected, a required amount of inorganic filler material 43 is added. The density of the second resin material 42B is 1.04 to 1.06 g / cm 3 The MFR value is in the range of 24.8 to 35.1 g / 10 min, the flexural modulus is in the range of 1906 to 2159 MPa, and the Izod impact strength is in the range of 17.5 to 24.6 kJ / m 2 As a result, the materials 1 to 4 of the second (own) resin material 42B are superior in MFR, flexural modulus, and Izod impact strength to the first resin material 41 (materials 1 to 4). The properties of the second (self) resin material 42B alone are density of 0.95 to 1.10 g / cm 3 is the approximate practical range, and 0.97 to 1.07 g / cm 3 A suitable practical range is 15.0 to 40.0 g / 10 min. from the viewpoint of moldability during injection molding, and a suitable practical range is 20.0 to 35.0 g / 10 min. Regarding the MFR of the second (self) resin material 42B, a rough practical range is 1500 to 2500 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1800 to 2300 MPa. Regarding the Izod impact strength of the second (self) resin material 42B, a rough practical range is 1500 to 2500 MPa from the viewpoint of the impact resistance (avoidance of cracking) of the product, and a suitable practical range is 6.0 to 35.0 kJ / m 2 The range is the approximate practical range, and further, 10.0 to 30.0 kJ / m 2 This range is a suitable practical range.
[0024] The second (first) resin material 42C (materials 1 to 4) shown in Table 4 of Fig. 4 is characterized in that the PP content is extremely large, the PE content is extremely small, and the other contents and inorganic filler content are also small. The density of the second (first) resin material 42C is 0.94 to 0.98 g / cm 3 The MFR is in the range of 9.6 to 14.0 g / 10 min, the flexural modulus is in the range of 1180 to 1324 MPa, and the Izod impact strength is in the range of 5.8 to 11.1 kJ / m 2 As a result, the second (first) resin material 42C (materials 1 to 4) has superior values of MFR, flexural modulus, and Izod impact strength compared to the first resin material 41 (materials 1 to 4). The second (first) resin material 42C has a density of 0.91 to 1.00 g / cm 3 The range of 0.91 to 0.96 g / cm is the approximate practical range. 3 A suitable practical range for the MFR is 3.0 to 30.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 4.0 to 25.0 g / 10 min. A suitable practical range for the flexural modulus of the second (first) resin material 42C is 900 to 1600 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1100 to 1400 MPa. A suitable practical range for the Izod impact strength of the second (first) resin material 42C is 4.0 to 25.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product. 2 The range is roughly practical, and further, 5.0 to 15.0 kJ / m 2 This range is a suitable practical range.
[0025] Furthermore, it is known from the inventors' experiments that when a PP component and a PE component are mixed, the following characteristics are obtained. That is, Fig. 2 is a graph showing the relationship between the PE content ratio in an RP material (a resin material made of PP and PE) and the weld strength, with the vertical axis of Fig. 2 showing the weld strength (MPa) and the horizontal axis of Fig. 2 showing the PE content ratio. According to Fig. 2, there is a tendency for the weld strength to gradually decrease from a PE content ratio of 0% (in this case, the weld strength is 32.6 MPa) toward a content ratio of 50% (in this case, the weld strength is 19.0 MPa). 2, if the PE content is 30% and the weld strength is about 23.0 MPa, and the PE content is in the range of 0% to 30% (preferably 0% to 20%), the weld strength is sufficiently maintained (i.e., the strength retention rate is 70% or more) and it is understood to be a strength (tolerable condition) that does not cause problems in commercialization. The weld strength was measured using a 150 x 100 x 4 mm test piece with a weld formed in the center, under the conditions specified in JIS K7161. The second (home) resin material 42A, second (self) resin material 42B, second (first) resin material 42C, etc. in this embodiment are resin materials mainly composed of PP (hereinafter may be referred to as "PP-mainly-component resin materials"), and when the PP-mainly-component resin material is mixed with the first resin material 41 (even if foreign matter other than PP and PE is mixed in, it can be generally ignored in terms of weld strength), it can be seen that the graph in Fig. 2 can be applied to the PE content ratio of the PP-mainly-component resin material and the first resin material 41. As a result, it can be seen that if the PE content ratio is in the range of 0 to 30%, the allowable range for the product strength of the RP material can be maintained.
[0026] Next, we will explain the material properties (product properties) of products molded from RP materials. The material properties of the product are related to the specific ranges (amount of components and material property values obtained by component analysis) of the RP material after melt kneading (see Table 1). In addition, the specific ranges of material properties can be divided into "high priority application" that is applied preferentially from the viewpoint of product usage, and "low priority application" (lower than "high" priority application). According to Table 1 below (specific range of resin materials), the material properties (product properties) of products molded from RP materials are density 1.00g / cm3 in order to reduce costs associated with weight reduction during transportation. 3 In other words, "PE content is 30% by weight or less" is "high priority application". Similarly, "As for the physical properties of the RP material after melt kneading, density is 1.00g / cm 3 On the other hand, "the inorganic filler is 15% or less by weight of the total weight" and "the Izod impact strength is 5.0 kJ / m 2 "The amount of inorganic filler added must be 15% by weight or less" is a "low priority application" item, but is of high importance in terms of reducing the weight of the product. In this case, the conditions defined in "high priority application" are defined as the highest priority conditions in this embodiment. The contents defined in "low priority application" are selected by selecting a method for setting conditions appropriately within the above conditions according to the characteristics of the product, etc., to ensure flexibility when designing products using RP materials. Note that the high or low priority application is not uniform but may change depending on the product's usage environment and product characteristics, etc. In particular, the conditions related to "low priority application" can be changed depending on the product's usage environment and product characteristics, etc.
[0027] [Table 1]
[0028] Next, the manufacturing method of this embodiment will be described with reference to the flow chart shown in FIG. 3. In FIG. 3, the material properties of the product to be commercialized, which will be molded from the final RP material, are grasped in advance. First, the material properties of the product to be commercialized are grasped, and the material properties (density, MFR, flexural modulus, Izod impact strength) are grasped in addition to the component analysis (in this case, the component ratio of "PP component, PE component, other components, inorganic filler") that constitutes the material properties (see Table 1). Hereinafter, this step is referred to as product property grasping step S1, and abbreviated as "S1" in FIG. 3. Both the component analysis values and the material property values are collectively referred to as product properties (material properties). Next, the components of the first resin material 41 are analyzed, and furthermore, the material physical properties are measured (Step S2). Hereinafter, this step is referred to as the component analysis / material physical property measurement step S2, and is abbreviated as "S2" in FIG. 3. In this case, the first resin material 41 is melt-kneaded, and in addition to the component analysis of the "PP component, PE component, other components, inorganic filler material" of the first resin material 41, the material physical properties "density, MFR, flexural modulus, Izod impact strength" are measured (Step S2). The material property measurement step of measuring the material properties in Step S2 corresponds to the "first measurement step" in the claims. Next, the results of the component analysis and material properties of the first resin material 41 are compared and verified with the results of the component analysis and material properties grasped in the product characteristic grasping step S1 (step S3). Hereinafter, such a comparison and verification step is referred to as a comparison and verification step S3, and is abbreviated as "S3" in FIG. 3. In step S4, the second (family) resin material 42A is subjected to component analysis and further to measurement of material properties. Hereinafter, the step of measuring the component analysis value and material properties of the second (family) resin material 42A is referred to as component analysis and material property measurement step S4, and is abbreviated as "S4" in FIG. 3. In this case, the second (family) resin material 42A alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the second (family) resin material 42A after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. The material property measurement step of measuring the material properties of the second (family) resin material 42A in step S4 corresponds to the "second measurement step" in the claims. In addition, if there is no plan to use the second (family) resin material 42A, it is not necessary to measure the material properties of the second (family) resin material 42A. In step S5, the second (own) resin material 42B is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the second (own) resin material 42B is referred to as component analysis and material property measurement step S5, and is abbreviated as "S5" in FIG. 3. In this case, the second (own) resin material 42B alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the second (own) resin material 42B after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. If there is no plan to use the second (own) resin material 42B, it is not necessary to measure the material properties of the second (own) resin material 42B. The material property measurement step of measuring the material properties of the second (own) resin material 42B in step S5 corresponds to the "second measurement step" in the claims. In step S6, the second (first) resin material 42C is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the second (first) resin material 42C is referred to as component analysis and material property measurement step S6, and is abbreviated as "S6" in FIG. 3. In this case, the second (first) resin material 42C alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the kneaded second (first) resin material 42C, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. The material property measurement step of measuring the material property of the second (first) resin material 42C in step S6 corresponds to the "second measurement step" in the claims. Note that if there is no plan to use the second (first) resin material 42C, it is not necessary to measure the material property of the second (first) resin material 42C.
[0029] In step S7, based on the material properties of the first resin material 41 measured in step S2 and the material properties of the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C measured in steps S4 to S6, the input amount of the first resin material 41 and the input amount of any one of the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C (a mixture of two or more types, if necessary) are calculated. Hereinafter, the step of calculating the input amount is referred to as the input amount calculation step S7, and is abbreviated as "S7" in FIG. 3.) The input amount calculation step S7 corresponds to the "calculation step" in the claims. In addition, for a resin material obtained by melt-kneading and molding any one of the second (home) resin material 42A, the second (own) resin material 42B and the second (first) resin material 42C (a mixture of two or more types is also called a mixed second resin material, but these may be collectively referred to as the second resin material 42), whose input amount has been calculated, if the PE component amount of the first resin material 41, whose component analysis value and material property value have been measured in step S6, is higher than the assumed PE component value of the RP material, it is preferable to carry out a process of reducing the input amount of the first resin material 41 from a predetermined assumed input amount and increasing the input amount of the second resin material 42 from a predetermined assumed input amount. In step S8, both the first resin material 41, the amount of which was calculated in S7, and the mixed second resin material, the amount of which was calculated in S7, are added, and the first resin material 41 and the second resin material 42 (including the mixed second resin material) that are melt-kneaded and molded are subjected to a component analysis of the molded product 45 (hereinafter referred to as the "molded first and second resin materials 45"), and further the material property values are measured (hereinafter this step is referred to as the component analysis and material property measurement step S8, and abbreviated as "S8" in FIG. 3). In this case, the "PP component, PE component, other components, inorganic ... In addition to component analysis of the "RP material," the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. If the inorganic filler component of the material properties (first and second molding resin materials 45) after melt-kneading falls within a specific range, there is no need to add additional inorganic filler material 43. (In this case, the specific range is when the content of the inorganic filler component in the RP material after melt-kneading is 15% by weight or less, so if the content exceeds 15% by weight, it will exceed the target (specific range). In this case, there is no need to add additional inorganic filler material 43.)
[0030] In step S9, for the first and second molding resin materials 45, the amount of inorganic filler material 43 to be added is calculated so that the material properties after melt-kneading of the RP material are within the target (specific range) product properties (material properties) grasped in S1. Hereinafter, the step of calculating the amount of inorganic filler material 43 to be added is referred to as calculation step S9, and is abbreviated as "S9" in FIG. 3. If the inorganic filler component is within the specific range and exceeds the upper limit of the specific range, the addition of new inorganic filler material 43 is eliminated (stopped). The input amount calculation step S9 corresponds to the "input amount calculation step" in the claims. In step S10, the inorganic filler material 43 whose amounts were calculated in S9 and the first and second molding resin materials 45 whose amounts were calculated are added, and the inorganic filler material 43 and the first and second molding resin materials 45 are melt-kneaded and molded to produce a molded product (hereinafter referred to as the "final molded body 46"), and the material properties of the molded product are measured. (Hereinafter, the step of measuring the component analysis values and material physical properties of the final molded body 46 is referred to as the component analysis / material physical property measurement step S10, and abbreviated as "S10" in FIG. 3. In this case, in addition to the component analysis of the "PP component, PE component, other components, and inorganic filler material" of the final molded body 46, the material properties of "density, MFR, flexural modulus, and Izod impact strength" are measured.) In step S11, the results of the component analysis and material properties of the final molded body 46 are compared with the results of the component analysis and material properties grasped in the product characteristic grasping step S1 to verify the results. Hereinafter, such a comparison verification step is referred to as the comparison verification step S11, and is abbreviated as "S11" in Fig. 3. If it is determined as a result of the comparison verification that the components of the material of the final molded body 46 are inappropriate, for example, a process of readjusting the amounts of the inorganic filler material 43 and the first and second molding resin materials 45 is performed. In step S11, if it is determined that the final molded body 46 that is melt-kneaded and molded can achieve the target product characteristics (material characteristics) identified in S1, the process proceeds to the next step S12. In step S12, the process proceeds to a manufacturing process in which products similar to the final molded body 46 are mass-produced.
[0031] In the case of the first resin material 41 shown in Table 1 of FIG. 4, the amount of circulation in the market is large, but the flexural modulus is 1000 MPa or less, which does not reach the flexural modulus of 1100 MPa (see Table 1). For this reason, it is difficult to manufacture recycled products of a specified quality with the first resin material 41 alone, since the flexural modulus is 1000 MPa or less. On the other hand, the "density, MFR, flexural modulus, and Izod impact strength" shown by the second (family) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C (see Tables 2 to 4 of FIG. 4) are often at the levels shown in Table 1, and it can be seen that recycled products of a specified quality can be manufactured when the second (family) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C are used. However, with regard to the distribution of second (household) resin material 42A, second (own) resin material 42B, and second (one) resin material 42C, the commercial relationships between the companies wishing to purchase RP materials and the sales companies have become deeper, and if the distribution volume of second (household) resin material 42A, second (own) resin material 42B, and second (one) resin material 42C decreases, it will be difficult for purchasing companies that do not have a commercial relationship with RP materials to obtain the desired quantities of second (household) resin material 42A, second (own) resin material 42B, and second (one) resin material 42C from the market when desired.
[0032] Incidentally, the present inventors have derived from the experimental data and knowledge they have accumulated thus far, a component analysis of the first resin material 41 and the second resin material 42 and measurement of the material properties. As a result, it has been found that the amount of the second resin material 42 added relative to the first resin material 41 is adjusted to mix, melt and knead the molded first and second resin materials 45, etc., to have an increased PP component and a higher flexural modulus, and that the final molded body 46, etc. can be used for commercialization. As a result of component analysis and measurement of the material properties of the first resin material 41, the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C, it is found that the first resin material 41, the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C contain at least PP, PE, and inorganic filler components, and that the PP content of the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C is greater than the PE content of the first resin material 41, and the PE content of the first resin material 41 is greater than the PE content of the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C. In addition, when it is assumed that the amount of PE in the first resin material 41 is higher than the assumed amount of PE in the RP material after melt-kneading, it was found that a method of reducing the amount of the first resin material 41 from the assumed amount and increasing the amount of the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C mixed and added from the assumed amount is effective. As a result, although the first resin material 41 alone has a large distribution volume, its use applications are limited because its flexural modulus is 1000 MPa or less. However, by adopting a measure of mixing the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C with the first resin material 41 and appropriately setting the compounding ratio, the amount of PE components after melt-kneading is reduced while the amount of PP components is increased, and further, the values of the flexural modulus and the like are increased, so that the use applications of the first resin material 41 are now in a promising situation. In other words, in the case of a manufacturing method in which the amounts of second (house) resin material 42A, second (own) resin material 42B, and second (first) resin material 42C added to the first resin material 41 are adjusted and melt-kneaded, it can be seen that the properties of the first resin material 41 are improved and it can be used effectively by adding second (house) resin material 42A, second (own) resin material 42B, and second (first) resin material 42C to the first resin material 41 in the compounding ratios shown in the table below, mixing them, and melt-kneading them.
[0033] A specific example of this manufacturing method will be described below. Comparative Example 1 and Example 1 use material 1 for the first resin material 41 in Table 1 of Fig. 4, and use material 2 for the second (first) resin material 42C in Table 4 of Fig. 4. Comparative Example 2 and Example 2 use material 1 for the first resin material 41 in Table 1 of Fig. 4, and use material 2 for the second (first) resin material 42C in Table 4 of Fig. 4. First, we disclose a manufacturing method for an RP material in which the compounding ratio is changed based on component detection of the first resin material 41 and the second (first) resin material 42C in a situation where the second (home) resin material 42A, the second (self) resin material 42B and the inorganic filler 43 are not available in sufficient quantities and only the first resin material 41 and the second (first) resin material 42C are used.
[0034] [Table 2]
[0035] In the above Comparative Example 1, the first resin material 41 and the second resin material 42, which is obtained by melting and kneading the second (first) resin material 42C alone, are melted and kneaded to produce a final molded body 46. The components (ratios) and material properties of Comparative Example 1 are as described above. In Comparative Example 1, the PE component is 32.8% by weight (background colored), and the specific range of the PE component does not satisfy the condition of 30% by weight or less. Similarly, the flexural modulus is 1012 MPa (background colored), and the specific range of the PE component does not satisfy the condition of 1100 or more by bending modulus. In order to solve this condition, measures are taken to change the ratio between the first resin material 41 and the second resin material 42 (adjusting the amounts of materials put in, etc.). That is, in the case of Comparative Example 1, the composition is the first resin material 41 (45% by weight) and the second resin material 42 (55% by weight), but in Example 1, the composition is changed to the first resin material 41 (30% by weight) and the second resin material 42 (70% by weight) by changing and adjusting the amounts of materials put in. The input amount adjustment is performed based on the results of component analysis and measurement of material properties, with the premise derived from accumulated experimental data, knowledge, etc. The result is as shown in Example 1 below.
[0036] [Table 3]
[0037] The final molded body 46 was subjected to a component analysis and the material properties were measured, and the breakdown values were as shown above. As a result, the PE component was 24.5% by weight, which satisfies the specific range condition ("high priority application") of "PE component being 30% by weight or less". It is also found that the flexural modulus is 1106 MPa, which satisfies the specific range condition ("low priority application") of "flexural modulus being 1100 MPa or more". It is also found that the MFR increased from 5.8 g / 10 min to 6.8 g / 10 min, which satisfies the specific range ("low priority application") of "MFR being 3.0 g / 10 min or more". The Izod impact strength was 5.2 kJ / m 2 from 5.4 J / m 2 The Izod impact strength increased to 5.0 kJ / m 2It can be seen that the specific range of "the inorganic filler is 15% by weight or less of the total weight" is satisfied ("Priority Application Low"). In addition, "The density of the RP material after melt kneading is 1.00 g / cm3 or less" is satisfied ("Priority Application Low"). 3 The condition for "high priority application" (specific range) of "less than" is met. From the results of Comparative Example 1 and Example 1, it can be seen that even in a situation where the second (home) resin material 42A and the second (self) resin material 42B are not available in sufficient quantities, by reducing the input amount of the first resin material 41 and increasing the input amount of the second (first) resin material 42C containing a large amount of PP components, the first resin material 41 can be effectively utilized. By taking this measure, the PE components after melt kneading are reduced while the PP components are increased, improving the rigidity and impact resistance of the RP material, and it can be seen that such a method of changing the compounding ratio is effective.
[0038] [Table 4]
[0039] Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the second (first) resin material 42C and the inorganic filler 43 in a situation where sufficient amounts of the second (home) resin material 42A and the second (self) resin material 42B cannot be obtained and only the first resin material 41, the second (first) resin material 42C and the inorganic filler 43 are used. In Comparative Example 2 and Example 2, the second (home) resin material 42A and the second (self) resin material 42B are not used, so the first resin material 41, the second resin material 42 obtained by melt-kneading the second (first) resin material 42C alone, and the inorganic filler 43 are melt-kneaded to form a final molded body 46. The components (ratios) of Comparative Example 2 are the first resin material 41 (50% by weight), the second resin material 42 obtained by melt-kneading the second (first) resin material 42C (40% by weight), and the inorganic filler 43 (10% by weight). In Comparative Example 2, the PE component is 34.7% by weight (with background color), which does not satisfy the condition of the specific range of the PE component being 30% by weight or less. Similarly, the material density is 1.02 g / cm 3(with background color) and the material density in the specific range ("high priority application") is 1.00 g / cm 3 Similarly, the Izod impact strength is less than 4.1 kJ / m 2 (Background colored) and the specific range of Izod impact strength is 5.0 kJ / m 2 The above conditions are not satisfied. In order to solve this situation, measures are taken to change the ratio of the first resin material 41, the second resin material 42, and the inorganic filler 43 (adjustment of input amount, etc.). That is, in the case of Comparative Example 2, the composition was the first resin material 41 (50% by weight), the second (first) resin material 42C (40% by weight), and the inorganic filler 43 (10% by weight), but by changing and adjusting the input amounts, the composition is changed to the first resin material 41 (15% by weight), the second (first) resin material 42C (80% by weight), and the inorganic filler 43 (5% by weight) in Example 2. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that the composition is derived from accumulated experimental data, knowledge, etc. When the final molded body 46 is component analyzed and the material properties are measured, the breakdown values are as follows.
[0040] [Table 5]
[0041] As a result, in Example 2, the PE component is 15.9% by weight, which satisfies the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). Similarly, the Izod impact strength is 4.1 kJ / m 2 to 5.0 kJ / m 2 The Izod impact strength increased to 5.0 kJ / m 2 It can be seen that the specific range ("low priority application") condition of "flexural modulus is 1100 MPa or more" is met. It can also be seen that the flexural modulus increases from 1351 MPa to 1390 MPa, which satisfies the specific range ("low priority application") condition of "flexural modulus is 1100 MPa or more". It can also be seen that the MFR increases from 4.6 g / 10 min to 7.6 g / 10 min, which satisfies the "low priority application" condition of "MFR is 3.0 g / 10 min or more". The material density is 0.97 g / cm 3and the specific range ("high priority application") is "material density is 1.00 g / cm 3 It can be seen that the condition of "less than 15% by weight" is satisfied. In addition, the component ratio of inorganic filler 43 is 7.8% by weight or less, and it can be seen that the condition of "the inorganic filler, which is the specific range of "low priority application", is 15% by weight or less with respect to the total weight" is satisfied. From the results of Comparative Example 2 and Example 2, it can be seen that even in a situation where the second (home) resin material 42A, the second (self) resin material 42B, and the third resin material 42C are not available in sufficient amounts and only the first resin material 41, the second (home) resin material 42A, and the inorganic filler 43 are used, the first resin material 41 can be effectively utilized by reducing the amount of the first resin material 41 input and increasing the amount of the second (first) resin material 42C that contains a large amount of PP components. By taking this measure, the PE components after melt-kneading decreased while the PP components increased, and the values of the flexural modulus and the like increased, so it can be seen that such a method of changing the compounding ratio is effective.
[0042] As described above in detail, the manufacturing method of the present embodiment includes the following components: 3a first measurement step (S2) of measuring material performance of a first resin material 41 (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law is applied; a second measurement step (S4 to S6) of measuring material performance of a second resin material 42 (which may contain an inorganic filler component) obtained from used plastic mainly composed of polypropylene; a calculation step (S7) of calculating input amounts of the first recycled resin material 41 and the second recycled resin material 42 (which may contain an inorganic filler component) based on the material performances of the first recycled resin material 41 and the second recycled resin material 42 (which may contain an inorganic filler component) measured in the first measurement step and the second measurement step; and a calculation step (S8) of calculating input amounts of the first recycled resin material 41 and the second recycled resin material 42 (which may contain an inorganic filler component) based on the calculated input amounts of the first recycled resin material 41 and the second recycled resin material 42 (which may contain an inorganic filler component) after melt-kneading the recycled plastic material so that the material performance falls within the specified range (density is 1.00 g / cm 3 and an input amount calculation step (S9) of calculating the input amount of the inorganic filler material 43 so that the total amount of the inorganic filler material 43 is less than 100%. In the case of the manufacturing method of the RP material of this embodiment, the second resin material 42 is mixed into the first resin material 41 and melt-kneaded, so that the flexural modulus and Izod impact strength of the RP material increase, and the melt-kneaded resin material (final molded body 46) can be used alone. As a result, as described in Non-Patent Document 1 ("Use Status of Waste Plastics in 2020"), the first resin material 41 cannot be effectively utilized despite its large circulation volume, and the first resin material 41 alone has limited uses. However, by mixing the second resin material 42 into the first resin material 41 and melt-kneading it, the material properties (flexural modulus value, etc.) of the material increase, improving the limited use. As a result, the first resin material 41, which is in large circulation, can be used in a more environmentally friendly manner than before, and the use of the RP material to which the Container Recycling Law is applied can be effectively promoted.
[0043] That is, while the second resin material 42 can be recycled by itself, the first resin material 41, which has a large inflow, is currently difficult to recycle by itself. Furthermore, among the second resin materials 42, the resin materials derived from the Automobile Recycling Law and the Home Appliance Recycling Law, in particular, are less in circulation than the first resin material 41. Furthermore, the business ties between the purchasing companies and the selling companies of RP materials are strong, making it difficult to obtain them from the distribution market and making it difficult to advance recycling. Under the current circumstances, however, by mixing an appropriate amount of the second resin material 42 with the first resin material 41 and melt-kneading it, the melt-kneaded resin material has physical properties superior to those of the first resin material 41, opening the way for recycling. Therefore, there is a high possibility that recycling will progress significantly for the first resin material 41, which has a large inflow. As recycling as a whole progresses, it can be said that the industrial effects will be extremely large.
[0044] The RP material of this embodiment contains the following components: 3 The recycled plastic material is manufactured so that its specific range is less than 1.00 g / cm. The recycled plastic material is a first recycled resin material 41 (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law is applied, and the input amount is calculated based on measured material performance. The recycled plastic material is a second recycled resin material 42 (which may contain an inorganic filler component) obtained from used plastic mainly composed of polypropylene, and the input amount is calculated based on measured material performance. The recycled plastic material is manufactured so that its specific range is less than 1.00 g / cm. The first recycled resin material 41 and the second recycled resin material 42 are manufactured so that their specific range is less than 1.00 g / cm. 3The inorganic filler material 43, the input amount of which is calculated so as to be within the range of 0.1 to 1.0 mm, and the first recycled resin material 41, the second recycled resin material 42, and the inorganic filler material 43, the input amounts of which are calculated, are melted and kneaded to form the RP material. In the case of the RP material of this embodiment, the first resin material 41 alone has limited uses, whereas in the case of the final molded body 46 in which the second resin material 42 is mixed into the first resin material 41 and melted and kneaded, the values of the flexural modulus and Izod impact strength increase, and the melted and kneaded resin material can be used in a wide range of applications, unlike the case of the first resin material 41 alone. As a result, the first resin material 41, which is widely distributed, can be utilized in an environmentally friendly manner, and the use of the RP material to which the Container and Packaging Recycling Law is applied can be effectively promoted. In addition, according to the present embodiment, a method of adjusting the input amount is adopted in which the second resin material 42 is used to adjust the input amount relative to the first resin material 41. However, it is not necessary to adopt the input amount adjustment method, and a method of setting an appropriate mixing ratio from the beginning may be adopted. The second resin material 42 that is added to improve the physical properties of the first resin material 41 may be virgin material other than recycled material, or may be second (home) resin material 42A, second (own) resin material 42B, or second (first) resin material 42C that has not yet been released to the market.
[0045] The following supplementary notes are provided. Supplementary Note 1 is as follows: The material properties are as follows: Density is 1.00 g / cm 3The manufacturing method for manufacturing a recycled plastic material with a specific range of less than 100% is characterized by having a first measurement step (S2) of measuring the material performance of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, a second measurement step (S4 to S6) of measuring the material performance of a second recycled resin material (which may contain an inorganic filler component) obtained from used plastic mainly composed of polypropylene, a calculation step (S7) of calculating the input amounts of the first recycled resin material and the second recycled resin material (which may contain an inorganic filler component) based on the material performances of the first recycled resin material and the second recycled resin material (which may contain an inorganic filler component) measured in the first measurement step and the second measurement step, and an input amount calculation step (S9) of calculating the input amount of inorganic filler material based on the calculated input amounts of the first recycled resin material and the second recycled resin material (which may contain an inorganic filler component) so that the material performance of the recycled plastic material after melt-kneading is within the specific range. Supplementary Note 2 is as follows: That is, in the manufacturing method of the recycled plastic material described in Supplementary Note 1, in the input amount calculation step, when the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range, the input of new inorganic filler material is eliminated. Supplementary Note 3 is as follows: That is, in the manufacturing method of the recycled plastic material described in Supplementary Note 1 or 2, when the material properties of the recycled plastic after molding are set to a specific range, a high or low priority application order is set, and the "high priority application" specifies that the polyethylene content is 30% by weight or less relative to the total weight of the recycled plastic material, and specifies that the polyethylene content is less than this, and the "low priority application" includes at least that the MFR is 3.0 g / 10 min or more. Supplementary Note 4 is as follows: That is, the method for producing a recycled plastic material according to any one of Supplementary Note 1 to 3 is characterized in that, when it is expected that the content of polyethylene in the first recycled resin material is higher than the expected content value of polyethylene in the recycled plastic material, the method further comprises an input amount adjustment step of reducing the input amount of the first recycled resin material below a predetermined expected input amount and increasing the input amount of the second recycled resin material above a predetermined expected input amount.
[0046] Appendix 5 is as follows: The material properties are density 1.00g / cm 3 The recycled plastic material has a specific range of less than or equal to the specific content, and is characterized in that it comprises a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and whose input amount is calculated based on measured material performance; a second recycled resin material (which may contain an inorganic filler component) obtained from used plastic whose main component is polypropylene, and whose input amount is calculated based on measured material performance; and an inorganic filler material whose input amount is calculated based on the calculated input amounts of the first recycled resin material and the second recycled resin material so that the material performance after melt-kneading of the recycled plastic material falls within the specific range, and the first recycled resin material, the second recycled resin material, and the inorganic filler material whose input amounts are calculated are melt-kneaded together.
[0047] Supplementary Note 6 is as follows: That is, in the recycled plastic material described in Supplementary Note 5, the polyethylene content in the molded recycled plastic material is adjusted and blended to be 30% by weight or less with respect to the total weight of the recycled plastic material. Supplementary Note 7 is as follows: That is, in the recycled plastic material according to Supplementary Note 5 or 6, the amount of the inorganic filler added is 15% by weight or less with respect to the total amount of the recycled plastic material before melt-kneading. Supplementary Note 8 is as follows: That is, in the recycled plastic material described in Supplementary Note 5 or 6, the specific range of the material performance satisfies all of the following conditions (1) to (3). (1) MFR is 3.0g / 10min or more, (2) Flexural modulus of 1100 MPa or more; (3) Izod impact strength is 5.0 kJ / m 2 End [Explanation of symbols]
[0048] 41 First recycled resin material (first resin material) 42 PP main component resin material Secondary resin material 42A 2nd (house) resin material (derived from recycled home appliance materials) 42B Second (self) resin material (derived from recycled automobile materials) 42C 2nd (first) resin material (derived from general recycled materials) 43 Inorganic filler materials S2 First measurement step S4 to S6 Second measurement step S7 Calculation step S9 Input amount calculation step
Claims
1. Material properties: density 1.00 g / cm 3 A manufacturing method for manufacturing a recycled plastic material having a specific range of less than A first measurement step of measuring material properties (including at least density) of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; A second measurement step of measuring the material properties (including at least density) of a second recycled resin material (which may contain an inorganic filler component) obtained from used plastics mainly composed of polypropylene; A calculation step of calculating the input amounts of the first recycled resin material and the second recycled resin material based on the material properties (including at least density) of the first recycled resin material and the second recycled resin material measured in the first measurement step and the second measurement step; A step of calculating an input amount of a new inorganic filler material based on the calculated input amounts of the first recycled resin material and the second recycled resin material so that the material performance (including at least density) after melt-kneading of the recycled plastic material falls within the specific range; A method for producing a recycled plastic material, comprising:
2. 2. The method for producing recycled plastic material according to claim 1, characterized in that, in the input amount calculation step, if the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range, the input of new inorganic filler material is stopped.
3. 3. The method for producing a recycled plastic material according to claim 1 or 2, characterized in that, when the material properties of the recycled plastic after molding are within a specific range, a high or low priority application order is set, in which a "high priority application" is set so that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and a "low priority application" is set so that the MFR is 3.0 g / 10 min or more.
4. A method for producing recycled plastic material as described in claim 1 or 2, characterized in that it includes an input amount adjustment step of reducing the input amount of the first recycled resin material below a predetermined estimated input amount and increasing the input amounts of the second recycled resin material and the inorganic filler material above the predetermined estimated input amounts when the polyethylene component amount of the first recycled resin material is higher than the estimated polyethylene component value of the recycled plastic material after molding.
5. Material properties: density 1.00 g / cm 3 A recycled plastic material with a specific range of less than First recycled resin materials (which may contain inorganic filler components) are obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and the input amount is calculated based on the measured material performance. A second recycled resin material (which may contain inorganic filler components) is obtained from used plastics that are primarily composed of polypropylene, and the input amount is calculated based on the measured material performance. Regarding the first recycled resin material and the second recycled resin material, an inorganic filler material whose input amount is calculated based on the calculated input amount of each of them so that the material performance after melt-kneading of the recycled plastic material falls within the specific range; A recycled plastic material characterized by being obtained by melt-kneading the first recycled resin material, the second recycled resin material, and the inorganic filler material, the amounts of which have been calculated.
6. 6. The recycled plastic material according to claim 5, characterized in that the polyethylene content in the molded recycled plastic material is adjusted and blended to be 30% by weight or less based on the total weight of the recycled plastic material.
7. 7. The recycled plastic material according to claim 5, wherein the inorganic filler is added in an amount of 15% by weight or less based on the total amount of the recycled plastic material before melt-kneading.
8. The recycled plastic material according to claim 5 or 6, wherein the specific range of material performance satisfies all of the following conditions (1) to (3). (1) MFR is 3.0 g / 10 min or more, (2) A flexural modulus of 1100 MPa or more; (3) Izod impact strength of 5.0 kJ / m 2 End
Citation Information
Patent Citations
Polypropylene-based resin composition and molded product therefrom
JP2005232413A
Resin composition for vehicular interior using crushed material of vehicular bumper mixed with insoluble substance as raw material, and molding thereof
JP2009173947A
PP compounds that retain excellent mechanical properties and exhibit improved or non-appearing tiger stripes.
JP2015537087A
Resin composition for seamless air bag covers, and seamless air bag covers or seamless instrument panels with air bag covers, made by using the composition
WO2006040825A1