Olefin polymerization catalyst, olefin polymer production method, and transition metal compound
A transition metal compound with a specific ligand structure addresses the narrow molecular weight distribution issue in existing olefin polymerization catalysts, producing polymers with broadened distributions and improved properties.
Patent Information
- Application Number
- JP2023198370
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2023-11-22
- Publication Date
- 2024-10-03
AI Technical Summary
Existing olefin polymerization catalysts using metallocene compounds produce polymers with relatively narrow molecular weight distributions, failing to meet market demands for broader distributions, particularly in high molecular weight components.
A transition metal compound with a specific ligand structure, represented by general formula (A-1), is used to create an olefin polymerization catalyst that expands molecular weight distribution, achieving bimodal distributions and unique properties in polymers.
The catalyst produces olefin polymers with broadened molecular weight distributions, enhancing melt fluidity and physical properties, suitable for various resin and elastomer applications.
Smart Images

Figure 2024134505000001 
Figure 2024134505000002 
Figure 2024134505000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel olefin polymerization catalyst using a transition metal complex compound, a method for polymerizing olefins, and a novel transition metal compound. In particular, the present invention is characterized by a transition metal compound having a structure in which multiple ligand sites are linked by specific substituents. [Background technology]
[0002] Catalysts consisting of metallocene compounds and cocatalysts such as organoaluminum oxy compounds are known as catalysts for producing olefin polymers such as ethylene-α-olefin copolymers and propylene polymers.
[0003] As such catalysts, for example, metallocene compounds containing a ligand having a structure in which multiple indenyl skeletons or skeletons obtained by partially hydrogenating the indenyl skeletons are crosslinked with relatively compact substituents, and polymerization catalysts and methods for producing olefin polymers using the same have been reported (e.g., Patent Document 1).
[0004] A polymerization catalyst in which such a metallocene compound is combined with one or more compounds selected from the group consisting of organoaluminum oxy compounds and organoboron compounds can produce homopolymers or copolymers of ethylene or α-olefins having 3 to 20 carbon atoms. Moreover, the obtained polymers tend to often have a relatively narrow molecular weight distribution.
[0005] On the other hand, Patent Document 2 discloses a metallocene compound having a structure in which a crosslinking group is bonded to a specific position of an indenyl skeleton, and an olefin polymerization catalyst using the same. Furthermore, Non-Patent Document 1 discloses organic synthesis reactions using various zirconium complex compounds. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] European Patent Publication No. 783022 [Patent Document 2] European Patent Publication No. 1059300 [Non-patent literature]
[0007] [Non-Patent Document 1] Dalton Trans. 2021, 50, 15802-25820 Summary of the Invention [Problem to be solved by the invention]
[0008] Olefin polymerization catalysts containing metallocene compounds have unique properties such as a tendency to give olefin polymers with relatively narrow molecular weight distributions and stereoregularity distributions, and olefin copolymers with relatively narrow composition distributions, but the market demands olefin polymers with higher performance.
[0009] For example, in terms of the melt flowability and rigidity of the resulting polymer, a broad molecular weight distribution may be preferable. Attempts have been made to obtain a wide molecular weight distribution olefin polymer by multi-stage polymerization using the above-mentioned olefin polymerization catalyst, but it seems that it may be difficult to produce a wide molecular weight distribution olefin polymer containing a polymer component with a particularly high molecular weight (Mz / Mw may be an index of this).
[0010] In view of the above, the present invention has been made with the objective of providing a transition metal compound capable of becoming an olefin polymerization catalyst having unprecedented characteristics, an olefin polymerization catalyst containing the same, and a process for producing an olefin polymer. [Means for solving the problem]
[0011] As a result of investigations conducted in consideration of the above-mentioned problems, the present inventors have found that a metallocene compound having a ligand with a specific structure can produce an olefin polymer having a molecular weight distribution that is not conceivable with the use of a conventional olefin polymerization catalyst containing a metallocene compound, and have completed the present invention. That is, the present invention has the following configuration.
[0012] [1] (A) a transition metal compound represented by the following general formula (A-1),
[0013] [ka]
[0014] [In the formula (A-1), R 1 is a substituent having two or more independent ring structures, R 2 , R 2' , R 3 , and R 3' each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 4 and R 5 each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group, or a nitrogen-containing group, M is a metal atom of Group 4 of the periodic table. (B) (B-1) Organometallic compound, (B-2) an organoaluminum oxy compound, and (B-3) A compound that reacts with the transition metal compound to form an ion pair At least one compound selected from the group consisting of A catalyst for olefin polymerization comprising:
[0015] [2] R 1is a substituent selected from a biphenyl group and a substituted biphenyl group.
[0016] [3] R 4 and R 5 is a halogen atom.
[0017] [4] The olefin polymerization catalyst according to any one of [1] to [3], wherein M is a transition metal atom selected from titanium, zirconium, and hafnium.
[0018] [5] A method for producing an olefin polymer, comprising polymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of [1] to [4].
[0019] [6] The method for producing an olefin polymer according to [5], wherein the olefin is selected from olefins having 2 to 30 carbon atoms.
[0020] [7] The method for producing an olefin polymer according to [5], wherein the olefin is selected from ethylene, propylene, or 1-butene.
[0021] [8] A transition metal compound represented by the following general formula (A-2):
[0022] [ka]
[0023] [In the formula (A-2), R 1 is a substituent having two or more independent ring structures, R 2 , R 2' , R 3 , and R 3'each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 4 and R 5 each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group, or a nitrogen-containing group, M' is a transition metal atom selected from titanium and hafnium. Effect of the Invention
[0024] According to the present invention, when a specific transition metal compound is used as a catalyst in the polymerization or copolymerization of ethylene or an olefin having 3 or more carbon atoms, an olefin polymer can be produced that has a tendency for the molecular weight distribution to be broadened even on the high molecular weight side (high Mz / Mw value). In addition, the olefin polymer may show a bimodal molecular weight distribution in GPC measurement. Such an olefin polymer may show unique properties in terms of melt flowability and various physical properties as a resin or elastomer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The olefin polymerization catalyst according to the present invention is characterized by containing (A) a specific transition metal compound and (B) a specific compound such as one containing an element of Group 13 of the periodic table. First, each of the above components will be described below.
[0026] [Transition metal compound (A)] The transition metal compound (A) used in the olefin polymerization catalyst of the present invention is represented by the following general formula (A-1) and is specified by satisfying the following requirements.
[0027] [ka]
[0028] [In the formula (A-1), R1 is a substituent having two or more independent ring structures, R 2 , R 2' , R 3 , and R 3' each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 4 and R 5 each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group, or a nitrogen-containing group, M is a metal atom in Group 4 of the periodic table.
[0029] (R 1 ) R 1 is a structure in which groups having a cyclic structure, preferably a 4- to 10-membered ring, such as a phenyl group, a cyclohexyl group, a cyclopentyl group, a cyclobutyl group, or a cycloheptyl group, are linked by a covalent bond, a hydrocarbon group, an oxygen atom (-O-: the preceding - indicates a covalent bond), or a nitrogen atom-containing group. Specifically, examples of groups having a structure in which cyclic structures are directly linked include a biphenyl group, a substituted biphenyl group, a bicyclohexyl group, a substituted bicyclohexyl group, a bicyclopentyl group, a substituted bicyclopentyl group, a bicyclobutyl group, a substituted bicyclobutyl group, a bicycloheptyl group, a substituted bicycloheptyl group, a bicyclooctyl group, and a bicyclooctyl group. In addition, examples include groups having a structure in which cyclic structures are linked via a hydrocarbon group such as a bisphenylmethylene group.
[0030] Among these, a relatively rigid structure is often preferred, and as a group having such a structure, a biphenyl group and a substituted biphenyl group are preferred. As the substituent of the substituted biphenyl group, R 2 , R 2' , R 3 , R 3' The same substituents as those mentioned above can be mentioned.
[0031] (R 2 , R 2' , R 3 , R 3' ) R 2 , R 2' , R 3 , and R 3' are each independently a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group.
[0032] R 2 , R 2' , R 3 , and R 3' are preferably each independently a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, a sulfur-containing group, or a phosphorus-containing group. 2 , R 2' , R 3 , and R 3' are groups which include the case where a plurality of each is present, and they can be bonded to each other to form a ring structure.
[0033] Examples of the hydrocarbon group having 1 to 20 carbon atoms include an alkyl group having 1 to 20 carbon atoms, a cyclic saturated hydrocarbon group having 3 to 20 carbon atoms, a linear unsaturated hydrocarbon group having 2 to 20 carbon atoms, and a cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms.
[0034] Examples of the alkyl group having 1 to 20 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decanyl; and branched saturated hydrocarbon groups such as isopropyl, isobutyl, s-butyl, t-butyl, t-amyl, neopentyl, 3-methylpentyl, 1,1-diethylpropyl, 1,1-dimethylbutyl, 1-methyl-1-propylbutyl, 1,1-dipropylbutyl, 1,1-dimethyl-2-methylpropyl, 1-methyl-1-isopropyl-2-methylpropyl, and cyclopropylmethyl. The number of carbon atoms in the alkyl group is preferably 1 to 6.
[0035] Examples of cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, norbornyl, 1-adamantyl, and 2-adamantyl groups, and groups in which the hydrogen atoms of these cyclic saturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 17 carbon atoms, such as 3-methylcyclopentyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 4-cyclohexylcyclohexyl, and 4-phenylcyclohexyl groups. The number of carbon atoms in the cyclic saturated hydrocarbon group is preferably 5 to 11.
[0036] Examples of the linear unsaturated hydrocarbon group having 2 to 20 carbon atoms include alkenyl groups such as ethenyl group (vinyl group), 1-propenyl group, 2-propenyl group (allyl group), 1-methylethenyl group (isopropenyl group), etc.; and alkynyl groups such as ethynyl group, 1-propynyl group, 2-propynyl group (propargyl group), etc. The number of carbon atoms in the linear unsaturated hydrocarbon group is preferably 2 to 4.
[0037] Examples of cyclic unsaturated hydrocarbon groups having 3 to 20 carbon atoms include cyclopentadienyl, norbornenyl, phenyl, naphthyl, indenyl, azulenyl, phenanthryl, and anthracenyl groups; groups in which hydrogen atoms of these cyclic unsaturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 15 carbon atoms, such as 3-methylphenyl (m-tolyl), 4-methylphenyl (p-tolyl), 4-ethylphenyl, 4-t-butylphenyl, 4-cyclohexylphenyl, biphenylyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, and 2,4,6-trimethylphenyl (mesityl); groups in which hydrogen atoms of a linear hydrocarbon group or a branched saturated hydrocarbon group are replaced with a cyclic saturated hydrocarbon group or a cyclic unsaturated hydrocarbon group having 3 to 19 carbon atoms, such as a benzyl group or a cumyl group. The number of carbon atoms of the cyclic unsaturated hydrocarbon group is preferably 6 to 10.
[0038] Examples of the silicon-containing group include alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and triisopropylsilyl group, which are groups in which carbon atoms in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms are replaced with silicon atoms; arylsilyl groups such as dimethylphenylsilyl group, methyldiphenylsilyl group, and t-butyldiphenylsilyl group; pentamethyldisilanyl group, trimethylsilylmethyl group, etc. The number of carbon atoms in the alkylsilyl group is preferably 1 to 10, and the number of carbon atoms in the arylsilyl group is preferably 6 to 18.
[0039] Examples of the nitrogen-containing group include an amino group, a nitro group, an N-morpholinyl group, and a group in which the =CH- structural unit in the aforementioned hydrocarbon group having 1 to 20 carbon atoms or silicon-containing group is replaced with a nitrogen atom, a group in which the -CH2- structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, or a group in which the -CH3 structural unit is replaced with a nitrogen atom or a nitrile group to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, such as a dimethylamino group, a diethylamino group, a dimethylaminomethyl group, a cyano group, a pyrrolidinyl group, a piperidinyl group, and a pyridinyl group. As the nitrogen-containing group, a dimethylamino group or an N-morpholinyl group is preferred.
[0040] Examples of the oxygen-containing group include a hydroxyl group, a group in which the -CH2- structural unit in the aforementioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group or nitrogen-containing group is replaced with an oxygen atom or a carbonyl group, or a group in which the -CH3 structural unit is replaced with an oxygen atom bonded to a hydrocarbon group having 1 to 20 carbon atoms, such as a methoxy group, ethoxy group, t-butoxy group, phenoxy group, trimethylsiloxy group, methoxyethoxy group, hydroxymethyl group, methoxymethyl group, ethoxymethyl group, t-butoxymethyl group, 1-hydroxyethyl group, Examples of the oxygen-containing group include 1-methoxyethyl group, 1-ethoxyethyl group, 2-hydroxyethyl group, 2-methoxyethyl group, 2-ethoxyethyl group, n-2-oxabutylene group, n-2-oxapentylene group, n-3-oxapentylene group, aldehyde group, acetyl group, propionyl group, benzoyl group, trimethylsilylcarbonyl group, carbamoyl group, methylaminocarbonyl group, carboxy group, methoxycarbonyl group, carboxymethyl group, ethoxycarboxymethyl group, carbamoylmethyl group, furanyl group, pyranyl group, etc. As the oxygen-containing group, a methoxy group is preferable.
[0041] Examples of halogen atoms include fluorine, chlorine, bromine, iodine, etc., which are elements of Group 17. Chlorine or bromine is preferred.
[0042] Examples of the halogen-containing group include a trifluoromethyl group, a tribromomethyl group, a pentafluoroethyl group, a pentafluorophenyl group, and the like, which are groups in which a hydrogen atom in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group, nitrogen-containing group, or oxygen-containing group is substituted with a halogen atom.
[0043] In the present invention, R 2 , R 2' , R 3 , R 3'The substituent is preferably a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing hydrocarbon group, or a nitrogen-containing hydrocarbon group, more preferably a hydrocarbon group or an oxygen-containing hydrocarbon group. The number of carbon atoms contained in the substituent is preferably 1 to 10, and more preferably 1 to 6.
[0044] (R 4 and R 5 ) R 4 and R 5 are each independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group or a nitrogen-containing group, and are preferably a halogen atom or a hydrocarbon group having 1 to 20 carbon atoms. Specific examples of the halogen atom, the hydrocarbon group having 1 to 20 carbon atoms, the oxygen-containing group and the nitrogen-containing group are, respectively, R 2 , R 2' , R 3 , R 3' The same atoms and specific examples of the substituents as those exemplified for the substituents are exemplified.
[0045] Specific examples of the halogen atom include fluorine, chlorine, bromine, and iodine, with chlorine or bromine being preferred, and chlorine being more preferred. The hydrocarbon group having 1 to 20 carbon atoms is preferably a hydrocarbon group having 1 to 4 carbon atoms, more preferably a hydrocarbon group selected from a methyl group or an ethyl group, and even more preferably a methyl group.
[0046] (M) M is an atom of a group 4 element of the periodic table, specifically titanium, zirconium, or hafnium. These atoms are elements that are considered to have high anion (coordination) polymerizability. Among these, zirconium and hafnium are preferred. In terms of the production of transition metal compounds (A), R 1 Considering that the substituent is a relatively large group, hafnium, which is larger than zirconium, may be preferable. However, the type of M is appropriately determined depending on the performance required as an olefin polymerization catalyst.
[0047] Specific examples of the transition metal compound (A) are shown below, but the transition metal compound (A) used in the present invention is not limited to these.
[0048] [ka]
[0049] [ka]
[0050] [ka]
[0051] [ka]
[0052] [ka]
[0053] [ka]
[0054] [ka]
[0055] [ka]
[0056] [ka]
[0057] [ka]
[0058] [ka]
[0059] [ka]
[0060] [ka]
[0061] [ka]
[0062] The transition metal compound (A) used in the present invention can obtain an olefin polymer having a wide molecular weight distribution in the polymerization of olefins, as described later. In particular, it is advantageous in producing an olefin polymer having a relatively large Mz / Mw value, which indicates that the distribution is broad on the high molecular weight side. In addition, such an olefin polymer has a unique feature that the chart obtained by GPC measurement often shows a bimodal distribution.
[0063] [Compound (B)] When olefins are polymerized using a transition metal compound (A), at least one compound (B) selected from the group consisting of (B-1) organometallic compounds, (B-2) organoaluminum oxy compounds, and (B-3) compounds that react with the transition metal compound (A) to form ion pairs can be used in combination with the transition metal compound (A). Each of these components will be described below.
[0064] ((B-1) Organometallic compound) As the organometallic compound (B-1) used in the present invention, specifically, compounds containing at least one element of Groups 1, 2, 12, and 13 of the periodic table represented by the following general formulas (B-1a) to (B-1c) can be mentioned:
[0065] R a p Al(ОR b ) q H r Y s …(B-1a) (In the general formula (B-1a), R a and R b may be the same or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, p is a number where 0 < p ≤ 3, q is a number where 0 ≤ q < 3, r is a number where 0 ≤ r < 3, s is a number where 0 ≤ s < 3, and m + n + p + q = 3.) An organoaluminum compound represented by;
[0066] M 3 AlR c 4…(B-1b) (In the general formula (B-1b), M 3 represents Li, Na or K, and R c represents a hydrocarbon group having 1 to 15 , preferably 1 to 4 carbon atoms.) A complex alkyl compound of an alkali metal of Group 1 of the periodic table and aluminum represented by;
[0067] R d R e M 4 …(B-1c) (In the general formula (B-1c), R d and R e may be the same or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and M 4 is Mg, Zn or Cd.) A dialkyl compound of an alkaline earth metal of Group 2 or a metal of Group 12 of the periodic table represented by;
[0068] Examples of the organoaluminum compound belonging to the general formula (B-1a) include compounds represented by the following general formulas (B-1a-1) to (B-1a-4):
[0069] R a p Al(OR b ) 3-p …(B-1a-1) (In formula (B-1a-1), R a and R b may be the same as or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and p is preferably a number satisfying 1.5 ≦ p ≦ 3.) An organoaluminum compound represented by;
[0070] R a p AlY 3-p …(B-1a-2) (In formula (B-1a-2), R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, and p is preferably a number satisfying 0 < p < 3.) An organoaluminum compound represented by;
[0071] R a p AlH 3-p …(B-1a-3) (In formula (B-1a-3), R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, and p is preferably a number satisfying 2 ≦ p < 3.) An organoaluminum compound represented by;
[0072] R a p Al(OR b ) q Y s …(B-1a-4) (In formula (B-1a-4), R a and R b may be the same as or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, Y represents a halogen atom, p is a number satisfying 0 < p ≦ 3, q is a number satisfying 0 ≦ q < 3, s is a number satisfying 0 ≦ s < 3, and p + q + s = 3.) An organoaluminum compound represented by.
[0073] More specific examples of the organoaluminum compound belonging to the general formula (B-1a) include tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tripropylaluminum, tripentylaluminum, trihexylaluminum, trioctylaluminum, and tridecylaluminum; tri-branched alkylaluminums such as triisopropylaluminum, triisobutylaluminum, trisec-butylaluminum, tritert-butylaluminum, tri2-methylbutylaluminum, tri3-methylbutylaluminum, tri2-methylpentylaluminum, tri3-methylpentylaluminum, tri4-methylpentylaluminum, tri2-methylhexylaluminum, tri3-methylhexylaluminum, and tri2-ethylhexylaluminum; Tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum; Triarylaluminum such as triphenylaluminum and tritolylaluminum; dialkylaluminum hydrides such as diisobutylaluminum hydride; (i-C4H9) x Al y (C5H 10 ) z (wherein x, y and z are positive numbers, and z≧2x), and other trialkenylaluminums, such as triisoprenylaluminum; Alkyl aluminum alkoxides such as isobutyl aluminum methoxide, isobutyl aluminum ethoxide, and isobutyl aluminum isopropoxide; Dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, and dibutylaluminum butoxide; Alkyl aluminum sesquialkoxides such as ethyl aluminum sesquiethoxide, butyl aluminum sesquibutoxide; R a 2.5 Al(OR b )0.5 Partially alkoxylated alkylaluminum having an average composition represented by the formula: a and R b may be the same or different and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; dialkylaluminum aryloxides such as diethylaluminum phenoxide, diethylaluminum (2,6-di-t-butyl-4-methylphenoxide), ethylaluminum bis(2,6-di-t-butyl-4-methylphenoxide), diisobutylaluminum (2,6-di-t-butyl-4-methylphenoxide), and isobutylaluminum bis(2,6-di-t-butyl-4-methylphenoxide); Dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide, and diisobutylaluminum chloride; Alkyl aluminum sesquihalides such as ethyl aluminum sesquichloride, butyl aluminum sesquichloride, and ethyl aluminum sesquibromide; partially halogenated alkylaluminums, such as alkylaluminum dihalides, such as ethylaluminum dichloride, propylaluminum dichloride, butylaluminum dibromide, and the like; Dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; Other partially hydrogenated alkylaluminums, such as alkylaluminum dihydrides, such as ethylaluminum dihydride, propylaluminum dihydride, etc.; Examples of the aluminum compounds include partially alkoxylated and halogenated alkylaluminum compounds such as ethylaluminum ethoxy chloride, butylaluminum butoxy chloride, and ethylaluminum ethoxy bromide.
[0074] Compounds similar to (B-1a) can also be used in the present invention, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms, such as (C2H5)2AlN(C2H5)Al(C2H5)2.
[0075] The compounds belonging to the general formula (B-1b) include LiAl(C2H5)4, LiAl(C7H 15 )4 can be mentioned as examples.
[0076] Examples of the compound belonging to the general formula (B-1c) include dimethylmagnesium, diethylmagnesium, dibutylmagnesium, butylethylmagnesium, dimethylzinc, diethylzinc, diphenylzinc, di-n-propylzinc, diisopropylzinc, di-n-butylzinc, diisobutylzinc, bis(pentafluorophenyl)zinc, dimethylcadmium, and diethylcadmium.
[0077] In addition, as the organometallic compound (B-1), methyllithium, ethyllithium, propyllithium, butyllithium, methylmagnesium bromide, methylmagnesium chloride, ethylmagnesium bromide, ethylmagnesium chloride, propylmagnesium bromide, propylmagnesium chloride, butylmagnesium bromide, butylmagnesium chloride, etc. can also be used.
[0078] In addition, a compound which forms the above-mentioned organoaluminum compound in the polymerization system, for example, a combination of an aluminum halide and an alkyl lithium, or a combination of an aluminum halide and an alkyl magnesium, may be used as the organometallic compound (B-1). It is also possible.
[0079] Among the organometallic compounds (B-1), organoaluminum compounds are preferred from the standpoint of catalytic activity. The organometallic compounds (B-1) as described above may be used singly or in combination of two or more kinds.
[0080] ((B-2) Organoaluminum oxy compound) The organoaluminum oxy compound (B-2) used in the present invention may be a conventionally known aluminoxane, or may be a benzene-insoluble organoaluminum oxy compound such as those exemplified in JP-A-2-78687.
[0081] Conventionally known aluminoxanes can be produced, for example, by the following method, and are usually obtained as a solution in a hydrocarbon solvent.
[0082] (1) A method in which an organoaluminum compound such as trialkylaluminum is added to a hydrocarbon medium suspension of a compound containing adsorbed water or a salt containing water of crystallization, such as magnesium chloride hydrate, copper sulfate hydrate, aluminum sulfate hydrate, nickel sulfate hydrate, or cerous chloride hydrate, to react the adsorbed water or the water of crystallization with the organoaluminum compound.
[0083] (2) A method in which water, ice or water vapor is allowed to act directly on an organoaluminum compound such as trialkylaluminum in a medium such as benzene, toluene, ethyl ether or tetrahydrofuran.
[0084] (3) A method in which an organoaluminum compound such as trialkylaluminum is reacted with an organotin oxide such as dimethyltin oxide or dibutyltin oxide in a medium such as decane, benzene, or toluene.
[0085] The aluminoxane may contain a small amount of an organometallic component. After the solvent or unreacted organoaluminum compound is removed by distillation from the recovered aluminoxane solution, the resulting aluminoxane may be redissolved in a solvent or suspended in a poor solvent for the aluminoxane.
[0086] Specific examples of the organoaluminum compound used in preparing the aluminoxane include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the general formula (B-1a). Among these, trialkylaluminum and tricycloalkylaluminum are preferred, and trimethylaluminum is particularly preferred.
[0087] The above organoaluminum compounds may be used singly or in combination of two or more.
[0088] Examples of the solvent used in the preparation of aluminoxane include aromatic hydrocarbons such as benzene, toluene, xylene, cumene, and cymene; aliphatic hydrocarbons such as pentane, hexane, heptane, octane, decane, dodecane, hexadecane, and octadecane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, cyclooctane, and methylcyclopentane; petroleum fractions such as gasoline, kerosene, and diesel; and halides of the above aromatic hydrocarbons, aliphatic hydrocarbons, and alicyclic hydrocarbons, especially chlorinated and brominated hydrocarbons. Furthermore, ethers such as ethyl ether and tetrahydrofuran can also be used. Among these solvents, aromatic hydrocarbons or aliphatic hydrocarbons are particularly preferred. These solvents can be used alone or in combination.
[0089] The organoaluminum oxy compound (B-2) according to the present invention includes at least one selected from aluminoxanes having a structure represented by the following general formula (B-2a) or (B-2b), and aluminoxanes having a structure comprising a repeating unit represented by the following general formula (B-2c) and a repeating unit represented by the following general formula (B-2d).
[0090] [ka]
[0091] In the general formula, R care each independently a hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an isopropenyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, a cyclohexyl group, a cyclooctyl group, a phenyl group, a tolyl group, and an ethylphenyl group. Among these examples, a methyl group, an ethyl group, and an isobutyl group are preferred, and a methyl group is particularly preferred, and in the general formulae (B-2a), (B-2b), and (B-2c), R c may be partially substituted with halogen atoms such as chlorine and bromine atoms, and the halogen content may be 40 mass % or less.
[0092] In the general formulae (B-2a) and (B-2b), r represents an integer of 2 to 500, preferably 6 to 300, and particularly preferably 10 to 100.
[0093] In the general formulae (B-2c) and (B-2d), s and t each represent an integer of 1 or more. The aluminoxane having a repeating unit represented by the general formula (B-2c) and a repeating unit represented by the general formula (B-2d) preferably has a molecular weight in the range of 200 to 2000 as measured by cryoscopic method in benzene.
[0094] The benzene-insoluble organoaluminum oxy-compound used in the present invention is preferably one in which the Al component dissolved in benzene at 60°C is usually 10% or less, preferably 5% or less, and particularly preferably 2% or less, calculated as Al atom, i.e., it is preferably insoluble or poorly soluble in benzene.
[0095] The organoaluminum oxy compound (B-2) used in the present invention may also include boron-containing organoaluminum oxy compounds represented by the following general formula (B-2e).
[0096] [ka]
[0097] In general formula (B-2e), R 15 represents a hydrocarbon group having 1 to 10 carbon atoms, and four R 16 may be the same or different and each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.
[0098] The boron-containing organoaluminum oxy compound represented by the general formula (B-2e) can be produced by reacting an alkylboronic acid represented by the following general formula (B-2f) with an organoaluminum compound in an inert solvent under an inert gas atmosphere at a temperature of −80° C. to room temperature for 1 minute to 24 hours.
[0099] R 15 -B(OH)2…(B-2f) In general formula (B-2f), R 15 is R in the general formula (B-2e) 15 represents the same group as
[0100] Specific examples of the alkylboronic acid represented by the general formula (B-2f) include methylboronic acid, ethylboronic acid, isopropylboronic acid, n-propylboronic acid, n-butylboronic acid, isobutylboronic acid, n-hexylboronic acid, cyclohexylboronic acid, phenylboronic acid, 3,5-difluoroboronic acid, pentafluorophenylboronic acid, and 3,5-bis(trifluoromethyl)phenylboronic acid. Among these, methylboronic acid, n-butylboronic acid, isobutylboronic acid, 3,5-difluorophenylboronic acid, and pentafluorophenylboronic acid are preferred. These are used alone or in combination of two or more.
[0101] Specific examples of the organoaluminum compound to be reacted with such an alkylboronic acid include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the above general formula (B-1a).
[0102] The organoaluminum compound is preferably a trialkylaluminum or a tricycloalkylaluminum, more preferably a trimethylaluminum, a triethylaluminum or a triisobutylaluminum, which may be used alone or in combination of two or more.
[0103] When an organoaluminum oxy compound (B-2) such as methylaluminoxane is used as a cocatalyst component in addition to the transition metal compound (A), extremely high polymerization activity for olefin compounds is exhibited.
[0104] The above organoaluminum oxy compounds (B-2) may be used singly or in combination of two or more.
[0105] ((B-3) A compound that reacts with a transition metal compound (A) to form an ion pair) Examples of the compound (B-3) (hereinafter referred to as "ionized ionic compound") used in the present invention that reacts with the transition metal compound (A) to form an ion pair include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and US Pat. No. 5,321,106. Furthermore, heteropoly compounds and isopoly compounds can also be mentioned.
[0106] Specifically, the Lewis acid includes a compound represented by BR3 (R is fluorine or a phenyl group which may have a substituent such as fluorine, a methyl group, or a trifluoromethyl group), such as trifluoroboron, triphenylboron, tris(4-fluorophenyl)boron, tris(3,5-difluorophenyl)boron, tris(4-fluoromethylphenyl)boron, tris(pentafluorophenyl)boron, tris(p-tolyl)boron, tris(o-tolyl)boron, and tris(3,5-dimethylphenyl)boron.
[0107] The ionized ionic compound may, for example, be a compound represented by the following general formula (B-3a).
[0108] [ka]
[0109] In general formula (B-3a), R 17 H + , a carbonium cation, an oxonium cation, an ammonium cation, a phosphonium cation, a cycloheptyltrienyl cation or a ferrocenium cation having a transition metal, and R 18 ~R 21 may be the same or different and are organic groups, preferably aryl groups or substituted aryl groups.
[0110] Specific examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation, tri(methylphenyl)carbonium cation, and tri(dimethylphenyl)carbonium cation.
[0111] Specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, tributylammonium cation, and tri(n-butyl)ammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as di(isopropyl)ammonium cation and dicyclohexylammonium cation.
[0112] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation.
[0113] R 17 As the cation, a carbonium cation and an ammonium cation are preferred, and in particular, a triphenylcarbonium cation, an N,N-dimethylanilinium cation, and an N,N-diethylanilinium cation are preferred.
[0114] Further, examples of the ionic compound include trialkyl-substituted ammonium salts, N,N-dialkylanilinium salts, dialkylammonium salts, and triarylphosphonium salts.
[0115] Specific examples of the trialkyl-substituted ammonium salt include triethylammonium tetra(phenyl)boron, tripropylammonium tetra(phenyl)boron, tri(n-butyl)ammonium tetra(phenyl)boron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o-tolyl)boron, tri(n-butyl)ammonium tetra(pentafluorophenyl)boron, tripropylammonium tetra(o,p-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(m,m-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(p-trifluoromethylphenyl)boron, tri(n-butyl)ammonium tetra(3,5-ditrifluoromethylphenyl)boron, and tri(n-butyl)ammonium tetra(o-tolyl)boron.
[0116] Specific examples of the N,N-dialkylanilinium salt include N,N-dimethylanilinium tetra(phenyl)boron, N,N-diethylanilinium tetra(phenyl)boron, and N,N,2,4,6-pentamethylanilinium tetra(phenyl)boron.
[0117] Specific examples of the dialkylammonium salt include di(1-propyl)ammonium tetra(pentafluorophenyl)boron, dicyclohexylammonium tetra(phenyl)boron, and the like.
[0118] Further examples of the ionized ionic compound include triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, ferrocenium tetra(pentafluorophenyl)borate, triphenylcarbenium pentaphenylcyclopentadienyl complex, N,N-diethylanilinium pentaphenylcyclopentadienyl complex, and boron compounds represented by the following formula (B-3b) or (B-3c).
[0119] [ka] In formula (B-3b), Et represents an ethyl group.
[0120] [ka] In formula (B-3c), Et represents an ethyl group.
[0121] Specific examples of the borane compound, which is an example of the ionizable ionic compound (compound (B-3)), include decaborane; Salts of anions such as bis[tri(n-butyl)ammonium]nonaborate, bis[tri(n-butyl)ammonium]decaborate, bis[tri(n-butyl)ammonium]undecaborate, bis[tri(n-butyl)ammonium]dodecaborate, bis[tri(n-butyl)ammonium]decachlorodecaborate, and bis[tri(n-butyl)ammonium]dodecachlorododecaborate; Examples of the salt include salts of metal borane anions such as tri(n-butyl)ammonium bis(dodecahydride dodecaborate) cobaltate(III) and bis[tri(n-butyl)ammonium]bis(dodecahydride dodecaborate) nickelate(III).
[0122] Specific examples of carborane compounds, which are examples of ionizable ionic compounds, include 4-carbanonaborane, 1,3-dicarbanonaborane, 6,9-dicarbadecaborane, dodecahydride-1-phenyl-1,3-dicarbanonaborane, dodecahydride-1-methyl-1,3-dicarbanonaborane, undecahydride-1,3-dimethyl-1,3-dicarbanonaborane, 7,8-dicarbaundecaborane, 2,7-dicarbaundecaborane, and undecahydride-7,8-dimethyl-1,3-dicarbanonaborane. 1-methyl-7,8-dicarboxylic acid borane, dodecahydride-11-methyl-2,7-dicarboxylic acid borane, tri(n-butyl)ammonium 1-carbadecaborate, tri(n-butyl)ammonium 1-carbaundecaborate, tri(n-butyl)ammonium 1-carbadodecaborate, tri(n-butyl)ammonium 1-trimethylsilyl-1-carbadecaborate, tri(n-butyl)ammonium bromo-1-carbadodecaborate, tri(n-butyl)ammonium ammonium 6-carbadecaborate, tri(n-butyl)ammonium 6-carbadecaborate, tri(n-butyl)ammonium 7-carbaundecaborate, tri(n-butyl)ammonium 7,8-dicaundecaborate, tri(n-butyl)ammonium 2,9-dicaundecaborate, tri(n-butyl)ammonium dodecahydride-8-methyl-7,9-dicaundecaborate, tri(n-butyl)ammonium undecahydride-8-ethyl-7,9-dicaundecaborate Salts of anions such as undecahydride, tri(n-butyl)ammonium undecahydride-8-butyl-7,9-dicarboxaborate, tri(n-butyl)ammonium undecahydride-8-allyl-7,9-dicarboxaborate, tri(n-butyl)ammonium undecahydride-9-trimethylsilyl-7,8-dicarboxaborate, tri(n-butyl)ammonium undecahydride-4,6-dibromo-7-carbaundecaborate; Tri(n-butyl)ammonium bis(nonahydride-1,3-dicarbanonaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)ferrate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)nickelate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cuprate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)aurate(III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarbandecaborate)ferrate salt (III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarboxaborate)chromate (III), tri(n-butyl)ammonium bis(tribromooctahydride-7,8-dicarboxaborate)cobaltate (III), tris[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)chromate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)manganate (IV), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)cobaltate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)nickelate (IV), and the like.
[0123] Heteropoly compounds, which are examples of ionizing ionic compounds, are compounds containing an atom selected from the group consisting of silicon, phosphorus, titanium, germanium, arsenic, and tin, and one or more atoms selected from the group consisting of vanadium, niobium, molybdenum, and tungsten. Specific examples of the acid include, but are not limited to, phosphovanadic acid, germanovanadic acid, arsenic vanadic acid, phosphoniobic acid, germanoniobic acid, siliconomolybdic acid, phosphomolybdic acid, titanomolybdic acid, germanomolybdic acid, arsenic molybdic acid, tinmolybdic acid, phosphotungstic acid, germanotungstic acid, tintungstic acid, phosphomolybdovanadic acid, phosphotungstovanadic acid, germanotungstovanadic acid, phosphomolybdotungstovanadic acid, germanomolybdotungstovanadic acid, phosphomolybdotungstic acid, phosphomolybdoniobic acid, and salts of these acids. Examples of the salts include salts of the acids with, for example, alkali metals of Group 1 or alkaline earth metals of Group 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts.
[0124] Isopoly compounds, which are examples of ionized ionic compounds, are compounds composed of metal ions of one type of atom selected from the group consisting of vanadium, niobium, molybdenum, and tungsten, and can be considered to be molecular ion species of metal oxides.Specific examples include, but are not limited to, vanadic acid, niobic acid, molybdic acid, tungstic acid, and salts of these acids.Furthermore, examples of the salts include salts of the acids with metals of Group 1 or 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts.
[0125] The above-mentioned ionizing ionic compound (compound (B-3) which reacts with the transition metal compound (A) to form an ion pair) may be used alone or in combination of two or more kinds.
[0126] The olefin polymerization catalyst according to the present invention may contain the transition metal compound (A) and at least one compound (B) selected from the group consisting of organometallic compounds (B-1), organoaluminum oxy compounds (B-2), and ionizing ionic compounds (B-3), and may also contain the following support (C) as necessary.
[0127] [(C) Carrier] The carrier (C) used in the present invention is an inorganic or organic compound, and is a granular or fine particle solid. By supporting the transition metal compound (A) and the compound (B) on the carrier (C), a polymer with good morphology can be obtained.
[0128] The inorganic compound is preferably a porous oxide, a solid aluminoxane compound, an inorganic halide, clay, a clay mineral, or an ion-exchangeable layered compound.
[0129] Specifically, the porous oxide may be SiO2, Al2O3, MgO, ZrO, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or a composite or mixture containing these, and further may be, for example, natural or synthetic zeolite, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. Among these, the porous oxide is preferably one containing SiO2 and / or Al2O3 as the main component.
[0130] The porous oxide may contain small amounts of carbonates, sulfates, nitrates, and oxides such as Na2CO3, K2CO3, CaCO3, MgCO3, Na2SO4, Al2(SO4)3, BaSO4, KNO3, Mg(NO3)2, Al(NO3)3, Na2O, K2O, and Li2O.
[0131] The properties of such porous oxides vary depending on the type and production method, but the porous oxides used in the present invention preferably have a particle size of 10 to 300 μm, more preferably 20 to 200 μm, and a specific surface area of 50 to 1000 m. 2 / g, more preferably 100 to 700m 2 / g and the pore volume is 0.3-3.0 cm 3 / g range. Such a porous oxide is calcined at 100 to 1000°C, preferably 150 to 700°C, as required, before use.
[0132] The solid aluminoxane compound includes at least one aluminoxane selected from the aluminoxanes represented by the formulas (B-2a) to (B-2d).
[0133] The solid aluminoxane used in the present invention is different from conventionally known olefin polymerization catalyst supports, and does not contain inorganic solid components such as silica or alumina or organic polymer components such as polyethylene or polystyrene, but is solidified with an alkylaluminum compound as the main component. The term "solid" used in the present invention means that the aluminoxane component (B-2) is substantially maintained in a solid state under the reaction environment in which it is used. More specifically, it means that when the transition metal compound (A) is contacted with the compound (B) to prepare a solid catalyst component for olefin polymerization as described below, the compound (B) is in a solid state under a specific temperature and pressure environment in an inert hydrocarbon solvent such as hexane or toluene used in the reaction. In addition, when suspension polymerization is performed using a solid catalyst component for olefin polymerization prepared using the compound (B) as described below, it is also a necessary requirement that the compound (B) contained in the catalyst component is in a solid state under a specific temperature and pressure environment in a hydrocarbon solvent such as hexane, heptane, or toluene. The same applies to bulk polymerization in which polymerization is performed in a liquefied monomer instead of a solvent, and gas-phase polymerization in which polymerization is performed in a monomer gas.
[0134] The easiest way to check whether the compound (B) is in a solid state under the above environment is to check visually, but it is often difficult to check visually, for example, during polymerization. In that case, it can be judged, for example, from the properties of the polymer powder obtained after polymerization and the state of adhesion to the reactor. Conversely, if the properties of the polymer powder are good and there is little adhesion to the reactor, even if a part of the compound (B) is eluted to some extent under the polymerization environment, it does not deviate from the gist of the present invention. Examples of indicators for judging the properties of the polymer powder include bulk density, particle shape, surface shape, and the degree of presence of amorphous polymers, but from the viewpoint of quantitativeness, polymer bulk density is preferred. The bulk density in the present invention is usually 0.01 to 0.9, preferably 0.05 to 0.6, and more preferably 0.1 to 0.5.
[0135] The solid aluminoxane used in the present invention has a solubility in n-hexane maintained at a temperature of 25° C. of usually 0 to 40 mol %, preferably 0 to 20 mol %, and particularly preferably 0 to 10 mol %.
[0136] The solubility of the solid aluminoxane used in the present invention in n-hexane was determined by adding 2 g of the solid aluminoxane carrier to 50 ml of n-hexane kept at 25° C., stirring for 2 hours, separating the solution using a G-4 glass filter, and measuring the aluminum concentration in the filtrate. Therefore, the solubility is determined as the ratio of aluminum atoms present in the filtrate to the amount of aluminum atoms equivalent to 2 g of the aluminoxane used.
[0137] The solid aluminoxane used in the present invention can be any known solid aluminoxane without any restrictions. Known production methods include, for example, JP-B-7-42301, JP-A-6-220126, JP-A-6-220128, JP-A-11-140113, JP-A-11-310607, JP-A-2000-38410, JP-A-2000-95810, and International Publication No. 2010 / 55652.
[0138] The average particle size of the solid aluminoxane used in the present invention is generally in the range of 0.01 to 50,000 μm, preferably 1 to 1,000 μm, and particularly preferably 1 to 200 μm.
[0139] The average particle size of solid aluminoxane is determined by observing the particles with a scanning electron microscope, measuring the particle size of 100 or more particles, and averaging the weights. The particle size of solid aluminoxane was determined by measuring the maximum length of the Pythagorean method from the particle image. That is, the length of the particle image sandwiched between two parallel lines in both the horizontal and vertical directions was measured, and the particle size was calculated using the following formula. Particle size = ((horizontal length) 2 +(Vertical length) 2 ) 0.5
[0140] The weight average particle diameter of the solid aluminoxane is calculated from the particle diameter calculated above according to the following formula. Average particle size=Σnd 4 / Σnd 3 (where n is the number of particles, d is the particle size)
[0141] The solid aluminoxane preferably used in the present invention has a specific surface area of 50 to 1000 m 2 / g, preferably 100 to 800m 2 / g and the pore volume is 0.1-2.5 cm 3 / g is preferable.
[0142] As the inorganic halide, MgCl2, MgBr2, MnCl2, MnBr2, etc. can be used. The inorganic halide can be used as it is, or can be used after being pulverized by a ball mill or a vibration mill. In addition, the inorganic halide can be dissolved in a solvent such as alcohol, and then precipitated into fine particles by a precipitating agent.
[0143] The clay is usually composed mainly of clay minerals. The ion-exchangeable layered compound is a compound having a crystal structure in which the planes formed by ionic bonds are stacked in parallel with each other with weak bonding force, and the ions contained therein are exchangeable. Most clay minerals are ion-exchangeable layered compounds. These clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used.
[0144] Examples of the clay, clay mineral, or ion-exchangeable layered compound include ionic crystalline compounds having layered crystal structures such as hexagonal close packing type, antimony type, CdCl2 type, and CdI2 type.
[0145] Furthermore, examples of clay and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, halloysite, etc. Ion-exchangeable layered compounds include crystalline acid salts of polyvalent metals, such as α-Zr(HAsO4)2·H2O, α-Zr(HPO4)2, α-Zr(KPO4)2·3H2O, α-Ti(HPO4)2, α-Ti(HAsO4)2·H2O, α-Sn(HPO4)2·H2O, γ-Zr(HPO4)2, γ-Ti(HPO4)2, and γ-Ti(NH4PO4)2·H2O.
[0146] Such clay, clay mineral, or ion-exchangeable layered compound preferably has a pore volume of 0.1 cc / g or more, particularly preferably 0.3 to 5 cc / g, having a radius of 20 Å or more, as measured by mercury intrusion porosimetry, where the pore volume is measured for a pore radius range of 20 to 30,000 Å by mercury intrusion porosimetry using a mercury porosimeter.
[0147] When a support having a pore volume of less than 0.1 cc / g and a radius of 20 Å or more is used, it tends to be difficult to obtain high polymerization activity.
[0148] It is also preferable to subject the clay and clay minerals used in the present invention to chemical treatment. As the chemical treatment, any of surface treatments that remove impurities attached to the surface and treatments that affect the crystalline structure of the clay can be used. Specific examples of chemical treatments include acid treatment, alkali treatment, salt treatment, and organic treatment. In addition to removing impurities from the surface, acid treatment increases the surface area by eluting cations such as Al, Fe, and Mg in the crystalline structure. In alkali treatment, the crystalline structure of the clay is destroyed, resulting in a change in the structure of the clay. In addition, salt treatment and organic treatment form ion complexes, molecular complexes, organic derivatives, etc., which can change the surface area and interlayer distance.
[0149] The ion-exchangeable layered compound used in the present invention may be a layered compound in which the space between layers is expanded by utilizing the ion exchangeability and exchanging the exchangeable ions between layers with other large bulky ions. Such bulky ions play a role of supporting the layered structure and are usually called pillars. The introduction of another substance between layers of a layered compound in this way is called intercalation. Examples of guest compounds to be intercalated include cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (R is a hydrocarbon group, etc.), [Al 13 O4(OH) 24 ] 7+ , [Zr4(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + Metal hydroxide ions such as these can be used. These compounds can be used alone or in combination of two or more. When intercalating these compounds, polymers obtained by hydrolysis of metal alkoxides (R indicates a hydrocarbon group, etc.) such as Si(OR)4, Al(OR)3, Ge(OR)4, and colloidal inorganic compounds such as SiO2 can also be used. Examples of pillars include oxides produced by intercalating the above metal hydroxide ions between layers and then dehydrating them with heat.
[0150] The clay, clay mineral, and ion-exchangeable layered compound used in the present invention may be used as is, or may be used after treatment such as ball milling or sieving. They may also be used after newly adding and adsorbing water or after heat dehydration treatment. Furthermore, they may be used alone or in combination of two or more kinds.
[0151] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred.
[0152] As described above, the carrier (C) is an inorganic or organic compound, and examples of the organic compound include granular or fine particle solids having a particle size in the range of 10 to 300 μm.Specific examples include (co)polymers produced mainly from α-olefins having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or (co)polymers produced mainly from vinylcyclohexane and styrene, and their modified products.
[0153] The olefin polymerization catalyst according to the present invention may further contain, in addition to the above-mentioned transition metal compound (A), the above-mentioned compound (B), and, if necessary, the support (C), the following specific organic compound component (D) may also be contained, if necessary.
[0154] [(D) Organic compound component] In the present invention, the organic compound component (D) is used, if necessary, for the purpose of improving the polymerization performance of the olefin polymerization catalyst of the present invention and the physical properties of the produced polymer (for example, the molecular weight of the produced polymer) (increasing the molecular weight, for example). Examples of such organic compounds include, but are not limited to, alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, and sulfonates.
[0155] The alcohols and phenolic compounds are generally selected from the group consisting of R 22 The formula represented by -OH is used, where R22 represents a hydrocarbon group having 1 to 50 carbon atoms (in the case of phenols, the carbon number is 6 to 50) or a halogenated hydrocarbon group having 1 to 50 carbon atoms (in the case of phenols, the carbon number is 6 to 50).
[0156] Alcohols include R 22 The phenolic compound is preferably one in which the α,α'-positions of the hydroxyl group are substituted with a hydrocarbon having 1 to 20 carbon atoms.
[0157] The carboxylic acid is usually R 23 The one represented by -COOH is used. 23 represents a hydrocarbon group having 1 to 50 carbon atoms or a halogenated hydrocarbon group having 1 to 50 carbon atoms, and is particularly preferably a halogenated hydrocarbon group having 1 to 50 carbon atoms.
[0158] As the phosphorus compound, phosphoric acids having a P-O-H bond, phosphates having a P-OR or P=O bond, and phosphine oxide compounds are preferably used. The sulfonate salt includes those represented by the following general formula (Da).
[0159] [ka]
[0160] In the general formula (Da), M 5 is an atom in groups 1 to 14 of the periodic table, and R 24 is hydrogen, carbon number Z is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a halogenated hydrocarbon group having 1 to 20 carbon atoms, t is an integer of 1 to 7, u is an integer of 1 to 7, and tu is 1 or greater.
[0161] <Production method of olefin polymer> The process for producing an olefin polymer according to the present invention includes a step of polymerizing or copolymerizing an olefin in the presence of the above-mentioned olefin polymerization catalyst to obtain an olefin polymer. As described above, in this specification, the term "olefin" refers to any compound having a polymerizable double bond.
[0162] In the polymerization, the components constituting the catalyst of the present invention may be used in any manner and added in any order to a polymerization vessel. Examples of the manner include the following.
[0163] (1) A method in which the transition metal compound (A) is added alone to a polymerization reactor. (2) A method in which the transition metal compound (A) and the compound (B) are added to a polymerization reactor in any order.
[0164] (3) A method in which a catalyst component in which a transition metal compound (A) is supported on a carrier (C) and a compound (B) are added to a polymerization reactor in any order. (4) A method in which a catalyst component in which the compound (B) is supported on a carrier (C) and a transition metal compound (A) are added to a polymerization reactor in any order.
[0165] (5) A catalyst component comprising a transition metal compound (A) and a compound (B) supported on a carrier (C) is added to a polymerization reactor. (6) A method in which a catalyst component in which a transition metal compound (A) and a compound (B) are supported on a carrier (C), and the compound (B) are added to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different.
[0166] (7) A method in which the catalyst component in which the compound (B) is supported on the carrier (C), the transition metal compound (A), and the compound (B) are added to the polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different.
[0167] (8) A method in which a component in which a transition metal compound (A) is supported on a carrier (C) and a component in which a compound (B) is supported on a carrier (C) are added to a polymerization reactor in any order. (9) A method of adding a component in which a transition metal compound (A) is supported on a carrier (C), a component in which a compound (B) is supported on a carrier (C), and a compound (B) to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different.
[0168] (10) A method in which the transition metal compound (A), the compound (B), and the organic compound component (D) are added to a polymerization reactor in any order.
[0169] (11) A method in which the compound (B) and the organic compound component (D) which have been contacted in advance, and the transition metal compound (A) are added to a polymerization reactor in any order. (12) A method in which the compound (B), the organic compound component (D) supported on the carrier (C), and the transition metal compound (A) are added to a polymerization reactor in any order.
[0170] (13) A method in which a catalyst component in which a transition metal compound (A) and a compound (B) have been contacted in advance, and an organic compound component (D) are added to a polymerization reactor in any order. (14) A method in which a catalyst component in which a transition metal compound (A) and a compound (B) have been contacted in advance, compound (B), and an organic compound component (D) are added to a polymerization reactor in any order. (15) A method in which a catalyst component in which a transition metal compound (A) is contacted with a compound (B) in advance, and a component in which a compound (B) is contacted with an organic compound component (D) in advance are added to a polymerization vessel in any order. In this case, the compound (B) contacted with the transition metal compound (A) and the compound (B) contacted with the organic compound component (D) may be the same or different.
[0171] (16) A method in which a transition metal compound (A) supported on a carrier (C), a compound (B), and an organic compound component (D) are added to a polymerization reactor in any order. (17) A method in which a component in which a transition metal compound (A) is supported on a carrier (C), and a component in which a compound (B) and an organic compound component (D) are previously contacted with each other are added to a polymerization reactor in any order.
[0172] (18) A method in which a catalyst component prepared by previously contacting a transition metal compound (A), a compound (B) and an organic compound component (D) in any order is added to a polymerization reactor. (19) A method in which a catalyst component in which a transition metal compound (A), a compound (B) and an organic compound component (D) have been contacted in advance, and compound (B) are added to a polymerization vessel in any order. In this case, compound (B) that is contacted with transition metal compound (A) and organic compound component (D) and compound (B) that is added alone may be the same or different.
[0173] (20) A method of adding a catalyst comprising a transition metal compound (A), a compound (B) and an organic compound component (D) supported on a carrier (C) to a polymerization reactor. (21) A method of adding a catalyst component in which a transition metal compound (A), a compound (B) and an organic compound component (D) are supported on a carrier (C), and the compound (B) to a polymerization vessel in any order. In this case, the compound (B) supported on the carrier (C) and the compound (B) added alone may be the same or different.
[0174] In the above-mentioned solid catalyst component having the transition metal compound (A) supported on the support (C) and the solid catalyst component having the transition metal compound (A) and the compound (B) supported on the support (C), an olefin may be prepolymerized, or a catalyst component may be further supported on the prepolymerized solid catalyst component.
[0175] In the present invention, the (co)polymerization can be carried out by either a liquid phase polymerization method such as solution polymerization or suspension polymerization, or a gas phase polymerization method. Specific examples of the inert hydrocarbon medium used in the liquid phase polymerization method include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane, and mixtures thereof, and the olefin itself to be subjected to the (co)polymerization can also be used as a solvent.
[0176] When olefin polymerization is carried out using the above-mentioned olefin polymerization catalyst, the transition metal compound (A) is usually used in an amount of 10 -12 ~10 -2 moles, preferably 10 -10 ~10 -3 It is used in molar amounts.
[0177] The organometallic compound (B-1) is used in an amount such that the molar ratio of the organometallic compound (B-1) to the total transition metal atoms (M) in the transition metal compound (A) [(B-1) / M] is usually 0.01 to 100,000, preferably 0.05 to 50,000. The organoaluminum oxy compound (B-2) is used in an amount such that the molar ratio of the aluminum atoms in the organoaluminum oxy compound (B-2) to the total transition metals (M) in the transition metal compound (A) [(B-2) / M] is usually 10 to 500,000, preferably 20 to 100,000. The compound (ionizing ionic compound) (B-3) that reacts with the transition metal compound (A) to form an ion pair is used in an amount such that the molar ratio of the ionizing ionic compound (B-3) to the transition metal atom (M) in the transition metal compound (A) [(B-3) / M] is usually 1 to 50, preferably 1 to 30, and more preferably 1 to 20.
[0178] The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-1)] to the organometallic compound (B-1) is usually 0.01 to 10, preferably 0.1 to 5. The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-2)] to the organoaluminum oxy compound (B-2) is usually 0.001 to 2, preferably 0.005 to 1. The organic compound component (D) is used in an amount such that the molar ratio [(D) / (B-3)] to the ionizing ionic compound (B-3) is usually 0.01 to 10, preferably 0.1 to 5.
[0179] The polymerization temperature of the olefin using such an olefin polymerization catalyst is usually in the range of −50 to +200° C., preferably 0 to 170° C. The polymerization pressure is usually normal pressure to 100 kg / cm. 2-G, preferably normal pressure to 50 kg / cm 2 Under the conditions of -G, the polymerization reaction can be carried out in any of batch, semi-continuous and continuous modes. Furthermore, the polymerization can be carried out in two or more stages with different reaction conditions.
[0180] The molecular weight of the resulting olefin polymer can be adjusted by the presence of hydrogen in the polymerization system or by changing the polymerization temperature, and can also be adjusted by the amount of compound (B) used.
[0181] The hydrogen is a chain transfer agent, which is a component that reduces molecular weight. Even if it is used in combination with an olefin polymerization reaction, it tends to have little effect on polymerization activity. The olefin polymerization catalyst containing the transition metal compound (A) of the present application exhibits a property that makes it easy to produce a component with a high molecular weight, and therefore has the advantage of having a high degree of freedom in adjusting the molecular weight.
[0182] The olefin that can be polymerized by the olefin polymerization catalyst of the present invention is not particularly limited as long as it has a polymerizable double bond, and may be a linear or branched α-olefin having 2 to 30, preferably 2 to 20, and more preferably 2 to 10 carbon atoms, such as ethylene, propylene, 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene; Examples of cyclic olefins include those having 3 to 30, preferably 3 to 20, and more preferably 3 to 10 carbon atoms, such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene, and 2-methyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene.
[0183] The olefin polymerization catalyst of the present invention is more preferably used for homopolymerization of ethylene, copolymerization of ethylene with an olefin having 3 to 20 carbon atoms, preferably a linear or branched α-olefin having 3 to 10 carbon atoms, homopolymerization of propylene, or copolymerization of propylene with an olefin selected from ethylene and α-olefins having 4 to 20 carbon atoms. The α-olefins may be used alone or in combination of two or more kinds.
[0184] In the case of copolymerization of ethylene with an α-olefin having 3 to 20 carbon atoms, preferably 3 to 10 carbon atoms, the α-olefin (hereinafter also referred to as olefin A) is not particularly limited as long as it exhibits the effects of the present invention, but for example, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, and 1-decene are preferred. These α-olefins may be used alone or in combination of two or more. Among these, at least one selected from propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene is more preferred.
[0185] When ethylene is used as the α-olefin and the above olefin A is used, the ratio of the amounts of ethylene to the above olefin A used is usually 1:10 to 5000:1, preferably 1:5 to 1000:1, in terms of ethylene:olefin A (molar ratio).
[0186] The ratio of the amount of propylene to the olefin (olefin B) selected from the group consisting of ethylene and α-olefins having 4 to 20 carbon atoms (molar ratio of propylene to the above-mentioned olefin B) used is usually 1:10 to 5000:1, preferably 1:5 to 1000:1. Preferred examples of olefin B are the same as those of olefin A except for propylene.
[0187] The olefin polymerization catalyst of the present invention may (co)polymerize known linear unsaturated hydrocarbons having polar groups (for example, carbonyl groups, hydroxyl groups, ether bond groups, etc.).
[0188] The olefin polymerization catalyst of the present invention may also be used to (co)polymerize vinylcyclohexane, dienes or polyenes.
[0189] The diene or polyene may be a cyclic or chain compound having 4 to 30 carbon atoms, preferably 4 to 20 carbon atoms, and two or more double bonds. Specific examples include butadiene, isoprene, 4-methyl-1,3-pentadiene, 1,3-pentadiene, 1,4-pentadiene, 1,5-hexadiene, 1,4-hexadiene, 1,3-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, ethylidenenorbornene, vinylnorbornene, and dicyclopentadiene; 7-Methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 5,9-dimethyl-1,4,8-decatriene; Further aromatic vinyl compounds, for example mono- or polyalkylstyrenes such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, etc.; Functional group-containing styrene derivatives such as methoxystyrene, ethoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, o-chlorostyrene, p-chlorostyrene, and divinylbenzene; Examples include 3-phenylpropylene, 4-phenylpropylene, and α-methylstyrene.
[0190] The compounds such as the above-mentioned olefins used in the olefin polymerization catalyst of the present invention are not limited to compounds derived from fossil resources such as petroleum, but may also be compounds derived from plants or other so-called bio-derived compounds.
[0191] The transition metal compound (A) used in the present invention is 1When an olefin polymer is produced using an olefin polymerization catalyst containing this structure, it tends to be possible to obtain a polymer having a wide molecular weight distribution. The reason for this is unclear at present, but the present inventors consider it as follows.
[0192] In the transition metal compound (A) represented by the formula (A-1), R 1 The two cyclopentadienyl (or indenyl) skeletons connected by R 1 Since it is a relatively large structure and is bonded to specific positions of the two cyclopentadienyl skeletons, the distance between them is large and it is expected that it can take a relatively large number of conformations. In addition, when bonding to the transition metal atom M, the distance between M is expected to be relatively large. Therefore, the distance between the transition metal atom M and the ligand is expected to be relatively large compared to conventional metallocene compounds, resulting in a loose bond. Therefore, the structure of the transition metal compound (A) is considered to be relatively variable and highly likely to take multiple conformations.
[0193] Furthermore, metallocene compounds with different conformations are expected to show different performance as olefin polymerization catalysts. This change in conformation leads to a state in which olefin polymerization catalysts having multiple types of active sites coexist, which is thought to enable the production of polymers with a wide molecular weight distribution. In addition, when the distance between the M and the cyclopentadienyl skeleton is large, the by-production of hydrogen as a chain transfer agent is suppressed, and an olefin polymer with a high molecular weight is concomitantly produced, which may result in a molecular weight distribution that is broadened toward the high molecular weight side.
[0194] Conventional olefin polymerization catalysts containing metallocene compounds have been characterized by a relatively narrow molecular weight distribution, but for the reasons mentioned above, the olefin polymerization catalyst of the present invention can be said to be a unique catalyst that exhibits a specific molecular weight distribution.
[0195] [Olefin polymer] According to the present invention, in the presence of an olefin polymerization catalyst containing a useful and novel transition metal compound (A) having the specific structure described above, an olefin selected from one or more α-olefins having 2 to 30 carbon atoms is polymerized to homopolymerize ethylene, or to copolymerize ethylene with at least one olefin A selected from olefins having 3 to 20 carbon atoms, or to polymerize an α-olefin such as propylene, thereby making it possible to produce an olefin polymer having a specific molecular weight distribution.
[0196] One embodiment of the olefin polymer includes an ethylene-based polymer containing ethylene-derived structural units in the range of preferably 50 to 100 mol%, more preferably 70 to 100 mol%, and even more preferably 90 to 100 mol%. The ethylene-based polymer contains the olefin A-derived structural units in the range of preferably 0 to 50 mol%, more preferably 0 to 30 mol%, and even more preferably 0 to 10 mol% in total. However, the total of the content of the ethylene-derived structural units and the content of the olefin A-derived structural units is 100 mol%. The ethylene-based polymer having the olefin A-derived structural units in the above range has excellent moldability. In addition, the olefin A-derived structural units may be contained within the scope of the present invention. The content of these can be measured by nuclear magnetic resonance spectroscopy, or, when a standard substance is available, infrared spectroscopy, or the like.
[0197] Among these polymers, ethylene homopolymer, ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-propylene-1-butene copolymer, ethylene-1-octene polymer, ethylene-1-hexene polymer, ethylene-4-methyl-1-pentene polymer, ethylene-propylene-1-octene polymer, ethylene-propylene-1-hexene polymer, and ethylene-propylene-4-methyl-1-pentene polymer are particularly preferred. The above copolymers are usually random copolymers, but may also be so-called block copolymers (impact copolymers) obtained by mixing or continuously producing two or more types selected from these polymers.
[0198] Among the polymers having the structural units described above, the ethylene polymer is preferably an α-olefin polymer consisting essentially of structural units derived from an α-olefin having 2 to 20 carbon atoms. "Substantially" means that the proportion of structural units derived from an α-olefin having 2 to 20 carbon atoms is 95% by weight or more with respect to all structural units.
[0199] In the case of α-olefin polymers, it is possible to obtain olefin polymers with relatively high regularity that exhibit a melting point.
[0200] In the above-mentioned olefin polymer, the weight average molecular weight measured by gel permeation chromatography (GPC) is not particularly limited, but is preferably 10,000 to 5,000,000, more preferably 10,000 to 2,000,000, and particularly preferably 20,000 to 1,000,000. The molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is not particularly limited, but is preferably 4 to 20, more preferably 5 to 10. In addition, the value of Mz / Mw, which is considered to be an index of the molecular weight distribution having a spread toward the high molecular weight side, is preferably 3 to 10, more preferably 3.5 to 6.
[0201] The olefin polymer obtained by the olefin polymerization catalyst of the present invention has the above-mentioned molecular weight distribution, and therefore has good melt fluidity and excellent moldability, and therefore can efficiently obtain various molded articles such as injection molded articles, extrusion molded articles, blow molded articles, and spherical molded articles. In addition, necking and surging during film molding are improved, and high-quality films can be efficiently obtained. Also, fewer fisheyes are expected.
[0202] In the case of an ethylene-based polymer, the density of the olefin polymer is not particularly limited, but is preferably 875 kg / m 3 More than 975kg / m 3 It is preferable that:
[0203] In the olefin polymer, the intrinsic viscosity [η] in decalin at 135° C. is not particularly limited, but is preferably 0.1 to 40 dl / g, more preferably 0.5 to 15 dl / g, and particularly preferably 1 to 10 dl / g.
[0204] The melt mass flow rate (MFR; unit: g / 10 min) of the olefin polymer measured according to ASTM D1238 standard at 190°C under a load of 2.16 kg or at 230°C under a load of 2.16 kg depending on the melting point of the obtained olefin polymer is not particularly limited, but is preferably 0.001 g / 10 min or more and 300 g / 10 min or less, and more preferably 0.001 g / 10 min or more and 200 g / 10 min or less.
[0205] In addition, it is preferable that the value (I10 / I2) obtained by dividing the MFR value measured under conditions of 190°C or 230°C and a load of 10 kg according to ASTM D1238 by the MFR value measured under conditions of 190°C and a load of 2.16 kg is 5.0 or more and less than 300. The details of the conditions for measuring the above physical properties are as described in the Examples.
[0206] Some of the transition metal compounds (A) used in the present invention are novel compounds, and their structures are specified by the following formula (A-2).
[0207] [ka]
[0208] [In the formula (A-2), R 1 is a substituent having two or more independent ring structures, R 2 , R 2' , R 3 , R 3' is a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group, R 4 , R 5 is a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group, or a nitrogen-containing group, M' is a transition metal atom selected from titanium and hafnium.
[0209] R 2 , R 2' , R 3 , R 3' , R 4 , and R 5 Specific examples and preferred examples of each substituent are the same as those of the same symbols in formula (A-1).
[0210] The transition metal compound represented by the general formula (A-2) can be produced by synthesizing a corresponding ligand using a known organic synthesis technique such as a coupling method as described in the synthesis example section of the examples below, anionizing the ligand, and then reacting the anion with a corresponding transition metal halide.
[0211] <<Production method of transition metal compound (A)>> The method for producing the transition metal compound (A) is not particularly limited, and for example, the "Synthesis Example" in the Examples described later can be used. The transition metal compound (A) may also be synthesized using a known reaction. The transition metal compound (A) may also be synthesized by synthesizing each part by a known synthesis method and bonding them by a known method. As an example, the transition metal compound (A) can be synthesized by the method shown below.
[0212] [ka]
[0213] The transition metal compound (A) can be synthesized by dissolving the ligand in a solvent, reacting it with two equivalents of a strong base, and then reacting it with a metal chloride. Representative strong bases include organolithium reagents such as butyllithium and methyllithium. Preferred solvents include hydrocarbon solvents such as hexane, heptane, cyclohexane, and toluene, or diethyl ether, cyclopentyl methyl ether, tetrahydrofuran, and tert-butyl methyl ether.
[0214] [ka]
[0215] Alternatively, the ligand and the transition metal amide complex (M(NR a 2) and 4) are reacted to obtain the R 4 , R 5 It is possible to synthesize a complex in which R is a dialkylamino group. a The amide complex obtained may be used as it is in a polymerization reaction, or may be reacted with a chlorinating agent to obtain R. 4 , R 5 The chlorinating agent can convert the R b n SiCl 4-n (n is a value from 0 to 3), and examples of such compounds include SiCl4, Me2SiCl2, and Me3SiCl.
[0216] [ka]
[0217] The transition metal compound (A) can also be synthesized by reacting a ligand with an alkyl metal complex. cis not particularly limited, but examples thereof include a methyl group, an ethyl group, and a benzyl group. 4 , R 5 It is possible to synthesize a compound having a hydrocarbon group.
[0218] [ka]
[0219] R 4 , R 5 As a method for introducing a hydrocarbon group into R 4 , R 5 A transition metal compound (A) having a halogen atom in R is reacted with a Grignard reagent or an organolithium reagent to obtain the compound R 4 , R 5 It is possible to introduce a hydrocarbon group into the compound. Furthermore, such a compound can react with a compound having an OH group to introduce an oxygen-containing group or a substituted aryl group.
[0220] As described above, such a compound can be suitably used as an olefin polymerization catalyst, and can produce a polymer having a specific molecular weight distribution. EXAMPLES
[0221] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0222] [Measurement method] [Structure of transition metal compound] The structure of the transition metal compound is 1 H-NMR spectra were determined using a 400 MHz JNM-ECZ400S / L1 model manufactured by JEOL Ltd. or a 500 MHz AVANCE NEO cryo-500 model manufactured by Bruker Biospin.
[0223] [Polymer stereoregularity] The stereoregularity of a polymer (triad isotacticity (mm)) is 13Calculated from C-NMR spectrum measurement.
[0224] [Polymer weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the olefin polymer were determined by gel permeation chromatography (GPC). They were calculated from the molecular weight distribution curve obtained by a gel permeation chromatograph (high temperature size exclusion chromatograph) "HLC-8321GPC·HT type" manufactured by Tosoh Corporation, and the operating conditions were as follows.
[0225] <Apparatus and conditions used> Measuring device: Gel permeation chromatograph HLC-8321GPC·HT type (Tosoh Corporation) Analysis software: Chromatography Data System Empower3 (trademark, manufactured by Waters) Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HTL x 2 (Inner diameter 7.5mm x length 30cm, Tosoh Corporation) Mobile phase: o-Dichlorobenzene [ODCB] (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) Detector: Differential refractometer (built into the device) Column temperature: 140°C Flow rate; 1.0mL / min Injection volume: 400μL Sampling time interval: 0.5 seconds Sample concentration: 0.15% (w / v) Molecular weight calibration: Monodisperse polystyrene (Tosoh Corporation) / molecular weight 495 to 20.6 million Molecular weight conversion: PS (polystyrene) conversion / standard conversion method
[0226] [Limiting viscosity] Measured in decalin at 135°C according to ASTM D4020 standard.
[0227] [Synthesis Example 1] A stirrer tip was placed in a thoroughly dried 500mL three-neck flask under a nitrogen atmosphere, and a three-way cock and a thermometer were attached. 150mL of dehydrated dichloromethane, 7.9g of indene, and 12.9g of 2,6-di-tert-butyl-4-methylpyridine were added and stirred while cooling in an ice bath. 9.8mL of trifluoromethanesulfonic anhydride was slowly added dropwise, and after the addition, the temperature was raised to room temperature and stirred overnight. Hexane was added and stirred for a while, and then insoluble matter was filtered off. The filtrate was placed in a separatory funnel, and the organic layer was washed with a 0.5mol / L aqueous hydrochloric acid solution to separate the organic layer and the aqueous layer. The organic layer was then washed with water and saturated saline. The organic layer was dried over magnesium sulfate, and the magnesium sulfate was filtered off. The organic layer was concentrated using a rotary evaporator to obtain a crude product. The crude product was purified by silica gel column chromatography to obtain 14.9g of compound A represented by the following formula. NMR data of compound A 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ3.49 (d, J = 2.2 Hz, 2 H), 6.38 (t, J = 2.2 Hz, 1 H), 7.31-7.45 (m, 3 H), 7.48 (d, J = 7.1 Hz, 1 H).
[0228] [ka]
[0229] [Synthesis Example 2] A thoroughly dried 1000 mL three-neck flask was placed in a nitrogen atmosphere, and a stirrer tip, a three-way cock and a thermometer were attached. 25 g of 1,2-dibromobenzene, dehydrated THF 250mL was added and cooled in a dry ice acetone bath. While being careful not to exceed -75°C in the internal temperature, n-butyllithium hexane solution (1.6mol / L) was slowly dropped. After dropping, the temperature was gradually raised and stirring was performed overnight. 200mL of water was added, followed by tert-butyl methyl ether to extract the organic layer. The organic layer and the aqueous layer were separated using a separatory funnel, and the organic layer was washed with saturated saline. The organic layer was dried over magnesium sulfate, and the magnesium sulfate was filtered off. The filtrate was concentrated using a rotary evaporator to obtain 16.9 grams of crude product. When left to stand at room temperature, the entire product solidified. The solid was broken down with a spatula, washed with 15ml of hexane, and filtered. The hexane washing operation was performed a total of three times. The washed solid was dried under reduced pressure to obtain 10.6 grams of compound B represented by the following formula (yield 64%). NMR data of compound B 1 H NMR(400 MHz, CDCl3, 298 K, δ in ppm) δ7.23-7.29 (m, 4 H), 7.35-7.41 (m, 2 H), 7.65-7.69 (m, 2 H).
[0230] [ka]
[0231] [Synthesis Example 3] A 300 mL three-neck flask was thoroughly dried and equipped with a stirrer tip, a three-way cock and a thermometer under a nitrogen atmosphere. 6.2 g of compound B and 60 mL of dehydrated diethyl ether were added. The mixture was stirred while being cooled in a dry ice acetone bath until the internal temperature did not exceed -75°C. While being careful not to drop the solution, 27.5 mL of n-butyllithium hexane solution (1.6 mol / L) was slowly added dropwise. After the addition, the mixture was stirred for 2 hours while cooled, and then the temperature was raised to room temperature. Stirring was continued overnight. The flask was cooled in a dry ice acetone bath, and 8.6 mL of trimethoxyborane was slowly added dropwise. After the addition, the temperature was raised to room temperature, and the mixture was stirred at room temperature for 4 hours. 70 mL of 2 mol / L aqueous hydrochloric acid was added to quench the reaction. The organic layer and the aqueous layer were separated using a separatory funnel, and the organic layer was washed with water and saturated saline. The organic layer was dried over magnesium sulfate, and the magnesium sulfate was filtered off. The filtrate was concentrated using a rotary evaporator to obtain a crude product containing compound C represented by the following formula. The compound obtained was used in the next step without further purification.
[0232] [ka]
[0233] [Synthesis Example 4] A stirrer tip was placed in a thoroughly dried 500mL three-neck flask under a nitrogen atmosphere, and a three-way cock and a thermometer were attached. 3.7 grams of compound C, 1.2 grams of tetrakis(triphenylphosphine)palladium, 9.0 grams of cesium carbonate, 7.8 grams of potassium fluoride dihydrate, 3.5 grams of sodium bromide, 9.0 grams of compound A, and 130 mL of dehydrated toluene were added, and the mixture was heated and stirred at 80°C for 3 hours. After cooling to room temperature, 200 mL of water was added and stirred. The reaction solution was filtered through Celite, and the filtrate was added to a separatory funnel to separate the organic layer and the aqueous layer. The organic layer was washed with water and saturated saline, and then dried over magnesium sulfate. After filtering off the magnesium sulfate, the mixture was concentrated using a rotary evaporator to obtain 8.35 grams of crude product. The crude product was purified by silica gel column chromatography to obtain 3.38 grams of compound D represented by the following formula (yield 58%). NMR data of compound D 1H NMR(400 MHz, CDCl3, 300 K, δ in ppm) δ2.74-3.01 (m, 4H), 5.66 (t, J = 2.0 Hz, 2 H), 6.81-6.87 (m, 2 H), 6.94-7.03(m, 4H), 7.11-7.17 (m, 2H), 7.28-7.41 (m, 6H), 7.45-7.51 (m, 2H).
[0234] [ka]
[0235] [Synthesis Example 5] A stirrer tip was placed in a thoroughly dried 1000mL three-neck flask under a nitrogen atmosphere, and a three-way cock and a thermometer were attached. 251.8mg of tetrakisdimethylamido zirconium, 450mL of dehydrated toluene, and 295.5mg of compound D were added and heated under reflux overnight. After distilling off the toluene, the flask was brought into a glove box. Hexane was added and stirred, and insoluble matter was filtered off. The filtrate was concentrated to obtain 505mg of a crude product containing an amide complex. A stirrer tip was placed in a thoroughly dried 100mL three-neck flask under a nitrogen atmosphere, and a three-way cock and a thermometer were attached. The crude product synthesized above was dissolved in 35mL of dehydrated toluene, and 0.58g of dichlorodimethylsilane was added. Heating and stirring were carried out at 60°C and continued overnight. The flask was brought into a glove box, and insoluble matter was filtered off using a filter with a pore size of 3μm. The solid matter on the filter was washed with dehydrated toluene and then with dehydrated hexane, and dried under reduced pressure to obtain 194.5mg of compound E represented by the following formula as a yellow solid (yield 46%). NMR data of compound E 11H NMR (500 MHz, CDCl3, 298 K, δ in ppm) δ 6.41 (d, J = 4.0 Hz, 2H), 6.50 (d, J = 4.0 Hz, 2H), 7.23 - 7.29 (m, 2H), 7.32 - 7.40 (m, 4H), 7.48 (td, J = 1.5, 7.6 Hz, 2H), 7.52 (td, J = 1.5, 7.6 Hz, 2H), 7.58 (d, J = 8.5 Hz, 2H), 8.03 (d, J = 8.5 Hz, 2H), 8.09 (dd, J = 1.5, 7.6 Hz, 2H). 13 13C NMR (126 MHz, CDCl3, 298 K, δ in ppm) δ 112.0, 112.6, 118.7, 123.2, 125.2, 126.5, 126.5, 127.3, 127.8, 128.1, 128.2, 128.9, 131.5, 134.8, 139.5
[0236] [Chemical Example 6]
[0237] [Synthesis Example 6] A stirrer tip was placed in a thoroughly dried 1000mL three-neck flask under a nitrogen atmosphere, and a three-way cock and a thermometer were attached. 334mg of tetrakisdimethylamidohafnium, 450mL of dehydrated toluene, and 303mg of compound D were added and heated under reflux for 12 days. After the toluene was distilled off, the flask was brought into a glove box. Hexane was added and stirred, and the insoluble matter was filtered off. The filtrate was concentrated to obtain a crude product containing 600mg of amide complex. A small amount of hexamethyldisiloxane was added, the whole was stirred, and then allowed to stand. The supernatant was removed by decantation. A small amount of hexane was added to the solid matter, the whole was stirred, and then allowed to stand. The supernatant was removed by decantation. A small amount of hexane was added to the solid matter again, and the solid matter was stirred and then allowed to stand, resulting in a yellow precipitate. The precipitate was filtered using a membrane filter with a pore size of 3μm, and the solid matter on the filter was washed with a small amount of hexane. The solid matter was dried under reduced pressure to obtain 98 mg of compound F represented by the following formula (yield 19%). NMR data of compound F 1 H NMR(500 MHz, CDCl3, 298 K, δ in ppm) δ2.27 (s, 12H), 5.98 (dd, J = 0.6, 3.7 Hz, 2H), 6.33 (d, J = 3.7 Hz, 2H), 6.95-7.00 (m, 2H), 7.09-7.14 (m, 2H), 7.32-7.40 (m, 4H), 7.44-7.49 (m, 2H), 7.52 (dt, J = 0.6, 8.2 Hz, 2H), 7.99 (dd, J = 0.6, 7.9 Hz, 2H), 8.10-8.13 (m, 2H). 13 C NMR(126 MHz, CDCl3, 298 K, δ in ppm) δ47.0, 98.8, 107.5, 117.2, 121.8, 122.8, 123.5, 124.1, 124.2, 126.1, 127.3, 128.2, 129.4, 133.15, 133.20, 139.6.
[0238] [ka]
[0239] [Synthesis Example 7] Compound G represented by the following formula was synthesized based on the method described in US Pat. No. 5,360,921.
[0240] [ka]
[0241] [Synthesis Example 8] Compound H represented by the following formula was synthesized by the method described in European Patent Publication 0754698.
[0242] [ka]
[0243] [Synthesis Example 9] Compound I represented by the following formula was synthesized according to the method described in Example 8 of European Patent Publication No. 1059300.
[0244] [ka]
[0245] [Example 1] 250mL of toluene was charged into a glass reactor with an internal volume of 500mL, which had been thoroughly purged with nitrogen, and ethylene was passed through at 100L / hr to saturate the liquid and gas phases. Then, 0.5mmol of methylaluminoxane (calculated as aluminum atom) and 0.5μmol of compound E were added to initiate polymerization. Ethylene was continuously fed at 100L / hr, and polymerization was carried out for 5 minutes at an internal temperature of 50°C under normal pressure, after which polymerization was terminated by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750mL of methanol containing a small amount of hydrochloric acid to precipitate the polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours to obtain 2.2 grams of ethylene polymer. The physical properties of the obtained polymer are shown in Table 1.
[0246] [Example 2] 250 mL of toluene was charged into a glass reactor with an internal volume of 500 mL, which had been thoroughly purged with nitrogen, and ethylene was passed through at 100 L / hr to saturate the liquid and gas phases. Then, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, 0.25 μmol of compound E, and 1.0 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to start polymerization. Polymerization was started by adding ethylene. Ethylene was continuously fed at 100 L / hr, and polymerization was carried out for 5 minutes at an internal temperature of 50°C under normal pressure, and then polymerization was stopped by adding a small amount of methanol. After the polymerization was completed, the reactant was added to 750 mL of methanol containing a small amount of hydrochloric acid to precipitate a polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours to obtain 1.6 grams of ethylene polymer. The physical properties of the obtained polymer are shown in Table 1.
[0247] [Example 3] Under a nitrogen atmosphere, 2.4 mg (4.4 μmol) of compound E was placed in a Schlenk flask, 4.4 mL of toluene and 0.88 mL (0.88 mmol, 1 mmol / mL) of a toluene solution of triisobutylaluminum were added, and the mixture was stirred at room temperature for 10 minutes or more to prepare a catalyst solution with a transition metal compound (compound E) concentration of 0.84 μmol / mL. In a SUS autoclave with a capacity of 15 mL and fully purged with nitrogen, 0.2 mL (0.05 M) of a heptane solution of triisobutylaluminum and 0.54 mL of heptane as a polymerization solvent were placed and stirred at 600 rpm. The obtained solution was heated to 60° C., and then the inside of the autoclave was pressurized with propylene until the total pressure reached 7 bar. The autoclave was charged with 0.96 mL of the catalyst solution (concentration of compound E was 0.84 μmol / mL, amount was 0.80 μmol), 1.6 mL (0.005 mmol / mL) of a toluene solution of triphenylcarbenium tetrakis(pentafluorophenyl)borate, and then 0.7 mL of heptane to initiate polymerization. After polymerization for 60 minutes at 60° C., a small amount of isobutyl alcohol was added to terminate the polymerization. Methanol and 1 mL (1 M) of hydrochloric acid were added to the obtained polymer solution, and the mixture was stirred at room temperature for a while. The precipitated polymer was filtered, washed with acetone, and then dried under reduced pressure at 80°C for 10 hours to obtain 0.0389mg of propylene polymer. NMR analysis of the propylene polymer showed that the mmmm, which indicates regularity, was 56.8%, the weight average molecular weight (Mw) was 43,100, and the Mw / Mn, which is an index of molecular weight distribution, was 6.18. The physical properties of the obtained polymer are shown in Table 1.
[0248] [Comparative Example 1] 250 mL of toluene was charged into a glass reactor with an internal volume of 500 mL, which had been thoroughly purged with nitrogen, and ethylene was passed through at 100 L / hr to saturate the liquid and gas phases. Then, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, 0.05 μmol of compound G, and 0.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to start polymerization. Polymerization was started by adding propylene. Propylene was continuously fed at 100 L / hr, and polymerization was carried out for 5 minutes at normal pressure and an internal temperature of 50°C, after which polymerization was stopped by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750 mL of methanol containing a small amount of hydrochloric acid to precipitate the polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours, and 0.064 grams of ethylene polymer was obtained. The physical properties of the obtained polymer are shown in Table 1.
[0249] [Comparative Example 2] 250 mL of toluene was charged into a glass reactor with a capacity of 500 mL, which had been thoroughly purged with nitrogen, and ethylene was passed through at 100 L / hr to saturate the liquid and gas phases. Then, 0.2 mmol of triisobutylaluminum in terms of aluminum atom, 5 μmol of compound H, and 20 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were added to start polymerization. Polymerization was started by adding propylene. Propylene was continuously fed at 100 L / hr, and polymerization was carried out for 5 minutes at normal pressure and an internal temperature of 50°C, after which polymerization was stopped by adding a small amount of methanol. After polymerization was completed, the reactant was added to 750 mL of methanol containing a small amount of hydrochloric acid to precipitate the polymer. After washing with the same solvent, it was dried under reduced pressure at 80°C for 10 hours, and 0.852 grams of ethylene polymer was obtained. The physical properties of the obtained polymer are shown in Table 1.
[0250] [Table 1]
[0251] [Comparative Example 3] A catalyst solution having a compound I concentration of 0.46 μmol / mL and a triisobutylaluminum concentration of 0.91 mmol / mL was prepared in the same manner as in Example 3, except that compound I was used instead of compound E and the amounts of each component were adjusted. In addition, propylene was polymerized in the same manner as in Example 3, except that 0.5 mL of the catalyst solution (concentration of compound I: 0.46 μmol / mL) was used instead of compound E so that the amount of compound I was 0.23 μmol, 0.46 mL of toluene was further added, and the polymerization time was 5 minutes, to obtain a propylene polymer. The weight average molecular weight (Mw) of the resulting polymer was 5,990, and the molecular weight distribution was 1.75.
[0252] The olefin polymerization catalyst containing Compound I gave polymers with a relatively narrow molecular weight distribution, similar to the olefin polymerization catalyst containing a general transition metal complex compound, and the molecular weight was also lower than that of the olefin polymerization catalyst containing the transition metal complex compound of the present invention. From these viewpoints, it is understood that the olefin polymerization catalyst containing Compound I has properties different from those of the olefin polymerization catalyst of the present invention. In addition, the structure of compound I is outside the scope of the transition metal compound (A) used in the present invention, but has a similar structure. Therefore, it is natural to think that compound I may also undergo mutations as described in paragraphs 0193-0194 above, and may be capable of taking multiple conformations. However, due to the structure of compound I, the various conformations tend to be easily in a symmetrical relationship such as enantiomers, so it is considered that the fluctuations in reaction rate, chain transfer rate, etc. are relatively small, and the difference in performance that affects the molecular weight distribution is small.
Claims
1. (A) a transition metal compound represented by the following general formula (A-1), 【Chemistry 1】 [In formula (A-1), R 1 is a substituent having two or more independent ring structures, R 2 , R 2' , R 3 , and R 3' each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 4 and R 5 each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group, or a nitrogen-containing group, M is a metal atom of Group 4 of the periodic table. (B) (B-1) organometallic compound, (B-2) an organoaluminum oxy compound, and (B-3) A compound that reacts with the transition metal compound (A) to form an ion pair. At least one compound selected from the group consisting of A catalyst for olefin polymerization comprising:
2. The R 1 2. The olefin polymerization catalyst according to claim 1, wherein is a substituent selected from a biphenyl group and a substituted biphenyl group.
3. The R 4 and R 5 The olefin polymerization catalyst according to claim 1, wherein is a halogen atom.
4. 2. The olefin polymerization catalyst according to claim 1, wherein M is a transition metal atom selected from titanium, zirconium, and hafnium.
5. A method for producing an olefin polymer, comprising polymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of claims 1 to 4.
6. The method for producing an olefin polymer according to claim 5, wherein the olefin is selected from olefins having 2 to 30 carbon atoms.
7. The process for producing an olefin polymer according to claim 5, wherein the olefin is selected from the group consisting of ethylene, propylene and 1-butene.
8. A transition metal compound represented by the following general formula (A-2): 【Chemistry 2】 [In the formula (A-2), R 1 is a substituent having two or more independent ring structures, R 2 , R 2' , R 3 , and R 3' each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a diene-based divalent derivative group; R 4 and R 5 each independently represents a substituent selected from a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group, or a nitrogen-containing group, M' is a transition metal atom selected from titanium and hafnium.
Citation Information
Patent Citations
Ethylenic polymer composition
EP0783022A1
Indenyl compounds for the polymerisation of olefins
EP1059300A1