Method for producing recycled plastic material, and recycled plastic material

By measuring and adjusting the properties of recycled resin materials, the method addresses quality and cost issues in recycled plastics, enabling their effective use in manufacturing.

JP2024134501APending Publication Date: 2024-10-03GIFU PLAST IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023189691
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-11-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The quality of recycled plastic materials varies significantly due to contamination with foreign substances and resin imbalance, making them difficult to use in manufacturing products of consistent quality, and their high cost relative to virgin materials hinders their adoption by businesses and consumers.

Method used

A method involving measurement and adjustment of material properties of recycled resin materials, including polypropylene, polyethylene, and inorganic fillers, to achieve specific ranges of density, melt flow rate, flexural modulus, and Izod impact strength, ensuring compatibility and quality for manufacturing.

Benefits of technology

This approach enables the production of recycled plastic materials with consistent strength and environmental sustainability, overcoming quality inconsistencies and cost barriers, facilitating their wider use in manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134501000001_ABST
    Figure 2024134501000001_ABST
Patent Text Reader

Abstract

To provide an excellent recycled plastic material which can expand a range of usage while considering the environment, when using a recycled resin obtained from a used plastic container package to which the Law for Promotion of Sorted Collection and Recycling of Containers and Packaging is applied.SOLUTION: A first resin material 41 is acquired from a used plastic container package to which the Law for Promotion of Sorted Collection and Recycling of Containers and Packaging is applied. A second resin material 42A derived from a household electric recycled material is acquired from a RP material to which the Law for Promotion of Sorted Collection and Recycling of Containers and Packaging is applied. A third resin material 42B derived from an automobile recycled material is acquired from a RP material to which the Law on Recycling of End-of-Life Vehicles is applied. A fourth resin material 42C derived from a general recycled material is acquired from an RP material to which both the Law for Promotion of Sorted Collection and Recycling of Containers and Packaging, and the Law on Recycling of End-of-Life Vehicles are not applied. The RP material is molded by charging one kind of the second to fourth resin materials 42A, 42B and 42C in addition to the first resin material 41, as necessary, charging an inorganic filler material 43, and melt-kneading the mixture.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a recycled plastic material using recycled resin (hereinafter sometimes referred to as "R resin") obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law (hereinafter abbreviated as "Container and Packaging Recycling Law") applies, and to the recycled plastic material. [Background technology]

[0002] In recent years, in the development of plastic products, it is desirable to use recycled materials rather than virgin materials. In particular, since the establishment of the Containers and Packaging Recycling Law, the use of recycled materials covered by this law has been recommended. This is because, as described in Non-Patent Document 1 ("Use of Waste Plastics in 2020"), packaging containers / containers account for 47.5% (3.9 million tons) of the "total amount of waste plastic generated," and packaging containers / containers account for 77.1% (3.16 million tons) of the "general waste by category," and the volume of waste (waste plastic) related to packaging containers / containers in circulation is large. Therefore, if recycling of R resin subject to the Containers and Packaging Recycling Law progresses, the recycling of all waste plastics will also progress, so there is a strong demand for the use of recycled plastic materials to which the Containers and Packaging Recycling Law applies. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Japan Plastics Industry Federation Magazine Plastics June 2022 Issue Pages 79-83 Author Masashi Hanba Publisher Japan Industrial Publishing Co., Ltd. Published June 10, 2022 Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, recycled plastic materials (hereinafter sometimes referred to as "RP materials") have a bias in quality depending on the origin of the material. In addition, while there is a considerable amount of unshipped and unused RP materials due to production losses and processing losses of RP materials, there is also a considerable amount of used waste (used waste may be contaminated with foreign matter even after cleaning). Therefore, unlike virgin materials with a constant material quality, various resins, foreign matter, etc. are mixed into RP materials, and the material properties tend to be easily deteriorated, biased, and varied. This is particularly noticeable for RP materials to which the Containers and Packaging Recycling Law applies. Therefore, various ingenuity and effort are required to manufacture products of a certain level of quality using RP materials to which the Containers and Packaging Recycling Law applies, and it is not necessarily easy to promote the use of RP materials to which the Containers and Packaging Recycling Law applies. In addition, regarding the distribution of RP materials, if the selling price is the same as that of virgin materials, businesses will not be motivated to purchase and manufacture RP materials. Furthermore, if the price of products using RP materials does not fall, general consumers may not be motivated to purchase products using RP materials, even if they recognize the importance of recycling. Therefore, in order to promote the use of RP materials, it is important that the price falls compared to that of virgin materials. Furthermore, while those who wish to purchase plastic-related virgin materials can purchase them steadily by placing an order with a company that manufactures and sells them, those who wish to purchase RP materials cannot purchase them if the company that supplies them cannot obtain recycled raw materials. Therefore, the business ties between the companies that purchase RP materials and the sales companies are strong, and companies that do not have a commercial relationship with the sales companies are in a situation where they cannot obtain the desired amount of RP materials from the market when they wish to purchase them. Furthermore, when promoting the use of RP materials to which the Containers and Packaging Recycling Law applies, environmentally friendly recycling is also strongly requested. The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide an excellent method for producing an RP material, which can be expanded in use while being environmentally friendly by effectively utilizing R resin obtained from RP materials to which the Container and Packaging Recycling Law is applied, and the RP material. [Means for solving the problem]

[0005] In order to solve the above problems, the manufacturing method of the present invention has the following means. That is, as means 1, a first measurement step is performed to measure the material properties of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and a second recycled resin material (which may contain an inorganic filler component) obtained from used plastics not subject to the Container and Packaging Recycling Law and to which the Home Appliance Recycling Law applies, or a third recycled resin material (which may contain an inorganic filler component) obtained from used plastics to which the Automobile Recycling Law applies, or a fourth recycled resin material (which may contain an inorganic filler component) obtained from used plastics not subject to the Container and Packaging Recycling Law and to which neither the Home Appliance Recycling Law nor the Automobile Recycling Law applies is performed to measure the material properties of the second to fourth recycled resin materials. The method includes a second measuring step of measuring the amount of the first recycled resin material and the amount of a mixture of at least one or at least two of the second to fourth recycled resin materials (which may contain an inorganic filler component) based on the material properties of the first recycled resin material and the second to fourth recycled resin materials measured in the first measuring step and the second measuring step, and a calculation step of calculating the amount of a new inorganic filler material to be added based on the calculated amounts of the first recycled resin material and the mixture of at least one or at least two of the second to fourth recycled resin materials (which may contain an inorganic filler component) so that the material properties of the recycled plastic material after melt-kneading are within a specific range. Note that the mixture of at least one or at least two of the first recycled resin material and the second to fourth recycled resin materials may contain an inorganic filler component, so that the inorganic filler component is calculated to determine whether the material properties of the recycled plastic material after melt-kneading exceed the upper limit of a specific range.

[0006] As a second method, in the first method, when the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range in the input amount calculation step, the input of new inorganic filler material is stopped.

[0007] As a third measure, in the first or second measure, when the material properties of the recycled plastic after molding are set to a specific range, it is preferable to set a high or low priority application order to be applied preferentially, and to stipulate that the "high priority application" is that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and that the "low priority application" is to include at least that the MFR (based on JIS standard K7210) is 4.0 g / 10 min or more.

[0008] As a fourth means, in any one of the first and third means, it is preferable that the first to fourth recycled resin materials each contain at least polypropylene and polyethylene, the polypropylene content of the second to fourth recycled resin materials is greater than the polypropylene content of the first recycled resin material, and the polyethylene content of the first recycled resin material is greater than the polyethylene content of the second to fourth recycled resin materials.

[0009] As a fifth aspect, in any one of the first to fourth means, when it is expected that the polyethylene content of the first recycled resin material is higher than the expected polyethylene content of the recycled plastic material, it is preferable to provide an input amount adjustment step of reducing the input amount of the first recycled resin material from a predetermined expected input amount and increasing the input amount of any one or a mixture of at least two or more of the second to fourth recycled resin materials from a predetermined expected input amount. Note that in any one of the first to fourth means, it is preferable that the input amount adjustment step is performed based on the results of component analysis of the recycled plastic material and measurement of the material properties.

[0010] The invention of the present invention has the following means. That is, as a means 6, a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, a second recycled resin material (which may contain an inorganic filler component) obtained from used plastics not subject to the Container and Packaging Recycling Law but to which the Home Appliance Recycling Law applies, a third recycled resin material (which may contain an inorganic filler component) obtained from used plastics not subject to the Container and Packaging Recycling Law but to which the Automobile Recycling Law applies, a fourth recycled resin material (which may contain an inorganic filler component) obtained from general used plastics not subject to the Container and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law, a mixture of one or at least two of the second to fourth recycled resin materials (which may contain an inorganic filler component), and the first recycled resin material (which may contain an inorganic filler component) are added, melted, and kneaded to form a molded product.

[0011] As a seventh measure, in the sixth measure, the recycled plastic material after molding preferably contains at least polypropylene, polyethylene, and an inorganic filler, and the polypropylene content is greater than the polyethylene content, and the polyethylene content is adjusted to be 30% by weight or less based on the total weight of the recycled plastic material. (Hereinafter, polypropylene may be simply referred to as "PP" and polyethylene may be simply referred to as "PE.")

[0012] As a means 8, in the means 6 or 7, it is preferable that a mixture of any one or at least two or more of the second to fourth recycled resin materials has a higher MFR (based on JIS standard K7210) value than the first recycled resin material.

[0013] As a ninth aspect, in any one of the sixth to eighth aspects, it is preferable that the MFR (based on JIS standard K7210) value of the recycled plastic material after molding is 4.0 g / 10 min or more. Effect of the Invention

[0014] According to the present invention, by effectively utilizing recycled resin obtained from used plastic containers and packaging to which the Containers and Packaging Recycling Law applies, it is possible to provide a manufacturing method for a recycled plastic material that is excellent in strength and other properties and can be expanded in use while being environmentally friendly, and a recycled plastic material. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic diagram showing a manufacturing process of an embodiment of the present invention; [Diagram 2] 4 is a graph showing the relationship between the polyethylene content and the weld strength in the embodiment. [Diagram 3] 4 is a flowchart showing a manufacturing process in the embodiment. [Figure 4] FIG. 4 is an explanatory diagram showing component values ​​and physical property values ​​of first to fourth resin materials in the embodiment. [Diagram 5] FIG. 4 is an explanatory diagram showing a specific range of a resin material used in the embodiment. [Figure 6] FIG. 2 is an explanatory diagram showing Comparative Examples 1 and 2 and Examples 1 and 2 in the embodiment. [Figure 7] 4A and 4B are explanatory diagrams showing Comparative Examples 3 and 4 and Examples 3 and 4 in the embodiment. [Figure 8] FIG. 4 is an explanatory diagram showing Comparative Examples 5 and 6 and Examples 5 and 6 in the embodiment. [Figure 9] 4A and 4B are explanatory diagrams showing Comparative Examples 7 and 8 and Examples 7 and 8 in the embodiment. [Figure 10] FIG. 11 is an explanatory diagram showing Comparative Examples 9 and 10 and Examples 9 and 10 in the embodiment. [Figure 11] FIG. 12 is an explanatory diagram showing Comparative Examples 11 and 12 and Examples 11 and 12 in the same embodiment. [Figure 12] FIG. 2 is an explanatory diagram showing the blending results of Comparative Examples 1 to 12 and Examples 1 to 12 in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 shows a schematic diagram of the RP material being melt-kneaded and molded in the embodiment. Fig. 2 shows a graph showing the relationship between the PE content and the weld strength in the embodiment. Fig. 3 is a flow chart showing the manufacturing process for manufacturing the RP material, and Fig. 4 shows the component values ​​and physical property values ​​of the first to fourth resin materials in the embodiment. Fig. 5 shows the specific range of the resin materials. 1 can feed pellet material 37 (comprised of a first resin material 41, second to fourth resin materials 42A, 42B, 42C, or an inorganic filler material 43, etc., which will be described later) into its hopper 36, and the pellet material 37 is conveyed in a conveying section 38 equipped with an internal screw. The extruder 35 can melt-knead and mold the fed pellet material 37 inside, and can also discharge the pellet material 37 from a discharge port 39 as new pellet material. For the melt-kneading method, a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer, etc. can be used. In the pellet material 37 of this embodiment, a recycled resin material 41 (hereinafter, this recycled resin material 41 is referred to as "first resin material 41") obtained from used plastic container packaging to which the Container Recycling Law is applied is an essential component. In addition, as an optional component of the pellet material 37, a recycled resin material 42A (hereinafter, this recycled resin material 42A is referred to as "second resin material 42A") obtained from used plastic to which the Home Appliance Recycling Law is applied can be included. In addition, as another optional component of the pellet material 37, a recycled resin material 42B (hereinafter, this recycled resin material 42B is referred to as "third resin material 42B") obtained from used plastic to which the Automobile Recycling Law is applied can be included. Furthermore, as an optional component of the pellet material 37, a recycled resin material 42C (hereinafter, this recycled resin material 42C is referred to as "fourth resin material 42C") obtained from general used RP material to which none of the Container Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law is applied can be included. As shown in FIG. 4, the first to fourth resin materials 41, 42A, 42B, and 42C contain a polypropylene (hereinafter referred to as "PP") component, a polyethylene (hereinafter referred to as "PE") component, an inorganic filler component, and other components (hereinafter referred to as "others"). Depending on the origin of the product, etc., there is a bias in the amount of components, etc., and the physical properties are variable. In addition, an inorganic filler material 43 can be added to the pellet material 37 as an optional component to improve rigidity or increase specific gravity (density). The first to fourth resin materials 41, 42A, 42B, and 42C contain an inorganic filler component, and have the effect of improving rigidity according to the amount of the component. If the desired rigidity is insufficient, additional inorganic filler material 43 can be added. The inorganic filler material 43 may be any known material that does not affect the properties of the plastic material and improves rigidity. Examples of inorganic filler materials include carbonates, sulfates, silicates, phosphates, borates, oxides, and hydrates of calcium, magnesium, titanium, aluminum, iron, zinc, etc., or powders of these hydrates. Specific examples include calcium carbonate, magnesium carbonate, zinc oxide, titanium oxide, silica, alumina, clay, talc, kaolin, aluminum hydroxide, magnesium hydroxide, aluminum silicate, magnesium silicate, calcium silicate, aluminum sulfate, magnesium sulfate, calcium sulfate, magnesium phosphate, barium sulfate, silica sand, carbon black, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium sulfite, sodium sulfate, potassium titanate, bentonite, wollastonite, dolomite, graphite, etc. These may be contained alone or in combination of two or more kinds. 1 are illustrated in the form of pellets for ease of understanding, but the form is not necessarily limited to pellets. The resin material discharged from the discharge port 39 of the extrusion molding machine 35 may be in the form of pellets or in other forms.

[0017] The inventors and researchers of the present application have studied the material properties, component analysis, market trends, and application fields of RP materials for many years. As a result, they have found that the presence of various resins in RP materials makes them susceptible to deterioration, deviation, bias, and variation in physical properties. They have also found that differences in the product origins of RP materials tend to cause specific trends in material properties and component analysis, which can be roughly categorized into the following (1) to (4). (1) A first resin material 41 obtained from used plastic containers and packaging to which the Containers and Packaging Recycling Law applies (in this case, the first resin material 41 (first recycled resin material) can be said to be a resin material derived from the Containers and Packaging Recycling Law). (2) The second resin material 42A obtained from an RP material that is not subject to the application of the Containers and Packaging Recycling Law but is subject to the Home Appliance Recycling Law (in this case, the second resin material 42A (second recycled resin material) can be said to be a resin material derived from the Home Appliance Recycling Law). (3) A third resin material 42B obtained from an RP material that is not subject to the application of the Containers and Packaging Recycling Law but is subject to the Automobile Recycling Law (in this case, the third resin material 42B (third recycled resin material) can be said to be a resin material derived from the Automobile Recycling Law). (4) A fourth resin material 42C obtained from a general RP material to which none of the Containers and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law applies (in this case, the fourth resin material 42C (fourth recycled resin material) is different from the first resin material 41, the second resin material 42A, and the third resin material 42B, and can be said to be a resin material derived from a general material).

[0018] The official name of the Packaging Recycling Law is the Law Concerning Promotion of Separate Collection and Recycling of Containers and Packaging (the provisions and definitions of the Law will be cited as necessary). Specific targets include, for example, packaging film and food trays, but the items covered by the Law are limited. (R resin materials obtained from items covered by the Law are resin materials derived from packaging recycling materials and correspond to No. 1 Resin Material 41, but the content is subject to change in accordance with amendments to the Law, etc.) The official name of the Home Appliance Recycling Law is the Law Concerning the "Law Concerning the Recycling of Specified Household Appliances" (the provisions and definitions of the law will be cited as necessary). The items covered are four types of home appliances (air conditioners, televisions, refrigerators, freezers, washing machines, and clothes dryers), but the used plastics to which the law applies are limited to those discarded from ordinary households and offices. Therefore, even if the four types of home appliances are covered by the law, there are cases in which the law does not apply due to differences in the source of disposal. (R resin materials obtained from items covered by the law are resin materials derived from home appliance materials and correspond to second resin material 42A, but the content is subject to change in accordance with amendments to the Home Appliance Recycling Law, etc.) The official name of the Automobile Recycling Law is the "Law Concerning Recycling, etc. of End-of-Life Automobiles" (the provisions and definitions of the law will be cited as necessary). The law defines "automobiles" and the specific objects of the law are limited to, for example, automobile bumpers and automobile interior materials. (The R resin material obtained from objects covered by the law is a resin material derived from automobile materials and corresponds to the third resin material 42B, but the content is subject to change in accordance with amendments to the Automobile Recycling Law, etc.) In addition, there are R resin materials obtained from general used RP materials to which the Container Recycling Law, Home Appliance Recycling Law, and Automobile Recycling Law do not apply. For example, (1) R resin materials obtained from RP materials of items other than the four types of home appliances to which the Home Appliance Recycling Law applies, and (2) resin materials obtained from RP materials of motorcycles to which the Automobile Recycling Law does not apply. (This R resin material is a resin material derived from general materials and corresponds to the fourth resin material 42C, but the content is subject to change according to changes in the Container Recycling Law, Home Appliance Recycling Law, and Automobile Recycling Law, etc.) Due to such legal treatment, the second to fourth resin materials 42A, 42B, and 42C have similarities in composition and material properties, but there are differences in composition and material properties depending on the origin of the product related to the applicable law, resulting in specific trends.

[0019] 4 shows Tables 1 to 4. Table 1 shows the component values ​​by weight % of PP, PE, inorganic filler, and other components (hereinafter referred to as "others") for four groups of materials (material 1, material 2, material 3, and material 4) of the first resin material 41, and further shows four physical property values ​​(in this case, density, melt flow rate (hereinafter referred to as "MFR"), flexural modulus, and Izod impact strength). Tables 2 to 4, like Table 1, show the weight percent values ​​of the components (PP components, PE components, inorganic filler components, other components) of each material (material 1, material 2, material 3, material 4) for the second resin material 42A, the third resin material 42B, and the fourth resin material 42C, as well as four physical property values ​​(in this case, density, MFR, flexural modulus, Izod impact strength). The indication of materials 1 to 4 for each resin material (41, 42A, 42B, 42C) may be four or less or more. Furthermore, the four physical properties to be measured may include other physical properties as necessary.

[0020] Next, a method for measuring the material properties of a resin material will be described. The melt flow rate (hereinafter referred to as "MFR"), which represents one of the material properties of a resin material, can be measured using a Melt Indexer G-02 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the MFR measurement method (JIS K7210, 230 degrees Celsius, load 2.16 kg). The flexural modulus, which represents one of the material properties of a resin material, can be measured using a Bentograph B-2 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the flexural property measurement method (JIS K7171). The Izod impact strength, which represents one of the material properties of a resin material, can be measured using an impact tester IT (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the Izod impact measurement method (JIS K7110). The material density, which represents one of the material properties of a resin material, can be measured using an electronic specific gravity meter SD-200L (manufactured by Alpha Mirage Co., Ltd.) by the density and specific gravity measurement method (JIS K7112). The MFR of the material 1 of the first resin material 41 shown in the table is 3.1 g / 10 min. The flexural modulus of the material 1 of the first resin material 41 is 666 MPa. The Izod impact strength of the material 1 of the first resin material 41 is 4.6 kJ / m 2The material density of the material 1 of the first resin material 41 is 0.96 g / cm 3 The component values ​​of PP, PE, other resins, and inorganic fillers that have been subjected to component analysis are listed in the columns for Material 2, Material 3, and Material 4 of the first resin material 41. For example, an infrared spectrophotometer FT / IR-4X manufactured by JASCO Corporation can be used to measure PP, PE, and other resins in the resin material, but other devices may also be used. The amount of inorganic filler is measured using the amount of combustion residue. For example, an electric crucible furnace FUC030FB manufactured by Advantec Toyo Co., Ltd. can be used. These values ​​are shown in the columns of Tables 1 to 4 (Material 1, Material 2, Material 3, Material 4) in FIG.

[0021] Next, the resin materials shown in Tables 1 to 4 in Fig. 4 will be described. First, the first resin material 41 (materials 1 to 4) will be described. The first resin material 41 is characterized in that it has a large PE content and a small PP content, and also has a small other content and inorganic filler content. The density of materials 1 to 4 is 0.94 to 0.97 g / cm 3 The MFR value is in the range of 3.0 to 3.8 g / 10 min, the flexural modulus is in the range of 666 to 937 MPa, and the Izod impact strength is in the range of 4.6 to 8.4 kJ / m 2 They are scattered within a range of about The first resin material 41 has a density of 0.90 to 0.98 g / cm 3 The range of 0.93 to 0.96 g / cm is the approximate practical range. 3 This range is a suitable practical range. From the viewpoint of moldability during injection molding, the MFR of the first resin material 41 is roughly in the practical range of 1.0 to 10.0 g / 10 min, and more preferably in the practical range of 3.0 to 7.0 g / 10 min. From the viewpoint of rigidity (strength) of the product, the flexural modulus of the first resin material 41 is roughly in the practical range of 400 to 1200 MPa, and more preferably in the practical range of 600 to 1100 MPa. From the viewpoint of impact resistance of the product (avoidance of cracking easily), the Izod impact strength of the first resin material 41 is roughly in the practical range of 3.0 to 20.0 kJ / m 2 The range is roughly practical, and further, 5.0 to 15.0 kJ / m 2 This range is a suitable practical range.

[0022] The second resin material 42A (materials 1 to 4) shown in Table 2 of Fig. 4 is characterized in that the PP content is extremely large and the PE content is extremely small, and the other contents and inorganic filler contents are also small. The density of the second resin material 42A is 0.91 to 0.92 g / cm 3 The MFR value is in the range of 25.4 to 28.7 g / 10 min, the flexural modulus is in the range of 1259 to 1370 MPa, and the Izod impact strength is in the range of 6.0 to 7.3 kJ / m 2 As a result, the second resin material 42A (materials 1 to 4) is superior to the first resin material 41 (materials 1 to 4) in terms of MFR, flexural modulus, and Izod impact strength. The second resin material 42A has a density of 0.91 to 0.97 g / cm 3 The range of 0.91 to 0.94 g / cm is the approximate practical range. 3A suitable practical range for the MFR of the second resin material 42A is 10.0 to 35.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 15.0 to 30.0 g / 10 min. A suitable practical range for the flexural modulus of the second resin material 42A is 1000 to 1600 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1100 to 1400 MPa. A suitable practical range for the Izod impact strength of the second resin material 42A is 4.0 to 15.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product. 2 The range is the approximate practical range, and further, 6.0 to 12.0 kJ / m 2 This range is a suitable practical range.

[0023] Further, the third resin material 42B (materials 1 to 4) shown in Table 3 of Fig. 4 is characterized by a large PP content and a small PE content, and is characterized by a large inorganic filler content compared to the first resin material 41, the second resin material 42A, and the fourth resin material 42C. Therefore, when using the third resin material 42B (materials 1 to 4), since the third resin material 42B (materials 1 to 4) itself contains a large amount of inorganic filler components, there are cases where no additional inorganic filler material 43 is used. However, when the inorganic filler components of the third resin material 42B (materials 1 to 4) itself are less than expected, a required amount of inorganic filler material 43 is added. The density of the third resin material 42B is 1.04 to 1.06 g / cm 3 The MFR value is in the range of 24.8 to 35.1 g / 10 min, the flexural modulus is in the range of 1906 to 2159 MPa, and the Izod impact strength is in the range of 17.5 to 24.6 kJ / m 2 As a result, materials 1 to 4 of the third resin material 42B are superior to the first resin material 41 (materials 1 to 4) in terms of MFR, flexural modulus, and Izod impact strength. The third resin material 42B has a density of 0.95 to 1.10 g / cm 3 is the approximate practical range, and 0.97 to 1.07 g / cm3 A suitable practical range for the MFR of the third resin material 42B is 15.0 to 40.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 20.0 to 35.0 g / 10 min. A suitable practical range for the flexural modulus of the third resin material 42B is 1500 to 2500 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1800 to 2300 MPa. A suitable practical range for the Izod impact strength of the third resin material 42B is 6.0 to 35.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product. 2 The range is the approximate practical range, and further, 10.0 to 30.0 kJ / m 2 This range is a suitable practical range.

[0024] The fourth resin material 42C (materials 1 to 4) shown in Table 4 in Fig. 4 is characterized in that the PP content is extremely large, the PE content is extremely small, and the other contents and inorganic filler content are also small. The density of the fourth resin material 42C is 0.94 to 0.98 g / cm 3 The MFR is in the range of 9.6 to 14.0 g / 10 min, the flexural modulus is in the range of 1180 to 1324 MPa, and the Izod impact strength is in the range of 5.8 to 11.1 kJ / m 2 As a result, the fourth resin material 42C (materials 1 to 4) has superior values ​​of MFR, flexural modulus, and Izod impact strength compared to the first resin material 41 (materials 1 to 4). The fourth resin material 42C has a density of 0.91 to 1.0 g / cm 3 The range of 0.91 to 0.96 g / cm is the approximate practical range. 3A suitable practical range for the MFR is 3.0 to 30.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 4.0 to 25.0 g / 10 min. A suitable practical range for the flexural modulus of the fourth resin material 42C is 900 to 1600 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1100 to 1400 MPa. A suitable practical range for the Izod impact strength of the fourth resin material 42C is 4.0 to 25.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product. 2 The range is roughly practical, and further, 5.0 to 15.0 kJ / m 2 This range is a suitable practical range.

[0025] In addition, when PP and PE components are mixed, the inventors of the present application have found that the following characteristics are obtained as a result of experiments. That is, FIG. 2 is a graph showing the relationship between the PE content ratio in an RP material (a resin material made of PP and PE) and the weld strength, with the vertical axis of FIG. 2 showing the weld strength (MPa) and the horizontal axis of FIG. 2 showing the PE content ratio. According to FIG. 2, the weld strength gradually decreases from a PE content ratio of 0% (in this case, the weld strength is 32.6 MPa) toward a PE content ratio of 50% (in this case, the weld strength is 19.0 MPa). In FIG. 2, the PE content ratio is 30% and the weld strength is about 23.0 MPa, and if the PE content ratio is in the range of 0% to 30% (preferably, in the range of 0% to 20%), it is understood that the weld strength is sufficiently maintained (i.e., the strength retention rate is 70% or more), and is a strength (allowable condition) that does not cause problems in commercialization. The weld strength was measured using a test piece of 150 x 100 x 4 mm with a weld formed in the center, under the conditions specified in JIS K7161. In the case of mixing resin materials (hereinafter referred to as "PP-based resin materials") that are PP-based such as second to fourth resin materials 42A, 42B, 42C as in this embodiment with first resin material 41 (foreign matter other than PP and PE can be generally ignored in terms of weld strength even if it is mixed in), it was found that the graph in Fig. 2 applies when the PE content ratio of the PP-based resin material and first resin material 41 is 0% to 30%. As a result, it was found that if the PE content ratio is in the range of 0 to 30%, the allowable range for the product strength of the RP material can be maintained. Next, the material properties (product properties) of products molded from RP materials will be explained using Figure 5. The material properties of the product are related to the specific ranges (amounts of components and material properties values ​​obtained by component analysis) of the RP material after melt kneading. In addition, the specific ranges of material properties can be divided into "high priority application" that is applied preferentially from the viewpoint of product usage, and "low priority application" (lower than "high" priority application). According to Figure 5, "PE content is 30% by weight or less" is "high priority application". In addition, "content of inorganic filler component of RP material after melt kneading is 16% by weight or less", "density is 1.1g / cm3 as physical property of RP material after melt kneading" is "high priority application". 3 "MFR is 4.0g / 10min or more," "Flexural modulus is 1000MPa or more," and "Izod impact strength is 5.0kJ / m 2 "Low priority application" means that the conditions specified in "High priority application" are the most important conditions. Within the above conditions specified in "Low priority application", a method for setting the conditions appropriately according to the characteristics of the product is selected to ensure flexibility when designing products using RP materials. Note that the level of priority application is not uniform but may change depending on the product's usage environment and characteristics. In particular, "Low priority application" can be changed depending on the product's usage environment and characteristics.

[0026] Next, the manufacturing method of this embodiment will be described with reference to the flow chart shown in FIG. 3. In FIG. 3, the material properties of the product to be commercialized, which will be molded from the final RP material, are grasped in advance. First, the material properties of the product to be commercialized are grasped, and the material properties (density, MFR, flexural modulus, Izod impact strength) are grasped in addition to the component analysis (in this case, the component ratio of "PP component, PE component, other components, inorganic filler material") that constitutes the material properties. Hereinafter, this step will be referred to as product property grasping step S1, and abbreviated as "S1" in FIG. 3. Both the component analysis values ​​and the material property values ​​will be collectively referred to as product properties (material properties). Next, the components of the first resin material 41 are analyzed, and furthermore, the material physical properties are measured (Step S2). Hereinafter, this step is referred to as the component analysis / material physical property measurement step S2, and is abbreviated as "S2" in FIG. 3. In this case, the first resin material 41 is melt-kneaded, and in addition to the component analysis of the "PP component, PE component, other components, inorganic filler material" of the first resin material 41, the material physical properties "density, MFR, flexural modulus, Izod impact strength" are measured (Step S2). The material property measurement step of measuring the material properties in Step S2 corresponds to the "first measurement step" in the claims. Next, the results of the component analysis and material properties of the first resin material 41 are compared and verified with the results of the component analysis and material properties grasped in the product characteristic grasping step S1 (step S3). Hereinafter, such a comparison and verification step is referred to as a comparison and verification step S3, and is abbreviated as "S3" in FIG. 3.

[0027] In step S4, the second resin material 42A is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the second resin material 42A is referred to as component analysis and material property measurement step S4, and is abbreviated as "S4" in FIG. 3. In this case, the second resin material 42A alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the second resin material 42A after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. The material property measurement step of measuring the material property of the second resin material 42A in step S4 corresponds to the "second measurement step" in the claims. Note that if there is no plan to use the second resin material 42A, it is not necessary to measure the material property of the second resin material 42A.

[0028] In step S5, the third resin material 42B is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the third resin material 42B is referred to as component analysis and material property measurement step S5, and is abbreviated as "S5" in FIG. 3. In this case, the third resin material 42B alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the third resin material 42B after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. If there is no plan to use the third resin material 42B, it is not necessary to measure the material properties of the resin material 42B. The material property measurement step of measuring the material properties of the third resin material 42B in step S5 corresponds to the "second measurement step" in the claims. In step S6, the fourth resin material 42C is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the fourth resin material 42C is referred to as component analysis and material property measurement step S6, and is abbreviated as "S6" in FIG. 3. In this case, the fourth resin material 42C alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the fourth resin material 42C after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. The material property measurement step of measuring the material property of the fourth resin material 42C in step S6 corresponds to the "second measurement step" in the claims. Note that if there is no plan to use the fourth resin material 42C, it is not necessary to measure the material property of the fourth resin material 42C.

[0029] In step S7, based on the material properties of the first resin material 41 measured in step S2 and the material properties of the second resin material 42A, the third resin material 42B, and the fourth resin material 42C measured in steps S4 to S6, the input amount of the first resin material 41 and the input amount of any one of the second resin material 42A, the third resin material 42B, and the fourth resin material 42C (a mixture of two or more types, if necessary) are calculated. Hereinafter, the step of calculating the input amount is referred to as the input amount calculation step S7, and is abbreviated as "S7" in FIG. 3. The input amount calculation step S7 corresponds to the "calculation step" in the claims. Note that the resin material obtained by melt-kneading and molding any one of the second resin material 42A, the third resin material 42B, and the fourth resin material 42C, the input amount of which is calculated (a mixture of two or more types, if necessary) is referred to as the mixed second to fourth resin materials 44. In this case, if the PE component amount of the first resin material 41, whose component analysis value and material property value are measured in step S6, is higher than the assumed PE component value of the RP material, it is preferable to carry out a process of reducing the input amount of the first resin material 41 from the predetermined assumed input amount and increasing the input amount of the mixed second to fourth resin mixtures 44 from the predetermined assumed input amount. In step S8, both the first resin material 41, the amount of which was calculated in S7, and the mixed second to fourth resin materials 44, the amount of which was calculated in S7, are added, and the first resin material 41 and the mixed second to fourth resin materials 44 are melt-kneaded and molded into a molded product 45 (hereinafter referred to as "molded first to fourth resin materials 45"). The components of the molded product 45 are analyzed, and the material properties are measured (hereinafter this step is referred to as component analysis / material property measurement step S8, and abbreviated as "S8" in FIG. 3). In this case, the "PP component, PE component, other components, In addition to component analysis of the "inorganic filler material," the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. If the inorganic filler component of the material properties (first to fourth molded resin materials 45) after melt-kneading falls within a specific range, there is no need to add additional inorganic filler material 43. (In this case, the specific range is when the content of the inorganic filler component in the RP material after melt-kneading is 16% by weight or less, so if the content exceeds 16% by weight, it will exceed the target (specific range), and there is no need to add additional inorganic filler material 43.)

[0030] In step S9, for the first to fourth molding resin materials 45, the amount of inorganic filler material 43 to be added is calculated so that the material properties after melt-kneading of the RP material are within the target (specific range) product properties (material properties) grasped in S1. Hereinafter, the step of calculating the amount of inorganic filler material 43 to be added is referred to as calculation step S9, and is abbreviated as "S9" in Fig. 3. If the inorganic filler component of the material properties falls within the specific range, it is possible to eliminate the addition of the inorganic filler material 43. The input amount calculation step S9 corresponds to the "input amount calculation step" in the claims. In step S10, the inorganic filler material 43 whose input amount was calculated in S9 and the first to fourth molding resin materials 45 whose input amount was calculated are input, and the inorganic filler material 43 and the first to fourth molding resin materials 45 that are melt-kneaded and molded are molded, and the material properties of the molded product (hereinafter referred to as "final molded body 46") are measured (hereinafter, the step of measuring the component analysis values ​​and material physical property values ​​of the final molded body 46 is referred to as component analysis / material physical property measurement step S10, and abbreviated as "S10" in Figure 3). In this case, in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the final molded body 46, the material physical properties "density, MFR, flexural modulus, Izod impact strength" are measured). In step S11, the results of the component analysis and material properties of the final molded body 46 are compared and verified with the results of the component analysis and material properties ascertained in the product characteristic ascertainment step S1. Hereinafter, such a comparison verification step is referred to as the comparison verification step S11, and is abbreviated as "S11" in Fig. 3. If it is determined as a result of the comparison verification that the components of the material of the final molded body 46 are inappropriate, a step of adjusting the amounts of the inorganic filler material 43 and the first to fourth molded resin materials 45 added is performed. In step S11, if it is determined that the final molded body 46 that is melt-kneaded and molded can achieve the target product characteristics (material characteristics) identified in S1, the process proceeds to the next step S12. In step S12, the process proceeds to a manufacturing process in which products similar to the final molded body 46 are mass-produced.

[0031] The first resin material 41 shown in Table 1 of FIG. 4 is widely distributed on the market, but its flexural modulus is 1000 MPa or less (it does not reach the flexural modulus of 1000 MPa shown in FIG. 5). For this reason, it is difficult to manufacture an RP material using the first resin material 41 alone. On the other hand, the "density, MFR, flexural modulus, and Izod impact strength" shown by the second to fourth resin materials 42A, 42B, and 42C (see Tables 2 to 4 of FIG. 4) reach the levels shown in FIG. 5, and it is understood that an RP material can be manufactured when the second to fourth resin materials 42A, 42B, and 42C are used. However, with regard to the distribution of the second through fourth resin materials 42A, 42B, 42C, the commercial relationships between the companies wishing to purchase RP materials and the sales companies have become closer, and if the distribution amount of the second through fourth resin materials 42A, 42B, 42C decreases, it will be difficult to obtain the desired quantities of the second through fourth resin materials 42A, 42B, 42C from the market when desired. Incidentally, the present inventors have derived from the experimental data and knowledge they have accumulated thus far, a component analysis of the first resin material 41, and the second to fourth resin materials 42A, 42B, 42C, and measurement of the material properties. As a result, it has been found that by adjusting the amounts of the second to fourth resin materials 42A, 42B, 42C added relative to the first resin material 41 and mixing, melting, and kneading them, the PP component of, for example, the molded first to fourth resin materials 45, etc. is increased, the bending elastic modulus value is increased, and the molded final body 46, etc. can be used for commercialization. In particular, the first to fourth resin materials 41, 42A, 42B, 42C were subjected to component analysis and material property measurement, and as a result, it was found that the first to fourth resin materials 41, 42A, 42B, 42C contain at least PP, PE and inorganic filler components, and that the PP content of the second to fourth recycled resin materials 42A, 42B, 42C is greater than the PE content of the first resin material 41, and the PE content of the first resin material 41 is greater than the PE content of the second to fourth resin materials 42A, 42B, 42C. In addition, when it is assumed that the amount of PE in the first resin material 41 is higher than the assumed amount of PE in the RP material after melt-kneading, it has been found that a method of reducing the amount of the first resin material 41 from a predetermined assumed amount and increasing the amount of any one or at least two or more of the second to fourth resin materials 42A, 42B, and 42C mixed and added from a predetermined assumed amount is effective. As a result, although the first resin material 41 alone has a large distribution volume, its applications are limited because its flexural modulus is 1000 MPa or less. However, by adopting a measure of mixing the second to fourth resin materials 42A, 42B, and 42C into the first resin material 41 and appropriately setting the blending ratio, the amount of PE after melt-kneading decreases while the amount of PP increases, and further, the values ​​of the flexural modulus and the like increase, opening up prospects for the applications of the first resin material 41. That is, in the case of a manufacturing method in which the amounts of the second to fourth resin materials 42A, 42B, and 42C added to the first resin material 41 are adjusted and melt-kneaded, it has been found that the characteristics of the first resin material 41 can be improved and it can be effectively used by adding the second to fourth resin materials 42A, 42B, and 42C to the first resin material 41 in the compounding ratios shown in Figures 6 to 11, mixing them, and melt-kneading them. A specific example of this method will be disclosed below with reference to Figures 6 to 11. Figure 12 summarizes the above results of Figures 6 to 11.

[0032] Comparative Examples 1 to 12 and Examples 1 to 5 will be described with reference to Fig. 6 to Fig. 12. Comparative Examples 1 to 12 and Examples 1 to 12 use material 3 for the first resin material 41 in Table 1 of Fig. 4, and material 2 for the second resin material 42A in Table 2 of Fig. 4. However, a material other than material 3 for the first resin material 41 in Table 1 of Fig. 4 may be used, and a material other than material 2 for the second resin material 42A in Table 2 of Fig. 4 may be used. (Comparative Example 1 and Example 1) First, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41 and the second resin material 42A in a situation where sufficient amounts of the third resin material 42B, the fourth resin material 42C and the inorganic filler 43 are not available and only the first resin material 41 and the second resin material 42A are used. In Comparative Example 1 and Example 1, the third resin material 42B, the fourth resin material 42C and the inorganic filler 43 are not used, and a final molded body 46 is formed from the second to fourth resin mixture 44 obtained by melt-kneading the second resin material 42A and the first resin material 41, and the first to fourth resin materials 45 are melt-kneaded. The components (ratios) of Comparative Example 1 are a first resin material 41 (55% by weight) and a second to fourth resin mixture 44 obtained by melt-kneading a second resin material 42A (45% by weight). In contrast, the components (ratios) of Example 1 are a first to fourth resin mixture 45 obtained by melt-kneading a first resin material 41 (50% by weight) and a second to fourth resin mixture 44 obtained by melt-kneading a second resin material 42A (50% by weight). In this case, the first to fourth resin materials 45 become the final molded body 46 because the inorganic filler 43 is not used. The final molded body 46 was subjected to a component analysis and the material properties were measured, and the breakdown was as follows: In Comparative Example 1, the PP component was 66.9% by weight, the PE component was 31.1% by weight, the other resin components were 0.9% by weight, the inorganic filler component was 1.2% by weight, and the material density was 0.94 g / cm 3 , MFR is 8.4g / 10min, flexural modulus is 1100MPa, Izod impact strength is 7.0kJ / m 2 As a result, in Comparative Example 1, the PE component is 31.1% by weight (with background color), which does not satisfy the condition that the PE component is 30% by weight or less, which is a specific range. In order to solve this condition, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixtures 44. That is, in the case of Comparative Example 1, the mixture is the first resin material 41 (55% by weight) and the second resin material 42A (45% by weight), but in Example 1, the mixture is changed to the first resin material 41 (50% by weight) and the second resin material 42A (50% by weight) by changing and adjusting the input amount. This adjustment of the input amount is made based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 1, the PP component was 69.5% by weight, the PE component was 28.5% by weight, the other resin components were 0.9% by weight, the inorganic filler component was 1.1% by weight, and the material density was 0.94 g / cm 3, MFR is 9.4g / 10min, flexural modulus is 1118MPa, Izod impact strength is 7.0kJ / m 2 In this Example 1, the PE content is 28.5% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"), and the condition of "material density is 1.1 g / cm3" which is a specific range ("low priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2 The results of Comparative Example 1 and Example 1 show that even in a situation where the third resin material 42B, the fourth resin material 42C, and the inorganic filler 43 are not available in sufficient quantities, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of second resin material 42A that contains a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, improving the rigidity, impact resistance, and the like of the RP material, and therefore showed that such a method of changing the compounding ratio is effective.

[0033] (Comparative Example 2 and Example 2) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41 and the third resin material 42B in a situation where sufficient amounts of the second resin material 42A, the fourth resin material 42C and the inorganic filler 43 are not available and only the first resin material 41 and the third resin material 42B are used. In Comparative Example 2 and Example 2, the inorganic filler 43, the second resin material 42A, and the fourth resin material 42C are not used, and the first resin material 41 is melt-kneaded with the second to fourth resin mixture 44 formed by melt-kneading the third resin material 42B to form a final molded body 46 of the molded first to fourth resin materials 45. The components (ratios) of Comparative Example 2 are the first resin material 41 (55% by weight) and the second to fourth resin mixture 44 formed by melt-kneading the third resin material 42B (45% by weight). In contrast, the components (ratios) of Example 2 are the material 3 (50% by weight) of the first resin material 41 and the second to fourth resin mixture 44 formed by melt-kneading the third resin material 42B (50% by weight). The final molded body 46 was subjected to a component analysis to measure the material properties, and the breakdown values ​​were as follows: In Comparative Example 2, the PP component was 54.3% by weight, the PE component was 32.0% by weight, the other resin components were 2.9% by weight, the inorganic filler component was 10.9% by weight, and the material density was 1.01 g / cm 3 , MFR is 8.1g / 10min, flexural modulus is 1517MPa, Izod impact strength is 10.8kJ / m 2 As a result, in Comparative Example 2, the PE component is 32.0% by weight (with background color), which does not satisfy the condition that the PE component is 30% by weight or less, which is the specific range. In order to solve this condition, a measure (adjustment of input amount, etc.) is taken to change the ratio between the material 3 of the first resin material 41, the second to fourth resin mixture 44, and the inorganic filler 43. That is, in the case of Comparative Example 2, the composition of the first resin material 41 (55% by weight) and the third resin material 42B (45% by weight) is changed by adjusting the input amount, and in Example 2, the composition of the first resin material 41 (50% by weight) and the third resin material 42B (50% by weight) is changed. This adjustment of the input amount is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 2, the PP component was 55.5% by weight, the PE component was 29.5% by weight, the other resin components were 3.1% by weight, the inorganic filler component was 11.9% by weight, and the material density was 1.01 g / cm 3 , MFR is 9.0g / 10min, flexural modulus is 1581MPa, Izod impact strength is 11.4kJ / m 2 In this Example 2, the PE content is 29.5% by weight, which satisfies the specific range ("high priority application") condition of "PE content is 30% by weight or less." It was also found that the MFR increased from 8.1 g / 10 min to 9.0 g / 10 min, and the flexural modulus increased from 1517 MPa to 1581 MPa. In this case, "Material density is 1.1g / cm3" which is "Priority application low" (specific range) 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 2 and Example 2 show that even in a situation where the second resin material 42A, the fourth resin material 42C, and the inorganic filler 43 are not available in sufficient amounts and the first resin material 41 and the third resin material 42B are used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of third resin material 42B, which contains a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, demonstrating that such a method of changing the compounding ratio is effective.

[0034] (Comparative Example 3 and Example 3) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41 and the fourth resin material 42C in a situation where sufficient amounts of the second resin material 42A, the third resin material 42B and the inorganic filler 43 are not available and only the first resin material 41 and the fourth resin material 42C are used. In Comparative Example 3 and Example 3, the second resin material 42A, the third resin material 42B, and the inorganic filler 43 are not used, and the second to fourth resin mixture 44 obtained by melt-kneading the fourth resin material 42C and the first resin material 41 are melt-kneaded to form a molded final body 46 of the molded first to fourth resin materials 45. The components (ratios) of Comparative Example 3 are made of the material 3 (55% by weight) of the first resin material 41 and the second to fourth resin mixture 44 obtained by melt-kneading the fourth resin material 42C (45% by weight). In contrast, the components (ratios) of Example 3 are made of the first resin material 41 (45% by weight) and the second to fourth resin mixture 44 obtained by melt-kneading the fourth resin material 42C (55% by weight). The final molded body 46 was subjected to a component analysis and the material properties were measured, and the breakdown values ​​were as follows: In Comparative Example 3, the PP component was 63.7% by weight, the PE component was 32.4% by weight (background color), the other resin components were 1.2% by weight, the inorganic filler material components were 2.7% by weight, and the material density was 0.96 g / cm 3 , MFR is 5.9g / 10min, flexural modulus is 1063MPa, Izod impact strength is 6.8kJ / m 2As a result, in Comparative Example 3, the PE component is 32.4% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 3, the mixture is changed from the first resin material 41 (55% by weight) and the fourth resin material 42C (45% by weight) to the first resin material 41 (45% by weight) and the fourth resin material 42C (55% by weight) in Example 3 by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 3, the PP component was 68.3% by weight, the PE component was 27.6% by weight, the other resin components were 1.2% by weight, the inorganic filler component was 2.9% by weight, and the material density was 0.95 g / cm 3 , MFR is 6.8g / 10min, flexural modulus is 1091MPa, Izod impact strength is 6.8kJ / m 2 In this Example 3, the PE content is 27.6% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). It was also found that the MFR increased from 5.9 g / 10 min to 6.8 g / 10 min, and furthermore, the flexural modulus increased from 1063 MPa to 1091 MPa. In this case, the PE content is 27.6% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 3 and Example 3 show that even in a situation where the second resin material 42A, the third resin material 42B, and the inorganic filler 43 are not available in sufficient amounts and the first resin material 41 and the fourth resin material 42C are used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of fourth resin material 42C that contains a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, demonstrating that such a method of changing the compounding ratio is effective.

[0035] (Comparative Example 4 and Example 4) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the second resin material 42A and the inorganic filler 43 in a situation where sufficient amounts of the third resin material 42B and the fourth resin material 42C are not available and only the first resin material 41, the second resin material 42A and the inorganic filler 43 are used. In Comparative Example 4 and Example 4, the third resin material 42B and the fourth resin material 42C are not used, and the second to fourth resin mixture 44 obtained by melt-kneading the second resin material 42A, and the first to fourth resin materials 45 obtained by melt-kneading the first resin material 41 and the inorganic filler 43 are molded into a final molded body 46. The components (ratios) of Comparative Example 4 are the first resin material 41 (55% by weight), the second to fourth resin mixture 44 obtained by melt-kneading the second resin material 42A (35% by weight), and the inorganic filler 43 (10% by weight). In contrast, the components (ratios) of Example 4 are the first resin material 41 (50% by weight), the second to fourth resin mixture 44 obtained by melt-kneading the second resin material 42A (40% by weight), and the inorganic filler 43 (10% by weight). Regarding the final molded body 46 obtained by melt-kneading the first to fourth resin mixtures 45 and the inorganic filler 43, the final molded body 46 was subjected to a component analysis and the material properties were measured, and the breakdown was as follows: In Comparative Example 4, the PP component was 57.3% by weight, the PE component was 30.8% by weight (background color), the other resin components were 0.9% by weight, the inorganic filler component was 11.1% by weight, and the material density was 1.01 g / cm 3, MFR is 6.3g / 10min, flexural modulus is 1495MPa, Izod impact strength is 5.5kJ / m 2 As a result, in Comparative Example 4, the PE component is 30.8% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 4, the mixture is changed from the first resin material 41 (55% by weight) and the second resin material 42A (35% by weight) to the first resin material 41 (50% by weight) and the second resin material 42A (40% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 4, the PP component was 59.9% by weight, the PE component was 28.2% by weight, the other resin components were 0.8% by weight, the inorganic filler component was 11.1% by weight, and the material density was 1.01 g / cm 3 , MFR is 7.2g / 10min, flexural modulus is 1522MPa, Izod impact strength is 5.5kJ / m 2 In this Example 4, the PE content is 28.2% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). It was also found that the MFR increased from 6.3 g / 10 min to 7.2 g / 10 min, and furthermore, the flexural modulus increased from 1495 MPa to 1522 MPa. In this case, the PE content is 28.2% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 4 and Example 4 show that even in a situation where the third resin material 42B and the fourth resin material 42C are not available in sufficient amounts and the first resin material 41, the second resin material 42A and the inorganic filler 43 are used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of second resin material 42A that contains a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, and therefore it was found that such a method of changing the compounding ratio is effective.

[0036] (Comparative Example 5 and Example 5) Next, a manufacturing method for an RP material is disclosed in which, in a situation where sufficient amounts of the second and third resin materials 42A, 42B are not available and only the first resin material 41, the fourth resin material 42C and the inorganic filler 43 are used, the compounding ratio is changed based on component detection of the first resin material 41, the fourth resin material 42C and the inorganic filler 43. In Comparative Example 5 and Example 5, the second and third resin materials 42A and 42B are not used, and the second to fourth resin mixture 44 is formed by melt-kneading the fourth resin material 42C, and the first resin material 41 and the inorganic filler 43 are melt-kneaded to form the first to fourth resin materials 45. The components (ratios) of Comparative Example 5 are the first resin material 41 (55% by weight), the second to fourth resin mixture 44 is formed by melt-kneading the fourth resin material 42C (35% by weight), and the inorganic filler 43 (10% by weight). In contrast, the components (ratios) of Example 5 are the first resin material 41 (50% by weight), the second to fourth resin mixture 44 is formed by melt-kneading the fourth resin material 42C (40% by weight), and the inorganic filler 43 (10% by weight). Regarding the final molded body 46 obtained by melt-kneading the first to fourth resin mixtures 45 and the inorganic filler 43, the final molded body 46 was subjected to a component analysis and the material properties were measured, and the breakdown was as follows: In Comparative Example 5, the PP component was 54.8% by weight, the PE component was 31.8% by weight (background color), the other resin components were 1.1% by weight, the inorganic filler component was 12.3% by weight, and the material density was 1.02 g / cm 3, MFR is 4.7g / 10min, flexural modulus is 1451MPa, Izod impact strength is 5.4kJ / m 2 As a result, in Comparative Example 5, the PE component is 31.8% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 5, the mixture is changed from the first resin material 41 (55% by weight) and the fourth resin material 42C (35% by weight) to the first resin material 41 (50% by weight) and the fourth resin material 42C (40% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 5, the PP component was 57.1% by weight, the PE component was 29.4% by weight, the other resin components were 1.1% by weight, the inorganic filler component was 12.4% by weight, and the material density was 1.02 g / cm 3 , MFR is 5.1g / 10min, flexural modulus is 1472MPa, Izod impact strength is 5.4kJ / m 2 In Example 5, the PE content is 29.4% by weight, which satisfies the specific range (high priority application) condition of "PE content is 30% by weight or less." It was also found that the MFR increased from 4.7 g / 10 min to 5.1 g / 10 min, and the flexural modulus increased from 1451 MPa to 1472 MPa. In this case, "Material density is 1.1g / cm3" which is "Priority application low" (specific range) 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 5 and Example 5 show that even in a situation where the second and third resin materials 42A, 42B are not available in sufficient amounts and only the first resin material 41, the fourth resin material 42C and the inorganic filler 43 are used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 added and increasing the amount of fourth resin material 42C containing a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, demonstrating that such a method of changing the compounding ratio is effective.

[0037] (Comparative Example 6 and Example 6) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the second resin material 42A and the fourth resin material 42C in a situation where sufficient amounts of the third resin material 42B and the inorganic filler 43 are not available and only the first resin material 41, the second resin material 42A and the fourth resin material 42C are used. In Comparative Example 6 and Example 6, the third resin material 42B and the inorganic filler 43 are not used, and the second to fourth resin mixture 44 is obtained by melt-kneading the second resin material 42A and the fourth resin material 42C, and the first resin material 41 is melt-kneaded with the second to fourth resin mixture 45 to form a final molded body 46. The components (ratios) of Comparative Example 6 are the second to fourth resin mixture 44 obtained by melt-kneading the first resin material 41 (55% by weight), the second resin material 42A (25% by weight), and the fourth resin material 42C (20% by weight). On the other hand, the components (ratios) of Example 6 are the first resin material 41 (50% by weight), the second resin material 42A (30% by weight), and the fourth resin material 42C (20% by weight). In this case, the inorganic filler 43 is not used, so the first to fourth resin materials 45 form the final molded body 46. The final molded body 46 was subjected to a component analysis, and the material properties were measured, and the breakdown was as follows: In Comparative Example 6, the PP component was 65.5% by weight, the PE component was 31.7% by weight (background color), the other resin components were 1.0% by weight, the inorganic filler material components were 1.9% by weight, and the material density was 0.95 g / cm 3, MFR is 7.2g / 10min, flexural modulus is 1083MPa, Izod impact strength is 6.9kJ / m 2 As a result, in Comparative Example 6, the PE component is 31.7% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 6, the mixture is changed from the first resin material 41 (55% by weight) and the second resin material 42A (25% by weight) to the first resin material 41 (50% by weight) and the second resin material 42A (30% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 6, the PP component was 68.1% by weight, the PE component was 29.1% by weight, the other resin components were 1.0% by weight, the inorganic filler component was 1.8% by weight, and the material density was 0.95 g / cm 3 , MFR is 8.0g / 10min, flexural modulus is 1101MPa, Izod impact strength is 6.9kJ / m 2 In Example 6, the PE content is 29.1% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). It was also found that the MFR increased from 7.2 g / 10 min to 8.0 g / 10 min, and furthermore, the flexural modulus increased from 1083 MPa to 1101 MPa. In this case, the PE content is 29.1% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2 The condition of "being equal to or greater than" is met. From the results of Comparative Example 6 and Example 6, it can be seen that even in a situation where the third resin material 42B and inorganic filler 43 are not available in sufficient amounts and only the first resin material 41, the second resin material 42A and the fourth resin material 42C are used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of second resin material 42A that contains a large amount of PP components. As a result of this measure, the PE components after melt-kneading decreased while the PP components increased, and numerical values ​​such as the flexural modulus increased, so it was found that such a method of changing the compounding ratio is effective.

[0038] (Comparative Example 7 and Example 7) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the second resin material 42A, the fourth resin material 42C and the inorganic filler 43 in a situation where a sufficient amount of the third resin material 42B is not available and the first resin material 41, the second resin material 42A, the fourth resin material 42C and the inorganic filler 43 are used. In Comparative Example 7 and Example 7, the third resin material 42B is not used, and the second to fourth resin mixture 44 is obtained by melt-kneading the second resin material 42A and the fourth resin material 42C, and the first resin material 41 and the inorganic filler 43 are melt-kneaded to form the first to fourth resin materials 45. The components (ratios) of Comparative Example 7 are the first resin material 41 (55% by weight), the second to fourth resin mixture 44 is obtained by melt-kneading the second resin material 42A (20% by weight) and the fourth resin material 42C (15% by weight), and the inorganic filler 43 (10% by weight). The components (ratios) of Example 7 are the first resin material 41 (50% by weight), the second to fourth resin mixture 44 is obtained by melt-kneading the material 2 of the second resin material 42A (20% by weight) and the fourth resin material 42C (20% by weight), and the inorganic filler 43 (10% by weight). The final molded body 46 (first to fourth resin mixtures 45) obtained by melt-kneading the second to fourth resin mixtures 44 and the inorganic filler 43 (10% by weight) was analyzed for components and the material properties were measured, and the breakdown was as follows: In Comparative Example 7, the PP component was 56.2% by weight, the PE component was 31.2% by weight, the other resin components were 1.0% by weight, the inorganic filler component was 11.6% by weight, and the material density was 1.02 g / cm 3, MFR is 5.6g / 10min, flexural modulus is 1476MPa, Izod impact strength is 5.4kJ / m 2 As a result, in Comparative Example 7, the PE component is 31.2% by weight (with background color), which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this condition, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 7, the mixture is changed from the first resin material 41 (55% by weight) and the fourth resin material 42C (15% by weight) to the first resin material 41 (50% by weight) and the fourth resin material 42C (20% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 7, the PP component was 58.5% by weight, the PE component was 28.8% by weight, the other resin components were 1.0% by weight, the inorganic filler component was 11.7% by weight, and the material density was 1.02 g / cm 3 , MFR is 6.0g / 10min, flexural modulus is 1497MPa, Izod impact strength is 5.5kJ / m 2 In Example 7, the PE content is 28.8% by weight, which satisfies the specific range (high priority application) condition of "PE content is 30% by weight or less." It was also found that the MFR increased from 5.6 g / 10 min to 6.0 g / 10 min, and the flexural modulus increased from 1476 MPa to 1497 MPa. In this case, "Material density is 1.1g / cm3" which is "Priority application low" (specific range) 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 7 and Example 7 show that even in a situation where a sufficient amount of third resin material 42B is not available and first resin material 41, second resin material 42A, fourth resin material 42C and inorganic filler 43 are used, first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of fourth resin material 42C containing a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, demonstrating that such a method of changing the compounding ratio is effective.

[0039] (Comparative Example 8 and Example 8) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41 and the second and third resin materials 42A, 42B in a situation where sufficient amounts of the fourth resin material 42C and inorganic filler 43 are not available and only the first resin material 41 and the second and third resin materials 42A, 42B are used. In Comparative Example 8 and Example 8, the fourth resin material 42C and the inorganic filler 43 are not used, and the second to fourth resin mixture 44, which is obtained by melt-kneading the second and third resin materials 42A and 42B, and the first resin material 41 are melt-kneaded to form the first to fourth resin materials 45, which are the final molded body 46. In this case, the inorganic filler 43 is not used, so the first to fourth resin materials 45 become the final molded body 46. The components (ratios) of Comparative Example 8 are made of the material 3 (55% by weight) of the first resin material 41 and the second to fourth resin mixture 44 (the second resin material 42A (25% by weight) and the third resin material 42B (20% by weight)). The components (ratios) of Example 8 are made of the material 3 (50% by weight) of the first resin material 41 and the second to fourth resin mixture 44 (the second resin material 42A (30% by weight) and the third resin material 42B (20% by weight)). The final molded body 46 was subjected to a component analysis, and the material properties were measured, and the breakdown was as follows: In Comparative Example 8, the PP component was 61.3% by weight, the PE component was 31.5% by weight (background color), the other resin components were 1.8% by weight, the inorganic filler component was 5.5% by weight, and the material density was 0.97 g / cm 3, MFR is 8.2g / 10min, flexural modulus is 1285MPa, Izod impact strength is 8.5kJ / m 2 As a result, in Comparative Example 8, the PE component is 31.5% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 8, the mixture is changed from the first resin material 41 (55% by weight) and the second resin material 42A (25% by weight) to the first resin material 41 (50% by weight) and the second resin material 42A (30% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 8, the PP component was 63.9% by weight, the PE component was 28.9% by weight, the other resin components were 1.8% by weight, the inorganic filler component was 5.4% by weight, and the material density was 0.97 g / cm 3 , MFR is 9.2g / 10min, flexural modulus is 1303MPa, Izod impact strength is 8.5kJ / m 2 In Example 8, the PE content is 28.9% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). It was also found that the MFR increased from 8.2 g / 10 min to 9.2 g / 10 min, and furthermore, the flexural modulus increased from 1285 MPa to 1303 MPa. In this case, the PE content is 28.9% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 8 and Example 8 show that even in a situation where the fourth resin material 42C and inorganic filler 43 are not available in sufficient amounts and the first resin material 41 and the second and third resin materials 42A and 42B are used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of second resin material 42A that contains a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, demonstrating that such a method of changing the compounding ratio is effective.

[0040] (Comparative Example 9 and Example 9) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the third and fourth resin materials 42B, 42C in a situation where sufficient amounts of the second resin material 42A and the inorganic filler 43 are not available and only the first resin material 41, the third and fourth resin materials 42B, 42C are used. In Comparative Example 9 and Example 9, the second resin material 42A and the inorganic filler 43 are not used, and the second to fourth resin mixture 44 obtained by melt-kneading the third and fourth resin materials 42B and 42C is melt-kneaded with the first resin material 41 to form a final molded body 46 of the molded first to fourth resin materials 45. The components (ratios) of Comparative Example 9 are made of the material 3 (55% by weight) of the first resin material 41, the second to fourth resin mixture 44 obtained by melt-kneading the third resin material 42B (20% by weight) and the fourth resin material 42C (25% by weight). In contrast, the components (ratios) of Example 9 are made of the material 3 (50% by weight) of the first resin material 41, the second to fourth resin mixture 44 obtained by melt-kneading the third resin material 42B (20% by weight) and the fourth resin material 42C (30% by weight). The final molded body 46 was subjected to a component analysis, and the material properties were measured, and the breakdown was as follows: In Comparative Example 9, the PP component was 59.5% by weight, the PE component was 32.2% by weight (background color), the other resin components were 2.0% by weight, the inorganic filler component was 6.3% by weight, and the material density was 0.98 g / cm 3 , MFR is 6.8g / 10min, flexural modulus is 1265MPa, Izod impact strength is 8.3kJ / m 2As a result, in Comparative Example 9, the PE component is 32.2% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 9, the mixture is changed from the first resin material 41 (55% by weight) and the fourth resin material 42C (25% by weight) to the first resin material 41 (50% by weight) and the fourth resin material 42C (30% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 9, the PP component was 61.8% by weight, the PE component was 29.8% by weight, the other resin components were 2.0% by weight, the inorganic filler component was 6.4% by weight, and the material density was 0.98 g / cm 3 , MFR is 7.3g / 10min, flexural modulus is 1279MPa, Izod impact strength is 8.3kJ / m 2 In Example 9, the PE content is 29.8% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). It was also found that the MFR increased from 6.8 g / 10 min to 7.3 g / 10 min, and furthermore, the flexural modulus increased from 1265 MPa to 1279 MPa. In this case, the PE content is 29.8% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2 The condition of "being equal to or greater than" is met. From the results of Comparative Example 9 and Example 9, it can be seen that even in a situation where the second resin material 42A and inorganic filler 43 are not available in sufficient amounts and the first resin material 41 and the third and fourth resin materials 42B and 42C are used, by reducing the amount of first resin material 41 added and increasing the amount of fourth resin material 42C containing a large amount of PP components, the first resin material 41 can be effectively used. As a result of this measure, the PE components after melt-kneading decreased while the PP components increased, and numerical values ​​such as the flexural modulus increased, so it was found that such a method of changing the compounding ratio is effective.

[0041] (Comparative Example 10 and Example 10) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first to fourth resin materials 41, 42A, 42B, and 42C in a situation where a sufficient amount of inorganic filler 43 is not available and the first to fourth resin materials 41, 42A, 42B, and 42C are used. In Comparative Example 10 and Example 10, the second to fourth resin materials 42A, 42B, and 42C are all melt-kneaded to form a second to fourth resin mixture 44 without using inorganic filler 43, and the first resin material 41 is melt-kneaded to form a first to fourth resin material 45 to form a final molded body 46. In this case, since inorganic filler 43 is not used, the first to fourth resin materials 45 become the final molded body 46. The components (ratios) of Comparative Example 10 are the second to fourth resin mixture 44, which is melt-kneaded with the first resin material 41 (55% by weight), the second resin mixture 42A (20% by weight), the material 2 of the third resin material 42B (15% by weight), and the fourth resin material 42C (10% by weight). The components (ratios) of Example 10 are material 3 (50% by weight) of the first resin material 41, second resin mixture 42A (25% by weight), third resin material 42B (15% by weight) and fourth resin material 42C (10% by weight) which are melt-kneaded to form second to fourth resin mixture 44. The components of final molded body 46 are analyzed and the material properties are measured, and the breakdown is as follows. That is, in Comparative Example 10, the PP component is 62.0% by weight, the PE component is 31.7% by weight (background color), other resin components are 1.7% by weight, the inorganic filler component is 4.8% by weight, and the material density is 0.97 g / cm. 3, MFR is 7.7g / 10min, flexural modulus is 1231MPa, Izod impact strength is 8.0kJ / m 2 As a result, in Comparative Example 10, the PE component is 31.7% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 10, the mixture is changed from the first resin material 41 (55% by weight) and the second resin material 42A (20% by weight) to the first resin material 41 (50% by weight) and the second resin material 42A (25% by weight) in Example 10 by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 10, the PP component was 64.6% by weight, the PE component was 29.1% by weight, the other resin components were 1.6% by weight, the inorganic filler component was 4.7% by weight, and the material density was 0.96 g / cm 3 , MFR is 8.5g / 10min, flexural modulus is 1248MPa, Izod impact strength is 8.1kJ / m 2 In Example 10, the PE content is 29.1% by weight, which satisfies the specific range (high priority application) condition of "PE content is 30% by weight or less." It was found that the MFR increased from 7.7 g / 10 min to 8.5 g / 10 min, and further, the flexural modulus increased from 1231 MPa to 1248 MPa. In this case, "Material density is 1.1g / cm3" which is "Priority application low" (specific range) 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 10 and Example 10 show that even in a situation where a sufficient amount of inorganic filler 43 is not available and first resin material 41 and fourth resin materials 42A, 42B, and 42C are used, first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 added and increasing the amount of second resin material 42A containing a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of the flexural modulus and the like, demonstrating that such a method of changing the compounding ratio is effective.

[0042] (Comparative Example 11 and Example 11) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the third resin material 42B and the inorganic filler 43 in a situation where sufficient amounts of the second resin material 42A and the fourth resin material 42C are not available and the first resin material 41, the third resin material 42B and the inorganic filler 43 are used. In Comparative Example 11 and Example 11, the second to fourth resin mixture 44 is melt-kneaded using the third resin material 42B without using the second resin material 42A and the fourth resin material 42C, and the first to fourth resin materials 45 are melt-kneaded with the first resin material 41 and the inorganic filler 43 to form a final molded body 46. The components (ratios) of Comparative Example 11 are the second to fourth resin mixture 44 melt-kneaded with the first resin material 41 (55% by weight) and the third resin material 42B (40% by weight), and the inorganic filler 43 (5% by weight). In contrast, the components (ratios) of Example 11 are the second to fourth resin mixture 44 melt-kneaded with the first resin material 41 (50% by weight) and the third resin material 42B (45% by weight), and the inorganic filler 43 (5% by weight). Regarding the final molded body 46 obtained by melt-kneading the first to fourth resin mixtures 45 and the inorganic filler 43, the components were analyzed and the material properties were measured, and the breakdown was as follows: In Comparative Example 11, the PP component was 50.9% by weight, the PE component was 31.7% by weight (background color), the other resin components were 2.7% by weight, the inorganic filler component was 14.8% by weight, and the material density was 1.04 g / cm 3 , MFR is 6.9g / 10min, flexural modulus is 1670MPa, Izod impact strength is 9.2kJ / m2 As a result, in Comparative Example 11, the PE component is 31.7% by weight, which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this situation, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 11, the mixture was the first resin material 41 (55% by weight) and the third resin material 42B (40% by weight), but in Example 11, the mixture is changed to the first resin material 41 (50% by weight) and the third resin material 42B (45% by weight) by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 11, the PP component was 52.1% by weight, the PE component was 29.3% by weight, the other resin components were 2.9% by weight, the inorganic filler component was 15.8% by weight, and the material density was 1.04 g / cm 3、 MFR is 7.8g / 10min, flexural modulus is 1747MPa, Izod impact strength is 9.8kJ / m 2 In Example 11, the PE content is 29.3% by weight, which satisfies the specific range (high priority application) condition of "PE content is 30% by weight or less." It was also found that the MFR increased from 6.9 g / 10 min to 7.8 g / 10 min, and the flexural modulus increased from 1670 MPa to 1747 MPa. In this case, the "low priority application" (specific range) "material density is 1.1 g / cm 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 11 and Example 11 show that even in a situation where second resin material 42A and fourth resin material 42C are not sufficiently available, first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 input and increasing the amount of third resin material 42B, which contains a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, and thus increased the values ​​of bending elastic modulus, etc., demonstrating that such a method of changing the compounding ratio is effective.

[0043] (Comparative Example 12 and Example 12) Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first to fourth resin materials 41, 42A, 42B, 42C and the inorganic filler 43 while all of the first resin material 41, the second resin material 42A, the third resin material 42B, the fourth resin material 42C and the inorganic filler 43 are utilized. In Comparative Example 12 and Example 12, a final molded body 46 is formed from a second to fourth resin mixture 44 obtained by melt-kneading all of the second to fourth resin materials 42A, 42B, and 42C, a first resin material 41, and a molded first to fourth resin materials 45 obtained by melt-kneading the first resin material 41 and an inorganic filler 43. In Comparative Example 12 and Example 12, a final molded body 46 is formed from a second to fourth resin mixture 44 obtained by melt-kneading all of the second to fourth resin materials 42A, 42B, and 42C, and a first resin material 41 and an inorganic filler 43. The components (ratios) of Comparative Example 12 are a first resin material 41 (55% by weight), a second resin material 42A (20% by weight), a third resin material 42B (10% by weight), and a fourth resin material 42C (10% by weight) melted and kneaded to form a second to fourth resin mixture 44, and an inorganic filler 43 (5% by weight). In contrast, the components (ratios) of Example 12 are a first resin material 41 (50% by weight), a second resin material 42A (20% by weight), a third resin material 42B (10% by weight), and a fourth resin material 42C (15% by weight) melted and kneaded to form a second to fourth resin mixture 44, and an inorganic filler 43 (5% by weight). Regarding the final molded body 46 obtained by melt-kneading the first to fourth resin mixtures 45 and the inorganic filler 43, the final molded body 46 was subjected to a component analysis and the material properties were measured, and the breakdown was as follows: In Comparative Example 12, the PP component was 58.6% by weight, the PE component was 31.4% by weight, the other resin components were 1.4% by weight, the inorganic filler component was 8.7% by weight, and the material density was 0.99 g / cm 3 , MFR is 6.6g / 10min, flexural modulus is 1330MPa, Izod impact strength is 6.8kJ / m 2 As a result, in Comparative Example 12, the PE component is 31.4% by weight (with background color), which does not satisfy the condition of "PE component is 30% by weight or less" which is a specific range ("high priority application"). In order to solve this condition, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second to fourth resin mixture 44. That is, in the case of Comparative Example 12, the mixture of the first resin material 41 (55% by weight) and the fourth resin material 42C (10% by weight) is changed to the mixture of the first resin material 41 (50% by weight) and the fourth resin material 42C (15% by weight) in Example 12 by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, assuming that it is derived from accumulated experimental data, knowledge, etc. As a result, in Example 12, the PP component was 60.9% by weight, the PE component was 29.0% by weight, the other resin components were 1.4% by weight, the inorganic filler component was 8.8% by weight, and the material density was 0.99 g / cm 3 , MFR is 7.1g / 10min, flexural modulus is 1347MPa, Izod impact strength is 6.8kJ / m 2 In Example 12, the PE content is 29.0% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). It was also found that the MFR increased from 6.6 g / 10 min to 7.1 g / 10 min, and furthermore, the flexural modulus increased from 1330 MPa to 1347 MPa. In this case, the PE content is 29.0% by weight, which satisfies the condition of "PE content is 30% by weight or less" which is a specific range ("high priority application"). 3 MFR is 4.0g / 10min or more, flexural modulus is 1000MPa or more, Izod impact strength is 5.0kJ / m 2The results of Comparative Example 12 and Example 12 show that even in a situation where the first resin material 41, the second to fourth resin materials 42A, 42B, 42C, and the inorganic filler 43 can all be used, the first resin material 41 can be effectively utilized by reducing the amount of first resin material 41 added and increasing the amount of fourth resin material 42C containing a large amount of PP components. This approach reduced the amount of PE components after melt-kneading while increasing the amount of PP components, improving the rigidity, impact resistance, and the like of the RP material, demonstrating that the method of changing the compounding ratio based on component detection is effective. When examining this situation, as is clear from Comparative Examples 1 to 12 and Examples 1 to 12, the MFR value of the first resin material 41 is 4.0 g / 10 min or less, while the MFRs of the second to fourth resin materials 42A, 42B, 42C are higher than that of the first resin material 41, and the MFR value of the resin material obtained by kneading and melting the first resin material 41 with the second to fourth resin materials 42A, 42B, 42C is 4.0 g / 10 min or more. This shows that the material properties, including the flexural modulus and Izod impact strength, of the resin material obtained by melt-kneading the second to fourth resin materials 42A, 42B, 42C with the first resin material 41 are greatly improved compared to the first resin material 41. FIG. 12 summarizes the results of FIGS. 6 to 11, and shows that a method of reducing the amount of first resin material 41 added below a predetermined expected amount, while increasing the amount of any one or a mixture of at least two or more of second to fourth resin materials 42A, 42B, 42C added above the predetermined expected amount, is effective.

[0044] As described above in detail, according to the invention of the manufacturing method of this embodiment, the RP material of this embodiment includes the following components: (1) a first measurement step (S2) for measuring the material properties of a first resin material 41 obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, (2) a second resin material 42A obtained from an RP material not subject to the Container and Packaging Recycling Law but to which the Home Appliance Recycling Law applies, (3) a third resin material 42B obtained from an RP material not subject to the Container and Packaging Recycling Law but to which the Automobile Recycling Law applies, and (4) a fourth resin material 42C obtained from a general RP material not subject to the Container and Packaging Recycling Law and not subject to either the Home Appliance Recycling Law or the Automobile Recycling Law. The method includes a second measurement step (S4 to S6) for measuring material properties, a calculation step (S7) for calculating the input amount of the first resin material 41 and the input amounts of the second to fourth resin materials 42A, 42B, 42C for the first resin material 41 and the second to fourth resin materials 42A, 42B, 42C measured in the first and second measurement steps, and an input amount calculation step (S9) for determining the input amount of inorganic filler material 43 based on the calculated input amounts for the first resin material 41 and the second to fourth resin materials 42A, 42B, 42C so that the material properties after melting and kneading of the RP material are within a specific range. In the case of the manufacturing method of the RP material of this embodiment, the flexural modulus of the RP material increases by mixing the second to fourth resin materials 42A, 42B, and 42C into the first resin material 41 and melting and kneading them, and the melted and kneaded resin material (final molded body 46) can be used alone. As a result, as described in Non-Patent Document 1 ("Use of Waste Plastics in 2020"), the first resin material 41 has a large circulation volume but cannot be effectively utilized, and the first resin material 41 alone has limited uses. However, by mixing the second to fourth resin materials 42A, 42B, and 42C into the first resin material 41 and melting and kneading them, the material properties (flexural modulus value, etc.) of the material increase, improving the limited uses. As a result, the first resin material 41, which has a large circulation volume, can be used in a more environmentally friendly manner than before, and the use of RP materials to which the Container Recycling Law is applied can be effectively promoted. That is, the second to fourth resin materials 42A, 42B, and 42C have superior physical properties compared to the first resin material 41, and the second to fourth resin materials 42A, 42B, and 42C can be recycled by themselves, whereas the first resin material 41, which has a large inflow, is currently difficult to recycle by itself. In addition, among the second to fourth resin materials 42A, 42B, and 42C, the resin materials derived from the Automobile Recycling Law and the Home Appliance Recycling Law, in particular, are less distributed than the first resin material 41. Furthermore, in terms of business between purchasing companies and sales companies of RP materials, Under the current circumstances in which the first resin material 41 is strongly bound to the second resin material 42A, 42B, and 42C and difficult to obtain from the distribution market, and recycling is therefore difficult to advance, by mixing an appropriate amount of the second to fourth resin materials 42A, 42B, and 42C with the first resin material 41 and melting and kneading the mixture, the melted and kneaded resin material has superior physical properties compared to those of the first resin material 41, opening the way for recycling. Therefore, there is a high possibility that recycling will progress significantly for the first resin material 41, which has a large inflow volume. In general, it can be said that the overall progress in recycling will have an extremely large effect on industry.

[0045] The RP material of this embodiment includes the following components (1) to (4): (1) a first resin material 41 obtained from used plastic containers and packaging to which the Container Recycling Law applies, (2) a second resin material 42A obtained from an RP material not subject to the Container Recycling Law but to which the Home Appliance Recycling Law applies, (3) a third resin material 42B obtained from an RP material not subject to the Container Recycling Law but to which the Automobile Recycling Law applies, and (4) a fourth resin material 42C obtained from a general RP material not subject to the Container Recycling Law and not subject to either the Home Appliance Recycling Law or the Automobile Recycling Law, and is formed by adding a mixture of any one or at least two or more of the second to fourth resin materials 42A, 42B, and 42C and the first resin material 41, melting and kneading them. In the case of the RP material of this embodiment, the first resin material 41 alone has limited uses, whereas in the case of a molded final body 46 in which the second to fourth resin materials 42A, 42B, and 42C are mixed into the first resin material 41 and melt-kneaded, the values ​​of the flexural modulus and the like increase, and the melt-kneaded resin material can be used in a wide range of applications, unlike the case of the first resin material 41 alone. As a result, the first resin material 41, which is widely distributed, can be used in an environmentally friendly manner, and the use of RP materials to which the Containers and Packaging Recycling Law applies can be effectively promoted. In this embodiment, a method of adjusting the input amount is adopted in which one or more of the second to fourth resin materials 42A, 42B, and 42C are used in combination with the first resin material 41 to adjust the input amount. However, it is not necessary to adopt the input amount adjustment method, and a method of setting an appropriate mixing ratio from the beginning may be adopted. The second to fourth resin materials 42A, 42B, 42C that are added to improve the physical properties of the first resin material 41 may be virgin materials other than recycled materials, or the second to fourth resin materials 42A, 42B, 42C that have not yet been released to the market may be used.

[0046] The following supplementary notes are provided. Supplementary note 1 is as follows: A first measurement step measures the material properties of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and a second measurement step measures the material properties of a second recycled resin material (which may contain an inorganic filler component) obtained from used plastics not subject to the Container and Packaging Recycling Law and to which the Home Appliance Recycling Law applies, or a third recycled resin material (which may contain an inorganic filler component) obtained from used plastics to which the Automobile Recycling Law applies, or a fourth recycled resin material (which may contain an inorganic filler component) obtained from used plastics not subject to the Container and Packaging Recycling Law and to which neither the Home Appliance Recycling Law nor the Automobile Recycling Law applies The method is characterized by having a second measurement step of calculating an input amount of the first recycled resin material and an input amount of a mixture of any one or at least two or more of the second to fourth recycled resin materials (which may contain an inorganic filler component) based on the material properties of the first recycled resin material and the second to fourth recycled resin materials measured in the first measurement step and the second measurement step; and an input amount calculation step of calculating an input amount of a new inorganic filler material based on the calculated input amounts of the first recycled resin material and the mixture of any one or at least two or more of the second to fourth recycled resin materials (which may contain an inorganic filler component) so that the material properties of the recycled plastic material after melt-kneading are within a specific range. Supplementary Note 2 is as follows: That is, in the manufacturing method of the recycled plastic material described in Supplementary Note 1, in the input amount calculation step, when the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range, the input of new inorganic filler material is eliminated. Supplementary Note 3 is as follows: That is, in the manufacturing method of the recycled plastic material described in Supplementary Note 1 or 2, when the material properties of the recycled plastic after molding are set to a specific range, a high or low priority application order is set, and the "high priority application" specifies that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and the "low priority application" includes at least that the MFR is 4.0 g / 10 min or more. Supplementary Note 4 is as follows: That is, in the method for producing a recycled plastic material according to any one of Supplementary Note 1 to 3, the first to fourth recycled resin materials all contain at least polypropylene and polyethylene, and the second to fourth recycled resin materials are selected so that the polypropylene content of the second to fourth recycled resin materials is greater than the polypropylene content of the first recycled resin material, and the polyethylene content of the first recycled resin material is greater than the polyethylene content of the second to fourth recycled resin materials. Supplementary Note 5 is as follows: That is, in the manufacturing method of the recycled plastic material according to any one of Supplementary Note 1 to 4, when it is expected that the content of polyethylene in the first recycled resin material is higher than the expected content value of polyethylene in the recycled plastic material, the method is characterized by comprising an input amount adjustment step of reducing the input amount of the first recycled resin material below a predetermined expected input amount and increasing the input amount of any one type or a mixture of at least two types of the second to fourth recycled resin materials above the predetermined expected input amount. Supplementary Note 6 is as follows: That is, the present invention is characterized in that a first recycled resin material obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, a second recycled resin material obtained from used plastics not subject to the Container and Packaging Recycling Law and to which the Home Appliance Recycling Law applies, a third recycled resin material obtained from used plastics not subject to the Container and Packaging Recycling Law and to which the Automobile Recycling Law applies, a fourth recycled resin material obtained from used plastics not subject to the Container and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law, and a mixture of one or at least two of the second to fourth recycled resin materials are added to the first recycled resin material, melted and kneaded to form the product. Supplementary Note 7 is as follows: That is, in the recycled plastic material described in Supplementary Note 6, the molded recycled plastic material contains at least polypropylene, polyethylene, and an inorganic filler, and is characterized in that the polypropylene content is greater than the polyethylene content, and the polyethylene content is adjusted and blended to be 30% by weight or less based on the total weight of the recycled plastic material. Supplementary Note 8 is as follows: In other words, in the recycled plastic materials described in Supplementary Notes 6 and 7, any one or a mixture of at least two or more of the second to fourth recycled resin materials is characterized by having a higher MFR value than the first recycled resin material. Supplementary Note 9 is as follows: That is, in the recycled plastic material according to any one of Supplementary Note 6 to 8, the recycled plastic material after molding has an MFR value of 4.0 g / 10 min or more. [Explanation of symbols]

[0047] 41 First recycled resin material (first resin material) 42A Second resin material (derived from recycled home appliance materials) 42B Third resin material (derived from recycled automobile materials) 42C 4th resin material (derived from general recycled materials) 43 Inorganic filler materials S2 First measurement step S4 to S6 Second measurement step S7 Calculation step S9 Input amount calculation step

Claims

1. A first measurement step of measuring material properties of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; a second measurement step of measuring material properties of the second to fourth recycled resin materials with respect to a second recycled resin material (which may contain an inorganic filler component) obtained from used plastics to which the Container and Packaging Recycling Law is not applied and the Home Appliance Recycling Law is applied, or a third recycled resin material (which may contain an inorganic filler component) obtained from used plastics to which the Automobile Recycling Law is applied, or a fourth recycled resin material (which may contain an inorganic filler component) obtained from used plastics to which the Container and Packaging Recycling Law is not applied and to which neither the Home Appliance Recycling Law nor the Automobile Recycling Law is applied; a calculation step of calculating an input amount of the first recycled resin material and an input amount of a mixture of at least one of the second to fourth recycled resin materials (which may contain an inorganic filler component) based on the material properties of the first recycled resin material and the second to fourth recycled resin materials measured in the first measurement step and the second measurement step; a step of calculating an input amount of new inorganic filler material based on the calculated input amounts of the first recycled resin material and any one or a mixture of at least two or more of the second to fourth recycled resin materials (which may contain inorganic filler components) so that the material properties of the recycled plastic material after melt-kneading are within a specific range.

2. 2. The method for producing recycled plastic materials according to claim 1, characterized in that, in the input amount calculation step, if the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range, the input of new inorganic filler material is stopped.

3. 3. The method for producing recycled plastic material according to claim 1 or 2, characterized in that, when the material properties of the recycled plastic after molding are within a specific range, a high or low priority application order is set, in which a "high priority application" is set so that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and a "low priority application" includes at least an MFR of 4.0 g / 10 min or more.

4. A method for producing recycled plastic materials as described in claim 1 or 2, characterized in that all of the first to fourth recycled resin materials contain at least polypropylene and polyethylene, the polypropylene content of the second to fourth recycled resin materials is greater than the polypropylene content of the first recycled resin material, and the polyethylene content of the first recycled resin material is greater than the polyethylene content of the second to fourth recycled resin materials.

5. A method for producing recycled plastic materials as described in claim 1 or 2, characterized in that when it is expected that the amount of polyethylene contained in the first recycled resin material is higher than the assumed polyethylene content value of the recycled plastic material, the method includes an input amount adjustment step of reducing the amount of the first recycled resin material added below a predetermined assumed input amount and increasing the amount of any one or a mixture of at least two or more of the second to fourth recycled resin materials added above the predetermined assumed input amount.

6. A first recycled resin material (which may contain inorganic filler components) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; A second recycled resin material (which may contain inorganic filler components) obtained from used plastics that are not subject to the Container and Packaging Recycling Law but are subject to the Home Appliance Recycling Law; A third recycled resin material (which may contain inorganic filler components) obtained from used plastics that are not subject to the Container and Packaging Recycling Law and are subject to the Automobile Recycling Law; A fourth recycled resin material (which may contain inorganic filler components) obtained from used plastics to which none of the Container and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law apply; A recycled plastic material characterized in that a mixture of at least one or more of the second to fourth recycled resin materials (which may contain an inorganic filler component) and the first recycled resin material (which may contain an inorganic filler component) are added, melted, kneaded, and molded.

7. The recycled plastic material according to claim 6, characterized in that the molded recycled plastic material contains at least polypropylene, polyethylene, and an inorganic filler, and the polypropylene content is greater than the polyethylene content and the polyethylene content is adjusted to be 30% by weight or less based on the total weight of the recycled plastic material.

8. The recycled plastic material according to claim 6 or 7, characterized in that any one or a mixture of at least two or more of the second to fourth recycled resin materials has a higher MFR value than the first recycled resin material.

9. 8. The recycled plastic material according to claim 6, wherein the MFR value of the recycled plastic material after molding is 4.0 g / 10 min or more.

Citation Information

Patent Citations

  • Polypropylene-based resin composition and molded product therefrom

    JP2005232413A

  • Resin composition for vehicular interior using crushed material of vehicular bumper mixed with insoluble substance as raw material, and molding thereof

    JP2009173947A

  • PP compounds that retain excellent mechanical properties and exhibit improved or non-appearing tiger stripes.

    JP2015537087A

  • Resin composition for seamless air bag covers, and seamless air bag covers or seamless instrument panels with air bag covers, made by using the composition

    WO2006040825A1